Oil-resistant paper, method for suppressing degree of smoke generation at heating of oil-resistant paper, method for suppressing reduction of rupture strength at heating of oil-resistant paper, and paper container for heating using oil-resistant paper

The oil-resistant paper with UV-irradiated pulp fibers and a fluorine-based agent effectively suppresses smoke and maintains strength at high temperatures, addressing the limitations of conventional papers and plastics in toaster ovens.

JP2024142534APending Publication Date: 2024-10-11UNI CHARM CORP
View PDF 1 Cites 0 Cited by

Patent Information

Application Number
JP2023054694
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Filing Date
2023-03-30
Publication Date
2024-10-11

AI Technical Summary

Technical Problem

Conventional oil-resistant paper emits smoke when heated at high temperatures and loses strength, making it unsuitable for prolonged use in toaster ovens, and plastic containers pose environmental concerns.

Method used

The oil-resistant paper is composed of at least 90% pulp fibers with a fluorine-based oil-resistant agent on one side, and UV irradiation enhances its smoke suppression and strength retention by converting cellulose and hemicellulose into polymers, increasing pyrolysis temperature.

Benefits of technology

The paper suppresses smoke generation for at least 16 minutes at 250°C and maintains a bursting strength of 0.3 MPa or more, suitable for use as a paper container in toaster ovens without deforming.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024142534000001_ABST
    Figure 2024142534000001_ABST
Patent Text Reader

Abstract

To provide oil-resistant paper capable of suppressing smoke generation and having required strength, even when heated at high temperatures for a required time to the extent that food is scorched.SOLUTION: Oil-resistant paper 1 has a first surface 11, a second surface 12 located on the opposite side, and at least 90 mass% of pulp fibers, and contains a fluorine-based oil-resistant agent in at least the first surface 11 of the first and second surfaces 11, 12, and has a smoke generation time of at least 16 minutes in a smoke generation test at 250°C.SELECTED DRAWING: Figure 1
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to grease-resistant paper, a method for suppressing the level of smoke generation from grease-resistant paper when heated, a method for suppressing a decrease in burst strength of grease-resistant paper when heated, and a paper container for heating that uses grease-resistant paper. [Background technology]

[0002] Grease-resistant paper for use in electric ovens has been publicly known. For example, Patent Document 1 discloses grease-resistant paper having a paper base material and an oil-resistant layer, the oil-resistant layer containing a polylactic acid resin and a polyvinyl alcohol resin and / or a starch compound in a weight ratio of 70:30 to 98:2. [Prior art documents] [Patent documents]

[0003] [Patent Document 1] JP2020-128616A Summary of the Invention [Problem to be solved by the invention]

[0004] The grease-resistant paper disclosed in Patent Document 1 has excellent water resistance and oil resistance, and also has a certain degree of heat resistance at high temperatures, so it can be used, for example, as containers for frozen foods that are heated in a toaster oven.

[0005] However, when this type of conventional greaseproof paper was used as a paper container for food in a toaster oven, there was a problem that it would emit smoke when heated at a high temperature of nearly 250°C for more than 5 minutes until the food was browned. Therefore, it was not possible to heat the food to a browning point. In addition, the strength of the greaseproof paper was reduced by heating, and the shape of the paper container became unstable, making it difficult to remove from the oven, etc.

[0006] Unlike plastic containers, paper containers cannot withstand the high temperatures and harsh use of a toaster oven, and so frozen foods are often placed in plastic containers and heated in a microwave oven. In this case, frozen foods are heated in a plastic container, but there are issues with the taste, such as uneven heating and not being able to brown the food. There are also environmental issues with using plastic containers. Therefore, there was a demand for paper containers that could contribute to both deliciousness when heated and environmental issues.

[0007] The present invention is an improvement over conventional grease-resistant paper, and aims to provide grease-resistant paper that can suppress smoke generation and has the required strength, even when heated at high temperatures for the required time to the extent that food is browned. [Means for solving the problem]

[0008] In order to solve the above-mentioned problems, the first invention of the present application relates to an grease-resistant paper having a first side, a second side located on the opposite side, and at least 90% by mass of pulp fibers, wherein at least the first side of the first and second sides contains a fluorine-based grease-resistant agent.

[0009] The first invention of the present application is the greaseproof paper, which is characterized in that the smoke generation time in the below-mentioned smoke generation test at 250°C is at least 16 minutes. [Smoke test] A test piece (100mm x 100mm) is placed in an electric oven set at 250℃, and heating is started with the test piece laid horizontally between the upper and lower heaters.The test piece is then observed through the observation window of the electric oven, and the time until it is possible to recognize smoke coming from the test piece with the smoke generation identification mark in the background is measured, and this time is regarded as the smoke generation time.

[0010] The second invention of the present application relates to an grease-resistant paper having a first side, a second side located on the opposite side, and at least 90% by mass of pulp fibers, wherein at least the first side of the first and second sides contains a fluorine-based grease-resistant agent.

[0011] The greaseproof paper according to the second aspect of the present invention is characterized in that the burst strength of the greaseproof paper after heating at 250° C. for 10 minutes is 0.3 MPa or more.

[0012] The first and second inventions of the present application include the following preferred embodiments. (1) The burst strength of the greaseproof paper after heating at 250°C for 20 minutes is 0.2 MPa or more. (2) The grease-resistant paper is irradiated with ultraviolet light UV-A from an ultraviolet lamp under the following irradiation conditions on at least the first surface of the first and second surfaces. [Ultraviolet lamp irradiation conditions] (1) Wavelength range: 315-400 μm (2) Ultraviolet intensity: 120mW / cm 2 (3) Irradiance: 120mW sec / cm 2 (4) Irradiation time: 1 second (3) The amount of the grease-resistant agent contained on the first surface side of the grease-resistant paper is greater than the amount of the grease-resistant agent contained on the second surface side. (4) The fiber density on the first surface side is higher than the fiber density on the second surface side. (5) The pulp fibers contain pulp fibers derived from coniferous trees and pulp fibers derived from broad-leaved trees, and the content of the pulp fibers derived from the coniferous trees is higher than the content of the pulp fibers derived from the broad-leaved trees. (6) Mass is 250 to 400 g / m 2 , the thickness is 0.2~0.5mm. (7) The difference in smoke generation time between when the first surface of the grease-resistant paper is irradiated with ultraviolet light UV-A and when the second surface of the grease-resistant paper is irradiated with ultraviolet light UV-A is within 90 seconds.

[0013] The third invention of the present application relates to a method for reducing the level of smoke generated when greaseproof paper is heated.

[0014] The method according to the third invention of the present application is characterized in that at least one of the two surfaces of the grease-resistant paper contains a fluorine-based grease-resistant agent, and at least one of the surfaces of the heat-resistant paper is irradiated with ultraviolet light via an ultraviolet lamp for a required period of time.

[0015] The fourth invention of the present application relates to a method for suppressing a decrease in burst strength of greaseproof paper when heated.

[0016] The method according to the fourth invention of the present application is characterized in that at least one of the two surfaces of the grease-resistant paper is coated with a fluorine-based grease-resistant agent, and at least the one surface of the heat-resistant paper is irradiated with ultraviolet light via an ultraviolet lamp for a required period of time.

[0017] The fifth invention of the present application is a paper container for heating that uses grease-resistant paper. Effect of the Invention

[0018] The grease-resistant paper of the present invention is able to suppress smoke generation even when heated at high temperatures for the required time to brown food, and has the required burst strength, making it suitable for use as a paper tray container for heating. [Brief description of the drawings]

[0019] The drawings show specific embodiments of the present invention, including essential features of the invention as well as alternative and preferred embodiments. [Figure 1] FIG. 1A is a perspective view of the grease-resistant paper of the present invention; FIG. 1B is a cross-sectional view of the grease-resistant paper of the present invention taken along line I(a)-I(a). [Diagram 2] FIG. 1 is a perspective view of a paper tray container made of grease-resistant paper. [Diagram 3] (a) A diagram showing a paper tray container using conventional grease-resistant paper after being heated to a high temperature and removed from a toaster oven, (b) A diagram showing a paper tray container using the grease-resistant paper of the present invention after being heated to a high temperature and removed from a toaster oven. [Figure 4] (a) and (b) Schematic showing the smoke generation test. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0020] The following embodiment relates to greaseproof paper 1 shown in Figures 1 and 2, which is primarily used for heating in ovens (toaster ovens, oven ranges), etc., and includes not only essential configurations of the invention, but also optional and preferred configurations.

[0021] Referring to Figures 1(a) and (b), the grease-resistant paper 1 of the present invention is composed of a paper base material 10 made mainly from pulp fibers, and has a thickness direction, a front surface (first side) 11 and a back surface (second side) 12, a front layer (oil-resistant agent coating layer) 13 to which an oil-resistant agent is applied (coated) forming the first side 11, a back layer (oil-resistant agent internally added layer) 14 to which an oil-resistant agent is internally added forming the second side 12, and an intermediate layer (water-resistant layer) 15 located between the front and back layers 13, 14.

[0022] As shown in FIG. 2, the grease-resistant paper 1 can be suitably used as a material for a heating paper tray container (paper container) 20 for carrying fried foods (frozen foods) such as French fries, fried chicken, and croquettes, which are heated at high temperatures in a toaster oven, as well as gratin, pizza, and foods other than processed foods such as cooked rice, grilled fish, and side dishes prepared in ordinary households.

[0023] The paper base material 10 has been subjected to a water-resistant treatment and has relatively strong water resistance as a whole. Specifically, the paper base material 10 has a cup water absorbency of 150 to 230 g / m 2 The paper substrate 10 has a water resistance of 60 min. The cup water absorbency is 300 g / m 2 - The water absorption is lower than that of general printing paper after 60 minutes or more, and it can be said that it can suppress the penetration of moisture and oil generated from food to the opposite side. In this way, since the paper base material 10 has a relatively high water resistance, the intermediate layer 15 can also be said to be a (strong) water-resistant layer. Regarding water resistance, the water absorption amount of the surface 11 after 60 minutes was measured according to JIS P 8140 (1976) Water Absorption Test Method for Paper and Paperboard (Cobb method).

[0024] The oil-resistant agent applied to the front surface 11 (front layer 13) and added to the back surface 12 (back layer 14) is a fluorine-based oil-resistant agent, and examples of such agents include anionic fluorine-based resins and cationic fluorine-based resins. Commercially available anionic fluorine-based oil-resistant agents include Asahi Guard (registered trademark) AG-E080 and AG-E090 manufactured by Asahi Glass Co., Ltd., Unidyne (registered trademark) TG-8111 and TG8731 manufactured by Daikin Industries, Ltd., and Solvera (registered trademark) PT5060 and PT5045 manufactured by Solvay. Commercially available cationic fluorine-based oil-resistant agents include Asahi Guard (registered trademark) AG-E060 and AG-E070 manufactured by Asahi Glass Co., Ltd., and CAPSTONE (registered trademark) P620 and P623 manufactured by DuPont.

[0025] Since the amount of oil-resistant agent applied to the surface layer 13 is greater than the amount of oil-resistant agent added to the back layer 14, it can be said that the surface layer 13 has higher oil resistance than the back layer. The amount of oil-resistant agent applied to the surface layer 13 is 3.0 to 15.0 g / m 2 The coating can be applied to the paper substrate 10 by a known coating method such as a curtain coater, a spray coater, or a roll coater.

[0026] The paper base material 10 used in the grease-resistant paper 1 of the present invention is made by papermaking a paper material containing 90% by mass of pulp fiber, fillers, various auxiliary agents, etc., and examples of such paper include fine paper, medium quality paper, lightly coated paper, coated paper, one-sided glossy paper, bleached or unbleached kraft paper (acidic paper or neutral paper), or paperboard or white paperboard used for corrugated board, white board, chipboard, etc.

[0027] Any material normally used for papermaking can be used as the raw material for the pulp fibers that make up the paper base material 10. For example, chemical pulps such as bleached hardwood kraft pulp (LBKP), bleached softwood kraft pulp (NBKP), bleached hardwood sulfite pulp (LBSP), and bleached softwood sulfite pulp (NBSP), unbleached, semi-bleached, or bleached pulps such as stone ground pulp (GP), pressurized stone ground pulp (PGW), refiner ground pulp (RGP), chemi-ground pulp (CGP), thermomechanical pulp (TMP), and chemi-thermomechanical pulp (CTMP), and sulfite pulp can be used.

[0028] In the pulp fibers, it is preferable that the blending ratio of softwood-derived pulp fibers is higher than that of hardwood-derived pulp fibers in order to increase the strength and density of the paper base material 10. Also, the blending ratio of softwood-derived pulp fibers may be higher in the front layer 13 than in the back layer.

[0029] The weight of the paper substrate 10 is preferably 250 g / m 2 Above, 250~400g / m 2 By setting the mass of the paper substrate 10 within the above range, it is possible to maintain the strength required for forming the oil-resistant layer. 2 In the following cases, the strength is low, and the paper tray container 20 cannot maintain its shape, and the shape may collapse especially after heating. 2 If the bending moment exceeds this value, when the paper tray container 20 is made, the base material is likely to buckle at the fold during the manufacturing process, causing the paper base material 10 to crack and tending to reduce the oil resistance of the fold.

[0030] The thickness of the paper substrate 10 is preferably 0.2 to 0.5 mm. A thickness gauge (PEACOCK DIAL THICKNESS GAUSE, diameter 50 mm, measurement pressure 3 g / cm 2 ) was measured.

[0031] The density of the paper base material 10 is 0.6 to 1.5 g / cm 3It is preferable that the density is 0.8 to 1.0 g / cm 3 It is more preferable that the density of the paper base material 10 is within this range. When the density of the paper base material 10 is within this range, the paper base material 10 has a strength that does not easily lose its shape when used as a paper tray container 20 while maintaining the required breathability, and has good moldability after high-temperature heating. Note that good moldability after high-temperature heating means that even if the greaseproof paper 1 is molded into a paper tray container for food or the like and heated at high temperature (220 to 280°C) in a toaster oven, the paper tray container is unlikely to deform.

[0032] In the paper base material 10 constituting the greaseproof paper 1 according to the present invention, the fiber densities of the front layer 13, back layer 14 and intermediate layer 15 may be different, and the fiber density on the front surface 11 side may be different from the fiber density on the back surface 12 side. Normally, in calendared paper, there may be a difference in fiber density on both sides, but for example, in the paper base material 10, when the fiber density on the front surface 11 side is higher than the fiber density on the back surface 12 side, it can be said that the oil resistance of the front layer 13 coated with an oil-resistant agent is improved and the sheet strength of the entire greaseproof paper 1 is also increased.

[0033] The paper base material 10 may contain additives. Examples of additives include fixing agents such as aluminum sulfate and cationic polymer electrolytes, paper strength enhancers such as clay, talc, calcium carbonate, calcined kaolin, aluminum oxide, aluminum hydroxide, titanium oxide, and starch, wet strength enhancers such as melamine resin and urea resin, and various other auxiliary agents such as drainage agents, dyes for adjusting color tone such as bluing, and fluorescent dyes. When titanium oxide is contained in the paper base material 10, even if oil from food penetrates into the paper base material 10, the transparency or blackening of the paper base material 10 due to the oil-soaked parts can be made less noticeable.

[0034] Normally, when greaseproof paper is used as a material for food paper trays and containers, etc., when it is heated to high temperatures of 220-300°C in an oven (including toaster ovens and oven ranges), the moisture in the pulp that constitutes the paper base evaporates, causing smoke, filling the toaster oven with smoke and causing a burnt smell to adhere to the food. In order to suppress the smoke generated by the greaseproof paper, it is possible to put it in a dryer during the manufacturing process, but if it is left for a long time after drying, the pulp will reabsorb moisture and the smoke suppression effect when used will not be fully demonstrated.

[0035] As a result of extensive research, the applicant has found that the required smoke suppression effect can be achieved by irradiating ultraviolet light onto at least one of the front and back surfaces 11, 12 of the greaseproof paper 1. It is believed that irradiating the greaseproof paper 1 with ultraviolet light moves the molecules in the pulp, causing glucose to fly off and polymerizing cellulose and hemicellulose, thereby increasing the pyrolysis temperature even when heated at high temperatures, thereby achieving the smoke suppression effect. Furthermore, as shown in the measurement results described below, by irradiating the grease-resistant paper 1 with ultraviolet light, the hardening strength is improved, and when the grease-resistant paper 1 is used as a paper tray container 20 for placing food on, after heating in an oven or the like, the paper tray container 20 can be used as a container (dishware) for eating as is.

[0036] Here, "smoke suppression effect when heated at high temperatures" refers to the smoke suppression effect when heated for 16 minutes or more at 250°C, assuming high temperatures in a toaster oven until food is browned. Conventional greaseproof paper starts to emit smoke when heated for about 10 minutes at 250°C, so if no smoke is emitted even after 16 minutes, it can be said to have excellent smoke suppression effect.

[0037] As mentioned above, the mass of the paper base material 10 is 250 g / m 2 From the viewpoint of heat resistance, when the mass of the paper base material 10 is relatively small, heat from the outside is easily transferred and the heat resistance is reduced. 2By satisfying the above, the film has excellent heat resistance and can exhibit a smoke suppression effect when the surface is heated to a high temperature.

[0038] When molding a paper tray container using such grease-resistant paper 1, at least one of the front and back surfaces 11, 12 of the grease-resistant paper 1 may be irradiated with ultraviolet light before molding the paper tray container, or after molding the grease-resistant paper 1 into a paper tray container, at least one of the front and back surfaces of the paper tray container may be irradiated with ultraviolet light.

[0039] It is not possible to distinguish whether the greaseproof paper 1 has been irradiated with ultraviolet light or not just by looking at its appearance; for example, no difference in appearance was observed between irradiated and unirradiated paper even when observed under an electron microscope at 300x magnification. However, after irradiation with ultraviolet light, the irradiated surface turns slightly yellow, so it can be distinguished by the difference in yellowness. The yellowness of the greaseproof paper 1 can be measured using a color difference meter in accordance with JIS-Z8722.

[0040] [Table 1]

[0041] Table 1 shows the sheet configurations of the greaseproof paper 1 according to the present invention in Examples 1 to 3 and Comparative Examples 1 to 4, the change in oil repellency (kit method) before and after UV irradiation, the change in burst strength before and after heating in an oven toaster, and the smoke evaluation after heating. The properties in the table were measured by the following methods.

[0042] <Mass> Three samples measuring 100 mm x 100 mm were cut out from each greaseproof paper, the mass of each sample was measured with a measuring device, and the mass per unit area (g / m) was calculated from the average. 2 "Mass before drying" is the mass of the grease-resistant paper before it is dried in a dryer, "mass after drying" is the mass of the grease-resistant paper after it has been dried in a dryer until its moisture content reaches around 1%, and "mass after irradiation" is the mass of the grease-resistant paper after it has been irradiated with UV light under the conditions below.

[0043] <Thickness Dimension> Regarding the thickness dimension of each material, it was measured by a thickness gauge (PEACOCK DIAL THICKNESS GAUGE with a diameter of 50 mm and a measuring pressure of 3 g / cm 2 ).

[0044] <Density> The density of each oil-resistant paper was calculated by dividing its mass by its thickness dimension (g / cm 3 ).

[0045] <Oil Repellency (Kit Method)> "Oil Repellency (Kit Method) Before UV Irradiation" refers to the oil repellency of each oil-resistant paper before UV irradiation, and "Oil Repellency (Kit Method) After UV Irradiation" refers to the oil repellency of each oil-resistant paper after UV irradiation under the following conditions. The oil repellency was measured by the TAPP UM-557 method (kit method). Generally, the oil repellency (kit oil resistance) that can be used as oil-resistant paper is grade 5 or above, and if the oil repellency is grade 9 or above, it can be said to have high oil repellency.

[0046] <UV Irradiation> UV irradiation was performed on the surface where food is placed, the opposite back surface, and both the front and back surfaces with an ultraviolet lamp under the following conditions to irradiate ultraviolet UV-A. 〔Irradiation Conditions of Ultraviolet Lamp〕 (1) Wavelength range: 315 - 400 μm (2) Ultraviolet intensity: 120 mW / cm 2 (3) Irradiation dose: ··· 120 mW·sec / cm 2 (4) Irradiation time ··· 1 second

[0047] <Burst Strength> "Burst strength / before oven heating" is the burst strength of each grease-resistant paper before heating in a toaster oven, "Burst strength / oven heating 250℃*10min" is the burst strength of the grease-resistant paper after heating in a toaster oven at a high temperature of 250℃ for 10 minutes, and "Burst strength / oven heating 250℃*20min" is the burst strength of the grease-resistant paper after heating in a toaster oven at a high temperature of 250℃ for 20 minutes.

[0048] The bursting strength was measured according to JIS-P8131 (2009) Bursting Strength Test Method for Paper and Paperboard Using a Mullen High Pressure Tester. The bursting index is specified in JIS-P8131 (2009). The bursting index is the bursting strength of the greaseproof paper measured according to JIS-P8131 (2009) expressed in megapascals (MPa) divided by the mass.

[0049] <Smoke rating> The smoke evaluation was based on the results of the smoke generation test for each greaseproof paper, as shown in Figures 4(a) and (b), using the following procedure. [Smoke generation (evaluation) test] 1) Equipment used · Oven toaster (heating tester: Zojirushi Corporation ET-GN30) Digital camera ·L-shaped bracket Stopwatch 2) Smoke identification markings A metal L-shaped metal fitting 41 is prepared, and a line in a specified color (e.g., red) is drawn with a magic marker on at least one surface of L-shaped metal fitting 41 to identify the presence or absence and the degree of smoke generation from the greaseproof paper, to serve as smoke generation identification mark 42. This L-shaped metal fitting 41 is set behind and in front of observation window 40a of toaster oven 40. 3) Test piece A greaseproof paper test piece 101 measuring 100×100 mm is dried in a toaster oven 40 at 50° C. for 1 hour and used for a smoke generation evaluation test. Two test pieces 101 are prepared. In addition, the surface irradiated with UV rays (front surface 11 or back surface 12) is placed facing heaters (heating parts) 44, 45 of the toaster oven 40 and heated. 4) Test procedure (1) Toaster oven 40 is set to 250° C. and left for 10 minutes as a conditioning treatment (preheating treatment) before use. (2) Open the observation window 40a, and lay one of the two test pieces horizontally at a position halfway between the upper and lower heaters 44, 45. Place the UV-irradiated test piece 101 between the observation window 40a and the smoke generation identification sign 42 with the surface 111 facing up. (3) After closing the observation window 40a, the test piece 101 and the smoke identification mark 42 are observed from outside the observation window 40a while continuing to heat the toaster oven, and the time until the color of the mark (designated color) can no longer be identified due to smoke from the test piece 101 is measured. The measured time at that time is regarded as the smoke generation time of the surface of that test piece 101, and the second test piece 101 is similarly measured, and the average value is regarded as the smoke generation time of the surface 111. (4) Such measurements were performed in both cases where only the back surface 112 was irradiated with UV light and where both the front and back surfaces 111 and 112 were irradiated with UV light.

[0050] <Example 1> The surface of the paper is coated with a fluorine-based oil-resistant agent, and the back side is made of grease-resistant paper with a fluorine-based oil-resistant agent added to it.

[0051] <Example 2> Grease-resistant paper coated with a fluorine-based oil-resistant agent on both the front and back sides was used.

[0052] <Example 3> The front surface is coated with a fluorine-based oil-resistant agent, and the back surface is covered with a coating layer made of a synthetic resin such as polyethylene or polypropylene.

[0053] <Comparative Example 1> The same greaseproof paper as in Example 1 was used, but not exposed to UV light.

[0054] <Comparative Example 2> The same greaseproof paper as in Example 2 was used, but not exposed to UV light.

[0055] <Comparative Example 3> The same greaseproof paper as in Example 3 was used, but not exposed to UV light.

[0056] <Comparative Example 4> The paper used is waterproof and has an oil-resistant coating on both sides and no additives.

[0057] <Measurement results> As shown in Table 1, the greaseproof paper 1 of Examples 1 and 2 and the greaseproof paper of Comparative Examples 1 and 2 have an oil repellency of Grade 9 or higher, and thus have relatively high oil repellency. In addition, the smoke evaluation of Comparative Example 1 was 780 seconds, whereas in Example 1, the smoke evaluation was 1098 seconds when only the front side was irradiated with UV, 1014 seconds when only the back side was irradiated with UV, and 1100 seconds when both the front and back sides were irradiated with UV, meaning that after UV irradiation, the smoke evaluation was 1000 seconds or more in all cases, which was 200 seconds or more longer before smoke was generated compared to Comparative Example 1, i.e., when no UV irradiation was performed.

[0058] Moreover, the smoke evaluation for Comparative Example 2 was 417 seconds, whereas in Example 2, when only the front side was irradiated with UV, the smoke evaluation was 480 seconds, when only the back side was irradiated with UV, the smoke evaluation was 478 seconds, and when both the front and back sides were irradiated with UV, the smoke evaluation was 482 seconds. In all cases, after UV irradiation, the time until smoke began was 470 seconds or more, which was 30 seconds or more longer than in Comparative Example 2, i.e., when no UV irradiation was performed.

[0059] In addition, the smoke evaluation for Comparative Example 3 was 341 seconds, whereas in Example 3, when only the front surface was irradiated with UV light, the smoke evaluation was 407 seconds, when only the back surface (without oil-resistant agent) was irradiated with UV light, the smoke evaluation was 330 seconds, and when both the front and back surfaces were irradiated with UV light, the smoke evaluation was 400 seconds. In other words, the front and both surfaces irradiated with UV light both took longer than 400 seconds, which was about 60 seconds longer than in Comparative Example 2, i.e., when no UV light was irradiated.

[0060] In addition, in Comparative Example 4, the smoke evaluation was 650 seconds when there was no UV irradiation, and 650 to 660 seconds when UV was irradiated only on the front side, only on the back side, and on both the front and back sides, showing almost no difference in the time until smoke was generated.

[0061] As described above, greaseproof paper has a smoke-suppressing effect when exposed to UV light. Therefore, when the greaseproof paper is used as a paper tray container for food, even if the food is heated to 250°C for 16 minutes or more to the point where it browns, smoke is suppressed inside the toaster oven, the food can be visually observed browning, and the heated food can be removed at the appropriate time.

[0062] Regarding burst strength, in Comparative Example 1, the burst index before heating in a toaster oven was 1.45 MPa, whereas the burst index after heating for 10 minutes at 250°C was 0.16 MPa, and the burst index after heating for 20 minutes at 250°C was 0.1 MPa, and the tensile strength decreased by 90% or more after heating. Meanwhile, in Example 1, the burst index before heating in a toaster oven was 1.48-1.50 MPa, whereas the burst index after heating for 10 minutes at 250°C was 0.33-0.35 MPa, and the burst index after heating for 20 minutes at 250°C was 0.23-0.25 MPa, and the tensile strength decreased by 80% or more after heating.

[0063] In addition, in Examples 2 and 3 and Comparative Examples 2 to 4, when heated at 250° C. for 20 minutes, the initial shape could not be maintained due to thermal decomposition and carbonization, and therefore measurement was impossible.

[0064] Normally, when heat-resistant paper is used as a paper tray container, if the bursting strength after heating is 0.2 MPa or less, when a cook grasps the handle portion 21 of the paper tray container 20 to remove it from the oven range, as shown in Figure 3(a), the paper tray container 20 will be unable to withstand the weight including food and will break, and the paper tray container cannot be used as a container (dishware) for eating.

[0065] As described above, the grease-resistant paper 1 according to the present invention has a bursting index of 0.33 to 0.35 MPa after heating for 10 minutes at 250° C. and a bursting index of 0.23 to 0.25 MPa after heating for 20 minutes at 250° C., and has a bursting index of 0.2 MPa or more even after heating for 20 minutes at 250° C. Therefore, as shown in Fig. 3(b), even after heating for 20 minutes at 250° C., when a cook grasps the gripping portion 21 of the paper tray container 20 to remove it from the oven range, the paper tray container 20 does not deform under its own weight, and can be used as a container (dishware) for eating as is.

[0066] Again, referring to the measurement results of Example 1, the burst strength was almost the same in all patterns, including when only the front surface coated with the oil-resistant agent was irradiated with UV light, when only the back surface containing the oil-resistant agent was irradiated with UV light, and when both the front and back surfaces were irradiated with UV light. Also, the smoke evaluation was almost the same in the cases where only the front surface was irradiated with UV light and where both the front and back surfaces were irradiated with UV light.

[0067] Moreover, from the measurement results of the smoke evaluation of Examples 1 to 3, there was no significant difference in burst strength between the case where only the front surface 11 was irradiated with UV light and the case where only the back surface 12 was irradiated with UV light.

[0068] [Table 2]

[0069] Table 2 shows the results of measuring the burst strength and evaluating the smoke after UV irradiation on both the front and back sides of the grease-resistant paper, which has the same composition as the grease-resistant paper of Example 1, but with different masses. Specifically, the mass before drying of Example 4 was 254.2 g / m 2 , and the mass before drying of Example 5 was 314.2 g / m 2 , and the mass before drying of Example 6 was 404.2 g / m 2 , and the mass before drying of Comparative Example 5 was 214.2 g / m 2 It was.

[0070] As shown in Table 2, in Examples 4 to 6, the smoke evaluation was 1000 seconds or more, and the burst index after heating at 250°C for 20 minutes was 0.2 MPa or more, whereas in Comparative Example 5, the smoke evaluation was 712 seconds, and the burst index after heating at 250°C for 20 minutes was 0.1 MPa. From these results, it can be seen that in order for the UV-irradiated greaseproof paper to exhibit the required burst strength and smoke suppression effect, a mass of 250 g / m2 is required. 2 It is preferable that this is the case. [Explanation of symbols]

[0071] 1 Greaseproof paper 10 Paper base material 11 Surface 12 Back side 40 Toaster oven 40a Viewing window 42 Smoke Identification Markings 101 Test piece

Claims

1. An grease-resistant paper having a first surface and a second surface opposite thereto, and at least 90% by mass of pulp fibers, the paper containing a fluorine-based grease-resistant agent on at least the first surface of the first and second surfaces, The greaseproof paper is characterized in that the smoke generation time in the following smoke generation test at 250°C is at least 16 minutes. [Smoke test] A test piece (100 mm x 100 mm) is placed in an electric oven set to 250°C, and heating is started with the test piece laid horizontally at the midpoint between the upper and lower heaters. After that, the test piece is observed through the observation window of the electric oven, and the time until it is possible to recognize smoke being generated from the test piece with the smoke generation identification mark in the background is measured, and this time is regarded as the smoke generation time.

2. An grease-resistant paper having a first surface and a second surface opposite thereto, and at least 90% by mass of pulp fibers, the paper containing a fluorine-based grease-resistant agent on at least the first surface of the first and second surfaces, The grease-resistant paper, characterized in that the burst strength of the grease-resistant paper after heating at 250°C for 10 minutes is 0.3 MPa or more.

3. 3. The grease-resistant paper according to claim 2, wherein the burst strength of the grease-resistant paper after heating at 250° C. for 20 minutes is 0.2 MPa or more.

4. The grease-resistant paper is the grease-resistant paper according to any one of claims 1 to 3, wherein at least the first surface of the first and second surfaces is irradiated with ultraviolet light UV-A by an ultraviolet lamp under the following irradiation conditions. [Ultraviolet lamp irradiation conditions] (1) Wavelength range: 315 to 400 μm (2) Ultraviolet light intensity: 120 mW / cm 2 (3) Irradiation: 120 mW / sec / cm 2 (4) Irradiation time: 1 second

5. The grease-resistant paper according to any one of claims 1 to 4, wherein the amount of the grease-resistant agent contained on the first surface side is greater than the amount of the grease-resistant agent contained on the second surface side.

6. The grease-resistant paper according to any one of claims 1 to 5, wherein the fiber density on the first surface side is higher than the fiber density on the second surface side.

7. The grease-resistant paper according to any one of claims 1 to 6, wherein the pulp fibers contain pulp fibers derived from coniferous trees and pulp fibers derived from broad-leaved trees, and the content of the pulp fibers derived from the coniferous trees is higher than the content of the pulp fibers derived from the broad-leaved trees.

8. Mass is 250 to 400 g / m 2 The greaseproof paper according to any one of claims 1 to 7, having a thickness of 0.2 to 0.5 mm.

9. The grease-resistant paper according to claim 1 or 4, wherein the difference in smoke generation time between when the first surface is irradiated with ultraviolet light UV-A and when the second surface is irradiated with ultraviolet light UV-A is within 90 seconds.

10. A method for reducing the level of smoke generated when greaseproof paper is heated, comprising: The method is characterized in that at least one of the two surfaces of the grease-resistant paper contains a fluorine-based grease-resistant agent, and at least the one surface of the heat-resistant paper is irradiated with ultraviolet light via an ultraviolet lamp for a required period of time.

11. A method for suppressing a decrease in burst strength of greaseproof paper when heated, comprising: A method comprising coating at least one of the two surfaces of the grease-resistant paper with a fluorine-based grease-resistant agent, and irradiating at least the one surface of the heat-resistant paper with ultraviolet light via an ultraviolet lamp for a required period of time.

12. A paper container for heating, using the grease-resistant paper according to any one of claims 1 to 11.

Citation Information

Patent Citations

  • Oil-resistant paper

    JP2020128616A