Styrenic resin extrusion foam and method for producing the same

A styrenic resin foam composition with styrene-(meth)acrylic acid copolymer, hydro(chloro)fluoroolefins, and alkyl chlorides addresses the insufficiencies of existing foams, achieving superior heat insulation and resistance for building and refrigerated vehicle insulation.

JP2024142607APending Publication Date: 2024-10-11KANEKA CORP
View PDF 4 Cites 0 Cited by

Patent Information

Application Number
JP2023054816
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Filing Date
2023-03-30
Publication Date
2024-10-11

AI Technical Summary

Technical Problem

Existing styrenic resin foams lack sufficient heat insulation properties and heat resistance, despite the use of additives like graphite and hydrofluoroolefins, with hydrochlorofluoroolefins posing challenges in achieving both properties simultaneously.

Method used

A styrenic resin foam composition comprising a styrene-(meth)acrylic acid copolymer, hydro(chloro)fluoroolefins, and alkyl chlorides, with specific ratios and additives to enhance heat insulation and resistance, including flame retardants and stabilizers for improved performance.

Benefits of technology

The solution results in a styrenic resin foam with excellent heat insulation and heat resistance, maintaining thickness and appearance, suitable for building insulation and refrigerated vehicle applications.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024142607000001
    Figure 2024142607000001
Patent Text Reader

Abstract

To provide a styrenic resin extrusion foam which achieves both excellent heat insulation and heat resistance.SOLUTION: A styrenic resin extrusion foam contains a styrenic resin and a foaming agent, where 20 to 80 wt.% of a styrene-(meth)acrylic acid-based copolymer is contained in 100 wt.% of the styrenic resin, and hydro(chloro)fluoroolefin is contained as a foaming agent.SELECTED DRAWING: None
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to an extruded styrene-based resin foam and a method for producing the same. [Background technology]

[0002] Extruded styrene resin foams are generally produced continuously by heating and melting a styrene resin composition using an extruder or the like, then adding a blowing agent under high pressure conditions, cooling to a predetermined resin temperature, and then extruding the resulting mixture into a low pressure region.

[0003] Due to their excellent workability and heat insulating properties, styrene-based resin extruded foams are used, for example, as heat insulating materials for structures. In recent years, there has been an increasing demand for energy saving in houses and buildings, and there is a demand for technological development of foams with higher heat insulating properties than conventional ones.

[0004] As a method for producing a highly heat-insulating foam, there have been proposed a production method in which graphite or titanium oxide is added in a predetermined range as a heat radiation suppressant (see, for example, Patent Document 1), and a production method for an extruded styrene resin foam that uses, as a foaming agent, environmentally friendly fluorinated olefins (hydrofluoroolefins and hydrochlorofluoroolefins) that have an ozone depletion potential of zero and a small global warming potential, or alkyl chlorides such as methyl chloride and ethyl chloride (see, for example, Patent Documents 2 to 4). [Prior art documents] [Patent documents]

[0005] [Patent Document 1] JP 2013-221110 A [Patent Document 2] Special Publication No. 2008-546892 [Patent Document 3] JP 2019-189811 A [Patent Document 4] JP 2019-108416 A Summary of the Invention [Problem to be solved by the invention]

[0006] However, in the styrene-based resin extrusion foam described in the above patent document, the heat radiation suppressant such as graphite and the blowing agent such as hydrofluoroolefin can impart excellent heat insulation to the foam, but it is not sufficient.On the other hand, hydrochlorofluoroolefin, which can impart further heat insulation, has a problem that it is difficult to have sufficient heat resistance.

[0007] SUMMARY OF THE PRESENT EMBODIMENTS Accordingly, an object of the present invention is to provide an extruded styrene resin foam having excellent heat insulation and heat resistance. [Means for solving the problem]

[0008] In order to solve the above problems, the present inventors have conducted extensive research and have found that a combination of a specific styrene-based resin and a specific foaming agent can achieve both excellent heat insulation and excellent heat resistance, which could not be achieved by conventional techniques, and have thus completed the present invention. The present invention includes the following aspects. That is, the present invention provides [1] A styrene-based resin extruded foam comprising a styrene-based resin and a foaming agent, The styrene-based resin includes a styrene-(meth)acrylic acid-based copolymer, The content of the styrene-(meth)acrylic acid copolymer in 100% by weight of the styrene resin is 20 to 80% by weight, The foaming agent contains 5.0 to 10.0 parts by weight of a hydro(chloro)fluoroolefin relative to 100 parts by weight of the styrene-based resin, A styrene-based resin extruded foam having a thermal conductivity of 0.021 W / mK or less; [2] The extruded styrene-based resin foam according to [1], wherein the content of the (meth)acrylic acid-derived constitutional units is 5 to 20% by weight based on 100% by weight of all constitutional units of the styrene-(meth)acrylic acid-based copolymer. [3] The extruded styrene-based resin foam according to any one of [1] to [2], further comprising an alkyl chloride, the content of which is 3.0 to 6.0 parts by weight per 100 parts by weight of the total styrene-based resin in the extruded styrene-based resin foam. [4] The extruded styrene-based resin foam according to any one of [1] to [3], wherein the extruded styrene-based resin foam contains 1.0 part by weight or more and 5.0 parts by weight or less of graphite per 100 parts by weight of the styrene-based resin. [5] The extruded styrene-based resin foam according to any one of [1] to [4], characterized in that the dimensional change rate of the extruded styrene-based resin foam when heated in an 80°C atmosphere for 24 hours is within 5%. [6] The apparent density of the styrene-based resin extruded foam is 20 to 60 kg / m 3 The extruded styrene-based resin foam according to any one of [1] to [5], [7] The extruded styrene resin foam according to any one of [1] to [6], wherein the extruded styrene resin foam has a thickness of 10 mm or more and 150 mm or less. Effect of the Invention

[0009] According to the present invention, a styrene-based resin foam that can achieve both excellent heat insulation and heat resistance can be obtained. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0010] An embodiment of the present invention will be described below, but the present invention is not limited thereto. The present invention is not limited to each configuration described below, and various modifications are possible within the scope of the claims. The technical scope of the present invention also includes embodiments and examples obtained by appropriately combining the technical means disclosed in different embodiments and examples. In addition, all academic literature and patent documents described in this specification are incorporated herein by reference. In addition, unless otherwise specified in this specification, "A to B" representing a numerical range means "A or more and B or less."

[0011] Styrene-(meth)acrylic acid copolymers are generally used for the purpose of imparting heat resistance and chemical resistance because they are superior to polystyrene in heat resistance and chemical resistance, but since they have properties similar to polystyrene as a base, it is difficult to imagine that they are particularly excellent in improving thickness buildability. When hydro(chloro)fluoroolefin is used as a blowing agent for polystyrene resin, the bubbles of the styrene resin extrusion foam tend to become finer, and the thickness buildability of the styrene resin extrusion foam tends to be impaired. However, by using at least two types of styrene resin, one of which contains a styrene-(meth)acrylic acid copolymer, and a blowing agent containing a hydro(chloro)fluoroolefin and an alkyl chloride, it is possible to achieve excellent heat insulation and excellent thickness buildability. Note that "(meth)acrylic" means "methacrylic and / or acrylic".

[0012] An embodiment of the present invention will be described below. [1. Extruded styrene resin foam] The styrene-based resin extruded foam according to one embodiment of the present invention is characterized in that the styrene-based resin contains a specific amount of a styrene-(meth)acrylic acid copolymer, and contains a hydro(chloro)fluoroolefin and an alkyl chloride as a foaming agent.

[0013] (1-1. Styrene-based resin) The styrene-based resin extruded foam according to one embodiment of the present invention contains a styrene-based resin, which is composed of a blend of at least two types of styrene-based resin, one of which is a styrene-(meth)acrylic acid-based copolymer. That is, the styrene-based resin contains (i) a styrene-(meth)acrylic acid-based copolymer and (ii) a styrene-based polymer other than (i) (hereinafter referred to as "other styrene-based polymer"). Here, examples of (ii) other styrene-based polymers include homopolymers of styrene-based monomers (polystyrene), copolymers of two or more types of styrene-based monomers, or copolymers of styrene-based monomers and other monomers.

[0014] Examples of styrene monomers constituting (i) styrene-(meth)acrylic acid copolymers and (ii) other styrene polymers include styrene, methylstyrene, dimethylstyrene, ethylstyrene, diethylstyrene, isopropylstyrene, bromostyrene, dibromostyrene, tribromostyrene, chlorostyrene, dichlorostyrene, vinyltoluene, and vinylxylene.

[0015] Examples of monomers other than styrene monomers and (meth)acrylic acid include polyfunctional vinyl compounds such as divinylbenzene; (meth)acrylic acid ester compounds such as methyl acrylate, methyl methacrylate, ethyl acrylate, ethyl methacrylate, butyl acrylate, and butyl methacrylate; acrylonitrile; diene compounds such as butadiene; unsaturated carboxylic acid anhydrides such as maleic anhydride and itaconic anhydride; and N-alkyl-substituted maleimide compounds such as N-methylmaleimide, N-butylmaleimide, N-cyclohexylmaleimide, N-phenylmaleimide, N-(2)-chlorophenylmaleimide, N-(4)-bromophenylmaleimide, and N-(1)-naphthylmaleimide. The (i) styrene-(meth)acrylic acid copolymer may also contain the other monomers as a constituent unit.

[0016] The amount of the styrene monomer contained in the other styrene polymer is preferably 80 to 100% by weight, and more preferably 90 to 100% by weight, based on 100% by weight of the constituent units of the other styrene polymer.

[0017] Each of (i) the styrene-(meth)acrylic acid copolymer and (ii) the other styrene polymer may be one type, or two or more types of polymers may be combined.

[0018] For the purpose of adjusting the MFR, melt viscosity during molding, melt tension, etc. of the styrene-based resin used in one embodiment of the present invention, (i) the styrene-(meth)acrylic acid-based copolymer and / or (ii) other styrene-based polymer may have a branched structure. These may be used alone, or two or more types different in copolymerization components, molecular weights, molecular weight distributions, branched structures, and / or MFRs may be mixed and used.

[0019] In one embodiment of the present invention, the content of (i) styrene-(meth)acrylic acid copolymer is 10% by weight or more and 80% by weight or less in 100% by weight of styrene-based resin. From the viewpoint of easily improving the heat resistance of the extruded styrene-based resin foam, it is preferably 22% by weight or more and 78% by weight or less, more preferably 25% by weight or more and 75% by weight or less, even more preferably 30% by weight or more and 70% by weight or less, particularly preferably 35% by weight or more and 65% by weight or less, more particularly preferably 40% by weight or more and 60% by weight or less, and most preferably 45% by weight or more and 55% by weight or less.

[0020] In one embodiment of the present invention, the (meth)acrylic acid-derived structural unit contained in the (i) styrene-(meth)acrylic acid-based copolymer is preferably 5 to 20% by weight, more preferably 5 to 17% by weight, and even more preferably 5 to 15% by weight, based on 100% by weight of the (i) styrene-(meth)acrylic acid-based copolymer. If the (meth)acrylic acid component contained in the (i) styrene-(meth)acrylic acid-based copolymer is less than 5% by weight, the (meth)acrylic acid component is too small, so that the effect of thickening may be difficult to achieve. On the other hand, if the (meth)acrylic acid component is more than 20% by weight, the (meth)acrylic acid component is too large, so that the elongation during foaming is poor, and foaming may be inhibited. The styrene-based monomer-derived structural unit contained in the styrene-(meth)acrylic acid-based copolymer is preferably 80 to 95% by weight, and more preferably 85 to 95% by weight, based on 100% by weight of the styrene-(meth)acrylic acid-based copolymer.

[0021] In one embodiment of the present invention, the MFR of the styrene resin is preferably 0.1 to 50 g / 10 min, because (i) it is excellent in molding processability during extrusion foaming, (ii) it is easy to adjust the discharge amount during molding, the thickness, width, apparent density, and closed cell ratio of the obtained styrene resin extruded foam to desired values, (iii) it is excellent in foamability (the thickness, width, apparent density, closed cell ratio, and surface properties of the foam are easily adjusted to desired conditions), (iv) it is possible to obtain an extruded styrene resin foam with excellent appearance, and (v) it is possible to obtain an extruded styrene resin foam with a good balance of properties (for example, mechanical strength such as compressive strength, bending strength, or bending deflection amount, toughness, etc.). Furthermore, the MFR of the styrene resin is more preferably 0.3 to 30 g / 10 min, and particularly preferably 0.5 to 25 g / 10 min, from the viewpoint of the balance between molding processability and foamability, and mechanical strength and toughness. In one embodiment of the present invention, the MFR is measured according to JIS K7210-1 (2014) Method A and test condition H (test temperature 200° C., load 5 kg).

[0022] Resins other than the styrene resin may be contained within a range that does not impair the effects of the present invention. Examples of the other resins include polyethylene resin, polypropylene resin, polyolefin resin, polyethylene terephthalate, etc. The content of the other resin is preferably 20 parts by weight or less, more preferably 10 parts by weight or less, and even more preferably 5 parts by weight or less, relative to 100 parts by weight of the styrene resin.

[0023] (1-2. Foaming Agent) The extruded styrene-based resin foam in one embodiment of the present invention contains hydro(chloro)fluoroolefin as a foaming agent. This improves the heat insulating properties of the extruded styrene-based resin foam. Note that "hydro(chloro)fluoroolefin" means "hydrofluoroolefin and / or hydrochlorofluoroolefin".

[0024] The hydrofluoroolefin used in one embodiment of the present invention is not particularly limited, but tetrafluoropropene and hexafluorobutene are preferred from the viewpoint of low gas thermal conductivity and safety.Specific examples include trans-1,3,3,3-tetrafluoropropene (trans-HFO-1234ze), cis-1,3,3,3-tetrafluoropropene (cis-HFO-1234ze), 2,3,3,3-tetrafluoropropene (trans-HFO-1234yf), and cis-1,1,1,4,4,4-hexafluoro-2-butene (cis-HFO-1336mzz).The hydrochlorofluoroolefin used in one embodiment of the present invention is not particularly limited, but hydrochlorotrifluoropropene is preferred from the viewpoint of low gas thermal conductivity and safety. Specifically, trans-1-chloro-3,3,3-trifluoropropene (trans-HCFO-1233zd), trans-1-chloro-2,3,3,3-trifluoropropene (trans-HCFO-1224yd), 2-chloro-3,3,3-trifluoropropene (HCFO-1233xf), dichlorotrifluoropropene (HCFO1223), 1-chloro-2,3,3-trifluoropropene (HCFO-1233 yd), 1-chloro-1,3,3-trifluoropropene (HCFO-1233zb), 2-chloro-1,3,3-trifluoropropene (HCFO-1233xe), 2-chloro-2,2,3-trifluoropropene (HCFO-1233xc), 3-chloro-1,2,3-trifluoropropene (HCFO-1233ye), 3-chloro-1,1,2-trifluoropropene (HCFO-1233yc), etc. These hydrofluoroolefins and hydrochlorofluoroolefins may be used alone or in combination of two or more.

[0025] As one embodiment of the present invention, from the viewpoint of the thermal insulation properties of the extruded styrene-based resin foam, hydrochlorofluoroolefin is preferred, and its content is preferably 5.0 to 10.0 parts by weight, more preferably 6.0 to 10.0 parts by weight, and even more preferably 7.0 to 8.0 parts by weight, per 100 parts by weight of the total styrene-based resin in the extruded styrene-based resin foam.

[0026] When the content of hydro(chloro)fluoroolefin is less than 5.0 parts by weight, the effect of improving the heat insulation by hydro(chloro)fluoroolefin tends not to be expected. On the other hand, when the content of hydro(chloro)fluoroolefin is more than 10.0 parts by weight, the hydro(chloro)fluoroolefin separates from the resin melt during extrusion foaming, and spot holes (traces where localized lumps of hydro(chloro)fluoroolefin break through the surface of the extruded foam and are released into the outside air) are generated on the surface of the extruded foam, or the closed cell ratio is reduced, which may impair the heat insulation.

[0027] The alkyl chloride used in one embodiment of the present invention is preferably an alkyl chloride having 1 to 3 carbon atoms, such as ethyl chloride or methyl chloride. One type may be used, or two or more types may be used in combination.

[0028] In one embodiment of the present invention, the content of the alkyl chloride is preferably 3.0 to 6.0 parts by weight, more preferably 3.5 to 5.5 parts by weight, based on 100 parts by weight of the total styrene resin in the extruded styrene resin foam. If the content exceeds 6.0 parts by weight, the alkyl chloride significantly plasticizes the styrene resin, and the heat resistance of the obtained extruded styrene resin foam may deteriorate.

[0029] Other blowing agents include saturated hydrocarbons having 3 to 5 carbon atoms, such as propane, n-butane, i-butane, n-pentane, i-pentane, and neopentane; ethers such as dimethyl ether, diethyl ether, methyl ethyl ether, isopropyl ether, n-butyl ether, diisopropyl ether, furan, furfural, 2-methylfuran, tetrahydrofuran, and tetrahydropyran; dimethyl ketone, methyl ethyl ketone, diethyl ketone, methyl-n-propyl ketone, methyl-n-butyl ketone, methyl-i-butyl ketone, and methyl Examples of organic blowing agents include ketones such as ethyl-n-amyl ketone, methyl-n-hexyl ketone, ethyl-n-propyl ketone, and ethyl-n-butyl ketone; saturated alcohols having 1 to 4 carbon atoms such as methanol, ethanol, propyl alcohol, i-propyl alcohol, butyl alcohol, i-butyl alcohol, and t-butyl alcohol; and carboxylates such as methyl formate, ethyl formate, propyl formate, butyl formate, amyl formate, methyl propionate, and ethyl propionate. Inorganic blowing agents such as water and carbon dioxide can also be used. These other blowing agents may be used alone or in combination of two or more.

[0030] In one embodiment of the present invention, the content of the other foaming agent is preferably 1.0 to 3.0 parts by weight, and more preferably 1.5 to 2.5 parts by weight, based on 100 parts by weight of the total styrene-based resin in the extruded styrene-based resin foam.

[0031] Among the other blowing agents, from the viewpoints of foaming property and foam moldability, etc., saturated hydrocarbons having 3 to 5 carbon atoms, saturated alcohols having 1 to 4 carbon atoms, dimethyl ether, diethyl ether, methyl ethyl ether, etc. are preferred. From the viewpoints of the combustibility of the blowing agent, the flame retardancy or heat insulating property of the foam, etc., carbon dioxide is preferred. Among these, dimethyl ether is particularly preferred from the viewpoint of the plasticizing effect.

[0032] (1-3. Flame retardants) In one embodiment of the present invention, a flame retardant is added to the extruded styrene-based resin foam, thereby imparting flame retardancy to the resulting extruded styrene-based resin foam.

[0033] As the flame retardant, a bromine-based flame retardant is preferably used. Specific examples of the bromine-based flame retardant in one embodiment of the present invention include hexabromocyclododecane, tetrabromobisphenol A-bis(2,3-dibromo-2-methylpropyl)ether, tetrabromobisphenol A-bis(2,3-dibromopropyl)ether, tris(2,3-dibromopropyl)isocyanurate, and aliphatic bromine-containing polymers such as brominated styrene-butadiene block copolymers. These may be used alone or in combination of two or more.

[0034] Among these, tetrabromobisphenol A-bis(2,3-dibromo-2-methylpropyl)ether, mixed brominated flame retardants consisting of tetrabromobisphenol A-bis(2,3-dibromopropyl)ether, brominated styrene-butadiene block copolymer, and hexabromocyclododecane are preferably used because they have good extrusion operation and do not adversely affect the heat resistance of the foam, etc. These substances may be used alone or as a mixture.

[0035] The content of the bromine-based flame retardant in the styrene-based resin extruded foam in one embodiment of the present invention is preferably 1.0 to 8.0 parts by weight, more preferably 1.5 to 7.0 parts by weight, and even more preferably 2.0 to 6.0 parts by weight, based on 100 parts by weight of the styrene-based resin. If the content of the bromine-based flame retardant is less than 1.0 part by weight, it is difficult to obtain good properties as a foam such as flame retardancy, while if it exceeds 8.0 parts by weight, the stability and surface properties during foam production may be impaired. However, it is more preferable that the content of the flame retardant is appropriately adjusted according to the amount of foaming agent added, the apparent density of the foam, and the type or content of additives having a flame retardant synergistic effect, so that the flame retardancy specified in JIS A 9521 Measurement Method A is obtained.

[0036] In one embodiment of the present invention, a radical generator can be used in combination with the styrene-based resin extrusion foam in order to improve the flame retardancy. Specific examples of the radical generator include 2,3-dimethyl-2,3-diphenylbutane, poly-1,4-diisopropylbenzene, 2,3-diethyl-2,3-diphenylbutane, 3,4-dimethyl-3,4-diphenylhexane, 3,4-diethyl-3,4-diphenylhexane, 2,4-diphenyl-4-methyl-1-pentene, and 2,4-diphenyl-4-ethyl-1-pentene. Peroxides such as dicumyl peroxide are also used. Among them, those stable under the resin processing temperature conditions are preferred, specifically 2,3-dimethyl-2,3-diphenylbutane and poly-1,4-diisopropylbenzene are preferred, and the preferred amount of the radical generator to be added is 0.05 to 0.5 parts by weight relative to 100 parts by weight of the styrene-based resin.

[0037] Furthermore, for the purpose of improving flame retardancy, in other words as a flame retardant auxiliary, phosphorus-based flame retardants such as phosphate esters and phosphine oxides can be used in combination within a range that does not impair thermal stability. Examples of phosphate esters include triphenyl phosphate, tris(tributylbromoneopentyl)phosphate, tricresyl phosphate, trixylyleneyl phosphate, cresyl diphenyl phosphate, 2-ethylhexyl diphenyl phosphate, trimethyl phosphate, triethyl phosphate, tributyl phosphate, tris(2-ethylhexyl)phosphate, tris(butoxyethyl)phosphate, and condensed phosphate esters, and triphenyl phosphate and tris(tributylbromoneopentyl)phosphate are particularly preferred. In addition, triphenylphosphine oxide is preferred as a phosphine oxide-type phosphorus-based flame retardant. These phosphate esters and phosphine oxides may be used alone or in combination of two or more. The preferred amount of the phosphorus-based flame retardant to be added is 0.1 to 2 parts by weight based on 100 parts by weight of the styrene-based resin.

[0038] (1-4. Stabilizers) In one embodiment of the present invention, a stabilizer for a flame retardant can be used. Specific examples of the stabilizer include, but are not limited to, (i) epoxy compounds such as bisphenol A diglycidyl ether type epoxy resin, cresol novolac type epoxy resin, and phenol novolac type epoxy resin, (ii) polyhydric alcohol esters, which are reaction products of polyhydric alcohols such as pentaerythritol, dipentaerythritol, and tripentaerythritol with monovalent carboxylic acids such as acetic acid and propionic acid, or divalent carboxylic acids such as adipic acid and glutamic acid, and which are mixtures of esters having one or more hydroxyl groups in the molecule and may contain a small amount of the raw material polyhydric alcohol, and (iii) triethylene glycol-bis-3-(3-tert-butyl-4-hydroxy-5-methylphenyl)propionate, pentaerythritol tetrakis[3-( (iv) phosphite-based stabilizers such as 3,9-bis(2,4-di-tert-butylphenoxy)-2,4,8,10-tetraoxa-3,9-diphosphaspiro[5.5]undecane, 3,9-bis(2,6-di-tert-butyl-4-methylphenoxy)-2,4,8,10-tetraoxa-3,9-diphosphaspiro[5.5]undecane, and tetrakis(2,4-di-tert-butyl-5-methylphenyl)-4,4'-biphenylene diphosphonite), and the like are preferably used since they do not deteriorate the flame retardant performance of the foam and improve the thermal stability of the foam. These stabilizers may be used alone or in combination of two or more kinds. The preferred amount of stabilizer to be added is 0.1 to 2 parts by weight based on 100 parts by weight of the styrene-based resin.

[0039] (1-5. Heat radiation suppressants) A heat radiation inhibitor may be added to the extruded styrene-based resin foam according to one embodiment of the present invention in order to improve heat insulation. In one embodiment of the present invention, graphite or carbon black can be used as the heat radiation inhibitor. Examples of graphite include scaly (flake) graphite, clayey graphite, spherical graphite, and artificial graphite. Among these, it is preferable to use graphite whose main component is scaly (flake) graphite because of its high heat radiation inhibitory effect. Graphite with a fixed carbon content of 80% or more is preferable, and graphite with a fixed carbon content of 85% or more is more preferable. By setting the fixed carbon content within the above range, a foam having high heat insulation properties can be obtained.

[0040] The average particle size of the graphite is preferably 15 μm or less, more preferably 10 μm or less. By setting the average particle size within the above range, the specific surface area of ​​the graphite increases, and the probability of collision with heat radiation increases, thereby enhancing the heat radiation suppression effect. The average particle size means the particle size at which the cumulative volume of the total particle volume is 50% (volume average particle size by laser diffraction scattering method) when the particle size distribution is measured and analyzed by a laser diffraction scattering method based on the Mie theory in accordance with ISO13320:2009 and JIS Z8825:2013.

[0041] In one embodiment of the present invention, the graphite content is preferably 0.5 parts by weight or more and 5.0 parts by weight or less, and more preferably 1.0 parts by weight or more and 3.0 parts by weight or less, relative to 100 parts by weight of the styrene-based resin. If the content is less than 0.5 parts by weight, a sufficient heat radiation suppression effect cannot be obtained. If the content is more than 5.0 parts by weight, the heat radiation suppression effect corresponding to the content cannot be obtained, and there is no cost advantage.

[0042] The heat radiation inhibitor refers to a substance having the properties of reflecting, scattering, and absorbing light in the near infrared or infrared region. By containing a heat radiation inhibitor, a foam having high heat insulation properties can be obtained. As the heat radiation inhibitor that can be used in the present invention, in addition to graphite, white particles such as titanium oxide, barium sulfate, zinc oxide, aluminum oxide, and antimony oxide can be used. These may be used alone or in combination of two or more. Among the white particles, titanium oxide or barium sulfate is preferred from the viewpoint of a large radiation suppression effect, and titanium oxide is more preferred. The average particle size of the white particles is not particularly limited, but in consideration of effectively reflecting infrared rays and coloring to resin, for example, titanium oxide is preferably 0.1 μm to 10 μm, and more preferably 0.15 μm to 5 μm.

[0043] The content of the white particles in one embodiment of the present invention is preferably 1.0 parts by weight or more and 3.0 parts by weight or less, more preferably 1.5 parts by weight or more and 2.5 parts by weight or less, based on 100 parts by weight of the styrene resin. The white particles have a smaller heat radiation suppression effect than graphite, and when the content of the white particles is less than 1.0 part by weight, the white particles hardly have a heat radiation suppression effect even if they are contained. When the content of the white particles is more than 3.0 parts by weight, the heat radiation suppression effect corresponding to the content cannot be obtained, while the flame retardancy of the foam tends to deteriorate.

[0044] The total content of the heat radiation inhibitor in one embodiment of the present invention is preferably 1.0 parts by weight or more and 6.0 parts by weight or less, more preferably 2.0 parts by weight or more and 5.0 parts by weight or less, based on 100 parts by weight of the styrene-based resin. When the total content of the heat radiation inhibitor is less than 1.0 part by weight, it is difficult to obtain heat insulation, while the content of the solid additive such as the heat radiation inhibitor increases, so that the number of nucleation points increases, so that the bubbles of the foam become finer, and the elongation of the resin itself deteriorates, which tends to make it difficult to impart a beautiful surface to the extruded foam and to make the extruded foam thicker. However, when the total content of the heat radiation inhibitor exceeds 6.0 parts by weight, it tends to be particularly poor in imparting a beautiful surface to the extruded foam and making the extruded foam thicker, and further, the extrusion stability tends to be impaired, and the flame retardancy tends to be impaired.

[0045] (1-6. Other additives) In one embodiment of the present invention, further, as necessary, additives such as inorganic compounds such as silica, calcium silicate, wollastonite, kaolin, clay, mica, calcium carbonate, sodium stearate, calcium stearate, magnesium stearate, barium stearate, liquid paraffin, olefin wax, stearylamide compounds, phenol antioxidants, phosphorus stabilizers, nitrogen stabilizers, sulfur stabilizers, light resistance stabilizers such as benzotriazoles and hindered amines, cell size regulators such as talc, flame retardants other than the above, antistatic agents, colorants such as pigments, and plasticizers may be contained in the styrene resin, as long as the effects of one embodiment of the present invention are not impaired. In addition, as necessary, other resins (e.g., thermoplastic resins such as polyphenylene ether resins), elastomers, and rubber components (e.g., diene rubber-reinforced polystyrene, acrylic rubber-reinforced polystyrene, etc.) may be used in combination with the styrene resin, as long as the effects of one embodiment of the present invention are not impaired. The amount of the other additives added is preferably 0 to 2 parts by weight based on 100 parts by weight of the styrene-based resin.

[0046] (1-7. Physical Properties) The thermal conductivity of the styrene-based resin extruded foam according to one embodiment of the present invention is not particularly limited, but from the viewpoint of thermal insulation considering that the foam functions, for example, as a thermal insulation material for building, or as a thermal insulation material for refrigerators or refrigerated vehicles, the thermal conductivity measured at an average temperature of 23°C one week after production is preferably 0.0244 W / mK or less, more preferably 0.0224 W / mK or less, and particularly preferably 0.0204 W / mK or less.

[0047] The apparent density of the extruded styrene-based resin foam according to one embodiment of the present invention is, for example, 20 kg / m from the viewpoint of heat insulation and light weight in consideration of its function as a heat insulating material for buildings, or a heat insulating material for refrigerators or refrigerated vehicles. 3 More than 60kg / m 3 It is preferably equal to or less than 25 kg / m 3 More than 40kg / m 3 The following is the result.

[0048] The closed cell ratio of the extruded styrene-based resin foam according to one embodiment of the present invention is preferably 90% or more, more preferably 95% or more. If the closed cell ratio is less than 90%, the foaming agent will dissipate from the extruded foam early, resulting in a decrease in heat insulation.

[0049] The average bubble diameter in the thickness direction of the styrene-based resin extruded foam according to one embodiment of the present invention is preferably 0.05 mm or more and 0.5 mm or less, more preferably 0.05 mm or more and 0.4 mm or less, and particularly preferably 0.05 mm or more and 0.3 mm or less. In general, the smaller the average bubble diameter, the shorter the distance between the bubble walls of the foam, so that the range of movement of the bubbles of the extruded foam when shaping the extruded foam during extrusion foaming is narrow, making deformation difficult, and it tends to be difficult to impart a beautiful surface to the extruded foam and to produce a thickness of the extruded foam. When the average bubble diameter in the thickness direction of the styrene-based resin extruded foam is smaller than 0.05 mm, it becomes particularly difficult to impart a beautiful surface to the extruded foam and to produce a thickness of the extruded foam. On the other hand, when the average bubble diameter in the thickness direction of the styrene-based resin extruded foam exceeds 0.5 mm, there is a risk that sufficient heat insulation cannot be obtained.

[0050] The average cell diameter of the extruded styrene resin foam according to one embodiment of the present invention can be evaluated as follows using a microscope (DIGITAL MICROSCOPE VHX-900, manufactured by KEYENCE CORPORATION).

[0051] The obtained styrene-based resin extruded foam was observed from the extrusion direction at a widthwise center and at a location 150 mm from one end in the widthwise direction to the opposite end (the same location for both ends in the widthwise direction) at three locations in total at the center in the thickness direction, using the microscope, and a 100x magnified photograph was taken. Similarly, the extrusion direction vertical cross sections at the center in the thickness direction at three locations in the width direction were observed from the width direction using the microscope, and a 100x magnified photograph was taken. Three 2 mm straight lines were drawn arbitrarily in the thickness direction of the magnified photograph (three lines for each observation location and each observation direction), and the number a of bubbles in contact with the straight lines was measured. From the measured number a of bubbles, the average bubble diameter A in the thickness direction for each observation location was calculated by the following formula (1). The average value of the three locations (two directions at each location) was taken as the average bubble diameter A (average value) in the thickness direction of the styrene-based resin extruded foam. Average bubble diameter A (mm) in the thickness direction at each observation point = 2 × 3 / number of bubbles a ···(1).

[0052] The cross sections perpendicular to the extrusion direction of the obtained styrene-based resin extruded foam at the center in the width direction and at a location 150 mm from one end in the width direction to the opposite end (the same location for both ends in the width direction) were observed from the width direction using the microscope, and 100x magnified photographs were taken. Three 2 mm straight lines were drawn in the extrusion direction of the enlarged photograph (three lines for each observation location), and the number b of bubbles in contact with the straight lines was measured. From the measured number b of bubbles, the average bubble diameter B in the extrusion direction for each observation location was calculated using the following formula (2). The average value of the three locations was taken as the average bubble diameter B (average value) in the extrusion direction of the styrene-based resin extruded foam. Average bubble diameter in the extrusion direction at each observation point B (mm) = 2 × 3 / number of bubbles b (2).

[0053] The obtained styrene-based resin extruded foam was observed from the extrusion direction at a total of three locations, namely, the widthwise center and a location 150 mm from one end in the widthwise direction to the opposite end (the same location for both ends in the widthwise direction), in a widthwise vertical cross section, and a 100x magnified photograph was taken. Three 2 mm straight lines were drawn at random in the widthwise direction of the enlarged photograph (three lines for each observation location), and the number c of bubbles in contact with the straight lines was measured. From the measured number c of bubbles, the average cell diameter C in the width direction for each observation location was calculated by the following formula (3). The average value of the three locations was taken as the average cell diameter C (average value) in the width direction of the styrene-based resin extruded foam. Average bubble diameter C (mm) in the width direction at each observation point = 2 × 3 / number of bubbles c (3).

[0054] The cell deformation ratio of the extruded styrene-based resin foam according to one embodiment of the present invention is preferably 0.7 to 2.0, more preferably 0.8 to 1.5, and even more preferably 0.8 to 1.2. If the cell deformation ratio is less than 0.7, the compressive strength is low, and the extruded foam may not have a strength suitable for the intended use. In addition, the cells tend to return to a spherical shape, and the extruded foam tends to have poor dimensional (shape) retention. On the other hand, if the cell deformation ratio exceeds 2.0, the number of cells in the thickness direction of the extruded foam is reduced, and the effect of improving the heat insulation due to the cell shape is reduced.

[0055] The cell deformation ratio of the extruded styrene resin foam according to one embodiment of the present invention can be calculated from the above-mentioned average cell diameter by the following formula (4). Bubble deformation rate (unitless) = A (average value) / {〔B (average value) + C (average value)〕 / 2} (4).

[0056] In one embodiment of the present invention, the thickness of the styrene-based resin extruded foam is, from the viewpoints of thermal insulation, bending strength, and compressive strength in consideration of its function as, for example, a thermal insulation material for building, or a thermal insulation material for refrigerators or refrigerated vehicles, preferably from 10 mm to 150 mm, more preferably from 15 mm to 130 mm, even more preferably from 20 mm to 130 mm, still more preferably from 20 mm to 120 mm, and particularly preferably from 30 mm to 120 mm.

[0057] As described in the examples and comparative examples of the present invention, in the case of an extruded styrene resin foam, after it is shaped by extrusion foaming, both surfaces of a plane perpendicular to the thickness direction may be cut to a depth of about 5 mm on each side in the thickness direction to obtain the product thickness. However, unless otherwise specified, the thickness of the extruded styrene resin foam according to one embodiment of the present invention refers to the uncut thickness after it has been shaped by extrusion foaming.

[0058] Thus, according to one embodiment of the present invention, it is possible to easily obtain an extruded styrene-based resin foam having excellent heat insulation and flame retardancy, a beautiful appearance, and a sufficient thickness suitable for use. From these viewpoints, the extruded styrene-based resin foam of the present invention is particularly useful as a heat insulating material for buildings and a heat insulating material for the body of a refrigerated vehicle.

[0059] The dimensional change rate of the styrene-based resin extruded foam according to one embodiment of the present invention is calculated from the volume change rate from the dimensional change when heated in an atmosphere at 80° C. for 24 hours in each of the thickness direction, width direction, and length direction, and is within 5%, more preferably within 3%. If the dimensional change rate at 80° C. is within the above range, the dimensional change is small, so that even if the styrene-based resin extruded foam is placed flat under the sunlight in summer, the dimensions are unlikely to change and the workability is excellent. The above-mentioned heating dimensional change rate means that the volume change rate is calculated from the dimensional change rate due to shrinkage and expansion caused by heating. Specifically, the dimensional change rate within 5% means that it is -5% or more and +5% or less.

[0060] 2. Method for producing extruded styrene resin foam The components already explained in [1. Extruded styrene resin foam] are used by reference, and the explanation thereof will be omitted here.

[0061] As one embodiment of the method for producing the extruded styrene resin foam of the present invention, the following method can be mentioned.

[0062] A method for producing an extruded styrene-based resin foam by extruding and foaming an expandable styrene-based resin composition obtained by melt-kneading a styrene-based resin and a foaming agent, the method satisfying the following (a) to (c): (a) the styrene-based resin comprises a styrene-(meth)acrylic acid-based copolymer, (b) the content of the styrene-(meth)acrylic acid copolymer in 100% by weight of the styrene resin is 20 to 80% by weight, (c) The blowing agent comprises a hydro(chloro)fluoroolefin, an alkyl chloride and water.

[0063] By using water in addition to hydro(chloro)fluoroolefin and alkyl chloride as a blowing agent to be added to the styrene-based resin, the thickness buildability of the styrene-based resin can be easily improved, and an extruded styrene-based resin foam that stably achieves both heat insulation and thickness buildability can be produced.

[0064] In one embodiment of the manufacturing method according to the present invention, other foaming agents may be added as the foaming agent, and the other foaming agents described above in [1. Extruded styrene resin foam] may be similarly preferably used. In addition, chemical foaming agents such as azo compounds and tetrazole may be used.

[0065] In one embodiment of the manufacturing method according to the present invention, the total amount of foaming agent added is preferably 2 to 20 parts by weight, more preferably 2 to 15 parts by weight, based on 100 parts by weight of the styrene-based resin. If the amount of foaming agent added is 2 parts by weight or more, the expansion ratio can be sufficiently increased, so that the properties of the resin foam, such as light weight and heat insulating properties, are easily exhibited. If the amount of foaming agent added is 20 parts by weight or less, the occurrence of defects such as voids in the foam can be prevented.

[0066] In one embodiment of the manufacturing method according to the present invention, it is preferable to add a water-absorbing material in order to perform stable extrusion foam molding. Specific examples of the water-absorbing material used in one embodiment of the present invention include water-absorbing polymers such as polyacrylate polymers, starch-acrylic acid graft copolymers, polyvinyl alcohol polymers, vinyl alcohol-acrylate copolymers, ethylene-vinyl alcohol copolymers, acrylonitrile-methyl methacrylate-butadiene copolymers, polyethylene oxide copolymers and their derivatives, as well as fine powders having hydroxyl groups on the surface such as anhydrous silica (silicon oxide) having silanol groups on the surface [for example, AEROSIL manufactured by Nippon Aerosil Co., Ltd. is commercially available], etc.; water-absorbing or water-swelling layered silicates such as smectite and swelling fluoromica, and their organically treated products; and porous materials such as zeolite, activated carbon, alumina, silica gel, porous glass, activated clay, diatomaceous earth, and bentonite. The amount of the water-absorbing substance added is appropriately adjusted depending on the amount of water added, but is preferably 0.01 to 5 parts by weight, and more preferably 0.1 to 3 parts by weight, per 100 parts by weight of the styrene-based resin.

[0067] First, the styrene resin and, if necessary, the various additives described above are fed to the heat-melting section of an extruder having a die slit section (in other words, the resin composition is fed to the heat-melting section of the extruder). At this time, a foaming agent can be mixed into the resin composition under high pressure conditions at any stage (for example, during or after the resin composition is heated and melted). This is the melting process.

[0068] Thereafter, the foamable molten material obtained in the melting step is cooled to a temperature suitable for extrusion foaming, and then the fluid gel is extruded through the die slit into a low pressure region (e.g., an atmospheric pressure region) to form an extruded styrene resin foam. This is the foaming step.

[0069] In the melting step, examples of the method for blending various additives with the styrene-based resin include a method for adding various additives to the styrene-based resin and mixing them by dry blending; a method for adding various additives to the molten styrene-based resin from a supply section provided midway through the extruder; a method for preparing a master batch in which various additives are incorporated into the styrene-based resin at a high concentration using an extruder, kneader, Banbury mixer, rolls or the like, and mixing the master batch with the styrene-based resin by dry blending; and a method for supplying various additives to the extruder using supply equipment separate from the styrene-based resin.

[0070] The heating temperature in the heat melting section is equal to or higher than the temperature at which the styrene resin used melts. The heating temperature is preferably a temperature (for example, about 150°C to 260°C) at which molecular deterioration of the resin due to the influence of additives and the like is suppressed as much as possible. The melt kneading time in the heat melting section cannot be uniquely defined because it varies depending on the extrusion amount of the styrene resin per unit time and / or the type of extruder used as the melt kneading section, and can be appropriately set as the time required for the styrene resin, the foaming agent, and the additives to be uniformly dispersed and mixed.

[0071] As the melt-kneading section, a mechanism used in normal extrusion foaming can be used without any particular limitation, and examples thereof include a screw-type extruder.

[0072] The pressure at which the foaming agent is added or injected is not particularly limited, and may be any pressure higher than the internal pressure of an extruder or the like.

[0073] In the foaming step, the method of extrusion foaming may be, for example, a method in which the above-mentioned fluid gel is released from a high pressure region to a low pressure region through a die slit portion having a straight slit shape used for extrusion molding. In this way, an extruded foam is obtained. Note that the shape of the die slit portion is not particularly limited, and various die slit portions in the technical field can be used.

[0074] The extruded styrene resin foam may be molded into a plate-like foam, i.e., an extruded foam plate. For example, the extruded foam obtained as described above can be molded into a plate-like foam having a large cross-sectional area by using a molding die installed in close contact with or in contact with a slit die and a molding roll installed adjacent to the downstream side of the molding die. The desired cross-sectional shape, surface properties, and quality of the foam can be obtained by adjusting the flow surface shape of the molding die and the die temperature. EXAMPLES

[0075] Examples of the present invention will be described below, but the present invention is not limited to these.

[0076] [Raw materials] The raw materials used in the examples and comparative examples are as follows. Styrene-based resin Polystyrene A [PS Japan Co., Ltd., 680; MFR 7.0g / 10min] Polystyrene B [PS Japan Co., Ltd., G9401; MFR 2.1g / 10min] Styrene-methacrylic acid copolymer [PS Japan Co., Ltd., G9001; MFR 1.5g / 10min, methacrylic acid content 8% by weight] Heat radiation suppressant Graphite [Marutoyo Foundry Manufacturing Co., Ltd., M-885; flake graphite, average particle size 5.5 μm, fixed carbon content 89%] ○Flame retardants Mixture of tetrabromobisphenol A bis(2,3-dibromo-2-methylpropyl) ether and tetrabromobisphenol A bis(2,3-dibromopropyl) ether as brominated flame retardants [GR-125P, manufactured by Daiichi Kogyo Seiyaku Co., Ltd.] Flame retardant assistant ·Triphenylphosphine oxide [Sumitomo Corporation Chemicals] Stabilizers Bisphenol-A glycidyl ether [ADEKA Corporation, EP-13] Dipentaerythritol-adipic acid reaction mixture [Ajinomoto Fine-Techno Co., Ltd., Plain Riser ST210] Triethylene glycol-bis-3-(3-tert-butyl-4-hydroxy-5-methylphenyl)propionate [Songwon Japan, Sonnox 2450FF] Other additives Talc [Talc Powder PK-Z, manufactured by Hayashi Kasei Co., Ltd.] Calcium stearate [Sakai Chemical Industry Co., Ltd., SC-P] Bentonite [Hojun Co., Ltd., Bengelbright 11K] Silica [Evonik Degussa Japan Co., Ltd., Carplex BS-304F] Stearic acid monoglyceride [Riken Vitamin Co., Ltd., Rikemal S-100P] ○Foaming agent · HFO-1234ze [Taiyo Liquefied Gas Co., Ltd.] ·HCFO-1233zd [Taiyo Liquefied Gas Co., Ltd.] Ethyl chloride [Nippon Specialty Chemical Industry Co., Ltd.] ·water.

[0077] [Measurement method] In the examples and comparative examples, various parameters were measured and evaluated according to the following measurement methods.

[0078] (1) Thickness of styrene-based resin extruded foam (before cutting) The thickness of the extruded foam plate with a cross section of 60 mm thick x 1000 mm wide obtained in [Preparation of extruded foam] described later was measured at three points in total, namely, the center in the width direction and a point 150 mm from one end in the width direction to the opposite end (the same point on both ends in the width direction) using a vernier caliper [Mitutoyo Corporation, M-type standard vernier caliper N30]. The average value of the three points was regarded as the thickness of the extruded styrene resin foam.

[0079] (2) Apparent density (kg / m 3 ) The weight of the resulting extruded styrene resin foam was measured, and its length (in the extrusion direction), width and thickness were also measured.

[0080] From the measured weight and each dimension, the apparent density of the extruded styrene resin foam was calculated based on the following formula. The unit of apparent density was then expressed as kg / m 3 was converted to. Apparent density (g / cm 3 ) = foam weight (g) / foam volume (cm 3 ).

[0081] (3) Closed cell ratio Test pieces measuring 40 mm thick, 25 mm long (in the extrusion direction), and 25 mm wide were cut out from three locations of the obtained extruded styrene foam: the widthwise center, a location 150 mm from one end in the widthwise direction toward the opposite end, and a location 150 mm from the other end in the widthwise direction toward the opposite end. The test pieces were measured according to procedure C of ASTM-D2856-70, and the closed cell ratio of each test piece was calculated by the following formula. The average value of the closed cell ratios at the three locations was taken as the closed cell ratio of the extruded styrene foam. Closed cell ratio (%)=(V1-W / ρ)×100 / (V2-W / ρ) Here, V1(cm 3 ) is the true volume of the test piece (excluding the volume of the part that is not an independent bubble) measured using an air comparison type specific gravity meter [Tokyo Science Co., Ltd., air comparison type specific gravity meter, model 1000]. V2 (cm 3) is the apparent volume calculated from the outer dimensions of the test piece measured using a vernier caliper [Mitutoyo Corporation, M-type standard vernier caliper N30]. W (g) is the total weight of the test piece. Also, ρ (g / cm 3 ) is the density of the styrene resin that constitutes the extruded foam, and is 1.05 (g / cm 3 ) was decided.

[0082] (4) Average bubble diameter in the thickness direction For the obtained extruded styrene resin foam, the average cell diameter in the thickness direction was measured using a microscope [DIGITAL MICROSCOPE VHX-900, manufactured by KEYENCE CORPORATION] as described above.

[0083] (5) Thermal conductivity According to JIS A 9521, a test piece of 50 mm thickness × 300 mm length (extrusion direction) × 300 mm width cut from a styrene-based resin extrusion foam was used to measure thermal conductivity at an average temperature of 23°C using a thermal conductivity measuring device [Eiko Seiki Co., Ltd., HC-074]. Specifically, after production of the styrene-based resin extrusion foam, a test piece of the above dimensions was cut out and left to stand under standard temperature condition class 3 (23°C ± 5°C) and standard humidity condition class 3 (50 + 20, -10% RH) conditions specified in JIS K 7100, and then the thermal conductivity was measured one week (7 days) after production of the styrene-based resin extrusion foam.

[0084] (6) JIS flammability In accordance with JIS A 9521, a test piece having a thickness of 10 mm, a length (in the extrusion direction) of 200 mm, and a width of 25 mm was used to evaluate the flammability according to the following criteria. The produced styrene-based resin extrusion foam was cut into a test piece having the above dimensions, and the test piece was left to stand under the conditions of standard temperature condition Class 3 (23°C ± 5°C) and standard humidity condition Class 3 (50 + 20, -10% RH) specified in JIS K 7100. One week (7 days) after the production of the styrene-based resin extrusion foam, the test piece was used to evaluate the flammability. ○: Meets the criteria of "flame goes out within 3 seconds, there is no residual fuel, and the fire does not burn beyond the flammability limit indicator line." ×: Does not meet the above criteria.

[0085] (7) Dimensional change rate The dimensional change rate of the styrene-based resin extrusion foam of the present invention was measured by using a test piece cut out from the styrene-based resin extrusion foam with a thickness of 50 mm x length (extrusion direction) of 300 mm x width of 300 mm, and measuring the dimensions of each part of the length, width, and thickness of the test piece with a vernier caliper after leaving it for one day or more under the conditions of standard temperature condition class 3 (23°C ± 5°C) and standard humidity condition class 3 (50 + 20, -10% RH). Next, the test piece after the dimension measurement was heated at a predetermined temperature, here 80°C, for 24 hours, and the heated test piece was left for one day under the conditions of standard temperature condition class 3 (23°C ± 5°C) and standard humidity condition class 3 (50 + 20, -10% RH), and then the dimensions of the same parts as before heating were measured.

[0086] (Production example) [Preparation of graphite master batch] 48% by weight of polystyrene A, 50% by weight of graphite [M-885, manufactured by Marutoyo Foundry Manufacturing Co., Ltd.], and 2.0% by weight of stearic acid monoglyceride [Rikemal S-100P, manufactured by Riken Vitamin Co., Ltd.] (based on a total weight of 100% by weight of polystyrene A, graphite, and stearic acid monoglyceride) were charged into a Banbury mixer and mixed at 5 kgf / cm. 2 The resin was melt-kneaded for 20 minutes without heating or cooling under a load of 1.5 kg / hr. The resin temperature was measured and found to be 190° C. The strand-shaped resin was fed to a ruder and extruded through a die with small holes attached to the tip at a discharge rate of 250 kg / hr. The strand-shaped resin was cooled and solidified in a water bath at 30° C. and then cut into graphite masterbatches.

[0087] Example 1 [Preparation of resin mixture] The materials shown in Table 1 (materials other than the foaming agent) were dry-blended in the composition shown in Table 1 to obtain a resin mixture.

[0088] [Preparation of extruded foam] The obtained resin composition was supplied at about 800 kg / hr to an extruder in which a single screw extruder (first extruder) with a diameter of 150 mm, a single screw extruder (second extruder) with a diameter of 200 mm, and a cooler were connected in series.

[0089] The resin composition supplied to the first extruder was heated to 250°C to melt or plasticize it, and kneaded to obtain a resin composition, and the foaming agent shown in Table 1 was injected into the resin composition near the tip of the first extruder.

[0090] The resin composition was then cooled to the resin temperature shown in Table 1 in the second extruder and cooler connected to the first extruder, and extruded into the atmosphere at the foaming pressure shown in Table 1 through a die (slit die) with a rectangular cross section and a thickness shown in Table 1, which was attached to the tip of the cooler, and then an extruded foam board with a cross section of 60 mm thick x 1000 mm wide was obtained using a molding die placed in close contact with the die and a molding roll placed downstream of it. The evaluation results of the obtained foam are shown in Table 1.

[0091] (Examples 2 to 4) An extruded foam was obtained in the same manner as in Example 1, except that the composition and production conditions were changed as shown in Table 1. The physical properties of the obtained extruded foam are shown in Table 1.

[0092] (Comparative Examples 1 to 4) An extruded foam was obtained in the same manner as in Example 1, except that the composition and production conditions were changed as shown in Table 1. The physical properties of the obtained extruded foam are shown in Table 1.

[0093] As can be seen from Examples 1 to 4 and Comparative Examples 1 to 3, by including a styrene-methacrylic acid copolymer in a specific range in a styrene-based resin and including a specific foaming agent, it is possible to easily obtain an extruded styrene-based resin foam having excellent heat insulation properties, a beautiful surface, and a sufficient thickness suitable for use.

[0094] [Table 1] [Industrial Applicability]

[0095] The extruded styrene-based resin foam according to one embodiment of the present invention can be used, for example, as a heat insulating material, a sound absorbing material, a core material for a vacuum heat insulating material, a cushioning material, and a filler material.

Claims

1. A styrene-based resin extruded foam comprising a styrene-based resin and a foaming agent, The styrene-based resin includes a styrene-(meth)acrylic acid-based copolymer, the content of the styrene-(meth)acrylic acid-based copolymer in 100% by weight of the styrene-based resin is 20 to 80% by weight, The foaming agent contains 5.0 to 10.0 parts by weight of a hydro(chloro)fluoroolefin relative to 100 parts by weight of the styrene-based resin, A styrene-based resin extruded foam having a thermal conductivity of 0.021 W / mK or less.

2. The extruded styrene-based resin foam according to claim 1, wherein the content of the (meth)acrylic acid-derived constituent units is 5 to 20% by weight based on 100% by weight of all constituent units of the styrene-(meth)acrylic acid-based copolymer.

3. The styrene-based resin extruded foam according to any one of claims 1 to 2, further comprising an alkyl chloride, and the content of the alkyl chloride is 3.0 to 6.0 parts by weight per 100 parts by weight of the total styrene-based resin in the styrene-based resin extruded foam.

4. The extruded styrene-based resin foam according to any one of claims 1 to 2, comprising 1.0 part by weight or more and 5.0 parts by weight or less of graphite per 100 parts by weight of the styrene-based resin.

5. The extruded styrene-based resin foam according to any one of claims 1 to 2, characterized in that the dimensional change rate of the extruded styrene-based resin foam when heated in an atmosphere of 80 ° C. for 24 hours is within 5%.

6. The apparent density of the styrene-based resin extruded foam is 20 to 60 kg / m 3 The extruded styrene-based resin foam according to any one of claims 1 to 2.

7. The extruded styrene-based resin foam according to any one of claims 1 to 2, wherein the thickness of the extruded styrene-based resin foam is 10 mm or more and 150 mm or less.

Citation Information

Patent Citations

  • Foaming agents and compositions containing fluorinated olefins, and foaming methods

    JP2008546892A

  • Extruded styrene resin foam and method for producing the same

    JP2013221110A

  • Styrenic resin extrusion foamed body and manufacturing method thereof

    JP2019108416A

  • Styrenic resin extrusion expanded material

    JP2019189811A