Method for producing extruded foamed particle of polypropylene-based resin having branched structure, and method for producing foamed molding

The method addresses the challenges of high open cell ratio and melt tension in polypropylene resin foam particles by using a specialized manufacturing process with a melt-kneading and granulation system, resulting in improved moldability and efficiency.

JP2024142608APending Publication Date: 2024-10-11KANEKA CORP
View PDF 2 Cites 0 Cited by

Patent Information

Application Number
JP2023054818
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Filing Date
2023-03-30
Publication Date
2024-10-11

AI Technical Summary

Technical Problem

Conventional methods for producing polypropylene resin foam particles with a branched structure face challenges in achieving a low open cell ratio and high melt tension, limiting their moldability and efficiency.

Method used

A method involving a manufacturing device with a melt-kneading section and granulation section, using a polypropylene resin with a branched structure and a blowing agent, where the resin is melt-kneaded and extruded under specific conditions, including a shearing speed and residence time, to produce foam particles with controlled cell structure.

Benefits of technology

The method achieves polypropylene resin foam particles with a low open cell ratio and controlled melt tension, enhancing moldability and production efficiency.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024142608000001
    Figure 2024142608000001
Patent Text Reader

Abstract

To provide a method for producing a polypropylene-based resin extruded foamed particles with low open cell rate.SOLUTION: A method for producing extruded foamed polypropylene-based resin particles comprises: a melt-kneading step of melt-kneading a polypropylene-based resin having a branched structure and a foaming agent by using a production apparatus equipped with a melt-kneading section having a plurality of screws and a granulation section having a die to obtain a resin composition; and an extrusion foaming step of discharging the resin composition obtained in the melt-kneading step through the die into a region having a lower pressure than the internal pressure of the production apparatus, wherein a temperature of the resin composition in the final part of the melt-kneading section is equal to or lower than the melting point of the polypropylene-based resin having a branched structure + 65°C, and the residence time of the polypropylene-based resin having a branched structure in the production apparatus is 40 seconds or less.SELECTED DRAWING: None
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a method for producing extruded foamed beads of a polypropylene resin having a branched structure, and a method for producing a foamed molded article. [Background technology]

[0002] The polypropylene resin in-mold foamed article obtained by using the expanded polypropylene resin particles has the advantages of in-mold foamed articles, such as freedom in shape, excellent cushioning properties, light weight, and excellent heat insulating properties.

[0003] Examples of methods for producing polypropylene-based resin expanded beads include a batch expansion method, which is a discontinuous process, and an extrusion expansion method, which is a continuous process. The extrusion expansion method has many advantages in terms of efficiency and environment, but has a problem that it is difficult to obtain polypropylene-based resin expanded beads with good moldability. As a means for solving this problem, the use of modified polypropylene resin with improved melt tension as a raw material has been considered. For example, as a technique for obtaining polypropylene-based resin expanded beads by extrusion foaming, Patent Document 1 discloses a method for producing polypropylene-based resin expanded beads by melt-kneading a polypropylene-based resin having a branched structure and a foaming agent using an extruder, then cooling, extruding the obtained molten resin at a specific temperature into a low-pressure region at a specific temperature, and chopping it. In addition, Patent Document 2 discloses a production method in which a polypropylene-based resin having a branched structure and a foaming agent are melt-kneaded with a screw of an extruder at a specific power (P2), and expanded beads are produced at a discharge amount (Q2), and the ratio of P2 to Q2 (P2 / Q2) satisfies 0.190 kWh / kg or less. [Prior art documents] [Patent documents]

[0004] [Patent Document 1] International Publication No. 2022 / 050375 [Patent Document 2] International Publication No. 2022 / 163627 Summary of the Invention [Problem to be solved by the invention]

[0005] However, the conventional techniques relating to polypropylene resin compositions having a branched structure as disclosed in Patent Documents 1 and 2 have room for improvement in the open cell ratio of the resulting expanded beads, and require the use of a polypropylene-based resin having a branched structure with high melt tension as a raw material. One embodiment of the present invention has been made in consideration of the above problems, and an object of the present invention is to provide expanded beads having a low open cell ratio, or to provide a method for obtaining expanded beads having a low open cell ratio from a branched polypropylene-based resin having low melt tension. [Means for solving the problem]

[0006] The present invention relates to (1) A method for producing extruded foamed polypropylene-based resin particles, comprising: a melt-kneading step of melt-kneading a polypropylene-based resin having a branched structure and a foaming agent in a production apparatus equipped with a melt-kneading section having a plurality of screws and a granulating section having a die to obtain a resin composition; and an extrusion foaming step of discharging the resin composition obtained in the melt-kneading step through the die into a region having a lower pressure than the internal pressure of the production apparatus, wherein the temperature of the resin composition in the final part of the melt-kneading section is equal to or lower than the melting point of the polypropylene-based resin having a branched structure + 65°C, and the residence time of the polypropylene-based resin having a branched structure in the production apparatus is 40 seconds or less. (2) The shear rate of the screw is 100 s ―1 The method for producing extruded polypropylene resin beads according to (1), (3) The method for producing extruded polypropylene-based resin foamed beads according to (1) or (2), wherein the number of parts of the foaming agent is 1.0 to 5.0 parts by weight per 100 parts by weight of the polypropylene-based resin having a branched structure. (4) The method for producing extruded polypropylene resin foamed beads according to (1) or (2), wherein the foaming agent is at least one selected from the group consisting of CO2, propane, butane, pentane, and nitrogen. (5) The method for producing extruded polypropylene resin foam beads according to (1) or (2), wherein the melt strength of the polypropylene resin having a branched structure is 2.0 cN or more. (6) The method for producing extruded polypropylene resin foam beads according to (1) or (2), wherein the extruded polypropylene resin foam beads have a melt flow rate of 4.5 g / 10 min or less at 230° C.; (7) A method for producing a polypropylene resin foamed molded article, which comprises molding the extruded polypropylene resin foamed beads obtained by (1) or (2). Regarding. Effect of the Invention

[0007] According to one embodiment of the present invention, a method for producing expanded beads having a low open cell content can be provided. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0008] An embodiment of the present invention will be described below, but the present invention is not limited thereto. The present invention is not limited to each configuration described below, and various modifications are possible within the scope of the claims. In addition, embodiments or examples obtained by appropriately combining the technical means disclosed in different embodiments or examples are also included in the technical scope of the present invention. Furthermore, new technical features can be formed by combining the technical means disclosed in each embodiment. All academic documents and patent documents described in this specification are incorporated herein by reference. In addition, unless otherwise specified in this specification, "A to B" representing a numerical range means "A or more (including A and greater than A) and B or less (including B and smaller than B)".

[0009] In this specification, the term "polypropylene-based resin having a branched structure" refers to (a) a polypropylene-based resin in which molecules of a polypropylene-based resin in which a branched structure has not been introduced are partially cross-linked with each other, and (b) a polypropylene-based resin in which a diene compound other than (poly)propylene has been introduced as a branched chain into a polypropylene-based resin in which a branched structure has not been introduced.

[0010] In this specification, the "polypropylene resin without a branched structure" may be referred to as a "linear polypropylene resin", the "polypropylene resin with a branched structure" may be referred to as a "branched polypropylene resin", and the "linear polypropylene resin" and the "branched polypropylene resin" may be collectively referred to as a "polypropylene resin". The linear polypropylene resin may also be considered as a raw material for the branched polypropylene resin.

[0011] In this specification, a linear polypropylene resin refers to a resin that contains 50 mol % or more of structural units derived from propylene monomers, based on 100 mol % of all structural units contained in the resin.

[0012] In this specification, the "structural unit derived from a propylene monomer" may be referred to as a "propylene unit." In addition, in this specification, a branched polypropylene resin refers to a resin in which the main chain of the branched polypropylene resin contains 50 mol % or more of structural units derived from a propylene monomer, out of 100 mol % of all structural units contained in the main chain. The "main chain" of a branched polypropylene resin refers to a structure derived from a linear polypropylene resin, which is a raw material of the branched polypropylene resin.

[0013] The production method of the present invention uses a production apparatus equipped with a melt-kneading section having a plurality of screws and a granulation section having a die, and includes a melt-kneading step of melt-kneading a resin composition containing a polypropylene-based resin having a branched structure and a foaming agent in the melt-kneading section, and an extrusion-foaming step of extruding the resin composition obtained in the melt-kneading step through the die into a region having a lower pressure than the internal pressure of the production apparatus, wherein the resin temperature in the final part of the melting section is melting point +65°C or less, and the residence time of the polypropylene-based resin having a branched structure in the production apparatus is 40 seconds or less. This is a production method for extruded polypropylene-based resin foamed beads.

[0014] <Branched polypropylene resin> The branched polypropylene resin is a modified polypropylene resin obtained by introducing a branched structure into a linear polypropylene resin.

[0015] A linear polypropylene resin refers to a resin that contains 50 mol % or more of structural units derived from propylene monomers, based on 100 mol % of all structural units contained in the resin.

[0016] The method for introducing a branched structure into a linear polypropylene-based resin is not particularly limited, and examples thereof include (1) a method of irradiating a linear polypropylene-based resin with radiation, and (2) a method of melt-kneading a mixture containing a linear polypropylene-based resin, a monomer selected from the group consisting of conjugated dienes and vinyl aromatic compounds, and a radical polymerization initiator.

[0017] A specific example of the method (1) above is the method described in JP-T-2002-542360.

[0018] A specific example of the above method (2) is a method in which a linear polypropylene resin, a monomer selected from a conjugated diene and a vinyl aromatic compound, and a radical polymerization initiator are melt-kneaded at a temperature at which the linear polypropylene resin melts and the radical polymerization initiator decomposes.

[0019] <Straight-chain polypropylene resin> Examples of the linear polypropylene resin include homopolypropylene resin, random polypropylene resin, and block polypropylene resin. Of these, the random polypropylene resin is preferred.

[0020] <Homopolypropylene resin> The homopolypropylene resin refers to a homopolymer of a propylene monomer.

[0021] <Random polypropylene resin> A random polypropylene resin is a random copolymer of a propylene monomer and a monomer other than propylene. A random polypropylene resin contains 50 mol% or more of structural units derived from a propylene monomer and less than 50 mol% of structural units derived from a monomer other than a propylene monomer, out of 100 mol% of all structural units contained in the resin. In this specification, a "structural unit derived from a propylene monomer" may also be referred to as a "propylene unit". In this specification, a "structural unit derived from a monomer other than a propylene monomer" may also be referred to as a "comonomer unit".

[0022] Examples of the comonomer include (a) α-olefins having 2 or 4 to 12 carbon atoms, such as ethylene, 1-butene, isobutene, 1-pentene, 3-methyl-1-butene, 1-hexene, 4-methyl-1-pentene, 3,4-dimethyl-1-butene, 1-heptene, 3-methyl-1-hexene, 1-octene, and 1-decene; (b) cyclic olefins, such as cyclopentene, norbornene, and tetracyclo[6,2,11,8,13,6]-4-dodecene; and (c) 5-methylene-2-olefins. -norbornene, 5-ethylidene-2-norbornene, 1,4-hexadiene, methyl-1,4-hexadiene, 7-methyl-1,6-octadiene, and other dienes; and (d) vinyl monomers such as vinyl chloride, vinylidene chloride, acrylonitrile, methacrylonitrile, vinyl acetate, acrylic acid, acrylic acid esters, methacrylic acid, methacrylic acid esters, maleic acid, maleic anhydride, styrene-based monomers, vinyl toluene, and divinyl benzene.

[0023] Examples of the acrylic acid ester include methyl acrylate, ethyl acrylate, butyl acrylate, hexyl acrylate, 2-ethylhexyl acrylate, lauryl acrylate, stearyl acrylate, 2-hydroxyethyl acrylate, 2-hydroxypropyl acrylate, and glycidyl acrylate.

[0024] Examples of methacrylic acid esters include methyl methacrylate, ethyl methacrylate, butyl methacrylate, hexyl methacrylate, 2-ethylhexyl methacrylate, lauryl methacrylate, stearyl methacrylate, 2-hydroxyethyl methacrylate, 2-hydroxypropyl methacrylate, and glycidyl methacrylate.

[0025] Styrenic monomers include styrene, methylstyrene, dimethylstyrene, alpha-methylstyrene, para-methylstyrene, ethylstyrene, diethylstyrene, isopropylstyrene, t-butylstyrene, bromostyrene, dibromostyrene, tribromostyrene, chlorostyrene, dichlorostyrene, and trichlorostyrene.

[0026] The random polypropylene resin preferably has a structural unit derived from an α-olefin having 2 or 4 to 12 carbon atoms as a comonomer unit, more preferably a structural unit derived from ethylene, 1-butene, isobutene, 1-pentene, 3-methyl-1-butene, 1-hexene, 4-methyl-1-pentene, 3,4-dimethyl-1-butene, 1-heptene, 3-methyl-1-hexene, 1-octene and / or 1-decene, more preferably a structural unit derived from ethylene, 1-butene, isobutene, 1-pentene, 3-methyl-1-butene, 1-hexene and / or 4-methyl-1-pentene, even more preferably a structural unit derived from ethylene, 1-butene, isobutene and / or 1-pentene, and even more preferably a structural unit derived from ethylene and / or 1-butene.

[0027] The random polypropylene resin preferably contains 90 mol % or more of propylene units, more preferably 93 mol % or more, even more preferably 94 mol % or more, and particularly preferably 95 mol % or more, of all structural units contained in the random polypropylene resin.

[0028] <Block polypropylene resin> Block polypropylene resins include ethylene-propylene block copolymers, propylene-butene block copolymers, and ethylene-propylene-butene block copolymers. Propylene-ethylene block copolymers are propylene-based polymers in which ethylene-based polymers and ethylene-propylene rubber-like copolymers are dispersed in a linear polymer mainly composed of propylene, forming an island-in-a-sea structure.

[0029] <Monomer selected from conjugated dienes and vinyl aromatic compounds> Examples of conjugated dienes include butadiene, isoprene, 1,3-heptadiene, 2,3-dimethylbutadiene, and 2,5-dimethyl-2,4-hexadiene. These conjugated diene compounds may be used alone or in combination of two or more. Among these conjugated diene compounds, butadiene and isoprene are particularly preferred because (a) they are inexpensive and easy to handle, and (b) the reaction proceeds uniformly.

[0030] Examples of vinyl aromatic compounds include styrene; methylstyrenes such as o-methylstyrene, m-methylstyrene, p-methylstyrene, α-methylstyrene, β-methylstyrene, dimethylstyrene, and trimethylstyrene; chlorostyrenes such as α-chlorostyrene, β-chlorostyrene, o-chlorostyrene, m-chlorostyrene, p-chlorostyrene, dichlorostyrene, and trichlorostyrene; bromostyrenes such as o-bromostyrene, m-bromostyrene, p-bromostyrene, dibromostyrene, and tribromostyrene; o-fluorostyrene, m-fluorostyrene, p-fluorostyrene, di Examples of the vinyl aromatic compound include fluorostyrenes such as fluorostyrene and trifluorostyrene; nitrostyrenes such as o-nitrostyrene, m-nitrostyrene, p-nitrostyrene, dinitrostyrene and trinitrostyrene; vinylphenols such as o-hydroxystyrene, m-hydroxystyrene, p-hydroxystyrene, dihydroxystyrene and trihydroxystyrene; divinylbenzenes such as o-divinylbenzene, m-divinylbenzene and p-divinylbenzene; isopropenylstyrenes such as o-diisopropenylbenzene, m-diisopropenylbenzene and p-diisopropenylbenzene, etc. Among the above-mentioned vinyl aromatic compounds, styrene and / or methylstyrene are preferred because (a) they are inexpensive and easy to handle, and (b) the reaction proceeds uniformly.

[0031] The amount of the conjugated diene or the like used is preferably 0.01 to 5.00 parts by weight, more preferably 0.10 to 3.00 parts by weight, and even more preferably 0.10 to 2.00 parts by weight, based on 100 parts by weight of the linear polypropylene resin.

[0032] <Radical polymerization initiator> The radical polymerization initiator is an organic peroxide capable of abstracting hydrogen from a linear polypropylene resin, a conjugated diene compound, etc. Examples of the radical polymerization initiator include organic peroxides such as ketone peroxides, peroxyketals, hydroperoxides, dialkyl peroxides, diacyl peroxides, peroxydicarbonates, and peroxyesters.

[0033] As the organic peroxide, those having a particularly high hydrogen abstraction ability are preferred. Examples of organic peroxides having a high hydrogen abstraction ability include peroxyketals such as 1,1-bis(t-butylperoxy)3,3,5-trimethylcyclohexane, 1,1-bis(t-butylperoxy)cyclohexane, n-butyl 4,4-bis(t-butylperoxy)valerate, and 2,2-bis(t-butylperoxy)butane; dicumyl peroxide, 2,5-dimethyl-2,5-di(t-butylperoxy)hexane, α,α'-bis(t-butylperoxy-m-isopropyl)benzene, t-butylcumyl peroxide, di-t-butyl peroxide, and 2,5-dimethyl-2,5- Suitable examples of the organic peroxide include dialkyl peroxides such as di(t-butylperoxy)-3-hexyne; diacyl peroxides such as benzoyl peroxide; peroxy esters such as t-butylperoxyoctate, t-butylperoxyisobutyrate, t-butylperoxylaurate, t-butylperoxy3,5,5-trimethylhexanoate, t-butylperoxyisopropylcarbonate, 2,5-dimethyl-2,5-di(benzoylperoxy)hexane, t-butylperoxyacetate, t-butylperoxybenzoate, and di-t-butylperoxyisophthalate; and the like. Among these, t-butylperoxyisopropylcarbonate and / or t-butylperoxybenzoate are preferred. These organic peroxides may be used alone or in combination of two or more.

[0034] The amount of the radical polymerization initiator used is preferably 0.01 to 5.00 parts by weight, more preferably 0.10 to 3.00 parts by weight, more preferably 0.10 to 2.00 parts by weight, and particularly preferably 0.10 to 1.50 parts by weight, relative to 100 parts by weight of the linear polypropylene resin.

[0035] In the above method (2), examples of the device for melt-kneading the linear polypropylene-based resin, the monomer such as conjugated diene, and the radical polymerization initiator include kneaders such as rolls, co-kneaders, Banbury mixers, Brabenders, single-screw extruders, and twin-screw extruders; horizontal stirrers such as twin-screw surface renewal machines and twin-screw multi-disk devices; and vertical stirrers such as double helical ribbon stirrers. Of these, it is preferable to use a kneader, and in particular, extruders such as single-screw extruders and twin-screw extruders are preferable from the viewpoint of productivity.

[0036] There is no particular restriction on the order or method of mixing and kneading the linear polypropylene resin, the monomer such as conjugated diene, and the radical polymerization initiator. The linear polypropylene resin, the monomer such as conjugated diene, and the radical polymerization initiator may be mixed and then melt-kneaded, or the linear polypropylene resin may be melt-kneaded and then the monomer such as conjugated diene or the radical polymerization initiator may be mixed simultaneously or separately, all at once or in portions. The temperature of the kneader is preferably 130°C or higher and 300°C or lower. The time for melt-kneading is generally preferably 1 minute or higher and 60 minutes or lower.

[0037] <Physical properties of branched polypropylene resin> The melting point (Tm) of the branched polypropylene resin is not particularly limited, but is preferably from 130.0°C to 165.0°C, and more preferably from 135.0°C to 155.0°C.

[0038] In this specification, the melting point is a value determined by measurement using differential scanning calorimetry.

[0039] The cold crystallization temperature (Tc) of the branched polypropylene resin is not particularly limited, but is preferably from 90.0°C to 130.0°C, and more preferably from 100.0°C to 125.0°C.

[0040] In this specification, the cold crystallization temperature is a value determined by measurement using differential scanning calorimetry.

[0041] The melt flow rate (MFR) of the branched polypropylene resin is not particularly limited, but is preferably 0.5 g / 10 min to 50 g / 10 min, and more preferably 0.5 g / 10 min to 30 g / 10 min.

[0042] In this specification, the MFR is a value determined by measurement at a temperature of 230°C in accordance with ISO1133.

[0043] The melt tension (MT) of the branched polypropylene resin is not particularly limited, but is preferably from 5 cN to 20 cN, and more preferably from 5 cN to 15 cN.

[0044] In this specification, the melt tension is measured using a Capilograph 1D (manufactured by Toyo Seiki Seisakusho, Japan). Specifically, the steps are as follows: (1) A sample resin (branched polypropylene resin) for measurement is filled into a barrel with a diameter of 9.55 mm heated to a test temperature (200°C); (2) The sample resin is then heated for 10 minutes in the barrel heated to the test temperature (200°C); (3) The sample resin is then discharged in a string-like form from a capillary die (diameter 1.0 mm, length 10 mm) at a constant piston descending speed (10 mm / min), while passing this string-like material through a tension detection pulley located 350 mm below the capillary die, and then winding using a winding roll is started; (4) After the take-up of the string-like material becomes stable, the winding speed of the string-like material is increased at a constant rate from an initial speed of 1.0 m / min until it reaches a speed of 200 m / min in 4 minutes; (5) The load applied to the pulley with the load cell when the string-like material breaks is measured as the melt tension.

[0045] <Foaming agent> The foaming agent of the present invention is not particularly limited as long as it is a foaming agent generally used in extrusion foaming.The foaming agent can be, for example, (a) (a-1) aliphatic hydrocarbons such as propane, normal butane, isobutane, normal pentane, isopentane, hexane, etc.; (a-2) alicyclic hydrocarbons such as cyclopentane, cyclobutane, etc.; (a-3) ethers such as dimethyl ether, diethyl ether, methyl ethyl ether, etc.; (a-4) fluorinated hydrocarbons such as difluoroethane, etc.; (a-5) alcohols such as methanol, ethanol, etc.; (a-6) inorganic gases such as air, nitrogen, carbon dioxide, etc.; and (a-7) physical foaming agents such as water, and (b) chemical foaming agents including pyrolysis type foaming agents such as sodium bicarbonate, azodicarbonamide, dinitrosopentamethylenetetramine, etc.

[0046] In the manufacturing method of the present invention, the foaming agent is preferably an inorganic gas, more preferably carbon dioxide gas, because of its low production cost and low environmental load. Also, it is preferable to use only carbon dioxide gas as the foaming agent, and to substantially not contain any foaming agent other than carbon dioxide gas, which is mentioned above as an example of the foaming agent. Specifically, the content of the foaming agent other than carbon dioxide gas, which is mentioned above as an example of the foaming agent, in the resin composition is preferably 0.01 parts by weight or less, more preferably 0.001 parts by weight or less, even more preferably 0.0001 parts by weight or less, and particularly preferably 0 parts by weight, relative to 100 parts by weight of the resin composition.

[0047] In the second production method, the amount of the foaming agent used may be appropriately adjusted depending on the type of foaming agent and the expansion ratio of the target foam. In the production method of the present invention, the total amount of the foaming agent used is preferably 1 to 20 parts by weight, more preferably 1 to 15 parts by weight, even more preferably 1 to 10 parts by weight, and particularly preferably 2 to 10 parts by weight, relative to 100 parts by weight of the resin composition. The "amount of the foaming agent used" can also be called the "content of the foaming agent in the resin composition."

[0048] <Other resins and rubbers> The resin composition of the present invention may further contain a resin other than the branched polypropylene-based resin (sometimes referred to as "other resins") and / or rubber, as long as the effect of the present invention is not impaired. The other resins and rubbers may be collectively referred to as "other resins, etc." Examples of the other resins include (a) linear polypropylene-based resins such as ethylene / propylene random copolymers, ethylene / propylene block copolymers, ethylene / propylene alternating copolymers, and propylene homopolymers, (b) ethylene-based resins such as high-density polyethylene, medium-density polyethylene, low-density polyethylene, linear low-density polyethylene, linear very low-density polyethylene, ethylene / vinyl acetate copolymers, ethylene / acrylic acid copolymers, and ethylene / methacrylic acid copolymers, and (c) styrene-based resins such as polystyrene, styrene / maleic anhydride copolymers, and styrene / ethylene copolymers. Examples of the rubbers include olefin-based rubbers such as ethylene / propylene rubber, ethylene / butene rubber, ethylene / hexene rubber, and ethylene / octene rubber. The content of the other resins in the resin composition of the present invention is, for example, preferably 60 parts by weight or less, more preferably 40 parts by weight or less, and even more preferably 20 parts by weight or less, relative to 100 parts by weight of the branched polypropylene resin. The lower limit of the content of the other resins is not particularly limited, and may be, for example, 0 part by weight relative to 100 parts by weight of the branched polypropylene resin.

[0049] <Bubble nucleating agent> The resin composition of the present invention may contain a bubble nucleating agent for the purpose of controlling the number and shape of bubbles in the resulting extruded foamed particles. Examples of the bubble nucleating agent include a mixture of sodium bicarbonate and citric acid, monosodium citrate, talc, and calcium carbonate. These bubble nucleating agents may be used alone or in combination of two or more.

[0050] The amount of the bubble nucleating agent used, in other words, the content of the bubble nucleating agent in the resin composition of the present invention, is not particularly limited. The amount of the bubble nucleating agent used is, for example, preferably 0.01 to 5.00 parts by weight, more preferably 0.01 to 3.50 parts by weight, even more preferably 0.01 to 1.00 parts by weight, and particularly preferably 0.01 to 0.50 parts by weight, relative to 100 parts by weight of the branched polypropylene resin.

[0051] <Other ingredients> The resin composition of the present invention may further contain, as other components as necessary, (a) stabilizers such as antioxidants, metal deactivators, phosphorus-based processing stabilizers, ultraviolet absorbers, ultraviolet stabilizers, fluorescent brighteners, metal soaps, and antacid adsorbents, and / or (b) additives such as crosslinkers, chain transfer agents, lubricants, plasticizers, fillers, reinforcing agents, flame retardants, colorants, and antistatic agents. These other components may be used alone or in combination of two or more.

[0052] The manufacturing apparatus used in the manufacturing method of the present invention includes a melt kneading section having a plurality of screws and a granulation section having a die. The manufacturing apparatus may further include a transport section and / or a cooling section. When the manufacturing apparatus includes a transport section and a cooling section, (a) the melt kneading section, the transport section, the cooling section, and the granulation section are connected, and (b) the melt kneading section, the transport section, the cooling section, and the granulation section are arranged in this order from the upstream side to the downstream side in the extrusion direction of the resin composition. When the manufacturing apparatus includes a transport section and a cooling section, (a) the transport section and the cooling section may be provided in a reversed order on the upstream side and the downstream side, and (b) the transport section may be provided both upstream and downstream of the cooling section. The transport section can be omitted if the pressure of the resin composition in the pipe from the melt kneading section to the granulation section is sufficiently low. In addition, if the temperature of the resin composition is sufficiently reduced at the outlet of the melt kneading section, the cooling section may be omitted.

[0053] As the melt-kneading section having a plurality of screws, for example, a twin-screw extruder having two screws is preferable because it has good mixing properties. Also, the melt-kneading section preferably has a screw configuration that prevents the foaming agent injected into the melt-kneading section from flowing backward to the upstream side. That is, as the melt-kneading section having a plurality of screws, a twin-screw extruder having a two-screw configuration with a backflow prevention function is more preferable. The transport section is composed of a transport member for transporting the resin composition from the melt kneading section to the granulation section. The transport member may be a known transport member used in the extrusion foaming method, such as a gear pump. The gear pump is a useful member for maintaining or appropriately increasing the pressure of the flow of the resin composition.

[0054] The cooling section is composed of a cooling member that cools the resin composition transported from the transport section (melt kneading section when the transport section is omitted). The cooling member may be a known cooling member used in the extrusion foaming method. Examples of the cooling member include a single screw extruder or a static mixer. The resin composition is cooled to a predetermined temperature by gradually cooling the resin composition while mixing it at a low shear rate with the single screw extruder or the static mixer.

[0055] The die in the granulation section has at least one hole (sometimes referred to as a discharge hole) for discharging the molten kneaded product. The shape of the cross section of the hole in the die perpendicular to the extrusion direction (hereinafter sometimes simply referred to as the "shape of the die hole") is not particularly limited. Since extruded foamed particles having a spherical or nearly spherical shape can be obtained, the shape of the hole in the die is preferably a perfect circle, a nearly circle, an ellipse, a square, or the like. The number and diameter of the holes in the die are not particularly limited. From the viewpoint of maintaining an appropriate size of the foamed particles in the in-mold foam molding process, the die preferably has holes with a diameter of, for example, 0.1 mm to 2.0 mm, and more preferably has holes with a diameter of 0.4 mm to 1.5 mm. It is more preferable that the die has a plurality of holes (for example, two or more). In this specification, when the shape of the hole in the die is not a perfect circle, the diameter of the hole in the die refers to the diameter of the inscribed circle of the shape of the hole in the die.

[0056] <Melting and kneading process> The melt-kneading step is a step of melting the branched polypropylene resin in a melt-kneading section of a production apparatus and dissolving a foaming agent in the branched polypropylene resin. The second melt-kneading step can also be said to be a step of preparing a melt-kneaded product of the resin composition of the present invention having a branched polypropylene resin and a foaming agent.

[0057] In the melt-kneading step, the blowing agent is finally dissolved in the branched polypropylene resin. In the melt-kneading step, the order and method of supplying the branched polypropylene resin and the blowing agent to the melt-kneading section are not particularly limited, but for example, the branched polypropylene resin is supplied to the melt-kneading section, and the branched polypropylene resin is melt-kneaded; thereafter, the blowing agent is supplied to the melt-kneaded branched polypropylene resin from a raw material supply port in the middle of the melt-kneading section, that is, the resin composition is prepared (completed) in the melt-kneading section, and the resin composition is further melt-kneaded. When other resins, bubble nucleating agents and other components are added to the resin composition as required, the method and order of supplying these raw materials to the melt-kneading section are not particularly limited. The other resins, bubble nucleating agents and other components may be added simultaneously with the branched polypropylene resin and / or the foaming agent, or may be added separately and in random order.

[0058] The temperature of the resin composition at the final part of the melt-kneading process is preferably the melting point of the branched polypropylene resin +30°C to 65°C, more preferably the melting point +35°C to 60°C, and even more preferably the melting point +40°C to 60°C. By being at least 30°C above the melting point, the viscosity of the resin composition can be sufficiently reduced, and kneading with the foaming agent can be carried out efficiently. By being at most 60°C above the melting point, thermal degradation of the branched polypropylene resin can be suppressed, and expanded particles with a low open cell ratio can be obtained.

[0059] The melt-kneading process may further include, for example, a step of melt-kneading the resin composition by the method described above, and then lowering the temperature of the melt-kneaded resin composition within a temperature range in which the melt-kneaded resin composition does not solidify.

[0060] <Extrusion foaming process> The extrusion foaming process is a process in which the resin composition obtained in the melt kneading process, i.e., the melt kneaded resin composition, is extruded through a die into a region where the pressure is lower than the internal pressure of the manufacturing apparatus, and the extruded resin composition is chopped. The extrusion foaming process produces extruded foam particles. Therefore, the extrusion foaming process can also be called a granulation process for granulating extruded polypropylene resin foam particles.

[0061] In the extrusion foaming step, the region into which the resin composition obtained in the melt-kneading step is extruded is not particularly limited as long as the pressure is lower than the internal pressure of the production apparatus. For example, in the extrusion foaming step, the resin composition obtained in the melt-kneading step may be extruded into a gas phase or a liquid phase.

[0062] In the extrusion foaming process, the resin composition extruded into a region where the pressure is lower than the internal pressure of the manufacturing apparatus immediately starts to foam. In the extrusion foaming process, the resin composition may be chopped during foaming, or the resin composition that has finished foaming may be chopped. When the resin composition is chopped during foaming, the chopped resin composition can complete foaming in the region to which it is extruded.

[0063] Depending on the region where the resin composition obtained by melt kneading is extruded and the method of chopping the resin composition, it can be roughly divided into two types: granulation process, cold cut method, and die face cut method. The cold cut method includes a method in which a resin composition containing a foaming agent extruded from a die is foamed, cooled through a water tank, and then a strand-shaped foam is taken out and chopped (strand cut method). The die face cut method is a method in which the resin composition extruded from the hole of the die is cut with a rotating cutter while in contact with the surface of the die or while leaving a small gap.

[0064] The die face cutting method is further divided into three methods based on the difference in the cooling method. That is, the underwater cutting method (hereinafter sometimes referred to as UWC), the watering cutting method (hereinafter sometimes referred to as WRC), and the hot cutting method (hereinafter sometimes referred to as HC). The UWC method is a method in which cooling water adjusted to a predetermined pressure is filled in a chamber attached to the tip of the die so that it contacts the resin discharge surface of the die, and the resin composition extruded from the hole of the die is cut underwater. The WRC method is a method in which a cooling drum in which cooling water flows along the inner peripheral surface of the cooling drum connected to the die is placed downstream from the die, and the resin composition cut by the cutter is cooled in the cooling water while foaming in the air or after foaming. The HC method is a method in which the resin composition is cut by a cutter in the air, and the cut resin composition is cooled in the air while foaming in the air or after foaming. The HC method also includes a mist cutting method that further includes a step of spraying a mixed mist of water and air.

[0065] In the extrusion foaming step, the resin composition obtained in the melt kneading step is extruded into a liquid phase (for example, UWC). The liquid phase is not particularly limited, but is preferably water because it can be produced cheaply and safely. The temperature of the liquid phase is not particularly limited, but is preferably 20°C to 90°C, more preferably 25°C to 85°C, more preferably 30°C to 80°C, even more preferably 35°C to 80°C, and particularly preferably 40°C to 80°C, because it is easy to obtain extruded foamed particles with little mutual adhesion between the extruded foamed particles. In this specification, the temperature of the liquid phase can be measured by a thermometer installed so as to be in contact with the liquid phase. The liquid phase pressure for the resin composition within the region is not particularly limited, but is preferably 0.05 MPa·G to 0.60 MPa·G, more preferably 0.07 MPa·G to 0.55 MPa·G, more preferably 0.10 MPa·G to 0.50 MPa·G, even more preferably 0.10 MPa·G to 0.45 MPa·G, and particularly preferably 0.10 MPa·G to 0.40 MPa·G, because this facilitates keeping the open cell ratio of the resulting extruded foamed beads low and keeping the mutual adhesion of the resulting extruded foamed beads low. In this specification, "MPa·G" is intended to mean that MPa indicates gauge pressure.

[0066] In the present invention, the residence time of the branched polypropylene resin in the production apparatus, specifically, the total time from the start of the melt kneading process to the discharge into the low pressure region in the extrusion foaming process, is 40 seconds or less, preferably 10 to 35 seconds, more preferably 15 to 30 seconds. By making the residence time 40 seconds or less, it is possible to suppress the thermal deterioration of the branched polypropylene resin and the decrease in melt tension. By making the residence time 10 seconds or more, it is preferable because the branched polypropylene resin and the foaming agent can be sufficiently kneaded.

[0067] The shear rate of the extruder screw is 20 to 100 s -1 Less than 30-90s is preferable. -1 More preferably, 40 to 80 s -1is even more preferable. -1 This makes it possible to obtain expanded beads having a low open cell ratio.

[0068] The expanded polypropylene resin beads obtained in the present invention can be molded by a known method to obtain an expanded polypropylene resin bead molded article. EXAMPLES

[0069] The present invention is not limited to the following examples.

[0070] <MFR of branched polypropylene resin at 230℃> First, the extruded foamed beads obtained in the Examples and Comparative Examples were subjected to the following steps (f1) to (f5) in order to return the resin to obtain a resin mass.

[0071] (f1) The extruded foam particles were placed in a dryer whose temperature had been adjusted to 160°C; (f2) Then, using a vacuum pump, the pressure inside the dryer was reduced to -0.05 MPa (gauge pressure) to -0.10 MPa (gauge pressure) over a period of 5 to 10 minutes; (f3) Then, the extruded foam particles were left in the dryer for 30 minutes to prepare a resin lump (returned resin); (f4) Then, the temperature inside the dryer was cooled to room temperature, and the pressure inside the dryer was returned to normal pressure; (f5) Then, the resin lump was taken out of the dryer. The resin block obtained by resin reconstitution was used as a sample and measured using an MFR measuring device specified in JIS K 7210. The measurement conditions were an orifice diameter of 2.0959 ± 0.0050 mmφ, an orifice length of 8.000 ± 0.025 mm, a load of 2160 g, and a temperature of 230 ± 0.2°C.

[0072] <Branched polypropylene resin manufacturing equipment> As an extruder used for producing a polypropylene-based resin having a branched structure, a device equipped with a melt-kneading section having a screw and a die at the end in the extrusion direction was used. As the melt-kneading section, a twin-screw extruder was used that had (a) a co-rotating twin screw with a diameter of φ46 mm in a cylinder, (b) a raw material supply port (polypropylene-based resin supply feeder) at the upstream end in the extrusion direction, and (c) two further raw material supply ports (radical polymerization initiator supply pump and conjugated diene compound supply pump) in the middle of the cylinder. The ratio L1 / D1 of the effective length L1 and the diameter D1 of the screw in the first melt-kneading section was 30.7.

[0073] <Production of polypropylene resin having branched structure> The following steps (1) to (5) were carried out in order to produce a branched polypropylene resin: (1) 100 parts by weight of random polypropylene resin (F-724NPC, manufactured by Prime Polymer Co., Ltd.) and 1.33 parts by weight of a mixture of t-butylperoxyisopropyl monocarbonate and 2,2-di(t-butylperoxy)butane as a radical polymerization initiator were fed to a twin-screw extruder (having a twin screw having a shaft diameter of φ46 mm and rotating in the same direction) at 70 kg / h; (2) 0.55 parts by weight of isopropyl per 100 parts by weight of random polypropylene resin was fed to a twin-screw extruder (having a twin screw having a shaft diameter of φ46 mm) at a pressure of 70 kg / h; (3) The mixture in the twin-screw extruder was melt-kneaded under conditions of a cylinder temperature of 200°C (i.e., the temperature of the melt-kneading section of 200°C) and a screw rotation speed (N1) of 258 rpm to obtain a molten kneaded product (branched polypropylene-based resin); (4) The obtained molten kneaded product (branched polypropylene-based resin) was extruded from a die provided at the end of the twin-screw extruder at a discharge rate of 70 kg / h, and the extruded strands were water-cooled in a water tank; (5) The strands were chopped in a pelletizer provided at the end of the water tank to obtain pellet-shaped branched polypropylene-based resin.

[0074] The obtained branched polypropylene resin had an MFR of 3.8 g / 10 min and a melt tension of 10.6 cN at 230° C. Here, the compounding ratio of each radical polymerization initiator in the mixture of radical polymerization initiators (t-butylperoxyisopropyl monocarbonate:2,2-di(t-butylperoxy)butane) was 1:2.

[0075] <Extrusion foaming machine> In the following examples and comparative examples, an extrusion foaming device used for producing polypropylene-based resin extruded foam particles was a device in which a melt kneading section, a cooling section, a transport section, a diverter valve, and a granulation section were connected in series. As the melt kneading section, a twin-screw extruder was used, which had two screws, a raw material supply section at one end, and a foaming agent supply section in the middle of the screws. As the cooling section, a static mixer was used. The granulation section had a die with six holes with a hole diameter of 0.8 mm.

[0076] Example 1 A resin mixture was prepared by blending 100 parts by weight of a polypropylene resin having a branched structure (branched polypropylene resin) and 0.2 parts by weight of talc as a bubble nucleating agent. The resin mixture was then mixed with a 100-mm-diameter olefin resin having a screw diameter D of 40 mm, a ratio of the effective length L of the screw to the diameter D (L / D) of 30, a cylinder temperature of 195°C, and a screw rotation speed of 150 rpm (shear rate of 49.9 s -1 The resin mixture was fed to a twin-screw extruder (1000-mm2) at a rate of 90 kg / h. During the melt-kneading, only carbon dioxide gas as a foaming agent was injected into the twin-screw extruder from the foaming agent feed section, and the resulting composition was further melt-kneaded. The amount of foaming agent fed to the twin-screw extruder was 2.5 parts by weight. The temperature of the resin composition at the final part of the melt-kneading section was 197°C.

[0077] The melt-kneaded composition was passed through the cooling section, the transport section, the diverter valve, and the die of the granulation section, and discharged into a region filled with water as a liquid phase at a pressure lower than the internal pressure of the extrusion foaming machine. The water pressure was 0.2 MPa. The extruded composition was chopped with a cutter in the region filled with water (liquid phase) to obtain spherical or nearly spherical extruded polypropylene resin beads. The time from when 10 kg of the resin mixture was supplied to the extrusion foaming machine until 10 kg of the foamed beads were discharged from the die was measured, and it was found that the average residence time was 24.0 seconds. The obtained extruded polypropylene resin beads were collected by subjecting them to a centrifugal dehydrator. The obtained extruded polypropylene resin beads were resin-returned, and the MFR of the obtained resin mass was measured by the method described above. The MFR is shown in Table 1.

[0078] [Table 1] Example 2 Screw speed: 206 rpm (shear rate: 68.5 s -1 ) Extruded foam particles were produced in the same manner as in Example 1, except that the above-mentioned step was changed to the above-mentioned step.

[0079] Comparative Example 1 Screw speed: 350 rpm (shear rate: 116.3 s -1 Extruded foam particles were produced in the same manner as in Example 1, except that the above-mentioned step was changed to the above-mentioned step.

[0080] Comparative Example 2 The screw diameter D was 25 mm, the ratio of the effective length L of the screw to the diameter D (L / D) was 30, the cylinder temperature was 195°C, and the screw rotation speed was 101 rpm (shear rate 61.5 s -1 The resin mixture was fed to a twin-screw extruder of 1000 mm diameter (1.0 mm) at a rate of 8.4 kg / h. Except for this, the extruded foam particles were produced in the same manner as in Example 1.

[0081] Comparative Example 3 The screw speed was set at 120 rpm (shear rate 35.4 s -1Extruded foam beads were produced in the same manner as in Comparative Example 2, except that the feed rate of the resin mixture was changed to 10.0 kg / h.

[0082] Example 3 Screw speed: 220 rpm (shear rate: 64.9 s -1 Extruded foam beads were produced in the same manner as in Comparative Example 2, except that the feed rate of the resin mixture was changed to 25.0 kg / h.

[0083] Example 4 Screw speed: 300 rpm (shear rate: 88.5 s -1 Extruded foam beads were produced in the same manner as in Comparative Example 2, except that the feed rate of the resin mixture was changed to 25.0 kg / h.

Claims

1. A method for producing extruded foamed polypropylene-based resin particles, comprising: a melt-kneading step of melt-kneading a polypropylene-based resin having a branched structure and a foaming agent in a production apparatus equipped with a melt-kneading section having a plurality of screws and a granulation section having a die to obtain a resin composition; and an extrusion foaming step of discharging the resin composition obtained in the melt-kneading step through the die into a region having a lower pressure than the internal pressure of the production apparatus, wherein the temperature of the resin composition in the final part of the melt-kneading section is equal to or lower than the melting point of the polypropylene-based resin having a branched structure + 65°C, and the residence time of the polypropylene-based resin having a branched structure in the production apparatus is 40 seconds or less.

2. The shear rate of the screw is 100 s ―1 The method for producing extruded polypropylene resin foam beads according to claim 1, wherein the extruded polypropylene resin foam beads are:

3. The method for producing extruded polypropylene resin foam particles according to claim 1 or 2, wherein the number of parts of the foaming agent is 1.0 to 5.0 parts by weight based on 100 parts by weight of the polypropylene resin having a branched structure.

4. The blowing agent is CO 2 3. The method for producing extruded polypropylene resin foam particles according to claim 1, wherein the gas is at least one selected from the group consisting of propane, butane, pentane and nitrogen.

5. 3. The method for producing extruded polypropylene resin foam beads according to claim 1, wherein the branched polypropylene resin has a melt strength of 2.0 cN or more.

6. 3. The method for producing extruded polypropylene resin foam beads according to claim 1, wherein the extruded polypropylene resin foam beads have a melt flow rate of 4.5 g / 10 min or less at 230°C.

7. A method for producing a polypropylene resin foamed article, which comprises molding the extruded polypropylene resin beads obtained according to claim 1 or 2.

Citation Information

Patent Citations

  • Extruded foam particles and method for producing same

    WO2022050375A1

  • Method for producing polypropylene-based resin having branched structure, method for producing extrusion-foamed particles, and method for producing foamed molded article

    WO2022163627A1