Method for manufacturing thermoplastic resin extrusion foaming board and extruder

A two-zone molding process with cooling and lubrication in the extrusion foaming method addresses mold clogging and surface issues, enabling stable production of large cross-sectional area foams with good surface properties using small extruders.

JP2024142609APending Publication Date: 2024-10-11KANEKA CORP
View PDF 2 Cites 0 Cited by

Patent Information

Application Number
JP2023054819
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Filing Date
2023-03-30
Publication Date
2024-10-11

AI Technical Summary

Technical Problem

Existing extrusion foaming methods face issues with porous mold walls becoming clogged, leading to poor surface properties and increased frictional resistance, especially when producing thick plate-shaped foams with small-sized extruders, resulting in unstable production processes.

Method used

A method involving a two-zone molding process with a cooling block in the first zone and a lubricating medium injection in the second zone, where the foam surface is cooled and lubricated to improve slipperiness, allowing stable production of large cross-sectional area foams with good surface properties using a small-sized extruder.

Benefits of technology

The method enables the stable production of board-like extruded foams with large cross-sectional areas and improved surface properties, even with small extruders, by reducing friction and preventing mold clogging.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024142609000001_ABST
    Figure 2024142609000001_ABST
Patent Text Reader

Abstract

To provide a method for manufacturing a thermoplastic resin extrusion foaming board that can easily and stably obtain a board-like extruded foam with a large cross-sectional area having a satisfactory surface property.SOLUTION: A method for manufacturing a thermoplastic resin extrusion foaming board performs molding by extruding and foaming a foamable thermoplastic resin composition melted and kneaded in an extruder from a die 11 into a molding die. The molding die includes: a first molding zone 2 having a cooling block 21 which can be cooled by a cooling medium; and a second molding zone 3 having a lubrication medium injection mechanism and located downstream of the first molding zone 2. The method for manufacturing a thermoplastic resin extrusion foaming board comprises steps of: cooling a surface of the foam while foaming the foamable thermoplastic resin composition extruded from the die 11 in the first molding zone 2; and moving the foam so that a lubrication medium is placed on a contact surface of an inner wall surface in the second molding zone 3 in the foam which has passed through the first molding zone 2 in the second molding zone 3.SELECTED DRAWING: Figure 1
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a method for producing a thermoplastic resin foam, and more particularly to a method for producing a plate-shaped thermoplastic resin foam having a desired cross section by extrusion foaming. [Background technology]

[0002] Thermoplastic resin foams are widely used as industrial products with excellent heat insulation and shock-absorbing properties. The most widely used manufacturing method is the extrusion foaming method, in which a thermoplastic resin containing a foaming agent is extruded from an extruder to produce a foam.

[0003] Furthermore, in order to produce a thick, plate-like foam of a desired shape by extrusion foaming, a molding die is attached to the tip of a nozzle at the tip of an extruder, and the extrudate is foamed in this molding die and extruded into the desired shape. There have been various attempts to obtain thick foams by modifying such molding dies. Patent documents 1 and 2 propose a method in which the walls of the molding die are made of porous plates through which water or air can be allowed to flow and used as a lubricant when the extrudate moves within the die, thereby obtaining thick, plate-like foams with good surface properties. [Prior art documents] [Patent documents]

[0004] [Patent Document 1] Japanese Patent Application Publication No. 10-44220 [Patent Document 2] Japanese Patent Application Publication No. 10-67043 Summary of the Invention [Problem to be solved by the invention]

[0005] However, in the extrusion foaming method, the porous plate on the wall of the mold may become clogged, making it impossible for the fluid to flow out. In that case, the extrudate comes into contact with the surface of the porous plate, resulting in extremely poor surface properties. Even if clogging does not occur, it is difficult for the entire surface of the foam to come into uniform contact with the surface of the porous plate, and the foam comes into strong contact with the porous surface locally, which increases the frictional resistance between the foam and the surface of the porous plate, and tends to deteriorate the surface properties of the foam. In particular, when the foam is strongly pressed into the mold by slowing down the take-up speed, for example, to obtain a plate-shaped foam with a large cross-sectional area using a small-sized extruder, that is, when a strong back pressure is applied to mold the foam, the tendency for the surface properties of the foam to deteriorate and the porous plate to become clogged becomes significant.

[0006] SUMMARY OF THE PRESENT EMBODIMENT An object of the present invention is to easily and stably produce a board-shaped extruded foam having a large cross-sectional area and good surface properties, even when a small-sized extruder is used. [Means for solving the problem]

[0007] As a result of intensive research in light of the above problems, the inventors discovered that by undergoing a specific molding process, the slipperiness of the foam surface can be improved, and that even when molding is performed under strong back pressure, a foam can be obtained without deterioration of the surface properties, thereby arriving at the present invention.

[0008] That is, the present invention is a method for producing an extruded thermoplastic resin foam board, which comprises extruding and foaming a foamable thermoplastic resin composition obtained by melt-kneading in an extruder through a die into a molding die, the molding die being: 1) a first forming zone having a cooling block that can be cooled by a cooling medium; and 2) a second forming zone downstream of the first forming zone, the second forming zone having a lubricant injection mechanism; and a step of cooling a surface of the foam while foaming the foamable thermoplastic resin composition extruded from the die in the first molding zone, and a step of moving the foam in the second molding zone so that a lubricating medium is present on a contact surface of the foam that has passed through the first molding zone with an inner wall surface of the second molding zone. In the present invention, the temperature of the cooling medium is preferably 3°C to 80°C. In the present invention, the lubricating medium is preferably a liquid. In the present invention, the lubricant injection mechanism is preferably disposed upstream of the second forming zone. In the present invention, the forming coefficient α represented by the following formula (1) is preferably 0.12 or more. Forming coefficient α=A F / (A Ex ×(Expansion ratio) (2 / 3) )...Equation (1) (In the above formula (1), A F is the cross-sectional area (m 2 ) and A Ex is the cross-sectional area of ​​the barrel of the extruder (m 2 ) and (Expansion Ratio) indicates the expansion ratio of the thermoplastic resin extruded foam board. In the present invention, it is preferable that the speed at which the foam passes through the outlet of the molding die (foam speed V) satisfies the following formula (2). Foam speed V (m / min) ≦ [foam discharge volume / 60] / (0.12×A Ex ×(Expansion ratio) (2 / 3) )...Equation (2) (In the above formula (2), the foam discharge volume (m 3 / time) is calculated by the following formula (3); Foam discharge volume (m 3 / hour) = discharge amount (kg / hour) / resin density (kg / m 3 ) × foaming ratio (times) ··· Equation (3), A Ex is the cross-sectional area of ​​the barrel of the extruder (m 2) and (Expansion Ratio) indicates the expansion ratio of the thermoplastic resin extruded foam board. In the present invention, the foamable thermoplastic resin composition preferably contains a thermoplastic resin, a foaming agent, and a moldability improver. In the present invention, the thermoplastic resin is preferably a polyolefin resin. In the present invention, the polyolefin resin is preferably a polyethylene resin. In the present invention, the extruded thermoplastic resin foam board preferably has an expansion ratio of 5 to 30, an average cell diameter of 100 to 600 μm, a closed cell ratio of 70% or more, and a thickness of 20 mm or more. The present invention also provides an extruder for a thermoplastic resin extrusion foam board having a molding die, comprising: The molding die is 1) a first forming zone having a cooling block that can be cooled by a cooling medium; and 2) a second forming zone downstream of the first forming zone, the second forming zone having a lubricant injection mechanism; In the first molding zone, the foamable thermoplastic resin composition extruded from the die is foamed while cooling the foam surface; In the second molding zone, the foam is moved so that a lubricating medium is present on a contact surface of the foam that has passed through the first molding zone with an inner wall surface of the second molding zone. This invention relates to an extruder for thermoplastic resin extruded foam board. Effect of the Invention

[0009] According to the present invention, even when a small-sized extruder is used, it is possible to easily and stably obtain a board-shaped extruded foam having a large cross-sectional area and good surface properties. [Brief description of the drawings]

[0010] [Figure 1] FIG. 2 is a longitudinal sectional view of a portion of the device used in the examples and comparative examples of the present specification. [Diagram 2]2 is a cross-sectional view taken along line AA in FIG. 1. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0011] The manufacturing method of the present invention is a method for forming an extruded thermoplastic resin foam board by extruding and foaming a molten foamable thermoplastic resin into a molding die, and the molding die includes: 1) a first molding zone having a cooling block capable of being cooled by a refrigerant or the like; 2) A second forming zone located downstream of the first forming zone. Using a molding die having a step of foaming the foamable thermoplastic resin composition extruded from the die in the first molding zone while cooling the foam surface; a step of moving the foam in the second molding zone so that a lubricating medium is present on the contact surface of the foam that has passed through the first molding zone with the inner wall surface of the second molding zone; That is, in the first molding zone, a foamable thermoplastic resin in a molten state is extruded from a die of an extruder to be foamed, and the foam surface is cooled while being introduced into the second molding zone, and the foam is molded by moving the foam surface cooled in the first molding zone with a lubricating medium interposed between the foam surface and the inner wall surface of the second molding zone.

[0012] The foam in the present invention includes not only foams in a state in which foaming and molding have been completed, but also foams in the middle of foaming extruded from an extruder, i.e., foams in the process of becoming a board-like foam.

[0013] A representative example of the manufacturing method of the present invention will be described with reference to the drawings. FIG. 1 of the attached drawings is a vertical cross-sectional view of an apparatus used in the Examples and Comparative Examples of the present specification according to one embodiment of the present invention, and FIG. 2 is a cross-sectional view taken along the line A-A' in FIG. 1. A rectangular die 11 is connected to the tip (downstream end) of an extruder (not shown) and is provided with a die opening 12 therein. The opening is used to release the molten resin containing a foaming agent under atmospheric pressure, thereby initiating foaming. A first molding zone 2 and a second molding zone 3 of a molding die are connected to the tip of the rectangular die 11.

[0014] The first molding zone 2 is a zone in which the foam is allowed to grow large, and has a shape in which the cross-sectional thickness and cross-sectional width of the foam flow path 23 are greatly increased. In the present invention, it is important to greatly expand the cross section of the foam in the first molding zone 2 and to solidify the foam surface to some extent to form a surface layer that can withstand friction with the mold. For this reason, the first molding zone according to this embodiment is provided with a cooling block 21 that can be cooled by a cooling medium.

[0015] The cooling block 21 preferably has the refrigerant passages 22 at least on the upper and lower surfaces of the foam passage 23. This makes it possible to cool the surface in contact with the foam. Furthermore, the side blocks 24 located on the sides of the foam flow path 23 do not need to have a cooling mechanism, but in order to obtain a foam with a beautiful surface, it is preferable that they have a cooling mechanism. The side blocks 24 may be disposed as necessary.

[0016] There are no particular limitations on the cooling block 21 other than that it must have the ability to cool the foam surface it comes into contact with, but it is preferable that it has the ability to adjust the temperature of the foam contact surface by passing a cooling medium through it. The temperature of the cooling medium is preferably 3°C to 80°C. If the temperature is lower than 3°C, the foam surface in contact with the cooling medium will be strongly solidified and will not expand easily, making it difficult to obtain a large cross-sectional area. On the other hand, if the temperature is higher than 80°C, the surface cooling effect is likely to be insufficient, and the foam surface may be torn off or wrinkles may occur due to increased frictional resistance, which may deteriorate the surface condition of the foam. The lower limit of the cooling medium temperature is preferably 5°C, and more preferably 10°C. The upper limit of the cooling medium temperature is preferably 60°C, and more preferably 40°C.

[0017] The surface of the cooling block 21 that comes into contact with the foam is preferably uniformly smooth in order to prevent scratches on the surface of the foam. Uniformly smooth means that the surface has a substantially uniform flat surface with substantially no small holes. The surface that comes into contact with the foam may be coated with a coating such as a fluorine coating to impart sliding properties.

[0018] The configuration and shape of the cooling block 21 may be appropriately adjusted depending on the foaming ratio, cross-sectional area, and surface properties of the target foam. For example, in Fig. 1, the cooling block 21 has an inclined portion and a parallel portion, but it may have only an inclined portion or only a parallel portion.

[0019] It is preferable that at least the initial stage of foaming (the left side in FIG. 1, the rectangular die 11 side) has an inclined portion, and it is more preferable that the region following the inclined portion has a parallel portion.

[0020] The angle of the inclined portion may be one step, or may be configured to vary stepwise.

[0021] Moreover, it is preferable that the connecting portion where the angle changes and the connecting portion with the parallel portion have an arc shape in order to reduce the change.

[0022] The initial rise angle of the cooling block 21 is preferably 10 degrees to 80 degrees, more preferably 20 degrees to 70 degrees, and more preferably 30 degrees to 60 degrees. If the angle is less than 10 degrees, it is difficult to ensure contact between the foam and the mold in that section, and the cooling effect on the surface may be weakened. If the angle is 80 degrees or more, the initial growth of the foam in the thickness direction may be more than necessary hindered, making it difficult to increase the thickness of the final foam.

[0023] In the first molding zone, it is preferable that no lubricating medium is present on the contact surface with the foam. In the first molding zone, the foam, whose surface is still soft immediately after being extruded from the rectangular die 11, expands while being in contact with the die. Therefore, by not having a lubricating medium present, it becomes easy to make the entire foam surface uniformly contact the inner wall surface of the molding die, which is effective in forming a uniform surface layer that can withstand friction with the die contact surface. In particular, when the foam is stored inside the molding die and molded, if a lubricating medium is present in the first molding zone, it becomes difficult for the soft foam surface immediately after extrusion to uniformly contact the molding die, and therefore unevenness in the surface quality of the foam is likely to occur.

[0024] There is no particular restriction on the length of the first molding zone, but it is preferably 20 mm to 100 mm, with a lower limit of 30 mm, and more preferably 40 mm. The upper limit of the length is preferably 80 mm, and more preferably 70 mm. If the lower limit is less than 20 mm, it may be difficult to obtain the desired surface cooling effect, and if the upper limit is 100 mm or more, cooling may proceed too much, making it difficult to obtain a sufficient cross-sectional area of ​​the foam.

[0025] The second molding zone is a zone in which the shape of the foam is adjusted. This zone is also a zone in which a large frictional force occurs because the contact area between the foam and the molding die is large. Therefore, in the present invention, it is important to adjust the shape of the foam while interposing a lubricant between the inner wall surface of the second molding zone and the contact surface of the foam.

[0026] The location of the lubricant injection mechanism for injecting the lubricant may be after the first molding zone, but is preferably at the entrance side of the second molding zone where the resistance between the foam and the molding die becomes particularly large.

[0027] The method of injecting the lubricant involves providing a flow path that allows the lubricant to flow at least across the entire or partial width of the top and bottom surfaces, and injecting the lubricant from the lubricant inlet pipe 31 through the flow path to the foam flow path 33. The lubricant pipe 31 may be a structure in which a single pipe is connected to the mold, or a flow path (hole) that is connected to the outside may be directly provided in the mold. The presence of the lubricant on the foam flow path surface in this way can provide a sliding effect on the surface of the foam even if it comes into strong contact with the foam, making it possible to stabilize the process.

[0028] It is preferable to inject the lubricating medium uniformly across the entire width of the flow path, for example by utilizing small gaps between the joining surfaces of the parts that make up the mold. However, partial injection through small holes, for example, can also be effective.

[0029] When small holes are used, the hole diameter is preferably 2 mm or less, and the interval between the small holes (arrangement pitch) is preferably 70 mm or less. The hole diameter is preferably 1.5 mm or less, more preferably 1.0 mm or less, and the arrangement pitch is preferably 50 mm or less, even more preferably 30 mm or less. If the hole diameter exceeds 2 mm, the small holes tend to be easily clogged with foam, and if the arrangement pitch exceeds 70 mm, the uniformity of the lubricating medium tends to be easily lost. There are no particular restrictions on the lower limits of the hole diameter and the arrangement pitch, but in order to avoid problems such as the small holes being blocked, the hole diameter is preferably 0.1 mm or more, and the arrangement pitch is preferably 5 mm or more in terms of the effort required for processing and the strength of the mold.

[0030] In the present invention, the surface of the foam is cooled in the first molding zone, and the foam moves to the second molding zone while the surface has a certain degree of hardness. If the surface of the foam is soft and uneven, the lubricating medium may accumulate in one area, and its effect may be halved. However, if the surface of the foam has a certain degree of hardness and smoothness, even a small amount of the lubricating medium can be arranged in a uniform thin film, and it is believed that the lubricating effect can be fully exerted.

[0031] There are no particular restrictions on the material of the molding block 32 that constitutes the second molding zone as long as it does not adversely affect the sliding of the foam, but preferred materials include metal with a surface finish and a coating that imparts sliding properties, such as a fluorine coating, or polytetrafluoroethylene (PTFE).

[0032] The molding block 32 may be provided with a cooling mechanism using a cooling medium or the like similar to that of the cooling block 21 in order to further cool the surface of the foam.

[0033] As the fluid to be injected as the lubricating medium, various types of gases and liquids can be used.

[0034] The gas that can be used may be air, dry air, nitrogen, or the like.

[0035] As the liquid, water, water vapor, polyethylene glycol, paraffins, oils, etc. can be used. Note that water vapor is defined as a liquid in this application because it is quickly liquefied after injection into the mold and acts substantially as a liquid. Among these, the use of water and water vapor is preferred because they are inexpensive and safe, and can provide even greater lubricity when used in combination with additives such as moldability improvers.

[0036] The temperature, flow rate, etc. of each fluid can be appropriately adjusted according to the foam quality such as the surface condition, thickness, width, and cross-sectional cell state of the foam. When the foam surface is insufficiently cooled, and the foam surface is torn off, or the frictional resistance increases and wrinkles are generated, and the surface condition of the foam tends to deteriorate, it is possible to adjust the temperature lower, increase the flow rate, etc. to promote the cooling of the foam surface. On the other hand, when the lubricity in the mold is sufficient and the surface skin layer is too thick, making it difficult to obtain the width dimension, it is possible to adjust the temperature higher, decrease the flow rate, etc. to suppress the cooling of the foam surface. Specifically, the temperature of the fluid used is preferably 5 to 120°C, more preferably 7 to 110°C, and more preferably 10 to 100°C. In addition, the flow rate is preferably 30 to 500 mL / min, more preferably 50 to 400 mL / min, and more preferably 80 to 300 mL / min on the upper and lower surfaces of the mold. A mold for adjusting the shape and size may be further used downstream of the second molding zone of the present invention, and a cooling mechanism may be provided for these.

[0037] The thermoplastic resin used in this embodiment may be a polyolefin resin such as polyethylene or polypropylene, a styrene resin such as polystyrene, a polyester resin such as polyethylene terephthalate, or a polyvinyl halide resin such as polyvinyl chloride, either alone or as a mixture of two or more kinds. Since the surface of the foam of polyolefin resin before cooling and solidifying is soft and easily damaged, the effect of the manufacturing method of the present invention is outstanding. In particular, it is effective when molding a polyethylene non-crosslinked extruded foam board using a more flexible polyethylene resin.

[0038] The polyethylene resin of the present invention can be any resin generally used for foams, and examples thereof include resins containing 50 mol% or more of ethylene component units, such as high-density polyethylene, low-density polyethylene, linear low-density polyethylene, ethylene-vinyl acetate copolymer, ethylene-propylene copolymer, ethylene-propylene-butene-1 copolymer, ethylene-butene-1 copolymer, ethylene-hexene-1 copolymer, ethylene-4-methylpentene-1 copolymer, and ethylene-octene-1 copolymer. These polyethylene resins can be used alone or as a mixture of two or more kinds, or two or more kinds of the same resin type with different densities can be mixed and used. Among them, it is preferable to use 60 wt% or more of low-density polyethylene, which has good foamability. Examples of mixtures of two or more kinds of polyethylene resins include a mixture of low-density polyethylene and linear low-density polyethylene.

[0039] The blowing agents used in this embodiment include physical blowing agents such as hydrocarbons such as propane, butane, isobutane, and pentane, chlorinated hydrocarbons such as methyl chloride and ethyl chloride, lower alcohols such as methanol, ethanol, and propanol, ethers such as ethyl ether and dimethyl ether, and inorganic gases such as nitrogen, carbon dioxide, air, argon, and water, and chemical blowing agents such as sodium bicarbonate, azodicarbonamide, and dinitrosopentamethylenetetramine, which may be used alone or as a mixed gas. These blowing agents may be mixed in an amount of 0.01 to 50 parts by weight based on 100 parts by weight of the thermoplastic resin.

[0040] In this embodiment, it is preferable to use a moldability improver in order to improve the lubricity of the foam in the molding die. As the moldability improver, any one that is mixed with the thermoplastic resin in the extruder and has the effect of reducing the frictional resistance with the molding die during foaming can be used. Specifically, metal soaps such as calcium stearate, magnesium stearate, and zinc stearate; fatty acid esters such as stearic acid monoglyceride and stearyl stearylate; fatty acid amides such as stearic acid amide and methylene bisstearic acid amide; hydrocarbons such as polyethylene wax and paraffin; higher alcohols such as stearyl alcohol, higher fatty acids such as stearic acid, etc. can be mentioned. The amount of these moldability improvers to be added may be adjusted as necessary, but from the perspective of the balance between the lubricity with the molding die and the foamability, it is preferably 0.1 to 3 parts by weight, and more preferably 0.3 to 2 parts by weight, per 100 parts by weight of the thermoplastic resin.

[0041] In the present embodiment, in addition to the thermoplastic resin, the moldability improver, and the foaming agent, additives such as a bubble-forming nucleating agent, a flame retardant, a stabilizer, a lubricant, a plasticizer, a pigment, a dye, and an antistatic agent may be appropriately used in the foamable thermoplastic resin composition.

[0042] The dimensions of the extruded thermoplastic resin foam board (foamed plate) produced by the present invention can be varied depending on the capacity of the extruder and the shape of the die, but the production method of the present invention is characterized in that it is easy to produce a foamed plate having a large cross-sectional area even with a small-sized extruder, which was difficult to do with conventional methods. The cross-sectional area here refers to the product of the dimensions in the foam thickness direction and width direction at a surface of the foamed plate cut at a plane perpendicular to the extrusion direction.

[0043] To obtain a plate-shaped foam with a large cross-sectional area, it is necessary to accumulate a large amount of foam inside the molding die by controlling the production speed of the foam (the speed at which it passes through the molding die outlet) to a slow speed using a take-off machine or the like located downstream of the molding die. However, if this "accumulation" is strengthened, the resistance of the molding die surface increases, and the foam surface may peel off, or in severe cases, the foam may get clogged inside the die, making it difficult to perform stable extrusion.

[0044] The present invention is an effective method for obtaining a foam plate having a large cross-sectional area relative to the size of the extruder.

[0045] Specifically, the extruder can be suitably used to produce a foam having a molding coefficient α of 0.12 or more, as calculated by the following formula (1). Furthermore, the extruder can be more suitably used in the present invention when the molding coefficient α is 0.14 or more, particularly 0.16 or more. Note that a molding coefficient α of 0.12 or more means that a plate-shaped foam having a large cross-sectional area is formed relative to the size of the extruder.

[0046] Forming factor α = A F / (A Ex ×(Expansion ratio) (2 / 3) )...Equation (1) (In the above formula (1), A F is the cross-sectional area of ​​the thermoplastic resin extruded foam board (m 2 ), A Ex is the cross-sectional area of ​​the extruder barrel (m 2 ), (Expansion ratio) indicates the expansion ratio of the thermoplastic resin extruded foam board. In order to obtain a plate-shaped foam having a large cross-sectional area and good surface properties even with a small extruder size, the speed at which the foam passes through the molding die outlet (foam speed V) may be set to satisfy the following formula (2). Here, the constant 0.12 on the right side of formula (2) corresponds to the molding coefficient α in formula (1), and may be set to a larger value in order to increase the cross section of the foam. When the foam speed V is small, molding with strong "accumulation" occurs, and the resistance of the foam to the molding die becomes strong, so that burrs and scratches are likely to occur on the surface. However, according to the present invention, even when the foam speed is slowed, it is possible to obtain a foam with good surface properties (burrs and scratches on the surface are suppressed). Note that molding with strong "accumulation" refers to controlling the foam speed to a low speed using a take-up machine or the like arranged downstream of the molding die, so that the foam is more firmly accumulated inside the molding die. Foam speed V (m / min) ≦ Foam discharge volume / 60 / (0.12 × A Ex ×(Expansion ratio) (2 / 3) )...Equation (2) In the above formula (2), A Ex is the cross-sectional area of ​​the extruder barrel (m 2 ) and foam discharge volume (m 3 / time) is calculated using the following formula (3). Foam discharge volume (m 3 / hour) = discharge amount (kg / hour) / resin density (kg / m 3 ) × foaming ratio (times) Formula (3) The (expansion ratio) in the above formulas (2) and (3) represents the expansion ratio of the extruded thermoplastic resin foam board.

[0047] Furthermore, the method of the present invention can be suitably used to produce a foamed plate having a fine average cell diameter. Foamed plates having a fine average cell diameter have thin cell membranes that tend to tear off when the surface layer comes into contact with a molding die with a small resistance, but the method of the present invention makes it possible to easily produce a foamed plate having a large cross-sectional area without causing such problems.

[0048] The thermoplastic resin extruded foam board obtained by the manufacturing method according to this embodiment has an expansion ratio of preferably 5 to 30, and more preferably 6 to 25, from the viewpoint of easily achieving a balance of strength that affects processability and workability, as well as exhibiting light weight, cushioning properties, and heat insulation properties that are characteristic of foams.

[0049] The thermoplastic resin extruded foam board obtained by the manufacturing method according to this embodiment preferably has an average bubble diameter of 100 μm or more and 600 μm or less, and more preferably 120 μm or more and 500 μm or less, from the viewpoints of appearance, cushioning properties, heat insulation properties, product protection properties when used as a cushioning material, and the like.

[0050] The extruded thermoplastic resin foam board obtained by the manufacturing method according to the present embodiment preferably has a closed cell ratio of 70% or more, more preferably 75% or more, from the viewpoints of cushioning properties, heat insulation properties, etc. The upper limit of the closed cell ratio is preferably 100%.

[0051] The extruded thermoplastic resin foam board obtained by the manufacturing method according to the present embodiment has a thickness of preferably 20 mm or more, more preferably 30 mm or more, from the viewpoint of easy application to heat insulating materials and cushioning materials. There is no particular upper limit on the thickness, but from the viewpoint of the difficulty in ensuring the thickness by extrusion foaming, it is usually 150 mm or less.

[0052] The extruder used in the present invention can be any known extruder used for thermoplastic resins, but it is necessary that the resin and foaming agent can be mixed and cooled to a temperature suitable for foaming. Examples of the extruder include kneading and cooling devices such as single-screw extruders, twin-screw extruders, cooling mixers, and static mixers, or devices that are connected in multiple stages, which can heat the polymer material to an appropriate temperature and knead it while applying an appropriate shear stress under pressure, but are not limited to these.

[0053] In the present invention, a device capable of adjusting the foam speed V by sandwiching the foam from above and below or from the left and right can be used. The part for sandwiching the foam can be in the form of a roll or belt. EXAMPLES

[0054] The present invention will be described in more detail below with reference to examples, but the present invention is not limited to these examples.

[0055] In the examples and comparative examples, the test methods and judgment criteria used for various evaluations are as follows.

[0056] <Closed bubble rate> A test piece having a width of 20 mm, a thickness of 20 mm, and a length of 30 mm was prepared from each foam obtained in the Examples and Comparative Examples. The volume Vc (cm) of the test piece was measured using an air pycnometer (Tokyo Science Co., Ltd., air comparison specific gravity meter Model 1000) in accordance with the method described in ASTM D2856. 3 Next, the same test piece after the measurement was submerged in a measuring cylinder containing ethanol, and the apparent volume Va (cm 3 ) was measured, and the closed cell ratio (%) was calculated according to the following formula. Closed cell rate (%) = (Vc / Va) x 100 The measurement was carried out for three test pieces, and the average value was regarded as the closed cell ratio of the foam.

[0057] <Foam density> The weight W (g) of the test piece used in the measurement of the closed cell ratio and the volume Va (cm) obtained by the above-mentioned submersion method 3 ) was calculated using the following formula: Foam density (g / cm 3 )=W / Va.

[0058] <Expansion ratio> The foam density (g / cm 3 ) and resin density (g / cm 3 ) was calculated using the following formula:

[0059] Expansion ratio (times) = resin density / foam density.

[0060] <Average bubble diameter> The foams obtained in the examples and comparative examples were cut into 3 arbitrary cross sections perpendicular to the extrusion direction at a length of 20 mm in the extrusion direction to prepare sample A. Furthermore, cubic sample B with sides of 5 to 10 mm was cut out from sample A at the following measurement points. Each observation surface (thickness direction, width direction, extrusion direction) of sample B was cut with a double-edged razor [Feather, high stainless double-edged] with great care not to destroy the bubble membrane (cell membrane), and the cut surface was observed with a microscope [Keyence, VHX-900]. In the obtained image, a line segment with a length of 4000 μm was drawn, the number of bubbles n through which the line segment passed was measured, and the bubble diameter was calculated by the following formula. Bubble diameter (μm) = 4000 / n This measurement was carried out at each measurement point in the thickness direction, width direction and extrusion direction, and the arithmetic mean value of these values ​​was taken as the average cell diameter (μm). *) Measurement locations: The average cell diameter was measured at the following five points on each of three random cross sections perpendicular to the extrusion direction of the foam. Center (measurement point 1) - Center and midway between both ends in the width direction (measurement points 2 and 3) - Center and midway between the top and bottom ends in the thickness direction (measurement points 4 and 5).

[0061] <Foam cross-sectional area A F > A F was calculated by multiplying the foam thickness and width dimensions described below.

[0062] 1) Foam thickness The thickness was measured at three randomly selected cross sections of a 1m long foam sample at the following positions. The average value of the nine positions was recorded as the thickness. ·Center in width direction (measurement point 1) 25mm inward from both ends in the width direction (measurement points 2 and 3) 2) Foam width dimension The width of the foam sample, 1 m in length, was measured at 5 random positions at 200 mm intervals, and the average value was taken as the width dimension.

[0063] <Forming coefficient α> The molding coefficient α was calculated as a measure of the strength of molding (degree of pressing into the die) by the following formula 1). Forming factor α = A F / (A Ex ×(Expansion ratio) (2 / 3) )...Equation 1) Foam cross-sectional area A F (m 2 ): Value calculated using the method described above Extruder barrel cross-sectional area A Ex (m 2 ): Cross-sectional area of ​​the barrel of the last extruder used Expansion ratio: Value calculated by the method described above.

[0064] <Moldability> The surface properties and extrusion state of the foam were evaluated according to the following criteria. A: Beautiful surface B: Small wrinkles can be seen here and there. C: Small wrinkles are visible throughout D: The surface quality of the foam is uneven, such as scratches on the surface, or clogging occurs in the mold.

[0065] Example 1 Low-density polyethylene (Ube Maruzen Polyethylene "C470", MFR 2.0g / 10min, density 918kg / m 3100 parts by weight of the mixture was mixed with 3.0 parts by weight of a chemical foaming agent (EE275F, manufactured by Eiwa Kasei, sodium bicarbonate-citric acid-based thermal decomposition type foaming agent master batch) as a bubble nucleating agent and 1.0 parts by weight of monoglyceride stearic acid as a moldability improver, and the mixture was fed to a Φ40 twin-screw-Φ90mm single-screw tandem extruder. After melting in the first extruder (Φ40 twin-screw) set at 230°C, 3.5 parts by weight of isobutane as a foaming agent was injected and mixed, cooled in the second extruder (Φ90mm) set at 97°C, and then extruded at a discharge rate of 50 kg / hour under atmospheric pressure from a rectangular die (opening 50mm x 4mm) connected to the tip of the extruder. The molding dies shown in Figures 1 and 2 were used. The first molding zone used a metal block through which cooling water could pass (15°C water passed, surface fluorine coating), and the second molding zone used a PTFE block. Steam was also introduced from the lubricant inlet pipe, and the steam was introduced into the foam flow path through the gap between the metal block and the PTFE block. The foam extruded from the die was stored in the molding die while adjusting the take-up speed with the take-up machine, and a plate-shaped foam with a large cross-sectional area was obtained without clogging in the die. The obtained plate-shaped foam had no voids, a high closed cell rate, fine cells, and good surface properties without burrs or scratches. The moldability evaluation results of the obtained plate-shaped foam are shown in Table 1.

[0066] (Examples 2 to 3) A foamed plate was obtained in the same manner as in Example 1, except that the formulation was adjusted as shown in Table 1 and the take-up speed was changed. The moldability evaluation results of the obtained foamed plate are shown in Table 1.

[0067] Example 4 Except for changing the material of the second molding zone to a fluorine-coated metal block, a foam was obtained in the same manner as in Example 2. The moldability evaluation results of the obtained foam are shown in Table 1.

[0068] Example 5 A foam was obtained in the same manner as in Example 2, except that the type of second forming zone lubricant was changed to water at 15° C. The moldability evaluation results of the obtained foam are shown in Table 1.

[0069] Comparative Example 1 Except for using a PTFE block in the first molding zone, foam molding was carried out in the same manner as in Example 2. When the extruded foam was accumulated in the molding die by slowing down the take-up speed to obtain a plate-shaped foam of about 130 mm wide x 53 mm thick, the surface became ragged and the foam eventually clogged the die, making molding impossible.

[0070] Comparative Example 2 Except for not using a lubricant in the second molding zone, foam molding was carried out in the same manner as in Example 2. When the take-up speed was slowed down to obtain a plate-shaped foam of about 130 mm wide x 53 mm thick, and the extruded foam was accumulated in the molding die, the foam repeatedly stopped and advanced in short intervals, a so-called stick-and-slip phenomenon, occurred, and the process was unstable. Also, cracks and tears were found in places on the surface.

[0071] Comparative Example 3 Foam molding was carried out in the same manner as in Example 1, except that a porous block was used in the first molding zone and the second molding zone, and 85°C hot water was injected as a lubricant through the small holes in the block. When the take-up speed was slowed down to accumulate the extruded foam in the molding die, the surface was not uniform with scratches here and there, the foam sometimes tended to clog, and the process was not stable.

[0072] [Table 1] [Explanation of symbols]

[0073] 11. Rectangular Dice 12 Die opening 2. First molding zone of the mold 21 Cooling block 22... Refrigerant passage 23...Foam Channel 24 Side block 3. Second molding zone of the mold 31...Lubricating medium introduction piping 32 Molded block 33...Foam channel

Claims

1. A method for producing an extruded thermoplastic resin foam board, comprising extruding and foaming a foamable thermoplastic resin composition obtained by melt-kneading in an extruder through a die into a molding die, the method comprising the steps of: The molding die is 1) a first forming zone having a cooling block that can be cooled by a cooling medium; and 2) a second forming zone downstream of the first forming zone, the second forming zone having a lubricant injection mechanism; a step of cooling a surface of a foam in the first molding zone while foaming the foamable thermoplastic resin composition extruded from the die; a step of moving the foam in the second molding zone so that a lubricating medium is present on a contact surface of the foam that has passed through the first molding zone with an inner wall surface of the second molding zone; A method for producing a thermoplastic resin extruded foam board comprising:

2. The method for producing a thermoplastic resin extruded foam board according to claim 1, wherein the temperature of the cooling medium is 3°C to 80°C.

3. The method for producing a thermoplastic resin extruded foam board according to claim 1 or 2, wherein the lubricating medium is a liquid.

4. The lubricant injection mechanism is disposed upstream of the second forming zone. A method for producing the extruded thermoplastic resin foam board according to claim 1 or 2.

5. The method for producing an extruded thermoplastic resin foam board according to claim 1 or 2, wherein a molding coefficient α represented by the following formula (1) is 0.12 or more. Forming coefficient α = A F / (A Ex ×(Expansion ratio) (2/3) )...Formula (1) (In the above formula (1), A F is the cross-sectional area of ​​the thermoplastic resin extruded foam board (m 2 ), and A Ex is the barrel cross-sectional area of ​​the extruder (m 2 ) and (Expansion Ratio) indicates the expansion ratio of the thermoplastic resin extruded foam board.

6. 3. The method for producing an extruded thermoplastic resin foam board according to claim 1, wherein the speed at which the foam passes through the molding die outlet (foam speed V) satisfies the following formula (2): Foam speed V (m / min)≦[foam discharge volume / 60] / (0.12 x A Ex ×(Expansion ratio) (2/3) )...Formula (2) (In the above formula (2), the foam discharge volume (m 3 / time) is calculated by the following formula (3); Foam discharge volume (m 3 / hour) = discharge amount (kg / hour) / resin density (kg / m 3 ) × expansion ratio (times) ... formula (3), A Ex is the barrel cross-sectional area of ​​the extruder (m 2 ) and (Expansion Ratio) indicates the expansion ratio of the thermoplastic resin extruded foam board.

7. The method for producing an extruded thermoplastic resin foam board according to claim 1 or 2, wherein the expandable thermoplastic resin composition comprises a thermoplastic resin, a foaming agent, and a moldability improver.

8. The method for producing an extruded thermoplastic resin foam board according to claim 1 or 2, wherein the thermoplastic resin is a polyolefin-based resin.

9. The method for producing an extruded thermoplastic resin foam board according to claim 8, wherein the polyolefin-based resin is a polyethylene-based resin.

10. The thermoplastic resin extrusion foam board has an expansion ratio of 5 to 30, an average bubble diameter of 100 μm to 600 μm, a closed cell ratio of 70% or more, and a thickness of 20 mm or more.

11. An extruder for thermoplastic resin extrusion foam board having a molding die, The molding die is 1) a first forming zone having a cooling block that can be cooled by a cooling medium; and 2) a second forming zone downstream of the first forming zone, the second forming zone having a lubricant injection mechanism; In the first molding zone, the foamable thermoplastic resin composition extruded from the die is foamed while cooling the foam surface; In the second molding zone, the foam is moved so that a lubricating medium is present on a contact surface of the foam that has passed through the first molding zone with an inner wall surface of the second molding zone. Extruder for thermoplastic extruded foam board.

Citation Information

Patent Citations

  • Production of thermoplastic resin foam and mold therefor

    JP1998044220A

  • Manufacture of thermoplastic resin foam panel and mold therefor

    JP1998067043A