Sensor element and gas sensor
A peel-resistant electrode composed of noble metal and zirconia with controlled TM ratio and porosity addresses electrode peeling in gas sensors, enhancing sensor durability and measurement precision.
Patent Information
- Application Number
- JP2023055208
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Filing Date
- 2023-03-30
- Publication Date
- 2024-10-11
AI Technical Summary
Electrodes in gas sensors containing zirconia sometimes peel off from the solid electrolyte layer, leading to performance issues.
The sensor element incorporates a peel-resistant electrode made of noble metal and zirconia, with a specific TM ratio of 1 to 10 and porosity of 3% to 65%, which suppresses peeling due to stress and volume expansion during thermal transformations.
The peel-resistant electrode effectively prevents electrode separation from the solid electrolyte layer, ensuring long-term reliability and accuracy of gas concentration measurements.
Smart Images

Figure 2024142851000001_ABST
Abstract
Description
[Technical field]
[0001] The present invention relates to a sensor element and a gas sensor. [Background technology]
[0002] Conventionally, gas sensors that detect the concentration of a specific gas such as NOx in a measurement gas such as an automobile exhaust gas are known. For example, Patent Document 1 describes a gas sensor including a sensor element having an element body, a main pump cell, an auxiliary pump cell, and a measurement pump cell. The element body is provided with a measurement gas flow section that includes an oxygen ion conductive solid electrolyte layer and introduces and flows a measurement gas. The main pump cell has an inner main pump electrode disposed in a first internal space of the measurement gas flow section, and an outer main pump electrode disposed in a portion of the element body exposed to the measurement gas on the outside. The auxiliary pump cell has an inner auxiliary pump electrode disposed in a second internal space downstream of the first internal space of the measurement gas flow section, and an outer auxiliary pump electrode disposed in a portion of the element body exposed to the measurement gas on the outside. The measurement pump cell has an inner measurement electrode disposed in the measurement chamber downstream of the second internal space in the measurement gas flow section, and an outer measurement electrode disposed in a portion exposed to the measurement gas on the outside of the element body. When this sensor element is used to detect the concentration of NOx, first, the oxygen concentration of the measurement gas is adjusted in the first internal space and the second internal space by the main pump cell and the auxiliary pump cell. Then, the NOx in the measurement gas after the oxygen concentration has been adjusted is reduced in the measurement chamber. The concentration of NOx in the measurement gas is detected based on the pump current that flows when the measurement pump cell pumps out the oxygen generated by the reduction of NOx. Each electrode of each pump cell of the sensor element, such as the inner main pump electrode, is made of, for example, Pt and zirconia (ZrO 2 ) and an electrode including the same. [Prior art documents] [Patent documents]
[0003] [Patent Document 1] JP 2022-091669 A Summary of the Invention [Problem to be solved by the invention]
[0004] However, in a sensor element having an electrode containing zirconia, the electrode may peel off from the solid electrolyte layer.
[0005] The present invention has been made to solve such problems, and has as its main object to suppress peeling of an electrode from a solid electrolyte layer. [Means for solving the problem]
[0006] In order to achieve the above-mentioned main object, the present invention adopts the following means.
[0007] [1] The sensor element of the present invention comprises: A sensor element for detecting a concentration of a specific gas in a measurement gas, comprising: an element body having an oxygen ion conductive solid electrolyte layer and a measurement gas flow section for introducing and flowing the measurement gas therein; a peel-off resistant electrode disposed on the solid electrolyte layer of the element body; Equipped with The peel-off resistant electrode contains a precious metal and zirconia, and has a TM ratio (Ht / Hm) of a peak height Ht of a T phase of zirconia to a peak height Hm of an M phase of zirconia in a Raman spectrum measured using Raman spectroscopy, which is 1 or more and 10 or less, and a porosity of 3% or more and 65% or less. It is something.
[0008] In this sensor element, the peel-resistant electrode disposed on the solid electrolyte layer contains a precious metal and zirconia, the TM ratio of the zirconia in the peel-resistant electrode is 1 or more and 10 or less, and the porosity of the peel-resistant electrode is 3% or more and 65% or less. In such a peel-resistant electrode, the TM ratio of 1 or more and the porosity of 65% or less suppresses peeling of the peel-resistant electrode from the solid electrolyte layer due to stress. Furthermore, the TM ratio of the peel-resistant electrode is 10 or less and the porosity is 3% or more suppresses peeling of the peel-resistant electrode from the solid electrolyte layer due to volume expansion caused by TM transformation of the zirconia in the peel-resistant electrode. The inventors confirmed this through experiments and analysis.
[0009] [2] In the above-mentioned sensor element (the sensor element described in [1] above), the peel-resistant electrode may have a porosity of 50% or less. This makes it possible to further suppress peeling of the peel-resistant electrode from the solid electrolyte layer due to stress.
[0010] [3] In the sensor element described above (the sensor element described in [1] or [2] above), the peel-resistant electrode may have a porosity of 40% or less. This can further prevent the peel-resistant electrode from peeling off from the solid electrolyte layer due to stress.
[0011] [4] In the above-mentioned sensor element (the sensor element according to any one of [1] to [3] above), the peel-resistant electrode may have a maximum pore diameter of 5 μm or more and 17 μm or less. When the peel-resistant electrode has a maximum pore diameter of 17 μm or less, peeling of the peel-resistant electrode caused by stress can be further suppressed. When the peel-resistant electrode has a maximum pore diameter of 5 μm or more, peeling of the peel-resistant electrode caused by volume expansion due to TM transformation of zirconia can be further suppressed.
[0012] [5] In the above-mentioned sensor element (the sensor element according to any one of [1] to [4] above), the peel-resistant electrode may have a thickness of 5 μm or more and 30 μm or less. When the thickness of the peel-resistant electrode is 30 μm or less, peeling caused by volume expansion due to TM transformation of zirconia in the peel-resistant electrode can be further suppressed. When the thickness of the peel-resistant electrode is 5 μm or more, peeling caused by oxidation of the precious metal in the peel-resistant electrode can be suppressed.
[0013] [6] In the sensor element described above (the sensor element according to any one of [1] to [5] above), the peel-resistant electrode has an area of 5 mm2 as viewed in the thickness direction. 2 More than 20mm 2 The area of the peel-resistant electrode may be 20 mm or less. 2 When the area of the peel-resistant electrode is 5 mm or less, peeling caused by volume expansion due to TM transformation of zirconia in the peel-resistant electrode can be further suppressed. 2 By satisfying the above, peeling caused by oxidation of the precious metal in the peel-resistant electrode can be suppressed.
[0014] [7] The above-mentioned sensor element (the sensor element described in any one of [1] to [6]) includes a pump cell having an inner pump electrode disposed in the measurement gas flow portion and an outer pump electrode disposed in a portion of the element body exposed to the measurement gas, and at least one of the inner pump electrode and the outer pump electrode may have the peel-resistant electrode.
[0015] [8] The above-mentioned sensor element (the sensor element described in [7]) includes a main pump cell having, as the pump cell, an inner main pump electrode as the inner pump electrode arranged in a first internal space of the measured gas flow part, and an outer main pump electrode as the outer pump electrode; an auxiliary pump cell having an inner auxiliary pump electrode as the inner pump electrode arranged in a second internal space downstream of the first internal space of the measured gas flow part, and an outer auxiliary pump electrode as the outer pump electrode; and a measurement pump cell having an inner measurement electrode as the inner pump electrode and an outer measurement electrode as the outer pump electrode arranged in a measurement chamber downstream of the second internal space of the measured gas flow part, wherein the inner main pump electrode may have the peeling resistance.
[0016] [9] A gas sensor of the present invention includes the sensor element according to any one of the above items [1] to [8]. Therefore, the gas sensor can obtain the same effects as those of the above-mentioned sensor element, such as the effect of suppressing peeling of the peel-resistant electrode from the solid electrolyte layer. [Brief description of the drawings]
[0017] [Figure 1] 1 is a schematic cross-sectional view illustrating an example of the configuration of a gas sensor 100. FIG. [Diagram 2] FIG. 4 is a partially enlarged top view of the periphery of the inner pump electrode 22. [Diagram 3] FIG. 4 is a block diagram showing the electrical connection relationship between a control device 95 and each cell, etc. [Figure 4] FIG. 11 is a schematic cross-sectional view of a sensor element 201 according to a modified example. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0018] Next, an embodiment of the present invention will be described with reference to the drawings. FIG. 1 is a schematic cross-sectional view showing an example of the configuration of a gas sensor 100 according to an embodiment of the present invention. FIG. 2 is a partially enlarged view of the periphery of the inner pump electrode 22 in a cross section of the spacer layer 5 of the sensor element 101 cut along the front-rear and left-right directions, as viewed from above. In FIG. 2, the second diffusion rate-controlling portion 13 and the third diffusion rate-controlling portion 30 are shown by dotted lines for reference. FIG. 3 is a block diagram showing the electrical connection relationship between the control device 95 and each cell and the heater 72. This gas sensor 100 is attached to a pipe such as an exhaust gas pipe of an internal combustion engine. The gas sensor 100 detects a specific gas concentration, which is the concentration of a specific gas such as NOx or ammonia in the measured gas, using the exhaust gas of the internal combustion engine as the measured gas. In this embodiment, the gas sensor 100 measures the NOx concentration as the specific gas concentration. The gas sensor 100 includes a sensor element 101 having an element body 102 in the shape of a long rectangular parallelepiped, cells 21, 41, 50, 80 to 83 included in the sensor element 101, a heater section 70 provided inside the sensor element 101, and a control device 95 that has variable power sources 24, 46, 52 and a heater power source 76 and controls the entire gas sensor 100. The longitudinal direction of the sensor element 101 (the left-right direction in FIG. 1) is defined as the front-rear direction, the thickness direction of the sensor element 101 (the up-down direction in FIG. 1) is defined as the up-down direction, and the width direction of the sensor element 101 (the direction perpendicular to the front-rear direction and the up-down direction) is defined as the left-right direction.
[0019] The element body 102 is made of zirconia (ZrO 2 The element body 102 is a laminate in which six layers, namely, a first substrate layer 1, a second substrate layer 2, a third substrate layer 3, a first solid electrolyte layer 4, a spacer layer 5, and a second solid electrolyte layer 6, each of which is made of an oxygen ion conductive solid electrolyte layer such as SiO 2 , are laminated in this order from the bottom as viewed in the drawing. The solid electrolyte forming these six layers is dense and airtight. The element body 102 is manufactured, for example, by laminating ceramic green sheets corresponding to each layer after performing a predetermined processing and printing a circuit pattern thereon, and further firing the sheets to integrate them.
[0020] On the tip side (the left end side in FIG. 1 ) of sensor element 101 (element body 102), between the lower surface of second solid electrolyte layer 6 and the upper surface of first solid electrolyte layer 4, there are formed adjacent to each other and in communication with each other in this order: gas inlet 10, first diffusion rate-controlling section 11, buffer space 12, second diffusion rate-controlling section 13, first internal space (oxygen concentration adjusting chamber) 20, third diffusion rate-controlling section 30, second internal space (oxygen concentration adjusting chamber) 40, fourth diffusion rate-controlling section 60, and third internal space (measurement chamber) 61.
[0021] The gas inlet 10, the buffer space 12, the first internal void 20, the second internal void 40, and the third internal void 61 are spaces inside the sensor element 101, which are defined by an upper portion cut out of the spacer layer 5, the lower portion cut out by the upper surface of the first solid electrolyte layer 4, and the sides cut out by the side surfaces of the spacer layer 5.
[0022] The first diffusion rate-controlling section 11, the second diffusion rate-controlling section 13, and the third diffusion rate-controlling section 30 are each provided as two horizontally elongated slits (with the opening extending in the direction perpendicular to the drawing). The fourth diffusion rate-controlling section 60 is provided as one horizontally elongated slit (with the opening extending in the direction perpendicular to the drawing) formed as a gap with the lower surface of the second solid electrolyte layer 6. The portion from the gas inlet 10 to the third internal space 61 is also referred to as a measurement gas flow section.
[0023] The sensor element 101 (element body 102) includes a reference gas introduction section 49 for passing a reference gas from the outside of the sensor element 101 to the reference electrode 42 when measuring the NOx concentration. The reference gas introduction section 49 includes a reference gas introduction space 43 and a reference gas introduction layer 48. The reference gas introduction space 43 is a space provided inward from the rear end surface of the sensor element 101. The reference gas introduction space 43 is provided between the upper surface of the third substrate layer 3 and the lower surface of the spacer layer 5, at a position defined by the side surface of the first solid electrolyte layer 4. The reference gas introduction space 43 opens at the rear end surface of the sensor element 101, and this opening functions as an inlet portion 49a of the reference gas introduction section 49. The reference gas is introduced into the reference gas introduction space 43 from the inlet portion 49a. The reference gas introduction section 49 introduces the reference gas introduced from the inlet portion 49a into the reference electrode 42 while providing a predetermined diffusion resistance to the reference gas. In this embodiment, the reference gas is air.
[0024] The reference gas introduction layer 48 is provided between the upper surface of the third substrate layer 3 and the lower surface of the first solid electrolyte layer 4. The reference gas introduction layer 48 is a porous body made of ceramics such as alumina. A portion of the upper surface of the reference gas introduction layer 48 is exposed in the reference gas introduction space 43. The reference gas introduction layer 48 is formed so as to cover the reference electrode 42. The reference gas introduction layer 48 allows the reference gas to flow from the reference gas introduction space 43 to the reference electrode 42.
[0025] Reference electrode 42 is an electrode formed in a manner to be sandwiched between the upper surface of third substrate layer 3 and first solid electrolyte layer 4, and as described above, is surrounded by reference gas introduction layer 48 which is connected to reference gas introduction space 43. In addition, as will be described later, reference electrode 42 can be used to measure the oxygen concentrations (oxygen partial pressures) in first internal space 20, second internal space 40, and third internal space 61.
[0026] In the measurement gas flow section, the gas inlet 10 is a section that opens to the external space, and the measurement gas is introduced into the sensor element 101 from the external space through the gas inlet 10. The first diffusion rate-controlling section 11 is a section that imparts a predetermined diffusion resistance to the measurement gas introduced from the gas inlet 10. The buffer space 12 is a space provided for guiding the measurement gas introduced from the first diffusion rate-controlling section 11 to the second diffusion rate-controlling section 13. The second diffusion rate-controlling section 13 is a section that imparts a predetermined diffusion resistance to the measurement gas introduced from the buffer space 12 into the first internal space 20. When the measurement gas is introduced from the outside of the sensor element 101 to the first internal space 20, the measurement gas is suddenly taken into the sensor element 101 from the gas inlet 10 due to pressure fluctuations of the measurement gas in the external space (exhaust pressure pulsations if the measurement gas is automobile exhaust gas), but is not introduced directly into the first internal space 20, but is introduced into the first internal space 20 after the pressure fluctuations of the measurement gas are canceled through the first diffusion rate-controlling section 11, the buffer space 12, and the second diffusion rate-controlling section 13. As a result, the pressure fluctuations of the measurement gas introduced into the first internal space 20 are almost negligible. The first internal space 20 is provided as a space for adjusting the oxygen partial pressure in the measurement gas introduced through the second diffusion rate-controlling section 13. The oxygen partial pressure is adjusted by the operation of the main pump cell 21.
[0027] The main pump cell 21 is an electrochemical pump cell including an inner pump electrode 22 having a ceiling electrode portion 22a provided on almost the entire lower surface of the second solid electrolyte layer 6 facing the first internal space 20, an outer pump electrode 23 provided in a region corresponding to the ceiling electrode portion 22a on the upper surface of the second solid electrolyte layer 6 in a manner exposed to the outside of the sensor element 101, and the second solid electrolyte layer 6, the spacer layer 5, and the first solid electrolyte layer 4 which form a current path between these electrodes.
[0028] The inner pump electrode 22 is formed across the upper and lower solid electrolyte layers (the second solid electrolyte layer 6 and the first solid electrolyte layer 4) that define the first internal space 20, and the spacer layer 5 that provides the side walls. Specifically, a ceiling electrode portion 22a is formed on the lower surface of the second solid electrolyte layer 6 that provides the ceiling surface of the first internal space 20, and a bottom electrode portion 22b is formed on the upper surface of the first solid electrolyte layer 4 that provides the bottom surface. Side electrode portions 22c and 22d (see FIG. 2) are formed on the side wall surfaces (inner surfaces) of the spacer layer 5 that constitute both side walls of the first internal space 20 so as to connect the ceiling electrode portion 22a and the bottom electrode portion 22b, and are arranged in a tunnel-shaped structure at the arrangement sites of the side electrode portions. The side electrode portions 22c and 22d are members that play the role of leads (conducting portions) that connect the ceiling electrode portion 22a and the bottom electrode portion 22b to each other and electrically connect them to each other.
[0029] In the main pump cell 21, by applying a desired voltage Vp0 between the inner pump electrode 22 and the outer pump electrode 23 and flowing a pump current Ip0 in a positive or negative direction between the inner pump electrode 22 and the outer pump electrode 23, it is possible to pump oxygen in the first internal space 20 out to the external space, or to pump oxygen from the external space into the first internal space 20.
[0030] In addition, in order to detect the oxygen concentration (oxygen partial pressure) in the atmosphere in the first internal space 20, an electrochemical sensor cell, i.e., an oxygen partial pressure detection sensor cell 80 for controlling the main pump, is configured by the inner pump electrode 22, the second solid electrolyte layer 6, the spacer layer 5, the first solid electrolyte layer 4, the third substrate layer 3, and the reference electrode 42.
[0031] The oxygen concentration (oxygen partial pressure) in the first internal space 20 can be determined by measuring the electromotive force (voltage V0) in the main pump control oxygen partial pressure detection sensor cell 80. Furthermore, the pump current Ip0 is controlled by feedback controlling the voltage Vp0 of the variable power supply 24 so that the voltage V0 becomes a target value. This allows the oxygen concentration in the first internal space 20 to be maintained at a predetermined constant value.
[0032] The third diffusion rate-controlling section 30 is a section that applies a predetermined diffusion resistance to the measurement gas whose oxygen concentration (oxygen partial pressure) has been controlled by the operation of the main pump cell 21 in the first internal space 20, and guides the measurement gas to the second internal space 40.
[0033] The second internal space 40 is provided as a space for further adjusting the oxygen partial pressure by the auxiliary pump cell 50 for the measurement gas introduced through the third diffusion rate-controlling section 30 after the oxygen concentration (oxygen partial pressure) has been adjusted in advance in the first internal space 20. This makes it possible to keep the oxygen concentration in the second internal space 40 constant with high accuracy, thereby enabling the gas sensor 100 to measure the NOx concentration with high accuracy.
[0034] The auxiliary pump cell 50 is an auxiliary electrochemical pump cell that is composed of an auxiliary pump electrode 51 having a ceiling electrode portion 51a provided on almost the entire lower surface of the second solid electrolyte layer 6 facing the second internal space 40, an outer pump electrode 23 (not limited to the outer pump electrode 23, but any appropriate electrode on the outside of the sensor element 101 will suffice), the second solid electrolyte layer 6, the spacer layer 5, and the first solid electrolyte layer 4.
[0035] The auxiliary pump electrode 51 is disposed in the second internal space 40 in a tunnel-shaped structure similar to that of the inner pump electrode 22 provided in the first internal space 20. That is, a ceiling electrode portion 51a is formed on the lower surface of the second solid electrolyte layer 6 which provides the ceiling surface of the second internal space 40, and a bottom electrode portion 51b is formed on the upper surface of the first solid electrolyte layer 4 which provides the bottom surface of the second internal space 40. Side electrode portions (not shown) connecting the ceiling electrode portion 51a and the bottom electrode portion 51b are formed on both wall surfaces of the spacer layer 5 which provide the side walls of the second internal space 40, respectively, forming a tunnel-shaped structure.
[0036] In the auxiliary pump cell 50, by applying a desired voltage Vp1 between the auxiliary pump electrode 51 and the outer pump electrode 23, it is possible to pump oxygen in the atmosphere within the second internal space 40 out to the external space or pump oxygen from the external space into the second internal space 40.
[0037] In addition, in order to control the oxygen partial pressure in the atmosphere within the second internal space 40, an electrochemical sensor cell, i.e., an oxygen partial pressure detection sensor cell 81 for controlling the auxiliary pump, is constituted by the auxiliary pump electrode 51, the reference electrode 42, the second solid electrolyte layer 6, the spacer layer 5, the first solid electrolyte layer 4, and the third substrate layer 3.
[0038] The auxiliary pump cell 50 performs pumping using a variable power supply 52 whose voltage is controlled based on the electromotive force (voltage V1) detected by the auxiliary pump control oxygen partial pressure detection sensor cell 81. This allows the oxygen partial pressure in the atmosphere in the second internal space 40 to be controlled to a low partial pressure that does not substantially affect the measurement of NOx.
[0039] In addition, the pump current Ip1 is used to control the electromotive force of the main pump control oxygen partial pressure detection sensor cell 80. Specifically, the pump current Ip1 is input as a control signal to the main pump control oxygen partial pressure detection sensor cell 80, and the above-mentioned target value of the voltage V0 is controlled to always keep a constant gradient of the oxygen partial pressure in the measurement gas introduced from the third diffusion rate-controlling part 30 into the second internal space 40. When used as a NOx sensor, the oxygen concentration in the second internal space 40 is kept constant at about 0.001 ppm by the action of the main pump cell 21 and the auxiliary pump cell 50.
[0040] The fourth diffusion rate-controlling part 60 is a part that applies a predetermined diffusion resistance to the measurement gas whose oxygen concentration (oxygen partial pressure) has been controlled by the operation of the auxiliary pump cell 50 in the second internal space 40, and guides the measurement gas to the third internal space 61. The fourth diffusion rate-controlling part 60 serves to limit the amount of NOx flowing into the third internal space 61.
[0041] The third internal space 61 is provided as a space for carrying out a process for measuring the nitrogen oxide (NOx) concentration in the measurement gas, which has been introduced through the fourth diffusion-controlling part 60 after the oxygen concentration (oxygen partial pressure) has been adjusted in advance in the second internal space 40. The measurement of the NOx concentration is mainly carried out in the third internal space 61 by the operation of the measurement pump cell 41.
[0042] The measurement pump cell 41 measures the NOx concentration in the measurement gas in the third internal space 61. The measurement pump cell 41 is an electrochemical pump cell including a measurement electrode 44 provided on the upper surface of the first solid electrolyte layer 4 facing the third internal space 61, an outer pump electrode 23, the second solid electrolyte layer 6, a spacer layer 5, and the first solid electrolyte layer 4. The measurement electrode 44 also functions as a NOx reduction catalyst that reduces NOx present in the atmosphere in the third internal space 61.
[0043] In the measurement pump cell 41, oxygen produced by decomposition of nitrogen oxides in the atmosphere surrounding the measurement electrode 44 is pumped out, and the amount of oxygen produced can be detected as a pump current Ip2.
[0044] In order to detect the oxygen partial pressure around the measurement electrode 44, an electrochemical sensor cell, i.e., an oxygen partial pressure detection sensor cell 82 for controlling the measurement pump, is configured by the first solid electrolyte layer 4, the third substrate layer 3, the measurement electrode 44, and the reference electrode 42. The variable power supply 46 is controlled based on the electromotive force (voltage V2) detected by the oxygen partial pressure detection sensor cell 82 for controlling the measurement pump.
[0045] The measurement gas introduced into the second internal space 40 reaches the measurement electrode 44 in the third internal space 61 through the fourth diffusion-controlling part 60 under conditions in which the oxygen partial pressure is controlled. Nitrogen oxides in the measurement gas around the measurement electrode 44 are reduced (2NO→N 2 +O 2) oxygen is generated. The generated oxygen is then pumped by the measurement pump cell 41, and at that time, the voltage Vp2 of the variable power supply 46 is controlled so that the voltage V2 detected by the measurement pump control oxygen partial pressure detection sensor cell 82 becomes constant (target value). Since the amount of oxygen generated around the measurement electrode 44 is proportional to the concentration of nitrogen oxides in the measurement gas, the pump current Ip2 in the measurement pump cell 41 is used to calculate the nitrogen oxide concentration in the measurement gas.
[0046] Furthermore, by combining the measurement electrode 44, the first solid electrolyte layer 4, the third substrate layer 3, and the reference electrode 42 to form an oxygen partial pressure detection means as an electrochemical sensor cell, it is possible to detect an electromotive force corresponding to the difference between the amount of oxygen generated by reduction of the NOx components in the atmosphere around the measurement electrode 44 and the amount of oxygen contained in the reference gas, thereby making it possible to determine the concentration of the NOx components in the measured gas.
[0047] Furthermore, the second solid electrolyte layer 6, the spacer layer 5, the first solid electrolyte layer 4, the third substrate layer 3, the outer pump electrode 23, and the reference electrode 42 constitute an electrochemical sensor cell 83, and the electromotive force (voltage Vref) obtained by this sensor cell 83 makes it possible to detect the oxygen partial pressure in the measured gas outside the sensor.
[0048] In the gas sensor 100 having such a configuration, the main pump cell 21 and the auxiliary pump cell 50 are operated to supply a measurement gas in which the oxygen partial pressure is always kept at a constant low value (a value that has substantially no effect on the measurement of NOx) to the measurement pump cell 41. Therefore, the NOx concentration in the measurement gas can be known based on the pump current Ip2 that flows when oxygen generated by the reduction of NOx is pumped out of the measurement pump cell 41, which is approximately proportional to the NOx concentration in the measurement gas.
[0049] The sensor element 101 includes a heater section 70 that adjusts the temperature by heating and keeping the sensor element 101 warm in order to increase the oxygen ion conductivity of the solid electrolyte. The heater section 70 includes a heater connector electrode 71, a heater 72, a through hole 73, a heater insulating layer 74, and a pressure relief hole 75.
[0050] The heater connector electrode 71 is an electrode formed in a manner to contact the lower surface of the first substrate layer 1. By connecting the heater connector electrode 71 to a heater power supply 76 (see FIG. 3), it is possible to supply power from the heater power supply 76 to the heater section 70.
[0051] The heater 72 is an electrical resistor sandwiched between the second substrate layer 2 and the third substrate layer 3. The heater 72 is connected to a heater connector electrode 71 via a through hole 73, and generates heat when power is supplied from a heater power source 76 through the heater connector electrode 71, thereby heating and keeping warm the solid electrolyte that forms the sensor element 101.
[0052] The heater 72 is embedded throughout the entire area from the first internal space 20 to the third internal space 61, and is capable of adjusting the temperature of the entire sensor element 101 to a temperature at which the solid electrolyte is activated.
[0053] The heater insulating layer 74 is an insulating layer made of an insulator such as alumina and formed on the upper and lower surfaces of the heater 72. The heater insulating layer 74 is formed for the purpose of obtaining electrical insulation between the second substrate layer 2 and the heater 72, and between the third substrate layer 3 and the heater 72.
[0054] The pressure relief hole 75 is a portion that penetrates the third substrate layer 3 and the reference gas introduction layer 48 and is provided so as to communicate with the reference gas introduction space 43, and is formed for the purpose of mitigating the increase in internal pressure that accompanies an increase in temperature within the heater insulation layer 74.
[0055] Here, the electrodes 22, 23, 42, 44, and 51 will be described. Each of the electrodes 22, 23, 42, 44, and 51 contains a precious metal. The inner pump electrode 22, the auxiliary pump electrode 51, and the measurement electrode 44 each contain a first-class precious metal having catalytic activity as a precious metal. Examples of the first-class precious metal include at least one of Pt, Rh, Ir, Ru, and Pd. The outer pump electrode 23 and the reference electrode 42 also contain a first-class precious metal. The inner pump electrode 22 and the auxiliary pump electrode 51 also contain a second-class precious metal as a precious metal that suppresses the catalytic activity of the first-class precious metal for a specific gas (NOx). As a result, the inner pump electrode 22 and the auxiliary pump electrode 51 have a weakened ability to reduce the NOx component in the measurement gas. Examples of the second-class precious metal include Au. The measurement electrode 44 does not contain a second-class precious metal. This makes the electrode 44 more capable of reducing NOx components in the measurement gas than the inner pump electrode 22 and the auxiliary pump electrode 51. The measurement electrode 44 preferably contains at least one of Pt and Rh among the first class precious metals, and may contain both Pt and Rh. The outer pump electrode 23 and the reference electrode 42 also preferably do not contain a second class precious metal. Each of the electrodes 22, 23, 42, 44, and 51 is made of a precious metal and an oxide having oxygen ion conductivity (e.g., ZrO 2 Each of the electrodes 22, 23, 42, 44, and 51 is preferably a porous body. In this embodiment, the inner pump electrode 22 and the auxiliary pump electrode 51 are made of a cermet containing Pt and ZrO 2 The outer pump electrode 23 and the reference electrode 42 were both made of Pt and ZrO 2 The measurement electrode 44 is a porous cermet electrode made of Pt, Rh and ZrO 2 The porous cermet electrode was made of
[0056] Each of the electrodes 22, 23, 42, 44, and 51 is made of zirconia (ZrO 2 In the case where zirconia contains yttria (Y2 O 3 ), calcia (CaO), and magnesia (MgO), and the partially stabilized zirconia may contain one or more of these as a stabilizer.
[0057] The inner pump electrode 22 includes a precious metal (here, Pt) and zirconia, and has a TM ratio, which is a ratio Ht / Hm of a peak height Ht of a T phase (tetragonal crystal) of zirconia to a peak height Hm of an M phase (monoclinic crystal) of zirconia in a Raman spectrum measured by Raman spectroscopy, of 1 to 10, and a porosity of 3% to 65% (hereinafter, referred to as a peel-resistant electrode). Specifically, the ceiling electrode portion 22a and the bottom electrode portion 22b of the inner pump electrode 22 are each configured as a peel-resistant electrode. The porosity of the peel-resistant electrode is preferably 50% or less, and more preferably 40% or less. The porosity of the peel-resistant electrode may be less than 5%, more than 40%, or less than 5% or more than 40%.
[0058] The peel-resistant electrode preferably has a maximum pore size of 5 μm or more and 17 μm or less. The peel-resistant electrode preferably has a thickness of 5 μm or more and 30 μm or less. The peel-resistant electrode preferably has an area of 5 mm2 or more as viewed in the thickness direction. 2 More than 20mm 2It is preferable that the thickness direction is equal to or less than 100 mm. The thickness direction is the direction perpendicular to the surface on which the peel-resistant electrodes are disposed. The area of the peel-resistant electrodes is the area of the surface opposite to the surface in contact with the surface of the peel-resistant electrodes. Therefore, the thickness direction of the ceiling electrode portion 22a of the two peel-resistant electrodes of the inner pump electrode 22 is the direction perpendicular to the lower surface (upper surface of the inner circumferential surface of the first inner space 20) of the second solid electrolyte layer 6 on which the ceiling electrode portion 22a is disposed, that is, the vertical direction. The area of the ceiling electrode portion 22a is the area of the lower surface of the ceiling electrode portion 22a (the surface opposite to the surface in contact with the lower surface of the second solid electrolyte layer 6) viewed along the thickness direction (here, the vertical direction). The thickness direction of the bottom electrode portion 22b of the two peel-resistant electrodes of the inner pump electrode 22 is the direction perpendicular to the upper surface (lower surface of the inner circumferential surface of the first inner space 20) of the first solid electrolyte layer 4 on which the bottom electrode portion 22b is disposed, that is, the vertical direction. The area of bottom electrode portion 22b is the area of the upper surface of bottom electrode portion 22b (the surface opposite to the surface in contact with the upper surface of first solid electrolyte layer 4) viewed along the thickness direction (here, the vertical direction). In this embodiment, as shown in FIG. 2, the shape of the upper surface of bottom electrode portion 22b when viewed along the thickness direction (here, the vertical direction) is a rectangle, so the area of this rectangle (the product of the front-to-back length and the left-to-right length) is taken as the area of bottom electrode portion 22b. Similarly, in this embodiment, the shape of the lower surface of ceiling electrode portion 22a when viewed along the thickness direction is a rectangle (not shown), so the product of the front-to-back length and the left-to-right length of the lower surface of ceiling electrode portion 22a is taken as the area of ceiling electrode portion 22a.
[0059] In this embodiment, the inner pump electrode 22 has two peeling-resistant electrodes (ceiling electrode portion 22a and bottom electrode portion 22b), and the ceiling electrode portion 22a and the bottom electrode portion 22b may differ from each other in one or more of the TM ratio, porosity, maximum pore diameter, thickness, and area. The ceiling electrode portion 22a and the bottom electrode portion 22b each preferably have a porosity of 50% or less, and more preferably have a porosity of 40% or less. The ceiling electrode portion 22a and the bottom electrode portion 22b each preferably satisfy one or more of the above-mentioned numerical ranges of the maximum pore diameter, thickness, and area.
[0060] The TM ratio of the zirconia of the peel-resistant electrode is a value derived as follows using a Raman spectrum measured by Raman spectroscopy. For example, when deriving the TM ratio of the bottom electrode portion 22b, first, the sensor element 101 is cut so as to cut the spacer layer 5 along the front-rear and left-right directions, and the surface (here, the top surface) of the bottom electrode portion 22b inside the sensor element 101 is exposed to be used as an observation surface. Next, a laser beam is irradiated onto the observation surface using, for example, a Raman spectrometer to obtain a Raman spectrum. The Raman spectrum is measured at 70 cm -1 ~800cm -1 and calculate the maximum and minimum intensity values within this range. The minimum value is then subtracted from the overall intensity, and the spectrum is normalized by the value of maximum value minus minimum value to obtain spectrum SP. Next, the spectrum SP is fitted using software (e.g., LabSpec, an operating software manufactured by Horiba, Ltd.) to remove the background from spectrum SP. Next, of the spectrum SP after background removal, the spectrum with a Raman shift of 260 cm -1 The peak P1 located closest to the peak height Ht of the T phase is determined as the peak derived from the T phase, and the intensity of the peak P1 is calculated as the peak height Ht of the T phase. -1 The peak P2 closest to the T phase is identified as the peak derived from the M phase, and the intensity of this peak P2 is calculated as the M phase peak height Hm. Based on the thus calculated T phase peak height Ht and M phase peak height Hm, the TM ratio of the bottom electrode portion 22b is calculated as Ht / Hm. The TM ratio of the ceiling electrode portion 22a is also determined as a value derived in the same manner as above.
[0061] The porosity, maximum pore diameter, and thickness of the peel-resistant electrode are values derived as follows using an image (SEM image) obtained by observation using a scanning electron microscope (SEM). For example, when deriving the porosity, maximum pore diameter, and thickness of the bottom electrode portion 22b, first, the sensor element 101 is cut along the thickness direction of the bottom electrode portion 22b so that the cross section of the bottom electrode portion 22b is the observation surface, and the cut surface is filled with resin and polished to obtain an observation sample. Next, the magnification of the SEM is set to 3000 times, and an observation surface of the observation sample is photographed to obtain an SEM image of three or more fields of view. Next, the obtained image is analyzed, and a threshold value is determined by a discriminant analysis method (Otsu's binarization) from the brightness distribution of the brightness data of the pixels in the image. After that, each pixel in the image is binarized into an object part and a pore part based on the determined threshold value, and the area of the object part and the area of the pore part are calculated. Then, the ratio of the area of the pore parts to the total area (the total area of the object part and the pore parts) is derived as the porosity (unit: %). In addition, the length of the longest line segment that can be drawn in the SEM image so as to overlap only with the pixels of the pore parts (so as not to overlap with the pixels of the object part) is derived as the maximum pore diameter (unit: μm). The thickness (unit: μm) of the bottom electrode part 22b is also derived based on the thickness of the bottom electrode part 22b in the SEM image. The porosity, maximum pore diameter, and thickness of the ceiling electrode part 22a are also values derived in the same manner as above.
[0062] 3, the control device 95 includes the variable power supplies 24, 46, 52, the heater power supply 76, and a control unit 96. The control unit 96 is a microprocessor including a CPU 97 and a storage unit 98. The storage unit 98 is a non-volatile memory that allows information to be rewritten, and can store, for example, various programs and various data. The control unit 96 receives the voltage V0 of the oxygen partial pressure detection sensor cell 80 for controlling the main pump, the voltage V1 of the oxygen partial pressure detection sensor cell 81 for controlling the auxiliary pump, the voltage V2 of the oxygen partial pressure detection sensor cell 82 for controlling the measurement pump, the voltage Vref of the sensor cell 83, the pump current Ip0 flowing through the main pump cell 21, the pump current Ip1 flowing through the auxiliary pump cell 50, and the pump current Ip2 flowing through the measurement pump cell 41. The control unit 96 also outputs control signals to the variable power sources 24, 46, 52 to control the voltages Vp0, Vp1, Vp2 output by the variable power sources 24, 46, 52, thereby controlling the main pump cell 21, the measurement pump cell 41, and the auxiliary pump cell 50. The control unit 96 outputs control signals to the heater power source 76 to control the power supplied from the heater power source 76 to the heater 72. The memory unit 98 also stores target values V0*, V1*, V2*, etc., which will be described later. The CPU 97 of the control unit 96 controls the cells 21, 41, 50 by referring to these target values V0*, V1*, V2*.
[0063] The control unit 96 performs an auxiliary pump control process to control the auxiliary pump cell 50 so that the oxygen concentration in the second internal space 40 becomes a target concentration. Specifically, the control unit 96 controls the auxiliary pump cell 50 by feedback-controlling the voltage Vp1 of the variable power source 52 so that the voltage V1 becomes a constant value (referred to as a target value V1*). The target value V1* is determined as a value that causes the oxygen concentration in the second internal space 40 to become a predetermined low concentration that does not substantially affect the measurement of NOx.
[0064] The control unit 96 performs a main pump control process to control the main pump cell 21 so that the pump current Ip1 flowing when the auxiliary pump cell 50 adjusts the oxygen concentration in the second internal space 40 by the auxiliary pump control process becomes a target current (referred to as a target value Ip1*). Specifically, the control unit 96 sets (feedback controls) a target value (referred to as a target value V0*) of the voltage V0 based on the pump current Ip1 so that the pump current Ip1 flowing by the voltage Vp1 becomes a constant target value Ip1*. Then, the control unit 96 feedback controls the voltage Vp0 of the variable power supply 24 so that the voltage V0 becomes the target value V0* (i.e., so that the oxygen concentration in the first internal space 20 becomes the target concentration). This main pump control process keeps the gradient of the oxygen partial pressure in the measurement gas introduced from the third diffusion rate-controlling unit 30 into the second internal space 40 constant. The target value V0* is set to a value such that the oxygen concentration in the first internal space 20 is higher and lower than 0%. The pump current Ip0 flowing during the main pump control process changes according to the oxygen concentration of the measurement gas (i.e., the measurement gas around the sensor element 101) flowing into the measurement gas flow section from the gas inlet 10. Therefore, the control section 96 can also detect the oxygen concentration in the measurement gas based on the pump current Ip0.
[0065] The above-mentioned main pump control process and auxiliary pump control process are also collectively referred to as an adjustment pump control process. The first internal space 20 and the second internal space 40 are also collectively referred to as an oxygen concentration adjustment chamber. The main pump cell 21 and the auxiliary pump cell 50 are also collectively referred to as an adjustment pump cell. The control unit 96 performs the adjustment pump control process, causing the adjustment pump cell to adjust the oxygen concentration in the oxygen concentration adjustment chamber.
[0066] Furthermore, the control unit 96 performs a measurement pump control process to control the measurement pump cell 41 so that the voltage V2 becomes a constant value (referred to as a target value V2*) (i.e., so that the oxygen concentration in the third internal space 61 becomes a predetermined low concentration). Specifically, the control unit 96 controls the measurement pump cell 41 by feedback-controlling the voltage Vp2 of the variable power supply 46 so that the voltage V2 becomes the target value V2*. Oxygen is pumped out of the third internal space 61 by this measurement pump control process.
[0067] By performing the measurement pump control process, oxygen is pumped out from the third internal space 61 so that the amount of oxygen generated by reduction of NOx in the measurement gas in the third internal space 61 becomes substantially zero. Then, the control unit 96 obtains the pump current Ip2 as a detection value corresponding to the oxygen generated in the third internal space 61 derived from the specific gas (here, NOx), and calculates the NOx concentration in the measurement gas based on this pump current Ip2.
[0068] A relational expression (for example, a linear or quadratic function) or a map is stored as a correspondence relationship between the pump current Ip2 and the NOx concentration in the storage unit 98. Such a relational expression or map can be obtained in advance by experiment.
[0069] The control unit 96 performs a heater control process in which a control signal is output to the heater power supply 76 to control the temperature of the heater 72 to a target temperature (e.g., 800°C). Here, the temperature of the heater 72 can be expressed by an equation that is a linear function of the resistance value of the heater 72. In the heater control process, the control unit 96 calculates the resistance value of the heater 72 as a value that can be regarded as the temperature of the heater 72 (a value that can be converted into a temperature), and feedback controls the heater power supply 76 so that the calculated resistance value becomes the target resistance value (resistance value corresponding to the target temperature). The control unit 96 can, for example, obtain the voltage of the heater 72 and the current flowing through the heater 72, and calculate the resistance value of the heater 72 based on the obtained voltage and current. The control unit 96 may calculate the resistance value of the heater 72 by, for example, a three-terminal method or a four-terminal method. When energizing the heater 72, the heater power supply 76 adjusts the power supplied to the heater 72 by, for example, changing the value of the voltage applied to the heater 72 based on a control signal from the control unit 96.
[0070] Incidentally, the control device 95, including the variable power sources 24, 46, 52 and the heater power source 76 shown in FIG. 3, is actually connected to each electrode inside the sensor element 101 via lead wires (not shown) formed within the sensor element 101 and connector electrodes (not shown) formed on the rear end side of the sensor element 101 (only the heater connector electrode 71 is shown in FIG. 1).
[0071] Next, an example of a method for manufacturing the sensor element 101 of the gas sensor 100 is described below. First, six unfired ceramic green sheets containing an oxygen ion conductive solid electrolyte such as zirconia as a ceramic component are prepared. A plurality of sheet holes and necessary through holes used for positioning during printing and lamination are formed in advance in the green sheets. A space to be a measurement gas flow section is provided in advance by punching or the like in the green sheet to be the spacer layer 5. Similarly, a space to be a reference gas introduction space 43 is provided in the green sheet to be the first solid electrolyte layer 4. Then, a pattern printing process and a drying process are performed to form various patterns on each ceramic green sheet corresponding to each of the first substrate layer 1, the second substrate layer 2, the third substrate layer 3, the first solid electrolyte layer 4, the spacer layer 5, and the second solid electrolyte layer 6. Specifically, the patterns to be formed are, for example, the patterns of the above-mentioned electrodes, the lead wires connected to the electrodes, the reference gas introduction layer 48, the heater section 70, and the like. The pattern printing is performed by applying a pattern forming paste prepared according to the characteristics required for each forming target on the green sheet using a known screen printing technique. The pattern that becomes the inner pump electrode 22 is formed separately into a pattern that becomes the ceiling electrode portion 22a after firing, a pattern that becomes the bottom electrode portion 22b after firing, and a pattern that becomes the side electrode portion 22c and the side electrode portion 22d after firing. The patterns that become the side electrode portion 22c and the side electrode portion 22d can be formed, for example, by known through-hole printing. The drying process is also performed using a known drying means. After the pattern printing and drying are completed, a printing and drying process of an adhesive paste for laminating and bonding the green sheets corresponding to each layer is performed. Then, the green sheets on which the adhesive paste is formed are laminated in a predetermined order while being positioned by the sheet holes, and are pressed by applying a predetermined temperature and pressure condition to form a single laminate. The laminate obtained in this way contains a plurality of unfired element bodies that become the element body 102 after firing. The laminate is cut to obtain a plurality of unsintered element bodies having the size of the sensor element 101. The unsintered element bodies are then fired at a predetermined firing temperature to obtain the sensor element 101.
[0072] Once the sensor element 101 is obtained in this manner, a sensor assembly is manufactured in which the sensor element 101 is incorporated into an element encapsulation body (not shown), and a protective cover or the like is attached. Then, the sensor element 101 and the control device 95 are electrically connected to obtain the gas sensor 100.
[0073] The paste for forming the pattern of the peel-resistant electrode (here, each of the ceiling electrode portion 22a and the bottom electrode portion 22b of the inner pump electrode 22) can be prepared by kneading, for example, a powder of a precious metal (here, Pt and Au), a powder of zirconia, a stabilizer for zirconia, and a solvent. In this embodiment, the stabilizer is yttria. The paste for forming the pattern of the peel-resistant electrode may contain a pore-forming material. Examples of the pore-forming material include polymeric materials such as acrylic resin. The TM ratio of the zirconia of the peel-resistant electrode can be adjusted by adjusting, for example, one or more of the content ratio of the stabilizer in the paste, the crushing time of the zirconia powder before kneading, and the firing temperature of the pattern of the peel-resistant electrode (and thus the firing temperature of the unfired element body). For example, by increasing the content ratio of the stabilizer, the proportion of the crystal system of the T phase of zirconia becomes higher than the M phase at room temperature after firing, and thus the TM ratio can be increased. In addition, the higher the firing temperature, the greater the proportion of the T-phase crystal system compared to the M-phase, and the TM ratio can be increased. The longer the pulverization time of the zirconia powder, the smaller the particle size of the zirconia powder becomes, and the easier it is to exist as a T-phase, and the TM ratio can be increased. For example, the pulverization time of the zirconia powder before preparing the paste for forming the pattern of the peel-resistant electrode is set to 10 hours or more and 100 hours or less, the ratio B / A of the content ratio B (mol%) of the stabilizer to the content ratio A (mol%) of the zirconia in the paste is set to 2 or more and 8 or less, and the firing temperature is set to 1200°C or more and 1500°C or less, so that the TM ratio of the zirconia in the peel-resistant electrode can be set to 1 or more and 10 or less. The porosity and maximum pore size of the peel-resistant electrode can be adjusted, for example, by adjusting the particle size and content ratio of the pore-forming material contained in the paste for forming the pattern of the peel-resistant electrode. The thickness of the peel-resistant electrode can be adjusted, for example, by adjusting the viscosity of the paste for forming the pattern of the peel-resistant electrode, or by changing the number of printings during pattern formation. The area of the peel-resistant electrode can be adjusted, for example, by adjusting the shape of a mask used for screen printing during pattern formation.
[0074] Next, an example of use of the gas sensor 100 will be described. The CPU 97 of the control unit 96 first starts the heater control process described above, and controls the heater power supply 76 so that the temperature of the heater 72 becomes a target temperature (for example, 800° C.). When the temperature of the heater 72 reaches the target temperature (or near the target temperature), the CPU 97 starts controlling the pump cells 21, 41, 50 described above (adjustment pump control process and measurement pump control process) and acquiring the voltages V0, V1, V2, Vref from the sensor cells 80 to 83 described above. When the measurement gas is introduced from the gas inlet 10 in this state, the measurement gas passes through the first diffusion rate-controlling section 11, the buffer space 12, and the second diffusion rate-controlling section 13, and reaches the first internal space 20. Next, the oxygen concentration of the measurement gas is adjusted by the main pump cell 21 and the auxiliary pump cell 50 in the first internal space 20 and the second internal space 40, and the adjusted measurement gas reaches the third internal space 61. Then, the CPU 97 detects the NOx concentration in the measurement target gas based on the acquired pump current Ip2 and the correspondence relationship stored in the storage unit 98.
[0075] In the sensor element 101 of the gas sensor 100 thus configured, as described above, the ceiling electrode portion 22a and the bottom electrode portion 22b of the inner pump electrode 22 are configured as peel-resistant electrodes in which the TM ratio of zirconia is 1 to 10 and the porosity is 3% to 65%. This makes it possible to suppress peeling of the ceiling electrode portion 22a and the bottom electrode portion 22b from the solid electrolyte layer (here, the second solid electrolyte layer 6 and the first solid electrolyte layer 4) from each other. More specifically, the TM ratio of the ceiling electrode portion 22a is 1 or more and the porosity is 65% or less, so that peeling of the ceiling electrode portion 22a from the second solid electrolyte layer 6 due to stress can be suppressed. In addition, the TM ratio of the ceiling electrode portion 22a is 10 or less and the porosity is 3% or more, so that peeling of the ceiling electrode portion 22a from the second solid electrolyte layer 6 due to volume expansion caused by TM transformation of zirconia can be suppressed. Similarly, by having the TM ratio of bottom electrode portion 22b be 1 or more and the porosity be 65% or less, it is possible to suppress peeling of bottom electrode portion 22b from first solid electrolyte layer 4 caused by stress. Also, by having the TM ratio of bottom electrode portion 22b be 10 or less and the porosity be 3% or more, it is possible to suppress peeling of bottom electrode portion 22b from first solid electrolyte layer 4 caused by volume expansion due to TM transformation of zirconia. The inventors confirmed this through experiments and analyses.
[0076] The reason why such an effect is obtained is considered to be as follows. Since the sensor element 101 is heated by the heater 72 during use, thermal expansion occurs in the solid electrolyte layer (each of layers 1 to 6) of the element body 102 and the inner pump electrode 22, and stress is applied to the inner pump electrode 22. At this time, the higher the TM ratio of zirconia in the ceiling electrode portion 22a, the higher the toughness of the ceiling electrode portion 22a tends to be, and peeling of the ceiling electrode portion 22a due to stress tends to be suppressed. In addition, since the strength of the ceiling electrode portion 22a decreases when the porosity of the ceiling electrode portion 22a is high, peeling of the ceiling electrode portion 22a due to stress tends to be suppressed as the porosity is lower. Therefore, it is considered that the toughness and strength of the ceiling electrode portion 22a are increased by the ceiling electrode portion 22a having a TM ratio of 1 or more and a porosity of 65% or less, and peeling of the ceiling electrode portion 22a from the second solid electrolyte layer 6 due to stress is suppressed. On the other hand, when the ceiling electrode portion 22a contains zirconia, the TM transformation of zirconia (change in crystal structure from T phase (tetragonal) to M phase (monoclinic)) may occur due to heat during use of the sensor element 101, and the volume of the zirconia may expand. As a result, the volume of the ceiling electrode portion 22a may gradually expand as the period of use of the sensor element 101 increases. There is a concern that the ceiling electrode portion 22a may peel off from the second solid electrolyte layer 6 due to excessive volume expansion caused by the TM transformation of zirconia in the ceiling electrode portion 22a. In contrast, in this embodiment, the TM ratio of the zirconia in the ceiling electrode portion 22a is 10 or less, so that the proportion of the T phase in the zirconia in the ceiling electrode portion 22a is low and the proportion of the M phase is high compared to when the TM ratio is greater than 10. Therefore, the proportion of the T phase, which is the source of the change to the M phase, is low in the zirconia in the ceiling electrode portion 22a of this embodiment, so that the reduction rate of the TM ratio due to the TM transformation is small, and the expansion rate of the volume of the ceiling electrode portion 22a due to the TM transformation is small. As a result, even if the sensor element 101 is used for a long period of time, the volume expansion rate of the ceiling electrode portion 22a due to TM transformation is small, and it is believed that peeling of the ceiling electrode portion 22a from the second solid electrolyte layer 6 due to volume expansion due to TM transformation is suppressed.In addition, the higher the porosity of the ceiling electrode portion 22a, the more space there is inside the ceiling electrode portion 22a, so even if the volume expansion of the ceiling electrode portion 22a occurs due to the TM transformation, the outer dimensions of the ceiling electrode portion 22a are less likely to change, and peeling of the ceiling electrode portion 22a tends to be suppressed. Therefore, it is considered that peeling of the ceiling electrode portion 22a from the second solid electrolyte layer 6 caused by the volume expansion of zirconia due to the TM transformation of the ceiling electrode portion 22a is suppressed by having the TM ratio of the ceiling electrode portion 22a be 10 or less and the porosity be 3% or more. From the above, peeling of the ceiling electrode portion 22a from the second solid electrolyte layer 6 caused by stress during use of the sensor element 101 can be suppressed by having the TM ratio of the zirconia of the ceiling electrode portion 22a be 1 or more and 10 or less and the porosity be 3% or more and 65% or less, and peeling of the ceiling electrode portion 22a from the second solid electrolyte layer 6 caused by the volume expansion of zirconia due to the TM transformation of the ceiling electrode portion 22a when the sensor element 101 is used for a long period of time can also be suppressed. As described above, the lower the porosity, the more the ceiling electrode portion 22a tends to be prevented from peeling off due to stress. From this viewpoint, the porosity of the ceiling electrode portion 22a is preferably 50% or less, more preferably 40% or less. Similarly, for the bottom electrode portion 22b, the TM ratio of zirconia is 1 to 10 and the porosity is 3% to 65%, so that the peeling off of the bottom electrode portion 22b from the first solid electrolyte layer 4 caused by stress during use of the sensor element 101 can be prevented, and the peeling off of the bottom electrode portion 22b from the first solid electrolyte layer 4 caused by volume expansion due to TM transformation of zirconia in the bottom electrode portion 22b when the sensor element 101 is used for a long period of time can also be prevented. The porosity of the bottom electrode portion 22b is preferably 50% or less, more preferably 40% or less.
[0077] In addition, the smaller the pore diameter of the ceiling electrode portion 22a, the stronger the strength of the ceiling electrode portion 22a tends to be, and the effect of suppressing the peeling of the ceiling electrode portion 22a from the second solid electrolyte layer 6 due to stress tends to be enhanced. From this viewpoint, the maximum pore diameter of the ceiling electrode portion 22a is preferably 17 μm or less. On the other hand, the larger the pore diameter of the ceiling electrode portion 22a, the larger the space inside the ceiling electrode portion 22a, so that even if the volume expansion due to the TM transformation of the ceiling electrode portion 22a occurs, the outer dimensions of the ceiling electrode portion 22a are less likely to change, and the peeling of the ceiling electrode portion 22a tends to be suppressed. From this viewpoint, the maximum pore diameter of the ceiling electrode portion 22a is preferably 5 μm or more. Similarly, from the viewpoint of suppressing the peeling of the bottom electrode portion 22b from the first solid electrolyte layer 4 due to stress, the maximum pore diameter of the bottom electrode portion 22b is preferably 17 μm or less. From the viewpoint of suppressing the peeling of the bottom electrode portion 22b due to the TM transformation, the maximum pore diameter of the bottom electrode portion 22b is preferably 5 μm or more.
[0078] The smaller the thickness of the ceiling electrode portion 22a, the smaller the volume of the ceiling electrode portion 22a and the smaller the magnitude of volume expansion in the thickness direction of the ceiling electrode portion 22a (not the expansion coefficient but the difference in thickness before and after expansion) tend to be, so that peeling off of the ceiling electrode portion 22a from the second solid electrolyte layer 6 due to volume expansion caused by the TM transformation of zirconia tends to be suppressed. From this viewpoint, the thickness of the ceiling electrode portion 22a is preferably 30 μm or less. On the other hand, the smaller the thickness of the ceiling electrode portion 22a, the smaller the volume of the ceiling electrode portion 22a tends to be, so that the amount of precious metal in the ceiling electrode portion 22a tends to be reduced. And, the precious metal in the ceiling electrode portion 22a oxidizes with the use of the sensor element 101, and the oxidized precious metal is more likely to evaporate than before oxidation, so that the precious metal in the ceiling electrode portion 22a decreases and the ceiling electrode portion 22a becomes brittle. Therefore, the smaller the thickness of the ceiling electrode portion 22a, the more likely it is that the ceiling electrode portion 22a will become brittle due to deterioration (oxidation of the precious metal) of the ceiling electrode portion 22a, and the more likely it is that the ceiling electrode portion 22a will peel off from the second solid electrolyte layer 6. From this perspective, the thickness of the ceiling electrode portion 22a is preferably 5 μm or more. Similarly, from the perspective of suppressing peeling of the bottom electrode portion 22b from the first solid electrolyte layer 4 due to TM transformation, the thickness of the bottom electrode portion 22b is preferably 30 μm or less. From the perspective of suppressing peeling due to oxidation of the precious metal in the bottom electrode portion 22b, the thickness of the bottom electrode portion 22b is preferably 5 μm or more.
[0079] As with the thickness, the area of the ceiling electrode portion 22a viewed in the thickness direction also tends to be smaller as the area becomes smaller, and the magnitude of volume expansion in the direction along the surface on which the ceiling electrode portion 22a is disposed (not the expansion rate but the difference in length before and after expansion) tends to be smaller, so that peeling of the ceiling electrode portion 22a from the second solid electrolyte layer 6 due to volume expansion caused by the TM transformation of zirconia tends to be suppressed. From this perspective, the area of the ceiling electrode portion 22a is set to 20 mm 2It is preferable that the area of the ceiling electrode portion 22a is 5 mm or less. In addition, since the volume of the ceiling electrode portion 22a tends to be smaller as the area of the ceiling electrode portion 22a is smaller, there is a concern that the ceiling electrode portion 22a may easily become brittle due to deterioration of the ceiling electrode portion 22a (oxidation of the precious metal), and the ceiling electrode portion 22a may easily peel off from the second solid electrolyte layer 6. From this viewpoint, the area of the ceiling electrode portion 22a is preferably 5 mm 2 Similarly, from the viewpoint of suppressing the peeling of the bottom electrode portion 22b from the first solid electrolyte layer 4 due to the TM transformation, the area of the bottom electrode portion 22b is preferably 20 mm 2 From the viewpoint of suppressing peeling caused by oxidation of the precious metal in the bottom electrode portion 22b, the area of the bottom electrode portion 22b is preferably 5 mm 2 More preferably, it is equal to or greater than this.
[0080] In addition, when the zirconia changes from the T phase to the M phase in the ceiling electrode portion 22a, the value of the TM ratio decreases, so that the TM transformation of zirconia caused by the use of the sensor element 101 may cause the TM ratio of the ceiling electrode portion 22a to change from a value of 1 to 10 to a value less than 1. In addition, depending on the temperature during use of the sensor element 101, the zirconia may change from the M phase to the T phase in the ceiling electrode portion 22a, causing the value of the TM ratio to increase, and as a result, the TM ratio of the ceiling electrode portion 22a may change from a value of 1 to 10 to a value exceeding 10. However, in the sensor element 101 of this embodiment, when the sensor element 101 is unused, that is, when the TM transformation of zirconia caused by the use of the sensor element 101 is not occurring, the TM ratio of zirconia in the ceiling electrode portion 22a may be 1 to 10. The same applies to the bottom electrode portion 22b.
[0081] Here, the correspondence between the components of this embodiment and the components of the present invention will be clarified. Each of the first substrate layer 1, the second substrate layer 2, the third substrate layer 3, the first solid electrolyte layer 4, the spacer layer 5, and the second solid electrolyte layer 6 of this embodiment corresponds to a solid electrolyte layer of the present invention, the element body 102 corresponds to an element body, and the ceiling electrode portion 22a arranged on the second solid electrolyte layer 6 and the bottom electrode portion 22b arranged on the first solid electrolyte layer 4 correspond to peel-resistant electrodes, respectively. Also, the inner pump electrode 22 corresponds to an inner pump electrode and an inner main pump electrode. In addition, the outer pump electrode 23 corresponds to the outer pump electrode, the outer main pump electrode, the outer auxiliary pump electrode, and the outer measurement electrode, the main pump cell 21 corresponds to the pump cell and the main pump cell, the auxiliary pump electrode 51 corresponds to the inner pump electrode and the inner auxiliary pump electrode, the auxiliary pump cell 50 corresponds to the auxiliary pump cell, the third internal space 61 corresponds to the measurement chamber, the measurement electrode 44 corresponds to the inner pump electrode and the inner measurement electrode, and the measurement pump cell 41 corresponds to the measurement pump cell.
[0082] The sensor element 101 provided in the gas sensor 100 of the present embodiment described above in detail includes the ceiling electrode portion 22a and the bottom electrode portion 22b (two peel-resistant electrodes) that contain a precious metal and zirconia, have a TM ratio of 1 to 10, and have a porosity of 3% to 65%. The ceiling electrode portion 22a and the bottom electrode portion 22b have a TM ratio of 1 or more and a porosity of 65% or less, so that peeling of the ceiling electrode portion 22a and the bottom electrode portion 22b from the second solid electrolyte layer 6 and the first solid electrolyte layer 4 caused by stress can be suppressed. Furthermore, the ceiling electrode portion 22a and the bottom electrode portion 22b have a TM ratio of 10 or less and a porosity of 3% or more, so that peeling of the ceiling electrode portion 22a and the bottom electrode portion 22b from the second solid electrolyte layer 6 and the first solid electrolyte layer 4 caused by volume expansion due to TM transformation of zirconia can be suppressed. Furthermore, by having the porosity of ceiling electrode portion 22a and bottom electrode portion 22b be 50% or less, stress-induced peeling of ceiling electrode portion 22a and bottom electrode portion 22b from second solid electrolyte layer 6 and first solid electrolyte layer 4 can be further suppressed. By having the porosity of ceiling electrode portion 22a and bottom electrode portion 22b be 40% or less, stress-induced peeling of ceiling electrode portion 22a and bottom electrode portion 22b from second solid electrolyte layer 6 and first solid electrolyte layer 4 can be further suppressed.
[0083] Furthermore, by setting the maximum pore diameter of the ceiling electrode portion 22a and the bottom electrode portion 22b to 17 μm or less, peeling of the ceiling electrode portion 22a and the bottom electrode portion 22b due to stress can be further suppressed. By setting the maximum pore diameter of the ceiling electrode portion 22a and the bottom electrode portion 22b to 5 μm or more, peeling of the ceiling electrode portion 22a and the bottom electrode portion 22b due to volume expansion caused by TM transformation of zirconia can be further suppressed.
[0084] Furthermore, by making the thickness of ceiling electrode portion 22a and bottom electrode portion 22b 5 μm or more, peeling from the second solid electrolyte layer 6 and the first solid electrolyte layer 4 caused by oxidation of the precious metal in ceiling electrode portion 22a and bottom electrode portion 22b can be suppressed. By making the thickness of ceiling electrode portion 22a and bottom electrode portion 22b 30 μm or less, peeling from the second solid electrolyte layer 6 and the first solid electrolyte layer 4 caused by volume expansion of ceiling electrode portion 22a and bottom electrode portion 22b due to TM transformation of zirconia can be further suppressed.
[0085] The area of the ceiling electrode portion 22a and the bottom electrode portion 22b as viewed in the thickness direction is 5 mm 2 This makes it possible to suppress peeling from the second solid electrolyte layer 6 and the first solid electrolyte layer 4 caused by oxidation of the precious metal in the ceiling electrode portion 22a and the bottom electrode portion 22b. 2 By making the thickness of the upper electrode portion 22a and the lower electrode portion 22b equal to or smaller than this, peeling off of the ceiling electrode portion 22a and the bottom electrode portion 22b from the second solid electrolyte layer 6 and the first solid electrolyte layer 4 caused by volume expansion due to the TM transformation of zirconia can be further suppressed.
[0086] It goes without saying that the present invention is not limited to the above-described embodiment, and can be embodied in various forms within the technical scope of the present invention.
[0087] For example, in the above-mentioned embodiment, the inner pump electrode 22 has the ceiling electrode portion 22a and the bottom electrode portion 22b as a peel-resistant electrode, but is not limited thereto. For example, only one of the ceiling electrode portion 22a and the bottom electrode portion 22b may be a peel-resistant electrode. Even in this case, the electrode portion of the ceiling electrode portion 22a and the bottom electrode portion 22b configured as a peel-resistant electrode can obtain the effect of suppressing peeling from the solid electrolyte layer as in the above-mentioned embodiment. In addition, one or more of the side electrode portion 22c and the side electrode portion 22d may have the same characteristics as a peel-resistant electrode. That is, the inner pump electrode 22 (ceiling electrode portion 22a, bottom electrode portion 22b, side electrode portion 22c, and side electrode portion 22d) may have the characteristics of a peel-resistant electrode as a whole. However, in the above-mentioned embodiment, the ceiling electrode portion 22a and the bottom electrode portion 22b are regarded as different peel-resistant electrodes, and the peel-resistant electrodes disposed on different arrangement surfaces or disposed apart from each other are regarded as different peel-resistant electrodes. For example, even if the ceiling electrode portion 22a, the bottom electrode portion 22b, the side electrode portion 22c, and the side electrode portion 22d all have the characteristics of peel-resistant electrodes, the area of the peel-resistant electrode is not the sum of these electrodes 22a to 22d, but the area value is defined for each of the ceiling electrode portion 22a, the bottom electrode portion 22b, the side electrode portion 22c, and the side electrode portion 22d. In addition, the inner pump electrode 22 may have only one of the ceiling electrode portion 22a and the bottom electrode portion 22b, and the one electrode may be a peel-resistant electrode. In this way, the case where the inner pump electrode 22 itself is one peel-resistant electrode is also included in the case of "having a peel-resistant electrode".
[0088] In the above-described embodiment, the ceiling electrode portion 22a and the bottom electrode portion 22b of the inner pump electrode 22 are each formed in a substantially rectangular parallelepiped shape, but are not limited to this shape. For example, the ceiling electrode portion 22a and the bottom electrode portion 22b may be formed in a cylindrical shape.
[0089] In the above-described embodiment, the inner pump electrode 22 of the electrodes 22, 23, 42, 44, and 51 of the sensor element 101 has a peel-resistant electrode, but this is not limited thereto. It is sufficient that the sensor element 101 has a peel-resistant electrode disposed on the solid electrolyte layer, and for example, it is sufficient that at least one of the electrodes 22, 23, 42, 44, and 51 has a peel-resistant electrode. If at least one of the electrodes 22, 23, 42, 44, and 51 has a peel-resistant electrode, the effect of suppressing peeling from the solid electrolyte layer can be obtained for that peel-resistant electrode, as in the above-described embodiment. For example, at least one of the inner pump electrode 22 and the outer pump electrode 23, which are electrodes constituting a part of the main pump cell 21, may have a peel-resistant electrode. Among the electrodes 22, 23, 42, 44, and 51, at least one of the inner pump electrode 22, the outer pump electrode 23, the measurement electrode 44, and the auxiliary pump electrode 51, which are electrodes constituting at least one part of the pump cells (the main pump cell 21, the auxiliary pump cell 50, and the measurement electrode 44), may have a peel-resistant electrode, or all of them may have a peel-resistant electrode. All of the electrodes 22, 23, 42, 44, and 51 may have a peel-resistant electrode. As with the ceiling electrode portion 22a and the bottom electrode portion 22b of the above-mentioned embodiment, the peel-resistant electrodes other than the ceiling electrode portion 22a and the bottom electrode portion 22b preferably have a porosity of 50% or less, more preferably a porosity of 40% or less, a maximum pore diameter of 5 μm or more and 17 μm or less, a thickness of 5 μm or more and 30 μm or less, and an area viewed along the thickness direction of 5 mm 2 More than 20mm 2 It is preferable that the thickness of the electrode is 5 μm or less or the area is 5 mm or less. Oxidation of the precious metal in the electrode is particularly likely to occur in the electrode through which the pump current flows. For this reason, the inner pump electrode 22, the outer pump electrode 23, the measurement electrode 44, and the auxiliary pump electrode 51, which are electrodes constituting at least a part of each of the pump cells 21, 50, and 41, among the electrodes 22, 23, 42, 44, and 51, are preferably set to 5 μm or more in thickness or 5 mm or less in area. 2It is highly significant that the thickness of the inner pump electrode 22 is 5 μm or more. Furthermore, since the pump current Ip0 of the main pump cell 21, which is located at the most upstream side of the measurement gas flow section, tends to be larger than the pump currents Ip1 and Ip2 of the auxiliary pump cell 50 and the measurement pump cell 41, the inner pump electrode 22 is particularly susceptible to oxidation of the precious metal. From this viewpoint, it is preferable that at least the inner pump electrode 22 of the electrodes 22, 23, 42, 44, 51 has a peel-resistant electrode, and further, the thickness of the peel-resistant electrode is 5 μm or more and the area is 5 mm 2 More preferably, the number of electrodes is set to 1 or more. In addition, even when one or more of the electrodes 22, 23, 42, 44, 51 have a peel-resistant electrode, as described above, the peel-resistant electrodes arranged on different arrangement surfaces or arranged at a distance from each other are regarded as separate peel-resistant electrodes. For example, even when the ceiling electrode portion 51a and the bottom electrode portion 51b of the auxiliary pump electrode 51 are both peel-resistant electrodes, the area of the peel-resistant electrode is not the sum of the ceiling electrode portion 51a and the bottom electrode portion 51b, but the area values are defined separately for the ceiling electrode portion 51a and the bottom electrode portion 51b. Similarly, even when the ceiling electrode portion 22a and the ceiling electrode portion 51a are both peel-resistant electrodes, the ceiling electrode portion 22a and the ceiling electrode portion 51a are regarded as separate peel-resistant electrodes because they are separated from each other. In addition, the case where one or more of the electrodes 22, 23, 42, 44, 51 are one peel-resistant electrode is also included in the case of "having a peel-resistant electrode". For example, in the above-described embodiment, the measurement electrode 44 is one electrode disposed on one arrangement surface, but the case where the measurement electrode 44 is a peel-resistant electrode is also included in the case where "the measurement electrode 44 has a peel-resistant electrode." The same applies to the outer pump electrode 23 and the reference electrode 42 in the above-described embodiment.
[0090] In the above-described embodiment, the outer pump electrode 23 serves as an electrode paired with the inner pump electrode 22 in the main pump cell 21 (also referred to as the outer main pump electrode), as an electrode paired with the auxiliary pump electrode 51 in the auxiliary pump cell 50 (also referred to as the outer auxiliary pump electrode), and as an electrode paired with the measurement electrode 44 in the measurement pump cell 41 (also referred to as the outer measurement electrode), but is not limited to this. Any one or more of the outer main pump electrode, the outer auxiliary pump electrode, and the outer measurement electrode may be provided outside the element body separately from the outer pump electrode 23 so as to be in contact with the measured gas.
[0091] In the above-described embodiment, the outer pump electrode 23 is exposed to the outside of the sensor element 101, but the present invention is not limited thereto and the outer pump electrode 23 may be provided outside the element body (layers 1 to 6) so as to be in contact with the measured gas. For example, the sensor element 101 may include a porous protective layer that covers the element body (layers 1 to 6), and the outer pump electrode 23 may also be covered by the porous protective layer.
[0092] In the above-described embodiment, the sensor element 101 of the gas sensor 100 includes the first internal space 20, the second internal space 40, and the third internal space 61, but is not limited thereto. For example, the sensor element 201 shown in FIG. 4 may not include the third internal space 61. In the modified sensor element 201 shown in FIG. 4, the gas inlet 10, the first diffusion rate-controlling section 11, the buffer space 12, the second diffusion rate-controlling section 13, the first internal space 20, the third diffusion rate-controlling section 30, and the second internal space 40 are adjacently formed in this order between the lower surface of the second solid electrolyte layer 6 and the upper surface of the first solid electrolyte layer 4 in a manner that they communicate with each other. The measurement electrode 44 is disposed on the upper surface of the first solid electrolyte layer 4 in the second internal space 40. The measurement electrode 44 is covered with the fourth diffusion rate-controlling section 45. The fourth diffusion rate-controlling section 45 is made of alumina (Al 2 O 3) or the like. The fourth diffusion rate-controlling portion 45 has a role of limiting the amount of NOx flowing into the measurement electrode 44, similar to the fourth diffusion rate-controlling portion 60 of the above-described embodiment. The fourth diffusion rate-controlling portion 45 also functions as a protective film for the measurement electrode 44. The ceiling electrode portion 51a of the auxiliary pump electrode 51 is formed up to just above the measurement electrode 44. Even with the sensor element 201 having such a configuration, the NOx concentration can be detected based on, for example, the pump current Ip2, similar to the above-described embodiment. In this case, the periphery of the measurement electrode 44 functions as a measurement chamber.
[0093] In the above-mentioned embodiment, the sensor element 101 detects the NOx concentration in the measured gas, but is not limited to this, as long as it detects the concentration of the specific gas in the measured gas. For example, the specific gas concentration may be other oxide concentrations, not limited to NOx. When the specific gas is an oxide, oxygen is generated when the specific gas itself is reduced in the third internal space 61 as in the above-mentioned embodiment, so that the measurement pump cell 41 can obtain a detection value (e.g., pump current Ip2) corresponding to this oxygen to detect the specific gas concentration. In addition, the specific gas may be a non-oxide such as ammonia. When the specific gas is a non-oxide, the specific gas is converted to an oxide (e.g., ammonia is converted to NO) and oxygen is generated when the converted gas is reduced in the third internal space 61, so that the measurement pump cell 41 can obtain a detection value (e.g., pump current Ip2) corresponding to this oxygen to detect the specific gas concentration. For example, the inner pump electrode 22 of the first internal space 20 functions as a catalyst, so that ammonia can be converted to NO in the first internal space 20.
[0094] In the above-mentioned embodiment, the element body 102 of the sensor element 101 is a laminate having a plurality of solid electrolyte layers (layers 1 to 6), but is not limited thereto. The element body 102 of the sensor element 101 may include at least one solid electrolyte layer having oxygen ion conductivity. For example, in FIG. 1, the layers 1 to 5 other than the second solid electrolyte layer 6 may be layers made of a material other than a solid electrolyte layer (for example, a layer made of alumina). In this case, each electrode of the sensor element 101 may be disposed on the second solid electrolyte layer 6. For example, the measurement electrode 44 in FIG. 1 may be disposed on the lower surface of the second solid electrolyte layer 6. Also, the reference gas introduction space 43 may be disposed on the spacer layer 5 instead of the first solid electrolyte layer 4, the reference gas introduction layer 48 may be disposed between the second solid electrolyte layer 6 and the spacer layer 5 instead of between the first solid electrolyte layer 4 and the third substrate layer 3, and the reference electrode 42 may be disposed behind the third internal space 61 and on the lower surface of the second solid electrolyte layer 6.
[0095] In the above-described embodiment, the control unit 96 sets (feedback controls) the target value V0* of the voltage V0 based on the pump current Ip1 so that the pump current Ip1 becomes the target value Ip1*, and feedback controls the pump voltage Vp0 so that the voltage V0 becomes the target value V0*, but other control may be performed. For example, the control unit 96 may feedback control the pump voltage Vp0 based on the pump current Ip1 so that the pump current Ip1 becomes the target value Ip1*. That is, the control unit 96 may omit obtaining the voltage V0 from the main pump control oxygen partial pressure detection sensor cell 80 and setting the target value V0*, and directly control the pump voltage Vp0 (and thus control the pump current Ip0) based on the pump current Ip1. EXAMPLES
[0096] Hereinafter, specific examples of sensor elements will be described as examples, although the present invention is not limited to the following examples.
[0097] [Examples 1 to 20, Comparative Examples 1 to 4] The sensor elements 101 were fabricated by the same manufacturing method as the gas sensor 100 of the embodiment shown in FIG. 1 and FIG. 2, and used as Examples 1 to 20 and Comparative Examples 1 to 4. In each of Examples 1 to 20 and Comparative Examples 1 to 4, the inner pump electrode 22 was made of Pt and ZrO 2 and a stabilizer. In the sensor elements 101 of Examples 1 to 20 and Comparative Examples 1 to 4, the type of stabilizer used, the TM ratio of zirconia, the porosity, the maximum pore diameter, the thickness, and the area of the bottom electrode portion 22b of the inner pump electrode 22 were changed in various ways as shown in Table 1 by the above-mentioned methods. The ceiling electrode portion 22a of the inner pump electrode 22 was formed using the same paste as the bottom electrode portion 22b. A plurality of sensor elements 101 of Examples 1 to 20 and Comparative Examples 1 to 4 were each produced.
[0098] [TM ratio measurement] The TM ratios shown in Table 1 were measured for each of Examples 1 to 20 and Comparative Examples 1 to 4 by the above-mentioned method using one of the plurality of sensor elements 101 described above. The Raman spectrum was measured using a laser Raman spectrometer LabRAM ARAMIS manufactured by Horiba, Ltd., and the operation software LabSpec. The optical system was a Czerny-Turner type spectrometer using the backscattering method, and a semiconductor pumped solid-state laser (DPSS, 532 nm) was used as the light source. Before measuring the sample, calibration was performed using a Si wafer. The Raman spectrum was measured with a hole (confocal hole diameter) of 400 μm and a central wave number of the spectrometer of 520 cm. -1 The slit was 100 μm, the grating was 1800 gr / mm, and the objective lens was 100x. The measurement was performed in Duoscan mode. The measurement range was a 50 μm × 50 μm range on the upper surface of the bottom electrode part 22b of the inner pump electrode 22, and the TM ratio was calculated from the average intensity obtained within that range, and was used as the TM ratio of the bottom electrode part 22b.
[0099] [Table 1]
[0100] [Measurement of maximum stress before durability test] For each of Examples 1 to 20 and Comparative Examples 1 to 4, the maximum stress of the bottom electrode portion 22b of the inner pump electrode 22 was measured by a Sebastian test using one of the above-mentioned multiple sensor elements 101 before the durability tests (autoclave test and continuous atmospheric test) described below were performed. The measuring machine used was an AG-X (100 kN) manufactured by Shimadzu Corporation. During the test, the sensor element 101 was first cut so as to cut the spacer layer 5 along the front-rear and left-right directions to expose the upper surface of the bottom electrode portion 22b of the inner pump electrode 22 inside the sensor element 101. Next, the bottom electrode portion 22b was pulled upward at a speed of 0.5 mm / min, and the maximum stress of the bottom electrode portion 22b was measured based on the load when the bottom electrode portion 22b peeled off from the first solid electrolyte layer 4. The higher the maximum stress, the more suppressed the peeling of the bottom electrode portion 22b due to the stress caused by thermal expansion during use of the above-mentioned sensor element 101 is (the peeling resistance is high). Table 1 shows the maximum stress [MPa] before the durability test for each of Examples 1 to 20 and Comparative Examples 1 to 4.
[0101] [Autoclave test] For each of Examples 1 to 20 and Comparative Examples 1 to 4, an autoclave test was performed using one of the above-mentioned multiple sensor elements 101 to evaluate the peeling resistance of the bottom electrode portion 22b of the inner pump electrode 22. Specifically, for each of Examples 1 to 20 and Comparative Examples 1 to 4, the sensor element 101 and a container with an internal volume of 100 milliliters containing about 3 g of water were placed in an autoclave, and left for 10 hours at a temperature of 250°C, at which TM transformation is likely to occur. Thereafter, the sensor element 101 was removed from the autoclave, and the sensor element 101 was cut to expose the bottom electrode portion 22b, and the presence or absence and the degree of peeling of the bottom electrode portion 22b were confirmed. When the bottom electrode portion 22b was not peeled off from the first solid electrolyte layer 4, the peel resistance was judged as excellent (A). When a part of the bottom electrode portion 22b was peeled off from the first solid electrolyte layer 4, the peel resistance was judged as good (B). When the bottom electrode portion 22b was completely peeled off from the first solid electrolyte layer 4, the peel resistance was judged as poor (F). The higher the evaluation of the peel resistance after the autoclave test, the more the peeling of the bottom electrode portion 22b from the first solid electrolyte layer 4 caused by the volume expansion due to the TM transformation of zirconia described above is suppressed. The evaluation results of the peel resistance in the autoclave test for each of Examples 1 to 20 and Comparative Examples 1 to 4 are shown in Table 1.
[0102] [Continuous atmospheric testing] For each of Examples 1 to 20 and Comparative Examples 1 to 4, an air continuous test was performed using one of the above-mentioned multiple sensor elements 101 to evaluate the peeling resistance of the bottom electrode portion 22b of the inner pump electrode 22. Specifically, first, for each of Examples 1 to 20 and Comparative Examples 1 to 4, the control unit 96 was connected to the sensor element 101, and the sensor element 101 was exposed to the air atmosphere. In this state, the control unit 96 continuously performed the heater control process, the adjustment pump control process, the measurement pump control process, and the like in the same manner as in the above-mentioned example of using the gas sensor 100, thereby driving the sensor element 101 for 1000 hours. Thereafter, the sensor element 101 was cut to expose the bottom electrode portion 22b, and the presence or absence and the degree of peeling of the bottom electrode portion 22b were confirmed. When the bottom electrode portion 22b was not peeled off from the first solid electrolyte layer 4, the peel resistance was judged as excellent (A); when a part of the bottom electrode portion 22b was peeled off from the first solid electrolyte layer 4, the peel resistance was judged as good (B); and when the bottom electrode portion 22b was completely peeled off from the first solid electrolyte layer 4, the peel resistance was judged as poor (F). In the continuous air test, the oxygen concentration around the bottom electrode portion 22b is high, so the deterioration of the bottom electrode portion 22b (oxidation of the precious metal) is promoted. Therefore, the higher the evaluation of the peel resistance after the continuous air test, the more the peeling from the first solid electrolyte layer 4 caused by the oxidation of the precious metal in the bottom electrode portion 22b is suppressed. Table 1 shows the evaluation results of the peel resistance in the continuous air test for each of Examples 1 to 20 and Comparative Examples 1 to 4.
[0103] As can be seen from Table 1, in Examples 1 to 20 in which the TM ratio of the zirconia of the bottom electrode part 22b is 1 to 10 and the porosity is 3% to 65%, the maximum stress before the durability test was 50 MPa or more, and the evaluation of the peeling resistance after the autoclave test was excellent (A) or good (B). In contrast, in Comparative Example 1 in which the TM ratio of the bottom electrode part 22b is less than 1 and Comparative Example 3 in which the porosity is more than 65%, the maximum stress before the durability test was a low value of 30 MPa. In addition, in Comparative Example 2 in which the TM ratio of the bottom electrode part 22b is more than 10 and Comparative Example 4 in which the porosity is less than 3%, the evaluation of the peeling resistance after the autoclave test was poor (F). From these results, it was confirmed that the peeling of the bottom electrode part 22b from the first solid electrolyte layer 4 due to stress can be suppressed by having the TM ratio of the zirconia of the bottom electrode part 22b be 1 or more and the porosity be 65% or less. It was also confirmed that when the TM ratio of the zirconia in the bottom electrode portion 22b is 10 or less and the porosity is 3% or more, peeling caused by volume expansion due to TM transformation of the zirconia in the bottom electrode portion 22b can be suppressed.
[0104] Comparing Examples 1 to 18 in which the TM ratio of the zirconia of the bottom electrode part 22b is 1 to 10, the porosity is 3% to 65%, and the maximum pore size is 5 μm to 17 μm, it was confirmed that the higher the TM ratio and / or the lower the porosity, the higher the maximum stress before the durability test and the higher the effect of suppressing peeling due to stress. In addition, comparing Examples 1 to 10 and 13 to 18 except for Examples 11 and 12 in which the TM ratio is relatively high and the maximum stress before the durability test is high, it is considered that if the porosity is 50% or less, the value of the maximum stress before the durability test will be a relatively high value of 60 MPa or more regardless of the TM ratio (even if the TM ratio is close to the lower limit value 1 of 1 to 10). In addition, if the porosity is 40% or less, the value of the maximum stress before the durability test will be a relatively high value of 80 MPa or more regardless of the TM ratio (even if the TM ratio is close to the lower limit value 1 of 1 to 10).
[0105] The TM ratio of the zirconia in the bottom electrode portion 22b is 1 to 10, the porosity is 3% to 65%, the thickness is 5 μm to 30 μm, and the area is 5 mm 2 More than 20mm 2 Among the following Examples 1 to 14, 19, and 20, Example 19, in which the maximum pore diameter of the bottom electrode portion 22b exceeds 17 μm, had a maximum stress of 50 MPa before the durability test. In contrast, Examples 1 to 14, and 20, in which the maximum pore diameter is 17 μm or less, all had relatively high maximum stresses of 60 MPa or more before the durability test. From these results, it is considered that by making the maximum pore diameter of the bottom electrode portion 22b 17 μm or less, peeling of the bottom electrode portion 22b due to stress can be further suppressed.
[0106] The TM ratio of the zirconia in the bottom electrode portion 22b is 1 to 10, the porosity is 3% to 65%, the thickness is 5 μm to 30 μm, and the area is 5 mm 2 More than 20mm 2 Among the following Examples 1 to 14, 19, and 20, Example 20, in which the maximum pore diameter of the bottom electrode part 22b is less than 5 μm, was evaluated as good (B) in terms of peel resistance after the autoclave test. In contrast, Examples 1 to 14, in which the maximum pore diameter is 5 μm or more, were all evaluated as excellent (A) in terms of peel resistance after the autoclave test. From these results, it is considered that by having the maximum pore diameter of the bottom electrode part 22b be 5 μm or more, peeling due to volume expansion due to TM transformation of zirconia in the bottom electrode part 22b can be further suppressed. In addition, although Example 19 has a maximum pore diameter of 5 μm or more, the evaluation of peel resistance after the autoclave test was good (B). This is considered to be due to the fact that the maximum pore diameter of Example 19 exceeds 17 μm, and the strength of the bottom electrode part 22b itself is lower than that of Examples 1 to 14. In other words, since stress is also applied to the bottom electrode portion 22b due to the volume expansion caused by the TM transformation of the bottom electrode portion 22b, it is believed that the strength of the bottom electrode portion 22b itself in Example 19 is lower than that of Examples 1 to 14, which is why the peel resistance after the autoclave test was rated good (B).
[0107] The TM ratio of the zirconia in the bottom electrode portion 22b is 1 to 10, the porosity is 3% to 65%, the maximum pore diameter is 5 μm to 17 μm, and the area is 5 mm 2 More than 20mm 2 Among the following Examples 1 to 16, Example 15, in which the thickness of bottom electrode part 22b exceeds 30 μm, was evaluated as good (B) in peel resistance after autoclave testing. In contrast, Examples 1 to 14 and 16, in which the thickness is 30 μm or less, were all evaluated as excellent (A) in peel resistance after autoclave testing. From these results, it is considered that by making the thickness of bottom electrode part 22b 30 μm or less, peeling due to volume expansion caused by TM transformation of zirconia in bottom electrode part 22b can be further suppressed.
[0108] The TM ratio of the zirconia in the bottom electrode portion 22b is 1 to 10, the porosity is 3% to 65%, the maximum pore diameter is 5 μm to 17 μm, and the area is 5 mm 2 More than 20mm 2 Among the following Examples 1 to 16, Example 16, in which the thickness of bottom electrode portion 22b is less than 5 μm, was evaluated as good (B) in terms of peel resistance after the continuous atmospheric test. In contrast, Examples 1 to 15, in which the thickness is 5 μm or more, were all evaluated as excellent (A) in terms of peel resistance after the continuous atmospheric test. From these results, it is considered that by making bottom electrode portion 22b thicker than 5 μm, peeling from first solid electrolyte layer 4 due to oxidation of the precious metal in bottom electrode portion 22b can be suppressed.
[0109] Among Examples 1 to 14, 17, and 18 in which the TM ratio of the zirconia in the bottom electrode portion 22b is 1 to 10, the porosity is 3% to 65%, the maximum pore diameter is 5 μm to 17 μm, and the thickness is 5 μm to 30 μm, 2 In Example 17, which has an area exceeding 20 mm 2 , the peel resistance after the autoclave test was evaluated as good (B). 2 In the following Examples 1 to 14 and 18, the peel resistance after the autoclave test was evaluated as excellent (A). 2It is believed that by keeping the thickness of the bottom electrode portion 22b at or below 100 nm, peeling caused by volume expansion due to TM transformation of zirconia in the bottom electrode portion 22b can be further suppressed.
[0110] Among Examples 1 to 14, 17, and 18 in which the TM ratio of the zirconia in the bottom electrode portion 22b is 1 to 10, the porosity is 3% to 65%, the maximum pore diameter is 5 μm to 17 μm, and the thickness is 5 μm to 30 μm, 2 In Example 18, in which the area was less than 5 mm, the peel resistance after the continuous air test was evaluated as good (B). 2 In all of the above-mentioned Examples 1 to 14 and 17, the evaluation of the peel resistance after the continuous atmospheric test was excellent (A). 2 It is believed that the above can suppress peeling from first solid electrolyte layer 4 due to oxidation of the precious metal in bottom electrode portion 22b.
[0111] In Example 19, like Examples 1 to 14, the thickness of the bottom electrode portion 22b is 5 μm or more and 30 μm or less and the area is 5 mm 2 More than 20mm 2 As shown below, the evaluation of the peeling resistance after the continuous atmospheric test was good (B). This is because, as described above, the bottom electrode part 22b of Example 19 has a maximum pore size exceeding 17 μm, and the strength of the bottom electrode part 22b itself is lower than that of Examples 1 to 14, so that when the inner pump electrode 22 becomes brittle due to oxidation of the precious metal in the bottom electrode part 22b, the bottom electrode part 22b of Example 19 is more likely to peel off than that of Examples 1 to 14.
[0112] In all of Examples 1 to 8, 11 to 20 in which yttria was used as the stabilizer, Example 9 in which calcia was used as the stabilizer, and Example 10 in which magnesia was used as the stabilizer, it was confirmed that similar peeling resistance was obtained when the TM ratio of the zirconia in the bottom electrode portion 22b was 1 or more and 10 or less and the porosity was 3% or more and 65% or less.
[0113] Results similar to those in Table 1 were obtained for the ceiling electrode portion 22a, which was formed using the same paste as the bottom electrode portion 22b. [Industrial Applicability]
[0114] INDUSTRIAL APPLICABILITY The present invention can be used in a gas sensor for detecting the concentration of a specific gas, such as NOx, in a measurement gas, such as an exhaust gas from an automobile. [Explanation of symbols]
[0115] 1 first substrate layer, 2 second substrate layer, 3 third substrate layer, 4 first solid electrolyte layer, 5 spacer layer, 6 second solid electrolyte layer, 10 gas inlet, 11 first diffusion rate limiting portion, 12 buffer space, 13 second diffusion rate limiting portion, 20 first internal space, 21 main pump cell, 22 inner pump electrode, 22a ceiling electrode portion, 22b bottom electrode portion, 22c, 22d side electrode portion, 23 outer pump electrode, 24 variable power supply, 30 third diffusion rate limiting portion, 40 second internal space, 41 measurement pump cell, 42 reference electrode, 43 reference gas introduction space, 44 measurement electrode, 46 variable power supply, 48 reference gas introduction layer, 49 reference gas introduction portion, 49a inlet portion, 50 auxiliary pump cell, 51 auxiliary pump electrode, 51a ceiling electrode portion, 51b bottom electrode portion, 52 Variable power source, 60 fourth diffusion rate limiting portion, 61 third internal space, 70 heater portion, 71 heater connector electrode, 72 heater, 73 through hole, 74 heater insulating layer, 75 pressure release hole, 76 heater power source, 80 oxygen partial pressure detection sensor cell for controlling main pump, 81 oxygen partial pressure detection sensor cell for controlling auxiliary pump, 82 oxygen partial pressure detection sensor cell for controlling measurement pump, 83 sensor cell, 95 control device, 96 control unit, 97 CPU, 98 memory unit, 100 gas sensor, 101, 201 sensor element, 102 element body
Claims
1. A sensor element for detecting a concentration of a specific gas in a measurement gas, comprising: an element body having an oxygen ion conductive solid electrolyte layer and a measurement gas flow section for introducing and flowing the measurement gas therein; a peel-off resistant electrode disposed on the solid electrolyte layer of the element body; Equipped with The peel-off resistant electrode contains a precious metal and zirconia, and has a TM ratio (Ht / Hm) of a peak height Ht of a T phase of zirconia to a peak height Hm of an M phase of zirconia in a Raman spectrum measured using Raman spectroscopy, which is 1 or more and 10 or less, and a porosity of 3% or more and 65% or less. Sensor element.
2. The peel-resistant electrode has a porosity of 50% or less. The sensor element according to claim 1 .
3. The peel-resistant electrode has a porosity of 40% or less. The sensor element according to claim 1 .
4. The peel-resistant electrode has a maximum pore diameter of 5 μm or more and 17 μm or less. The sensor element according to any one of claims 1 to 3.
5. The peel-resistant electrode has a thickness of 5 μm or more and 30 μm or less. The sensor element according to any one of claims 1 to 3.
6. The peel-resistant electrode has an area of 5 mm when viewed in the thickness direction. 2 More than 20mm 2 Below is the The sensor element according to any one of claims 1 to 3.
7. The sensor element according to any one of claims 1 to 3, a pump cell including an inner pump electrode disposed in the measurement gas flow portion and an outer pump electrode disposed in a portion of the element body exposed to the measurement gas; Equipped with At least one of the inner pump electrode and the outer pump electrode has the peeling-resistant electrode. Sensor element.
8. The pump cell includes: a main pump cell including an inner main pump electrode as the inner pump electrode and an outer main pump electrode as the outer pump electrode, the inner main pump electrode being disposed in a first internal space of the measurement gas flow portion; an auxiliary pump cell including an inner auxiliary pump electrode as the inner pump electrode and an outer auxiliary pump electrode as the outer pump electrode, the inner auxiliary pump electrode being disposed in a second inner space downstream of the first inner space in the measurement gas flow portion; a measurement pump cell including an inner measurement electrode as the inner pump electrode and an outer measurement electrode as the outer pump electrode, the inner measurement electrode being disposed in a measurement chamber downstream of the second internal space in the measurement target gas flow portion; Equipped with The inner main pump electrode includes the anti-peeling electrode. The sensor element according to claim 7.
9. A gas sensor comprising the sensor element according to any one of claims 1 to 3.
Citation Information
Patent Citations
Nondestructive inspection method and nondestructive inspection device
JP2006084179A
Translucent zirconia sintered body and manufacturing method thereof and application thereof
JP2017105689A
SENSOR ELEMENT OF NOx SENSOR AND METHOD FOR MANUFACTURING SENSOR ELEMENT OF NOx SENSOR
JP2022113129A
Method for manufacturing gas sensor element, gas sensor element, and gas sensor
WO2020246174A1
Gas sensor
JP2022091669A