Pipe inner surface Anti-corrosion pipe and manufacturing method therefor
By removing the laitance and paste layers from centrifugally cast iron pipes and applying a powder coating without heating, the method addresses corrosion and maintains pipe integrity and flow efficiency.
Patent Information
- Application Number
- JP2023055410
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Filing Date
- 2023-03-30
- Publication Date
- 2024-10-11
- Estimated Expiration
- Not applicable · inactive patent
AI Technical Summary
Cast iron pipes used in water supply systems face challenges with corrosion, particularly due to the formation of irregularities on the inner surface during centrifugal casting, which affect water flow and require extensive polishing, and heating for epoxy resin coating can weaken the mortar lining or cause cracks.
A method involving centrifugal casting followed by removal of the laitance and paste layers, leaving only the mortar layer, and applying a powder coating layer without heating the entire pipe, ensuring a stable and smooth inner surface.
The method results in a stable powder coating layer that prevents corrosion and maintains the strength of the mortar lining, reducing labor and avoiding cracks, even with thermosetting resins.
Smart Images

Figure 2024142978000001_ABST
Abstract
Description
[Technical field]
[0001] This invention relates to corrosion protection of cast iron pipes. [Background technology]
[0002] Ductile iron pipes are stronger than plastic pipes, and are widely used for water pipes, including trunk water pipes. However, since ductile iron pipes are made of cast iron, they will corrode in the state they are cast, so both the exterior and interior, including the joints, must be thoroughly anti-corrosive treated before use. Furthermore, when used in a water supply system, water quality must be hygienic, and when used in a sewer system, acid resistance, etc. are required. Due to these demands, mortar linings and epoxy resin powder coatings are applied to the interior of cast iron pipes. In particular, epoxy resin powder coating is more resistant to acids than mortar linings, and is often used to coat the interior of cast iron pipes for sewer systems.
[0003] Straight pipes are often manufactured using centrifugal casting, mainly because they are easier to manufacture. However, unlike the outer surface, the inner surface is cast without contacting a metal mold or sand form, so it is easy for fine irregularities to form on the surface. If these irregularities affect the smoothness of the surface of the mortar lining or epoxy resin powder coating, they will create resistance to the water passing through the inner surface, slowing down the water flow, so it is desirable to make the inner surface as smooth as possible. For this reason, the inner surface is polished to increase its smoothness. However, the inner surface polishing process, which involves scraping the surface of the cast iron pipe itself, is time-consuming.
[0004] Patent Document 1 describes a procedure in which the polishing process after casting is omitted, a mortar lining is applied once, and then the lathance layer (impurity layer) is polished off, followed by an epoxy resin powder coating to ensure smoothness. The lathance layer is a layer that forms on the surface during mortar lining, and is a layer of lightweight impurities that has gathered further inward than the mortar layer, which has a sufficient amount of aggregate (sand), and the paste layer, which forms on the surface side of the mortar layer and has less aggregate. Removing this lathance layer by polishing can greatly reduce the amount of work required compared to a polishing process that scrapes the surface of the cast iron pipe itself.
[0005] However, when applying epoxy resin powder coating, it is necessary to heat the cement mortar layer in advance so that the powder coating can easily melt. This heating may cause the strength of the mortar lining to decrease or cracks to form. As a means to avoid this, Patent Document 2 proposes a method in which, after removing the latency layer from the surface of the mortar lining, the powder coating is supplied to the inner surface of the pipe without heating and made uniform by centrifugal force, and then an infrared heater is inserted into the inside of the pipe to heat and melt only the powder coating layer to form a surface coating layer. [Prior art documents] [Patent documents]
[0006] [Patent Document 1] Japanese Patent Application Publication No. 9-158113 [Patent Document 2] Japanese Patent Application Publication No. 9-276794 Summary of the Invention [Problem to be solved by the invention]
[0007] However, the length of cast iron pipes used for water supply is about 4 to 6 m, and it is difficult to insert an infrared heater from the outside to the inside of the pipe to heat it accurately. Also, when using thermosetting powder paint, there are cases where a sufficient curing reaction cannot be obtained by simply heating the surface layer after applying it with an infrared heater.
[0008] Therefore, the object of this invention is to provide a method for preventing the deterioration of the strength of the mortar lining and the occurrence of cracks due to heating when powder coating the inner surface of a cast iron pipe, while minimizing the increase in the amount of work required and providing sufficient corrosion protection for the inner surface. [Means for solving the problem]
[0009] The present invention relates to The inner surface of the cast iron pipe has a mortar layer derived from the mortar lining and a powder coating layer formed by melting the powder coating, The powder coating layer solves the above problem by using an inner surface corrosion-resistant cast iron pipe that is in contact with the inner surface of the mortar layer.
[0010] That is, when the inner surface of a cast iron pipe is lined with mortar, the cement mortar layer formed is composed of a mortar layer with sufficient aggregate, a paste layer with less aggregate formed on the surface side of the mortar layer, and a laitance layer of light impurities that has gathered further inward than the paste layer, in that order from the inner surface of the cast iron pipe. Conventionally, the laitance layer was removed by grinding and then a thin layer of liquid paint was applied on top of it, but this invention is characterized in that not only the laitance layer but also the paste layer with low strength is removed to expose the mortar layer, and then powder coating is performed. This is because it was found that it is not the entire cement mortar layer but mainly the paste layer with less aggregate and low strength that is prone to strength loss and cracks when the cement mortar layer is heated. By forming a powder coating layer on the mortar layer from which the paste layer has been removed, the layer becomes thinner when the paste layer is removed, but only the strong parts of the mortar layer remain, so that the stability during heating is increased, and powder coating can be performed in such a way that the entire layer can be heated and sufficiently cured, and the obtained powder coating layer can be stabilized. In particular, even if the powder coating is a thermosetting coating, it can be sufficiently cured.
[0011] The method for manufacturing an internally corrosion-resistant cast iron pipe according to the present invention includes the following steps: supplying cement mortar onto the inner surface of the cast iron pipe while rotating the pipe to form a cement mortar layer; a step of polishing and removing the laitance layer and the paste layer present on the surface side of the cement mortar layer after the cement mortar layer has hardened, so that only the mortar layer remains; heating the entire cast iron pipe on which the mortar layer remains; applying a powder coating to the surface of the mortar layer after heating; A method for carrying out the above can be adopted.
[0012] In addition, the manufacturing method of the internally corrosion-resistant cast iron pipe according to the present invention includes the steps of: A configuration may be adopted in which the temperature of the cast iron pipe in the step of applying the powder paint immediately after heating is 240° C. or higher and 330° C. or lower. This allows the powder paint to be sufficiently cured even when the resin used in the paint is a thermosetting resin. Effect of the Invention
[0013] In the manufacturing method of the internally corrosion-resistant cast iron pipe according to the present invention, the paste layer of the cement mortar layer is removed, and only the mortar layer containing sufficient aggregate remains, so that even if the entire pipe is heated, the strength of the mortar layer and the occurrence of cracks can be suppressed. This allows stable coating with powder paint by heating the entire pipe. Furthermore, even in applications where a thick powder coating is required, it can be cured by sufficient heating. The internally corrosion-resistant cast iron pipe thus obtained, in which the mortar layer and the powder coating layer are in contact with each other, i.e., the paste layer is not interposed between these two layers, has few cracks and a stable powder coating layer. [Brief description of the drawings]
[0014] [Figure 1] (a) is a cross-sectional view showing the outline of the internally corrosion-resistant cast iron pipe according to the present invention, (b) is an enlarged cross-sectional view of the straight pipe portion of (a). [Diagram 2] (a) A cross-sectional view of the step of forming a cement mortar layer in the manufacture of an internally corrosion-resistant cast iron pipe according to the present invention; (b) A cross-sectional view of the step of the cement mortar layer hardening and splitting; (c) A cross-sectional view of the step of removing the paste layer and the laitance layer; (d) A cross-sectional view of the step of forming a powder coating layer on the mortar layer. [Diagram 3] (a) A cross-sectional view of an example of a shape when forming a cement mortar layer, (b) a side view of (a), and (c) a side view of another example of the shape. [Figure 4] Cross-sectional view when vibration is applied [Diagram 5] (a) Cross-sectional view of an example of a shape when polishing a cement mortar layer, (b) side view of (a), (c) side view of another example of a shape [Figure 6] (a) A cross-sectional view of an example of a form when a powder coating layer is formed, (b) a side view of (a), and (c) a side view of another example of the form. [Figure 7] A photograph showing the state of the separation of the cement mortar layer formed on the surface of the cast iron pipe in the example. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0015] Hereinafter, the embodiment of the present invention will be described in detail. This invention relates to an internally corrosion-protected cast iron pipe in which a corrosion-protective layer 20 is provided on the inner surface of a straight section 13 formed between an insertion port 11 and a receiving port 12 in a straight cast iron pipe 1 as shown in Fig. 1(a). As shown in the enlarged cross-sectional view of Fig. 1(b), the corrosion-protective layer 20 in this invention has a mortar layer 23 and a powder coating layer 22, and these two layers are in contact with each other. The mortar layer 23 is made of mortar containing a large amount of aggregate such as sand, and the powder coating layer 22 is made of hardened powder paint, which is a resin.
[0016] The manufacturing procedure of the inner surface corrosion-resistant cast iron pipe having the corrosion-resistant layer 20 will be described with reference to Figs. 2(a)-(d). First, the inner surface of the cast iron pipe 1 is coated with a cement mortar layer 21 lined with cement mortar (Fig. 2(a)). Due to the centrifugal force applied during and after coating, the distribution of aggregate (sand) contained in the cement mortar layer 21 is biased, and the aggregate content increases toward the cast iron pipe 1 side (outer periphery). The outer periphery side (lower side in the figure) where there is more aggregate is called the mortar layer 23, and the inner periphery side (upper side in the figure) where there is less aggregate is called the paste layer 24. Furthermore, light impurities contained in the cement mortar gather on the paste layer 24, forming a laitance layer 25. The state in which the cement mortar layer 21 is separated is shown in Fig. 2(b).
[0017] Although there is no clear boundary between the mortar layer 23 and the paste layer 24, the difference between them is such that a person skilled in the art can clearly distinguish the presence or absence of large aggregate by visual inspection. The paste layer 24 contains almost no large aggregate, and even if it does contain some fine sand, it is mixed in.
[0018] Of the cement mortar layer 21 thus separated, the laitance layer 25 and paste layer 24 on the surface side are scraped away to expose the mortar layer 23 (Fig. 2(c)). It is acceptable for not only the paste layer 24 but also the mortar layer 23 to be scraped away to some extent. As described above, the paste layer 24 contains almost no aggregate, so when the aggregate can be clearly seen on the scraped surface, it can be determined that the mortar layer 23 has been reached. A powder coating layer 22 made of powder paint is formed on the inner surface of the exposed mortar layer 23 (Fig. 2(d)). In this way, the corrosion protection layer 20 is formed where the mortar layer 23 and the powder coating layer 22 are in contact with each other.
[0019] A centrifugal cast cast iron pipe can be suitably used as the cast iron pipe 1 used in the present invention. The type of cast iron pipe is not particularly limited, and a general ductile iron pipe can be used.
[0020] The cement mortar used in this invention can be a general mortar M made of cement containing aggregate. The ratio of cement to aggregate in mortar M can be about 1.6 to 2.4 parts by mass of cement to aggregate.
[0021] Examples of powder paints that can be used in this invention include epoxy resin powder paints, acrylic resin powder paints, etc. In particular, since the entire pipe must be sufficiently heated before use, even thermosetting resins such as epoxy resin powder paints can be suitably used.
[0022] An example of the procedure for performing mortar lining with mortar M will be described with reference to the cross-sectional view of Fig. 3(a) and the side view of Fig. 3(b). The construction device for performing mortar lining comprises a rotating roller 31 and an injection cart 32. The injection cart 32 is provided with a tank 33 for storing mortar M, and an injection lance 34 for transporting and injecting the mortar M into the inner surface of the cast iron pipe 1 (the insertion port 11 and the receiving port 12 are omitted for illustration purposes. The same applies to the following drawings). A conveyor for transporting the mortar M is provided inside the injection lance 34, and the mortar M sent by the conveyor is injected into the inner surface of the cast iron pipe 1 from a nozzle 36 at the tip of the injection lance 34.
[0023] The cast iron pipe 1 is placed between a pair of rotating rollers 31, 31 arranged in parallel with the same height. The pair of rotating rollers 31, 31 are arranged at both axial ends of the cast iron pipe 1. One of the rotating rollers 31 is rotated by a drive device (not shown), and the rotation is transmitted to the cast iron pipe 1 to rotate the cast iron pipe 1 around the pipe axis. Mortar M poured downward from the nozzle 36 is introduced around the entire circumference while spreading out due to centrifugal force as the pipe rotates.
[0024] The injection cart 32 also has a traveling device 38 capable of traveling in the axial direction of the cast iron pipe 1. By introducing mortar M while moving the injection cart 32 in the axial direction of the pipe and rotating the cast iron pipe 1 in the circumferential direction by the rotating rollers 31, it is possible to form a uniform cement mortar layer 21 over the entire inner circumference of the cast iron pipe 1. The thickness of this cement mortar layer 21 is preferably about 5 to 16 mm.
[0025] In an embodiment, the rollers 31 and the cast iron pipe 1 may be placed on a carriage 39 that is movable in the axial direction, and the tank 33 and the injection lance 34 may be fixed on the carriage 39. This embodiment is shown in FIG. 3(c).
[0026] After the cement mortar layer 21 is formed, it is preferable to perform a vibration process in which the cast iron pipe 1a is rotated at high speed and given a moderate micro-vibration in order to compact the cement mortar layer 21 densely before curing and hardening the cement. This causes the cement mortar layer 21 to be separated into the mortar layer 23, the paste layer 24, and the laitance layer 25. An example of this process will be described with reference to the cross-sectional view of FIG. 4. The cast iron pipe 1a on which the cement mortar layer 21 is formed is supported by a rotating roller 41 similar to the rotating roller 31 described above. In addition, an iron vibrating roller 42 is attached to the upper part of the cast iron pipe 1a in contact with its outer circumferential surface. When the rotating roller 41 rotates, the rotational force of the cast iron pipe 1a is transmitted, and the vibrating roller 42 also rotates. A vibrator 43 consisting of a well-known vibrator or the like is connected above the vibrating roller 42. The vibrator 43 causes the vibrating roller 42 to continue to vibrate slightly while rotating, and the vibration is transmitted to the cast iron pipe 1a. The transmission of this micro-vibration compacts the cement mortar layer 21, pushing out any voids remaining in the mortar and preventing the occurrence of remaining voids.
[0027] The separated mortar layer 23, paste layer 24, and laitance layer 25 are cured to promote the hardening reaction of the cement and become layers made of strong cement. As a means of curing, steam curing is preferable because it allows the curing to proceed quickly.
[0028] After the curing process, before the next powder coating layer 22 is formed, the laitance layer 25 and the paste layer 24 are polished and removed from the surface side of the cement mortar layer 21. An example of this polishing process will be described with reference to the cross-sectional view of FIG. 5(a) and the side view of FIG. 5(b). The polishing device for polishing comprises the same rotating roller 51 as above and the polishing carriage 52. The polishing carriage 52 is provided with a lifter-type rotating shaft lifting device 53 and a rotating shaft 54, and a polishing wheel 55 is attached to the tip of the rotating shaft 54. As the polishing wheel 55, a bundle of sandpaper radially bundled together can be used. The polishing carriage 52 is provided with a traveling device 56 that can travel in the axial direction of the cast iron pipe 1a. The traveling device 56 allows the polishing wheel 55 to be set at any position in the axial direction of the cast iron pipe 1a.
[0029] The grinding carriage 52 is advanced so that the grinding wheel 55 is inserted into the cast iron pipe 1a being rotated by the rotating roller 51, and the grinding wheel 55 is lowered by the rotating shaft lifting device 53 while rotating the rotating shaft 54, and the grinding wheel 55 is pressed against the surface of the cement mortar layer 21 formed earlier. The surface of the cement mortar layer 21 of the rotating cast iron pipe 1a is ground by the rotation of the grinding wheel 55. At this time, in order to sufficiently remove the paste layer 24 and ensure smoothness, a part of the surface side of the mortar layer 23 may be scraped off. This is because the boundary between the paste layer 24 and the mortar layer 23 is not uniform, and it is easier to completely remove the paste layer 24 by scraping off the mortar layer 23 to a certain extent. By moving the grinding carriage 52 in the axial direction, the entire inner circumference of the rotating cast iron pipe 1a can be ground to further improve the smoothness.
[0030] This step may also be carried out in the opposite manner to that shown in FIG. 5(b), in which the cast iron pipe 1a side is moved in the axial direction by a traveling device 57 and the rotary shaft lifting device 53 side is fixed as shown in FIG. 5(c).
[0031] Here, the thickness of the mortar layer 23 remaining after polishing is desirably 4 mm or more. If it is less than 4 mm, it is not possible to sufficiently hide wrinkles on the inner surface of the pipe during casting, and problems with the smoothness of the inner surface are likely to occur. On the other hand, it is preferable that it is 15 mm or less. If it exceeds 15 mm, the reduction in the water flow area becomes too large, and depending on the amount of water flow, a pipe with a larger nominal diameter is required, resulting in too much waste. For example, in a conventional method of removing only the laitance layer 25 for a cast iron pipe with a nominal diameter of 1650, the paste layer 24 and the mortar layer 23 are often combined to have a thickness of 15 mm or more, but in the present invention, the paste layer 24 is removed to obtain a thickness within the above range.
[0032] Next, regardless of which of the above procedures is adopted, a powder coating is applied to the surface of the exposed mortar layer 23 to form the powder coating layer 22, which covers the entire inner peripheral side of the mortar layer 23. The method of applying the powder coating to the surface of the mortar layer 23 can be a method of sufficiently heating the cast iron pipe 1, 1a together with the mortar layer 23, and then applying the powder coating to the surface and allowing it to harden. Since the paste layer 24 has been removed in the above process, there is almost no risk of the heating causing a decrease in strength or the generation of cracks.
[0033] The powder coating may contain components other than the resin, such as fillers, to the extent that the smoothness and coverage of the surface of the powder coating layer 22 can be ensured. For example, silica sand can be used.
[0034] It is desirable to heat the cast iron pipes 1, 1a and the mortar layer 23 sufficiently before applying the powder paint. It is preferable that the temperature reached by heating is 240°C or higher, since this allows the curing reaction to proceed sufficiently even with thermosetting paints such as epoxy resin powder paint. On the other hand, it is preferable that the temperature is 330°C or lower. If the temperature is too high, some deterioration may occur in the mortar layer 23 even if the paste layer 24 has been removed.
[0035] The heating method includes a method of heating the entire cast iron pipe 1, 1a by placing it in a gas furnace with an atmospheric temperature of 300° C. or more. In order to eliminate temperature unevenness as much as possible, it is preferable to heat it for about 30 to 60 minutes.
[0036] An example of the procedure for forming the powder coating layer 22 will be described with reference to the cross-sectional view of FIG. 6(a) and the side view of FIG. 6(b). Here, an embodiment in which an epoxy resin coating is used as the powder coating is shown as an example. The cast iron pipe 1a having the mortar layer 23 is placed on the rotating roller 61 as described above and rotated. On the other hand, a paint storage and supply tank 63 for storing and supplying the epoxy resin powder coating, a paint discharge section 64 for discharging the epoxy resin powder coating 66, and a pipe 65 for conveying the coating from the paint storage and supply tank 63 to the paint discharge section 64 are arranged on a piping cart 62 having a traveling device 68 that moves in the axial direction. As the rotating roller 61 rotates, the traveling device 68 is operated to move in the axial direction, and the epoxy resin powder coating 66 is discharged from the paint discharge section 64 into the pipe, so that the epoxy resin powder coating covers the surface of the mortar layer 23, forming the powder coating layer 22 that covers the entire mortar layer 23.
[0037] This step may also be carried out in the opposite manner to that shown in FIG. 6(b), in which the cast iron pipe 1a side is moved in the axial direction by a traveling device 75 and the piping side is fixed, as shown in FIG. 6(c).
[0038] If the thickness of the powder coating layer 22 formed by applying the above-mentioned epoxy resin powder coating is 300 μm or more, the cast iron pipe can be sufficiently protected from corrosion.
[0039] The epoxy resin powder coating is not particularly limited, but a coating specified in JWWA G 112 (Epoxy powder coating for the inner surface of ductile iron pipes for water supply) can be used. It contains at least an epoxy resin as a base agent and a hardener. It may also contain pigments and other additives. EXAMPLES
[0040] The present invention will be specifically described below with reference to examples in which an internally corrosion-resistant cast iron pipe according to the present invention was actually manufactured. The cast iron pipe used was an S-shaped ductile iron pipe with a nominal diameter of 1650 manufactured by Kurimoto Iron Works Co., Ltd. Cement mortar was poured into this pipe and laid down to a uniform thickness using centrifugal force, forming a cement mortar layer while separating it into layers. After laying, the pipe was steam cured for one day, allowing the cement mortar layer to harden while remaining separated into a laitance layer, paste layer, and mortar layer. The average thickness of the cement mortar layer was 16 mm.
[0041] An abrasive wheel was introduced into the tube to remove the laitance and paste layers on the surface, leaving a remaining mortar layer with an average thickness of 10 mm.
[0042] The cast iron pipe, with only the mortar layer remaining, was placed in a gas furnace with an atmospheric temperature of 350°C and heated for 60 minutes. When it was removed, the temperature of the pipe was 300°C. At this stage, no surface abnormalities such as cracks were found on the surface of the internal mortar layer.
[0043] The pipe taken out of the furnace was introduced into the apparatus shown in Figure 6, and while rotating, an epoxy resin powder coating was applied to the surface of the mortar layer so that the average thickness of the powder coating layer became 400 μm. The resulting coating was then allowed to harden by natural cooling and then allowed to cool to obtain an internally corrosion-resistant cast iron pipe.
[0044] <Cross-section photo for reference> In the above example, after the separated cement mortar layer 21 was formed and hardened, the cast iron pipe was cut together with the cement mortar layer 21. A photograph of the cut surface is shown in Figure 7. The laitance layer 25 on the surface from the surface side (upper side) cannot be seen in this photograph because it peeled off when cut. The subsequent part where no aggregate is visible and looks uniform is the paste layer 24, and underneath that is the mortar layer 23 where the cross section of gravel is clearly formed, and it was confirmed that the paste layer 24 and the mortar layer 23 can be easily distinguished by visual inspection. [Explanation of symbols]
[0045] 1,1a Cast iron pipe 11 Insertion port 12 Underbite 13 Straight section 20 Anticorrosive Layer 21 Cement mortar layer 22 Powder coating layer 23 Mortar layer 24 Paste layer 25 Laitance layer 31, 41, 51, 61 Rotating roller 32 Injection trolley 33 Tank 34 Injection Lance 36 spout 38, 56, 57, 68, 75 Running gear 39 Trolley 42 Vibration roller 43 Vibrator 52 Polishing Cart 53 Rotation axis lifting device 54 Rotation axis 55 Abrasive Wheel 62 Piping Trolley 63 Paint storage and supply tank 64 Paint discharge part 65 Piping 66 Epoxy resin powder coating M Mortar
Claims
1. The inner surface of the cast iron pipe has a mortar layer derived from the mortar lining and a powder coating layer formed by melting the powder coating, The powder coating layer is in contact with the inner surface of the mortar layer.
2. 2. The internally corrosion-resistant cast iron pipe according to claim 1, wherein the powder coating is a thermosetting coating.
3. supplying cement mortar onto the inner surface of the cast iron pipe while rotating the pipe to form a cement mortar layer; a step of polishing and removing the laitance layer and the paste layer present on the surface side of the cement mortar layer after the cement mortar layer has hardened, so that only the mortar layer remains; heating the entire cast iron pipe on which the mortar layer remains; applying a powder coating to the surface of the mortar layer after heating; A manufacturing method for inner surface corrosion-resistant cast iron pipes.
4. The method for manufacturing an internally corrosion-resistant cast iron pipe according to claim 3, wherein the powder paint is a thermosetting paint.
5. The method for manufacturing an internally corrosion-protected cast iron pipe according to claim 3 or 4, wherein the temperature of the cast iron pipe in the step of applying the powder paint is 240° C. or higher and 330° C. or lower.
Citation Information
Patent Citations
High pressure water injection device for road
JP1997158113A
Method of lining inside surface of ductile pipe
JP1997276794A