Silicon electrode plate

A laminated silicon electrode plate with single-crystal and polycrystalline silicon layers, aligned to resist cracking, addresses thermal stress issues in plasma processing apparatuses, ensuring stable operation and reduced particle generation.

JP2024143018AInactive Publication Date: 2024-10-11MITSUBISHI MATERIALS CORP
View PDF 1 Cites 0 Cited by

Patent Information

Application Number
JP2023055469
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Filing Date
2023-03-30
Publication Date
2024-10-11
Estimated Expiration
Not applicable · inactive patent

AI Technical Summary

Technical Problem

The increasing power of high-frequency waves in plasma processing apparatuses leads to insufficient cooling of silicon electrode plates, causing thermal stress and potential cracking due to warping and heat distribution, with single-crystal silicon being prone to cracks and polycrystalline silicon risking particle generation during plasma etching.

Method used

A silicon electrode plate structure comprising a laminated single-crystal silicon plate and polycrystalline silicon plate, where the cleavage planes are aligned differently, with a bonding layer of aluminum, to reinforce the structure and suppress cracking, and ensure stable operation.

Benefits of technology

The laminated structure effectively suppresses cracking and particle generation, providing a stable silicon electrode plate that can withstand thermal stress and maintain performance in plasma processing.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024143018000001_ABST
    Figure 2024143018000001_ABST
Patent Text Reader

Abstract

To provide a silicon electrode plate that can suppress the occurrence of cracks and can be used stably.SOLUTION: A silicon electrode plate 10 is used in a plasma processing apparatus and has a plasma generating surface where plasma is generated, and has a structure in which a single crystal silicon plate 11 and a polycrystalline silicon plate 12 are laminated, with at least the plasma generating surface being composed of the single crystal silicon plate 11. It is preferable that the proportion of the polycrystalline silicon plate 12 in the plate thickness direction is within a range of 10% to 95%.SELECTED DRAWING: Figure 1
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a silicon electrode plate for use in a plasma processing apparatus. [Background technology]

[0002] Conventionally, in plasma processing apparatuses such as plasma etching apparatuses and plasma CVD apparatuses used in semiconductor device manufacturing processes, an electrode plate and a stand connected to a high-frequency power source are arranged, for example, one above the other in a chamber of the apparatus, and a silicon wafer is placed on the stand. A high-frequency voltage is applied while gas is caused to flow toward the silicon wafer through through holes formed in the electrode plate, thereby generating plasma and performing processing such as etching on the silicon wafer.

[0003] In the above-mentioned plasma processing apparatus and the like, silicon members are widely used to suppress metal contamination in the chamber. For example, a silicon electrode plate having a structure in which a plurality of ventilation holes are formed in a silicon plate material is used as an electrode plate for use in a plasma processing apparatus. The silicon electrode plate has a plasma generating surface that generates plasma, and a cooling plate made of, for example, aluminum is disposed on the surface opposite to the plasma generating surface.

[0004] Here, in order to suppress the generation of contamination and particles, the silicon members disposed in the chamber of a plasma processing apparatus or the like are made of single crystal silicon, which is the same material as the wafer to be processed, as shown in Patent Document 1, for example. [Prior art documents] [Patent documents]

[0005] [Patent Document 1] Patent No. 3744726 Summary of the Invention [Problem to be solved by the invention]

[0006] In recent years, in the above-mentioned plasma processing apparatus, the output of high frequency waves applied has been dramatically increased in order to improve the processing speed and processing accuracy of wafers, and accordingly, the heat input from the plasma to the silicon electrode plate has been increasing. As described above, a cooling plate is placed on the side of the silicon electrode plate opposite the plasma generation surface. However, as the heat input increases, the cooling of the silicon electrode plate and surrounding components becomes insufficient, and warping due to thermal expansion and heat distribution of the surrounding components may occur, which may result in cracks in the silicon electrode plate.

[0007] In particular, since single crystal silicon has a tendency to crack along the cleavage plane, when bending stress, such as that caused by applying a load along the cleavage direction, acts on the silicon electrode plate, cracks tend to occur easily. On the other hand, polycrystalline silicon such as columnar crystal silicon has a lower Young's modulus and is more easily deformed than single crystal silicon, and has excellent bending strength and tends to be less likely to break. However, since polycrystalline silicon has crystal grain boundaries, when plasma is generated, the crystal grain size is selectively etched, which may easily generate particles.

[0008] The present invention has been made in consideration of the above-mentioned circumstances, and an object of the present invention is to provide a silicon electrode plate that can suppress the occurrence of cracks and can be used stably. [Means for solving the problem]

[0009] In order to solve the above problems, the silicon electrode plate of aspect 1 of the present invention is a silicon electrode plate used in a plasma processing apparatus and having a plasma generating surface where plasma is generated, characterized in that it has a structure in which a single crystal silicon plate and a polycrystalline silicon plate are laminated, and at least the plasma generating surface is composed of the single crystal silicon plate.

[0010] According to the silicon electrode plate of the first aspect of the present invention, since the single crystal silicon plate and the polycrystalline silicon plate are laminated, the cleavage plane of the polycrystalline silicon is not aligned with the cleavage plane of the single crystal and the cleavage direction is different. Therefore, the silicon electrode plate of the first aspect can suppress the occurrence of cracks in the silicon electrode plate even when bending stress is applied. Furthermore, since at least the plasma generating surface is made of the single crystal silicon plate, generation of particles can be suppressed, and stable use is possible.

[0011] A silicon electrode plate according to a second aspect of the present invention is characterized in that in the silicon electrode plate according to the first aspect, the proportion of the polycrystalline silicon plate in the plate thickness direction is within a range of 10% to 95%. According to the silicon electrode plate of aspect 2 of the present invention, the thickness-wise ratio of the polycrystalline silicon plate is within the range of 10% or more and 95% or less, so that the silicon electrode plate can be reliably reinforced and the occurrence of cracks in the silicon electrode plate can be reliably suppressed even when bending stress is applied.

[0012] A silicon electrode plate according to a third aspect of the present invention is the silicon electrode plate according to the first or second aspect, characterized in that the polycrystalline silicon plate is a columnar crystal silicon plate. According to the silicon electrode plate of the third aspect of the present invention, since the polycrystalline silicon plate is a columnar crystal silicon plate, the bending strength is further superior, the silicon electrode plate can be further reinforced reliably, and the occurrence of cracks in the silicon electrode plate can be reliably suppressed.

[0013] The silicon electrode plate of the fourth aspect of the present invention is characterized in that, in the silicon electrode plate of the third aspect, the crystal orientation of the bonding surface of the single crystal silicon plate and the crystal orientation of the bonding surface of the columnar crystal silicon plate are different from each other. According to the silicon electrode plate of the fourth aspect of the present invention, the crystal orientation of the bonding surface of the single crystal silicon plate and the crystal orientation of the bonding surface of the columnar crystal silicon plate are different from each other. Therefore, when bending stress is applied, the single crystal silicon plate and the columnar crystal silicon plate reinforce each other, so that the silicon electrode plate can be further reinforced reliably and the occurrence of cracks in the silicon electrode plate can be reliably suppressed.

[0014] The silicon electrode plate of aspect 5 of the present invention is characterized in that, in the silicon electrode plate of any one of aspects 1 to 4, a bonding layer containing Al as a main component is formed between the single crystal silicon plate and the polycrystalline silicon plate. According to the silicon electrode plate of the fifth aspect of the present invention, a bonding layer containing Al as a main component is formed between the single crystal silicon plate and the polycrystalline silicon plate, and this bonding layer serves as a stress buffer layer, thereby further improving the strength of the silicon electrode plate.

[0015] A silicon electrode plate according to a sixth aspect of the present invention is characterized in that in the silicon electrode plate according to any one of the first to fourth aspects, the single crystal silicon plate and the polycrystalline silicon plate are directly bonded to each other. According to the silicon electrode plate of aspect 6 of the present invention, the single crystal silicon plate and the polycrystalline silicon plate are directly bonded to each other, which makes it possible to further suppress contamination within the chamber of a plasma processing apparatus or the like. Effect of the Invention

[0016] According to the present invention, it is possible to provide a silicon electrode plate that can suppress the occurrence of cracks and can be used stably. [Brief description of the drawings]

[0017] [Figure 1] 1A and 1B are schematic explanatory diagrams of a silicon electrode plate according to an embodiment of the present invention, in which (a) is a perspective view and (b) is an enlarged explanatory view of a bonding portion. [Diagram 2] 2 is a flow diagram showing a method for producing the silicon member shown in FIG. [Diagram 3] 1A and 1B are schematic explanatory diagrams of a silicon electrode plate according to another embodiment of the present invention, in which (a) is a perspective view and (b) is an enlarged explanatory view of a bonding portion. [Figure 4] 4 is a flow diagram showing a method for manufacturing the silicon member shown in FIG. [Diagram 5] FIG. 11 is a schematic explanatory diagram of a silicon electrode plate according to another embodiment of the present invention. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0018] A silicon electrode plate according to an embodiment of the present invention will be described below. A silicon electrode plate according to one embodiment of the present invention is disposed in a chamber of a plasma processing apparatus such as a plasma etching apparatus or a plasma CVD apparatus used in a semiconductor device manufacturing process.

[0019] As shown in FIG. 1(a), the silicon electrode plate 10 of this embodiment has a plurality of ventilation holes 10A penetrating in the thickness direction. As shown in Figures 1(a) and (b), the silicon electrode plate 10 of this embodiment has a structure in which a first silicon plate 11 and a second silicon plate 12 are bonded in the thickness direction, and the first silicon plate 11 and the second silicon plate 12 are laminated with a bonding layer 15 interposed therebetween.

[0020] In this embodiment, the above-mentioned bonding layer 15 is made of aluminum or an aluminum alloy. Here, the surface of the first silicon plate 11 opposite to the bonding surface 11a (the upper surface in FIG. 1) serves as a plasma generating surface where plasma is generated. In this embodiment, the first silicon plate 11 is made of a single crystal silicon plate, and the second silicon plate 12 is made of a polycrystalline silicon plate.

[0021] The first silicon plate 11, which is made of a single crystal silicon plate, is entirely made of a single crystal and has the same atomic arrangement. Here, the crystal orientation of the plasma generating surface and the bonding surface 11a may be the (100) plane, the (111) plane, or the (110) plane.

[0022] The second silicon plate 12 made of a polycrystalline silicon plate is made up of a plurality of crystals. In this embodiment, the second silicon plate 12 is preferably a columnar crystal silicon plate obtained by slicing an ingot grown in one direction.

[0023] The columnar crystal silicon plate is manufactured by slicing an ingot, which has been crystal-grown in one direction, in a direction perpendicular to the crystal growth direction. The crystal growth direction can be (100), (110), or (111), and the crystal orientation of the bonding surface 12a of the second silicon plate 12, which is made of the columnar crystal silicon plate, can be the (100) plane, the (111) plane, or the (110) plane. In this embodiment, the crystal orientation of the bonding surface 11a of the first silicon plate 11 made of a single crystal silicon plate and the crystal orientation of the bonding surface 12a of the second silicon plate 12 made of a columnar crystal silicon plate are set to be different from each other.

[0024] In this embodiment, the ratio in the plate thickness direction of the second silicon plate 12 made of a polycrystalline silicon plate is preferably within a range of 10% to 95%. The ratio of the second silicon plate 12 made of a polycrystalline silicon plate in the plate thickness direction is more preferably 50% or more. The ratio of the second silicon plate 12 made of a polycrystalline silicon plate in the plate thickness direction is further preferably 90% or less, and more preferably 80% or less.

[0025] Next, a method for manufacturing the silicon electrode plate 10 according to the present embodiment will be described with reference to FIG.

[0026] The method for manufacturing the silicon electrode plate 10 according to this embodiment includes a silicon plate preparation step S01, a silicon plate processing step S02, an Al layer formation step S03, a lamination step S04, and a bonding step S05, as shown in FIG.

[0027] Each step of the method for producing the silicon electrode plate 10 according to this embodiment will be described in detail below.

[0028] (Silicon plate preparation process S01) First, a single crystal silicon plate that will become the first silicon plate 11 and a polycrystalline silicon plate that will become the second silicon plate 12 are prepared. At this time, a single crystal silicon plate (first silicon plate 11) is cut out from a single crystal silicon ingot so that the crystal orientation of the plasma generation surface and the bonding surface 11a of the first silicon plate 11 is in a specific direction. Furthermore, a polycrystalline silicon plate (second silicon plate 12) is cut out from the polycrystalline silicon ingot. In this embodiment, the columnar crystal silicon plate (second silicon plate 12) is cut out from a columnar crystal silicon ingot that has been directionally solidified.

[0029] (Silicon plate processing process S02) The cut single crystal silicon plate (first silicon plate 11) and polycrystalline silicon plate (second silicon plate 12) are mechanically processed to adjust their outer shapes. In addition, the surfaces are cut to adjust the planar shape of the surfaces. Furthermore, in this embodiment, a hole drilling process is performed on the single crystal silicon plate (first silicon plate 11) and the polycrystalline silicon plate (second silicon plate 12) to form through holes that will become the vent holes 10A.

[0030] (Al layer formation step S03) An Al layer is formed on at least one of the bonding surface 11a of the single crystal silicon plate (first silicon plate 11) and the bonding surface 12a of the polycrystalline silicon plate (second silicon plate 12). There is no particular limitation on the method for forming the Al layer, and existing techniques such as vapor deposition and sputtering can be appropriately selected and applied. Here, the thickness of the Al layer is preferably within the range of 0.05 μm to 2.00 μm.

[0031] (Lamination process S04) Next, a single crystal silicon plate (first silicon plate 11) and a polycrystalline silicon plate (second silicon plate 12) are laminated in the thickness direction with an Al layer interposed therebetween.

[0032] (Joining process S05) Next, the single crystal silicon plate (first silicon plate 11) and the polycrystalline silicon plate (second silicon plate 12) stacked as described above are heated while being pressurized in the stacking direction, and the single crystal silicon plate (first silicon plate 11) and the polycrystalline silicon plate (second silicon plate 12) are bonded via the bonding layer 15.

[0033] Here, the heating temperature in the bonding step S05 is preferably within a range of 500° C. or more and 650° C. or less. Moreover, the holding time at the heating temperature in the bonding step S05 is preferably within a range of 1 hour to 16 hours. Furthermore, the pressure load in the joining step S05 is preferably set to 0.01 MPa or more and 10.00 MPa or less.

[0034] Through the various steps described above, the silicon electrode plate 10 of this embodiment is manufactured.

[0035] According to the silicon electrode plate 10 of this embodiment configured as described above, the first silicon plate 11 made of a single crystal silicon plate and the second silicon plate 12 made of a polycrystalline silicon plate are stacked together. Therefore, the silicon electrode plate 10 is reinforced by the second silicon plate 12, and even when bending stress is applied, it is possible to suppress the occurrence of cracks in the silicon electrode plate 10. Furthermore, since the plasma generating surface of the silicon electrode plate 10 is constructed from the first silicon plate 11 made of a single crystal silicon plate, the generation of particles can be suppressed, and the device can be used stably.

[0036] In the silicon electrode plate 10 of this embodiment, when the thickness-wise ratio of the second silicon plate 12 made of a polycrystalline silicon plate is within the range of 10% or more and 95% or less, the silicon electrode plate 10 can be reliably reinforced, and even when bending stress is applied, the occurrence of cracks in the silicon electrode plate 10 can be reliably suppressed.

[0037] In the silicon electrode plate 10 of this embodiment, when the polycrystalline silicon plate constituting the second silicon plate 12 is a columnar crystal silicon plate, the bending strength of the second silicon plate 12 is even better, the silicon electrode plate 10 can be further reinforced reliably, and the occurrence of cracks in the silicon electrode plate 10 can be reliably suppressed.

[0038] In the silicon electrode plate 10 of this embodiment, when the crystal orientation of the bonding surface 11a of the first silicon plate 11 made of a single crystal silicon plate and the crystal orientation of the bonding surface 12a of the second silicon plate 12 made of a columnar crystal silicon plate are different from each other, when bending stress is applied, the first silicon plate 11 made of a single crystal silicon plate and the second silicon plate 12 made of a columnar crystal silicon plate reinforce each other, thereby further reliably reinforcing the silicon electrode plate 10 and making it possible to reliably suppress the occurrence of cracks in the silicon electrode plate 10.

[0039] In the silicon electrode plate 10 of this embodiment, when a bonding layer 15 mainly composed of Al is formed between the first silicon plate 11 made of a single crystal silicon plate and the second silicon plate 12 made of a polycrystalline silicon plate, this bonding layer 15 serves as a stress buffer layer, thereby enabling further improvement in strength.

[0040] Although the embodiment of the present invention has been described above, the present invention is not limited to this, and can be modified as appropriate without departing from the technical concept of the invention.

[0041] In this embodiment, the bonding layer 15 mainly made of Al is formed between the first silicon plate 11 made of a single crystal silicon plate and the second silicon plate 12 made of a polycrystalline silicon plate, but the present invention is not limited to this, and may be a silicon electrode plate 110 having a structure in which a first silicon plate 111 made of a single crystal silicon plate and a second silicon plate 112 made of a polycrystalline silicon plate are directly bonded together, as shown in Fig. 3. This silicon electrode plate 110 also has a plurality of air holes 110A formed therein.

[0042] The silicon electrode plate 110 shown in FIG. 3 is manufactured, for example, by the manufacturing method shown in the flow chart of FIG. The method for manufacturing the silicon electrode plate 110 shown in FIG. 3 includes a silicon plate preparation step S101, a surface treatment step S102, a lamination step S103, a bonding step S014, and a processing step S105, as shown in FIG.

[0043] (Silicon plate preparation process S101) First, a single crystal silicon plate that will become the first silicon plate 111 and a polycrystalline silicon plate that will become the second silicon plate 112 are prepared. At this time, a single crystal silicon plate (first silicon plate 111) is cut out from a single crystal silicon ingot so that the crystal orientation of the plasma generation surface and bonding surface 111a of the first silicon plate 111 is in a specific direction. Furthermore, a polycrystalline silicon plate (second silicon plate 112) is cut out from the polycrystalline silicon ingot.

[0044] (Surface treatment step S102) Next, the bonding surface 111a of the cut single crystal silicon plate (first silicon plate 111) and the bonding surface 112a of the cut polycrystalline silicon plate (second silicon plate 112) are polished to a surface roughness (arithmetic mean roughness) Ra of 0.2 μm or less. Furthermore, after polishing, the bonding surface 111a of the single crystal silicon plate (first silicon plate 111) and the bonding surface 112a of the polycrystalline silicon plate (second silicon plate 112) may be subjected to a hydrophilic treatment such as an oxygen plasma treatment or application of a silane coupling agent.

[0045] (Lamination process S103) Next, the surface-treated single crystal silicon plate (first silicon plate 111) and the polycrystalline silicon plate (second silicon plate 112) are laminated in the thickness direction so that their bonding surfaces 111a and 112a are in contact with each other.

[0046] (Joining process S104) Next, the single crystal silicon plate (first silicon plate 111) and the polycrystalline silicon plate (second silicon plate 112) stacked as described above are heated while being pressurized in the stacking direction, to directly bond the single crystal silicon plate (first silicon plate 111) and the polycrystalline silicon plate (second silicon plate 112).

[0047] Here, the heating temperature in the bonding step S104 is preferably within a range of 500° C. or more and 1300° C. or less. Moreover, the holding time at the heating temperature in the bonding step S104 is preferably within a range of 1 hour to 16 hours. Furthermore, the pressure load in the joining step S104 is preferably set to 0.01 MPa or more and 15.00 MPa or less.

[0048] (Processing process S105) The directly bonded single crystal silicon plate (first silicon plate 111) and polycrystalline silicon plate (second silicon plate 112) are mechanically processed to adjust the outer shape. Furthermore, holes are drilled in the single crystal silicon plate (first silicon plate 111) and the polycrystalline silicon plate (second silicon plate 112) to form the ventilation holes 110A.

[0049] Through the various steps described above, the silicon electrode plate 110 shown in FIG. 3 is manufactured. In the silicon electrode plate 110 shown in FIG. 3, a single crystal silicon plate (first silicon plate 111) and a polycrystalline silicon plate (second silicon plate 112) are directly bonded to each other, which makes it possible to further suppress contamination within a chamber of a plasma processing apparatus or the like.

[0050] In addition, in this embodiment, the structure is described as having two silicon plates stacked, but there is no particular limit to the number of stacked sheets. For example, as shown in Fig. 5, a silicon electrode plate 210 may be configured such that a polycrystalline silicon plate 212 is stacked as an intermediate layer between two single crystal silicon plates 211 and 213. Note that a plurality of air holes 210A are also formed in this silicon electrode plate 210.

[0051] In the silicon electrode plate 210 shown in FIG. 5, the surface exposed to the inside of the chamber is composed of single crystal silicon plates 211, 213, and therefore the etching resistance is further improved, and it can be used stably for a longer period of time. The bonding between the single crystal silicon plates 211, 213 and the polycrystalline silicon plate 212 may be performed using an Al layer as shown in the flow diagram of FIG. 2, or directly as shown in the flow diagram of FIG. 4, or a combination of these. EXAMPLES

[0052] The results of confirmatory experiments conducted to confirm the effectiveness of the present invention will be described below.

[0053] A single crystal silicon plate, a polycrystalline silicon plate, and a columnar crystal silicon plate, each with a diameter of 200 mm, were prepared. The single crystal silicon plate and the columnar crystal silicon plate were cut from an ingot so that the crystal orientation of the bonding surface was the crystal orientation shown in Table 1. Then, various silicon plates were joined by the joining method shown in Table 1 so as to have the structure shown in Table 1, and a silicon electrode plate having a thickness of 10 mm was manufactured.

[0054] Here, in Table 1, "Al bonding" was performed according to the procedure shown in the flow chart of Figure 2 under the conditions of Al layer thickness: 1 μm, heating temperature: 600°C, holding time: 2 hours, and pressurizing pressure: 3 MPa. In addition, for "direct bonding" in Table 1, the bonding surfaces were mirror-finished and then oxygen plasma treated in the procedure shown in the flow chart of Figure 4, and the conditions were heating temperature: 1000°C, holding time: 5 hours, and pressure: 6 MPa.

[0055] As a conventional example, a 10 m thick silicon electrode plate composed only of a single crystal silicon plate was prepared.

[0056] Five bending test pieces (width 4 mm, thickness 3 mm, length 40 mm) were taken from each of the silicon electrode plates of the above-mentioned invention example and conventional example, and a three-point bending test was carried out at room temperature using a Shimadzu Tadashi Autograph AG-X to measure the bending strength and Young's modulus, and the average value of the five pieces was calculated. The bending strength and Young's modulus of the inventive examples were evaluated relative to the bending strength of the conventional example. The calculated average values ​​were used to calculate the rate of change in bending strength of the inventive examples relative to the bending strength of the conventional example, and the rate of change in Young's modulus of the inventive examples relative to the Young's modulus of the conventional example. The evaluation results are shown in Table 1.

[0057] [Table 1]

[0058] In comparison with the conventional example, the bending strength was significantly improved and the Young's modulus was decreased in the present invention examples 1 to 8. Therefore, it was found that the present invention examples 1 to 8 are more easily deformed and have higher strength than the conventional example, and are capable of sufficiently suppressing the occurrence of cracks. In addition, when comparing invention examples 1 and 2, it was found that the bending strength of the columnar crystal silicon plate was improved compared to the polycrystalline silicon plate having random crystal orientation.

[0059] Furthermore, when comparing Examples 1, 4, and 5 of the present invention, it was found that the bending strength was further improved by arranging the crystal orientation of the bonding surface of the single crystal silicon plate and the crystal orientation of the bonding surface of the columnar crystal silicon plate to be different from each other. Furthermore, when comparing Inventive Examples 3, 6, and 7, it was found that there was a tendency for bending strength to improve by increasing the thickness ratio of the polycrystalline silicon plate. It was also confirmed that even in the case of a three-layer structure as in Example 8 of the present invention, the bending strength could be sufficiently improved.

[0060] As a result of the above, it was confirmed that the present invention can provide a silicon electrode plate that can suppress the occurrence of cracks and can be used stably. [Explanation of symbols]

[0061] 10,110,210 Silicon electrode plate 11 First silicon member 12 Second silicon member

Claims

1. A silicon electrode plate used in a plasma processing apparatus and having a plasma generating surface for generating plasma, 1. A silicon electrode plate having a structure in which a single crystal silicon plate and a polycrystalline silicon plate are laminated, wherein at least the plasma generating surface is constituted by the single crystal silicon plate.

2. 2. The silicon electrode plate according to claim 1, wherein the ratio of the thickness of the polycrystalline silicon plate in the plate thickness direction is within a range of 10% to 95%.

3. 3. The silicon electrode plate according to claim 1, wherein the polycrystalline silicon plate is a columnar crystal silicon plate.

4. 4. The silicon electrode plate according to claim 3, wherein a crystal orientation of the bonding surface of the single crystal silicon plate and a crystal orientation of the bonding surface of the columnar crystal silicon plate are different from each other.

5. 2. The silicon electrode plate according to claim 1, further comprising a bonding layer mainly composed of Al formed between the single crystal silicon plate and the polycrystalline silicon plate.

6. 2. The silicon electrode plate according to claim 1, wherein the single crystal silicon plate and the polycrystalline silicon plate are directly bonded to each other.