Silicon member and method for manufacturing silicon member

The silicon member addresses joint strength and contamination issues by using a high Si content and controlled bonding process, ensuring heat resistance and broad etching gas compatibility.

JP2024143019AInactive Publication Date: 2024-10-11MITSUBISHI MATERIALS CORP
View PDF 8 Cites 0 Cited by

Patent Information

Application Number
JP2023055470
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Filing Date
2023-03-30
Publication Date
2024-10-11
Estimated Expiration
Not applicable · inactive patent

AI Technical Summary

Technical Problem

Existing silicon electrode plates in plasma processing apparatuses face issues with joint strength due to eutectic alloys having insufficient heat resistance, potential for voids and shrinkage cavities, and contamination risks from eutectic-forming elements, limiting the use of corrosive etching gases and expanding ventilation holes.

Method used

A silicon member composed of plate-like members joined with a Si content of 90 mass% or more and metal elements other than Si at 5 mass% or less, bonded via oxygen, with a bonding strength of 5 MPa or more, using a manufacturing process involving surface grinding, OH group introduction, lamination, and dehydration condensation under controlled pressure and temperature.

Benefits of technology

The solution provides a silicon member with enhanced heat resistance, reduced contamination risk, and the ability to use a wider range of etching gases, ensuring stable operation by maintaining strong joint integrity.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024143019000003
    Figure 2024143019000003
  • Figure 2024143019000004
    Figure 2024143019000004
  • Figure 2024143019000005
    Figure 2024143019000005
Patent Text Reader

Abstract

To provide a silicon member in which a plurality of plate-like members are reliably bonded, has excellent heat resistance, and is capable of suppressing the occurrence of contamination, and a method for manufacturing the silicon member.SOLUTION: A silicon component used in a plasma processing apparatus has a structure in which a plurality of plate-shaped components made of a Si-containing material are bonded in the thickness direction, the Si content at the bonded portions between the plate-shaped components is 90 mass% or more, the total content of metal elements other than Si is 5 mass% or less, and the bond strength between the plate-shaped components is 5 MPa or more.SELECTED DRAWING: None
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a silicon member used in a plasma processing apparatus and a method for manufacturing the silicon member. [Background technology]

[0002] Conventionally, in plasma processing apparatuses such as plasma etching apparatuses and plasma CVD apparatuses used in semiconductor device manufacturing processes, an electrode plate and a stand connected to a high-frequency power source are arranged, for example, one above the other in a chamber of the apparatus, and a silicon wafer is placed on the stand. A high-frequency voltage is applied while gas is caused to flow toward the silicon wafer through through holes formed in the electrode plate, thereby generating plasma and performing processing such as etching on the silicon wafer.

[0003] In the above-mentioned plasma processing apparatus and the like, silicon members are widely used to suppress metal contamination in the chamber. For example, an electrode plate used in a plasma processing apparatus is a silicon member having a plate-like member with a plurality of ventilation holes formed therein.

[0004] Silicon members disposed in a chamber of a plasma processing apparatus or the like gradually wear away with use. For this reason, there is a demand for bonding a worn silicon member to another silicon member and reusing the resulting silicon bonded body as the silicon member.

[0005] In addition, there is a risk that the plasma generated on the plasma surface side of the electrode plate will enter the surface opposite to the plasma surface through the vent hole and damage the surrounding members of the electrode plate. In order to suppress this, it is conceivable to make the vent hole have a complex curved shape. In order to form a vent hole of such a complex shape, it is conceivable to join a plurality of plate-shaped members each having a through hole in the thickness direction, and to form a groove that communicates the through holes between the joining surfaces of the silicon plates.

[0006] For example, Patent Document 1 discloses a silicon electrode plate in which a plurality of silicon plate-shaped electrode members are bonded in the thickness direction. In Patent Document 1, a eutectic forming element such as Al, In, Sn, etc. is disposed between plate-shaped electrode members and heat-treated to form a joint consisting of Si and the eutectic forming element, thereby joining the plate-shaped electrode members together. [Prior art documents] [Patent documents]

[0007] [Patent Document 1] Patent No. 6146840 Summary of the Invention [Problem to be solved by the invention]

[0008] However, in the silicon electrode plate described in Patent Document 1, the joint is made of a eutectic alloy with silicon (e.g., an Al-Si eutectic alloy, etc.), so there is a risk of cracks occurring in the joint and heat resistance is insufficient. In addition, there is a risk of voids or shrinkage cavities occurring in the joint, which reduces the joint strength.

[0009] Furthermore, since eutectic forming elements such as Al, In, and Sn are present in the joint, there is a risk of the joint deteriorating when a corrosive gas is used as the etching gas, which poses a problem of limitations on the etching gas that can be used. In addition, when the electrode plate wears down and the vent hole expands with use, the eutectic forming elements such as Al, In, and Sn contained in the joint may cause contamination.

[0010] The present invention has been made in consideration of the above-mentioned circumstances, and aims to provide a silicon member in which a plurality of plate-shaped members are reliably bonded, has excellent heat resistance, and is capable of suppressing the occurrence of contamination, and a method for manufacturing the silicon member. [Means for solving the problem]

[0011] In order to solve the above problems, the silicon member of aspect 1 of the present invention is a silicon member used in a plasma processing apparatus, and has a structure in which a plurality of plate-shaped members made of a Si-containing material are bonded in the thickness direction, the Si content at the bonded portions between the plate-shaped members is 90 mass% or more, the total content of metal elements other than Si is 5 mass% or less, and the bond strength between the plate-shaped members is 5 MPa or more.

[0012] According to the silicon member of the first aspect of the present invention, the Si content in the joint between the plate-like members is 90 mass% or more, and the total content of metal elements other than Si is limited to 5 mass% or less, so that the generation of contamination in the plasma processing device can be suppressed. In addition, it becomes possible to use a corrosive etching gas, and a wide range of etching gases can be selected. In addition, since the joint is not made of a eutectic alloy, the heat resistance is excellent. The bonding strength between the plate-like members is set to 5 MPa or more, and the plate-like members are reliably bonded to each other with sufficient strength. Therefore, the silicon member can be stably used as a silicon member for a plasma processing apparatus.

[0013] The silicon component of aspect 2 of the present invention is characterized in that, in the silicon component of aspect 1, the total content of Al, Ti, Cr, Mn, Fe, Co, Ni, Cu, In, Sn, Zn, Y, Mo, Hf, Ta, W, and Pb as metal elements other than Si in the joint is 5 mass% or less. According to the silicon member of aspect 2 of the present invention, the total content of metal elements other than Si in the joint, namely Al, Ti, Cr, Mn, Fe, Co, Ni, Cu, In, Sn, Zn, Y, Mo, Hf, Ta, W, and Pb, is 5 mass% or less, thereby making it possible to suppress the occurrence of contamination and to select an even wider range of etching gases.

[0014] The silicon member of a third aspect of the present invention is the silicon member of the first or second aspect, characterized in that the plate-like members are bonded to each other at the bonding portion via oxygen. According to the silicon member of the third aspect of the present invention, the plate-like members are bonded to each other at the bonding portion via oxygen, and the silicon members can be bonded to each other firmly.

[0015] A silicon member according to a fourth aspect of the present invention is the silicon member according to any one of the first to third aspects, characterized in that the void ratio in the joint is 20% or less. According to the silicon member of the fourth aspect of the present invention, the void ratio in the bonded portion is 20% or less, so that the silicon members are firmly bonded to each other, and the bonding strength can be sufficiently improved.

[0016] The manufacturing method of a silicon member of aspect 5 of the present invention is a manufacturing method of a silicon member for manufacturing a silicon member of any one of aspects 1 to 4, and includes a stacking process of directly stacking a plurality of the plate-like members, and a joining process of heating the stacked plate-like members while applying pressure to each other in the stacking direction to join the plate-like members to each other, characterized in that in the joining process, the pressure load is in the range of 3 MPa or more and 12 MPa or less, the heating temperature is in the range of 600°C or more and 1300°C or less, and the holding time at the heating temperature is in the range of 2 hours or more and 10 hours or less.

[0017] According to the manufacturing method of a silicon member of aspect 5 of the present invention, a bonding process is included in which the stacked plate-like members are heated while being pressed in the stacking direction to bond the plate-like members to each other. This does not require the use of bonding materials, and makes it possible to prevent metal elements other than silicon from being included in the bonded portion. In the bonding process, the pressure load is in the range of 3 MPa or more and 12 MPa or less, the heating temperature is in the range of 600°C or more and 1300°C or less, and the holding time at the heating temperature is in the range of 2 hours or more and 15 hours or less. This allows the OH groups present on the bonding surfaces of the plate-like members to bond with each other and undergo a dehydration condensation reaction, thereby making it possible to firmly bond the plate-like members together.

[0018] The method for manufacturing a silicon member of aspect 6 of the present invention is characterized in that, in the method for manufacturing a silicon member of aspect 5, it further includes, prior to the lamination step, an OH group introduction treatment step of introducing an OH group into the bonding surface of the plate-like member. According to the method for manufacturing a silicon member of aspect 6 of the present invention, an OH group introduction process for introducing OH groups into the bonding surfaces of the plate-like members is included. This makes it possible to provide a sufficient amount of OH groups on the bonding surfaces of the plate-like members, and to firmly bond the plate-like members together through a dehydration condensation reaction. Effect of the Invention

[0019] According to the present invention, it is possible to provide a silicon member in which a plurality of plate-like members are reliably bonded, which has excellent heat resistance and is capable of suppressing the occurrence of contamination, and a method for manufacturing this silicon member. [Brief description of the drawings]

[0020] [Figure 1] 1A and 1B are explanatory diagrams showing an example of a silicon member according to an embodiment of the present invention, in which (a) is a perspective view and (b) is an enlarged explanatory view of a cross section taken along line XX of a bonding portion. [Diagram 2] 1 is an explanatory diagram showing a bonding state between silicon members according to an embodiment of the present invention; [Diagram 3] FIG. 1 is a flow diagram showing a method for manufacturing a silicon member according to an embodiment of the present invention. [Figure 4] 1 is a schematic diagram illustrating a tensile test in an embodiment, in which (a) is a test piece, (b) is a test piece and a tensile test fixture, and (c) is a tensile test machine. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0021] A silicon member according to an embodiment of the present invention and a method for manufacturing the silicon member will be described below. The silicon member of this embodiment is, for example, a silicon member disposed in a chamber of a plasma processing apparatus such as a plasma etching apparatus or a plasma CVD apparatus used in a semiconductor device manufacturing process, and in this embodiment, is a silicon electrode plate having a structure in which a plurality of air holes are formed in a plate-shaped member. In the silicon member of this embodiment, a plurality of silicon electrode plates that have been worn down through use are bonded together to be used as a regenerated silicon electrode plate having a structure in which a plurality of silicon electrode plates are bonded in the thickness direction.

[0022] As shown in FIG. 1(a), the silicon member 10 of this embodiment has a plurality of ventilation holes 10A penetrating in the thickness direction. As shown in Figs. 1(a) and 1(b), the silicon member 10 according to the present embodiment has a structure in which a first plate-shaped member 11 and a second plate-shaped member 12 are bonded in the thickness direction, and the first plate-shaped member 11 and the second plate-shaped member 12 are directly bonded to each other. The first plate-shaped member 11 and the second plate-shaped member 12 are made of a Si-containing material such as silicon, silicon nitride, or silicon carbide. The first plate-shaped member 11 and the second plate-shaped member 12 may be made of a single crystal silicon plate, a polycrystalline silicon plate, or a columnar crystal silicon plate. A single crystal silicon plate is made of a single crystal as a whole, and has the same atomic arrangement, while a polycrystalline silicon plate is made of a plurality of crystals. A columnar crystal silicon plate is manufactured by slicing an ingot grown in one direction in a direction perpendicular to the crystal growth direction.

[0023] In this embodiment, the total content of metal elements other than Si in the joint between the first plate-shaped member 11 and the second plate-shaped member 12 is set to 5 mass % or less. The total content of metal elements other than Si in the joint between the first plate-like member 11 and the second plate-like member 12 is preferably 1 mass% or less, and more preferably 0.5 mass% or less. The lower limit of the total content of metal elements other than Si in the joint is not particularly limited, but may be 0 mass%. In this embodiment, the total content of Al, Ti, Cr, Mn, Fe, Co, Ni, Cu, In, Sn, Zn, Y, Mo, Hf, Ta, W, and Pb as metal elements other than Si in the joint is preferably 5 mass% or less. The total content of Al, Ti, Cr, Mn, Fe, Co, Ni, Cu, In, Sn, Zn, Y, Mo, Hf, Ta, W, and Pb as metal elements other than Si in the joint is preferably 1 mass% or less, and more preferably 0.5 mass% or less. In this embodiment, the metal elements other than Si in the joint are preferably one or more of Al, Ti, Cr, Mn, Fe, Co, Ni, Cu, In, Sn, Zn, Y, Mo, Hf, Ta, W, and Pb. In addition, the lower limit of the total content of metal elements other than Si in the joint, namely Al, Ti, Cr, Mn, Fe, Co, Ni, Cu, In, Sn, Zn, Y, Mo, Hf, Ta, W, and Pb, is not particularly limited, but may be 0 mass%.

[0024] In this embodiment, the bonding strength between the first plate-shaped member 11 and the second plate-shaped member 12 is set to 5 MPa or more. The bonding strength between the first plate-like member 11 and the second plate-like member 12 is preferably 8 MPa or more, and more preferably 10 MPa or more.

[0025] In this embodiment, the void ratio in the joint between the first plate-shaped member 11 and the second plate-shaped member 12 is preferably 20% or less. The void ratio in the joint between the first plate-like member 11 and the second plate-like member 12 is preferably 10% or less, and more preferably 1% or less. There is no particular lower limit to the void ratio, but it may be 0%.

[0026] In the silicon member 10 of this embodiment, as shown in FIG. 2, the first plate-shaped member 11 and the second plate-shaped member 12 are preferably bonded together via oxygen (O). More specifically, OH groups are present on the bonding surface of the first plate-like member 11 and the bonding surface of the second plate-like member 12, and these OH groups bond together to generate water, which evaporates through dehydration condensation, bonding Si on the bonding surface of the first plate-like member 11 and Si on the bonding surface of the second plate-like member 12 via oxygen (O). This allows the first plate-like member 11 and the second plate-like member 12 to be firmly bonded together.

[0027] Next, a method for manufacturing the silicon member 10 according to the present embodiment will be described with reference to FIG.

[0028] As shown in FIG. 3, the manufacturing method of the silicon member 10 according to this embodiment includes a surface grinding process S01 for grinding the surfaces of the first plate-shaped member 11 and the second plate-shaped member 12, an OH group introduction process S02 for introducing OH groups to the bonding surfaces of the first plate-shaped member 11 and the second plate-shaped member 12, a lamination process S03 for forming a laminate of the first plate-shaped member 11 and the second plate-shaped member 12, a bonding process S04 for heating the laminate while applying pressure in the stacking direction to bond the first plate-shaped member 11 and the second plate-shaped member 12, a processing process S05, and a finishing process S06.

[0029] Each step of the method for producing the silicon member 10 according to this embodiment will be described in detail below.

[0030] (Surface grinding process S01) The surfaces of the first plate-shaped member 11 and the second plate-shaped member 12 are ground by a grinding machine. In this embodiment, two used silicon electrode plates are prepared, and the surfaces (plasma surfaces) of these used silicon electrode plates are ground by a grinding machine to form the first plate-shaped member 11 and the second plate-shaped member 12. By grinding the plasma surface, the portion of the vent hole on the plasma surface side that has expanded in diameter due to wear during use is removed. Then, the surfaces of the first plate-shaped member 11 and the second plate-shaped member 12 are polished using a slurry containing an abrasive such as colloidal silica or diamond abrasive grains.

[0031] (OH group introduction process S02) Next, OH groups are introduced into the bonding surfaces of the first plate-shaped member 11 and the second plate-shaped member 12. Examples of the method for introducing OH groups include oxygen plasma, H 2 O 2 +H 2 SO 4 It is possible to appropriately select and apply an existing method such as applying an oxidizing agent such as the above or applying water. If there are sufficient OH groups on the bonding surfaces of the first plate-shaped member 11 and the second plate-shaped member 12 after the surface grinding step S01, the OH group introduction treatment step S02 may be omitted.

[0032] (Lamination process S03) Next, the first plate-shaped member 11 and the second plate-shaped member 12 are laminated so that their bonding surfaces face each other to form a laminate. Note that OH groups are present on the bonding surfaces of the first plate-shaped member 11 and the second plate-shaped member 12, respectively.

[0033] (Joining process S04) Next, the laminate is heated while being pressed in the lamination direction, so that the first plate-shaped member 11 and the second plate-shaped member 12 are directly bonded together. Here, in the joining step S04, the pressure load is within a range of 3 MPa to 12 MPa, the heating temperature is within a range of 600° C. to 1300° C., and the holding time at the heating temperature is within a range of 2 hours to 15 hours.

[0034] By stacking the first plate-like member 11 and the second plate-like member 12, which have OH groups on their bonding surfaces, and applying pressure and heat to them, as shown in Figure 2, the OH groups bond together and a dehydration condensation reaction progresses, resulting in bonding between Si on the bonding surface of the first plate-like member 11 and Si on the bonding surface of the second plate-like member 12 via oxygen (O).

[0035] By setting the pressure load at 3 MPa or more in the bonding step S04, the bonding surfaces can be sufficiently adhered to each other, and the first plate-shaped member 11 and the second plate-shaped member 12 can be bonded via oxygen. In addition, by setting the pressure load at 3 MPa or more, the occurrence of cracks in the first plate-shaped member 11 and the second plate-shaped member 12 can be suppressed. The lower limit of the pressure load in the joining step S04 is preferably 3 MPa or more, more preferably 6 MPa or more, and the upper limit of the pressure load is preferably 15 MPa or less, more preferably 12 MPa or less.

[0036] By setting the heating temperature in the bonding step S04 to 600° C. or higher, the dehydration condensation reaction can be sufficiently advanced, and the first plate-shaped member 11 and the second plate-shaped member 12 can be bonded via oxygen. In addition, by setting the heating temperature to 1300° C. or lower, deformation and thermal deterioration of the first plate-shaped member 11 and the second plate-shaped member 12 can be suppressed. The lower limit of the heating temperature in the bonding step S04 is preferably 600° C. or higher, and more preferably 1000° C. or higher. The upper limit of the heating temperature is preferably 1300° C. or lower, and more preferably 1200° C. or lower.

[0037] By setting the holding time at the heating temperature in the bonding step S04 to 600 hours or more, the dehydration condensation reaction can be sufficiently advanced, and the first plate-shaped member 11 and the second plate-shaped member 12 can be bonded via oxygen. In addition, by setting the holding time at the heating temperature to 15 hours or less, deformation and thermal deterioration of the first plate-shaped member 11 and the second plate-shaped member 12 can be suppressed. The lower limit of the holding time at the heating temperature in the bonding step S04 is preferably 2 hours or more, more preferably 5 hours or more, and the upper limit of the holding time at the heating temperature is preferably 15 hours or less, more preferably 10 hours or less.

[0038] (Processing process S05) Next, the air holes 10A are formed by drilling or laser processing in the bonded body of the first plate-like member 11 and the second plate-like member 12. In addition, the outer shape is processed by cutting.

[0039] (Finishing process S06) The surface of the bonded body of the first plate-like member 11 and the second plate-like member 12 is polished using a slurry containing an abrasive such as colloidal silica or diamond abrasive grains. After polishing, the bonded body is washed with running water. Ultrasonic cleaning, degreasing cleaning, and acid cleaning may also be performed. Acid etching may also be performed before polishing.

[0040] Through the various steps described above, the silicon member 10 of this embodiment is manufactured.

[0041] According to the silicon member 10 of the present embodiment configured as described above, the total content of metal elements other than Si in the joint between the first plate-shaped member 11 and the second plate-shaped member 12 is limited to 5 mass% or less, so that it is possible to suppress the occurrence of contamination in the plasma processing apparatus. In addition, it is possible to use a corrosive etching gas, and it is possible to select a wide range of etching gases. Furthermore, since the joint is not made of a eutectic alloy, it has excellent heat resistance. Furthermore, since the bonding strength between the first plate-shaped member 11 and the second plate-shaped member 12 is 10 MPa or more, the first plate-shaped member 11 and the second plate-shaped member 12 are reliably bonded together with sufficient strength, and can be used satisfactorily as an electrode plate.

[0042] In the silicon member 10 of this embodiment, when the total content of Al, Ti, Cr, Mn, Fe, Co, Ni, Cu, In, Sn, Zn, Y, Mo, Hf, Ta, W, and Pb as metal elements other than Si at the joint is 5 mass% or less, the occurrence of contamination within the plasma processing apparatus can be sufficiently suppressed and a wider range of etching gases can be selected.

[0043] In the silicon member 10 of this embodiment, as shown in FIG. 2, when the first plate-shaped member 11 and the second plate-shaped member 12 are bonded via oxygen, the plate-shaped members can be firmly bonded to each other.

[0044] In the silicon member 10 of this embodiment, when the void ratio at the joint between the first plate-shaped member 11 and the second plate-shaped member 12 is 20% or less, the first plate-shaped member 11 and the second plate-shaped member 12 are firmly joined, and the joining strength can be sufficiently improved.

[0045] The manufacturing method of the silicon member 10 of this embodiment includes a lamination process S03 in which the first plate-shaped member 11 and the second plate-shaped member 12 are directly laminated together, and a bonding process S04 in which the laminated first plate-shaped member 11 and the second plate-shaped member 12 are heated while being pressurized in the stacking direction to bond the first plate-shaped member 11 and the second plate-shaped member 12 together. In the bonding process S04, the pressure load is in the range of 3 MPa or more and 12 MPa or less, the heating temperature is in the range of 600°C or more and 1250°C or less, and the holding time at the heating temperature is in the range of 2 hours or more and 15 hours or less. Therefore, OH groups present on the bonding surfaces of the first plate-shaped member 11 and the second plate-shaped member 12 bond with each other and undergo a dehydration condensation reaction, making it possible to firmly bond the first plate-shaped member 11 and the second plate-shaped member 12 together. Furthermore, since no bonding material is used to bond the plate-like members together, it is possible to prevent metal elements other than silicon from being included in the bonded portion.

[0046] In the manufacturing method of the silicon member 10 of this embodiment, if an OH group introduction processing step S02 for introducing OH groups into the bonding surfaces of the first plate-shaped member 11 and the second plate-shaped member 12 is included before the lamination step S03, a sufficient amount of OH groups can be provided on the bonding surfaces of the first plate-shaped member 11 and the second plate-shaped member 12, making it possible to firmly bond the plate-shaped members together by a dehydration condensation reaction.

[0047] Although the embodiment of the present invention has been described above, the present invention is not limited to this, and can be modified as appropriate without departing from the technical concept of the invention. For example, in this embodiment, the silicon member has been described as a recycled silicon electrode plate formed by joining two used silicon electrode plates, but this is not limited to this, and the silicon member may be any member formed by joining plate-shaped members made of a Si-containing material together, or may be three or more plate-shaped members joined together.

[0048] For example, in the present embodiment, the joining step S04 is followed by the processing step S05 of forming the vent hole 10A, but the present invention is not limited to this, and the first plate-shaped member and the second plate-shaped member may be previously processed to form the vent hole 10A, and these may be laminated and joined together. By forming through holes and grooves in the first plate-shaped member and the second plate-shaped member, it is possible to form the vent hole 10A having a curved complex shape. EXAMPLES

[0049] The results of confirmatory experiments conducted to confirm the effectiveness of the present invention will be described below.

[0050] Two silicon plate members (φ350 mm×t5 mm) were prepared. Then, two plate members were bonded together under the conditions shown in Table 1. In addition, in Examples 1 to 7 of the present invention and Comparative Examples 1 to 3, direct bonding was performed without using a bonding material. In Comparative Example 4, bonding was performed using an Al foil as a bonding material. In Comparative Example 5, bonding was performed using an elastomer material containing silicone and a conductive filler as a bonding material. The obtained silicon member was evaluated as follows. The evaluation results are shown in Table 2.

[0051] (Si content and metal element content other than Si in joint) The cross section along the lamination direction of the silicon member was observed with a scanning electron microscope (JSM-IT500HR manufactured by JEOL Ltd.), and the bonding layer in the cross section was subjected to linear analysis of elements at a magnification of 5000 times. Using the quantitative function of the software attached to the device (energy dispersive X-ray analysis), a semi-quantitative analysis was performed on the elements detected as Si in the bonding area. Note that, since carbon (C), nitrogen (N), oxygen (O), etc. are easily detected due to environmental factors, the observation was performed immediately after ion milling. In addition, due to the measurement principle, the accuracy of background correction for light elements is poor, so in the direct bonding of the present invention, the ratio of metal elements other than Si was set to 5 mass% or less, and the ratio of Si was set to 90 mass% or more. In addition, the total content of Al, Ti, Cr, Mn, Fe, Co, Ni, Cu, In, Sn, Zn, Y, Mo, Hf, Ta, W, and Pb was evaluated by line analysis.

[0052] (Joining strength) As shown in Figure 4, the obtained silicon member was cut into 10 mm squares, and the surface opposite to the joining surface of the plate-like member was joined to a tensile test jig using an adhesive. The plate-like member was then set in a universal tensile tester, and a tensile test was carried out at a speed of 0.1 mm / min. When the adhesive strength between the plate-like member and the tensile test jig exceeded 10 MPa, it was noted as "10 MPa or more."

[0053] (Void ratio) The ultrasonic inspection device irradiated ultrasonic waves in the thickness direction, and the locations where the reflected waves were found at the joint positions were determined as voids. The ultrasonic inspection image obtained was then binarized, and the ratio of the void area to the total joint area of ​​the joint was determined as the void ratio.

[0054] (exterior) The appearance of the obtained silicon member was visually observed and evaluated for the presence or absence of cracks or chips. Those that were found to have cracks or chips were marked with "X", and those that were not found to have cracks or chips were marked with "O".

[0055] (Heat resistance test) The obtained silicon parts were held at 700°C for 24 hours, and ultrasonic inspection was carried out before and after heating to 700°C. As a result of the inspection, parts that showed cracks or peeling were marked with "X", and parts that showed no change in the ultrasonic inspection image (change in bonding rate) were marked with "◎".

[0056] [Table 1]

[0057] [Table 2]

[0058] In Comparative Example 1, the pressure load during bonding was as large as 20 MPa, causing cracks in the silicon member. Note that no evaluation of bonding strength was performed. In Comparative Example 2, the pressure load during bonding was as low as 1 MPa, and the plate-like members could not be bonded sufficiently, resulting in a low bonding strength of 3 MPa. In Comparative Example 3, the heating temperature during bonding was low at 200° C., and the plate-like members could not be bonded sufficiently, resulting in a low bonding strength of 2 MPa. In Comparative Example 4, since Al was used as the bonding material, the total content of metal elements other than Si in the bonding portion was 100 mass %, which caused a risk of contamination and insufficient heat resistance. In Comparative Example 5, an elastomer material containing silicone and conductive filler was used as the bonding material, so the Si content in the bonding part was 30 mass% and the total content of metal elements other than Si was 40 mass%, which resulted in a risk of contamination and insufficient heat resistance.

[0059] In contrast, in Examples 1 to 7 of the present invention, the silicon plate-like members were directly bonded to each other without using a bonding material, so the total content of metal elements other than Si in the bonded portion was 5 mass% or less, there was no risk of contamination, and the heat resistance was excellent. In addition, the bond strength was 5 MPa or more, and the plate-like members were firmly bonded to each other.

[0060] As a result of the above, it was confirmed that the present invention can provide a silicon component in which multiple plate-like members are reliably bonded, has excellent heat resistance, and is capable of suppressing the occurrence of contamination, as well as a method for manufacturing this silicon component. [Explanation of symbols]

[0061] 10 Silicone parts 11 First plate-shaped member 12 Second plate-shaped member

Claims

1. A silicon member used in a plasma processing apparatus, A structure in which a plurality of plate-shaped members made of a Si-containing material are bonded in the thickness direction, the Si content at the bonded portions between the plate-shaped members is 90 mass% or more, and the total content of metal elements other than Si is 5 mass% or less, A silicon member, characterized in that the bonding strength between the plate-like members is 5 MPa or more.

2. The silicon member according to claim 1, characterized in that the total content of Al, Ti, Cr, Mn, Fe, Co, Ni, Cu, In, Sn, Zn, Y, Mo, Hf, Ta, W, and Pb as metal elements other than Si in the joint is 5 mass% or less.

3. 2. The silicon member according to claim 1, wherein the plate-like members are bonded to each other at the bonding portion via oxygen.

4. 2. The silicon member according to claim 1, wherein a void ratio in the joint is 20% or less.

5. A method for producing a silicon member according to any one of claims 1 to 4, comprising the steps of: The method includes a lamination process of directly laminating a plurality of the plate-like members, and a joining process of heating the laminated plate-like members while applying pressure to each other in a lamination direction, thereby joining the plate-like members to each other, The method for manufacturing a silicon member, wherein in the bonding step, the pressure load is in the range of 3 MPa or more and 12 MPa or less, the heating temperature is in the range of 600°C or more and 1300°C or less, and the holding time at the heating temperature is in the range of 2 hours or more and 15 hours or less.

6. 6. The method for manufacturing a silicon member according to claim 5, further comprising, before the lamination step, a step of introducing OH groups into the joining surfaces of the plate-like members.

Citation Information

Patent Citations

  • Joint structure for constituting member and method therefor, and member for semiconductor manufacturing apparatus

    JP2000286244A

  • Joining member and method of manufacturing joining member

    JP2006278807A

  • Silicon direct bonding method

    JP2007184546A

  • Method for manufacturing substrate

    JP2012161831A

  • Substrate bonding apparatus and substrate bonding method

    JP2018201022A