Unsaturated polyester resin composition, molding material and molded article

The unsaturated polyester resin composition addresses surface irregularities and antiviral effectiveness in molded products by using specific ratios of low-shrinkage agents and silver-containing antiviral agents, enhancing both appearance and antiviral properties.

JP2024143046AActive Publication Date: 2024-10-11JAPAN COMPOSITE
View PDF 4 Cites 0 Cited by

Patent Information

Application Number
JP2023055523
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Filing Date
2023-03-30
Publication Date
2024-10-11
Estimated Expiration
2043-03-30

AI Technical Summary

Technical Problem

Molded products made from unsaturated polyester resin compositions exhibit poor mechanical properties, water resistance, and uneven surfaces, which can lead to issues like scumming and reduced antiviral effectiveness due to improper adjustment of antiviral agent content.

Method used

An unsaturated polyester resin composition is formulated with specific ratios of low-shrinkage agents and silver-containing antiviral agents, such as silver-supported phosphate or silicate glass, to improve surface smoothness and antiviral properties while suppressing scumming.

Benefits of technology

The composition effectively reduces surface irregularities and enhances antiviral resistance, improving the appearance and gloss of molded products by optimizing the content ratios of low-shrinkage and silver-containing antiviral agents.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024143046000001
    Figure 2024143046000001
  • Figure 2024143046000002
    Figure 2024143046000002
Patent Text Reader

Abstract

To provide an unsaturated polyester resin composition which is reduced in surface unevenness and can exhibit excellent antiviral property, and enables the improvement of the appearance thereof (glossiness and suppression of the occurrences of scumming), molding material including the unsaturated polyester resin composition, and a molded article including the cured product of the molding material.SOLUTION: An unsaturated polyester resin composition includes unsaturated polyester, a polymerizable monomer, a shrinkage reducing agent, and a silver-containing antiviral agent. A content ratio of the shrinkage reducing agent is 1.2 pts.mass or more and 50.0 pts.mass or less with respect to 100 pts.mass of the unsaturated polyester. A content ratio of the silver-containing antiviral agent is 7.0 pts.mass or more and 60.0 pts.mass or less with respect to 100 pts.mass of the unsaturated polyester.SELECTED DRAWING: None
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to an unsaturated polyester resin composition, a molding material, and a molded article. [Background technology]

[0002] Conventionally, molded articles made of molding materials containing unsaturated polyester resin compositions (particularly, sheet molding compounds (SMC), bulk molding compounds (BMC), and thick molding compounds (TMC)) have been used in a wide range of fields due to their excellent mechanical properties, water resistance, and corrosion resistance.

[0003] On the other hand, from the viewpoint of hygiene, it is known to incorporate an antibacterial agent into an unsaturated polyester resin composition.

[0004] As such an unsaturated polyester resin composition, for example, a thermosetting resin composition containing an unsaturated polyester resin and a silver-glass based inorganic antibacterial agent has been proposed (see, for example, the examples of Patent Document 1 below). [Prior art documents] [Patent documents]

[0005] [Patent Document 1] JP 2000-037742 A Summary of the Invention [Problem to be solved by the invention]

[0006] On the other hand, there are cases where an antiviral agent is used instead of an antibacterial agent. In such cases, from the viewpoint of improving the antiviral properties, it has been considered to increase the amount of the antiviral agent, but it has been found that when a molded article has unevenness, there is a problem in that the antiviral properties corresponding to the blended amount of the antiviral agent are not expressed.

[0007] The present invention provides an unsaturated polyester resin composition that can reduce surface irregularities to exhibit excellent virus resistance and improve appearance (gloss and suppression of the occurrence of scumming); a molding material containing the unsaturated polyester resin composition; and a molded article containing a cured product of the molding material. [Means for solving the problem]

[0008] The present invention [1] is an unsaturated polyester resin composition comprising an unsaturated polyester, a polymerizable monomer, a low-profile agent, and a silver-containing antiviral agent, in which the content of the low-profile agent is 1.2 parts by mass or more and 50.0 parts by mass or less per 100 parts by mass of the unsaturated polyester, and the content of the silver-containing antiviral agent is 7.0 parts by mass or more and 60.0 parts by mass or less per 100 parts by mass of the unsaturated polyester.

[0009] The present invention [2] includes the unsaturated polyester resin composition according to the above [1], in which the silver-containing antiviral agent includes silver-loaded phosphate or silver-loaded silicate glass.

[0010] The present invention [3] comprises the unsaturated polyester resin composition according to the above [1] or [2], in which the silver-containing antiviral agent has a silver content of 1 mass% or more.

[0011] The present invention [4] includes the unsaturated polyester resin composition according to any one of the above [1] to [3], further comprising a curing agent, the 10-hour half-life temperature of the curing agent being 103°C or lower.

[0012] The present invention [5] includes a molding material containing the unsaturated polyester resin composition according to any one of the above [1] to [4] and reinforcing fibers.

[0013] The present invention [6] includes a molded article, characterized in that it contains a cured product of the molding material described in [5] above. Effect of the Invention

[0014] In the unsaturated polyester resin composition of the present invention, the content ratio of the shrinkage reducing agent and the content ratio of the silver-containing antiviral agent are each within a predetermined range. Therefore, a molded article obtained by using this unsaturated polyester resin composition can reduce surface irregularities and exhibit excellent virus resistance, and can also improve appearance (gloss and suppression of scumming).

[0015] The molding material of the present invention contains the unsaturated polyester resin composition of the present invention. Therefore, a molded article obtained by using this molding material can reduce surface irregularities, exhibit excellent virus resistance, and improve appearance (gloss and suppression of scumming).

[0016] The molded article of the present invention contains a cured product of the molding material of the present invention, and therefore can exhibit excellent virus resistance by reducing surface irregularities, and can also improve appearance (gloss and suppression of scumming). DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0017] 1. Unsaturated polyester resin composition The unsaturated polyester resin composition contains an unsaturated polyester, a polymerizable monomer, a shrinkage reducing agent, and a silver-containing antiviral agent.

[0018] <Unsaturated polyester> Unsaturated polyester is obtained by reacting polybasic acid with polyhydric alcohol. Each raw material used in this reaction may be used alone or in combination with other raw materials depending on the required performance. Also, it may be modified with dicyclopentadiene (DCPD).

[0019] In the following description, the unsaturated polyester resin is composed of an unsaturated polyester and a polymerizable monomer (described later).

[0020] The polybasic acid includes a polybasic acid having an ethylenically unsaturated double bond as an essential component (hereinafter referred to as an ethylenically unsaturated bond-containing polybasic acid) and a polybasic acid not having an ethylenically unsaturated double bond as an optional component (hereinafter referred to as an ethylenically unsaturated bond-free polybasic acid).

[0021] Examples of the ethylenically unsaturated bond-containing polybasic acid include ethylenically unsaturated aliphatic dibasic acids and their anhydrides, halides of ethylenically unsaturated aliphatic dibasic acids, and alkyl esters of ethylenically unsaturated aliphatic dibasic acids.

[0022] Examples of ethylenically unsaturated aliphatic dibasic acids include maleic acid, fumaric acid, itaconic acid, and dihydromuconic acid. Examples of ethylenically unsaturated bond-containing polybasic acids include acid anhydrides derived from the above ethylenically unsaturated aliphatic dibasic acids. Examples of ethylenically unsaturated bond-containing polybasic acids include maleic anhydride. Examples of ethylenically unsaturated bond-containing polybasic acids include maleic anhydride.

[0023] Examples of polybasic acids not containing ethylenically unsaturated bonds include saturated aliphatic polybasic acids, saturated alicyclic polybasic acids, aromatic polybasic acids, anhydrides of these acids, halides of these acids, and alkyl esters of these acids.

[0024] Examples of the saturated aliphatic polybasic acid include saturated aliphatic dibasic acids.

[0025] Examples of saturated aliphatic dibasic acids include oxalic acid, malonic acid, succinic acid, methylsuccinic acid, 2,2-dimethylsuccinic acid, 2,3-dimethylsuccinic acid, hexylsuccinic acid, glutaric acid, 2-methylglutaric acid, 3-methylglutaric acid, 2,2-dimethylglutaric acid, 3,3-dimethylsuccinic acid, adipic acid, pimelic acid, suberic acid, azelaic acid, and sebacic acid. Examples of saturated aliphatic polybasic acids include acid anhydrides derived from the above-mentioned saturated aliphatic dibasic acids. Examples of acid anhydrides derived from saturated aliphatic dibasic acids include oxalic anhydride and succinic anhydride.

[0026] Examples of the saturated alicyclic polybasic acid include saturated alicyclic dibasic acids.

[0027] Examples of saturated alicyclic dibasic acids include HET acid, 1,2-hexahydrophthalic acid, 1,1-cyclobutanedicarboxylic acid, and 1,4-cyclohexanedicarboxylic acid (cis- or trans-1,4-cyclohexanedicarboxylic acid or a mixture thereof). Examples of saturated alicyclic polybasic acids include acid anhydrides derived from the above-mentioned saturated alicyclic dibasic acids. Examples of acid anhydrides derived from saturated alicyclic dibasic acids include HET acid anhydride.

[0028] Examples of aromatic polybasic acids include aromatic dibasic acids.

[0029] Examples of aromatic dibasic acids include phthalic acid (orthophthalic acid, isophthalic acid, terephthalic acid), trimellitic acid, and pyromellitic acid. Examples of aromatic polybasic acids include acid anhydrides derived from the above aromatic dibasic acids. Examples of acid anhydrides derived from aromatic dibasic acids include phthalic anhydride. Examples of aromatic dibasic acids include isophthalic acid.

[0030] The polybasic acids can be used alone or in combination of two or more kinds.

[0031] When the polybasic acid includes an ethylenically unsaturated bond-containing polybasic acid and an ethylenically unsaturated bond-free polybasic acid, the content of the ethylenically unsaturated bond-containing polybasic acid is, for example, 50 mol% or more, preferably 60 mol% or more, more preferably 70 mol% or more, and, for example, 95 mol% or less, preferably 90 mol% or less, based on 100 mol of the total polybasic acid. The content of the ethylenically unsaturated bond-free polybasic acid is, for example, 5 mol% or more, preferably 10 mol% or more, and, for example, 50 mol% or less, preferably 40 mol% or less, more preferably 30 mol% or less.

[0032] Polyhydric alcohols include, for example, dihydric and trihydric alcohols.

[0033] Examples of dihydric alcohols include aliphatic diols, alicyclic diols, and aromatic diols. Examples of aliphatic diols include alkanediols and ether diols. Examples of alkanediols include alkanediols having 2 to 10 carbon atoms. Examples of alkanediols having 2 to 10 carbon atoms include ethylene glycol, propylene glycol (1,2- or 1,3-propanediol or a mixture thereof), butylene glycol (1,2- or 1,3- or 1,4-butylene glycol or a mixture thereof), 1,5-pentanediol, 1,6-hexanediol, neopentyl glycol, 2-methyl-1,3-propanediol, 2-butyl-2-ethyl-1,3-propanediol, 3-methyl-1,5-pentanediol, 2,2,2-trimethylpentanediol, and 3,3-dimethylolheptane. Examples of ether diols include diethylene glycol, triethylene glycol, and dipropylene glycol. Examples of alicyclic diols include cyclohexanediol (1,2- or 1,3- or 1,4-cyclohexanediol or a mixture thereof), cyclohexanedimethanol (1,2- or 1,3- or 1,4-cyclohexanedimethanol or a mixture thereof), cyclohexanediethanol (1,2- or 1,3- or 1,4-cyclohexanediethanol or a mixture thereof), and hydrogenated bisphenol A. Examples of aromatic diols include an ethylene oxide adduct of bisphenol A and a propylene oxide adduct of bisphenol A.

[0034] Examples of trihydric alcohols include glycerin, trimethylolpropane, and triisopropanolamine.

[0035] The polyhydric alcohol is preferably a dihydric alcohol. The polyhydric alcohol is more preferably an aliphatic diol. The polyhydric alcohol is further preferably an alkanediol having 2 to 10 carbon atoms. The polyhydric alcohol is particularly preferably an alkanediol. The polyhydric alcohol is most preferably propylene glycol, neopentyl glycol, hydrogenated bisphenol A, an ethylene oxide adduct of bisphenol A, and a propylene oxide adduct of bisphenol A.

[0036] The polyhydric alcohols can be used alone or in combination of two or more kinds.

[0037] The unsaturated polyester is prepared by reacting a polybasic acid with a polyhydric alcohol.

[0038] The equivalent ratio of the polyhydric alcohol to the polybasic acid (hydroxyl groups of the polyhydric alcohol / carboxyl groups of the polybasic acid) is, for example, 0.9 or more, preferably 0.95 or more, and for example, 1.2 or less, preferably 1.1 or less.

[0039] The reaction temperature is, for example, 150° C. or more, preferably 190° C. or more, and for example, 250° C. or less, preferably 230° C. or less.

[0040] In the above reaction, a known solvent and a known reaction catalyst can be added, if necessary.

[0041] This allows the preparation of an unsaturated polyester.

[0042] The acid value of the unsaturated polyester (measurement method: in accordance with JIS K6901 (2008)) is, for example, 5 mgKOH / g or more, preferably 10 mgKOH / g or more, and for example, less than 40 mgKOH / g, preferably 30 mgKOH / g or less.

[0043] The weight average molecular weight of the unsaturated polyester is, for example, 2,000 or more, preferably 4,000 or more, and for example, 25,000 or less, preferably 20,000 or less.

[0044] The weight average molecular weight is a weight average molecular weight calculated in terms of polystyrene by gel permeation chromatography (GPC), and can be determined by measuring the unsaturated polyester by GPC.

[0045] The unsaturated polyesters can be used alone or in combination of two or more kinds.

[0046] The content of the unsaturated polyester is, relative to 100 parts by mass of the total amount of the unsaturated polyester, the polymerizable monomer, and the low shrinkage agent, for example, 20 parts by mass or more, preferably 40 parts by mass or more, more preferably 45 parts by mass or more, and for example, 80 parts by mass or less, preferably 60 parts by mass or less, more preferably 55 parts by mass or less, and even more preferably 50 parts by mass or less.

[0047] <Polymerizable monomer> Examples of the polymerizable monomer include styrene-based monomers and (meth)acrylic acid ester-based monomers.

[0048] Styrenic monomers include, for example, styrene, vinyltoluene, t-butylstyrene, and chlorostyrene.

[0049] Examples of (meth)acrylic acid ester monomers include (meth)acrylic acid alkyl esters, (meth)acrylic acid allyl esters, ring-containing (meth)acrylic acid esters, (meth)acrylic acid hydroxyalkyl esters, (meth)acrylic acid alkoxyalkyl esters, (meth)acrylic acid aminoalkyl esters, (meth)acrylic acid fluoroalkyl esters, and polyfunctional (meth)acrylic acid esters. Examples of (meth)acrylic acid alkyl esters include methyl (meth)acrylate, ethyl (meth)acrylate, isopropyl (meth)acrylate, butyl (meth)acrylate, n-butyl (meth)acrylate, t-butyl (meth)acrylate, isobutyl (meth)acrylate, 2-ethylhexyl (meth)acrylate, lauryl (meth)acrylate, tridecyl (meth)acrylate, and stearyl (meth)acrylate. Examples of (meth)acrylic acid allyl esters include allyl (meth)acrylate. Examples of ring-containing (meth)acrylic acid esters include cyclohexyl (meth)acrylate, benzyl (meth)acrylate, isobornyl (meth)acrylate, glycidyl (meth)acrylate, tetrahydrofurfuryl (meth)acrylate, dicyclopentenyl (meth)acrylate, dicyclopentanyl (meth)acrylate, and dicyclopentenyloxyethyl (meth)acrylate. Examples of hydroxyalkyl (meth)acrylic acid esters include 2-hydroxyethyl (meth)acrylate and 2-hydroxypropyl (meth)acrylate. Examples of alkoxyalkyl (meth)acrylic acid esters include 2-methoxyethyl (meth)acrylate and 2-ethoxyethyl (meth)acrylate. Examples of aminoalkyl (meth)acrylic acid esters include dimethylaminoethyl (meth)acrylate, diethylaminoethyl (meth)acrylate, and chloride salts thereof. Examples of the fluoroalkyl (meth)acrylate include trifluoroethyl (meth)acrylate and heptadecafluorodecyl (meth)acrylate.Examples of polyfunctional (meth)acrylic acid esters include ethylene glycol di(meth)acrylate, diethylene glycol di(meth)acrylate, trimethylolpropane tri(meth)acrylate, pentaerythritol tetra(meth)acrylate, and dipentaerythritol hexa(meth)acrylate.

[0050] As the polymerizable monomer, preferably, styrene-based monomer and (meth)acrylic acid alkyl ester are mentioned. As the polymerizable monomer, more preferably, styrene and methyl methacrylate are mentioned. As the polymerizable monomer, more preferably, styrene is mentioned.

[0051] The polymerizable monomers can be used alone or in combination of two or more kinds.

[0052] The content of the polymerizable monomer, relative to 100 parts by mass of the total amount of the unsaturated polyester, the polymerizable monomer, and the low shrinkage agent, is, for example, 20 parts by mass or more, preferably 30 parts by mass or more, more preferably 40 parts by mass or more, even more preferably 42 parts by mass or more, and for example, 75 parts by mass or less, preferably 60 parts by mass or less, more preferably 50 parts by mass or less.

[0053] <Low shrinkage agent> When a molded article is obtained using this unsaturated polyester resin composition, the low shrinkage agent is blended in order to suppress cure shrinkage and heat shrinkage of the molded article and to improve the appearance.

[0054] Examples of the low shrinkage agent include polyethylene, polystyrene, styrene-based thermoplastic elastomer, crosslinked polystyrene, polyvinyl acetate-polystyrene block copolymer, polyvinyl acetate, polymethyl methacrylate, and saturated polyester resin. Preferred examples of the low shrinkage agent include polystyrene and crosslinked polystyrene.

[0055] The low shrinkage agent can be used alone or in combination of two or more. Preferably, polystyrene and cross-linked polystyrene are used in combination as the low shrinkage agent. When polystyrene and cross-linked polystyrene are used in combination as the low shrinkage agent, the content of polystyrene is, for example, 30 parts by mass or more, preferably 40 parts by mass or more, and, for example, 60 parts by mass or less, preferably 48 parts by mass or less, based on 100 parts by mass of the total of polystyrene and cross-linked polystyrene. The content of cross-linked polystyrene is, for example, 40 parts by mass or more, preferably 52 parts by mass or more, and, for example, 70 parts by mass or less, preferably 60 parts by mass or less, based on 100 parts by mass of the total of polystyrene and cross-linked polystyrene.

[0056] Alternatively, the low shrinkage agent can be dissolved in the polymerizable monomer to prepare a polymerizable monomer solution of the low shrinkage agent.

[0057] In the polymerizable monomer solution of the low shrinkage agent, the solids concentration of the low shrinkage agent is, for example, 20 mass % or more, and for example, 70 mass % or less, preferably 40 mass % or less.

[0058] The low profile agents can be used alone or in combination of two or more.

[0059] The content of the low shrinkage agent, relative to 100 parts by mass of the total amount of the unsaturated polyester, polymerizable monomer, and low shrinkage agent, is, for example, 0.1 parts by mass or more, preferably 0.5 parts by mass or more, more preferably 1 part by mass or more, even more preferably 3 parts by mass or more, particularly preferably 5 parts by mass or more, and for example, 25 parts by mass or less, preferably 20 parts by mass or less, more preferably 15 parts by mass or less, even more preferably 10 parts by mass or less.

[0060] The content of the low shrinkage agent is, relative to 100 parts by mass of the unsaturated polyester, 1.2 parts by mass or more, preferably 2.0 parts by mass or more, more preferably 5.0 parts by mass or more, even more preferably 10.0 parts by mass or more, particularly preferably 13.0 parts by mass or more, and is 50.0 parts by mass or less, preferably 45.0 parts by mass or less, more preferably 35.0 parts by mass or less, even more preferably 25.0 parts by mass or less, particularly preferably 20.0 parts by mass or less, and most preferably 15.0 parts by mass or less.

[0061] When the content ratio of the shrinkage reducing agent relative to 100 parts by mass of the unsaturated polyester is equal to or higher than the lower limit, the appearance (specifically, gloss) can be improved. In addition, as described in detail below, it has been found that the surface irregularities of the molded article can be reduced, which allows the antiviral properties to be expressed according to the content ratio of the silver-containing antiviral agent, thereby improving the antiviral properties.

[0062] On the other hand, if the content ratio of the shrinkage reducing agent to 100 parts by mass of the unsaturated polyester is less than the lower limit, the appearance (specifically, gloss) is deteriorated. In addition, as will be described in detail later, the surface unevenness of the molded product cannot be reduced. Therefore, it was found that the antiviral property corresponding to the content ratio of the silver-containing antiviral agent cannot be expressed, and the antiviral property is deteriorated.

[0063] Furthermore, when the content of the shrinkage reducing agent relative to 100 parts by mass of the unsaturated polyester is equal to or less than the above upper limit, the appearance (specifically, suppression of scumming) can be improved.

[0064] On the other hand, if the content ratio of the shrinkage reducing agent relative to 100 parts by mass of the unsaturated polyester exceeds the above upper limit, the appearance (specifically, suppression of scumming) deteriorates.

[0065] <Silver-containing antiviral agent> The silver-containing antiviral agent has the ability to inactivate viruses. The silver-containing antiviral agent can also have the ability to inhibit the proliferation of bacteria. In other words, the silver-containing antiviral agent may function as an antibacterial agent, and is not intended to limit the contents of the present application.

[0066] Silver-containing antiviral agents include, for example, silver-bearing materials.

[0067] The silver-loaded material is a material in which silver (eg, silver ions) is loaded on a carrier, and examples thereof include silver-loaded phosphate, silver-loaded silicate glass, and silver-zinc-loaded zeolite.

[0068] In the silver-loaded phosphate, silver (eg, silver ions) is loaded onto a phosphate, and examples thereof include silver-loaded zirconium phosphate and silver-loaded calcium phosphate.

[0069] Silver-loaded silicate glass is a glass in which silver (eg, silver ions) is loaded onto the silicate glass, and examples thereof include silver-loaded glass, silver-loaded sodium silicate, silver-loaded calcium silicate, and silver-zinc-loaded calcium silicate.

[0070] As the silver-containing antiviral agent, from the viewpoint of improving resistance to warm water and suppressing yellowing, preferably, silver-supported phosphate and silver-supported silicate glass are used. As the silver-containing antiviral agent, more preferably, silver-supported zirconium phosphate, silver-supported glass, and silver-zinc-supported calcium silicate are used. As the silver-containing antiviral agent, further preferably, silver-supported zirconium phosphate and silver-supported glass are used. As the silver-containing antiviral agent, particularly preferably, silver-supported zirconium phosphate is used.

[0071] The silver-containing antiviral agent is prepared, for example, by preparing a support, and then reacting a silver compound (e.g., silver nitrate) and, if necessary, a zinc compound (e.g., zinc nitrate), followed by drying and calcination. The silver-containing antiviral agent is also prepared, for example, by simultaneously melting and pulverizing the support component, the silver compound, and, if necessary, the zinc compound. The silver-containing antiviral agent is prepared by various known methods, and the preparation method is not limited to the above preparation method.

[0072] In the silver-containing antiviral agent, the silver carrier may be, for example, zirconium phosphate, calcium phosphate, silicate glass, sodium silicate, calcium silicate, or zeolite.Preferably, the carrier may be zirconium phosphate, silicate glass, or calcium silicate.More preferably, the carrier may be zirconium phosphate or silicate glass.More preferably, the carrier may be zirconium phosphate.

[0073] The above supports can be used alone or in combination of two or more kinds.

[0074] In the silver-containing antiviral agent, the silver content is, for example, 0.5% by mass or more, and from the viewpoint of improving antiviral properties, preferably, 1% by mass or more, more preferably, 2% by mass or more, even more preferably, 3% by mass or more, particularly preferably, 5% by mass or more, and most preferably, 10% by mass or more, and for example, 30% by mass or less.

[0075] The silver content can be measured, for example, by fluorescent X-ray analysis.

[0076] In some cases, the silver-containing antiviral agents are also available commercially as antibacterial agents.

[0077] Silver-containing antiviral agents can be used alone or in combination of two or more types.

[0078] The content of the silver-containing antiviral agent, relative to 100 parts by mass of the total amount of the unsaturated polyester, polymerizable monomer, and low shrinkage agent, is, for example, more than 2.0 parts by mass, preferably 3.0 parts by mass or more, more preferably 4.5 parts by mass or more, even more preferably 8.0 parts by mass or more, and for example, 28.0 parts by mass or less, preferably 23.0 parts by mass or less, more preferably 20.0 parts by mass or less, even more preferably 15.0 parts by mass or less, and particularly preferably 12.0 parts by mass or less.

[0079] The content of the silver-containing antiviral agent is, relative to 100 parts by mass of the unsaturated polyester, 7.0 parts by mass or more, preferably 9.0 parts by mass or more, more preferably 12.0 parts by mass or more, even more preferably 20.0 parts by mass or more, and is 60.0 parts by mass or less, preferably 48.0 parts by mass or less, more preferably 45.0 parts by mass or less, even more preferably 30.0 parts by mass or less, and particularly preferably 22.0 parts by mass or less.

[0080] When the content ratio of the silver-containing antiviral agent relative to 100 parts by mass of the unsaturated polyester is equal to or more than the above lower limit, the antiviral property is improved.

[0081] On the other hand, if the content ratio of the silver-containing antiviral agent relative to 100 parts by mass of the unsaturated polyester is less than the above lower limit, the antiviral property decreases.

[0082] Furthermore, when the content ratio of the silver-containing antiviral agent relative to 100 parts by mass of the unsaturated polyester is equal to or less than the above upper limit, the appearance (specifically, gloss) can be improved.

[0083] On the other hand, if the content ratio of the silver-containing antiviral agent relative to 100 parts by mass of the unsaturated polyester exceeds the upper limit, the appearance (specifically, gloss) is deteriorated, and smoothness is reduced due to particles of the silver-containing antiviral agent.

[0084] <Additives> If necessary, additives may be blended into the unsaturated polyester resin composition within the range that does not impair the effects of the present invention.

[0085] Examples of additives include curing agents, polymerization inhibitors, release agents, colorants, thickeners, flame retardants, wetting and dispersing agents, pattern materials, antibacterial agents, hydrophilic agents, photocatalysts, UV absorbers, UV stabilizers, separation inhibitors, silane coupling agents, antistatic agents, thixotropic agents, thixotropic stabilizers, and polymerization accelerators. The additives can be used alone or in combination of two or more.

[0086] [Hardening agent] Examples of the curing agent include peroxides. Examples of the peroxides include benzoyl peroxide, t-butylperoxyisopropyl carbonate (10-hour half-life temperature: 99°C), t-amylperoxyisopropyl carbonate (10-hour half-life temperature: 96°C), t-hexylperoxyisopropyl monocarbonate, 1,1-bis(t-butylperoxy)cyclohexane, t-butylperoxy-2-ethylhexanoate, amylperoxy-2-ethylhexanoate, 2-ethylhexylperoxy-2-ethylhexanoate, t-butylperoxybenzoate (10-hour half-life temperature: 104°C), t-hexylperoxybenzoate, and t-hexylperoxyacetate. As the curing agent, preferably, t-butyl peroxy isopropyl carbonate, t-amyl peroxy isopropyl carbonate, t-butyl peroxy benzoate, t-butyl-2-ethylhexanoate, t-hexyl peroxy acetate are listed. As the curing agent, more preferably, t-butyl peroxy isopropyl carbonate, t-amyl peroxy isopropyl carbonate, t-hexyl peroxy acetate are listed. As the curing agent, more preferably, t-amyl peroxy isopropyl carbonate, t-hexyl peroxy acetate are listed.

[0087] The 10-hour half-life temperature of the curing agent is, for example, 110°C or less, and preferably, from the viewpoint of improving the appearance (specifically, gloss), 103°C or less, more preferably 100°C or less, and even more preferably 97°C or less, and for example, 80°C or more.

[0088] The 10-hour half-life temperature can be determined by measuring the temperature at which the curing agent reaches its 10-hour half-life when a solution in which the peroxide bond concentration contained in the curing agent is dissolved in benzene to be 0.1 mol / L is thermally decomposed.

[0089] The curing agents can be used alone or in combination of two or more kinds.

[0090] The content of the curing agent is, for example, 0.1 parts by mass or more, preferably 0.5 parts by mass or more, and for example, 5 parts by mass or less, preferably 2 parts by mass or less, relative to 100 parts by mass of the total amount of the unsaturated polyester, the polymerizable monomer, and the low shrinkage agent.

[0091] [Polymerization inhibitor] The polymerization inhibitor is a component that is added to adjust the pot life and the curing reaction.

[0092] Examples of the polymerization inhibitor include hydroquinone compounds, benzoquinone compounds, catechol compounds, phenol compounds, and N-oxyl compounds.

[0093] As the polymerization inhibitor, preferably, a benzoquinone compound, a hydroquinone compound, and an N-oxyl compound are mentioned.

[0094] An example of the benzoquinone compound is parabenzoquinone.

[0095] Examples of the hydroquinone compound include hydroquinone, methylhydroquinone, and t-butylhydroquinone. A preferred example of the hydroquinone compound is t-butylhydroquinone.

[0096] More preferred examples of the polymerization inhibitor include benzoquinone compounds and N-oxyl compounds.

[0097] The content of the polymerization inhibitor is, relative to 100 parts by mass of the total amount of the unsaturated polyester, the polymerizable monomer, and the low shrinkage agent, for example, 0.01 parts by mass or more, preferably 0.05 parts by mass or more, and for example, 0.5 parts by mass or less, preferably 0.2 parts by mass or less, and more preferably 0.1 parts by mass or less.

[0098] [Release agent] Examples of the release agent include fatty acids, fatty acid metal salts, liquid waxes, fluoropolymers, and silicon-based polymers. Examples of the fatty acids include stearic acid and lauric acid. Examples of the fatty acid metal salts include zinc stearate and calcium stearate.

[0099] The release agent is preferably a fatty acid metal salt, more preferably zinc stearate.

[0100] The release agents can be used alone or in combination of two or more kinds.

[0101] The content of the release agent is, for example, 1 part by mass or more, preferably 3 parts by mass or more, and for example, 10 parts by mass or less, relative to 100 parts by mass of the total amount of the unsaturated polyester, the polymerizable monomer, and the low shrinkage agent.

[0102] [Filling material] Examples of the filler include inorganic fillers. Examples of the inorganic filler include oxides (e.g., alumina, titanium oxide), hydroxides (e.g., magnesium hydroxide, aluminum hydroxide), carbonates (e.g., calcium carbonate), sulfates (e.g., barium sulfate), silicas (e.g., crystalline silica, fused silica, fumed silica, dry silica (aerosil)), hollow fillers, silicates (e.g., silica sand, diatomaceous earth, glass powder, glass balloons, mica, clay, kaolin, talc), fluorides (e.g., fluorite), phosphates (e.g., calcium phosphate), metal powders, ceramics, milled fibers, and clay minerals (e.g., smectite).

[0103] The fillers preferably include hydroxides and carbonates, and more preferably include aluminum hydroxide and calcium carbonate.

[0104] The fillers can be used alone or in combination of two or more.

[0105] The content of the filler is, relative to 100 parts by mass of the total amount of the unsaturated polyester, the polymerizable monomer, and the low shrinkage agent, for example, 50 parts by mass or more, preferably 100 parts by mass or more, more preferably 150 parts by mass or more, and for example, 300 parts by mass or less, preferably 200 parts by mass or less.

[0106] [Coloring agent] The colorant is not particularly limited, and examples of the colorant include polyester toners mixed with known pigments such as titanium oxide, carbon black, red iron oxide, and phthalocyanine blue.

[0107] As the colorant, preferably, a polyester toner is used.

[0108] The colorants can be used alone or in combination of two or more kinds.

[0109] The content of the colorant is, for example, 1 part by mass or more, preferably 5 parts by mass or more, and for example, 20 parts by mass or less, relative to 100 parts by mass of the total amount of the unsaturated polyester, the polymerizable monomer, and the low shrinkage agent.

[0110] [Thickener] The thickener is blended to thicken the unsaturated polyester resin composition to a viscosity suitable for heat compression molding. The thickener is preferably blended before (preferably immediately before) impregnating the unsaturated polyester resin composition into reinforcing fibers (described later).

[0111] Examples of the thickener include alkaline earth metal oxides and alkaline earth metal hydroxides. Examples of the alkaline earth metal oxides include magnesium oxide. Examples of the alkaline earth metal hydroxides include magnesium hydroxide and calcium hydroxide.

[0112] As the thickener, preferably, an alkaline earth metal oxide is used, and more preferably, magnesium oxide is used.

[0113] The thickeners can be used alone or in combination of two or more kinds.

[0114] The content ratio of the thickener is, for example, 0.5 parts by mass or more and, for example, 10 parts by mass or less, preferably 3 parts by mass or less, relative to 100 parts by mass of the total amount of the unsaturated polyester, the polymerizable monomer, and the low shrinkage agent.

[0115] <Preparation of Unsaturated Polyester Resin Composition> The unsaturated polyester resin composition is prepared by mixing an unsaturated polyester, a polymerizable monomer, a shrinkage reducing agent, a silver-containing antiviral agent, and additives that are blended as necessary.

[0116] In the above preparation, the unsaturated polyester resin can also be prepared by dissolving the unsaturated polyester in a polymerizable monomer (preferably styrene) in advance and, if necessary, adding the above additives.

[0117] In preparing the unsaturated polyester resin, the content ratio of the polymerizable monomer is, for example, 50 parts by mass or more, preferably 60 parts by mass or more, and for example, 80 parts by mass or less, preferably 70 parts by mass or less, relative to 100 parts by mass of the unsaturated polyester.

[0118] In addition, after preparing the unsaturated polyester resin, when this unsaturated polyester resin is mixed with other components (the shrinkage reducing agent, the silver-containing antiviral agent, and the additives), a polymerizable monomer can also be further blended.

[0119] In the unsaturated polyester resin composition, the content of the shrinkage reducing agent and the content of the silver-containing antiviral agent are each within a predetermined range. Therefore, a molded article obtained by using this unsaturated polyester resin composition can reduce surface irregularities and exhibit excellent virus resistance, and can also improve appearance (gloss and suppression of scumming).

[0120] A molding material can be prepared by blending reinforcing fibers with such an unsaturated polyester resin composition. A molded article can be obtained from such a molding material by a known method.

[0121] 2.Molding material The molding material includes an unsaturated polyester resin composition and reinforcing fibers.

[0122] <Reinforced fiber> Examples of reinforcing fibers include inorganic fibers, organic fibers, and natural fibers. Examples of inorganic fibers include glass fibers, carbon fibers, metal fibers, and ceramic fibers. Examples of organic fibers include polyvinyl alcohol-based fibers, polyester-based fibers, polyamide-based fibers, fluororesin-based fibers, and phenol-based fibers. Examples of natural fibers include hemp and kenaf.

[0123] As the reinforcing fiber, preferably, inorganic fiber is used, and more preferably, glass fiber is used.

[0124] Examples of the shape of the reinforcing fibers include cloth (e.g., roving cloth), mat (e.g., chopped strand mat, preformable mat, continuous strand mat, and surfacing mat), strand, roving, nonwoven fabric, and paper.

[0125] The length of the reinforcing fibers is not particularly limited and is, for example, 1.5 mm or more, and from the viewpoint of improving strength, preferably 5 mm or more, more preferably 20 mm or more, and for example, 80 mm or less, preferably 40 mm or less.

[0126] <Preparation of molding material> To prepare the molding material, the unsaturated polyester resin composition is mixed with the reinforcing fibers, specifically, the reinforcing fibers are impregnated with the unsaturated polyester resin composition.

[0127] The method for preparing the unsaturated polyester resin composition may be a known method.Specifically, SMC (sheet molding compound), TMC (thick molding compound), and BMC (bulk molding compound) may be used.Preferably, SMC and TMC may be used, and more preferably, SMC may be used.

[0128] The content ratio of the reinforcing fibers relative to the molding material is, for example, 15 mass % or more and, for example, 60 mass % or less, preferably 30 mass % or less.

[0129] This gives a molding material (preferably a sheet-like molding material) containing the unsaturated polyester resin composition and the reinforcing fibers.

[0130] This molding material contains the unsaturated polyester resin composition, and therefore, a molded article obtained by using this molding material can exhibit excellent virus resistance by reducing surface irregularities, and can also improve appearance (gloss and suppression of scumming).

[0131] 3. Molded products The molded article includes a cured product of the molding material.

[0132] To harden the molding material, the molding material is first aged to thicken it so that it can be subjected to heat compression molding (described later).

[0133] In the aging, the aging temperature is, for example, 20° C. or more and, for example, 50° C. or less. The aging time is, for example, 8 hours or more and, for example, 120 hours or less.

[0134] This allows the molding material to retain its shape.

[0135] The molding material is then heated and compression molded by a known method.

[0136] The conditions of the heat compression molding are appropriately set according to the purpose and use. In the heat compression molding, the molding temperature is, for example, 100° C. or more, and, for example, 200° C. or less. The molding pressure is, for example, 0.1 MPa or more, preferably 1 MPa or more, more preferably 5 MPa or more, and, for example, 20 MPa or less, preferably 15 MPa or less.

[0137] This causes the molding material to be shaped and hardened, resulting in a molded product.

[0138] The molded article contains a cured product of the molding material, and therefore can exhibit excellent virus resistance by reducing surface irregularities, and can also improve appearance (gloss and suppression of scumming).

[0139] The above-mentioned molding material may be subjected to a single press process as it is for shaping, but it may also be laminated on the back side with a molding material that does not contain a silver-containing antiviral agent to form a two-layer structure and then subjected to integral press molding (two-layer molding). In such a case, the molded product has, in order, a first layer molded from a molding material that contains a silver-containing antiviral agent and a second layer molded from a molding material that does not contain a silver-containing antiviral agent. If an expensive silver-containing antiviral agent is used, the cost of raw materials increases, but the increase in raw material costs can be suppressed by implementing two-layer molding.

[0140] The molding material used on the back side of the two-layer molding (molding material that does not contain a silver-containing antiviral agent) is not particularly limited. This allows the molding material obtained by two-layer molding to obtain a molded product with reduced raw material costs compared to a single material without compromising the antiviral performance of the surface.

[0141] The weight ratio of the molding material containing the silver-containing antiviral agent (the material of the first layer) to the molding material not containing the silver-containing antiviral agent (the material of the second layer) is, for example, 0.6 or more, preferably 0.9 or more, and for example, 1.4 or less, preferably 1.1 or less.

[0142] 4. Effects In molded products made from molding materials using unsaturated polyester, a defective appearance accompanied by a partial loss of gloss on the surface of the molded product can occur, a phenomenon known as scumming. The cause of scumming is a combination of factors, including low-shrinkage agent components that are poorly compatible with unsaturated polyesters separating and depositing during molding, contaminating the surface, and polymerizable monomers vaporizing during heat compression molding, gelling and causing roughness on the surface of the molded product.

[0143] There has been no previous knowledge that there is a correlation between the manifestation of antiviral properties and the unevenness of the surface of a molded article. However, through intensive research, it has been found that by setting the content ratio of the shrinkage reducing agent and the content ratio of the silver-containing antiviral agent in an unsaturated polyester resin composition within a predetermined range, a molded article obtained using this unsaturated polyester resin composition has excellent antiviral properties and appearance (gloss and suppression of the occurrence of scumming).

[0144] Specifically, in a molded article obtained using the unsaturated polyester resin composition, increasing the amount of a silver-containing antiviral agent has been considered from the viewpoint of improving the antiviral properties. However, it has been found that when the molded article has unevenness, there is a problem in that the expected antiviral properties corresponding to the blended amount of the silver-containing antiviral agent are not exhibited.

[0145] On the other hand, in this unsaturated polyester resin composition, since the content ratio of the shrinkage reducing agent is within a predetermined range, the surface unevenness can be reduced. Therefore, the antiviral property according to the content ratio of the silver-containing antiviral agent can be expressed, and the antiviral property can be improved. Furthermore, since the content ratio of the shrinkage reducing agent is within a predetermined range, the appearance (gloss and suppression of the occurrence of scumming) can be improved.

[0146] The molding material contains the unsaturated polyester resin composition, and therefore, a molded article obtained by using this molding material can exhibit excellent virus resistance by reducing surface irregularities, and can also improve appearance (gloss and suppression of scumming).

[0147] The molded article contains a cured product of the molding material, and therefore can exhibit excellent virus resistance by reducing surface irregularities, and can also improve appearance (gloss and suppression of scumming). EXAMPLES

[0148] The present invention will be described in more detail below with reference to examples. However, the following description is an embodiment of the present invention, and the present invention is not limited to these descriptions.

[0149] Specific numerical values ​​of the blending ratio (content ratio), physical property values, parameters, etc. used in the following description can be replaced with the upper limit values ​​(numerical values ​​defined as "not more than" or "less than") or lower limit values ​​(numerical values ​​defined as "not less than" or "exceeding") of the corresponding blending ratio (content ratio), physical property values, parameters, etc. described in the above "Form for carrying out the invention." In addition, unless otherwise specified in the following description, "parts" and "%" are based on mass.

[0150] <Preparation of Unsaturated Polyester Resin> Manufacturing Example 1 A flask equipped with a thermometer, a nitrogen gas inlet tube, a reflux condenser and a stirrer was used as a reactor. 2.0 mol of isophthalic acid, 5.5 mol of propylene glycol and 5.0 mol of neopentyl glycol were charged into this reactor, and polycondensation reaction was carried out at a temperature of 200 to 210°C while stirring under a nitrogen gas atmosphere. When the acid value reached 10 mgKOH / g, the mixture was cooled to 150°C, 8.0 mol of maleic anhydride was charged, and the reaction was carried out again at 210 to 220°C for 8 hours to obtain an unsaturated polyester with an acid value of 29.0 mgKOH / g.

[0151] Next, 60 parts by mass of the obtained unsaturated polyester was mixed with 40 parts by mass of styrene, thereby obtaining an unsaturated polyester resin (solid content concentration: 60% by mass).

[0152] <Preparation of silver-containing antiviral agent> Preparation Example 1 (Preparation of Silver-Supported Zirconium Phosphate) While stirring an aqueous solution of zirconium oxynitrate, phosphoric acid was added to the solution so that the ratio of zirconium to phosphorus was 2:3. The pH of the reaction solution was adjusted to 3 with an aqueous sodium hydroxide solution, and after heating and refluxing for 80 hours, the precipitate was filtered, washed with water, and dried to obtain crystalline zirconium phosphate. Next, 100 g of the obtained zirconium phosphate was added to 1 L of a 0.5 wt% aqueous silver nitrate solution and stirred at 60°C for 3 hours, after which the obtained slurry was filtered, washed with water, dried, and calcined at 900°C for 4 hours to obtain silver-supported zirconium phosphate (average particle size 1 μm).

[0153] Preparation Example 2 (Preparation of silver-loaded glass) As a glass raw material, P 2 O 5 60% by weight, CaO 30% by weight, B 2 O 3 7% by weight, Ag 2After uniformly mixing O at a ratio of 3% by weight in a universal mixer, the mixture was heated in a melting furnace at 1300°C for 3 hours to obtain a molten glass. The molten glass obtained was then poured into running water at 30°C to form a glass body, which was then simultaneously crushed in water to obtain coarsely pulverized glass with a volume average particle size of about 10 mm. The glass was then subjected to primary intermediate pulverization in a ball mill and secondary intermediate pulverization in a rotating roll. Next, 7 parts by mass of aggregated silica particles were added to 100 parts by mass of the coarsely pulverized glass, and fine pulverization was carried out in a vertical mill to obtain a glass with a volume average primary particle size (D50) of 1 μm and a specific surface area of ​​88,000 cm. 2 / cm 3 Thus, a silver-loaded glass having the formula:

[0154] Preparation Example 3 (Preparation of silver-zinc supported calcium silicate) 44 parts by weight of quicklime and SiO 2 A mixture of 52 parts by weight of silica with a content of 99% or more and an average particle size of 12 microns, 4 parts by weight of aluminum hydroxide, 2 parts by weight of potassium hydroxide, and 150 parts by weight of water was heated under high temperature and pressure (180°C, 10 kg / cm 2 ) and reacted in an autoclave for 3 hours. The slurry after the reaction was washed with distilled water, and when the supernatant liquid became pH 8 or less, the solid was taken out and dried at 110°C, and then crushed to 200-400 mesh to obtain tobermorite (calcium silicate). Next, 3 g of the obtained calcium silicate powder was mixed with 500 ml of silver nitrate aqueous solution (20.0 mM) and 500 ml of zinc nitrate aqueous solution (100 mM) and reacted at 25°C for 24 hours, after which the solid was separated, washed with distilled water, and dried in vacuum to obtain silver-zinc supported calcium sodium silicate.

[0155] Preparation Example 4 (Preparation of Silver-Zinc Supported Zeolite) 0.5 kg of commercially available A-type zeolite powder was mixed with water, stirred, and degassed, and then an appropriate amount of 0.5N nitric acid solution was added to adjust the pH to 5-7 to obtain 1.0 kg of slurry. Furthermore, a mixed aqueous solution of silver nitrate (0.09 M / L) and zinc nitrate (0.40 M / L) was added to make the total volume 3 kg, and the mixture was stirred at 60°C for 24 hours. The zeolite powder was then filtered, washed with water, and dried by heating to obtain silver-zinc supported zeolite.

[0156] Preparation Example 5 (Preparation of acrylic acid-based polymer antiviral agent) 300 parts of a water-soluble polymer of methacrylic acid / sodium p-styrenesulfonate=70 / 30 and 30 parts of sodium sulfate were dissolved in 6595 parts of water and charged into a polymerization tank equipped with a stirrer. Next, 15 parts of 2,2'azobis-(2,4-dimethylvaleronitrile) were dissolved in 2700 parts of acrylonitrile and 300 parts of methyl acrylate, and charged into a polymerization tank to polymerize at 60°C for 3 hours, thereby obtaining polymer particles A containing nitrile groups with an average particle diameter of 78 μm. Next, 10 parts of the polymer particles A were immersed in 200 parts of an aqueous solution containing N-methyl-3,3'-iminobis(propylamine) in an amount 30 times that of the particles, treated at a treatment temperature of 85°C for 3 hours, washed with water, and dried to obtain an acrylic acid-based polymer antiviral agent.

[0157] <Preparation of Unsaturated Polyester Resin Composition and Molding Material> Example 1 The following components were added in order and mixed to prepare an unsaturated polyester resin composition. Unsaturated polyester resin: 78 parts by mass of the unsaturated polyester resin of Production Example 1 (solid content concentration 60% by mass, 46.8 parts by mass of unsaturated polyester, 31.2 parts by mass of styrene) Polymerizable monomer: 10 parts by mass of styrene Shrinkage reducing agent: 8 parts by weight of polystyrene solution (solid content concentration 36% by weight, polystyrene 2.8 parts by weight, styrene 5.2 parts by weight), cross-linked polystyrene 4 parts by weight (solid content concentration 100% by weight) Silver-containing antiviral agent: 10 parts by mass of silver-loaded zirconium phosphate of Preparation Example 1 Filler: 80 parts by weight of aluminum hydroxide, 80 parts by weight of calcium carbonate Polymerization inhibitor: parabenzoquinone 0.07 parts by mass Hardener: 1 part by mass of t-amylperoxyisopropyl carbonate Release agent: zinc stearate 5 parts by weight Colorant: Polyester toner 10 parts by weight

[0158] Next, 1.0 part of magnesium oxide was added as a thickener to the unsaturated polyester resin composition, and then reinforcing fiber rovings cut into continuous 1-inch pieces were added in such a proportion that the reinforcing fiber content was 25 mass %, and a press molding material (SMC) with a thickness of 2 mm was prepared using a known SMC impregnation machine.

[0159] Examples 2 to 5, Examples 7 to 11, and Comparative Examples 1 to 6 An unsaturated polyester resin composition and a molding material were prepared in the same manner as in Example 1. However, the formulation of each component was changed based on the descriptions in Tables 1 and 2.

[0160] Example 6 An unsaturated polyester resin composition and a molding material were prepared according to the formulation of the components shown in Table 1 in the same manner as in Example 1, and used as a surface layer molding material (molding material containing a silver-containing antiviral agent).

[0161] Similarly, the following components were added in order while being mixed. In this way, an unsaturated polyester resin composition and a molding material were prepared, which was used as a back surface layer molding material (molding material not containing a silver-containing antiviral agent). Unsaturated polyester resin: 78 parts by mass of the unsaturated polyester resin of Production Example 1 (solid content concentration 60% by mass, 46.8 parts by mass of unsaturated polyester, 31.2 parts by mass of styrene) Polymerizable monomer: 3 parts by mass of styrene Shrinkage reducing agent: 19 parts by weight of polystyrene solution (solid content 36% by weight, polystyrene 6.8 parts by weight, styrene 12.2 parts by weight) Filler: 160 parts by weight of calcium carbonate Polymerization inhibitor: parabenzoquinone 0.04 parts by mass Hardener: 1 part by weight of t-butyl peroxybenzoate Release agent: zinc stearate 5 parts by weight Colorant: Polyester toner 10 parts by weight

[0162] <Evaluation> [Silver content of silver-containing antiviral agents] The silver content of each silver-containing antiviral agent was measured using an X-ray fluorescence analyzer (manufactured by Rigaku Corporation, product name ZSX Primus2, rhodium tube, vacuum atmosphere conditions).

[0163] For each silver-containing antiviral agent, the silver content was as follows: Silver-loaded zirconium phosphate of Preparation Example 1: Silver content 17% by mass Silver-loaded glass of Preparation Example 2: Silver content 3.69% by mass Silver-zinc-supported calcium silicate of Preparation Example 3: Silver content: 1.65% by mass Silver-zinc-supported zeolite of Preparation Example 4: Silver content: 3.45% by mass

[0164] [Production of test specimens] The molding materials of Examples 1 to 5, Examples 7 to 11, and Comparative Examples 1 to 6 were subjected to hot compression molding (molding pressure: 10 MPa, molding temperature: 145°C / 130°C, pressure holding time: 5 minutes) using a flat metal plate to obtain flat test pieces of 300 mm x 300 mm x 4 mm. The surface on the molding temperature side of 145°C was designated as the front side, and performance evaluation was carried out on the front side.

[0165] Example 6 (Implementation of two-layer molding) The surface layer molding material and the back layer molding material were laminated in a weight ratio of 50:50, charged into a flat plate mold, and subjected to heat compression molding (molding pressure: 10 MPa, molding temperature: 145°C / 130°C, pressure holding time: 5 minutes) to obtain a flat plate-shaped test piece of 300 mm x 300 mm x 4 mm. The surface on the molding temperature side of 145°C was regarded as the front side, and performance evaluation was carried out on the front side.

[0166] [Color tone] The appearance of the test pieces of each Example and Comparative Example was visually observed. The color tone was evaluated based on the following criteria. The results are shown in Tables 1 and 2. {standard} Good: The color tone was the same as that of polyester toner (white). Yellowing: The entire test piece or a part of it was yellowed.

[0167] [exterior] (smoothness) The smoothness of the test pieces of each Example and Comparative Example was evaluated. Specifically, the smoothness was evaluated visually based on the clarity of the images of window frames, fluorescent lights, etc. reflected on the surface of the test piece. The smoothness was evaluated based on the following criteria. The results are shown in Tables 1 and 2. {standard} ◯: The image was free of waviness and had good gloss. Δ: Wavyness was observed in part of the image, and the gloss was slightly poor. ×: Waviness was observed over the entire image, and the gloss was poor.

[0168] (Glossy) The gloss of the test pieces (145°C molded surface) of each Example and Comparative Example was measured in accordance with JIS Z8741 (1997) under the conditions of an incident angle of 60° and a receiving angle of 60°. The measurement positions were each of the four corners and the center of the test piece, and the average of five measured values ​​was calculated. The results are shown in Tables 1 and 2.

[0169] (Scumming) The surface of the test piece of each Example and Comparative Example was visually inspected for the presence or absence of scumming. Scumming was evaluated based on the following criteria. The results are shown in Tables 1 and 2. {standard} ○: No scumming was observed by visual inspection. △: Slight scumming was observed visually. ×: A large amount of scumming was observed by visual inspection.

[0170] [Hot water resistance] The test pieces of each Example and Comparative Example were subjected to a one-sided boiling test on the molded surface at 145°C under the condition of 500 hours in hot water at 93°C. The ΔE between the test pieces before and after the boiling test was measured using a color difference meter. The results are shown in Tables 1 and 2.

[0171] [Antiviral properties (antiviral test activity value)] Durability tests were conducted on the test pieces of each Example and Comparative Example to evaluate their antiviral properties. Specifically, antiviral performance tests were conducted on the following test pieces in accordance with the antiviral test method (ISO21702) to evaluate their antiviral activity against influenza viruses. The results are shown in Tables 1 and 2.

[0172] (Test piece before durability test) The pristine specimens were evaluated.

[0173] (Test piece after water resistance test) The test conforms to the water resistance category 2 of the durability test category determined by SIAA (Society of International Antibacterial Products). The test specimen was immersed in 50°C water for 16 hours and then evaluated.

[0174] (Test piece after light resistance test) The test conforms to light resistance category 1 of the durability test categories set by the SIAA (Society of International Association of Antibacterial Products). The test pieces were evaluated after 8 hours of exposure (18 minutes of water spraying out of a 120 minute cycle) using a sunshine weatherometer.

[0175] [Table 1]

[0176] [Table 2]

Claims

1. An unsaturated polyester, A polymerizable monomer, A shrinkage reducing agent; and a silver-containing antiviral agent, the content of the shrinkage reducing agent is 1.2 parts by mass or more and 50.0 parts by mass or less based on 100 parts by mass of the unsaturated polyester, An unsaturated polyester resin composition, wherein a content ratio of the silver-containing antiviral agent is 7.0 parts by mass or more and 60.0 parts by mass or less relative to 100 parts by mass of the unsaturated polyester.

2. 2. The unsaturated polyester resin composition of claim 1, wherein the silver-containing antiviral agent comprises a silver-loaded phosphate or a silver-loaded silicate glass.

3. 2. The unsaturated polyester resin composition according to claim 1, wherein the silver-containing antiviral agent has a silver content of 1 mass% or more.

4. Further, it contains a hardener, 2. The unsaturated polyester resin composition according to claim 1, wherein the curing agent has a 10-hour half-life temperature of 103° C. or lower.

5. A molding material comprising the unsaturated polyester resin composition according to any one of claims 1 to 4 and reinforcing fibers.

6. A molded article comprising a cured product of the molding material according to claim 5.

Citation Information

Patent Citations

  • Unsaturated polyester resin composition

    JP1989306463A

  • Artificial marble-treated article

    JP2005255467A

  • Anti-coronavirus agent

    WO2005037296A1

  • Manufacture of thermosetting resin molded body

    JP2000037742A