Mixture of cyclic acid anhydrides, curable resin composition and cured product thereof
A mixture of cyclic acid anhydrides with controlled peak areas, produced via a Diels-Alder reaction, addresses slow crystallization and stability issues, offering enhanced thermal and dimensional stability for carbon fiber composites.
Patent Information
- Application Number
- JP2023055549
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Filing Date
- 2023-03-30
- Publication Date
- 2024-10-11
AI Technical Summary
Existing cyclic acid anhydrides derived from renewable resources suffer from slow crystallization rates, poor handling properties, and inadequate thermal and dimensional stability, limiting their use in carbon fiber reinforced composite materials.
A mixture of cyclic acid anhydrides with specific peak area ratios, produced through a Diels-Alder reaction of 1,3-p-menthadiene and maleic anhydride, is formulated to achieve high crystallization rates and improved thermal and dimensional stability, allowing for pellet or marble forms that enhance handling and suitability for carbon fiber composites.
The mixture provides excellent heat resistance and dimensional stability, enabling effective use in carbon fiber reinforced materials with improved manufacturing efficiency and performance.
Smart Images

Figure 2024143065000001 
Figure 2024143065000002 
Figure 2024143065000003
Abstract
Description
[Technical field]
[0001] The present invention relates to a mixture of cyclic acid anhydrides, a curable resin composition, and a cured product thereof, which are suitable for use in electrical and electronic components such as semiconductor encapsulants, printed wiring boards, and build-up laminates, lightweight, high-strength materials such as carbon fiber reinforced plastics and glass fiber reinforced plastics, 3D printing applications, and adhesives. [Background technology]
[0002] Epoxy resins are widely used in various fields due to their excellent mechanical strength, heat resistance, adhesiveness, gas barrier properties, etc. It has been well known that acid anhydrides are effective as curing agents for epoxy resins, and acid anhydrides have been used in applications such as small and large casting, impregnation molding, and powder coatings because they are less toxic and odorous than amine curing agents, and they generate less heat and shrink in volume during curing.
[0003] Hardeners such as epoxy resins and acid anhydrides have often been derived from petroleum as raw materials. In recent years, however, concerns have arisen over the depletion of petroleum resources, and methods of recycling many materials using renewable resources such as plants or by decomposing the hardened materials are being investigated. [Prior art documents] [Patent documents]
[0004] [Patent Document 1] Japanese Patent Application Publication No. 55-118920 [Patent Document 2] Japanese Patent Application Publication No. 01-167326 [Patent Document 3] Japanese Patent Application Publication No. 07-018059 [Patent Document 4] JP 2014-025036 A Summary of the Invention [Problem to be solved by the invention]
[0005] Patent documents 1 to 4 describe 1-isopropyl-4-methyl-bicyclo[2.2.2]oct-5-ene-2,3-dicarboxylic anhydride synthesized by addition reaction of 1,3-p-menthadiene and maleic anhydride as renewable resources such as plants. The applicant of the present application produced 1-isopropyl-4-methyl-bicyclo[2.2.2]oct-5-ene-2,3-dicarboxylic anhydride by the method described in these documents, and confirmed that the crystallization rate was slow.
[0006] When the crystallization rate is slow, the liquid is generally placed in a drum or other container and allowed to crystallize over time, after which it is crushed with a hammer from outside the drum or other container, or heated and melted in an oven before use. This makes handling very difficult.
[0007] On the other hand, if the crystallization rate is fast, it becomes possible to process the material into pellets, granules, or marbles, and the handling properties are greatly improved. Also, if the crystallization rate is fast, it becomes possible to process the material into granules or marbles by dropping the liquid droplets onto a conveyor and cooling the material during transport on the conveyor.
[0008] In addition, it was revealed that the curable resin composition containing the acid anhydride had a problem that the heat resistance (Tg) of the cured product was low and the linear expansion coefficient was large, so that when the cured product was removed from the mold and cooled to room temperature, thermal shrinkage occurred. Therefore, in order to use the composition in carbon fiber reinforced composite materials, it was necessary to improve the thermal stability and dimensional stability.
[0009] The present invention has been made in consideration of the above-mentioned problems, and aims to provide a cyclic acid anhydride mixture, a curable resin composition, and a method for producing the cyclic acid anhydride mixture, which have excellent heat resistance and dimensional stability. [Means for solving the problem]
[0010] That is, the present invention is as shown in the following [1] to [7]. In the present invention, "(Numerical value 1) to (Numerical value 2)" indicates that the upper and lower limits are included. [1] A mixture of cyclic acid anhydrides including a cyclic acid anhydride represented by the following formula (Aa), a cyclic acid anhydride represented by the following formula (Ab), and a cyclic acid anhydride represented by the following formula (Ac): A mixture of cyclic acid anhydrides, in which, when the sum of the peak areas of the cyclic acid anhydrides represented by the formulas (Aa) to (Ac) is taken as 100% in gas chromatography analysis of the mixture of cyclic acid anhydrides, the peak area of the cyclic acid anhydride represented by the formula (Aa) is 0.1% or more and 1.0% or less, the peak area of the cyclic acid anhydride represented by the formula (Ab) is 98.0% or more and 99.0% or less, and the peak area of the cyclic acid anhydride represented by the formula (Ac) is 0.1% or more and 1.0% or less.
[0011] [ka]
[0012] [2] The mixture of cyclic acid anhydrides according to the above item [1], which is dissolved at 80° C. and then allowed to stand at 10° C. for 0.1 to 1.5 hours until crystallization. [3] The mixture of cyclic acid anhydrides according to the preceding item [1] or [2] is in the form of pellets, granules, or marbles. [4] A curable resin composition comprising the mixture of cyclic acid anhydrides according to any one of the above items [1] to [3], an epoxy resin, and a curing accelerator. [5] A cured product obtained by curing the curable resin composition described in the above item [4]. [6] A carbon fiber reinforced composite material obtained by curing the curable resin composition according to the above item [4]. [7] A method for producing a mixture of cyclic acid anhydrides according to any one of the above items [1] to [3], which is obtained by reacting 1,3-p-menthadiene, maleic anhydride and a solvent at 40 to 80°C, and then concentrating the solvent. Effect of the Invention
[0013] According to the present invention, it is possible to provide a cyclic acid anhydride mixture and a curable resin composition having excellent heat resistance and dimensional stability, and also to provide an inexpensive method for producing the cyclic acid anhydride mixture. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0014] The mixture of cyclic acid anhydrides of the present embodiment is composed of a cyclic acid anhydride represented by the following formula (Aa), a cyclic acid anhydride represented by the following formula (Ab), and a cyclic acid anhydride represented by the following formula (Ac). When the sum of the peak areas of the cyclic acid anhydrides represented by the formulas (Aa) to (Ac) is taken as 100% in gas chromatography analysis, the peak area of the cyclic acid anhydride represented by the formula (Aa) is 0.1% to 1.0%, the peak area of the cyclic acid anhydride represented by the formula (Ab) is 98.0% to 99.0%, and the peak area of the cyclic acid anhydride represented by the formula (Ac) is 0.1% to 1.0%. The mixture of cyclic acid anhydrides has a high crystallization rate and can be provided in the form of pellets, granules, or marbles. It can also be used for carbon fiber reinforced composite materials with high thermal resistance and dimensional stability.
[0015] [ka]
[0016] When the mixture of cyclic acid anhydrides is analyzed by gas chromatography, the peak area of the cyclic acid anhydride represented by formula (Aa) is preferably 0.1% or more and 1.0% or less, more preferably 0.1% or more and 0.8% or less, and particularly preferably 0.1% or more and 0.5% or less, when the sum of the peak areas of the cyclic acid anhydrides represented by formula (Aa) to (Ac) is taken as 100%.
[0017] When the mixture of cyclic acid anhydrides is analyzed by gas chromatography, the peak area of the cyclic acid anhydride represented by formula (Aa) to (Ac) is taken as 100%, and the peak area of the cyclic acid anhydride represented by formula (Ab) is preferably 98.0% or more and 99.0% or less, more preferably 98.5% or more and 99.0% or less, and particularly preferably 98.8% or more and 99.0% or less.
[0018] When the mixture of cyclic acid anhydrides is analyzed by gas chromatography, the peak area of the cyclic acid anhydride represented by formula (Ac) is preferably 0.1% or more and 1.0% or less, more preferably 0.1% or more and 0.8% or less, and particularly preferably 0.1% or more and 0.5% or less, when the sum of the peak areas of the cyclic acid anhydrides represented by formulas (Aa) to (Ac) is taken as 100%.
[0019] The gas chromatography analysis was carried out under the following conditions. Gas chromatography (GC) measurements Equipment: 8890GC System (Agilent Technologies) Column: HP-5MS (Agilent Technologies) Column flow rate: 1.2 ml / min Oven: 100℃ (2min) - 5℃ / min - 300℃ (3min) Injection port: 300℃, injection volume 1.0 μl Detector: FID (300 °C)
[0020] The mixture of cyclic acid anhydrides of this embodiment can be easily obtained by addition reaction of 1,3-p-menthadiene and maleic anhydride. The addition reaction conditions are the same as those of the usual Diels-Alder reaction. In other words, the reaction ratio is preferably about equimolar or slightly excess of maleic anhydride to 1,3-p-menthadiene.
[0021] The reaction may be carried out using a suitable solvent for the reaction system, such as aromatic hydrocarbons and alicyclic hydrocarbons (e.g., n-heptane, benzene, toluene, xylene, cyclohexane, etc.) The reaction temperature is preferably 40 to 80°C, more preferably 40 to 70°C, and particularly preferably 45 to 65°C.
[0022] The cyclic acid anhydride mixture of this embodiment may be in any state, such as a solid, molten, or solution state, but is preferably in a solid state, and is more preferably in the form of pellets, granules, or marbles in view of uniform crystallization and ease of handling.
[0023] The method for forming into pellets, granules, or marbles is not particularly limited, but examples of pellet manufacturing equipment include a belt drum flaker manufactured by Nippon Coke & Engineering Co., Ltd., a steel belt conveyor manufactured by Nippon Steel Conveyor Co., Ltd., and a flaker manufactured by Mitsubishi Materials Techno Corp. The size of the pellets, granules, and marbles is not particularly limited, but taking into consideration handling during the manufacturing process and handling during secondary molding, a size of 0.1 mm to 10 mm is preferable, and 1 mm to 5 mm is more preferable.
[0024] The melting point of the mixture of cyclic acid anhydrides of this embodiment is preferably 60 to 80° C., more preferably 61.5 to 80° C. The crystallization rate measured under the following conditions is preferably 0.1 to 1.5 hours, more preferably 0.5 to 1.5 hours.
[0025] The crystallization acceleration in this embodiment was measured under the following conditions. <Crystallization rate measurement conditions> The mixture of cyclic acid anhydrides was allowed to stand in an oven at 80°C for 1 hour to dissolve, and then 0.02 g of the solution of the mixture of dissolved cyclic acid anhydrides was dropped into a tray maintained at 10°C and allowed to stand, and the time until the transparent liquid crystallized and completely turned cloudy and solidified was measured.
[0026] The curable resin composition of the present embodiment contains the mixture of the cyclic acid anhydride, an epoxy resin, and a curing accelerator. The epoxy resin is not particularly limited and can be appropriately selected from commonly used epoxy resins. Among them, an epoxy resin having two or more epoxy groups in one molecule is preferable. Examples of epoxy resins having two or more epoxy groups in one molecule include various polyfunctional epoxy resins such as naphthalene type, phenol novolac type, cresol novolac type, phenol aralkyl type, biphenyl type, hydroxybenzaldehyde type, dicyclopentadiene type, glycidyl ester type, glycidyl amine type, hydantoin type, and isocyanurate type. These epoxy resins may be used alone or in combination of two or more types.
[0027] The epoxy equivalent of the epoxy resin is not particularly limited, but from the viewpoint of the heat resistance and water absorbency of the cured product, it is preferably 100 to 350 (g / eq), and more preferably 150 to 300 (g / eq).
[0028] From the viewpoints of heat resistance, electrical properties and water absorbency, the epoxy resin is preferably at least one type of multifunctional epoxy resin selected from the group consisting of dicyclopentadiene type, o-cresol novolac type, naphthalene type, biphenyl type, phenol aralkyl type and trisphenolmethane type, and has an epoxy equivalent of 100 to 350 (g / eq), and more preferably at least one type of multifunctional epoxy resin selected from the group consisting of dicyclopentadiene type, o-cresol novolac type, naphthalene type and trisphenolmethane type, and has an epoxy equivalent of 150 to 300 (g / eq).
[0029] The content of the epoxy resin in the curable resin composition is not particularly limited, but from the viewpoints of moldability and heat resistance, it is preferably 10 wt % to 80 wt %, and more preferably 40 wt % to 50 wt %, of the total weight of the curable resin composition.
[0030] In the curable resin composition of the present embodiment, the amount of the cyclic acid anhydride mixture used is preferably 0.7 to 1.2 equivalents relative to 1 equivalent of the epoxy group of the epoxy resin. If the amount is less than 0.7 equivalents relative to 1 equivalent of the epoxy group or exceeds 1.2 equivalents, curing may be incomplete and good cured properties may not be obtained.
[0031] In addition to the mixture of cyclic acid anhydrides, the curable resin composition may further contain other curing agents as necessary. The other curing agents can be appropriately selected from the curing agents usually used in curable resin compositions. Examples of the other curing agents include acid anhydride compounds other than the mixture of cyclic acid anhydrides, phenolic resins, etc.
[0032] Examples of the acid anhydride compound other than the mixture of cyclic acid anhydrides include phthalic anhydride, maleic anhydride, trimellitic anhydride, pyromellitic anhydride, hexahydrophthalic anhydride, tetrahydrophthalic anhydride, methylnadic anhydride, nadic anhydride, glutaric anhydride, dimethylglutaric anhydride, diethylglutaric anhydride, succinic anhydride, methylhexahydrophthalic anhydride, methyltetrahydrophthalic anhydride, etc. Among these, at least one selected from the group consisting of phthalic anhydride, trimellitic anhydride, hexahydrophthalic anhydride, tetrahydrophthalic anhydride, methylhexahydrophthalic anhydride, methyltetrahydrophthalic anhydride, glutaric anhydride, dimethylglutaric anhydride, and diethylglutaric anhydride is preferred. In addition, from the viewpoint of the handling and workability of the curable resin composition, an acid anhydride compound that is solid at room temperature is preferred.
[0033] The curable resin composition of the present embodiment can also adjust the gelation time by using a curing accelerator. Examples of curing accelerators that can be used include imidazoles such as 2-methylimidazole, 2-ethylimidazole, and 2-ethyl-4-methylimidazole, tertiary amines such as 2-(dimethylaminomethyl)phenol and 1,8-diaza-bicyclo[5,4,0]undecene-7, phosphines such as triphenylphosphine, and metal compounds such as tin octylate. The curing accelerator is used in an amount of 0.01 to 5.0 parts by weight per 100 parts by weight of the epoxy resin, as necessary.
[0034] The curable resin composition of the present embodiment may further contain various additives as exemplified below, as necessary. However, the curable resin composition of the present embodiment is not limited to the additives below, and may contain various additives well known in the art, as necessary.
[0035] The curable resin composition of the present embodiment may further contain a flame retardant as necessary for the purpose of imparting flame retardancy. The flame retardant is not particularly limited, and examples thereof include phosphorus compounds such as red phosphorus, phosphoric acid esters, and triphenylphosphine oxide coated with a thermosetting resin such as a phenolic resin; nitrogen-containing compounds such as melamine, melamine derivatives, melamine-modified phenolic resins, compounds having a triazine ring, cyanuric acid derivatives, and isocyanuric acid derivatives; phosphorus and nitrogen-containing compounds such as cyclophosphazene; metal complex compounds such as dicyclopentadienyl iron; zinc compounds such as zinc oxide, zinc stannate, zinc borate, and zinc molybdate; metal oxides such as iron oxide and molybdenum oxide; and metal hydroxides such as aluminum hydroxide and magnesium hydroxide. Examples of the flame retardant include known organic or inorganic compounds and metal hydroxides containing halogen atoms, antimony atoms, nitrogen atoms, or phosphorus atoms.
[0036] The curable resin composition of the present embodiment may further contain an inorganic filler as necessary. Specific examples of the inorganic filler include fine powders of fused silica, crystalline silica, glass, alumina, calcium carbonate, zirconium silicate, calcium silicate, silicon nitride, aluminum nitride, boron nitride, beryllia, zirconia, zircon, fosterite, steatite, spinel, mullite, titania, talc, clay, mica, etc., or beads obtained by sphering these.
[0037] Inorganic fillers having a flame retardant effect may be used, such as aluminum hydroxide, magnesium hydroxide, composite metal hydroxides such as a composite hydroxide of magnesium and zinc, and zinc borate.
[0038] When the curable resin composition contains an inorganic filler, its content is not particularly limited as long as the effect of this embodiment can be obtained. The content of the inorganic filler is preferably 50% by weight or more in the total weight of the curable resin composition, more preferably 60% by weight to 95% by weight from the viewpoint of flame retardancy, and even more preferably 70% by weight to 90% by weight. By containing an inorganic filler, the thermal expansion coefficient, thermal conductivity, elastic modulus, etc. of the cured product can be improved to desired properties. When the content of the inorganic filler is 50% by weight or more, the effect of improving these properties can be obtained more effectively. Also, when it is 95% by weight or less, the viscosity increase of the curable resin composition is more suppressed, sufficient fluidity is easily obtained, and moldability is further improved.
[0039] The curable resin composition of the present embodiment may further contain an antioxidant as necessary. This can prevent oxidation of the cured product of the curable resin composition, and can suppress weight loss of the cured product even when left in a high-temperature environment. Electrical properties are further improved.
[0040] Examples of the antioxidant include phenol-based antioxidants, phosphite-based antioxidants, sulfur-based antioxidants, hindered amine-based antioxidants, etc. These antioxidants may be used alone or in combination of two or more.
[0041] When the curable resin composition contains an antioxidant, the content is not particularly limited as long as the weight loss suppression effect is achieved. From the viewpoint of the heat resistance (high Tg) of the curable resin composition, the content of the antioxidant is preferably 0.5 parts by weight to 20 parts by weight, more preferably 1 part by weight to 10 parts by weight, based on 100 parts by weight of the total amount of the epoxy resin. By making the content of the antioxidant 0.5 parts by weight or more, the effect of suppressing the weight loss of the cured product can be sufficiently obtained, and by making the content of the antioxidant 20 parts by weight or less, the heat resistance (high Tg) of the cured product is suppressed from decreasing.
[0042] The curable resin composition of the present embodiment may further contain a coupling agent as necessary. This improves the adhesion between the resin component and the inorganic filler, and improves the electrical properties. The coupling agent may be appropriately selected from compounds that are commonly used. Examples of the coupling agent include known coupling agents such as various silane-based compounds such as epoxysilane, mercaptosilane, aminosilane, alkylsilane, ureidosilane, vinylsilane, styrylsilane, methacrylsilane, acrylicsilane, and sulfidosilane, titanium-based compounds, aluminum chelate compounds, and aluminum / zirconium-based compounds. Among these, silane-based compounds are preferred. These coupling agents may be used alone or in combination of two or more.
[0043] When the curable resin composition contains a coupling agent, the content is preferably 0.05 to 5.0 parts by weight, and more preferably 0.1 to 4.5 parts by weight, based on 100 parts by weight of the total amount of the inorganic filler. By making the content 0.05 parts by weight or more, the adhesion to the frame, etc. can be further improved.
[0044] The method for preparing the curable resin composition of the present embodiment is not particularly limited, but each component may be mixed uniformly or may be prepolymerized. For example, a mixture containing the compound of the present embodiment is heated in the presence or absence of a curing accelerator or a polymerization initiator, and in the presence or absence of a solvent to form a prepolymer. Similarly, an amine compound, a compound having an ethylenically unsaturated bond, a maleimide compound, a cyanate ester compound, polybutadiene and its modified products, polystyrene and its modified products, inorganic fillers, and other additives may be added to form a prepolymer. The mixing or prepolymerization of each component is carried out using, for example, an extruder, a kneader, a roll, or the like in the absence of a solvent, and a reaction kettle with a stirrer in the presence of a solvent.
[0045] The curable resin composition of the present embodiment is obtained by uniformly mixing the above-mentioned components. The method for producing the curable resin composition of the present embodiment is not particularly limited, but for example, the composition can be obtained by thoroughly mixing the epoxy resin with a curing agent, a curing accelerator, an inorganic filler, a mold release agent, a silane coupling agent, an additive, etc., using an extruder, a kneader, a roll, a planetary mixer, etc., until the mixture is uniform.
[0046] The obtained curable resin composition can be formed into various forms such as a resin sheet, a prepreg, etc. The prepreg form can be obtained, for example, by heating and melting the curable resin composition and / or the resin sheet of the present embodiment to reduce the viscosity and impregnating the composition into a fiber substrate.
[0047] The curable resin composition of the present embodiment may be dissolved in a solvent such as toluene, xylene, acetone, methyl ethyl ketone, methyl isobutyl ketone, dimethylformamide, dimethylacetamide, or N-methylpyrrolidone as necessary to form a varnish-like composition (hereinafter, simply referred to as varnish), which may be impregnated into a substrate such as glass fiber, carbon fiber, polyester fiber, polyamide fiber, alumina fiber, or paper, and dried by heating to produce a prepreg. The solvent used in this case is in an amount that occupies 10 to 70% by weight, preferably 15 to 70% by weight, of the mixture of the curable resin composition of the present embodiment and the solvent.
[0048] The prepreg is cut into a desired shape, laminated, and then the epoxy resin composition is heated and cured while applying pressure to the laminate by press molding, autoclave molding, sheet winding molding, etc., to obtain a carbon fiber reinforced plastic (CFRP). Copper foil or an organic film can also be laminated when laminating the prepreg.
[0049] In addition to the above-mentioned methods, CFRP can also be obtained by molding using known methods. For example, a resin transfer molding technique (RTM method) can be used in which a carbon fiber substrate (usually a carbon fiber fabric) is cut, laminated, and shaped to prepare a preform (a preform before being impregnated with resin), the preform is placed in a mold, the mold is closed, resin is injected to impregnate the preform, and the resin is hardened, and then the mold is opened to remove the molded product. In addition, a type of RTM method, such as the VaRTM method, the SCRIMP (Seeman's Composite Resin Infusion Molding Process) method, and the CAPRI (Controlled Atmospheric Pressure Resin Infusion) method, which is described in JP-T 2005-527410, can be used, which more appropriately controls the resin injection process, especially the VaRTM method, by evacuating a resin supply tank to a pressure lower than atmospheric pressure, using cyclic compression, and controlling the net molding pressure. In addition, other methods that can be used include the film stacking method, in which the fiber substrate is sandwiched between resin sheets (films), the method of attaching powdered resin to the reinforcing fiber substrate to improve impregnation, the molding method (Powder Impregnated Yarn) that uses a fluidized bed or fluid slurry method in the process of mixing the resin into the fiber substrate, and the method of blending resin fibers into the fiber substrate.
[0050] Examples of carbon fibers include acrylic, pitch, and rayon carbon fibers, and among them, acrylic carbon fibers having high tensile strength are preferably used. As the form of carbon fibers, twisted yarn, untwisted yarn, non-twisted yarn, etc. can be used, but untwisted yarn or non-twisted yarn is preferably used because it has a good balance between the formability and strength properties of the fiber-reinforced composite material.
[0051] The cured product of the curable resin composition of the present embodiment can be used for various applications other than the above-mentioned applications such as CFRP. Examples of the applications include adhesives, paints, coating agents, molding materials (including sheets, films, CFRP, etc.), encapsulants for semiconductor elements, encapsulants for liquid crystal display elements, encapsulants for organic EL elements, printed wiring boards (BGA substrates, build-up substrates, etc.), and electric / electronic parts, 3D printing, as well as additives for other resins, etc.
[0052] The adhesives include adhesives for civil engineering, construction, automobiles, general office use, medical use, and adhesives for electronic materials. Among these, adhesives for electronic materials include interlayer adhesives for multilayer boards such as build-up boards, die bonding agents, semiconductor adhesives such as underfills, underfills for reinforcing BGAs, and mounting adhesives such as anisotropic conductive films (ACFs) and anisotropic conductive pastes (ACPs), and are applicable to various uses.
[0053] When the curable resin composition of this embodiment is applied to a semiconductor element encapsulant, the curable resin composition of this embodiment is placed on a lead frame equipped with a semiconductor element, a semiconductor package substrate, and molded by a melt casting method, a transfer molding method, an injection molding method, a compression molding method, or the like, and further heated at 80 to 200° C. for 2 to 10 hours to obtain a cured product. Examples of semiconductor devices manufactured using this encapsulant include potting, dipping, and transfer mold encapsulation for capacitors, transistors, diodes, light-emitting diodes, ICs, and LSIs, potting encapsulation for COB, COF, TAB, and the like of ICs and LSIs, underfill for flip chips, and encapsulation (including reinforcing underfill) when mounting IC packages such as QFP, BGA, and CSP.
[0054] When the curable resin composition of the present embodiment is applied to a printed wiring board application, a prepreg can be obtained by heating and melting the composition to reduce the viscosity and impregnating the composition into reinforcing fibers such as glass fibers and polyamide fibers. Specific examples of the composition include glass fibers such as E glass cloth, D glass cloth, S glass cloth, Q glass cloth, spherical glass cloth, NE glass cloth, and T glass cloth, and / or organic fibers, but are not particularly limited thereto. The shape of the substrate is not particularly limited, but examples include woven fabric, nonwoven fabric, roving, chopped strand mat, and the like. In addition, as the weaving method of the woven fabric, plain weave, sash weave, twill weave, and the like are known, and these known weaves can be appropriately selected and used according to the intended application and performance. In addition, woven fabrics that have been subjected to fiber opening treatment or glass woven fabrics that have been surface-treated with a silane coupling agent or the like are preferably used. The thickness of the substrate is not particularly limited, but is preferably about 0.01 to 0.4 mm. Moreover, the varnish can be impregnated into reinforcing fibers and dried by heating to obtain a prepreg, which can be used to prepare a copper clad laminate (CCL). The obtained prepreg and CCL can be hot-press molded to prepare a laminate using the curable resin composition of the present embodiment. The laminate is not particularly limited as long as it has one or more prepregs, and may have any other layers. Moreover, a sheet-shaped adhesive can be obtained by applying the varnish onto a release film, removing the solvent under heating, and performing B-stage formation. This sheet-shaped adhesive can be used as an interlayer insulating layer in a multilayer board or an adhesive sheet when mounting a semiconductor. The curable resin composition of the present embodiment can also be suitably used for special board materials such as package boards (substrates) and HDI (high density interconnect). EXAMPLES
[0055] The present invention will be described in more detail below with reference to examples, but the present invention is not limited to such examples. In the following, parts are by weight unless otherwise specified.
[0056] Various analytical methods were carried out under the following conditions. ·GC / MS measurement (EI, CI) Equipment: GC-2020Plus / GCMS-QP2020 (Shimadzu Corporation) Column: HP-5MS (Agilent Technologies) Column flow rate: 1.2 ml / min Oven: 50℃ (2min)-10℃ / min-300℃ (18min) Mass range: m / z 35~800 Ion source: 230℃ Inlet: 320 ℃, injection volume 1.0 μl
[0057] ·GC measurement Equipment: 8890GC System (Agilent Technologies) Column: HP-5MS (Agilent Technologies) Column flow rate: 1.2 ml / min Oven: 100℃ (2 min) - 5℃ / min - 300℃ (3 min) Injection port: 300℃, injection volume 1.0μl Detector: FID (300 °C)
[0058] [Synthesis Example 1] In a four-neck flask, 49.1 parts of toluene and 25.8 parts of α-terpinene (1,3-p-menthadiene, manufactured by Guangxi Jie Xin Fragrance Co., Ltd.) were placed, and the mixture was heated to 45°C and stirred. 16.7 parts of maleic anhydride manufactured by Junsei Chemical Co., Ltd. were added to this solution in four portions over one hour. After the addition was completed, the mixture was stirred at 45°C for one hour. After the reaction was completed, the mixture was concentrated under reduced pressure at 185°C to obtain 37 parts of a mixture of cyclic acid anhydrides (A-1).
[0059] [Synthesis Example 2] The same procedure as in Synthesis Example 1 was carried out except that the reaction temperature was changed to 65°C, and 35 parts of a cyclic acid anhydride mixture (A-2) was obtained.
[0060] [Synthesis Example 3] The same procedure as in Synthesis Example 1 was carried out except that the reaction temperature was changed to 85° C. and toluene was not used, to obtain 37 parts of a cyclic acid anhydride mixture (A-3).
[0061] [Synthesis Example 4] The same procedure as in Synthesis Example 1 was carried out except that the reaction temperature was changed to 185° C. and toluene was not used, to obtain 34 parts of a cyclic acid anhydride mixture (A-4).
[0062] The structures of the mixtures of cyclic acid anhydrides obtained in Synthesis Examples 1 to 4 were identified by GC / MS measurement, and the area percentages when the sum of the peak areas of the cyclic acid anhydrides represented by formulae (Aa) to (Ac) measured by GC was taken as 100% are shown in Table 1.
[0063] The melting point and crystallization rate were measured under the following conditions. <Melting point measurement conditions> Differential scanning calorimeter: Linseis CHIP DSC Gas flow rate: N2 gas 50ml / min Heating rate: 20℃ / min Measurement temperature range: 30℃-270℃
[0064] <Crystallization rate measurement conditions> The mixtures of cyclic acid anhydrides obtained in Synthesis Examples 1 to 4 were allowed to stand in an oven at 80° C. for 1 hour to dissolve. 0.02 g of the solution in which the mixture of cyclic acid anhydrides was dissolved was dropped into a tray maintained at 10° C. and allowed to stand. The time until the transparent liquid crystallized and completely became cloudy and solidified was measured.
[0065] [Table 1]
[0066] [Example 1, Comparative Examples 1 and 2] The mixtures of cyclic acid anhydrides obtained in Synthesis Examples 1 to 4, epoxy resins, and curing accelerators were mixed in the weight ratios shown in Table 2, and cured at 120°C for 2 hours and then at 160°C for 6 hours to produce cured products. Physical properties were evaluated under the following conditions.
[0067] <Heat resistance (Tg) and linear expansion coefficient measurement conditions> Thermomechanical analyzer: TMA Q400 (TA Instruments) Measurement temperature range: 30~350℃ Heating rate: 2℃ / min Tg: The point at which the linear expansion coefficient changes Coefficient of linear expansion (CTE): Change in unit dimension in the ranges of 50-90℃ and 260-290℃ Standards: Compliant with JIS K-7244
[0068] [Table 2]
[0069] RE-310S: Bisphenol A type epoxy resin (manufactured by Nippon Kayaku Co., Ltd.) 2E4MZ: 2-ethyl-4-methylimidazole (manufactured by Shikoku Kasei Co., Ltd.)
[0070] As shown in Tables 1 and 2, the acid anhydride mixture of the present invention has a fast crystallization rate, and the curable resin composition thereof has excellent heat resistance and low linear expansion coefficient (dimensional stability), and therefore can be suitably used for carbon fiber reinforced composite materials.
Claims
1. A mixture of cyclic acid anhydrides including a cyclic acid anhydride represented by the following formula (A-a), a cyclic acid anhydride represented by the following formula (A-b), and a cyclic acid anhydride represented by the following formula (A-c): A mixture of cyclic acid anhydrides, in which, when the sum of the peak areas of the cyclic acid anhydrides represented by the formulas (A-a) to (A-c) is taken as 100% in a gas chromatographic analysis of the mixture of cyclic acid anhydrides, the peak area of the cyclic acid anhydride represented by the formula (A-a) is 0.1% or more and 1.0% or less, the peak area of the cyclic acid anhydride represented by the formula (A-b) is 98.0% or more and 99.0% or less, and the peak area of the cyclic acid anhydride represented by the formula (A-c) is 0.1% or more and 1.0% or less. 【Chemistry 1】
2. 2. The cyclic acid anhydride mixture according to claim 1, which is dissolved at 80° C., and then allowed to stand at 10° C. for 0.1 to 1.5 hours until crystallization.
3. 2. The cyclic acid anhydride mixture according to claim 1, which is in the form of pellets, granules, or marbles.
4. A curable resin composition comprising the mixture of cyclic acid anhydrides according to any one of claims 1 to 3, an epoxy resin, and a curing accelerator.
5. A cured product obtained by curing the curable resin composition according to claim 4.
6. A carbon fiber reinforced composite material obtained by curing the curable resin composition according to claim 4.
7. The method for producing the cyclic acid anhydride mixture according to any one of claims 1 to 3, which is obtained by reacting 1,3-p-menthadiene, maleic anhydride and a solvent at 40 to 80 ° C., and then concentrating the solvent.
Citation Information
Patent Citations
Preparation method of seven-membered cyclic carbonate monomer and polycarbonate based on D-A reaction
CN115703789A
Curable epoxy resin composition
JP1980118920A
Compound having lactone structure
JP2004315465A
New lactone compound
JP2005023063A
New alicyclic compound, method for producing the same and polymer composition
JP2008088154A