Styrenic resin foamed particle, packing of beads cushioning material, foamed particle molded body
Foamed styrenic resin particles with controlled molecular weights and branching, along with high closed cell ratios, address the challenge of maintaining rigidity and restorability while being lightweight, suitable for packaging and cushioning materials.
Patent Information
- Application Number
- JP2023055553
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Filing Date
- 2023-03-30
- Publication Date
- 2024-10-11
AI Technical Summary
Foamed styrenic resin particles struggle to maintain a well-balanced combination of rigidity, restorability, and lightness, particularly when the expansion ratio is increased, leading to reduced restorability and insufficient rigidity.
The development of foamed styrenic resin particles with specific molecular weight ranges (1 million to 5 million), a molecular weight ratio of Z-average to number-average molecular weight of 5 or more, a branching degree of 0.2 per 1000 units, and a closed cell ratio of 85% or more, along with controlled cell diameter and thickness variations, enhances restorability and rigidity.
The particles achieve excellent restorability and rigidity even at high bulk ratios, maintaining a well-balanced performance due to increased cell membrane strength and closed cell ratio, ensuring effective use in packaging and cushioning applications.
Smart Images

Figure 2024143069000001_ABST
Abstract
Description
[Technical field]
[0001] The present invention relates to expanded styrene-based resin beads, a filling for a bead cushion material using the same, and an expanded bead molding. [Background technology]
[0002] Styrene-based resin expanded beads are used for various purposes. For example, expanded bead moldings obtained by molding the expanded beads in a mold are suitable for use as packaging containers and cushioning materials for heavy objects. The expanded beads are also suitable for use as padding for cushioning materials in their original form. For such purposes, they are required to have appropriate rigidity, excellent recovery properties, and the ability to be used repeatedly.
[0003] For example, Patent Document 1 proposes expanded styrene resin beads having an expansion ratio of 20 to 50, a narrow particle size distribution, and a high Z-average molecular weight. According to Patent Document 1, such expanded styrene resin beads have a low settling rate and can withstand repeated use, and are therefore suitable for bead cushion applications. [Prior art documents] [Patent documents]
[0004] [Patent Document 1] JP 2019-73653 A Summary of the Invention [Problem to be solved by the invention]
[0005] In recent years, in addition to rigidity and resilience, a higher degree of lightness is sometimes required for the expanded styrene resin beads used in the above-mentioned applications. Usually, when the expansion ratio of the expanded beads is increased in order to increase the lightness, the resilience of the expanded beads is likely to decrease, and the beads are unlikely to return to their original state when a load is repeatedly applied. For example, in the expanded beads of Patent Document 1, when the expansion ratio is increased, the resilience is significantly decreased, and the beads are not able to withstand repeated use. In addition, when the expansion ratio is increased, the rigidity is likely to become insufficient, so that it is difficult for the expanded beads of Patent Document 1 to satisfy all of the rigidity, resilience, and lightness.
[0006] The present invention has been made in view of the above background, and aims to provide styrene-based resin expanded beads that can combine excellent resilience, rigidity, and light weight in a well-balanced manner, and a filling for a bead cushion material using the same, and an expanded bead molding. [Means for solving the problem]
[0007] One aspect of the present invention resides in the following expanded styrene resin particles [1] to [8]. [1] Expanded beads made of a styrene-based resin, The expanded beads have a bulk ratio of 30 to 150 times, The weight average molecular weight Mw' of the styrene-based resin is 1 million or more and 5 million or less, the ratio Mz' / Mn' of the Z-average molecular weight Mz' to the number-average molecular weight Mn' of the styrene-based resin is 5 or more (wherein the weight-average molecular weight Mw', the number-average molecular weight Mn' and the Z-average molecular weight Mz' are determined by a GPC-MALS method); The styrene-based resin expanded particles have a branching degree of 0.2 or more per 1,000 styrene units.
[0008] [2] The expanded styrene-based resin particles according to [1], wherein the ratio Mz' / Mn' of the Z-average molecular weight Mz' to the number-average molecular weight Mn' of the styrene-based resin is 7 or more. [3] The expanded styrene-based resin particles according to [1] or [2], wherein the styrene-based resin has a weight-average molecular weight Mw' of 1.5 million or more.
[0009] [4] The expanded styrene-based resin particles according to any one of [1] to [3], wherein the styrene-based resin has a tetrahydrofuran insoluble content of 0.1 mass % or less (including 0). [5] The expanded styrene resin beads according to any one of [1] to [4], wherein the expanded beads have a bulk ratio of 80 to 150. [6] The expanded styrene resin beads according to any one of [1] to [5], wherein the expanded beads have a closed cell rate of 85% or more.
[0010] [7] The expanded styrene resin beads according to any one of [1] to [6], wherein the average bubble diameter of the expanded beads is 10 μm or more and 100 μm or less, and the coefficient of variation of the bubble diameter is 20% or less. [8] The expanded styrene-based resin beads according to any one of [1] to [7], wherein the average cell thickness of the expanded beads is 1 μm or more and 8 μm or less, and the coefficient of variation of the cell thickness is 35% or less. [9] The expanded styrene resin beads according to any one of [1] to [8], wherein the expanded beads have an average particle size of 3 to 10 mm.
[0011] Another aspect of the present invention resides in the expanded styrene resin particles according to the following
[10] .
[10] A filling for a bead cushion material, comprising the styrene-based resin foam particles described in any one of [1] to [9].
[0012] Yet another aspect of the present invention is the foamed bead molding according to the following
[11] .
[11] An expanded bead molding obtained by molding the expanded styrene-based resin beads according to any one of [1] to [9] in a mold. Effect of the Invention
[0013] According to the above-mentioned aspect, it is possible to provide styrene-based resin expanded beads that can combine excellent resilience, rigidity, and light weight in a well-balanced manner, and a filling for a bead cushion material and an expanded bead molding using the same. [Brief description of the drawings]
[0014] [Figure 1] FIG. 1 is an enlarged photograph (magnification: 200 times) of the cross section of the expanded beads of Example 1. [Diagram 2] FIG. 2 is an enlarged photograph (magnification: 2500 times) of the cell membrane in the expanded beads of Example 1. [Diagram 3] FIG. 3 is an enlarged photograph (magnification: 2500 times) of a cell membrane at a different site from that in FIG. 2 in the expanded beads of Example 1. [Figure 4] FIG. 4 is an enlarged photograph (magnification: 200 times) of the cross section of the expanded beads of Comparative Example 1. [Diagram 5] FIG. 5 is an enlarged photograph (magnification: 2500 times) of the cell membrane in the expanded beads of Comparative Example 1. [Figure 6] FIG. 6 is an enlarged photograph (magnification: 2500 times) of the cell membrane of a site different from that of FIG. 5 in the expanded beads of Comparative Example 1. [Figure 7] FIG. 7 is a diagram showing an example of a Debye Plot obtained when a styrene-based resin is measured by a GPC-MALS method. [Figure 8] FIG. 4 is a graph showing a simulation result in the first embodiment. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0015] In this specification, the alphabets and numbers in parentheses do not limit the present invention in any way. In addition, "expandable styrene resin particles" may be referred to as "expandable resin particles", "styrene resin expanded particles" may be referred to as "expanded particles", and "expanded particle moldings" may be referred to as "molded bodies". In addition, when the symbol "~" is used to express a numerical range, it is used in a sense including the numerical values written before and after it.
[0016] [Application] The expanded beads are used as they are as a stuffing for a bead cushion material, or are used to manufacture an expanded bead molded article. In this case, it is possible to provide a stuffing for a bead cushion material and an expanded bead molded article that are lightweight yet have excellent resilience and rigidity. The molded article is manufactured by, for example, molding a large number of expanded beads in a mold, and a molded article is obtained in which the expanded beads are fused to each other.
[0017] [Styrene-based resin] The expanded beads are composed of a styrene resin. The styrene resin has a weight average molecular weight Mw' of 1 million or more and 5 million or less, and a ratio Mz' / Mn' of the Z average molecular weight Mz' to the number average molecular weight Mn' of the styrene resin is 5 or more. The branching degree B per 1000 styrene units of the styrene resin is 100% or more. m,1000 is 0.2 or more.
[0018] The expanded beads have a weight average molecular weight Mw', a ratio Mz' / Mn' and a branching degree of B m,1000 is within the above-mentioned range, the expanded beads have a good balance of excellent resilience, rigidity, and light weight as described above. This is believed to be because the expanded beads made of the styrene resin having the above-mentioned specified branched structure can increase the strength of the bubble film and the closed cell ratio even when the bulk ratio is high, and the closed cell ratio is likely to be maintained high even after compression. Therefore, the expanded beads have excellent resilience and rigidity even when the bulk ratio is high. In addition, the expanded bead molding obtained by fusing the expanded beads to each other has excellent resilience and rigidity even when the molding ratio is high.
[0019] In this specification, the absolute molecular weight is represented with a prime symbol (’), and the relative molecular weight is represented without a prime symbol. That is, the weight-average molecular weight Mw’, the number-average molecular weight Mn’, and the Z-average molecular weight Mz’ are all absolute molecular weights, and the weight-average molecular weight Mw, the number-average molecular weight Mn, and the Z-average molecular weight Mz are all relative molecular weights in terms of linear polystyrene conversion.
[0020] The weight-average molecular weight Mw’, the number-average molecular weight Mn’, the Z-average molecular weight Mz’, and the degree of branching are determined by the GPC-MALS method. The GPC-MALS method is a technique that combines gel permeation chromatography (i.e., GPC) and a multi-angle light scattering detector (i.e., MALS). By the GPC-MALS method, the absolute molecular weight of the styrene resin and the root-mean-square radius of gyration <Rg 2 > corresponding to the molecular size can be measured, and from the measurement results, the degree of branching of the styrene resin can be determined. The basic principle of the GPC-MALS method is described below.
[0021] <Basic Principle of GPC-MALS Method> The styrene resin is dissolved in a solvent such as tetrahydrofuran (i.e., THF) to prepare a styrene resin solution, and when this is subjected to GPC measurement, polymers with larger molecular sizes elute earlier, so the styrene resin is separated by molecular size. Subsequently, by subjecting the separated styrene resin solution to MALS measurement, the weight-average molecular weight Mw’ and the root-mean-square radius of gyration <Rg 2 > of the styrene resin separated by molecular size can be calculated.
[0022] Specifically, a laser beam is irradiated onto the styrene resin solution separated by molecular size by GPC, and the scattered light intensity generated from the styrene resin solution by Rayleigh scattering is measured. From the obtained measurement values, Mw’ and <Rg 2 > are calculated using the following formula (1) and the Debye plot shown in FIG. 7.
[0023]
Number
[0024] K * :Optical parameters (4π 2 n0 2 (dn / dc) 2 / [λ0 4 N A ]) n0: Refractive index of the solvent dn / dc: refractive index concentration increment λ0: Wavelength of incident light in a vacuum N A :Avogadro's number c: Sample concentration (g / mL) R(θ): Rayleigh ratio of excess scattering Mw': Weight average molecular weight (g / mole) P(θ): interference factor P(θ)=(1-2{(4π / λ)sin(θ / 2)} 2 <Rg 2 > / 3!+···) λ: Wavelength in the measurement system λ0 / n0 <Rg 2 >: Mean square radius of gyration A2: Second virial coefficient
[0025] Figure 7 shows the results of measurements of styrene resin solutions with different resin concentrations using the GPC-MALS method. * c / R(θ) and the horizontal axis (X axis) is "sin 2 This is an example of a Debye plot in which the weight average molecular weight Mw' of the styrene resin separated by molecular size by GPC is calculated from the intercept (Y-axis intercept) of the regression line obtained from the Debye plot and the mean square radius of gyration of the styrene resin. <Rg 2 In GPC measurements, the concentration at each elution time is very low, so if the second virial coefficient A2 is set to 0, the weight average molecular weight Mw' and the root mean square radius of gyration of the styrene resin separated by molecular size by GPC are <Rg 2 > can be calculated using the following formulas (2) and (3), respectively.
[0026]
number
[0027]
number
[0028] K * c / R0: K at angle θ = 0° * c / R(θ) dy / dx: Initial slope of the regression line
[0029] The number average molecular weight Mn', weight average molecular weight Mw', and Z average molecular weight Mz' determined by the GPC-MALS method are absolute molecular weights of the styrene-based resin. On the other hand, the number average molecular weight Mn, weight average molecular weight Mw, and Z average molecular weight Mz determined by the GPC method using linear polystyrene having a known molecular weight as the standard substance are the relative molecular weights of the styrene-based resin.
[0030] The shrinkage factor g of the styrene resin is calculated as follows: Root mean square radius of gyration of the styrene resin <Rg 2 > B and the root mean square radius of gyration of linear styrene resin <Rg 2 > L The ratio of these is taken as the shrinkage factor g, and the shrinkage factor g can be calculated based on the following formulas (4) to (8). Then, the branching degree B m The degree of branching is based on the assumption that the styrene resin has a three-chain branched structure. The degree of branching is the degree of long chain branching.
[0031] Contraction factor g w , degree of branching per molecule B m,w , degree of branching per 1000 units of styrene B m,1000 is calculated using the following formulas (4) to (8).
[0032]
number
[0033]
number
[0034]
number
[0035]
number
[0036]
number
[0037] In the above formula, g i is the contraction factor in interval i, B m,j is the branching degree in interval i, c i is the concentration in interval i.
[0038] <Weight average molecular weight Mw'> The weight average molecular weight Mw' of the styrene resin is 1 million or more and 5 million or less. If Mw' is too low, the expanded beads may not be able to exhibit sufficient restoring property and rigidity when the bulk ratio is high. From the viewpoint of further improving the restoring property and rigidity, Mw' of the styrene resin is preferably 1.5 million or more, more preferably 1.8 million or more, and even more preferably 2 million or more. On the other hand, if Mw' is too high, the expandability may decrease and expanded beads with a desired bulk ratio may not be obtained. From the viewpoint of more easily increasing the bulk ratio of the expanded beads, Mw' is preferably 4 million or less, more preferably 3.5 million or less, and even more preferably 3 million or less.
[0039] <Ratio of Z-average molecular weight Mz' to number-average molecular weight Mn', Mz' / Mn'> The ratio Mz’ / Mn’ of the Z-average molecular weight Mz’ to the number-average molecular weight Mn’ of the styrene resin is 5 or more. When Mz’ / Mn’ is less than 5, the molecular weight distribution of the styrene resin becomes narrow. As a result, when the bulk expansion ratio is high, there is a possibility that the resilience and rigidity of the foamed particles cannot be achieved in good balance. Mz’ / Mn’ is preferably 7 or more, more preferably 8 or more. In this case, since the molecular weight distribution is wider, the strain curability described later is more sufficiently expressed, and the resilience and rigidity of the foamed particles when the bulk expansion ratio is high can be improved in better balance. Further, from the viewpoint of achieving both the resilience and rigidity of the foamed particles and the molded body at a higher level, Mz’ / Mn’ is preferably 25 or less, more preferably 20 or less, and still more preferably 15 or less.
[0040] <Number-average molecular weight Mn’> From the viewpoint of more surely enhancing the resilience and rigidity of the foamed particles, the number-average molecular weight Mn’ of the styrene resin is preferably 300,000 or more, more preferably 500,000 or more. Further, from the viewpoint of more surely enhancing the foamability of the styrene resin, Mn’ is preferably 1,200,000 or less, more preferably 1,000,000 or less.
[0041] <Z-average molecular weight Mz’> From the viewpoint of further expanding the molecular weight distribution and more surely enhancing the resilience and rigidity of the foamed particles, the Z-average molecular weight Mz’ of the styrene resin is preferably 3.5 million or more, more preferably 4 million or more, still more preferably 5 million or more. Further, from the viewpoint of more surely enhancing the foamability of the styrene resin, Mz’ is preferably 12 million or less, more preferably 8 million or less.
[0042] <Shrinkage factor g w > From the viewpoint of more surely enhancing the resilience and rigidity of the foamed particles, the shrinkage factor g of the styrene resin w is preferably 0.85 or less, more preferably 0.8 or less, and still more preferably 0.75 or less. Further, the shrinkage factor g w is preferably 0.5 or more.
[0043] <Degree of branching per 1000 units of styrene> The branching degree of the styrene resin per 1000 styrene units is 0.2 or more. If it is less than 0.2, the branching points of the styrene resin are few or too far apart, so that when the bulk ratio is high, the recovery property and rigidity of the expanded beads may not be balanced. From the viewpoint of improving the recovery property and rigidity in a more balanced manner, the branching degree per 1000 styrene units is preferably 0.25 or more, more preferably 0.3 or more. The branching degree per 1000 styrene units is preferably 2 or less, more preferably 1 or less.
[0044] The content of the component derived from the polyfunctional monomer in the polymer chain constituting the styrene-based resin is preferably less than 50 mass ppm (including 0) in 100 parts by mass of the styrene-based resin. In this case, even if the component derived from the polyfunctional monomer such as divinylbenzene is small, the effect that the expanded beads have high bulk ratio and both restorability and rigidity is remarkable. From the viewpoint of making this effect more remarkable, the content of the component derived from the polyfunctional monomer is more preferably 30 mass ppm or less (including 0), even more preferably 20 mass ppm or less (including 0), and even more preferably substantially 0. Such a styrene-based resin can be obtained by producing a styrene-based resin without using a polyfunctional monomer such as divinylbenzene as a branching agent for forming a branched structure. Specifically, it can be produced by the method described below.
[0045] Even when the bulk ratio of the expanded beads is high, from the viewpoint of achieving a better balance between the restoring property and the rigidity of the expanded beads, the melt flow rate (i.e., MFR) of the styrene resin is preferably less than 2 g / 10 min, more preferably less than 1 g / 10 min, and even more preferably 0.8 or less. The melt flow rate of the styrene resin is a value measured under the conditions of a test temperature of 200° C. and a load of 5 kg based on JIS K7210-1:2014.
[0046] The ratio Mz / Mw of the Z-average molecular weight Mz to the weight-average molecular weight Mw of the styrene resin is preferably less than 2.5. In this case, even when the expanded beads have a high bulk ratio, the effect of achieving a good balance between the restorability and rigidity of the expanded beads can be obtained. The weight-average molecular weight Mw, the Z-average molecular weight Mz, and the number-average molecular weight Mn are relative molecular weights, and are measured by gel permeation chromatography (i.e., GPC) using linear polystyrene as a standard substance.
[0047] Examples of the styrene-based resin include a homopolymer of a styrene-based monomer, a copolymer of a styrene-based monomer and another monomer, and a mixture of two or more of these. The styrene-based resin may be a copolymer containing a component derived from a monomer other than a styrene monomer within a range that does not impair the effects of the present invention, but the structural unit derived from the styrene-based monomer in the copolymer is preferably 50% by mass or more, more preferably 60% by mass or more, and even more preferably 80% by mass or more. The styrene-based resin is preferably a homopolymer of a styrene-based monomer.
[0048] Examples of the styrene monomer include styrene, α-methylstyrene, o-methylstyrene, m-methylstyrene, p-methylstyrene, p-ethylstyrene, 2,4-dimethylstyrene, p-methoxystyrene, pn-butylstyrene, pt-butylstyrene, o-chlorostyrene, m-chlorostyrene, p-chlorostyrene, 2,4,6-tribromostyrene, styrenesulfonic acid, and sodium styrenesulfonate. The above styrene monomers may be used alone or in combination of two or more kinds. As the styrene monomer, styrene is preferred.
[0049] Examples of the other monomers copolymerizable with the styrene-based monomer include unsaturated fatty acids and anhydrides thereof, such as acrylic acid, methacrylic acid, and maleic anhydride; acrylic acid esters, such as methyl acrylate, ethyl acrylate, propyl acrylate, butyl acrylate, and 2-ethylhexyl acrylate; methacrylic acid esters, such as methyl methacrylate, ethyl methacrylate, propyl methacrylate, butyl methacrylate, and 2-ethylhexyl methacrylate; hydroxyethyl acrylate, hydroxypropyl acrylate, hydroxyethyl methacrylate, hydroxyethyl ...methacrylate, hydroxyethyl methacrylate, hydroxyethyl methacrylate, hydroxyethyl methacrylate, hydroxyethyl methacrylate, hydroxyethyl methacrylate, hydroxyethyl methacrylate, hydroxyethyl methacrylate vinyl compounds containing a hydroxyl group, such as hydroxypropyl methacrylate; vinyl compounds containing a nitrile group, such as acrylonitrile and methacrylonitrile; organic acid vinyl compounds, such as vinyl acetate and vinyl propionate; olefin compounds, such as ethylene, propylene, 1-butene and 2-butene; diene compounds, such as butadiene, isoprene and chloroprene; vinyl halide compounds, such as vinyl chloride and vinyl bromide; vinylidene halide compounds, such as vinylidene chloride; and maleimide compounds, such as N-phenylmaleimide and N-methylmaleimide.
[0050] Specific examples of styrene-based resins include polystyrene, rubber-modified polystyrene (e.g., high-impact polystyrene), styrene-(meth)acrylonitrile copolymer, styrene-(meth)acrylic acid copolymer, styrene-methyl(meth)acrylate copolymer, styrene-maleic anhydride copolymer, etc. In this specification, (meth)acrylonitrile represents at least one of acrylonitrile and methacrylonitrile, and (meth)acrylic acid represents at least one of acrylic acid and methacrylic acid.
[0051] [Expandable resin particles] The expanded beads are produced by expanding expandable resin beads. The expandable resin beads contain a styrene-based resin and a foaming agent, and are obtained, for example, by impregnating resin beads made of the above-mentioned styrene-based resin with the foaming agent.
[0052] As the foaming agent, a physical foaming agent such as a hydrocarbon can be used. As the hydrocarbon, for example, a chain aliphatic hydrocarbon such as propane, normal butane, isobutane, normal pentane, isopentane, neopentane, normal hexane, etc. can be used. The foaming agent may be used alone or in combination of two or more. From the viewpoint of more easily foaming the styrene-based resin having the above-mentioned predetermined branched structure, it is preferable to use butane and pentane in combination as the foaming agent. From the viewpoint of easily expanding the expandable resin particles and easily obtaining expanded particles with a high bulk ratio, the content of the blowing agent in the expandable resin particles is preferably 3 parts by mass or more, and more preferably 5 parts by mass or more, relative to 100 parts by mass of the styrene-based resin. From the viewpoint of suppressing shrinkage immediately after expansion and easily obtaining expanded particles with a high bulk ratio, the content is preferably 10 parts by mass or less, and more preferably 8 parts by mass or less.
[0053] From the viewpoint of making it easier to expand the expandable resin particles composed of the styrene-based resin having the above-mentioned predetermined branched structure and from the viewpoint of improving the moldability of the expanded particles in the mold under low molding pressure conditions, it is preferable that the expandable resin particles contain a plasticizer. As the plasticizer, alicyclic hydrocarbons such as cyclohexane; carboxylic acid esters such as liquid paraffin, di-2-ethylhexyl phthalate, and di-2-ethylhexyl adipate; (meth)acrylic acid alkyl esters such as butyl stearate; and higher fatty acid esters such as glycerin tristearate can be used. From the viewpoint of making it easier to expand the expandable resin particles and to obtain expanded particles with a high bulk ratio, it is more preferable that the expandable resin particles contain an alicyclic hydrocarbon such as cyclohexane as a plasticizer. From the viewpoint of making it easier to obtain expanded particles with a high bulk ratio, the content of the plasticizer in the expandable resin particles is preferably 0.2 parts by mass or more and 3 parts by mass or less, and more preferably 0.5 parts by mass or more and 2 parts by mass or less, relative to 100 parts by mass of the styrene-based resin.
[0054] The expandable resin particles may contain additives such as a cell regulator, an antioxidant, an ultraviolet absorber, and a light stabilizer, as long as the intended object of the present invention can be achieved.
[0055] As the cell regulator, polyethylene wax, methyl methacrylate copolymer, talc, silica, ethylene bisstearylamide, etc. can be used. As the antioxidant, a phenol-based antioxidant, a phosphorus-based antioxidant, a sulfur-based antioxidant, or the like can be used.
[0056] As the ultraviolet absorbing agent, a benzotriazole-based ultraviolet absorbing agent, a benzophenone-based ultraviolet absorbing agent, or the like can be used. As the light stabilizer, a hindered amine compound or the like can be used.
[0057] The average particle diameter of the expandable resin particles is, for example, 0.5 mm to 2 mm. The average particle diameter of the expandable resin particles means the particle diameter at an integrated value of 63% in the particle size distribution obtained by a laser diffraction / scattering method. The average particle diameter is measured, for example, by a particle size distribution measuring device "Militrack JPA" manufactured by Nikkiso Co., Ltd.
[0058] [Foam particles] The expanded beads have excellent restoring properties and rigidity even when the bulk ratio is high. This is because the expanded beads are made of a styrene-based resin having the above-mentioned predetermined branched structure, and therefore, even when the bulk ratio is high, the strength of the bubble film can be increased and the closed cell ratio can be increased, and the closed cell ratio is likely to be maintained high even after compression. The reason why the expanded beads have such an effect is not clear, but is thought to be as follows. The expanded beads are made of a styrene-based resin having a weight average molecular weight Mw', a ratio Mz' / Mn' of the Z-average molecular weight to the number average molecular weight, and a branching degree within the above range. The styrene-based resin having such a branched structure is thought to have a large number of branching points constituting the polymer chain (i.e., a high branching degree), a structure in which the branching points are appropriately spaced apart, and further, a molecular weight is large and the molecular weight distribution is wide. Therefore, it is thought that the strength of the bubble film of the expanded beads is increased. Furthermore, it is thought that strain hardening is expressed, and the styrene-based resin constituting the bubble film is prevented from being stretched and broken during foaming, or from forming a thin-walled portion. As a result, the thickness of the cell membrane of the expanded beads is likely to be uniform. Similarly, the cell diameter of the expanded beads is likely to be uniform. From these facts, it is believed that the expanded beads have an increased cell membrane strength and a high closed cell ratio, and that the closed cell ratio is likely to be maintained high even after compression, and that the expanded beads have excellent recovery property and rigidity even when the bulk ratio is high.
[0059] The bulk ratio of the expanded beads is 30 times or more and 150 times or less. The expanded beads made of the above styrene-based resin have excellent restoring properties and rigidity even at a high bulk ratio of 30 times or more and 150 times or less. If the bulk ratio of the expanded beads is too low, the lightness of the expanded beads may be impaired. The bulk ratio of the expanded beads is preferably 50 times or more, more preferably 80 times or more. In this case, since the bulk ratio of the expanded beads is higher, the lightness is further improved, and the effect that the restoring properties and rigidity are well-balanced and excellent even at a high bulk ratio is remarkable. On the other hand, if the bulk ratio of the expanded beads is too high, it may be difficult to maintain high restoring properties and rigidity. From this viewpoint, the bulk ratio of the expanded beads is preferably 120 times or less. The method for measuring the bulk ratio of the expanded beads will be described in the examples.
[0060] The closed cell ratio of the expanded beads is preferably 85% or more. In this case, the effect of achieving a well-balanced and excellent recovery property and rigidity even at a high bulk ratio is remarkable. From the viewpoint of making this effect even more remarkable, the closed cell ratio of the expanded beads is more preferably 86% or more, and even more preferably 88% or more. In particular, when the bulk ratio is 30 times or more and 150 times or less, or 80 times or more and 150 times or less, and the closed cell ratio is within the above range, the above effect is even more remarkable. The method for measuring the closed cell ratio of the expanded beads will be described in the Examples.
[0061] The restoring property of the expanded beads is evaluated by the settling rate measured by a settling test. Usually, the higher the bulk ratio of the expanded beads, the more likely the restoring property is to decrease, and the larger the settling rate. When the bulk ratios of the expanded beads are the same, the expanded beads with a smaller settling rate are judged to have better restoring properties. The settling rate of the expanded beads is preferably 15% or less, more preferably 12% or less. Even when the bulk ratio is high, the expanded beads have excellent restoring properties, and the settling rate can be set within the above range. The settling rate is measured by repeatedly compressing the expanded beads, leaving the compressed expanded beads still for a predetermined time, and evaluating the extent to which the volume has been restored. A specific method for measuring the settling rate will be described in the examples.
[0062] The expanded beads tend to have a high closed cell ratio even after a load is applied by compression. Specifically, the expanded beads tend to generally maintain the original closed cell ratio after the settling test described below. This is thought to result in the expanded beads tending to have a small settling ratio and excellent restorability even when the bulk ratio is high. From the viewpoint of further improving the restorability of the expanded beads, the closed cell ratio of the expanded beads after the settling test is preferably 85% or more, more preferably 86% or more, and even more preferably 88% or more. A method for measuring the closed cell ratio of the expanded beads after the settling test will be described in the Examples.
[0063] The ratio [c1 / c0] of the closed cell rate c1 of the expanded beads after the sag test to the closed cell rate c0 of the expanded beads before the sag test (i.e., the closed cell rate of the expanded beads) is preferably 0.95 or more, more preferably 0.98 or more. The upper limit of the ratio [c1 / c0] is 1. Similarly, the difference [c0-c1] between the closed cell rate c0 of the expanded beads before the sag test and the closed cell rate c1 of the expanded beads after the sag test is preferably 3% or less, more preferably 2% or less. The lower limit of the difference [c0-c1] is 0. In these cases, the effect of achieving a well-balanced and excellent recovery property and rigidity even at a high bulk ratio is remarkable.
[0064] The average bubble diameter of the expanded beads is preferably 10 μm or more and 100 μm or less, and the coefficient of variation of the bubble diameter is preferably 20% or less. This means that the bubbles of the expanded beads are formed relatively uniformly. In this case, it is considered that the closed cell ratio is likely to be maintained high even after compression, and as a result, the effect of the recovery property and rigidity being well-balanced and excellent even at a high bulk ratio is remarkable. Such expanded beads can be obtained, for example, by using a styrene-based resin that exhibits the above-mentioned strain hardening property as the base resin. From the viewpoint of further remarkable effect of the recovery property and rigidity being well-balanced and excellent even at a high bulk ratio, the average bubble diameter is more preferably 30 μm or more and 80 μm or less. From the same viewpoint, the coefficient of variation of the bubble diameter is more preferably 15% or less, and even more preferably 10% or less. The method for measuring the average bubble diameter of the expanded beads and its coefficient of variation will be described in the examples.
[0065] The average bubble thickness of the expanded beads is preferably 1 μm or more and 8 μm or less, and the coefficient of variation of the bubble thickness is preferably 35% or less. This means that the thickness of the bubble membrane of the expanded beads is relatively uniform. In this case, it is considered that the closed cell ratio is likely to be maintained high even after compression, and as a result, the effect of the recovery property and rigidity being well-balanced and excellent even at a high bulk ratio is remarkable. Such expanded beads can be obtained, for example, by using a styrene-based resin that exhibits the above-mentioned strain hardening property as the base resin. From the viewpoint of further remarkable effect of the recovery property and rigidity being well-balanced and excellent even at a high bulk ratio, the average bubble thickness of the expanded beads is more preferably 2 μm or more and 5 μm or less. From the same viewpoint, the coefficient of variation of the bubble thickness is more preferably 30% or less, and even more preferably 28% or less.
[0066] The average particle diameter of the foamed particles is preferably 3 to 10 mm. In this case, in the application of filling the bead cushion material, the effect that the feel during use is good can be obtained, and in the application of the molded body, the filling property into the mold during in-mold molding is improved. From the same viewpoint, the average particle diameter of the foamed particles is more preferably 3 to 6 mm. The average particle diameter of the foamed particles can be determined in the same manner as the average particle diameter of the above-mentioned expandable resin particles.
[0067] <THF insoluble content> The tetrahydrofuran (that is, THF) insoluble content of the foamed particles is preferably 0.1% by mass or less (including 0). Such foamed particles are realized, for example, by not containing components derived from polyfunctional monomers in the polymer chain of the styrene-based resin. That is, even though the styrene-based resin has a high molecular weight and many long-chain branches, by not containing components derived from polyfunctional monomers in the polymer chain, the THF insoluble content can be made 0.1% by mass or less (including 0). Since the styrene-based resin has many branched chains and the THF insoluble content is 0.1% by mass or less (including 0), the styrene-based resin is likely to exhibit strain hardening properties. Also, it is considered that the expandability is further enhanced. From the same viewpoint, the proportion of the THF insoluble content in the styrene-based resin is preferably 0.05% by mass or less (including 0), and more preferably 0.01% by mass or less (including 0). The measurement method of the THF insoluble content will be described in the examples.
[0068] From the viewpoint of enhancing the in-mold moldability of the foamed particles under conditions of low molding pressure, the foamed particles preferably contain a plasticizer. The plasticizers that can be used are as described above. From the viewpoint of further improving the in-mold moldability, the foamed particles more preferably contain an alicyclic hydrocarbon such as cyclohexane as the plasticizer. From the viewpoint of further improving the in-mold moldability, the content of the plasticizer in the foamed particles is preferably 0.2 parts by mass or more and 3 parts by mass or less, and more preferably 0.5 parts by mass or more and 2 parts by mass or less with respect to 100 parts by mass of the styrene-based resin.
[0069] Conventionally, it has been considered that a styrene resin having a large molecular weight, for example, a weight average molecular weight Mw' within the above range, has low expandability, and it is difficult to obtain expanded beads with a desired expansion ratio. On the other hand, the expanded beads described above have a high bulk ratio, even though the base resin is a styrene resin having a large molecular weight. This is considered to be because the ratio Mz' / Mn' of the Z average molecular weight Mz' to the number average molecular weight Mn' of the styrene resin is a predetermined value or more, and the branching degree per 1000 styrene units is a predetermined value or more, so that the molecular weight distribution is wide, the number of branching points is large, and the branching points are appropriately spaced apart, resulting in an increased expandability even with the above-mentioned high molecular weight. Another reason is thought to be the low amount of tetrahydrofuran (i.e., THF) insoluble matter in the expanded beads.
[0070] [Foamed bead molding] The expanded bead molding is produced by molding styrene resin expanded beads in a mold. The molding is formed by fusing a large number of expanded beads to each other. The molding is obtained by molding the expanded beads in a mold. The molded body uses expanded beads composed of a styrene resin having the above-mentioned predetermined branched structure as the expanded beads constituting the molding, and has excellent restoring properties and rigidity even when the molding magnification is high. Furthermore, the molded body can increase the closed cell ratio even when the molding magnification is high, and the closed cell ratio is likely to be maintained high even after compression, and has high restoring properties.
[0071] The molding magnification of the expanded bead molding is preferably 30 times or more and 150 times or less. The expanded bead molding made of the above styrene-based resin has excellent restoring property and rigidity even at a high bulk magnification of 30 times or more and 150 times or less. From the viewpoint of making this effect prominent, the molding magnification is preferably 50 times or more, and more preferably 80 times or more. From the viewpoint of more reliably exhibiting the restoring property and rigidity of the molding, the molding magnification is preferably 120 times or less. The method for measuring the molding magnification will be described in the examples.
[0072] The closed cell ratio of the molded body is preferably 85% or more. In this case, the effect of having a well-balanced and excellent recovery property and rigidity even at a high bulk ratio is remarkable. From the viewpoint of making this effect more remarkable, the closed cell ratio of the molded body is more preferably 86% or more, and even more preferably 88% or more. In particular, when the bulk ratio is 30 times or more and 150 times or less, or 80 times or more and 150 times or less, and the closed cell ratio is within the above range, the above effect is even more remarkable. The method for measuring the closed cell ratio of the molded body will be described in the examples.
[0073] The restoring property of the molded body is evaluated by the compression set. Usually, the higher the molded body magnification, the more the restoring property is likely to decrease, and the compression set is large. When the molded body magnification is the same, the molded body with a smaller compression set is judged to have better restoring property. The compression set of the molded body is preferably 15% or less, more preferably 12% or less. Even when the molded body magnification is high, the molded body has excellent restoring property, and the compression set can be set within the above range. The compression set is measured by applying 25% strain in a compression test according to JIS K7220:2006. A specific method for measuring the compression set will be described in the examples.
[0074] The molded article is likely to exhibit a high closed cell ratio even after a load is applied by compression. Specifically, the original closed cell ratio is likely to be maintained in the molded article after the compression test in the measurement of 50% deformation compressive stress described later. This is considered to result in the molded article having a small compression permanent set and excellent restoring properties even at a high magnification. From the viewpoint of further improving the restoring properties of the molded article, the closed cell ratio of the molded article after the compression test is preferably 80% or more, more preferably 82% or more, and even more preferably 84% or more. The method for measuring the closed cell ratio of the molded article after the compression test will be described in the Examples.
[0075] The ratio [C1 / C0] of the closed cell percentage C1 of the molded body after the compression test to the closed cell percentage C0 of the molded body before the compression test (i.e., the closed cell percentage of the molded body) is preferably 0.90 or more, more preferably 0.92 or more, and even more preferably 0.94 or more. The upper limit of the ratio [C1 / C0] is 1. Similarly, the difference [C0-C1] between the closed cell percentage C0 of the molded body before the compression test and the closed cell percentage C1 of the molded body after the sag test is preferably 8% or less, more preferably 6% or less, and even more preferably 5% or less. The lower limit of the difference [C0-C1] is 0. In these cases, the effect of achieving a well-balanced and excellent recovery property and rigidity even at a high magnification is remarkable.
[0076] The fusion rate of the molded article is preferably 60% or more. In this case, the expanded beads constituting the molded article are sufficiently fused to each other, and the desired mechanical properties can be exhibited. From this viewpoint, the fusion rate of the molded article is more preferably 80% or more, and even more preferably 85% or more. By molding in a mold using the expanded beads, the fusion rate can be kept within the above range even when the molded article has a high magnification. The method for measuring the fusion rate of the molded article will be described in the examples.
[0077] [Method of manufacturing styrene-based resin] The styrene-based resin constituting the expanded beads is produced, for example, by carrying out a dispersion step, an impregnation step, a polymerization initiation step, and an additional impregnation polymerization step.
[0078] [Dispersion process] In the dispersion step, the styrene-based resin core particles are dispersed in an aqueous medium. The styrene-based resin core particles are hereinafter referred to as "core particles" as appropriate. The method for dispersing the core particles in an aqueous medium is not particularly limited, and for example, a suspending agent and a surfactant can be added to the aqueous medium together with the core particles and mixed. The dispersion step can be carried out, for example, in a closed container such as an autoclave.
[0079] (nuclear particle) The core particle contains a styrene-based resin. The styrene-based resin in the core particle usually has a linear polymer chain, but may contain a branched chain. The core particle may contain a resin other than the styrene-based resin, but the content of the styrene-based resin in the core particle is preferably 70% by mass or more, more preferably 85% by mass or more, and even more preferably 90% by mass or more, and it is particularly preferable that the substantial resin component is a styrene-based resin.
[0080] The average particle diameter of the core particles is preferably 0.3 to 1.2 mm. When the average particle diameter of the core particles is 0.3 mm or more, the amount of fine particles generated in the hyperbranched styrene-based resin can be reduced. When the average particle diameter of the core particles is 1.2 mm or less, the specific surface area of the core particles is increased, and the impregnation of the core particles with the styrene-based monomer is improved. The average particle diameter of the core particles is more preferably 0.3 to 1.0 mm, and further preferably 0.3 to 0.5 mm.
[0081] (aqueous medium) As the aqueous medium, water such as deionized water can usually be used. The aqueous medium may contain a water-soluble organic solvent such as alcohol, so long as the core particles are not dissolved therein.
[0082] (Surfactant) Examples of the surfactant include anionic surfactants, cationic surfactants, amphoteric surfactants, and nonionic surfactants. Among these, the surfactant preferably has at least one selected from the group consisting of anionic surfactants, cationic surfactants, and nonionic surfactants. Specific examples include alkyl sulfonates (e.g., sodium dodecyl sulfonate), alkyl benzene sulfonates (e.g., sodium dodecyl benzene sulfonate), polyoxyalkyl ether phosphates, alkyl dimethyl ethyl ammonium ethyl sulfates, higher alcohols, glycerin fatty acid esters, sorbitan fatty acid esters, polyoxyethylene alkyl ethers, and fatty acid salts. One type of surfactant may be used, or two or more types may be used.
[0083] (electrolyte) In the dispersion step, an electrolyte may be added to the aqueous medium together with the surfactant. Examples of the electrolyte that may be used include lithium chloride, potassium chloride, sodium chloride, sodium sulfate, sodium nitrate, sodium carbonate, sodium bicarbonate, sodium acetate, and sodium succinate.
[0084] (Suspension) Examples of the suspending agent include hydrophilic polymers such as polyvinyl alcohol, methyl cellulose, and polyvinylpyrrolidone; and poorly water-soluble inorganic salts such as calcium triphosphate, magnesium nitrate, magnesium pyrophosphate, hydroxyapatite, aluminum oxide, talc, kaolin, and bentonite. One or more types of suspending agents may be used. Either one or both of the hydrophilic polymer and the poorly water-soluble inorganic salt may be used. When a poorly water-soluble inorganic salt is used as a suspending agent, it is preferable to use an anionic surfactant such as sodium alkylsulfonate or sodium alkylbenzenesulfonate in combination.
[0085] The amount of the suspending agent used is preferably 0.01 to 5 parts by mass relative to 100 parts by mass of the total amount of the core particles and the styrene-based monomer added. When a suspending agent made of a poorly water-soluble inorganic salt is used in combination with an anionic surfactant, it is preferable to use 0.05 to 3 parts by mass of the suspending agent and 0.0001 to 0.5 parts by mass of the anionic surfactant relative to 100 parts by mass of the total amount of the core particles and the styrene-based monomer added.
[0086] [Impregnation process] In the impregnation step, a styrene-based monomer and a polymerization initiator are added to the aqueous medium after the dispersion step, and the core particles are impregnated with the styrene-based monomer and the polymerization initiator at a temperature at which the polymerization of the styrene-based monomer does not substantially proceed. By impregnating the core particles with the polymerization initiator together with the styrene-based monomer, the core particles can be sufficiently impregnated with the polymerization initiator. In addition to the core particles, the aqueous medium after the dispersion step contains a suspending agent and a surfactant, which are added as necessary. The polymerization initiator is, for example, an organic peroxide, and preferably contains at least an organic peroxide. The temperature at which the polymerization of the styrene-based monomer does not substantially proceed is a temperature at which the polymerization initiator (specifically, the organic peroxide) does not substantially decompose.
[0087] From the viewpoint of suppressing the decomposition of the polymerization initiator, the temperature of the aqueous medium in the impregnation process is set to (T 1 / 2 -15)℃ or less, and (T 1 / 2 It is more preferable to set the temperature at −18° C. or lower. 1 / 2 is the 10-hour half-life temperature (unit: °C) of the polymerization initiator. On the other hand, from the viewpoint of preventing a decrease in the impregnation of the styrene-based monomer into the core particles, the temperature of the aqueous medium in the impregnation step is preferably 70°C or higher, and more preferably 75°C or higher. The temperature of the aqueous medium in the impregnation step may be constant or may be changed, for example by gradually increasing, but is preferably within the above range.
[0088] The time for the impregnation step is preferably 0.5 to 2.0 hours, and more preferably 1.0 to 2.0 hours, from the viewpoint of sufficiently impregnating the core particles with the styrene-based monomer and the polymerization initiator.
[0089] If the amount of the styrene-based monomer added is too small, the core particles may not be sufficiently plasticized, and the polymerization initiator may not be sufficiently impregnated into the core particles. On the other hand, if the amount of the styrene-based monomer added is too large, the styrene-based monomer may polymerize outside the core particles, which may easily generate fine particles. Therefore, the amount of the styrene-based monomer added in the impregnation step is preferably 10 to 200 parts by mass relative to 100 parts by mass of the core particles. From the viewpoint of further improving the impregnation property, the amount of the styrene-based monomer added is more preferably 20 parts by mass or more, and even more preferably 30 parts by mass or more, relative to 100 parts by mass of the core particles. From the viewpoint of further preventing the generation of fine particles, the amount of the styrene-based monomer added is more preferably 100 parts by mass or less, and even more preferably 60 parts by mass or less, relative to 100 parts by mass of the core particles.
[0090] (Polymerization initiator) As the polymerization initiator, at least an organic peroxide is usually used, and a polymerization initiator other than the organic peroxide may be used in combination.
[0091] Examples of organic peroxides include benzoyl peroxide, dilauroyl peroxide, t-butylperoxy-2-ethylhexanoate, t-butylperoxyisobutyrate, t-hexylperoxy-2-ethylhexanoate, t-amylperoxy-2-ethylhexanoate, 1-cyclohexyl-1-methylethylperoxy-2-ethylhexanoate, 1,1,3,3-tetramethylbutylperoxy-2-ethylhexanoate, 2,5-dimethyl-2,5-bis-(2-ethylhexanoylperoxy)hexane, t-butylperoxyisopropyl monocarbonate, t-butylperoxy-2-ethylhexyl monocarbonate, t-butylperoxybenzoate, t-amylperoxyisopropyl carbonate, Examples of the organic peroxide include t-amylperoxy-2-ethylhexyl carbonate, t-hexylperoxy isopropyl carbonate, t-butylperoxy-3,5,5-trimethylhexanoate, 1,1-bis(t-butylperoxy)-3,3,5-trimethylcyclohexane, 1,1-bis(t-butylperoxy)-2-methylcyclohexane, 1,1-bis(t-butylperoxy)cyclohexane, 1,1-bis(t-butylperoxy)cyclododecane, 2,2-bis(t-butylperoxy)butane, 1,1-bis(t-hexylperoxy)-3,3,5-trimethylcyclohexane, 1,1-bis(t-hexylperoxy)cyclohexane, and 2,2-bis(4,4-di-t-butylperoxycyclohexyl)propane. These organic peroxides may be used alone or in combination of two or more.
[0092] 10-hour half-life temperature T of the polymerization initiator 1 / 2 The temperature is preferably 85 to 120° C., and more preferably 90 to 110° C. When two or more kinds of organic peroxides are used as the polymerization initiator, the 10-hour half-life temperature of the organic peroxide having the lowest 10-hour half-life temperature is set as T 1 / 2The organic peroxide is preferably one whose 10-hour half-life temperature falls within the above range and has a high hydrogen abstraction ability. Examples of such organic peroxides include organic peroxides that generate t-butoxy radicals, such as t-butylperoxyisopropyl monocarbonate, t-butylperoxy-2-ethylhexyl monocarbonate, and t-butylperoxybenzoate; and organic peroxides that generate cumyloxy radicals, such as dicumyl peroxide.
[0093] The polymerization initiator may contain a polymerization initiator other than an organic peroxide. From the viewpoint of facilitating a hydrogen abstraction reaction, however, the polymerization initiator preferably contains 70% by mass or more of an organic peroxide, preferably contains 85% by mass or more of an organic peroxide, and more preferably consists of an organic peroxide.
[0094] The amount of the polymerization initiator added is preferably 0.1 to 2.0 parts by mass relative to 100 parts by mass of the total amount of the core particles and the styrene-based monomer added. This range makes it easier to cause the hydrogen abstraction reaction without excessively decreasing productivity. From the viewpoint of further enhancing this effect, the amount of the polymerization initiator added is more preferably 0.2 to 1.5 parts by mass relative to 100 parts by mass of the total amount of the core particles and the styrene-based monomer added.
[0095] (Oxygen concentration in aqueous medium) The oxygen concentration of the aqueous medium at a temperature of 30°C is preferably 4 mg / L or more. Oxygen in the aqueous medium functions as a polymerization inhibitor in the aqueous medium and inhibits the generation of fine particles. Therefore, the higher the oxygen concentration in the aqueous medium, the higher the yield of the styrene-based resin. From the viewpoint of further suppressing the generation of fine particles, the oxygen concentration at a temperature of 30°C is more preferably 5 mg / L or more. In addition, the generation of fine particles can also be suppressed by adding 30 to 200 mass ppm of a water-soluble polymerization inhibitor such as sodium nitrite to the aqueous medium.
[0096] [Polymerization initiation step] In the polymerization initiation step, the aqueous medium after the impregnation step is heated to initiate polymerization of the styrene monomer in the styrene resin core particles. Core particles impregnated with a polymerization initiator and a styrene monomer are dispersed in the aqueous medium after the impregnation step. Polymerization of the styrene monomer is initiated by raising the temperature of the aqueous medium in the polymerization initiation step.
[0097] Specifically, it is preferable to raise the temperature to a temperature at which the polymerization initiator (specifically, the organic peroxide) is substantially decomposed, thereby initiating the polymerization of the styrene-based monomer. From the viewpoint of productivity, the temperature of the aqueous medium is set to (T 1 / 2 -10)℃ or higher, and (T 1 / 2 It is more preferable to set the temperature at -5°C or higher. The time for heating up to the above temperature (i.e., polymerization initiation temperature) is not particularly limited, but it is preferably 3 hours or more, more preferably 5 hours or more, from the viewpoint that the polymerization of the styrene-based monomer in the core particles proceeds during the heating and the content of the styrene-based monomer in the core particles can be easily controlled to 10 mass% or less in the additional impregnation polymerization step described below. On the other hand, it is preferable to set the time within 10 hours from the viewpoint of productivity.
[0098] [Additional impregnation polymerization step] In the additional impregnation polymerization step, a styrene-based monomer is additionally added to the aqueous medium after the polymerization initiation step. Then, while the core particles are impregnated with the styrene-based monomer, the styrene-based monomer in the core particles is graft-polymerized to the polymer chain of the styrene-based resin. That is, in the additional impregnation polymerization step, the styrene-based monomer is additionally added to the aqueous medium containing the core particles in which the polymerization of the styrene-based monomer has started after the polymerization initiation step, and the core particles are impregnated with the styrene-based monomer and polymerized.
[0099] If the amount of the styrene monomer added in the additional impregnation polymerization step is too small, branched chains may not be generated sufficiently. On the other hand, if the amount is too large, polymerization between the styrene monomers outside the core particles may occur easily, and the yield of the styrene resin may decrease. Therefore, the amount of the styrene monomer added in the additional impregnation polymerization step is preferably 50 to 700 parts by mass relative to 100 parts by mass of the core particles. From the viewpoint of generating branched chains more sufficiently, the amount of the styrene monomer added to 100 parts by mass of the core particles is more preferably 100 parts by mass or more, and even more preferably 200 parts by mass or more. From the viewpoint of increasing the yield of the styrene resin, the amount of the styrene monomer added to 100 parts by mass of the core particles is more preferably 600 parts by mass or less, and even more preferably 550 parts by mass or less.
[0100] In the additional impregnation polymerization step, it is preferable to maintain the content (specifically, concentration) of the styrene monomer in the core particles at 10% by mass or less. In other words, it is preferable to maintain the polymerization rate at 90% or more. The styrene monomer can be added intermittently or continuously. By passing through the polymerization initiation step, the polymerization of the styrene monomer is initiated in the core particles as a reaction field. In the additional impregnation polymerization step, by maintaining the content of the styrene monomer in the core particles at 10% by mass or less, not only the polymerization between the styrene monomers themselves but also the hydrogen abstraction reaction is likely to occur, and the graft polymerization of the styrene monomer to the styrene resin (i.e., polymer) is likely to occur, and branched chains are likely to be generated. From the viewpoint of further increasing the degree of long chain branching, the content of the styrene monomer in the core particles in the additional impregnation polymerization step is more preferably 8% by mass or less, and even more preferably 6% by mass or less.
[0101] In the additional impregnation polymerization step, it is preferable to maintain the content of the styrene monomer in the core particles at 10% by mass or less as described above, but the content of the styrene monomer in the core particles can exceed 10% by mass within the range in which the above-mentioned styrene resin is obtained. The time during which the content of the styrene monomer in the core particles exceeds 10% by mass is preferably 20% or less, more preferably 10% or less, of the total time of the additional impregnation polymerization step. It is most preferable to keep the content of the styrene monomer in the core particles at 10% by mass or less throughout the entire additional impregnation polymerization step. From the viewpoint of sufficient growth of the branched chains, the time of the additional impregnation polymerization step is preferably 150 minutes or more, more preferably 180 minutes or more. From the viewpoint of production efficiency, the upper limit of the time of the additional impregnation polymerization step is preferably about 600 minutes.
[0102] The content of the styrene monomer in the core particles in the additional impregnation polymerization step can be calculated based on the chemical properties of the polymerization initiator used in the polymerization, the polymerization rate of styrene calculated from the polymerization temperature, etc., and the content of the styrene monomer in the core particles in the additional impregnation polymerization step can be adjusted by adjusting the timing and addition rate (addition rate) of the additional addition of the styrene monomer so as to obtain a desired content based on the calculated value. The content of the styrene monomer in the actual core particles can be obtained by extracting the core particles during polymerization from the reaction system and using the method described below.
[0103] It is believed that the lower the content of the styrene monomer in the core particles, the easier it is for not only the polymerization initiation reaction but also the hydrogen abstraction reaction to occur, and the degree of branching is improved. Furthermore, as mentioned above, by setting the average particle size of the core particles to 1.2 mm or less, the specific surface area is increased, the impregnation of the styrene monomer is improved, and branching is more easily generated.
[0104] (Chain transfer agent) In the additional impregnation polymerization step, it is preferable to polymerize the styrene monomer in the presence of a chain transfer agent. In this case, it becomes easier to obtain a styrene resin having a weight average molecular weight Mw' of 1 million to 5 million, a ratio Mz' / Mn' of the Z average molecular weight Mz' to the number average molecular weight Mn' of 5 or more, and a branching degree of 0.2 or more per 1000 units of styrene, and in particular, it becomes easier to obtain a styrene resin having a weight average molecular weight Mw' of 1 million to 5 million, a ratio Mz' / Mn' of the Z average molecular weight Mz' to the number average molecular weight Mn' of 7 or more, and a branching degree of 0.2 or more per 1000 units of styrene. The chain transfer agent is a molecule that causes a chain transfer reaction of radical reactive molecules such as the growing end radical of the polymer chain, the radical on the polymer chain, the styrene monomer radical, and the initiator radical in the reaction field during polymerization. Examples of the chain transfer agent that can be used include α-methylstyrene dimer (hereinafter, appropriately referred to as "αMSD"), n-octyl mercaptan, t-nonyl mercaptan, n-dodecyl mercaptan, t-dodecyl mercaptan, phenylthiol, cyclohexanethiol, 4,4'-thiobisbenzenethiol, trimethylolpropane tris(3-mercaptopropionate), pentaerythritol tetrakis(3-mercaptopropionate), 4-methylbenzenethiol, 3-mercaptopropionate isooctyl, 1,8-dimercapto-3,6-dioxaoctane, bromotrichloromethane, carbon tetrachloride, 1,4-naphthoquinone, 2,4-diphenyl-4-methyl-1-pentene, and pentaphenylethane. It is preferable to use α-methylstyrene dimer because it is possible to obtain a styrene-based resin that has little odor and is not colored.
[0105] In the case where a chain transfer agent is added, the chain transfer agent may be present together with the styrene-based monomer in the additional impregnation polymerization step. i The total amount of chain transfer agent added to t The ratio of (i.e., M t / M i If M is too small, the molecular weight distribution may become narrow. t / M iIf M is too large, the weight average molecular weight Mw' may become small or the degree of branching may become small, and as a result, strain hardening may become difficult to exhibit. t / M i It is preferable to adjust M to 0.1 to 0.6. From the viewpoint of further increasing the strain hardening property of the styrene-based resin, t / M i is more preferably 0.12 or more, and even more preferably 0.15 or more. t / M i is preferably 0.5 or less, and more preferably 0.4 or less.
[0106] Examples of the method of adding the chain transfer agent include the following (I) to (IV). The methods (I) to (IV) may be any one of the methods or a combination of a plurality of methods. In other words, the chain transfer agent can be added by at least one of the methods (I) to (IV). (I) A method in which a chain transfer agent is incorporated into core particles before the dispersion step. (II) A method in which the core particles are impregnated with a chain transfer agent in the impregnation step. (III) A method in which core particles are impregnated with a chain transfer agent in the polymerization initiation step. (IV) A method in which the core particles are impregnated with a chain transfer agent in an additional impregnation polymerization step.
[0107] In the case of (I), a chain transfer agent can be contained in the core particles before adding to the aqueous medium. Specifically, a styrene-based resin and a chain transfer agent are mixed, and the core particles are produced by granulation. This results in styrene-based resin core particles containing the chain transfer agent.
[0108] In the case of (II), the core particles can be impregnated with a chain transfer agent in the impregnation step. The chain transfer agent can be impregnated into the core particles by adding it to the aqueous medium in the impregnation step. The chain transfer agent may be added to the aqueous medium at the same timing as the styrene monomer and the polymerization initiator, or may be added at a different timing. It is preferable that the chain transfer agent is added to the aqueous medium together with the styrene monomer and the polymerization initiator. In this case, the chain transfer agent is sufficiently dispersed in the core particles together with the styrene monomer and the polymerization initiator in the impregnation step. Therefore, in the polymerization initiation step and the additional impregnation polymerization step, it is possible to achieve both the suppression of side reactions such as the cleavage reaction of the polymer chain and the hydrogen abstraction reaction of the polymer chain, and the long chain branching degree of the styrene resin can be sufficiently increased.
[0109] In the case of (III), the core particles can be impregnated with a chain transfer agent in the polymerization initiation step. The chain transfer agent can be added during or after the temperature increase.
[0110] In the case of (IV), the core particles can be impregnated with a chain transfer agent in the additional impregnation polymerization step. Specifically, after the polymerization initiation step, the core particles can be impregnated with the chain transfer agent while the content of the styrene monomer in the core particles is set to 10 mass% or less while additionally adding a styrene monomer to the aqueous medium. The timing of adding the chain transfer agent may be such that the chain transfer agent is added all at once at the beginning of the additional impregnation polymerization step, or may be added at a predetermined addition rate, for example. The addition rate may also be changed, for example, by gradually decreasing it. When the chain transfer agent is added in the additional impregnation polymerization step, it is preferable to add the styrene monomer and the chain transfer agent in a mixed state.
[0111] When a chain transfer agent is used, it is preferable to impregnate the core particles with the chain transfer agent in the impregnation step as in (II) among (I) to (IV). In this case, the chain transfer agent can be present near the polymerization initiator in the core particles before the polymerization initiation step, so that a part of the highly reactive radicals generated in the polymerization initiation step or the additional impregnation polymerization step can be replaced with radicals with moderately low reactivity by a chain transfer reaction before side reactions such as polymer chain cleavage reactions occur. As a result, a branched styrene-based resin having a wider molecular weight distribution, a higher degree of branching, and a high level of melt tension and high fluidity can be obtained. This allows the styrene-based resin to fully express strain hardening properties, and the effect of the expanded beads having both resilience and rigidity at a high bulk ratio is remarkable.
[0112] (Temperature conditions) The temperature condition of the additional impregnation polymerization step is not particularly limited. From the viewpoint of facilitating the hydrogen abstraction reaction, the temperature of the aqueous medium in the additional impregnation polymerization step is set to (T 1 / 2 -10)℃~(T 1 / 2 +20)°C, and (T 1 / 2 -5)℃~(T 1 / 2 +10)° C. The temperature of the aqueous medium in the additional impregnation polymerization step may be constant or may be gradually increased or otherwise changed so long as it is within the above range.
[0113] In addition, the 10-hour half-life temperature T 1 / 2 The temperature of the aqueous medium in the impregnation step is 85 to 120°C, and the temperature of the aqueous medium in the impregnation step is 70°C or higher (T 1 / 2 -15) ° C. or less, and the temperature of the aqueous medium in the additional impregnation polymerization step is (T 1 / 2 -10)℃ or more (T 1 / 2 +20)° C. or lower. In this case, the core particles can be sufficiently impregnated with the styrene monomer, the initiator, and the chain transfer agent in the impregnation step before substantially starting the polymerization, and the polymerization initiation reaction and the hydrogen abstraction reaction can occur in the additional impregnation polymerization step.
[0114] In the above-mentioned additional impregnation polymerization step, it is preferable to maintain the concentration of the styrene monomer in the core particle, which is the polymerization reaction field, within a specific range, and polymerize the styrene monomer in the presence of a chain transfer agent. Furthermore, it is preferable to adjust the ratio of the total amount of the chain transfer agent to the total amount of the polymerization initiator to within a predetermined range. This makes it possible to increase the number of branching points of the styrene resin to increase the branching degree, and to increase the molecular weight of the styrene resin. In addition, it is possible to avoid gelation by widening the distance between the branching points to increase the long chain branching degree, and it is also possible to increase the fluidity, which is believed to make it easier to develop strain hardening properties.
[0115] Usually, in the reaction field during polymerization of styrene-based monomers, a polymerization initiator and many styrene-based monomers are present, and the initiator radicals generated from the polymerization initiator and the growing end radicals of the polymer chain preferentially react with the vinyl groups of the styrene-based monomers, so that it is considered that a linear styrene-based resin is easily formed. On the other hand, when the concentration of the styrene-based monomer in the reaction field is low as in the above-mentioned additional impregnation polymerization process, the polymer chains become relatively more numerous, so that it is considered that the initiator radicals and the growing end radicals of the polymer chains tend to cause not only polymerization reactions with the styrene-based monomers but also hydrogen abstraction reactions of the polymer chains. As a result, it is considered that radicals are generated on the polymer chains by the hydrogen abstraction reaction, and the styrene-based monomers are graft-polymerized to the radicals on the polymer chains, or the growing end radicals of the polymer chains are recombined, so that branched chains are generated in the polymer chains.
[0116] Since the position where the branched chain is generated in the polymer chain is in a sterically crowded state, it is considered that further branched chains are unlikely to be generated near the generated branch point. In other words, it is considered that a hydrogen abstraction reaction occurs again on the polymer chain that is distant from the branch point to such an extent that no steric hindrance occurs, and a branched chain is generated. Therefore, since the branched chain is generated while the branch points are appropriately separated, it is considered that a styrene-based resin having many branched chains can be obtained without gelation.
[0117] In order to generate many branched chains, it is necessary to increase the radical concentration in the polymerization system during the additional impregnation polymerization step to increase the frequency of hydrogen abstraction reactions on the polymer chains. However, if the concentration of highly reactive initiator radicals is increased by increasing the amount of initiator added or increasing the temperature in the additional impregnation polymerization step to promote decomposition of the initiator, undesirable side reactions such as polymer chain cleavage reactions are likely to occur, making it impossible to obtain a styrene-based resin having a desired branched structure.
[0118] On the other hand, in radical polymerization, a chain transfer agent is used to adjust the molecular weight of a polymer chain to a low value, and is not usually added to synthesize a polymer chain having a high molecular weight. However, by adjusting the ratio of the total amount of the chain transfer agent to the total amount of the polymerization initiator to be added within a predetermined range, a styrene-based resin having a high branching degree and a high molecular weight is produced without causing a decrease in molecular weight. The present inventors have found that the styrene-based resin thus obtained is more likely to satisfy the conditions that the weight average molecular weight Mw' is from 1 million to 5 million, the ratio Mz' / Mn' of the Z average molecular weight Mz' to the number average molecular weight Mn' is 5 or more, and the branching degree per 1000 styrene units is 0.2 or more, and more preferably that the weight average molecular weight Mw' is from 1 million to 5 million, the ratio Mz' / Mn' of the Z average molecular weight Mz' to the number average molecular weight Mn' is 7 or more, and the branching degree per 1000 styrene units is 0.2 or more, and that expanded beads composed of a styrene-based resin satisfying these conditions exhibit strain hardening during expansion and have both resilience and rigidity even at a high bulk ratio.
[0119] The reason why the ratio of the total amount of chain transfer agent added to the total amount of polymerization initiator added is adjusted within a predetermined range, the molecular weight is not reduced, and instead a styrene-based resin with a high degree of branching and a high molecular weight is produced is believed to be that when the concentration of the styrene-based monomer in the core particles is within a specific range, a part of highly reactive radicals such as initiator radicals is replaced by radicals with moderately low reactivity through chain transfer reaction, and while side reactions such as polymer chain cleavage reaction are suppressed, a styrene-based resin with a high degree of branching and a high molecular weight is produced by a hydrogen abstraction reaction of the polymer chain. When the total amount of chain transfer agent added to the total amount of polymerization initiator added is too small, it is believed that side reactions such as polymer chain cleavage reaction cannot be suppressed, and conversely, when the total amount of chain transfer agent added to the total amount of polymerization initiator added is too large, it is believed that the hydrogen abstraction reaction is difficult to occur, and in either case, it is difficult to obtain a styrene-based resin with a high degree of branching and a high molecular weight.
[0120] In addition, since a chain transfer agent originally produces a low molecular weight polymer, it is considered that a styrene-based resin with a low molecular weight is also produced by a part of the chain transfer agent that is not involved in the production of branched chains. As a result, a styrene-based resin with a high branching degree and a high molecular weight produced by a hydrogen abstraction reaction and a styrene-based resin with a low molecular weight produced by a chain transfer reaction are simultaneously produced, and it is considered that the molecular weight distribution of the resulting styrene-based resin is broadened. Such a styrene-based resin has many branched chains and is also long. The use of a chain transfer agent makes it easier to obtain a styrene-based resin that satisfies the conditions that the weight average molecular weight Mw' is 1 million or more and 5 million or less, the ratio Mz' / Mn' of the Z average molecular weight Mz' to the number average molecular weight Mn' is 5 or more, and the branching degree per 1000 units of styrene is 0.2 or more. However, even if a chain transfer agent is not used, it is possible to obtain a styrene-based resin that satisfies the above conditions, for example, by maintaining the content (specifically, the concentration) of the styrene monomer in the core particles in the additional impregnation polymerization step to 10 mass% or less as described above.
[0121] In the method for producing a styrene-based resin, it is possible to produce a styrene-based resin without necessarily using a polyfunctional monomer (i.e., a branching agent). That is, the above-mentioned styrene-based resin can be produced by using a polyfunctional monomer, by reducing the amount of the polyfunctional monomer used, for example, to substantially close to zero, or by not using a polyfunctional monomer. Reducing the amount of the polyfunctional monomer used or not using a polyfunctional monomer leads to further prevention of gelation and further improvement of fluidity. However, it is also possible to add a polyfunctional monomer as long as gelation does not occur during polymerization.
[0122] The amount of the polyfunctional monomer added in the aqueous medium is preferably 0.2 parts by mass or less, more preferably 0.1 parts by mass or less, and even more preferably 0, relative to 100 parts by mass of the core particles. When the polyfunctional monomer is added, it can be added in any step, for example, in the impregnation step, polymerization initiation step, additional impregnation polymerization step, etc.
[0123] The polyfunctional monomer is, for example, a monomer having two or more radically polymerizable double bonds, and examples of the polyfunctional monomer include divinylbenzene, trivinylbenzene, divinyltoluene, divinylnaphthalene, trimethylolpropane triacrylate, ethylene glycol diacrylate, propylene glycol diacrylate, 1,3-butylene diol diacrylate, hexanediol diacrylate, and cyclohexanediol diacrylate.
[0124] [Residual Monomer Polymerization Step] After the additional impregnation polymerization step, a residual monomer polymerization step can be carried out to polymerize the styrene monomer remaining in the styrene resin. The residual monomer polymerization step is a step that is carried out selectively.
[0125] [Other steps] After the additional impregnation polymerization step or the residual monomer polymerization step, the inside of the sealed container is cooled, and the styrene-based resin is taken out of the sealed container, to obtain, for example, a particulate styrene-based resin. Specifically, the particulate shape is exemplified by a spherical shape, an ellipsoid shape, etc., but also includes shapes similar to these in appearance. In addition, a washing step can be performed in which the suspending agent, surfactant, etc. attached to the styrene-based resin are washed with water. In addition, a coating step can be performed in which the surface of the styrene-based resin is coated with a functional component such as an antistatic agent. The washing step and the coating step are selectively performed.
[0126] [Production of expandable resin particles] The expandable resin particles are produced by impregnating the particulate styrene resin obtained as described above with a blowing agent. Specifically, for example, the particulate styrene resin is supplied into a closed container together with an aqueous medium and a suspending agent added as necessary, and dispersed in the aqueous medium, and the closed container is heated and the blowing agent is pressed in, so that the styrene resin particles can be impregnated with the blowing agent. When the blowing agent is impregnated, a plasticizer made of an alicyclic hydrocarbon such as cyclohexane may be impregnated together with the blowing agent. The type and amount of the blowing agent and plasticizer impregnated into the styrene resin particles are as described above. The styrene-based resin after the additional impregnation polymerization step or the residual monomer polymerization step may be impregnated with a blowing agent without being taken out of the sealed container.
[0127] A washing step can be carried out in which the suspending agent, surfactant, etc. adhering to the obtained expandable resin particles are washed off with water. Also, a coating step can be carried out in which the surface of the expandable resin particles is coated with a functional component such as an antistatic agent. The washing step and the coating step are steps that are selectively carried out.
[0128] [Production of foamed beads] The expanded beads are produced by heating and expanding the expandable resin beads with a heating medium. Specifically, for example, the expandable resin beads can be expanded by introducing a heating medium such as steam into a pre-expansion machine to which the expandable resin beads have been supplied.
[0129] [Production of foamed bead moldings] The expanded bead molding is produced by molding the expanded beads in a mold. Specifically, the expanded beads are filled into a molding die such as a metal mold, and a heating medium such as steam is supplied to fuse the expanded beads to each other, thereby obtaining an expanded bead molding having a desired shape. EXAMPLES
[0130] Next, the present invention will be described in more detail with reference to examples, but the present invention is not limited to these examples, and various modifications are possible without departing from the gist of the present invention. "Parts" and "%" are based on mass unless otherwise specified. The temperature inside the autoclave refers to the temperature of the aqueous medium.
[0131] [Production of nuclear particles] (Production Example 1) The internal volume of the container equipped with a stirrer is 1 m 3 Into the autoclave, 350 kg of deionized water, 2.1 kg of calcium phosphate tribasic (manufactured by Taihei Chemical Industry Co., Ltd., 20.5% slurry) as a suspending agent, 0.158 kg of sodium dodecylbenzenesulfonate (10% aqueous solution) as a surfactant, 0.053 kg of disodium dodecyldiphenylethersulfonate (manufactured by Kao Corporation, Pelex SSH 10% aqueous solution) as a surfactant, and 0.535 kg of sodium acetate as an electrolyte were added.
[0132] Next, 0.975 kg of t-butylperoxy-2-ethylhexanoate (manufactured by NOF Corporation, Perbutyl O) and 0.284 kg of t-butylperoxy-2-ethylhexyl monocarbonate (manufactured by NOF Corporation, Perbutyl E) as polymerization initiators and 15.4 g of 4-tert-butylcatechol as a polymerization inhibitor were dissolved in 390 kg of styrene, and this was fed into the autoclave while stirring at 110 rpm. After the gas phase in the autoclave was replaced with nitrogen, the temperature was raised to 90°C over 1 hour and 15 minutes.
[0133] After reaching 90°C, the temperature was increased to 100°C over 5 hours. After reaching 100°C, the stirring speed was changed to 90 rpm, and the temperature was increased to 115°C over 1 hour and 30 minutes. The mixture was kept at 115°C for 2 hours and 40 minutes, and then cooled to 40°C over 2 hours. During the temperature increase to 90°C, 1.95 g of potassium persulfate was added to the autoclave as a suspension aid when the temperature reached 60°C.
[0134] After cooling, the contents were removed, and the tribasic calcium phosphate adhering to the surface of the styrene-based resin particles was dissolved with nitric acid. The contents were then dehydrated and washed using a centrifuge, and the moisture adhering to the particle surface was removed using an airflow dryer to obtain styrene-based resin particles.
[0135] The obtained styrene resin particles were sieved to take out particles with a diameter of 0.5 to 1.3 mm (average particle diameter 0.8 mm). These were used as core particles. The average particle diameter d63 of the styrene resin particles was measured using a particle size distribution measuring device "Militrack JPA" manufactured by Nikkiso Co., Ltd.
[0136] Example 1 [Production of styrene-based resin particles] <Dispersion process> The internal volume is 1.5m and equipped with a stirrer. 3 450 kg of deionized water, 2.80 kg of sodium pyrophosphate, and 7.00 kg of magnesium nitrate were fed into the autoclave, and magnesium pyrophosphate was synthesized as a suspension agent in the autoclave by salt exchange. 0.140 kg of sodium alkylsulfonate (Kao Corporation, Latemul PS, 40% aqueous solution) was fed into the autoclave as a surfactant, and 70.0 kg of styrene-based resin particles (core particles) obtained in Production Example 1 were fed into the autoclave, and the gas phase in the autoclave was replaced with nitrogen. Specifically, the inside of the autoclave was pressurized to 0.3 MPa (G) with nitrogen, and then the gas in the autoclave was released until the pressure in the autoclave reached atmospheric pressure.
[0137] <Impregnation process> Next, the temperature was raised to 80° C. while stirring at 50 rpm. After reaching 80° C., the stirring speed was changed to 100 rpm, and 100 kg of deionized water, 0.180 kg of sodium alkylsulfonate (Kao Corporation, Latemul PS, 40% aqueous solution), 24.7 kg of styrene (styrene-based monomer), and t-butylperoxy-2-ethylhexyl monocarbonate (NOF Corporation, Perbutyl E;BE, 10-hour half-life temperature T 1 / 2 A mixture of 1.38 kg of styrene (99.0°C) and 0.20 kg of α-methylstyrene dimer (NOF Corporation, Nohumer MSD) as a chain transfer agent was prepared into an emulsion using a homogenizer, and the emulsion was fed into an autoclave. The autoclave was then pressurized with nitrogen to 0.1 MPa (G) and held at 80°C for 15 minutes.
[0138] <Polymerization initiation step> The contents were then heated to 105° C. over 1 hour while being stirred at 100 rpm.
[0139] <Additional impregnation polymerization process> After reaching 105°C, the contents were held for 7 hours and 30 minutes while stirring at 100 rpm. From the time when the temperature inside the autoclave reached 105°C, 316.6 kg of styrene (styrene monomer) was continuously added to the autoclave at a rate of 0.77 kg / min over a period of 7 hours and 30 minutes. In addition, when adding styrene, a simulation was performed based on the above-mentioned addition conditions, the chemical properties of the polymerization initiator used in the polymerization, and the polymerization rate of styrene calculated from the polymerization temperature, and styrene was additionally added so that the styrene content in the core particles during the addition of styrene was 10 mass% or less.
[0140] As a representative example of the simulation results, FIG. 8 shows a graph of the simulation results in Example 1. The graph has the elapsed time (hr) on the horizontal axis, the content (mass%) of the styrene-based monomer in the core particles in the additional impregnation polymerization step on the vertical axis on the left, and the polymerization temperature (°C) on the vertical axis on the right. In the graph, the change in the styrene content in the core particles with respect to the elapsed time is shown by a solid line, and the change in the polymerization temperature with respect to the elapsed time is shown by a dashed line. As exemplified in FIG. 8, the relationship between the elapsed time, the styrene-based monomer in the core particles, and the polymerization temperature can be derived from a simulation based on the polymerization rate calculated from the polymerization conditions. Based on this relationship, the addition of the styrene-based monomer (specifically, styrene) can be adjusted so that the content of the styrene-based monomer in the core particles is 10 mass% or less.
[0141] <Residual Monomer Polymerization Process> After the additional impregnation polymerization step, the aqueous medium was heated to 120°C over 2 hours while stirring the contents at 100 rpm, and then maintained at 120°C for 3 hours to polymerize the unreacted styrene monomer.
[0142] <Cooling process> After the residual monomer polymerization step, the aqueous medium was cooled to 35° C. over 6 hours while stirring the contents at 100 rpm. After cooling the inside of the autoclave, the styrene resin particles taken out of the autoclave were washed with dilute nitric acid to dissolve and remove the suspending agent attached to the resin particle surface, then washed with water and dehydrated by a centrifuge. After coating with 0.01 parts by mass of polyoxyethylene lauryl ether (value relative to 100 parts by mass of styrene resin) as an antistatic agent, the moisture on the resin particle surface was removed by an airflow dryer. In this way, styrene resin particles were produced.
[0143] [Production of expandable resin particles] Equipped with a stirrer, the internal volume is 0.05 m 318.33 kg of deionized water, 92 kg of sodium pyrophosphate, and 229 kg of magnesium nitrate were fed into the autoclave, and magnesium pyrophosphate was synthesized as a suspension agent in the autoclave by salt exchange. 4.6 g of sodium alkylsulfonate (Kao Corporation, Ramtel PS, 40% aqueous solution) as a surfactant and 16.67 kg of the above styrene-based resin particles were fed into the autoclave, and then the gas phase in the autoclave was replaced with nitrogen. Specifically, the inside of the autoclave was pressurized to 0.3 MPa (G) with nitrogen, and then the gas in the autoclave was released until the pressure in the autoclave reached atmospheric pressure.
[0144] The temperature was then increased to 100°C while stirring at 180 rpm. After reaching 100°C, the contents were held for 3 hours while stirring at 180 rpm, and then the temperature was increased to 120°C over 1 hour. After being held at 120°C for 6 hours, it was cooled to 35°C over 4 hours. After the temperature inside the autoclave reached 100°C, 330g of cyclohexane, 300g of pentane, and 1550g of isobutane were continuously added to the autoclave over a period of 45 minutes.
[0145] After cooling the inside of the autoclave, the styrene resin particles (specifically, expandable styrene resin particles) taken out from the autoclave were washed with dilute nitric acid to dissolve and remove the suspending agent attached to the resin particle surface, then washed with water and dehydrated by a centrifuge. Furthermore, the moisture on the resin particle surface was removed by an airflow dryer.
[0146] Next, a mixture of 0.14 parts by mass of zinc stearate, 0.05 parts by mass of glycerin monostearate, and 0.05 parts by mass of glycerin tristearate was added to 100 parts by mass of expandable resin particles and mixed. In this way, the expandable resin particles were coated with various additives. The physical properties of the expandable resin particles thus obtained were measured by the method described below. The results are shown in Table 1.
[0147] [Production of foamed beads] Next, the expandable resin particles were expanded to produce expanded particles. Specifically, the expandable resin particles were placed in a pre-expansion device (DAISEN "DYHL-500U"), and steam of 0.02 MPa (G) was supplied to heat the expandable resin particles. By heating, the expandable resin particles reached the bulk density shown in Table 2 (specifically, 10 kg / m 3 The expandable resin particles were expanded until the expansion ratio reached 1.0. The physical properties of the expanded particles were measured by the methods described below. The results are shown in Table 2.
[0148] [Production of foamed bead moldings] The expanded beads were left to stand at room temperature for 1 day to mature, and then filled into the cavity of the mold of a molding machine (DSM-0705VS manufactured by DABO). The mold cavity was a rectangular parallelepiped shape with a length of 350 mm, a width of 65 mm, and a thickness of 25 mm. Steam at a pressure of 0.08 MPa (G) was supplied into the cavity to heat the expanded beads for 10 seconds, and then cooled for a predetermined period of time. The expanded beads molding was then removed from the mold. In this way, an expanded beads molding was obtained. The obtained expanded beads molding was dried at a temperature of 40°C for 1 day and then used for various evaluations. The results are shown in Table 2.
[0149] Example 2 The steam pressure during the production of foamed beads was changed to 0.01 MPa (G) and the bulk density was 23 kg / m 3 The procedure was the same as in Example 1, except that the expanded beads were prepared as follows.
[0150] Example 3 The amount of t-butylperoxy-2-ethylhexyl monocarbonate added as a polymerization initiator was changed to 1.45 kg without using αMSD to produce expandable resin particles with a bulk density of 12 kg / m 3 The procedure was the same as in Example 1, except that the expanded beads were prepared as follows.
[0151] Example 4 The steam pressure during the production of foamed beads was changed to 0.01 MPa (G) to achieve a bulk density of 18 kg / m 3 The procedure was the same as in Example 3, except that the expanded beads were prepared as follows.
[0152] Example 5 After the production of the styrene resin particles, a step was added in which the styrene resin particles were melt-kneaded in a small twin-screw extruder manufactured by Technobel Co., Ltd. at 50 rpm and a resin temperature of 200°C to produce mini-pellets with a major axis of 1.4 mm. The mini-pellets were used as the styrene resin particles. Except for this point, a bulk density of 11 kg / m was obtained by the same method as in Example 1. 3 The foamed beads were prepared as follows.
[0153] Example 6 The bulk density was 10 kg / m by the same method as in Example 1, except that the polymerization initiator in the production of styrene-based resin particles was changed to 1.44 kg of t-butyl peroxybenzoate. 3 The foamed beads were prepared as follows.
[0154] Example 7 The same method as in Example 1 was used except that the steam pressure during the production of the expanded beads was changed to 0.025 MPa (G). 3 The foamed beads were prepared as follows.
[0155] Comparative Example 1 Comparative Example 1 is an example of expanded beads made of linear polystyrene. In this example, expandable resin particles were produced as follows. First, a 1.5 m 3Into the autoclave, 370 kg of deionized water, 1.53 kg of tribasic calcium phosphate (20.5% slurry), 0.13 kg of sodium α-olefin sulfonate (10% aqueous solution), 0.04 kg of disodium alkylbiphenyl disulfonate (10% aqueous solution), and 0.56 kg of sodium acetate (electrolyte) were placed. Next, 1.38 kg of benzoyl peroxide, 0.396 kg of t-butylperoxy-2-ethylhexyl monocarbonate ("Perbutyl E" manufactured by NOF Corporation), 0.396 kg of dicumyl peroxide ("Percumyl D" manufactured by NOF Corporation), 2.96 kg of liquid paraffin, 0.39 kg of polyethylene wax powder ("Polyethylene Wax 1000" manufactured by Toyo Adle Co., Ltd.), and 7.4 g of 4-t-butylcatechol ("DIC-TBC" manufactured by DIC Corporation, a polymerization inhibitor) were mixed with 370 kg of styrene, and the mixture was charged into an autoclave while stirring at a rotation speed of 110 rpm. Next, the air in the autoclave was replaced with nitrogen, and the temperature was raised to 90°C over 1.5 hours. After reaching the temperature of 90°C, the temperature in the autoclave was raised to 100°C over 5 hours. After that, the temperature in the autoclave was further raised to 112°C over 1 hour and 30 minutes, and the autoclave was kept at the temperature of 112 for 50 minutes. Then, the temperature was cooled to 35°C over about 6 hours. During the temperature rise from the above-mentioned temperature 90°C to the temperature 100°C, 4 hours after reaching 90°C, 11.5 kg of pentane (a mixture of 80% n-pentane and 20% isopentane) and 20.7 kg of isobutane were pressed into the autoclave over 60 minutes as a foaming agent. After cooling, the contents (expandable particles) were taken out of the autoclave, and nitric acid was added to the expandable particles in order to remove the tribasic calcium phosphate attached to the surface of the expandable particles, followed by dehydration with a centrifuge and removal of moisture attached to the surface with a fluidized bed dryer. In this way, expandable particles having an average particle size of about 1.0 mm were obtained. Next, the expandable particles were sieved to select and take out particles of 0.5 to 1.4 mm. Then, 0.005 parts by mass of N,N-bis(2-hydroxyethyl)alkylamine (antistatic agent) was added to 100 parts by mass of the expandable particles to coat the expandable particles with an antistatic agent. Furthermore, 0.1 parts by mass of zinc stearate, 0.002 parts by mass of glycerin tristearate, 0.017 parts by mass of glycerin distearate, and 0.05 parts by mass of glycerin monostearate were added to 100 parts by mass of the expandable particles to coat the expandable particles with the mixture. Except for these points, the bulk density was adjusted to 10 kg / m by the same method as in Example 1. 3 The foamed beads were prepared as follows.
[0156] Comparative Example 2 The steam pressure during the production of foamed beads was changed to 0.01 MPa (G) and the bulk density was 17 kg / m 3 The procedure was the same as in Comparative Example 1, except that the foamed beads were prepared as follows.
[0157] Comparative Example 3 The procedure was the same as in Example 1, except that the amounts of pentane and isobutane added during the production of expandable resin particles were changed to 150 g and 780 g, respectively, to produce expandable resin particles.
[0158] Comparative Example 4 The procedure was the same as in Example 1, except that the amounts of pentane and isobutane added during the production of expandable resin particles were changed to 300 g and 3100 g, respectively, to produce expandable resin particles.
[0159] Comparative Example 5 Styrenic resin particles were prepared using hyperbranched polystyrene "HP-555" manufactured by DIC Corporation. Specifically, the particles were melt-kneaded in a small twin-screw extruder manufactured by Technobel Corporation at 50 rpm and a resin temperature of 200°C to produce mini-pellets with a major axis of 1.4 mm. In this way, styrene-based resin particles were obtained. Next, expandable resin particles were prepared using the styrene-based resin particles, and the bulk density of the resin particles was increased to 13 kg / m by the same method as in Example 1. 3The foamed beads were prepared as follows.
[0160] Comparative Example 6 The steam pressure during the production of foamed beads was changed to 0.01 MPa (G) to a bulk density of 20 kg / m 3 The procedure was the same as in Comparative Example 5, except that the expanded beads were prepared as described above.
[0161] The examples and comparative examples were evaluated by the following methods. The results are shown in Tables 1 to 4. The expanded beads were evaluated after being left to stand for 24 hours at a relative humidity of 50%, a temperature of 23°C, and 1 atm to condition the beads, and the expanded bead molded bodies were evaluated after being left to stand for 12 hours at a temperature of 23°C to condition the molded bodies.
[0162] [Evaluation of expandable resin particles] [Absolute molecular weight (GPC-MALS)] The absolute molecular weight was measured for the styrene resin particles used in the preparation of the expandable resin particles. The absolute molecular weight was measured by measuring the number average molecular weight Mn', weight average molecular weight Mw', and Z average molecular weight Mz' of the styrene resin by the GPC-MALS method. Specifically, the measurements were performed using a Shimadzu Corporation Prominence LC-20AD (2HGE) / WS system and a Wyatt Technology Corporation multi-angle light scattering detector DAWN HELEOS II under the conditions of eluent: tetrahydrofuran (THF) and flow rate: 1.0 ml / min. As columns, one TSKgel HHR-H and two TSKgel GMHHR columns manufactured by Tosoh Corporation were connected in series. The measurements were analyzed using Wyatt's analysis software ASTRA, and the number average molecular weight Mn', weight average molecular weight Mw', and Z average molecular weight Mz' of the styrene resin were obtained. The analysis was performed using a value of 0.185 ml / g for the concentration increment dn / dc of the refractive index.
[0163] [Polystyrene equivalent molecular weight (GPC)] The relative molecular weight was measured for the styrene resin particles used in the preparation of the expandable resin particles. The relative molecular weight was measured by measuring the number average molecular weight (Mn), weight average molecular weight (Mw), and Z average molecular weight (Mz) of the styrene resin by gel permeation chromatography (GPC) using linear polystyrene as the standard substance. Specifically, the measurements were performed using Tosoh Corporation's HLC-8320GPC EcoSEC under the following conditions: eluent: tetrahydrofuran (THF), flow rate: 0.6 ml / min, and sample concentration: 0.1 wt%. As columns, one TSKguardcolumn SuperH-H and two TSK-GEL SuperHM-H were connected in series. That is, the styrene resin was dissolved in tetrahydrofuran (THF) and the molecular weight was measured by GPC. The measured values were then calibrated with standard polystyrene (linear) to determine the number average molecular weight Mn, weight average molecular weight Mw, and Z average molecular weight Mz of the styrene resin.
[0164] [Contraction factor, branching degree] The shrinkage factor and branching degree of the styrene resin particles used to prepare the expandable resin particles were measured. The ratio of the square of the radius of rotation (Rb) of the styrene resin to the square of the radius of rotation (Rl) of the linear styrene resin was defined as the shrinkage factor g, and the branching degree B m,w , branching degree B m,1000 In this analysis, the degree of branching was calculated assuming that the styrene resin had three branched chains. For linear polystyrene, data on the styrene resin obtained in the manufacturing example used as the core particles was used.
[0165] The production of styrene-based resin was started under the same conditions as in each of the examples and comparative examples, and the temperature of the reactor was cooled to 30°C within 10 minutes in each system at the start of the additional impregnation polymerization process, 3 hours after the start of the additional impregnation polymerization process, and at the end of the additional impregnation polymerization process, and the styrene-based resin particles being polymerized were taken out. Next, the styrene-based resin particles were dissolved in N,N-dimethylformamide (DMF). The amount of residual styrene in the styrene-based resin particles was quantified by gas chromatography (GC) for the dissolved matter, and the content of the styrene-based monomer in the core particles at the start of the additional impregnation polymerization process, 3 hours after the start of the additional impregnation polymerization process, and at the end of the additional impregnation polymerization process was confirmed. The quantification was performed by calibrating with a calibration curve. As a result, it was confirmed that the content of the styrene-based monomer in the core particles by simulation and the content of the styrene-based monomer in the core particles actually measured were consistent. In addition, the arithmetic average value of the content of the styrene-based monomer in the core particles at the start of the additional impregnation polymerization process, 3 hours after the start of the additional impregnation polymerization process, and at the end of the additional impregnation polymerization process was calculated.
[0166] The measurement conditions for gas chromatography are as follows. Equipment used: Shimadzu gas chromatograph GC-2014s Column packing: [Liquid phase name] DOP-B [Liquid phase impregnation rate] 30% by mass [Carrier particle size] 60 / 80 mesh [Carrier treatment method] AW-DMCS (water washing, calcination, acid treatment, silane treatment) Column material: Glass column with inner diameter of 3 mm and length of 4000 mm Carrier gas: N2 Detector: FID (Flame Ionization Detector) Quantitation: Internal standard method
[0167] [Physical foaming agent and plasticizer content in expandable resin particles] The contents of butane and pentane used as blowing agents, and cyclohexane used as a plasticizer were measured by the following method. 1 g of precisely weighed expandable resin particles was dissolved in 25 ml of N,N-dimethylformamide (DMF) to prepare a sample solution. This sample solution was used for measurement by gas chromatography (i.e., GC), and the contents of butane, pentane, and cyclohexane in the expandable resin particles were quantified. The contents of the blowing agents (specifically butane and pentane) and plasticizers (specifically cyclohexane) per 100 parts by mass of the resin component in the expandable resin particles were as shown in Tables 1 and 3. The measurement conditions for gas chromatography are as follows. Measurement equipment: Shimadzu Corporation gas chromatograph GC-2014s Column material: Glass column with inner diameter of 3 mm and length of 4000 mm Column packing: [Liquid phase name] DOP-B [Liquid phase impregnation rate] 30% by mass [Carrier particle size] 60 / 80 mesh [Carrier treatment method] AW-DMCS (water washing, calcination, acid treatment, silane treatment) Carrier gas: N2 Detector: FID (Flame Ionization Detector) Quantification method: internal standard method
[0168] [Evaluation of foam particles] [Physical foaming agent and plasticizer content in expanded beads] The contents of the physical blowing agent and the plasticizer in the expandable resin particles were measured in the same manner as described above, except that expanded particles were used as the measurement sample instead of the expandable resin particles. The contents of the blowing agent and plasticizer in the expanded beads are expressed as the amounts relative to 100 parts by mass of the styrene-based resin.
[0169] [Tetrahydrofuran insolubles (THF insolubles)] A 1 g sample was precisely weighed out from the expanded beads, 30 ml of tetrahydrofuran was added to the sample, and the sample was immersed at 23° C. for 24 hours, shaken for 5 hours, and allowed to stand. The supernatant was then removed by decantation, and 10 ml of tetrahydrofuran was added again, the sample was allowed to stand, the supernatant was removed by decantation, and the sample was dried at 23° C. for 24 hours. The weight after drying was measured, and the THF insoluble content was calculated using the following formula (9). THF insolubles (%) = [weight of insolubles after drying / weight of sample] × 100 (9)
[0170] [Closed cell ratio c0 of foamed beads] The closed cell ratio of the expanded beads was measured using an air comparison type specific gravity meter based on procedure C described in ASTM-D2856-70. Specifically, first, the bulk volume after conditioning was about 20 cm 3 The foamed particles were used as a measurement sample, and the apparent volume Va of the measurement sample was accurately measured by the ethanol immersion method as described below. After the measurement of the apparent volume, the measurement sample was thoroughly dried, and the true volume Vx of the measurement sample was measured using an air comparison type specific gravity meter 930 (manufactured by Toshiba Beckman Co., Ltd.) in accordance with procedure C described in ASTM-D2856-70.
[0171] Using the apparent volume Va and true volume Vx of the measurement sample thus obtained, the closed cell ratio (unit: %) of the measurement sample was calculated based on the following formula (10). The above operation was performed for each of the five measurement samples, and the arithmetic mean value of the closed cell ratios of the five measurement samples was taken as the closed cell ratio of the expanded beads. Closed cell ratio=(Vx-W / ρ)×100 / (Va-W / ρ) ···(10)
[0172] The symbols in formula (10) have the following meanings: Vx: The true volume of the measurement sample measured by the above method, i.e., the sum of the volume of the resin constituting the foamed beads and the total volume of the air bubbles in the closed cell part in the foamed beads (unit: cm 3 ) Va: The apparent volume of the sample measured by the rise in the water level when the sample is submerged in a measuring cylinder containing ethanol (unit: cm 3 ) W: Mass of the measurement sample (unit: g) ρ: Density of the resin that composes the foamed particles (unit: g / cm 3 )
[0173] [Bulk density of expanded particles] The foamed particles after the conditioning were placed in a graduated cylinder so that they would naturally pile up, and the bulk volume (unit: L) of the foamed particles was read from the graduations on the graduated cylinder. In this example, the bulk volume of the foamed particles in the graduated cylinder was set to 1 L. The mass (unit: g) of the foamed particles in the graduated cylinder was then divided by the bulk volume described above, and the unit was further converted to obtain the bulk density (unit: kg / m 3 ) was calculated.
[0174] [Bulk magnification] The bulk ratio (unit: times) of the expanded beads is determined by the density of the styrene resin that constitutes the expanded beads (specifically, 1000 kg / m 3 ) was divided by the bulk density.
[0175] [Settling rate] The settling rate is an index of the restoring property of expanded beads. When the bulk ratio of expanded beads is the same, expanded beads with a smaller settling rate are judged to have better restoring property. The settling rate was measured by the following settling test. Specifically, first, a container of a given volume (e.g., 78 mm in diameter) was filled with expanded beads up to a given position (e.g., a position with a volume of 330 mL). The volume of the expanded beads filled at this time was V0 (in this example, V0 = 330 mL, for example). A jig installed on the top of the container was lowered to push the expanded beads in the container at a speed of 10 mm / min, and when a load of 650 N was applied to the expanded beads in the container, the load from the jig was removed, and the expanded beads compressed in the container were restored to their original state. The application of the load and the restoration of the expanded beads from the compressed state were repeated 100 times (sag test). After the sag test, the expanded beads were left to stand in the container for one day, and then the volume V1 [unit: mL] of the expanded beads occupying the container was measured. The sag rate R was calculated by the following formula (11). R = (V0 - V1) / V0 (11)
[0176] [Closed cell ratio c1 after settling test] The foamed beads were subjected to a sag test, and then the closed cell ratio was measured. The sag test and the method for measuring the closed cell ratio were as described above. In addition, the ratio [c1 / c0] of the closed cell ratio of the foamed beads before the sag test to the closed cell ratio c0 and the difference [c0-c1] from the closed cell ratio c0 of the foamed beads before the sag test were calculated.
[0177] [Particle size] The particle size of the expanded beads (specifically, the average particle size) refers to the particle size at an integrated value of 63% in the particle size distribution obtained by the laser diffraction / scattering method. Specifically, the average particle size was measured using a particle size distribution measuring device "Militrack JPA" manufactured by Nikkiso Co., Ltd.
[0178] [Average bubble diameter, coefficient of variation] The average cell diameter and the coefficient of variation of the cell diameter of the expanded beads were measured as follows. First, the expanded beads were divided into two parts passing through the center of the expanded beads, and a photograph was taken with a scanning electron microscope so that the entire cut surface of one part was captured. Next, in the obtained cross-sectional photograph, lines extending from approximately the center of the cut surface of the expanded beads to the surface of the expanded beads and dividing the cut surface into eight parts while changing the angle by 45° each (specifically, eight lines extending from approximately the center of the cut surface of the expanded beads to the surface of the particles) were drawn, and the number of bubbles intersecting with these lines was counted. The total length of each line was divided by the number of bubbles counted to obtain the bubble diameter of the expanded beads. This operation was performed in the same manner for 20 expanded beads, and the arithmetic average value of the bubble diameters of each expanded bead was used as the average value of the bubble diameters of the expanded beads. The standard deviation of the bubble diameters of each bubble of the expanded beads was divided by the average value of the bubble diameters of the expanded beads to obtain the coefficient of variation of the bubble diameters. The value given by the square root of the unbiased variance was used as the standard deviation.
[0179] [Bubble film thickness, coefficient of variation] The average bubble thickness and the coefficient of variation of the bubble thickness were measured as follows. In the measurement of the average bubble diameter, the bubble film intersecting with the eight lines drawn on the cross-section photograph of the expanded beads was used as the measurement target for bubble thickness. The thickness of each of the measured bubble films was measured at approximately the center position, and the arithmetic average value was used as the bubble film thickness of the expanded beads. This operation was performed in the same manner for 20 expanded beads, and the arithmetic average value of the bubble film thickness of each expanded bead was used as the average bubble film thickness of the expanded beads. The standard deviation of each bubble film thickness of the expanded beads was divided by the average bubble film thickness of the expanded beads to obtain the coefficient of variation of the bubble diameter. The value given by the square root of the unbiased variance was used as the standard deviation.
[0180] [Evaluation of foamed bead moldings] [Molded object magnification] The molding magnification (unit: times) is determined by the density of the styrene resin that constitutes the foamed beads (specifically, 1000 kg / m 3 ) is the density of the foamed bead molding (unit: kg / m 3 The density of the expanded bead molding was calculated by dividing the mass (unit: kg) of the molding by the volume (unit: m) of the molding calculated based on its outer dimensions. 3 ) was divided by
[0181] [Fusion rate of molded body] The molded body was folded in the longitudinal direction so as to be approximately equally divided and broken. The exposed fracture surface was visually observed, and the number of expanded beads whose interfaces between the expanded beads had peeled off and the number of expanded beads whose internal fracture had been counted. Then, the ratio of the number of expanded beads whose internal fracture had been relative to the total number of expanded beads exposed on the fracture surface, that is, the total number of expanded beads whose interfaces between the expanded beads had peeled off and the number of expanded beads whose internal fracture had been calculated. The value expressed as a percentage (%) was taken as the fusion rate.
[0182] [Closed cell ratio C0 of molded body] The closed cell ratio of the molded product was measured using an air comparison type specific gravity meter based on procedure C described in ASTM-D2856-70. Specifically, a measurement sample with a length of 2.5 cm × width of 2.5 cm × height of 2.5 cm was cut out from the center of the molded product, and its geometric volume Va (unit: cm 3 ) was obtained. Specifically, Va is the product of the length (unit: cm), width (unit: cm), and height (unit: cm) of the measurement sample. Next, the true volume Vx of the measurement sample was measured using an air comparison specific gravity meter 930 (Toshiba Beckman Co., Ltd.) in accordance with procedure C described in ASTM-D2856-70.
[0183] Using the geometric volume Va and true volume Vx of the measurement sample thus obtained, the closed cell ratio (unit: %) of the measurement sample was calculated based on the following formula (12). The above operation was performed for each of the five measurement samples, and the arithmetic mean value of the closed cell ratios of the five measurement samples was taken as the closed cell ratio of the molded body. Closed cell ratio=(Vx-W / ρ)×100 / (Va-W / ρ) ···(12)
[0184] The symbols in formula (12) have the following meanings: Vx: The true volume of the measurement sample measured by the above method, i.e., the sum of the volume of the resin constituting the molded body and the total volume of the air bubbles in the closed cell part in the molded body (unit: cm 3 ) Va: Geometric volume of the measurement sample (unit: cm 3 ) W: Mass of the measurement sample (unit: g) ρ: Density of the resin that composes the molded body (unit: g / cm 3 )
[0185] [50% deformation compressive stress] The 50% deformation compressive stress is an index of the rigidity of the molded body. When the molded body magnification is about the same, a molded body with a larger 50% deformation compressive stress is judged to have superior rigidity. In addition, when the molding conditions are similar, the 50% deformation compressive stress of the molded body reflects the rigidity of the original expanded beads, so the 50% deformation compressive stress is also an index of the rigidity of the expanded beads constituting the molded body. In other words, expanded beads with excellent rigidity are expanded beads that can mold a molded body with excellent rigidity. A rectangular parallelepiped test piece with a length of 50 mm, a width of 50 mm, and a thickness of 25 mm was cut out from the center of the molded body so as not to include the skin surface on the surface of the molded body, that is, the surface that was in contact with the inner surface of the mold during molding in the mold. Using this test piece, a compression test was performed in which the test piece was compressed to a strain amount of 80% at a compression speed of 10 mm / min based on JIS K6767:1999, and a stress-strain curve was obtained, and the compressive stress at 50% strain was determined as the 50% deformation compressive stress.
[0186] [Closed cell ratio C1 after compression test] The closed cell ratio of the molded body after the compression test in the 50% deformation compressive stress measurement was measured. Specifically, the molded body after the compression test was left to stand at 23°C for 24 hours, and the closed cell ratio was measured. The method for measuring the closed cell ratio was as described above. In addition, the ratio [C1 / C0] of the closed cell ratio of the molded body before the compression test to the closed cell ratio C0 and the difference [C0-C1] from the closed cell ratio C0 of the molded body before the compression test were calculated.
[0187] [Compression set] Compression set is an index of the recovery of a molded body. When the molded body magnification is the same, a molded body with a smaller compression set is judged to have better recovery. A rectangular parallelepiped test piece measuring 50 mm long x 50 mm wide x 25 mm thick was cut out from the center of the molded body, without including the skin surface on the surface of the molded body, that is, the surface that was in contact with the inner surface of the mold during molding in the mold. Using this test piece, compression set was measured in accordance with JIS K 6767:1999. The compression speed was 10 mm / min, and the amount of strain was 25%.
[0188] [Table 1]
[0189] [Table 2]
[0190] [Table 3]
[0191] [Table 4]
[0192] As can be seen from Tables 1 and 2, the expanded beads of the Examples have a high bulk ratio of 30 to 150 times, but have a low settling rate and high recovery. The molded bodies obtained by molding the expanded beads of the Examples in a mold have a high bulk ratio, but have a low compression set and high recovery, as well as a high compression stress and excellent rigidity. It is considered that such effects are further exerted by the fact that the expanded beads of the Examples are made of a predetermined styrene-based resin, that the closed cell ratio is maintained high even after compression, that the bubbles are uniformly formed, and that the bubble film made of the styrene-based resin has a sufficient thickness and is uniform in thickness. The uniformity of the diameter of the bubbles 11 and the uniformity of the thickness of the bubble film 12 of the expanded beads 1 of the Examples can also be seen from Figures 1 to 3. The molded bodies of the Examples had a high fusion rate even when the molded body magnification was high. This is believed to be because expanded beads have a high closed cell ratio even when the bulk ratio is high, and the thickness of the cell membrane is uniform, so that the cells are likely to be prevented from breaking during molding.
[0193] The expanded beads of the examples can be obtained by being composed of a styrene-based resin having a weight-average molecular weight Mw' of 1 million to 5 million, a ratio Mz' / Mn' of Z-average molecular weight Mz' to number-average molecular weight Mn' of 5 or more, and a branching degree of 0.2 or more per 1000 styrene units. The expanded beads molding of the examples in which the expanded beads are fused to each other can be obtained by molding the expanded beads in a mold.
[0194] Also, for example, comparison between Example 1 and Example 3 reveals that expanded beads and molded articles thereof made of a styrene-based resin in which the ratio Mz' / Mn' of the Z-average molecular weight Mz' to the number-average molecular weight Mn' is 7 or more have better restoring properties and rigidity. Also, for example, comparison between Example 1 and Example 7 reveals that even when the same styrene-based resin is used as the base resin, the uniformity of the cell diameter and cell film thickness of the resulting expanded beads may differ depending on the conditions for expanding the expandable resin beads, and expanded beads and molded articles thereof with higher uniformity in these properties have better restoring properties and rigidity.
[0195] On the other hand, as can be seen from Tables 3 and 4, in Comparative Examples 1 and 2, the expanded beads are made of a linear styrene resin having no branched structure with a branching degree of 0, and the weight-average molecular weight Mw' of the styrene resin is also low. Therefore, compared with the examples having the same bulk ratio, the settling rate is high and the restoring property is insufficient. In addition, compared with the examples having the same bulk ratio, the molded body obtained by molding the expanded beads in a mold has a large compression permanent set and insufficient restoring property, and also has a low compressive stress and insufficient rigidity. In addition, the expanded beads of Comparative Examples 1 and 2 have a large coefficient of variation of the bubble diameter and a low uniformity of the bubbles, and a large coefficient of variation of the bubble film thickness and a low uniformity of the bubble film thickness. It can be seen from Figures 4 to 6 that the uniformity of the diameter of the bubbles 91 and the thickness of the bubble film 92 of the expanded beads 9 of Comparative Example 1 are low, and a thin-walled portion 925 having a thickness smaller than the surrounding area was formed in the bubble film 92. Although not shown, a thin-walled portion was also formed in the expanded beads of Comparative Example 2. However, since the expanded beads of Comparative Example 1 had a higher bulk ratio, more thin-walled portions were formed than in Comparative Example 2, and the coefficient of variation of the cell thickness was higher.
[0196] In Comparative Examples 3 and 4, the bulk ratio of the expanded beads is insufficient. In Comparative Example 3, the content of the foaming agent in the expandable resin beads was too low, so the expandable resin beads could not be sufficiently expanded. In Comparative Example 4, the content of the foaming agent in the expandable resin beads was too high, so the expanded beads significantly shrunk immediately after expansion. In Comparative Examples 3 and 4, the expanded beads could not be expanded to the desired ratio as described above, and the bulk ratio was insufficient, so other evaluations were omitted.
[0197] The expanded beads of Comparative Examples 5 and 6 are composed of a styrene-based resin having a branched structure but small Mw' and Mz' / Mn'. Therefore, compared with the examples of the same bulk ratio, the settling rate is high and the restoring property is slightly insufficient. Furthermore, the molded articles obtained by molding the expanded beads in a mold have a large compression permanent set and slightly insufficient restoring property, as well as a low compressive stress and slightly insufficient rigidity, compared with the molded articles of the examples of the same bulk ratio. Furthermore, the expanded beads of Comparative Examples 5 and 6 have a large coefficient of variation of the bubble diameter and low bubble uniformity, and a large coefficient of variation of the bubble film thickness and low bubble film thickness uniformity.
[0198] The expanded beads of the Examples are lightweight yet excellent in resilience and rigidity, and therefore can be used as expanded bead molded articles for packaging containers and cushioning materials for heavy items, etc., and are also suitable as stuffing for bead cushion materials, taking advantage of the properties of the expanded beads themselves. For example, a bag filled with a large number of expanded beads is used as a stuffing.
[0199] The above describes the embodiments of the styrene-based resin expanded beads, expanded bead moldings, and filling for bead cushion materials according to the present invention based on examples. However, the specific embodiments of the present invention are not limited to those of the examples, and the configurations can be changed as appropriate within the scope of the invention without departing from the spirit of the invention. [Explanation of symbols]
[0200] 1. Styrene resin foam particles 11 Bubbles 12 Bubble membrane
Claims
1. The expanded particles are made of a styrene-based resin, The expanded beads have a bulk ratio of 30 to 150 times, The weight average molecular weight Mw' of the styrene-based resin is 1 million or more and 5 million or less, the ratio Mz' / Mn' of the Z-average molecular weight Mz' to the number-average molecular weight Mn' of the styrene-based resin is 5 or more (wherein the weight-average molecular weight Mw', the number-average molecular weight Mn' and the Z-average molecular weight Mz' are determined by a GPC-MALS method); The expanded styrene resin particles have a branching degree of 0.2 or more per 1,000 styrene units.
2. 2. The expanded styrene resin beads according to claim 1, wherein the ratio Mz' / Mn' of the Z-average molecular weight Mz' to the number-average molecular weight Mn' of the styrene resin is 7 or more.
3. 3. The expanded styrene resin beads according to claim 1, wherein the styrene resin has a weight average molecular weight Mw' of 1.5 million or more.
4. 3. The expanded styrene-based resin beads according to claim 1, wherein the styrene-based resin has a tetrahydrofuran insoluble content of 0.1% by mass or less (including 0).
5. 3. The expanded styrene resin beads according to claim 1, wherein the expanded beads have a bulk ratio of 80 to 150.
6. 3. The expanded styrene resin beads according to claim 1, wherein the expanded beads have a closed cell rate of 85% or more.
7. 3. The expanded styrene resin beads according to claim 1, wherein the average cell diameter of the expanded beads is 10 μm or more and 100 μm or less, and the coefficient of variation of the cell diameter is 20% or less.
8. 3. The expanded styrene resin beads according to claim 1, wherein the average cell thickness of the expanded beads is from 1 μm to 8 μm, and the variation coefficient of the cell thickness is 35% or less.
9. The expanded styrene resin beads according to claim 1 or 2, wherein the average particle diameter of the expanded beads is 3 to 10 mm.
10. 3. A bead cushion filling material comprising the expanded styrene resin particles according to claim 1 or 2.
11. 3. An expanded bead molding produced by molding the expanded styrene-based resin beads according to claim 1 or 2 in a mold.
Citation Information
Patent Citations
Styrene-based polymer having long-chain branched structure and its production
JP1999035636A
Expandable polystyrenic resin particle and its production method, pre-expanded particle and expanded molded product
JP2008133449A
Expandable polystyrene resin particle and manufacturing method of polystyrene resin foam-molded item
JP2008150410A
Expanded styrene resin bead and molded object formed from expanded styrene resin bead
JP2009108237A
Polystyrene-based resin particle, foamable resin particle, methods for producing them, foam particle and molded foam
JP2013159683A