Resin composition, pellets, and molded article
The resin composition, combining maleic anhydride-modified polyethylene and specific structural units with polycarbonate resin, addresses the issue of poor scratch resistance and hue balance in colored molded products, achieving superior abrasion resistance and color intensity in molded articles.
Patent Information
- Application Number
- JP2023055593
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Filing Date
- 2023-03-30
- Publication Date
- 2024-10-11
AI Technical Summary
Existing resin compositions containing polycarbonate resin with bisphenol C-derived structural units and pigments suffer from poor scratch resistance, appearance, and hue balance, particularly when colored molded products are required.
A resin composition is formulated with 0.3 to 1.5 parts by mass of maleic anhydride-modified polyethylene and 0.04 to 2.0 parts by mass of pigment blended with a polycarbonate resin containing specific structural units, ensuring a balanced blend of 5 mol% or more of the structural units represented by formula (1) and optionally formula (2), with a maleic anhydride-modified polyethylene having an acid value of 40 mgKOH/g or more.
The composition achieves molded articles with excellent scratch resistance, appearance, and hue, as demonstrated by low ΔGross60° values and favorable L* values, indicating improved abrasion resistance and color intensity.
Smart Images

Figure 2024143095000001 
Figure 2024143095000002 
Figure 2024143095000003
Abstract
Description
[Technical field]
[0001] The present invention relates to a resin composition, a pellet, and a molded article, and in particular to a resin composition containing a polycarbonate resin as a main component. [Background technology]
[0002] Polycarbonate resins are excellent in mechanical strength, electrical properties, transparency, etc., and are widely used as engineering plastics in various fields such as the electrical and electronic equipment field, the automotive field, etc. In recent years, in these fields, molded products have become thinner, less expensive, smaller, and lighter, and further performance improvements in molding materials are required, and several proposals have been made.
[0003] For example, Patent Document 1 discloses a resin composition in which a fatty acid ester such as behenyl behenate is blended with a polycarbonate resin that contains a structural unit derived from bisphenol C. [Prior art documents] [Patent documents]
[0004] [Patent Document 1] JP 2020-063332 A Summary of the Invention [Problem to be solved by the invention]
[0005] The resin composition described in Patent Document 1 is characterized by excellent scratch resistance and transparency. However, depending on the application of the polycarbonate resin, there may be a need for a molded product that is colored while also having excellent scratch resistance. In this case, it is considered to add a pigment to the polycarbonate resin in order to color the molded product. When a pigment is added, the L *However, the present inventors have conducted research and found that a resin composition containing a polycarbonate resin containing a structural unit derived from bisphenol C, a component for improving scratch resistance, and a colorant has poor scratch resistance, poor appearance, and L * It was found that there are cases where the value can be high. The present invention aims to solve such problems, and to provide a resin composition capable of providing a molded article having a well-balanced and excellent scratch resistance, appearance, and color, as well as pellets and molded articles using the resin composition. [Means for solving the problem]
[0006] In view of the above-mentioned problems, the present inventors have conducted research and have found that the above-mentioned problems can be solved by blending a maleic anhydride-modified polyethylene and a pigment in a predetermined ratio with a polycarbonate resin containing a structural unit represented by formula (1), such as a polycarbonate resin containing a structural unit derived from bisphenol C. Specifically, the above problems were solved by the following means. <1> A resin composition comprising 100 parts by mass of a polycarbonate resin, 0.3 to 1.5 parts by mass of a maleic anhydride modified polyethylene, and 0.04 to 2.0 parts by mass of a pigment, wherein the polycarbonate resin contains a structural unit represented by formula (1) in a proportion of 5 mol % or more of all structural units. Formula (1) [ka] (In formula (1), R 1 represents a methyl group, and R 2 represents a hydrogen atom or a methyl group, and X 1 represents one of the following formulas: [ka] R 3 and R 4 each independently represents a hydrogen atom or a methyl group, and Z represents a group that bonds with C to form an alicyclic hydrocarbon having 6 to 12 carbon atoms which may have a substituent. <2> The polycarbonate resin further contains a structural unit represented by formula (2): <1> The resin composition according to claim 1. Formula (2) [ka] (In formula (2), X 2 represents one of the following formulas: [ka] R 3 and R 4 each independently represents a hydrogen atom or a methyl group, and Z represents a group that bonds with C to form an alicyclic hydrocarbon having 6 to 12 carbon atoms which may have a substituent. <3> The polycarbonate resin contains, among all structural units, 10 to 90 mol % of structural units represented by formula (1) and 90 to 10 mol % of structural units represented by formula (2) (however, the total of the structural units represented by formula (1) and the structural units represented by formula (2) does not exceed 100 mol %), <2> The resin composition according to claim 1. <4> The acid value of the maleic anhydride modified polyethylene is 40 mgKOH / g or more. <1> ~ <3> 10. The resin composition according to claim 9 . <5> The polycarbonate resin includes a polycarbonate resin that is a material recycled polycarbonate resin containing a structural unit represented by formula (2). <1> ~ <4> 10. The resin composition according to claim 9 . <6> The pigment comprises a black pigment. <1> ~ <5> 10. The resin composition according to claim 9 . <7> The polycarbonate resin further contains a structural unit represented by formula (2), The polycarbonate resin contains, among all structural units, 10 to 90 mol % of structural units represented by formula (1) and 90 to 10 mol % of structural units represented by formula (2) (provided that the sum of the structural units represented by formula (1) and the structural units represented by formula (2) does not exceed 100 mol %), The acid value of the maleic anhydride modified polyethylene is 40 mgKOH / g or more. <1> ~ <6> 10. The resin composition according to claim 9 . Formula (2) [ka] (In formula (2), X 2 represents one of the following formulas: [ka] R 3 and R 4 each independently represents a hydrogen atom or a methyl group, and Z represents a group that bonds with C to form an alicyclic hydrocarbon having 6 to 12 carbon atoms which may have a substituent. <8> <1> ~ <7> 2. A pellet of the resin composition according to claim 1. <9> <1> ~ <7> 2. A molded article molded from the resin composition according to claim 1. <10> <8> A molded article formed from the pellets according to claim 1. Effect of the Invention
[0007] INDUSTRIAL APPLICABILITY The present invention makes it possible to provide a resin composition capable of providing a molded article having a well-balanced excellent scratch resistance, appearance and color, as well as pellets and molded articles using the resin composition. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0008] Hereinafter, an embodiment of the present invention (hereinafter, simply referred to as "the present embodiment") will be described in detail. Note that the present embodiment is an example for explaining the present invention, and the present invention is not limited to the present embodiment. In this specification, the use of "to" means that the numerical values before and after it are included as the lower limit and upper limit. In this specification, various physical properties and characteristic values are those at 23° C. unless otherwise specified. If the measurement methods, etc. described in the standards shown in this specification vary from year to year, they will be based on the standards as of January 1, 2023, unless otherwise stated.
[0009] The resin composition of the present embodiment is characterized in that it contains 0.3 to 1.5 parts by mass of maleic anhydride modified polyethylene and 0.04 to 2.0 parts by mass of a pigment per 100 parts by mass of a polycarbonate resin, and that the polycarbonate resin contains a structural unit represented by formula (1) in a proportion of 5 mol % or more of all structural units. By adopting such a constitution, it is possible to obtain a resin composition which is capable of providing a molded product having a good balance of scratch resistance, appearance and color. In this embodiment, in addition to the polycarbonate resin and the pigment, maleic anhydride-modified polyethylene is blended. Since maleic anhydride has excellent compatibility with polycarbonate resin, it is presumed that the maleic anhydride portion is compatible with the polycarbonate resin, and the polyethylene portion is likely to be present on the surface of the molded product. In particular, maleic anhydride-modified polyethylene is usually blended as a compatibility / dispersion agent for additives (fillers) in a resin composition, and it is surprising that the scratch resistance is improved as in the present invention. In addition, as shown in the examples described below, the effect of the present invention is also surprising from the viewpoint that the effect is not obtained even when maleic anhydride-modified polypropylene is used.
[0010] Formula (1) [ka] (In formula (1), R 1 represents a methyl group, and R 2 represents a hydrogen atom or a methyl group, and X 1 represents one of the following formulas: [ka] R 3 and R 4 each independently represents a hydrogen atom or a methyl group, and Z represents a group that bonds with C to form an alicyclic hydrocarbon having 6 to 12 carbon atoms which may have a substituent.
[0011] The details of this embodiment will be described below.
[0012] <Polycarbonate resin> The resin composition of the present embodiment contains the structural unit represented by formula (1) in a proportion of 5 mol % or more of all structural units. By containing the structural unit represented by formula (1), a molded article having excellent scratch resistance can be obtained. Formula (1) [ka] (In formula (1), R 1 represents a methyl group, and R 2 represents a hydrogen atom or a methyl group, and X 1 represents one of the following formulas: [ka] R 3 and R 4 each independently represents a hydrogen atom or a methyl group, and Z represents a group that bonds with C to form an alicyclic hydrocarbon having 6 to 12 carbon atoms which may have a substituent.
[0013] In the constitutional unit represented by formula (1), R 2 is preferably a hydrogen atom. In formula (1), X 1 but, [ka] If R 3 and R 4 At least one of the groups is preferably a methyl group, and it is more preferable that both of the groups are methyl groups. Also, X 1 but, [ka] In this case, Z is bonded to the carbon C bonded to the two phenyl groups in the above formula (1) to form a divalent alicyclic hydrocarbon group having 6 to 12 carbon atoms. Examples of the divalent alicyclic hydrocarbon group include cycloalkylidene groups such as a cyclohexylidene group, a cycloheptylidene group, a cyclododecylidene group, an adamantylidene group, and a cyclododecylidene group. Examples of the alicyclic hydrocarbon having a substituent formed by bonding Z to C include the methyl- and ethyl-substituted alicyclic hydrocarbon groups described above. Examples of the substituted groups include those having a methyl or ethyl substituent. Among these, a cyclohexylidene group, a methyl-substituted cyclohexylidene group (preferably a 3,3,5-trimethyl-substituted cyclohexylidene group), and a cyclododecylidene group are preferred.
[0014] In formula (1), X 1 is preferably the following structure: [ka]
[0015] A specific preferred example of the structural unit represented by the above formula (1) is 2,2-bis(3-methyl-4-hydroxyphenyl)propane, that is, a structural unit composed of bisphenol C (carbonate structural unit).
[0016] In the present embodiment, the polycarbonate resin may contain only one type of constitutional unit represented by formula (1), or may contain two or more types.
[0017] In this embodiment, the polycarbonate resin containing the structural unit represented by formula (1) may further contain a structural unit represented by formula (2). Here, containing the structural unit represented by formula (2) means that the polycarbonate resin contained in the resin composition of this embodiment may be a polycarbonate resin containing a structural unit represented by formula (1) and a structural unit represented by formula (2), or may be a blend of a polycarbonate resin containing a structural unit represented by formula (1) and a polycarbonate resin containing a structural unit represented by formula (2). By containing the structural unit represented by formula (2), the heat resistance of the obtained molded article tends to be further improved. Formula (2) [ka] In formula (2), X 2 represents one of the following formulas: [ka] R 3 and R 4 each independently represents a hydrogen atom or a methyl group, and Z represents a group that bonds with C to form an alicyclic hydrocarbon having 6 to 12 carbon atoms which may have a substituent.
[0018] In formula (2), X 2 but, [ka] If R 3 and R 4 At least one of the groups is preferably a methyl group, and it is more preferable that both of the groups are methyl groups. Also X 2 but, [ka] In this case, Z is bonded to the carbon C bonded to the two phenyl groups in the above formula (2) to form a divalent alicyclic hydrocarbon group having 6 to 12 carbon atoms. Examples of the divalent alicyclic hydrocarbon group include cycloalkylidene groups such as a cyclohexylidene group, a cycloheptylidene group, a cyclododecylidene group, an adamantylidene group, and a cyclododecylidene group. Substituted groups include those having a methyl substituent or an ethyl substituent. Among these, a cyclohexylidene group, a methyl-substituted cyclohexylidene group (preferably a 3,3,5-trimethyl-substituted cyclohexylidene group), and a cyclododecylidene group are preferred. In formula (2), X 2 is preferably the following structure: [ka]
[0019] In this embodiment, the polycarbonate resin may contain only one type of constitutional unit represented by formula (2), or may contain two or more types.
[0020] In the present embodiment, the polycarbonate resin may contain other structural units in addition to the structural unit represented by formula (1) and the structural unit represented by formula (2). Examples of other structural units include structural units derived from dihydroxy compounds shown below.
[0021] Bis(4-hydroxyphenyl)methane, 2,2-bis(4-hydroxyphenyl)butane, 2,2-bis(4-hydroxyphenyl)pentane, 2,2-bis(4-hydroxyphenyl)-4-methylpentane, 2,2-bis(4-hydroxy-3-methylphenyl)propane, 2,2-bis(4-hydroxy-3,5-dimethylphenyl)propane, 2,2-bis(4-hydroxy-3-(1-methylethyl)phenyl)propane, 2,2-bis(4-hydroxy-3-tert-butylphenyl)propane, 2,2-bis(4-hydroxy -3-(1-methylpropyl)phenyl)propane, 2,2-bis(4-hydroxy-3-cyclohexylphenyl)propane, 2,2-bis(4-hydroxy-3-phenylphenyl)propane, 1,1-bis(4-hydroxyphenyl)decane, 1,1-bis(4-hydroxyphenyl)cyclohexane, 1,1-bis(4-hydroxyphenyl)-1-phenylethane, 1,1-bis(4-hydroxyphenyl)phenylmethane, 1,1-bis(4-hydroxy-3-methylphenyl)cyclohexane, 1,1-bis(4-hydroxy-3, 5-dimethylphenyl)cyclohexane, 1,1-bis(4-hydroxy-3-(1-methylethyl)phenyl)cyclohexane, 1,1-bis(4-hydroxy-3-tert-butylphenyl)cyclohexane, 1,1-bis(4-hydroxy-3-(1-methylpropyl)phenyl)cyclohexane, 1,1-bis(4-hydroxy-3-cyclohexylphenyl)cyclohexane, 1,1-bis(4-hydroxy-3-phenylphenyl)cyclohexane, 1,1-bis(4-hydroxy-3-methylphenyl)-1-phenylethane, 1,1-bis(4-hydroxy-3,5-dimethylphenyl)-1-phenylethane, 1,1-bis(4-hydroxy-3-(1-methylethyl)phenyl)-1-phenylethane, 1,1-bis(4-hydroxy-3-tert-butylphenyl)-1-phenylethane, 1,1-bis(4-hydroxy-3-(1-methylpropyl)phenyl)-1-phenylethane, 1,1-bis(4-hydroxy-3-cyclohexylphenyl)-1-phenylethane, 1,1-bis(4-hydroxy-3-phenylphenyl)-1-phenylethane, 1,1-bis(4-hydroxyphenyl)cyclopentane, 1,1-bis(4-hydroxyphenyl)cyclooctane, 4,4'-(1,3-phenylenediisopropylidene)bisphenol, 4,4'-(1,4-phenylenediisopropylidene)bisphenol, 9,9-bis(4-hydroxyphenyl)fluorene, 9,9-bis(4-hydroxy-3-methylphenyl)fluorene, 4,4'-dihydroxybenzophenone, 4,4'-dihydroxyphenyl ether, 4,4'-dihydroxybiphenyl, 1,1-bis(4-hydroxyphenyl)-3,3,5-trimethylcyclohexane, 1,1-bis(4-hydroxy-6-methyl-3-tert-butylphenyl)butane.
[0022] In addition, as an embodiment of other structural units, the structural unit represented by formula (2) described in paragraph 0008 of WO 2017 / 099226, the description in paragraphs 0043 to 0052 of WO 2017 / 099226, and the description in JP 2011-046769 A can be referred to, the contents of which are incorporated herein by reference.
[0023] In the polycarbonate resin used in this embodiment, the ratio of the structural unit represented by formula (1) in all structural units is 5 mol% or more, preferably 10 mol% or more, more preferably 12 mol% or more, and even more preferably 14 mol% or more, and may be 35 mol% or more, 50 mol% or more, 70 mol% or more, 75 mol% or more, or 80 mol% or more depending on the application, etc. By making it equal to or more than the lower limit, the surface hardness of the molded article tends to be increased. In the polycarbonate resin used in this embodiment, the ratio of the structural unit represented by formula (1) in all structural units may be 100 mol%, preferably 90 mol% or less, and may be 88 mol% or less, 86 mol% or less, 65 mol% or less, 60 mol% or less, 50 mol% or less, 30 mol% or less, 25 mol% or less, or 20 mol% or less depending on the application, etc. By making it equal to or less than the upper limit, the impact resistance of the obtained molded article tends to be further improved, and the heat resistance of the molded article also tends to be improved. Furthermore, by making the content equal to or less than the above upper limit, weather resistance also tends to be improved.
[0024] In the polycarbonate resin used in this embodiment, the ratio of the structural unit represented by formula (2) is preferably 10 mol% or more, more preferably 12 mol% or more, and even more preferably 14 mol% or more, and may be 35 mol% or more, 50 mol% or more, 70 mol% or more, 75 mol% or more, or 80 mol% or more depending on the application. By making it equal to or more than the lower limit, the impact resistance of the obtained molded article tends to be further improved, and the heat resistance of the molded article also tends to be improved. Furthermore, by making it equal to or more than the lower limit, the weather resistance also tends to be improved. In the polycarbonate resin used in this embodiment, the ratio of the structural unit represented by formula (2) is 95 mol% or less, preferably 90 mol% or less, in the total structural units, and may be 88 mol% or less, 86 mol% or less, 65 mol% or less, 60 mol% or less, 50 mol% or less, 30 mol% or less, 25 mol% or less, or 20 mol% or less depending on the application. By setting the content to be equal to or less than the upper limit, the surface hardness of the molded article tends to be increased. However, the total amount of the structural units represented by formula (1) and the structural units represented by formula (2) does not exceed 100 mol %.
[0025] In the polycarbonate resin used in the present embodiment, the total of the constitutional units represented by the above formula (1) and the constitutional units represented by the formula (2) preferably accounts for 90% by mass or more, more preferably 95% by mass or more, and even more preferably 99% by mass or more of all constitutional units excluding terminal groups. The upper limit of the total is 100% by mass or less.
[0026] The polycarbonate resin used in the present embodiment is preferably in the following form. (A1) Polycarbonate resin containing a structural unit represented by formula (1) (A2) A blend of a polycarbonate resin containing a structural unit represented by formula (1) and a polycarbonate resin containing a structural unit represented by formula (2) (A3) Polycarbonate resin containing a structural unit represented by formula (1) and a structural unit represented by formula (2) (A4) A blend of a polycarbonate resin containing a structural unit represented by formula (1) and a polycarbonate resin containing a structural unit represented by formula (1) and a structural unit represented by formula (2). (A5) A blend of a polycarbonate resin containing a structural unit represented by formula (2) and a polycarbonate resin containing a structural unit represented by formula (1) and a structural unit represented by formula (2). (A6) A blend of a polycarbonate resin containing a structural unit represented by formula (1), a polycarbonate resin containing a structural unit represented by formula (2), and a polycarbonate resin containing a structural unit represented by formula (1) and a structural unit represented by formula (2). (A7) In the above (A1) to (A6), the polycarbonate resin or the polycarbonate resin constituting the blend thereof contains a structural unit represented by formula (1) and a structural unit other than the structural unit represented by formula (2). (A8) A blend of the polycarbonate resin or blend of the above (A1) to (A7) with a polycarbonate resin comprising other structural units.
[0027] The lower limit of the viscosity average molecular weight (Mv) of the polycarbonate resin used in the present embodiment is preferably 5,000 or more, more preferably 8,000 or more, even more preferably 10,000 or more, and even more preferably 12,000 or more. The upper limit of Mv is preferably 50,000 or less, more preferably 30,000 or less, even more preferably 29,000 or less, and even more preferably 27,000 or less. By setting the viscosity average molecular weight to the above lower limit or more, moldability is improved and molded articles having high mechanical strength can be obtained, whereas by setting the viscosity average molecular weight to the above upper limit or less, the flowability of the resin composition is improved and thin-walled molded articles can be efficiently produced. When the resin composition contains two or more kinds of polycarbonate resins, the total is the sum of values obtained by multiplying the viscosity average molecular weight of each polycarbonate resin by the mass fraction. In particular, the viscosity average molecular weight of the polycarbonate resin containing the constitutional unit represented by formula (1) is preferably 15,000 to 30,000. Also, the viscosity average molecular weight of the polycarbonate resin containing the constitutional unit represented by formula (2) is preferably 12,000 to 28,000, and more preferably 18,000 to 27,000. The viscosity average molecular weight (Mv) of a polycarbonate resin is calculated from the intrinsic viscosity (η) (unit: dL / g) at 20°C using an Ubbelohde viscometer with methylene chloride as a solvent, and then calculated from the following Schnell viscosity formula. η = 1.23 × 10 -4 Mv 0.83
[0028] The method for producing the polycarbonate resin used in the present embodiment is not particularly limited, but for example, the description in paragraphs 0027 to 0043 and the Examples of JP-A-2014-065901 can be referred to, the contents of which are incorporated herein by reference.
[0029] Furthermore, the polycarbonate resin (particularly, the polycarbonate resin containing the constitutional unit represented by formula (2)) may be not only a virgin raw material but also a polycarbonate resin regenerated from a used product (so-called material recycled polycarbonate resin). Examples of the used product include optical recording media such as optical disks; light guide plates; transparent vehicle components such as automobile window glass, automobile headlamp lenses, and windshields; containers such as water bottles; eyeglass lenses; soundproof walls, glass windows, corrugated sheets, and other building components. In addition, crushed products obtained from non-conforming products, scraps, sprues, runners, and the like, or pellets obtained by melting these may also be used. However, the polycarbonate resin that has been material recycled is preferably 80% by mass or less, more preferably 60% by mass or less, and may be 40% by mass or less of the polycarbonate resin contained in the resin composition. The lower limit of the content of the polycarbonate resin that has been material recycled may be 0% by mass of the polycarbonate resin contained in the resin composition, but is preferably 10% by mass or more from the viewpoint of environmental load.
[0030] The content of the polycarbonate resin in the resin composition of this embodiment is preferably 85% by mass or more, more preferably 90% by mass or more, even more preferably 95% by mass or more, and even more preferably 97% by mass or more, based on 100% by mass of the resin composition. By making it equal to or more than the lower limit, the heat resistance of the molded product obtained tends to be improved. In addition, the upper limit of the content of the polycarbonate resin in the resin composition of this embodiment is the amount in which all components other than the maleic anhydride-modified polyethylene and the pigment are polycarbonate resin.
[0031] <Maleic anhydride modified polyethylene> The resin composition of the present embodiment contains 0.3 to 1.5 parts by mass of maleic anhydride-modified polyethylene per 100 parts by mass of polycarbonate resin. By containing maleic anhydride-modified polyethylene, the scratch resistance of the obtained molded article is improved.
[0032] The acid value of the maleic anhydride-modified polyethylene used in this embodiment is usually 20 mgKOH / g or more, preferably 40 mgKOH / g or more, more preferably 45 mgKOH / g or more, even more preferably 50 mgKOH / g or more, and even more preferably 55 mgKOH / g or more. By making it equal to or more than the lower limit, the scratch resistance and color of the obtained molded product tend to be further improved. In addition, the upper limit of the acid value of the maleic anhydride-modified polyethylene is preferably 100 mgKOH / g or less, more preferably 80 mgKOH / g or less. By making it equal to or less than the upper limit, the scratch resistance tends to be further improved. The acid value is measured as described in the Examples section below. When the resin composition contains two or more types of maleic anhydride-modified polyethylene, the acid value here is the sum of the acid values of each maleic anhydride-modified polyethylene multiplied by the blending amount (mass) fraction of each maleic anhydride-modified polyethylene.
[0033] The maleic anhydride-modified polyethylene in this embodiment has a molecular weight measured by a viscosity method of preferably 500 or more, more preferably 800 or more, and even more preferably 1000 or more, and preferably 5000 or less, more preferably 3000 or less, and even more preferably 2000 or less. By making the molecular weight equal to or more than the lower limit, the scratch resistance tends to be improved. By making the molecular weight equal to or less than the upper limit, the L * tends to be lower. When the resin composition contains two or more types of maleic anhydride modified polyethylene, the molecular weight referred to here is the molecular weight of the mixture of maleic anhydride modified polyethylenes.
[0034] The polyethylene constituting the maleic anhydride modified polyethylene used in this embodiment is one in which 70% by mass or more of all constituent units are ethylene units, preferably 75% by mass or more of ethylene units, preferably 80% by mass or more of ethylene units, preferably 85% by mass or more of ethylene units, preferably 90% by mass or more of ethylene units, preferably 95% by mass or more of ethylene units, and may be 99% by mass or more of ethylene units. Examples of components other than ethylene units constituting the polyethylene units in this embodiment include propylene units, butene units, etc.
[0035] The content of maleic anhydride-modified polyethylene in the resin composition of this embodiment is 0.3 parts by mass or more, preferably 0.4 parts by mass or more, more preferably 0.5 parts by mass or more, even more preferably 0.6 parts by mass or more, and even more preferably 0.7 parts by mass or more, relative to 100 parts by mass of polycarbonate resin. By making it equal to or more than the lower limit, the scratch resistance of the obtained molded article tends to be improved. In addition, the content of maleic anhydride-modified polyethylene in the resin composition of this embodiment is 1.5 parts by mass or less, preferably 1.4 parts by mass or less, more preferably 1.2 parts by mass or less, even more preferably 1.1 parts by mass or less, even more preferably 1.0 parts by mass or less, and even more preferably 0.9 parts by mass or less, relative to 100 parts by mass of polycarbonate resin. By making it equal to or less than the upper limit, the plate appearance of the obtained molded article tends to be improved. In addition, the moldability of the resin composition also tends to be improved. The resin composition of the present embodiment may contain only one type of maleic anhydride-modified polyethylene, or may contain two or more types. When two or more types are contained, the total amount is preferably in the above range.
[0036] The resin composition of this embodiment may or may not contain polyolefins other than maleic anhydride-modified polyethylene. An example of the resin composition of this embodiment is a resin composition that is substantially free of polyolefins other than maleic anhydride-modified polyethylene. "Substantially free" means that the content of polyolefins other than maleic anhydride-modified polyethylene contained in the resin composition is 10% by mass or less of the content of maleic anhydride-modified polyethylene, preferably less than 1% by mass, more preferably less than 0.1% by mass, and even more preferably less than 0.01% by mass.
[0037] <Pigments> The resin composition of the present embodiment contains 0.04 to 2.0 parts by mass of a pigment relative to 100 parts by mass of a polycarbonate resin. By containing a pigment, a molded product having excellent hue can be obtained. The pigment may be a chromatic pigment or an achromatic pigment, preferably an achromatic pigment, and may be an inorganic pigment or an organic pigment, preferably an inorganic pigment.
[0038] Examples of inorganic pigments include sulfide pigments such as carbon black, cadmium red, and cadmium yellow; silicate pigments such as ultramarine; oxide pigments such as titanium oxide, zinc white, red iron oxide, chromium oxide, iron black, titanium yellow, zinc-iron brown, titanium-cobalt green, cobalt green, cobalt blue, copper-chromium black, and copper-iron black; chromate pigments such as yellow lead and molybdate orange; and ferrocyanide pigments such as iron blue.
[0039] Examples of organic pigments include phthalocyanine pigments such as copper phthalocyanine blue and copper phthalocyanine green; azo pigments such as nickel azo yellow; methine pigments, pyrazolone pigments, thioindigo pigments, perinone pigments, perylene pigments, quinacridone pigments, dioxazine pigments, isoindolinone pigments, quinophthalone pigments, and other condensed polycyclic pigments; anthraquinone pigments, heterocyclic pigments, and methyl pigments. In the present embodiment, the pigment preferably contains a black pigment, and more preferably contains carbon black. By blending the black pigment in the resin composition of the present embodiment, the blackness can be increased. The black pigment in this embodiment is also intended to include a pigment that exhibits black color by blending two or more chromatic pigments.
[0040] The content of the pigment in the resin composition of this embodiment is, relative to 100 parts by mass of the polycarbonate resin, 0.04 parts by mass or more, preferably 0.08 parts by mass or more, more preferably 0.1 parts by mass or more, even more preferably 0.3 parts by mass or more, and 2.0 parts by mass or less, preferably 1.6 parts by mass or less, more preferably 1.2 parts by mass or less, even more preferably 1.0 part by mass or less, and may be 0.8 parts by mass or less. By setting the content of the pigment within the above range, the effect of adding the pigment is more effectively exhibited. The resin composition of the present embodiment may contain only one type of pigment, or may contain two or more types. When two or more types are contained, the total amount is preferably in the above range.
[0041] The resin composition of the present embodiment may or may not contain a dye. An example of the resin composition of the present embodiment is a resin composition that is substantially free of a dye. The term "substantially free of dye" means that the content of the dye contained in the resin composition is 10% by mass or less of the content of the pigment, preferably less than 1% by mass, more preferably less than 0.1% by mass, and even more preferably less than 0.01% by mass.
[0042] In the resin composition of this embodiment, the mass ratio of maleic anhydride-modified polyethylene to pigment contained in the resin composition (maleic anhydride-modified polyethylene / pigment) is preferably 0.4 or more, more preferably 0.5 or more, even more preferably 0.6 or more, even more preferably 0.7 or more, and even more preferably 0.74 or more. By making it equal to or more than the lower limit, the scratch resistance of the obtained molded article tends to be further improved, and the appearance tends to be further improved. In addition, the mass ratio maleic anhydride-modified polyethylene / pigment is preferably 10 or less, more preferably 5 or less, even more preferably 3 or less, even more preferably 2 or less, even more preferably 1.5 or less, and may be 1.3 or less. By making it equal to or less than the upper limit, the L of the obtained molded article * The value can be made smaller and still tend to result in improved appearance.
[0043] <Stabilizer> The resin composition of the present embodiment may contain a stabilizer. The stabilizers include heat stabilizers and antioxidants. As the heat stabilizer, a phosphorus-based stabilizer is preferably used. Any known phosphorus stabilizer can be used. Specific examples include phosphorus oxoacids such as phosphoric acid, phosphonic acid, phosphorous acid, phosphinic acid, and polyphosphoric acid; metal acid pyrophosphates such as sodium acid pyrophosphate, potassium acid pyrophosphate, and calcium acid pyrophosphate; phosphates of Group 1 or Group 2B metals such as potassium phosphate, sodium phosphate, cesium phosphate, and zinc phosphate; organic phosphate compounds, organic phosphite compounds, and organic phosphonite compounds, with organic phosphite compounds being particularly preferred.
[0044] As the antioxidant, a hindered phenol-based stabilizer is preferably used. Specific examples of hindered phenol stabilizers include pentaerythritol tetrakis[3-(3,5-di-tert-butyl-4-hydroxyphenyl)propionate], octadecyl-3-(3,5-di-tert-butyl-4-hydroxyphenyl)propionate, thiodiethylene bis[3-(3,5-di-tert-butyl-4-hydroxyphenyl)propionate], N,N'-hexane-1,6-diylbis[3-(3,5-di-tert-butyl-4-hydroxyphenyl)propionamide], 2,4-dimethyl-6-(1-methylpentadecyl)phenol, diethyl[[3,5-bis(1,1-dimethylethyl)-4-hydroxyphenyl]methyl]phosphate, 3,3',3'',5,5',5''-hexa-tert-butyl-a,a',a''-(mesityle) 4,6-bis(octylthiomethyl)-o-cresol, ethylene bis(oxyethylene) bis[3-(5-tert-butyl-4-hydroxy-m-tolyl)propionate], hexamethylene bis[3-(3,5-di-tert-butyl-4-hydroxyphenyl)propionate], 1,3,5-tris(3,5-di-tert-butyl -4-hydroxybenzyl)-1,3,5-triazine-2,4,6(1H,3H,5H)-trione, 2,6-di-tert-butyl-4-(4,6-bis(octylthio)-1,3,5-triazin-2-ylamino)phenol, 2-[1-(2-hydroxy-3,5-di-tert-pentylphenyl)ethyl]-4,6-di-tert-pentylphenyl acrylate, and the like.
[0045] Specific examples of such hindered phenol stabilizers include "Irganox (registered trademark; the same applies hereinafter) 1010" and "Irganox 1076" manufactured by BASF, and "ADK STAB AO-50" and "ADK STAB AO-60" manufactured by ADEKA Corporation.
[0046] The content of the stabilizer in the resin composition of the present embodiment is usually 0.001 parts by mass or more, preferably 0.005 parts by mass or more, more preferably 0.01 parts by mass or more, and usually 1 part by mass or less, preferably 0.5 parts by mass or less, more preferably 0.3 parts by mass or less, relative to 100 parts by mass of the polycarbonate resin. By setting the content of the stabilizer within the above range, the effect of adding the stabilizer is more effectively exhibited. The resin composition of the present embodiment may contain only one type of stabilizer, or may contain two or more types. When two or more types are contained, the total amount is preferably in the above range.
[0047] <Other ingredients> The resin composition of the present embodiment may contain, in addition to the polycarbonate resin, the maleic anhydride-modified polyethylene, the pigment, and the stabilizer blended as necessary, other components other than those described above as necessary, so long as the desired physical properties are not significantly impaired. Examples of the other components include other thermoplastic resins, reinforcing materials, various resin additives, etc. Examples of resin additives include ultraviolet absorbers, release agents, antistatic agents, flame retardants, flame retardant assistants, antifogging agents, lubricants, antiblocking agents, flow improvers, plasticizers, dispersants, antibacterial agents, and impact improvers. The resin additives may be contained in one type, or in any combination and ratio of two or more types. For details of these, refer to the descriptions in paragraphs 0059 to 0080 of JP 2014-065901 A and the descriptions in paragraphs 0069 to 0093 of JP 2018-165017 A, the contents of which are incorporated herein by reference. In particular, for the ultraviolet absorbent, the descriptions in paragraphs 0059 to 0062 of JP2016-216534A can be referred to, and the contents of these are incorporated into this specification. In particular, for the antistatic agent, the descriptions in paragraphs 0063 to 0067 of JP2016-216534A can be referred to, and the contents of these are incorporated herein by reference. In particular, for flame retardants, the disclosures in paragraphs 0068 to 0075 of JP2016-216534A can be referred to, the contents of which are incorporated herein by reference.
[0048] The resin composition of the present embodiment is prepared so that the total amount of the polycarbonate resin, the maleic anhydride modified polyethylene, the pigment, and the stabilizer blended as necessary is 100% by mass. The resin composition of the present embodiment may also be configured to be substantially free of reinforcing material, which means that the proportion of reinforcing material in 100% by mass of the resin composition is less than 5% by mass, preferably less than 3% by mass, and more preferably less than 1% by mass. The resin composition of the present embodiment may also be configured to be substantially free of glass fibers, which means that the proportion of glass fibers in 100% by mass of the resin composition is less than 5% by mass, preferably less than 3% by mass, and more preferably less than 1% by mass.
[0049] <Physical properties of resin composition> The resin composition of the present embodiment is preferably excellent in abrasion resistance. In particular, the value of ΔGross60° after abrasion resistance test of a molded article molded from the resin composition is preferably 6.0 or less, more preferably 5.3 or less, even more preferably 3.0 or less, and even more preferably 2.5 or less. The lower limit is ideally 0, but practically 0.1 or more. The ΔGross60° after the scratch resistance test is measured according to the method described in the Examples section below.
[0050] The resin composition of the present embodiment is preferably excellent in jet blackness. In particular, the L of a molded product obtained by molding the resin composition to a thickness of 2 mm is * is preferably 6.0 or less, more preferably 5.3 or less, even more preferably 5.0 or less, and even more preferably 4.5 or less. The lower limit is ideally 0, but a value of 0.1 or more is practical. L of molded product * is measured according to the method described in the Examples below.
[0051] <Method of producing resin composition> The method for producing the resin composition of the present embodiment is not limited, and a wide variety of known methods for producing polycarbonate resin compositions can be used. Specifically, the polycarbonate resin, the maleic anhydride-modified polyethylene, the pigment, and other components to be mixed as necessary are mixed in advance using various mixers such as a tumbler or a Henschel mixer, and then melt-kneaded using a mixer such as a Banbury mixer, a roll, a Brabender, a single-screw kneading extruder, a twin-screw kneading extruder, or a kneader. Some of the components, such as pigments, may be made into a master batch with a thermoplastic resin and then blended. In this embodiment, it is preferable to mix the pigment as a masterbatch. The thermoplastic resin used in the masterbatch is not particularly limited, but examples thereof include styrene-based resins and polycarbonate-based resins. The ratio of the pigment in the masterbatch is preferably 10 to 60% by mass, and more preferably 20 to 50% by mass. The melt-kneading temperature is not particularly limited, but is usually in the range of 240 to 320°C.
[0052] <Molded products> One form of the resin composition of the present embodiment is pellets. The above-mentioned resin composition or pellets can be molded into a molded article by various molding methods. That is, the molded article of the present embodiment is molded from the resin composition or pellets of the present embodiment. The shape of the molded article is not particularly limited and can be appropriately selected depending on the use and purpose of the molded article, and examples thereof include film-like, rod-like, cylindrical, annular, circular, elliptical, polygonal, irregularly shaped, hollow, frame-like, box-like, panel-like, etc. Among these, panel-like articles are preferred, and the thickness is, for example, about 1 mm to 5 mm.
[0053] The method for forming the molded article is not particularly limited, and a conventionally known molding method can be adopted, for example, injection molding, injection compression molding, extrusion molding, profile extrusion, transfer molding, hollow molding, gas-assisted hollow molding, blow molding, extrusion blow molding, IMC (in-mold coating molding) molding, rotational molding, multi-layer molding, two-color molding, insert molding, sandwich molding, foam molding, pressure molding, etc. In particular, the resin composition of this embodiment is suitable for molded articles obtained by injection molding, injection compression molding, and extrusion molding. However, it goes without saying that the resin composition of this embodiment is not limited to molded articles obtained by these methods.
[0054] The molded article of the present embodiment is suitable for use in parts for electric and electronic devices, office automation equipment, mobile information terminals, machine parts, home appliances, vehicle parts, various containers, lighting equipment, stationery, office supplies, etc. Among these, it is particularly suitable for use in housings for electric and electronic devices, office automation equipment, information terminal devices, and home appliances, lighting equipment, and vehicle parts (particularly vehicle interior parts), and is particularly suitable for use in vehicle interior parts. EXAMPLES
[0055] The present invention will be described in more detail below with reference to examples. The materials, amounts, ratios, processing contents, processing procedures, etc. shown in the following examples can be appropriately changed without departing from the spirit of the present invention. Therefore, the scope of the present invention is not limited to the specific examples shown below. If the measuring instruments used in the examples are difficult to obtain due to discontinuation or the like, measurements can be made using other instruments with equivalent performance.
[0056] 1. Raw materials The raw materials shown in Table 1 below were used. [Table 1]
[0057] <Production Example 1: Production of Polycarbonate Resin A-2> 26.14 moles (6.75 kg) of bisphenol C (BPC) and 26.79 moles (5.74 kg) of diphenyl carbonate were placed in an aluminum (SUS) reactor (internal volume: 10 L) equipped with a stirrer and a distillate condenser. The inside of the reactor was replaced with nitrogen gas, and the temperature was raised to 220°C in a nitrogen gas atmosphere over 30 minutes. Next, the reaction liquid in the reactor was stirred, and cesium carbonate (Cs2CO3) was added as a transesterification catalyst to the molten reaction liquid at a ratio of 1.5 × 10 -6 The reaction solution was stirred and fermented in a nitrogen gas atmosphere at 220° C. for 30 minutes. Next, the pressure in the reactor was reduced to 100 Torr over 40 minutes at the same temperature, and the reaction was continued for another 100 minutes to distill off phenol. Next, the temperature in the reactor was raised to 284°C over 60 minutes, and the pressure was reduced to 3 Torr, and phenol equivalent to almost the entire theoretical amount was distilled out. Next, the pressure in the reactor was kept below 1 Torr at the same temperature, and the reaction was continued for another 60 minutes to complete the polycondensation reaction. At this time, the stirring speed of the stirrer was 38 rpm, the temperature of the reaction liquid immediately before the end of the reaction was 289°C, and the stirring power was 1.00 kW. Next, the reaction liquid in the molten state was fed into a twin-screw extruder, and p-toluenesulfonate in an amount four times by mole relative to the cesium carbonate was fed from the first feed port of the twin-screw extruder and kneaded with the reaction liquid. Thereafter, the reaction liquid was extruded into strands through the die of the twin-screw extruder and cut with a cutter to obtain pellets of polycarbonate resin A-2.
[0058] <Acid value measurement> The acid value of the polyolefin wax indicates the number of milligrams of potassium hydroxide required to neutralize the acid contained in 1 g of the polyolefin wax, and was measured by a method in accordance with JIS K0070. That is, a precisely weighed sample was dissolved in a mixed solvent of mixed xylene:n-butanol = 1:1 by mass ratio to obtain a sample solution. Next, this sample solution was titrated with a previously standardized N / 10 alcohol solution of potassium hydroxide (7 g of special grade potassium hydroxide was added with 5 g of ion-exchanged water, and the volume was adjusted to 1 L (liter) with primary ethyl alcohol, and the titer was standardized to F with N / 10 hydrochloric acid and 1% phenolphthalein solution), and the titer was calculated from the neutralization amount according to the following formula. Acid value (mgKOH / g) = (N / 10 KOH titration amount (mL) x F x 5.61) / (sample (g) x 0.01)
[0059] 2. Examples 1 to 7 and Comparative Examples 1 to 8 <Compound> The components listed in Table 1 above were blended in the proportions (each component is in parts by mass) listed in Table 2 or Table 3 below, mixed in a tumbler for 20 minutes, and then melt-kneaded using a twin-screw extruder ("TEM-26SX" manufactured by Shibaura Machine Co., Ltd.) at a cylinder temperature of 260°C and a discharge rate of 25 kg / h, and a resin composition (pellets) was obtained by strand cutting.
[0060] <Hue rating (L * )> The pellets obtained above were dried in a hot air circulation dryer at 100°C for 5 hours, and then a flat plate-shaped test piece having an area of 150 x 100 mm and a thickness of 2 mm was obtained using an injection molding machine ("α-2000i-150B" manufactured by Fanuc Corporation) at a cylinder temperature of 270°C and a mold temperature of 70°C.
[0061] The L of the test piece obtained above * The values were measured. L * The L value was measured using a color difference meter SE6000 manufactured by Nippon Denshoku Industries Co., Ltd., in reflection mode, D65, and a 10° field of view, at the center of the flat test piece. * The lower the value, the darker the color.
[0062] <ΔGross60° after scratch test> The pellets obtained above were dried in a hot air circulation dryer at 100°C for 5 hours, and then a flat plate-shaped test piece having an area of 150 x 100 mm and a thickness of 2 mm was obtained using an injection molding machine ("α-2000i-150B" manufactured by Fanuc Corporation) at a cylinder temperature of 270°C and a mold temperature of 70°C.
[0063] The 60-degree specular gloss (Gross60°) was measured in the center of the test piece obtained by the above method using a gloss meter (Nippon Denshoku Industries Co., Ltd., "VG7000") based on JIS Z 8741. The test piece was subjected to an abrasion test using a flat abrasion tester (Daiei Scientific Instruments Co., Ltd., "PA-300A") with a 45R abrasive (Daiei Seisakusho Co., Ltd.) as the abrasive, gauze (Kawamoto Sangyo Co., Ltd., medical gauze type I) as the abrasive cloth, a load of 500g, a speed of 40 times / min, and 500 reciprocations. The 60-degree specular gloss of the scar after the abrasion test was measured, and the difference in 60-degree specular gloss before and after abrasion, ΔGross60°, was calculated. The lower the ΔGross60° value, the better the scratch resistance.
[0064] <Plate appearance> After the scratch test, the appearance of the flat test piece with an area of 150 × 100 mm and a thickness of 2 mm prepared for ΔGross60 was visually inspected and rated as follows. The evaluation was performed by five experts and judged by majority vote. A: The appearance was good. B: Other than A above (poor appearance, etc.)
[0065] <Overall rating> The above L * The overall evaluation was based on ΔGross60° after the scratch test and the appearance of the plate. A:L * The value is 4.5 or less, ΔGross60° is 3.0 or less, and the plate appearance is rated A. B: Other than A and C (e.g., L * The value is more than 4.5 and not more than 6.0, ΔGross60° is more than 3.0 and not more than 7.0, and the plate appearance is rated A, etc.) C:L *At least one of the following is satisfied: value is greater than 6.0, ΔGross60° is greater than 7.0, and plate appearance is rated B.
[0066] [Table 2]
[0067] [Table 3]
[0068] In Tables 2 and 3 above, the proportion (parts by mass) of the pigment itself indicates the proportion (parts by mass) of the pigment in the master batch (ie, the carbon black in the carbon black master batch) relative to 100 parts by mass of the resin component. As is clear from the above results, the resin composition of the present invention is * The value was low, the scratch resistance was excellent, and the plate appearance was also good (Examples 1 to 7). That is, molded products having a good balance of scratch resistance, appearance, and color were obtained. In contrast, when no maleic anhydride modified polyethylene was included (Comparative Example 1) or when the content was small even if the maleic anhydride modified polyethylene was included (Comparative Example 2), the scratch resistance was poor. Furthermore, when the content of maleic anhydride modified polyethylene was high (Comparative Example 3), the scratch resistance was poor and the appearance of the plate was also poor. Furthermore, when acid-unmodified polyethylene was used (Comparative Example 5), when another maleic anhydride copolymer was used (Comparative Example 6), and when an alkene-maleic anhydride copolymer was used (Comparative Examples 7 and 8), the scratch resistance was poor. In particular, when maleic anhydride-modified polypropylene was used, the scratch resistance was remarkably poor, and therefore the effect of the present invention was found to be surprising. On the other hand, when a dye was used instead of a pigment (Comparative Example 4), a molded product having a good balance of scratch resistance, appearance and hue could not be obtained.
Claims
1. A resin composition comprising 100 parts by mass of a polycarbonate resin, 0.3 to 1.5 parts by mass of a maleic anhydride-modified polyethylene, and 0.04 to 2.0 parts by mass of a pigment, wherein the polycarbonate resin contains a structural unit represented by formula (1) in a proportion of 5 mol % or more of all structural units. Formula (1) 【Chemistry 1】 (In formula (1), R 1 represents a methyl group, R 2 represents a hydrogen atom or a methyl group, X 1 represents one of the following formulas: 【Chemistry 2】 R 3 and R 4 each independently represents a hydrogen atom or a methyl group, and Z represents a group that bonds with C to form an alicyclic hydrocarbon having 6 to 12 carbon atoms which may have a substituent.
2. The resin composition according to claim 1 , wherein the polycarbonate resin further comprises a structural unit represented by formula (2): Formula (2) 【Chemistry 3】 (In formula (2), X 2 represents one of the following formulas: 【Chemistry 4】 R 3 and R 4 each independently represents a hydrogen atom or a methyl group, and Z represents a group that bonds with C to form an alicyclic hydrocarbon having 6 to 12 carbon atoms which may have a substituent.
3. The polycarbonate resin contains, among all structural units, 10 to 90 mol % of structural units represented by formula (1) and 90 to 10 mol % of structural units represented by formula (2) (provided that the sum of the structural units represented by formula (1) and the structural units represented by formula (2) does not exceed 100 mol %). The resin composition according to claim 2.
4. 3. The resin composition according to claim 1, wherein the maleic anhydride-modified polyethylene has an acid value of 40 mgKOH / g or more.
5. The resin composition according to claim 1 or 2, wherein the polycarbonate resin comprises a polycarbonate resin obtained by material recycling of a polycarbonate resin containing a structural unit represented by formula (2).
6. The resin composition according to claim 1 or 2, wherein the pigment comprises a black pigment.
7. The polycarbonate resin further contains a structural unit represented by formula (2), The polycarbonate resin contains, among all structural units, 10 to 90 mol % of structural units represented by formula (1) and 90 to 10 mol % of structural units represented by formula (2) (provided that the sum of the structural units represented by formula (1) and the structural units represented by formula (2) does not exceed 100 mol %); 2. The resin composition according to claim 1, wherein the maleic anhydride-modified polyethylene has an acid value of 40 mgKOH / g or more. Formula (2) 【Chemistry 5】 (In formula (2), X 2 represents one of the following formulas: 【Chemistry 6】 R 3 and R 4 each independently represents a hydrogen atom or a methyl group, and Z represents a group that bonds with C to form an alicyclic hydrocarbon having 6 to 12 carbon atoms which may have a substituent.
8. A pellet of the resin composition according to claim 1, 2 or 7.
9. A molded article molded from the resin composition according to claim 1, 2 or 7.
10. A molded article formed from the pellets of claim 8.
Citation Information
Patent Citations
Resin composition, laminate-molded article and recycling method
JP2003253111A
Polycarbonate resin composition and molded article
JP2017071675A
Polycarbonate resin composition and molding
JP2018141077A
Laminate, article and method of manufacturing laminate
JP2020175550A
Polycarbonate resin composition and molding
JP2021127385A