Connection electric wire and manufacturing method for connection electric wire

The method addresses resin dripping and contamination issues by using specific viscosity ranges for curable resins to form a dual-layer sealing layer, ensuring effective sealing and reduced material use, enhancing productivity and environmental resilience.

JP2024143134APending Publication Date: 2024-10-11FURUKAWA ELECTRIC CO LTD +1
View PDF 8 Cites 0 Cited by

Patent Information

Application Number
JP2023055648
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Filing Date
2023-03-30
Publication Date
2024-10-11

AI Technical Summary

Technical Problem

Existing methods for forming sealing layers on connecting wires result in resin dripping, contamination, increased material consumption, and reduced productivity, while failing to provide adequate sealing under harsh environmental conditions.

Method used

A manufacturing method involving the use of a first curable resin liquid with viscosity of 51 to 1500 mPa·s, followed by a second curable resin liquid, such as a photocurable or thermofusible resin, to form a sealing layer with controlled thickness, reducing dripping and enhancing sealing properties.

Benefits of technology

The method produces connecting wires with high sealing performance under normal and harsh environments, minimizing resin consumption and improving productivity.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024143134000001_ABST
    Figure 2024143134000001_ABST
Patent Text Reader

Abstract

To provide a manufacturing method for a connection electric wire, which is highly productive while suppressing contamination due to dripping of resin liquid, and which can further improve the sealing properties of the connection electric wire obtained, and a connection electric wire obtained by the manufacturing method.SOLUTION: A manufacturing method for a connecting electric wire in which a connection portion where conductors of multiple insulated electric wires are connected to each other is sealed with an insulating sealing layer includes the steps of immersing the connecting portion in a first curable resin liquid, pulling out the connecting portion after the immersion, immersing the connecting portion in a second curable resin liquid, and curing the second curable resin liquid, in this order, and the viscosity of the first curable resin liquid is 51 to 1500 mPa s, and the second curable resin liquid contains a photocurable resin and / or a heat-melting resin.SELECTED DRAWING: Figure 1
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to an electric connection wire and a method for manufacturing the electric connection wire. [Background technology]

[0002] In wiring an insulated electric wire, when a branch wire is branched off from a trunk wire, trunk wires are connected in series, or a pine-needle connection is made, the insulating coating layer covering the insulated electric wire is peeled off and the exposed conductor is connected to form a connection. The formed connection is protected by wrapping its outer periphery with insulating tape or by covering it with a connection member such as a splice unit. In particular, when the connection is required to be waterproof, the connection is sealed with an insulating resin or the like to form a sealing layer. In forming the sealing layer, a method has been proposed in which two types of resin liquids (resin materials, resin compositions) with different viscosities are used to fill the gaps between the insulated wires or conductors with resin without leaving any gaps. Specifically, a method is known in which the connection part is immersed in a resin liquid with a lower viscosity, the resin liquid is allowed to penetrate into the small gaps between the insulated wires or conductors with the low-viscosity resin liquid, the resin liquid is hardened, and then the connection part is immersed in a resin liquid with a higher viscosity, and the resin liquid is hardened to form the sealing layer.

[0003] For example, Patent Document 1 proposes a technique for bundling a plurality of electric wires from which the covering has been removed to expose a plurality of core wires, and welding the plurality of core wires to form a welded portion for waterproofing between the plurality of core wires. This waterproofing method involves waterproofing the welded portion with a first sealant having a viscosity of 1 Pa sec or less, and then waterproofing the welded portion with a second sealant having a viscosity of 10 to 70 Pa sec.

[0004] Patent Document 2 discloses a manufacturing method for a wire harness having a splice portion in which conductors are connected to each other and a sealing layer that seals the splice portion, the manufacturing method including a connecting step of connecting the conductors to each other to form the splice portion, a first resin material application step of immersing the splice portion in a first resin material having a first viscosity in an uncured state and then removing the first resin material, a first curing step of curing the first resin material applied to the splice portion, a second resin material application step of immersing the splice portion in a second resin material having a second viscosity in an uncured state and then removing the second resin material, and a second curing step of curing the second resin material applied to the splice portion, wherein the first viscosity is in the range of 10 to 50 mPa s and the second viscosity is set to be higher than the first viscosity. [Prior art documents] [Patent documents]

[0005] [Patent Document 1] JP 2003-9334 A [Patent Document 2] JP 2022-167488 A Summary of the Invention [Problem to be solved by the invention]

[0006] The present inventors have conducted research and found that when manufacturing a connecting electric wire having a sealing layer made of two resin layers, if the sealing layer is formed using a resin liquid having a viscosity of 10 to 50 mPa·s as the first resin, as in the manufacturing method described in the above Patent Document 2, the first resin liquid is likely to drip downward and contaminate the surrounding area during the period from when the splice part (connection part) is immersed in the first resin liquid and pulled up until it is cured, or during the period from when it is pulled up until it is immersed in the second resin liquid. In addition, it has become clear that the amount of resin consumed increases by the amount of the dripping resin liquid, resulting in increased manufacturing costs. In addition, the method described in the above Patent Document 1 proposes a method of filling a cap (protective member) with silicone rubber and immersing and leaving a welded part (connection part) in the silicone rubber to form a waterproof structure, but since it takes a long time for silicone rubber to harden, there are problems such as a need to secure storage space and a decrease in productivity due to work stagnation. Also, in order to prevent the liquid silicone rubber before hardening from leaking from the cap, it is necessary to use a cap with a long overall length, which is also a factor that reduces the degree of freedom in wiring the connecting wires. Furthermore, when the connecting wire is used for applications such as a wire harness, it is expected that the connecting wire will be used under severe environmental conditions, and therefore a sealing performance higher than that of conventional wires is required.

[0007] In view of the above problems, the present invention aims to provide a method for manufacturing a connecting electric wire, which is highly productive while suppressing contamination due to dripping of resin liquid, and which can further improve the sealing properties of the resulting connecting electric wire, and a connecting electric wire obtained by the manufacturing method. [Means for solving the problem]

[0008] As a result of intensive research by the inventors to solve the above problems, in manufacturing a connecting electric wire having a sealing layer formed on a connecting portion, by setting the viscosity of the first curable resin liquid within a specific range, it is possible to suppress the first curable resin liquid from dripping down even when the connecting portion is immersed in the first curable resin liquid and then pulled up, and the consumption of the first curable resin liquid can be reduced, and since the first curable resin liquid can be attached to the connecting portion while maintaining a sufficient amount, the thickness of the layer made of the first curable resin obtained by curing the resin liquid can be controlled to be thick, and by making the second curable resin liquid contain a light (ultraviolet) curable resin and / or a heat-melting resin, it is possible to reduce manufacturing costs, and further, it is possible to obtain a connecting electric wire that can seal and protect the connecting portion at a sufficiently high level even in harsh environments. Based on these findings, further research was conducted and the present invention was completed.

[0009] That is, the above problems were solved by the following means. <1> A method for manufacturing a connecting electric wire in which a connection portion in which conductors of a plurality of insulated electric wires are connected to each other is sealed with an insulating sealing layer, comprising the steps of: Immersing the connection portion in a first curable resin liquid; removing the connection portion after the immersion; immersing the connection portion in a second curable resin liquid; and a step of curing the second curable resin liquid, in this order. The viscosity of the first curable resin liquid is 51 to 1500 mPa·s, and the second curable resin liquid contains a photocurable resin and / or a heat-fusible resin. A method for manufacturing a connecting wire. <2> The thickness of the layer made of the first curable resin formed by curing the first curable resin liquid is 30 to 300 μm. <1> The manufacturing method described in <3> The viscosity of the first curable resin liquid is 80 to 1000 mPa·s, and the thickness of the layer made of the first curable resin obtained by curing the first curable resin liquid is 42 to 230 μm. <1> or <2> The manufacturing method described in <4> The viscosity of the second curable resin liquid is higher than the viscosity of the first curable resin liquid. <1> ~ <3> 13. A method for producing a connecting wire according to any one of claims 1 to 12. <5> The first curable resin liquid contains a photocurable resin. <1> ~ <4> 13. A method for producing a connecting wire according to any one of claims 1 to 12. <6> The first curable resin liquid contains a moisture curable resin. <1> ~ <5> 13. A method for producing a connecting wire according to any one of claims 1 to 12. <7> The first curable resin liquid contains an anaerobic curable resin. <1> ~ <6> 13. A method for producing a connecting wire according to any one of claims 1 to 12. <8> The second curable resin liquid is filled into a protective member before use. <1> ~ <7> 13. A method for producing a connecting wire according to any one of claims 1 to 12. <9> The connecting wire is a wire harness. <1> ~ <8> 13. A method for producing a connecting wire according to any one of claims 1 to 12. <10> A connecting wire in which a connection portion where conductors of a plurality of insulated wires are connected to each other is sealed with an insulating sealing layer, The sealing layer has a layer made of a first curing resin and a layer made of a second curing resin covering the layer made of the first curing resin, the layer made of the first curing resin has a thickness of 30 to 300 μm, and the second curing resin contains a photocurable resin and / or a heat-meltable resin. <11> The thickness of the layer made of the first cured resin is 42 to 230 μm. <10> The connecting wire described in <12> The first curable resin includes a photocurable resin. <10> or <11> The connecting wire described in <13> The first curable resin includes a moisture curable resin. <10> ~ <12> 2. A connecting wire according to any one of claims 1 to 11. <14> The first curable resin includes an anaerobic curable resin. <10> ~ <13> 2. A connecting wire according to any one of claims 1 to 11. <15> The sealing layer is covered with a protective member. <10> ~ <14> 2. A connecting wire according to any one of claims 1 to 11. <16> The connecting wire is a wire harness. <10> ~ <15> 2. A connecting wire according to any one of claims 1 to 11.

[0010] In the present invention, a numerical range expressed using "to" means a range including the numerical values ​​before and after it as the lower limit and upper limit. Effect of the Invention

[0011] According to the method for producing a connecting wire of the present invention, a connecting wire capable of sealing and protecting a connection at a sufficiently high level not only in normal environments but also in harsh environments can be obtained with excellent productivity. The connecting wire of the present invention can seal and protect a connection at a sufficiently high level not only in normal environments but also in harsh environments, and has excellent productivity. [Brief description of the drawings]

[0012] [Figure 1] 1 is a schematic diagram showing an embodiment of a connecting wire of the present invention. [Diagram 2] 1 is a schematic diagram showing a cross-sectional view of one embodiment of a connecting wire of the present invention. [Diagram 3] 1A to 1C are explanatory diagrams illustrating an embodiment of a method for producing an electric connector according to the present invention. [Figure 4] FIG. 4 is an explanatory diagram illustrating an example of a method for producing a connector wire, which is not the production method of the present invention. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0013] Preferred embodiments of the present invention will be described below, but the present invention is not limited to the following embodiments except as defined in the present invention.

[0014] [Method of manufacturing connection wire] The method for manufacturing a connecting electric wire of the present invention (hereinafter also referred to as the manufacturing method of the present invention) includes, in this order, a step of immersing a connection portion in which the conductors of multiple insulated electric wires are connected to each other in a first curable resin liquid, a step of lifting the connection portion after the immersion, a step of immersing the connection portion in a second curable resin liquid, and a step of curing the second curable resin liquid attached to the connection portion. In the manufacturing method of the present invention, the viscosity of the first curable resin liquid is controlled to 51 to 1500 mPa·s, and the second curable resin liquid contains a photocurable resin and / or a heat-fusible resin.

[0015] Hereinafter, a preferred embodiment of the present invention will be described with reference to the drawings. Note that the present invention is not limited to the embodiments shown below, except as specified in the present invention. In addition, the description of the connecting wires and the like described with reference to the drawings below is not limited to the forms shown in the drawings, but is applied as a description of the configuration or invention-specific matters of the present invention.

[0016] FIG. 1 is a schematic diagram showing an embodiment of a connection wire obtained by the manufacturing method of the present invention. In the connection wire 1, the covering 12 at the ends of a plurality of insulated electric wires 10 is peeled off, and the exposed conductors 11 are connected to each other to form a connection 13. The connection 13 is sealed by an insulating sealing layer 20. In this specification, the region from the connection to the conductor where no connection is formed and the covering is also collectively referred to as a "connection, etc." In addition, in the connection, etc., all of the conductors in the part where the insulating covering layer is peeled off may form a connection (there may be no conductor where no connection is formed). In the present invention, "the connection where the conductors of a plurality of insulated electric wires are connected to each other is sealed by an insulating sealing layer" means that the region including the connection is sealed by an insulating sealing layer. In other words, it means that the above-mentioned connection is sealed by an insulating sealing layer. Fig. 2 is a schematic cross-sectional view taken along the dashed line of the electric connection wire 1 shown in Fig. 1. The sealing layer 20 has a layer made of a first cured resin 22 and a layer made of a second cured resin 24. 1 and 2 show a connecting wire 1 in which seven insulated wires 10 having a circular cross section are connected, but in the present invention, the number of insulated wires 10 to be connected is not particularly limited. In addition, in Fig. 1 and 2, the conductor portions 11 are connected to each other using a crimp terminal 14 to form a connection portion 13, but in the present invention, the method of connecting the conductor portions 11 to each other is not particularly limited.

[0017] Fig. 3 shows one embodiment of the manufacturing method of the present invention. Also, Fig. 4 shows one example of a manufacturing method of an electric connecting wire that is not the manufacturing method of the present invention. Note that the viscosity of the first hardening resin liquid 21 shown in Fig. 3 is 51 to 1500 mPa·s, and the viscosity of the first hardening resin liquid 21' shown in Fig. 4 is 10 to 50 mPa·s. FIG. 3(A) shows a process of immersing the connection portion 13 of the insulated electric wire 10 in the first curable resin liquid 21 filled in a container (a process of immersing in the first curable resin liquid). FIG. 3(B) shows a process of immersing the connection portion 13 in the first curable resin liquid 21 and then lifting the connection portion 13 from the container filled with the first curable resin liquid 21 (a process of lifting the connection portion after immersion). Since the viscosity of the first curable resin liquid 21 used in the manufacturing method of the present invention is controlled to a range of 51 to 1500 mPa·s, as shown in FIG. 3(B), the first curable resin liquid 21 does not drip to the bottom and a sufficient amount of the first curable resin liquid 21 adheres to the connection portion 13. The first curable resin liquid 21 may be cured before being immersed in the second curable resin liquid 23, or may be moved to the process of immersing in the second curable resin liquid 23 without being cured. FIG. 3(C) shows a process of immersing the connection portion 13 etc. in an insulating cap (protective member) 25 filled with a second curable resin liquid 23 (a process of immersing in a second curable resin liquid), and then a process of hardening the second curable resin liquid 23 to form a second curable resin 24 (a process of hardening the second curable resin liquid). On the other hand, in FIG. 4 showing an example of a method for manufacturing a connecting wire that is not the method of the present invention, the viscosity of the first curable resin liquid 21' shown in FIG. 4(A) is 10 to 50 mPa·s. Therefore, as shown in FIG. 4(B), after the connection portion 13 and the like are pulled up from a container filled with the first curable resin liquid 21, a part of the first curable resin liquid 21' drips down, and the first curable resin liquid 21' moves downward to form a long, teardrop-like shape. Therefore, as shown in FIG. 4(C), an insulating cap 25 filled with the second curable resin liquid 23 is used that is longer in length to match the shape of the first curable resin liquid 21', and the amount of the second curable resin liquid 23 filled is also increased. The characteristic features of the manufacturing method of the present invention will be described below.

[0018] <Insulated wire> The insulated wire used in the manufacturing method of the present invention is not particularly limited, and may be, for example, an insulated wire commonly used for automobile wire harnesses, etc. The insulated wire has a conductor and an insulating coating layer that covers the outer periphery of the conductor.

[0019] (conductor) The shape and material of the conductor of the insulated wire are not particularly limited as long as it functions as a conductor. For example, the conductor may have a shape and material used in insulated wires used in wire harnesses for automobiles. The conductor may be a single wire or a twisted wire, a bare wire, or a plated or enamel-coated wire. Metal materials forming the conductor include soft copper, copper alloy, aluminum, etc.

[0020] (insulating coating layer) The type of the insulating coating layer of the insulated wire is not particularly limited as long as it has the desired insulating properties. For example, insulating resins used in wire harnesses for automobiles can be used. The insulating coating layer is preferably an extrusion coating layer formed by extrusion coating an insulating thermoplastic resin or a composition containing the resin. The thickness of the insulating coating layer is not particularly limited, and is usually about 0.15 to 5 mm.

[0021] (Connection) In one embodiment of the manufacturing method of the present invention, as shown in Figures 1 and 2, the insulating coating layer (coating portion) at the tip of the multiple insulated electric wires is peeled off to expose the conductors, and the conductors are connected to each other to form a connection portion. There are no particular limitations on the method for forming the connection portion, as long as the conductors are electrically connected to each other. For example, arc welding, laser welding, ultrasonic bonding, etc. may be used, or a crimp connection using a crimp terminal such as a P-type sleeve or a B-type sleeve may be used.

[0022] <Sealing layer> In the manufacturing method of the present invention, the insulating sealing layer has a layer made of a first curable resin formed by curing a first curable resin liquid, and a layer made of a second curable resin formed by curing a second curable resin liquid, which covers the periphery of the first curable resin layer. In the manufacturing method of the present invention, the layer made of the first curable resin is formed by dip coating, in which the connection portion is immersed in the first curable resin liquid and then pulled up. The process of forming the sealing layer is described below.

[0023] <Step of immersing in first curable resin liquid> In the manufacturing method of the present invention, the layer made of the first curing resin among the sealing layers of the obtained connecting electric wire is formed by immersing the connection part, etc. in the first curing resin liquid filled in a container, pulling it out, and then curing it. The resin contained in the first curing resin liquid includes a curing resin (resin composition) that forms the first curing resin by curing, which will be described later. For example, a photo (ultraviolet) curing resin, a moisture curing resin, an anaerobic curing resin, a thermosetting resin, etc. can be used. The connection parts and the like are preferably immersed in the first curable resin liquid so that the covering part is covered with the first curable resin liquid for 5 mm or more from the boundary with the exposed conductor part. The immersion time can be appropriately set according to the viscosity of the first curable resin liquid so that the first curable resin liquid penetrates into small gaps (details) of the connection parts and the like. For example, the immersion time can be 1 minute or less, 30 seconds or less, or 10 seconds or less. Usually, the immersion time is preferably 1 second or more.

[0024] The viscosity of the first curable resin liquid is 51 to 1500 mPa·s as described above. By setting the viscosity within such a range, when the connection part or the like is immersed in the first curable resin liquid and then pulled up, the first curable resin liquid is held attached to the connection part or the like, and the liquid can be prevented from moving downward, and excessive dripping can be suppressed. From the viewpoint of more reliably holding the first curable resin liquid and preventing it from moving downward, and further preventing excessive dripping, the viscosity of the first curable resin liquid is preferably 70 mPa·s or more, more preferably 80 mPa·s or more, even more preferably 100 mPa·s or more, and even more preferably 125 mPa·s or more. In addition, from the viewpoint of permeating the first curable resin liquid into the fine parts of the connection part or the like in a short time, the viscosity of the first curable resin liquid is preferably 1300 mPa·s or less, more preferably 1000 mPa·s or less, and even more preferably 800 mPa·s or less. A preferred range of the viscosity is 70 to 1300 mPa·s, more preferably 80 to 1000 mPa·s, even more preferably 100 to 1000 mPa·s, and still more preferably 125 to 800 mPa·s.

[0025] In the present invention, the viscosity of the curable resin liquid is the viscosity at the temperature of the resin liquid at the time when the connection part is immersed. The viscosity at the temperature can be measured, for example, by a B-type viscometer (for example, manufactured by Eiko Seiki Co., Ltd., product name: Digital Viscometer DVNext). A B-type viscometer is a type of rotational viscometer in which a rotor called a spindle rotor is immersed in the liquid and rotated by a motor to measure the flow resistance. When using a B-type viscometer, the measurement can be performed by adjusting the rotation speed (0.01 to 250 rpm) so that the torque range (%) is within the range of 10 to 100% using a spindle attached to the digital viscometer DVNext (model number: LV DVNX). In addition, for example, when the curable resin liquid is a commercially available product, the viscosity can be the viscosity described in the pamphlet of the commercially available product. Furthermore, the temperature may be, for example, room temperature in the manufacture of the connecting wire of the present invention, and when a photo-(ultraviolet) curable resin, moisture curable resin, or anaerobic curable resin is used as the curable resin liquid, the viscosity may be the viscosity at 25°C.

[0026] <Process of pulling up the connection part after immersion> The connection parts and the like immersed in the first curable resin liquid filled in the container are then pulled out from the container. When the pulling speed is sufficiently slow and the viscosity of the resin liquid is low, the thickness of the resin liquid by dip coating is governed by the viscosity of the liquid and the surface tension at the gas-liquid interface. Therefore, the following relational expression is established for the thickness (h, unit: m):

[0027] TIFF2024143134000002.tif20170

[0028] In the above formula (1), the parameters are as follows: U: Pulling speed (m / s) η: Viscosity of the curable resin liquid (Pa s = kg m / s) ρ: Density of the curable resin liquid (kg / m 3 ) γ: Surface tension of curable resin liquid (N / m) g: Gravitational acceleration (m / s 2 )

[0029] The lifting speed can be appropriately set according to the viscosity, density, and surface tension of the first curable resin liquid, and the thickness of the layer made of the first curable resin to be formed. From the viewpoint of ensuring a sufficient amount of the first curable resin liquid to be attached to the connection portion, etc., the lifting speed is preferably 150 mm / min or less, more preferably 100 mm / min or less, and even more preferably 80 mm / min or less. From the viewpoint of increasing the production speed, the speed is preferably 10 mm / min or more, more preferably 30 mm / min or more, and even more preferably 50 mm / min or more. The preferred range of the speed is 10 to 150 mm / min, more preferably 30 to 100 mm / min, and even more preferably 50 to 80 mm / min.

[0030] The manufacturing method of the present invention may further include a step of curing the first curable resin liquid in the step of pulling up the connection portion after immersion (i.e., after the connection portion, etc., is immersed in the first curable resin liquid and then pulled up, and before being immersed in the second curable resin liquid), or may not include a step of curing the first curable resin liquid. In the case where a process of curing the first curable resin liquid is included between immersing the connection part, etc. in the first curable resin liquid and pulling it out and immersing it in the second curable resin liquid, the first curable resin liquid is cured to become the first curable resin at the stage of immersion in the second curable resin liquid, and therefore a clear interface is formed between the layer made of the first curable resin and the layer made of the second curable resin in the resulting connecting electric wire.

[0031] <Step of immersing in second curable resin liquid> In the manufacturing method of the present invention, the layer made of the second curable resin in the sealing layer of the obtained connecting electric wire is formed by immersing the connection part after the step of lifting the connection part after the immersion in a second curable resin liquid and then curing it. The second curable resin liquid contains a light (ultraviolet) curable resin and / or a heat-fusible (hot melt) resin as described above. The resin liquid is cured to form a layer made of the second curable resin described below. In the manufacturing method of the present invention, by making the second curable resin liquid contain a photocurable resin and / or a heat-meltable resin, the second curable resin liquid can be cured quickly in the step of curing the second curable resin liquid following this step, and the time required for manufacturing the connecting wire can be shortened. In addition, for example, when the second curable resin liquid is filled into a protective member as described below and cured while being filled in the protective member, the second curable resin liquid can be cured quickly by light irradiation or cooling, so there is little risk of the resin liquid leaking from the protective member, and the size of the protective member can be made smaller.

[0032] The connection portions are preferably immersed in the second hardening resin liquid to a position where the first hardening resin liquid or the first hardening resin adhering to the connection portions and the like is completely covered.

[0033] The viscosity of the second curable resin liquid is not particularly limited, and is preferably higher than the viscosity of the first curable resin liquid from the viewpoint of preventing dripping. For example, the viscosity of the second curable resin liquid is preferably 200 mPa·s or more higher than the viscosity of the first curable resin liquid, more preferably 400 mPa·s or more higher, and also preferably 600 mPa·s or more higher. The viscosity of the second curable resin liquid is preferably 400 to 10,000 mPa·s, more preferably 500 to 8,000 mPa·s, even more preferably 600 to 7,000 mPa·s, and even more preferably 700 to 6,000 mPa·s.

[0034] The second curable resin liquid may be filled in, for example, an insulating protective member (insulating cap, etc.). This allows the second curable resin liquid to be cured together with the protective member, and the sealing layer can be effectively protected by the protective member. The material of the protective member is not particularly limited, and for example, the protective member described below can be used.

[0035] <Step of curing the second curable resin liquid> The method of curing the second curable resin liquid can be appropriately set depending on the type of the second curable resin liquid. For example, when the second curable resin liquid is a light (ultraviolet) curable resin liquid, the resin liquid can be cured by irradiating the resin liquid with light (ultraviolet). When the second curable resin liquid is a heat-fusible resin, the resin liquid can be cured by cooling (or leaving it at room temperature). Furthermore, in the case where the step of lifting up the connection portion after immersion in the first curable resin liquid does not include a step of curing the first curable resin liquid, the first curable resin liquid and the second curable resin liquid can be cured simultaneously in this step. For example, when the first curable resin liquid and the second curable resin liquid are both light (ultraviolet) curable resins, the first curable resin liquid and the second curable resin liquid can be cured at once by irradiating light (ultraviolet) rays, so that the time required for manufacturing can be shortened. In addition, when the first curable resin liquid is a moisture curable resin or an anaerobic curable resin and the second curable resin liquid is a light (ultraviolet) irradiable resin, the second curable resin liquid is cured by irradiating light (ultraviolet) rays to stabilize the shape of the sealing layer, and the first curable resin inside naturally hardens over time while maintaining the shape of the sealing layer. Furthermore, for example, when the first curable resin liquid is a moisture curable resin or an anaerobic curable resin and the second curable resin liquid is a heat-melting resin, by cooling the second curable resin liquid to harden the second curable resin liquid and stabilize the shape of the sealing layer, the first curable resin inside naturally hardens over time while maintaining the shape of the sealing layer. Note that, for example, when the second curable resin liquid is a heat-melting resin liquid, it is preferable that the first curable resin liquid is a curable resin having a wide usable temperature range (for example, -40 to 100°C, -40 to 120°C, -40°C to 150°C, -40°C to 200°C, etc.).

[0036] [Connecting wire] The electric connector of the present invention is an electric connector manufactured by the manufacturing method of an electric connector of the present invention. Therefore, the details of the insulated wires and the connection part of the insulated wires used in the electric connector of the present invention are as described above. The connecting wire of the present invention has conductors of a plurality of insulated wires connected together at connection portions, and the connection portions are sealed with an insulating sealing layer, the sealing layer having a layer made of a first cured resin and a layer made of a second cured resin covering the layer made of the first cured resin, the layer made of the first cured resin having a thickness of 30 to 300 μm, and the second cured resin containing a photocurable resin and / or a heat-meltable resin.

[0037] <Sealing layer> The electric connecting wire of the present invention has a sealing layer for sealing the connection portion. The sealing layer has a layer made of a first cured resin and a layer made of a second cured resin covering the first cured resin layer.

[0038] (1st cured resin) The layer made of the first curable resin is a layer formed by sealing (covering) the connection portion with an insulating resin. The type of the first curable resin is not particularly limited, and is a cured resin formed by curing the first curable resin liquid, and preferably includes, for example, a light (ultraviolet) curable resin, a moisture curable resin, an anaerobic curable resin, a thermosetting resin, or the like.

[0039] Examples of the photo (ultraviolet) curable resin include a resin obtained by photocuring a composition having a photoradical polymerization initiator and a compound capable of radical polymerization by the action of the photoradical polymerization initiator (radical polymerizable compound), and a resin obtained by photocuring a composition having a photocationic polymerization initiator and a compound capable of cationic polymerization by the action of the photocationic polymerization initiator (cationic polymerizable compound).

[0040] Moreover, the light (ultraviolet) curable resin is more preferably a cured product of a dark curable resin that cures even in areas not directly exposed to light. Specifically, it is preferable for the dark curable resin to be a resin in which a long-life active compound is generated by light irradiation (ultraviolet irradiation), the active compound diffuses into the curable resin liquid, and acts on a radical polymerization initiator that is not directly exposed to light to generate radicals and cure the curable resin liquid.

[0041] Examples of the thermosetting resin include a resin obtained by thermally curing a composition having a thermal radical polymerization initiator and a radical polymerizable compound, and a resin obtained by thermally curing a composition having a thermal cationic polymerization initiator and a cationic polymerizable compound. The thermosetting resin may also be a cured product of a thermosetting phenolic resin, an epoxy resin, a urethane resin, a urea resin, an alkyd resin, or the like.

[0042] The anaerobically curable resin is stable in air and can be cured by contacting with metal ions in the absence of oxygen. The moisture-curing resin may be a resin that is cured by contacting with moisture in the air or the like.

[0043] Specific examples of the first cured resin include cyanoacrylate resin, acrylic resin, epoxy resin, silicone resin, urethane resin, polyamide resin, fluororesin, polyvinyl butyral resin, phenolic resin, polyimide resin, acrylic rubber, polyester resin, modified polyolefin resin, etc., and the cured resin may be composed of one or more of these. The first curable resin preferably includes the photo (ultraviolet) curable resin, moisture curable resin, or anaerobic curable resin. The photo (ultraviolet) curable resin is preferably an acrylic resin. The moisture curable resin is preferably a cyanoacrylate resin or a silicone resin, more preferably a cyanoacrylate resin. The anaerobic curable resin is preferably an acrylic resin (e.g., an acrylic acid ester resin).

[0044] In the electric connecting wire of the present invention, the thickness of the layer made of the first curable resin is 30 to 300 μm as described above. By controlling the viscosity of the first curable resin liquid to 51 to 1500 mPa·s, the connection part is pulled up from the first curable resin liquid and the first curable resin liquid is cured, whereby the thickness of the layer made of the first curable resin can be obtained. From the viewpoint of further improving the sealing property, the thickness of the layer is preferably 37 μm or more, more preferably 42 μm or more, even more preferably 47 μm or more, and even more preferably 55 μm or more. From the same viewpoint, the thickness of the layer is preferably 275 μm or less, more preferably 230 μm or less, and even more preferably 200 μm or less. The thickness is preferably in the range of 37 to 275 μm, more preferably 42 to 230 μm, even more preferably 47 to 230 μm, and even more preferably 55 to 200 μm.

[0045] The "thickness of the layer made of the first cured resin" means the minimum distance between the outermost surface of the connection part and the outermost surface of the layer made of the first cured resin in a cross section perpendicular to the longitudinal direction of the insulated electric wire so as to include the connection part. For example, in Figs. 1 and 2, the connection part is connected by a crimp terminal, so that the "thickness of the layer made of the first cured resin" is the minimum distance between the outermost surface of the crimp terminal and the outermost surface of the layer made of the first cured resin. Also, for example, when conductors are joined by ultrasonic bonding, the "thickness of the layer made of the first cured resin" is the minimum distance between the outermost surface of the joined conductors and the outermost surface of the layer made of the first cured resin. The thickness can be the thickness calculated by the above formula (1), or the thickness can be confirmed by cutting the resulting connecting wire perpendicular to the longitudinal direction of the insulated wire so as to include the joint, edging the cross section, and then examining the cross section with an optical microscope or a microscope.

[0046] (Second cured resin) The layer made of the second cured resin is an insulating cured resin layer that covers the surface of the layer made of the first cured resin that seals the connection portion. In the electric wire connection of the present invention, the second cured resin contains a light (ultraviolet) curable resin and / or a heat-melting resin. The light (ultraviolet) irradiated resin is the same as that described in the first curing resin. From the viewpoint of the thermal effect on the coating insulating layer of the insulated electric wire, it is preferable to use a resin having a softening point in the range of about 50 to 180°C as the heat-melting resin, and in addition to polyolefin resins such as polyethylene and polypropylene, ethylene-vinyl acetate copolymers, ethylene-ethyl acrylate copolymers, and acid-modified polyolefins such as maleic acid can be suitably used. In the present invention and this specification, the "heat-melting resin" means a resin in a state in which the heat-melting resin is solidified by lowering the temperature after being heat-melted.

[0047] The first and second curable resins may be the same or different. For example, when the first curable resin is a light (ultraviolet) curable resin, by making the second curable resin also a light (ultraviolet) curable resin, the first curable resin and the second curable resin can be cured simultaneously by irradiation with light (ultraviolet). In addition, for example, when the first curing resin is a light (ultraviolet) curing resin, a moisture curing resin, or an anaerobic curing resin, the second curing resin can be, for example, a heat-melting resin. From the viewpoint of adhesion with the first curing resin, the heat-melting resin is preferably a heat-melting resin having a polar group, such as modified polyolefin, polyurethane, polyester, or polyamide, and from the viewpoint of heat resistance, a heat-melting resin such as modified polypropylene, polyester, or polyamide is more preferable.

[0048] The sealing layer may have an insulating protective member (such as an insulating cap) on its outermost layer, and the sealing layer may be covered with the protective member. When the sealing layer has the protective member, the connection parts and the like can be protected more effectively. The material constituting the protective member is not particularly limited, and materials generally used in forming a sealing layer can be used. Protective members available on the market can also be used. For example, protective materials such as (crosslinked) polyethylene, polypropylene, vinyl chloride, polyethylene terephthalate, and polycarbonate are preferable. When crosslinked polyethylene is used as the protective member, it can be shrunk by heating with a hot dryer or the like. Therefore, the outer diameter of the protective member can be reduced by inserting the conductor part of the connecting wire into the crosslinked polyethylene protective member and then heating and shrinking it, which not only improves the vehicle mountability but also reduces the amount of resin filled in the protective member. In addition, since the inside of the protective member may be filled with a second curable resin liquid and may be used as is to form a sealing layer and then cured, for example, when the second curable resin is a light (ultraviolet) curable resin, it is preferable to use a material with high light transmittance such as polyethylene, polypropylene, etc. In addition, when the second curable resin is a heat-melting resin, it is preferable to use a material with high heat resistance such as cross-linked polyethylene, polyethylene terephthalate, polycarbonate, etc.

[0049] The connecting wire of the present invention is preferably used for a wire harness (preferably an automobile wire harness). In the present invention and this specification, the wire harness is a general term for a bundle of electric wires arranged in various places of a vehicle, such as an engine room, an instrument panel, and inside a door, according to environmental performance. EXAMPLES

[0050] The present invention will be described in more detail based on the following examples and comparative examples, but the present invention is not limited to these.

[0051] Details of the resins used in this example were as follows: <First curable resin liquid> Cyanoacrylate adhesive (moisture-curing, odorless, non-whitening instant adhesive, product number: Z84X (referred to as "Z84X" in the table below), viscosity 60 mPa s, manufactured by Alteco) Cyanoacrylate adhesive (moisture-curing, general-purpose instant adhesive, product name: ThreeBond 1743 (referred to as "1743" in the table below), viscosity: 100 mPa s, manufactured by ThreeBond Co., Ltd.) Cyanoacrylate adhesive (moisture curing, high peel strength, impact resistant instant adhesive, product name: ThreeBond 1733 (referred to as "1733" in the table below), viscosity: 150 mPa s, manufactured by ThreeBond Co., Ltd.) Cyanoacrylate adhesive (moisture-curing, general-purpose instant adhesive, product name: ThreeBond 1745 (referred to as "1745" in the table below), viscosity: 500 mPa s, manufactured by ThreeBond Co., Ltd.) Cyanoacrylate adhesive (moisture-curing, impact-resistant and heat-resistant instant adhesive, product name: ThreeBond 1783 (referred to as "1783" in the table below), viscosity: 800 mPa s, manufactured by ThreeBond Co., Ltd.) Cyanoacrylate adhesive (moisture-curing, instant adhesive, product name: ThreeBond 7786 (referred to as "7786" in the table below), viscosity: 1000 mPa s, manufactured by ThreeBond Co., Ltd.) Cyanoacrylate adhesive (moisture-curing, highly moisture-resistant instant adhesive, product name: ThreeBond 1757 (referred to as "1757" in the table below), viscosity: 1200 mPa s, manufactured by ThreeBond Co., Ltd.) Cyanoacrylate adhesive (moisture curing, high peel strength, impact resistant instant adhesive, product name: ThreeBond 1735 (referred to as "1735" in the table below), viscosity: 1500 mPa s, manufactured by ThreeBond Co., Ltd.) Light-curing adhesive (product number: AY-4856 (referred to as "AY4856" in the table below)), viscosity: 100 mPa s, manufactured by Alteco) Acrylate adhesive (ultraviolet-curable resin, product name: ThreeBond 3021J (referred to as "3021J" in the table below), viscosity: 135 mPa s, manufactured by ThreeBond Co., Ltd.) Acrylate adhesive (ultraviolet-curable resin, product name: ThreeBond 3094B (referred to as "3094B" in the table below), viscosity: 150 mPa s, manufactured by ThreeBond Co., Ltd.) Acrylate adhesive (ultraviolet-curable resin, product name: ThreeBond 3042B (referred to as "3042B" in the table below), viscosity: 500 mPa s, manufactured by ThreeBond Co., Ltd.) Acrylate adhesive (ultraviolet-curable resin, product name: ThreeBond 3003J (referred to as "3003J" in the table below), viscosity: 1300 mPa s, manufactured by ThreeBond Co., Ltd.) Cyanoacrylate adhesive (moisture curing, instant adhesive for bonding metal, product name: ThreeBond 1702 (referred to as "1702" in the table below), viscosity: 35 mPa s, manufactured by ThreeBond Co., Ltd.) Cyanoacrylate adhesive (moisture-curing, light-curing, product name: LOCTITE 4304 (referred to as "4304" in the table below), viscosity: 35 mPa s, manufactured by Henkel) Methacrylate ester adhesive (anaerobic curing, anaerobic sealant, product name: ThreeBond 1344J (referred to as "1344J" in the table below), viscosity: 650 mPa s, manufactured by ThreeBond Co., Ltd.) The above viscosities are all measured at room temperature (25° C.). <Second hardening resin liquid> Acrylate adhesive (ultraviolet-curable resin, product name: ThreeBond 3006D (referred to as "3006D" in the table below), viscosity: 2.0 Pa s, manufactured by ThreeBond Co., Ltd.) Light-curing adhesive (product number: AY-4031 (referred to as "AY4031" in the table below), viscosity: 6000 mPa s, manufactured by Alteco) Hot melt adhesive (main component: polyamide resin, product number: TEC7785-12 (referred to as "7785-12" in the table below), softening point: 155°C, viscosity (180°C): 5500mPa s, manufactured by Sanyo Life Materials Co., Ltd.) The viscosities of the acrylate adhesive and the photocurable adhesive are both measured at room temperature (25°C), and the viscosity of the hot melt adhesive is measured at 180°C.

[0052] Example 1 Three 0.75 sq copper wires (insulated wires) with a total length of 200 mm and three 0.75 sq aluminum wires (insulated wires) with a total length of 200 mm were used, and the polyvinyl chloride (PVC) insulating coating layer was removed within a range of 15 mm from one end of each wire to expose the conductor. The conductors were then joined together using an ultrasonic joining machine (manufactured by Nippon Avionics Co., Ltd.) to form a connection. The cyanoacrylate adhesive (product name: Z84X) shown in Table 1 below was used as the first curable resin liquid. The acrylate adhesive (product name: ThreeBond 3006D) shown in Table 1 below was used as the second curable resin liquid, and was filled in a polypropylene container in advance. Under a condition of 25°C, the connection part was immersed in the first curable resin liquid for 5 seconds to a position where the coated part was immersed by about 5 mm, and then pulled up at a pulling speed of 100 mm / min. 10 seconds after being pulled up, the connection part was immersed in the second curable resin liquid in the same manner while still attached to the first curable resin liquid, and the polypropylene container was exposed to ultraviolet light with an intensity of 1000 mW / cm. 2 The second curable resin liquid was cured by irradiating ultraviolet light at 400 K for 30 seconds. Thus, a connecting electric wire was obtained, which is made of a plurality of insulated electric wires whose connecting parts are sealed with resin. The first curable resin liquid naturally hardens while the connecting electric wire obtained is left at room temperature. Thus, the connecting electric wire of the present invention is obtained, in which a layer made of the first curable resin is formed in contact with the connecting parts, and a layer made of the second curable resin is formed in contact with the layer made of the first curable resin.

[0053] (Examples 2 to 14, 19) A connecting wire was produced in the same manner as in Example 1, except that the first curable resin liquid and the second curable resin liquid were the curable resin liquids shown in the following Table 1. In Example 4, a mixed liquid (shown as "1743, 1733" in the following Table 1) in which a cyanoacrylate adhesive (product name: ThreeBond 1743) and a cyanoacrylate adhesive (product name: ThreeBond 1733) were mixed in a mass ratio of 1:1 was used as the first curable resin liquid. The first curable resin liquid in Examples 2 to 9 and 19 naturally cures while the resulting electric connecting wire is left at room temperature, and the first curable resin liquid in Examples 10 to 14 cures together with the second curable resin liquid by ultraviolet irradiation.

[0054] (Examples 15 and 16) The first curable resin liquid and the second curable resin liquid were the curable resin liquids shown in Table 1 below, and the connection parts and the like were immersed in the first curable resin liquid and pulled out, and then left to stand for 4 hours (Example 15) before being immersed in the second curable resin liquid, or the ultraviolet intensity was 1000 mW / cm. 2 A connecting wire was produced in the same manner as in Example 1, except that a step of curing the first curable resin liquid was added by irradiating the first curable resin liquid with ultraviolet light at 1000 rpm for 30 seconds (Example 16).

[0055] (Example 17) In the same manner as in Example 1, partial areas of the conductor portions of the three copper electric wires and the three aluminum electric wires were ultrasonically joined to form connection portions. As the first curable resin liquid, a cyanoacrylate adhesive (product name: ThreeBond 1743) shown in Table 1 below was used. As the second curable resin liquid, a hot melt adhesive (product name: TEC7785-12) shown in Table 1 below was dissolved in advance at 180°C and filled into a polyethylene terephthalate container. Under a condition of 25°C, the connection part was immersed in the first curable resin liquid for 5 seconds to a position where the coated part was immersed about 5 mm, and then pulled up at a pulling speed of 100 mm / min. 10 seconds after being pulled up, the connection part was immersed in the second curable resin liquid previously dissolved at 180°C with the first curable resin liquid still attached thereto, and was left to stand at room temperature for 5 minutes while immersed in the polyethylene terephthalate container to cool. In this way, the first curable resin liquid and the second curable resin liquid were cured to form a layer made of the first curable resin in contact with the connection portion, and a layer made of the second curable resin in contact with the layer made of the first curable resin was formed, thereby obtaining a connecting wire of the present invention. Note that the first curable resin liquid naturally cures while the obtained connecting wire is left at room temperature.

[0056] (Example 18) A connecting wire was prepared in the same manner as in Example 17 above, except that the connecting portion, etc. was immersed in the first curable resin liquid, then removed, and then left to stand for 4 hours before being immersed in the second curable resin liquid.

[0057] (Example 20) A connecting wire was produced in the same manner as in Example 17 above, except that the first curable resin liquid was a curable resin liquid shown in Table 1 below.

[0058] (Comparative Examples 1 and 3) A connecting wire was produced in the same manner as in Example 1 above, except that the first curable resin liquid and the second curable resin liquid were the curable resin liquids shown in Table 1 below.

[0059] (Comparative Examples 2 and 4) The connection parts, etc. are immersed in the first curable resin liquid, and then left to stand for 4 hours after being removed and immersed in the second curable resin liquid, or exposed to ultraviolet light with an intensity of 1000 mW / cm 2 Electrical connectors were produced in the same manner as in Comparative Example 1 or 3, except that the first curable resin liquid was cured by irradiation with ultraviolet light at 400 V for 30 seconds.

[0060] (Thickness of layer made of first cured resin) The thickness (h, unit: m) of the layer made of the first curing resin in the connecting electric wires of Examples 1 to 20 and Comparative Examples 1 to 4 was calculated by the following (Formula 1) using each parameter based on the type of the first curing resin liquid. The calculation results are also shown in Table 1 below in μm conversion.

[0061] TIFF2024143134000003.tif20170

[0062] In the above formula (1), the parameters are as follows: U: Pulling speed (m / s) η: Viscosity of the curable resin liquid (Pa s = kg m / s) ρ: Density of the curable resin liquid (kg / m 3 ) γ: Surface tension of curable resin liquid (N / m) g: Gravitational acceleration (m / s 2 )

[0063] When the first curable resin liquid was a moisture curable resin (Examples 1 to 9, 15, 17, and 18, and Comparative Examples 1 and 2), the parameters used in the above (Equation 1) were as follows. U=0.001667m / s η = (viscosity of the first curable resin liquid shown in Table 1 below) Pa s ρ=1050kg / m 3 γ=0.0343N / m g=9.8m / s 2

[0064] When the first curable resin liquid was an anaerobic curable resin (Examples 19 and 20) or an ultraviolet curable resin (Examples 10 to 14 and 16, Comparative Examples 3 and 4), the parameters used in the above (Equation 1) were as follows. U=0.001667m / s η = (viscosity of the first curable resin liquid shown in Table 1 below) Pa s ρ=1070kg / m 3 γ=0.0398N / m g=9.8m / s 2

[0065] (Measurement of droplet count) In the manufacture of the electric connecting wires of Examples 1 to 20 and Comparative Examples 1 to 4, the number of droplets of the first curable resin liquid that dripped down from the connecting portion was counted during the period from when the connecting portion was immersed in the first curable resin liquid and then pulled out until when the connecting portion was immersed in the second curable resin, and was evaluated based on the following evaluation criteria. Note that, for example, when the first curable resin liquid is irradiated with ultraviolet light or left to stand at room temperature to be cured, and then immersed in the second curable resin liquid, the liquid that dripped down during the ultraviolet light irradiation or the standing at room temperature was also included in the above-mentioned "number of droplets". The results are also shown in Table 1 below. -Evaluation criteria- Number of droplets is 5 or more: × Number of droplets: 3-4: △ Number of droplets: 1 to 2: Droplet count is 0:◎

[0066] The following evaluation tests were carried out on each of the obtained connecting wires. The results are shown in Table 1 below.

[0067] (Watertightness test) For each of the resulting connecting wires, one of the six insulated wires that make up the connecting wire was selected, and air was pumped into it using a regulator, and the other five wires immersed in water in a tank were evaluated for air leakage (initial watertightness). The air pressure was gradually increased from 0 kPa to 100 kPa, and the air pressure at the time of air leakage was recorded and evaluated according to the following evaluation criteria. -Evaluation criteria- ×: Air leak occurred before the air pressure reached 20 kPa. △: No air leak occurred when the air pressure was 20 kPa, but air leak occurred before the air pressure reached 50 kPa. ○: No air leak occurred when the air pressure was 50 kPa, but air leak occurred before the air pressure reached 100 kPa. ◎: No air leak occurred even when the air pressure reached 100 kPa.

[0068] (Thermal shock test) Each of the obtained connecting wires was heated at 125°C for 30 minutes and then cooled at -40°C for 30 minutes, which constituted one cycle, and this cycle was repeated 500 times in total. Thereafter, a water stoppage test was conducted, and the water stoppage was evaluated based on the above evaluation criteria (water stoppage after durability).

[0069] [Table 1]

[0070] In the electric connecting wires of Comparative Examples 1 to 4 obtained using the first curable resin liquid with a viscosity of 35 mPa s, the first curable resin liquid dripped during the production of the electric connecting wire, causing contamination of the surrounding area. In addition, the obtained electric connecting wires had poor initial water stoppage properties (water stoppage properties immediately after production), and the electric connecting wires of Comparative Examples 2 and 4 in particular further deteriorated in water stoppage properties after thermal shock cycles. In contrast, in the electric connecting wires of Examples 1 to 20 obtained by using the first curable resin liquid having a viscosity of 51 to 1500 mPa s, dripping of the first curable resin liquid during production of the electric connecting wires was effectively suppressed, and the obtained electric connecting wires had excellent initial water tightness and further maintained the water tightness sufficiently even after thermal shock cycles. [Explanation of symbols]

[0071] 1 Connecting wire 10 Insulated wire 11 Conductor 12 Covering part 13 Connection 14 Crimp terminal 20 Sealing layer 21, 21' 1st hardening resin liquid 22 First cured resin 23 Second hardening resin liquid 24 Second cured resin 25 Insulating cap (protective material)

Claims

1. A method for manufacturing a connecting electric wire in which a connection portion at which conductors of a plurality of insulated electric wires are connected to each other is sealed with an insulating sealing layer, comprising the steps of: immersing the connection portion in a first curable resin liquid; removing the connection portion after the immersion; immersing the connection portion in a second curable resin liquid; and a step of curing the second curable resin liquid, in this order. The viscosity of the first curable resin liquid is 51 to 1500 mPa·s, and the second curable resin liquid contains a photocurable resin and / or a heat-meltable resin. A method for manufacturing a connecting wire.

2. 2. The method according to claim 1, wherein the layer made of the first curable resin formed by curing the first curable resin liquid has a thickness of 30 to 300 μm.

3. The viscosity of the first curable resin liquid is 80 to 1000 mPa s, and the thickness of the layer made of the first curable resin obtained by curing the first curable resin liquid is 42 to 230 μm. The manufacturing method according to claim 1 or 2.

4. The method for producing an electric connection wire according to claim 1 , wherein the second hardening resin liquid has a higher viscosity than the first hardening resin liquid.

5. The method for producing an electric connection wire according to claim 1 , wherein the first curable resin liquid includes a photocurable resin.

6. The method for producing an electric connection wire according to claim 1 , wherein the first curable resin liquid contains a moisture curable resin.

7. The method for producing an electric connection wire according to claim 1 , wherein the first hardening resin liquid contains an anaerobic hardening resin.

8. The method for producing an electric connection wire according to claim 1 or 2, wherein the second curable resin liquid is used by filling a protective member.

9. The method for producing an electric connection wire according to claim 1 or 2, wherein the electric connection wire is a wire harness.

10. A connecting wire in which a connection portion where conductors of a plurality of insulated wires are connected to each other is sealed with an insulating sealing layer, the sealing layer has a layer made of a first cured resin and a layer made of a second cured resin covering the layer made of the first cured resin, the layer made of the first cured resin has a thickness of 30 to 300 μm, and the second cured resin contains a photocurable resin and / or a heat-melting resin.

11. The electric wire according to claim 10, wherein the layer made of the first cured resin has a thickness of 42 to 230 μm.

12. The electric connection wire according to claim 10 or 11, wherein the first curable resin includes a photocurable resin.

13. The electric connection wire according to claim 10 or 11, wherein the first curable resin comprises a moisture curable resin.

14. The electric connection wire according to claim 10 or 11, wherein the first cured resin comprises an anaerobically cured resin.

15. The electric connection wire according to claim 10 or 11, wherein the sealing layer is covered with a protective member.

16. The electric connection wire according to claim 10 or 11, wherein the electric connection wire is a wire harness.

Citation Information

Patent Citations

  • Deposited wire

    JP1993182526A

  • Electroluminescent element and manufacture thereof

    JP1995320868A

  • Inter-wire water cutoff method

    JP2009099451A

  • Method for producing wire harness, and the wire harness

    JP2011113692A

  • Electric wire connection method and wiring harness

    JP2012130225A