Photochromic article, glasses, and method for manufacturing photochromic article

By employing a primer layer with a polymer containing hydroxyl and (meth)acryloyl groups and blocked isocyanate, the adhesion issue between the photochromic layer and base material is resolved, resulting in a stable and effective photochromic article.

JP2024143167APending Publication Date: 2024-10-11HOYA LENS THAILAND LTD

Patent Information

Application Number
JP2023055698
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Filing Date
2023-03-30
Publication Date
2024-10-11

AI Technical Summary

Technical Problem

The challenge lies in improving the adhesion between the photochromic layer and the base material in photochromic articles, as existing methods using moisture-curable polyurethane resins lead to increased viscosity during storage, affecting coating properties.

Method used

A primer layer formed from a polymer composition containing a polymer with hydroxyl and (meth)acryloyl groups and blocked isocyanate is used between the substrate and the photochromic layer, which suppresses viscosity increase during storage and enhances adhesion.

Benefits of technology

This approach results in a photochromic article with excellent adhesion between the photochromic layer and the base material, ensuring stable and effective performance.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024143167000001
    Figure 2024143167000001
  • Figure 2024143167000002
    Figure 2024143167000002
  • Figure 2024143167000003
    Figure 2024143167000003
Patent Text Reader

Abstract

To provide a photochromic article in which a photochromic layer and a base material attach to each other tightly.SOLUTION: The photochromic article sequentially includes a base material, a primer layer formed from a primer layer formation polymer composition, and a photochromic layer including a photochromic compound. The primer layer formation polymer composition includes a polymer with a hydroxy group and a (meth) acryloyl group and block isocyanate.SELECTED DRAWING: None
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to photochromic articles, eyeglasses and methods for making photochromic articles. [Background technology]

[0002] A photochromic compound is a compound that exhibits a property (photochromic property) of developing a color under irradiation of light in a wavelength range having photoresponsiveness and fading under non-irradiation. Hereinafter, an article containing a photochromic compound is referred to as a photochromic article. For example, Patent Document 1 discloses an optical article in which a layer containing a photochromic compound (photochromic layer) is provided on a substrate. [Prior art documents] [Patent documents]

[0003] [Patent Document 1] Patent No. 4405833 specification Summary of the Invention [Problem to be solved by the invention]

[0004] The present inventors have conducted extensive research to improve the adhesion between a photochromic layer and a substrate, aiming to improve the performance of photochromic articles.

[0005] That is, an object of one aspect of the present invention is to provide a photochromic article having excellent adhesion between a photochromic layer and a substrate. [Means for solving the problem]

[0006] As a result of extensive research, the inventors have newly discovered that it is possible to provide a photochromic article having excellent adhesion between the photochromic layer and the substrate by providing a primer layer formed from a polymer composition for forming a primer layer, which comprises a polymer having a hydroxy group and a (meth)acryloyl group, and a blocked isocyanate, between the photochromic layer and the substrate. Incidentally, in order to improve the adhesion between the photochromic layer and the substrate, Patent Document 1 (JP Patent No. 4405833) proposes providing a polyurethane resin layer formed from a moisture-curing polyurethane resin between the substrate and the photochromic layer. However, since moisture-curing polyurethane resins cure by reacting with moisture in the air, the liquid viscosity tends to increase easily due to the reaction with moisture in the air during storage. In contrast, it has also been found that the above-mentioned polymer composition for forming a primer layer can exhibit excellent coatability after storage because it is possible to suppress the increase in viscosity during storage. This is presumably because the isocyanate contained in the above-mentioned polymer composition for forming a primer layer is a blocked isocyanate in which the isocyanate group is protected by a blocking agent, and therefore the reaction between the hydroxyl group and the isocyanate group of the above-mentioned polymer during storage can be suppressed. However, the present invention is not limited to the presumption described in this specification.

[0007] One aspect of the present invention is as follows. [1] A substrate, A primer layer formed from a primer layer-forming polymer composition; a photochromic layer including a photochromic compound; in that order, The polymer composition for forming a primer layer is A polymer having a hydroxy group and a (meth)acryloyl group; Blocked isocyanate, A photochromic article comprising: [2] The photochromic article according to [1], wherein the polymer is a (meth)acrylic polymer. [3] The photochromic article according to [1], wherein the photochromic layer is a cured layer obtained by curing a (meth)acrylate-based polymerizable composition containing a photochromic compound. [4] The photochromic article according to [2], wherein the photochromic layer is a cured layer obtained by curing a (meth)acrylate-based polymerizable composition containing a photochromic compound. [5] The photochromic article according to any one of [1] to [4], which is a spectacle lens, a goggle lens, a visor portion of a sun visor, or a shielding member of a helmet. [6] The photochromic article according to [5], which is a spectacle lens. [7] Glasses equipped with the eyeglass lens described in [6]. [8] Applying a polymer composition for forming a primer layer onto a substrate to form a primer layer; forming a photochromic layer containing a photochromic compound on the formed primer layer; Including, The polymer composition for forming a primer layer is A polymer having a hydroxy group and a (meth)acryloyl group; Blocked isocyanate, Including, heat-treating the laminate obtained by forming the photochromic layer; The method of making a photochromic article further comprises: [9] The method for producing a photochromic article according to [8], wherein the polymer is a (meth)acrylic polymer.

[10] A method for producing a photochromic article according to [8], comprising forming the photochromic layer by curing a (meth)acrylate-based polymerizable composition containing a photochromic compound.

[11] A method for producing a photochromic article according to [9], comprising forming the photochromic layer by curing a (meth)acrylate-based polymerizable composition containing a photochromic compound.

[12] The method for producing a photochromic article according to any one of [8] to

[11] , wherein the photochromic article is a spectacle lens, a goggle lens, a visor portion of a sun visor, or a shield member of a helmet. Effect of the Invention

[0008] According to one aspect of the present invention, a photochromic article having excellent adhesion between a photochromic layer and a substrate can be provided. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0009] [Photochromic items] The photochromic article according to one embodiment of the present invention will be described in further detail below.

[0010] The photochromic article has a substrate, a primer layer, and a photochromic layer in this order. In one embodiment, the primer layer can be a layer adjacent to the photochromic layer, and can be a layer adjacent to the substrate or a layer provided on the substrate. Here, "adjacent" means that it is in direct contact without any other layer.

[0011] <Base material> The photochromic article may have a photochromic layer on a substrate selected according to the type of the article. As an example of the substrate, the spectacle lens substrate may be a plastic lens substrate or a glass lens substrate. The glass lens substrate may be, for example, a lens substrate made of inorganic glass. As the lens substrate, a plastic lens substrate is preferable from the viewpoint of being lightweight, difficult to break, and easy to handle. Examples of the plastic lens substrate include (meth)acrylic resin, styrene resin, polycarbonate resin, allyl resin, allyl carbonate resin such as diethylene glycol bisallyl carbonate resin (CR-39), vinyl resin, polyester resin, polyether resin, urethane resin obtained by reacting an isocyanate compound with a hydroxy compound such as diethylene glycol, thiourethane resin obtained by reacting an isocyanate compound with a polythiol compound, and a cured product (generally called a transparent resin) obtained by curing a curable composition containing a (thio)epoxy compound having one or more disulfide bonds in the molecule. As the lens substrate, a non-dyed one (colorless lens) or a dyed one (dyed lens) may be used. The refractive index of the lens substrate can be, for example, about 1.50 to 1.75. However, the refractive index of the lens substrate is not limited to the above range, and may be within the above range or may be above or below the above range. In the present invention and this specification, the refractive index refers to the refractive index for light with a wavelength of 500 nm. The lens substrate may be a lens with refractive power (so-called prescription lens) or a lens without refractive power (so-called non-prescription lens).

[0012] The spectacle lens can be various lenses such as a single-focus lens, a multifocal lens, a progressive power lens, etc. The type of lens is determined by the surface shapes of both sides of the lens substrate. The surface of the lens substrate may be convex, concave, or flat. In normal lens substrates and spectacle lenses, the object side surface is convex and the eyeball side surface is concave. However, the present invention is not limited thereto. The photochromic layer can usually be provided on the object side surface of the lens substrate, but may also be provided on the eyeball side surface.

[0013] <Primer layer> The primer layer is formed from a polymer composition for forming a primer layer, which contains a polymer having a hydroxy group and a (meth)acryloyl group, and a blocked isocyanate.

[0014] (polymer) In the present invention and this specification, the term "(meth)acryloyl group" is used to mean both acryloyl group and methacryloyl group, and the term "(meth)acryloyloxy group" is used to mean both acryloyloxy group and methacryloyloxy group. In the above polymer, the acryloyl group may be contained in the form of an acryloyloxy group, and the methacryloyl group may be contained in the form of a methacryloyloxy group. This also applies to (meth)acrylates described later.

[0015] In the present invention and in this specification, a "polymer" may be a homopolymer or a copolymer.

[0016] The polymer may contain a hydroxyl group and a (meth)acryloyl group in the side chain of the polymer. The present inventors speculate that the hydroxyl group contained in the polymer contributes to forming a bond between the substrate and the primer layer together with the isocyanate group regenerated by dissociating the blocking agent of the blocked isocyanate, and the (meth)acryloyl group contained in the polymer contributes to forming a bond between the photochromic layer and the primer layer. It is believed that the adhesion between the photochromic layer and the substrate can be improved by forming these bonds.

[0017] The main skeleton of the polymer is not particularly limited. In one embodiment, the polymer may be a (meth)acrylic polymer. In the present invention and this specification, the term "(meth)acrylic polymer" refers to a homopolymer or copolymer of (meth)acrylate. The details of "(meth)acrylate" will be described later.

[0018] As the polymer having a hydroxyl group and a (meth)acryloyl group, a polymer synthesized by a known method can be used, or a commercially available product can be used. An example of a commercially available product is a reactive polymer (RP-274S) manufactured by KSM Co., Ltd.

[0019] (Blocked isocyanate) A blocked isocyanate is an isocyanate in which the isocyanate group is protected with a blocking agent. The blocking agent inhibits the reaction of the isocyanate group, and when the blocking agent is dissociated by heat treatment, the isocyanate group is regenerated, and the regenerated isocyanate group can undergo a crosslinking reaction with an active hydrogen-containing group (e.g., a hydroxyl group).

[0020] Examples of the blocked isocyanate include blocked isocyanates of polyisocyanates such as diisocyanates and triisocyanates. The types of isocyanates include adduct type, biuret type, and isocyanurate type, and biuret type and isocyanurate type are preferred. A blocking agent that can be dissociated at a temperature at which deformation or deterioration of the substrate is unlikely to occur is preferred, and from this point of view, preferred blocking agents include diethyl allomate (DEM), dimethylpyrazole (DMP), and the like. A plurality of isocyanate groups contained in the isocyanate may be protected by different blocking agents. For example, a blocked isocyanate containing DEM and DMP as blocking agents can also be used.

[0021] (Preparation of polymer composition for forming primer layer) In the polymer composition for forming a primer layer, the content of the blocked isocyanate relative to the total of the polymer and the blocked isocyanate (100% by mass) can be, for example, 30.0% by mass or more and 60.0% by mass or less. The content of the polymer relative to the total of the polymer and the blocked isocyanate (100% by mass) can be, for example, 30.0% by mass or more, 40.0% by mass or more, or 50.0% by mass or more. The content of the polymer can be, for example, 90.0% by mass or less, 80.0% by mass or less, 70.0% by mass or less, or 60.0% by mass or less. The polymer composition for forming a primer layer may contain one or more of the above polymers and may contain one or more of blocked isocyanates. In the present invention and this specification, when two or more types of a certain component are contained, the content of the component refers to the total content of the two or more types.

[0022] The polymer composition for forming a primer layer may contain one or more of known polymerization initiators that can function as a polymerization initiator for the (meth)acryloyl group of the polymer. The polymer composition for forming a primer layer may contain a polymerization initiator in a content ranging from 0.01 to 3.0% by mass, for example, with the total solid content being 100% by mass. In the present invention and this specification, the term "total solid content" for a certain composition refers to the total amount of all components excluding the solvent.

[0023] The polymerization initiator is preferably a radical polymerization initiator. In addition, as the polymerization initiator, a photopolymerization initiator or a thermal polymerization initiator can be used, and the photopolymerization initiator is preferred from the viewpoint of progressing the polymerization reaction in a short time. Examples of the photoradical polymerization initiator include benzoin ketals such as 2,2-dimethoxy-1,2-diphenylethane-1-one; α-hydroxyketones such as 1-hydroxycyclohexyl phenyl ketone, 2-hydroxy-2-methyl-1-phenylpropan-1-one, and 1-[4-(2-hydroxyethoxy)phenyl]-2-hydroxy-2-methyl-1-propan-1-one; α-aminoketones such as 2-benzyl-2-dimethylamino-1-(4-morpholinophenyl)-butan-1-one and 1,2-methyl-1-[4-(methylthio)phenyl]-2-morpholinopropan-1-one; oxime esters such as 1-[(4-phenylthio)phenyl]-1,2-octadione-2-(benzoyl)oxime; bis(2,4,6-trimethylbenzoyl)phenylphosphine oxide, bis(2,6-dimethoxy ... phosphine oxides such as 2-(o-chlorophenyl)-4,5-diphenylimidazole dimer, 2-(o-chlorophenyl)-4,5-di(methoxyphenyl)imidazole dimer, 2-(o-fluorophenyl)-4,5-diphenylimidazole dimer, 2-(o-methoxyphenyl)-4,5-diphenylimidazole dimer, 2-(p-methoxyphenyl)-4,5-diphenylimidazole dimer; benzophenone compounds such as benzophenone, N,N'-tetramethyl-4,4'-diaminobenzophenone, N,N'-tetraethyl-4,4'-diaminobenzophenone, and 4-methoxy-4'-dimethylaminobenzophenone;quinone compounds such as 2-ethylanthraquinone, phenanthrenequinone, 2-tert-butylanthraquinone, octamethylanthraquinone, 1,2-benzanthraquinone, 2,3-benzanthraquinone, 2-phenylanthraquinone, 2,3-diphenylanthraquinone, 1-chloroanthraquinone, 2-methylanthraquinone, 1,4-naphthoquinone, 9,10-phenanthraquinone, 2-methyl-1,4-naphthoquinone, and 2,3-dimethylanthraquinone; benzoin ethers such as benzoin methyl ether, benzoin ethyl ether, and benzoin phenyl ether; benzoin compounds such as benzoin, methylbenzoin, and ethylbenzoin; benzyl compounds such as benzyl dimethyl ketal; acridine compounds such as 9-phenylacridine and 1,7-bis(9,9'-acridinylheptane); N-phenylglycine, coumarin, and the like. In the 2,4,5-triarylimidazole dimer, the substituents of the aryl groups of the two triarylimidazole moieties may be the same to give a symmetrical compound, or may be different to give an asymmetrical compound. A thioxanthone compound may be combined with a tertiary amine, such as a combination of diethylthioxanthone and dimethylaminobenzoic acid. Among these, α-hydroxyketones and phosphine oxides are preferred from the viewpoints of curability, transparency, and heat resistance.

[0024] The polymer composition for forming a primer layer may contain a catalyst that catalyzes the crosslinking reaction of an isocyanate group. The content of the catalyst may be, for example, in the range of 0.1 to 15.0% by mass, with the total solid content being 100% by mass. Examples of the catalyst include dibutyltin dilaurate, dibutylthione octate, dimethylcyclohexylamine, dimethylbenzylamine, trioctylamine, and bis((2-morpholinoethyl)ether).

[0025] The polymer composition for forming the primer layer can contain any solvent in any amount.

[0026] The polymer composition for forming a primer layer may further contain any amount of known additives that can be usually added to compositions for forming a primer layer. Known compounds may be used as the additives.

[0027] The polymer composition for forming a primer layer can be prepared by mixing the various components described above simultaneously or successively in any order.

[0028] The primer layer can be formed on the substrate by applying the above-mentioned primer layer-forming polymer composition to the substrate and drying the applied composition to remove part or all of the solvent. The drying process may be performed so that part or all of the solvent can be removed. For example, the drying process can be performed by air drying at room temperature. The "room temperature" described in this specification is a temperature in the range of 20 to 25°C. The substrate surface before application can be subjected to one or more of known pretreatments such as alkali treatment and UV ozone treatment for cleaning the substrate surface. In addition, a layer other than the hard coat layer may be formed on the substrate surface to which the primer layer is applied. As the application method, known application methods such as spin coating and dip coating can be adopted, and from the viewpoint of uniformity of application, spin coating is preferred.

[0029] The curing treatment for reacting the (meth)acryloyl group of the polymer contained in the primer layer and the heat treatment for dissociating the blocking agent of the blocked isocyanate will be described later.

[0030] The thickness of the primer layer can be, for example, 3 μm or more, and preferably 4 μm or more, and the thickness of the primer layer can be, for example, 15 μm or less, and preferably 10 μm or less.

[0031] <Photochromic layer> <<Polymerizable compounds>> The photochromic article has a photochromic layer containing a photochromic compound on the primer layer. The photochromic layer can be a cured layer obtained by curing a photochromic layer-forming polymerizable composition. The photochromic layer-forming polymerizable composition can be, for example, a (meth)acrylate-based polymerizable composition. In the present invention and this specification, the term "(meth)acrylate-based polymerizable composition" refers to a polymerizable composition containing a (meth)acrylate. The term "(meth)acrylate" is used to include acrylate and methacrylate. The term "acrylate" refers to a compound having one or more acryloyl groups in one molecule. The term "methacrylate" refers to a compound having one or more methacryloyl groups in one molecule. For a (meth)acrylate, the functionality is the number of groups selected from the group consisting of acryloyl groups and methacryloyl groups contained in one molecule. In the present invention and this specification, "methacrylate" refers to a group containing only a methacryloyl group as a (meth)acryloyl group, and a group containing both an acryloyl group and a methacryloyl group as a (meth)acryloyl group is called an acrylate. In addition, unless otherwise specified, the described group may have a substituent or may be unsubstituted. When a certain group has a substituent, examples of the substituent include an alkyl group (e.g., an alkyl group having 1 to 6 carbon atoms), a hydroxyl group, an alkoxy group (e.g., an alkoxy group having 1 to 6 carbon atoms), a halogen atom (e.g., a fluorine atom, a chlorine atom, a bromine atom), a cyano group, an amino group, a nitro group, an acyl group, a carboxy group, an aryl group, and a polyether group. In addition, the "carbon number" of a group having a substituent means the carbon number of the portion not including the substituent.

[0032] A (meth)acrylate-based polymerizable composition, which is one embodiment of the polymerizable composition for forming a photochromic layer, will be described below. However, the following embodiment is merely an example, and the present invention is not limited to only this example.

[0033] In one embodiment, the polymerizable composition for forming a photochromic layer can be a (meth)acrylate-based polymerizable composition containing one or more polymerizable compounds selected from the group consisting of the following Component A, the following Component B, and the following Component C.

[0034] (Component A) Component A is a polyfunctional (meth)acrylate containing a polyalkylene glycol moiety and having a molecular weight of 500 or more. In the present invention and this specification, the term "polyalkylene glycol moiety" refers to a polyfunctional (meth)acrylate having a molecular weight of 500 or more and having a molecular weight of 500 or more. [ka] In formula 2, R represents an alkylene group, n represents the number of repetitions of the alkoxy group represented by RO and is 2 or more. * represents the bonding position where the partial structure represented by formula 2 is bonded to the adjacent atom. The number of carbon atoms in the alkylene group represented by R can be 1 or more or 2 or more, and can be, for example, 5 or less or 4 or less. Specific examples of the alkylene group represented by R include an ethylene group, a propylene group, and a tetramethylene group. n is 2 or more, and can be, for example, 30 or less, 25 or less, or 20 or less. In one embodiment, component A can have the above partial structure in which R represents an ethylene group, that is, a polyethylene glycol moiety. In another embodiment, component A can have a polyethylene glycol moiety. can have the above partial structure in which R represents a propylene group, i.e., a polypropylene glycol moiety.

[0035] The molecular weight of component A is 500 or more. In the present invention and this specification, the molecular weight of the multimer is the theoretical molecular weight calculated from the structural formula determined by structural analysis of the compound or the raw material charging ratio during production. The molecular weight of component A is 500 or more, preferably 510 or more, more preferably 520 or more, preferably 550 or more, more preferably 570 or more, even more preferably 600 or more, even more preferably 630 or more, and even more preferably 650 or more. From the viewpoint of increasing the hardness of the photochromic layer, the molecular weight of component A is preferably, for example, 2000 or less, 1500 or less, 1200 or less, 1000 or less, or 800 or less.

[0036] Component A is a polyfunctional (meth)acrylate, and may be, for example, a bifunctional, trifunctional, tetrafunctional, or pentafunctional (meth)acrylate, and is preferably a bifunctional or trifunctional (meth)acrylate. Component A may contain only acryloyl groups, only methacryloyl groups, or acryloyl and methacryloyl groups as (meth)acryloyl groups. That is, component A may be an acrylate or methacrylate.

[0037] In one embodiment, component A can be a non-cyclic polyfunctional (meth)acrylate. In the present invention and this specification, "non-cyclic" means that it does not contain a cyclic structure. In contrast, "cyclic" means that it contains a cyclic structure. The non-cyclic polyfunctional (meth)acrylate refers to a bifunctional or higher functional (meth)acrylate that does not contain a cyclic structure. A specific example of such component A is a polyalkylene glycol di(meth)acrylate represented by the following formula 3.

[0038] [ka]

[0039] In formula 3, R 1 and R 2Each independently represents a hydrogen atom or a methyl group, R represents an alkylene group, and n represents the number of repetitions of the alkoxy group represented by RO, which is 2 or more. R and n are as described above for the partial structure represented by formula 2. The polyalkylene glycol di(meth)acrylate represented by formula 3 may contain only an acryloyl group, only a methacryloyl group, or both an acryloyl group and a methacryloyl group as the (meth)acryloyl group. Specific examples of the polyalkylene glycol di(meth)acrylate represented by formula 3 include polyethylene glycol di(meth)acrylate, polypropylene glycol di(meth)acrylate, and polytetramethylene glycol di(meth)acrylate.

[0040] A specific example of Component A is a tri(meth)acrylate represented by the following formula 4. The tri(meth)acrylate represented by formula 4 may contain only acryloyl groups, only methacryloyl groups, or both acryloyl groups and methacryloyl groups as (meth)acryloyl groups.

[0041] [ka]

[0042] In formula 4, R 40 , R 41 , R 44 , R 45 , R 47 and R 48 each independently represents an alkylene group; R 43 represents an alkyl group, R 42 , R 46 and R 49 each independently represents a hydrogen atom or a methyl group; 41 n2 represents the number of repeats of the alkoxy group represented by the formula: 45 n3 represents the number of repeats of the alkoxy group represented by the formula: 48This indicates the number of repetitions of the alkoxy group represented by the following formula:

[0043] Equation 4 will now be explained in more detail.

[0044] R in Equation 4 41 , R 45 and R 48 is as described above for R in formula 2. n1, n2, and n3 in formula 4 are as described above for n in formula 2. In formula 4, R 41 , R 45 and R 48 may be the same, or two or three may be different. The same applies to n1, n2, and n3.

[0045] R 42 , R 46 and R 49 each independently represents a hydrogen atom or a methyl group. The tri(meth)acrylate represented by formula 4 may contain only acryloyl groups, only methacryloyl groups, or both acryloyl groups and methacryloyl groups as (meth)acryloyl groups.

[0046] R 43 The number of carbon atoms in the alkyl group represented by R can be 1 or more, or 2 or more, and can be, for example, 5 or less, or 4 or less. 43 The alkyl group represented by R can be a straight chain alkyl group or a branched alkyl group. 43 Specific examples of the alkyl group represented by the formula (I) include a methyl group and an ethyl group.

[0047] R 40 , R 44 and R 47 each independently represents an alkylene group. The number of carbon atoms in such an alkylene group can be 1 or more or 2 or more, and can be, for example, 5 or less or 4 or less. Specific examples thereof include an ethylene group, a propylene group, and a tetramethylene group.

[0048] A specific example of the tri(meth)acrylate represented by formula 4 is trimethylolpropane polyoxyethylene ether tri(meth)acrylate.

[0049] Monofunctional (meth)acrylate From the viewpoint of increasing the (meth)acryloyl group content of the polymerizable composition containing the (meth)acrylate, a (meth)acrylate having a high ratio of (meth)acryloyl groups in the molecule is preferred. From this viewpoint, a low molecular weight monofunctional (meth)acrylate is preferred, and a monofunctional (meth)acrylate having a molecular weight of 150 or less is more preferred. The monofunctional (meth)acrylate having a molecular weight of 150 or less may be a cyclic monofunctional (meth)acrylate or an acyclic monofunctional (meth)acrylate. A specific example of a cyclic monofunctional (meth)acrylate having a molecular weight of 150 or less is glycidyl (meth)acrylate. A specific example of an acyclic monofunctional (meth)acrylate having a molecular weight of 150 or less is n-butyl (meth)acrylate. The molecular weight of the monofunctional (meth)acrylate having a molecular weight of 150 or less may be, for example, 100 or more, but is not limited thereto.

[0050] Multifunctional (meth)acrylate As described above, from the viewpoint of increasing the (meth)acryloyl group content of the polymerizable composition containing the (meth)acrylate, a (meth)acrylate having a high ratio of (meth)acryloyl groups in the molecule is preferred. From this viewpoint, a polyfunctional (meth)acrylate having a smaller molecular weight than component A is also preferred. As such a polyfunctional (meth)acrylate, a polyfunctional (meth)acrylate having a larger number of functions than the polyfunctional (meth)acrylate used as component A is also preferred. The molecular weight of such a polyfunctional (meth)acrylate is preferably less than 500, 400 or less, 300 or less, or 200 or less. The molecular weight can be, for example, 100 or more, but is not limited thereto. In addition, such a polyfunctional (meth)acrylate can be, for example, a polyfunctional (meth)acrylate having 10 or more functions (for example, 10 or more and 15 or less functions). Specific examples include poly[(3-methacryloyloxypropyl)silsesquioxane] derivatives described in the Examples section below.

[0051] Examples of (meth)acrylates that may be included in the (meth)acrylate-based polymerizable composition, which is a photochromic layer-forming polymerizable composition, include a monofunctional (meth)acrylate represented by the following formula 1 (hereinafter also referred to as "component B") and a bifunctional (meth)acrylate represented by the following formula 5 (hereinafter also referred to as "component C"). In one embodiment, the (meth)acrylate-based polymerizable composition may be a polymerizable composition containing one or more (meth)acrylates selected from the group consisting of a monofunctional (meth)acrylate represented by the following formula 1 and a bifunctional (meth)acrylate represented by the following formula 5. In another embodiment, the (meth)acrylate-based polymerizable composition may be a polymerizable composition that does not contain one or more (meth)acrylates selected from the group consisting of a monofunctional (meth)acrylate represented by the following formula 1 and a bifunctional (meth)acrylate represented by the following formula 5. In one embodiment, the (meth)acrylate-based polymerizable composition may also contain component B as a monofunctional (meth)acrylate having a molecular weight of 150 or less.

[0052] (Component B) Component B is a monofunctional (meth)acrylate represented by the following formula 1.

[0053] [ka]

[0054] Formula 1 will now be described in more detail.

[0055] In formula 1, R 10 represents a hydrogen atom or a methyl group. The monofunctional (meth)acrylate represented by formula 1 may be an acrylate or a methacrylate.

[0056] R 11 R represents a linear alkyl group having 3 or more carbon atoms or a branched alkyl group having 3 or more carbon atoms. These alkyl groups may be unsubstituted or may have a substituent. The substituent is not particularly limited, and examples thereof include the various substituents described above. 11 The number of carbon atoms in the linear or branched alkyl group represented by the formula (I) is 3 or more, preferably 4 or more, more preferably 5 or more, and further preferably 6 or more, 7 or more, 8 or more, 9 or more, 10 or more, and 11 or more. On the other hand, from the viewpoint of the solubility of the photochromic compound in the composition, the number of carbon atoms is preferably 15 or less, more preferably 14 or less, and further preferably 13 or less, and 12 or less.

[0057] The molecular weight of the monofunctional (meth)acrylate represented by formula 1 can be, for example, 100 or more, and can be, for example, 300 or less. However, it is not limited to the above range. As described above, in one embodiment, the monofunctional (meth)acrylate represented by formula 1 can be a monofunctional (meth)acrylate having a molecular weight of 150 or less. Specific examples of the monofunctional (meth)acrylate represented by formula 1 include n-butyl (meth)acrylate, 2-ethylhexyl (meth)acrylate, isodecyl (meth)acrylate, and n-lauryl (meth)acrylate.

[0058] (Component C) Component C is represented by the following formula 5: [ka] It is a (meth)acrylate represented by the formula:

[0059] In formula 5, R 3 and R 4 each independently represents a hydrogen atom or a methyl group, and m represents an integer of 1 or greater. m is 1 or greater and can be, for example, 10 or less, 9 or less, 8 or less, 7 or less, or 6 or less.

[0060] The molecular weight of component C can be, for example, 400 or less, and from the viewpoint of further increasing the coloring density of the photochromic layer, it is preferably 350 or less, more preferably 300 or less, and even more preferably 250 or less. In addition, the molecular weight of component C can be, for example, 100 or more, 150 or more, or 200 or more.

[0061] Component C may contain only acryloyl groups, only methacryloyl groups, or both acryloyl groups and methacryloyl groups as (meth)acryloyl groups. Specific examples of component C include 1,9-nonanediol di(meth)acrylate, 1,6-hexanediol di(meth)acrylate, and 1,10-decanediol di(meth)acrylate.

[0062] In the (meth)acrylate-based polymerizable composition, the content of component A is preferably 50% by mass or more, more preferably 55% by mass or more, and even more preferably 60% by mass or more, based on the total amount of polymerizable compounds contained in the composition being 100% by mass. In one embodiment, component A can be the component that occupies the largest amount among the multiple polymerizable compounds contained in the composition. In addition, the content of component A can be 90% by mass or less, 85% by mass or less, or 80% by mass or less, based on the total amount of polymerizable compounds contained in the composition being 100% by mass. In one embodiment, the composition can contain only one type of component A, and in another embodiment, can contain two or more types. When two or more types of component A are contained, the content of component A is the total content of two or more types. This point is also true for the contents of other components in the present invention and this specification.

[0063] The (meth)acrylate-based polymerizable composition may contain the above-mentioned various (meth)acrylates in an amount such that the (meth)acryloyl group content of the composition is 3.50 mmol / g or more. For example, the (meth)acrylate-based polymerizable composition preferably contains 5% by mass or more, more preferably 10% by mass or more, and more preferably 15% by mass or more of a monofunctional (meth)acrylate having a molecular weight of 150 or less, based on the total amount of polymerizable compounds contained in the composition being 100% by mass. In addition, the content of the monofunctional (meth)acrylate having a molecular weight of 150 or less is preferably 30% by mass or less, more preferably 25% by mass or less, based on the total amount of polymerizable compounds contained in the composition being 100% by mass.

[0064] The (meth)acryloyl group content of the (meth)acrylate-based polymerizable composition is preferably 3.50mmol / g or more, more preferably 3.55mmol / g or more, even more preferably 3.60mmol / g or more, even more preferably 3.65mmol / g or more, even more preferably 3.70mmol / g or more, and even more preferably 3.75mmol / g or more, from the viewpoint of improving the weather resistance of the photo layer. The (meth)acryloyl group content of the (meth)acrylate-based polymerizable composition can be, for example, 5.00mmol / g or less, 4.50mmol / g or less, or 4.00mmol / g or less, or it may exceed the value exemplified here.

[0065] The "(meth)acryloyl group content" of a polymerizable composition containing a (meth)acrylate is calculated as follows. The content of each (meth)acrylate is calculated by taking the total amount of (meth)acrylate contained in the polymerizable composition as "1" on a mass basis. For each (meth)acrylate, the "(meth)acryloyl group content x the above content" is calculated. The sum of the values ​​thus calculated for all the (meth)acrylates contained in the polymerizable composition is regarded as the (meth)acryloyl group content of the polymerizable composition.

[0066] The photochromic compound contained in the photochromic layer undergoes structural change through an excited state upon irradiation with light such as sunlight. The structure after structural change through light irradiation can be called a "colored body". In contrast, the structure before light irradiation can be called a "colorless body". Note that "colorless" in the colorless body is not limited to complete colorlessness, but includes cases where the color is lighter than the colored body. After structural change to a colored body through light irradiation, the faster the rate of structural change from the colored body to the colorless body, the faster the fading rate. In the photochromic layer, the easier the molecular movement of the photochromic compound in the matrix formed by the polymerization reaction of the polymerizable compound is, the faster the rate of the structural change will be. From the viewpoint of increasing the rate, a flexible matrix is ​​considered to be desirable. In regard to the above points, it is presumed that component A can contribute to making the matrix flexible. In detail, it is considered that the molecular weight of component A is 500 or more, and that component A has a polyalkylene glycol moiety, are the reasons why a flexible matrix can be formed by component A. In addition, the (meth)acryloyl group content of the (meth)acrylate-based polymerizable composition being 3.50 mmol / g or more is considered to contribute to the formation of a rigid polymer network between molecules in the matrix formed from the (meth)acrylate-based polymerizable composition. In the matrix having a rigid polymer network, the diffusion of active species that may cause a decrease in weather resistance can be suppressed, which is presumably the reason why the (meth)acrylate-based polymerizable composition can form a photochromic layer with excellent weather resistance.

[0067] The content of the polymerizable compound in the (meth)acrylate-based polymerizable composition (when a plurality of polymerizable compounds are included, the total content thereof) can be, for example, 80% by mass or more, 85% by mass or more, or 90% by mass or more, with the total amount of the composition being 100% by mass. The content of the polymerizable compound in the (meth)acrylate-based polymerizable composition can be, for example, 99% by mass or less, 95% by mass or less, 90% by mass or less, or 85% by mass or less, with the total amount of the composition being 100% by mass. The (meth)acrylate-based polymerizable composition may or may not contain a solvent. When a solvent is included, any solvent can be used in any amount as long as it does not inhibit the progress of the polymerization reaction of the polymerizable composition.

[0068] <<Photochromic compounds>> The composition contains a photochromic compound together with the polymerizable compound. As the photochromic compound contained in the composition, a known compound exhibiting photochromic properties can be used. The photochromic compound can exhibit photochromic properties, for example, with respect to ultraviolet light. For example, the photochromic compound can be exemplified by compounds having a known skeleton exhibiting photochromic properties, such as azobenzenes, spiropyrans, spirooxazines, naphthopyrans, indenonaphthopyrans, phenanthropyrans, hexaarylbisimidazoles, donor-acceptor Stenhouse adducts (DASA), salicylideneanilines, dihydropyrenes, anthracene dimers, fulgides, diarylethenes, phenoxynaphthacenequinones, and stilbenes. As preferred photochromic compounds, fulgimide compounds, spirooxazine compounds, chromene compounds, indeno-condensed naphthopyran compounds, and the like can be exemplified. In addition, the photochromic compound may be one or more selected from the group consisting of photochromic compounds represented by general formula A, photochromic compounds represented by general formula B, and photochromic compounds represented by general formula C, as described in WO2022 / 138966. The photochromic compounds may be used alone or in combination of two or more. The content of the photochromic compound in the composition may be, for example, about 0.1 to 15% by mass, with the total amount of the composition being 100% by mass, but is not limited to this range.

[0069] <<Other Ingredients>> The photochromic layer-forming polymerizable composition may contain at least one of various additives that may be generally contained in a polymerizable composition in any content, in addition to the polymerizable compound and the photochromic compound. An example of an additive that may be contained in the photochromic layer-forming polymerizable composition is a polymerization initiator for promoting a polymerization reaction. The above description can be referred to for the polymerization initiator. The content of the polymerization initiator may be, for example, in the range of 0.1 to 5.0% by mass, with the total amount of the composition being 100% by mass.

[0070] The photochromic layer-forming polymerizable composition may further contain any amount of known additives that can be usually added to compositions containing a photochromic compound, such as surfactants, antioxidants, radical scavengers, light stabilizers, ultraviolet absorbers, color inhibitors, antistatic agents, fluorescent dyes, dyes, pigments, fragrances, plasticizers, silane coupling agents, etc. Known compounds may be used as these additives.

[0071] The photochromic layer-forming polymerizable composition can be prepared by mixing the various components described above simultaneously or sequentially in any order.

[0072] The photochromic layer can be formed by applying a photochromic layer-forming polymerizable composition onto the primer layer and curing the applied composition. The above description can be referred to for the application method. The curing treatment can be light irradiation and / or heat treatment, and light irradiation is preferred from the viewpoint of progressing the curing reaction in a short time. The curing treatment conditions may be determined according to the types of various components (such as the above-described polymerizable compound and polymerization initiator) contained in the photochromic layer-forming polymerizable composition and the composition of the above composition. The thickness of the photochromic layer thus formed is preferably in the range of, for example, 5 to 80 μm, and more preferably in the range of 20 to 60 μm. It is presumed that the curing treatment performed here can promote the reaction of the (meth)acryloyl group of the above polymer contained in the primer layer, thereby forming a bond between the photochromic layer and the primer layer.

[0073] The photochromic article having the above-mentioned photochromic layer may or may not have one or more functional layers in addition to the various layers described above. Examples of the functional layer include layers known as functional layers of optical articles, such as a protective layer for improving durability, a hard coat layer, an antireflection layer, a water-repellent or hydrophilic antifouling layer, and an antifogging layer. For example, the protective layer can be found in paragraphs 0009 to 0021, 0026 of JP 2021-107909 A and the description of the examples of the same publication.

[0074] <Heat treatment> The laminate in which the primer layer and the photochromic layer are formed on the substrate can be subjected to a heat treatment before or after the formation of the functional layer. The heat treatment performed here can dissociate the blocking agent of the blocked isocyanate to regenerate the isocyanate group. It is presumed that the regenerated isocyanate can contribute to the formation of a bond between the substrate and the primer layer together with the hydroxyl group of the polymer. The heat treatment can be performed at a temperature equal to or higher than the dissociation temperature of the blocking agent contained in the blocked isocyanate.

[0075] The photochromic article can be an optical article, and one form of the optical article is a spectacle lens. In addition, one form of the optical article can also be a goggle lens, a sun visor visor, a helmet shielding member, etc. A photochromic layer-forming polymerizable composition is applied to the substrate for these optical articles via a primer layer, and the applied composition is cured to form a photochromic layer, thereby obtaining an optical article having an anti-glare function.

[0076] [glasses] One aspect of the present invention relates to glasses having a spectacle lens, which is one form of the photochromic article. Details of the spectacle lens included in the glasses are as described above. By including such a spectacle lens, the glasses can exhibit an anti-glare effect like sunglasses, for example, outdoors, when the photochromic compound included in the photochromic layer is irradiated with sunlight and colored, and when returning indoors, the photochromic compound fades, thereby recovering transparency. For the configuration of the frame, etc. of the glasses, known techniques can be applied.

[0077] [Method of manufacturing photochromic products] One aspect of the present invention is Applying a primer layer-forming polymer composition onto a substrate to form a primer layer; forming a photochromic layer containing a photochromic compound on the formed primer layer; Including, The polymer composition for forming a primer layer is A polymer having a hydroxy group and a (meth)acryloyl group; Blocked isocyanate, Including, heat-treating the laminate obtained by forming the photochromic layer; The method of making a photochromic article further comprises: Regarding.

[0078] According to the above-mentioned manufacturing method, a photochromic article having excellent adhesion between the substrate and the photochromic layer can be manufactured. For details of the above-mentioned manufacturing method, the above description can be referred to. EXAMPLES

[0079] The present invention will be further described below with reference to examples, although the present invention is not limited to the embodiments shown in the examples.

[0080] <Base material> The various substrates described below are plastic lens substrates described below. In each substrate, the object side surface is a convex surface, and the eyeball side surface is a concave surface. Substrate 4 (refractive index 1.59) is a substrate with hard coat layers on both sides, and the polymer composition for forming a primer layer described below was applied to the hard coat layer surface. Substrate 1: Refractive index 1.50 (diethylene glycol bisallyl carbonate resin (CR-39)) Base material 2: Refractive index 1.53 (urea resin) Base material 3: Refractive index 1.55 (diallyl phthalate resin) Base material 4: Refractive index 1.59 (polycarbonate resin) Base material 5: Refractive index 1.60 (urethane resin) Base material 6: Refractive index 1.67 (thiourethane resin)

[0081] [Examples 1 to 6] <Production of eyeglass lenses (photochromic products)> The plastic lens substrate was immersed in a 10% by weight aqueous solution of sodium hydroxide (liquid temperature 60°C) for 5 minutes, then washed with pure water and dried. After that, a primer layer was formed on the convex surface (object side surface) of the plastic lens substrate. Specifically, the mixture obtained by mixing the various components shown in Table 1 was thoroughly stirred and then degassed using a rotation-revolution type stirring and degassing device. The thus obtained polymer composition for forming a primer layer was stored in a room temperature environment for one week, and then applied to the convex surface of a plastic lens substrate shown in Table 3 by spin coating in an environment with a temperature of 25°C and a relative humidity of 50%, and then air-dried in the same environment for 5 minutes to form a primer layer. The thickness of the formed primer layer was 4 μm. The viscosity of the polymer composition for forming a primer layer after one week of storage was the same as that before storage. A polymerizable composition for forming a photochromic layer ((meth)acryloyl group content: 3.61 mmol / g) prepared as follows was applied onto the primer layer by spin coating. The spin coating was performed by the method described in JP 2005-218994 A. Thereafter, the polymerizable composition for forming a photochromic layer applied onto the primer layer was irradiated with ultraviolet light (wavelength 405 nm) in a nitrogen atmosphere (oxygen concentration 500 ppm or less) to cure the composition and form a photochromic layer. The thickness of the formed photochromic layer was 40 μm. On the photochromic layer thus formed, a protective layer was formed by the method described in Example 1 of JP-A-2021-107909. The thickness of the formed protective layer was 15 μm. Thereafter, the laminate in which the primer layer, the photochromic layer and the protective layer were formed in this order on the substrate was heat-treated in a heating furnace at an atmospheric temperature of 90° C. for 2 hours. In this way, a spectacle lens having the substrate, the primer layer, the photochromic layer and the protective layer in this order was produced.

[0082] [Table 1]

[0083] (Preparation of polymerizable composition for forming photochromic layer) The ingredients shown in Table 2 were mixed in the amounts shown in Table 2 in a plastic container. The mixture of polymerizable compounds thus obtained was mixed with the following photochromic compound (indeno-condensed naphthopyran compound represented by the structural formula described in U.S. Pat. No. 6,296,785), photoradical polymerization initiator (bis(2,4,6-trimethylbenzoyl)phenylphosphine oxide (Omnirad819 manufactured by IGM Resin BV)), antioxidant (bis[3-(3-tert-butyl-4-hydroxy-5-methylphenyl)propionic acid][ethylene bis(oxyethylene)]), and light stabilizer (bis(1,2,2,6,6-pentamethyl-4-piperidyl) sebacate) and thoroughly stirred. Then, the mixture was degassed using a rotation-revolution type stirring and degassing device. Thus, a polymerizable composition for forming a photochromic layer was prepared. The content of the above components, taking the total amount of the composition as 100% by mass, is as follows: the mixture of the above polymerizable compounds is 94.9% by mass, the photochromic compound is 3% by mass, the photoradical polymerization initiator is 0.3% by mass, the antioxidant is 0.9% by mass, and the light stabilizer is 0.9% by mass.

[0084] [Table 2]

[0085] [ka]

[0086] [Comparative Example 1] A polymer composition for forming a primer layer was prepared by the method described in Example 1, except that a biuret type triisocyanate in which the isocyanate group was not protected with a blocking agent was used instead of the blocked isocyanate. When the prepared polymer composition for forming a primer layer was stored in a room temperature environment for one week, the viscosity significantly increased compared to before storage, and the composition could not be used for application by spin coating.

[0087] [Adhesion evaluation] Three eyeglass lenses were prepared for each of Examples 1 to 6. The prepared eyeglass lenses were evaluated for adhesion by the cross-cut method according to JIS K5600-5-6:1999. The number of remaining squares per 100 total squares is shown in Table 3. If the number of remaining squares is 99 or more, it can be said that the adhesion is excellent. From the results shown in Table 3, it can be confirmed that each of the eyeglass lenses of Examples 1 to 6 has excellent adhesion between the substrate and the photochromic layer.

[0088] [Table 3]

[0089] The various aspects and configurations described in this specification may be combined in any combination of two or more.

[0090] The embodiments disclosed herein should be considered to be illustrative and not restrictive in all respects. The scope of the present invention is defined by the claims, not the above description, and is intended to include all modifications within the meaning and scope of the claims. [Industrial Applicability]

[0091] The present invention is useful in technical fields such as glasses, goggles, sun visors, helmets, etc.

Claims

1. A substrate; A primer layer formed from a primer layer-forming polymer composition; a photochromic layer including a photochromic compound; in that order, The polymer composition for forming a primer layer is a polymer having a hydroxy group and a (meth)acryloyl group; Blocked isocyanate, A photochromic article comprising:

2. The photochromic article of claim 1 , wherein the polymer is a (meth)acrylic polymer.

3. The photochromic article according to claim 1 , wherein the photochromic layer is a cured layer obtained by curing a (meth)acrylate-based polymerizable composition containing a photochromic compound.

4. The photochromic article according to claim 2 , wherein the photochromic layer is a cured layer obtained by curing a (meth)acrylate-based polymerizable composition containing a photochromic compound.

5. The photochromic article according to any one of claims 1 to 4, which is a spectacle lens, a goggle lens, a visor portion of a sun visor, or a shield member of a helmet.

6. 6. The photochromic article of claim 5 which is a spectacle lens.

7. A pair of glasses comprising the eyeglass lens according to claim 6.

8. Applying a primer layer-forming polymer composition onto a substrate to form a primer layer; forming a photochromic layer containing a photochromic compound on the formed primer layer; Including, The polymer composition for forming a primer layer is a polymer having a hydroxy group and a (meth)acryloyl group; Blocked isocyanate, Including, heat-treating the laminate obtained by forming the photochromic layer; The method of making a photochromic article further comprises:

9. The method of claim 8 , wherein the polymer is a (meth)acrylic polymer.

10. The method for producing a photochromic article according to claim 8, comprising forming the photochromic layer by curing a (meth)acrylate-based polymerizable composition containing a photochromic compound.

11. The method for producing a photochromic article according to claim 9, comprising forming the photochromic layer by curing a (meth)acrylate-based polymerizable composition containing a photochromic compound.

12. The method for producing a photochromic article according to any one of claims 8 to 11, wherein the photochromic article is a spectacle lens, a goggle lens, a visor portion of a sun visor, or a shield member of a helmet.

Citation Information

Patent Citations

  • Polarizing photochromic articles

    JP2014523541A

  • Photochromic article having at least partially intersecting polarized photochromic dichromatic layers and a fixed polarizing layer

    JP2015531893A

  • Primer composition and photochromic layered body

    WO2017039019A1

  • Laminates, optical components, methods for manufacturing them, and coating liquids

    JP4405833B2

Cited By

  • Game machine

    JP2024166283A

  • Game machine

    JP2024166284A

  • Game machine

    JP2024166285A

  • Game machine

    JP2024169547A

  • Game machine

    JP2024169551A