Substrate and electroless copper plating method
By using a graphene oxide layer and copper coating without surface oxidation, the substrate achieves reduced transmission loss, addressing the rough interface issue in conventional copper plating methods and enhancing circuit board performance.
Patent Information
- Application Number
- JP2023055770
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Filing Date
- 2023-03-30
- Publication Date
- 2024-10-11
AI Technical Summary
Conventional electroless copper plating methods require surface roughening of the base material for catalyst support, leading to a rough interface that increases transmission loss of high-frequency electrical signals, making it difficult to use substrates as circuit boards effectively.
A substrate with a layer of graphene oxide and/or its derivative, followed by a copper coating, without surface oxidation treatment, to maintain a smooth interface and reduce transmission loss.
The method allows for the production of substrates with reduced transmission loss even at high frequencies, enabling efficient use as circuit boards.
Smart Images

Figure 2024143218000001_ABST
Abstract
Description
[Technical field]
[0001] The present invention relates to a substrate and an electroless copper plating method, and more particularly to a substrate used as a printed wiring board or the like, an electroless copper plating method, a method for manufacturing a substrate, and a product formed using the substrate. [Background technology]
[0002] Electroless plating is a method of forming a metal film on the plated object mainly by chemical reaction. Unlike electroplating using a DC power source, it is characterized by the supply of electrons from the base metal surface or a reducing agent for reduction. In particular, the copper film obtained by electroless copper plating is characterized by being inexpensive to form, having excellent electrical conductivity and heat dissipation, and being less likely to crack due to its low hardness. This type of electroless copper plating is used to make printed wiring boards, and various researches are being conducted in response to the increasing demand for high-performance printed wiring boards.
[0003] Conventional electroless copper plating requires (1) oxidation treatment (surface roughening treatment) of the substrate surface and (2) pretreatment with Pd particles as a catalyst for the plating reaction (reduction reaction) in order to improve adhesion and plating properties to the substrate (see, for example, Patent Document 1). [Prior art documents] [Patent documents]
[0004] [Patent Document 1] Japanese Patent Application Publication No. 63-168077 Summary of the Invention [Problem to be solved by the invention]
[0005] In conventional methods, the substrate surface must be roughened by oxidation treatment in order to support the catalyst. This roughens the interface between the copper coating and the surface to be plated, making it difficult to sufficiently reduce the transmission loss of high-frequency electrical signals when the substrate is used as a circuit board (see Figure 2, for example).
[0006] The present invention has been made in consideration of the above-mentioned current situation, and has an object to provide a method for easily producing a substrate having a copper coating, and for sufficiently reducing transmission loss even at high frequencies when the substrate is used as a circuit board. [Means for solving the problem]
[0007] The inventors have investigated various methods by which a substrate having a copper coating can be easily produced and transmission loss can be sufficiently reduced even at high frequencies when the substrate is used as a circuit substrate. They have found that a substrate having a base material, a layer of graphene oxide and / or a derivative thereof, and a copper coating, in that order, allows graphene oxide and its derivatives to perform their function of supporting various catalyst particles, etc., even without roughening the surface of the substrate, and the interface between the copper coating and the surface to be plated can remain smooth, thereby sufficiently reducing transmission loss even at high frequencies when the substrate is used as a circuit substrate. They have conceived the invention by which the above-mentioned problems can be brilliantly solved.
[0008] That is, the present invention (1) is a substrate characterized by having, in this order, a base material, a layer of graphene oxide and / or a derivative thereof, and a copper coating.
[0009] The present invention (2) is the substrate of the present invention (1), further comprising a layer of a metal element and / or a metal compound between the layer of graphene oxide and / or a derivative thereof and the copper coating.
[0010] The present invention (3) is the substrate of the present invention (1) or (2), which has not been subjected to an oxidation treatment.
[0011] The present invention (4) is a substrate according to any one of the present inventions (1) to (3), which is a circuit substrate.
[0012] The present invention (5) is an electroless copper plating method comprising the steps of forming a layer of graphene oxide and / or a derivative thereof on an upper side of a substrate, and forming a copper coating on the layer of graphene oxide and / or a derivative thereof by electroless copper plating.
[0013] The present invention (6) is the electroless copper plating method of the present invention (5), further comprising a step of forming a layer of a metal element and / or a metal compound on the layer of graphene oxide and / or a derivative thereof.
[0014] The present invention (7) relates to the electroless copper plating method according to the present invention (5) or (6), characterized in that the step of forming the copper coating is carried out using a plating composition containing a copper compound, a reducing agent, and water.
[0015] The present invention (8) is the electroless copper plating method according to any one of the present inventions (5) to (7), characterized in that it does not include a step of subjecting the substrate to an oxidation treatment.
[0016] The present invention (9) is a method for producing a substrate, comprising the steps of forming a layer of graphene oxide and / or a derivative thereof on an upper side of a base material, and forming a copper coating on the layer of graphene oxide and / or a derivative thereof by electroless copper plating.
[0017] The present invention (10) is a product constructed using the substrate of any one of the present inventions (1) to (4). Effect of the Invention
[0018] The substrate of the present invention can be easily produced, and when the substrate is used as a circuit board, the transmission loss can be sufficiently reduced even at high frequencies. [Brief description of the drawings]
[0019] [Figure 1] FIG. 1 is a schematic diagram showing a substrate having, in this order, a base material, a layer of graphene oxide and / or a derivative thereof, a layer of an elemental metal and / or a metal compound, and a copper coating. [Diagram 2] FIG. 2 is a schematic diagram showing a substrate produced by a conventional method. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0020] The present invention will be described in detail below. In addition, a combination of two or more of the preferred features of the present invention described in the following paragraphs is also a preferred embodiment of the present invention.
[0021] <Substrate> The substrate of the present invention comprises at least a substrate, a layer of graphene oxide and / or a derivative thereof, and a copper coating, in that order. In the following, the graphene oxide and / or its derivative layer, the substrate, and the copper coating will be described in that order.
[0022] (Layer of graphene oxide and / or its derivatives) The layer of graphene oxide and / or its derivative is a layer including graphene oxide and / or its derivative. Graphene oxide is a polar (hydrophilic) compound, and when a metal element or a metal compound is used as a catalyst for electroless copper plating, it can be supported by sufficiently interacting with the metal element or the metal compound by utilizing its hydrophilicity, and can also sufficiently interact with a substrate such as a hydrophobic substrate by intermolecular force due to its flake shape. In this way, the layer of graphene oxide and / or its derivative can exert an adhesive effect and play a role as a bridge between the substrate and the catalyst (see, for example, FIG. 1). In addition, the layer of graphene oxide and / or its derivative has high water resistance and stability, and is sufficiently suppressed from flowing out, mixing, or reacting when a catalyst-containing solution is applied. Furthermore, graphene oxide is essentially electronically and ionically conductive, so it does not hinder conduction in the substrate of the present invention.
[0023] The graphene oxide is a material in which oxygen is bonded to a graphitic carbon material such as graphene by oxidizing the material (oxygen is bonded to the carbon material), and the oxygen is present in the graphitic carbon material as a hydrophilic functional group such as a carboxyl group, a carbonyl group, a hydroxyl group, or an epoxy group. Generally, graphene is a 2It refers to a sheet consisting of one layer in which carbon atoms bonded by bonds are arranged in a plane, and a stack of many graphene sheets is called graphite, but the graphene oxide and / or derivatives thereof (layer of graphene oxide and / or derivatives thereof) in the present invention includes not only a sheet consisting of only one layer of carbon atoms, but also one having a structure in which about 2 to 100 layers are stacked. The graphene oxide and / or derivatives thereof (layer of graphene oxide and / or derivatives thereof) is preferably a sheet consisting of only one layer of carbon atoms or one having a structure in which about 2 to 20 layers are stacked, and more preferably a sheet consisting of only one layer of carbon atoms.
[0024] The graphene oxide may be reduced graphene oxide. The reduced graphene oxide is obtained through a process of removing hydrophilic functional groups from graphene oxide and reducing the graphene oxide, and may be obtained through a process of removing hydrophilic functional groups from graphene oxide in the graphene oxide layer after forming the graphene oxide layer.
[0025] The graphene oxide derivative is not particularly limited, but is preferably one in which a functional group such as a nitrogen-containing group is introduced into a hydrophilic functional group of graphene oxide by treating graphene oxide with an amine or ammonia. For example, compounds for treating (reacting) graphene oxide include ammonia, alkylamines (including primary, secondary, tertiary and quaternary ammonium), and arylamines, and the amino groups in these compounds that may have a substituent may be present in a single molecule (ethylenediamine, diethylenetriamine, phenylenediamine, etc.). Furthermore, polymers such as polyethyleneimine, polyallylamine, and polydiallyldimethylammonium chloride having a plurality of amino groups may be used. This further improves the interaction between the graphene oxide derivative and a metal element or metal compound as a substrate or catalyst. In the treatment step, the compound is preferably allowed to act on graphene oxide in a graphene oxide dispersion to form a graphene oxide derivative in advance and then form a film, or the compound is preferably allowed to act on the graphene oxide layer after forming a graphene oxide layer to obtain a graphene oxide derivative layer. In the above treatment process, the derivatization is possible by simply contacting graphene oxide (anionic) with the compound (cationic), but it is also preferable to actively form bonds to further enhance the interaction. For example, the reaction can be accelerated by heating or adding a catalyst.
[0026] As described above, the graphene oxide or its derivative may further have a functional group such as a nitrogen-containing group, and for example, the content of nitrogen as a constituent element with respect to all constituent elements is preferably 1 mol % or more and 10 mol % or less. Note that, the graphene oxide or its derivative preferably has the content of carbon, hydrogen, and oxygen as constituent elements with respect to all constituent elements of 90 mol % or more.
[0027] The graphene oxide or derivative thereof preferably has a ratio of the number of carbon atoms to the number of oxygen atoms (C / O) of 5.5 or less. The ratio is more preferably 5 or less, and even more preferably 4 or less. When the ratio is in this range, there are sufficient oxygen functional groups capable of interacting with each other, and the effect can be exerted. Moreover, the ratio is preferably 1 or more from the viewpoint of ensuring the graphene skeleton structure. The ratio of the number of carbon atoms to the number of oxygen atoms can be confirmed by the ratio of the total peak area in the O1s region to the total peak area in the C1s region obtained by XPS measurement.
[0028] In the graphene oxide or derivative thereof layer, the mass ratio of the graphene oxide or derivative thereof is preferably 80 mass% or more, more preferably 90 mass% or more, further preferably 95 mass% or more, and particularly preferably 99 mass% or more. Among them, it is most preferable that the graphene oxide or derivative thereof layer is substantially composed of graphene oxide or derivative thereof. In the case where the layer of graphene oxide or a derivative thereof contains a component other than graphene oxide, examples of the component include a conductive assistant, a binder, a colorant, a solvent, and the like.
[0029] The layer of graphene oxide or a derivative thereof preferably has an average thickness of 1 to 100 nm, more preferably 20 nm or less, and further preferably 5 nm or less. The average thickness can be measured by measuring the thickness at five randomly selected points in the layer of graphene oxide or a derivative thereof using an atomic force microscope or a scanning electron microscope and calculating the average value.
[0030] (base material) As the substrate, various known substrates can be used, which can ensure that the strength and other properties of the substrate of the present invention are sufficient. Examples of the substrate include insulating substrates such as glass, polyethylene terephthalate (PET), epoxy resin, polyimide resin, and glass epoxy resin; conductive substrates such as metal films, indium tin oxide (ITO) films, indium zinc oxide (IZO) films, graphite films, graphene films, and carbon nanotube films; and among these, insulating substrates are preferred, and glass and resin are more preferred in that a smooth substrate can be produced. Note that, by using graphene oxide or a derivative thereof according to the present invention, electroless copper plating can be suitably performed on smooth substrates such as glass and resin, which have been difficult to use as substrates for electroless copper plating in the past.
[0031] The substrate may or may not be surface-treated by hydrophilization treatment such as UV / ozone treatment, amine treatment, ammonia treatment, etc., but a treated substrate (more preferably a glass substrate or a resin substrate such as PET) is preferred, which is surface-treated by at least one treatment selected from the group consisting of hydrophilization treatment, amine treatment, and ammonia treatment. For example, one of the more preferred embodiments of the present invention is a glass substrate (MAS) having amino groups on its surface, which is obtained by surface-treating a glass substrate by amine treatment and / or ammonia treatment. This can further enhance the interaction with the layer of graphene oxide or a derivative thereof.
[0032] The substrate is preferably not subjected to an oxidation treatment (surface roughening treatment). In other words, the substrate is preferably not roughened by an oxidation treatment. In the substrate of the present invention, even if the substrate is not subjected to an oxidation treatment, graphene oxide or a derivative thereof can exhibit the performance of supporting various catalyst particles and the like. Furthermore, since the substrate is not subjected to an oxidation treatment, the interface between the copper coating and the surface to be plated can be made smoother, and when the substrate of the present invention is used as a circuit board, for example, it can be a highly efficient circuit board.
[0033] The substrate preferably has a water contact angle of 40 degrees or more, more preferably 50 degrees or more, further preferably 60 degrees or more, and particularly preferably 70 degrees or more. Even though the surface of the substrate is thus hydrophobic, it can sufficiently interact with a layer of graphene oxide or a derivative thereof, which is in the form of a flake. The contact angle can be measured by a sessile drop method.
[0034] The average thickness of the substrate is preferably 10 μm or more and 50 mm or less, more preferably 50 μm or more, and more preferably 10 mm or less. The average thickness can be measured by measuring the thickness at five randomly selected points on the substrate using a caliper and calculating the average value.
[0035] (copper coating) The copper coating is a coating containing copper as a main component, and is a plating layer. The term "containing copper as a main component" means that the content of copper as a constituent element in the copper coating is 80 mol % or more. The copper coating is usually present on the surface of the substrate, but it does not have to be present on the entire substrate surface; it may be present on only a portion of the substrate surface after etching or the like, and may be, for example, in the form of a wiring. The copper coating is preferably located on the upper surface side (uppermost layer) of a conductive layer composed of the copper coating and, if desired, other conductive films.
[0036] The content of copper as a constituent element in the copper coating is preferably 90 mol % or more, more preferably 95 mol % or more, and even more preferably 99 mol % or more. Of these, it is most preferable that the copper coating is substantially composed of copper. When the copper coating contains a component other than copper, the component may include a conductive assistant, a colorant, a solvent, etc. The copper coating may have an oxide film formed on its surface by air oxidation or the like.
[0037] The average thickness of the copper coating is preferably 100 nm or more and 100 μm or less, more preferably 1 μm or more, and even more preferably 10 μm or less. The average thickness can be measured by measuring the thickness at five randomly selected points on the copper coating using the device described in the Examples and calculating the average value.
[0038] The volume resistivity of the copper coating is 1.0×10 -6 Ωcm or more, 1.0×10 -5 It is preferable that the electrical conductivity is Ωcm or less, which allows the substrate of the present invention to exhibit sufficient electrical conductivity when used as a circuit substrate or the like. The volume resistivity of the copper coating is measured by the method described in the examples.
[0039] (Layer of metal element and / or metal compound) The substrate of the present invention may further have a layer of a metal element and / or a metal compound between the layer of graphene oxide and / or a derivative thereof and the copper coating. That is, the substrate of the present invention preferably has a base material, a layer of graphene oxide and / or a derivative thereof, a layer of a metal element and / or a metal compound, and a copper coating in this order. The metal element and / or metal compound usually functions as a catalyst for electroless copper plating.
[0040] Examples of the metal constituting the simple metal and / or metal compound include aluminum, iron, cobalt, nickel, tin, lead, antimony, bismuth, copper, silver, palladium, iridium, platinum, and gold, and one or more of these can be used. The metal is preferably a noble metal such as silver, gold, or palladium, or copper, and more preferably silver. Silver can be stabilized in a nanoparticle state by graphene oxide or a derivative thereof. Examples of the metal compound include metal oxides, metal hydroxides, metal halides, and metal nitrates. The layer of a simple metal and / or a metal compound includes a layer in which the simple metal and / or a metal compound exists in a particulate state (eg, nanoparticle state) as well as a layer in which the metal exists as ions.
[0041] The metal element and / or metal compound is preferably in a particulate form, such as fine powder, powder, granules, flakes, polyhedrons, rods, or shapes containing curved surfaces. The metal element and / or metal compound preferably has an average particle size of 10 nm or more and 10 μm or less. By using such an average particle size, the reduction reaction of the copper compound can be more efficiently carried out. The average particle size can be measured by a particle size distribution measuring device.
[0042] In the layer of the metal element and / or metal compound, the mass ratio of the metal element and / or metal compound is preferably 80 mass% or more, more preferably 90 mass% or more, further preferably 95 mass% or more, and particularly preferably 99 mass% or more. Among them, it is most preferable that the layer of the metal element and / or metal compound is substantially composed of the metal element and / or metal compound. When the layer of the simple metal and / or metal compound contains a component other than the simple metal or metal compound, examples of the component include a conductive assistant and a solvent.
[0043] The average thickness of the layer of the simple metal and / or metal compound is preferably 10 nm or more and 100 μm or less, more preferably 50 nm or more, and more preferably 10 μm or less. The average thickness can be measured by using a vernier caliper or a stylus type step gauge to measure the thickness at five randomly selected points in the layer of the simple metal and / or metal compound, and calculating the average value.
[0044] Although the copper coating may be present on the layer of the simple metal and / or metal compound, it is preferable that the copper coating is present directly on the layer of the simple metal and / or metal compound, i.e., the layer of the simple metal and / or metal compound is preferably the layer to be plated.
[0045] The substrate of the present invention is preferably a circuit board. When the substrate of the present invention is a circuit board, the transmission loss can be sufficiently reduced even at high frequencies. The copper coating is usually arranged as wiring on the substrate surface.
[0046] <Electroless copper plating method> The present invention also relates to an electroless copper plating method including a step of forming a layer of graphene oxide and / or a derivative thereof on an upper side of a substrate, and a step of forming a copper coating on the layer of graphene oxide and / or a derivative thereof by electroless copper plating.
[0047] (Step of forming a layer of graphene oxide and / or its derivative on the upper side of the substrate) The above step is not particularly limited, but can be easily performed, for example, by a method (contact method) of contacting a substrate with an aqueous dispersion of graphene oxide and / or a derivative thereof. The contact method is not particularly limited, but suitable examples include a method of impregnating a substrate with an aqueous dispersion of graphene oxide and / or a derivative thereof, and a method of spin-coating a substrate with an aqueous dispersion of graphene oxide and / or a derivative thereof. This allows the above-mentioned graphene oxide layer and / or a layer of a derivative thereof to be formed on the substrate. When the substrate is impregnated in an aqueous dispersion of graphene oxide and / or a derivative thereof, the impregnation time can be 5 seconds or more and 5 hours or less. In addition, it is preferable to include a washing step after the contact step. The washing step can effectively remove excess graphene oxide and impurities. The washing step is preferably performed by immersing the substrate in a washing liquid, spraying the substrate with the washing liquid, or the like. The washing liquid is not particularly limited, and may be an aqueous dispersion liquid partially containing an organic dispersion medium or an inorganic component, but is preferably composed of only water.
[0048] The above-mentioned aqueous dispersion of graphene oxide can be obtained by dispersing graphite oxide in water, exfoliating the layers by ultrasonic treatment, homogenizer treatment, or the like, and dispersing graphene oxide in water. The above-mentioned aqueous dispersion of a graphene oxide derivative can be obtained by subjecting graphene oxide to a derivatization treatment, purifying it as necessary, and dispersing it in water. The aqueous dispersion medium may be an aqueous dispersion liquid containing an organic dispersion medium in part, but is preferably composed of water only. The concentration of the graphene oxide and / or its derivative in the aqueous dispersion is preferably 10 mg / L or more, more preferably 30 g / L or less, more preferably 20 g / L or less, and even more preferably 10 g / L or less.
[0049] The step of forming the graphene oxide and / or derivative thereof is preferably carried out at a temperature of 5 to 120° C., for example. After the graphene oxide and / or derivative thereof layer is formed, the graphene oxide and / or derivative thereof layer may be heat-treated. This can improve the hardness of the layer and stabilize it. When the heat treatment is performed, the temperature is preferably 60 to 200° C., and more preferably 70 to 150° C. The heat treatment time is preferably 5 minutes to 5 hours, and more preferably 10 minutes to 2 hours.
[0050] The graphene oxide can be obtained by oxidizing graphite using any of the Hummers method, the Brodie method, the Staudenmaier method, etc., or by using a method in which a permanganate is added to a mixed solution containing graphite and sulfuric acid, employing the Hummers method as the oxidation method. Furthermore, an oxidation reaction stopping step, a concentration step, a purification step, a peeling step, etc. can be performed as necessary. The graphene oxide derivative can be obtained by treating the graphene oxide with an amine, ammonia, etc. For example, a nitrogen-containing group can be introduced into a hydrophilic functional group of the graphene oxide by mixing an aqueous dispersion in which the graphene oxide is dispersed with an amine and / or ammonia and reacting the mixture.
[0051] (A process for forming a copper coating on the top of a layer of graphene oxide and / or its derivatives by electroless copper plating) The step of forming the copper coating can be performed by electroless copper plating. This allows the copper coating to be suitably formed on the layer of graphene oxide and / or its derivative. As described later, the formation of the copper coating on the layer of graphene oxide and / or its derivative preferably means forming a layer of a metal simple substance and / or a metal compound on the layer of graphene oxide and / or its derivative, and forming the copper coating on the layer of the metal simple substance and / or the metal compound.
[0052] The step of forming the copper coating is usually carried out using a plating composition containing a copper compound, a reducing agent, and a solvent. As the solvent for the plating composition, water, an organic solvent, or a mixture of water and an organic solvent can be used. As the organic solvent, an alcohol-based solvent can be preferably used. The solvent is preferably water or a mixture of water and an organic solvent, and more preferably water. That is, the plating composition preferably contains a copper compound, a reducing agent, and water. As the water, ion-exchanged water, industrial water, tap water, etc. can be preferably used. Examples of the copper compound include copper oxide, copper hydroxide, copper sulfate, and hydrates thereof. Among these, copper sulfate and its hydrate are preferred.
[0053] In the plating composition, the ratio of the copper compound is preferably 0.015M or more and 0.075M or less. When the ratio of the copper compound is 0.015M or more, the volume resistivity can be lowered. When the ratio of the copper compound is 0.075M or less, the film thickness can be made more sufficient. More preferably, the ratio of the copper compound is 0.03M or more and 0.06M or less.
[0054] The reducing agent is not particularly limited as long as it can reduce the copper compound to obtain metallic copper, but is typically formaldehyde, glyoxylic acid, etc., and glyoxylic acid is preferred. The ratio of the reducing agent in the plating composition is preferably 0.05M or more and 0.40M or less. When the ratio of the reducing agent is 0.05M or more, the surface condition of the copper coating is more excellent. When the ratio of the reducing agent is 0.40M or less, the volume resistivity can be made lower. The ratio of the reducing agent is more preferably 0.08M or more and 0.25M or less.
[0055] The plating composition preferably further contains a ligand component that coordinates to monovalent copper ions and / or divalent copper ions. In particular, the plating composition more preferably contains a ligand component that coordinates to monovalent copper ions and a ligand component that coordinates to divalent copper ions. Examples of the ligand component include a hexadentate ligand such as ethylenediaminetetraacetic acid (EDTA) and a bidentate ligand such as 2,2'-bipyridyl. Note that 2,2'-bipyridyl coordinates to monovalent copper ions, and EDTA coordinates to divalent copper ions. In the plating composition, the ligand component may or may not be coordinated to the copper ion (derived from the copper compound).
[0056] When the plating composition contains a ligand component that coordinates to a monovalent copper ion, the mass proportion of the ligand component (excluding copper ions) that coordinates to a monovalent copper ion in 1 L of the plating composition is preferably 0.01 mg or more and 1 mg or less, and more preferably 0.1 mg or more and 0.5 mg or less.
[0057] When the plating composition contains a ligand component that coordinates to divalent copper ions, the ratio of the ligand component (excluding copper ions) that coordinates to divalent copper ions in the plating composition is preferably 0.1 M or more and 1 M or less, and more preferably 0.2 M or more and 0.5 M or less.
[0058] The plating composition preferably has a pH of 10 or more. This improves the solubility of by-products of the reduction reaction, such as oxalates, and allows the copper coating to be more suitably formed. The pH is more preferably 11 or more. The pH is preferably 14 or less, and more preferably 13 or less. To adjust the pH, a base such as sodium hydroxide or potassium hydroxide can be used as appropriate. The pH is measured at 25° C. using a pH meter.
[0059] The step of forming the copper coating can be carried out at, for example, 5 to 100°C, and is preferably carried out at 50 to 80°C. The step of forming the copper coating can be carried out for, for example, 5 minutes to 24 hours, and is preferably carried out for 30 minutes to 12 hours. After the copper coating is formed, it is preferable to heat treat the copper coating. This improves the quality of the copper coating. The heat treatment temperature is preferably 80 to 500° C., and more preferably 100 to 400° C. The heat treatment time is preferably 10 minutes to 6 hours, and more preferably 20 minutes to 3 hours.
[0060] (Step of forming a layer of a metal element and / or a metal compound on the top of a layer of graphene oxide and / or a derivative thereof) The electroless copper plating method of the present invention preferably further comprises a step of forming a layer of a metal element and / or a metal compound on the layer of the graphene oxide and / or a derivative thereof, which is usually performed before the step of forming a copper coating by electroless copper plating on the layer of the graphene oxide and / or a derivative thereof.
[0061] The step of forming the layer of the metal element and / or metal compound can be easily performed by a method (contact method) of contacting a layer of graphene oxide and / or a derivative thereof with an aqueous dispersion of the metal element and / or metal compound. The contact method is not particularly limited, but a preferred example is a method of impregnating a substrate having a layer of graphene oxide and / or a derivative thereof with an aqueous dispersion of the metal element and / or metal compound. This allows the layer of the metal element and / or metal compound to be easily formed on the layer of graphene oxide and / or a derivative thereof. When the substrate having the layer of graphene oxide and / or its derivative is impregnated with the aqueous dispersion of a metal element and / or a metal compound, the impregnation time can be 5 seconds or more and 5 hours or less, and the temperature can be 30 to 85° C.
[0062] The aqueous dispersion of the metal element and / or metal compound can be obtained by dispersing or dissolving the metal element and / or metal compound in water. The aqueous dispersion medium may be an aqueous dispersion liquid containing an organic dispersion medium in part, but is preferably composed of water only. The concentration of the metal element and / or metal compound in the aqueous dispersion is preferably 0.01 M or more, and more preferably 0.05 M or more. The concentration is preferably 2 M or less, more preferably 1 M or less, and even more preferably 0.5 M or less.
[0063] The electroless copper plating method of the present invention may further include a step of washing the surface of the substrate or the like with water and a step of drying the surface between each step.
[0064] It is preferable that the electroless copper plating method of the present invention does not include a step of oxidizing the substrate. Even if the electroless copper plating method of the present invention does not include a step of oxidizing the substrate, the layer of graphene oxide and / or a derivative thereof formed in the step of forming a layer of graphene oxide and / or a derivative thereof can exhibit the performance of supporting various catalyst particles, etc. Furthermore, since the substrate is not oxidized, the interface between the copper coating and the surface to be plated can be made smoother, and when the substrate of the present invention is used as a circuit board, for example, it can be a highly efficient circuit board.
[0065] The electroless copper plating method of the present invention may be carried out in air or in an inert gas atmosphere such as nitrogen, helium, argon, etc. Also, it may be carried out under pressurized conditions, normal pressure conditions, or reduced pressure conditions.
[0066] <Substrate manufacturing method> The present invention is also a method for producing a substrate, comprising the steps of forming a layer of graphene oxide and / or a derivative thereof on an upper side of a base material, and forming a copper coating on the layer of graphene oxide and / or a derivative thereof by electroless copper plating.
[0067] <Product> The present invention also relates to a product formed using the substrate of the present invention. Examples of the products include various products equipped with printed circuit boards, such as electronic components used in home appliances, in-vehicle devices, transport equipment, and communication equipment. EXAMPLES
[0068] The present invention will be described in more detail below with reference to examples, but the present invention is not limited to these examples. In addition, unless otherwise specified, "parts" means "parts by mass" and "%" means "% by mass".
[0069] [Raman spectrum measurement] The Raman spectroscopic analysis was carried out using the following equipment and conditions. Measurement equipment: Raman microscope (JASCO Corporation, NRS-3100) Measurement conditions: 532 nm laser, 20x objective lens, 1 second CCD capture time, integration 32 times (resolution=4cm -1 ) Measurement content: The presence of graphene oxide is confirmed by the presence or absence of the G and D bands that are characteristic of graphene oxide.
[0070] [X-ray photoelectron spectroscopy (XPS)] The analysis was performed under the following conditions to confirm the oxygen and carbon contents. Shimadzu Kratos AXIS-NOVA X-ray source, output AlKα - 100W, pass energy 40eV, neutralization gun ON
[0071] [Evaluation of physical properties of copper film] Film thickness [μm]: Measured with a micrometer (Mitutoyo, QuantuMike) or a tabletop scanning electron microscope (JEOL, JCM-6000) with an energy dispersive X-ray analyzer (SEM-EDS). Surface condition: The presence or absence of segregation and pores in the deposited copper film was evaluated using a digital microscope and a benchtop SEM. Average volume resistivity [Ωcm]: The sheet resistance value [Ω / □] was measured at 10 points on each copper film using a resistivity meter (Mitsubishi Chemical Corporation, MCP-T360) and a four-probe probe (Mitsubishi Chemical Corporation, MCP-TPQPP) by the four-probe method, and the values multiplied by the film thickness [cm] were averaged to calculate the average.
[0072] [Preparation Example 1] Preparation of graphene oxide dispersion A graphene oxide dispersion was synthesized by the following process. 15 g of graphite (Z-25 manufactured by Ito Graphite Co., Ltd.) and 640 g of sulfuric acid (manufactured by Fujifilm Wako Pure Chemical Industries, Ltd.) were placed in a reaction vessel, and 45 g of potassium permanganate (manufactured by Fujifilm Wako Pure Chemical Industries, Ltd.) was added while adjusting the temperature to 30° C. After the addition, the temperature was raised to 35° C. for 30 minutes, and the reaction was allowed to proceed for 2 hours. After the reaction, 1070 ml of water and 42 ml of 30% hydrogen peroxide solution (manufactured by Fujifilm Wako Pure Chemical Industries, Ltd.) were added to the reaction solution to stop the reaction. The resulting reaction solution was purified by repeatedly removing the supernatant through static sedimentation and redispersing with ion-exchanged water. After purification, a peeling operation was performed using a homogenizer to prepare graphene oxide dispersion (1) (1.2% aqueous dispersion). The obtained graphene oxide was found to be a single layer by observation under an electron microscope. The C / O ratio calculated by XPS analysis was 1.82.
[0073] [Preparation Example 2] Preparation of plating solution A 5.0 mM 2,2'-bipyridyl aqueous solution was mixed with a mixed solution of 0.045 M CuSO4, 0.36 M EDTA, and 0.10 M glyoxylic acid to give a concentration of 2.0 ppm, and the pH was adjusted to 12.0 with a KOH aqueous solution using a benchtop pH meter (HORIBA, F-53) to obtain a plating solution.
[0074] [Examples 1-4] The graphene oxide dispersion (1) was diluted 10 times with distilled water to obtain a 0.12 wt% graphene oxide aqueous dispersion. A slide glass (Example 1, contact angle 22.5 degrees), a glass surface modified with an amino group (Example 2, Matsunami Glass Industry Co., Ltd., MAS-01, contact angle 45.0 degrees), a PET film (Example 3, Kokuyo Co., Ltd., VF-5, contact angle 80 degrees), and a UV / ozone treated PET film (Example 4, contact angle 50 degrees) were cut into 15 x 26 mm pieces, washed with distilled water / Solmix, and immersed in a 0.12 wt% graphene oxide aqueous dispersion for 1 hour to produce a graphene oxide thin film substrate. After impregnation, excess graphene oxide components were removed by washing with water. The graphene oxide thin film substrate was immersed in a 0.10 M AgNO3 aqueous solution that had been previously bubbled with nitrogen gas for 10 minutes to remove dissolved oxygen, and then heated at 75°C for 30 minutes, whereby Ag ions were reduced by graphene oxide to prepare an AgNPs / graphene oxide substrate carrying silver nanoparticles (AgNPs). The AgNPs / graphene oxide substrate was immersed and washed in distilled water at least three times to remove excess AgNO3 aqueous solution. In all samples, absorption at 200-500 nm due to surface plasmon resonance of AgNPs was confirmed by UV-vis, and a peak due to graphene oxide was confirmed by Raman analysis.
[0075] 20 mL of the plating solution obtained in Preparation Example (2) was added to a fluorine-treated container, and the solution was heated uniformly to 60°C in an aluminum bath to reproduce a plating bath. The AgNPs / graphene oxide substrate obtained above was fixed with a polyethylene-coated wire (Daiso Industries, A-wire color No. 06) that had been deformed so that it could be held diagonally. While being careful not to let the AgNPs / GO substrate touch the inner wall or bottom of the container, it was immersed until it was completely immersed in the plating bath, and electroless copper plating was performed for 1 hour. After plating, it was rinsed with ethanol and dried in the air. The obtained copper film thickness was 3 μm, and the volume resistivity was 5.6 × 10 -6 Ωcm (Example 1), 3.9×10 -6 Ωcm (Example 2), 6.4×10 -6 Ωcm (Example 3), 4.6×10 -6In terms of volume resistivity, the glass having an amine surface and the PET having been subjected to a hydrophilic treatment were better than the untreated glass. [Explanation of symbols]
[0076] 1: Base material 2: Layer of graphene oxide and / or its derivatives 3: Layer of metal element and / or metal compound 4: Copper coating 11: Substrate etched with an oxidizing etchant 12: Palladium nanoparticle layer 13: Copper coating
Claims
1. A substrate comprising, in this order, a base material, a layer of graphene oxide and / or a derivative thereof, and a copper coating.
2. The substrate according to claim 1 , further comprising a layer of a metal element and / or a metal compound between the layer of graphene oxide and / or its derivative and the copper coating.
3. 3. The substrate according to claim 1, wherein the base material is not subjected to an oxidation treatment.
4. 3. The substrate according to claim 1, which is a circuit board.
5. An electroless copper plating method comprising the steps of: forming a layer of graphene oxide and / or a derivative thereof on an upper side of a substrate; and forming a copper coating on the layer of graphene oxide and / or a derivative thereof by electroless copper plating.
6. The electroless copper plating method according to claim 5 , further comprising a step of forming a layer of a metal element and / or a metal compound on the layer of graphene oxide and / or a derivative thereof.
7. 7. The method for electroless copper plating according to claim 5, wherein the step of forming the copper film is carried out using a plating composition containing a copper compound, a reducing agent, and water.
8. 7. The electroless copper plating method according to claim 5, further comprising the step of oxidizing the substrate.
9. A method for manufacturing a substrate, comprising: a step of forming a layer of graphene oxide and / or a derivative thereof on an upper side of a base material; and a step of forming a copper coating on the layer of graphene oxide and / or a derivative thereof by electroless copper plating.
10. A product constructed using the substrate according to claim 1 or 2.
Citation Information
Patent Citations
Flexible circuit board and manufacturing method thereof
CN111031664A
Flexible printed circuit and method for manufacturing the same
EP3657917A1
Plating method of resin using graphene thin film
JP2011241479A
Plating and method for forming same
JP2020515711A
Manufacture of printed wiring board