Dip-molded body, and latex for dip molding

By adjusting the tensile storage modulus and using a specific plasticizer, chlorosulfonated polyolefin gloves are made flexible and less fatiguing, addressing the inflexibility and fatigue issues of existing gloves.

JP2024143220APending Publication Date: 2024-10-11SUMITOMO SEIKA CHEM CO LTD
View PDF 5 Cites 0 Cited by

Patent Information

Application Number
JP2023055779
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Filing Date
2023-03-30
Publication Date
2024-10-11

AI Technical Summary

Technical Problem

Chlorosulfonated polyolefin gloves are inflexible and cause fatigue when worn for long periods due to high tensile modulus, limiting their use in applications requiring both flexibility and protective properties.

Method used

Adjusting the tensile storage modulus of chlorosulfonated polyolefin latex to 1-10 MPa and incorporating a specific plasticizer, such as a reactive plasticizer, to produce a dip-molded article with improved flexibility and reduced fatigue.

Benefits of technology

The solution results in a flexible dip-molded article that reduces hand fatigue and maintains excellent protective properties, making it suitable for prolonged use.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024143220000001
    Figure 2024143220000001
  • Figure 2024143220000002
    Figure 2024143220000002
  • Figure 2024143220000003
    Figure 2024143220000003
Patent Text Reader

Abstract

To provide a chlorosulfonated polyolefin molded body (especially gloves) that is flexible, has little fatigue even when worn and used for a long time, and has excellent protective properties.SOLUTION: A dip-molded body is produced by dip-molding a chlorosulfonated polyolefin latex, and has a thickness of 0.3 mm or more, and a tensile storage modulus of 1 to 10 MPa at 25°C and 1 Hz.SELECTED DRAWING: None
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present disclosure relates to a dip-molded article and a composition for preparing a dip-molded article (a dip-molding latex). More specifically, the present disclosure relates to a dip-molded article containing a chlorosulfonated polyolefin and having excellent flexibility, and a dip-molding latex composition for producing the same. [Background technology]

[0002] Rubber gloves and sacks are widely used for housework, various industrial purposes such as food industry and electronic component manufacturing industry, and medical purposes. Rubber gloves and sacks are worn to protect the hands from chemicals such as acids and alkalis, poisonous substances, organic solvents, or blades, heat, radiation, etc. as their basic function. In addition, important functions such as not tiring even when used for a long time and not easily deteriorating even when repeatedly bent are also required. For example, Patent Document 1 discloses a method for producing a dip-molded product obtained by dip-molding a dip-molding composition containing a carboxy-modified nitrile rubber latex and an organic peroxide, and that the latex particles in the carboxy-modified nitrile rubber latex contain 50 to 90% by weight of methyl ethyl ketone insoluble matter, thereby obtaining a glove having excellent tensile strength and bending fatigue resistance, and in which the glove is unlikely to lose adhesion and tracking ability to the hand when worn when made into a rubber glove.

[0003] Gloves made of chlorosulfonated polyolefin are generally not disposable and are thicker than other rubber gloves. Therefore, they are less flexible than other rubber gloves when bending the fingers, and may feel stiff and cause fatigue after long hours of work. However, they are more resistant to strong acids and strong alkalis than other rubber gloves, so they are often used in particularly dangerous work. On the other hand, it is difficult to make them thinner and more flexible from the viewpoint of worker protection.

[0004] Known methods for producing chlorosulfonated polyolefin rubber gloves include a method of dissolving rubber in an organic solvent (e.g., Patent Document 2) and a method of producing gloves using rubber latex (e.g., Patent Documents 3 and 4). [Prior art documents] [Patent documents]

[0005] [Patent Document 1] Patent No. 4839676 [Patent Document 2] Japanese Patent Application Publication No. 05-230702 [Patent Document 3] JP 2011-032590 A [Patent Document 4] Patent No. 7033242 Summary of the Invention [Problem to be solved by the invention]

[0006] The present inventors have conducted studies with the aim of providing a chlorosulfonated polyolefin molded product (particularly a glove) which is flexible, causes little fatigue even when worn for a long period of time, and has excellent protective properties. [Means for solving the problem]

[0007] The present inventors have conducted extensive research into the relationship between the physical properties of a dip-molded product obtained from a chlorosulfonated polyolefin latex and the wearing comfort of the dip-molded product (e.g., a glove), and have found that if the tensile storage modulus of the dip-molded product obtained at 1 Hz and 25°C is 1 MPa or more and less than 10 MPa, the product is flexible and does not easily cause fatigue even when worn for a long time. Furthermore, the present inventors have conducted extensive research to find conditions necessary for obtaining a dip-molded product that satisfies the above conditions, and have found that a dip-molded product that satisfies the above physical properties (tensile storage modulus) can be obtained by adjusting the structure of the chlorosulfonated polyolefin that constitutes the latex or the blending of the dip-molding latex composition. In particular, the present inventors have found that a dip-molded product that satisfies the above physical properties can be obtained by setting the chlorine content in the chlorosulfonated polyolefin within a specific range or by using a dip-molding latex composition blended with a specific plasticizer.

[0008] The present disclosure includes, for example, the subject matter described in the following sections: Section 1. A dip-molded article produced by dip-molding a chlorosulfonated polyolefin latex, The thickness is 0.3 mm or more, The tensile storage modulus at 25°C and 1Hz is 1 to 10MPa. Dip-molded body. Section 2. Item 2. The dip-molded article according to Item 1, wherein the chlorine content in the chlorosulfonated polyolefin constituting the chlorosulfonated polyolefin latex is 30 to 40% by mass. Section 3. 3. The dip-molded article according to item 1 or 2, wherein the chlorosulfonated polyolefin latex contains 5 to 20 parts by mass of a plasticizer based on 100 parts by mass of the chlorosulfonated polyolefin. Section 4. Item 4. The dip-molded article according to Item 3, wherein the plasticizer is a reactive plasticizer having a reactive group capable of crosslinking the chlorosulfonated polyolefin (e.g., animal and vegetable oil-based plasticizers such as castor oil, linseed oil, soybean oil, epoxidized linseed oil, epoxidized soybean oil, and epoxidized fatty acid; liquid rubber-based plasticizers such as liquid isoprene rubber, liquid butadiene rubber, liquid styrene butadiene rubber, liquid ethylene-propylene-diene rubber, and liquid acrylic rubber). Section 5. Item 5. The dip-molded article according to any one of Items 1 to 4, wherein the chlorosulfonated polyolefin is a chlorosulfonated polyethylene. Section 6. 6. The dip-molded article according to any one of items 1 to 5, having a tensile storage modulus of 0.5 to 5 MPa at 40° C. and 1 Hz. Section 7. Item 7. The dip-molded article according to any one of Items 1 to 6, wherein the molded article is a glove. Section 8. Item 7. The dip-molded article according to any one of Items 1 to 6, which is a sack. Effect of the Invention

[0009] It is possible to provide a chlorosulfonated polyolefin molded product (particularly a glove) that is flexible, causes little fatigue even when worn for a long period of time, and has excellent protective properties, thereby reducing the burden on the worker wearing the molded product (particularly on the hands and fingers). DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0010] Each embodiment included in the present disclosure will be described in more detail below. The present disclosure preferably includes a dip-molded product of a specific chlorosulfonated polyolefin latex, a chlorosulfonated polyolefin latex (a dip-molding composition) for preparing the dip-molded product, and the like, but is not limited thereto, and the present disclosure includes all that is disclosed in the present specification and that can be recognized by a person skilled in the art.

[0011] The dip-molded article included in the present disclosure is a dip-molded article produced by dip-molding a chlorosulfonated polyolefin latex, and has a thickness of 0.3 mm or more and a tensile storage modulus of 1 to 10 MPa at 25° C. and 1 Hz. Such a dip-molded article may be referred to as the dip-molded article of the present disclosure.

[0012] The tensile storage modulus of the dip-formed body of the present disclosure at 25° C. and 1 Hz is 1 to 10 MPa as described above. The upper or lower limit of the range is, for example, 1.1, 1.2, 1.3, 1.4, 1.5, 1.6, 1.7, 1.8, 1.9, 2, 2.1, 2.2, 2.3, 2.4, 2.5, 2.6, 2.7, 2.8, 2.9, 3, 3.1, 3.2, 3.3, 3.4, 3.5, 3.6, 3.7, 3.8, 3.9, 4, 4.1, 4.2, 4.3, 4.4, 4.5, 4.6, 4.7, 4.8, 4.9, 5, 5.1, 5.2, 5.3, 5. 4, 5.5, 5.6, 5.7, 5.8, 5.9, 6, 6.1, 6.2, 6.3, 6.4, 6.5, 6.6, 6.7, 6.8, 6.9, 7, 7.1, 7.2, 7.3, 7.4, 7.5, 7.6, 7.7, 7.8, 7.9, 8, 8.1, 8.2, 8.3, 8.4, 8.5, 8.6, 8.7, 8.8, 8.9, 9, 9.1, 9.2, 9.3, 9.4, 9.5, 9.6, 9.7, 9.8, or 9.9. For example, the range is more preferably 2 to 8 MPa, and even more preferably 2.5 to 7 MPa. By being 10 MPa or less, the feeling of tension is reduced when used as gloves or sacks, and fatigue is less likely to be felt when worn for a long time, which is preferable. Moreover, by making the pressure at least 1 MPa, the shape of the molded product can be more easily maintained, which is preferable.

[0013] The tensile storage modulus is a value measured by dynamic thermomechanical analysis at 25°C and 1 Hz. The measurement can be performed using a dynamic thermomechanical analyzer (e.g., RSA-G2 dynamic viscoelasticity measuring device manufactured by TA Instruments). More specifically, the measurement can be performed by applying a time-oscillating strain or stress to a rectangular test piece (length 3 cm, width 0.5 cm) while changing the temperature, and measuring the resulting stress or strain. In the present disclosure, the measurement is performed under the following conditions. Measurement mode: Tensile mode Temperature range: -70℃~120℃ Heating rate: 5℃ / min ·Measurement frequency: 1Hz

[0014] The dip-formed article of the present disclosure preferably has a tensile storage modulus of 0.5 to 5 MPa at 40°C and 1 Hz. The upper or lower limit of the range may be, for example, 0.6, 0.7, 0.8, 0.9, 1.1, 1.2, 1.3, 1.4, 1.5, 1.6, 1.7, 1.8, 1.9, 2, 2.1, 2.2, 2.3, 2.4, 2.5, 2.6, 2.7, 2.8, 2.9, 3, 3.1, 3.2, 3.3, 3.4, 3.5, 3.6, 3.7, 3.8, 3.9, 4, 4.1, 4.2, 4.3, 4.4, 4.5, 4.6, 4.7, 4.8, or 4.9. For example, the range is preferably 0.8 to 4 MPa, and more preferably 1 to 4 MPa.

[0015] The tensile storage modulus at 25°C and 1Hz or 40°C and 1Hz can be appropriately adjusted depending on the structure and molecular weight of the chlorosulfonated polyolefin constituting the chlorosulfonated polyolefin latex used, and the type and amount of additives contained in the dip molding composition containing the chlorosulfonated polyolefin latex. For example, if the chlorosulfonated polyolefin used has a highly crystalline structure (e.g., a low chlorine content), the storage modulus tends to be high. In addition, the storage modulus tends to be high when the amount of insoluble solid additives among the additives contained in the dip molding composition increases, and the storage modulus tends to be low when the amount of liquid additives increases.

[0016] As described above, the dip-formed article of the present disclosure has a thickness of 0.3 mm or more, and preferably 0.3 to 1 mm. The upper or lower limit of the range may be, for example, 0.35, 0.4, 0.45, 0.5, 0.55, 0.6, 0.65, 0.7, 0.75, 0.8, 0.85, 0.9, or 0.95 mm. For example, the range is more preferably 0.35 to 0.8 mm.

[0017] Chlorosulfonated polyolefins can be obtained by chlorinating and chlorosulfonating polyolefins. Examples of polyolefins include polymers or copolymers of α-olefins and copolymers of α-olefins and other polymerizable components.

[0018] Examples of α-olefins include ethylene, propylene, 1-butene, 1-pentene, 1-hexene, 4-methyl-1-pentene, 1-octene, 1-decene, etc. Other polymerizable components include linear dienes such as isoprene, 1,3-butadiene, 1,4-hexadiene, 1,6-octadiene, and 2-methyl-1,5-hexadiene; cyclic dienes such as 1,4-cyclohexadiene, dicyclopentadiene, 5-vinyl-2-norbornene, 5-ethylidene-2-norbornene, 5-methylene-2-norbornene, 5-isopropylidene-2-norbornene, and 6-chloromethyl-5-isopropenyl-2-norbornene; and vinyl compounds such as vinyl acetate, vinyl chloride, acrylonitrile, styrene, methyl acrylate, and methyl methacrylate.

[0019] The chlorosulfonated polyolefin is preferably a chlorosulfonated α-olefin polymer. In the chlorosulfonated α-olefin polymer, one kind of α-olefin may be used alone or two or more kinds of α-olefins may be used. When two or more kinds of α-olefins are used, it is preferable that one kind is ethylene.

[0020] More specifically, examples of chlorosulfonated polyolefins include chlorosulfonated polyethylene, chlorosulfonated ethylene-α-olefin copolymers, and chlorosulfonated α-olefin polymers. The "α-olefin" in the chlorosulfonated ethylene-α-olefin copolymers and chlorosulfonated α-olefin polymers refers to α-olefins other than ethylene. As the α-olefin other than ethylene, for example, propylene is preferred. That is, as the chlorosulfonated ethylene-α-olefin copolymers, for example, chlorosulfonated ethylene propylene copolymers are preferred, and as the chlorosulfonated α-olefin polymers, for example, chlorosulfonated propylene polymers are preferred.

[0021] The chlorosulfonated polyolefins may be used alone or in combination of two or more kinds.

[0022] The sulfur content in the chlorosulfonated polyolefin is preferably 0.5% by mass or more, and more preferably 0.8% by mass or more, and is preferably 2.0% by mass or less, and more preferably 1.5% by mass or less, and is preferably 0.5 to 2.0% by mass, and more preferably 0.8 to 1.5% by mass.

[0023] The chlorine content in the chlorosulfonated polyolefin of the present disclosure is not particularly limited, but is preferably 10% by mass or more, more preferably 20% by mass or more. Also, it is preferably 50% by mass or less, more preferably 40% by mass or less. Also, it is preferably 10 to 50% by mass, more preferably 20 to 40% by mass. In addition, when preparing a chlorosulfonated polyolefin latex that satisfies the below-mentioned condition (i), it is more preferable that the chlorine content of the condition (i) is further satisfied.

[0024] The sulfur content and chlorine content of the chlorosulfonated polyolefin can be measured by the oxygen flask combustion method.

[0025] The method of chlorinating and chlorosulfonating polyolefins includes a solution method in which polyolefins are dissolved in an organic solvent to carry out a homogeneous system, a suspension method in which polyolefins are suspended in a solvent to carry out a reaction, a melting method in which polyolefins are melted to carry out a reaction, and a gas phase method in which polyolefins are suspended in a gas phase to carry out a reaction. Among these, the solution method is preferred from the viewpoint of carrying out uniform chlorination and chlorosulfonation. Examples of the chlorinating agent and chlorosulfonating agent that can be used include a combination of chlorine gas and sulfurous acid gas, a combination of chlorine gas and sulfuryl chloride, and sulfuryl chloride alone. The chlorosulfonation reaction can be carried out by using a chlorinating agent and a chlorosulfonating agent, a radical generator, and a cocatalyst such as pyridine if necessary.

[0026] The chlorosulfonated polyolefin may be a commercially available product, for example, "TOSO-CSM" or "extos" available from Tosoh Corporation.

[0027] The chlorosulfonated polyolefin latex comprises a chlorosulfonated polyolefin, an aqueous dispersion medium, and an emulsifier.

[0028] Examples of the method for producing the chlorosulfonated polyolefin latex include a method of melting the chlorosulfonated polyolefin and dispersing it in water containing an emulsifier, a method of dissolving the chlorosulfonated polyolefin in an organic solvent, dispersing it in water containing an emulsifier, and then removing the organic solvent, etc. From the viewpoint of easy control of the particle size of the chlorosulfonated polyolefin latex, the latter method is preferred.

[0029] Examples of the method of dispersing in water using an organic solvent include a phase inversion emulsification method in which water is added to chlorosulfonated polyolefin dissolved in an organic solvent to form a water-in-oil (W / O) emulsion, and then water is added to invert the phase to an oil-in-water (O / W) emulsion, and a forced emulsification method in which chlorosulfonated polyolefin dissolved in an organic solvent is mechanically dispersed in water in the presence of an emulsifier using an emulsifier. These methods may be used alone or in combination.

[0030] The organic solvent is not particularly limited as long as it can dissolve the chlorosulfonated polyolefin and is not miscible with water, and examples thereof include aliphatic hydrocarbon solvents such as hexane, heptane, cyclohexane, etc.; aromatic hydrocarbon solvents such as benzene, toluene, xylene, etc.; chlorine-based hydrocarbon solvents such as chloroform, 1,2-dichloroethane, etc.; alcohol solvents such as 1-butanol, isobutanol, etc.; ester solvents such as ethyl acetate, isopropyl acetate, n-butyl acetate, etc.; ketone solvents such as methyl ethyl ketone, methyl isobutyl ketone, etc.; ether solvents such as diisopropyl ether, dibutyl ether, anisole, etc. These organic solvents may be used alone or in combination of two or more kinds.

[0031] The amount of the organic solvent used is not particularly limited, but is preferably set so that the concentration of the chlorosulfonated polyolefin becomes 5 to 25% by mass, and more preferably 8 to 20% by mass.

[0032] When an emulsifier is used, the emulsifier is not particularly limited, but anionic emulsifiers and nonionic emulsifiers are preferred, and anionic emulsifiers are particularly preferred.

[0033] Examples of the anionic emulsifier include polyoxyalkylene alkyl ether sulfates, polyoxyalkylene alkyl phenyl ether sulfates, alkyl benzene sulfonates, alkyl naphthalene sulfonates, alkyl diphenyl sulfonates, α-olefin sulfonates, alkyl sulfates, naphthalene sulfonate formalin condensates, dialkyl sulfosuccinates, polyoxyethylene alkyl ether acetates, rosin salts, and fatty acid salts. Among these, polyoxyalkylene alkyl ether sulfates and polyoxyalkylene alkyl phenyl ether sulfates are preferred from the viewpoint of excellent stability of the latex, and examples thereof include sodium polyoxyethylene lauryl ether sulfate, sodium polyoxyethylene tridecyl ether sulfate, sodium polyoxyethylene myristyl ether sulfate, sodium polyoxypropylene lauryl ether sulfate, sodium polyoxypropylene tridecyl ether sulfate, sodium polyoxyethylene polyoxypropylene lauryl ether sulfate, and sodium polyoxyethylene polyoxypropylene tridecyl ether sulfate.

[0034] When a fatty acid salt is used as the emulsifier, the fatty acid may be dissolved in a solution in which the chlorosulfonated polyolefin is dissolved in the organic solvent, and the organic solvent solution may be mixed with an aqueous solution in which a neutralizing agent is dissolved, to perform dispersion. Examples of the fatty acid include palmitic acid, stearic acid, oleic acid, and vaccenic acid, and examples of the neutralizing agent include sodium hydroxide, potassium hydroxide, ammonia, alkanolamine, and alkylamine.

[0035] Examples of the nonionic emulsifiers include polyoxyalkylene alkyl esters, polyoxyalkylene alkyl ethers, polyoxylethylene derivatives, polyoxyalkylene alkylphenyl ethers, sorbitan alkyl esters, sorbitan fatty acid esters, polyoxyethylene sorbitan fatty acid esters, polyoxyethylene sorbitol fatty acid esters, propylene glycol esters, glycerin fatty acid esters, polyoxyethylene fatty acid esters, polyoxyethylene hydrogenated castor oil, polyoxyethylene alkylamines, and alkyl alkanolamides.

[0036] The emulsifier may be used alone or in combination of two or more kinds. The amount of the emulsifier to be added is not particularly limited, but is preferably 0.1 to 15 parts by mass, more preferably 0.5 to 12 parts by mass, and particularly preferably 1 to 10 parts by mass, based on 100 parts by mass of the chlorosulfonated polyolefin.

[0037] As the emulsifying device, a known device can be used, for example, a paddle mixer, a planetary mixer, a homomixer, a homogenizer, a disperser mixer, etc. The emulsifying device may be of a batch type or a continuous type.

[0038] The temperature during emulsification can be appropriately set depending on the type of organic solvent used, and is usually about 5 to 70°C.

[0039] In order to remove the organic solvent from the emulsion obtained by the above method, it may be removed by distillation under normal pressure, reduced pressure or increased pressure. At this time, the concentration of the latex may be adjusted by simultaneously removing water as necessary. In the organic solvent removal operation, a defoamer may be used to suppress foaming caused by the emulsifier. Examples of the defoamer include mineral oil defoamers, silicone defoamers, acetylene defoamers, metal soap defoamers, acrylic defoamers, and fluorine defoamers. Among them, acetylene defoamers are preferred. These may be used alone or in combination of two or more. The amount of the defoamer used is preferably 100 to 2000 ppmwt per 100 parts by mass of chlorosulfonated polyolefin, depending on the amount of the emulsifier used. The defoamer may be added to the emulsion before the removal operation, or may be added appropriately during the removal operation. The method of addition may be a method of adding all at once, a method of dropping, a method of spraying, or the like.

[0040] When water is to be further removed in order to adjust the concentration after the removal of the organic solvent, it can be removed by a procedure such as distillation, centrifugation, membrane separation, or filtration.

[0041] The particle size of the chlorosulfonated polyolefin contained in the latex composition is not particularly limited, but the volume-based median particle size measured by a laser diffraction particle size distribution analyzer is preferably 0.1 to 10 μm, more preferably 0.3 to 5 μm, and particularly preferably 0.5 to 2 μm. When the particle size is within this range, a latex with excellent stability is easily obtained. The particle size can be adjusted by the type and amount of the organic solvent and emulsifier, the amount of water used, and the operating conditions of the emulsification device.

[0042] The chlorosulfonated polyolefin latex may be a commercially available product, such as "Seporex CSM-N" manufactured by Sumitomo Seika Chemicals Co., Ltd.

[0043] As the latex used in the dip molding composition, the chlorosulfonated polyolefin latex may be further mixed with natural rubber latex, polybutadiene rubber latex, polyisoprene rubber latex, acrylonitrile-butadiene rubber latex, hydrogenated acrylonitrile-butadiene rubber latex, styrene-butadiene rubber latex, hydrogenated styrene-butadiene rubber latex, acrylic rubber latex, ethylene-propylene-diene rubber latex, chloroprene rubber latex, butyl rubber latex, chlorinated polyolefin rubber latex, fluororubber latex, epichlorohydrin rubber latex, silicone rubber latex, urethane rubber latex, or the like, within a range that does not impair the effects.

[0044] In order to enhance the stability of the chlorosulfonated polyolefin latex, additives such as dispersion stabilizers such as polyvinyl alcohol, polyvinylpyrrolidone, and hydroxyethyl cellulose, and stabilizers such as dibutyl hydroxytoluene, 2,5-di-tert-butyl hydroquinone, and bisphenol A type epoxy resin may be added. Such additives may be added to the chlorosulfonated polyolefin latex after preparation, or, depending on the type of additive, may be added to the organic solvent solution or water used for emulsification during the preparation of the chlorosulfonated polyolefin latex. In addition, it is preferable that the additives are usually added as an aqueous solution or aqueous dispersion of each of them or a mixture. When the additives are added, it is preferable that the total amount of the additives is 0.1 to 10 parts by mass per 100 parts by mass of the chlorosulfonated polyolefin.

[0045] When the chlorosulfonated polyolefin latex is used as a dip molding composition, it is preferable that the latex further contains an additive. Examples of the additive include known additives such as rheology adjusters, antioxidants, defoamers, pH adjusters, chelating agents, vulcanizing agents, vulcanization accelerators, vulcanization accelerator assistants, acid acceptors, film-forming assistants, plasticizers, fillers, pigments, and gelling agents. These can be used alone or in combination of two or more.

[0046] Examples of rheology adjusters include polysaccharides such as cellulose, cellulose nanofiber, cellulose nanocrystal, hydroxyethyl cellulose, hydroxypropyl cellulose, hydroxypropyl methyl cellulose, carboxymethyl cellulose, chitin, chitosan, guar gum, and xanthan gum; water-soluble vinyl polymers such as polyacrylic acid, sodium polyacrylate, crosslinked polyacrylic acid, polyacrylamide, polyvinyl alcohol, polyvinyl methyl ether, and polyvinylpyrrolidone; and clay minerals such as montmorillonite, nontronite, saponite, beidellite, and hectorite.

[0047] Examples of the antiaging agent include phenol-based antiaging agents such as dibutylhydroxytoluene, 2,2'-methylenebis(4-ethyl-6-tert-butylphenol), 2,5-di-tert-butylhydroquinone, etc., amine-based antiaging agents such as N-phenyl-1-naphthylamine, di(4-octylphenyl)amine, etc., phosphorus-based antiaging agents such as tris(nonylphenyl)phosphite, etc., sulfur-based antiaging agents such as dilauryl thiodipropionate, 2-mercaptobenzimidazole, nickel dibutyldithiocarbamate, etc., bisphenol A type epoxy resins, etc. These may be used alone or in combination of two or more.

[0048] Examples of the defoaming agent include oil-based defoaming agents, mineral oil-based defoaming agents, silicone-based defoaming agents, polyether-based defoaming agents, etc. These may be used alone or in combination of two or more.

[0049] Examples of pH adjusters include sodium hydroxide, potassium hydroxide, sodium carbonate, potassium carbonate, ammonia, trimethylamine, triethanolamine, hydrochloric acid, sulfuric acid, phosphoric acid, citric acid, acetic acid, etc. These may be used alone or in combination of two or more.

[0050] Examples of the chelating agent include ethylenediaminetetraacetic acid, nitrilotriacetic acid, trans-1,2-diaminocyclohexanetetraacetic acid, diethylenetriaminepentaacetic acid, bis(aminoethyl)glycol ether-N,N,N',N'-tetraacetic acid, N-(2-hydroxyethyl)ethylenediamine-N,N',N'-triacetic acid, dihydroxyethylglycine, 1-hydroxyethane-1,1-diphosphonic acid, gluconic acid, citric acid, malic acid, tartaric acid, etc. These may be used alone or in combination of two or more.

[0051] Examples of the vulcanizing agent include sulfur such as powdered sulfur, sulfur flowers, precipitated sulfur, and colloidal sulfur, organic peroxides such as di-tert-butyl peroxide and dicumyl peroxide, maleimide compounds such as N,N'-m-phenylene bismaleimide, quinoid compounds such as p-quinone dioxime and p,p'-dibenzoylquinone dioxime, metal compounds such as magnesium oxide and lead oxide, and polyhydric alcohol compounds such as pentaerythritol, dipentaerythritol, sorbitol, and trimethylolpropane. These can be used alone or in combination of two or more.

[0052] Examples of vulcanization accelerators include diethyldithiocarbamic acid, dibutyldithiocarbamic acid, diphenyldithiocarbamic acid, sodium diethyldithiocarbamate, sodium dibutyldithiocarbamate, sodium diphenyldithiocarbamate, zinc diethyldithiocarbamate, zinc dibutyldithiocarbamate, zinc diphenyldithiocarbamate, 2-mercaptobenzothiazole, zinc 2-mercaptobenzothiazole, di-2-benzothiazolyl disulfide, 2-(4'-morpholino dithio)benzothiazole, trimethylthiourea, N,N'-diethylthiourea, 1,3-diphenylguanidine, 1,3-di-o-tolylguanidine, N-cyclohexyl-2-benzothiazolylsulfenamide, N-oxydiethylene-2-benzothiazolylsulfenamide, tetramethylthiuram disulfide, tetraethylthiuram disulfide, tetramethylthiuram monosulfide, dipentamethylenethiuram tetrasulfide, zinc isopropylxanthate, etc. These may be used alone or in combination of two or more. Examples of the vulcanization accelerator include metal oxides such as zinc oxide and magnesium oxide, and fatty acids such as stearic acid and palmitic acid. These may be used alone or in combination of two or more.

[0053] Examples of the acid acceptor include metal oxides such as lead oxide, magnesium oxide, zinc oxide, and calcium oxide, metal hydroxides such as magnesium hydroxide, calcium hydroxide, and aluminum hydroxide, clay minerals such as hydrotalcite, and epoxy compounds such as phenyl glycidyl ether, epoxidized soybean oil, epoxidized castor oil, sorbitol polyglycidyl ether, epoxidized polybutadiene, and polyglycidyl methacrylate. These can be used alone or in combination of two or more.

[0054] Examples of the film-forming aid include propylene glycol, propylene glycol monomethyl ether, propylene glycol monoethyl ether, propylene glycol monopropyl ether, ethylene glycol monoethyl ether, ethylene glycol monopropyl ether, ethylene glycol monoisopropyl ether, ethylene glycol mono n-butyl ether, ethylene glycol monoiso-butyl ether, ethylene glycol monotert-butyl ether, ethylene glycol monophenyl ether, diethylene glycol monoethyl ether, diethylene glycol monopropyl ether, diethylene glycol monoisopropyl ether, diethylene glycol mono n-butyl ether, diethylene glycol monoiso-butyl ether, diethylene glycol monotert-butyl ether, diethylene glycol monophenyl ether, diethylene glycol dimethyl ether, diethylene glycol methyl ethyl ether, triethylene glycol monobutyl ether, triethylene glycol dimethyl ether, tetraethylene glycol dimethyl ether, dipropylene glycol mono n-butyl ether, dipropylene glycol dimethyl ether, tripropylene glycol monomethyl ether, and 2,2,4-trimethyl-1,3-pentanediol monoisobutyrate. These can be used alone or in combination of two or more.

[0055] Examples of plasticizers include animal and vegetable oil-based plasticizers such as castor oil, linseed oil, soybean oil, epoxidized linseed oil, epoxidized soybean oil, epoxidized fatty acid, hydrogenated castor oil, and polyoxyethylene hydrogenated castor oil; synthetic oil-based plasticizers such as poly-α-olefins (e.g., polybutadiene) and their hydrogenated products, isobutene oligomers and their hydrogenated products, and polyisobutylene and their hydrogenated products; mineral oil-based plasticizers such as paraffin-based process oil and naphthene-based process oil; liquid rubber-based plasticizers such as liquid isoprene rubber, liquid butadiene rubber, liquid styrene butadiene rubber, liquid ethylene-propylene-diene rubber, and liquid acrylic rubber; dibutyl phthalate, dioctyl phthalate, benzyl butyl phthalate, Examples of suitable plasticizers include ester-based plasticizers such as diisononyl phthalate, dibutyl adipate, diisobutyl adipate, dioctyl adipate, diisononyl adipate, dibutyl sebacate, dibutyl maleate, dioctyl maleate, dioctyl fumarate, tributyl citrate, tributyl acetyl citrate, tributyl phosphate, trioctyl phosphate, tricresyl phosphate, tributyl trimellitate, trioctyl trimellitate, benzyl benzoate, dodecyl benzoate, and polyester polyol; and ether-based plasticizers such as polyethylene glycol, polypropylene glycol, polyethylene glycol dimethacrylate, and polypropylene glycol dimethacrylate. Among these, from the viewpoint of suppressing bleed-out, reactive plasticizers having reactive groups (reactive groups capable of crosslinking chlorosulfonated polyolefins, specifically, for example, epoxy groups or olefin groups) are preferred, and epoxidized animal and vegetable oil-based plasticizers and liquid rubber-based plasticizers are particularly preferred. These can be used alone or in combination of two or more.

[0056] Examples of the filler include carbon fiber, cellulose fiber, carbon black, silica, talc, clay, calcium carbonate, titanium oxide, and barium sulfate.

[0057] Examples of pigments include carbon black, titanium oxide, chromium oxide, Prussian blue, amber, nickel titanium yellow, viridian, cobalt blue, phthalocyanine blue, phthalocyanine green, molybdenum orange, chrome yellow, anthraquinone, quinacridone, etc. These may be used alone or in combination of two or more. Examples of gelling agents include sodium alginate, pectin (LM pectin, HM pectin), gellan gum (LA gellan gum, HA gellan gum), gum arabic, κ-carrageenan, ι-carrageenan, tragacanth gum, glucomannan, tremel gum, fucoidan, heparin, hyaluronic acid, rhamsan gum, diutan gum, sodium polyacrylate, etc. These may be used alone or in combination of two or more.

[0058] The amount of additives contained in the dip molding composition of the present disclosure is not particularly limited, but is preferably 5 to 50 parts by mass, and more preferably 5 to 30 parts by mass, per 100 parts by mass of the solid content (i.e., chlorosulfonated polyolefin) in the latex composition.

[0059] It is preferable to add a plasticizer as an additive to the composition for dip-molded body of the present disclosure. The amount of the plasticizer added is preferably 5 to 20 parts by mass, particularly preferably 7 to 18 parts by mass, per 100 parts by mass of the solid content (i.e., mainly chlorosulfonated polyolefin) in the latex composition. In addition, when preparing a chlorosulfonated polyolefin latex that satisfies the below-mentioned condition (ii), it is more preferable to further satisfy the condition (ii).

[0060] The chlorosulfonated polyolefin latex (composition for preparing a dip-molded article) capable of preparing the dip-molded article of the present disclosure satisfies at least one of the following conditions (i) and (ii), and preferably satisfies both. By using a chlorosulfonated polyolefin latex that satisfies either of these conditions (preferably both), the dip-molded article of the present disclosure can be particularly preferably prepared. (i) The chlorine content in the chlorosulfonated polyolefin constituting the chlorosulfonated polyolefin latex is 30 to 40% by mass. (ii) The plasticizer is contained in an amount of 5 to 20 parts by mass per 100 parts by mass of the chlorosulfonated polyolefin.

[0061] In the condition (i), the upper or lower limit of the chlorine content (30 to 40% by mass) in the chlorosulfonated polyolefin may be, for example, 31, 32, 33, 34, 35, 36, 37, 38, or 39% by mass.

[0062] In the condition (ii), the upper or lower limit of the amount of plasticizer (5 to 20 parts by mass) relative to 100 parts by mass of chlorosulfonated polyolefin may be, for example, 6, 7, 8, 9, 10, 11, 12, 13, 14, 15, 16, 17, 18, or 19 parts by mass.

[0063] In addition, when the chlorosulfonated polyolefin latex satisfies the condition (ii), the dip-molded article of the present disclosure can be particularly preferably prepared even if the condition (i) is not satisfied. Therefore, although not particularly limited, when the condition (ii) is satisfied, the chlorine content in the chlorosulfonated polyolefin may be less than 30% by mass or more than 40% by mass. For example, it may be 10% by mass or more and less than 30% by mass, or it may be 10 to 29% by mass. The upper or lower limit of the range may be, for example, 11, 12, 13, 14, 15, 16, 17, 18, 19, 20, 21, 22, 23, 24, 25, 26, 27, or 28% by mass. For example, the range may be 15% by mass or more and less than 30% by mass, or it may be, for example, 15 to 28% by mass. For example, it may be more than 40% by mass and less than 60% by mass, or it may be 41 to 60% by mass. The upper or lower limit of the range may be, for example, 42, 43, 44, 45, 46, 47, 48, 49, 50, 51, 52, 53, 54, 55, 56, 57, 58, or 59% by mass. For example, the range may be greater than 40% by mass and equal to or less than 55% by mass, or may be, for example, 41 to 55% by mass.

[0064] In addition, a dip-molded article prepared from a chlorosulfonated polyolefin latex (composition for preparing a dip-molded article) satisfying both of the conditions (i) and (ii) has particularly excellent flexibility, and even when worn for a long period of time, it causes little fatigue and has excellent protective properties.

[0065] In addition, when the latex of the present disclosure is used as a dip molding composition, other rubber latex may be contained within a range that does not impair the effect. Examples of such other latex include natural rubber latex, isoprene rubber latex, butadiene rubber latex, chloroprene rubber latex, butyl rubber latex, styrene-butadiene rubber latex, acrylic rubber latex, acrylonitrile-butadiene rubber latex, silicone rubber latex, fluororubber latex, epichlorohydrin rubber latex, and olefin rubber latex. In the case where these various rubber latexes are used in combination with the latex of the present disclosure as a dip molding composition, the content of the other rubber is preferably less than the content of the chlorosulfonated polyolefin, and is preferably, for example, 50 parts by mass or less, 40 parts by mass or less, 30 parts by mass or less, 20 parts by mass or less, 10 parts by mass or less, or 5 parts by mass or less relative to 100 parts by mass of the chlorosulfonated polyolefin.

[0066] The method for preparing the chlorosulfonated polyolefin latex preferred as the composition for preparing a dip-molded body is not particularly limited, and examples thereof include a method of mixing various additives with the chlorosulfonated polyolefin latex using a dispersing machine such as a ball mill, a bead mill, a kneader, or a disperser, a method of preparing an aqueous dispersion of desired additives in advance using a dispersing machine, and then mixing the aqueous dispersion with the chlorosulfonated polyolefin latex, and a method of mixing some additives with the chlorosulfonated polyolefin latex, and then mixing it with an aqueous dispersion of other additives.

[0067] The pH of the chlorosulfonated polyolefin latex cannot be generally determined because it varies depending on the type and amount of the emulsifier and additives used, but from the viewpoint of facilitating coagulation, the pH is preferably 5 or higher, and more preferably in the range of pH 7 to 12.

[0068] The chlorosulfonated polyolefin concentration of the chlorosulfonated polyolefin latex is preferably 20 to 60% by mass. The upper or lower limit of the range may be, for example, 21, 22, 23, 24, 25, 26, 27, 28, 29, 30, 31, 32, 33, 34, 35, 36, 37, 38, 39, 40, 41, 42, 43, 44, 45, 46, 47, 48, 49, 50, 51, 52, 53, 54, 55, 56, 57, 58, or 59% by mass. For example, the range is more preferably 25 to 50% by mass.

[0069] The chlorosulfonated polyolefin latex may be aged (also called pre-vulcanization) before being subjected to dip molding. The aging time cannot be generally determined because it depends on the type of additives and the aging temperature, but is preferably 1 to 7 days, more preferably 1 to 3 days. The aging temperature is preferably 10 to 50°C, more preferably 20 to 40°C.

[0070] After aging, it is preferable to store the product at a temperature of 30° C. or lower until it is used for dip molding. If the product is stored at a temperature higher than 30° C., aging will proceed further, and the mechanical strength of the resulting dip-molded product may decrease.

[0071] The dip-molded article can be obtained by dip-molding the above chlorosulfonated polyolefin latex (composition for preparing a dip-molded article).

[0072] The mold used for dip molding may be a mold that corresponds to the desired three-dimensional shape and is integrally formed from ceramic, metal, glass, plastic, etc. The surface of the mold may be finished to a matte finish or may be provided with other materials such as fibers or other types of rubber coatings depending on the purpose of the dip-molded product. In addition, the mold may be preheated before being immersed in the dip-molding composition.

[0073] It is preferable to use a coagulant to aggregate the rubber component before immersing the mold in the dip molding composition or after pulling the mold out of the dip molding composition. Methods for using the coagulant include a method of immersing the mold before immersing in the dip molding composition in a solution of the coagulant (hereinafter also referred to as a coagulation liquid) to attach the coagulant to the mold, and a method of immersing the mold on which the dip molding composition has been deposited in the coagulation liquid. From the viewpoint of obtaining a dip molded body with little thickness unevenness, a method of immersing the mold before immersing in the dip molding composition in a solution of the coagulant to attach the coagulant to the mold is preferable.

[0074] Examples of the coagulant include metal halides such as sodium chloride, potassium chloride, barium chloride, calcium chloride, magnesium chloride, zinc chloride, and aluminum chloride; metal nitrates such as sodium nitrate, potassium nitrate, barium nitrate, calcium nitrate, zinc nitrate, and aluminum nitrate; metal acetates such as sodium acetate, potassium acetate, barium acetate, calcium acetate, zinc acetate, and aluminum acetate; and water-soluble metal salts such as metal sulfates such as sodium sulfate, potassium sulfate, calcium sulfate, magnesium sulfate, and aluminum sulfate. Among these, from the viewpoint of high coagulation power, polyvalent metal salts that generate polyvalent metal ions are preferred, and water-soluble polyvalent metal salts are more preferred. As the polyvalent metal here, alkaline earth metals are preferred, calcium, barium, and magnesium are more preferred, and calcium is particularly preferred. In addition, as the coagulant, calcium chloride and calcium nitrate are particularly preferred from the viewpoint of high solubility in water. These coagulants may be used alone or in combination of two or more.

[0075] The coagulant is preferably used in the form of an aqueous solution. This aqueous solution may further contain a water-soluble organic solvent such as methyl alcohol or ethyl alcohol, or a nonionic surfactant. The concentration of the coagulant is not particularly limited, but is preferably 5 to 50 mass%, more preferably 10 to 40 mass%, and particularly preferably 15 to 35 mass%. The immersion time of the mold in the coagulant is not particularly limited, but is usually preferably 5 to 300 seconds, and more preferably 10 to 100 seconds.

[0076] After the casting mold is immersed in the coagulating liquid to adhere to the surface, the solvent of the coagulating liquid may be removed by drying. The drying temperature can be appropriately set depending on the type of solvent and salt used, and is preferably 60 to 150°C, and more preferably 80 to 120°C. The drying time is not particularly limited, but is preferably 1 to 600 seconds, and more preferably 5 to 300 seconds. By drying the coagulating liquid on the surface of the casting mold, it becomes easier to create a state in which the salt is uniformly adhered to the surface of the casting mold.

[0077] The time for immersing the mold in the chlorosulfonated polyolefin latex (dip molding composition) may be appropriately set so as to obtain a thickness of 0.3 mm or more, and is preferably 5 to 600 seconds, and more preferably 10 to 300 seconds.

[0078] After the mold is removed from the dip molding composition, the rubber film formed on the mold surface is usually dried by heating. The drying method is not particularly limited, and drying can be performed using a hot air heater, an infrared heater, a microwave heater, a high-frequency heater, or the like. The drying temperature is not particularly limited, but is preferably 50 to 160°C, more preferably 60 to 140°C, and particularly preferably 70 to 120°C. The drying time is not particularly limited, but is preferably 1 to 120 minutes, more preferably 10 to 100 minutes, and particularly preferably 20 to 60 minutes.

[0079] If necessary, the rubber film formed on the mold surface may be vulcanized by further heating. The heating conditions during vulcanization are not particularly limited, but are preferably 60 to 200°C, more preferably 80 to 180°C, and particularly preferably 100 to 160°C. By setting the heating temperature within this range, it is possible to achieve an appropriate vulcanization speed and to suppress deterioration of the rubber component due to excessive heating. The heating time for vulcanization may be appropriately selected depending on the heating temperature, and is usually 5 to 120 minutes. The heating method may be, for example, the same method as the heating method described above.

[0080] In addition, before or after heating the mold onto which the dip molding composition has been deposited, it is preferable to wash the mold with water or hot water in order to remove water-soluble impurities (e.g., excess emulsifier, surfactant, coagulant, uncoagulated latex, etc.). The temperature of the water or hot water used is preferably 20 to 80°C, more preferably 30 to 70°C. The washing time is preferably about 0.5 to 60 minutes.

[0081] The dip-molded article after drying (and further vulcanization as required) is detached from the mold. Methods of detachment include peeling from the mold by hand, peeling from the mold using a peeling roller, and peeling by water pressure or compressed air pressure. The dip-molded article may be further washed with water after being detached from the mold. Furthermore, if necessary, in order to prevent adhesion at the contact surfaces between the dip-molded articles and to improve the slipperiness during attachment and detachment, inorganic fine particles such as talc or calcium carbonate or organic fine particles such as cornstarch may be applied to the surface, an elastomer layer containing fine particles may be further formed on the surface, or the surface layer may be chlorinated.

[0082] The dip-formed article of the present disclosure has excellent flexibility and is less likely to cause fatigue even when worn for a long period of time, and is therefore particularly suitable for use as an article to be applied to the hands and fingers (for example, gloves and sacks).

[0083] In addition, in this specification, the term "comprising" includes "consisting essentially of" and "consisting of." In addition, the present disclosure includes any combination of the constituent elements described in this specification.

[0084] In addition, the various characteristics (properties, structures, functions, etc.) described in each embodiment of the present disclosure above may be combined in any way to specify the subject matter included in the present disclosure. In other words, the present disclosure includes all subject matter consisting of all combinations of each combinable characteristic described in this specification. EXAMPLES

[0085] The present disclosure will be specifically described below with reference to examples and comparative examples, but the present disclosure is not limited to these examples or the like.

[0086] <Evaluation method> Each of the Production Examples, Examples and Comparative Examples was evaluated by the following methods. (Solids concentration of latex) 2 g of the latex was sampled and dried at 120° C. for 1 hour to remove moisture, and then the mass of the residue was measured to measure the amount of solids (chlorosulfonated polyolefin). (Latex median particle size) The volumetric median particle diameter of the latex was measured using a laser diffraction particle size distribution analyzer (Shimadzu Corporation, product name "SALD-2000J") The particle diameter here is a value calculated by assuming that the particle to be measured that shows the same diffraction and scattering light pattern as a sphere with a diameter of 1 μm is 1 μm regardless of its shape. (Thickness of dip-molded body) The dip-molded product was cut 1 cm from the tip of the bag-shaped (sack-shaped) end to form a cylinder. This cylindrical dip-molded product was cut open in the longitudinal direction to form a rectangle (approximately 6 cm x approximately 4.7 cm). The resulting rectangle was roughly divided into thirds in the longitudinal direction, and the thickness was measured at each of the three points at the top, middle, and bottom, and the overall average was taken to be the thickness of the molded product. (Tensile storage modulus of dip-molded body) A rectangular test piece measuring 3 cm in length and 0.5 cm in width was cut out from the obtained dip-molded body, and the tensile storage modulus at 25°C and 40°C was measured using a TA Instruments dynamic viscoelasticity measuring device RSA-G2 in tensile mode at a measurement temperature of -70°C to 120°C, a heating rate of 5°C / min, and a measurement frequency of 1 Hz. (Evaluation of fit) The obtained dip-molded sack-shaped product was worn on the finger, and the stickiness when worn and the feeling of tension when bending and straightening the finger were evaluated. In addition, the finger was bent and straightened 100 times in succession, and the presence or absence of fatigue was evaluated every 10 times. The evaluation was performed by four people, who were given points according to the following criteria, and the average value was used as the evaluation result for each item.

[0087] [Table 1]

[0088] The higher the respective values, the more flexible the material is and the less likely it is to cause fatigue.

[0089] <Production Example 1> A 500 mL separable flask was charged with 45 g of chlorosulfonated polyethylene with a chlorine content of 30% by mass, 255 g of toluene, and 0.45 g of oleic acid, and the mixture was stirred at 85° C. for 4 hours to dissolve uniformly, preparing a rubber solution. Separately, 7.5 g of sodium polyoxyalkylene alkyl ether sulfate (NOF Corporation's product name "Trax ET-314") and 0.188 g of potassium hydroxide were dissolved in 170 g of ion-exchanged water to prepare an aqueous emulsifier solution. The entire amount of the emulsifier aqueous solution was added to the rubber solution, and the mixture was stirred and mixed for 10 minutes using a homomixer (TK Robomix, product name, Primix Corporation) to obtain an emulsion. The rotation speed and temperature during stirring and mixing were set to 12,000 rpm and 40°C, respectively. The obtained emulsion was heated to 40-70°C under reduced pressure of 40-90 kPa to distill off the toluene, and then concentrated to a solid content (chlorosulfonated polyethylene) concentration of 40% using an ultrafilter (ultrafiltration membrane: flat membrane type, molecular weight cutoff 200,000, material polysulfone), to obtain a chlorosulfonated polyethylene latex (median particle size 1.4 μm).

[0090] <Production Example 2> A chlorosulfonated polyethylene latex (median particle size: 1.6 μm) was obtained by the same procedure as in Production Example 1, except that the chlorosulfonated polyethylene was changed to a chlorosulfonated polyethylene having a chlorine content of 35% by mass.

[0091] <Production Example 3> A chlorosulfonated polyethylene latex (median particle size: 1.7 μm) was obtained by the same procedure as in Production Example 1, except that the chlorosulfonated polyethylene was changed to a chlorosulfonated polyethylene having a chlorine content of 40% by mass.

[0092] <Production Example 4> A chlorosulfonated polyethylene latex (median particle size: 0.9 μm) was obtained by the same procedure as in Production Example 1, except that the chlorosulfonated polyethylene was changed to a chlorosulfonated polyethylene having a chlorine content of 23% by mass.

[0093] <Production Example 5> A chlorosulfonated polyethylene latex (median particle size: 2.1 μm) was obtained by the same procedure as in Production Example 1, except that the chlorosulfonated polyethylene was changed to a chlorosulfonated polyethylene having a chlorine content of 43% by mass.

[0094] <Example 1> (Preparation of Dip Molding Composition) To the chlorosulfonated polyethylene latex obtained in Production Example 1, 15 parts by mass of epoxidized polybutadiene (manufactured by Nippon Soda Co., Ltd., product name "NISSO-PB JP100") was added as an acid acceptor, and the mixture was mixed for 1 hour at 12,000 rpm using a homomixer (TK Robomix, manufactured by Primix Corporation). 3 parts by mass of pentaerythritol (manufactured by Fujifilm Wako Pure Chemical Industries Co., Ltd., reagent) and 2 parts by mass of dipentamethylene thiuram tetrasulfide (manufactured by Ouchi Shinko Chemical Industry Co., Ltd., product name "Noccela TRA") were added, and the mixture was mixed for 1 hour at 12,000 rpm using a homomixer. 0.5 parts by mass of citrus-derived LM pectin (citrus-derived LM pectin (manufactured by Fujifilm Wako Pure Chemical Industries Co., Ltd., reagent, esterification degree 35) was added, and the mixture was stirred until completely dissolved to obtain a latex composition.

[0095] The parts by mass of each component used are values ​​relative to 100 parts by mass of chlorosulfonated polyethylene contained in the chlorosulfonated polyethylene latex.

[0096] (Production of dip-molded body) The ceramic mold was immersed in a 35% by mass aqueous solution of calcium nitrate for 5 seconds, and then dried for 300 seconds in a 160°C air dryer. The mold was then cooled to 74°C and immersed in the dip molding composition maintained at 25°C for 30 seconds, and then pulled out of the dip molding composition. The ceramic mold was dried for 20 minutes in a 100°C air dryer, and then immersed in 40°C hot water for 5 minutes to remove water-soluble impurities. After being pulled out of the hot water, the ceramic mold was dried for 10 minutes in a 100°C air dryer, and then further heated at 160°C for 20 minutes to perform vulcanization. After cooling to room temperature, the coating was peeled off from the ceramic mold to obtain a dip molded body. The ceramic mold used was a cylindrical ceramic mold of 10cm x 1.5cm (length x diameter), and a sack-shaped molded body was finally obtained. The thickness of the obtained dip molded body was 0.53mm.

[0097] <Example 2> A dip-molded article was obtained by carrying out the same operation as in Example 1, except that the chlorosulfonated polyethylene latex obtained in Production Example 2 was used.

[0098] <Example 3> The same procedure as in Example 1 was carried out except that the chlorosulfonated polyethylene latex obtained in Production Example 3 was used, to obtain a dip-molded article.

[0099] <Comparative Example 1> A dip-molded article was obtained in the same manner as in Example 1, except that the chlorosulfonated polyethylene latex obtained in Production Example 4 was used.

[0100] <Comparative Example 2> The same procedure as in Example 1 was carried out except that the chlorosulfonated polyethylene latex obtained in Production Example 5 was used, to obtain a dip-molded article.

[0101] [Table 2]

[0102] As shown in Table 2, when the chlorine content in the chlorosulfonated polyolefin was within the appropriate range, the tensile modulus at 25°C was low, and a dip-molded article was obtained that was free of tension and less prone to fatigue.

[0103] <Example 4> To the chlorosulfonated polyethylene latex obtained in Production Example 4, 0.5 parts by mass of citrus-derived LM pectin (citrus-derived LM pectin (reagent manufactured by Fujifilm Wako Pure Chemical Industries, esterification degree 35) was added and stirred until completely dissolved, and then 10 parts by mass of linseed oil (reagent manufactured by Kanto Chemical), 3 parts by mass, calculated as solid content, of an aqueous solution of sodium dibutyldithiocarbamate (manufactured by Ouchi Shinko Chemical Industry Co., Ltd., product name "Noccela TP"), and 10 parts by mass of tripropylene glycol monomethyl ether (manufactured by Nippon Nyukazai Co., Ltd., product name "Methylpropylene Triglycol") were added and further stirred to obtain a dip molding composition.

[0104] The parts by mass of each component used are values ​​relative to 100 parts by mass of chlorosulfonated polyethylene contained in the chlorosulfonated polyethylene latex.

[0105] (Production of dip-molded body) The ceramic mold was immersed in a 35% by mass aqueous solution of calcium nitrate for 5 seconds, and then dried in a 160°C air dryer for 300 seconds. The mold was then cooled to 74°C and immersed in the dip molding composition maintained at 25°C for 30 seconds, and then pulled out of the dip molding composition. The ceramic mold was dried in a 100°C air dryer for 20 minutes, and then heated at 160°C for 20 minutes to perform vulcanization. After cooling to room temperature, the coating was peeled off from the ceramic mold to obtain a dip molded body. The ceramic mold used was a cylindrical ceramic mold of 10cm x 1.5cm (length x diameter), and a sack-shaped molded body was finally obtained.

[0106] <Examples 5 to 12 and Comparative Examples 3 to 6> The same operation as in Example 4 was carried out with the formulation changed as shown in Table 3, except for 10 parts by mass of linseed oil, to obtain a dip-molded product. Note that phr in Table 3 indicates the part by mass value of each plasticizer used relative to 100 parts by mass of chlorosulfonated polyethylene contained in the chlorosulfonated polyethylene latex.

[0107] <Example 13> A dip-molded body was obtained by the same procedure as in Example 4, except that the chlorosulfonated polyethylene latex obtained in Production Example 2 was used and 10 parts by mass of epoxidized soybean oil was used instead of 10 parts by mass of linseed oil.

[0108] [Table 3]

[0109] As shown in Table 3, even if a latex that is poorly rated when no plasticizer is added is used, by adding an appropriate amount of plasticizer, it becomes flexible and it is possible to obtain a dip-molded product that is less prone to tension or fatigue. In addition, by satisfying both conditions (i) and (ii), it is possible to obtain a dip-molded product with even better flexibility.

Claims

1. A dip-molded article produced by dip-molding a chlorosulfonated polyolefin latex, The thickness is 0.3 mm or more, The tensile storage modulus at 25° C. and 1 Hz is 1 to 10 MPa. Dip-molded body.

2. 2. The dip-molded article according to claim 1, wherein the chlorine content in the chlorosulfonated polyolefin constituting the chlorosulfonated polyolefin latex is 30 to 40% by mass.

3. The dip-molded article according to claim 1, wherein the chlorosulfonated polyolefin latex contains 5 to 20 parts by mass of a plasticizer per 100 parts by mass of the chlorosulfonated polyolefin.

4. The dip-molded article according to claim 3 , wherein the plasticizer is a reactive plasticizer having an epoxy group or an olefin group.

5. 5. The dip-molded article according to claim 1, wherein the chlorosulfonated polyolefin is a chlorosulfonated polyethylene.

6. The dip-molded body according to any one of claims 1 to 4, having a tensile storage modulus of 0.5 to 5 MPa at 40°C and 1 Hz.

7. The dip-molded article according to any one of claims 1 to 4, wherein the molded article is a glove.

8. The dip-molded article according to any one of claims 1 to 4, which is a sack.

Citation Information

Patent Citations

  • Composition and method for manufacturing chlorosulfonated polyethylene latex and articles

    US8216652B1

  • JP1973039676A

  • Chemical-resistant glove

    JP1993230702A

  • Method for producing rubber glove, and rubber glove

    JP2011032590A

  • Method for manufacturing film-molded body

    JP7033242B1