Modified cyclic olefin resin, aqueous composition and cured coating

A modified cyclic olefin resin with an amino group in the side chain addresses the heat resistance and emulsifier limitations of conventional polyolefin resins, enabling effective electrodeposition coatings and packaging solutions.

JP2024143313AInactive Publication Date: 2024-10-11TOYOBO MC CORP
View PDF 1 Cites 0 Cited by

Patent Information

Application Number
JP2023055925
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Filing Date
2023-03-30
Publication Date
2024-10-11
Estimated Expiration
Not applicable · inactive patent

AI Technical Summary

Technical Problem

Conventional polyolefin resins are not suitable for applications requiring heat resistance, and existing electrodeposition coatings using emulsifiers face limitations.

Method used

A modified cyclic olefin resin with an amino group in the side chain, having specific amine and acid values, is developed for use in electrodeposition coatings without emulsifiers, offering excellent heat resistance and cationic electrodeposition properties.

Benefits of technology

The modified cyclic olefin resin provides superior heat resistance and is suitable for electrodeposition coatings, functional films, and packaging applications, including food, cosmetic, and medical packaging, without the need for emulsifiers.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024143313000001
    Figure 2024143313000001
  • Figure 2024143313000002
    Figure 2024143313000002
Patent Text Reader

Abstract

To provide a resin material that does not use emulsifiers, exhibits superior heat resistance, and is suitable for electrodeposition.SOLUTION: A modified cyclic olefin resin has functional groups located on side chains of the cyclic olefin resin, where the functional groups include an amino group.SELECTED DRAWING: None
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a modified cyclic olefin resin, and more particularly to a modified cyclic olefin resin, and an aqueous composition and a cured coating film using the same. [Background technology]

[0002] In recent years, with the trend towards smaller, thinner, and more functional electronic devices, there is a demand for highly functional materials with excellent insulation properties, heat resistance, chemical resistance, hydrolysis resistance, flame retardancy, dimensional stability, etc. In particular, for materials in the electrical and electronics field, there is a demand for materials with high heat resistance as well as insulation properties to ensure the safety and reliability of products.

[0003] In the electrical and electronic fields, metal products as electrical conductors usually require a coating of an insulating film. Electrodeposition coating is a useful method for forming an insulating film on the surface of a metal product. Electrodeposition coating is a method for forming a coating film of paint or resin on the surface of a coated object such as a metal product by passing an electric current through the electrodeposition paint. Since it can be applied uniformly even on objects with complex shapes, it is widely used in the electrical and electronic equipment field.

[0004] There are two types of electrodeposition coating: cationic electrodeposition coating and anionic electrodeposition coating. Cationic electrodeposition coating is a coating method in which an object to be coated, which is a cathode, is immersed in a cationic electrodeposition coating composition, and a voltage is applied to cause a positively charged resin to adhere to the object to be coated. On the other hand, anionic electrodeposition coating is a coating method in which an object to be coated, which is an anode, is immersed in an anionic electrodeposition coating composition, and a voltage is applied to cause a negatively charged resin to adhere to the object to be coated.

[0005] For electrodeposition coating, a water-based resin is used, and examples of commonly used resins include epoxy resins, acrylic resins, polyimide resins, polyamideimide resins, polyamide resins, polyolefins, and the like.

[0006] Patent Document 1 discloses an aqueous dispersion comprising a polyolefin resin, a neutralizing compound, and an emulsifier. [Prior art documents] [Patent documents]

[0007] [Patent Document 1] JP 2005-36076 A Summary of the Invention [Problem to be solved by the invention]

[0008] In recent years, the application of electrodeposition coating has expanded to include motor coils, metal substrate insulation films, etc., in addition to insulation films for electric and electronic components, but conventional polyolefin resins have been difficult to apply to fields that require heat resistance. In addition, Patent Document 1 uses an emulsifier.

[0009] The present invention has been made in view of the problems of the conventional technology. That is, an object of the present invention is to provide a resin material which does not use an emulsifier, has excellent heat resistance, and is suitable for electrodeposition coating. [Means for solving the problem]

[0010] As a result of extensive investigations, the present inventors have found that a modified cyclic olefin resin having an amino group in a side chain can solve the above problems, and have arrived at the present invention. That is, the present invention has the following configuration.

[0011] [1] A modified cyclic olefin resin having a functional group on a side chain of the cyclic olefin resin, the functional group including an amino group. [2] The modified cyclic olefin resin according to [1], having an amine value of 1,000 equivalents / ton or more and less than 10,000 equivalents / ton. [3] The modified cyclic olefin resin according to [1] or [2], wherein the functional group further has a carboxy group. [4] The modified cyclic olefin resin according to [3], having an acid value of 1,000 equivalents / ton or more and less than 10,000 equivalents / ton. [5] An aqueous composition comprising the modified cyclic olefin resin according to [1] and an aqueous medium. [6] The aqueous composition according to [4] or [5], further comprising a hardener. [7] The aqueous composition according to [4] or [5], which is for use in electrocoating. [8] A cured coating film obtained by curing the modified cyclic olefin resin of [1] or [2]. Effect of the Invention

[0012] The modified cyclic olefin resin of the present invention has excellent heat resistance and is suitable for cationic electrodeposition coating. Furthermore, it can be suitably used for coating materials for electrodeposition coating, water-based compositions, and laminates using the same without using an emulsifier. Furthermore, since the modified cyclic olefin resin of the present invention has excellent heat resistance, it can be used as an adhesive / coating agent for functional films in which a functional coating agent is applied to a film, as a food packaging material, a cosmetic packaging material, a medical packaging material, and a polarizing plate material. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0013] An embodiment of the present invention will be described in detail below. However, the present invention is not limited to this embodiment, and various modifications can be made within the scope of the above description.

[0014] <Modified cyclic olefin resin> The modified cyclic olefin resin of the present invention is a modified cyclic olefin resin having a functional group on a side chain of the cyclic olefin resin, and the functional group contains an amino group.

[0015] The cyclic olefin resin constituting the modified cyclic olefin resin of the present invention may be either a homopolymer (COP) made from only one type of cyclic olefin monomer, or a copolymer (COC) composed of one or more types of cyclic olefin monomer and comonomer.

[0016] Examples of the cyclic olefin monomer include bicyclic monomers such as norbornene and norbornadiene, tricyclic monomers such as dicyclopentadiene and dihydroxypentadiene, tetracyclic monomers such as tetracyclododecene, pentacyclic monomers such as cyclopentadiene trimer, and alkyl (methyl, ethyl, propyl, butyl, etc.) substituted monomers of these polycyclic monomers, alkenyl (vinyl, etc.) substituted monomers, alkylidene (ethylidene, etc.) substituted monomers, aryl (phenyl, tolyl, naphthyl, etc.) substituted monomers, etc. Among these, norbornene-based monomers selected from the group consisting of norbornene, tetracyclododecene, and alkyl substituted monomers thereof are particularly preferred.

[0017] The comonomer may be any monomer that is copolymerizable with the cyclic olefin monomer, and is preferably an alkene monomer. Examples of the alkene monomer include α-olefins such as ethylene, propylene, 1-butene, and 1-hexene, and isobutene. The alkene monomer may be linear or branched.

[0018] The monomer components constituting the cyclic olefin resin are preferably 50% by mass or more of the cyclic olefin monomer, more preferably 60% by mass or more of the cyclic olefin monomer. When the cyclic olefin monomer is 50% by mass or more of the total monomer components, the heat resistance is good. There are no particular limitations on the polymerization method and polymerization conditions when polymerizing the monomer components, and they may be appropriately set according to conventional methods.

[0019] The modified cyclic olefin resin of the present invention has a functional group in the side chain, and contains an amino group as the functional group. By having an amino group, it is possible to impart good cationic electrodeposition property to the cyclic olefin resin. The amino group is not particularly limited, but from the viewpoint of cationic electrodeposition property, a secondary amino group and a tertiary amino group are preferred, and a tertiary amino group is more preferred. The amino group may be an amino group present in a ring structure such as an alicyclic structure such as a piperidine ring, or an aromatic ring structure such as a pyridine ring.

[0020] The modified cyclic olefin resin of the present invention preferably has an amine value of 1,000 equivalents / ton or more, more preferably 3,000 equivalents / ton or more, and even more preferably 5,000 equivalents / ton or more. Also, it is preferably 10,000 equivalents / ton or less, more preferably 9,500 equivalents / ton or less, and even more preferably 9,000 equivalents / ton or less. If the amine value is within the above range, it is preferable because the cationic electrodeposition property is good.

[0021] The modified cyclic olefin resin of the present invention may further have a carboxy group as a functional group in the side chain. By having a carboxy group, it is possible to improve dispersibility or solubility in an aqueous medium and to impart reactivity with a curing agent. Here, the carboxy group may be an acid anhydride group.

[0022] When the modified cyclic olefin resin has a carboxy group, the acid value of the modified cyclic olefin resin is preferably 1,000 equivalents / ton or more, more preferably 3,000 equivalents / ton or more, and even more preferably 5,000 equivalents / ton or more. Also, it is preferably 10,000 equivalents / ton or less, more preferably 9,500 equivalents / ton or less, and even more preferably 9,000 equivalents / ton or less. When the acid value is the lower limit or more, it can improve dispersibility or solubility in an aqueous medium, or impart reactivity with a curing agent.

[0023] The lower limit of the weight average molecular weight (hereinafter abbreviated as "Mw") of the modified cyclic olefin resin is preferably 10,000 or more, more preferably 15,000 or more. The upper limit of Mw is preferably 1,000,000 or less, and even more preferably 500,000 or less. If the Mw of the modified cyclic olefin resin is equal to or more than the lower limit, the heat resistance is improved, which is preferable. If the Mw is equal to or less than the upper limit, the solubility in the solvent is good, which is preferable. The Mw of the modified cyclic olefin resin is determined by measurement using gel permeation chromatography (GPC).

[0024] The glass transition temperature of the modified cyclic olefin resin of the present invention is preferably 100° C. or higher, more preferably 120° C. or higher, and even more preferably 150° C. or higher. There is no particular upper limit, but it is, for example, 250° C. or lower. When the glass transition temperature is within the above range, the heat resistance is excellent.

[0025] <Method of producing modified cyclic olefin resin> The polymer according to the present invention can be obtained by polymerizing 5-norbornene-2,3-carboxylic anhydride, or can be produced by reacting a polymer obtained by polymerization of 5-norbornene-2,3-carboxylic anhydride with an alcohol having an amino group and a primary or secondary alcohol.

[0026] The polymer of 5-norbornene-2,3-dicarboxylic anhydride according to the present invention can be synthesized by subjecting a 5-norbornene-2,3-dicarboxylic anhydride monomer to ring-opening metathesis polymerization in a suitable solvent in the presence of a metal catalyst.

[0027] Solvents that can be used in the polymerization reaction of 5-norbornene-2,3-dicarboxylic anhydride are not particularly limited, and examples thereof include aromatic hydrocarbons, toluene, ethylbenzene, xylene, propylbenzene, isopropylbenzene, t-butylbenzene, mesitylene, and the like; capped glycol ethers such as propylene glycol monomethyl ether acetate, ethylene glycol monobutyl ether acetate, diethylene glycol monoethyl ether acetate, and the like; N-methyl-2-pyrrolidone, N,N-dimethylformamide, N,N-dimethylacetamide, dimethylsulfoxide, and the like; and mixtures thereof; and dimethylacetamide is preferably used.

[0028] When the polymerization is carried out in a solvent, the total concentration of the monomer and polymer is preferably 1 to 55% by weight, more preferably 2 to 50% by weight, and particularly preferably 5 to 45% by weight. If the total concentration of the monomer and polymer is 1% by weight or less, the productivity is poor, and if it is 55% by weight or more, the solution viscosity after polymerization is too high, which may make the subsequent handling difficult.

[0029] The polymerization temperature is not particularly limited, but is generally −30 to 200° C., and preferably 0 to 180° C. The polymerization time is not particularly limited, and is from 1 minute to 100 hours.

[0030] The catalyst used in the ring-opening metathesis polymerization includes a metal carbene organic complex, the metal being, but not necessarily, a transition metal such as ruthenium, molybdenum, osmium or tungsten. The catalyst used can be sufficiently reacted at 100 to 1,000 ppm based on the total weight of the monomers having polymerizable functional groups.

[0031] In such a polymerization reaction, a molecular weight regulator can be used to adjust the molecular weight of the polymer. Examples of such molecular weight regulators include α-olefins such as 1-butene, 1-pentene, 1-hexene, and 1-octene; styrenes such as styrene and vinyltoluene; ethers such as ethyl vinyl ether, i-butyl vinyl ether, and allyl glycidyl ether; halogen-containing vinyl compounds such as allyl chloride; and nitrogen-containing vinyl compounds such as acrylonitrile and acrylamide. A polymer having a desired molecular weight can be obtained by using 0.1 to 100 mol% of the molecular weight regulator relative to the monomer.

[0032] The method for producing the hydrogenated product involves hydrogenating the carbon-carbon double bonds in the polymer main chain in a solution in the presence of hydrogen and a hydrogenation catalyst. Examples of the hydrogenation catalyst used in the hydrogenation include homogeneous catalysts such as Ziegler catalysts consisting of a combination of a transition metal compound and an alkali metal compound, such as cobalt acetate and triethylaluminum, nickel acetylacetonate and triisobutylaluminum, titanocene dichloride and n-butyllithium, zirconocene dichloride and sec-butyllithium, and tetrabutoxytitanate and dimethylmagnesium; ruthenium-carbene catalysts, dichlorotris(triphenylphosphine)rhodium, and noble metal complex catalysts consisting of ruthenium compounds described in JP-A-7-2929, JP-A-7-149823, JP-A-11-209460, JP-A-11-158256, and JP-A-11-193323, etc. In addition, heterogeneous catalysts in which a metal such as nickel, palladium, platinum, rhodium, or ruthenium is supported on a carrier such as carbon, silica, diatomaceous earth, alumina, or titanium oxide, for example, nickel / silica or palladium / carbon, can be used. The hydrogenation reaction is usually carried out in an organic solvent, which can be appropriately selected depending on the solubility of the hydrogenated product to be produced, and the same organic solvent as the polymerization solvent can be used. Therefore, after the polymerization reaction, the hydrogenation catalyst can be added directly to the reaction mixture without replacing the solvent.

[0033] The hydrogenation reaction conditions may be appropriately selected depending on the type of hydrogenation catalyst used. The reaction temperature is usually -20 to 250°C, preferably -10 to 220°C, and more preferably 0 to 200°C. If the reaction temperature is less than -20°C, the reaction rate slows down, and conversely, if the reaction temperature exceeds 250°C, side reactions tend to occur. The hydrogen pressure is usually 0.01 to 10.0 MPa, preferably 0.05 to 8.0 MPa, and more preferably 0.1 to 5.0 MPa. If the hydrogen pressure is less than 0.01 MPa, the hydrogenation rate slows down, and if the hydrogen pressure exceeds 10.0 MPa, a high-pressure reactor is required. The hydrogenation reaction time is appropriately selected to control the hydrogenation rate. The reaction time is usually in the range of 0.1 to 50 hours, and 80% or more, preferably 90% or more, and more preferably 95% or more of the carbon-carbon double bonds in the main chain of the polymer can be hydrogenated.

[0034] After the hydrogenation reaction, it is preferable to remove the catalyst, which can be removed by known methods such as adsorption and removal using an adsorbent such as silica, alumina, activated carbon, etc., removal using an ion exchange resin, insolubilization of the catalyst residue by adding a chelating agent and then filtration, and solidification and separation of the polymer solution with a large amount of a poor solvent such as methanol followed by drying.

[0035] <Compound (A) Having an Amino Group and a Functional Group Reactive with an Acid Anhydride Group> The functional group (hereinafter also referred to as functional group (f)) reactive with an acid anhydride group possessed by the compound (A) (hereinafter also referred to as amino compound (A)) having a functional group reactive with an acid anhydride group and an amino group includes, for example, a hydroxyl group, a thiol group, an amino group, etc. (Note that when the functional group (f) is an amino group, the amino compound (A) is a polyamine compound having two or more amino groups together with the other amino group). By reacting the acid anhydride group of the acid anhydride group-containing cyclic olefin resin with the functional group (f) of the amino compound (A), a modified cyclic olefin resin having an amino group in the side chain is obtained. From the viewpoint of reactivity with an acid anhydride group, the functional group (f) is preferably a hydroxyl group.

[0036] Examples of the amino compound (A) include chain amine compounds such as N,N-dimethylethanolamine and 3-diethylamino-1-propanol, and cyclic amine compounds such as 3-hydroxy-1-methylpiperidine, 3-hydroxyquinuclidine, 1-methyl-4-piperidinemethanol, (1,4-diazabicyclo[2,2,2]octan-2-yl)methanol and 2-(2-hydroxyethyl)-1-methylpyrrolidine.

[0037] <Aqueous composition> The aqueous composition of the present invention is a composition containing the modified cyclic olefin resin of the present invention and an aqueous medium. The aqueous composition of the present invention may be a dispersion in which the modified cyclic olefin resin is dispersed in an aqueous medium, or a solution in which the modified cyclic olefin resin is dissolved in an aqueous medium.

[0038] The aqueous composition of the present invention may contain a neutralizing compound, a curing agent, a curing accelerator, an antioxidant, and the like.

[0039] As the neutralizing compound, for example, iodomethane, organic carboxylic acids such as formic acid, acetic acid, lactic acid, and butyric acid, and inorganic acids such as hydrochloric acid, sulfuric acid, and nitric acid can be added to cationize the N atom of the amino group.

[0040] Examples of the curing agent include epoxy resins and carbodiimide compounds. The epoxy resin is not particularly limited as long as it has two or more epoxy groups per molecule. For example, glycidyl ether epoxy resins such as bisphenol A type epoxy resins, bisphenol F type epoxy resins, bisphenol S type epoxy resins, or hydrogenated versions of these, phenol novolac type epoxy resins, cresol novolac type epoxy resins, glycidyl ester epoxy resins such as hexahydrophthalic acid glycidyl ester and dimer acid glycidyl ester, linear aliphatic epoxy resins such as epoxidized polybutadiene and epoxidized soybean oil, etc. may be mentioned. In addition, the epoxy resin may be modified with, for example, silicone, urethane, polyimide, polyamide, etc., and may contain sulfur atoms, nitrogen atoms, etc. in the molecular skeleton.

[0041] The carbodiimide compound is not particularly limited as long as it has a carbodiimide group in the molecule. A polycarbodiimide having two or more carbodiimide groups in the molecule is preferred. By using a polycarbodiimide, the carboxy group of the modified cyclic olefin resin reacts with the carbodiimide group, enhancing the interaction with the substrate and improving the adhesion.

[0042] The carbodiimide compound may be any of an aromatic carbodiimide compound, an alicyclic carbodiimide compound, and an aliphatic carbodiimide compound, which may be used alone or in combination of two or more. Examples of the aromatic carbodiimide compound include poly-m-phenylene carbodiimide, poly-p-phenylene carbodiimide, polytolylene carbodiimide, poly(diisopropylphenylene carbodiimide), poly(methyldiisopropylphenylene carbodiimide), and poly(4,4'-diphenylmethane carbodiimide). Examples of the alicyclic carbodiimide compound include poly-m-cyclohexylcarbodiimide, poly-p-cyclohexylcarbodiimide, poly(4,4'-dicyclohexylmethanecarbodiimide, poly(3,3'-dicyclohexylmethanecarbodiimide, etc. The aliphatic carbodiimide compound may be either a linear or branched aliphatic carbodiimide compound. Preferred are linear aliphatic carbodiimide compounds, and specific examples thereof include polymethylenecarbodiimide, polyethylenecarbodiimide, polypropylenecarbodiimide, polybutylenecarbodiimide, polypentamethylenecarbodiimide, polyhexamethylenecarbodiimide, etc. These may be used alone or in combination of two or more.

[0043] The curing accelerator is used for the purpose of promoting the reaction between the carboxy group of the modified cyclic olefin resin and the epoxy resin, and examples of the curing accelerator that can be used include tertiary amine-based curing accelerators, tertiary amine salt-based curing accelerators, and imidazole-based curing accelerators.

[0044] Examples of the tertiary amine curing accelerator include benzyldimethylamine, 2-(dimethylaminomethyl)phenol, 2,4,6-tris(dimethylaminomethyl)phenol, tetramethylguanidine, triethanolamine, N,N'-dimethylpiperazine, triethylenediamine, and 1,8-diazabicyclo[5.4.0]undecene.

[0045] Examples of the tertiary amine salt curing accelerator include formate, octylate, p-toluenesulfonate, o-phthalate, phenol salt, and phenol novolac resin salt of 1,8-diazabicyclo[5.4.0]undecene or 1,5-diazabicyclo[4.3.0]nonene.

[0046] Imidazole-based hardening accelerators include 2-methylimidazole, 2-undecylimidazole, 2-heptadecylimidazole, 1,2-dimethylimidazole, 2-methyl-4-ethylimidazole, 2-phenylimidazole, 2-phenyl-4-methylimidazole, 1-benzyl-2-methylimidazole, 1-benzyl-2-phenylimidazole, 2,4-diamino-6-[2'-methylimidazolyl-(1')]ethyl-s-triazine, 2,4-diamino-6-[2' -undecylimidazolyl-(1')]ethyl-s-triazine, 2,4-diamino-6-[2'-ethyl-4'-methylimidazolyl-(1')]ethyl-s-triazine, 2,4-diamino-6-[2'-ethyl-4'-methylimidazolyl-(1')]ethyl-s-triazine isocyanuric acid adduct, 2-phenylimidazole isocyanuric acid adduct, 2-phenyl-4,5-dihydroxymethylimidazole, 2-phenyl-4-methyl-5-hydroxymethylimidazole, etc. These curing accelerators may be used alone or in combination of two or more kinds.

[0047] When the aqueous composition of the present invention contains a curing accelerator, the content of the curing accelerator is preferably 0.5 to 10 parts by mass, and more preferably 1 to 5 parts by mass, relative to 100 parts by mass of the epoxy resin. When the content of the curing accelerator is within the above range, excellent adhesion and heat resistance are obtained.

[0048] Examples of the antioxidant include phenol-based antioxidants such as 2,6-di-tert-butyl-4-methylphenol, n-octadecyl-3-(3',5'-di-tert-butyl-4'-hydroxyphenyl)propionate, tetrakis[methylene-3-(3,5-di-tert-butyl-4-hydroxyphenyl)propionate]methane, pentaerythritol tetrakis[3-(3,5-di-t-butyl-4-hydroxyphenol, triethylene glycol-bis[3-(3-t-butyl-5-methyl-4-hydroxyphenyl)propionate]; Examples of the antioxidant include sulfur-based antioxidants such as 3,3'-thiodipropionate and dimyristyl-3,3'-dithiopropionate; and phosphorus-based antioxidants such as trisnonylphenyl phosphite and tris(2,4-di-tert-butylphenyl) phosphite. These may be used alone or in combination of two or more. The content of the antioxidant is preferably 0.1 to 10 parts by mass, more preferably 0.5 to 5 parts by mass, relative to 100 parts by mass of the modified cyclic olefin resin. By having the content of the antioxidant within the above range, heat resistance can be improved.

[0049] <Composition for electrodeposition paint> The aqueous composition of the present invention can be suitably used as an electrodeposition coating composition. In particular, the modified cyclic polyolefin resin used in the present invention has an amino group, and is particularly suitable for cationic electrodeposition. As an electrodeposition coating method using the aqueous composition of the present invention, a known electrodeposition coating method can be applied. Specifically, when cationic electrodeposition coating is performed using the aqueous composition of the present invention as an electrodeposition coating composition, cationic electrodeposition coating can be performed by a method including a step of immersing a coating target in the electrodeposition coating composition, and a step of applying a voltage between the coating target and the anode, using the coating target as the cathode, to electrodeposit a modified cyclic olefin resin film on the surface of the coating target.

[0050] The object to be coated is an article having a conductive portion to be coated, for example, an object having a portion to be coated made of metal such as copper, iron, steel, aluminum, etc. The shape of the object to be coated is not particularly limited as long as it can be brought into contact with the electrodeposition coating composition.

[0051] In cathodic electrocoating, for example, the object to be coated is the cathode, and a voltage of 1V or more is normally applied between the cathode and the anode. It can be done by applying a voltage of 500V or less. If the applied voltage is 1V or more, it is sufficient. If the voltage is 500V or less, power consumption can be reduced, making it economical.

[0052] In the present invention, when cationic electrodeposition coating is carried out using the electrodeposition coating composition, the temperature of the electrodeposition coating composition is, for example, 10 to 60°C.

[0053] In the present invention, the electrodeposition coating composition can be produced by mixing the aqueous composition of the present invention with various additives, if necessary. EXAMPLES

[0054] The present invention will be specifically described below with reference to examples. However, the present invention is not limited to the examples. In the examples and comparative examples, parts simply indicate parts by mass.

[0055] <Physical property evaluation method> (Acid value measurement) Using a 600MHz nuclear magnetic resonance spectrometer (hereinafter sometimes abbreviated as NMR), 1H-NMR and 13C-NMR measurements were performed under the following conditions, and the acid value was determined from the amount of the compound having an amino group introduced into the cyclic olefin resin. (13C-NMR measurement conditions) Equipment: BRUKER AVANCE NEO 600 spectrometer Measurement solvent: deuterated benzene / o-dichlorobenzene (volume ratio 2 / 8) Sample concentration: approx. 50 mg / approx. 0.60 mL ·Resonance frequency: 150.9MHz Flip angle: 30 degrees Data acquisition time: 2 seconds Pulse repetition time: 0.5 seconds Number of times accumulated: 512 ·Measurement temperature: 120℃ (1H-NMR measurement conditions) Equipment: BRUKER AVANCE NEO 600 spectrometer Measurement solvent: deuterated dimethyl sulfoxide, or deuterated dimethyl sulfoxide / hydrochloric acid (1 mol / L) (0.6 mL / 0.02 mL) Sample concentration: Approx. 20 mg / approx. 0.60 mL ·Resonance frequency: 600MHz Flip angle: 30 degrees Data acquisition time: 4 seconds Pulse repetition time: 1 second Number of times: 64 ·Measurement temperature: 30℃

[0056] (Measurement of glass transition temperature) Measurement was performed using a differential scanning calorimeter (SII, DSC-200). 5 mg of the sample was placed in an aluminum container with a lid, sealed, and cooled to -50°C using liquid nitrogen. The temperature was then increased to 150°C at a rate of 20°C / min, and the glass transition temperature (unit: °C) was determined as the temperature at the intersection of the extension of the baseline before the endothermic peak (below the glass transition temperature) and the tangent to the endothermic peak (the tangent showing the maximum slope between the rising part of the peak and the apex of the peak) in the endothermic curve obtained during the temperature increase process.

[0057] (Average particle size) The average particle size was measured by dynamic light scattering using a concentrated particle size analyzer "FPAR-1000" manufactured by Otsuka Electronics Co., Ltd. When preparing the water-based composition, a sample was taken before adding the curing agent, diluted with deionized water, and the light intensity was adjusted to a range of 15,000 to 40,000 cps. The measurement time was 60 seconds, the measurement temperature was 25°C, and the average particle size D50 (μm) obtained by histogram analysis was taken as the average particle size.

[0058] <Electrodeposition coating> A copper plate (the object to be coated) was used as the cathode and a stainless steel plate as the anode. The plate was immersed in the aqueous composition and a voltage of 100 V was applied to perform electrocoating on the surface of the copper plate. If a resin coating was obtained, it was marked with an O, and if not, it was marked with an X.

[0059] <Synthesis Example 1> (Preparation of modified cyclic olefin resin (P-1)) In a four-neck flask, 100 parts by weight of 5-norbornene-2,3-dicarboxylic anhydride (manufactured by Tokyo Chemical Industry Co., Ltd.) and 150 parts by weight of DMAc (manufactured by Mitsubishi Gas Chemical Co., Ltd.) as a solvent were added at room temperature under a nitrogen atmosphere at 40°C for 1 hour and stirred to dissolve. Next, 0.5 parts by weight of 1-hexene (manufactured by Tokyo Chemical Industry Co., Ltd.) and 0.03 parts by weight of dichloro[1,3-bis(2,4,6-trimethylphenyl)-2-imidazolidinylidene](benzylidene)(tricyclohexylphosphine)ruthenium(II) (manufactured by Sigma-Aldrich Co., Ltd.) were added. Furthermore, 54.3 parts by mass of N,N-dimethylethanolamine as an amino compound (A) and 81.5 parts by weight of DMAc were added and stirred for 2 hours, and then cooled to room temperature to obtain a polymerization solution. Next, as a hydrogenation step, the solution was thoroughly replaced with nitrogen and the internal volume was 1 L. 100 parts by weight were transferred to a SUS autoclave, and 5 parts by weight of Pd-C (Pd 10%) (about 55% water-wet product, manufactured by Tokyo Chemical Industry Co., Ltd.) were added, followed by hydrogen gas (H2) at a pressure of 5.0 MPaG, heating to 60°C and stirring for 4 hours to complete the hydrogenation reaction. Insoluble matter was removed by filtration, and the mixture was purified with a large excess of methyl ethyl ketone to obtain a modified cyclic olefin resin (P-1). The physical property measurements of the obtained modified cyclic olefin resin (P-1) are shown in Table 1.

[0060] <Synthesis Example 2> (Preparation of modified cyclic olefin resin (P-2)) In a four-neck flask, 100 parts by weight of 5-norbornene-2,3-dicarboxylic anhydride (manufactured by Tokyo Chemical Industry Co., Ltd.) and 150 parts by weight of DMAc (manufactured by Mitsubishi Gas Chemical Co., Ltd.) as a solvent were dissolved at room temperature under a nitrogen atmosphere at 40°C for 1 hour with stirring. Next, 0.5 parts by weight of 1-hexene (manufactured by Tokyo Chemical Industry Co., Ltd.) and further dichloro[1,3-bis(2,4,6-trimethylphenyl)-2-imidazolidinylidene] were added. 0.03 parts by weight of (benzylidene)(tricyclohexylphosphine)ruthenium(II) (Sigma-Aldrich Co., Ltd.) was added. Furthermore, 54.3 parts by weight of 3-hydroxy-1-methylpiperidine and 81.5 parts by weight of DMAc were added as amino compound (A) and stirred for 2 hours, and then cooled to room temperature to obtain a polymerization solution. Next, as a hydrogenation step, the solution was thoroughly purged with nitrogen and cooled to room temperature. 100 parts by weight were transferred to a 1.0L SUS autoclave, and 5 parts by weight of Pd-C (Pd 10%) (approximately 55% water-wet product, manufactured by Tokyo Chemical Industry Co., Ltd.) were added. Hydrogen gas (H2) was then introduced at a pressure of 5.0 MPaG, the temperature was raised to 60°C, and the mixture was stirred for 4 hours to complete the hydrogenation reaction. Insoluble matter was removed by filtration, and the mixture was purified with a large excess of methyl ethyl ketone to obtain a modified cyclic olefin resin (P-2). The physical properties of the modified cyclic olefin resin (P-2) obtained are shown in Table 1.

[0061] <Comparative Synthesis Example 1> (Preparation of polypropylene resin (p-4)) 280 parts by weight of ethylene-propylene copolymer (weight average molecular weight: 320,000, ethylene content 4.6 mol%), 21.2 parts by weight of maleic anhydride (Tokyo Chemical Industry Co., Ltd.), 4.2 parts by weight of dicumyl peroxide (Tokyo Chemical Industry Co., Ltd.), and 420 parts by weight of toluene were charged into an autoclave equipped with a stirrer and nitrogen replacement was performed for approximately 5 minutes, after which the reaction was carried out for 5 hours at 140°C while heating and stirring. After the reaction was completed, the reaction solution was poured into a large amount of methyl ethyl ketone to precipitate the resin, which was further washed several times with methyl ethyl ketone to remove unreacted monomers, and thoroughly dried under reduced pressure at 60°C and a pressure of 10 torr to obtain a modified polyolefin. 25 parts by weight of this polyolefin was dissolved in 125 parts by weight of toluene, and 8% by weight of N,N-dimethylethanolamine (manufactured by Tokyo Chemical Industry Co., Ltd.) and 5% by weight of polyoxyethylene styrenated phenyl ether (Noigen EA-197D, manufactured by Daiichi Kogyo Seiyaku Co., Ltd.) were added relative to the resin, and 100 parts by weight of deionized water was added and maintained at 50°C. The above solution was stirred for 10 minutes to obtain a pre-emulsion. The particle size of this pre-emulsion particle was measured, and the average particle size was 0.31 μm.

[0062] <Comparative Synthesis Example 2> (Preparation of polyimide resin (p-5)) In a four-neck flask under dry nitrogen, 43.8 parts by weight of 4,4'-diaminodiphenyl ether (manufactured by Tokyo Chemical Industry Co., Ltd.), which is a diamine, was dissolved in 369.7 parts by weight of N-methyl-2-pyrrolidone (manufactured by Tokyo Chemical Industry Co., Ltd.), which is a solvent. Then, 46.3 parts by weight of pyromellitic anhydride (manufactured by Tokyo Chemical Industry Co., Ltd.), which is a carboxylic acid anhydride, was dissolved in NMP, which is a solvent. Then, under a nitrogen environment, the mixture was synthesized while stirring at room temperature for 12 hours to prepare a solution of polyimide resin (p-5) containing polyamic acid.

[0063] [Table 1]

[0064] <Example 1> (Preparation of Water-Based Composition (d-1)) In a four-neck flask equipped with a stirrer, a reflux condenser, a thermometer, and a nitrogen inlet tube, 25 parts by weight of modified cyclic olefin resin (P-1), 10 parts by weight of NMP, 10 parts by weight of acetic acid, and 55 parts by weight of pure water were added, stirred at 80°C for 3 hours, and cooled to room temperature. The aqueous composition sampled here was almost in the state of an aqueous solution, and the average particle size (D50) could not be measured. Furthermore, a solution in which 1.5 parts by mass of TETRAD-X (tetraglycidyl-m-xylylenediamine, manufactured by Mitsubishi Gas Chemical Company, Inc.) as a curing agent was dissolved in 5 parts by mass of methyl ethyl ketone was added and stirred to obtain an aqueous composition (d-1).

[0065] <Examples 2 to 6> (Preparation of Water-Based Compositions (d-2) to (d-8)) Aqueous compositions (d-2) to (d-6) were prepared in the same manner as for the preparation of aqueous composition (d-1), except that the types and amounts of modified cyclic olefin resin and curing agent were changed as shown in Table 2. In (d-7) and (d-8), polypropylene resin (P-4) and polyimide resin (P-5) were used instead of modified cyclic olefin resin.

[0066] The raw materials used in the synthesis examples and working examples are as follows. (Amino Compound (A)) A1: N,N-Dimethylethanolamine A2: 3-Hydroxy-1-methylpiperidine A3: (1,4-diazabicyclo[2,2,2]octan-2-yl)methanol (hardening agent) H1: Tetraglycidyl-m-xylylenediamine (TETRAD-X, manufactured by Mitsubishi Gas Chemical Co., Ltd.) H2: Phenol novolac type epoxy resin (jER152, manufactured by Mitsubishi Chemical Corporation) H3: Tetraglycidyldiaminodiphenylmethane (jER604, Mitsubishi Chemical Corporation) (emulsifier) E1: Polyoxyethylene styrenated phenyl ether (Noigen EA-197D, Daiichi Kogyo Seiyaku Co., Ltd.) E2: Polyoxyethylene isodecyl ether (Noigen SD-80, Daiichi Kogyo Seiyaku Co., Ltd.)

[0067] The evaluation results of the aqueous compositions (d-1) to (d-8) are shown in Table 2.

[0068] [Table 2]

[0069] As can be seen from the results of Tables 1 and 2, the modified cyclic olefin resins of Examples 1 to 6 and the aqueous compositions using the same could be produced without the need for an emulsifier, and had good cationic electrodeposition coating properties. On the other hand, the modified olefin resin of Comparative Example 1 did not have an amino group, and therefore did not exhibit cationic electrodeposition properties. Furthermore, an aqueous composition could not be produced without an emulsifier. Comparative Example 2 is an example in which a polyimide resin was used instead of the modified olefin resin, but did not exhibit cationic electrodeposition properties. Furthermore, an aqueous composition could not be produced without an emulsifier. [Industrial Applicability]

[0070] The modified cyclic olefin resin of the present invention has excellent heat resistance and is suitable for cationic electrodeposition coating, and therefore can be suitably used as a paint for electrodeposition coating, a water-based composition, a laminate using the same, etc. Furthermore, it can be used as an adhesive / coating agent for functional films in which a functional coating agent is applied to a film, as a food packaging material, a cosmetic packaging material, a medical packaging material, and a polarizing plate material.

Claims

1. A modified cyclic olefin resin having a functional group on a side chain of the cyclic olefin resin, the functional group including an amino group.

2. The modified cyclic olefin resin according to claim 1, having an amine value of 1,000 equivalents / ton or more and less than 10,000 equivalents / ton.

3. The modified cyclic olefin resin according to claim 1 or 2, wherein the functional group further comprises a carboxy group.

4. The modified cyclic olefin resin according to claim 1, having an acid value of 1,000 equivalents / ton or more and less than 10,000 equivalents / ton.

5. 10. An aqueous composition comprising the modified cyclic olefin resin according to claim 1 and an aqueous medium, the aqueous composition being free of an emulsifier.

6. The aqueous composition according to claim 4 or 5, further comprising a hardener.

7. The aqueous composition according to claim 4 or 5, which is for electrodeposition coating.

8. A cured coating film obtained by curing the modified cyclic olefin resin of claim 1 or 2.

Citation Information

Patent Citations

  • High molecular weight polyolefin aqueous emulsion composition

    JP2005036076A