Protective sheet for work processing and manufacturing method of work individualized piece
A protective sheet with optimized layers addresses edge crack issues in chip-on-wafer singulation by stabilizing workpieces during grinding, improving yield through reduced cracking and collisions.
Patent Information
- Application Number
- JP2023055975
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Filing Date
- 2023-03-30
- Publication Date
- 2024-10-11
AI Technical Summary
Existing methods for singulating semiconductor chips with height differences, such as chip-on-wafer, face issues with edge cracks during backside grinding, leading to reduced yield due to wafer bending and collisions between pieces.
A protective sheet for workpiece processing is developed, comprising specific layers with tailored physical properties and thicknesses, including an adhesive layer, intermediate layer, and buffer layer, to minimize edge cracks during grinding.
The protective sheet effectively reduces edge cracks in singulated workpieces, enhancing the yield of laminated chips by stabilizing the workpiece during grinding and preventing collisions.
Smart Images

Figure 2024143347000001_ABST
Abstract
Description
[Technical field]
[0001] The present invention relates to a protective sheet for workpiece processing and a method for manufacturing a workpiece singulated product. In particular, the present invention relates to a protective sheet for workpiece processing suitable for use in a method for grinding the back surface of a workpiece and singulating the workpiece by the resulting stress, and a method for manufacturing a workpiece singulated product using the protective sheet for workpiece processing. [Background technology]
[0002] As various electronic devices become smaller and more multifunctional, the semiconductor chips mounted on them are also required to be smaller and thinner. Semiconductor chips are obtained by dividing a wafer on which multiple circuits are formed into individual circuits. In addition, in order to thin the chips, the backside of the semiconductor wafer is generally ground to adjust the thickness of the wafer. As a method for obtaining thinned chips, a method called dicing before grinding (DBG) is sometimes used, in which grooves of a predetermined depth are formed on the front side of the wafer at the intended division position, and then the wafer is ground from the backside, and the wafer is divided into individual pieces by the stress during grinding, and the chips are obtained. In DBG, backside grinding of the wafer and division of the wafer can be performed simultaneously, so thin chips can be manufactured efficiently.
[0003] Conventionally, when grinding the back surface of a workpiece such as a semiconductor wafer, or when manufacturing individual workpieces such as semiconductor chips by DBG, it is common to apply an adhesive tape called a backgrind sheet to the surface of the workpiece in order to protect the circuits on the surface of the workpiece and to hold the workpiece and the individual workpieces in place.
[0004] The backgrind sheet used in DBG is an adhesive tape having a substrate and an adhesive layer provided on one side of the substrate. As an example of such an adhesive tape, Patent Document 1 discloses an adhesive tape having a substrate, an adhesive layer provided on one side of the substrate, and a buffer layer provided on the other side, the thickness of the tape being equal to or less than a predetermined thickness.
[0005] As a variation of the above-mentioned pre-dicing method, a method has been proposed in which a modified region is provided inside the wafer by a laser, and the wafer is divided into individual pieces by stress during wafer back grinding. Hereinafter, this method may be referred to as LDBG (Laser Dicing Before Grinding). In LDBG, the wafer is cut in the crystal direction starting from the modified region, so that the occurrence of chipping can be reduced more than in the pre-dicing method using a dicing blade or the like. Also, compared to DBG, in which a groove of a predetermined depth is formed on the wafer surface by a dicing blade, there is no region where the wafer is scraped off by the dicing blade, that is, the kerf width is extremely small, so that the chip yield is excellent. [Prior art documents] [Patent documents]
[0006] [Patent Document 1] International Publication No. 2017 / 150676 Summary of the Invention [Problem to be solved by the invention]
[0007] In recent years, a method using chip-on-wafer (CoW) has become known as a method for mounting chips with circuits such as semiconductor chips at a high density. In this method, a chip-on-wafer is obtained by arranging multiple chips smaller than the wafer on the circuit surface of the wafer, and then the chip-on-wafer is divided into individual chips to obtain stacked chips.
[0008] In chip-on-wafer, multiple chips are arranged continuously on the surface of the workpiece and protrude from the surface of the wafer (workpiece). Therefore, on the surface of the workpiece, there is a height difference between the area where the chips are arranged and the other areas, and this height difference corresponds to the height of the arranged chips.
[0009] When performing DBG on a workpiece having such a height difference, a groove is formed along the planned dividing line of the workpiece, a backgrind sheet is attached to protect the surface, and the back surface of the workpiece is ground.
[0010] However, when the adhesive tape for semiconductor processing described in Patent Document 1 is used to singulate the chip-on-wafer by DBG, there is a problem that cracks (edge cracks) are likely to occur due to bending of the wafer caused by thinning of the wafer, collisions between singulated pieces, etc., especially at the peripheral portion (edge) of the wafer corresponding to the starting end and the end of the continuous height difference. When such edge cracks occur, the number of good stacked chips (singulated pieces) decreases, which has a significant impact on the yield of stacked chips.
[0011] The present invention has been made in consideration of the above-described situation, and aims to provide a protective sheet for workpiece processing that can reduce edge cracks in the workpiece fragments after grinding, even when a pre-dicing method is used to grind a workpiece having a surface with height differences, such as a chip-on-wafer, to obtain individual workpiece fragments, and to provide a method for manufacturing individual workpieces using the protective sheet for workpiece processing. [Means for solving the problem]
[0012] The aspects of the present invention are as follows.
[0013] [1] A protective sheet for workpiece processing, comprising an adhesive layer, an intermediate layer, a substrate, and a buffer layer laminated in this order, The shear storage modulus of the adhesive layer at 25°C is 0.18 MPa or less, The shear storage modulus of the intermediate layer at 25°C is 0.25 MPa or less, The Young's modulus of the substrate at 25°C is 1500 MPa or more, The tensile storage modulus of the buffer layer at 25°C is 250 MPa or less, The protective sheet for workpiece processing has an adhesive layer having a thickness of 30 μm or less, an intermediate layer having a thickness of 150 μm or more and 350 μm or less, and a buffer layer having a thickness of 10 μm or more and 100 μm or less.
[0014] [2] The protective sheet for workpiece processing according to [1], wherein the pressure-sensitive adhesive layer has a shear storage modulus of 0.03 MPa or more at 25°C.
[0015] [3] The protective sheet for workpiece processing according to [2], wherein the adhesive layer is energy ray curable.
[0016] [4] A protective sheet for workpiece processing according to any one of [1] to [3], wherein tan δ2 / tan δ1 is greater than 1 when the loss tangent of the adhesive layer at 25°C is tan δ1 and the loss tangent of the intermediate layer at 25°C is tan δ2.
[0017] [5] The protective sheet for workpiece processing according to any one of [1] to [4], wherein the protective sheet for workpiece processing has a thickness of 220 μm or more and 530 μm or less.
[0018] [6] A process of attaching a workpiece processing protective sheet according to any one of [1] to [5] to a surface of a workpiece having a front surface and a back surface opposite to the front surface; A step of forming a groove on a surface of a workpiece or a step of forming a modified region inside the workpiece; A step of grinding a workpiece having a workpiece processing protection sheet attached to a surface thereof and having grooves or modified regions formed thereon from a back surface thereof to separate the workpiece into a plurality of workpiece pieces starting from the grooves or modified regions; and peeling off the workpiece processing protection sheet from the plurality of workpiece individual pieces.
[0019] [7] A method for producing a workpiece singulated according to [6], wherein the surface has height differences. Effect of the Invention
[0020] According to the present invention, it is possible to provide a protective sheet for workpiece processing that can reduce cracks in the workpiece fragments after grinding, even when the workpiece is ground using a pre-dicing method to obtain individual workpieces, and to provide a method for manufacturing individual workpieces using the protective sheet for workpiece processing. [Brief description of the drawings]
[0021] [Figure 1] FIG. 1 is a schematic cross-sectional view of a chip-on-wafer, which is a workpiece having height differences on its surface. [Diagram 2] FIG. 2 is a schematic cross-sectional view showing an example of the protection sheet for workpiece processing according to this embodiment. [Diagram 3] FIG. 3 is a schematic cross-sectional view showing a state in which the protection sheet for workpiece processing according to this embodiment is attached to the surface of a workpiece (a chip-on-wafer as an example). DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0022] DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS The present invention will now be described in detail with reference to the accompanying drawings based on specific embodiments. First, the main terms used in this specification will be explained.
[0023] The work refers to a plate-like body to which a surface protection sheet is attached and then cut into individual pieces. Examples of the work include a circular wafer (including a case having an orientation flat), a rectangular panel level package, and a strip (rectangular substrate) sealed with molded resin. Among them, a wafer is preferable from the viewpoint of easily obtaining the effect of the present invention. The wafer may be, for example, a semiconductor wafer such as a silicon wafer, a gallium arsenide wafer, a silicon carbide wafer, a gallium nitride wafer, or an indium phosphide wafer, or an insulating wafer such as a glass wafer, a lithium tantalate wafer, or a lithium niobate wafer, or may be a reconstructed wafer made of a resin and a semiconductor used for producing a fan-out package or the like. From the viewpoint of easily obtaining the effect of the present invention, a semiconductor wafer or an insulating wafer is preferable, and a semiconductor wafer is more preferable.
[0024] Singulation of a work refers to dividing the work into individual circuits to obtain individual work pieces. For example, if the work is a wafer, the individual work pieces are chips, and if the work is a panel level package or a strip (rectangular substrate) sealed with molded resin, the individual work pieces are semiconductor packages.
[0025] The "front surface" of a workpiece refers to the side on which a circuit or the like is formed or on which the formation of a circuit or the like is planned, and the "back surface" of a workpiece refers to the side on which a circuit or the like is not formed or on which the formation of a circuit or the like is not planned.
[0026] DBG (Dicing Before Grinding) is a method in which grooves of a specified depth are formed on the surface of a wafer as a workpiece, and then the wafer is ground from the back side to separate the wafer by grinding. The grooves formed on the surface of the wafer are formed by methods such as blade dicing, laser dicing, and plasma dicing.
[0027] LDBG (Laser Dicing Before Grinding) is a variation of DBG in which a modified region is created inside the wafer as the workpiece using a laser, and cracks are caused to progress from the modified region due to stresses, etc., generated during grinding of the back surface of the wafer, thereby dividing the wafer into individual pieces.
[0028] The term "group of individual workpieces" refers to a plurality of individual workpieces held on the protective sheet for workpiece processing according to the present invention after the workpiece has been singulated. These individual workpieces, as a whole, form a shape similar to that of the workpiece. The term "group of stacked chips" refers to a plurality of stacked chips held on the protective sheet for workpiece processing according to the present invention after the wafer as the workpiece has been singulated. These chips, as a whole, form a shape similar to that of the wafer.
[0029] "(Meth)acrylate" is used as the term to refer to both "acrylate" and "methacrylate," and similar terms.
[0030] The "energy rays" refer to ultraviolet rays, electron beams, etc., and are preferably ultraviolet rays.
[0031] Unless otherwise specified, the "weight average molecular weight" is a polystyrene equivalent value measured by gel permeation chromatography (GPC). Measurements by such a method are performed, for example, using a high-speed GPC device "HLC-8120GPC" manufactured by Tosoh Corporation with a high-speed column "TSK guard column H XL -H", "TSK Gel GMH XL ", "TSK Gel G2000 H XL (All of the above are manufactured by Tosoh Corporation) connected in the above order, the column temperature was 40° C., the liquid flow rate was 1.0 mL / min, and the detector was a differential refractometer.
[0032] The release sheet is a sheet that releasably supports the pressure-sensitive adhesive layer, the buffer layer, etc. The term "sheet" is not limited to a specific thickness, and is used to include films.
[0033] The mass ratios in the explanations of compositions such as the pressure-sensitive adhesive layer composition are based on the active ingredient (solid content), and do not include the solvent unless otherwise specified.
[0034] (1. Protective sheet for workpiece processing) The protective sheet for work processing is used when processing a workpiece or the like that has circuits formed on one side (front side) and no circuits formed on the other side (back side) (i.e., a workpiece or a group of workpiece individual pieces obtained by individualizing a workpiece).
[0035] In this embodiment, the workpiece to be machined is preferably a workpiece having height differences on its surface. Examples of workpieces having height differences on their surface include chip-on-wafer (CoW) in which a plurality of chips are continuously arranged on the surface of the workpiece, workpieces having convex electrodes (bump electrodes, pillar electrodes, etc.) formed on the surface of the workpiece, and half-trim wafers in which a part of the edge of the workpiece is removed. In this embodiment, the workpiece having height differences is preferably a chip-on-wafer.
[0036] As shown in Fig. 1, a chip-on-wafer 50 is a wafer in which a plurality of chips 52 smaller than the wafer 51 are continuously arranged on the inner periphery of a plate-like body such as a wafer 51. Therefore, there is a height difference D between the top surface of the chip and an area on the wafer where the chip is not arranged. In this embodiment, the height difference D is 50 µm or more. The planar shape of the chip is usually a quadrangle such as a rectangle or a square.
[0037] When DBG is performed on a workpiece having such a height difference, a groove of a predetermined depth is formed on the surface of the workpiece, and then a protective sheet for workpiece processing is attached. The protective sheet for workpiece processing protects the surface during back grinding, but when a height difference occurs on the surface, it is necessary to embed and fix the chips arranged on the surface. If the embedding is insufficient, cracks may occur in the individual pieces due to bending of the wafer, collision between the individual pieces, etc., when the back grinding progresses and the wafer becomes thin, or when the wafer is singulated. Such cracks are particularly likely to occur at the peripheral portion (edge) of the wafer, which corresponds to the start and end of the continuous height difference, and are therefore called edge cracks. Edge cracks affect the yield of the individual pieces, so it is necessary to suppress edge cracks.
[0038] The present inventor found that the occurrence of edge cracks is influenced by the physical properties and size of the layers constituting the workpiece processing protection sheet in a complex manner. As a result, a workpiece processing protection sheet capable of suppressing edge cracks was obtained by optimizing the physical properties and size of each layer constituting the workpiece processing protection sheet. The following describes the workpiece processing protection sheet.
[0039] 2, the protective sheet for workpiece processing 1 according to this embodiment has a configuration in which an intermediate layer 20 and an adhesive layer 30 are laminated in this order on one main surface 10a of a substrate 10, and a buffer layer 40 is laminated on the other main surface 10b of the substrate 10. That is, the protective sheet for workpiece processing 1 has a configuration in which the adhesive layer 30, the intermediate layer 20, the substrate 10, and the buffer layer 40 are laminated in this order.
[0040] The thickness of the workpiece processing protection sheet may be within a range in which the effects of the present invention can be obtained. In this embodiment, the thickness of the workpiece processing protection sheet is preferably 220 μm or more and 530 μm or less. This suppresses edge cracks, facilitates production and storage, and improves handling as a workpiece processing protection sheet.
[0041] The thickness of the protection sheet for workpiece processing is more preferably 250 μm or more and 500 μm or less, and further preferably 300 μm or more and 450 μm or less.
[0042] Each element constituting the protection sheet for workpiece processing 1 shown in FIG. 2 will be described in detail below.
[0043] (2. Base material) The substrate is a rigid member that provides the rigidity of the protective sheet for workpiece processing. The substrate is made of a material capable of supporting the workpiece, and examples thereof include various resin films used as substrates for backgrinding tapes. By using such a resin film, the workpiece can be held without being damaged even if the thickness of the workpiece is reduced by grinding. The substrate may be made of a single-layer film made of one resin film, or may be made of a multi-layer film in which multiple resin films are laminated.
[0044] In this embodiment, the rigidity of the substrate is evaluated by Young's modulus. Specifically, the Young's modulus of the substrate at 25°C is 1500 MPa or more. By having the Young's modulus of the substrate within the above range, non-uniform vibration of the substrate is suppressed, and it becomes possible to stably support and hold the workpiece or the like (workpiece or group of individual pieces of the workpiece) during back grinding. As a result, edge cracks of the individual pieces of the workpiece can be suppressed.
[0045] The Young's modulus of the substrate at 25°C is preferably 1800 MPa or more, more preferably 2100 MPa or more, and even more preferably 2300 MPa or more. The upper limit of the Young's modulus is not particularly limited, but may be 4000 MPa or less. The Young's modulus of the substrate at 25°C is measured in accordance with JIS K 7127. That is, it is measured in the same manner as the measurement method specified in JIS K 7127, but the measurement conditions may be different. The specific measurement method will be described in the examples.
[0046] In this embodiment, the thickness of the substrate is preferably 10 μm or more and 100 μm or less, more preferably 25 μm or more and 85 μm or less, and even more preferably 38 μm or more and 75 μm or less, from the viewpoint of ease of handling and easier achievement of the effects of the present invention.
[0047] (2.1 Substrate material) The material of the substrate may be selected so that the Young's modulus of the substrate falls within the above range. In this embodiment, examples of the material of the substrate include polyesters such as polyethylene terephthalate, polyethylene naphthalate, polybutylene terephthalate, wholly aromatic polyesters, polyimides, polyamides, polycarbonates, polyacetals, modified polyphenylene oxides, polyphenylene sulfides, polysulfones, polyether ketones, biaxially oriented polypropylenes, etc. Among these, polyesters are preferred, and polyethylene terephthalate is more preferred.
[0048] At least one of the main surfaces of the substrate may be subjected to an adhesion treatment such as a corona treatment in order to improve adhesion with a layer formed on the main surface. Also, at least one of the main surfaces of the substrate may be provided with an easy-adhesion layer in order to improve adhesion with a layer formed on the main surface.
[0049] (3. Adhesive Layer) The adhesive layer is attached to the surface of the work (i.e., the surface on which a circuit or the like is formed). The adhesive layer protects the surface and supports the work until it is peeled off from the surface. The adhesive layer may be composed of one layer (single layer), or may be composed of two or more layers. When the adhesive layer has multiple layers, these multiple layers may be the same or different from each other, and the combination of layers constituting these multiple layers is not particularly limited.
[0050] In this embodiment, the thickness of the adhesive layer is 30 μm or less. When the thickness of the adhesive layer is within the above range, the adhesive layer tends to exhibit the function described below. The thickness of the adhesive layer is preferably 25 μm or less, and more preferably 20 μm or less. The lower limit of the thickness of one adhesive layer is not particularly limited as long as it can exhibit a predetermined adhesiveness, but in this embodiment, it may be 5 μm or more. The thickness of the adhesive layer means the thickness of the entire adhesive layer. For example, the thickness of an adhesive layer composed of multiple layers means the total thickness of all layers constituting the adhesive layer.
[0051] In this embodiment, the adhesive layer has the following physical properties, so that the adhesive layer can sufficiently conform to the height difference of the work surface and can fill the height difference well. As a result, the free movement of the work piece pieces is suppressed, and cracks caused by collisions between the work piece pieces can be suppressed.
[0052] (3.1. Shear storage modulus of adhesive layer) In this embodiment, the pressure-sensitive adhesive layer has a shear storage modulus (G1') of 0.18 MPa or less at 25°C. The shear storage modulus is an index of the ease of deformation (hardness) of the pressure-sensitive adhesive layer. In addition, when the pressure-sensitive adhesive layer is energy ray-curable, G1' is the shear storage modulus before energy ray irradiation.
[0053] The protective sheet for workpiece processing is usually attached to the surface of the workpiece at around room temperature, and since G1' is within the above range, it can fully follow the height difference of the surface. That is, when the workpiece is a chip-on-wafer, it can fully follow the shape of the chip and embed and fix the chip. As a result, even if the workpiece is thinned by back grinding, the workpiece is less likely to bend, and even if the workpiece is diced, the movement of the workpiece diced group is suppressed, and collisions can be suppressed. Such collisions are likely to occur at the periphery of the workpiece diced group, so edge cracks can be effectively suppressed.
[0054] The shear storage modulus (G1') of the pressure-sensitive adhesive layer at 25°C is preferably 0.13 MPa or less, more preferably 0.10 MPa or less, and even more preferably 0.07 MPa or less.
[0055] On the other hand, from the viewpoint of the cohesive strength of the adhesive constituting the adhesive layer, the shear storage modulus (G1') of the adhesive layer at 25°C is preferably 0.03 MPa or more, more preferably 0.04 MPa or more.
[0056] If G1' is too low, the adhesive layer will be soft and its cohesive strength will be low, and it will be more likely to penetrate into the height difference on the surface of the workpiece (grooves formed by DBG, areas between chips on a chip-on-wafer, etc.). If the adhesive layer penetrates into the height difference too much, it will be effective in suppressing edge cracks, but if the adhesive layer is energy curable, it may not be cured sufficiently by irradiation with energy rays to peel off the protective sheet for workpiece processing. If the curing is insufficient, the adhesive strength will not decrease sufficiently, and when peeled off, residue of the adhesive layer may be generated in the area where the adhesive layer penetrated too much (generation of adhesive residue).
[0057] Therefore, by setting the lower limit of G1' within the above range, it is possible to suppress the occurrence of adhesive residue upon peeling, particularly when the pressure-sensitive adhesive layer is energy ray curable.
[0058] In addition, when using the acrylic polymer (A) described later, the shear storage modulus of the pressure-sensitive adhesive layer can be adjusted by the type and amount of monomers constituting the acrylic polymer (A), the amount of energy ray curable groups introduced into the acrylic polymer (A), etc. For example, increasing the amount of energy ray curable groups tends to increase the storage modulus. Furthermore, it can also be appropriately adjusted by the amount of crosslinking agent and the amount of photopolymerization initiator blended in the pressure-sensitive adhesive layer.
[0059] The shear storage modulus (G1') of the adhesive layer and the loss tangent tanδ1 of the adhesive layer described below can be measured as follows. First, the material constituting the adhesive layer is used as a measurement sample of a predetermined size. Using a dynamic viscoelasticity measuring device, the measurement sample is twisted at a predetermined frequency within a predetermined temperature range to apply shear strain to the measurement sample, and the storage modulus and loss tangent of the measurement sample are measured. The shear storage modulus and loss tangent of the adhesive layer at 25°C are calculated from the measured modulus. Details of the measurement will be described in the Examples.
[0060] (3.2. Composition of Adhesive Layer) The adhesive layer is not particularly limited as long as it is made of an adhesive that satisfies the above-mentioned physical properties. In this embodiment, the adhesive layer is preferably energy ray curable. Since the adhesive layer of the workpiece processing protective sheet is energy ray curable, when it is attached to the workpiece, it sticks to the workpiece with high adhesive strength, and when it is peeled off from the workpiece, the adhesive strength can be reduced by irradiating energy rays. Therefore, when the workpiece processing protective sheet is peeled off, even if the workpiece is diced, it is easy to peel off from the group of diced workpieces while appropriately protecting chips, circuits, etc. on the workpiece.
[0061] The composition for the adhesive layer forming the adhesive layer preferably contains, as an adhesive resin capable of imparting adhesiveness to the adhesive layer, for example, an acrylic polymer, a polyurethane, a rubber polymer, a polyolefin, a silicone polymer, etc. Of these, an acrylic polymer is preferred.
[0062] The adhesive layer composition may have energy ray curability by blending an energy ray curable compound separately from the adhesive resin, but it is preferable that the above-mentioned adhesive resin itself is energy ray curable. When the adhesive resin itself has energy ray curability, an energy ray curable group is introduced into the adhesive resin, and it is preferable that the energy ray curable group is introduced into the main chain or side chain of the adhesive resin.
[0063] In addition, when an energy ray curable compound is blended separately from the adhesive resin, a monomer or oligomer having an energy ray curable group is used as the energy ray curable compound. The oligomer is an oligomer having a weight average molecular weight (Mw) of less than 10,000, for example, urethane (meth)acrylate. In addition, even if the adhesive resin itself has energy ray curability, the composition for adhesive layer may be blended with an energy ray curable compound other than the adhesive resin.
[0064] Hereinafter, a more detailed description will be given of the case where the energy ray-curable adhesive resin contained in the composition for adhesive layer is an acrylic polymer (hereinafter also referred to as "acrylic polymer (A)").
[0065] (3.2.1 Acrylic polymer (A)) The acrylic polymer (A) is an acrylic polymer having an energy ray curable group introduced therein and a structural unit derived from a (meth)acrylate. The energy ray curable group is preferably introduced into a side chain of the acrylic polymer.
[0066] The acrylic polymer (A) is preferably a reaction product obtained by reacting an acrylic copolymer (A0) having a structural unit derived from an alkyl (meth)acrylate (a1) and a structural unit derived from a functional group-containing monomer (a2) with an energy ray-curable substance (Xa) having an energy ray-curable group.
[0067] As the alkyl (meth)acrylate (a1), an alkyl (meth)acrylate having an alkyl group with 1 to 18 carbon atoms is used. Specific examples include methyl (meth)acrylate, ethyl (meth)acrylate, propyl (meth)acrylate, n-butyl (meth)acrylate, n-pentyl (meth)acrylate, n-hexyl (meth)acrylate, 2-ethylhexyl (meth)acrylate, isooctyl (meth)acrylate, n-decyl (meth)acrylate, n-dodecyl (meth)acrylate, n-tridecyl (meth)acrylate, myristyl (meth)acrylate, palmityl (meth)acrylate, and stearyl (meth)acrylate. Among these, the alkyl (meth)acrylate (a1) is preferably an alkyl (meth)acrylate having an alkyl group with 4 to 8 carbon atoms. Specifically, 2-ethylhexyl (meth)acrylate and n-butyl (meth)acrylate are preferred because it is easier to set the shear storage modulus (G1') within the above-mentioned range and the tan δ2 / tan δ1 within the range described below. These may be used alone or in combination of two or more.
[0068] From the viewpoint of improving the adhesive strength of the pressure-sensitive adhesive layer to be formed, the content of the structural units derived from the alkyl (meth)acrylate (a1) in the acrylic polymer (A0) is preferably 40 to 95 mass%, more preferably 50 to 90 mass%, and even more preferably 60 to 85 mass%, relative to all structural units (100 mass%) of the acrylic polymer (A0).
[0069] For example, the alkyl (meth)acrylate (a1) may contain ethyl (meth)acrylate and methyl (meth)acrylate in addition to the above-mentioned 2-ethylhexyl (meth)acrylate and n-butyl (meth)acrylate. By containing these monomers, it becomes easier to adjust the adhesive performance of the adhesive layer to a desired one.
[0070] The functional group-containing monomer (a2) is a monomer having a functional group such as a hydroxy group, a carboxy group, an epoxy group, an amino group, a cyano group, a nitrogen atom-containing ring group, or an alkoxysilyl group. Among these, at least one selected from a hydroxy group-containing monomer, a carboxy group-containing monomer, and an epoxy group-containing monomer is preferred. Examples of the hydroxy group-containing monomer include hydroxyalkyl (meth)acrylates such as 2-hydroxyethyl (meth)acrylate, 2-hydroxypropyl (meth)acrylate, 3-hydroxypropyl (meth)acrylate, 2-hydroxybutyl (meth)acrylate, 3-hydroxybutyl (meth)acrylate, and 4-hydroxybutyl (meth)acrylate; and unsaturated alcohols such as vinyl alcohol and allyl alcohol.
[0071] Examples of the carboxyl group-containing monomer include (meth)acrylic acid, maleic acid, fumaric acid, and itaconic acid.
[0072] The epoxy-containing monomer includes an epoxy group-containing (meth)acrylic acid ester and a non-acrylic epoxy group-containing monomer. The epoxy group-containing (meth)acrylic acid ester includes, for example, glycidyl (meth)acrylate, β-methylglycidyl (meth)acrylate, (3,4-epoxycyclohexyl)methyl (meth)acrylate, 3-epoxycyclo-2-hydroxypropyl (meth)acrylate, etc. The non-acrylic epoxy group-containing monomer includes, for example, glycidyl crotonate, allyl glycidyl ether, etc.
[0073] As the functional group-containing monomer (a2), among the above, a hydroxy group-containing monomer is more preferable, among which a hydroxyalkyl (meth)acrylate is more preferable, 2-hydroxyethyl (meth)acrylate and 4-hydroxybutyl (meth)acrylate are further preferable, and 2-hydroxyethyl (meth)acrylate is particularly preferable.
[0074] By using a hydroxyalkyl (meth)acrylate as the component (a2), it becomes possible to react the energy ray-curable substance (Xa) with the acrylic polymer (A0) relatively easily.
[0075] The content of the structural units derived from the functional group-containing monomer (a2) in the acrylic polymer (A0) is preferably 4 to 30 mass%, more preferably 8 to 26 mass%, and even more preferably 12 to 22 mass%, based on the total structural units (100 mass%) of the acrylic polymer (A0).
[0076] If the content is 4% by mass or more, a certain amount of functional groups that become reaction sites with the energy ray curable material (Xa) can be secured. Therefore, the adhesive layer can be appropriately cured by irradiation with energy rays, so that the adhesive strength after irradiation with energy rays can be reduced. Also, if the content is 30% by mass or less, a sufficient pot life can be secured when applying a solution of the adhesive layer composition to form an adhesive layer, and it becomes easier to set the shear storage modulus (G1') within the above-mentioned range and tan δ2 / tan δ1 within the range described below.
[0077] The acrylic polymer (A0) may be a copolymer of an alkyl (meth)acrylate (a1) and a functional group-containing monomer (a2), or may be a copolymer of the (a1) component, the (a2) component, and a monomer (a3) other than the (a1) and (a2) components.
[0078] Examples of the other monomers (a3) include (meth)acrylates having a cyclic structure such as cyclohexyl (meth)acrylate, benzyl (meth)acrylate, isobornyl (meth)acrylate, dicyclopentanyl (meth)acrylate, dicyclopentenyl (meth)acrylate, and dicyclopentenyloxyethyl (meth)acrylate, as well as vinyl acetate and styrene. The other monomers (a3) may be used alone or in combination of two or more.
[0079] The content of the structural units derived from the other monomer (a3) in the acrylic polymer (A0) is preferably 0 to 8 mass%, more preferably 0 to 4 mass%, and even more preferably 0 to 2 mass%, relative to all structural units (100 mass%) of the acrylic polymer (A0).
[0080] The energy ray curable substance (Xa) is a compound having an energy ray curable group and a substituent (hereinafter, simply referred to as "reactive substituent") that can react with a functional group in the structural unit derived from the (a2) component of the acrylic polymer (A0). Examples of the energy ray curable group include a (meth)acryloyl group and a vinyl group, and a (meth)acryloyl group is preferred. In addition, the energy ray curable substance (Xa) is preferably a compound having 1 to 5 energy ray curable groups per molecule.
[0081] The reactive substituent in the energy ray curable substance (Xa) may be appropriately changed depending on the functional group possessed by the functional group-containing monomer (a2), and may be, for example, an isocyanate group, a carboxyl group, an epoxy group, etc., with the isocyanate group being preferred from the viewpoint of reactivity, etc. When the energy ray curable substance (Xa) has an isocyanate group, for example, when the functional group of the functional group-containing monomer (a2) is a hydroxyl group, it becomes possible for the substance to easily react with the acrylic polymer (A0).
[0082] Specific examples of the energy ray curable substance (Xa) include (meth)acryloyloxyethyl isocyanate, meta-isopropenyl-α,α-dimethylbenzyl isocyanate, (meth)acryloyl isocyanate, allyl isocyanate, glycidyl (meth)acrylate, (meth)acrylic acid, etc. These energy ray curable substances (Xa) may be used alone or in combination of two or more. Among these, (meth)acryloyloxyethyl isocyanate is preferred from the viewpoint of having a suitable isocyanate group as the reactive substituent and being a compound with an appropriate distance between the main chain and the energy ray curable group.
[0083] Since it is easier to adjust the shear storage modulus (G1') to the above-mentioned range and the tan δ2 / tan δ1 to the range described below, the energy ray-curable substance (Xa) is reacted with the functional groups in an amount of preferably 50 to 95 equivalents, more preferably 80 to 92 equivalents, of the total amount (100 equivalents) of functional groups derived from the functional group-containing monomer (a2) in the acrylic polymer (A0).
[0084] The weight average molecular weight (Mw) of the acrylic polymer (A) is preferably from 100,000 to 1,200,000, more preferably from 150,000 to 800,000, and even more preferably from 200,000 to 600,000. By having such an Mw, it is possible to impart appropriate adhesiveness to the pressure-sensitive adhesive layer.
[0085] The content of the acrylic polymer (A) is preferably 70 to 98 mass %, more preferably 80 to 96 mass %, and even more preferably 85 to 94 mass %, relative to the total amount (100 mass %) of the composition for pressure-sensitive adhesive layer.
[0086] Even when the adhesive resin has energy ray curability, the composition for adhesive layer may contain an energy ray curable compound other than the adhesive resin. As such an energy ray curable compound, a monomer or oligomer having an unsaturated group in the molecule and capable of being polymerized and cured by irradiation with energy rays is preferable.
[0087] Specific examples include polyvalent (meth)acrylate monomers such as trimethylolpropane tri(meth)acrylate, pentaerythritol (meth)acrylate, pentaerythritol tetra(meth)acrylate, dipentaerythritol hexa(meth)acrylate, 1,4-butylene glycol di(meth)acrylate, and 1,6-hexanediol (meth)acrylate; and oligomers such as urethane (meth)acrylate, polyester (meth)acrylate, polyether (meth)acrylate, and epoxy (meth)acrylate.
[0088] (3.2.2. Crosslinking Agents) The pressure-sensitive adhesive layer composition preferably further contains a crosslinking agent. By crosslinking the acrylic polymer (A) with the crosslinking agent, the pressure-sensitive adhesive layer is appropriately formed as a coating film, and the pressure-sensitive adhesive layer is easily able to exhibit the desired function.
[0089] Examples of the crosslinking agent include an isocyanate-based crosslinking agent, an epoxy-based crosslinking agent, an aziridine-based crosslinking agent, and a chelate-based crosslinking agent, and among these, an isocyanate-based crosslinking agent is preferred. The crosslinking agents may be used alone or in combination of two or more kinds.
[0090] Examples of the isocyanate crosslinking agent include polyisocyanate compounds. Specific examples of the polyisocyanate compound include aromatic polyisocyanates such as tolylene diisocyanate, diphenylmethane diisocyanate, and xylylene diisocyanate, aliphatic polyisocyanates such as hexamethylene diisocyanate, and alicyclic polyisocyanates such as isophorone diisocyanate and hydrogenated diphenylmethane diisocyanate. In addition, biuret and isocyanurate forms of these compounds, as well as adducts which are reactants with low-molecular active hydrogen-containing compounds such as ethylene glycol, propylene glycol, neopentyl glycol, trimethylolpropane, and castor oil, are also included.
[0091] Since it is easier to set the shear storage modulus (G1') in the above-mentioned range and tan δ2 / tan δ1 in the below-mentioned range, the content of the crosslinking agent is preferably 0.1 to 5 parts by mass, more preferably 0.2 to 3 parts by mass, and even more preferably 0.3 to 1.5 parts by mass, relative to 100 parts by mass of the acrylic polymer (A).
[0092] (3.2.3. Photopolymerization initiator) The pressure-sensitive adhesive layer composition preferably further contains a photopolymerization initiator, which facilitates the progress of energy ray curing of the pressure-sensitive adhesive layer by ultraviolet light or the like.
[0093] Examples of the photopolymerization initiator include acetophenone, 2,2-diethoxybenzophenone, 4-methylbenzophenone, 2,4,6-trimethylbenzophenone, Michler's ketone, benzoin, benzoin methyl ether, benzoin ethyl ether, benzoin isopropyl ether, benzoin isobutyl ether, benzyl diphenylsulfide, tetramethylthiuram monosulfide, benzyl dimethyl ketal, dibenzyl, diacetyl, 1-chloroanthraquinone, 2-chloroanthraquinone, 2-ethylanthraquinone, 2,2-dimethoxy-2-phenylacetophenone, 1-hydroxybenzoyl ether ... Examples of photopolymerization initiators include low molecular weight polymerization initiators such as 2-methyl-1-[4-(methylthio)phenyl]-2-morpholinopropanone-1,2-benzyl-2-dimethylamino-1-(4-morpholinophenyl)-butanone-1,2-hydroxy-2-methyl-1-phenyl-propan-1-one, diethylthioxanthone, isopropylthioxanthone, and 2,4,6-trimethylbenzoyldiphenyl-phosphine oxide, and oligomerized polymerization initiators such as oligo{2-hydroxy-2-methyl-1-[4-(1-methylvinyl)phenyl]propanone}. The photopolymerization initiator may be used alone or in combination of two or more kinds. Among the above, 2,2-dimethoxy-2-phenylacetophenone and 1-hydroxycyclohexyl-phenyl ketone are preferred.
[0094] The content of the photopolymerization initiator is preferably 2 to 12 mass %, more preferably 4 to 10 mass %, and further preferably 5 to 8 mass %, relative to the total amount (100 mass %) of the composition for pressure-sensitive adhesive layer.
[0095] The pressure-sensitive adhesive layer composition may contain other additives within the range that does not impair the effects of the present invention. Examples of other additives include tackifiers, antioxidants, softeners (plasticizers), fillers, rust inhibitors, pigments, dyes, etc. When these additives are contained, the content of each additive is preferably 0.01 to 6 parts by mass, more preferably 0.02 to 2 parts by mass, based on 100 parts by mass of the acrylic polymer (A).
[0096] (4. Middle Class) The intermediate layer is a layer provided between the adhesive layer and the substrate in the protective sheet for workpiece processing. The intermediate layer may be formed directly on the substrate, but as described above, when another layer such as an easy-adhesion layer is provided on the substrate, the intermediate layer is formed on the other layer. The intermediate layer may be composed of one layer (single layer), or may be composed of two or more layers. When the intermediate layer has multiple layers, these multiple layers may be the same or different from each other, and the combination of layers constituting these multiple layers is not particularly limited.
[0097] In this embodiment, the thickness of the intermediate layer is 150 μm or more and 350 μm or less. By having the thickness of the intermediate layer within the above range, the function of the intermediate layer described below tends to be easily exhibited. The thickness of the intermediate layer is preferably 175 μm or more and 330 μm or less, and more preferably 200 μm or more and 310 μm or less. The thickness of the intermediate layer means the thickness of the entire intermediate layer. For example, the thickness of an intermediate layer composed of multiple layers means the total thickness of all layers constituting the intermediate layer.
[0098] In this embodiment, the intermediate layer has the following physical properties, so that the intermediate layer can sufficiently conform to the height difference of the work surface and can fill the height difference well. As a result, free movement of the work piece pieces is suppressed, and cracks caused by collisions between the work piece pieces can be suppressed.
[0099] (4.1. Shear storage modulus of the intermediate layer) In this embodiment, the shear storage modulus (G2') of the intermediate layer at 25°C is 0.25 MPa or less. The shear storage modulus is an index of the ease of deformation (hardness) of the intermediate layer. Note that, when the intermediate layer is energy ray curable, G2' is the shear storage modulus before energy ray irradiation.
[0100] The protective sheet for workpiece processing is usually applied to the surface of the workpiece at around room temperature, but since G2' is within the above range, the intermediate layer is easily deformed together with the adhesive layer, and can sufficiently follow the height difference of the surface. In other words, when the workpiece is a chip-on-wafer, the intermediate layer can sufficiently follow the shape of the arranged chip, and the chip can be embedded and fixed together with the adhesive layer. As a result, even if the workpiece is thinned by back grinding and the workpiece is bent, diced, etc., the movement of the workpiece diced group is suppressed, and collisions can be suppressed. Such collisions are likely to occur around the outer edge of the workpiece diced group, so edge cracks can be effectively suppressed.
[0101] The shear storage modulus (G2') of the intermediate layer at 25°C is preferably 0.20 MPa or less, and more preferably 0.17 MPa or less. On the other hand, the lower limit of the shear storage modulus (G2') of the intermediate layer at 25°C is not particularly limited as long as the effects of the present invention can be obtained, but from the viewpoint of easier handling, it is preferably 0.02 MPa or more, and more preferably 0.05 MPa or more.
[0102] The shear storage modulus of the intermediate layer can be adjusted by the amount of the acrylic polymer (B) described later and the amount of the energy ray curable group introduced into the acrylic polymer (B). For example, the storage modulus tends to increase when the amount of the acrylic polymer (B) or the amount of the energy ray curable group is increased. In addition, the storage modulus can be appropriately adjusted by the type and amount of the monomer constituting the acrylic polymer (B), the amount of the crosslinking agent and the amount of the photopolymerization initiator incorporated in the intermediate layer, and the like.
[0103] The shear storage modulus of the intermediate layer can be measured in the same manner as the above-mentioned method for measuring the shear storage modulus of the pressure-sensitive adhesive layer, and the details of the measurement will be described in the Examples.
[0104] (4.2. Ratio of loss tangent of intermediate layer to loss tangent of adhesive layer) In this embodiment, when the loss tangent of the pressure-sensitive adhesive layer at 25° C. is tanδ1 and the loss tangent of the intermediate layer is tanδ2, tanδ2 / tanδ1 is preferably greater than 1, more preferably 1.5 or more, and even more preferably 2.0 or more. There is no particular upper limit for tanδ2 / tanδ1, but it may be 5 or less, 4 or less, or 3.5 or less. By setting tanδ2 / tanδ1 to these upper limits or less, interlayer peeling between the intermediate layer and the pressure-sensitive adhesive layer is more easily prevented.
[0105] The loss tangent tan δ2 of the intermediate layer can be measured in the same manner as the loss tangent tan δ1 of the pressure-sensitive adhesive layer described above. The details of the measurement will be described in the Examples.
[0106] The ratio (tan δ2 / tan δ1) of the loss tangent of the adhesive layer to the loss tangent of the intermediate layer is greater than 1, which indicates that the intermediate layer has stronger viscous properties than the adhesive layer. When the tan δ2 / tan δ1 is within the above range, the intermediate layer is more easily deformed and fills in height differences than the adhesive layer when the protective sheet for workpiece processing is attached to the workpiece, so that even if the workpiece is diced, the movement of the diced workpieces is suppressed, and collisions can be suppressed. In other words, edge cracks can be further suppressed.
[0107] (4.3. Composition of the Intermediate Layer) The intermediate layer is a layer formed from a composition for intermediate layer. The composition for intermediate layer is not particularly limited as long as it satisfies the above-mentioned physical properties. In the present embodiment, the composition for intermediate layer preferably contains two or more kinds of acrylic polymers. Specifically, the composition for intermediate layer preferably contains a non-energy ray curable acrylic polymer (B) and an energy ray curable acrylic polymer (C) having a weight average molecular weight of 50,000 to 250,000. The intermediate layer containing the acrylic polymers (B) and (C) exhibits cohesive force due to the acrylic polymer (B) and stress relaxation property due to the low molecular weight acrylic polymer (C).
[0108] Therefore, the intermediate layer has high retention performance for the adherend, for example, good conformability to height differences formed on the surface of the workpiece, etc. Therefore, it is possible to prevent damage to the workpiece and infiltration of grinding chips or grinding water into the workpiece surface during back grinding of the workpiece.
[0109] The acrylic polymer (B) and the acrylic polymer (C) will be described in detail below.
[0110] (4.3.1. Acrylic polymer (B)) The acrylic polymer (B) is a non-energy ray curable polymer having a structural unit derived from a (meth)acrylate. The acrylic polymer (B) more preferably has a structural unit derived from an alkyl (meth)acrylate (b1) and a structural unit derived from a functional group-containing monomer (b2).
[0111] The copolymerization form of the acrylic polymer (B) is not particularly limited, and may be a block copolymer or a random copolymer.
[0112] As the alkyl (meth)acrylate (b1), an alkyl (meth)acrylate having an alkyl group with 1 to 18 carbon atoms is used. Specific examples include methyl (meth)acrylate, ethyl (meth)acrylate, propyl (meth)acrylate, n-butyl (meth)acrylate, n-pentyl (meth)acrylate, n-hexyl (meth)acrylate, 2-ethylhexyl (meth)acrylate, isooctyl (meth)acrylate, n-decyl (meth)acrylate, n-dodecyl (meth)acrylate, n-tridecyl (meth)acrylate, myristyl (meth)acrylate, palmityl (meth)acrylate, and stearyl (meth)acrylate. The alkyl (meth)acrylate (b1) may be used alone or in combination of two or more.
[0113] The content of the structural units derived from the alkyl (meth)acrylate (b1) in the acrylic polymer (B) is preferably 60 to 98 mass%, more preferably 75 to 95 mass%, and even more preferably 85 to 92 mass%, relative to all structural units (100 mass%) of the acrylic polymer (B).
[0114] If this content is 60 mass% or more, it is easy to improve the ability to conform to the height difference of the work surface, etc. Also, if it is 98 mass% or less, it is possible to ensure a certain amount or more of the constitutional unit derived from the (b2) component.
[0115] Among the above, the alkyl(meth)acrylate (b1) is preferably an alkyl(meth)acrylate having an alkyl group with 1 to 8 carbon atoms, and more preferably contains an alkyl(meth)acrylate having an alkyl group with 4 to 8 carbon atoms (hereinafter sometimes referred to as monomer (Y)), in order to adjust the storage modulus of the intermediate layer to an appropriate value. Specifically, the monomer (Y) is preferably 2-ethylhexyl(meth)acrylate or n-butyl(meth)acrylate, and particularly preferably 2-ethylhexyl acrylate or n-butyl acrylate.
[0116] Here, all of the alkyl (meth)acrylate (b1) constituting the acrylic polymer (B) may be the monomer (Y), or only a part of the alkyl (meth)acrylate (b1) may be the monomer (Y).
[0117] The functional group-containing monomer (b2) is a monomer having a functional group such as a hydroxy group, a carboxy group, an epoxy group, an amino group, a cyano group, a nitrogen atom-containing cyclic group, an alkoxysilyl group, etc. Among the above, the functional group-containing monomer (b2) is preferably at least one selected from the group consisting of a hydroxy group-containing monomer, a carboxy group-containing monomer, and an epoxy group-containing monomer.
[0118] Examples of hydroxy group-containing monomers include hydroxyalkyl (meth)acrylates such as 2-hydroxyethyl (meth)acrylate, 2-hydroxypropyl (meth)acrylate, 3-hydroxypropyl (meth)acrylate, 2-hydroxybutyl (meth)acrylate, 3-hydroxybutyl (meth)acrylate, and 4-hydroxybutyl (meth)acrylate; and unsaturated alcohols such as vinyl alcohol and allyl alcohol.
[0119] Examples of the carboxy group-containing monomer include (meth)acrylic acid, maleic acid, fumaric acid, and itaconic acid.
[0120] The epoxy-containing monomer includes an epoxy group-containing (meth)acrylic acid ester and a non-acrylic epoxy group-containing monomer. The epoxy group-containing (meth)acrylic acid ester includes, for example, glycidyl (meth)acrylate, β-methylglycidyl (meth)acrylate, (3,4-epoxycyclohexyl)methyl (meth)acrylate, 3-epoxycyclo-2-hydroxypropyl (meth)acrylate, etc. The non-acrylic epoxy group-containing monomer includes, for example, glycidyl crotonate, allyl glycidyl ether, etc.
[0121] The functional group-containing monomer (b2) may be used alone or in combination of two or more kinds.
[0122] Among the functional group-containing monomers (b2), carboxy group-containing monomers are more preferred, among which (meth)acrylic acid is even more preferred, and acrylic acid is the most preferred. When a carboxy group-containing monomer is used as the functional group-containing monomer (b2), the cohesive strength of the intermediate layer is increased, and the retention performance of the intermediate layer is further improved.
[0123] The content of the structural units derived from the functional group-containing monomer (b2) in the acrylic polymer (B) is preferably 4 to 30 mass%, more preferably 6 to 20 mass%, and even more preferably 8 to 15 mass%, based on the total structural units (100 mass%) of the acrylic polymer (B).
[0124] If the content of the structural unit derived from the component (b2) is 4% by mass or more, the cohesive strength of the intermediate layer is high, and compatibility with the acrylic polymer (C) described below is also easily improved. On the other hand, if the content is 30% by mass or less, it is easier to set the shear storage modulus (G2') and tan δ2 / tan δ1 within the above-mentioned ranges.
[0125] The acrylic polymer (B) may be a copolymer of an alkyl (meth)acrylate (b1) and a functional group-containing monomer (b2), or may be a copolymer of the (b1) component, the (b2) component, and a monomer (b3) other than the (b1) and (b2) components.
[0126] Examples of the other monomers (b3) include (meth)acrylates having a cyclic structure such as cyclohexyl (meth)acrylate, benzyl (meth)acrylate, isobornyl (meth)acrylate, dicyclopentanyl (meth)acrylate, dicyclopentenyl (meth)acrylate, and dicyclopentenyloxyethyl (meth)acrylate, as well as vinyl acetate and styrene. The other monomers (b3) may be used alone or in combination of two or more.
[0127] The content of the structural units derived from the other monomer (b3) in the acrylic polymer (B) is preferably 0 to 8 mass%, more preferably 0 to 4 mass%, and even more preferably 0 to 2 mass%, relative to all structural units (100 mass%) of the acrylic polymer (B).
[0128] The weight average molecular weight (Mw) of the acrylic polymer (B) is preferably 250,000 to 1,200,000, more preferably 300,000 to 900,000, even more preferably 400,000 to 800,000, and even more preferably 500,000 to 700,000. By setting Mw to the upper limit or less, the acrylic polymer (B) has good compatibility with the acrylic polymer (C), and it is easier to set the shear storage modulus (G2') and tan δ2 / tan δ1 within the above range. In addition, by setting Mw within the above range, it is easier to improve the retention performance of the protection sheet for workpiece processing.
[0129] The content of the acrylic polymer (B) in the intermediate layer composition is preferably 40 to 95 mass%, more preferably 50 to 92 mass%, and even more preferably 55 to 88 mass%, relative to the total amount (100 mass%) of the intermediate layer composition.
[0130] (4.3.2. Acrylic Polymer (C)) The acrylic polymer (C) is an acrylic polymer having energy ray curability due to the introduction of an energy ray curable group. The weight average molecular weight (Mw) of the acrylic polymer (C) is 50,000 to 250,000. In this embodiment, by using the acrylic polymer (C) in the intermediate layer, it is considered that the acrylic polymer (C) reacts with the energy ray curable component in the pressure-sensitive adhesive layer and bonds when irradiated with energy rays. Therefore, coupled with the relatively small difference in shear storage modulus, the interlayer strength between the intermediate layer and the pressure-sensitive adhesive layer after energy ray curing is improved.
[0131] If the Mw of the acrylic polymer (C) is less than 50,000, when the protective sheet for workpiece processing is stored for a long period of time, a part of the acrylic polymer (C) component migrates into the adhesive layer, and the adhesive strength of the protective sheet for workpiece processing becomes unstable, and the adhesive layer may be excessively cured after energy ray irradiation. As a result, when the protective sheet for workpiece processing is used after a long period of storage, or when it is left attached to an adherend for a long period of time, the interlayer strength between the intermediate layer and the adhesive layer after energy ray irradiation may be insufficient. In addition, when the Mw of the acrylic polymer (C) is more than 250,000, the interlayer strength between the intermediate layer and the adhesive layer after energy ray irradiation is also likely to decrease.
[0132] From the above viewpoints, the weight average molecular weight (Mw) of the acrylic polymer (C) is preferably from 60,000 to 220,000, more preferably from 70,000 to 200,000, and further preferably from 80,000 to 180,000.
[0133] The acrylic polymer (C) is an acrylic polymer having an energy ray curable group introduced therein and a structural unit derived from (meth)acrylate. The energy ray curable group of the acrylic polymer (C) is preferably introduced into a side chain of the acrylic polymer. The energy ray curable group may be any group containing an energy ray curable carbon-carbon double bond, and examples of the energy ray curable group include a (meth)acryloyl group and a vinyl group, among which a (meth)acryloyl group is preferred.
[0134] The acrylic polymer (C) is more preferably a reaction product obtained by reacting an acrylic copolymer (C0) having a structural unit derived from an alkyl (meth)acrylate (c1) and a structural unit derived from a functional group-containing monomer (c2) with an energy ray-curable substance (Xc) having an energy ray-curable group.
[0135] The copolymerization form of the acrylic polymer (C0) is not particularly limited, and may be any of a block copolymer, a random copolymer, and the like.
[0136] As the alkyl(meth)acrylate (c1), an alkyl(meth)acrylate having an alkyl group with a carbon number of 1 to 18 is used. As the alkyl(meth)acrylate (c1), an alkyl(meth)acrylate having an alkyl group with a carbon number of 1 to 18 is used. Specific examples include methyl(meth)acrylate, ethyl(meth)acrylate, propyl(meth)acrylate, n-butyl(meth)acrylate, n-pentyl(meth)acrylate, n-hexyl(meth)acrylate, 2-ethylhexyl(meth)acrylate, isooctyl(meth)acrylate, n-decyl(meth)acrylate, n-dodecyl(meth)acrylate, n-tridecyl(meth)acrylate, myristyl(meth)acrylate, palmityl(meth)acrylate, and stearyl(meth)acrylate. The alkyl (meth)acrylate (c1) may be used alone or in combination of two or more kinds.
[0137] The content of the structural unit derived from alkyl (meth)acrylate (c1) in the acrylic polymer (C0) is preferably 40 to 90% by mass, more preferably 50 to 85% by mass, and even more preferably 60 to 80% by mass, based on the total structural units (100% by mass) of the acrylic polymer (C0). If this content is 40% by mass or more, the shape of the intermediate layer formed can be sufficiently maintained. Also, if it is 90% by mass or less, a certain amount of structural units derived from the (c2) component, which become reaction sites with the energy ray-curable material (Xc), can be secured.
[0138] The alkyl(meth)acrylate (c1) is preferably an alkyl(meth)acrylate having an alkyl group with 1 to 8 carbon atoms, and more preferably contains a monomer (Y) (i.e., an alkyl(meth)acrylate having an alkyl group with 4 to 8 carbon atoms). Suitable compounds as the monomer (Y) are the same as those of (b1) above, and n-butyl(meth)acrylate is particularly preferred.
[0139] Here, all of the alkyl (meth)acrylate (c1) contained in the acrylic polymer (C0) may be the monomer (Y), but it is preferable that a part of it is the monomer (Y).
[0140] The functional group-containing monomer (c2) is preferably a monomer having a functional group such as a hydroxy group, a carboxy group, an epoxy group, an amino group, a cyano group, a nitrogen atom-containing ring group, or an alkoxysilyl group. Among these, at least one selected from a hydroxy group-containing monomer, a carboxy group-containing monomer, and an epoxy group-containing monomer is preferred. Specific examples of these compounds include the same compounds as those exemplified as the component (a2).
[0141] As the functional group-containing monomer (c2), a hydroxy group-containing monomer is preferable, and among them, various hydroxyalkyl (meth)acrylates such as 2-hydroxyethyl (meth)acrylate are more preferable. By using the hydroxyalkyl (meth)acrylate, it becomes possible to react the acrylic polymer (C0) with the energy ray curable material (Xc) relatively easily.
[0142] In addition, the functional groups in the functional group-containing monomer (b2) used in the acrylic polymer (B) and the functional group-containing monomer (c2) used in the acrylic polymer (C) may be the same or different, but are preferably different. That is, for example, if the functional group-containing monomer (b2) is a carboxyl group-containing monomer, the functional group-containing monomer (c2) is preferably a hydroxyl group-containing monomer. In this way, when the functional groups are different from each other, for example, it is possible to preferentially crosslink the acrylic polymer (C) with a crosslinking agent described later, which makes it easier to improve the retention performance of the above-mentioned workpiece processing protection sheet.
[0143] The content of the structural unit derived from the functional group-containing monomer (c2) in the acrylic polymer (C0) is preferably 5 to 40% by mass, more preferably 15 to 35% by mass, and even more preferably 20 to 32% by mass, based on the total structural units (100% by mass) of the acrylic copolymer (C0). If it is 5% by mass or more, a relatively large number of reaction sites with the energy ray curable material (Xc) can be secured, and it becomes easy to introduce the energy polymerizability into the side chain. Also, if it is 40% by mass or less, it becomes easier to set the shear storage modulus (G2') and tanδ2 / tanδ1 in the above-mentioned range.
[0144] The acrylic polymer (C0) may be a copolymer of an alkyl (meth)acrylate (c1) and a functional group-containing monomer (c2), or may be a copolymer of a (c1) component, a (c2) component, and a monomer (c3) other than the (c1) and (c2) components.
[0145] Examples of the other monomer (c3) include (meth)acrylates having a cyclic structure such as cyclohexyl (meth)acrylate, benzyl (meth)acrylate, isobornyl (meth)acrylate, dicyclopentanyl (meth)acrylate, dicyclopentenyl (meth)acrylate, and dicyclopentenyloxyethyl (meth)acrylate, as well as vinyl acetate and styrene.
[0146] The content of the structural units derived from the other monomer (c3) in the acrylic polymer (C0) is preferably 0 to 8 mass%, more preferably 0 to 4 mass%, and even more preferably 0 to 2 mass%, relative to all structural units (100 mass%) of the acrylic polymer (C0).
[0147] The energy ray-curable substance (Xc) is a compound having an energy ray-curable group and a substituent (hereinafter also simply referred to as a "reactive substituent") capable of reacting with a functional group in a structural unit derived from the component (c2) of the acrylic polymer (C0).
[0148] As described above, examples of the energy ray-curable group include a (meth)acryloyl group and a vinyl group, and a (meth)acryloyl group is preferred. The energy ray-curable substance (Xc) is preferably a compound having 1 to 5 energy ray-curable groups per molecule.
[0149] The reactive substituent in the energy ray curable substance (Xc) may be appropriately changed depending on the functional group possessed by the functional group-containing monomer (c2), and may be, for example, an isocyanate group, a carboxyl group, an epoxy group, etc., with the isocyanate group being preferred from the viewpoint of reactivity, etc. If the energy ray curable substance (Xc) has an isocyanate group, for example, when the functional group of the functional group-containing monomer (c2) is a hydroxyl group, it becomes possible for the substance to easily react with the acrylic polymer (C0).
[0150] Specific examples of the energy ray curable substance (Xc) include (meth)acryloyloxyethyl isocyanate, meta-isopropenyl-α,α-dimethylbenzyl isocyanate, (meth)acryloyl isocyanate, allyl isocyanate, glycidyl (meth)acrylate, (meth)acrylic acid, etc. These energy ray curable substances (Xc) may be used alone or in combination of two or more kinds.
[0151] Among these, (meth)acryloyloxyethyl isocyanate is preferred from the viewpoint of having a suitable isocyanate group as the reactive substituent and being a compound in which the distance between the main chain and the energy ray-curable group is appropriate.
[0152] In the energy ray curable substance (Xc), preferably 50 to 95 equivalents, more preferably 60 to 90 equivalents, and even more preferably 70 to 85 equivalents are reacted with the functional groups of the functional group-containing monomer (c2) in the acrylic polymer (C) out of the total amount (100 equivalents) of functional groups. If the amount is 50 equivalents or more, it becomes easier to set the shear storage modulus (G2') and tan δ2 / tan δ1 in the above-mentioned ranges.
[0153] In the intermediate layer composition, the content of the acrylic polymer (C) is preferably 5 to 50 mass % relative to the total amount (100 mass %) of the intermediate layer composition, more preferably 10 to 47 mass %, and even more preferably 20 to 43 mass %. By making the content of the acrylic polymer (C) relatively small in this manner, the stress relaxation property of the intermediate layer is improved, resulting in an intermediate layer with high conformability to height differences.
[0154] Furthermore, when the content of the acrylic polymer (C) is reduced, the shear storage modulus of the intermediate layer after energy ray curing does not become so high, making it possible to reduce the difference in the shear storage modulus described above, and making it easier to prevent delamination.
[0155] (4.3.3. Crosslinking Agents) The intermediate layer composition preferably further contains a crosslinking agent. Examples of the crosslinking agent include isocyanate-based crosslinking agents, epoxy-based crosslinking agents, aziridine-based crosslinking agents, and metal chelate-based crosslinking agents, and among these, isocyanate-based crosslinking agents are preferred. When an isocyanate-based crosslinking agent is used, for example, when the acrylic polymer (C) has a hydroxyl group, the crosslinking agent preferentially crosslinks the acrylic polymer (C).
[0156] The composition for the intermediate layer is crosslinked by the crosslinking agent, for example, by heating after application. The intermediate layer is formed by appropriately forming a coating film by crosslinking the acrylic polymer, particularly the low molecular weight acrylic polymer (C), etc., and the intermediate layer is easily able to function as an intermediate layer.
[0157] The content of the crosslinking agent is preferably 0.1 to 10 parts by mass, more preferably 0.15 to 6 parts by mass, and further preferably 0.2 to 3 parts by mass, based on 100 parts by mass of the total amount of the acrylic polymer (B) and the acrylic polymer (C). If the content is 10 parts by mass or less, it becomes easier to set the shear storage modulus (G2') and tan δ2 / tan δ1 in the above-mentioned ranges.
[0158] Examples of the isocyanate crosslinking agent include polyisocyanate compounds. Specific examples of the polyisocyanate compound include aromatic polyisocyanates such as tolylene diisocyanate, diphenylmethane diisocyanate, and xylylene diisocyanate, aliphatic polyisocyanates such as hexamethylene diisocyanate, and alicyclic polyisocyanates such as isophorone diisocyanate and hydrogenated diphenylmethane diisocyanate. In addition, biuret and isocyanurate forms of these compounds, as well as adducts which are reactants with low-molecular active hydrogen-containing compounds such as ethylene glycol, propylene glycol, neopentyl glycol, trimethylolpropane, and castor oil, are also included.
[0159] These may be used alone or in combination of two or more. Among the above, an adduct of an aromatic polyisocyanate such as tolylene diisocyanate with a polyhydric alcohol (for example, trimethylolpropane) is preferred.
[0160] Examples of epoxy crosslinking agents include 1,3-bis(N,N'-diglycidylaminomethyl)cyclohexane, N,N,N',N'-tetraglycidyl-m-xylylenediamine, ethylene glycol diglycidyl ether, 1,6-hexanediol diglycidyl ether, trimethylolpropane diglycidyl ether, diglycidylaniline, diglycidylamine, etc. These may be used alone or in combination of two or more.
[0161] Examples of metal chelate crosslinking agents include compounds in which acetylacetone, ethyl acetoacetate, tris(2,4-pentanedionate), etc. are coordinated to polyvalent metals such as aluminum, iron, copper, zinc, tin, titanium, nickel, antimony, magnesium, vanadium, chromium, zirconium, etc. These may be used alone or in combination of two or more.
[0162] Examples of the aziridine crosslinking agent include diphenylmethane-4,4'-bis(1-aziridinecarboxamide), trimethylolpropane tri-β-aziridinylpropionate, tetramethylolmethane tri-β-aziridinylpropionate, toluene-2,4-bis(1-aziridinecarboxamide), triethylenemelamine, bisisophthaloyl-1-(2-methylaziridine), tris-1-(2-methylaziridine)phosphine, trimethylolpropane tri-β-(2-methylaziridine)propionate, and hexa[1-(2-methyl)-aziridinyl]triphosphatriazine.
[0163] (4.3.4. Photopolymerization initiator) The intermediate layer composition preferably further contains a photopolymerization initiator. By containing the photopolymerization initiator, the intermediate layer composition is easily cured by energy rays such as ultraviolet rays.
[0164] Examples of the photopolymerization initiator include acetophenone, 2,2-diethoxybenzophenone, 4-methylbenzophenone, 2,4,6-trimethylbenzophenone, Michler's ketone, benzoin, benzoin methyl ether, benzoin ethyl ether, benzoin isopropyl ether, benzoin isobutyl ether, benzyl diphenylsulfide, tetramethylthiuram monosulfide, benzyl dimethyl ketal, dibenzyl, diacetyl, 1-chloroanthraquinone, 2-chloroanthraquinone, 2-ethylanthraquinone, 2,2-dimethoxy-2-phenylacetophenone, 1-hydroxybenzoyl ether ... Examples of photopolymerization initiators include low molecular weight polymerization initiators such as 2-methyl-1-[4-(methylthio)phenyl]-2-morpholinopropanone-1,2-benzyl-2-dimethylamino-1-(4-morpholinophenyl)-butanone-1,2-hydroxy-2-methyl-1-phenyl-propan-1-one, diethylthioxanthone, isopropylthioxanthone, and 2,4,6-trimethylbenzoyldiphenyl-phosphine oxide, and oligomerized polymerization initiators such as oligo{2-hydroxy-2-methyl-1-[4-(1-methylvinyl)phenyl]propanone}. These photopolymerization initiators may be used alone or in combination of two or more. Among these, 1-hydroxycyclohexyl-phenyl ketone is preferred.
[0165] The content of the photopolymerization initiator is usually 1 to 8 mass% relative to the total amount (100 mass%) of the intermediate layer composition. However, in order to set the shear storage modulus of the intermediate layer within the above range, it is better to make the content relatively small, preferably 1.5 to 6 mass%, and more preferably 2 to 4 mass%.
[0166] The intermediate layer composition may contain other additives within the range that does not impair the effects of the present invention. Examples of other additives include antioxidants, softeners (plasticizers), fillers, rust inhibitors, pigments, dyes, tackifiers, etc. When these additives are contained, the content of each additive is preferably 0.01 to 6 parts by mass, more preferably 0.01 to 2 parts by mass, based on 100 parts by mass of the acrylic polymer (B).
[0167] (5.Buffer layer) The buffer layer is a layer formed on the main surface of the substrate opposite to the main surface on which the adhesive layer and the intermediate layer are formed. The buffer layer is a soft layer compared to the substrate, and relieves the stress generated during back grinding of the workpiece. The buffer layer may be formed directly on the substrate, but as described above, when other layers such as an easy-adhesion layer are provided on the substrate, the buffer layer is formed on the other layers. The buffer layer may be composed of one layer (single layer), or may be composed of two or more layers. When the buffer layer has multiple layers, these multiple layers may be the same or different from each other, and the combination of layers constituting these multiple layers is not particularly limited.
[0168] In this embodiment, the thickness of the buffer layer is 10 μm or more and 100 μm or less. When the thickness of the buffer layer is within the above range, the buffer layer tends to exhibit the functions described below. The thickness of the buffer layer is preferably 25 μm or more and 85 μm or less, and more preferably 40 μm or more and 75 μm or less. The thickness of the buffer layer means the thickness of the entire buffer layer. For example, the thickness of a buffer layer composed of multiple layers means the total thickness of all layers that make up the buffer layer.
[0169] When the workpiece to which the protective sheet for workpiece processing is attached is ground on the suction table, the protective sheet for workpiece processing is placed on the suction table so that the buffer layer of the protective sheet for workpiece processing comes into contact with the suction table, and in this embodiment, since the buffer layer has the following physical properties, the buffer layer is sufficiently adsorbed to the suction table, and the protective sheet for workpiece processing and the workpiece are firmly fixed. As a result, the free movement of the group of workpiece individual pieces is suppressed, and cracks caused by collisions between the individual pieces of the workpiece can be suppressed.
[0170] (5.1. Tensile storage modulus of the buffer layer) In this embodiment, the tensile storage modulus (E') of the buffer layer at 25°C is 250 MPa or less. The tensile storage modulus is an index of the ease of deformation (hardness) of the buffer layer. In addition, when the buffer layer is energy ray curable, E' is the tensile storage modulus after irradiation with energy rays.
[0171] The workpiece processing protective sheet is usually attached to the surface of the workpiece at near room temperature, and then fixed to the suction table for back grinding. Since E' is within the above range, the buffer layer is appropriately deformed by suction and is sufficiently fixed to the suction table. Therefore, the workpiece processing protective sheet on which the buffer layer is formed and the workpiece to which the workpiece processing protective sheet is attached are also sufficiently fixed to the suction table. As a result, even if the workpiece is thinned by back grinding and the workpiece is bent, diced, etc., the movement of the workpiece diced group is suppressed, and collisions can be suppressed. Such collisions are likely to occur at the periphery of the workpiece diced group, so edge cracks can be effectively suppressed.
[0172] The tensile storage modulus (E') of the buffer layer at 25° C. is preferably 200 MPa or less, and more preferably 170 MPa or less. On the other hand, the lower limit of the tensile storage modulus (E') of the buffer layer at 25° C. is not particularly limited as long as the effects of the present invention can be obtained, but is, for example, 100 MPa or more.
[0173] The tensile storage modulus of the buffer layer can be adjusted by the amount of the energy ray curable compound to be described later, the amount of the energy ray curable group contained in the energy ray curable compound, etc. For example, the modulus tends to increase when the amount of the energy ray curable compound or the amount of the energy ray curable group is increased. In addition, the modulus can be appropriately adjusted by the amount of the crosslinking agent and the amount of the photopolymerization initiator to be incorporated in the buffer layer.
[0174] The tensile storage modulus of the buffer layer can be measured as follows. First, the material constituting the buffer layer is used as a measurement sample of a predetermined size. When the buffer layer is energy ray curable, the material constituting the buffer layer after irradiation with energy rays is used as the measurement sample. A dynamic viscoelasticity measuring device is used to apply a strain to the measurement sample at a predetermined frequency within a predetermined temperature range to measure the elastic modulus of the measurement sample. The tensile storage modulus of the buffer layer at 25°C is calculated from the measured elastic modulus. Details of the measurement will be described in the examples.
[0175] (5.2. Composition of the buffer layer) The buffer layer is not particularly limited as long as it is made of a material that satisfies the above-mentioned physical properties. For example, the buffer layer may be a layer formed from a buffer layer composition containing an energy ray curable compound, or may be made of a film such as a polypropylene film, an ethylene-vinyl acetate copolymer film, an ionomer resin film, an ethylene-(meth)acrylic acid copolymer film, an ethylene-(meth)acrylic acid ester copolymer film, an LDPE film, or an LLDPE film.
[0176] (5.3. Composition for forming buffer layer) In this embodiment, the buffer layer is preferably a layer formed from a buffer layer-forming composition containing an energy ray curable compound. The buffer layer-forming composition containing an energy ray curable compound is cured by being irradiated with energy rays to form a buffer layer (cured product). The content ratio of each polymer unit in the buffer layer usually corresponds to the ratio (feed ratio) of each component constituting the buffer layer-forming composition.
[0177] More specifically, the buffer layer forming composition containing the energy ray curable compound preferably contains urethane (meth)acrylate (d1), and more preferably contains an energy ray curable compound (d3) having an alicyclic group or heterocyclic group having 6 to 20 ring atoms and an energy ray curable compound (d4) having a functional group. The buffer layer forming composition may contain a polyfunctional energy ray curable compound (d2) in addition to the above components (d1), (d3) and (d4). The buffer layer forming composition may contain an energy ray curable compound (d5) other than the components (d1) to (d4) and a photopolymerization initiator in addition to the above components. The buffer layer forming composition may contain other additives within the range that does not impair the effects of the present invention.
[0178] Hereinafter, each component contained in the buffer layer-forming composition containing the energy ray-curable compound will be described in detail.
[0179] (5.3.1 Urethane (meth)acrylates (d1)) The urethane (meth)acrylate (d1) is a compound having at least a (meth)acryloyl group and a urethane bond, and has the property of being polymerized and cured by irradiation with energy rays. The urethane (meth)acrylate (d1) is an oligomer or a polymer.
[0180] The weight average molecular weight (Mw) of component (d1) is preferably 1,000 to 100,000, more preferably 2,000 to 60,000, and even more preferably 3,000 to 20,000. The number of (meth)acryloyl groups in component (d1) (hereinafter also referred to as "functionality") may be monofunctional, bifunctional, or trifunctional or higher, but is preferably monofunctional or bifunctional.
[0181] Component (d1) can be obtained, for example, by reacting a polyol compound with a polyisocyanate compound to obtain a terminal isocyanate urethane prepolymer, and then reacting a (meth)acrylate having a hydroxyl group. Component (d1) may be used alone or in combination of two or more kinds.
[0182] The polyol compound used as the raw material of component (d1) is not particularly limited as long as it has two or more hydroxyl groups. It may be any of a difunctional diol, a trifunctional triol, and a polyol having four or more functional groups, but a difunctional diol is preferred, and a polyester type diol or a polycarbonate type diol is more preferred.
[0183] Examples of the polyisocyanate compound include aliphatic polyisocyanates such as tetramethylene diisocyanate, hexamethylene diisocyanate, and trimethylhexamethylene diisocyanate; alicyclic diisocyanates such as isophorone diisocyanate, norbornane diisocyanate, dicyclohexylmethane-4,4'-diisocyanate, dicyclohexylmethane-2,4'-diisocyanate, and ω,ω'-diisocyanate dimethylcyclohexane; and aromatic diisocyanates such as 4,4'-diphenylmethane diisocyanate, tolylene diisocyanate, xylylene diisocyanate, tolidine diisocyanate, tetramethylene xylylene diisocyanate, and naphthalene-1,5-diisocyanate.
[0184] Among these, isophorone diisocyanate, hexamethylene diisocyanate, and xylylene diisocyanate are preferred.
[0185] The above-mentioned polyol compound is reacted with a polyisocyanate compound to give a terminal isocyanate urethane prepolymer, and then a hydroxyl group-containing (meth)acrylate is reacted with the urethane (meth)acrylate (d1). The hydroxyl group-containing (meth)acrylate is not particularly limited as long as it is a compound having a hydroxyl group and a (meth)acryloyl group in at least one molecule.
[0186] Specific examples of (meth)acrylates having a hydroxy group include hydroxyalkyl (meth)acrylates such as 2-hydroxyethyl (meth)acrylate, 2-hydroxypropyl (meth)acrylate, 4-hydroxybutyl (meth)acrylate, 4-hydroxycyclohexyl (meth)acrylate, 5-hydroxycyclooctyl (meth)acrylate, 2-hydroxy-3-phenyloxypropyl (meth)acrylate, pentaerythritol tri(meth)acrylate, polyethylene glycol mono(meth)acrylate, and polypropylene glycol mono(meth)acrylate; hydroxy group-containing (meth)acrylamides such as N-methylol (meth)acrylamide; and reaction products obtained by reacting a diglycidyl ester of vinyl alcohol, vinylphenol, or bisphenol A with (meth)acrylic acid; and the like.
[0187] Among these, hydroxyalkyl (meth)acrylate is preferred, and 2-hydroxyethyl (meth)acrylate is more preferred.
[0188] The conditions for reacting the isocyanate-terminated urethane prepolymer and the (meth)acrylate having a hydroxyl group are preferably such that the reaction is carried out at 60 to 100° C. for 1 to 4 hours in the presence of a solvent and a catalyst, which are added as necessary.
[0189] The content of component (d1) in the buffer layer forming composition is preferably 20 to 80 mass%, more preferably 30 to 70 mass%, and even more preferably 40 to 65 mass%, relative to the total amount (100 mass%) of the buffer layer forming composition.
[0190] (5.3.2 Multifunctional energy ray-curable compound (d2)) The polyfunctional energy ray curable compound refers to a compound other than component (d1) having two or more energy ray curable unsaturated groups. The energy ray curable unsaturated group is a functional group containing a carbon-carbon double bond, and examples thereof include a (meth)acryloyl group, a vinyl group, an allyl group, and a vinylbenzyl group. Two or more types of energy ray curable unsaturated groups may be combined. A three-dimensional network structure (crosslinked structure) is formed by reacting an energy ray curable unsaturated group in the polyfunctional energy ray curable compound with an energy ray curable unsaturated group in component (d1) or by reacting energy ray curable unsaturated groups in component (d2) with each other. When a polyfunctional energy ray curable compound is used, the number of crosslinked structures formed by energy ray irradiation increases compared to when a compound containing only one energy ray curable unsaturated group is used, so that the buffer layer exhibits unique viscoelasticity, and it becomes easier to relieve stress during back grinding.
[0191] In addition, although there is some overlap between the definition of component (d2) and the definition of component (d3) or component (d4) described later, the overlapping parts are included in component (d2). For example, a compound having an alicyclic group or heterocyclic group with 6 to 20 ring atoms and having two or more energy ray-curable unsaturated groups is included in the definitions of both component (d2) and component (d3), but in the present invention, the compound is included in component (d2). In addition, a compound containing a functional group such as a hydroxyl group, an epoxy group, an amide group, or an amino group and having two or more energy ray-curable unsaturated groups is included in the definitions of both component (d2) and component (d4), but in the present invention, the compound is included in component (d2).
[0192] From the above viewpoints, the number of energy ray-curable unsaturated groups (number of functional groups) in the polyfunctional energy ray-curable compound is preferably 2 to 10, and more preferably 3 to 6.
[0193] The weight average molecular weight of the component (d2) is preferably 30-40,000, more preferably 100-10,000, and even more preferably 200-1,000.
[0194] Specific examples of component (d2) include diethylene glycol di(meth)acrylate, ethylene glycol di(meth)acrylate, tetraethylene glycol di(meth)acrylate, neopentyl glycol di(meth)acrylate, 1,6-hexanediol di(meth)acrylate, trimethylolpropane tri(meth)acrylate, pentaerythritol tri(meth)acrylate, pentaerythritol tetra(meth)acrylate, dipentaerythritol hexa(meth)acrylate, divinylbenzene, vinyl (meth)acrylate, divinyl adipate, and N,N'-methylenebis(meth)acrylamide. Among these, dipentaerythritol hexa(meth)acrylate is preferred. Note that component (d2) may be used alone or in combination of two or more.
[0195] The content of component (d2) in the buffer layer forming composition is preferably 0 to 30 mass%, more preferably 0 to 20 mass%, and even more preferably 0 to 10 mass%, relative to the total amount (100 mass%) of the buffer layer forming composition.
[0196] (5.3.3 Energy ray-curable compound (d3) having an alicyclic group or heterocyclic group having 6 to 20 ring atoms) Component (d3) is an energy ray curable compound other than component (d1) that has an alicyclic group or a heterocyclic group having 6 to 20 ring atoms, and is preferably a compound having at least one (meth)acryloyl group, more preferably a compound having one (meth)acryloyl group. By using component (d3), the film formability of the obtained buffer layer forming composition can be improved.
[0197] The definition of component (d3) overlaps with the definition of component (d4) described below, but the overlapping portion is included in component (d4). For example, a compound having at least one (meth)acryloyl group, an alicyclic group or heterocyclic group having 6 to 20 ring atoms, and a functional group such as a hydroxyl group, an epoxy group, an amide group, or an amino group is included in the definitions of both component (d3) and component (d4), but in the present invention, the compound is included in component (d4).
[0198] Specific examples of the component (d3) include alicyclic group-containing (meth)acrylates such as isobornyl (meth)acrylate, dicyclopentenyl (meth)acrylate, dicyclopentanyl (meth)acrylate, dicyclopentenyloxy (meth)acrylate, cyclohexyl (meth)acrylate, and adamantane (meth)acrylate; heterocyclic group-containing (meth)acrylates such as tetrahydrofurfuryl (meth)acrylate and morpholine (meth)acrylate; etc. The component (d3) may be used alone or in combination of two or more kinds.
[0199] Of the alicyclic group-containing (meth)acrylates, isobornyl (meth)acrylate is preferred, and of the heterocyclic group-containing (meth)acrylates, tetrahydrofurfuryl (meth)acrylate is preferred.
[0200] The content of component (d3) in the buffer layer forming composition is preferably 10 to 60 mass%, more preferably 20 to 55 mass%, and even more preferably 25 to 50 mass%, relative to the total amount (100 mass%) of the buffer layer forming composition.
[0201] (5.3.4 Energy ray-curable compound having a functional group (d4)) Component (d4) is an energy ray-curable compound other than component (d1) that contains a functional group such as a hydroxyl group, an epoxy group, an amide group, or an amino group, and is preferably a compound having at least one (meth)acryloyl group, more preferably a compound having one (meth)acryloyl group.
[0202] The component (d4) has good compatibility with the component (d1), and the viscosity of the buffer layer-forming composition can be easily adjusted to an appropriate range. In addition, the buffer layer has good buffer performance even if it is relatively thin.
[0203] Examples of the component (d4) include hydroxyl group-containing (meth)acrylates, epoxy group-containing compounds, amide group-containing compounds, amino group-containing (meth)acrylates, etc. Among these, hydroxyl group-containing (meth)acrylates are preferred.
[0204] Examples of hydroxyl group-containing (meth)acrylates include 2-hydroxyethyl (meth)acrylate, 2-hydroxypropyl (meth)acrylate, 3-hydroxypropyl (meth)acrylate, 2-hydroxybutyl (meth)acrylate, 3-hydroxybutyl (meth)acrylate, 4-hydroxybutyl (meth)acrylate, phenylhydroxypropyl (meth)acrylate, and 2-hydroxy-3-phenoxypropyl acrylate. Among these, 2-hydroxypropyl (meth)acrylate and 3-hydroxypropyl (meth)acrylate are more preferred. The component (d4) may be used alone or in combination of two or more.
[0205] In order to improve the film-forming properties of the buffer layer-forming composition, the content of component (d4) in the buffer layer-forming composition is preferably 0 to 30 mass %, more preferably 1 to 20 mass %, and even more preferably 2 to 10 mass %, relative to the total amount (100 mass %) of the buffer layer-forming composition.
[0206] (5.3.5 Energy ray-curable compound (d5) other than components (d1) to (d4)) The buffer layer-forming composition may contain an energy ray-curable compound (d5) other than the above components (d1) to (d4) within the range that does not impair the effects of the present invention.
[0207] Examples of the component (d5) include alkyl (meth)acrylates having an alkyl group having 1 to 20 carbon atoms, and vinyl compounds such as styrene, hydroxyethyl vinyl ether, hydroxybutyl vinyl ether, N-vinyl formamide, N-vinyl pyrrolidone, and N-vinyl caprolactam. The component (d5) may be used alone or in combination of two or more kinds.
[0208] The content of component (d5) in the buffer layer forming composition is preferably 0 to 20 mass%, more preferably 0 to 10 mass%, even more preferably 0 to 5 mass%, and particularly preferably 0 to 2 mass%, relative to the total amount (100 mass%) of the buffer layer forming composition.
[0209] 5.3.6 Photoinitiators It is preferable that the buffer layer-forming composition further contains a photopolymerization initiator from the viewpoints of shortening the polymerization time by light irradiation and reducing the amount of light irradiation when forming the buffer layer.
[0210] Examples of photopolymerization initiators include benzoin compounds, acetophenone compounds, acylphosphinoxide compounds, titanocene compounds, thioxanthone compounds, peroxide compounds, and photosensitizers such as amines and quinones. More specifically, examples of photopolymerization initiators include 1-hydroxycyclohexyl-phenyl ketone, 2-hydroxy-2-methyl-1-phenyl-propan-1-one, benzoin, benzoin methyl ether, benzoin ethyl ether, benzoin isopropyl ether, benzyl phenyl sulfide, tetramethylthiuram monosulfide, azobisisobutyrolnitrile, dibenzyl, diacetyl, 8-chloroanthraquinone, and bis(2,4,6-trimethylbenzoyl)phenylphosphine oxide. These photopolymerization initiators may be used alone or in combination of two or more. Among these, 2-hydroxy-2-methyl-1-phenyl-propan-1-one is preferred.
[0211] The content of the photopolymerization initiator in the buffer layer forming composition is preferably 0.1 to 10 parts by mass, more preferably 0.5 to 7 parts by mass, and even more preferably 0.8 to 4 parts by mass, relative to 100 parts by mass of the total amount of the buffer layer forming composition.
[0212] 5.3.7 Other Additives The buffer layer forming composition may contain other additives within the range that does not impair the effects of the present invention. Examples of other additives include antistatic agents, antioxidants, softeners (plasticizers), fillers, rust inhibitors, pigments, dyes, etc. When these additives are blended, the content of each additive in the buffer layer forming composition is preferably 0.01 to 6 parts by mass, more preferably 0.1 to 3 parts by mass, based on 100 parts by mass of the total amount of the energy ray curable compounds.
[0213] (6. Manufacturing method of protective sheet for workpiece processing) The method for manufacturing the protective sheet for workpiece processing according to the present embodiment can be a known method, for example, a method in which an intermediate layer and an adhesive layer are formed on one main surface of a substrate, and a buffer layer is formed on the other main surface of the substrate.
[0214] First, as a composition for forming a pressure-sensitive adhesive layer, for example, a composition for a pressure-sensitive adhesive layer or a coating liquid obtained by diluting the composition for a pressure-sensitive adhesive layer with a solvent is prepared. Similarly, as a composition for forming an intermediate layer, for example, a composition for an intermediate layer or a coating liquid obtained by diluting the composition for an intermediate layer with a solvent is prepared. Similarly, as a composition for forming a buffer layer, for example, a composition for forming a buffer layer or a coating liquid obtained by diluting the composition for forming a buffer layer with a solvent is prepared.
[0215] Examples of the solvent include organic solvents such as methyl ethyl ketone, acetone, ethyl acetate, tetrahydrofuran, dioxane, cyclohexane, n-hexane, toluene, xylene, n-propanol, and isopropanol.
[0216] Then, for example, the buffer layer-forming composition or a coating solution thereof is applied to the release-treated surface of the first release sheet by a known method such as spin coating, spray coating, bar coating, knife coating, roll coating, blade coating, die coating, gravure coating, etc., and dried as necessary to form a coating film, which is then semi-cured to form a buffer layer-forming film on the first release sheet. The buffer layer-forming film formed on the first release sheet is attached to a substrate, and the buffer layer-forming film is completely cured to form a buffer layer.
[0217] In the above, the process sequence is shown in which the buffer layer-forming composition or its coating liquid is applied to the first release sheet and then the substrate is laminated thereto. However, the buffer layer may also be formed on the substrate by the reverse process sequence, i.e., by applying the buffer layer-forming composition or its coating liquid to the substrate and then laminating the first release sheet thereto.
[0218] In this embodiment, the coating film is preferably cured by irradiation with energy rays. The energy rays for semi-curing are preferably ultraviolet rays, and the illuminance thereof is 60 to 320 mW / cm. 2 The light intensity is preferably 30 to 1000 mJ / cm. 2 The energy ray for complete curing is preferably ultraviolet light, and the illuminance is preferably 80 to 400 mW / cm. 2 The light intensity is preferably 200 to 1500 mJ / cm 2 The curing of the coating film may be carried out in a single curing treatment, or may be carried out in several separate steps.
[0219] Next, the intermediate layer composition or its coating liquid is applied to the release-treated surface of the second release sheet by a known method, and if necessary, heated and dried to form an intermediate layer on the second release sheet. Thereafter, the intermediate layer on the second release sheet and the surface of the substrate on which the buffer layer is not formed are bonded together, and the second release sheet is removed.
[0220] Next, the adhesive layer composition or its coating liquid is applied to the release-treated surface of the third release sheet by a known method, and if necessary, heated and dried to form an adhesive layer on the third release sheet. Then, the adhesive layer on the third release sheet and the intermediate layer on the substrate are laminated together to obtain a workpiece processing protective sheet in which the intermediate layer and the adhesive layer are formed in this order on one main surface of the substrate, and a buffer layer is formed on the other main surface of the substrate. Then, the first release sheet is removed. The third release sheet may be removed when the workpiece processing protective sheet is used.
[0221] (7. Method for manufacturing workpieces) As described above, the protective sheet for workpiece processing according to the present invention is preferably used in a method for applying DBG or LDBG to a workpiece having a height difference on its surface to separate the workpiece. As a non-limiting example of the use of the protective sheet for workpiece processing, a method for producing a workpiece separated product will be described in more detail below.
[0222] Specifically, the method for producing a workpiece singulated product according to this embodiment includes at least the following steps 1 to 4. Step 1: A step of attaching the above-mentioned protective sheet for workpiece processing to the surface of a workpiece having a front surface and a back surface opposite to the front surface. Step 2: forming a groove on the surface of the workpiece, or forming a modified region inside the workpiece Step 3: A step of grinding the workpiece having a protective sheet for workpiece processing attached to its surface and having grooves or modified regions formed thereon from its back surface to separate the workpiece into a plurality of workpiece pieces starting from the grooves or modified regions. Step 4: A step of peeling off the protective sheet for workpiece processing from the plurality of workpieces.
[0223] Each step of the manufacturing method of the above-mentioned workpiece singulation will be described in detail below. In the following description, the surface of the workpiece has height differences, and a chip-on-wafer is used as a specific example. In this case, a specific example of the workpiece singulation is, for example, a stacked chip.
[0224] (Process 1) In step 1, as shown in Fig. 3, the adhesive layer of the protective sheet for workpiece processing 1 according to this embodiment is attached to the surface 50a of the chip-on-wafer 50. In the chip-on-wafer 50, a plurality of chips 52 are arranged on the surface of the wafer 51. However, since the physical properties of each layer constituting the protective sheet for workpiece processing are optimized, the adhesive layer and the intermediate layer can well conform to the steps between the chips, and the plurality of chips can be sufficiently embedded and fixed.
[0225] (Process 2) In step 2, grooves are formed on the surface of the chip-on-wafer. Alternatively, modified regions are formed inside the chip-on-wafer. In step 2, the grooves and modified regions are formed so as to follow the dividing lines that will be formed when the wafer is divided into individual pieces in step 3, which will be described later.
[0226] The grooves formed in step 2 are shallower than the thickness of the wafer. The grooves can be formed by dicing using a known wafer dicing device or the like. In addition, when the grooves are formed, step 2 is performed before step 1.
[0227] In addition, the modified region formed in process 2 is an embrittled portion inside the wafer, and is the starting point for the modified region of the wafer to be destroyed and diced into chips due to the thinning of the wafer caused by grinding in the grinding process or the application of grinding force.
[0228] The modified region is formed by irradiating a laser focused on the inside of the wafer, and the modified region is formed inside the wafer. The laser may be irradiated from the front side or the back side of the wafer. In the embodiment in which the modified region is formed, when the step 2 is performed after the step 1 and the laser is irradiated from the front side of the wafer, the laser is irradiated to the wafer through the protective sheet for workpiece processing.
[0229] The chip-on-wafer with the workpiece processing protective sheet attached and the grooves or modified regions formed thereon is placed on the suction table with the front side thereof, and is held by the suction table. Since the workpiece processing protective sheet is attached to the front side of the chip-on-wafer, the buffer layer of the workpiece processing protective sheet is placed on the suction table side and is suctioned. At this time, since the physical properties of each layer constituting the workpiece processing protective sheet are optimized, the buffer layer is appropriately deformed by suction, and the entire workpiece processing protective sheet, including the workpiece processing protective sheet near the peripheral portion (edge), is well fixed to the suction table.
[0230] (Step 3) After steps 1 and 2, the back surface of the chip-on-wafer on the suction table is ground to separate the chip-on-wafer into a plurality of individual pieces (a stacked chip group).
[0231] Here, when grooves are formed in the wafer, the back grinding is performed so as to thin the wafer at least to the position where the bottom of the groove is reached. By this back grinding, the grooves become cuts penetrating the wafer, and the wafer is divided by the cuts to obtain a group of workpieces (stacked chips).
[0232] At this time, the physical properties and thickness of the adhesive layer and intermediate layer of the workpiece processing protection sheet are controlled within the above-mentioned range, so that the adhesive layer and intermediate layer sufficiently embed and fix each chip. Therefore, even if the wafer is thinned by the back grinding, the bending of the wafer can be suppressed, or even if the wafer is divided into individual pieces and becomes a stacked chip group, the collision between the stacked chips can be suppressed. As described above, such a collision is likely to occur at the periphery of the wafer, but the crack (edge crack) caused by the collision can be suppressed.
[0233] In addition, since the physical properties of the base material of the protective sheet for workpiece processing are controlled within the above-mentioned range, uneven vibrations do not occur even during back grinding, and the wafer and stacked chip group can be stably held, so that even if the wafer is thinned and divided into individual pieces, bending of the wafer, collisions between stacked chips, etc. can be suppressed. In other words, edge cracks can be suppressed.
[0234] Furthermore, since the physical properties and thickness of the buffer layer of the workpiece processing protective sheet are controlled within the above-mentioned ranges, even if stress is applied to the wafer during back grinding, the workpiece processing protective sheet and the wafer to which the workpiece processing protective sheet is attached are sufficiently fixed and held on the suction table, so that even if the wafer is thinned and divided into individual pieces, bending of the wafer, collision between stacked chips, etc. can be suppressed. In other words, edge cracks can be suppressed.
[0235] In addition, when a modified region is formed, the grinding surface (wafer back surface) may reach the modified region by grinding, but it does not have to reach the modified region strictly. That is, the wafer may be divided starting from the modified region at the end of back surface grinding, or may not be divided. When divided, it is sufficient that at least a part of the wafer is divided. Even in this case, the wafer and the stacked chip group are well fixed due to the function exerted by each layer of the workpiece processing protective sheet, and bending of the wafer, collision between stacked chips, etc. can be suppressed. That is, edge cracks can be suppressed.
[0236] When back grinding is completed, the regions of the chip-on-wafer that have not been singulated may be singulated, for example, by attaching a pick-up tape (described later) and then stretching the pick-up tape.
[0237] After the back surface is ground using a grinding wheel, stress relief such as dry polishing may be performed prior to picking up the stacked chips.
[0238] The shape of the individualized laminated chips may be square or elongated, such as rectangular. The thickness of the individualized laminated chips is not particularly limited, but the thickness of the individualized wafer portion is preferably about 5 to 100 μm, more preferably 10 to 45 μm. According to LDBG, it is easy to make the thickness of the individualized laminated chips 50 μm or less, more preferably 10 to 45 μm. The size of the individualized laminated chips is not particularly limited. For example, the chip area is preferably 600 mm 2 Less than 400mm, more preferably 2 Less than 120mm, more preferably 2 is less than.
[0239] (Step 4) Next, the protective sheet for workpiece processing is peeled off from the individual chip-on-wafer (i.e., stacked chip group). This step is performed, for example, by the following method.
[0240] First, when the adhesive layer of the protective sheet for workpiece processing is energy ray curable, the adhesive layer is cured by irradiating it with energy rays. For example, the illuminance of the energy rays is 120 to 280 mW / cm 2 The amount of energy is 100-1000mJ / cm 2 The energy ray is preferably ultraviolet ray.
[0241] Next, a pick-up tape is applied to the back side of the stacked chip group, and the position and direction are adjusted so that the chips can be picked up. At this time, a ring frame located on the outer periphery of the wafer is also applied to the pick-up tape, and the outer periphery of the pick-up tape is fixed to the ring frame. The wafer and the ring frame may be applied to the pick-up tape at the same time, or may be applied at different times. Next, the protective sheet for workpiece processing is peeled off from the stacked chips held on the pick-up tape.
[0242] In step 1, when the protective sheet for workpiece processing is attached to the surface of the chip-on-wafer, if the adhesive layer is too soft, the adhesive layer may penetrate between the chips. In this case, the energy beam irradiated to peel off the sheet may not reach the adhesive layer that has penetrated too far, or the energy beam may not cure properly due to the influence of oxygen in the air. As a result, the adhesive may not cure and its adhesive strength may not decrease sufficiently. If the protective sheet for workpiece processing is peeled off in this state, the adhesive whose adhesive strength has not decreased may remain on the side of the laminated chip (glue residue).
[0243] However, by controlling the shear storage modulus (G1') of the adhesive layer to be equal to or greater than the above-mentioned lower limit, excessive penetration of the adhesive layer between the chips is suppressed, and the adhesive layer has hardness even if it is not sufficiently cured with energy rays, so that the occurrence of glue residue can be suppressed.
[0244] Thereafter, the plurality of chips on the pickup tape are picked up, and the stacked chips are then fixed onto a substrate or the like for a device to manufacture the device.
[0245] The pick-up tape is not particularly limited, but may be, for example, an adhesive sheet including a substrate and an adhesive layer provided on one surface of the substrate.
[0246] Although the embodiment of the present invention has been described above, the present invention is not limited to the above embodiment, and may be modified in various aspects within the scope of the present invention. EXAMPLES
[0247] The present invention will be described in more detail below using examples, but the present invention is not limited to these examples.
[0248] The measurement and evaluation methods in the present examples are as follows.
[0249] (Shear storage modulus and loss tangent of adhesive layer and intermediate layer) In the examples and comparative examples described below, a pressure-sensitive adhesive layer was formed on a release sheet using a pressure-sensitive adhesive layer composition. A plurality of pressure-sensitive adhesive layers thus formed were prepared, and the pressure-sensitive adhesive layers were laminated together to produce a pressure-sensitive adhesive layer laminate having a thickness of 1 mm. Similarly, an intermediate layer was formed on a release sheet using a composition for an intermediate layer, and the intermediate layers were laminated together to produce a pressure-sensitive adhesive layer laminate having a thickness of 1 mm.
[0250] The obtained laminate of the pressure-sensitive adhesive layer and the laminate of the intermediate layer were each punched out into a cylindrical shape with a diameter of 8 mm, and the release sheet was removed to prepare a sample for measuring the shear storage modulus and loss tangent.
[0251] The shear storage modulus (G1') and loss tangent (tanδ1) of the adhesive layer were measured using an Anton Paar rheometer MCR302. Both ends of the sample in the thickness direction were sandwiched between parallel plates, and the sample was twisted around the thickness direction of the sample as the axis of rotation under the following conditions: measurement temperature -30 to 100°C, gap 1 mm, strain 0.05 to 0.5%, and angular frequency 1 Hz, to apply shear force to the sample, and the shear storage modulus and shear loss modulus were measured. The shear storage modulus (G1') and loss tangent (tanδ1) at 25°C were calculated from the obtained measured values.
[0252] The shear storage modulus (G2') and loss tangent (tan δ2) of the intermediate layer were measured under the same conditions as those for the shear storage modulus (G1') and loss tangent (tan δ1) of the adhesive layer, and the shear storage modulus (G2') and loss tangent (tan δ2) at 25°C were calculated from the obtained measurements.
[0253] (Tensile storage modulus of the buffer layer) In the examples and comparative examples described below, a buffer layer having a thickness of 100 μm was formed on a release sheet using a buffer layer forming composition. The energy rays were irradiated under a nitrogen atmosphere to completely cure the layer, so as not to cause insufficient energy ray curing due to oxygen inhibition. The formed buffer layer was cut to a width of 4 mm and a length of 25 mm to prepare a sample for measuring the tensile storage modulus.
[0254] The tensile storage modulus (E') of the buffer layer was measured using a Rheovibron DDV-0.1FP manufactured by Orientec Co., Ltd. The tensile storage modulus of the above-mentioned sample for measuring the tensile storage modulus was measured in tension mode from -30°C to 100°C under the measurement conditions of a frequency of 1Hz, a chuck distance of 15mm, and a heating rate of 3°C / min. The tensile storage modulus (E') at 25°C was calculated from the obtained measurements.
[0255] (Evaluation method for edge cracks) In each of the examples and comparative examples, a circular thermosetting tape was attached to a silicon mirror wafer having a diameter of 8 inches and a thickness of 730 μm as a pseudo step layer in an area 10 mm (10,000 μm) inside from the outer periphery of the wafer so as to have a thickness of 80 μm, and heated to form a hard resin film layer. Next, using a dicing device (manufactured by DISCO, product name "DFD6361"), the wafer having the pseudo step layer was half-cut (diced) so as to form a square area of 3 mm x 3 mm in size at a depth of 150 μm from the front surface of the silicon wafer (580 μm when measured from the back surface of the silicon wafer) and under the condition of a half-cut width of 50 μm. By the half-cut processing, a pseudo chip-on-wafer in which a plurality of resin films (80 μm thick) of 3 mm x 3 mm in size were arranged on the inner periphery of the wafer was obtained.
[0256] The protective sheets for workpiece processing prepared in the examples and comparative examples were applied to the surface of a simulated chip-on-wafer (the surface on which the resin film was disposed) using a backgrind tape laminator (manufactured by Lintec Corporation, device name "RAD-3510F / 12") under conditions of an application speed of 3.0 mm / sec, application temperature at room temperature (25°C), and roller pressure of 0.35 MPa.
[0257] Then, using a back grinding machine (manufactured by Disco, machine name "DGP8760"), the back grinding was performed until the thickness of the silicon wafer became 130 μm, and pseudo chip-on-wafers were singulated. After singulation, the singulated objects present in a ring-shaped region 8 to 15 mm from the outer periphery of the wafer were observed with a digital microscope (manufactured by KEYENCE, product name "VHX-7000"), and the number of singulated objects in which cracks occurred was evaluated. Note that chips that were not square (e.g. triangular chips) were also observed, and if a crack occurred, it was counted as one chip.
[0258] (Method for evaluating adhesive residue) In each of the examples and comparative examples, three individual pseudo chip-on-wafers with a protective sheet for workpiece processing attached were prepared using the same method as the edge crack evaluation method described above. A dicing tape (manufactured by Lintec Corporation, product name "D-886H") was mounted as a pickup tape on the pseudo chip-on-wafer using a mounter (manufactured by Lintec Corporation, product name "RAD-2510F / 12") and fixed to a separately prepared ring frame. After mounting, the protective sheet for workpiece processing was irradiated with UV (illuminance: 230 mW / cm 2 , Light amount: 380mJ / cm 2 ) and then using a mounter (manufactured by Lintec Corporation, product name "RAD-2510F / 12"), the protective sheet for workpiece processing was peeled off at an angle of 45° to the dicing line. For the first pseudo chip-on-wafer, the peeling speed was set to 2 mm / sec (condition 1), for the second pseudo chip-on-wafer, the peeling speed was set to 2.5 mm / sec (condition 2), and for the third pseudo chip-on-wafer, the peeling speed was set to 4 mm / sec (condition 3).
[0259] After peeling off the protective sheet for workpiece processing, the dicing tape was irradiated with UV light, and 10 pieces were randomly picked out from the individual pieces with the resin film, and the four sides of the individual pieces were observed with a digital microscope (Keyence Corporation, product name "VHX-7000") to evaluate the presence or absence of adhesive residue. If adhesive residue was found on one or more of the 10 individual pieces, it was determined that adhesive residue had occurred. The adhesive residue after individualization was evaluated according to the following criteria. ○: No adhesive residue was observed under all three conditions. △: Adhesive residue occurred only under condition 3. ×: Adhesive residue occurred under condition 3, and adhesive residue occurred under at least one of conditions 1 and 2.
[0260] Example 1 (1) Base material First, a colorless and transparent PET film (manufactured by Toyobo Co., Ltd.) with an easy-adhesion coating layer on both sides, having a thickness of 50 μm and a Young's modulus of 2550 MPa at 25° C., was prepared as a substrate (substrate 1).
[0261] (2) Preparation of buffer layer-forming composition α A bifunctional urethane acrylate oligomer (UA-1) having a weight average molecular weight (Mw) of approximately 5,000 was obtained by reacting a terminal isocyanate urethane prepolymer obtained by reacting a polyester diol with isophorone diisocyanate with 2-hydroxyethyl acrylate.
[0262] A buffer layer-forming composition α was prepared by blending 50 parts by mass of urethane acrylate oligomer (UA-1, corresponding to component (d1)), 45 parts by mass of isobornyl acrylate (IBXA, corresponding to component (d3)), and 5 parts by mass of hydroxypropyl acrylate (HPA, corresponding to component (d4)), and further blending 1.0 part by mass of 2-hydroxy-2-methyl-1-phenyl-propan-1-one (manufactured by IGM Resins, product name "Omnirad 1173") as a photopolymerization initiator (i-1).
[0263] (3) Preparation of intermediate layer composition β A non-energy ray curable acrylic polymer (B-1) (Mw: 600,000) was obtained by copolymerizing 90 parts by mass of n-butyl acrylate (BA) and 10 parts by mass of acrylic acid (AA).
[0264] Separately from the acrylic polymer (B-1), 60 parts by mass of n-butyl acrylate (BA), 10 parts by mass of methyl methacrylate (MMA), and 30 parts by mass of 2-hydroxyethyl acrylate (2HEA) were copolymerized to obtain an acrylic polymer, which was then reacted with 2-methacryloyloxyethyl isocyanate (MOI) so as to add to 80 equivalents of the hydroxyl groups out of the total hydroxyl groups (100 equivalents) of the acrylic polymer, to obtain an energy ray-curable acrylic polymer (C-1) (Mw: 100,000).
[0265] To 100 parts by mass of non-energy ray curable acrylic polymer (B-1), 13.4 parts by mass of energy ray curable acrylic polymer (C-1), 2.35 parts by mass of an isocyanate-based crosslinking agent (manufactured by Tosoh Corporation, product name "Coronate L") as a crosslinking agent (CL-1), and 3.71 parts by mass of 1-hydroxycyclohexyl-phenyl ketone (manufactured by IGM Resins, product name "Omnirad 184") as a photopolymerization initiator (i-2) were added, and a coating liquid of intermediate layer composition β was prepared in which the solid content concentration was adjusted to 32% using methyl ethyl ketone.
[0266] (4) Preparation of Pressure-Sensitive Adhesive Layer Composition γ An energy ray-curable acrylic resin (A-1) (Mw: 200,000) was obtained by reacting an acrylic polymer obtained by copolymerizing 70 parts by mass of n-butyl acrylate (BA), 20 parts by mass of ethyl acrylate (EA), and 10 parts by mass of 2-hydroxyethyl acrylate (2HEA) with 2-methacryloyloxyethyl isocyanate (MOI) so as to add to 90 equivalents of the total hydroxyl groups (100 equivalents) of the acrylic polymer.
[0267] 100 parts by mass of this energy ray-curable acrylic copolymer (A-1) was mixed with 0.86 parts by mass of an isocyanate-based crosslinking agent (Tosoh Corporation, Coronate L) as the crosslinking agent (CL-1) and 7.3 parts by mass of 2,2-dimethoxy-2-phenylacetophenone (IGM Resins, product name "Omnirad 651") as the photopolymerization initiator (i-3), and diluted with toluene to prepare a coating liquid of adhesive layer composition γ with a solids concentration of 25% by mass.
[0268] (Production of protective sheets for workpiece processing) The prepared buffer layer-forming composition α was applied to one side of the above-mentioned substrate to form a coating film, which was then semi-cured by irradiating the coating film with ultraviolet light to form a buffer layer-forming film having a thickness of 15 μm.
[0269] The above ultraviolet irradiation was performed using a belt conveyor type ultraviolet irradiation device (manufactured by iGraphics, device name "US2-0801") and a high-pressure mercury lamp (manufactured by iGraphics, device name "H08-L41") with a lamp height of 230 mm, output of 80 W / cm, light wavelength of 365 nm, and illuminance of 90 mW / cm. 2 , irradiation light amount 50mJ / cm 2 The irradiation conditions were as follows:
[0270] Next, the surface of the formed buffer layer formation film was bonded to the release-treated surface of a first release sheet (manufactured by Lintec Corporation, product name "SP-PET381031", thickness: 38 μm), and ultraviolet light was irradiated again from the release sheet side on which the buffer layer formation film was formed (illuminance: 110 mW / cm 2 , Light intensity: 475mJ / cm 2 ) to completely cure the buffer layer-forming film, thereby forming a buffer layer having a thickness of 15 μm. This produced a first laminate having a structure of release sheet / buffer layer / substrate.
[0271] Next, a coating solution of the prepared intermediate layer composition β was applied to the release-treated surface of a second release sheet (manufactured by Lintec Corporation, product name "SP-PET381031", thickness: 38 μm), and the resulting coating was dried by heating to form an intermediate layer 60 μm thick on the release sheet.
[0272] The intermediate layer formed was attached to the surface of the substrate opposite to the surface on which the buffer layer was formed in the first laminate. The operation of laminating the intermediate layer formed on the release sheet and the intermediate layer attached to the substrate was repeated until the thickness of the intermediate layer reached 240 μm. At that time, each release sheet that was no longer needed was peeled off and removed. This resulted in a second laminate having a configuration of release sheet / buffer layer / substrate / intermediate layer (thickness: 240 μm) / release sheet.
[0273] Next, the prepared coating solution of the adhesive layer composition γ was applied to the release-treated surface of a third release sheet (manufactured by Lintec Corporation, product name "SP-PET381031", thickness: 38 μm) and dried by heating to form an adhesive layer 10 μm thick on the release sheet.
[0274] The release sheet located on the intermediate layer in the second laminate was peeled off, and the exposed intermediate layer was bonded to the adhesive layer on the release sheet to produce a protective sheet for workpiece processing having a structure of release sheet / buffer layer (thickness: 15 μm) / base material (thickness: 50 μm) / intermediate layer (thickness: 240 μm) / adhesive layer (thickness: 10 μm) / release sheet.
[0275] (Examples 2 to 5, 7, Comparative Examples 1, 2 and 5) A protective sheet for workpiece processing was obtained in the same manner as in Example 1, except that the composition and thickness of the buffer layer, the composition and thickness of the intermediate layer, and the composition and thickness of the adhesive layer were changed to the compositions or thicknesses shown in Table 1.
[0276] (Examples 6, 8 to 12) A protective sheet for workpiece processing was obtained in the same manner as in Example 2, except that the acrylic polymer (A-2) below was used instead of the acrylic polymer (A-1) in the adhesive layer composition to give the composition shown in Table 1, and the composition of the intermediate layer was the composition shown in Table 1.
[0277] An acrylic polymer was obtained by copolymerizing 60 parts by mass of 2-ethylhexyl acrylate (2EHA), 20 parts by mass of ethyl acrylate (EA), and 20 parts by mass of 2-hydroxyethyl acrylate (HEA), and 2-methacryloyloxyethyl isocyanate (MOI) was reacted with the acrylic polymer so as to add to 60 equivalents of the hydroxyl groups out of the total hydroxyl groups (100 equivalents) of the acrylic polymer, to obtain an energy ray curable acrylic polymer (A-2) (Mw: 200,000).
[0278] Comparative Example 3 A protective sheet for workpiece processing was obtained in the same manner as in Example 3, except that 50 parts by mass of a urethane acrylate oligomer (manufactured by Sartomer Corporation, CN8888) (corresponding to UA-2, component (d1)) was used instead of 50 parts by mass of the urethane acrylate oligomer (UA-1) in the buffer layer-forming composition.
[0279] Comparative Example 4 A protection sheet for workpiece processing was obtained in the same manner as in Example 2, except that a colorless, transparent, unstretched polypropylene film (substrate 2) having a thickness of 80 μm and a Young's modulus of 750 MPa at 25° C. was used as the substrate.
[0280] (Comparative Examples 6 to 9) A protective sheet for workpiece processing was obtained in the same manner as in Example 2, except that the acrylic polymer (B-2) below was used instead of the acrylic polymer (B-1) in the intermediate layer composition to give the composition shown in Table 1.
[0281] A non-energy ray curable acrylic polymer (B-2) (Mw: 600,000) was obtained by copolymerizing 40 parts by mass of 2-ethylhexyl acrylate (2EHA), 50 parts by mass of methyl acrylate (MA), and 10 parts by mass of acrylic acid (AA).
[0282] [Table 1]
[0283] The above measurements and evaluations were carried out on the obtained samples (Examples 1 to 12 and Comparative Examples 1 to 9). The results are shown in Table 2.
[0284] [Table 2]
[0285] From Table 2, it was confirmed that when the shear storage modulus of the adhesive layer and intermediate layer, the tensile storage modulus of the buffer layer, and the Young's modulus of the substrate are within the above-mentioned ranges, and the thicknesses of the adhesive layer, intermediate layer, and buffer layer are within the above-mentioned ranges, edge cracks are less likely to occur even when a wafer having height differences on its surface, such as a chip-on-wafer, is diced into individual pieces using a pre-dicing method. [Explanation of symbols]
[0286] 1…Protection sheet for workpiece processing 10...Base material 20. Middle class 30...Adhesive layer 40...Buffer layer
Claims
1. A protective sheet for work processing, comprising an adhesive layer, an intermediate layer, a substrate, and a buffer layer laminated in this order, the pressure-sensitive adhesive layer has a shear storage modulus of 0.18 MPa or less at 25°C; The intermediate layer has a shear storage modulus of 0.25 MPa or less at 25°C; The Young's modulus of the substrate at 25° C. is 1500 MPa or more, The tensile storage modulus of the buffer layer at 25° C. is 250 MPa or less; A protective sheet for workpiece processing, wherein the thickness of the adhesive layer is 30 μm or less, the thickness of the intermediate layer is 150 μm or more and 350 μm or less, and the thickness of the buffer layer is 10 μm or more and 100 μm or less.
2. The protective sheet for workpiece processing according to claim 1 , wherein the pressure-sensitive adhesive layer has a shear storage modulus of 0.03 MPa or more at 25° C.
3. The protection sheet for workpiece processing according to claim 2 , wherein the pressure-sensitive adhesive layer is energy ray curable.
4. 4. The protective sheet for work processing according to claim 1, wherein tan δ2 / tan δ1 is greater than 1, where tan δ1 is the loss tangent of the adhesive layer at 25°C and tan δ2 is the loss tangent of the intermediate layer at 25°C.
5. 4. The protective sheet for workpiece processing according to claim 1, wherein the protective sheet for workpiece processing has a thickness of 220 μm or more and 530 μm or less.
6. A step of attaching the protective sheet for workpiece processing according to any one of claims 1 to 3 to a surface of a workpiece having a front surface and a back surface opposite to the front surface; A step of forming a groove on a surface of the workpiece or a step of forming a modified region inside the workpiece; A step of grinding a workpiece having the workpiece processing protective sheet attached to its surface and the groove or the modified region formed thereon from its back surface side to separate the workpiece into a plurality of workpiece pieces starting from the groove or the modified region; A method for manufacturing a workpiece singulated product, comprising a step of peeling off the workpiece processing protection sheet from the plurality of workpiece singulated products.
7. The method for producing individual workpieces according to claim 6 , wherein the surface has a difference in height.
Citation Information
Patent Citations
Method for processing adhesive sheet and semiconductor wafer, and method for producing semiconductor chip
JP2010215769A
Adhesive tape for semiconductor processing and method for manufacturing semiconductor device
JP2020038985A
Semiconductor wafer surface protection film and method for manufacturing semiconductor device
WO2017006549A1
Adhesive tape for semiconductor processing, and semiconductor device manufacturing method
WO2018066480A1
Adhesive tape for semiconductor processing and method for producing semiconductor device
WO2017150676A1