Metal mask base material, method for manufacturing metal mask base material, and method for manufacturing metal mask
A metal mask base material with a KAM value of 2.18° or more, made from an iron-nickel alloy and processed through rolling and annealing, addresses excessive wet etching issues, ensuring precise through-hole formation and preventing warping in metal masks for high-definition applications.
Patent Information
- Application Number
- JP2023056040
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Filing Date
- 2023-03-30
- Publication Date
- 2024-10-11
AI Technical Summary
The challenge of forming high-definition pixels in organic EL display devices and other electronic components using metal masks is exacerbated by excessive wet etching, which enlarges through-holes in the metal masks, leading to variations in etching and potential warping.
A metal mask base material made of an iron-nickel alloy with a KAM value of 2.18° or more, manufactured through rolling and annealing processes, is used to prevent excessive wet etching and warping, ensuring precise through-hole formation.
The solution effectively suppresses the enlargement of through-holes and reduces warping, enabling high-definition pattern formation in metal masks for organic EL display devices and other electronic components.
Smart Images

Figure 2024143391000001_ABST
Abstract
Description
[Technical field]
[0001] The present disclosure relates to a metal mask substrate, a method for manufacturing a metal mask substrate, and a method for manufacturing a metal mask. [Background technology]
[0002] One example of a method for forming pixels in an organic EL display device is a vacuum deposition method. In the vacuum deposition method, a metal mask made of metal and having a plurality of through holes is used. Each through hole has a shape corresponding to the shape of a pixel, and the plurality of through holes are arranged according to the arrangement of the pixels. Each through hole is a passage through which a deposition material for forming the pixels passes. A thin metal plate made of an iron-nickel alloy is used as a material for forming the metal mask (see, for example, Patent Document 1).
[0003] When manufacturing a metal mask from a thin metal plate, a resist layer is first formed on the surface of the thin metal plate, and then a resist pattern is formed from the resist layer. A plurality of through holes are then formed in the thin metal plate by wet etching using the resist pattern. [Prior art documents] [Patent documents]
[0004] [Patent Document 1] International Publication No. 2018 / 235862 Summary of the Invention [Problem to be solved by the invention]
[0005] Meanwhile, various electronic devices equipped with an organic EL display device are required to display high-definition images. Therefore, pixels of the organic EL display device and, in turn, metal masks for forming the pixels are required to be highly precise. For example, in a metal mask for forming high-definition pixels of about 500 ppi, the maximum dimension of the opening located on the surface of the metal thin plate is miniaturized to several tens of μm. In the formation of through holes with miniaturized openings, excessive wet etching is performed in some of the through holes among the multiple through holes, which causes a new problem that the through holes become larger.
[0006] These issues are not limited to metal masks used to form pixels in organic EL display devices, but are also common to metal masks used to form patterns used in electronic devices and electronic components other than organic EL display devices, for example. [Means for solving the problem]
[0007] The metal mask substrate for solving the above problems is a metal plate made of an iron-nickel alloy, which has a step size of 0.5 μm, a KAM value of 2.18° or more obtained by electron backscatter diffraction method when a boundary where the difference in crystal orientation is 5° or more is regarded as a grain boundary, and has a thickness of 10 μm to 30 μm.
[0008] A method for manufacturing a metal mask substrate for solving the above problems is a method for manufacturing a metal mask substrate, which is a metal plate made of an iron-nickel alloy. The manufacturing method includes rolling a base material of the metal plate to obtain a rolled material, and annealing the rolled material at a temperature of 720°C or less. When a step size is set to 0.5 μm and a boundary where the difference in crystal orientation is 5° or more is regarded as a grain boundary, the KAM value obtained by electron backscatter diffraction method in the metal plate is 2.18° or more, and the metal plate has a thickness of 10 μm or more and 30 μm or less.
[0009] A method for manufacturing a metal mask for solving the above problems includes forming a resist layer on a metal plate, forming a resist pattern from the resist layer, and forming a plurality of through holes in the metal plate by wet etching using the resist pattern. In the metal plate, when a step size is set to 0.5 μm and a boundary where the difference in crystal orientation is 5° or more is regarded as a grain boundary, a KAM value obtained by electron backscatter diffraction method is 2.18° or more, and the metal plate has a thickness of 10 μm to 30 μm.
[0010] According to the above metal mask substrate, the KAM value of the metal mask substrate is 2.18° or more, so that when multiple through holes are formed in the metal mask substrate, some of the multiple through holes are prevented from becoming larger.
[0011] In the metal mask substrate, the KAM value may be 2.76° or less. In the above-described method for producing a metal mask substrate, the annealing may include annealing the rolled material at a temperature of 300° C. or higher, and the KAM value may be 2.76° or less.
[0012] According to the above metal mask substrate, it is possible to suppress residual strain in the metal mask substrate to such an extent that the metal mask substrate does not warp after wet etching of the metal mask substrate.
[0013] In the method for producing a metal mask, forming the plurality of through holes includes forming the through holes such that each through hole has an opening on the first surface of the metal plate and each opening has an area of 1600 μm 2 forming the plurality of through holes as follows:
[0014] According to the above-mentioned method for manufacturing a metal mask, the openings in the resist pattern for forming the openings in the metal mask have a very small area, which makes it difficult for an etching solution to penetrate into the openings in the resist pattern. As a result, etching is likely to vary within the surface of the metal mask substrate, and the effect of the metal mask substrate having a KAM value of 2.18° or more can be more significantly obtained. Effect of the Invention
[0015] According to the above-described metal mask substrate, method for manufacturing a metal mask substrate, and method for manufacturing a metal mask, it is possible to prevent some of the through holes of the plurality of through holes in the metal mask from becoming large. [Brief description of the drawings]
[0016] [Figure 1] FIG. 1 is a perspective view showing a metal mask substrate. [Diagram 2] FIG. 2 is a cross-sectional view of the metal mask substrate shown in FIG. [Diagram 3] FIG. 3 is a plan view that shows a schematic diagram of pixels that are set on the observation surface of the metal mask substrate when calculating the KAM value. [Figure 4] FIG. 4 is a process diagram showing a process in which excessive wet etching progresses locally in a metal mask substrate. [Diagram 5] FIG. 5 is a process diagram showing a process in which excessive wet etching progresses locally in a metal mask substrate. [Figure 6] FIG. 6 is a process diagram showing a process in which excessive wet etching progresses locally on a metal mask substrate. [Figure 7] FIG. 7 is a schematic diagram for explaining pitting corrosion that occurs in a metal mask substrate. [Figure 8] FIG. 8 is a process diagram showing a process in which excessive wet etching progresses locally in a metal mask substrate. [Figure 9] FIG. 9 is a plan view showing the metal mask. [Figure 10] FIG. 10 is an enlarged plan view of a portion of the metal mask shown in FIG. [Figure 11] FIG. 11 is a cross-sectional view showing a first example of the structure of the metal mask shown in FIG. [Figure 12] FIG. 12 is a cross-sectional view showing a second example of the structure of the metal mask shown in FIG. [Figure 13] FIG. 13 is a process diagram showing one step included in the method for producing a metal mask substrate. [Figure 14] FIG. 14 is a process diagram showing one step included in the method for producing a metal mask substrate. [Figure 15] FIG. 15 is a process diagram showing one step included in the method for manufacturing a metal mask. [Figure 16] FIG. 16 is a process diagram showing one step included in the method for manufacturing a metal mask. [Figure 17] FIG. 17 is a process diagram showing one step included in the method of manufacturing a metal mask. [Figure 18] FIG. 18 is a process diagram showing one step included in the method of manufacturing a metal mask. [Figure 19] FIG. 19 is a process diagram showing one step included in the method of manufacturing a metal mask. [Figure 20] FIG. 20 is a process diagram showing one step included in the method of manufacturing a metal mask. [Figure 21] FIG. 21 is a graph showing the relationship between the KAM value and the incidence rate of localized etching. [Figure 22] FIG. 22 is an SEM image of the surface of a test piece including openings, the SEM image including openings where localized etching has progressed and openings where localized etching has not occurred. [Figure 23] FIG. 23 is a graph showing the relationship between the annealing temperature and the KAM value. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0017] An embodiment of a metal mask substrate, a metal mask substrate, and a method for manufacturing a metal mask will be described with reference to Figures 1 to 23. The metal mask of this embodiment is an example of a metal mask, and is a deposition mask used to form pixels included in an organic EL display device.
[0018] [Substrate for metal masks] The metal mask substrate will be described with reference to FIGS. The metal mask substrate 10 shown in FIG. 1 is a metal plate made of an iron-nickel alloy. The metal mask substrate 10 has a thickness T of 10 μm or more and 30 μm or less. The metal mask substrate 10 has a front surface 10F and a back surface 10R, which is the surface opposite to the front surface 10F. The thickness T of the metal mask substrate 10 is the distance between the front surface 10F and the back surface 10R. From the viewpoint of improving the handleability of the metal mask substrate 10, the thickness of the metal mask substrate 10 is preferably 10 μm or more, and more preferably 15 μm or more. From the viewpoint of preventing the through holes formed in the metal mask substrate 10 from casting a shadow on the deposition material that has entered the through holes, the thickness of the metal mask substrate 10 is preferably 30 μm or less, and more preferably 20 μm or less. The shadow cast on the deposition material is called the shadow effect of the metal mask. From the viewpoints of improving the handleability of the metal mask substrate 10 and suppressing the shadow effect of the metal mask, the thickness of the metal mask substrate 10 is preferably 10 μm or more and 30 μm or less.
[0019] The metal mask substrate 10 preferably contains 35% by mass or more and 36.5% by mass or less of nickel element, with the remainder being iron element. The metal mask substrate 10 may contain an additive element other than nickel element and iron element. The additive element may be a metal element or a nonmetal element. The metal element may be, for example, manganese (Mn), magnesium (Mg), aluminum (Al), chromium (Cr), molybdenum (Mo), or cobalt (Co). The nonmetal element may be silicon element, phosphorus (P), sulfur (S), or chlorine (Cl). In the metal mask substrate 10, the sum of the additive elements may be, for example, 1% by mass or less.
[0020] FIG. 2 shows a cross-sectional structure of the metal mask substrate 10. As shown in FIG. 2, the metal mask substrate 10 is composed of a main layer 10A, a first surface layer 10B1, and a second surface layer 10B2. The main layer 10A is located between the first surface layer 10B1 and the second surface layer 10B2. The first surface layer 10B1 includes the front surface 10F of the metal mask substrate 10. The second surface layer 10B2 includes the back surface 10R of the metal mask substrate 10. The first surface layer 10B1 and the second surface layer 10B2 are each a natural oxide film of an iron-nickel alloy. In contrast, in the main layer 10A, the iron-nickel alloy is not oxidized by an oxidizing agent present around the alloy. Therefore, the oxygen element content in each of the surface layers 10B1 and 10B2 is higher than the oxygen element content in the main layer 10A. The thickness of each of the surface layers 10B1 and 10B2 may be, for example, greater than 0 nm and less than 10 nm, or greater than 0 nm and less than 5 nm.
[0021] Of the metal elements contained in metal mask substrate 10, iron and nickel become non-conductors when oxidized. First surface layer 10B1 and second surface layer 10B2 contain iron and nickel, and are therefore composed of non-conductors. Among the elements that can be contained in metal mask substrate 10, aluminum, chromium, and cobalt also become non-conductors when oxidized.
[0022] FIG. 3 is a schematic diagram for explaining the KAM value measured on the metal mask substrate 10. As shown in FIG. In the metal mask substrate 10 of the present disclosure, when the step size is set to 0.5 μm and a boundary where the difference in crystal orientation is 5° or more is regarded as a grain boundary, the KAM value obtained by electron backscatter diffraction is 2.18° or more. According to the metal mask substrate 10 of the present disclosure, the KAM value of the metal mask substrate 10 is 2.18° or more, and therefore, when multiple through holes are formed in the metal mask substrate 10, some of the multiple through holes are prevented from becoming large.
[0023] When measuring the KAM value of the metal mask substrate 10, first, the surface 10F of the metal mask substrate 10 is prepared, thereby creating an observation surface. At this time, 1 / 10 of the thickness of the metal mask substrate 10 is removed from the surface 10F of the metal mask substrate 10 by buffing and ion milling. Next, the KAM value is measured by the electron backscatter diffraction (EBSD) method for a measurement area of 50 μm square on the observation surface using a field emission scanning electron microscope (FE-SEM). At this time, the step size is set to 0.5 μm, and the KAM value is measured when a boundary where the difference in crystal orientation is 5° or more is regarded as a grain boundary. The KAM value is measured for five measurement areas randomly selected from the observation surface that do not overlap, and the average value of the KAM values obtained in each measurement area is set as the KAM value of the metal mask substrate 10.
[0024] As shown in Figure 3, an electron beam is irradiated onto irradiation points SP arranged with a step size SS of 0.5 μm. A hexagonal region in the measurement area centered on the irradiation point SP is defined as a pixel PX, and the crystal orientation at the irradiation point SP contained in that pixel PX is regarded as the crystal orientation of that pixel PX. Note that among the multiple pixels PX contained in the measurement area, adjacent pixels PX share one side at the outer edge of the pixel PX.
[0025] When calculating the KAM value, the crystal orientation at each pixel PX is calculated. Next, the average value of the crystal orientations is calculated for the six pixels PX adjacent to that pixel PX that belong to the same crystal grain. At this time, pixels PX whose crystal orientations differ by 5° or more from the crystal orientation of the pixel PX being calculated are recognized as pixels PX that do not belong to the same crystal grain. Next, the difference value between the crystal orientation of the pixel PX being calculated and the average value of the crystal orientations of the adjacent pixels PX is calculated. The absolute value of this difference value is set as the KAM value for the pixel PX being calculated.
[0026] For example, among the pixels PX shown in FIG. 3, a pixel PX with high density dots is set as the first pixel PX1. When calculating the KAM value of the first pixel PX1, the average value of the crystal orientations of six second pixels PX2 that are adjacent to the first pixel PX1 and are low density dots is calculated. In this case, among the second pixels PX2, the second pixels PX2 that have a crystal orientation that differs from the crystal orientation of the first pixel PX1 by 5° or more are excluded from the calculation of the average value. Then, the difference value between the crystal orientation of the first pixel PX1 and the average value of the crystal orientations of the second pixels PX2 is calculated. The absolute value of the difference value is the KAM value of the first pixel PX1.
[0027] The KAM value is calculated for all pixels PX included in the measurement area. Then, the average value for all pixels PX is calculated, and the average value is set as the KAM value for the measurement area. After the KAM values for the five measurement areas are calculated, the average value for the five measurement areas is calculated, thereby obtaining the KAM value of the metal mask substrate 10.
[0028] The KAM value is an index that represents the degree of distortion in the crystal lattice contained within a crystal grain. The larger the KAM value within a crystal grain, the greater the distortion of the crystal lattice.
[0029] The mechanism by which localized etching progresses in the metal mask substrate 10 will be described with reference to Figures 4 to 8. Figures 4 to 6 and 8 show schematic diagrams of the process of wet-etching the metal mask substrate 10 using a second resist pattern formed on the rear surface 10R of the metal mask substrate 10. Figure 7 is a schematic diagram for explaining pitting corrosion that occurs when the metal mask substrate 10 is wet-etched.
[0030] 4, when the metal mask substrate 10 is wet-etched, a second resist pattern RP2 is formed on the rear surface 10R of the metal mask substrate 10. The second resist pattern RP2 has second through holes RP2A. When viewed from a viewpoint facing the rear surface 10R, the second resist pattern RP2 is formed on the rear surface 10R of the metal mask substrate 10 by wet etching via the second through holes RP2A to a depth of 1600 μm. 2 In order to enable the formation of higher resolution pixels, the area of the opening may be 900 μm or less. 2 It is preferable that:
[0031] 5, when wet etching the metal mask substrate 10 from the rear surface 10R of the metal mask substrate 10, an etching solution ES is supplied to the second resist pattern RP2. The etching solution is, for example, an etching solution containing chloride ions, and may be a ferric chloride solution. The wet etching method may be, for example, spray etching. When the wet etching method is spray etching, the etching solution ES supplied to the second resist pattern RP2 has a flow along a predetermined direction.
[0032] A part of the etching solution ES supplied to the second resist pattern RP2 flows into the second through hole RP2A. At this time, as described above, the opening area of the second through hole RP2A is 1600 μm 2 Since the area is small enough to form an opening having an area smaller than the area of the second through hole RP2A, it is difficult to uniformly supply the etching liquid ES to the entire second through hole RP2A.
[0033] 6, the etching solution ES supplied to part of second through hole RP2A etches part of the part of back surface 10R that is exposed in second through hole RP2A. As described above, back surface 10R of metal mask substrate 10 is included in second surface layer 10B2, and therefore part of second surface layer 10B2 is etched.
[0034] 7, when etching solution ES is supplied to second surface layer 10B2, the concentration of chloride ions becomes high only in a portion of second surface layer 10B2. As a result, second surface layer 10B2, which is passive, is locally destroyed by the chloride ions, causing pitting corrosion in a portion of metal mask substrate 10. The portion of main layer 10A exposed from second surface layer 10B2 functions as an anode, and second surface layer 10B2 functions as a cathode. This causes the following reaction:
[0035] (Anode reaction) Fe → Fe 2+ +2e - (Hydrolysis reaction) Fe 2+ +2H2O → Fe(OH)2+2H + (Cathode reaction) O2+2H2O+4e - → 4OH - That is, the dissolved iron ions at the anode undergo a hydrolysis reaction, which acidifies the pitted areas, suppressing passivation and allowing further etching of the pitted areas.
[0036] 8, the etching of the portion of main layer 10A exposed from second surface layer 10B2 proceeds at a higher rate than the etching of the entire portion exposed from second through hole RP2A. As a result, recess 10AH is formed by localized etching, and therefore the opening located on back surface 10R becomes larger in some of the through holes among the plurality of through holes, and thus the size of the through holes becomes larger.
[0037] In this respect, according to the metal mask substrate 10 of the present disclosure, the distortion of the crystal lattice in the main layer 10A becomes large, and therefore the distortion of the crystal lattice in the first surface layer 10B1 and the second surface layer 10B2 formed on the surface of the main layer 10A also becomes large. As a result, the first surface layer 10B1 and the second surface layer 10B2 become rough, and the first surface layer 10B1 and the second surface layer 10B2 have many places where the etching solution ES can easily enter. As a result, the amount of the main layer 10A that is removed by pitting corrosion can be distributed to multiple places, so that the etching is prevented from progressing locally in a part of the metal mask substrate 10. That is, the opening located on the back surface 10R is prevented from becoming large in some of the multiple through holes, and thus the through holes are prevented from becoming large.
[0038] The KAM value of the metal mask substrate 10 may be 2.76° or less. This makes it possible to suppress residual strain in the metal mask substrate 10 to a degree that does not cause warping of the metal mask substrate 10 after wet etching of the metal mask substrate 10. The KAM value of the metal mask substrate 10 is negatively correlated with the annealing temperature performed on the rolled material in the manufacturing process of the metal mask substrate 10. The KAM value tends to decrease as the annealing temperature increases.
[0039] As described above, if the KAM value of the metal mask substrate 10 is 2.76° or less, it is possible to anneal the rolled material at a temperature at which the residual distortion in the metal mask substrate 10 can be suppressed to a level that does not cause distortion in the metal mask substrate 10 after wet etching.
[0040] [Metal mask] The metal mask will be described with reference to FIGS. The metal mask 20 shown in FIG. 9 is formed from a metal mask substrate 10 made of an iron-nickel alloy. The maximum thickness of the metal mask 20 is 10 μm or more and 30 μm or less. The metal mask 20 has a back surface 20R and a plurality of through holes 20H having openings in the back surface 20R. The back surface 20R is an example of a first surface. The area of the opening is 1600 μm. 2 From the viewpoint of enabling the formation of higher resolution pixels, the area of the opening may be 900 μm 2 It is preferable that:
[0041] According to the metal mask 20 of the present disclosure, the KAM value of the metal mask substrate 10, and therefore the KAM value of the metal mask 20, is 2.18° or more. 2 Even when forming the through holes 20H having miniaturized openings of 100 mm or less, excessive wet etching is prevented from progressing locally in the metal mask substrate 10. Therefore, some of the through holes 20H among the plurality of through holes 20H are prevented from becoming large.
[0042] The metal mask 20 has a back surface 20R and a front surface 20F that is the surface opposite to the back surface 20R. When a deposition pattern is formed using the metal mask 20, the back surface 20R faces a deposition target and the front surface 20F faces a deposition source. The metal mask 20 is used to form pixels included in an organic EL display device.
[0043] The metal mask 20 includes a mask portion 20A and a peripheral portion 20B surrounding the mask portion 20A. In the example shown in FIG. 8, the metal mask 20 includes a plurality of mask portions 20A. A plurality of through holes 20H are formed in each mask portion 20A. Each through hole 20H penetrates the metal mask 20 in the thickness direction of the metal mask 20. Each through hole 20H is a passage for the deposition material. The deposition material passes through the through holes 20H to form a deposition pattern having a predetermined shape on the deposition target. The peripheral portion 20B does not have a through hole 20H. Of the metal mask 20, the peripheral portion 20B has the maximum thickness. The mask portion 20A may or may not have the maximum thickness.
[0044] The metal mask 20 may include an oxide layer made of an oxide of an iron-nickel alloy. The oxide layer includes the back surface 20R of the metal mask 20. That is, the oxide layer corresponds to the first surface layer 10B1 of the metal mask substrate 10 described above. According to the metal mask 20, since the metal mask 20 includes the oxide layer, pitting corrosion is likely to occur in the metal mask substrate 10 used to form the metal mask 20 when the through holes 20H of the metal mask 20 are formed. Therefore, it is more effective for the metal mask substrate 10 to have a KAM value of 2.18° or more.
[0045] FIG. 10 shows the shape of the through-hole 20H as viewed from a side facing the rear surface 20R of the metal mask 20. As shown in FIG. As shown in Fig. 10, the second opening 20H2 of the through hole 20H may have, for example, a square shape. In the example shown in Fig. 10, the second opening 20H2 has a square shape with each corner having a curvature. The center of curvature of each corner is located within the second opening 20H2. In each second opening 20H2, the length L of one side is, for example, 40 µm or less, and therefore the area of the second opening 20H2 is 1600 µm. 2 The shape of the second opening 20H2 is not limited to a square shape, but may be a quadrangular shape other than a square shape, or may be a circular shape. 2If this is the case, the length of one side of the second opening 20H2 is 30 μm or less.
[0046] On the front surface 20F, the second openings 20H2 are arranged according to a predetermined rule. In the example shown in Fig. 9, the second openings 20H2 are arranged in a lattice pattern. The second openings 20H2 may be arranged in a staggered pattern, for example.
[0047] Figures 11 and 12 show the cross-sectional structure of the metal mask 20 along a plane perpendicular to the front surface 20F of the metal mask 20. Figure 11 shows the cross-sectional structure of a first example of the metal mask 20, while Figure 12 shows the cross-sectional structure of a second example of the metal mask 20. Note that Figure 11 shows the cross-sectional structure of the metal mask 20 when the metal mask substrate 10 is etched only from the front surface 10F. In contrast, Figure 12 shows the cross-sectional structure of the metal mask 20 when the metal mask substrate 10 is etched from both the front surface 10F and the back surface 10R.
[0048] 11, in the first example of the metal mask 20, the first opening 20H1 of the through hole 20H is located on the front surface 20F, and the second opening 20H2 is located on the back surface 20R. The through hole 20H has a shape that tapers from the front surface 20F to the back surface 20R. That is, the area of the through hole 20H in a plane perpendicular to the thickness direction monotonically decreases from the front surface 20F to the back surface 20R. The through hole 20H has a substantially arc shape.
[0049] 12, in the second example of the metal mask 20, the first opening 20H1 of the through hole 20H is located on the front surface 20F, and the second opening 20H2 is located on the back surface 20R. The through hole 20H has a large hole portion 20HL and a small hole portion 20HS. The large hole portion 20HL has a shape tapered in the direction from the front surface 20F to the back surface 20R, and the small hole portion 20HS has a shape tapered in the direction from the back surface 20R to the front surface 20F.
[0050] That is, the area of the large hole portion 20HL in a plane perpendicular to the thickness direction monotonically decreases in the direction from the front surface 20F to the back surface 20R, and the area of the small hole portion 20HS monotonically decreases in the direction from the back surface 20R to the front surface 20F. Therefore, the area of the through hole 20H in a plane perpendicular to the thickness direction is smallest at the connection portion between the large hole portion 20HL and the small hole portion 20HS.
[0051] In the case of a metal mask 20 formed using the metal mask substrate 10 of the present disclosure, regardless of whether it is the first or second example described above, the second openings 20H2 are prevented from becoming larger in some of the through holes 20H among the multiple through holes 20H, and therefore the size of the through holes 20H is prevented from becoming larger.
[0052] [Method of manufacturing metal mask substrate] A method for producing a metal mask substrate will be described with reference to FIGS. The method for manufacturing a metal mask substrate of the present disclosure is a method for manufacturing a metal mask substrate, which is a metal plate made of an iron-nickel alloy. The manufacturing method includes rolling a base material of a metal plate to obtain a rolled material, and annealing the rolled material at a temperature of 720°C or less. As described above, in the metal plate, when the step size is set to 0.5 μm and the boundary where the difference in crystal orientation is 5° or more is regarded as a grain boundary, the KAM value obtained by electron backscatter diffraction method is 2.18° or more. The metal plate has a thickness of 10 μm or more and 30 μm or less. Hereinafter, the method for manufacturing a metal mask substrate will be described in detail with reference to the drawings.
[0053] 13, in the method for producing the metal mask substrate 10, first, a base material 31A made of an iron-nickel alloy is prepared. The base material 31A has a strip shape extending along the extension direction D1. Next, the base material 31A is rolled to obtain a rolled material 31B. In this case, for example, after hot rolling, cold rolling and annealing are alternately performed one or more times to obtain the rolled material 31B.
[0054] When rolling the base material 31A, for example, the base material 31A is transported along a transport direction D2 toward a rolling device 50 equipped with a pair of rolling rollers 51, 52 so that the extension direction D1 of the base material 31A and the transport direction D2 in which the base material 31A is transported are parallel to each other.
[0055] The base material 31A may be a steel billet obtained by hot forging of a slab, for example. The thickness of the steel billet may be, for example, 150 mm or more and 250 mm or less. In hot rolling, the steel billet is rolled until it has a thickness of 3 mm or more and 20 mm or less, thereby obtaining a hot rolled material. In alternating cold rolling and annealing, the hot rolled material is rolled until it has a thickness of 10 μm or more and 30 μm or less, thereby obtaining a rolled material 31B. The rolled material 31B is wound around a core C, but the rolled material 31B may be handled in a state of being stretched into a strip without being wound around the core C.
[0056] When cold rolling is performed multiple times, the reduction in the final cold rolling may be 30% or more and 95% or less. When cold rolling is performed multiple times, the reduction in the cold rolling may be decreased each time from the first cold rolling to the final cold rolling. The reduction is calculated by the following formula.
[0057] Rolling reduction rate (%)={(T0-T1) / T0}×100 In the above formula, T0 is the thickness of the rolling object, and T1 is the thickness of the plate material obtained by rolling.
[0058] 14, the rolled material 31B obtained by rolling a steel billet is annealed using an annealing device 53. This makes it possible to reduce the residual stress caused in the rolled material 31B by rolling, and therefore it is possible to obtain a metal mask substrate 10 with reduced residual stress. As described above, in the manufacturing method of the metal mask substrate 10 of the present disclosure, the rolled material 31B obtained through rolling is annealed at a temperature of 720°C or lower. This makes it possible to obtain a metal mask substrate 10 having a KAM value of 2.18° or higher.
[0059] As described above, when the base material 31A is subjected to hot rolling, followed by repeated cold rolling and annealing one or more times, the annealing temperature for the rolled material 31B obtained by these processes is set to a temperature of 720°C or lower.
[0060] The rolled material 31B may be annealed at a temperature of 300°C or higher. This makes it possible to obtain a metal mask substrate 10 having a KAM value of 2.76° or less. From the viewpoint of suppressing warping of the metal mask substrate 10 after etching and suppressing the occurrence of localized etching, it is preferable that the temperature in the final annealing performed after rolling is 300°C or higher and 720°C or lower. By setting the temperature in the final annealing to 300°C or higher, it is possible to reduce residual stress generated in the rolled material 31B by rolling, and thus it is possible to suppress warping after etching.
[0061] In the annealing after rolling, the rolled material 31B may be annealed while being pulled along the transport direction D2. That is, tension annealing may be performed on the rolled material 31B. This makes it possible to further reduce the residual stress generated in the rolled material 31B by rolling.
[0062] The rolling and annealing described above may be modified as follows. For example, a rolling device including a plurality of pairs of rolling rollers may be used for rolling. In addition, in the annealing after rolling, the rolled material 31B may be annealed in a state where it is wound around the core C, instead of annealing the rolled material 31B while pulling the rolled material 31B along the transport direction D2.
[0063] When the rolled material 31B wound around the core C is annealed after rolling, the metal mask substrate 10 obtained after annealing may be warped according to the diameter of the metal mask substrate 10 due to the rolled material 31B being wound around the core C. Therefore, depending on the size of the diameter of the metal mask substrate 10 when wound around the core C and the material constituting the base material 31A, it is preferable to anneal the rolled material 31B while pulling it along the transport direction D2.
[0064] [Metal mask manufacturing method] A method for manufacturing a metal mask will be described with reference to FIGS. The manufacturing method of the metal mask 20 of the present disclosure includes forming a resist layer on a metal plate, forming a resist pattern from the resist layer, and forming a plurality of through holes in the metal plate by wet etching using the resist pattern. As described above, in the metal plate, when the step size is set to 0.5 μm and the boundary where the difference in crystal orientation is 5° or more is regarded as a grain boundary, the KAM value obtained by the electron backscatter diffraction method is 2.18° or more. The metal plate has a thickness of 10 μm or more and 30 μm or less. Hereinafter, the manufacturing method of the metal mask 20 will be described in detail with reference to the drawings. Note that, for convenience of illustration, in FIG. 15 to FIG. 20, the process of forming one through hole in the second example of the above-mentioned metal mask 20 is illustrated.
[0065] As shown in Fig. 15, a first resist layer R1 is located on the front surface 10F of the metal mask substrate 10. The first resist layer R1 is formed of, for example, a negative resist. A second resist layer R2 is located on the back surface 10R. The second resist layer R2 is formed of, for example, a negative resist. The first resist layer R1 and the second resist layer R2 may be formed of a positive resist. Each of the resist layers R1 and R2 may be a dry film resist or may be formed of a coating type resist.
[0066] As shown in Fig. 16, after the first resist layer R1 and the second resist layer R2 are exposed, the first resist layer R1 and the second resist layer R2 are developed. As a result, a first resist pattern RP1 is formed from the first resist layer R1, and a second resist pattern RP2 is formed from the second resist layer R2. A developer such as an aqueous sodium carbonate solution is used to develop each of the resist layers R1 and R2.
[0067] The first resist pattern RP1 has a first through hole RP1A. The first through hole RP1A penetrates the first resist pattern RP1 along the thickness direction of the first resist pattern RP1. The second resist pattern RP2 has a second through hole RP2A. The second through hole RP2A penetrates the second resist pattern RP2 along the thickness direction of the second resist pattern RP2. When viewed from a viewpoint opposite to the plane in which the first resist pattern RP1 extends, the second through hole RP2A is located within the first through hole RP1A.
[0068] As shown in FIG. 17, a first protective layer PL1 is formed on the surface of the first resist pattern RP1. By forming the first protective layer PL1, the first through holes RP1A are blocked, thereby preventing the etching solution from reaching the metal mask substrate 10 through the first through holes RP1A. Next, the metal mask substrate 10 is etched from the rear surface 10R using the second resist pattern RP2. For example, an etching solution containing chloride ions is used to etch the metal mask substrate 10. The etching solution may be a ferric chloride solution as described above. This forms small holes 10HS opening on the rear surface 10R.
[0069] The thickness of the resist patterns RP1 and RP2 may be 10 μm or less, preferably 7 μm or less, and more preferably 5 μm or less. The thinner the resist patterns RP1 and RP2 are, the more easily the etching liquid penetrates into the through holes RP1A and RP2A of the resist patterns RP1 and RP2.
[0070] At this time, each small hole portion 10HS has an opening on the rear surface 10R of the metal mask substrate 10, and the area of each opening is 1600 μm 2 A plurality of small holes 10HS may be formed as follows: The area of each opening located on the rear surface 10R is, for example, 1600 μm 2 Further, the area of each opening may be less than or equal to 900 μm 2 It is preferable that:
[0071] In this case, the area of the openings in the second resist pattern RP2 for forming the openings in the metal mask 20 is also very small, which makes it difficult for the etching solution to penetrate into the openings in the second resist pattern RP2. As a result, etching is likely to vary within the surface of the metal mask substrate 10, and the effect of the metal mask substrate 10 having a KAM value of 2.18° or more can be more significantly obtained.
[0072] 18, the first protective layer PL1 is removed from the front surface of the first resist pattern RP1. The second resist pattern RP2 is also removed from the rear surface 10R of the metal mask substrate 10. Next, the rear surface 10R of the metal mask substrate 10 is covered with the second protective layer PL2. At this time, the second protective layer PL2 is formed on the rear surface 10R such that a part of the second protective layer PL2 fills the small hole portion 10HS.
[0073] As shown in FIG. 19, the metal mask substrate 10 is etched from the front surface 10F using the first resist pattern RP1. To etch the metal mask substrate 10, an etching solution containing, for example, chloride ions is used, as in the case of forming the small hole portions 10HS. As described above, the etching solution may be a ferric chloride solution. This forms large hole portions 10HL that open to the front surface 10F. The large hole portions 10HL are formed to reach parts of the second protective layer PL2 filled in the small hole portions 10HS, thereby connecting the large hole portions 10HL to the small hole portions 10HS.
[0074] 20, the first resist pattern RP1 is removed from the front surface 10F of the metal mask substrate 10, and the second protective layer PL2 is removed from the back surface 10R. This results in a metal mask 20 having through holes 20H. In the through holes 20H, the large hole portions 20HL correspond to the large hole portions 10HL formed in the metal mask substrate 10, and the small hole portions 20HS correspond to the small hole portions 10HS formed in the metal mask substrate 10. Furthermore, the front surface 20F of the metal mask 20 corresponds to the front surface 10F of the metal mask substrate 10, and the back surface 20R of the metal mask 20 corresponds to the back surface 10R of the metal mask substrate 10.
[0075] When the second protective layer PL2 is formed on the rear surface 10R of the metal mask substrate 10, the second resist pattern RP2 does not have to be removed from the rear surface 10R of the metal mask substrate 10. In this case, the second protective layer PL2 is formed on the second resist pattern RP2. The second protective layer PL2 is formed so that a part of the second protective layer PL2 fills the small hole portion 10HS and also fills the second through hole RP2A of the second resist pattern RP2. After the large hole portion 10HL is formed in the metal mask substrate 10, the second resist pattern RP2 is removed from the metal mask substrate 10 together with the second protective layer PL2.
[0076] Furthermore, when the first example of the metal mask 20 is manufactured, the process of etching the metal mask substrate 10 from the back surface 10R is omitted. Therefore, the process of forming the second resist pattern RP2 on the back surface 10R is also omitted. When the metal mask substrate 10 is etched from the front surface 10F, a protective layer is formed on the back surface 10R of the metal mask substrate 10.
[0077] [Example] An example and a comparative example will be described with reference to FIGS. [Example 1] A slab made of an iron-nickel alloy and having a thickness of 200 mm was prepared. Next, a steel billet was produced by hot forging the slab. Then, the steel billet was hot rolled until it had a thickness of 400 μm, to obtain a hot-rolled material. Next, cold rolling and annealing were alternately performed three times to obtain a rolled material having a thickness of 25 μm. At this time, the reduction ratio in the first cold rolling was set to 70%, the reduction ratio in the second cold rolling was set to 62.5%, and the reduction ratio in the third cold rolling was set to 44.4%. As a result, the total reduction ratio of the rolled material after three cold rollings were performed on the hot rolled material before cold rolling was set to 93.8%. Then, tension annealing was performed on the rolled material. At this time, the annealing temperature of the rolled material in tension annealing was set to 620 ° C, and the holding time was set to 4.5 seconds. As a result, a metal mask substrate of Example 1 having a thickness of 25 μm was obtained.
[0078] [Example 2] A metal mask substrate of Example 2 was obtained in the same manner as in Example 1, except that the annealing temperature in the tension annealing was changed to 680°C.
[0079] [Example 3] A metal mask substrate of Example 3 was obtained in the same manner as in Example 1, except that the annealing temperature in the tension annealing was changed to 720°C.
[0080] [Comparative Example 1] A metal mask substrate of Comparative Example 1 was obtained in the same manner as in Example 1, except that the annealing temperature in the tension annealing was changed to 760°C.
[0081] [Comparative Example 2] A metal mask substrate of Comparative Example 2 was obtained in the same manner as in Example 1, except that the annealing temperature in the tension annealing was changed to 800°C.
[0082] [Comparative Example 3] A metal mask substrate of Comparative Example 3 was obtained in the same manner as in Example 1, except that the annealing temperature in the tension annealing was changed to 900°C.
[0083] [Evaluation method] [KAM value] When measuring the KAM value, first, a thickness of 2.5 μm was removed from the surface of each metal mask substrate by buffing and ion milling. This created an observation surface. Next, using an FE-SEM (SU-70, Hitachi High-Technologies Corporation) and an OIM (Orientation Imaging Microscopy) crystal orientation measurement device (Digiview 5 type, TSL Solutions Corporation), the KAM value was measured by the EBSD method for a 50 μm square observation area on the observation surface. At this time, the step size was set to 0.5 μm, and the boundary where the difference in crystal orientation was 5° or more was regarded as a grain boundary. After measuring the KAM value for five randomly selected non-overlapping measurement areas on the observation surface of each metal mask substrate, the average value of the KAM values obtained in each measurement area was set as the KAM value of each metal mask substrate. Note that the data collection software and data analysis software included in the OIM crystal orientation measurement device were used to calculate the KAM value.
[0084] [etching] A dry film resist having a thickness of 10 μm was attached to the surface of each metal mask substrate. Then, square through holes with a side length of 25 μm were formed in the dry film resist by photolithography, thereby obtaining a resist pattern. At this time, the pitch of the through holes was set to 50 μm. Then, the metal mask substrate was etched using a ferric chloride solution so that the etching depth was 8 μm. At this time, the concentration of the etching solution was set to 50 degrees Baume, and the temperature of the etching solution was set to 50° C. Next, the resist pattern was removed from the surface of the deposition metal mask substrate to obtain an etched test piece.
[0085] The surface of each test piece was photographed using a laser microscope (VK-X3000, manufactured by Keyence Corporation) to obtain an image of the surface including a plurality of openings. Then, the area of 1000 openings included in the surface was calculated by image analysis. The average value of the areas of the 10 openings from the smallest opening to the 10th smallest opening among the 1000 openings was calculated, and the average value was set as a reference value. Then, an opening having an area 1.2 times or more larger than the reference value was regarded as an opening in which local etching had progressed and was larger than the other openings. Then, the percentage of the openings in which local etching had progressed among the 1000 openings was calculated.
[0086] [Evaluation Results] For the metal mask substrates of each Example and Comparative Example, the annealing temperature set during tension annealing, the KAM value, and the occurrence rate, which is the percentage of openings where localized etching has progressed, are as shown in Table 1 below.
[0087] [Table 1]
[0088] As shown in Table 1, the KAM value of the metal mask substrate was found to be 2.31° in Example 1, 2.23° in Example 2, and 2.18° in Example 3. It was also found to be 2.11° in Comparative Example 1, 2.07° in Comparative Example 2, and 1.92° in Comparative Example 3. Thus, in Examples 1 to 3, the KAM value was found to be 2.18° or more and 2.31° or less. In contrast, in Comparative Examples 1 to 3, the KAM value was found to be 1.92° or more and 2.11° or less.
[0089] It was also found that the incidence of localized etching was 0% in Examples 1 to 3, 20.0% in Comparative Example 1, 69.5% in Comparative Example 2, and 95.6% in Comparative Example 3.
[0090] In this way, it was confirmed that the progress of localized etching was suppressed by the KAM value being 2.18° or more. Also, as shown in Fig. 21, it was confirmed that the progress of localized etching was suppressed more rapidly by the KAM value being 2.11° compared to the case where the KAM value was larger than 2.11°, and further, it was confirmed that the progress of localized etching did not occur by the KAM value being 2.18° or more.
[0091] FIG. 22 is an example of an SEM image of the surface of a test piece obtained from the metal mask substrate of Comparative Example 1. As shown in Fig. 22, it was found that the multiple openings located on the surface 40F of the test piece included a first opening 40A1 where no local etching occurred and a second opening 40A2 where local etching progressed. It was found that the area of the second opening 40A2 was larger than that of the first opening 40A1, and the depth of the recess having the second opening 40A2 was deeper than that of the recess having the first opening 40A1. It was also found that the surface roughness of the bottom of the recess having the second opening 40A2 was large, so that the bottom was not imaged.
[0092] FIG. 23 shows the relationship between the annealing temperature during tension annealing and the KAM value of the metal mask substrate. As shown in Fig. 23, it was confirmed that there is a negative correlation between the annealing temperature during tension annealing and the KAM value of the metal mask substrate. Furthermore, an approximation curve represented by the following formula was obtained from the annealing temperature and the KAM value. In Fig. 23, the approximation curve is indicated by a dashed line.
[0093] y=-0.0014x+3.1764 Based on the above formula, the KAM values obtained were as follows: When the annealing temperature was 550°C, the KAM value was 2.41°, when the annealing temperature was 500°C, the KAM value was 2.48°, and when the annealing temperature was 450°C, the KAM value was 2.55°. When the annealing temperature was 400°C, the KAM value was 2.62°, when the annealing temperature was 350°C, the KAM value was 2.69°, and when the annealing temperature was 300°C, the KAM value was 2.76°.
[0094] When the annealing temperature in tension annealing is 300°C or higher, warping of the metal mask substrate is suppressed after wet etching of the metal mask substrate. From the viewpoint of suppressing warping of the metal mask substrate, it is preferable that the KAM value is 2.76° or less.
[0095] As described above, according to one embodiment of the metal mask substrate, the method for manufacturing a metal mask substrate, and the method for manufacturing a metal mask, the following effects can be obtained. (1) When the KAM value of the metal mask substrate 10 is 2.18° or more, when multiple through holes are formed in the metal mask substrate 10, some of the multiple through holes are prevented from becoming larger.
[0096] (2) When the KAM value of the metal mask substrate 10 is 2.76° or less, it is possible to suppress the residual distortion of the metal mask substrate to such an extent that the metal mask substrate does not warp after wet etching of the metal mask substrate 10.
[0097] (3) The area of the opening formed on the rear surface 10R of the metal mask substrate 10 is 1600 μm 2If it is below this value, the area of the openings in the second resist pattern RP2 for forming the openings is also very small, which makes it difficult for the etching solution to penetrate into the openings in the second resist pattern RP2. As a result, etching is likely to vary within the surface of the metal mask substrate 10, and the effect of the metal mask substrate 10 having a KAM value of 2.18° or more can be more significantly obtained.
[0098] The above-described embodiment can be modified as follows. [Application] The metal mask is not limited to a metal mask used to form pixels in an organic EL display device. The metal mask may be, for example, a mask for forming a pattern used in electronic devices or electronic components other than an organic EL display device. The metal mask may be used by a deposition method or a sputtering method. The through holes in the metal mask may have an arrangement corresponding to the pattern formed using the metal mask in a plan view facing the back surface. Such a metal mask allows for high-definition patterns, which in turn allows for the realization of smaller, lighter, and thinner electronic devices and electronic components that require high-definition patterns. [Explanation of symbols]
[0099] 10...Substrate for metal masks 10A…Main layer 10B1…1st surface layer 10B2…Second surface layer 10F…Surface 10R…Back 20...Metal mask 20H…Through hole
Claims
1. A metal mask substrate which is a metal plate made of an iron-nickel alloy, When the step size is set to 0.5 μm and a boundary where the difference in crystal orientation is 5° or more is regarded as a grain boundary, the KAM value obtained by electron backscatter diffraction is 2.18° or more; The thickness is 10 μm or more and 30 μm or less. Substrate for metal masks.
2. The KAM value is 2.76° or less. The metal mask substrate according to claim 1 .
3. A method for producing a metal mask substrate, which is a metal plate made of an iron-nickel alloy, comprising the steps of: rolling the base material of the metal plate to obtain a rolled material; Annealing the rolled material at a temperature of 720° C. or less; In the metal plate, when a step size is set to 0.5 μm and a boundary where the difference in crystal orientation is 5° or more is regarded as a grain boundary, the KAM value obtained by electron backscatter diffraction method is 2.18° or more; The metal plate has a thickness of 10 μm or more and 30 μm or less. A method for manufacturing a metal mask substrate.
4. Annealing includes annealing the rolled material at a temperature of 300° C. or more; The KAM value is 2.76° or less. The method for producing the metal mask substrate according to claim 3 .
5. forming a resist layer on a metal plate; forming a resist pattern from the resist layer; and forming a plurality of through holes in the metal plate by wet etching using a resist pattern; In the metal plate, when a step size is set to 0.5 μm and a boundary where the difference in crystal orientation is 5° or more is regarded as a grain boundary, the KAM value obtained by electron backscatter diffraction method is 2.18° or more; The metal plate has a thickness of 10 μm or more and 30 μm or less. A method for manufacturing a metal mask.
6. The formation of the plurality of through holes means that each through hole has an opening on the first surface of the metal plate, and each opening has an area of 1600 μm 2 forming the plurality of through holes as follows: The method for producing the metal mask according to claim 5 .
Citation Information
Patent Citations
Method for producing thin plate for metal masks, and thin plate for metal masks
WO2018235862A1