Thermoelectric wafer and method of manufacturing the same

JP2024143442APending Publication Date: 2024-10-11LINTEC CORP
View PDF 1 Cites 0 Cited by

Patent Information

Application Number
JP2023056127
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Filing Date
2023-03-30
Publication Date
2024-10-11

AI Technical Summary

Benefits of technology

【0007】 本発明によれば、優れた機械的強度を有する熱電ウェハ及びその製造方法を提供することができる。

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024143442000001_ABST
    Figure 2024143442000001_ABST
Patent Text Reader

Abstract

To provide a thermoelectric wafer having excellent mechanical strength and a method of manufacturing the same.SOLUTION: A thermoelectric wafer includes a thermoelectric element layer including a thermoelectric semiconductor material, the thermoelectric wafer has an edge region and a recessed region surrounded by the edge region, and the thickness of the edge region is greater than the thickness of the recessed region.SELECTED DRAWING: Figure 1
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a thermoelectric wafer and a method for manufacturing the same. [Background technology]

[0002] 2. Description of the Related Art Conventionally, as one of the means for effectively utilizing energy, there has been a device that directly converts thermal energy into electrical energy and vice versa using a thermoelectric conversion module having a thermoelectric effect such as the Seebeck effect or the Peltier effect. As a thermoelectric conversion module, for example, a configuration of a so-called π-type thermoelectric conversion element is known. The π-type thermoelectric conversion element is configured by providing a pair of electrodes spaced apart from each other on a substrate, for example, providing a P-type thermoelectric element layer on one electrode and an N-type thermoelectric element layer on the other electrode, also spaced apart from each other, and connecting the upper surfaces of both thermoelectric element layers to a common electrode on the opposing substrate. In recent years, in order to improve thermoelectric performance and mass productivity, thin-film P-type thermoelectric element layers and N-type thermoelectric element layers have been formed into wafers, and thermoelectric conversion modules have been mass-produced. Patent Document 1 discloses, for example, a structure having a film of a fibrous semiconductor material (which can be used as a high-performance device such as a thermoelectric conversion element, a light-emitting element, or a nanowire solar cell) on a base (wafer), and further having a bank made of an addition-curing silicone resin on the edge of the base (wafer). [Prior art documents] [Patent documents]

[0003] [Patent Document 1] JP 2018-85441 A Summary of the Invention [Problem to be solved by the invention]

[0004] However, in Patent Document 1, the banks made of addition-curing silicone resin at the ends of the base (wafer) are provided in order to fill the spaces between the multiple fibrous semiconductor materials (A) formed with filler (C), and no consideration is given to the mechanical strength of the base (wafer).

[0005] In view of the above, an object of the present invention is to provide a thermoelectric wafer having excellent mechanical strength and a method for manufacturing the same. [Means for solving the problem]

[0006] As a result of extensive research to solve the above problems, the inventors discovered that by making the thickness of the edge region of a thermoelectric wafer greater than the thickness of the recessed region surrounded by the edge region, it is possible to suppress cracks, breakage, etc. that occur in the thermoelectric wafer due to mechanical strength, and thus completed the present invention. That is, the present invention provides the following [1] to [5]. [1] A thermoelectric wafer comprising a thermoelectric element layer including a thermoelectric semiconductor material, the thermoelectric wafer having an edge region and a recessed region surrounded by the edge region, the thickness of the edge region being greater than the thickness of the recessed region. [2] The thermoelectric wafer according to [1] above, wherein the ratio of the length of the end region of the thermoelectric wafer in the direction of the recessed region to the maximum distance from the edge of the thermoelectric wafer to approximately the center of the thermoelectric wafer is 0.001 or more. [3] A thermoelectric wafer according to [1] or [2] above, wherein the ratio of the thickness of the edge region to the minimum thickness of the recessed region is 1.01 or greater. [4] A method for producing a thermoelectric wafer, comprising the following steps (A) to (C): (A) A step of obtaining a coating film formed from a thermoelectric semiconductor composition containing a thermoelectric semiconductor material (B) a step of subjecting the coating film to a heating and pressurizing treatment in a region other than the edge region to form a recessed region surrounded by the edge region, thereby obtaining a thermoelectric wafer precursor. (C) A step of sintering the thermoelectric wafer precursor to obtain a thermoelectric wafer comprising a thermoelectric element layer. The method for manufacturing a thermoelectric wafer, wherein the thermoelectric wafer comprises an edge region of the thermoelectric wafer and a recessed region surrounded by the edge region, the thickness of the edge region being greater than the thickness of the recessed region. [5] The method for producing a thermoelectric wafer according to the above [4], wherein the thermoelectric element layer is made of a thermoelectric semiconductor composition containing the thermoelectric semiconductor material, a binder resin, and an ionic compound. Effect of the Invention

[0007] According to the present invention, it is possible to provide a thermoelectric wafer having excellent mechanical strength and a method for manufacturing the same. [Brief description of the drawings]

[0008] [Figure 1] FIG. 2 is an explanatory diagram showing an example of a thermoelectric wafer of the present invention. [Diagram 2] 1A to 1C are explanatory views showing an example of steps according to a method for producing a thermoelectric wafer of the present invention in the order of steps. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0009] [Thermoelectric wafer] The thermoelectric wafer of the present invention is a thermoelectric wafer consisting of a thermoelectric element layer containing a thermoelectric semiconductor material, and is characterized in that the thermoelectric wafer has an edge region and a recessed region surrounded by the edge region, and the thickness of the edge region is greater than the thickness of the recessed region. In the present invention, by making the thickness of the edge region of the thermoelectric wafer greater than the thickness of the recessed region surrounded by the edge region, the mechanical strength of the edge region can be increased, and cracks and breakages, etc., that occur in the thermoelectric wafer due to mechanical damage, etc. that occurs during handling in the manufacturing process or during processing in later processes can be suppressed.

[0010] In this specification, a film made of a thermoelectric semiconductor composition before drying may be simply referred to as a "composition film", and a film after drying may be simply referred to as a "coating film". Furthermore, a film obtained by compressing after heating and pressurizing treatment may be simply referred to as a "thermoelectric wafer precursor". Furthermore, a film obtained after firing a thermoelectric wafer precursor may be simply referred to as a "thermoelectric element layer" or a "thermoelectric wafer". Furthermore, chips obtained by singulating a thermoelectric wafer may be simply referred to as a "thermoelectric chip" or "chip".

[0011] In this specification, preferred definitions may be selected arbitrarily, and combinations of preferred definitions may be considered more preferred. In this specification, the expression "XX to YY" means "at least XX and at most YY." In this specification, the lower limit and upper limit described in stages for the preferred numerical range (e.g., the range of the content, etc.) can be independently combined. For example, the description "preferably 10 to 90, more preferably 30 to 60" can be combined with the "preferable lower limit (10)" and the "more preferable upper limit (60)" to form "10 to 60."

[0012] FIG. 1 is an explanatory diagram showing an example of a thermoelectric wafer of the present invention, in which (a) is a plan view of a thermoelectric wafer 1 and (b) is a cross-sectional view of the thermoelectric wafer 1. The thermoelectric wafer 1 is a circular wafer having an edge region 2 and a recessed region 3 surrounded by the edge region 2, where D is the diameter, P is the length of the edge region 2, C1 is the thickness of the edge region 2, Q is the diameter of the recessed region 3, and C2 is the thickness of the recessed region 3.

[0013] The ratio of the length of the end region of the thermoelectric wafer in the direction of the recessed region to the maximum distance from the end to approximately the center of the thermoelectric wafer is preferably 0.001 or more, more preferably 0.01 to 0.20, and even more preferably 0.03 to 0.10. When the ratio of the length of the end region of the thermoelectric wafer in the direction of the recessed region to the maximum distance from the edge of the thermoelectric wafer to approximately the center is within this range, a reduction in the effective area of ​​the thermoelectric wafer is suppressed, and the number of thermoelectric chips (with the same specifications) obtained by dicing the thermoelectric wafer can be maintained. Here, the "maximum distance from the edge to the approximate center of the thermoelectric wafer" means, for example, the distance from the circumferential edge to the center of the circle when the shape of the thermoelectric wafer is circular as shown in Fig. 1. Also, for example, when the shape of the thermoelectric wafer is rectangular as described below, it means the distance from each corner of the rectangle to the intersection of the diagonal lines.

[0014] The ratio of the thickness of the edge region to the minimum thickness of the recessed region of the thermoelectric wafer is preferably 1.01 or more, more preferably 1.01 to 3.00, even more preferably 1.10 to 2.50, and particularly preferably 1.20 to 2.00. When the ratio of the thickness of the end region to the minimum thickness of the recessed region of the thermoelectric wafer is within this range, it becomes easier to improve the mechanical strength of the end portion of the thermoelectric wafer.

[0015] When the ratio of the thickness of the end region to the minimum thickness of the recessed region of the thermoelectric wafer, and the ratio of the length of the end region of the thermoelectric wafer in the direction of the recessed region to the maximum distance from the edge of the thermoelectric wafer to approximately the center are both within the above ranges, it is possible to maintain the number of thermoelectric chips (with the same specifications) obtained by dicing the thermoelectric wafer, and to suppress the occurrence of cracks and breakage at the end of the thermoelectric wafer.

[0016] The thickness of a thermoelectric wafer consisting of a thermoelectric element layer obtained by the firing treatment described below, that is, the thickness of the recessed area of ​​the thermoelectric wafer, is preferably 10 to 800 μm, more preferably 15 to 600 μm, and further preferably 20 to 420 μm. When the thickness of the thermoelectric wafer is within this range, the wafer is mechanically stable, and the occurrence of defects such as cracks and warping is easily suppressed.

[0017] The shape of the thermoelectric wafer is not particularly limited, but may be a circle, an ellipse, a square, a rectangle, or the like. The size of the thermoelectric wafer is not particularly limited, but from the viewpoint of mass-producing a plurality of chips at once, the diameter is 30 mm to 500 mm for a circle, and each side is 10 mm to 500 mm for a square or rectangle.

[0018] (Support) In the present invention, it is preferable to use a support as a support for the coating film. The support is not particularly limited, and examples thereof include glass, silicon, ceramics, and resin films, etc. From the viewpoint of flexibility, resin films are preferred, and further, from the viewpoint of heat resistance, heat-resistant resin films are more preferred. The heat-resistant resin film is not particularly limited, but a polyimide film, a polyamide film, a polyetherimide film, a polyaramid film, a polyamideimide film, or a fluorine-based film (polytetrafluoroethylene, a tetrafluoroethylene-hexafluoropropylene copolymer, a tetrafluoroethylene-perfluoroalkylvinyl ether copolymer) is preferable, and further, a polyimide film is particularly preferable because of its high versatility. From the viewpoints of flexibility, heat resistance, and dimensional stability, the thickness of the heat-resistant resin film is preferably 50 to 1000 μm, more preferably 75 to 500 μm, and even more preferably 100 to 200 μm. The glass transition temperature (Tg) of the heat-resistant resin film is preferably 200° C. or higher, more preferably 220° C. or higher, and even more preferably 250° C. or higher. Here, Tg refers to the temperature at the maximum point of tan δ (loss modulus / storage modulus) obtained by a differential scanning calorimeter (measured in the range of 0 to 500° C. at a heating rate of 5° C. / min).

[0019] <Thermoelectric element layer> The thermoelectric wafer used in the present invention is composed of a thermoelectric element layer. The thermoelectric element layer is preferably formed from a thermoelectric semiconductor composition containing a thermoelectric semiconductor material (hereinafter sometimes referred to as "thermoelectric semiconductor particles"), a binder resin, and an ionic compound (ionic liquid, inorganic ionic compound).

[0020] (Filling rate) The thermoelectric element layer constituting the thermoelectric wafer of the present invention may contain voids that contain air trapped during the formation of the coating film and gas components derived from the binder resin during heating. When the filling rate is defined as the ratio of the area of ​​the thermoelectric conversion material to the area of ​​a vertical cross section including the center of the thermoelectric element layer (the remaining area is considered as voids), the filling rate is preferably 0.900 to 0.999, more preferably 0.920 to 0.990, and further preferably 0.940 to 0.980. When the filling rate is within this range, the electrical resistivity of the thermoelectric conversion material in the thermoelectric element layer can be reduced, and the thermoelectric performance of the thermoelectric element layer can be improved. In the definition of the filling rate, the thermoelectric conversion material means the thermoelectric element layer excluding voids. The filling rate can be measured by the filling rate evaluation described in the Examples.

[0021] (Thermoelectric semiconductor materials) The thermoelectric semiconductor material is preferably pulverized to a predetermined size using, for example, a fine grinding device, and then used as thermoelectric semiconductor particles. The particle size of the thermoelectric semiconductor particles is preferably 10 nm to 100 μm, more preferably 50 nm to 50 μm, and further preferably 3 μm to 30 μm. The average particle size of the thermoelectric semiconductor particles was obtained by measurement using a laser diffraction particle size analyzer (Malvern, Mastersizer 3000) and was taken as the median value of the particle size distribution.

[0022] As the thermoelectric semiconductor material used in the present invention, there is no particular limitation as long as it can generate a thermoelectromotive force by applying a temperature difference. For example, bismuth-telluride-based thermoelectric semiconductor materials such as P-type bismuth telluride and N-type bismuth telluride; telluride-based thermoelectric semiconductor materials such as GeTe and PbTe; antimony-telluride-based thermoelectric semiconductor materials; zinc-antimony-based thermoelectric semiconductor materials such as ZnSb and Zn3Sb 2、 Zn4Sb3; silicon-germanium-based thermoelectric semiconductor materials such as SiGe; bismuth selenide-based thermoelectric semiconductor materials such as Bi2Se3; β-FeSi2, CrSi2, MnSi 1.73 , Mg2Si and other silicide-based thermoelectric semiconductor materials; oxide-based thermoelectric semiconductor materials; Heusler materials such as FeVAl, FeVAlSi, FeVTiAl, and sulfide-based thermoelectric semiconductor materials such as TiS2 are used.

[0023] Among these, the thermoelectric semiconductor material used in the present invention is preferably a bismuth-telluride-based thermoelectric semiconductor material such as P-type bismuth telluride or N-type bismuth telluride. In the P-type bismuth telluride, the carriers are holes and the Seebeck coefficient is a positive value. For example, Bi X Te3Sb 2-X represented by is preferably used. In this case, X is preferably 0 < X ≦ 0.8, more preferably 0.4 ≦ X ≦ 0.6. When X is greater than 0 and less than or equal to 0.8, the Seebeck coefficient and electrical conductivity increase, and the characteristics as a P-type thermoelectric conversion material are maintained, which is preferable. Further, in the N-type bismuth telluride, the carriers are electrons and the Seebeck coefficient is a negative value. For example, Bi2Te 3-Y Se Y represented by is preferably used. In this case, Y is preferably 0 ≦ Y ≦ 3 (when Y = 0: Bi2Te3), more preferably 0.1 < Y ≦ 2.7. When Y is 0 to 3, the Seebeck coefficient and electrical conductivity increase, and the characteristics as an N-type thermoelectric conversion material are maintained, which is preferable.

[0024] The content of the thermoelectric semiconductor particles in the thermoelectric semiconductor composition is preferably 30 to 99% by mass, more preferably 50 to 96% by mass, and even more preferably 70 to 95% by mass. If the content of the thermoelectric semiconductor particles is within the above range, the Seebeck coefficient (absolute value of the Peltier coefficient) is large, and the decrease in electrical conductivity is suppressed, and only the thermal conductivity decreases, so that a film exhibiting high thermoelectric performance and having sufficient film strength and flexibility can be obtained, which is preferable.

[0025] Moreover, the thermoelectric semiconductor particles are preferably those that have been subjected to an annealing treatment (hereinafter sometimes referred to as "annealing treatment A"). By carrying out annealing treatment A, the crystallinity of the thermoelectric semiconductor particles is improved, and further, the surface oxide film of the thermoelectric semiconductor particles is removed, so that the Seebeck coefficient (absolute value of the Peltier coefficient) of the thermoelectric conversion material is increased, and the thermoelectric figure of merit can be further improved.

[0026] (binder resin) The binder resin used in the present invention has the effect of physically binding the thermoelectric semiconductor material (thermoelectric semiconductor particles) together, and can increase the flexibility of the thermoelectric conversion module while facilitating the formation of a thin film by coating or the like.

[0027] The binder resin is appropriately selected depending on the temperature of the heat treatment of the thermoelectric semiconductor material and the baking (annealing) temperature. It is preferable to heat the material at a temperature higher than the decomposition temperature of the binder resin. Furthermore, it is more preferable to use a resin that maintains various physical properties such as mechanical strength and thermal conductivity without being impaired when the coating film made of the thermoelectric semiconductor composition is subjected to a heat treatment or the like to cause crystal growth of the thermoelectric semiconductor particles. In this specification, the term "decomposition temperature" refers to the temperature at which the mass reduction rate by thermogravimetry (TG) is 100% (the mass after decomposition is less than 1% of the mass before decomposition). The decomposition temperature of the binder resin is preferably 150 to 400°C.

[0028] As such a binder resin, a thermoplastic resin or a curable resin can be used. Examples of the thermoplastic resin include polyolefin resins such as polyethylene, polypropylene, polyisobutylene, and polymethylpentene; polycarbonate; thermoplastic polyester resins such as polyethylene terephthalate and polyethylene naphthalate; polyvinyl polymers such as polystyrene, acrylonitrile-styrene copolymer, polyvinyl acetate, ethylene-vinyl acetate copolymer, vinyl chloride, polyvinylpyridine, polyvinyl alcohol, and polyvinylpyrrolidone; polyurethane; and cellulose derivatives such as ethyl cellulose. Examples of the curable resin include thermosetting resins and photocurable resins. Examples of the thermosetting resin include epoxy resins and phenolic resins. Examples of the photocurable resin include photocurable acrylic resins, photocurable urethane resins, and photocurable epoxy resins. These may be used alone or in combination of two or more. Among these, thermoplastic resins are preferred, polycarbonate and cellulose derivatives such as ethyl cellulose are more preferred, and polycarbonate is particularly preferred.

[0029] The content of the binder resin in the thermoelectric semiconductor composition is preferably 0.1 to 20 mass %, more preferably 0.5 to 15 mass %, and further preferably 1.0 to 10 mass %.

[0030] <Ionic Compounds> (Ionic Liquid) The ionic liquid that can be contained in the thermoelectric semiconductor composition is a molten salt formed by combining a cation and an anion, and refers to a salt that can exist in a liquid state in any temperature range from -50°C to less than 400°C. Ionic liquids have characteristics such as extremely low vapor pressure and nonvolatility, excellent thermal stability and electrochemical stability, low viscosity, and high ionic conductivity, and therefore can effectively suppress the reduction in electrical conductivity between thermoelectric semiconductor materials as a conductive auxiliary. In addition, ionic liquids exhibit high polarity based on an aprotic ionic structure and have excellent compatibility with binder resins, so that the electrical conductivity of the thermoelectric element layer can be made uniform.

[0031] The ionic liquid may be a known or commercially available one. For example, a mixture of a cationic component such as a pyridinium, pyrimidinium, pyrazolium, pyrrolidinium, piperidinium, imidazolium, etc., and a derivative thereof; a tetraalkylammonium-based amine-based cation and a derivative thereof; a phosphine-based cation such as a phosphonium, trialkylsulfonium, tetraalkylphosphonium, etc., and a derivative thereof; a lithium cation and a derivative thereof; and a mixture of a Cl cation and ... - , Br - , I - , AlCl4 - , Al2Cl7 - , BF4 - , PF6 - , ClO4 - , NO3 - , CH3COO - , CF3COO - , CH3SO3 - , CF3SO3 - , (FSO2)2N - , (CF3SO2)2N - , (CF3SO2)3C - , AsF6 - , SbF6 - , NbF6 - , TaF6 - , F(HF) n - , (CN)2N - , C4F9SO3 - , (C2F5SO2)2N- , C3F7COO - , (CF3SO2)(CF3CO)N - and an anion component such as the above.

[0032] The ionic liquid preferably has a decomposition temperature of 300° C. or higher. If the decomposition temperature is within the above range, the effect as a conductive auxiliary agent can be maintained even when a coating film made of the thermoelectric semiconductor composition is annealed, as described below.

[0033] The content of the ionic liquid in the thermoelectric semiconductor composition is preferably 0.01 to 50 mass%, more preferably 0.4 to 30 mass%, and further preferably 0.8 to 20 mass%. When the content of the ionic liquid is within the above range, the decrease in electrical conductivity is effectively suppressed, and a film having high thermoelectric performance is obtained.

[0034] (Inorganic ionic compounds) The inorganic ionic compound that can be contained in the thermoelectric semiconductor composition is a compound composed of at least a cation and an anion. The inorganic ionic compound exists in a solid state in a wide temperature range of 400 to 900°C and has characteristics such as high ionic conductivity, so that it can suppress the decrease in electrical conductivity between thermoelectric semiconductor materials as a conductive auxiliary.

[0035] The content of the inorganic ionic compound in the thermoelectric semiconductor composition is preferably 0.01 to 50 mass%, more preferably 0.5 to 30 mass%, and further preferably 1.0 to 10 mass%. If the content of the inorganic ionic compound is within the above range, the decrease in electrical conductivity can be effectively suppressed, and as a result, a film with improved thermoelectric performance can be obtained. In addition, when an inorganic ionic compound and an ionic liquid are used in combination as the ionic compound, the total content of the inorganic ionic compound and the ionic liquid in the thermoelectric semiconductor composition is preferably 0.01 to 50 mass%, more preferably 0.5 to 30 mass%, and even more preferably 1.0 to 10 mass%.

[0036] The thickness of the coating film made of the thermoelectric semiconductor composition is preferably 10 to 1000 μm, more preferably 20 to 800 μm, and further preferably 30 to 650 μm.

[0037] <Solder acceptance layer> The solder-receiving layer has a function of joining the thermoelectric conversion material layer and the solder material layer on the opposing electrode side that constitutes the thermoelectric conversion module, and is directly joined to the thermoelectric conversion material layer.

[0038] The solder-receiving layer preferably contains a metal material. The metal material is preferably at least one selected from gold, silver, nickel, aluminum, rhodium, platinum, chromium, palladium, tin, and an alloy containing any of these metal materials. Among these, a two-layer structure of gold, silver, nickel, aluminum, or tin and gold is preferable, and from the viewpoints of material cost, high thermal conductivity, and bonding stability, silver, nickel, and aluminum are more preferable.

[0039] The thickness of the solder-receiving layer is preferably 10 nm to 50 μm, more preferably 50 nm to 16 μm, further preferably 200 nm to 4 μm, and particularly preferably 500 nm to 3 μm. When the thickness of the solder-receiving layer is within this range, the adhesion to the surface of the thermoelectric conversion material layer and the adhesion to the surface of the solder material layer on the electrode side constituting the thermoelectric conversion module are excellent, and a highly reliable bond can be obtained. In addition, since the electrical conductivity as well as the thermal conductivity can be maintained at a high level, the thermoelectric performance of the thermoelectric conversion module is maintained without being reduced. The solder-receiving layer may be a single layer formed by directly depositing a metal material, or may be a multilayer formed by laminating two or more metal materials.

[0040] [Method of Manufacturing Thermoelectric Wafer] The method for producing a thermoelectric wafer of the present invention includes the following steps (A) to (C): (A) A step of obtaining a coating film formed from a thermoelectric semiconductor composition containing a thermoelectric semiconductor material (B) a step of subjecting the coating film to a heating and pressurizing treatment in a region other than the edge region to form a recessed region surrounded by the edge region, thereby obtaining a thermoelectric wafer precursor. (C) A step of sintering the thermoelectric wafer precursor to obtain a thermoelectric wafer comprising a thermoelectric element layer. The thermoelectric wafer is characterized by comprising an edge region of the thermoelectric wafer and a recessed region surrounded by the edge region, the edge region having a thickness greater than a thickness of the recessed region.

[0041] In the following description, step (A), step (B), and step (C) may also be referred to as a "coating step," a "heating and pressurizing step," and a "firing step," respectively, in that order. The method for producing a thermoelectric wafer according to the present invention will now be described with reference to the drawings.

[0042] FIG. 2 is an explanatory diagram showing an example of steps according to the manufacturing method of a thermoelectric wafer of the present invention in the order of steps, in which (a) is a cross-sectional configuration diagram including a coating film 12 formed from a thermoelectric semiconductor composition on a support 11, (b) is a cross-sectional configuration diagram showing an embodiment in which the coating film 12 and a heating and pressing jig 13 are opposed to each other, (c) is a cross-sectional configuration diagram showing an embodiment in which the coating film 12 is heated and pressed from both sides of the support 11 and the coating film 12 using a heating and pressing device (not shown), (d) is a cross-sectional configuration diagram showing an embodiment including a thermoelectric wafer precursor 14 obtained by the heating and pressing treatment, (e) is a cross-sectional configuration diagram showing an embodiment after the heating and pressing jig 13 has been released from the thermoelectric wafer precursor 14, and (f) is a cross-sectional configuration diagram of a thermoelectric wafer 15 obtained after the support 11 has been peeled off and the thermoelectric wafer precursor 14 has been subjected to a firing treatment.

[0043] Process (A): Coating process The method for producing a thermoelectric wafer of the present invention includes a coating step. The coating step is a step of forming a composition film on a support from a thermoelectric semiconductor composition containing a thermoelectric semiconductor material, and drying the composition film to obtain a coating film. For example, in the above-mentioned FIG. 2(a), it is a step of obtaining a coating film 12 formed from a thermoelectric semiconductor composition on a support 11.

[0044] The details of the thermoelectric semiconductor composition containing the thermoelectric semiconductor material used for forming the coating film are as described above.

[0045] The method of applying the thermoelectric semiconductor composition as a composition film includes known methods such as screen printing, flexographic printing, gravure printing, spin coating, dip coating, die coating, spray coating, bar coating, applicator, and doctor blade methods, and is not particularly limited. The resulting composition film is then dried to form a coating film. As the drying method, a conventionally known drying method such as hot air drying, heat roll drying, infrared irradiation, etc. can be used. The heating temperature is usually 80 to 150°C, and the heating time varies depending on the heating method, but is usually several seconds to several tens of minutes. Furthermore, when a solvent is used in the preparation of the thermoelectric semiconductor composition, the heating temperature is not particularly limited as long as it is within a temperature range in which the solvent used can be dried.

[0046] The thermoelectric wafer may be further annealed (hereinafter, sometimes referred to as "annealing treatment B") as necessary, even after the firing treatment described later. By carrying out the annealing treatment B, the thermoelectric performance can be further stabilized, and the thermoelectric semiconductor particles in the thermoelectric conversion material wafer can be further crystal-grown, thereby further improving the thermoelectric performance. The annealing treatment B is not particularly limited, but is usually carried out under an inert gas atmosphere such as nitrogen or argon with a controlled gas flow rate, under a reducing gas atmosphere, or under vacuum conditions, and is carried out at 100 to 500°C for several minutes to several tens of hours, depending on the heat-resistant temperature of the thermoelectric semiconductor composition used.

[0047] Step (B): Heat and pressure step The method for producing a thermoelectric wafer of the present invention includes a heating and pressurizing step. The heating and pressurizing step is a step of subjecting the coating film to a heating and pressurizing treatment. For example, in (b) and (c) of FIG. 2 described above, a heating and pressurizing device (not shown) is used to perform a heating and pressurizing treatment on the coating film 12 from both sides of the support 11 and the coating film 12 via a heating and pressurizing jig 13 to form a recessed region surrounded by the end region of the coating film 12, and in (c), further pressure compression is performed to obtain a thermoelectric wafer precursor 14 in which the thickness of the coating film is reduced.

[0048] The heating and pressurizing treatment in the heating and pressurizing step can be carried out by a known method, for example, by using a hydraulic press, a vacuum press, or the like. The heating temperature is 100 to 400° C., and the pressure is 40 to 300 MPa. The heating and pressurizing treatment time is not particularly limited, but is preferably from a few seconds to a few hours, and more preferably from a few minutes to a few tens of minutes.

[0049] Step (C): Firing process The method for producing a thermoelectric wafer of the present invention includes a firing process. The firing treatment step is a step of firing the thermoelectric wafer precursor formed from the coating film compressed in step (B) to obtain a thermoelectric wafer consisting of a thermoelectric element layer. For example, in (d) of FIG. 2 described above, thermoelectric wafer precursor 14 obtained by heating and pressurizing treatment and compression is peeled off from support 11, and in (e) the thermoelectric wafer precursor 14 is fired to obtain thermoelectric wafer 15 consisting of a thermoelectric element layer. By carrying out the firing treatment, the thermoelectric performance can be stabilized and the thermoelectric semiconductor particles in the thermoelectric semiconductor composition in the coating film can be caused to undergo crystal growth, thereby further improving the thermoelectric performance of the thermoelectric wafer consisting of the thermoelectric element layer.

[0050] The calcination treatment is not particularly limited, but is usually carried out under an inert gas atmosphere such as nitrogen or argon, under a reducing gas atmosphere, or under vacuum conditions with the gas flow rate controlled. The temperature of the firing treatment depends on the thermoelectric semiconductor particles, resin, ionic compounds (ionic liquids, inorganic ionic compounds), etc. used in the thermoelectric semiconductor composition and is adjusted appropriately, but is usually 260 to 600°C, preferably 280 to 550°C. The time for the firing treatment is not particularly limited, but is usually from several minutes to several tens of hours, and preferably from several minutes to several hours.

[0051] The method for producing a thermoelectric conversion material wafer of the present invention preferably further comprises a solder-receiving layer forming step as a post-step. The solder-receiving layer forming step is a step of obtaining a solder-receiving layer by performing plating or the like on the thermoelectric wafer, that is, the thermoelectric element layer. The solder receiving layer has a function of joining the thermoelectric element layer and the solder material layer on the opposing electrode side that constitutes the thermoelectric conversion module, and is directly joined to the thermoelectric element layer.

[0052] The metal material used to form the solder-receiving layer, the thickness of the solder-receiving layer, etc. are as described above.

[0053] The solder-receiving layer is preferably formed using the above-mentioned metal material. Since the solder-receiving layer is required to have high electrical conductivity and high thermal conductivity in order to maintain thermoelectric performance, it is preferable to use a solder-receiving layer formed by electrolytic plating, electroless plating, or vacuum film formation.

[0054] The thermoelectric wafer produced by the method for producing a thermoelectric wafer of the present invention, or the thermoelectric wafer having a solder-receiving layer formed thereon, may be further divided into individual pieces in a dicing step. The dicing step is a step of dividing the thermoelectric wafer into individual thermoelectric chips. From the viewpoint of processing accuracy and process stability, the division is preferably performed by attaching the thermoelectric wafer to a dicing tape and using a dicing blade. The thermoelectric wafer of the present invention and the thermoelectric wafer produced by the method for producing the same cause few chips to fly off during dicing, and therefore the production yield of the resulting thermoelectric chips is improved.

[0055] (Manufacture of thermoelectric conversion modules) A thermoelectric conversion module can be manufactured by combining multiple thermoelectric chips (P-type thermoelectric chips, N-type thermoelectric chips) described above obtained by dicing a thermoelectric wafer produced by the thermoelectric wafer manufacturing method of the present invention, or a thermoelectric wafer having a solder receiving layer formed thereon. From the standpoint of thermoelectric performance, the thermoelectric conversion module can be manufactured by mounting (arranging) a P-type thermoelectric chip and an N-type thermoelectric chip so that they are connected via electrodes to form a so-called π-type or in-plane type thermoelectric conversion module. EXAMPLES

[0056] The present invention will now be described in more detail with reference to examples, but the present invention is not limited to these examples in any way.

[0057] The occurrence of edge cracks in the thermoelectric wafers produced in the Examples and Comparative Examples and the suitability of the thermoelectric wafers including the solder-receiving layer for post-processing were evaluated by the following methods.

[0058] (a) Edge crack evaluation For the thermoelectric wafers obtained in the examples and comparative examples, edge cracks were measured using an ultrasonic flaw detection device (manufactured by Burns Japan, model name "C-SAM D9600"), and the obtained analysis image was binarized using image processing software (manufactured by National Institutes of Health, ImageJ ver.1.44P) by setting the contrast to the maximum value in "Brightness / Contrast." The dark areas in the binarization process were regarded as crack areas, and the bright areas as thermoelectric semiconductor material in the thermoelectric element layer, and the edge cracks were evaluated according to the following criteria. A: No cracks (edge ​​cracks) were observed in the edge region of the thermoelectric wafer. B: One or more cracks were identified in the edge region of the thermoelectric wafer (edge ​​cracks).

[0059] (b) Post-process suitability evaluation A thermoelectric wafer having two solder-receiving layers was fabricated by sequentially providing a nickel layer (thickness: 5 μm) as the first layer and a gold layer (thickness: 40 nm) as the second layer by electroless plating on the thermoelectric wafers obtained in the examples and comparative examples. The thermoelectric wafer with the solder-receiving layer was attached to a dicing tape, and cracks in the thermoelectric wafer were observed using a digital microscope (manufactured by Keyence Corporation, model name: VHX-5000, magnification: 20 times), and the cracks were evaluated according to the following criteria. P: No cracks (edge ​​cracks) were found in the edge region of the thermoelectric wafer, and the wafer was suitable for post-processing. Q: One or more cracks (edge ​​cracks) were found in the edge region of the thermoelectric wafer, making it unsuitable for post-processing.

[0060] (c) Filling rate evaluation The thermoelectric wafers obtained in the examples and comparative examples were diced into individual rectangular parallelepipeds (10 mm x 10 mm) to form thermoelectric element layers. A longitudinal section including the center of the thermoelectric element layer was cut out using a polishing device (manufactured by Refine Tech Co., Ltd., model name: Refine Polisher HV) and the longitudinal section was observed using a scanning electron microscope (SEM) (manufactured by Keyence Corporation). Next, the proportion of the area of ​​the thermoelectric conversion material in the area of ​​the longitudinal section of the thermoelectric element layer (filling rate) was calculated using image processing software (manufactured by National Institutes of Health, ImageJ ver.1.44P). To measure the filling rate, a 500x magnification SEM image (longitudinal cross section) was used, and the measurement range was set to an arbitrary position on the thermoelectric element layer, surrounded by 1280 pixels in the width direction and 220 pixels in the thickness direction, and the image was cut out. The cut-out image was binarized by setting the contrast to the maximum value in "Brightness / Contrast", and the dark areas in the binarization process were considered to be voids and the bright areas were considered to be thermoelectric conversion material, and the filling rate of the thermoelectric conversion material was calculated using "Threshold". The filling rate was calculated for three SEM images and the average value was calculated.

[0061] Example 1 <Preparation of thermoelectric wafer> (1) Preparation of coating solution for thermoelectric semiconductor composition As a thermoelectric semiconductor particle, P-type bismuth telluride Bi 0.4 Te 3.0 Sb 1.6 A coating liquid was prepared consisting of a thermoelectric semiconductor composition in which 78.5 parts by mass of particles (average particle size 16.0 μm), 15.5 parts by mass of polyethylene carbonate (decomposition temperature: 250 ° C.) as a binder resin, 0.8 parts by mass of N-butylpyridinium bromide as an ionic liquid, which is an ionic compound, and 5.18 parts by mass of N-methylpyrrolidone as a solvent were mixed and dispersed. The average particle size of the particles was determined by particle size distribution measurement using a laser diffraction particle size analyzer (Malvern, Mastersizer 3000). (2) Preparation of thermoelectric wafer The coating solution prepared in (1) was applied onto a polyimide film (Ube Industries, product name "Kapton 500H", 100 mm x 160 mm x 125 μm thick) using a screen printer, and the film was dried by heating at a temperature of 110° C. for 20 minutes to form a coating film with a thickness of 600 μm. Next, the coating film and the polyimide film were punched into a circle with a diameter of 60 mm (radius of 30 mm) using a hand press machine (Dumbbell, model name: SDL-100). Next, a SUS plate (SUS304, thickness: 20 mm) having a diameter of 60 mm and a groove 100 μm deep in an area of ​​1 mm around the periphery was placed opposite the surface of the coating film opposite the surface in contact with the polyimide film, and then heated and pressurized at 250°C and 50 MPa for 15 minutes using an electric heater press (heating and pressing device) (manufactured by Sansho Industry Co., Ltd., model name: 500 kN) to compress the thickness of the edge area 1 mm around the periphery of the coating film to 380 μm, and the thickness of the recessed area surrounded by the edge area 1 mm around the periphery to 285 μm, thereby obtaining a thermoelectric wafer precursor. Furthermore, the thermoelectric wafer precursor peeled off from the polyimide film was heated at a heating rate of 5 K / min in an atmosphere of a mixed gas of hydrogen and argon (hydrogen:argon = 3 vol%:97 vol%) and held at a baking (annealing) temperature of 430°C for 30 minutes to produce a thermoelectric wafer.

[0062] Comparative Example 1 In Example 1, a SUS plate having a diameter of 60 mm and a groove 100 μm deep in a 1 mm region on the outer periphery was replaced with a SUS plate of the same specifications but without a groove, and a heat and pressure treatment was performed to compress the thickness of the 1 mm edge region, which is the outer periphery of the thermoelectric wafer precursor, to 283 μm and the thickness of the region surrounded by the edge region to 289 μm. A thermoelectric wafer was produced in the same manner as in Example 1.

[0063] The results of the edge crack evaluation, post-processing suitability evaluation, and filling rate evaluation of the thermoelectric wafers obtained in Example 1 and Comparative Example 1 are shown in Table 1.

[0064] [Table 1]

[0065] It can be seen that the thermoelectric wafer of Example 1, which satisfies the specification of the present invention in which the thickness of the edge region is greater than the thickness of the recessed region, does not suffer from edge cracks and is also well suited for subsequent processes such as the process of forming a solder-receiving layer and the process of attaching to a dicing tape, compared to the thermoelectric wafer of Comparative Example 1, which does not satisfy the specification of the present invention. [Industrial Applicability]

[0066] According to the thermoelectric wafer of the present invention, since it is a thermoelectric wafer having excellent mechanical strength and has suitability for post-processing, the thermoelectric wafer can be mass-produced in one go and can be divided into individual pieces and used as thermoelectric chips of a thermoelectric conversion module. For example, it can be applied to power generation applications in which exhaust heat from various combustion furnaces such as factories, waste combustion furnaces, and cement combustion furnaces, exhaust heat from automobile combustion gases, and exhaust heat from electronic devices are converted into electricity. For cooling purposes, it can be applied to the temperature control of various sensors such as CPUs (Central Processing Units) used in smartphones and various computers in the field of electronic equipment, CMOS (Complementary Metal Oxide Semiconductors), CCD (Charge Coupled Devices), and further MEMS (Micro Electro Mechanical Systems), light receiving elements, and the like. [Explanation of symbols]

[0067] 1: Thermoelectric wafer (thermoelectric element layer) 2: End area 3: Concave area 4: Thermoelectric wafer (thermoelectric element layer) 11:Support 12: Coating film 13: Heat and pressure jig 14: Thermoelectric wafer precursor 15: Thermoelectric wafer D: diameter of the thermoelectric wafer Q: Diameter of the recessed area P: Length of the end region C1: Thickness of the edge region C2: Thickness of the recessed area

Claims

1. 1. A thermoelectric wafer comprising a thermoelectric element layer including a thermoelectric semiconductor material, the thermoelectric wafer having an edge region and a recessed region surrounded by the edge region, the thickness of the edge region being greater than the thickness of the recessed region.

2. 2. The thermoelectric wafer of claim 1, wherein a ratio of a length of the end region of the thermoelectric wafer in the direction of the recessed region to a maximum distance from an end of the thermoelectric wafer to an approximate center of the thermoelectric wafer is 0.001 or more.

3. 10. The thermoelectric wafer of claim 1 , wherein a ratio of the thickness of said edge region to the minimum thickness of said recessed region is greater than or equal to 1.

01.

4. A method for producing a thermoelectric wafer, comprising the following steps (A) to (C): (A) A step of obtaining a coating film formed from a thermoelectric semiconductor composition containing a thermoelectric semiconductor material (B) A step of subjecting the coating film to a heating and pressurizing treatment in a region other than the edge region to form a recessed region surrounded by the edge region, thereby obtaining a thermoelectric wafer precursor. (C) A step of sintering the thermoelectric wafer precursor to obtain a thermoelectric wafer comprising a thermoelectric element layer. The method for manufacturing a thermoelectric wafer, wherein the thermoelectric wafer comprises an edge region of the thermoelectric wafer and a recessed region surrounded by the edge region, the thickness of the edge region being greater than the thickness of the recessed region.

5. The method for producing a thermoelectric wafer according to claim 4 , wherein the thermoelectric element layer is made of a thermoelectric semiconductor composition containing the thermoelectric semiconductor material, a binder resin, and an ionic compound.

Citation Information

Patent Citations

  • Composite having doped fibrous semiconductor material and filler

    JP2018085441A