Laminated film

The laminated film with a resin, adhesive, and surface protection layers addresses the issue of insufficient adhesive strength and durability in surface protection sheets by providing anti-scattering and anti-slip/peeling properties, ensuring safety and durability.

JP2024143554APending Publication Date: 2024-10-11NIPPON PAINT AUTOMOTIVE COATINGS
View PDF 1 Cites 0 Cited by

Patent Information

Application Number
JP2023056292
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Filing Date
2023-03-30
Publication Date
2024-10-11

AI Technical Summary

Technical Problem

Surface protection sheets applied to adherends lack sufficient adhesive strength and durability, leading to potential peeling or scattering when impacted, posing safety risks.

Method used

A laminated film comprising a resin layer, adhesive layer, and surface protection layer, with specific properties such as elongation at break, heat resistance, and adhesive strength ratios, ensuring anti-scattering, durability, and anti-slip/peeling properties.

Benefits of technology

The laminated film provides enhanced adhesive strength, creep resistance, and impact resistance, preventing scattering and peeling of adherends, thereby ensuring safety and durability.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024143554000001_ABST
    Figure 2024143554000001_ABST
Patent Text Reader

Abstract

To provide a laminated film having scattering prevention properties, durability (creep resistance) and displacement / peeling prevention performance when adhered to the surface of an adherend.SOLUTION: The elongation at break of the laminated film to an adherend under the condition of a tensile speed of 300 [mm / min] is 300 [%] to 1500 [%], the displacement amount of the laminated film after 80[°C] heat resistance test to the laminated film is 10 [mm] or less, AF(10) and AF(200) when the laminated film is adhered to the adherend satisfy the following relationship, 30≤[AF(10) / AF(200)]×100≤70, AF (10) indicates the adhesive strength of the laminated film to the adherend under the condition of a peeling speed of 10 [mm / min] and AF(200) indicates the adhesive strength of the laminated film to the adherend under the condition of a peeling speed of 200 [mm / min].SELECTED DRAWING: Figure 1
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a laminated film. [Background technology]

[0002] Patent Document 1 describes a surface protection sheet that, when attached to the surface of an adherend, prevents the adherend from flying off and falling when the adherend is subjected to impact, causing damage to the person involved or a third party. [Prior art documents] [Patent documents]

[0003] [Patent Document 1] Patent No. 6979295 Summary of the Invention [Problem to be solved by the invention]

[0004] Surface protection sheets that are applied to the surface of an adherend must have a certain level of adhesive strength and durability (creep resistance). Creep resistance indicates the resistance to deformation caused by continued application of a load. If these conditions are not met, there is a risk that the surface protection sheet will peel off or that the adherend will fly off and fall when an impact is applied.

[0005] An object of the present invention is to provide a laminated film that has shatterproof properties, durability (creep resistance), and slippage / peeling prevention properties. [Means for solving the problem]

[0006] A laminate film according to one aspect of the present invention has a resin layer, an adhesive layer disposed under the resin layer for adhering the resin layer to an adherend, and a surface protective layer formed on the resin layer, characterized in that the breaking elongation of the laminate film at a tensile speed of 300 mm / min is 300% to 1500%, the displacement of the laminate film after a heat resistance test at 80°C is 10 mm or less, and AF(10) and AF(200) when the laminate film is attached to an adherend satisfy the following relationship: 30≦[AF(10) / AF(200)]×100≦70, AF(10) indicates the adhesive strength of the laminate film to the adherend at a peel speed of 10 mm / min, and AF(200) indicates the adhesive strength of the laminate film to the adherend at a peel speed of 200 mm / min.

[0007] In the laminate film according to one aspect of the present invention, the puncture strength of the laminate film measured by a puncture strength test is preferably 40 [N] or more.

[0008] In the laminate film according to one aspect of the present invention, the adhesive layer is preferably composed of one or more layers.

[0009] In the laminate film according to one aspect of the present invention, the adhesive layer contains a styrene-based elastomer, and the styrene content of the styrene-based elastomer in the adhesive layer is preferably 17% to 27%.

[0010] In the laminate film according to one aspect of the present invention, the adherend is preferably made of a polycarbonate resin or an acrylic resin. Effect of the Invention

[0011] The laminated film according to the present invention has shatterproof properties, durability (creep resistance), and slippage / peeling prevention properties. [Brief description of the drawings]

[0012] [Figure 1]1(a) and (b) are diagrams showing the state in which a laminated film is applied to an adherend. [Diagram 2] FIG. 2 is a diagram showing the compositions of the adherends and laminate films in each of the Examples and Comparative Examples, and the results of verification tests on the laminate films. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0013] Hereinafter, various embodiments of the present invention will be described with reference to the drawings. It should be noted that the technical scope of the present invention is not limited to these embodiments, but covers the inventions described in the claims and their equivalents.

[0014] 1(a) and (b) are diagrams showing a state in which a laminate film 20 is applied to an adherend 10. FIG.

[0015] The adherend 10 is installed on roads, railways, airport facilities, etc., and is used for a light-transmitting plate provided as a part of a soundproof wall installed in the passage of the road, railway, etc. The adherend 10 is made of polycarbonate (PC) resin or acrylic (PMMA: Poly Methyl Methacrylate) resin, and the thickness of the adherend 10 is at least 5 mm in order to satisfy the soundproofing performance required for a soundproof wall.

[0016] The laminated film 20 is an adhesive film attached to the surface of the adherend 10 for the purpose of protecting the adherend 10 and preventing the adherend 10 from scattering or falling. The laminated film 20 is flexible and therefore bends flexibly under an external force. Therefore, the laminated film 20 can be easily attached to the surface of the adherend 10 even if the surface of the adherend 10 has a complex shape. The laminated film 20 is composed of a resin layer 21, an adhesive layer 22, a surface protective layer 23, and the like. The resin layer 21, the adhesive layer 22, and the surface protective layer 23 are all translucent.

[0017] In order to maintain the strength of the laminated film, the resin layer 21 preferably does not contain excessive turbidity, sediment, or significant particles. The particles refer to minute objects such as dust, fiber waste, and insects. For example, the resin layer 21 is made of a resin such as a thermoplastic elastomer (TPE), polycarbonate (PC), polyethylene terephthalate (PET), or poly methyl methacrylate (PMMA). Thermoplastic elastomers include thermoplastic polyurethane (TPU), thermoplastic polyolefin (TPO), thermoplastic polyester (TPE), thermoplastic polyamide (TPA), and polyvinyl chloride (PVC). The thickness of the resin layer 21 is preferably within a range of 38 μm to 1000 μm.

[0018] The adhesive layer 22 is disposed under the resin layer 21. The adhesive layer 22 functions as an adhesive for attaching the resin layer 21 to the adherend 10, and can firmly bond the adherend 10 and the resin layer 21. The adhesive layer 22 is composed of one or more layers, as shown in FIG. 1(a). For example, the adhesive layer 22 is composed of an upper end layer 221, an intermediate layer 222, and a lower end layer 223. The upper end layer 221 contacts the resin layer 21 and the intermediate layer 222, respectively. The intermediate layer 222 contacts the upper end layer 221 and the lower end layer 223, respectively. The lower end layer 223 contacts the intermediate layer 222 and the adherend 10, respectively. The upper end layer 221 and the lower end layer 223 have the same composition, and the intermediate layer 222 has a different composition from the upper end layer 221 and the lower end layer 223.

[0019] The upper end layer 221 and the lower end layer 223 are composed of additives such as a thermoplastic elastomer, a tackifier, a softener, an ultraviolet absorber, and a light stabilizer. The thermoplastic elastomer includes, for example, thermoplastic polystyrene (styrene-based elastomer) (TPS: Thermoplastic Polystyrene), thermoplastic polyurethane, thermoplastic polyolefin, thermoplastic polyester, thermoplastic polyamide, polyvinyl chloride, and polyvinyl butyral (PVB: Polyvinyl Butyral). The use of thermoplastic polystyrene is preferable from the viewpoint of heat resistance, weather resistance, and chemical resistance. The tackifier includes one or more resins selected from terpene resin, rosin resin, petroleum resin, coal resin, phenol resin, xylene resin, and the like. As the terpene resin, for example, α-pinene-based terpene resin, β-pinene-based terpene resin, dipentene-based terpene resin, aromatic modified terpene resin, terpene phenol resin, and hydrogenated terpene resin can be used. Examples of rosin resins include gum rosin, tall oil rosin, wood rosin, hydrogenated rosin, disproportionated rosin, polymerized rosin, and modified rosin. Examples of petroleum resins that can be used include aliphatic (C5) petroleum resins, aromatic (C9) petroleum resins, copolymerized (C5 / C9) petroleum resins, alicyclic (hydrogenated, dicyclopentadiene (DCPD)) petroleum resins, and styrene (styrene, substituted styrene) petroleum resins. Examples of coal resins that can be used include coumarone-indene resins. The softener is used to increase the plasticity of the upper end layer 221 and the lower end layer 223 to improve the efficiency of the work of constructing the laminated film 20 by the constructor while reducing the hardness of the resin layer 21, and includes one or more process oils selected from paraffinic process oils, naphthenic process oils, aromatic process oils, liquid polybutene, liquid polyisobutylene, and the like.

[0020] The intermediate layer 222 is made of a resin such as a thermoplastic elastomer, a polycarbonate resin, a polyethylene terephthalate, an acrylic resin, or polyvinyl chloride. The thermoplastic elastomer includes thermoplastic polystyrene (styrene-based elastomer), thermoplastic polyurethane, thermoplastic polyolefin, thermoplastic polyester, thermoplastic polyamide, polyvinyl chloride, and polyvinyl butyral.

[0021] The thickness of each of the upper end layer 221 and the lower end layer 223 is preferably within a range of 25 μm to 3000 μm.

[0022] The adhesive layer 22 may be configured as one layer as shown in Fig. 1(b). In this case, the adhesive layer 22 has the same composition as the above-mentioned upper end layer 221 and lower end layer 223. The thickness of the adhesive layer 22 is preferably within a range of 25 [μm] to 3000 [μm].

[0023] The surface protective layer 23 is formed on the resin layer 21 to protect the resin layer 21. The surface protective layer 23 is made of acrylic resin, polyester resin, urethane resin, silicone resin, fluorine resin, or the like. The thickness of the surface protective layer 23 is preferably within a range of 1 μm to 100 μm. Furthermore, the surface protective layer 23 may contain additives such as a surface conditioner, an ultraviolet absorbing agent, and a light stabilizer.

[0024] In order for the laminated film 20 to have shatterproof properties, the breaking elongation of the laminated film 20 at a tensile speed of 300 mm / min is preferably 300% to 1500%.

[0025] In order for the laminated film 20 to have durability (creep resistance), it is preferable that the amount of displacement of the laminated film 20 after a heat resistance test at 80° C. is 10 mm or less.

[0026] In order for the laminated film 20 to have shatter resistance, durability (creep resistance), and slippage / peeling prevention properties, it is preferable that AF(10) and AF(200) when the laminated film 20 is attached to the adherend 10 satisfy the following relationship: 30≦[AF(10) / AF(200)]×100≦70 Here, AF(10) indicates the adhesive strength of the laminated film 20 to the adherend when the peel speed is 10 [mm / min], and AF(200) indicates the adhesive strength of the laminated film 20 to the adherend when the peel speed is 200 [mm / min].

[0027] In order for the laminated film 20 to have shatterproof properties, the puncture strength of the laminated film 20 measured by a puncture strength test is preferably 40 [N] or more.

[0028] The adhesive layer 22 preferably contains a styrene-based elastomer so that the laminated film 20 has shatter resistance, durability (creep resistance), slippage / peeling prevention performance, and impact resistance. The styrene content of the styrene-based elastomer in the adhesive layer 22 is preferably 17% to 27%, and more preferably around 20%. EXAMPLES

[0029] FIG. 2 is a diagram showing the compositions of the adherend 10 and the laminated film 20 in each of the examples and comparative examples, as well as the results of a verification test on the laminated film 20. As shown in FIG.

[0030] In each of the examples and comparative examples, a laminated film 20 having the composition shown in FIG. 2 was attached to the adherend 10. The adhesive layer 22 of the laminated film 20 of Examples 1 to 5, 7, and 8 and Comparative Examples 1 to 3 does not have an intermediate layer 222 and is composed of one layer, as shown in FIG. 1(b). The adhesive layer 22 of the laminated film 20 of Example 6 has an intermediate layer 222 and is composed of an upper end layer 221, an intermediate layer 222, and a lower end layer 223, as shown in FIG. 1(a). "PC" in the adherend composition refers to polycarbonate resin, and "PMMA" refers to acrylic resin. "TPU" in the resin layer composition refers to thermoplastic polyurethane. "PMMA" in the surface protection layer composition refers to acrylic resin. "HALS" in the adhesive layer composition refers to a light stabilizer, "UVA" refers to an ultraviolet absorbing agent, and "PVC" in the adhesive layer composition refers to polyvinyl chloride. Furthermore, in the adhesive layer 22 of each of the examples and comparative examples, a styrene-based elastomer having a styrene content of 10 [wt%], 15 [wt%], 20 [wt%], or 30 [wt%] was used. A process oil having a dynamic viscosity of 10 [mm2 / s] or 100 [mm2 / s] was used. A tackifier having a softening point of 90 [℃] or 100 [℃] was used. A hindered amine-based HALS and a hydroxyphenyl triazine-based UVA were used.

[0031] (Method of manufacturing laminated film) On one side of the resin layer 21, a Baker-type applicator was used to apply a composition for a surface protective layer so that the dry film thickness was 30 [μm], and the composition was dried at 120 [℃] × 2.5 minutes to form a clear layer. Then, a laminator or the like was used to laminate a protective film on the surface of the clear layer at a temperature of 23 [℃]. After lamination, the clear layer was cured by curing for 4 days in a 50 [℃] environment. On the surface of the resin layer 21 opposite to the surface on which the surface protective layer 23 was formed, a Baker-type applicator was used to apply a composition for an adhesive layer so that the dry film thickness was 150 [μm], and the composition was dried at 100 [℃] × 10 minutes to apply an adhesive layer 22. Then, a laminator or the like was used to bond a separator to the adhesive layer 22. As a result, a laminated film 20 having an adhesive layer 22 was obtained.

[0032] Here, the following verification tests were carried out for each of the Examples and Comparative Examples, and the results are shown in FIG.

[0033] (Method of measuring AF(10)) In the application examples of each of the Examples and Comparative Examples, a first peel test was conducted to peel off a 25 mm wide laminate film 20 attached to an adherend 10. In the first peel test, a precision universal testing machine manufactured by Shimadzu Corporation was used to measure the adhesive strength when peeled off at 180 degrees at a peel speed of 10 mm / min. The laminate film 20 was attached to a 3 mm thick polycarbonate plate, which is an example of the adherend 10. The first peel test yielded the adhesive strength AF(10) [N / 25 mm] of the laminate film 20 when it was attached to a 3 mm thick polycarbonate plate.

[0034] (Measurement of AF(200) and calculation method of index value I) In the application examples of each of the Examples and Comparative Examples, a second peel test was conducted in which the laminated film 20 with a width of 25 mm attached to the adherend 10 was peeled off. In the second peel test, a precision universal testing machine manufactured by Shimadzu Corporation was used to measure the adhesive strength when peeled off at 180 degrees at a peel speed of 200 mm / min. The laminated film 20 was attached to a polycarbonate plate with a thickness of 3 mm, which is an example of the adherend 10. The second peel test gave the adhesive strength AF(200) [N / 25 mm] of the laminated film 20 when it was attached to a polycarbonate plate with a thickness of 3 mm. The calculation method of the index value I is as follows. Index value I=[AF(10) / AF(200)]×100

[0035] (Method of measuring breaking elongation of laminated film) In the construction examples of each of the examples and comparative examples, a tensile test was conducted to measure the breaking elongation when the laminated film 20 was pulled at a tensile speed of 300 [mm / min]. In the tensile test, the breaking elongation at the time of breaking was calculated when measured under a temperature condition of 23 [℃] using a precision universal testing machine manufactured by Shimadzu Corporation. The breaking elongation was calculated as follows. Breaking elongation (%) = [(sample length at break - sample length before measurement) / sample length before measurement] x 100 The breaking elongation [%] of the laminated film 20 was obtained by the tensile test.

[0036] (Method for measuring displacement after heat resistance test) In the application examples of each embodiment and comparative example, the laminated film 20 was heated at a heating temperature of 80°C for a heating time of 24 hours, and a heat resistance test was performed to measure the amount of displacement of the laminated film 20 after heating. In the heat resistance test, a laminated film 20 having a size of 9.0 cm x 7.5 cm was attached to a polycarbonate plate having a thickness of 3 mm and a size of 7.0 cm x 7.5 cm, which is an example of the adherend 10. At that time, the laminated film 20 was exposed by 2 cm, and the size of the laminated film 20 attached to the polycarbonate plate was adjusted to 7 cm x 7.5 cm. This is calculated as a load of 19 g being applied to the laminated film 20 having a size of 9.0 cm x 7.5 cm. Furthermore, a hole was made in the laminated film portion, a metal rod was inserted through the laminated film 20, and the laminated film 20 was placed in a suspended state in a constant temperature incubator, and a predetermined heat resistance test was performed. In the heat resistance test, the amount of displacement between the adherend 10 and the adhesive layer 22 or the amount of displacement between the adhesive layer 22 and the resin layer 21 after heating was measured with a ruler, and the larger value of either was taken as the amount of displacement [mm] of the laminated film 20.

[0037] (Method for measuring puncture strength of laminated film) In the application examples of each of the Examples and Comparative Examples, a puncture strength test was conducted to measure the puncture strength of the laminated film 20. For the puncture strength test, a digital force gauge was prepared with a rod with a diameter of 2 mm fixed to the tip, and the tip of the rod was grounded on the surface protective layer 23 of the laminated film 20. Under conditions of 23°C and 50% humidity, a force was applied to the rod grounded on the laminated film at a speed of 50 mm / min, and the strength at which the rod penetrated the laminated film 20 was measured.

[0038] As can be seen from Examples 1 to 8 and Comparative Examples 1 to 3 in FIG. 2, when the breaking elongation is within the range of 300[%] to 1500[%], the displacement of the laminated film 20 after a heat resistance test at 80[°C] is 10[mm] or less, and AF(10) and AF(200) when the laminated film 20 is attached to the adherend 10 satisfy the following relationship: 30≦[AF(10) / AF(200)]×100≦70 It was found that the laminated film 20 satisfied the requirements for shatter resistance, durability (creep resistance), and slippage / peeling prevention performance, that is, the overall evaluation was "OK."

[0039] It was also found that when the puncture strength of the laminated film 20 measured by a puncture strength test was 40 [N] or more, the laminated film 20 further satisfied the shatterproof property.

[0040] Furthermore, it was found that when the adhesive layer 22 contains a styrene-based elastomer and the styrene content of the styrene-based elastomer of the adhesive layer 22 is 17% to 27%, the laminated film 20 further satisfies the shatterproof properties, durability (creep resistance), and slippage / peeling prevention performance.

[0041] It should be understood by those skilled in the art that various changes, substitutions, and modifications can be made to the present invention without departing from the spirit and scope of the present invention. For example, the processes of the above-described parts may be executed in different orders as appropriate within the scope of the present invention. Furthermore, the above-described embodiments and modifications may be combined as appropriate within the scope of the present invention. [Explanation of symbols]

[0042] 10 Adherent 20 Laminated Film 21 Resin layer 22 Adhesive layer 23 Surface protective layer 221 Top layer 222 Middle Class 223 Bottom layer

Claims

1. A resin layer; an adhesive layer disposed under the resin layer for attaching the resin layer to an adherend; A laminated film having a surface protective layer formed on the resin layer, The breaking elongation of the laminated film at a tensile speed of 300 mm / min is 300% to 1500%. The amount of displacement of the laminated film after a heat resistance test at 80° C. is 10 mm or less, When the laminated film is attached to the adherend, AF(10) and AF(200) satisfy the following relationship: 30≦[AF(10) / AF(200)]×100≦70 AF(10) indicates the adhesive strength of the laminate film to the adherend when the peel rate is 10 [mm / min], and AF(200) indicates the adhesive strength of the laminate film to the adherend when the peel rate is 200 [mm / min]. A laminated film characterized by:

2. 2. The laminate film according to claim 1, wherein the puncture strength of the laminate film measured by a puncture strength test is 40 [N] or more.

3. The laminated film according to claim 1 , wherein the adhesive layer is composed of one or more layers.

4. The adhesive layer contains a styrene-based elastomer, The styrene content of the styrene-based elastomer in the adhesive layer is 17% to 27%. The laminated film according to any one of claims 1 to 3.

5. The laminate film according to any one of claims 1 to 3, wherein the adherend is made of a polycarbonate resin or an acrylic resin.

Citation Information

Patent Citations

  • Surface protection sheet and structure equipped with said sheet

    JP6979295B2