Organic polymer, curable composition, and cured product

By introducing a specific hydrolyzable group structure into the hydrolyzable silyl group-containing organic polymer, curability is enhanced, reducing the need for organotin compounds and enabling effective curing with less active catalysts.

JP2024143586APending Publication Date: 2024-10-11KANEKA CORP
View PDF 6 Cites 0 Cited by

Patent Information

Application Number
JP2023056344
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Filing Date
2023-03-30
Publication Date
2024-10-11

AI Technical Summary

Technical Problem

Conventional hydrolyzable silyl group-containing organic polymers exhibit insufficient curability, necessitating an improvement in their curing properties.

Method used

Introduction of a specific substituent as a hydrolyzable group on the silicon atom within the hydrolyzable silyl group-containing organic polymer, represented by a specific structural formula, to enhance curability.

Benefits of technology

The modified polymer demonstrates improved curability, allowing for reduced use of organotin compounds as curing catalysts and enabling effective curing with less active catalysts like amine compounds, while maintaining good curability.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024143586000001
    Figure 2024143586000001
  • Figure 2024143586000002
    Figure 2024143586000002
  • Figure 2024143586000003
    Figure 2024143586000003
Patent Text Reader

Abstract

To provide a hydrolyzable silyl group-containing organic polymer capable of exhibiting improved curability.SOLUTION: An organic polymer (A) has a hydrolyzable silyl group represented by formula (1). In the formula (1), R1 represents a hydrolyzable group; R2 represents a C1-20 substituted or unsubstituted monovalent hydrocarbon group; X represents a hydroxyl group or a hydrolyzable group other than R1; a is 1, 2 or 3; b is 0, 1 or 2; c is 0, 1 or 2; and a+b+c is 3 or less.SELECTED DRAWING: None
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to an organic polymer having a hydrolyzable silyl group, a curable composition, and a cured product. [Background technology]

[0002] Organic polymers that have hydroxyl groups or hydrolyzable groups on silicon atoms and have silicon-containing groups that can form siloxane bonds (hereinafter referred to as "hydrolyzable silyl groups") are known as moisture-reactive polymers. They are used in many industrial products such as sealants, adhesives, coating materials, paints, and pressure-sensitive adhesives because they cure through hydrolysis to form flexible rubber-like cured products.

[0003] As the hydrolyzable group that such hydrolyzable silyl group has on the silicon atom, a methoxy group is known. For example, Patent Document 1 discloses a polyoxyalkylene polymer having a trimethoxysilyl group. Such a silyl group is known to have relatively good curability and to cure in a short time. [Prior art documents] [Patent documents]

[0004] [Patent Document 1] International Publication No. 2013 / 047837 Summary of the Invention [Problem to be solved by the invention]

[0005] Conventionally known hydrolyzable silyl group-containing organic polymers may not have sufficient curability, and there is a demand for further improvement in the curability. In view of the above-mentioned current situation, an object of the present invention is to provide a hydrolyzable silyl group-containing organic polymer capable of exhibiting improved curability, a curable composition containing the polymer, and a cured product of the composition. [Means for solving the problem]

[0006] As a result of extensive research, the present inventors have found that the curability of a hydrolyzable silyl group-containing organic polymer can be improved by introducing a substituent having a specific structure as a hydrolyzable group that the hydrolyzable silyl group has on a silicon atom, and have arrived at the present invention.

[0007] That is, the present invention relates to an organic polymer (A) having a hydrolyzable silyl group represented by the following general formula (1).

[0008] [ka]

[0009] (In formula (1), R 1 R represents a hydrolyzable group represented by the following general formula (2). 2 represents a substituted or unsubstituted monovalent hydrocarbon group having 1 to 20 carbon atoms. X represents a hydroxyl group or R 1 a is 1, 2, or 3; b is 0, 1, or 2; c is 0, 1, or 2; and a+b+c is 3 or less.

[0010] [ka]

[0011] (In formula (2), R 3 R represents a substituted or unsubstituted divalent hydrocarbon group having 1 to 5 carbon atoms. 4 represents a hydrogen atom, a substituted or unsubstituted monovalent hydrocarbon group having 1 to 20 carbon atoms, or -OR 6 R 6 R represents a hydrogen atom or a substituted or unsubstituted monovalent hydrocarbon group having 1 to 20 carbon atoms. 5 represents an oxygen atom or a nitrogen atom bonded to any group. The present invention further relates to a curable composition comprising said organic polymer. Furthermore, the present invention also relates to a cured product obtained by curing the curable composition. Effect of the Invention

[0012] According to the present invention, it is possible to provide a hydrolyzable silyl group-containing organic polymer capable of exhibiting improved curability, a curable composition containing the polymer, and a cured product of the composition. The hydrolyzable silyl group-containing organic polymer according to the present invention can exhibit improved curability, and therefore in a curable composition containing the same, good curability can be achieved even if the amount of an organotin compound used as a curing catalyst is reduced or a curing catalyst (e.g., an amine compound, etc.) that is generally less active than an organotin compound is used. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0013] Hereinafter, an embodiment of the present invention will be described in detail. (Hydrolyzable Silyl Group-Containing Organic Polymer (A)) The organic polymer (A) according to the present embodiment has a hydrolyzable silyl group represented by the following general formula (1): The hydrolyzable silyl groups represented by the general formula (1) that can be contained in the organic polymer (A) may have the same structure or different structures.

[0014] [ka]

[0015] R in general formula (1) 1 R represents a hydrolyzable group represented by the following general formula (2). 1 When a plurality of are included, they may be the same or different.

[0016] [ka]

[0017] R in general formula (2) 3represents a substituted or unsubstituted divalent hydrocarbon group having 1 to 5 carbon atoms. The hydrocarbon group may be either saturated or unsaturated. The number of carbon atoms is preferably 1 to 4, more preferably 1 to 3, further preferably 1 or 2, and most preferably 1. When the hydrocarbon group has a substituent, the substituent is not particularly limited, and examples thereof include halogen groups such as a chloro group, alkoxy groups such as a methoxy group, and amino groups such as an N,N-diethylamino group.

[0018] R 3 Examples of R include unsubstituted alkylene groups such as methylene, ethylene, n-propylene, isopropylene, n-butylene, and tert-butylene; substituted alkylene groups such as chloromethylene, methoxymethylene, and N,N-diethylaminomethylene; and unsaturated hydrocarbon groups such as vinylene, isopropenylene, and allylene. Preferred are substituted or unsubstituted alkylene groups, more preferably methylene, ethylene, and propylene groups, even more preferably methylene and ethylene groups, and most preferably methylene groups. 3 When a plurality of are present, they may be the same or different.

[0019] R in general formula (2) 4 represents a hydrogen atom, a substituted or unsubstituted monovalent hydrocarbon group having 1 to 20 carbon atoms, or -OR 6 Represents R 6 represents a hydrogen atom, or a substituted or unsubstituted monovalent hydrocarbon group having 1 to 20 carbon atoms.

[0020] R 4 or R 6The hydrocarbon group which can be represented by may be either saturated or unsaturated, and may be either aliphatic, alicyclic, or aromatic. The number of carbon atoms in the hydrocarbon group is independently preferably 1 to 10, more preferably 1 to 8, further preferably 1 to 6, even more preferably 1 to 3, and particularly preferably 1 or 2. When the hydrocarbon group has a substituent, the substituent is not particularly limited, and examples thereof include a hydroxyl group, a halogen group such as a chloro group, an alkoxy group such as a methoxy group, and an amino group such as an N,N-diethylamino group.

[0021] R 4 Examples of the R include unsubstituted alkyl groups such as methyl, ethyl, n-propyl, isopropyl, n-butyl, tert-butyl, n-hexyl, 2-ethylhexyl, and n-dodecyl; substituted alkyl groups such as chloromethyl, methoxymethyl, N,N-diethylaminomethyl, and methylol; unsaturated hydrocarbon groups such as vinyl, isopropenyl, and allyl; cycloalkyl groups such as cyclohexyl; aryl groups such as phenyl, toluyl, and 1-naphthyl; and aralkyl groups such as benzyl. R is preferably a substituted or unsubstituted alkyl group or unsaturated hydrocarbon group, more preferably a methyl group, ethyl group, propyl group, vinyl group, methoxymethyl group, or methylol group, even more preferably a methyl group or methylol group, and particularly preferably a methyl group. 4 When a plurality of are present, they may be the same or different.

[0022] R 6 As a concrete example of 4 The specific examples are the same as those of R. 6 is preferably a substituted or unsubstituted alkyl group or an unsaturated hydrocarbon group, more preferably a methyl group, an ethyl group, a propyl group, or a vinyl group, and particularly preferably a methyl group. 6 When a plurality of are present, they may be the same or different.

[0023] R in general formula (2) 5represents an oxygen atom or a nitrogen atom bonded to any group. As shown in general formula (2), R 5 is bonded to the adjacent carbon atom by a double bond. This structure is called a divalent hydrocarbon group R 3 By bonding to an oxygen atom and a silicon atom via R, the curability of the hydrolyzable silyl group can be improved. 5 is preferably an oxygen atom.

[0024] R 5 In the above formula, examples of the optional group bonded to the nitrogen atom include a hydrogen atom, or a substituted or unsubstituted monovalent hydrocarbon group having 1 to 20 carbon atoms. The number of carbon atoms in the hydrocarbon group is preferably 1 to 10, more preferably 1 to 6, and even more preferably 1 to 3.

[0025] R in general formula (1) 1 The total number of carbon atoms contained in is not particularly limited, but may be about 2 to 20, preferably 3 to 10, more preferably 3 to 6, and particularly preferably 3 to 5.

[0026] R in general formula (1) 1 Preferred specific examples of the hydrolyzable group (that is, the hydrolyzable group represented by general formula (2)) include groups represented by the following formulas (3) to (9).

[0027] [ka]

[0028] [ka]

[0029] [ka]

[0030] [ka]

[0031] [ka]

[0032] [ka]

[0033] [ka]

[0034] R in general formula (1) 2 represents a substituted or unsubstituted monovalent hydrocarbon group having 1 to 20 carbon atoms. 2 When a plurality of are contained, they may be the same or different. The hydrocarbon group may be saturated or unsaturated, and may be aliphatic, alicyclic, or aromatic. The hydrocarbon group preferably has 1 to 10 carbon atoms, more preferably 1 to 8 carbon atoms, even more preferably 1 to 6 carbon atoms, even more preferably 1 to 3 carbon atoms, and particularly preferably 1 or 2 carbon atoms. When the hydrocarbon group has a substituent, the substituent is not particularly limited, and examples thereof include halogen groups such as a chloro group, alkoxy groups such as a methoxy group, and amino groups such as an N,N-diethylamino group.

[0035] R 2Examples of the R include unsubstituted alkyl groups such as methyl, ethyl, n-propyl, isopropyl, n-butyl, tert-butyl, n-hexyl, 2-ethylhexyl, and n-dodecyl; substituted alkyl groups such as chloromethyl, methoxymethyl, and N,N-diethylaminomethyl; unsaturated hydrocarbon groups such as vinyl, isopropenyl, and allyl; cycloalkyl groups such as cyclohexyl; aryl groups such as phenyl, toluyl, and 1-naphthyl; and aralkyl groups such as benzyl. R is preferably a substituted or unsubstituted alkyl group, more preferably a methyl group, an ethyl group, a chloromethyl group, or a methoxymethyl group, even more preferably a methyl group or a methoxymethyl group, and particularly preferably a methyl group. 2 When a plurality of are present, they may be the same or different.

[0036] In the general formula (1), X is a hydroxyl group or R 1 When general formula (1) contains a plurality of X's, they may be the same or different. R 1 The hydrolyzable group other than is not particularly limited and may be a known hydrolyzable group, for example, a hydrogen atom, a halogen atom, an alkoxy group, an acyloxy group, a ketoximate group, an amino group, an amide group, an acid amide group, an aminooxy group, a mercapto group, an alkenyloxy group, etc. Among these, an alkoxy group, an acyloxy group, a ketoximate group, and an alkenyloxy group are preferred. Since the hydrolysis is mild and easy to handle, an alkoxy group is more preferred, a methoxy group and an ethoxy group are further preferred, and a methoxy group is particularly preferred. When a plurality of Xs are present, they may be the same or different from each other.

[0037] In the general formula (1), a represents any one of 1, 2, and 3, b represents any one of 0, 1, and 2, and c represents any one of 0, 1, and 2. a is not limited to one number, and different numbers may coexist in the organic polymer (A). The same applies to b and c. a+b+c is 3 or less, preferably 2 or 3, and particularly preferably 3.

[0038] The organic polymer (A) may have only the hydrolyzable silyl group represented by the general formula (1) as the hydrolyzable silyl group, or may have the hydrolyzable silyl group represented by the general formula (1) and another hydrolyzable silyl group not included in the general formula (1). Such another hydrolyzable silyl group is not particularly limited, but an example thereof includes the hydrolyzable silyl group in which a is 0 in the general formula (1).

[0039] R of the hydrolyzable silyl group calculated for the entire organic polymer (A) 1 R out of the sum of X and 1 The higher the ratio (x), the more remarkable the effect of improving the curability. 1 The ratio (x) is preferably 1% or more, more preferably 5% or more, even more preferably 10% or more, and particularly preferably 20% or more. The upper limit is not particularly limited, and may be 100% or less, or may be 50% or less, or may be 30% or less.

[0040] The above mentioned R 1 The ratio (x) of R is a value calculated for the entire organic polymer (A), including not only the hydrolyzable silyl group represented by the general formula (1) but also other hydrolyzable silyl groups not included in the general formula (1). 1 The method for measuring the ratio (x) of the organic polymer (A) is as described in detail in the Examples section. 1 It can be calculated from the proportion of each hydrolyzable group by measuring with H NMR.

[0041] (Polymer backbone of hydrolyzable silyl group-containing organic polymer (A)) The hydrolyzable silyl group-containing organic polymer (A) according to this embodiment has a polymer skeleton (also called a main chain structure) and a polymer chain end bonded to the polymer skeleton. The polymer skeleton is a structure in which a plurality of monomer units are formed in succession by bonding a plurality of monomers by addition or condensation. The monomer species contained in the polymer skeleton may be one type, or a mixture of a plurality of types may be bonded.

[0042] The polymer chain end refers to a portion located at the end of the polymer skeleton. The number of polymer chain ends of the hydrolyzable silyl group-containing organic polymer (A) is 2 when the polymer skeleton is entirely linear, and is 3 or more when the polymer skeleton is entirely branched. When the polymer skeleton is a mixture of linear and branched structures, the number can be between 2 and 3 on average.

[0043] The hydrolyzable silyl group of the organic polymer (A) may be present in the polymer backbone and / or at the polymer chain end. Two or more hydrolyzable silyl groups may be present at one polymer chain end. When the organic polymer (A) according to the present embodiment is used as a curable resin for adhesives, sealing materials, elastic coating agents, pressure sensitive adhesives, etc., the hydrolyzable silyl group is preferably contained at the polymer chain end of the organic polymer (A).

[0044] The polymer skeleton (also referred to as the main chain structure) of the hydrolyzable silyl group-containing organic polymer (A) is not particularly limited, and various main chain structures can be used. Specifically, polyoxyalkylene polymers such as polyoxyethylene, polyoxypropylene, polyoxybutylene, polyoxytetramethylene, polyoxyethylene-polyoxypropylene copolymers, and polyoxypropylene-polyoxybutylene copolymers; hydrocarbon polymers such as ethylene-propylene copolymers, polyisobutylene, copolymers of isobutylene and isoprene, and hydrogenated polyolefin polymers obtained by hydrogenating these polyolefin polymers; polyolefins obtained by condensation of dibasic acids such as adipic acid with glycols, or ring-opening polymerization of lactones; Examples of such polymers include ester polymers, (meth)acrylic acid ester polymers obtained by radical polymerization of (meth)acrylic acid ester monomers such as methyl (meth)acrylate, ethyl (meth)acrylate, butyl (meth)acrylate, 2-ethylhexyl (meth)acrylate, and stearyl (meth)acrylate, vinyl copolymers obtained by radical polymerization of (meth)acrylic acid ester monomers, vinyl acetate, acrylonitrile, and styrene, polysulfide polymers, polyamide polymers, polycarbonate polymers, and diallyl phthalate polymers. In the above description, (meth)acrylic refers to acrylic and / or methacrylic.

[0045] Among these, saturated hydrocarbon polymers such as polyisobutylene, hydrogenated polyisoprene, and hydrogenated polybutadiene, polyoxyalkylene polymers, and (meth)acrylic acid ester polymers are preferred because they have relatively low glass transition temperatures and the resulting cured products have excellent cold resistance. Only one of these may be used, or two or more may be used in combination.

[0046] Polyoxyalkylene polymers and (meth)acrylic acid ester polymers are particularly preferred because they have high moisture permeability, excellent deep curing properties when made into a one-component curable composition, and excellent adhesive properties. Polyoxyalkylene polymers are more preferred, and polyoxypropylene is even more preferred.

[0047] A (meth)acrylic acid ester-based polymer is useful because, by combining various monomer compositions constituting the polymer, it is possible to obtain effects such as improving adhesiveness, improving heat resistance and weather resistance, and reducing the water absorption of a cured product obtained by curing a curable composition.

[0048] The polyoxyalkylene polymer is preferably a polymer having a repeating unit represented by -RO- (wherein R is a linear or branched alkylene group having 1 to 14 carbon atoms). R is more preferably a linear or branched alkylene group having 2 to 4 carbon atoms. Specific examples of the repeating unit represented by -RO- include -CHO-, -CHCHO-, -CHCH(CH)O-, -CHCH(CH)O-, -CHC(CH)(CH)O-, -CHCHCHCHO-, and the like. The main chain structure of the polyoxyalkylene polymer may be composed of only one type of repeating unit, or may be composed of two or more types of repeating units.

[0049] In particular, when the organic polymer (A) according to this embodiment is used as a curable resin such as a sealant or adhesive, a polyoxypropylene-based polymer having oxypropylene repeating units in an amount of 50% by weight or more, more preferably 80% by weight or more, of the polymer skeleton is preferred because it is amorphous and has a relatively low viscosity.

[0050] The main chain structure of the polyoxyalkylene polymer may be linear or may have a branched chain. When the polymer has a branched chain, the number of the branched chains is preferably 1 to 6 (i.e., the number of terminal hydroxyl groups is 3 to 8), more preferably 1 to 4 (i.e., the number of terminal hydroxyl groups is 3 to 6), and most preferably 1 (i.e., the number of terminal hydroxyl groups is 3). By having a branched chain, it is possible to obtain an effect of improving the restorability of the cured product. In addition, it is also expected to have an effect of reducing the water absorption of the cured product.

[0051] The polyoxyalkylene polymer is preferably one obtained by a ring-opening polymerization reaction of a cyclic ether compound in the presence of an initiator using a polymerization catalyst.

[0052] Examples of the cyclic ether compound include ethylene oxide, propylene oxide, butylene oxide, tetramethylene oxide, and tetrahydrofuran. These cyclic ether compounds may be used alone or in combination of two or more. Among the cyclic ether compounds, it is particularly preferable to use propylene oxide, since it can produce an amorphous polyether polymer having a relatively low viscosity.

[0053] Specific examples of the initiator include alcohols such as butanol, ethylene glycol, propylene glycol, propylene glycol monoalkyl ether, butanediol, hexamethylene glycol, neopentyl glycol, diethylene glycol, dipropylene glycol, triethylene glycol, glycerin, trimethylolmethane, trimethylolpropane, pentaerythritol, and sorbitol; and hydroxyl-terminated polyoxyalkylene polymers having a number average molecular weight of 300 to 4,000, such as polyoxypropylene diol, polyoxypropylene triol, polyoxyethylene diol, and polyoxyethylene triol.

[0054] Examples of the synthesis method of polyoxyalkylene polymers include, but are not limited to, a polymerization method using an alkali catalyst such as KOH, a polymerization method using a transition metal compound-porphyrin complex catalyst such as a complex obtained by reacting an organoaluminum compound with porphyrin as disclosed in JP-A-61-215623, a polymerization method using a composite metal cyanide complex catalyst as disclosed in JP-B-46-27250, JP-B-59-15336, U.S. Pat. No. 3,278,457, U.S. Pat. No. 3,278,458, U.S. Pat. No. 3,278,459, U.S. Pat. No. 3,427,256, U.S. Pat. No. 3,427,334, and U.S. Pat. No. 3,427,335, a polymerization method using a catalyst made of a polyphosphazene salt as exemplified in JP-A-10-273512, and a polymerization method using a catalyst made of a phosphazene compound as exemplified in JP-A-11-060722. A polymerization method using a double metal cyanide complex catalyst is more preferred for reasons of production cost and the fact that a polymer having a narrow molecular weight distribution can be obtained.

[0055] The hydrolyzable silyl group-containing organic polymer (A) may be a polyoxyalkylene polymer containing other bonds such as urethane bonds and urea bonds in the polymer skeleton, as long as the effect of the invention is not significantly impaired. A specific example of such a polymer is a polyurethane prepolymer.

[0056] The polyurethane prepolymer can be obtained by a known method, for example, by reacting a polyol compound with a polyisocyanate compound.

[0057] Specific examples of the polyol compound include polyether polyol, polyester polyol, polycarbonate polyol, and polyether polyester polyol.

[0058] Specific examples of the polyisocyanate compound include diphenylmethane diisocyanate, tolylene diisocyanate, xylylene diisocyanate, methylene-bis(cyclohexyl isocyanate), isophorone diisocyanate, and hexamethylene diisocyanate. The polyurethane prepolymer may be terminated with either a hydroxyl group or an isocyanate group.

[0059] From the viewpoint of obtaining a curable composition excellent in storage stability and workability, it is particularly preferable that the hydrolyzable silyl group-containing organic polymer (A) is a polyoxyalkylene polymer that does not contain a urethane bond, a urea bond, an ester bond, or an amide bond in the polymer skeleton.

[0060] The molecular weight distribution (Mw / Mn) of the hydrolyzable silyl group-containing organic polymer (A) is not particularly limited, but is preferably 1.6 or less, more preferably 1.5 or less, and particularly preferably 1.4 or less. From the viewpoint of improving various mechanical properties such as durability and elongation of the cured product, it is preferably 1.2 or less.

[0061] The number average molecular weight of the hydrolyzable silyl group-containing organic polymer (A), as polystyrene-equivalent molecular weight measured by GPC, is preferably 3,000 to 100,000, more preferably 5,000 to 50,000, and particularly preferably 8,000 to 35,000. When the number average molecular weight is within these ranges, the mechanical properties of the cured product are excellent, and since the amount of hydrolyzable silyl groups introduced is appropriate, it is possible to obtain an organic polymer (A) that exhibits good curability, has an easy-to-handle viscosity, and is excellent in workability while keeping production costs within an appropriate range.

[0062] The molecular weight of the hydrolyzable silyl group-containing organic polymer (A) can also be expressed as an end-group-converted molecular weight obtained by directly measuring the end group concentration of the polymer precursor before the introduction of the hydrolyzable silyl group by titration analysis based on the principle of the hydroxyl value measurement method of JIS K 1557-1 and the iodine value measurement method specified in JIS K 0070, and taking into consideration the structure of the polymer (the degree of branching determined by the polymerization initiator used). The end-group-converted molecular weight of the organic polymer (A) can also be obtained by preparing a calibration curve of the number average molecular weight obtained by general GPC measurement of the polymer precursor and the above-mentioned end-group-converted molecular weight, and converting the number average molecular weight obtained by GPC of the organic polymer (A) into the end-group-converted molecular weight.

[0063] In order to obtain a good rubber-like cured product, it is preferable that the hydrolyzable silyl groups (including both hydrolyzable silyl groups represented by general formula (1) and hydrolyzable silyl groups not encompassed by general formula (1); the same applies below) contained in the organic polymer (A) are present at the polymer chain terminals. Since this shows good curability and is likely to exhibit rubber elastic behavior, the number of hydrolyzable silyl groups per polymer chain terminal of the organic polymer (A) is preferably 0.5 or more on average, more preferably 0.6 or more, even more preferably 0.7 or more, and particularly preferably 0.8 or more.

[0064] The number of polymer chain ends per molecule of the organic polymer (A) is preferably 2 to 8, more preferably 2 to 4, and particularly preferably 2 or 3. The number of hydrolyzable silyl groups in one molecule of the organic polymer (A) is preferably from 1 to 7 on average, more preferably from 1 to 3.4, and particularly preferably from 1 to 2.6.

[0065] When the hydrolyzable silyl group-containing organic polymer (A) is branched, the hydrolyzable silyl group may be at the end of the main chain of the organic polymer, at the end of a side chain (branched chain), or at both. In particular, when the hydrolyzable silyl group is at the end of the main chain, the molecular weight between crosslinking points becomes long, which is preferable since it is easy to obtain a rubber-like cured product that has high strength, high elongation, and low elastic modulus.

[0066] (Method for producing organic polymer (A)) The method for producing the organic polymer (A) according to this embodiment is not particularly limited, but examples thereof include the following methods. Production method (i): A hydrolyzable silyl group -SiX not included in the general formula (1) d R 2 c (In the formula, R 2 , X, and c are as described above with respect to the general formula (1), d is 1, 2, or 3, and c+d is 3 or less. 1H to convert a part or all of the hydrolyzable groups X in the hydrolyzable silyl groups of the organic polymer (B) to specific hydrolyzable groups R 1 Hereinafter, this reaction is also referred to as an exchange reaction of hydrolyzable groups. The structure of the hydrolyzable silyl group-containing organic polymer (B) may be the same as the structure of the hydrolyzable silyl group-containing organic polymer (A) except for the hydrolyzable silyl group.

[0067] Production method (ii): A hydrosilane compound HSiR having a hydrolyzable silyl group represented by the general formula (1) is reacted with an organic polymer having a carbon-carbon unsaturated bond. 1 a X b R 2 c (In the formula, R 1 , X, R 2 , a, b, and c are as described above for general formula (1).) is subjected to a hydrosilylation reaction to introduce a hydrolyzable silyl group represented by general formula (1) into an organic polymer. In the hydrosilylation reaction, a known hydrosilylation catalyst may be appropriately used.

[0068] Manufacturing method (iii):R 5 The organic polymer (A) in which represents an oxygen atom is reacted with a primary amine compound HNR to convert the keto group (C=O) in the general formula (2) into an imino group (C=NR), where R 5 represents a nitrogen atom bonded to any group.

[0069] Manufacturing method (iv): OCN-W-SiR is added to the terminal hydroxyl group of a hydroxyl-terminated organic polymer. 1 a X b R 2 c (Wherein, W is a divalent organic group. R 1 , X, R 2 a, b, and c are as defined above) with an isocyanate group-containing silane compound represented by the formula (I).

[0070] The compound of general formula R 1 The hydroxyl group-containing compound (C) represented by H is R represented by general formula (2) as already defined for general formula (1). 1 It is a hydroxyl group-containing compound having a structure in which a hydrogen atom is bonded to the oxygen atom in the molecule.

[0071] The hydroxyl group-containing compound (C) includes organic compounds having a structure containing a hydroxyl group in the usual sense, as well as 1,3-diketones (e.g., acetylacetone) that coexist with an enol form due to keto-enol tautomerism.

[0072] Specific examples of the hydroxyl group-containing compound (C) are not particularly limited, and include, for example, hydroxyacetone, 4-hydroxy-2-butanone, acetoin, 3-hydroxy-3-methyl-2-butanone, propioin, 5-hydroxy-2-pentanone, diacetone alcohol, acetylacetone, methyl glycolate, methyl lactate, dihydroxyacetone, etc. As these hydroxyl group-containing compounds (C), only one type may be used, or two or more types may be used in combination.

[0073] The amount of the hydroxyl group-containing compound (C) used is preferably 0.1 parts by weight or more, more preferably 0.2 parts by weight or more, even more preferably 0.5 parts by weight or more, and particularly preferably 1 part by weight or more, relative to 100 parts by weight of the hydrolyzable silyl group-containing organic polymer (B). The upper limit is not particularly limited and may be appropriately set in consideration of the desired reaction rate, but may be, for example, 100 parts by weight or less. It is preferably 50 parts by weight or less, more preferably 30 parts by weight or less, and even more preferably 20 parts by weight or less. It may be 10 parts by weight or less.

[0074] The reaction between the hydrolyzable silyl group-containing organic polymer (B) and the hydroxyl group-containing compound (C) is preferably carried out in the presence of an organic solvent. From the viewpoint of reaction rate, the organic solvent is preferably an organic solvent with high polarity, specifically, alcohols such as methanol, ethanol, ethylene glycol, diethylene glycol, glycerin, etc.; amides such as dimethylformamide, N-methylpyrrolidone, etc.; sulfur compounds such as dimethylsulfoxide, etc.; nitriles such as acetonitrile, nitromethane, etc. may be mentioned. Only one type of organic solvent may be used, or two or more types may be used in combination.

[0075] The amount of the organic solvent used is preferably 1 part by weight or more, more preferably 2 parts by weight or more, and even more preferably 5 parts by weight or more, based on 100 parts by weight of the hydrolyzable silyl group-containing organic polymer (B). Although there is no particular upper limit, if the amount is too large, it takes a long time to remove the organic solvent after the reaction, so that the amount is preferably 100 parts by weight or less, more preferably 50 parts by weight or less, even more preferably 30 parts by weight or less, and particularly preferably 20 parts by weight or less.

[0076] The reaction between the hydrolyzable silyl group-containing organic polymer (B) and the hydroxyl group-containing compound (C) is preferably carried out in the presence of a catalyst in order to promote the reaction. As the catalyst, an acid, a base, a metal alkoxide, etc. can be used, but it is preferable to use an acid catalyst because the exchange reaction of the hydrolyzable group can proceed in a short time even with a small amount of use. Among them, Bronsted acids are particularly preferable.

[0077] Specific examples of the acid catalyst include hydrogen halide compounds such as hydrogen chloride and hydrogen bromide, sulfuric acid, nitric acid, trihaloacetic acids such as trifluoromethanesulfonic acid and trifluoroacetic acid, perchloric acid, solid acid catalysts, etc. Hydrogen halide compounds are preferred, and hydrogen chloride is particularly preferred.

[0078] The amount of the acid catalyst used is not particularly limited, but may be, for example, about 0.01 to 1 part by weight, or about 0.1 to 1 part by weight, per 100 parts by weight of the hydrolyzable silyl group-containing organic polymer (B).

[0079] The reaction temperature for the reaction between the hydrolyzable silyl group-containing organic polymer (B) and the hydroxyl group-containing compound (C) is not particularly limited, but may be about 0 to 120° C., or about 20 to 100° C. The reaction time is also not particularly limited, but may be about 10 minutes to 12 hours, or about 30 minutes to 5 hours.

[0080] After the exchange reaction of the hydrolyzable group is completed, the acid catalyst is preferably removed by volatilization under reduced pressure, captured by an epoxy compound, or deactivated by neutralization with a basic compound. In particular, it is preferable to capture the acid catalyst using an epoxy compound. The epoxy compound is not particularly limited and various types can be used, but epoxidized vegetable oils are particularly preferred. In addition, when the acid catalyst is a solid acid catalyst, it can be easily removed by filtration or the like.

[0081] After the reaction of the hydrolyzable silyl group-containing organic polymer (B) with the hydroxyl group-containing compound (C), or after deactivating the acidic catalyst by adding an epoxy compound when an epoxy compound is added, volatile components including unreacted hydroxyl group-containing compound (C) and organic solvents can be removed from the reaction system as necessary to obtain the organic polymer (A).

[0082] The volatile components may be left without being removed. In this case, the organic polymer (A) may contain any amount of the hydroxyl group-containing compound (C) and the organic solvent.

[0083] Examples of the method for obtaining the hydrolyzable silyl group-containing organic polymer (B) used in the production method (i) include the following methods (a) to (d). (a) After converting the terminal hydroxyl groups of a hydroxyl-terminated organic polymer to carbon-carbon unsaturated groups, HSiX d R 2 c (In the formula, R 2 , X, c, and d are as defined above).

[0084] (b) OCN-W-SiXd R 2 c (In the formula, R 2 , W, X, c, and d are as defined above),

[0085] (c) After converting the terminal hydroxyl groups of the hydroxyl-terminated organic polymer to carbon-carbon unsaturated groups, HS-W-SiX d R 2 c (In the formula, R 2 , W, X, c, and d are as defined above),

[0086] (d) A hydroxyl-terminated organic polymer is reacted with a polyisocyanate compound to synthesize an NCO-terminated organic polymer, and then the resulting polymer is subjected to reaction with HNR-W-SiX d R 2 c (Wherein, R is hydrogen or an alkyl group. R 2 , W, X, c, and d are as described above) or HS-W-SiX d R 2 c (In the formula, R 2 , W, X, c, and d are as defined above.

[0087] In the above methods (a) and (c), examples of the carbon-carbon unsaturated group include a vinyl group, an allyl group, a methallyl group, an allenyl group, and a propargyl group.

[0088] In each of the above-mentioned methods, the hydrolyzable silyl group-containing organic polymer (A) obtained by using a silane compound in which W is represented by a methylene group is preferred in that it exhibits extremely high curability.

[0089] The method (a) is preferred since it tends to give a hydrolyzable silyl group-containing organic polymer (A) having good storage stability, whereas the methods (b), (c) and (d) are preferred since they give a high conversion in a relatively short reaction time.

[0090] The introduction of hydrolyzable silyl groups by the method (a) has been proposed in JP-B-45-36319, JP-B-46-12154, JP-A-50-156599, JP-A-54-6096, JP-A-55-13767, JP-A-55-13468, JP-A-57-164123, JP-B-3-2450, U.S. Pat. No. 3,632,557, U.S. Pat. No. 4,345,053, U.S. Pat. No. 4,366,307, U.S. Pat. No. 4,960,844, and other publications. Examples of such polymers include those proposed in JP-A-61-197631, JP-A-61-215622, JP-A-61-215623, and JP-A-61-218632, in which a hydrolyzable silyl group is introduced by hydrosilylation or the like into a polyoxypropylene polymer having a high molecular weight and narrow molecular weight distribution, with a number average molecular weight of 6,000 or more and Mw / Mn of 1.6 or less, and a polymer proposed in JP-A-3-72527.

[0091] As described in WO 2013 / 180203, an organic polymer having two or more carbon-carbon unsaturated bonds at one polymer chain end is used to obtain an organic polymer (B) by the above methods (a) and (c), which has two or more hydrolyzable silyl groups at one polymer chain end. The organic polymer (A) produced from such an organic polymer (B) exhibits high curability, and the obtained cured product is expected to have high strength and high recovery.

[0092] <Curable composition> The above-mentioned organic polymer (A) having a hydrolyzable silyl group can constitute a curable composition containing the same.

[0093] (Hydrolyzable Silyl Group-Containing Organic Polymer (B)) The curable composition according to the present embodiment may contain only the hydrolyzable silyl group-containing organic polymer (A) as the curable polymer component, but may also contain the hydrolyzable silyl group-containing organic polymer (B) together with the hydrolyzable silyl group-containing organic polymer (A). The hydrolyzable silyl group-containing organic polymer (B) is as described above. The hydrolyzable silyl group-containing organic polymer (B) may be used alone or in combination of two or more kinds.

[0094] When the hydrolyzable silyl group-containing organic polymer (B) is blended, the blending ratio of the hydrolyzable silyl group-containing organic polymer (A) to the hydrolyzable silyl group-containing organic polymer (B) is not particularly limited, but is preferably 99:1 to 50:50, more preferably 95:5 to 60:40, and even more preferably 90:10 to 70:30, by weight ratio.

[0095] (curing catalyst) The curable composition according to this embodiment preferably contains a curing catalyst for the purpose of promoting the reaction of hydrolysis and condensation of the hydrolyzable silyl group, that is, the curing reaction.

[0096] As the curing catalyst, a conventionally known catalyst can be used. Specifically, an organic tin compound, a metal carboxylate, an amine compound, a carboxylic acid, an alkoxy metal, an inorganic acid, a mixture thereof, or the like can be used.

[0097] Specific examples of organic tin compounds include dibutyltin dilaurate, dibutyltin dioctanoate, dibutyltin bis(butyl maleate), dibutyltin diacetate, dibutyltin oxide, dibutyltin bis(acetylacetonate), a reaction product of dibutyltin oxide and a silicate compound, a reaction product of dibutyltin oxide and a phthalic acid ester, dioctyltin diacetate, dioctyltin dilaurate, dioctyltin bis(ethyl maleate), dioctyltin bis(octyl maleate), dioctyltin bis(acetylacetonate), dioctyltin distearate, dioctyltin oxide, and a reaction product of dioctyltin oxide and a silicate compound. Dioctyltin compounds are preferred due to the increasing interest in the environment in recent years.

[0098] Since the organic polymer (A) according to this embodiment can exhibit improved curability, the curable composition according to this embodiment does not contain an organotin compound, but can contain a curing catalyst (particularly, an amine compound, etc.) that is generally considered to have lower activity than an organotin compound. Even if the curable composition according to this embodiment contains an amine compound, it can exhibit good curability.

[0099] Specific examples of the metal carboxylate include tin carboxylate, bismuth carboxylate, titanium carboxylate, zirconium carboxylate, iron carboxylate, potassium carboxylate, calcium carboxylate, etc. The carboxylate group can be a combination of the following carboxylic acid with various metals.

[0100] Specific examples of the amine compound include amines such as octylamine, 2-ethylhexylamine, laurylamine, stearylamine, piperidine, 4-methylpiperidine, and hexamethyleneimine; nitrogen-containing heterocyclic compounds such as pyridine, 1,8-diazabicyclo[5,4,0]undecene-7 (DBU), and 1,5-diazabicyclo[4,3,0]nonene-5 (DBN); guanidines such as guanidine, phenylguanidine, and diphenylguanidine; biguanides such as butylbiguanide, 1-o-tolylbiguanide, and 1-phenylbiguanide; and ketimine compounds.

[0101] Specific examples of carboxylic acids include acetic acid, propionic acid, butyric acid, 2-ethylhexanoic acid, lauric acid, stearic acid, oleic acid, linoleic acid, neodecanoic acid, and versatic acid.

[0102] Specific examples of alkoxy metals include titanium compounds such as tetrabutyl titanate, titanium tetrakis(acetylacetonate), titanium ethylacetoacetate, and diisopropoxytitanium bis(ethylacetoacetate); aluminum compounds such as aluminum tris(acetylacetonate) and diisopropoxyaluminum ethylacetoacetate; and zirconium compounds such as zirconium tetrakis(acetylacetonate).

[0103] As other curing catalysts, fluorine anion-containing compounds, photoacid generators and photobase generators can also be used.

[0104] The curing catalyst may be a combination of two or more different catalysts. For example, the combination of the amine compound and a carboxylic acid or the amine compound and an alkoxy metal may provide an effect of improving reactivity.

[0105] The amount of the curing catalyst is preferably 0.001 to 20 parts by weight, more preferably 0.01 to 15 parts by weight, and particularly preferably 0.01 to 10 parts by weight, based on 100 parts by weight of the organic polymer (A) according to this embodiment. Furthermore, some curing catalysts may ooze onto the surface of the cured product after the curable composition is cured, or may contaminate the surface of the cured product. In such cases, the amount of the curing catalyst used is set to 0.01 to 3.0 parts by weight, so that the surface condition of the cured product can be kept good while ensuring the curability.

[0106] The curable composition according to the present embodiment may contain other additives, such as silicon compounds, adhesion promoters, plasticizers, solvents, diluents, silicates, fillers, sagging inhibitors, antioxidants, light stabilizers, UV absorbers, physical property regulators, tackifier resins, compounds containing epoxy groups, photocurable substances, oxygen curable substances, surface property improvers, epoxy resins, other resins, flame retardants, and foaming agents. In addition, the curable composition according to the present embodiment may contain various additives as necessary for the purpose of adjusting the physical properties of the composition or the cured product. Examples of such additives include, for example, curability regulators, radical inhibitors, metal deactivators, antiozonants, phosphorus-based peroxide decomposers, lubricants, pigments, and fungicides.

[0107] (Filler) The curable composition according to the present embodiment may contain various fillers, such as heavy calcium carbonate, colloidal calcium carbonate, magnesium carbonate, diatomaceous earth, clay, talc, titanium oxide, fumed silica, precipitated silica, crystalline silica, fused silica, anhydrous silicic acid, hydrous silicic acid, carbon black, ferric oxide, fine aluminum powder, zinc oxide, activated zinc oxide, PVC powder, PMMA powder, glass fiber and filament.

[0108] The amount of the filler used is preferably from 1 to 300 parts by weight, and more preferably from 10 to 250 parts by weight, based on 100 parts by weight of the organic polymer (A) according to this embodiment.

[0109] For the purpose of reducing the weight (specific gravity) of the composition, organic balloons or inorganic balloons may be added. The balloons are spherical fillers that are hollow inside, and the materials for these balloons include inorganic materials such as glass, shirasu, and silica, and organic materials such as phenol resin, urea resin, polystyrene, and saran.

[0110] The amount of the balloons used is preferably 0.1 to 100 parts by weight, and more preferably 1 to 20 parts by weight, based on 100 parts by weight of the organic polymer (A) according to this embodiment.

[0111] (Adhesion promoter) An adhesion promoter may be added to the curable composition according to the present embodiment. As the adhesion promoter, a silane coupling agent or a reaction product of a silane coupling agent may be added. Specific examples of the silane coupling agent include amino group-containing silanes such as γ-aminopropyltrimethoxysilane, γ-aminopropylmethyldimethoxysilane, N-β-aminoethyl-γ-aminopropyltrimethoxysilane, N-β-aminoethyl-γ-aminopropylmethyldimethoxysilane, N-phenyl-γ-aminopropyltrimethoxysilane, and (2-aminoethyl)aminomethyltrimethoxysilane; γ-isocyanatepropyltrimethoxysilane, γ-isocyanatepropyltriethoxysilane, and γ-isopropyltrimethoxysilane; Examples of the silanes include isocyanate group-containing silanes such as cyanate propyl methyl dimethoxy silane, α-isocyanate methyl trimethoxy silane, and α-isocyanate methyl dimethoxy methyl silane; mercapto group-containing silanes such as γ-mercapto propyl trimethoxy silane, γ-mercapto propyl triethoxy silane, and γ-mercapto propyl methyl dimethoxy silane; epoxy group-containing silanes such as γ-glycidoxy propyl trimethoxy silane and β-(3,4-epoxy cyclohexyl) ethyl trimethoxy silane. In addition, condensates of various silane coupling agents such as condensates of amino group-containing silanes and condensates of amino group-containing silanes and other alkoxy silanes; reactants of amino group-containing silanes and epoxy group-containing silanes, reactants of amino group-containing silanes and (meth)acrylic group-containing silanes, and the like can also be used. The adhesion promoters may be used alone or in combination of two or more.

[0112] The amount of the silane coupling agent used is preferably 0.1 to 20 parts by weight, and more preferably 0.5 to 10 parts by weight, based on 100 parts by weight of the organic polymer (A) according to this embodiment.

[0113] (Plasticizer) A plasticizer may be added to the curable composition according to this embodiment. Specific examples of plasticizers include phthalate compounds such as dibutyl phthalate, diisononyl phthalate (DINP), diheptyl phthalate, di(2-ethylhexyl) phthalate, diisodecyl phthalate (DIDP), and butyl benzyl phthalate; terephthalate compounds such as bis(2-ethylhexyl)-1,4-benzenedicarboxylate; non-phthalate compounds such as 1,2-cyclohexanedicarboxylate diisononyl ester; aliphatic polycarboxylic acid ester compounds such as dioctyl adipate, dioctyl sebacate, dibutyl sebacate, diisodecyl succinate, and tributyl acetyl citrate; unsaturated fatty acid ester compounds such as butyl oleate and methyl acetyl ricinoleate; alkylsulfonic acid phenyl esters; phosphate ester compounds; trimellitic acid ester compounds; chlorinated paraffins; hydrocarbon oils such as alkyl diphenyls and partially hydrogenated terphenyls; process oils; and epoxy plasticizers such as epoxidized soybean oil and epoxy benzyl stearate.

[0114] Also, a polymer plasticizer can be used. Specific examples of the polymer plasticizer include vinyl polymers, polyester plasticizers, polyether polyols such as polyethylene glycol and polypropylene glycol having a number average molecular weight of 500 or more, polyethers such as derivatives in which the hydroxyl groups of these polyether polyols are converted to ester groups, ether groups, etc., polystyrenes, polybutadiene, polybutene, polyisobutylene, butadiene-acrylonitrile, polychloroprene, etc. The plasticizers may be used alone or in combination of two or more kinds.

[0115] The polymer plasticizer may not have a hydrolyzable silyl group, but may have a hydrolyzable silyl group. A polymer plasticizer having a hydrolyzable silyl group acts as a reactive plasticizer and can prevent the migration of the plasticizer from the cured product. Examples of the hydrolyzable silyl group that the polymer plasticizer may have include those mentioned above as the hydrolyzable silyl group that the organic polymer (B) has. The number of hydrolyzable silyl groups contained in the polymeric plasticizer is preferably 1 or less, more preferably 0.8 or less, on average per molecule. The lower limit may be, for example, 0.01 or more. The number average molecular weight of the polymeric plasticizer having a hydrolyzable silyl group (particularly the oxyalkylene polymer having a hydrolyzable silyl group) is preferably lower than that of the organic polymer (A).

[0116] The amount of the plasticizer used is preferably 5 to 150 parts by weight, more preferably 10 to 120 parts by weight, and even more preferably 20 to 100 parts by weight, relative to 100 parts by weight of the organic polymer (A) according to this embodiment.

[0117] (Solvent, diluent) A solvent or diluent may be added to the curable composition according to this embodiment. The solvent and diluent are not particularly limited, but may be an aliphatic hydrocarbon, an aromatic hydrocarbon, an alicyclic hydrocarbon, a halogenated hydrocarbon, an alcohol, an ester, a ketone, an ether, or the like. When using a solvent or a diluent, the boiling point of the solvent is preferably 150°C or higher, more preferably 200°C or higher, and particularly preferably 250°C or higher, in view of the problem of air pollution when the composition is used indoors. The above solvents or diluents may be used alone or in combination of two or more kinds.

[0118] (Anti-sagging agent) The curable composition according to the present embodiment may contain an anti-sagging agent to prevent sagging and improve workability as necessary. Anti-sagging agents are not particularly limited, but examples thereof include polyamide waxes; hydrogenated castor oil derivatives; and metal soaps such as calcium stearate, aluminum stearate, and barium stearate. These anti-sagging agents may be used alone or in combination of two or more.

[0119] The amount of the sagging prevention agent used is preferably 0.1 to 20 parts by weight based on 100 parts by weight of the organic polymer (A) according to this embodiment.

[0120] (Antioxidants) An antioxidant (antiaging agent) can be used in the curable composition according to this embodiment. The use of an antioxidant can improve the weather resistance of the cured product. Examples of the antioxidant include hindered phenols, monophenols, bisphenols, and polyphenols. For example, Irganox 245, Irganox 1010, Irganox 1035, Irganox 1076, Irganox 1135, Irganox 1330, and Irganox 1520 (all manufactured by BASF); SONGNOX 1076 (manufactured by SONGWON), and BHT can be mentioned. Similarly, hindered amine light stabilizers such as TINUVIN 622LD, TINUVIN 144, TINUVIN 292, CHIMASSORB944LD, CHIMASSORB119FL (all manufactured by BASF); ADK STAB LA-57, ADK STAB LA-62, ADK STAB LA-67, ADK STAB LA-63, ADK STAB LA-68 (all manufactured by ADEKA Corporation); SANOL LS-2626, SANOL LS-1114, SANOL LS-744 (all manufactured by Sankyo Lifetech Co., Ltd.); and NOCRACK CD (manufactured by Ouchi Shinko Chemical Industry Co., Ltd.) can also be used. In addition, antioxidants such as SONGNOX4120, NOUGARD 445, and OKABEST CLX050 can also be used. Specific examples of antioxidants are also described in JP-A-4-283259 and JP-A-9-194731. The amount of the antioxidant used is preferably 0.1 to 10 parts by weight, and more preferably 0.2 to 5 parts by weight, based on 100 parts by weight of the organic polymer (A) according to this embodiment.

[0121] (Light stabilizer) A light stabilizer can be used in the curable composition according to the present embodiment. The use of a light stabilizer can prevent photo-oxidative deterioration of the cured product. Examples of light stabilizers include benzotriazole-based, hindered amine-based, and benzoate-based compounds, with hindered amine-based compounds being particularly preferred.

[0122] The amount of the light stabilizer used is preferably 0.1 to 10 parts by weight, and more preferably 0.2 to 5 parts by weight, based on 100 parts by weight of the organic polymer (A) according to this embodiment.

[0123] (UV absorber) The curable composition according to the present embodiment may contain an ultraviolet absorber. The use of an ultraviolet absorber may improve the surface weather resistance of the cured product. Examples of ultraviolet absorbers include benzophenone-based, benzotriazole-based, salicylate-based, substituted acrylonitrile-based, and metal chelate-based compounds, and benzotriazole-based compounds are particularly preferred, and examples of such ultraviolet absorbers include Tinuvin P, Tinuvin 213, Tinuvin 234, Tinuvin 326, Tinuvin 327, Tinuvin 328, Tinuvin 329, Tinuvin 571, Tinuvin 1600, and Tinuvin B75 (all manufactured by BASF). The amount of the ultraviolet absorber used is preferably 0.1 to 10 parts by weight, and more preferably 0.2 to 5 parts by weight, based on 100 parts by weight of the organic polymer (A) according to this embodiment.

[0124] (Physical property adjuster) The curable composition according to the present embodiment may contain a physical property adjuster for adjusting the tensile properties of the resulting cured product, if necessary. The physical property adjuster is not particularly limited, but examples thereof include alkylalkoxysilanes such as phenoxytrimethylsilane, methyltrimethoxysilane, dimethyldimethoxysilane, trimethylmethoxysilane, and n-propyltrimethoxysilane; arylalkoxysilanes such as diphenyldimethoxysilane and phenyltrimethoxysilane; alkylisopropenoxysilanes such as dimethyldiisopropenoxysilane, methyltriisopropenoxysilane, and γ-glycidoxypropylmethyldiisopropenoxysilane; trialkylsilylborates such as tris(trimethylsilyl)borate and tris(triethylsilyl)borate; silicone varnishes; and polysiloxanes. By using the physical property adjuster, the hardness of the curable composition according to the present embodiment can be increased when cured, or conversely, the hardness can be decreased to provide a breaking elongation. The physical property adjuster may be used alone or in combination of two or more kinds.

[0125] In particular, compounds that generate a compound having a monovalent silanol group in the molecule by hydrolysis have the effect of lowering the modulus of the cured product without worsening the stickiness of the surface of the cured product. In particular, compounds that generate trimethylsilanol are preferred. Examples of compounds that generate a compound having a monovalent silanol group in the molecule by hydrolysis include silicon compounds that are derivatives of alcohols such as hexanol, octanol, phenol, trimethylolpropane, glycerin, pentaerythritol, and sorbitol and generate silane monool by hydrolysis. Specific examples include phenoxytrimethylsilane, tris((trimethylsiloxy)methyl)propane, and the like.

[0126] The amount of the physical property adjuster used is preferably 0.1 to 10 parts by weight, and more preferably 0.5 to 5 parts by weight, based on 100 parts by weight of the organic polymer (A) according to this embodiment.

[0127] (tackifier resin) A tackifier resin can be added to the curable composition according to the present embodiment for the purpose of increasing the adhesiveness or adhesion to the substrate or for other reasons as necessary. There are no particular limitations on the tackifier resin, and any commonly used tackifier resin can be used.

[0128] Specific examples include terpene resins, aromatic modified terpene resins, hydrogenated terpene resins, terpene-phenol resins, phenol resins, modified phenol resins, xylene-phenol resins, cyclopentadiene-phenol resins, coumarone-indene resins, rosin resins, rosin ester resins, hydrogenated rosin ester resins, xylene resins, low molecular weight polystyrene resins, styrene copolymer resins, styrene block copolymers and their hydrogenated products, petroleum resins (e.g., C5 hydrocarbon resins, C9 hydrocarbon resins, C5C9 hydrocarbon copolymer resins, etc.), hydrogenated petroleum resins, DCPD resins, etc. These may be used alone or in combination of two or more.

[0129] The amount of the tackifier resin used is preferably 2 to 100 parts by weight, more preferably 5 to 50 parts by weight, and even more preferably 5 to 30 parts by weight, based on 100 parts by weight of the organic polymer (A) according to this embodiment.

[0130] (Compounds containing epoxy groups) In the curable composition according to the present embodiment, a compound containing an epoxy group can be used. The use of a compound having an epoxy group can improve the restorability of the cured product. Examples of the compound having an epoxy group include epoxidized unsaturated fats and oils, epoxidized unsaturated fatty acid esters, alicyclic epoxy compounds, compounds shown in epichlorohydrin derivatives, and mixtures thereof. Specific examples include epoxidized soybean oil, epoxidized linseed oil, bis(2-ethylhexyl)-4,5-epoxycyclohexane-1,2-dicarboxylate (E-PS), epoxy octyl stearate, and epoxy butyl stearate. The epoxy compound is preferably used in the range of 0.5 to 50 parts by weight per 100 parts by weight of the organic polymer (A) according to the present embodiment.

[0131] (light curing substance) A photocurable material can be used in the curable composition according to this embodiment. When a photocurable material is used, a film of the photocurable material is formed on the surface of the cured product, improving the stickiness and weather resistance of the cured product. Many compounds of this type are known, such as organic monomers, oligomers, resins, or compositions containing them. Representative compounds that can be used include unsaturated acrylic compounds, which are monomers, oligomers, or mixtures thereof having one or several acrylic or methacrylic unsaturated groups, polyvinyl cinnamates, or azido resins.

[0132] The amount of the photocurable substance used is preferably 0.1 to 20 parts by weight, and more preferably 0.5 to 10 parts by weight, based on 100 parts by weight of the organic polymer (A) according to this embodiment.

[0133] (oxygen curing substance) An oxygen-curable substance can be used in the curable composition according to the present embodiment. Examples of oxygen-curable substances include unsaturated compounds that can react with oxygen in the air, which react with oxygen in the air to form a cured film near the surface of the cured product, preventing the surface from becoming sticky and preventing dirt and dust from adhering to the surface of the cured product. Specific examples of oxygen-curable substances include drying oils such as tung oil and linseed oil, and various alkyd resins obtained by modifying these compounds; acrylic polymers, epoxy resins, and silicone resins modified with drying oils; and liquid polymers such as 1,2-polybutadiene, 1,4-polybutadiene, and C5-C8 diene polymers obtained by polymerizing or copolymerizing diene compounds such as butadiene, chloroprene, isoprene, and 1,3-pentadiene. These may be used alone or in combination of two or more.

[0134] The amount of the oxygen-curable substance used is preferably within a range of 0.1 to 20 parts by weight, more preferably 0.5 to 10 parts by weight, based on 100 parts by weight of the organic polymer (A) according to the present embodiment. As described in JP-A-3-160053, the oxygen-curable substance is preferably used in combination with a photocurable substance.

[0135] (Epoxy resin) The curable composition according to the present embodiment can be used in combination with an epoxy resin. The composition to which an epoxy resin is added is particularly preferred as an adhesive, particularly as an adhesive for exterior wall tiles. Examples of the epoxy resin include bisphenol A type epoxy resins and novolac type epoxy resins.

[0136] The ratio by weight of the epoxy resin to the organic polymer (A) according to this embodiment is preferably in the range of organic polymer (A) / epoxy resin=100 / 1 to 1 / 100.

[0137] When an epoxy resin is added, a curing agent for curing the epoxy resin can be used in combination with the curable composition according to the present embodiment. There are no particular limitations on the epoxy resin curing agent that can be used, and any commonly used epoxy resin curing agent can be used.

[0138] When a curing agent for an epoxy resin is used, the amount used is preferably within a range of 0.1 to 300 parts by weight per 100 parts by weight of the epoxy resin.

[0139] <<Preparation of Curable Composition>> The curable composition according to the present embodiment can be prepared as a one-component type in which all ingredients are mixed and sealed in advance and stored, and then cured by moisture in the air after application, or as a two-component type in which ingredients such as a curing catalyst, a filler, a plasticizer, and water are mixed separately as a curing agent, and the ingredients are mixed with the organic polymer composition before use. From the viewpoint of workability, the one-component type is preferred.

[0140] When the curable composition is of one-component type, all the components are mixed in advance, and therefore, it is preferable to use the components containing water after dehydration and drying in advance, or to dehydrate them by reducing pressure during mixing and kneading. In addition to the dehydration and drying method, the storage stability can be further improved by adding an alkoxysilane compound such as methyltrimethoxysilane, phenyltrimethoxysilane, n-propyltrimethoxysilane, vinyltrimethoxysilane, vinylmethyldimethoxysilane, γ-mercaptopropylmethyldimethoxysilane, γ-mercaptopropylmethyldiethoxysilane, or γ-glycidoxypropyltrimethoxysilane.

[0141] <Application> The curable composition according to the present embodiment can be used as a pressure sensitive adhesive, a sealing material for buildings, ships, automobiles, roads, etc., an adhesive, a waterproofing material, a coating waterproofing material, a mold release agent, an anti-vibration material, a vibration damping material, a soundproofing material, a foaming material, a paint, a spraying material, etc. The cured product obtained by curing the curable composition according to the present embodiment has excellent flexibility and adhesiveness, and can therefore be suitably used as a sealing material or adhesive.

[0142] The curable composition according to the present embodiment can be used in a wide range of applications, including electrical and electronic component materials such as solar cell back surface sealing materials, electrical and electronic components such as insulating coating materials for electric wires and cables, electrical insulating materials for devices, acoustic insulating materials, elastic adhesives, binders, contact adhesives, spray-type sealants, crack repair materials, tiling adhesives, adhesives for asphalt waterproofing materials, powder coatings, casting materials, medical rubber materials, medical adhesives, medical adhesive sheets, medical device sealants, dental impression materials, food packaging materials, and joint sealants for exterior materials such as sizing boards. It can be used for various applications such as adhesives, coating materials, anti-slip coating materials, buffer materials, primers, conductive materials for electromagnetic wave shielding, thermally conductive materials, hot melt materials, potting agents for electrical and electronic devices, films, gaskets, concrete reinforcing materials, temporary adhesives, various molding materials, and sealing materials for rust prevention and waterproofing of wired glass and laminated glass end faces (cut parts), liquid sealants used in automobile parts, large vehicle parts such as trucks and buses, train car parts, aircraft parts, ship parts, electrical parts, various machine parts, etc. For example, in automobiles, it can be used in a wide variety of applications such as adhesive installation of plastic covers, trims, flanges, bumpers, window mounting, interior parts, exterior parts, etc. Furthermore, since it can adhere to a wide range of substrates such as glass, porcelain, wood, metal, resin moldings, etc., either alone or with the help of a primer, it can also be used as various types of sealing compositions and adhesive compositions. The curable composition according to the present embodiment can also be used as an adhesive for interior panels, an adhesive for exterior panels, an adhesive for tiling, an adhesive for stone veneer, an adhesive for ceiling finishing, an adhesive for floor finishing, an adhesive for wall finishing, an adhesive for vehicle panels, an adhesive for assembling electric / electronic / precision equipment, an adhesive for bonding leather, textile products, fabric, paper, boards and rubber, a reactive post-crosslinking pressure-sensitive adhesive, a sealant for direct glazing, a sealant for double-glazing, a sealant for SSG construction, or a sealant for working joints of buildings, a material for civil engineering and bridge construction.Furthermore, it can also be used as an adhesive material such as an adhesive tape or an adhesive sheet.

[0143] The following items enumerate preferred aspects of the present disclosure, but the present invention is not limited to the following items. [Item 1] An organic polymer (A) having a hydrolyzable silyl group represented by the above general formula (1). (In formula (1), R 1 R represents a hydrolyzable group represented by the general formula (2). 2 represents a substituted or unsubstituted monovalent hydrocarbon group having 1 to 20 carbon atoms. X represents a hydroxyl group or R 1 a is 1, 2, or 3; b is 0, 1, or 2; c is 0, 1, or 2; and a+b+c is 3 or less. (In formula (2), R 3 R represents a substituted or unsubstituted divalent hydrocarbon group having 1 to 5 carbon atoms. 4 represents a hydrogen atom, a substituted or unsubstituted monovalent hydrocarbon group having 1 to 20 carbon atoms, or -OR 6 R 6 R represents a hydrogen atom or a substituted or unsubstituted monovalent hydrocarbon group having 1 to 20 carbon atoms. 5 represents an oxygen atom or a nitrogen atom bonded to any group. [Item 2] R 5 The organic polymer (A) according to item 1, wherein is an oxygen atom. [Item 3] R 1 is represented by any one of the formulas (3) to (9), [Item 4] 4. The organic polymer (A) according to any one of items 1 to 3, wherein the polymer skeleton of the organic polymer (A) is a polyoxyalkylene polymer. [Item 5] R contained in the entire organic polymer (A) 1 R out of the sum of X and 1 5. The organic polymer (A) according to any one of items 1 to 4, wherein the proportion (x) of is 10% or more. [Item 6] R contained in the entire organic polymer (A) 1 R out of the sum of X and 1 6. The organic polymer (A) according to any one of items 1 to 5, wherein the proportion (x) of is 20% or more. [Item 7] A curable composition comprising the organic polymer (A) according to any one of items 1 to 6. [Item 8] 8. A cured product obtained by curing the curable composition according to item 7. EXAMPLES

[0144] The present invention will be described in more detail below with reference to examples, but the present invention is not limited to these examples. The number average molecular weight in the examples is a GPC molecular weight measured under the following conditions. Liquid delivery system: Tosoh HLC-8420GPC Column: Tosoh TSKgel SuperH series Solvent: THF (tetrahydrofuran) Molecular weight: Polystyrene equivalent Measurement temperature: 40℃

[0145] Identification of the compound and the R hydrolyzable group 1 The ratio (x) was calculated using the following nuclear magnetic resonance (NMR) spectrometer: 1 This was measured by 1 H NMR. Equipment: AVANCE III HD500 digital equipment (BRUKER)

[0146] (Synthesis Example 1) Using polyoxypropylene glycol with a number average molecular weight of approximately 4,500 as an initiator, propylene oxide was polymerized with zinc hexacyanocobaltate glyme complex catalyst to obtain polyoxypropylene (P-1) with a number average molecular weight of 27,900 having hydroxyl groups at both ends. Sodium methoxide was added in an amount of 1.1 molar equivalents relative to the hydroxyl groups of the hydroxyl-terminated polyoxypropylene (P-1) as a 28% methanol solution. After removing the methanol by vacuum distillation, 1.3 molar equivalents of allyl chloride was added relative to the hydroxyl groups of the polymer (P-1) and reacted at 130°C for 1 hour, after which the allyl chloride was distilled off. The resulting unpurified allyl-terminated polyoxypropylene was mixed and stirred with n-hexane and water, after which the water was removed by centrifugation, and the hexane was removed from the resulting hexane solution by vacuum distillation to remove the metal salts in the polymer. As a result of the above, polyoxypropylene (Q-1) having carbon-carbon unsaturated bonds (allyl groups) was obtained. Next, 50 ppm of platinum divinyldisiloxane complex (3 wt% isopropanol solution in terms of platinum) and 0.89 wt. parts of trimethoxysilane were added to 100 wt. parts of polymer (Q-1) at 90°C to carry out a hydrosilylation reaction of the allyl groups in polymer (Q-1). The reaction was carried out at 90°C until trimethoxysilane was completely consumed, and then the volatile components were distilled off. As a result, polyoxypropylene (B-1) having trimethoxysilyl groups was obtained.

[0147] Example 1 To 100 parts by weight of polyoxypropylene (B-1) having trimethoxysilyl groups, 1800 ppm of 1% hydrogen chloride methanol solution was added, followed by the addition of 10 parts by weight of methanol and 2 parts by weight of hydroxyacetone, and the reaction was carried out at 70°C for 1 hour, after which 1800 ppm of epoxidized soybean oil (ADEKA O-130S) was added and stirred for 1 hour to remove hydrogen chloride. The volatile components were distilled off to obtain polyoxypropylene (A-1). 1 Analysis by H NMR spectroscopy revealed that the amount of methoxy groups in the trimethoxysilyl groups contained in the raw material was reduced, and the amount of hydrolyzable groups R 1 Furthermore, it was confirmed that the methoxy group and the hydrolyzable group R 1 R for the sum of 1 The ratio (x) was calculated by the above method and is shown in Table 1. The same applies below.

[0148] Example 2 To 100 parts by weight of polyoxypropylene (B-1) having trimethoxysilyl groups, 1800 ppm of 1% hydrogen chloride methanol solution was added, followed by the addition of 10 parts by weight of methanol and 4 parts by weight of hydroxyacetone, and the reaction was carried out at 70°C for 1 hour, after which 1800 ppm of epoxidized soybean oil (ADEKA O-130S) was added and stirred for 1 hour to remove hydrogen chloride. The volatile components were distilled off to obtain polyoxypropylene (A-2). 1 Analysis by H NMR spectroscopy revealed that the amount of methoxy groups in the trimethoxysilyl groups contained in the raw material was reduced, and the amount of hydrolyzable groups R 1 It was confirmed that this was occurring.

[0149] Example 3 To 100 parts by weight of polyoxypropylene (B-1) having trimethoxysilyl groups, 1800 ppm of 1% hydrogen chloride methanol solution was added, followed by the addition of 10 parts by weight of methanol and 6 parts by weight of hydroxyacetone, and the reaction was carried out at 70°C for 1 hour, after which 1800 ppm of epoxidized soybean oil (ADEKA O-130S) was added and stirred for 1 hour to remove hydrogen chloride. The volatile components were distilled off to obtain polyoxypropylene (A-3). 1 Analysis by H NMR spectroscopy revealed that the amount of methoxy groups in the trimethoxysilyl groups contained in the raw material was reduced, and the amount of hydrolyzable groups R 1 It was confirmed that this was occurring.

[0150] Example 4 To 100 parts by weight of polyoxypropylene (B-1) having trimethoxysilyl groups, 2700 ppm of 1% hydrogen chloride methanol solution was added, followed by the addition of 10 parts by weight of methanol and 3.7 parts by weight of 4-hydroxy-2-butanone, and the reaction was carried out at 70°C for 1 hour. After that, 2700 ppm of epoxidized soybean oil (ADEKA O-130S) was added and stirred for 1 hour to remove hydrogen chloride. The volatile components were distilled off to obtain polyoxypropylene (A-4). 1Analysis by H NMR spectroscopy revealed that the amount of methoxy groups in the trimethoxysilyl groups contained in the raw material was reduced, and the amount of hydrolyzable groups R 1 It was confirmed that this was occurring.

[0151] Example 5 To 100 parts by weight of polyoxypropylene (B-1) having trimethoxysilyl groups, 5400 ppm of 1% hydrogen chloride methanol solution was added, followed by 10 parts by weight of methanol and 4.3 parts by weight of 3-hydroxy-3-methyl-2-butanone, and the mixture was reacted at 70°C for 1 hour. After that, 5400 ppm of epoxidized soybean oil (ADEKA O-130S) was added and stirred for 1 hour to remove hydrogen chloride. The volatile components were distilled off to obtain polyoxypropylene (A-5). 1 Analysis by H NMR spectroscopy revealed that the amount of methoxy groups in the trimethoxysilyl groups contained in the raw material was reduced, and the amount of hydrolyzable groups R 1 It was confirmed that this was occurring.

[0152] Example 6 To 100 parts by weight of polyoxypropylene (B-1) having trimethoxysilyl groups, 5400 ppm of 1% hydrogen chloride methanol solution was added, followed by 15 parts by weight of methanol and 1.9 parts by weight of acetylacetone, and the mixture was reacted at 70°C for 1 hour, after which 5400 ppm of epoxidized soybean oil (ADEKA O-130S) was added and stirred for 1 hour to remove hydrogen chloride. The volatile components were distilled off to obtain polyoxypropylene (A-6). 1 The analysis was performed by H NMR spectroscopy, and the decrease in the methoxy groups in the trimethoxysilyl groups contained in the raw material was accompanied by the increase in the hydrolyzable groups R 1 It was confirmed that this was occurring.

[0153] Example 7 To 100 parts by weight of polyoxypropylene (B-1) having trimethoxysilyl groups, 1800 ppm of 1% hydrogen chloride methanol solution was added, followed by the addition of 10 parts by weight of methanol and 2.3 parts by weight of methyl glycolate, and the reaction was carried out at 70°C for 1 hour. After that, 1800 ppm of epoxidized soybean oil (ADEKA O-130S) was added and stirred for 1 hour to remove hydrogen chloride. The volatile components were distilled off to obtain polyoxypropylene (A-7). 1 The analysis was performed by H NMR spectroscopy, and the decrease in the methoxy groups in the trimethoxysilyl groups contained in the raw material was accompanied by the increase in the hydrolyzable groups R 1 It was confirmed that this was occurring.

[0154] Example 8 To 100 parts by weight of polyoxypropylene (B-1) having trimethoxysilyl groups, 5400 ppm of 1% hydrogen chloride methanol solution was added, followed by 15 parts by weight of methanol and 1.2 parts by weight of dihydroxyacetone, and the reaction was carried out at 70°C for 1 hour. After that, 5400 ppm of epoxidized soybean oil (ADEKA O-130S) was added and stirred for 1 hour to remove hydrogen chloride. The volatile components were distilled off to obtain polyoxypropylene (A-8). 1 The analysis was performed by H NMR spectroscopy, and the decrease in the methoxy groups in the trimethoxysilyl groups contained in the raw material was accompanied by the increase in the hydrolyzable group R 1 It was confirmed that this was occurring.

[0155] (Synthesis Example 2) To 100 parts by weight of polyoxypropylene (Q-1) having carbon-carbon unsaturated bonds (allyl groups) obtained in Synthesis Example 1, 50 ppm of platinum divinyldisiloxane complex (3 wt% isopropanol solution in terms of platinum) and 1.33 parts by weight of triethoxysilane were added to carry out a hydrosilylation reaction of the allyl groups of the polymer (Q-1). The reaction was carried out at 90°C until the triethoxysilane was completely consumed, and then the volatile components were distilled off. As a result, polyoxypropylene (B-2) having triethoxysilyl groups was obtained.

[0156] Example 9 To 100 parts by weight of polyoxypropylene (B-2) having triethoxysilyl groups, 2700 ppm of 1% hydrogen chloride methanol solution was added, followed by 14 parts by weight of ethanol and 3.2 parts by weight of hydroxyacetone, and the mixture was reacted at 70°C for 1 hour, after which 2700 ppm of epoxidized soybean oil (ADEKA O-130S) was added and stirred for 1 hour to remove hydrogen chloride. The volatile components were distilled off to obtain polyoxypropylene (A-9). 1 Analysis by H NMR spectroscopy revealed that the amount of ethoxy groups in the triethoxysilyl groups contained in the raw material was reduced, and the amount of hydrolyzable groups R 1 It was confirmed that this was occurring.

[0157] Example 10 To 100 parts by weight of polyoxypropylene (B-2) having triethoxysilyl groups, 2700 ppm of 1% hydrogen chloride methanol solution was added, followed by the addition of 10 parts by weight of ethanol and 6 parts by weight of hydroxyacetone, and the reaction was carried out at 70°C for 1 hour, after which 2700 ppm of epoxidized soybean oil (ADEKA O-130S) was added and stirred for 1 hour to remove hydrogen chloride. The volatile components were distilled off to obtain polyoxypropylene (A-10). 1 Analysis by H NMR spectroscopy revealed that the amount of ethoxy groups in the triethoxysilyl groups contained in the raw material was reduced, and the amount of hydrolyzable groups R 1 It was confirmed that this was occurring.

[0158] (Synthesis Example 3) To 100 parts by weight of the hydroxyl-terminated polyoxypropylene (P-1), 30 ppm of a bismuth (III) 2-ethylhexanoate solution (Bi: 25%) and 0.95 molar equivalents of (3-isocyanatepropyl)trimethoxysilane relative to the hydroxyl groups of the polymer were added, and a urethanization reaction was carried out on the hydroxyl groups of the polymer to obtain polyoxypropylene (B-3) having trimethoxysilyl groups.

[0159] Example 11 To 100 parts by weight of polyoxypropylene (B-3) having trimethoxysilyl groups, 5400 ppm of 1% hydrogen chloride methanol solution was added, followed by the addition of 10 parts by weight of methanol and 1.8 parts by weight of hydroxyacetone, and the reaction was carried out at 70°C for 3 hours. After that, 2700 ppm of epoxidized soybean oil (ADEKA O-130S) was added and stirred for 1 hour to remove hydrogen chloride. The volatile components were distilled off to obtain polyoxypropylene (A-11). 1 Analysis by H NMR spectroscopy revealed that the amount of methoxy groups in the trimethoxysilyl groups contained in the raw material was reduced, and the amount of hydrolyzable groups R 1 However, since the peaks corresponding to the hydrolyzable groups before and after the reaction overlapped, R 1 It was not possible to calculate the proportion (x) of

[0160] (Synthesis Example 4) To 100 parts by weight of polyoxypropylene (B-1) having trimethoxysilyl groups, 2700 ppm of 1% hydrogen chloride methanol solution was added, and then 22 parts by weight of ethanol was added and reacted at 70°C for 1 hour, after which 2700 ppm of epoxidized soybean oil (ADEKA O-130S) was added and stirred for 1 hour to remove hydrogen chloride. The volatile components were distilled off to obtain polyoxypropylene (A'-1). 1 Analysis by H NMR spectroscopy confirmed that the number of methoxy groups in the trimethoxysilyl groups contained in the raw material was reduced and that ethoxy groups were generated as hydrolyzable groups in the hydrolyzable silyl groups.

[0161] (Examples 12 to 22, Comparative Examples 1 to 4) Under an atmosphere of 23°C and relative humidity of 50%, 0.5 parts by weight of DBU (1,8-diazabicyclo[5,4,0]undecene-7, manufactured by Tokyo Chemical Industry Co., Ltd.) was added to 100 parts by weight of the polymer shown in Table 1 filled in a plastic container, and the mixture was stirred with a spatula for 1 minute to mix.

[0162] (Skinning time) The time when mixing was completed was defined as the start time of measurement, and the time when the surface was touched with a spatula and the composition to be evaluated no longer adhered to the spatula was defined as the skinning time. The results are shown in Table 1.

[0163] [Table 1]

[0164] As is clear from Table 1, the methoxy group in the trimethoxysilyl group of the polymer (B-1) was converted to a specific hydrolyzable group R by an exchange reaction using a specific hydroxyl group-containing compound. 1 The polymers (A-1) to (A-8) in which the hydrolyzable group R was replaced by the 1 It can be seen that the introduction of

[0165] Similarly, the ethoxy group in the triethoxysilyl group of the polymer (B-2) is converted to a specific hydrolyzable group R by an exchange reaction using hydroxyacetone. 1 The polymer (A-9) or (A-10) in which the hydrolyzable group R is replaced by the triethoxysilyl group has a shorter skinning time than the polymer (B-2) having a triethoxysilyl group. 1 It can be seen that the introduction of The same can be said from a comparison between Example (A-11) and Polymer (B-3).

[0166] In addition, from Examples 12 to 14, the hydrolyzable group R 1 It can be seen that the larger the ratio (x), the shorter the skinning time and the better the hardening property.

[0167] On the other hand, in Comparative Example 2, the methoxy group of the polymer (B-1) was converted to an ethoxy group (R 1The polymer (A'-1) in which the hydrolyzable group R is replaced with a group not corresponding to the above group has a lower curability than the polymer (B-1). 1 It is clear that this is due to the following.

Claims

1. An organic polymer (A) having a hydrolyzable silyl group, represented by the following general formula (1): [Formula 1] (In formula (1), R 1 R represents a hydrolyzable group represented by the following general formula (2). 2 represents a substituted or unsubstituted monovalent hydrocarbon group having 1 to 20 carbon atoms. X represents a hydroxyl group or R 1 a is 1, 2, or 3; b is 0, 1, or 2; c is 0, 1, or 2; and a+b+c is 3 or less. [Case 2] (In formula (2), R 3 R represents a substituted or unsubstituted divalent hydrocarbon group having 1 to 5 carbon atoms. 4 represents a hydrogen atom, a substituted or unsubstituted monovalent hydrocarbon group having 1 to 20 carbon atoms, or -OR 6 represents R 6 R represents a hydrogen atom or a substituted or unsubstituted monovalent hydrocarbon group having 1 to 20 carbon atoms. 5 represents an oxygen atom or a nitrogen atom bonded to any group.

2. R 5 The organic polymer (A) according to claim 1 , wherein is an oxygen atom.

3. R 1 The organic polymer (A) according to claim 2, wherein the organic polymer (A) is represented by any one of the following formulas (3) to (9): [C3] [C4] [C5] [C6] [C7] [C8] [C9]

4. The organic polymer (A) according to any one of claims 1 to 3, wherein the polymer skeleton of the organic polymer (A) is a polyoxyalkylene-based polymer.

5. R contained in the entire organic polymer (A) 1 Of the sum of and X, R 1 The organic polymer (A) according to any one of claims 1 to 3, wherein the ratio (x) is 10% or more.

6. R contained in the entire organic polymer (A) 1 Of the sum of and X, R 1 The organic polymer (A) according to any one of claims 1 to 3, wherein the ratio (x) is 20% or more.

7. A curable composition comprising the organic polymer (A) according to any one of claims 1 to 3.

8. A cured product obtained by curing the curable composition according to claim 7.

Citation Information

Patent Citations

  • Method for producing modified conjugated diene rubber, modified conjugated diene rubber and rubber composition

    JP2012193277A

  • Modified conjugated diene polymer, modified conjugated diene polymer composition and manufacturing method thereof

    JP2014055264A

  • Modified conjugated diene rubber, method for producing same, and rubber composition

    WO2012147565A1

  • Method for producing polyether

    WO2019203233A1

  • Method for issuing electronic money through gold coin recognition