Ph-responsive polymer and method for producing the same
A pH-responsive polymer with specific structural units addresses the challenge of maintaining solubility and insolubility for medical applications, providing high biocompatibility and water resistance by switching states based on pH conditions.
Patent Information
- Application Number
- JP2023056408
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Filing Date
- 2023-03-30
- Publication Date
- 2024-10-11
- Estimated Expiration
- Not applicable · inactive patent
AI Technical Summary
Existing biocompatible polymers face challenges in maintaining water solubility and insolubility states for medical applications, particularly due to poor temperature stability and solvent compatibility, leading to protein adsorption and reduced effectiveness.
Development of a pH-responsive polymer with specific structural units that switch between water-soluble and water-insoluble states based on pH conditions, allowing dissolution in safe polar solvents like water or ethanol and enhanced water resistance through hydrogenation of carboxyl groups.
The polymer exhibits high biocompatibility, low protein adsorption, and improved water resistance, suitable for medical applications by switching between soluble and insoluble states for enhanced performance in medical supplies and coatings.
Smart Images

Figure 2024143633000001 
Figure 2024143633000002 
Figure 2024143633000003
Abstract
Description
[Technical field]
[0001] The present invention relates to a polymer that is used primarily in the medical field and whose properties change in response to pH, and to a method for producing this polymer. [Background technology]
[0002] When artificial organs, tissues, medical devices, etc. are implanted in the body or used in contact with the living body, a defense reaction against these artificial foreign substances occurs. When an artificial material first comes into contact with a living body, plasma proteins are adsorbed, and cells adhere to the surface of the artificial material via the adsorbed proteins. As a result, blood clots are formed in the blood and adhere to the surface of the artificial material, and in connective tissue, the artificial material is covered with a collagen fibrous capsule. This makes it impossible for the artificial material to perform its original function of replacing the living body. In addition, when an artificial material comes into contact with a living body, complement in the plasma is activated, which triggers a series of immune reactions that kill the body's own cells.
[0003] To solve these problems, efforts are underway to develop biocompatible materials that have little or no interaction with biological components such as proteins and blood cells. In the biomedical field, polyethylene glycol (PEG) and materials to which PEG is added are widely used due to their high biocompatibility and hydrophilic properties. However, PEG loses its repulsive properties against proteins at temperatures above 35°C, making it prone to protein adsorption.
[0004] In addition, since biomembrane lipids have phosphorylcholine (PC) groups, which are phospholipid polar groups, polymers of 2-methacryloyloxyethyl phosphorylcholine (MPC) carrying PC groups have been developed (Non-Patent Document 1). Since MPC homopolymers have a betaine structure and are water-soluble, they have poor water resistance and may be dissolved or partially lost in vivo. In addition, alcohols, which are frequently used in medical settings, may cause the polymer to be dissolved or partially disintegrate. For this reason, although MPC homopolymers are biocompatible materials, they are not suitable as medical materials to be used in vivo. Since MPC has a methacryloyl group with excellent polymerizability, it can be copolymerized with various vinyl monomers, and it can be made water-insoluble by selecting the vinyl monomer to be copolymerized. However, water-insoluble polymers are difficult to use in medical products because they cannot be dissolved in safe polar solvents such as water or ethanol when they are applied to an article or when they are stretched or molded. For use in medical products, water-soluble polymers are desirable. Therefore, there is a demand for polymers that are water-soluble and can be dissolved in safe polar solvents such as water or ethanol during coating, stretching, and molding, and that can be made water-insoluble when in use to improve water resistance. [Prior art documents] [Non-patent literature]
[0005] [Non-Patent Document 1] Polymer Journal, Vol. 22, p. 355, 1990 Summary of the Invention [Problem to be solved by the invention]
[0006] An object of the present invention is to provide a biocompatible polymer that can be switched between a water-soluble state and a water-insoluble state by a simple operation, and a method for producing the polymer. [Means for solving the problem]
[0007] In order to solve the above problems, the present inventors have conducted extensive research and have found that [ka] A structural unit represented by the following formula (2): [ka] A structural unit represented by the following formula (3): [ka] and a structural unit represented by the following formula (4): [ka] Structural unit represented by (In formulas (1) to (4), R1 represents a hydrogen atom or a methyl group, R2 represents an oxygen atom or -NH-, and two n's independently represent an integer of 1 to 4.) At least one structural unit (a) selected from the group consisting of: The following formula (5) -CH2-CR3(CONH-R4-COOM)- (5) (In formula (5), R3 represents a hydrogen atom or a methyl group, R4 represents a linear or branched, saturated or unsaturated divalent hydrocarbon group having 5 to 16 carbon atoms, and M represents a hydrogen atom or a counter cation.) Contains a structural unit (b) represented by the ratio of the amount of the structural unit (b) to the total amount of the structural unit (a) and the structural unit (b) is 10 to 98 mol %, It has been found that a polymer having a number-average molecular weight of 5,000 or more has biocompatibility and can be made water-soluble or water-insoluble in response to pH. This polymer is water-soluble under alkaline conditions because M is a counter cation, and is water-insoluble under acidic conditions because M is a hydrogen atom, and has higher water resistance than when it is water-soluble.
[0008] The present invention has been completed based on the above findings, and provides the following [1] to [9]. [1] The following formula (1) [ka] A structural unit represented by the following formula (2): [ka] A structural unit represented by the following formula (3): [ka] and a structural unit represented by the following formula (4): [ka] Structural unit represented by (In formulas (1) to (4), R1 represents a hydrogen atom or a methyl group, R2 represents an oxygen atom or -NH-, and two n's independently represent an integer of 1 to 4.) At least one structural unit (a) selected from the group consisting of: The following formula (5) -CH2-CR3(CONH-R4-COOM)- (5) (In formula (5), R3 represents a hydrogen atom or a methyl group, R4 represents a linear or branched, saturated or unsaturated divalent hydrocarbon group having 5 to 16 carbon atoms, and M represents a hydrogen atom or a counter cation.) Contains a structural unit (b) represented by the ratio of the amount of the structural unit (b) to the total amount of the structural unit (a) and the structural unit (b) is 10 to 98 mol %, A polymer with a number average molecular weight of 5,000 or more. [2] The polymer according to [1], wherein the counter cation of M in the formula (5) is an alkali metal ion, an ammonium ion, or an organic cation. [3] The polymer according to [1] or [2], wherein R4 in the formula (5) is a linear, saturated, divalent hydrocarbon group having 8 to 12 carbon atoms. [4] The polymer according to [1] or [2], wherein the total amount of the structural unit (a) and the structural unit (b) is 40 mol % or more based on the total amount of the structural units constituting the polymer. [5] The polymer according to [1] or [2], which is used for suppressing protein adsorption. [6] A film, coating, fiber, or bulk molded article comprising the polymer according to [1] or [2]. [7] The following formula (6) [ka] A compound represented by the following formula (7): [ka] A compound represented by the following formula (8): [ka] and a compound represented by the following formula (9): [ka] (In formulas (6) to (9), R1 represents a hydrogen atom or a methyl group, R2 represents an oxygen atom or -NH-, and two n's independently represent an integer of 1 to 4.) and at least one compound having a betaine structure selected from the group consisting of compounds represented by the following formula (10): CH2=CR3(CONH-R4-COOM) (10) (In formula (10), R3 represents a hydrogen atom or a methyl group, R4 represents a linear or branched, saturated or unsaturated divalent hydrocarbon group having 5 to 16 carbon atoms, and M represents a hydrogen atom or a counter cation.) The method for producing the polymer according to [1], comprising a step of polymerizing a monomer containing a compound represented by the following formula: [8] A method for producing an article, comprising a step of molding the polymer according to [1] or [2] in a state where the polymer is dissolved in a polar solvent under alkaline conditions. [9] A method for improving the water resistance of an article produced by the method according to [8], by placing the article under acidic conditions. Effect of the Invention
[0009] The polymer of the present invention has high biocompatibility and can be used as a material for medical supplies or a covering material for medical supplies that are to be embedded in or in contact with a living body. In particular, the polymer of the present invention is suitable as a material for medical supplies or a covering material for medical supplies because of its low protein adsorption. In addition, the polymer of the present invention is water-soluble due to ionization of the carboxyl group under alkaline conditions, so it can be dissolved in a safe polar solvent such as water or ethanol and processed. The carboxyl group can be hydrogenated to make the polymer water-insoluble by placing it under acidic conditions before contacting the polymer with a living body. In the water-insoluble state, the polymer has excellent water resistance, so the polymer in the medical supplies or coating is unlikely to dissolve even when it comes into contact with water in the living body. Thus, the polymer of the present invention has both the property of being able to be dissolved in a safe polar solvent for processing and the property of being excellent in water resistance. Moreover, the switching between water-soluble and water-insoluble can be performed by a simple operation of adjusting the pH. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0010] The present invention will be described in detail below. (1) pH-responsive polymers The polymer of the present invention contains a structural unit represented by the above formula (1), a structural unit represented by the formula (2), a structural unit represented by the formula (3), and / or a structural unit represented by the formula (4) (structural unit (a)), and a structural unit (b) represented by the above formula (5), in which the ratio of the amount of structural unit (b) to the total amount of structural units (a) and (b) is 10 to 98 mol %, and the number average molecular weight is 5,000 or more. The structural units represented by formulas (1) to (4) have in common the fact that they each have a betaine structure.
[0011] In formula (1), formula (2), formula (3), and formula (4), the two n's can be independently 1, 2, 3, or 4. In formula (5), R4 is a linear or branched, saturated or unsaturated divalent hydrocarbon group having 5 to 16 carbon atoms, and the number of carbon atoms can be 6 or more, 7 or more, 8 or more, 9 or more, or 10 or more, and can be 15 or less, 14 or less, 13 or less, 12 or less, or 11 or less. Furthermore, R4 is preferably a linear saturated divalent hydrocarbon group, ie, an alkylene group.
[0012] M in formula (5) is a counter cation of the carboxyl group under alkaline conditions, and a hydrogen atom under acidic conditions. The alkaline conditions under which M becomes a counter cation of the carboxyl group vary depending on the structure of the polymer, but generally, M becomes a counter cation at pH 7.1 or higher. Similarly, the acidic conditions under which M becomes a hydrogen atom vary depending on the structure of the polymer, but generally, M becomes a hydrogen atom at pH 7.0 or lower.
[0013] Examples of the counter cation include alkali metal ions such as sodium ion, potassium ion, and lithium ion; ammonium ion; and organic cations such as organic ammonium ion. Examples of organic ammonium ions include cations quaternized by alkylation of aliphatic tertiary amines such as trimethylamine, triethylamine, tripropylamine, tributylamine, diisopropylethylamine, dimethylethylamine, dimethylpropylamine, dimethylbutylamine, dimethylpentylamine, dimethylhexylamine, dimethylheptylamine, dimethyloctylamine, dimethylnonylamine, dimethyldecylamine, dimethyllaurylamine, dimethylmyristylamine, dimethylstearylamine, and dimethyloleylamine; quaternary ammonium ions such as glycidyltrimethylammonium ion; quaternary imidazolium ions such as 1-decyl-3-methylimidazolium ion, 1-methyl-3-octylimidazolium ion, and 1-methyl-benzimidazolium ion; and quaternary pyridinium ions such as butylpyridinium ion and dodecylpyridinium ion. The counter cation of the carboxyl group may be a cation derived from an alkali to create alkaline conditions. The counter cation is preferably an alkali metal ion, and more preferably a sodium ion.
[0014] The polymer of the present invention may contain, as structural unit (a), one or more of the units represented by formulae (1) to (4), and may contain, as structural unit (a), one or more of the units represented by formulae (1), (2), (3), and / or (4). The polymer of the present invention may contain, as structural unit (b), one or more of the structural units (b).
[0015] The ratio of the amount of the structural unit (b) to the total amount of the structural unit (a) and the structural unit (b) can be 10 mol% or more, 20 mol% or more, 30 mol% or more, 40 mol% or more, 50 mol% or more, 60 mol% or more, 70 mol% or more, 80 mol% or more, or 90 mol% or more. Within this range, the sensitivity of the pH response is improved, and good water resistance is obtained under acidic conditions. In addition, the ratio of the amount of the structural unit (b) to the total amount of the structural unit (a) and the structural unit (b) can be 98 mol% or less, 95 mol% or less, 90 mol% or less, 80 mol% or less, 70 mol% or less, 60 mol% or less, 50 mol% or less, 40 mol% or less, 30 mol% or less, or 20 mol% or less. Within this range, the amount of the structural unit (a) is not too small, and sufficient protein adsorption suppression ability is obtained. The polymer of the present invention may be any of a random copolymer, a block copolymer, an alternating copolymer, and a graft copolymer. The polymer of the present invention may be any of a linear chain polymer and a branched chain polymer, but is preferably a linear chain polymer.
[0016] The number average molecular weight of the polymer of the present invention is 5,000 or more, but can be 10,000 or more, 50,000 or more, or 100,000 or more. Within this range, the polymer has sufficient mechanical strength and solvent resistance and is difficult to dissolve in water. The number average molecular weight can be 100,000,000 or less, 50,000,000 or less, 10,000,000 or less, or 5,000,000 or less. Within this range, the polymer is easily dissolved in a polar solvent such as water under alkaline conditions during molding processing.
[0017] The polymer of the present invention may have polymerizable structural units in addition to the structural units (a) and (b) as long as the protein adsorption inhibitory effect, biocompatibility, and pH responsiveness are not impaired. Examples of such structural units include vinyl monomers and diene monomers. Examples of aliphatic vinyl monomers include olefin monomers having one unsaturated bond (ethylene, propylene, etc.), carboxy group-containing monomers (acrylic acid, methacrylic acid, carboxyethyl acrylate, carboxypentyl acrylate, itaconic acid, maleic acid, fumaric acid, crotonic acid, isocrotonic acid, etc.), acid anhydride group-containing monomers (maleic anhydride, itaconic anhydride, etc.), hydroxyl group-containing monomers (2-hydroxyethyl (meth)acrylate, 2-hydroxypropyl ... (meth)acrylate hydroxyalkyl such as (meth)acrylates such as butyl acrylate, 3-hydroxypropyl acrylate, 4-hydroxybutyl acrylate, 6-hydroxyhexyl acrylate, 8-hydroxyoctyl acrylate, 10-hydroxydecyl acrylate, 12-hydroxylauryl acrylate, and (4-hydroxymethylcyclohexyl)methyl (meth)acrylate), sulfonic acid group- or phosphoric acid group-containing monomers (styrene sulfonic acid, allyl sulfonic acid, sodium vinyl sulfonate, etc.), acrylate, 2-(meth)acrylamido-2-methylpropanesulfonic acid, (meth)acrylamidopropanesulfonic acid, sulfopropyl (meth)acrylate, (meth)acryloyloxynaphthalenesulfonic acid, 2-hydroxyethyl acryloyl phosphate, etc.), epoxy group-containing monomers (glycidyl (meth)acrylate, methyl glycidyl (meth)acrylate, (meth)acrylic acid-2-ethyl glycidyl ether, allyl glycidyl ether, (meth)acrylic acid glycidyl ether, etc.), cyano group-containing monomers - (acrylonitrile, methacrylonitrile, etc.), isocyanate group-containing monomers (2-isocyanatoethyl (meth)acrylate, etc.), amide group-containing monomers ((meth)acrylamide; N,N-dimethyl (meth)acrylamide, N,N-diethyl (meth)acrylamide, N,N-dipropyl (meth)acrylamide, etc.), amino group-containing monomers (aminoethyl (meth)acrylate, N,N-dimethylaminoethyl (meth)acrylate, t-butylaminoethyl (meth)acrylate, etc.). The aromatic vinyl monomer may, for example, be styrene. Diene monomers include butadiene, isoprene, chloroprene, and the like.
[0018] The structural units other than the structural units (a) and (b) may be used alone or in combination of two or more. Even when the polymer of the present invention contains structural units other than the structural units (a) and (b), the ratio of the total amount of the structural units (a) and (b) to the total amount of the structural units constituting the polymer is preferably 40 mol% or more, 50 mol% or more, 60 mol% or more, 70 mol% or more, 80 mol% or more, 90 mol% or more, or 95 mol% or more. The polymer of the present invention is preferably composed only of the structural units (a) and (b).
[0019] (2) Method for producing the polymer of the present invention The polymer of the present invention described above is represented by the following formula (6): [ka] A compound represented by the following formula (7): [ka] A compound represented by the following formula (8): [ka] and a compound represented by the following formula (9): [ka] (In formulas (6) to (9), R1 represents a hydrogen atom or a methyl group, R2 represents an oxygen atom or -NH-, and two n's independently represent an integer of 1 to 4.) and at least one compound having a betaine structure selected from the group consisting of compounds represented by the following formula (10): CH2=CR3(CONH-R4-COOM) (10) (In formula (10), R3 represents a hydrogen atom or a methyl group, R4 represents a linear or branched, saturated or unsaturated divalent hydrocarbon group having 5 to 16 carbon atoms, and M represents a hydrogen atom or a counter cation.) and polymerizing a monomer containing a compound represented by the following formula (10):
[0020] The polymerization may be polyaddition, radical polymerization, ionic polymerization, etc. Polymerization conditions such as polymerization initiator, solvent, temperature, and time can be appropriately adjusted by those skilled in the art. The other conditions are as explained for the polymer of the present invention.
[0021] (3) A method for producing an article using the polymer of the present invention The polymer of the present invention described above can be dissolved in a solvent and molded into a shape such as a membrane (film, sheet), coating, fiber, block article, etc. That is, the polymer of the present invention can be dissolved in a solvent and molded to produce an article. Since the polymer of the present invention has excellent biocompatibility and low protein adsorption, it can be suitably used as a material for medical products that are embedded in a living body and used, such as artificial blood vessels, artificial heart valves, artificial joints, artificial skin, scaffolds for cell growth in artificial tissues or artificial bones, dental materials, tissue adhesives, cardiac pacemakers, stents, and surgical sutures; medical products that are used in contact with a living body, such as catheters, contact lenses, substrates for sustained release drug delivery, and endoscopes; medical products that are used in contact with materials separated from a living body, such as hemodialysis membranes and blood storage packs; and covering materials for these medical products. Medical supplies that are buried in the body and come into contact with body fluids for long periods of time may have the possibility of the polymer eluting in the body. However, the polymer of the present invention can be switched to a state with excellent water resistance before use, and therefore is particularly suitable for use as a material for medical supplies that are buried in the body.
[0022] The polymer of the present invention may be molded under alkaline conditions in a state of being dissolved in a polar solvent, such as water, a buffer solution, or a mixture of water or a buffer solution with other polar solvents. Examples of buffer solutions having a buffer range in the alkaline region include Tris-hydrochloric acid buffer solutions, phosphate buffer solutions, boric acid-sodium borate buffer solutions, carbonate-bicarbonate buffer solutions, and HEPES-NaOH buffer solutions. Examples of polar solvents other than water and buffer solutions include ethanol, isopropanol, polyhydric alcohols (polyethylene glycol, propylene glycol, dipropylene glycol, butylene glycol, glycerin, diglycerin, isoprene glycol, etc.).
[0023] The pH when dissolving in a polar solvent varies depending on the type of polymer, but generally, at pH 7.1 or higher, M of the structural unit represented by formula (5) can be made into a counter cation. The pH can be 7.5 or higher, 8 or higher, 9 or higher, 10 or higher, 11 or higher, 12 or higher, or 13 or higher. The pH can be 14 or lower, 13 or lower, 12 or lower, or 11 or lower.
[0024] To obtain alkaline conditions, a pH adjuster such as hydroxides such as sodium hydroxide and potassium hydroxide, ammonia, and organic amines such as monoethanolamine, diethanolamine, triethanolamine, monoisopropanolamine, diisopropanolamine, triisopropanolamine, and tetrahydroxypropylethylenediamine (these are organic amines that dissolve in ethanol) may be added to the solvent. Alternatively, the pH of a buffer solution having a buffering capacity in the alkaline region may be adjusted.
[0025] The polymer of the present invention can be molded by itself or in combination with other polymers.
[0026] By placing the molded polymer under acidic conditions, M in the structural unit represented by formula (5) becomes a hydrogen atom, improving water resistance. The pH for changing M in formula (5) to a hydrogen atom varies depending on the type of polymer, but can generally be pH 7.0 or less. The pH can be 6.5 or less, 6 or less, 5 or less, 4 or less, 3 or less, or 2 or less. The pH can be 1 or more, 2 or more, 3 or more, or 4 or more.
[0027] To achieve acidic conditions, inorganic acids such as hydrochloric acid and phosphoric acid, and organic acids such as acetic acid, malic acid, lactic acid, citric acid, fumaric acid, tartaric acid, succinic acid, gluconic acid, and adipic acid may be added to the solvent. Alternatively, acidic conditions may be achieved by using a buffer solution having a buffering capacity in the acidic range. Examples of buffer solutions having a buffering capacity in the acidic range include phosphate buffer solutions, acetic acid-sodium acetate buffer solutions, and citric acid-sodium citrate buffer solutions. EXAMPLES
[0028] The present invention will be described in more detail below by way of examples, but the present invention is not limited to these. (1) Polymer production Synthesis of compound of formula (10) (AaU monomer) In formula (10), R3 is a hydrogen atom, R4 is an alkylene group having 10 carbon atoms (-C 10 H 20 -) (hereinafter, sometimes abbreviated as "AaU monomer") was synthesized by the following procedure. 36g of sodium hydroxide and 1.5L of water were added to a beaker and completely dissolved. 40.3g of 11-aminoundecanoic acid was added to the solution and dissolved (Solution 1). Meanwhile, 50.5mL of acryloyl chloride and 100mg of 2,6-di-t-butylcresol were weighed and mixed in a beaker to dissolve the solids (Solution 2). Solution 2 was added dropwise to solution 1 while stirring. After stirring for 3 hours at room temperature, 6N hydrochloric acid was added to adjust the pH to 3. The precipitated solids were collected by filtration and washed with water. The filtered solids were dissolved in acetone and recrystallized using n-hexane as a poor solvent. The crystals were collected and this procedure was repeated twice.
[0029] Synthesis of Polymer of Example 1 (MPC:AaU=5:5) In formula (1), R1 is a methyl group, R2 is an oxygen atom, and two structural units in which n is 2 (structural units obtained by removing two hydrogen atoms from 2-methacryloyloxyethyl phosphorylcholine (MPC)), and in formula (5), R3 is a hydrogen atom, R4 is an alkylene group having 10 carbon atoms (-C 10 H 20 A polymer having structural units in which M is a sodium ion and M is a sodium ion in a molar ratio of 5:5 was synthesized by the following procedure. A three-neck flask was charged with 70% ethanol, 5.45 mmol of AaU monomer, and 5.99 mmol of sodium hydroxide. 5.45 mmol of MPC monomer was added to this solution, and 0.4 mol% of 4,4'-azobis(4-cyanovaleric acid) as a radical initiator was added. The monomer concentration was adjusted to 1M with 70% ethanol. The mixture was stirred at 70°C for 14 hours under an Ar atmosphere to polymerize. The mixture was quenched in an ice bath, and 50 ml of water at pH 9 was added. Ultrafiltration purification was performed at a pump speed of 200 to 350 rpm using a DICENE membrane pencil module HIT-HUS-0382. The polymer was recovered by freeze-drying. The number average molecular weight of the polymer, measured by the method described below, was 520,000.
[0030] Synthesis of Polymer of Example 2 (MPC:AaU=3:7) In formula (1), R1 is a methyl group, R2 is an oxygen atom, and two structural units in which n is 2 (structural units obtained by removing two hydrogen atoms from 2-methacryloyloxyethyl phosphorylcholine (MPC)), and in formula (5), R3 is a hydrogen atom, R4 is an alkylene group having 10 carbon atoms (-C 10 H 20 A polymer having structural units in which M is a sodium ion and M is a sodium ion in a molar ratio of 3:7 was synthesized by the following procedure. A three-neck flask was charged with 40% ethanol, 8.24 mmol of AaU monomer, and 8.36 mmol of sodium hydroxide. 3.53 mmol of MPC monomer was added to this solution, and 0.4 mol% of 4,4'-azobis(4-cyanovaleric acid) as a radical initiator was added. The monomer concentration was adjusted to 1M with 40% ethanol. The mixture was stirred at 70°C for 14 hours under an Ar atmosphere to polymerize. The mixture was quenched in an ice bath, and 50 ml of water at pH 9 was added. Ultrafiltration purification was performed at a pump speed of 200 to 350 rpm using a DICENE membrane pencil module HIT-HUS-0382. The polymer was recovered by freeze-drying. The number average molecular weight of the polymer, measured by the method described below, was 94,400.
[0031] Synthesis of Polymer of Example 3 (MPC:AaU=1:9) In formula (1), R1 is a methyl group, R2 is an oxygen atom, and two structural units in which n is 2 (structural units obtained by removing two hydrogen atoms from 2-methacryloyloxyethyl phosphorylcholine (MPC)), and in formula (5), R3 is a hydrogen atom, R4 is an alkylene group having 10 carbon atoms (-C 10 H 20 A polymer having structural units in which M is a sodium ion and M is a sodium ion in a molar ratio of 1:9 was synthesized by the following procedure. A three-neck flask was charged with 60% ethanol, 6.92 mmol of AaU monomer, and 6.81 mmol of sodium hydroxide. 0.78 mmol of MPC monomer was added to this solution, and 0.4 mol% of 4,4'-azobis(4-cyanovaleric acid) as a radical initiator was added. The monomer concentration was adjusted to 1M with 40% ethanol. The mixture was stirred at 70°C for 14 hours under an Ar atmosphere to polymerize. The mixture was quenched in an ice bath, and 50 ml of water at pH 9 was added. Ultrafiltration purification was performed at a pump speed of 200 to 350 rpm using a DICENE membrane pencil module HIT-HUS-0382. The polymer was recovered by freeze-drying. The number average molecular weight of the polymer, measured by the method described below, was 40,000,000.
[0032] Preparation of AA monomer Acrylic acid (hereinafter sometimes abbreviated as "AA monomer") was prepared as a compound similar to the compound of formula (10). Unlike the compound of formula (10), acrylic acid does not have an amide group or a hydrocarbon group corresponding to R4 in formula (10).
[0033] Synthesis of polymer (MPC:AA=5:5) of Comparative Example 1 70% ethanol, 5.45 mmol of AA monomer, and 5.99 mmol of sodium hydroxide were added to a three-neck flask. 5.45 mmol of MPC monomer and 0.4 mol% of 4,4'-azobis(4-cyanovaleric acid) as a radical initiator were added to this solution. The monomer concentration was adjusted to 1M with 70% ethanol. The mixture was stirred at 70°C for 14 hours under an Ar atmosphere and polymerized. The mixture was quenched in an ice bath and 50 ml of water at pH 9 was added. Ultrafiltration purification was performed at a pump speed of 200 to 350 rpm using a DICENE membrane pencil module HIT-HUS-0382. The polymer was recovered by freeze-drying. The number average molecular weight of the polymer, measured by the method described below, was 306,000.
[0034] (2) Physical property evaluation number average molecular weight The value was calculated in terms of standard polystyrene by gel permeation chromatography under the following conditions. (GPC conditions) Equipment: Shimadzu Prominence Column: Tosoh TSKgel α-M Sample concentration: 1mg / ml Mobile phase solvent: pH 8.0 phosphate buffer (mixture of Na2HPO4 and NaH2PO4 50 mM) / acetonitrile = 9 / 1 (volume ratio) Flow rate: 0.6mL / min Column temperature: 40℃
[0035] water resistance Each polymer was dissolved in a solution of sodium hydroxide aqueous solution at pH 10 / ethanol = 1:1 (volume ratio) to a concentration of 2 wt%. Each polymer solution was coated on a PET film with a bar coater #12 and dried at 100 °C for 10 minutes to prepare a PET film coated with each polymer. The PET film coated with each polymer was exposed to hydrochloric acid gas to hydrogenate the carboxyl groups. Next, the PET film coated with each polymer before and after exposure to hydrochloric acid gas was immersed in water for 24 hours. After 24 hours, the PET film coated with each polymer was taken out and dried to remove moisture. The membrane was stained with 1% by weight of rhodamine 6G, and the absorbance at 540 nm was measured using a spectrophotometer (V-670, manufactured by JASCO Corporation). Since rhodamine 6G is a dye that binds to carboxyl groups, the amount of AaU (or AA), and therefore the amount of membrane, can be quantified by staining with rhodamine 6G. The higher the absorbance, the greater the amount of remaining membrane.
[0036] Inhibits protein adsorption Each polymer was dissolved in a solution of sodium hydroxide aqueous solution at pH 10 / ethanol=1:1 (volume ratio). 50 μl of the polymer solution was added to each well of a highly protein-adsorbing microplate (Sumitomo Bakelite Co., Ltd., ELISA Plate H (MS-8596F)) and dried at 100°C for 20 minutes. This microplate was exposed to hydrochloric acid gas, and after exposure, each well was washed twice with 200 μl of phosphate buffer-physiological saline (PBS) (pH 7.2). Anti-IgG antibody labeled with horseradish peroxidase (HRP) was diluted 5000-fold with PBS (pH 7.2), and 100 μl of the diluted solution was added to wells not coated with the polymer and wells coated with the polymer, respectively, and left to stand at room temperature for 1 hour. The anti-IgG antibody solution in each well was discharged with a Pipetman (trade name), and 200 μL of PBS (pH 7.2) containing 0.05 wt% Tween 20 was added and discharged four times. TMB1-Component Microwell Peroxidase Substrate, Sure, a substrate for HRP, was added to each well. Then, 100 μl of TMB Blue (KPL) was added and the plate was left to stand at room temperature for 30 minutes. 100 μl of TMB Stop Solution (KPL) was added to each well, and the absorbance at 450 nm was measured using a plate reader. Higher absorbance indicates greater amount of bound IgG antibody. The rate of inhibition of IgG antibody adsorption by the polymer was calculated using the following formula. In the formula, the control is a well that was not coated with the polymer and was not exposed to the IgG antibody. IgG antibody adsorption inhibition rate = 1 - [(absorbance when IgG antibody is applied to polymer-coated wells - absorbance of control) / (absorbance when IgG antibody is applied to non-polymer-coated wells - absorbance of control)] x 100
[0037] The results are shown in Table 1. [Table 1] The polymer of Comparative Example 1, in which the monomer copolymerized with MPC was different from AaU of the present invention, had a decreased film amount and poor water resistance when immersed in water both before and after exposure to hydrochloric acid gas. In contrast, the polymers of Examples 1 to 3 of the present invention, which have the structural unit of AaU, had a decreased film amount when immersed in water under alkaline conditions before exposure to hydrochloric acid gas, i.e., poor water resistance, but the remaining film amount increased when exposed to hydrochloric acid gas, i.e., improved water resistance. The polymers of Examples 1 to 3 of the present invention showed improved water resistance after exposure to hydrochloric acid gas, and also showed an extremely high IgG adsorption inhibition rate of 99% or more. [Industrial Applicability]
[0038] The polymer of the present invention has excellent biocompatibility and protein adsorption inhibitory effect, and can be used for molding by dissolving in a safe polar solvent such as water or ethanol, and can have excellent water resistance after molding. Therefore, it can be suitably used as a material for medical supplies or a covering material.
Claims
1. The following formula (1) [Formula 1] a structural unit represented by the following formula (2): [chemical 2] a structural unit represented by the following formula (3): [C3] and a structural unit represented by the following formula (4): [C4] Structural unit represented by (In formulas (1) to (4), R 1 represents a hydrogen atom or a methyl group, R 2 represents an oxygen atom or -NH-, and two n's independently represent an integer of 1 to 4. At least one structural unit (a) selected from the group consisting of: The following formula (5) -CH 2 -CR 3 (CONH-R 4 -COOM)- (5) (In formula (5), R 3 represents a hydrogen atom or a methyl group, R 4 represents a linear or branched, saturated or unsaturated divalent hydrocarbon group having 5 to 16 carbon atoms, and M represents a hydrogen atom or a counter cation. The compound contains a structural unit (b) represented by the ratio of the amount of the structural unit (b) to the total amount of the structural unit (a) and the structural unit (b) is 10 to 98 mol %, A polymer having a number average molecular weight of 5,000 or more.
2. The polymer according to claim 1, wherein a counter cation of M in formula (5) is an alkali metal ion, an ammonium ion, or an organic cation.
3. R in formula (5) 4 3. The polymer according to claim 1, wherein is a linear, saturated, divalent hydrocarbon group having 8 to 12 carbon atoms.
4. 3. The polymer according to claim 1, wherein the total amount of the structural units (a) and (b) is 40 mol % or more based on the total amount of the structural units constituting the polymer.
5. The polymer according to claim 1 or 2, which is used for suppressing protein adsorption.
6. A film, coating, fiber, or bulk molded article comprising the polymer of claim 1 or 2.
7. The following formula (6) [C5] a compound represented by the following formula (7): [C6] a compound represented by the following formula (8): [C7] [C8] (In formulas (6) to (9), R 1 represents a hydrogen atom or a methyl group, R 2 represents an oxygen atom or -NH-, and two n's independently represent an integer of 1 to 4. and at least one compound having a betaine structure selected from the group consisting of compounds represented by the following formula (10): CH 2 =CR 3 (CONH-R 4 -COOM) (10) (In formula (10), R 3 represents a hydrogen atom or a methyl group, R 4 represents a linear or branched, saturated or unsaturated divalent hydrocarbon group having 5 to 16 carbon atoms, and M represents a hydrogen atom or a counter cation. using a monomer containing a compound represented by the formula: embedded image so that the ratio of the amount of the compound of formula (10) to the total amount of the compound having a betaine structure and the compound of formula (10) is 10 to 98 mol %.
8. A method for producing an article, comprising a step of molding the polymer according to claim 1 or 2 in a state where the polymer is dissolved in a polar solvent under alkaline conditions.
9. A method for improving the water resistance of an article made by the method of claim 8 by subjecting said article to acidic conditions.