Steel wire

A high-strength steel wire with controlled elemental composition and DSC peaks addresses the need for improved tensile strength and twisting properties, reducing delamination and enhancing tire performance.

JP2024143709AActive Publication Date: 2024-10-11KOBE STEEL LTD
View PDF 10 Cites 0 Cited by

Patent Information

Application Number
JP2023056506
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Filing Date
2023-03-30
Publication Date
2024-10-11
Estimated Expiration
2043-03-30

AI Technical Summary

Technical Problem

There is a need for high-strength steel wires with improved tensile strength and twisting properties to enhance fuel efficiency in automobiles while minimizing delamination during stranding, which existing technologies have not adequately addressed.

Method used

A steel wire composition with specific elemental percentages (C, Si, Mn, P, S, Cr, N, and optionally Cu, Ni) and controlled differential scanning calorimetry peaks (A and B) to achieve a tensile strength of 4100 MPa or more, with a ratio of A to B exceeding 1.00, enhancing ductility and reducing delamination.

Benefits of technology

The steel wire exhibits excellent tensile strength and twisting properties, effectively suppressing delamination during stranding, thereby improving tire performance and fuel efficiency.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024143709000001_ABST
    Figure 2024143709000001_ABST
Patent Text Reader

Abstract

To provide a steel wire which is suitable for a steel cord and has excellent tensile strength and twisting properties, and enables suppression of occurrence of delamination when the wire is twisted.SOLUTION: A steel wire has a predetermined composition, and DSC curve which is obtained by differential scanning calorimetry and has a first peak having the maximum value falling within the range of 100°C to 200°C and a second peak having the maximum value falling within the range of 300°C the 400°C, and satisfies the following formulas (1) and (2), wherein a diameter is 0.25 mm or more and 0.35 mm or less, and tensile strength is 4100 MPa or more. A≥1.50(J / g)...formula (1) B / A≥1.00...formula (2). Herein, A(J / g) denotes a heat generation amount of the sum total of the first peak, and B(J / g) denotes a heat generation amount of the sum total of the second peak.SELECTED DRAWING: Figure 1
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present disclosure relates to a high-strength steel wire having excellent torsional properties, and in particular to a steel wire suitable for steel cords used as reinforcing materials for automobile tires and the like. [Background technology]

[0002] There has been a demand for improved safety for occupants in vehicles, and for this purpose, the strength of the vehicle body has been improved. On the other hand, against the background of the worsening of the global warming problem, the movement to improve the fuel efficiency of automobiles is accelerating. It is known that reducing the weight of the vehicle body is effective in improving fuel efficiency.

[0003] In order to improve fuel efficiency of automobiles, there is a demand for higher strength steel wire for steel cords. Increasing the strength of steel wires allows the weight of steel wire used per tire to be reduced, which leads to lighter tires and improved fuel efficiency of automobiles. However, as the strength of the steel wire increases, the steel wire becomes brittle, and the risk of delamination occurring during twisting increases. Since delamination leads to a decrease in the strength of the tire cord, there is a demand for both strength and delamination resistance (twisting characteristics). Various methods have been proposed to improve both strength and twisting characteristics (for example, Patent Documents 1 to 3).

[0004] Patent Document 1 discloses a high-strength steel wire having excellent strength and ductility. The high-strength steel wire has a predetermined chemical composition, a wire diameter of 0.05 to 0.30 mm, and a DSC curve of differential scanning calorimetry showing multiple heat generation peaks in the temperature range of 100 to 450°C, and the total heat generation amount H in the temperature range of 100 to 450°C is 0.05 to 0.30 mm. 100~450 and the heat generation amount H in the temperature range of 280 to 420°C 280~420 satisfies the following formula (3). H 280~420 / H 100~450 <0.45···(3)

[0005] Patent Document 2 discloses an extra-fine high-carbon steel wire that has high strength and excellent ductility and does not undergo delamination during high-speed twisting. The extra-fine high-carbon steel wire is an extra-fine steel wire having a predetermined chemical composition and a wire diameter of 0.05 to 0.50 mm, and a differential scanning calorimetry curve A of this steel wire has an exothermic peak X in the temperature range of 60°C to 130°C, and the maximum height h of the exothermic peak with respect to a reference line Y connecting two points of 60°C and 130°C on the differential scanning calorimetry curve is 5 μW / mg or more.

[0006] Patent Document 3 discloses a method for producing a high-strength extra-fine steel wire that is both high-strength and has an excellent balance of strength and ductility. The method for producing the high-strength extra-fine steel wire involves patenting a steel material having a prescribed chemical composition, and then performing wire drawing including a skin pass process as a final finish to produce a high-strength extra-fine steel wire made of a fine pearlite structure with a tensile strength of 4000 MPa or more, and then performing aging treatment at an aging temperature T of 130 to 300°C for an aging time t such that the diffusion length L of carbon atoms falls within the range of 400 to 2000 nm. [Prior art documents] [Patent documents]

[0007] [Patent Document 1] JP 2019-056162 A [Patent Document 2] JP 2005-126765 A [Patent Document 3] JP 2008-208450 A Summary of the Invention [Problem to be solved by the invention]

[0008] In order to further improve the fuel efficiency of automobiles, there is a demand for further improvements in the strength (particularly tensile strength) and torsional properties of steel wires for steel cords. Therefore, an object of the present disclosure is to provide a steel wire that is suitable for a steel cord, has excellent tensile strength and torsional characteristics, and can suppress the occurrence of delamination during twisting. [Means for solving the problem]

[0009] Aspect 1 of the present invention is C: 0.95% by mass or more, 1.05% by mass or less, Si: 0.15% by mass or more, 0.40% by mass or less, Mn: 0.10 mass% or more, 0.50 mass% or less, P: more than 0 mass%, 0.030 mass% or less, S: more than 0% by mass, 0.030% by mass or less, Cr: 0.10 mass% or more and 0.30 mass% or less, and N: Contains 0.0010% by mass or more and 0.0080% by mass or less, The balance is iron and unavoidable impurities, The DSC curve obtained by differential scanning calorimetry has a first peak having a maximum value in the range of 100°C to 200°C and a second peak having a maximum value in the range of 300°C to 400°C, and satisfies the following formulas (1) and (2): The diameter is 0.25 mm or more and 0.35 mm or less, The steel wire has a tensile strength of 4100 MPa or more. A≧1.50(J / g)...Formula (1) B / A≧1.00...Equation (2) where A (J / g) is the sum of the heat values ​​of the first peaks, B (J / g) is the total heat value of the second peak.

[0010] Aspect 2 of the present invention is Cu: more than 0.01 mass% and 0.25 mass% or less, and The steel wire according to aspect 1, further comprising one or more selected from the group consisting of Ni: more than 0.01 mass % and 0.25 mass % or less. Effect of the Invention

[0011] According to the present disclosure, it is possible to provide a steel wire that is excellent in tensile strength and torsional characteristics and can suppress the occurrence of delamination during stranding. [Brief description of the drawings]

[0012] [Figure 1] 1 shows an example of a DSC curve of a steel wire according to an embodiment. [Diagram 2] The data for the examples and comparative examples are plotted with the horizontal axis representing the sum of the heat values ​​of the first peaks A (J / g) and the vertical axis representing the sum of the heat values ​​of the second peaks relative to A (B (J / g)). DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0013] When differential scanning calorimetry (DSC) is performed on the steel wire obtained after finish drawing, two major peaks are observed in the curve (Figure 1) with the horizontal axis representing temperature and the vertical axis representing heat quantity.

[0014] The first peak (first peak) 10 has a maximum value in the range of 100°C to 200°C, and the second peak (second peak) 20 has a maximum value in the range of 300°C to 400°C. Generally, the first peak 10 is said to be a peak caused by heat generation accompanying the fixation (age hardening) of dislocations (including mobile dislocations and immobile dislocations) introduced by finish drawing by C atoms dissolved in the ferrite phase in the pearlite structure of the steel wire. The area S of the first peak 10 10 A large heat generation rate (i.e., the sum of heat generated by age hardening when heating) means that age hardening due to processing heat during finish drawing is suppressed, and therefore indicates high ductility of the steel wire. Moreover, it is generally believed that the second peak 20 is caused by heat generated when carbon atoms that had pinned the dislocations are reprecipitated as cementite.

[0015] As a result of intensive research by the present inventors, it has been found that the area S of the first peak 10 can be reduced by optimizing the drawing conditions of the finish drawing. 10 Not only the area S of the second peak 20 20 and the area S of the first peak 10 10 The area S of the second peak 20 20 It was found that when the ratio reaches a certain level or more, the delamination during twisting decreases.

[0016] Area S of the second peak 20 20 The reason for the increase in area ratio (S 20 / S 10 The reason why delamination is reduced by controlling the thickness of the sheet to a predetermined value or more is not clear, but is presumed to be as follows.

[0017] The second peak 20 is related to the heat generated when cementite is re-precipitated and when mobile dislocations in the steel wire disappear with increasing temperature. The more mobile dislocations that disappear, the larger the area S of the second peak 20. 20 In addition, mobile dislocations are less entangled with each other than immobile dislocations, so they move and disappear more easily when the temperature is raised. Area S of the second peak 20 20 A large value of α indicates that there are many mobile dislocations that disappear in the temperature range corresponding to the second peak, in other words, there are many mobile dislocations introduced during wire drawing. A steel wire with many mobile dislocations in it, especially on its surface, is thought to have high ductility and to be able to suppress delamination during twisting.

[0018] On the other hand, if there are few mobile dislocations in the steel wire, the number of mobile dislocations that disappear due to temperature rise is reduced, so the area S of the second peak 20 20 Furthermore, if the number of mobile dislocations in the steel wire is small, the number of mobile dislocations on the surface of the steel wire is also small, so the ductility of the steel wire is low and it is believed that delamination occurs when twisting a high-strength steel wire.

[0019] Based on these findings, the present invention has been completed. Hereinafter, details of the steel wire and the manufacturing method thereof according to the embodiment of the present invention will be described.

[0020] <1.Chemical composition> The steel wire according to an embodiment of the present invention contains C: 0.95% by mass or more and 1.05% by mass or less, Si: 0.15% by mass or more and 0.40% by mass or less, Mn: 0.10% by mass or more and 0.50% by mass or less, P: more than 0% by mass and 0.030% by mass or less, S: more than 0% by mass and 0.030% by mass or less, Cr: 0.10% by mass or more and 0.30% by mass or less, and N: 0.0010% by mass or more and 0.0080% by mass or less. Each element will be described in detail below.

[0021] [C: 0.95% by mass or more, 1.05% by mass or less] C affects the cementite ratio and lamellar spacing in pearlite, improving tensile strength. Therefore, if the C content is low, the strength of the steel wire is insufficient. On the other hand, if the C content is excessive, cementite precipitates along the prior austenite grain boundaries during the hot rolling manufacturing process and patenting treatment, which not only inhibits strength improvement but also reduces wiredrawability and causes longitudinal cracks during twisting. From these viewpoints, the C content is set to 0.95 mass % or more and 1.05 mass % or less, preferably 0.97 mass % or more and 1.03 mass % or less, and more preferably 0.98 mass % or more and 1.02 mass % or less.

[0022] [Si: 0.15 mass% or more, 0.40 mass% or less] Silicon dissolves in the ferrite in the lamellar structure to improve strength, and also inhibits the precipitation of cementite at grain boundaries to improve ductility. However, the addition of large amounts of silicon embrittles the ferrite and reduces wire drawability. From these viewpoints, the Si content is set to 0.15 mass % or more and 0.40 mass % or less, preferably 0.17 mass % or more and 0.35 mass % or less, and more preferably 0.18 mass % or more and 0.30 mass % or less.

[0023] [Mn: 0.10 mass% or more, 0.50 mass% or less] Mn combines with S to form MnS, which helps to suppress hot cracking. However, adding a large amount of Mn increases hardenability and makes it easier for supercooled structures to form after hot rolling and patenting, which reduces wire drawability. From these viewpoints, the Mn content is set to 0.10 mass % or more and 0.50 mass % or less, preferably 0.20 mass % or more and 0.40 mass % or less, and more preferably 0.25 mass % or more and 0.35 mass % or less.

[0024] [P: more than 0 mass%, 0.030 mass% or less] P is an inevitable impurity that segregates at prior austenite grain boundaries and adversely affects wiredrawability. From this perspective, the P content is preferably as low as possible, and in the embodiment of the present invention, the P content is set to 0.030 mass% or less. The lower the P content, the better, but excessive reduction leads to reduced manufacturability and increased manufacturing costs. Therefore, the P content is greater than 0 mass% and equal to or less than 0.030 mass%, preferably equal to or more than 0.001 mass% and equal to or less than 0.020 mass%, and more preferably equal to or more than 0.002 mass% and equal to or less than 0.010 mass%.

[0025] [S: more than 0 mass%, 0.030 mass% or less] S is an inevitable impurity, and when used alone, it produces FeS, which causes hot cracking. Although it is rendered harmless as MnS by adding Mn, it is better to have as little S as possible, and in the embodiment of the present invention, the S content is set to 0.030 mass% or less. The lower the S content, the better, but excessive reduction leads to reduced manufacturability and increased manufacturing costs. Therefore, the S content is set to more than 0 mass% and 0.030 mass% or less, preferably 0.001 mass% or more and 0.020 mass% or less, and more preferably 0.002 mass% or more and 0.010 mass% or less.

[0026] [Cr: 0.10 mass% or more, 0.30 mass% or less] Cr refines pearlite lamellae and improves the tensile strength of steel wires. However, the addition of a large amount of Cr increases hardenability and makes it easier for supercooled structures to form after hot rolling or patenting treatment, which reduces wiredrawability. From these viewpoints, the Cr content is set to 0.10 mass % or more and 0.30 mass % or less, preferably 0.15 mass % or more and 0.28 mass % or less, and more preferably 0.18 mass % or more and 0.25 mass % or less.

[0027] [N: 0.0010 mass% or more, 0.0080 mass% or less] N not only generates nitride inclusions, but also causes strain aging, which reduces wiredrawability and promotes delamination. From this perspective, the N content is preferably as low as possible, and in the embodiment of the present invention, the N content is set to 0.0080 mass% or less. The lower the N content, the better, but excessive reduction also leads to reduced manufacturability. Therefore, the N amount is set to 0.0010 mass % or more and 0.0080 mass % or less, preferably 0.0015 mass % or more and 0.0060 mass % or less, and more preferably 0.0020 mass % or more and 0.0050 mass % or less.

[0028] The basic components are as described above, and in one preferred embodiment, the balance is iron and inevitable impurities. Examples of inevitable impurities include elements that are introduced due to the circumstances of raw materials, materials, manufacturing facilities, etc. In addition, for example, P and S, which are usually preferable as their content is small, are unavoidable impurities, but their composition ranges are separately specified as above. Therefore, in this specification, when referring to "unavoidable impurities" that make up the balance, this concept excludes elements whose composition ranges are separately specified.

[0029] (Other optional elements) Furthermore, in another preferred embodiment of the present invention, elements other than those described above may be contained as necessary within a range that does not impair the effects according to the embodiment of the present invention. The properties of the steel wire are further improved depending on the components contained.

[0030] Examples of such selected elements include one or more selected from the group consisting of Cu: more than 0.01 mass % and 0.25 mass % or less, and Ni: more than 0.01 mass % and 0.25 mass % or less. The details of the contents of the selective elements Cu and Ni are shown below.

[0031] [Cu: more than 0.01 mass%, 0.25 mass% or less] Cu may be added because it improves corrosion resistance, but it also reduces descaling properties during pickling. From these viewpoints, the Cu amount is preferably more than 0.01 mass% and 0.25 mass% or less, more preferably 0.03 mass% or more and 0.20 mass% or less, and particularly preferably 0.05 mass% or more and 0.10 mass% or less. Even if Cu is not intentionally added, it may be contained in an amount of about 0.01 mass % as an unavoidable impurity.

[0032] [Ni: more than 0.01 mass%, 0.25 mass% or less] Ni may be added since it is an element that improves corrosion resistance, but Ni also increases hardenability and makes it easier to generate a supercooled structure after patenting. From these viewpoints, the Ni amount is preferably more than 0.01 mass% and 0.25 mass% or less, more preferably 0.03 mass% or more and 0.20 mass% or less, and particularly preferably 0.05 mass% or more and 0.10 mass% or less. Even if Ni is not intentionally added, it may be contained at about 0.01 mass % as an unavoidable impurity.

[0033] <2.Physical properties> [Differential Scanning Calorimetry (DSC)] The steel wire according to the embodiment of the present invention exhibits the following characteristics when subjected to Differential Scanning Calorimetry (DSC). In a DSC curve obtained by differential scanning calorimetry, there is a first peak 10 having a maximum value in the range of 100°C to 200°C, and a second peak 20 having a maximum value in the range of 300°C to 400°C. If the sum of the calorific values ​​of the first peaks 10 is A (J / g) and the sum of the calorific values ​​of the second peaks 20 is B (J / g), the following formulas (1) and (2) are satisfied. A≧1.50(J / g)...Formula (1) B / A≧1.00...Equation (2)

[0034] There is one or more peaks (first peaks) 10 that show a maximum value in the range of 100° C. to 200° C. When there is one first peak 10, the area S 10 From the above, the sum A (J / g) of the heat values ​​of the first peaks 10 can be calculated. When there are multiple first peaks 10, the area S of the multiple first peaks 10 can be calculated. 10 From the sum of these, the total calorific value A (J / g) of the first peak 10 can be calculated. Similarly, there is one or more peaks (second peaks) 20 that show a maximum value in the range of 300° C. to 400° C. When there is one second peak 20, the area S 20 From the above, the sum B (J / g) of the heat values ​​of the second peaks 20 can be calculated. When there are multiple second peaks 20, the area S of the multiple second peaks 20 can be calculated. 20 From the sum of these, the total calorific value B (J / g) of the second peak 20 can be calculated.

[0035] Differential scanning calorimetry (DSC) is performed as follows. 20 mg of a steel wire sample is placed in a measurement chamber and heated in the range of 0 to 500°C. The temperature is increased in an argon atmosphere at a rate of 15°C / min to obtain a DSC curve. The measurement device may be, for example, an X-DSC7000 manufactured by Hitachi High-Tech Science Corporation. For each peak observed in the obtained DSC curve, a tangent line common to the two valleys located on both sides of the peak is drawn to form a reference line. In FIG. 1, the reference line RL of the first peak 10 is 10and the reference line RL of the second peak 20 20 The area of ​​the region enclosed by the DSC curve and the reference line (area S 10 , S 20 ) to calculate the "heat generation amount (J / g)".

[0036] In addition, when there are multiple first peaks 10 and multiple second peaks 20, if the multiple peaks can be separated, the area is calculated for each peak. If two or more of the multiple first peaks 10 overlap each other and it is difficult to separate them into individual peaks, the two or more overlapping peaks are treated as "one first peak 10" and the area S is calculated. 10 Similarly, if two or more of the multiple second peaks 20 overlap each other and it is difficult to separate them into individual peaks, the two or more overlapping peaks are treated as "one second peak 20" and the area S is calculated. 20 Request.

[0037] Equations (1) and (2) will now be explained.

[0038] [A≧1.50(J / g)...Equation (1)] In the DSC curve, the area S of the first peak 10 10 The larger the area S of the first peak 10, the more the age hardening (age embrittlement) during finish drawing is suppressed. 10 When the sum A (J / g) of the calorific values ​​of the first peaks 10 calculated from is 1.50 J / g or more (that is, when formula (1) is satisfied), delamination can be effectively suppressed. A is preferably 1.60 J / g or more, more preferably 1.70 J / g or more, and even more preferably 1.90 J / g or more.

[0039] [B / A≧1.00...Equation (2)] In the DSC curve, the area S of the second peak 20 20 It is considered that the area S of the second peak 20 represents not only the reprecipitation of cementite but also the amount of mobile dislocations in the steel wire surface layer. If the amount of mobile dislocations that are annihilated is large, it can be said that many mobile dislocations existed before the annihilation, and a steel wire containing many mobile dislocations has low delamination during twisting.20 When the sum B (J / g) of the heat generation amounts of the second peaks 20 calculated from is equal to or greater than the sum A (J / g) of the heat generation amounts of the first peaks 10, that is, when B / A is 1.00 or greater (i.e., when formula (2) is satisfied), the delamination suppression effect is large. B / A is preferably 1.20 or more, and more preferably 1.40 or more.

[0040] In addition, a steel wire that satisfies only one of formulas (1) and (2) does not have a sufficient effect of suppressing delamination, so the embodiment of the present invention targets only steel wires that satisfy both formulas (1) and (2).

[0041] Tensile strength (TS) The steel wire according to this embodiment has high tensile strength suitable for a steel cord. The specific tensile strength of the steel wire is 4100 MPa or more. The tensile strength is measured in accordance with JIS Z 2241:2022. Three test samples are taken from the steel wire and the tensile test is carried out three times. The chuck distance is 100 mm and the test speed is 20 mm / sec. If the wire breaks at the chuck, the measurement is invalid and the test is carried out again. The average of the measured breaking strength values ​​is the tensile strength (MPa) of the steel wire.

[0042] <3. Diameter of steel wire> If the diameter of the steel wire is small, when it is used as a steel cord, it is necessary to increase the number of twisted wires or the number of twisted wires woven into the rubber in order to ensure the strength of the tire, which results in a decrease in tire productivity and an increase in costs.On the other hand, if the diameter of the steel wire is large, the initial wire diameter becomes large accordingly, and wire drawability decreases. The diameter of the steel wire is 0.25 mm to 0.35 mm, preferably 0.27 mm to 0.33 mm, and more preferably 0.28 mm to 0.32 mm, which can improve tire productivity and suppress an increase in tire costs, and can also suppress a decrease in wire drawability.

[0043] A micrometer is used to measure the diameter. The diameter of a steel wire is measured at three different points along its length, and the average value is taken as the diameter of the steel wire.

[0044] <4. Manufacturing method> Next, a method for producing a steel wire according to an embodiment of the present invention will be described.

[0045] The hot-rolled wire rod used in the manufacture of the steel wire can be manufactured by a conventional method. An example of the method for manufacturing the hot-rolled wire rod will be described below. A steel billet (for example, a 155 mm square billet) produced by continuous casting and blooming is heated and held at 900°C to 1200°C for 30 to 240 minutes. Rough rolling and finish rolling are carried out to obtain wire rods with diameters of 4.0 mm to 6.0 mm. The coiling temperature after rolling is 850°C to 1000°C. After coiling, the wire is cooled to 650°C at a rate of 20 to 50°C / sec, held at 650°C to 550°C for 5 to 30 seconds, and then cooled to 400°C or lower at a rate of 5 to 15°C / sec.

[0046] The hot-rolled wire rod thus obtained is subjected to intermediate drawing and patenting treatment.

[0047] The conditions for intermediate wire drawing are to remove the rolling scale and to perform a coating treatment by a chemical method using acid or mechanical descaling. After that, dry wire drawing is performed to a diameter of 1.7 to 2.3 mm with a single area reduction rate of 17 to 23%. If it is not possible to process the wire to the specified wire diameter in one dry wire drawing, dry wire drawing may be performed again. Also, if the intermediate wire becomes embrittled midway and cannot be drawn, it may be softened by patenting treatment and then dry wire drawing may be performed again.

[0048] The conditions for the patenting treatment are, for example, heating at 900 to 1000°C for 30 seconds to 5 minutes to austenitize the inside of the wire, and then immersing it in a refrigerant at 500°C to 600°C in a molten lead fluidized bath for 5 to 30 seconds to cause pearlite transformation.

[0049] The intermediate wire drawing and patenting treatment may be repeated two or more times, but since the more repeated times, the lower the yield of the steel wire and the higher the manufacturing cost, it is preferable to repeat the process at most two times.

[0050] For the wire rod (intermediate wire rod) after the patenting treatment, it is sufficient if the pearlite fraction at the center of the cross section perpendicular to the longitudinal direction of the steel wire is equal to or greater than the pearlite fraction obtained by a normal patenting treatment, for example, 80%. However, the strength and torsional properties can be further improved by further increasing the pearlite fraction.

[0051] The pearlite fraction is measured, for example, by observing a cross section perpendicular to the longitudinal direction of the steel wire with a scanning electron microscope (SEM). In the SEM image (structure photograph), 10 parallel lines are drawn vertically at intervals of 2.0 μm, and 10 parallel lines are drawn horizontally (perpendicular to the vertical direction) at intervals of 1.5 μm. Of the lattice points (100 points) of the vertical and horizontal lines, the number of lattice points (corresponding to the pearlite fraction) located on the pearlite structure is counted.

[0052] The patented wire (intermediate wire) is then brass plated and then finish drawn to obtain a steel wire having a diameter of 0.25 to 0.35 mm. The finish drawing is preferably performed by wet drawing. Finish wire drawing is a continuous wire drawing process using dies arranged in multiple stages. The area reduction rate per pass of finish wire drawing is 10% to 18%, and the final wire speed is 50 to 1000 m / min. However, as described later, the area reduction rates of the final three passes and the optional final fourth pass (skin pass) may be outside the range of 10% to 18%. The bearing length of the die is, for example, 1 / 4 to 1 / 2 of the die diameter.

[0053] In the embodiment of the present invention, it is important to control the reduction in area in the last three passes of the finish wire drawing (referred to as the "final three passes"). The sum of the area reduction rates of the final three passes (referred to as the "total area reduction rate") is controlled to 12.0% to 18.0%. The "total area reduction rate" is the area reduction rate calculated from the diameter of the wire rod just before the final three passes and the diameter of the steel wire rod after the final three passes. The area reduction rate of each of the final three passes is controlled as follows: In this specification, the "final first pass" refers to the final pass, the "final second pass" refers to the pass immediately before the "final first pass," and the "final third pass" refers to the pass immediately before the "final second pass." Final 3rd pass: 5.0%~14.0% Final 2nd pass: 2.0%~9.9% Final pass: 2.0%~4.9%

[0054] By appropriately controlling the total area reduction rate and each area reduction rate for the final three passes, it is possible to obtain a steel wire in which the sum A (J / g) of the heat amounts of the first peaks 10 and the sum B (J / g) of the heat amounts of the second peaks 20 in the DSC curve satisfy the above-mentioned formulas (1) and (2).

[0055] Finish drawing is often performed by a slip-type wire drawing machine. In a slip-type wire drawing machine, the area reduction rate per pass is limited except for the final pass, so it may be difficult to achieve the low area reduction rate set for the final three passes as described above. The die holder may be processed so that three dies for performing the final three passes of this embodiment can be fixed instead of the conventional one die for the final pass.

[0056] Furthermore, a skin pass wire drawing with an area reduction rate of 2.0% to 4.9% may be added as the pass immediately before the final third pass (final fourth pass).

[0057] A person skilled in the art who has come into contact with the manufacturing method of the steel wire according to the embodiment of the present invention described above may be able to obtain the steel wire according to the present invention by a manufacturing method different from the above-mentioned manufacturing method through trial and error. EXAMPLES

[0058] The present invention will be described in more detail below with reference to examples. The present invention is not limited to the following examples, and may be modified as appropriate within the scope of the above and below-described aims, and all such modifications are within the technical scope of the present invention.

[0059] Steels having the chemical composition shown in Table 1 were melted in a converter, and then subjected to continuous casting, blooming, and finish rolling to produce hot-rolled wire rods with a diameter of 5.5 mm. The hot-rolled wire rods obtained were descaled and coated in the usual manner, and processed into wire rods with a diameter of 2.0 mm by intermediate drawing. The reduction in area per pass of the intermediate drawing was set to 20% or less.

[0060] The wire rod after intermediate drawing was heated at a heating temperature of 950°C for 1 minute to be austenitized, and then immersed in a fluidized bath maintained at 540°C for patenting treatment. The pearlite fraction in the center of the wire rod after patenting treatment was determined by the following method.

[0061] The wire after the patenting process was cut in a cross section perpendicular to the longitudinal direction, filled with resin, and then polished to a mirror finish. After polishing and etching with picral, the wire was observed with a scanning electron microscope (SEM) at a magnification of 4000 times from the center of the cross section (corresponding to the D / 2 position) to the D / 4 position, where D is the diameter of the steel wire (field of view dimensions: 24 μm × 18 μm). First, a first SEM observation was performed at an arbitrary D / 4 position. From that position, the wire was rotated 90° to the right with the center of the cross section (D / 2 position) as the rotation center, and a second SEM observation was performed at a D / 4 position different from the original measurement position (D / 4 position). This operation was repeated two more times, and SEM observation was performed once each at four different D / 4 positions (a total of four times). On each SEM image (structure photograph), 10 parallel lines were drawn vertically at intervals of 2.0 μm, and 10 parallel lines were drawn horizontally (perpendicular to the vertical direction) at intervals of 1.5 μm. Of the 100 grid points of the vertical and horizontal lines, the number of grid points (corresponding to the pearlite fraction) located on the pearlite structure was counted. The arithmetic average of the pearlite fractions obtained from each SEM image was calculated, and this was regarded as the pearlite fraction of the wire. In the wire rod after the patenting treatment of the example, the pearlite fraction was 94%.

[0062] The wire rod after the patenting process was brass plated in the usual way and then subjected to finish drawing (wet wire drawing). In the finish drawing, 23 passes of wire drawing were performed. From the 1st pass to the 19th pass, the area reduction rate of each pass was 14.5% to 17.5%. The area reduction rates of the final 3rd pass and the final 4th pass were as shown in Table 2. In addition, in Nos. 3, 6, and 7, a "skin pass drawing" with an area reduction rate of 2.0% to 4.9% was added as the final fourth pass. On the other hand, in Nos. 1, 2, 4, and 5, skin pass drawing was not added as the final fourth pass, so the area reduction rate of the final fourth pass listed in Table 2 was within the range of 10% to 18% (normal wire drawing pass).

[0063] The obtained steel wire was subjected to diameter measurement, differential scanning calorimetry, a tensile test, and a torsion test. The wire after patenting was also subjected to a tensile test. Various measurement and test methods will be described later. The measurement results are shown in Tables 2 and 3. In Tables 2 and 3, underlined values ​​indicate values ​​that are outside the range of the embodiment of the present invention.

[0064] [Table 1]

[0065] [Table 2]

[0066] [Table 3]

[0067] [1. Diameter measurement] The diameters of the wire rod after intermediate drawing and the steel wire obtained after finish drawing were measured as follows. A micrometer was used to measure the diameter. For the wire, the diameter was measured at three different points in the longitudinal direction, and the arithmetic average value was used as the diameter of the wire. Similarly, for the steel wire, the diameter was measured at three different points in the longitudinal direction, and the arithmetic average value was used as the diameter of the steel wire.

[0068] [2. Differential Scanning Calorimetry (DSC)] Differential scanning calorimetry (DSC) was carried out as follows. 20 mg of a steel wire sample was placed in a measurement chamber and heated in the range of 0 to 500°C. The temperature was increased at a rate of 15°C / min in an argon atmosphere to obtain a DSC curve. The measurement device used was an X-DSC7000 manufactured by Hitachi High-Tech Science Corporation. For each peak observed in the obtained DSC curve, a tangent line common to two valleys located on both sides of the peak was drawn to form a reference line. The area of ​​the region surrounded by the DSC curve and the reference line was calculated. The area S of the first peak 10 that shows a maximum value in the range of 100°C to 200°C 10 From this, the sum A (J / g) of the heat values ​​of the first peaks 10 was calculated. In addition, the area S of the second peak 20, which has a maximum value in the range of 300°C to 400°C, 20 From this, the sum of the heat values ​​of the second peaks 20, B (J / g), was calculated.

[0069] [3. Measurement of tensile strength (TS) (tensile test)] The tensile strength was measured in accordance with JIS Z 2241:2022. Three measurement samples with a length of approximately "chuck distance + 80 mm" (i.e., 180 to 280 mm) were taken from the wire rod after patenting and the steel wire after finish drawing, and tensile tests were performed three times. The chuck distance was 200 mm for the wire rod after patenting and 100 mm for the steel wire. The test speed was 20 mm / sec. If the specimen broke at the chuck, the measurement was invalid and a retest was performed. The arithmetic mean value of the measured breaking strength values ​​was taken as the tensile strength TS (MPa) of the steel wire.

[0070] [4. Evaluation of twisting characteristics] The torsional properties (delamination occurrence rate) of the steel wires after finish drawing were measured. Three or more test specimens with a length of 120 mm were taken from the steel wire, and a twisting test was performed until breakage, with the chuck distance set to 100 mm and the twisting speed set to 52 rpm. The fracture surface after breakage was observed with the naked eye to confirm the presence or absence of delamination. If the fracture surface was not a smooth surface perpendicular to the longitudinal direction of the steel wire, but was a crack along the longitudinal direction, it was determined that delamination had occurred. Since the wire was twisted, the torn surface was in a wavy state. The percentage (n / N) of the number of specimens with delamination to the total number of specimens tested N was used as the "delamination occurrence rate (%)". A delamination occurrence rate of 50% or less was considered to be acceptable.

[0071] Consider the results in Tables 2 and 3. In Nos. 1 to 3, in which the area reduction rate in the final three passes did not satisfy the numerical value specified in the embodiment of the present invention, the value of B / A did not satisfy formula (2). In No. 1, the value of A also did not satisfy formula (1). As a result, the delamination occurrence rate exceeded 50%. In Nos. 4 to 7, in which the area reduction rate in the final three passes satisfied the numerical value specified in the embodiment of the present invention, the value of A satisfied the formula (1) and the value of B / A satisfied the formula (2), and as a result, the delamination occurrence rate was 50% or less.

[0072] In Fig. 2, Nos. 1 to 6 are plotted on a graph with the horizontal axis being the sum A (J / g) of the calorific values ​​of the first peaks and the vertical axis being the sum B (J / g) of the calorific values ​​of the second peaks versus A. Nos. 4 to 7, which are working examples, are plotted within the range where A is 0.5 (J / g) or more and B / A is 1.00 or more. On the other hand, Nos. 1 to 3, which are comparative examples, are plotted outside the range where A is 0.5 (J / g) or more and B / A is 1.00 or more, because A is less than 0.5 (J / g) or B / A is less than 1.00. From FIG. 1 and the results of the delamination occurrence rate, it was found that samples plotted in the range where A is 0.5 (J / g) or more and B / A is 1.00 or more have a low delamination occurrence rate.

Claims

1. C: 0.95% by mass or more, 1.05% by mass or less, Si: 0.15% by mass or more, 0.40% by mass or less, Mn: 0.10% by mass or more, 0.50% by mass or less, P: more than 0 mass%, 0.030 mass% or less, S: more than 0 mass%, 0.030 mass% or less, Cr: 0.10% by mass or more and 0.30% by mass or less, and N: 0.0010% by mass or more and 0.0080% by mass or less; The balance is iron and unavoidable impurities, The DSC curve obtained by differential scanning calorimetry has a first peak having a maximum value in the range of 100°C to 200°C and a second peak having a maximum value in the range of 300°C to 400°C, and satisfies the following formulas (1) and (2): The diameter is 0.25 mm or more and 0.35 mm or less, A steel wire having a tensile strength of 4100 MPa or more. A≧1.50 (J / g)...Formula (1) B / A≧1.00...Formula (2) where A (J / g) is the sum of the heat release amounts of the first peaks, B (J / g) is the sum of the heat values ​​of the second peaks.

2. Cu: more than 0.01% by mass and 0.25% by mass or less; and The steel wire according to claim 1, further comprising one or more selected from the group consisting of Ni: more than 0.01 mass% and 0.25 mass% or less.

Citation Information

Patent Citations

  • Manufacture of steel wire for steel cord with generation of delamination suppressed

    JP1995265936A

  • High strength extra fine steel wire excellent in fatigue property and its production

    JP1996291369A

  • High strength extra fine steel wire

    JP1999199980A

  • Steel wire and its production

    JP1999241280A

  • Wire drawing type high strength steel wire rod and its production

    JP1999269607A