Crystalline boehmite powder, crystalline boehmite slurry, and methods for producing the same

The production of crystalline boehmite powder with controlled properties addresses the issue of diffusion limitations in catalysts, enhancing the performance of FCC catalysts by improving conversion rates and wear resistance through a house of cards structure.

JP2024143769APending Publication Date: 2024-10-11JGC CATALYSTS & CHEMICALS LTD
View PDF 2 Cites 0 Cited by

Patent Information

Application Number
JP2023056636
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Filing Date
2023-03-30
Publication Date
2024-10-11

AI Technical Summary

Technical Problem

Catalyst materials often lack sufficient voids for efficient diffusion of raw materials and products during catalytic reactions, which hinders the performance of catalysts like those used in fluid catalytic cracking (FCC) processes.

Method used

The development of crystalline boehmite powder with specific properties, including a crystallite diameter of 10 to 40 nm, a CBD of 0.10 to 0.35 g/ml, and a specific surface area of 60 to 160 m²/g, is produced through a method involving the mixing of gibbsite and pseudo-boehmite with controlled pH and hydrothermal treatment, resulting in a boehmite slurry with a house of cards structure for improved diffusion.

Benefits of technology

The crystalline boehmite powder enhances the catalytic performance of FCC catalysts by facilitating better diffusion of raw materials and products, thereby improving conversion rates and wear resistance.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024143769000001
    Figure 2024143769000001
  • Figure 2024143769000002
    Figure 2024143769000002
Patent Text Reader

Abstract

To provide crystalline boehmite powder which can improve the catalytic performance (e.g., conversion of hydrocarbon oil) of an FCC catalyst when crystalline boehmite is used as a matrix component of the FCC catalyst.SOLUTION: The crystalline boehmite powder has a crystallite diameter of 10 to 40 nm calculated from the peak of the (020) plane in X-ray diffraction measurement, a specific surface area of 60 to 160 m2 / g as measured by a nitrogen adsorption method, an aspect ratio of 7 or more as determined from observation with a scanning electron microscope, and a CBD of 0.10 to 0.35 g / ml.SELECTED DRAWING: None
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a crystalline boehmite powder and a crystalline boehmite slurry, and methods for producing the same. [Background technology]

[0002] Crystalline boehmite is used, for example, as a flame retardant, adsorbent, abrasive, catalyst support, or as a raw material for gamma-alumina and alpha-alumina. Crystalline boehmite with various characteristics depending on the application has been developed, and its manufacturing method has also been developed. For example, Patent Document 1 describes 50 The document discloses a method for producing crystalline boehmite having a particle size of 7 μm or less, and the crystalline boehmite produced by this method, and states that the crystalline boehmite is effective for forming a flame-retardant plastic mixture.

[0003] Patent Document 2 discloses boehmite product particles having a low aspect ratio or a spherical shape and a method for producing the same, and describes that the boehmite product particles have excellent flame retardant properties and the like. [Prior art documents] [Patent documents]

[0004] [Patent Document 1] Special Publication No. 2018-503583 [Patent Document 2] Special Publication No. 2011-515307 Summary of the Invention [Problem to be solved by the invention]

[0005] Catalyst materials are often required to have many pores to facilitate the diffusion of raw materials and products during catalytic reactions. It is believed that crystalline boehmite also has a good property of having many pores to facilitate diffusion and improve catalytic performance.

[0006] Furthermore, when crystalline boehmite is used as a matrix component of a fluid catalytic cracking catalyst (hereinafter also referred to as an "FCC catalyst") for hydrocarbon oils, it is desired that the crystalline boehmite contributes to improving the catalytic performance.

[0007] Therefore, an object of the present invention is to provide a crystalline boehmite powder and a slurry thereof that can improve the catalytic performance (e.g., the conversion rate of hydrocarbon oil) of an FCC catalyst when the crystalline boehmite is used as a matrix component of the FCC catalyst.

[0008] Furthermore, an object of the present invention is to provide a crystalline boehmite powder and a slurry thereof having such characteristics, specifically, a crystalline boehmite powder having a small CBD (Compact Bulk Density) and a not too large crystallite diameter, and a method for producing the slurry thereof. [Means for solving the problem]

[0009] The crystalline boehmite powder of the present invention has a crystallite diameter of 10 to 40 nm calculated from the peak of the (020) plane in X-ray diffraction measurement. This powder has a CBD of 0.10 to 0.35 g / ml and a specific surface area of ​​60 to 160 m2 measured by a nitrogen adsorption method. 2 / g, and the aspect ratio determined by observation with a scanning electron microscope is 7 or more.

[0010] In order to obtain such a crystalline boehmite powder, the present inventors have found a method for producing a crystalline boehmite slurry and a method for producing a crystalline boehmite powder, which include the following first to third steps.

[0011] First, in the first step, gibbsite, pseudo-boehmite that has not been subjected to peptization treatment, and water are mixed together so that the pH value does not become 7.0 or less to prepare a mixed liquid (1). Here, gibbsite has a volume-based d 50The pseudo-boehmite has a crystallite size of 2 to 6 nm calculated from the peak of the (020) plane in an X-ray diffraction measurement, and a volume-based d 50 The gibbsite and pseudo-boehmite are mixed in a ratio of 70 to 95 parts by mass and 5 to 30 parts by mass, calculated as Al2O3 (where the total amount of gibbsite and pseudo-boehmite calculated as Al2O3 is 100 parts by mass).

[0012] Next, in the second step, an inorganic basic compound is added to the mixed solution (1) prepared in the first step to prepare a mixed solution (2) having a pH of 9.0 to 12.5. The third step is to raise the temperature of the mixture (2) at a rate of 5 to 30° C. / hour and subject it to hydrothermal treatment at 150 to 190° C. for 0.5 to 24 hours.

[0013] In the method for producing crystalline boehmite powder, the crystalline boehmite slurry produced by the above-mentioned method for producing crystalline boehmite slurry is dried to produce crystalline boehmite powder. Effect of the Invention

[0014] INDUSTRIAL APPLICABILITY The present invention makes it possible to provide crystalline boehmite having a small CBD, which is useful as a catalyst material. For example, by using the crystalline boehmite powder of the present invention or a slurry thereof as a matrix component of an FCC catalyst, the catalytic performance of the FCC catalyst, for example, the conversion rate of a hydrocarbon oil, can be improved.

[0015] Furthermore, the manufacturing method of the present invention can produce crystalline boehmite powder and a slurry thereof having such properties, specifically, crystalline boehmite powder and a slurry thereof having a small CBD and a not too large crystallite size. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0016] Hereinafter, an embodiment of the present invention will be described in detail. [Crystalline boehmite powder] The crystalline boehmite powder according to the present invention is The crystallite size calculated from the peak of the (020) plane in X-ray diffraction measurement is 10 to 40 nm; Specific surface area measured by nitrogen adsorption method is 60-160m 2 / g, The aspect ratio as determined by observation with a scanning electron microscope is 7 or more, and CBD is between 0.10 and 0.35g / ml It is a powder of crystalline boehmite.

[0017] Each physical property will be described in detail. <Crystallite diameter> The crystallite size of crystalline boehmite calculated from the peak of the (020) plane in X-ray diffraction measurement is 10 to 40 nm.

[0018] When the crystallite size is in this range, it is suitable as a catalyst material. For example, by using this crystalline boehmite powder as a matrix component, it is possible to produce an FCC catalyst with excellent catalytic performance.

[0019] On the other hand, crystalline boehmite powder having a crystallite size larger than this range is unsuitable as a catalyst material. For example, an FCC catalyst produced using this crystalline boehmite powder as a matrix component may have significantly inferior catalytic performance or wear resistance. The crystallite size is preferably 15 to 40 nm, and more preferably 20 to 35 nm. The crystallite size can be determined by the following method or an equivalent method.

[0020] <Calculation method of crystallite size> First, prepare crystalline boehmite as a measurement sample. When the crystalline boehmite is in the form of a slurry, for example, the slurry is dried at 130° C. for 12 hours, and the residue is ground in a mortar to obtain a crystalline boehmite powder.

[0021] Next, the measurement sample is pulverized using a mortar, and an X-ray diffraction pattern is obtained using an X-ray diffractometer (e.g., RINT-1400, manufactured by Rigaku Corporation). Then, the full width at half maximum of the peak of the (020) plane of boehmite in the obtained X-ray diffraction pattern is measured, and the value calculated by the following Scherrer formula is adopted as the crystallite size.

[0022] D=Kλ / βcosθ D: Crystallite diameter (nm) K: Scherrer constant (K=0.94 in the present invention) λ: X-ray wavelength (0.15418nm, CuKα) β: Full width at half maximum (rad) θ: reflection angle

[0023] The crystallite size can be adjusted, for example, by changing the time of the hydrothermal treatment in the production method described below, by changing the ratio of aluminum to the inorganic basic compound during the hydrothermal treatment, or by changing the mixing ratio of gibbsite to pseudo-boehmite.

[0024] <Specific surface area> The specific surface area of ​​crystalline boehmite measured by the nitrogen adsorption method (the method described below or an equivalent method) is 60 to 160 m 2 When the specific surface area is in the above range, the crystallinity of the boehmite is easily maintained. The specific surface area is preferably 80 to 140 m 2 / g.

[0025] <Method of measuring specific surface area using nitrogen adsorption method> First, prepare crystalline boehmite as a measurement sample. When the crystalline boehmite is in the form of a slurry, for example, the slurry is dried at 130° C. for 12 hours, and the residue is ground in a mortar to obtain a crystalline boehmite powder.

[0026] Next, the measurement sample is placed in a magnetic crucible and sintered at 600°C for 2 hours, then placed in a desiccator and cooled to room temperature. Next, 0.3 g of the measurement sample is taken and the specific surface area (m2) of the sample is measured by the BET single point method using a fully automatic surface area measuring device. 2 / g) is measured.

[0027] The specific surface area can be adjusted, for example, by changing the time of the hydrothermal treatment in the production method described below, by changing the ratio of aluminum to the inorganic basic compound during the hydrothermal treatment, or by changing the mixing ratio of gibbsite to pseudo-boehmite.

[0028] <Crystal shape> The aspect ratio of crystalline boehmite, as determined by a scanning electron microscope (SEM) under the following conditions, is 7 or more, preferably 8 or more, and the upper limit thereof may be 50, for example.

[0029] <<How to calculate aspect ratio using SEM observation>> First, prepare crystalline boehmite as a measurement sample. When the crystalline boehmite is in the form of a slurry, for example, the slurry is dried at 130° C. for 12 hours, and the residue is ground in a mortar to obtain a crystalline boehmite powder.

[0030] The measurement sample is observed with a scanning electron microscope to obtain an SEM image of the crystal. The magnification is, for example, 50,000 to 300,000 times. 20 particles in which the flat surface of the plate-like particle can be observed are randomly selected from the image, and the longest diameter is measured. 20 particles in which the thickness of the plate-like particle can be observed are randomly selected from the image, and the shortest diameter (particle thickness) is measured. The aspect ratio is the value obtained by dividing the simple average longest diameter of the 20 particles by the simple average shortest diameter of the 20 particles. Image analysis software (for example, image analysis software Winroof2018 STANDARD manufactured by Mitani Shoji Co., Ltd.) may be used to measure the longest diameter and shortest diameter of the particles.

[0031] The aspect ratio can be adjusted, for example, by changing the time of the hydrothermal treatment in the production method described below, by changing the ratio of aluminum to the inorganic basic compound during the hydrothermal treatment, or by changing the mixing ratio of gibbsite to pseudo-boehmite. The crystalline boehmite preferably has a plate-like shape.

[0032] <CBD(Compact Bulk Density)> The CBD of crystalline boehmite measured by the following method is small, 0.10 to 0.35 g / ml. This crystalline boehmite is considered to form a house of cards structure because of such a small CBD. Therefore, when the crystalline boehmite powder of the present invention is used as a catalyst material, the resulting catalyst has many voids, which is considered to facilitate the diffusion of raw materials and product oil during catalytic reaction. For example, when the crystalline boehmite powder of the present invention is used as a matrix component of an FCC catalyst, it is considered that large voids are formed in the FCC catalyst, and the catalytic performance such as conversion rate can be improved. This CBD is preferably 0.15 to 0.30 g / ml.

[0033] How to measure CBD First, a crystalline boehmite powder is prepared as a measurement sample. When the crystalline boehmite is in the form of a slurry, for example, the slurry is dried at 130° C. for 12 hours and then ground in a mortar to obtain a crystalline boehmite powder.

[0034] Next, 25 g of the measurement sample is weighed out and transferred to a measuring cylinder with a capacity of 250 ml, and the measuring cylinder is attached to a Tyler type sieve shaker. The sample is tapped and filled with the Tyler type sieve shaker for 15 minutes, the measuring cylinder is removed, the sample surface is flattened, the filling volume is read, and the CBD is calculated.

[0035] CBD can be adjusted, for example, by changing the mixing ratio of gibbsite and pseudoboehmite in the production method described below. The crystalline boehmite powder of the present invention can be preferably used, for example, as a matrix component of an FCC catalyst, and can also be used as a catalyst material such as a hydrogenation catalyst, a hydrodesulfurization catalyst, an isomerization catalyst, an oxidation catalyst, or an exhaust gas purification catalyst.

[0036] [Crystalline boehmite slurry] The crystalline boehmite slurry according to the present invention is characterized by containing the above-mentioned crystalline boehmite powder according to the present invention and a dispersion medium.

[0037] Examples of the dispersion medium include water, methanol, ethanol, and 1-propanol, and among these, water is preferred. The concentration of the crystalline boehmite in the crystalline boehmite slurry is, for example, 5.0 to 30 mass %, and preferably 8.0 to 25 mass %, calculated as alumina (Al2O3).

[0038] As described above, the crystalline boehmite slurry according to the present invention has a low viscosity even at a high concentration, and for example, the viscosity (25°C) when the concentration of the crystalline boehmite is adjusted to 15 mass% is preferably 10 to 3000 cP. The concentration is adjusted by increasing or decreasing the amount of a dispersion medium, typically water, contained in the crystalline boehmite slurry.

[0039] The crystalline boehmite slurry may contain additives such as inorganic acids (sulfuric acid, hydrochloric acid, nitric acid, phosphoric acid, boric acid, etc.), inorganic bases (sodium hydroxide, potassium hydroxide, calcium hydroxide, ammonium hydroxide, etc.), organic acids (formic acid, acetic acid, citric acid, malic acid, tartaric acid, gluconic acid, succinic acid, oxalic acid, lactic acid, etc.), thickeners (polyvinyl alcohol, methyl cellulose, gum arabic, diatomaceous earth, bentonite, polyacrylamide, polyethylene oxide, polyacrylic acid esters, locust bean gum, etc.) or no additives, depending on the application, etc., within the range that does not impair the effects of the present invention.

[0040] [Method for producing crystalline boehmite slurry] The method for producing a crystalline boehmite slurry according to the present invention comprises the steps of: Volume-based d measured by laser diffraction / scattering method 50 70 to 95 parts by mass of gibbsite having a (median diameter) of 0.1 μm or more and less than 70 μm, calculated as Al2O3; The crystallite diameter calculated from the (020) plane peak in X-ray diffraction measurement is 2 to 6 nm, and the volume-based d 50 Pseudo-boehmite having a (median diameter) of 3 to 30 μm and not subjected to a peptization treatment is 5 to 30 parts by mass in terms of Al2O3 (wherein the total amount of gibbsite and pseudo-boehmite in terms of Al2O3 is 100 parts by mass), and water a first step of preparing a mixed solution (1) by mixing the above so that the pH does not become 7.0 or less; a second step of adding an inorganic basic compound to the mixed solution (1) to prepare a mixed solution (2) having a pH of 9.0 to 12.5; a third step of subjecting the mixed liquid (2) to a hydrothermal treatment at a temperature of 150 to 190° C. for 0.5 to 24 hours by increasing the temperature at a rate of 5 to 30° C. / hour; The present invention is characterized in that it includes: By this manufacturing method, the above-mentioned crystalline boehmite slurry according to the present invention can be manufactured.

[0041] (first step) The first step is a step of mixing gibbsite, pseudo-boehmite, and water to prepare a mixed liquid (1).

[0042] The volumetric basis of this gibbsite is d 50 (Median diameter) is 0.1 μm or more and less than 70 μm, preferably 1.0 μm or more and less than 65 μm. 50 However, if the amount is less than this range, it is difficult to control the reaction, and if it is greater than this range, the gibbsite settles quickly when suspended in water, making handling difficult. 50 More preferably, it is 2.0 μm or more and less than 60 μm. 50 If the diameter is small, the hydrothermal treatment time can be shortened, and therefore, it is more preferably 2.0 μm or more and less than 40 μm.

[0043] Examples of commercially available gibbsite include "C-303" (manufactured by Sumitomo Chemical Co., Ltd.) and "C-12" (manufactured by Sumitomo Chemical Co., Ltd.). This gibbsite has the following properties: 50 The powder may be ground appropriately so that the particle size falls within the above range. The grinding may be carried out using a ball mill, an attritor, a bead mill, a colloid mill, a high shear mixer, or the like.

[0044] <Method of measuring particle size distribution> The particle size distribution is measured using a laser diffraction / scattering particle size distribution analyzer by putting the sample into a solvent (water) so that the light transmittance is in the range of 70 to 95%, under the following conditions: circulation speed 5.0 L / min, ultrasonic irradiation for 1 minute, repeated 15 times, refractive index 1.66, or equivalent conditions.

[0045] Pseudo-boehmite is considered to function as a seed crystal during hydrothermal treatment, and has a crystallite size of 2 to 6 nm. If the crystallite size is smaller than this range, it is not preferable because the hydrothermal treatment requires a long time, and if it is too large, it is difficult to control the reaction.

[0046] The method for calculating the crystallite diameter of pseudo-boehmite is the same as the method for calculating the crystallite diameter of crystalline boehmite described above. The volumetric basis d of this pseudoboehmite 50 (Median diameter) is 3 to 30 μm. 50 However, if the thickness is smaller than this range, the liquid viscosity is high and handling is difficult, and if the thickness is larger than this range, the crystals do not function as seed crystals. 50 The thickness is preferably 5.0 to 20 μm.

[0047] An example of a commercially available pseudo-boehmite is "Catapal-A" (manufactured by Sasol). Pseudoboehmite is d 50 The powder may be ground appropriately so that the particle size falls within the above range. The grinding may be carried out using a ball mill, an attritor, a bead mill, a colloid mill, a high shear mixer, or the like.

[0048] d of pseudoboehmite50 The measurement method is the d 50 The measurement method is the same as that of The pseudo-boehmite may be prepared in the form of a slurry by a known method, and the pseudo-boehmite slurry may be mixed with gibbsite and water. For example, a method for producing such a pseudo-boehmite slurry includes a method in which an aqueous solution of sodium aluminate and an aqueous solution of aluminum sulfate are added to hot water at 60° C. while stirring the water to precipitate the pseudo-boehmite.

[0049] The pseudo-boehmite according to the present invention is mixed with gibbsite and water without peptization. By not peptizing the pseudo-boehmite, the aggregates of the pseudo-boehmite function as seed crystals, and the resulting crystalline boehmite also aggregates to form a card house structure, which is thought to reduce the CBD. In addition, by not peptizing the pseudo-boehmite, the process can be shortened, which is also excellent in industrial economy and productivity.

[0050] The water used is preferably ion-exchanged water, which may be provided in the form of a slurry containing pseudoboehmite and water. The mixing ratio of gibbsite and pseudo-boehmite, i.e., "mass of gibbsite:mass of pseudo-boehmite", is "70-95:30-5" in terms of Al2O3 (where the sum of the two is 100). If the amount of gibbsite is too small (the amount of pseudo-boehmite is too large), the CBD of the crystalline boehmite obtained from the crystalline boehmite slurry becomes large. Conversely, if the amount of gibbsite is too large (the amount of pseudo-boehmite is too small), the crystallite diameter of the obtained crystalline boehmite becomes large and the specific surface area becomes small. This "mass of gibbsite:mass of pseudo-boehmite" is preferably "75-90:25-10", more preferably "80-90:20-10".

[0051] The mixture (1) obtained by mixing gibbsite, pseudo-boehmite, and water is usually a slurry. The temperature at which the mixed liquid (1) is prepared by mixing gibbsite, pseudo-boehmite, and water is usually 5 to 90°C, and preferably 15 to 80°C.

[0052] These components are mixed so that the pH of the mixed solution (1) does not become 7.0 or less, and is used in the next step. In this way, the pseudo-boehmite does not undergo peptization under acidic conditions, and functions as a seed crystal while remaining in the form of aggregates, and crystalline boehmite with a small CBD is obtained.

[0053] (Second process) The second step is a step of adding an inorganic basic compound to the mixed solution (1) to prepare a mixed solution (2) having a pH of 9.0 to 12.5.

[0054] Examples of inorganic basic compounds include sodium hydroxide, potassium hydroxide, calcium hydroxide, etc., with sodium hydroxide being preferred. The mixed liquid (2) is usually a slurry.

[0055] The type and amount of the inorganic basic compound are adjusted so that the pH of the resulting mixed liquid (2) is usually 9.0 to 12.5, preferably 10.5 to 12.4. If the pH is lower than this lower limit, dissolution and reprecipitation of gibbsite and pseudo-boehmite does not proceed during the hydrothermal treatment, and a slurry containing not only the desired boehmite but also gibbsite is obtained, which is not preferable. The temperature when preparing the mixed liquid (2) by adding the inorganic basic compound to the mixed liquid (1) is usually 5 to 90°C, and preferably 15 to 80°C.

[0056] (Third step) The third step is a step of hydrothermally treating the mixed liquid (2) obtained in the second step to obtain a crystalline boehmite slurry.

[0057] The heat treatment temperature is usually 150 to 190°C, and preferably 160 to 190°C. The heat treatment time is usually 1 to 24 hours, preferably 1.5 to 18 hours. On the other hand, if the heat treatment temperature is excessively lower than this range, or if the heat treatment time is excessively shorter than this range, the hydrothermal reaction does not proceed sufficiently, resulting in a decrease in the yield of crystalline boehmite.

[0058] The temperature increase rate (that is, the rate at which the mixed liquid (2) obtained in the second step is increased to the above-mentioned heat treatment temperature) is usually 5 to 30° C. / hour, and preferably 15 to 30° C. / hour. On the other hand, if the heating rate is excessively higher than this range, the hydrothermal reaction does not proceed sufficiently, resulting in a decrease in the yield of crystalline boehmite.

[0059] The hydrothermal treatment may be carried out under autogenous pressure. For the hydrothermal treatment, an autoclave is usually used. The autoclave is preferably equipped with a stirring blade. The hydrothermal treatment can be carried out more uniformly by stirring the mixture (2) with the stirring blade.

[0060] (Fourth step) The method for producing a crystalline boehmite slurry according to the present invention may optionally include a fourth step of washing the slurry obtained in the third step.

[0061] In the fourth step, the slurry obtained in the third step is dehydrated, the obtained solid matter is washed with water (preferably, ion-exchanged water), and the obtained washed cake is suspended in a liquid medium (preferably, water such as ion-exchanged water) to prepare a washed crystalline boehmite slurry.

[0062] The temperature of the water used for washing is preferably set to 40 to 90°C. By carrying out the fourth step, impurities (such as sodium and sulfate) can be removed, and the slurry can be adjusted to a desired concentration by suspending the washed cake again in water or the like.

[0063] (Crystalline boehmite slurry) According to the method of the present invention, a crystalline boehmite slurry is produced. The crystalline boehmite contained in this crystalline boehmite slurry usually has the physical properties (crystallite size, specific surface area, crystal shape, CBD) described above in the description of the crystalline boehmite powder of the present invention.

[0064] The crystalline boehmite slurry produced by the method of the present invention has an alumina (Al2O3) equivalent concentration of, for example, 5.0 to 30 mass %, preferably 8.0 to 25 mass %. The concentration can be adjusted by increasing or decreasing the amount of water contained in the crystalline boehmite slurry.

[0065] Furthermore, when the concentration of this crystalline boehmite is adjusted to 15 mass %, the viscosity of the crystalline boehmite slurry (25° C.) is preferably 10 to 3000 cP. This crystalline boehmite slurry may contain the additives described in the above description of the crystalline boehmite slurry of the present invention within the range that does not impair the effects of the present invention, or may not contain any additives, depending on the application, etc. When an additive is contained, the additive is added by a conventional method at any stage of the above first to fourth steps.

[0066] The amount of impurities in the crystalline boehmite slurry is not particularly limited, but from the viewpoint of reducing the amount of impurities when used as a catalyst raw material, the amount of impurities in the crystalline boehmite slurry is preferably 5.0 mass% or less, more preferably 2.0 mass% or less, and even more preferably 0.4 mass% or less (wherein the total of the alumina (Al2O3) content in the crystalline boehmite slurry (i.e., the amount of crystalline boehmite converted into Al2O3) and the amount of impurities is 100 mass%). The amount of impurities in the crystalline boehmite slurry can be adjusted by changing the amount of impurities in the raw materials used in the first step, the amount of inorganic basic compound added in the second step, the amount and temperature of washing water in the fourth step, etc.

[0067] The crystalline boehmite slurry may be pulverized as appropriate within the range that does not impair the effects of the present invention. The pulverization may be performed using a ball mill, an attritor, a bead mill, a colloid mill, a high shear mixer, or the like.

[0068] The crystalline boehmite slurry produced by the method of the present invention can be preferably used as a material for, for example, a fluid catalytic cracking catalyst (FCC catalyst), and can also be preferably used as a catalyst for hydrogenation catalysts, hydrodesulfurization catalysts, isomerization catalysts, oxidation catalysts, exhaust gas purification catalysts, and the like.

[0069] [Method of manufacturing crystalline boehmite powder] The method for producing a crystalline boehmite powder according to the present invention comprises the steps of: A step (A) of producing a crystalline boehmite slurry by the method according to the present invention described above; A step (B) of drying the crystalline boehmite slurry produced in the step (A); The present invention is characterized in that it includes:

[0070] (Process (A)) Details of step (A) are as described above.

[0071] (Process (B)) In step (B), the crystalline boehmite slurry produced in step (A) may be washed with water before drying. The temperature of the water is preferably 40 to 90°C.

[0072] Drying may be performed, for example, by heating the washed crystalline boehmite slurry at, for example, 90 to 200° C. for 0.5 to 24 hours. The resulting dried product is preferably pulverized. The pulverization can be carried out by a conventional method such as using a mortar.

[0073] The drying may be performed by spray drying the crystalline boehmite slurry. In this case, the concentration of the crystalline boehmite slurry may be adjusted to, for example, 5 to 30 mass % in terms of Al2O3 by adding water.

[0074] For example, particles (spray-dried particles) are obtained by putting a crystalline boehmite slurry into a slurry tank of a spray dryer and spraying the crystalline boehmite slurry into a drying chamber through which an air current (e.g., an air flow) set at a temperature in the range of, for example, 120 to 600° C. The temperature of the air current decreases due to the spraying of the crystalline boehmite slurry, but the temperature at the outlet of the drying chamber is maintained in the range of, for example, 50 to 300° C. by using a heater or the like.

[0075] The particle size of the spray-dried particles can be controlled by adjusting the concentration, viscosity, spray amount, spray pressure, nozzle diameter of the spray dryer, hot air temperature, etc. of the crystalline boehmite slurry to be sprayed. The crystalline boehmite powder produced by the method of the present invention is usually composed of crystalline boehmite having the physical properties (crystallite size, specific surface area, crystal shape, CBD) described above in the description of the crystalline boehmite powder of the present invention.

[0076] The crystalline boehmite powder produced by the method of the present invention can be preferably used as a material for, for example, a fluid catalytic cracking catalyst (FCC catalyst), and can also be preferably used as a catalyst for hydrogenation catalysts, hydrodesulfurization catalysts, isomerization catalysts, oxidation catalysts, exhaust gas purification catalysts, and the like.

[0077] [Method for producing a fluid catalytic cracking catalyst for hydrocarbon oil] The method for producing a fluid catalytic cracking catalyst (FCC catalyst) for hydrocarbon oil according to the present invention is as follows: A step (α) of producing a crystalline boehmite slurry by the method according to the present invention described above, or producing a crystalline boehmite powder by the method according to the present invention described above; A step (β) of mixing the crystalline boehmite slurry and / or crystalline boehmite powder obtained in the step (α) with other components to produce a catalyst raw material slurry; A step (γ) of spray-drying the catalyst raw material slurry produced in the step (β) to obtain particles; a step (δ) of contacting the particles produced in the step (γ) with water containing an ammonium salt; The present invention is characterized in that it includes:

[0078] (Process (α)) The details of step (α) are as described above.

[0079] (Process (β)) In step (β), the crystalline boehmite slurry and / or crystalline boehmite powder produced in step (α), ultra-stable Y-type zeolites, a silica-based matrix-forming component, optionally water, optionally clay minerals, and optionally additives are mixed to produce a catalyst raw material slurry.

[0080] The ultra-stable Y-type zeolites, the silica-based matrix-forming component, the clay minerals, and the additives may be added in the form of powder or in the form of a slurry, and the order of adding the components is not important as long as a slurry can be prepared without causing gelation.

[0081] (Ultra-stable Y-type zeolites) Examples of ultrastable Y-type zeolites include ultrastable Y-type zeolite (USY) and rare earth metal-exchanged ultrastable Y-type zeolite (hereinafter also referred to as "REUSY"), which is obtained by introducing rare earth metals into USY by ion exchange or the like.

[0082] (Silica-based matrix forming component) The silica-based matrix forming component is usually prepared by mixing a silica source with an acid. Examples of the silica source include silica, silica gel (including silica hydrogel), silica sol (including silica hydrosol), and aqueous solutions of silicic acid (salts) (including orthosilicic acid (salts) and metasilicic acid (salts)) (e.g., water glass). As the silica sol and silicate salt, colloidal silica of sodium type, potassium type, lithium type, acid type, etc. can be used. Among these, silica sol and aqueous solutions of silicic acid (salts) are preferred.

[0083] The acid may be an inorganic acid, such as sulfuric acid, hydrochloric acid, nitric acid, or phosphoric acid, and among these, sulfuric acid, hydrochloric acid, and nitric acid are preferred, with sulfuric acid being particularly preferred.

[0084] (Clay minerals) The clay minerals that act as a bulking agent are clay and / or clay minerals, examples of which include kaolin, bentonite, kaolinite, halloysite, montmorillonite, etc., with kaolin being particularly preferred.

[0085] In step (β), the catalyst raw material slurry may be prepared by adding, in addition to these components, optional additives and water. Additives include silica alumina, activated alumina, aluminum hydroxide (including gibbsite), and the like.

[0086] This catalyst raw material slurry contains crystalline boehmite slurry and / or crystalline boehmite powder, for example, in an amount of 1 to 30 mass %, and preferably 3 to 20 mass %, calculated as Al2O3 (where the solid content in the catalyst raw material slurry is taken as 100 mass %).

[0087] The catalyst raw material slurry contains zeolite in an amount of, for example, 10 to 40 mass %, preferably 12 to 38 mass %, and more preferably 14 to 36 mass % (wherein the solid content in the catalyst raw material slurry is taken as 100 mass %).

[0088] The catalyst raw material slurry contains the above-mentioned silica-based matrix-forming component, calculated as the amount of SiO2, in an amount of, for example, 10 to 30 mass %, preferably 12 to 26 mass %, and more preferably 14 to 24 mass % (where the amount of solids in the catalyst raw material slurry (the same applies to all components other than the dispersion medium in the catalyst raw material slurry)) is taken as 100 mass %).

[0089] The catalyst raw material slurry contains the above-mentioned clay minerals in an amount of, for example, 10 to 60 mass %, preferably 14 to 56 mass %, and more preferably 18 to 52 mass % (where the solid content in the catalyst raw material slurry is taken as 100 mass %).

[0090] The catalyst raw material slurry contains the above-mentioned additives in an amount of, for example, 2 to 30 mass %, and preferably 5 to 20 mass % (where the solid content in the catalyst raw material slurry is taken as 100 mass %). The catalyst raw material slurry contains water as a dispersion medium.

[0091] The catalyst raw material slurry may contain small amounts of components other than water as a dispersion medium, such as methanol, ethanol, and acetone. The solids concentration of the catalyst raw material slurry is, for example, 10 to 50 mass %, and preferably 20 to 40 mass %, in order to perform spray drying of the catalyst raw material slurry without difficulty.

[0092] (Process (γ)) In the step (γ), the catalyst raw material slurry produced in the step (β) is spray-dried to obtain particles (hereinafter also referred to as “spray-dried particles”).

[0093] The spray-drying conditions may be appropriately changed depending on the solids concentration, viscosity, etc. of the catalyst raw material slurry, and are not particularly limited as long as the average particle size of the obtained spray-dried particles is in the average range of 50 to 90 μm, similar to that of general FCC catalyst particles.

[0094] For example, particles (spray-dried particles) are obtained by placing the catalyst raw material slurry in a slurry storage tank of a spray dryer and spraying the catalyst raw material slurry into a drying chamber through which an air current (e.g., an air current) set at a temperature in the range of, for example, 120 to 600° C. The temperature of this air current decreases as the catalyst raw material slurry is sprayed, but the temperature at the outlet of the drying chamber is maintained in the range of, for example, 50 to 300° C. by using a heater or the like.

[0095] The particle size of the spray-dried particles can be controlled by adjusting the concentration, viscosity, spray amount, spray pressure, nozzle diameter of the spray dryer, hot air temperature, and the like of the catalyst raw material slurry to be sprayed. The spray-dried particles may also be washed (eg, with water) and dried.

[0096] (Process (δ)) In step (δ), the spray-dried particles obtained in step (γ) are contacted with an aqueous solution containing a rare earth metal to introduce the rare earth metal into the zeolite in the spray-dried particles. This step (δ) produces an FCC catalyst.

[0097] In step (δ), the spray-dried particles are preferably suspended in water to prepare a suspension, and the suspension is contacted with an aqueous solution containing rare earth metals (RE) to be ion-exchanged. The obtained solid matter (FCC catalyst) may then be separated, washed and dried. The temperature of the water is preferably 40 to 80°C. In addition, the suspension may be filtered, and the filtered solid matter may be suspended again in water to remove unnecessary soluble substances present in the spray-dried particles.

[0098] The aqueous solution containing a rare earth metal can be prepared, for example, by dissolving a salt of the rare earth metal (for example, LaCl3) in water. The step (δ) is carried out so that the concentration of rare earth metal in the obtained fluid catalytic cracking catalyst is 0.5 to 3.5 mass%, preferably 0.7 to 3.0 mass%, calculated as rare earth metal oxide (RE2O3). The amount and concentration of the aqueous solution containing the rare earth metal are adjusted so that the rare earth metal oxide content is the desired content.

[0099] Not only when the ultra-stable Y-type zeolite is USY, but also when REUSY is used and some rare earth metal ions are removed (replaced with protons) from REUSY when preparing the catalyst raw material slurry in step (β) or when washing the spray-dried particles obtained in step (γ), a fluid catalytic cracking catalyst containing a desired amount of rare earth metal can be produced by carrying out step (δ).

[0100] According to the method of the present invention including the above steps (α) to (δ), a fluid catalytic cracking catalyst for hydrocarbon oil can be produced. EXAMPLES

[0101] The present invention will be described in detail below with reference to examples, but the present invention is not limited to these examples.

[0102] [Measurement method] In the examples, various measurements were carried out by the following methods.

[0103] <Slurry measurement> (Particle size distribution (d 50 )) The particle size distribution of the sample was measured using a laser diffraction / scattering particle size distribution analyzer (LA-950V2) manufactured by Horiba, Ltd. Specifically, the sample was placed in a solvent (water) so that the light transmittance was in the range of 70 to 95%, and the measurement was performed with a circulation speed of 5.0 L / min, ultrasonic irradiation for 1 minute, repetition times of 15, and a refractive index of 1.66.

[0104] <Measurement of powder> (Preparation of measurement samples) The washed cake obtained during the process of carrying out step 3 in each of the Examples and Comparative Examples was dried at 130° C. for 12 hours and then pulverized in a mortar to obtain a measurement sample.

[0105] (Crystallite size, crystal morphology and crystal shape) The measurement sample was subjected to X-ray diffraction analysis using an X-ray diffractometer (Rigaku Corporation, RINT-1400) to identify the crystal structure. Furthermore, the crystallite size was calculated from the peak of the (020) plane of boehmite by the above-mentioned method.

[0106] (Crystal shape) The measurement sample was observed by a scanning electron microscope (SEM) using the method described above to confirm the crystal shape and determine the aspect ratio. The scanning electron microscope used was a scanning electron microscope S-5500 from Hitachi High-Technologies Corporation, with a magnification of 50,000 to 300,000 times, and the image analysis software Winroof2018 STANDARD from Mitani Shoji Co., Ltd. was used as the image analysis software.

[0107] (specific surface area) The measurement sample was placed in a magnetic crucible and sintered at 600°C for 2 hours, then cooled to room temperature in a desiccator. Next, 0.3 g of the measurement sample was taken and the specific surface area (m 2 / g) was measured by the BET single point method.

[0108] (CBD) 25 g of crystalline boehmite powder was weighed out and transferred to a measuring cylinder with a capacity of 250 ml, and the measuring cylinder was attached to a Tyler type sieve shaker. The sample was tapped and filled in the Tyler type sieve shaker for 15 minutes, the measuring cylinder was removed, the sample surface was flattened, the filling volume was read, and the CBD was calculated.

[0109] [Example 1] (Step 1: Preparation of pseudo-boehmite) 9.09 kg of sodium aluminate aqueous solution with an Al2O3 equivalent concentration of 22% by mass was placed in a 100 L tank equipped with a steam jacket, and diluted with ion-exchanged water to 40.00 kg. Next, 230.8 g of sodium gluconate aqueous solution with a concentration of 26% by mass was added to this solution, and the mixture was heated to 60°C with stirring to obtain a mixed solution of sodium aluminate and sodium gluconate with an Al2O3 equivalent concentration of 5% by mass.

[0110] Separately from this mixed solution, 14.29 kg of an aqueous aluminum sulfate solution having a concentration of 7 mass % calculated as Al2O3 was diluted with 25.71 kg of ion-exchanged water and then heated to 60°C to prepare an aqueous aluminum sulfate solution.

[0111] Next, the aluminum sulfate aqueous solution was added to a mixed solution of sodium aluminate and sodium gluconate with an Al2O3 concentration of 5% by mass while stirring it over a period of 10 minutes to prepare an alumina hydrate slurry with an Al2O3 concentration of 3.8% by mass. The pH of the slurry was 7.2. The resulting alumina hydrate slurry was aged at 60°C for 60 minutes while stirring. The aged alumina hydrate slurry was then dehydrated under reduced pressure using a flat plate filter, and washed with 100 L of ion-exchanged water at 60°C. The cake (1) obtained by washing was suspended in ion-exchanged water to a concentration of 15% by mass in terms of Al2O3, to obtain a pseudo-boehmite slurry (1).

[0112] A small amount of the slurry was extracted for analysis, and the particles in the slurry were found to be pseudoboehmite particles, with a crystallite diameter of 3.6 nm and a volumetric d 50 The median diameter was 16 μm.

[0113] (Step 2: Preparation of crystalline boehmite by hydrothermal treatment) 0.60 kg of the pseudo-boehmite slurry (1) obtained in step 1 was mixed with gibbsite powder (1) (C-303 manufactured by Sumitomo Chemical Co., Ltd., Al2O3 equivalent concentration 66.6 mass%, d 50 0.77 kg of ammonium nitrate (median diameter: 5.6 μm) and 2.59 kg of ion-exchanged water were added to prepare a slurry with an Al2O3-equivalent concentration of 15 mass%. 49 g of a 48 mass% aqueous sodium hydroxide solution was added while stirring to obtain a uniform slurry (2) with a pH of 12.2. The slurry (2) was placed in a 5 L autoclave reactor, heated to 190°C at a rate of 25°C / hour while stirring, and held at the spontaneous pressure for 5 hours to obtain a slurry (3).

[0114] (Step 3: Washing of crystalline boehmite) 4.0 kg of the slurry (3) obtained in step 2 was dehydrated under reduced pressure using a flat plate filter, and then washed with 20 L of ion-exchanged water at 60°C to obtain a washed cake (2). The washed cake (2) was placed on a stainless steel tray and dried at 130°C for 12 hours, and then thoroughly ground in a mortar to obtain a crystalline boehmite powder (1). The obtained crystalline boehmite powder (1) was measured by the above-mentioned method. The production conditions and measurement results are shown in Table 1 (the same applies to the following Examples and Comparative Examples).

[0115] [Example 2] The washed cake (2) obtained in step 3 of Example 1 was diluted with ion-exchanged water to an Al2O3-equivalent concentration of 15 mass%, and thoroughly suspended to obtain a crystalline boehmite slurry (4). The slurry (4) was dried in a spray dryer with an inlet temperature of 250°C and an outlet temperature of 120°C as droplets to obtain a crystalline boehmite powder (2). The obtained crystalline boehmite powder (2) was measured by the above-mentioned method.

[0116] [Example 3] In step 2, gibbsite powder (1) was ground with a bead mill into gibbsite powder (2) (Sumitomo Chemical Co., Ltd., C-303 (Al2O3 equivalent concentration 66.6 mass%)) and the volumetric basis d 50 Crystalline boehmite powder (3) was produced and measured in the same manner as in Example 1, except that the amount of the powder (having a median diameter of 2.6 μm) was changed to 0.77 kg.

[0117] [Example 4] Crystalline boehmite powder (4) was produced and measured in the same manner as in Example 1, except that in step 2, the amount of pseudo-boehmite slurry (1) was changed to 0.28 kg, the amount of gibbsite powder (1) was changed to 0.84 kg, and the amount of ion-exchanged water was changed to 2.83 kg.

[0118] [Example 5] A crystalline boehmite powder (5) was produced and measured in the same manner as in Example 1, except that in step 2, the amount of the pseudo-boehmite slurry (1) was changed to 1.00 kg, the amount of the gibbsite powder (1) was changed to 0.68 kg, and the amount of ion-exchanged water was changed to 2.28 kg.

[0119] [Example 6] In step 2, the gibbsite powder (1) was mixed with gibbsite powder (3) (C-12 manufactured by Sumitomo Chemical Co., Ltd., Al2O3 equivalent concentration 66.6 mass%, d 50 A crystalline boehmite powder (6) was produced and measured in the same manner as in Example 1, except that the amount of powder (median diameter: 51 μm) was changed to 0.77 kg.

[0120] [Example 7] A crystalline boehmite powder (7) was produced and measured in the same manner as in Example 1, except that in step 2, the heating temperature was changed to 160° C. and the heating time was changed to 12 hours.

[0121] [Example 8] (Step 1: Preparation of boehmite) The pseudo-boehmite slurry (1) obtained in Example 1 was adjusted to pH 10.2 by adding ammonia water having a concentration of 15% by mass, and aged for 10 hours at 95° C. with stirring. The aged alumina hydrate slurry was dehydrated under reduced pressure using a plate filter, and then washed with 100 L of ion-exchanged water at 60° C.

[0122] The cake obtained by washing was suspended in ion-exchanged water so that the concentration in terms of Al2O3 was 15 mass %, to obtain a pseudo-boehmite slurry (8). A small amount of the slurry was extracted for analysis, and the particles in the slurry were found to be pseudoboehmite particles, with a crystallite diameter of 5.3 nm and a volumetric d 50 The median diameter was 6.8 μm.

[0123] (Step 2 and Step 3) Crystalline boehmite powder (8) was produced and measured in the same manner as in steps 2 and 3 of Example 1, except that the pseudo-boehmite slurry (1) was changed to 0.60 kg of pseudo-boehmite slurry (8).

[0124] [Example 9] A crystalline boehmite powder (9) was produced and measured in the same manner as in Example 1, except that in step 2, the amount of the 48% by mass aqueous sodium hydroxide solution was changed to 196 g.

[0125] [Comparative Example 1] A crystalline boehmite powder (10) was produced and measured in the same manner as in Example 1, except that in step 2, the pseudo-boehmite slurry (1) was not used, the amount of gibbsite powder (1) was changed to 0.90 kg, and the amount of ion-exchanged water was changed to 3.10 kg.

[0126] [Comparative Example 2] A crystalline boehmite powder (11) was produced and measured in the same manner as in Example 1, except that in step 2, the amount of the pseudo-boehmite slurry (1) was changed to 3.20 kg, the amount of the gibbsite powder (1) was changed to 0.18 kg, and the amount of ion-exchanged water was changed to 0.62 kg.

[0127] [Comparative Example 3] An aluminum hydroxide powder was produced and measured in the same manner as in Example 1, except that in step 2, the heating temperature was changed to 140°C.

[0128] [Comparative Example 4] An aluminum hydroxide powder was produced and measured in the same manner as in Example 1, except that in step 2, the heating rate was changed to 40° C. / hour.

[0129] [Table 1]

[0130] An example of application of the crystalline boehmite powder of the present invention to an FCC catalyst material will be described below. [Production and evaluation of FCC catalysts] [Catalyst Preparation Example 1] 2941 g of water glass (SiO2 concentration 17% by mass) and 1059 g of an aqueous sulfuric acid solution (sulfuric acid concentration 25%) were added simultaneously and continuously to prepare 4000 g of a silica binder solution with a SiO2 concentration of 12.5% ​​by mass. To this silica binder solution, 882 g of kaolin (solid content (weight remaining after ignition at 1000°C for 1 hour / weight before ignition treatment) 85% by mass), 378 g of aluminum hydroxide (crystal form: gibbsite, Al2O3 equivalent concentration: 66.6% by mass) as an active matrix, 1667 g of a slurry (Al2O3 equivalent concentration: 15% by mass, pH adjusted to 3.0 with sulfuric acid) prepared by suspending crystalline boehmite powder (1) in pure water as crystalline boehmite, and 2273 g of ultra-stable Y-type zeolite slurry (UCS 2.445 nm, SiO2 / Al2O3 molar ratio determined by fluorescent X-ray measurement: 7.1, solid content concentration: 33% by mass) whose pH was adjusted to 3.9 with sulfuric acid were added, and the mixture was thoroughly stirred to prepare a mixed slurry.

[0131] This mixed slurry was made into droplets and spray-dried in a spray dryer with an inlet temperature of 250° C. and an outlet temperature of 150° C. to obtain spherical particles with an average particle size of 70 μm. The obtained spray-dried particles were washed with hot water, then ion-exchanged with an aqueous ammonium sulfate solution and an aqueous rare earth metal chloride solution, and washed with hot water, so that the RE2O3 (RE is a rare earth metal element) content was 1.0 mass%. The catalyst particles were then dried in a dryer at an atmosphere of 150°C for 10 hours to obtain a fluid catalytic cracking catalyst C1.

[0132] [Catalyst Preparation Examples 2 to 4, Catalyst Preparation Comparative Examples 1 to 2] Fluid catalytic cracking catalysts C2 to C6 were obtained by carrying out the same operation as in catalyst preparation example 1 of FCC catalyst, except that the crystalline boehmite powder (1) was replaced with any of the crystalline boehmite powders (3), (4), (5), (10), and (11).

[0133] [Catalyst Preparation Comparative Example 3] Fluid catalytic cracking catalyst C7 was obtained by the same operation as in catalyst preparation example 1 of FCC catalyst, except that commercially available crystalline boehmite powder (crystal form: boehmite, crystallite size: 22 nm, CBD: 0.56 g / ml, Al2O3 equivalent concentration: 83 mass%) was used instead of the crystalline boehmite powder (1).

[0134] [Wear resistance test] The fluid catalytic cracking catalysts of the Catalyst Examples and Comparative Examples were evaluated by the attrition resistance index according to the method described in Catalyst Chemical Engineering Report, Vol. 13, No. 1, p. 65, 1996.

[0135] [Catalyst activity evaluation test] For each of the fluid catalytic cracking catalysts of the catalyst examples and the comparative catalyst examples, a performance evaluation test was performed using ACE-MAT (Advanced Cracking Evaluation-Micro Activity Test) under the same crude oil and the same reaction conditions. The fluid catalytic cracking catalyst C5 was not subjected to the performance evaluation test because its wear resistance had deteriorated. The results are shown in Table 2.

[0136] However, prior to conducting these performance evaluation tests, in order to simulate the condition of hydrothermal degradation in a catalyst regeneration tower, 1000 ppm of nickel (the mass of nickel divided by the mass of the catalyst) and 2000 ppm of vanadium (the mass of vanadium divided by the mass of the catalyst) were deposited in advance, and then the catalyst was steamed at 780°C for 13 hours to perform a pseudo-equilibrium treatment.

[0137] <Operating conditions> The reaction conditions in the catalyst performance evaluation test are as follows: Feedstock: A 50+50 mixture of desulfurized atmospheric residue (DSAR) and desulfurized vacuum gas oil (DSVGO) Catalyst / oil mass ratio (C / O): 5.0 (mass% / mass%) Reaction temperature: 520℃ 1) Conversion rate=100-(LCO+HCO) (mass%) 2) Boiling point range of gasoline: 30~216℃ 3) Boiling point range of LCO: 216~343℃ (LCO: Light Cycle Oil) 4) Boiling point range of HCO: 343℃+ (HCO: Heavy Cycle Oil) 5) LPG (liquid petroleum gas) 6) Dry Gas: Methane, Ethane and Ethylene

[0138] [Table 2]

Claims

1. The crystallite size calculated from the peak of the (020) plane in X-ray diffraction measurement is 10 to 40 nm; The specific surface area measured by the nitrogen adsorption method is 60 to 160 m 2 / g, The aspect ratio as determined by observation with a scanning electron microscope is 7 or more, CBD (Compact Bulk Density) is 0.10 to 0.35 g / ml; Crystalline boehmite powder.

2. A crystalline boehmite slurry comprising the crystalline boehmite powder according to claim 1 and a dispersion medium.

3. Volume-based d measured by laser diffraction / scattering method 50 Gibbsite having a median diameter of 0.1 μm or more and less than 70 μm is used as Al 2 O 3 Converted to 70 to 95 parts by weight, The crystallite diameter calculated from the peak of the (020) plane in X-ray diffraction measurement is 2 to 6 nm, and the volume-based d 50 The pseudo-boehmite having a median diameter of 3 to 30 μm and not subjected to peptization treatment is added to Al 2 O 3 5 to 30 parts by mass (excluding Al of gibbsite and pseudo-boehmite) 2 O 3 The total amount converted is 100 parts by mass. water a first step of preparing a mixed solution (1) by mixing the above in such a manner that the pH does not become 7.0 or less; a second step of adding an inorganic basic compound to the mixed solution (1) to prepare a mixed solution (2) having a pH of 9.0 to 12.5; a third step of heating the mixed liquid (2) at a rate of 5 to 30° C. / hour and subjecting it to a hydrothermal treatment at 150 to 190° C. for 0.5 to 24 hours; A method for producing a crystalline boehmite slurry comprising:

4. A step (A) of producing a crystalline boehmite slurry by the method according to claim 3; A step (B) of drying the crystalline boehmite slurry produced in the step (A); A method for producing a crystalline boehmite powder comprising the steps of:

5. A step (α) of producing a crystalline boehmite slurry by the method according to claim 3 or producing a crystalline boehmite powder by the method according to claim 4; a step (β) of producing a catalyst raw material slurry by mixing the crystalline boehmite slurry and / or the crystalline boehmite powder, ultra-stable Y-type zeolites, a silica-based matrix forming component, optionally water, optionally clay minerals, and optionally additives; A step (γ) of spray-drying the catalyst raw material slurry to obtain particles; contacting the particles with water containing an ammonium salt (δ); A method for producing a fluid catalytic cracking catalyst for hydrocarbon oil comprising the steps of:

Citation Information

Patent Citations

  • Method for producing nanodispersible boehmite and method for using it in flame-retardant synthetic resins

    JP2011515307A

  • Method for producing nanoscale crystalline boehmite

    JP2018503583A