Laminate and method for manufacturing laminate

The laminate with a high Clark stiffness surface layer and base material layer addresses the issue of white spots in PCR resin films by reducing surface protrusions, enhancing printing quality.

JP2024143772AInactive Publication Date: 2024-10-11YUPO CORP
View PDF 2 Cites 0 Cited by

Patent Information

Application Number
JP2023056642
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Filing Date
2023-03-30
Publication Date
2024-10-11
Estimated Expiration
Not applicable · inactive patent

AI Technical Summary

Technical Problem

Films made from PCR resin often contain coarse particles that form protrusions, leading to white spots during printing due to high maximum height and kurtosis, causing ink adhesion issues.

Method used

A laminate structure with a base material layer having a maximum height of 10 μm or more and a surface layer with a Clark stiffness of 10 cm³/100 or more is used to suppress white spots during printing.

Benefits of technology

The laminate effectively reduces the maximum height and kurtosis of the surface, preventing white spots and ensuring uniform ink adhesion, resulting in improved printing quality.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024143772000001_ABST
    Figure 2024143772000001_ABST
Patent Text Reader

Abstract

To provide means capable of suppressing occurrence of white spots during printing, in a laminate having a base material layer having a projection part having a large maximum height.SOLUTION: A laminate has a base material layer containing a thermoplastic resin, and a surface layer laminated on at least one surface of the base material layer, wherein a maximum height of the surface of the base material layer is 10 μm or more, and the surface layer is a film having Clark rigidity of 10 cm3 / 100 or more.SELECTED DRAWING: Figure 1
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a laminate and a method for producing the laminate. [Background technology]

[0002] In recent years, waste recycling has become more common in order to reduce environmental pollution caused by plastic waste. Recycled resins made from plastic waste can be reused for a variety of purposes. In particular, resins made from plastics that were purchased, used, and then discarded by consumers are called PCR (Post-Consumer Recycle) resins. Due to the growing demand to reduce environmental pollution, there is a strong demand for technology to promote the use of recycled sheets made from PCR resins.

[0003] However, PCR resin often contains various foreign matter that cannot be removed during the recycling process, as it has various foreign matter attached to it or contains particles and fibers that were used in the original product. Therefore, if PCR resin containing such foreign matter is used as it is as a film raw material, there is a problem that large protrusions are generated on the film surface.

[0004] To solve such problems, for example, Patent Document 1 proposes a composite film in which a layer containing a large amount of foreign matter is laminated on the surface of a layer containing a large amount of foreign matter, while Patent Document 2 proposes a laminate in which a surface layer having a thickness of 0.15 times or more the maximum particle size of the coarse particles is laminated on the surface of a base layer containing particles (coarse particles) as foreign matter. [Prior art documents] [Patent documents]

[0005] [Patent Document 1] JP 2000-141573 A [Patent Document 2] International Publication No. 2022 / 210896 Summary of the Invention [Problem to be solved by the invention]

[0006] As described above, films formed using PCR resin contain coarse particles as foreign matter, and the film surface containing such coarse particles has protrusions with large maximum heights and kurtosis (sharpness) due to the coarse particles. When printing is performed on such a film surface, there is a problem in that areas where ink does not adhere (whiteouts) are generated around the protrusions.

[0007] Therefore, the present invention has been made in consideration of the above-mentioned circumstances, and aims to provide a means for suppressing the occurrence of blank spots during printing in a laminate including a base material layer having protrusions with a large maximum height. [Means for solving the problem]

[0008] The present inventors have conducted extensive research to solve the above problems, and have found that a laminate having a base layer with a large maximum height on its surface and a surface layer (surface film) with a Clark stiffness of a specific value or more can suppress the occurrence of blank spots when printed, thereby completing the present invention.

[0009] That is, the above objects can be achieved by the present invention having the following configuration, and the present invention includes the following aspects and configurations.

[0010] One aspect of the present invention is 1. A laminate having a base layer containing a thermoplastic resin and a surface layer laminated on at least one surface of the base layer, the maximum height of the surface of the base layer being 10 μm or more, and the surface layer having a Clark stiffness of 10 cm 3 / 100 or more film, laminate; 2. In the laminate described in 1 above, the surface layer has a Clark stiffness of 10 to 40 cm 3 / 100 film is preferred; 3. In the laminate according to 1. or 2. above, the surface layer preferably has a thickness of 30 to 80 μm; 4. In the laminate according to any one of the above 1. to 3., the thickness of the laminate is preferably 80 to 400 μm; 5. In the laminate according to any one of the above 1. to 4., it is preferable that the thermoplastic resin contained in the base layer contains a recycled resin.

[0011] Another aspect of the present invention is 6. A substrate film containing a thermoplastic resin and having a maximum height of 10 μm or more on at least one side, the surface of which has a Clark stiffness of 10 cm 3 A method for producing a laminate, comprising: laminating a surface film having a surface roughness of 100 / 100 or more; 7. In the manufacturing method described in 6. above, it is preferable that the thickness of the base film is 20 to 340 μm, the base film contains the thermoplastic resin and particles, and the maximum particle size of the particles is 3 to 30 times the thickness of the base film; 8. In the manufacturing method according to 6. or 7. above, it is preferable that the surface film is attached while the surface of the base film is in a molten state. Effect of the Invention

[0012] According to the present invention, in a laminate including a base layer having protrusions with a large maximum height, the occurrence of blank spots during printing can be suppressed. [Brief description of the drawings]

[0013] [Figure 1] FIG. 1 is a cross-sectional view that illustrates a typical embodiment of a laminate according to the present invention. [Diagram 2] FIG. 2 is a cross-sectional view showing a schematic example of a different laminate structure of a laminate as an application example of the embodiment of FIG. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0014] One aspect of the present invention is a laminate having a base layer containing a thermoplastic resin and a surface layer laminated on at least one surface of the base layer, the maximum height of the surface of the base layer being 10 μm or more, and the surface layer having a Clark stiffness of 10 cm 3 / 100 or more. Hereinafter, the laminate having the above-mentioned configuration is also simply referred to as "the laminate according to the present invention". In addition, the base layer is also simply referred to as "the base layer according to the present invention", and the surface layer is also simply referred to as "the surface layer according to the present invention".

[0015] In another embodiment of the present invention, a substrate film containing a thermoplastic resin and having a maximum height of 10 μm or more on at least one surface has a Clark stiffness of 10 cm 3 A method for producing a laminate, comprising laminating a surface film having a film thickness of 1 / 100 or more. Hereinafter, the method for producing a laminate having the above-mentioned configuration will also be referred to simply as the "production method according to the present invention." The above-mentioned base film will also be referred to simply as the "base film according to the present invention," and the above-mentioned surface film will also be referred to simply as the "surface film according to the present invention."

[0016] Hereinafter, embodiments of the present invention will be described. Note that the present invention is not limited to the following embodiments.

[0017] In this specification, the range "X to Y" means "X or more and Y or less". Furthermore, unless otherwise specified, the operation and measurement of physical properties are performed under the conditions of room temperature (20 to 25°C) and relative humidity 40 to 50% RH. Furthermore, "A and / or B" includes each of A and B and all combinations of one or more, specifically, it means at least one of A and B, and it means A, B, and a combination of A and B. Furthermore, the term "(meth)acrylic" includes both acrylic and methacrylic. Thus, for example, the term "(meth)acrylic acid" includes both acrylic acid and methacrylic acid.

[0018] <Laminate> The laminate according to the present invention comprises a base layer containing a thermoplastic resin and having a surface with a maximum height of 10 μm or more;3 and a surface layer which is a film having a thickness of 1 / 100 or more, and the surface layer is laminated on a surface (a surface having a specific maximum height) of the base layer. The present inventors have surprisingly found that by having a surface layer having the above-mentioned configuration, it is possible to suppress the occurrence of blank spots during printing, even in a laminate including a base layer having protrusions with a large maximum height.

[0019] The mechanism by which the present invention provides the above-mentioned effects is believed to be as follows.

[0020] As described above, a film formed using a resin containing foreign matter such as a PCR resin contains coarse particles, and the surface of such a film has protrusions (coarse protrusions) with large maximum height and kurtosis (pointedness). When printing is performed on such a film surface, blanks occur around the protrusions, and it has been believed that such blanks are caused by the large maximum height and kurtosis (pointedness) of the protrusions. However, in the process of repeatedly studying techniques for suppressing blanks, the present inventors have closely studied the maximum height and kurtosis (pointedness) of the protrusions, and have surprisingly found that, of these, kurtosis (pointedness) does not have a significant effect on the occurrence of blanks, while the maximum height of the protrusions has a significant effect on the occurrence of blanks. Based on this knowledge, the inventors have conducted extensive research to reduce the maximum height. As a result, the Clark stiffness of a substrate layer having a protrusion with a large maximum height is 10 cm 3 It was found that by combining a film with a surface layer having a thickness of 100 / 100 or more, the maximum height of the laminate surface can be reduced, and as a result, white spots can be suppressed.

[0021] Generally, the stiffness of films and papers (hereinafter also referred to as "films, etc.") is defined by the Clark stiffness, Gurley stiffness, Taber stiffness, etc. Clark stiffness is an index showing how a film, etc. bends when bent under its own weight, and is a parameter proportional to the cube of the elastic modulus and thickness of the film, etc. Meanwhile, Gurley stiffness is an index showing the force required to bend a film, etc. to a certain angle, and Taber stiffness is an index showing the angle (flexure or bending) when a certain force is applied to a film, etc. to bend it. Among these, Clark stiffness is an index relating to the behavior of a film, etc. when it bends under its own weight, as will be described in detail below, and is a parameter that depends on the elastic modulus.

[0022] The laminate according to the present invention has a Clark stiffness of 10 cm 3 The surface layer has a Clark stiffness of 10 cm or more, and since such a film (surface layer) has sufficient elasticity, it acts like a cushion layer against the unevenness formed by the protrusions of the base layer, mitigating (absorbing) the unevenness on the surface of the base layer. As a result, even when a laminate is produced using a base layer with a large maximum surface height, the maximum height on the surface of the surface layer (surface of the laminate) can be reduced, thereby suppressing blank spots during printing. On the other hand, when a substrate layer with a large maximum surface height is used to produce a laminate, a substrate layer with a Clark stiffness of 10 cm or more is used. 3 When a film having a thickness of less than 1 / 100 is combined with the base layer, the film does not have sufficient elasticity and cannot function as a cushion layer as described above. Therefore, the maximum height of the protrusions of the base layer is not reduced and appears on the surface of the laminate, resulting in white spots.

[0023] Thus, the laminate of the present invention is 10 cm 3 By having a surface layer (surface film) having a Clark stiffness of 1 / 100 or more, blank spots during printing can be suppressed. Since the laminate according to the present invention has a reduced maximum height on its surface, it is possible to suppress not only blank spots but also the occurrence of uneven color density between the protrusions and the other parts (bulk parts). Therefore, according to the present invention, a laminate with good print quality is provided.

[0024] It should be noted that the above mechanism is merely speculation and does not limit the technical scope of the present invention in any way.

[0025] The structure of the laminate according to the present invention will be described below with reference to the drawings. Note that the dimensional ratios in the drawings are exaggerated for the convenience of explanation and may differ from the actual ratios.

[0026] The laminate 10 according to the present invention has a surface layer 2 on a base layer 1 containing a thermoplastic resin. The base layer 1 has a maximum height of its surface (the surface on which the surface layer 2 is laminated) of 10 μm or more. The surface layer 2 has a Clark stiffness of 10 cm 3 The film has a thickness of 10 μm or more. The surface layer 2 may be provided on at least one surface of the base layer 1. Thus, the surface layer 2 may be provided on only one surface (one side) of the base layer 1 as shown in FIG. 1, or may be provided on both surfaces (both sides) of the base layer 1 as shown in FIG. 2 (i.e., the base layer 1 may have a first surface layer on one surface and a second surface layer on the other surface). However, even if both second surface layers shown in FIG. 2 are surface layers according to the present invention, it is not necessary that the maximum heights of both of the two surfaces of the base layer 1 are 10 μm or more, and as long as only one of the surfaces has a maximum height of 10 μm or more, it is within the scope of the present invention.

[0027] When the laminate 10 in Fig. 1 is used as a printing paper and printing is performed on the laminate 10, the side A in Fig. 1 becomes the printing surface. When the laminate 10 in Fig. 2 is used as a printing paper, both the side A and the side B in Fig. 2 become the printing surfaces. In other words, the surface layer (first surface layer, second surface layer) 2 becomes the printing surface.

[0028] 1 and 2 show an example in which the base layer 1 is made of a single material (single layer), but the structure of the base layer 1 may be a multi-layer structure in which different materials are laminated in multiple layers, so long as the maximum height on the surface is 10 μm or more. Similarly, in FIG. 1 and 2, an example in which the surface layer 2 is made of a single material (single layer) is shown, but the structure of the surface layer 2 may be a multi-layer structure in which different materials are laminated in multiple layers, so long as the maximum height on the surface is 10 μm or more. 3As long as the film has a thickness of 100 / 100 or more, it may be a multilayer structure formed by laminating different materials in multiple layers. In addition, although a configuration in which the surface layer 2 is laminated directly on the base layer 1 (the base layer 1 and the surface layer 2 are adjacent to each other) is illustrated in Fig. 1 and Fig. 2, another layer such as an adhesive layer may be provided between the base layer 1 and the surface layer 2.

[0029] The laminate according to the present invention is suitably used as printing paper for labels, wrapping paper, posters, calendars, catalogs, advertisements, etc. That is, one embodiment of the laminate according to the present invention is printing paper. Here, "printing paper" refers to a paper obtained by forming a composition containing a synthetic resin into a film, that is, synthetic paper. Considering the above-mentioned applications, the thickness of the laminate is preferably 80 to 400 μm, more preferably 100 to 300 μm, and particularly preferably 120 to 250 μm.

[0030] The substrate layer and the surface layer constituting the laminate of the present invention will be described in detail below.

[0031] [1] Base material layer [1-1] Maximum height of base layer The laminate according to the present invention has a base layer. The base layer according to the present invention contains a thermoplastic resin, and the maximum height of its surface (the surface on which the surface layer is laminated) is 10 μm or more. In this specification, the "maximum height" refers to a value measured in accordance with JIS-B0601:2013.

[0032] The maximum height of the base layer according to the present invention is 10 μm or more, and in other embodiments, may be 12 μm or more, or may be 14 μm or more. Thus, according to the present invention, even when a base layer having a large maximum height is used, a laminate that is less likely to cause blank spots during printing can be provided.

[0033] From the viewpoint of easily reducing the maximum height of the laminate surface and more easily suppressing the occurrence of white spots, the smaller the maximum height of the base layer, the more preferable. For example, the maximum height of the base layer is preferably 30 μm or less, more preferably 25 μm or less, and particularly preferably 20 μm or less.

[0034] The substrate layer having the above maximum height may contain foreign particles (coarse particles), as described in detail below. As an example, the substrate layer may be formed from a thermoplastic resin composition containing coarse particles having a maximum particle diameter that is 3 to 30 times the thickness of the substrate layer (substrate film).

[0035] [1-2] Composition of the base layer (base film) [Thermoplastic resin] The base layer according to the present invention contains a thermoplastic resin. The "thermoplastic resin contained in the base layer" refers to a thermoplastic resin contained in the resin composition for forming the base layer, and is a resin that is in a molten state during the extrusion process when forming the base layer. The base layer according to the present invention preferably contains a thermoplastic resin as a main component. In this embodiment, the "main component" is preferably 40% by mass or more, more preferably 50% by mass or more, and particularly preferably 60% by mass or more, relative to the total mass of the entire base layer (the total mass of the entire base layer being 100% by mass). The upper limit of the content of the thermoplastic resin is not particularly limited, but may be 100% by mass or less.

[0036] From the viewpoint of effectively utilizing resources and reducing the environmental load, a preferred embodiment of the laminate according to the present invention is a laminate manufactured using recycled resin (PCR resin) containing coarse particles. Therefore, in one embodiment, the thermoplastic resin contained in the base layer preferably contains recycled resin. In this specification, the term "recycled resin" refers to a resin made by regenerating used plastic products, and is also called recycled plastic or PCR (Post-Consumer Recycle) resin. As described above, recycled resin often contains coarse particles as foreign matter. Since the recycled resin contains such coarse particles, when the base layer is formed, the coarse particles are also contained in the base layer, and a base layer having the above-mentioned maximum height is formed. In other words, the base layer having the above-mentioned maximum height may contain recycled resin and coarse particles derived from the recycled resin. Note that the coarse particles do not have to be derived from the recycled resin, and other components that can become coarse particles may be added to form the base layer.

[0037] The recycled resin contained in the base layer is not particularly limited as long as it is a thermoplastic resin, and examples thereof include thermoplastic resins such as polyolefin resins, polyester resins, polyamide resins, polystyrene resins, polyvinyl chloride resins, and polycarbonates. Among them, polyolefin resins are preferred from the viewpoint of water resistance and solvent resistance. That is, it is preferred that the recycled resin contains a polyolefin resin.

[0038] Suitable polyolefin-based resins include polypropylene-based resins, polyethylene-based resins, etc. That is, in one embodiment, the recycled resin preferably contains a polypropylene-based resin and / or a polyethylene-based resin.

[0039] Examples of polypropylene-based resins include propylene homopolymers (homopolypropylenes) and propylene copolymers mainly composed of propylene and copolymerized with α-olefins such as ethylene, 1-butene, 1-hexene, 1-heptene, 1-octene, and 4-methyl-1-pentene. The propylene-based copolymers may be binary or ternary or higher multi-component systems, and may be random or block copolymers.

[0040] The polyethylene resin has a density of, for example, 0.940 to 0.970 g / cm 3 High density polyethylene, with a density of 0.920-0.940g / cm 3 Medium density polyethylene, with a density of 0.900 to 0.920 g / cm 3 Examples of the thermoplastic resins include low-density polyethylene of about 1000 nm, copolymers mainly composed of ethylene and copolymerized with α-olefins such as propylene, butene, hexene, heptene, octene, and 4-methylpentene-1, maleic acid-modified ethylene-vinyl acetate copolymers, ethylene-vinyl acetate copolymers, ethylene-(meth)acrylic acid alkyl ester copolymers, ethylene-(meth)acrylic acid copolymers and metal salts thereof (metals include zinc, aluminum, lithium, sodium, potassium, and the like), ethylene-cyclic olefin copolymers, and maleic acid-modified polyethylene. The above thermoplastic resins may be used alone or in combination of two or more.

[0041] Among the above polyolefin resins, from the viewpoints of moldability and cost, it is more preferable that the recycled resin contains a propylene homopolymer (homopolypropylene) and / or high-density polyethylene.

[0042] The thermoplastic resin contained in the base layer may contain other thermoplastic resins in addition to the recycled resin. That is, the thermoplastic resin contained in the base layer may be only recycled resin, or may contain recycled resin and non-recycled resin (hereinafter also referred to as "resin other than recycled resin" or "virgin resin").

[0043] Specific examples of resins (virgin resins) other than recycled resins include those listed above as specific examples of recycled resins. Among them, from the viewpoint of water resistance and solvent resistance, the resins other than recycled resins preferably include polyolefin-based resins, more preferably polypropylene-based resins and / or polyethylene-based resins. Furthermore, from the viewpoint of moldability and cost, it is particularly preferable to include propylene homopolymers and / or high-density polyethylene.

[0044] In addition, the thermoplastic resin contained in the base layer as a resin other than the recycled resin is preferably the same type of thermoplastic resin as that of the surface layer described below. In this form, the adhesion between the surface layer and the base layer is excellent, and the durability of the laminate is improved.

[0045] The recycled resin and the resin other than the recycled resin (virgin resin) may be the same or different, but preferably contain the same type of thermoplastic resin. For example, when the base layer contains a virgin resin, and the type of the recycled resin is a propylene-based resin, the base layer preferably contains a propylene-based resin as the virgin resin. That is, it is preferable to form the base layer using a resin composition containing a recycled resin of a propylene-based resin and a virgin resin of a propylene-based resin.

[0046] The content of the recycled resin contained in the base layer according to the present invention is not particularly limited and can be appropriately selected according to the purpose. As an example, the content of the recycled resin is preferably 20% by mass or more, more preferably 35% by mass or more, and particularly preferably 50% by mass or more, based on the total mass of the entire base layer (the total mass of the base layer is 100% by mass). The upper limit of the content of the recycled resin is not particularly limited, but can be 100% by mass or less.

[0047] [Particles (coarse particles)] The base layer according to the present invention may contain particles with a large particle size (coarse particles). By containing coarse particles in this way, the maximum height of the surface of the base layer is likely to be within the above-mentioned predetermined range. As described above, when the thermoplastic resin contained in the base layer contains a recycled resin, the coarse particles derived from the recycled resin are often also contained in the base layer, so that the maximum height of the base layer surface tends to be large. In contrast, according to the present invention, even if a material containing such coarse particles (recycled resin) is used, it is possible to provide a laminate having high print quality by suppressing white spots. In this specification, the term "coarse particles" refers to particles having a large particle size relative to the thickness of the base layer, and as an example, the maximum particle size is 3 to 30 times the thickness of the base layer. In particular, when the thermoplastic resin constituting the base layer contains a recycled resin, the coarse particles derived from the recycled resin may be contained in the base layer. Although the quality of recycled resin is improving year by year, and the foreign matter contained therein tends to decrease and become finer, many of them still contain coarse particles with particle sizes of tens of μm to hundreds of μm. The maximum particle size of such coarse particles is, for example, 60 to 1200 μm, and another example, 100 to 900 μm. The particle size of the coarse particles in the base layer can be determined by observing a cross section of the base layer with a scanning electron microscope (SEM).

[0048] The type of coarse particles is not particularly limited, and may be, for example, various foreign matter contained in recycled resin. Such foreign matter includes various inorganic particles and organic particles (resin particles), and the shapes thereof include spherical, needle-like, plate-like, fibrous, and amorphous.

[0049] Examples of types of inorganic particles include calcium carbonate, talc, titanium oxide, metallic aluminum, and silica.

[0050] The organic particles include resin particles of a type different from the thermoplastic resin contained in the base layer. Note that such resin particles (organic particles) are not melted in the resin composition for forming the layer during the extrusion process when forming the base layer, and for example, when the thermoplastic resin contained in the base layer is a polyolefin resin, resin particles such as polyester resin and polyamide resin can be mentioned.

[0051] The content of the coarse particles contained in the base layer according to the present invention is preferably within the following range: the content of the coarse particles is preferably 0.1 to 30 mass%, more preferably 0.5 to 20 mass%, and particularly preferably 1 to 10 mass%, based on the total mass of the entire base layer (total mass of the base layer being 100 mass%).

[0052] [Pore forming material] The substrate layer according to the present invention may contain a pore-forming material to the extent that the strength is not impaired. When a layer (film) formed using a thermoplastic resin composition containing a pore-forming material is stretched at a predetermined temperature, a large number of fine pores are formed in the layer (film) with the pore-forming material as a nucleus. In this way, when the substrate layer is a stretched film, by containing a pore-forming material, pores are easily formed inside the substrate layer during the stretching process, and whiteness and opacity can be increased. In addition, it is possible to adjust the rigidity of the substrate layer. Thus, in one embodiment, the substrate layer can be a porous stretched layer (porous stretched film) containing a thermoplastic resin and a pore-forming material.

[0053] The pore-forming material may be the same as the inorganic filler and organic filler that can be contained in the surface layer described below. The pore-forming material may be used alone or in combination of two or more. The pore-forming material contained in the base layer and the inorganic filler and organic filler that can be contained in the surface layer described below in detail may be the same or different.

[0054] From the viewpoint of pore-forming ability, the content of the pore-forming material contained in the base layer according to the present invention is preferably 45 to 250 parts by mass, more preferably 60 to 200 parts by mass, even more preferably 75 to 150 parts by mass, and particularly preferably 100 to 150 parts by mass, relative to 100 parts by mass of the thermoplastic resin.

[0055] [Other ingredients (optional ingredients)] The base layer according to the present invention may contain other components (optional components) other than the above components, if necessary. Examples of such other components include known components such as antioxidants, light stabilizers, ultraviolet absorbers, crystal nucleating agents, antiblocking agents, plasticizers, slip agents such as fatty acid amides, dyes, pigments, release agents, and flame retardants. The other components (optional components) may be used alone or in combination of two or more.

[0056] From the viewpoint of improving durability outdoors, the base layer preferably contains an antioxidant, a light stabilizer, and the like.

[0057] Examples of the antioxidant include sterically hindered phenol-based antioxidants, phosphorus-based antioxidants, and amine-based antioxidants.

[0058] Examples of the light stabilizer include a sterically hindered amine light stabilizer, a benzotriazole light stabilizer, and a benzophenone light stabilizer.

[0059] The content of each of the antioxidant and the light stabilizer is not particularly limited, but is preferably within the range of 0.001 to 1 mass % relative to the total mass of the entire substrate layer (the total mass of the substrate layer being 100 mass %).

[0060] [1-3] Thickness of base layer (base film) The thickness of the substrate layer according to the present invention is not particularly limited, but in one embodiment, it is preferably 20 to 340 μm. As described above, the substrate layer has protrusions (unevenness) formed on its surface. Therefore, in this specification, the thickness of the substrate layer refers to the thickness excluding the height of the protrusions (the thickness of the portion where the protrusions are not formed). In other words, the thickness of the substrate layer refers to the thickness of the portion that does not include the coarse particles that form the protrusions.

[0061] As described later, when a laminate is manufactured by laminating a surface layer (surface film) and a base layer (base film), the thickness of the base layer is preferably 20 to 290 μm, more preferably 25 to 200 μm, even more preferably 30 to 150 μm, particularly preferably 30 to 100 μm, and most preferably 30 to 80 μm, in consideration of the productivity. When the thickness of the base layer is equal to or greater than the above lower limit, the thickness of the base layer is not too small relative to the particle diameter of the coarse particles, and as a result, the maximum height of the surface of the base layer is not too large. In addition, when a recycled resin is used for the base layer, the amount of recycled resin used per unit area of ​​the laminate increases, improving the value of the product as an environmentally friendly product. On the other hand, when the thickness of each layer is taken into consideration so that the laminate has the above-mentioned preferred thickness, the thickness of the base layer is set to the above upper limit or less, so that the surface layer can also be made sufficiently thick. Therefore, there is an advantage in that the Clark stiffness of the surface layer can be easily adjusted to a predetermined range because there is no need to make the surface layer excessively thin.

[0062] [2] Surface layer [2-1] Clark stiffness of surface layer The surface layer according to the present invention has a Clark stiffness of 10 cm 3 / 100 or more. In this specification, the term "Clark stiffness" refers to a value measured in accordance with JIS P 8143:2009. The largest Clark stiffness value among the Clark stiffness values ​​in each in-plane direction of the surface layer is taken as the Clark stiffness value of the surface layer. For example, when the surface layer is a uniaxially stretched film, it corresponds to the Clark stiffness in the machine direction (MD), when the surface layer is a biaxially stretched film, it corresponds to the larger of the MD direction or the direction perpendicular thereto (TD), and when the surface layer is a non-stretched film, it corresponds to the Clark stiffness in the MD direction.

[0063] The surface layer according to the present invention is made of a film, and the film (surface film) has a Clark stiffness of 10 cm 3 The Clark stiffness of the surface layer is 10 cm 3 By setting the ratio to 40 cm or more, the maximum height of the laminate surface caused by the protrusions on the surface of the base layer can be reduced, thereby suppressing white spots during printing, and also reducing kurtosis. 3 By setting the Clark stiffness of the surface layer to 13 cm or less, the surface layer has a suitable flexibility and can secure sufficient adhesion to the base layer having protrusions on the surface, which is preferable. 3 / 100 or more is preferable, and 20cm 3 From the viewpoint of further increasing the adhesion between the base layer and the surface layer, the Clark stiffness of the surface layer is preferably 35 cm 3 / 100 or less is preferable, 32cm 3 It is more preferable that the ratio is less than or equal to 100.

[0064] That is, in one embodiment, the surface layer has a Clark stiffness of 10 to 40 cm 3 It is preferable that the film has a Clark stiffness of 13 to 35 cm. 3 It is more preferable that the film has a Clark stiffness of 20 to 32 cm. 3 A film of 1 / 100 is particularly preferred.

[0065] The Clark stiffness of the surface layer (surface film) constituting the laminate can be obtained by measuring the surface layer (surface film) after it has been separated (peeled) from the base layer and is left in the form of only the surface layer (surface film).

[0066] [2-2] Thickness of surface layer (surface film) The thickness of the surface layer according to the present invention is not particularly limited, but is appropriately selected so as to satisfy the above Clark stiffness depending on the type of resin composition used to form the layer. In one embodiment, the thickness of the surface layer is preferably 30 to 80 μm. By setting the thickness of the surface layer within the above range, the conformability to the surface of the base layer having protrusions is improved. In addition, the surface layer (surface film) can be easily attached to the base layer. In still another embodiment, the thickness of the surface layer is preferably 40 to 70 μm.

[0067] [2-3] Structure of the surface layer (surface film) The surface layer according to the present invention is composed of a film. The film (surface film) constituting the surface layer may be a stretched film or a non-stretched film, but is preferably a stretched film from the viewpoint of ensuring a predetermined Clark stiffness. By using a stretched film, it becomes easy to make a surface film having a predetermined Clark stiffness while having a thinner thickness. When a recycled resin is used for the base layer, the proportion of the recycled resin in the entire laminate can be increased. Therefore, it is possible to form a thinner laminate while increasing the content ratio of the recycled resin. In addition, the form of stretching may be uniaxial stretching or biaxial stretching.

[0068] The structure of the surface layer (surface film) according to the present invention is not particularly limited, and may be a single-layer structure or a multi-layer structure consisting of two or more layers. From the viewpoint of facilitating the formation of a surface layer (surface film) having a predetermined Clark stiffness, it is preferable that the surface film has a multi-layer structure. As an example, the surface film may have a three-layer structure of surface layer (i) / base layer / surface layer (ii). According to such an embodiment, the base layer can impart suitable stiffness, opacity, lightness, etc. to the laminate. In addition, the surface layer (i) and the surface layer (ii) may have the same surface structure or different surface structures. For example, one surface layer (surface layer (i; the surface to be laminated with the base layer) may have a surface structure (i.e., a highly flexible surface structure) that has excellent adhesion to the above-mentioned base layer and is suitable for mitigating (absorbing) the maximum height of the surface of the base layer, and the other surface layer (surface layer (ii; the surface opposite to the surface to be laminated with the base layer) may have a surface structure suitable as a printing surface, thereby obtaining a laminate with better printability. More specifically, the surface layer (ii) may be an opaque print-receiving layer, or the surface layer (ii) may be made opaque by making it a porous layer, making it suitable as a printing surface.

[0069] Furthermore, from the viewpoint of easily forming a surface layer (surface film) having a predetermined Clark stiffness, in the case of a multi-layer structure of the surface film, it is preferable that at least one layer is stretched. From the same viewpoint, a suitable example of the multi-layer structure is a multi-layer structure in which a uniaxially stretched layer / biaxially stretched layer / uniaxially stretched layer are laminated in this order. In this way, by including a biaxially stretched layer, it is easy to obtain a surface layer (surface film) having a large Clark stiffness.

[0070] [2-4] Composition of the surface layer (surface film) The components constituting the surface layer (surface film) are not particularly limited, but are appropriately selected so as to satisfy the above Clark stiffness. In order to easily satisfy the above Clark stiffness, in a preferred embodiment, the surface layer contains a thermoplastic resin. From the same viewpoint, in a preferred embodiment, the surface layer contains a thermoplastic resin, and an inorganic filler and / or an organic filler.

[0071] [Thermoplastic resin] The thermoplastic resin contained in the surface layer preferably contains a resin other than the recycled resin, i.e., a virgin resin, and more preferably is a virgin resin. The surface layer (surface film) formed by the virgin resin has an advantage that it not only has a smooth surface, but also tends to have a large Clark stiffness compared to the case where the recycled resin is used. Therefore, it is preferable that the thermoplastic resin contained in the surface layer does not substantially contain recycled resin. Here, "substantially does not contain recycled resin" means that recycled resin is not blended at least intentionally, and it is acceptable that a small amount of recycled resin is inevitably included due to raw materials, manufacturing method, etc. The above-mentioned small amount means that the content of recycled resin is 1 mass % or less (preferably 0.5 mass % or less, more preferably 0.1 mass % or less) with respect to the total mass 100 mass % of the thermoplastic resin. In a preferred embodiment, the thermoplastic resin contained in the surface layer does not contain recycled resin (the content of recycled resin is 0 mass %).

[0072] Specific examples of the thermoplastic resin contained in the surface layer include the same resin as the thermoplastic resin contained in the base layer, and the thermoplastic resin can be used alone or in combination of two or more. Among them, from the viewpoint of water resistance and solvent resistance, it is preferable that the surface layer contains a polyolefin resin. Furthermore, from the viewpoint of moldability and cost, it is more preferable that the surface layer contains a propylene homopolymer and / or a high density polyethylene.

[0073] In addition, the thermoplastic resin contained in the surface layer is preferably the same type as the thermoplastic resin (preferably recycled resin) contained in the above-mentioned substrate layer. In such a form, the adhesion (adhesiveness) between the surface layer and the substrate layer is excellent, and the durability of the laminate is improved. Furthermore, in such a form, as described later, when the laminate is produced by a thermal lamination method, the adhesion (adhesiveness) is particularly improved. For example, when the substrate layer contains a polyolefin-based resin, it is preferable that the surface layer also contains a polyolefin-based resin. Furthermore, as another example, when the substrate layer contains a propylene-based resin, it is preferable that the surface layer also contains a propylene-based resin. Furthermore, as another example, when the substrate layer contains a propylene-based resin, and the surface layer has a three-layer structure of the above-mentioned surface layer (i) / base layer / surface layer (ii), and when the surface layer (i) is a layer laminated with the substrate layer (when the surface layer (i) is a layer facing the substrate layer), it is preferable that the surface layer (i) also contains a propylene-based resin. Furthermore, as another example, when the base layer contains high-density polyethylene and the surface layer has a three-layer structure of surface layer (i) / base layer / surface layer (ii) as described above, and surface layer (i) is a layer that is laminated with the base layer (when surface layer (i) is a layer facing the base layer), it is preferable that surface layer (i) also contains high-density polyethylene.

[0074] The content of the thermoplastic resin contained in the surface layer according to the present invention is not particularly limited, but the surface layer preferably contains a thermoplastic resin as a main component. In this embodiment, the "main component" preferably has a ratio of 40% by mass or more, more preferably 50% by mass or more, and particularly preferably 60% by mass or more, based on the total mass of the entire surface layer (the total mass of the surface layer being 100% by mass). The upper limit of the content of the thermoplastic resin is not particularly limited, but may be 100% by mass or less.

[0075] [Inorganic and organic fillers] The surface layer is preferably a film containing an inorganic filler and / or an organic filler. The inclusion of a filler tends to improve the Clark stiffness of the surface layer, for example, due to the effects of overlapping of plate-like fillers and formation of voids by spherical fillers during stretching.

[0076] In addition, the surface layer according to the present invention is a layer on which printing is performed. Therefore, in order to improve the visibility of the print, the surface layer is preferably opaque. From the viewpoint of forming an opaque surface layer, the surface layer preferably contains an inorganic filler and / or an organic filler in addition to the above-mentioned thermoplastic resin. When a thermoplastic resin composition for forming a surface layer containing a thermoplastic resin and an inorganic filler and / or an organic filler is melt-kneaded and extrusion-molded into a film, and then stretched, a large number of fine pores with the inorganic filler and / or organic filler as cores can be formed inside the film (a porous layer). This allows the formation of an opaque surface layer.

[0077] The type of inorganic filler is not particularly limited as long as it can whiten and opaque the surface layer (surface film).Specific examples of inorganic fillers include heavy calcium carbonate, light calcium carbonate, calcined clay, talc, diatomaceous earth, barium sulfate, magnesium oxide, aluminum oxide (alumina), zinc oxide, titanium dioxide, and silicon dioxide (silica).Furthermore, these may be surface-treated with fatty acid, polymer surfactant, antistatic agent, etc.

[0078] The type of organic filler is also not particularly limited. The organic filler is incompatible with the thermoplastic resin contained in the surface layer, and can be one having a melting point or glass transition temperature higher than the melting point of the thermoplastic resin contained in the surface layer. In addition, the organic filler is preferably one that is finely dispersed under the melt-kneading conditions of the thermoplastic resin constituting the surface layer. For example, when the thermoplastic resin constituting the surface layer is a polyolefin resin, examples of the organic filler include polyethylene terephthalate, polybutylene terephthalate, polyethylene naphthalate, polystyrene, polyamide, polycarbonate, nylon-6, nylon-6,6, polyethylene sulfide, polyphenylene sulfide, polyimide, polyether ketone, polyether ether ketone, polymethyl methacrylate, poly-4-methyl-1-pentene, homopolymers of cyclic olefins, and copolymers of cyclic olefins and ethylene, which have a melting point of 120 to 300°C or a glass transition temperature of 120 to 280°C. Alternatively, fine powder of a thermosetting resin such as melamine resin may be used. It is also preferable to crosslink the thermoplastic resin to make it infusible. In this specification, the melting point and glass transition temperature of the resin are intended to be values ​​measured by differential scanning calorimetry (DSC) in accordance with JIS K 7121:1987.

[0079] Among them, from the viewpoint of easy adjustment of particle size distribution, inorganic fillers are preferred as the filler contained in the surface layer.Furthermore, as the inorganic filler, calcium carbonate such as heavy calcium carbonate and light calcium carbonate, calcined clay, and talc are preferred because they have good pore forming properties and are inexpensive.Furthermore, it is also preferred to use titanium dioxide, zinc oxide, and barium sulfate in order to improve whiteness and opacity.

[0080] The inorganic fillers and organic fillers may be used alone or in combination of two or more. When two or more types are combined, the combination may be an inorganic filler and an organic filler.

[0081] The average particle size of the inorganic filler and the average dispersed particle size of the organic filler are preferably 0.01 to 30 μm, more preferably 0.1 to 20 μm, and further preferably 0.2 to 10 μm.

[0082] The average particle size of the inorganic filler can be, for example, the particle size corresponding to 50% cumulative on a volume basis (50% cumulative particle size) measured using a particle measuring device, for example, a laser diffraction particle measuring device "Microtrac" (manufactured by Nikkiso Co., Ltd.) Alternatively, the particle size of the organic filler dispersed in the thermoplastic resin by melt kneading and dispersion can be determined by measuring the maximum diameters of at least 10 particles by observing the cut surface of the surface layer (surface film) with an electron microscope, and averaging the maximum diameters to obtain the particle size.

[0083] When the surface layer (surface film) contains an inorganic filler and / or an organic filler, the content of the inorganic filler and the organic filler (the total content when two or more types are contained) is, from the viewpoint of making it easier to set the Clark stiffness of the surface layer (surface film) within a predetermined range and from the viewpoint of pore formability in the layer, preferably 20 to 250 parts by mass, more preferably 50 to 200 parts by mass, even more preferably 75 to 150 parts by mass, and particularly preferably 100 to 150 parts by mass, relative to 100 parts by mass of the thermoplastic resin.

[0084] [Other ingredients (optional ingredients)] The surface layer according to the present invention may contain other components (optional components) other than the above components, if necessary. Examples of such other components include the same optional components that may be contained in the above-mentioned base layer. The other components (optional components) may be used alone or in combination of two or more.

[0085] Among the above, from the viewpoint of enhancing durability outdoors, the surface layer preferably contains an antioxidant, a light stabilizer, etc. Examples of the antioxidant and the light stabilizer include the same antioxidant and the light stabilizer that can be contained in the above-mentioned base layer. The content of each of the antioxidant and the light stabilizer is not particularly limited, but is preferably within the range of 0.001 to 1 mass% with respect to the total mass of the entire surface layer (the total mass of the surface layer being 100 mass%). These are preferably added within a range that does not inhibit adhesion between the surface layer and the base layer.

[0086] [2-5] Porosity of the surface layer (surface film) As described above, when the surface layer (surface film) contains an inorganic filler and / or an organic filler in addition to a thermoplastic resin, pores may be formed inside the layer (film). The formation of such pores can impart opacity and lightness to the surface layer (surface film). The proportion of pores in the film can be expressed as the porosity.

[0087] From the viewpoint of obtaining opacity, the porosity of the surface layer (surface film) is preferably 10% or more, more preferably 12% or more, even more preferably 15% or more, and particularly preferably 20% or more. On the other hand, the porosity of the surface layer (surface film) is 10 cm Clark stiffness. 3 From the viewpoint of easily achieving a ratio of 100 to 100 and improving the mechanical strength, the ratio is preferably 60% or less, more preferably 57% or less, even more preferably 54% or less, and particularly preferably 50% or less.

[0088] The porosity of the surface layer (surface film) can be measured by observing the cross section of the surface layer (surface film) with an electron microscope, and determining the ratio of the area occupied by pores in the observed region. Specifically, an arbitrary part is cut from a surface layer (surface film) sample, embedded in epoxy resin and solidified, and then a cut surface perpendicular to the surface direction of the film is prepared using a microtome, and the cut surface is attached to an observation sample stage so that it becomes the observation surface, and gold or gold-palladium, etc. is evaporated on the observation surface, and the pores on the surface are observed at an arbitrary magnification (for example, 500 times to 3000 times magnification) that is easy to observe with an electron microscope, and the observed region is captured as image data, and the image is processed by an image analyzer to determine the area ratio of the pores, which can be determined as the porosity. In this case, the measured values ​​in the observation of any 10 or more points can be averaged to determine the porosity.

[0089] <<Method for manufacturing laminate>> The method for producing a laminate according to the present invention comprises the steps of: forming a laminate having a Clark stiffness of 10 cm on at least one surface of a base layer having a maximum height of 10 μm or more; 3 There are no particular limitations as long as it is possible to laminate a surface layer that is a film having a thickness of 100 mm or more. From the viewpoint of further reducing the maximum height and further improving the effect of suppressing white spots, it is preferable that the laminate according to the present invention is produced by laminating a base layer having the above-mentioned configuration and a surface layer (surface film) having the above-mentioned configuration.

[0090] That is, in a preferred embodiment, the method for producing a laminate according to the present invention comprises the steps of: forming a laminate having a Clark stiffness of 10 cm on at least one surface of a base film containing a thermoplastic resin and having a maximum height of 10 μm or more; 3 The present inventors have also surprisingly found that a laminate obtained by such a method (the manufacturing method according to the present invention) can suppress the occurrence of blank spots during printing.

[0091] The above Patent Documents 1 and 2 disclose a technique for producing a laminate by forming a specific surface layer on the surface of a layer containing coarse particles (i.e., a layer corresponding to the base film according to the present invention) by coextrusion molding or extrusion lamination. With regard to such a technique, the present inventors considered that, although the kurtosis (pointedness) of the protrusions appearing on the surface of the laminate is reduced compared to the protrusions occurring on the surface of the base layer, it would be desirable to further reduce the maximum height.

[0092] When the surface layer is formed by the co-extrusion molding or extrusion lamination method disclosed in Patent Document 1 and Patent Document 2, the resin forming the surface layer is laminated on the surface of the base layer in a soft state (molten state). In this case, the surface layer is formed in a state in which the resin forming the surface layer follows the unevenness of the surface of the base layer, and the effect of mitigating the unevenness of the surface of the base layer is reduced. In other words, the unevenness of the surface of the base layer is easily maintained on the surface of the laminate. In contrast, according to the manufacturing method of the present invention, a surface film having a specific Clark stiffness is bonded to a base layer having a large maximum height, so that the resin does not melt as described above, and therefore the effect of mitigating the unevenness of the surface of the base layer is excellent. Therefore, the laminate obtained by the manufacturing method of the present invention can suppress white spots during printing. Note that the above mechanism is speculation and does not limit the technical scope of the present invention in any way.

[0093] The manufacturing method according to the present invention will be described in detail below. The manufacturing method according to the present invention includes laminating the above-mentioned base film and the above-mentioned surface film (laminating step), but may further include manufacturing the base film (base film manufacturing step) and manufacturing the surface film before the laminating step. Each of these steps will be described below.

[0094] [1] Manufacturing process of base film (manufacturing method) The substrate film can be produced by using various known methods as is or with appropriate modifications, and the forming method is not particularly limited. The substrate film produced by any method is within the scope of the present invention as long as it does not deviate from the spirit of the present invention.

[0095] [1-1] Preparation of thermoplastic resin composition for base film In a preferred embodiment, the substrate film is produced using a thermoplastic resin composition for substrate film (thermoplastic resin composition for substrate layer) containing a thermoplastic resin (preferably a recycled resin) and coarse particles. The thermoplastic resin composition for substrate film can be obtained, for example, from a recycled resin raw material, or by mixing a recycled resin raw material with a virgin resin raw material. In this case, the pore-forming material and / or the optional component may be further added and mixed, if necessary. Here, the recycled resin raw material may be a commercially available recycled resin pellet, or may be a granular material obtained by crushing a molded product containing a thermoplastic resin (for example, synthetic paper, etc.). In addition, an example of a virgin resin raw material is a commercially available virgin resin pellet.

[0096] The mixing is preferably carried out by melt kneading, and the heating conditions are not particularly limited, and conventionally known techniques such as melt extrusion can be appropriately referred to. The heating temperature may be equal to or higher than the melting point of the thermoplastic resin (preferably recycled resin) and lower than the temperature at which the resin starts to deteriorate or decompose, for example, 180 to 300° C., and preferably 200 to 280° C. The heating time may be sufficient to melt the resin.

[0097] In one embodiment, the thermoplastic resin composition for a base film may contain recycled resin and coarse particles. In such a form, the maximum height of the base film (base layer) is likely to be within the above-mentioned predetermined range. Here, in one embodiment, the coarse particles may have a maximum particle diameter of 3 to 30 times the thickness of the base film. In this way, when the maximum particle diameter of the coarse particles in the base film is 3 to 30 times the thickness of the base film, the maximum height of the base film is likely to be within the above-mentioned predetermined range.

[0098] That is, in one embodiment of the manufacturing method according to the present invention, the thickness of the base film is 20 to 340 μm, the base film contains a thermoplastic resin (recycled resin) and particles (coarse particles), and the maximum particle diameter of the particles (coarse particles) can be 3 to 30 times the thickness of the base film. In yet another embodiment, the thickness of the base film is 30 to 80 μm, and the maximum particle diameter of the particles (coarse particles) contained in the base film can be 3 to 30 times the thickness of the base film. In this way, when the maximum particle diameter of the coarse particles and the thickness of the base film have the above-mentioned relationship, the maximum height of the surface of the base film (base layer) is likely to be within the above-mentioned predetermined range. In addition, in such a case, the maximum particle diameter of the coarse particles is, for example, 60 to 1200 μm, and another example, 100 to 900 μm. The maximum particle diameter of the coarse particles contained in the thermoplastic resin composition for the base film is determined by the following method.

[0099] (Method for measuring maximum particle size of coarse particles) 50 g of a thermoplastic resin composition for a base film containing coarse particles is pressed for 5 minutes at a temperature 70°C higher than the melting point of the main component resin in the resin composition, with a press pressure of 15 MPa, so that the sheet thickness becomes 300 μm. The sheet obtained by pressing as described above is then cooled at 20°C for 2 minutes to obtain a pressed sheet having a thickness of 300 μm, and a 90 mm x 90 mm piece is cut out from the pressed sheet. The pressed sheet cut out is held for 2 minutes in an oven set at a temperature 20°C higher than the melting point of the main component resin of the pressed sheet, and stretched 4 times in both length and width to obtain a stretched sheet sample having a thickness of 20 μm. For three of the stretched sheet samples, the particle diameter of the coarse particles contained in the sample is measured using a digital microscope with transmitted light. The measured particle diameter values ​​are rounded off to the nearest 10 μm, and the number of particles corresponding to the 100 μm diameter, 200 μm diameter, etc. is tallied in units of 100 μm. The number of particles is divided by the number of samples, which is 3, and the largest particle size among those that is 0.5 particles / sheet or more is defined as the "maximum particle size."

[0100] In the above, "main component resin" means the resin with the largest content among the thermoplastic resins contained in the thermoplastic resin composition for the base film, and if the total mass of the thermoplastic resins contained in the thermoplastic resin composition for the base film is 100 mass%, the proportion is preferably 50 mass% or more, more preferably 80 mass% or more, even more preferably 90 mass% or more, particularly preferably 95 mass% or more, and most preferably 99 mass% or more.

[0101] [1-2] Forming of base film The base film is not particularly limited, but can be formed as a film layer containing a thermoplastic resin, etc., using a method such as cast molding, calendar molding, rolling molding, inflation molding, etc., in which the molten resin composition for the base film (molten resin) is extruded into a sheet shape using a single-layer or multi-layer T-die, I-die, etc. connected to a screw-type extruder.

[0102] [1-3] Stretching of base film The substrate film may be a non-stretched film or a stretched film. When a stretched film is used, the substrate film may be stretched before laminating (bonding) the surface film, or may be stretched after laminating (bonding). There is no particular limitation on the stretching method, and a known method may be used.

[0103] [2] Surface film manufacturing process (manufacturing method) The surface film can be produced by using various known methods as is or with appropriate modifications, and the molding method is not particularly limited. Any surface film produced by any method is within the scope of the present invention as long as it does not deviate from the spirit of the present invention.

[0104] [2-1] Preparation of thermoplastic resin composition for surface film In a preferred embodiment, the surface film is produced using a thermoplastic resin composition for a surface film (thermoplastic resin composition for a surface layer) containing a thermoplastic resin. In another preferred embodiment, the surface film is produced using a thermoplastic resin composition for a surface film (thermoplastic resin composition for a surface layer) containing a thermoplastic resin and an inorganic filler and / or an organic filler. The thermoplastic resin composition for a surface film can be obtained, for example, from a thermoplastic resin or by mixing a thermoplastic resin with an inorganic filler and / or an organic filler. In this case, the above-mentioned optional components may be further added and mixed as necessary.

[0105] The mixing is preferably carried out by melt kneading, and the heating conditions are not particularly limited, and conventionally known techniques such as melt extrusion can be appropriately referred to. The heating temperature may be equal to or higher than the melting point of the thermoplastic resin and lower than the temperature at which the resin starts to deteriorate or decompose, for example, 180 to 300° C., and preferably 200 to 280° C. The heating time may be sufficient to melt the resin.

[0106] [2-2] Forming the surface film The method for forming the surface film is not particularly limited, and examples thereof include cast molding in which the molten thermoplastic resin composition for the surface film (molten resin) is extruded into a sheet shape using a single-layer or multi-layer T-die, I-die, etc. connected to a screw-type extruder, calendar molding, rolling molding, inflation molding, etc. The surface film may also be formed using a method in which a mixture of the thermoplastic resin composition for the surface film and an organic solvent or oil is cast or calendar molded, and then the solvent or oil is removed.

[0107] [Multi-layer surface film] As mentioned above, the surface film may have a multi-layer structure consisting of two or more layers. When forming the surface film into a multi-layer structure, various known methods can be used, and specific examples include a multi-layer die method using a feed block or a multi-manifold, and an extrusion lamination method using multiple dies. It is also possible to use a combination of a multi-layer die and extrusion lamination.

[0108] [2-3] Stretching of surface film As described above, the surface film is preferably a stretched film (stretched film). As a method for stretching the film, various conventionally known methods can be used, and the method is not particularly limited.

[0109] For example, the thermoplastic resin composition for the surface film is melt-kneaded using a screw-type extruder, and the molten resin is extruded using a T-die or I-die connected to the extruder to form a sheet, and then the sheet is stretched to obtain a resin film. As the stretching method, a roll-to-roll longitudinal stretching method using the difference in peripheral speed between rolls, a transverse stretching method using a tenter oven, and a sequential biaxial stretching method combining these can be used. In addition, a rolling method, a simultaneous biaxial stretching method using a combination of a tenter oven and a pantograph, and a simultaneous biaxial stretching method using a combination of a tenter oven and a linear motor can be used. Furthermore, a simultaneous biaxial stretching (inflation molding) method can be used in which the molten resin is extruded and molded into a tube shape using a circular die connected to a screw-type extruder, and then air is blown into the extruded resin.

[0110] As described above, when the surface film has a multi-layer structure, it is preferable that at least one layer is stretched. When stretching multiple layers, each layer may be stretched individually before lamination, or may be stretched together after lamination. Also, the stretched layer may be stretched again after lamination.

[0111] The stretching of the surface film is preferably carried out within a temperature range suitable for the thermoplastic resin contained in the film. When the thermoplastic resin used in the film is a non-crystalline resin, the stretching temperature of the surface film is preferably in a range equal to or higher than the glass transition temperature of the thermoplastic resin. When the thermoplastic resin used in the film is a crystalline resin, the stretching temperature is preferably in a range equal to or higher than the glass transition temperature of the non-crystalline part of the thermoplastic resin and equal to or lower than the melting point of the crystalline part of the thermoplastic resin. Specifically, the stretching temperature of the surface film is preferably 2 to 60°C lower than the melting point of the thermoplastic resin contained in the film.

[0112] The stretching speed when stretching the surface film is not particularly limited, but is preferably within the range of 20 to 350 m / min in order to stably perform film stretching. The stretching ratio when stretching the surface film is not particularly limited, and is appropriately determined in consideration of the properties of the thermoplastic resin used in the film.

[0113] For example, when a film containing a propylene homopolymer or a propylene copolymer as a thermoplastic resin is stretched in one direction, the stretching ratio is preferably about 1.2 times or more, more preferably 2 times or more, and the stretching ratio is preferably 12 times or less, more preferably 10 times or less. On the other hand, when the film is stretched biaxially, the stretching ratio is preferably 1.5 times or more, more preferably 10 times or more, in terms of areal stretching ratio, and the stretching ratio is preferably 60 times or less, more preferably 50 times or less.

[0114] Within the above range of stretching ratio, it becomes easy to control the Clark stiffness of the surface film within the above range, and the opacity of the film with voids formed therein tends to be improved. In addition, the surface film is less likely to break, and stable stretching tends to be possible.

[0115] [2-4] Surface oxidation treatment of surface film The surface film may be subjected to a surface oxidation treatment on its surface, which corresponds to the outermost layer of the laminate, before or after lamination with the base film to form a laminate. By performing the surface oxidation treatment, the adhesion of various printing inks is improved, and the printability is improved when the laminate according to the present invention is applied to various applications.

[0116] The surface oxidation treatment may be a treatment method selected from corona discharge treatment, flame treatment, plasma treatment, glow discharge treatment, ozone treatment, or a combination of these.

[0117] When performing the surface oxidation treatment, it is preferable to perform a corona discharge treatment or a flame treatment. When performing the corona discharge treatment, the treatment amount is preferably 600 to 12,000 J / m 2 (10~200W min / m 2 ), and more preferably 1,200 to 10,800 J / m 2 (20~180W min / m 2 ).

[0118] [2-5] Clark stiffness control A surface film having a Clark stiffness within the above-mentioned specified range can be manufactured as appropriate by a person skilled in the art. As an example, it is effective to appropriately select the thickness of the surface film, the type of thermoplastic resin contained in the surface film, the content of inorganic filler and / or organic filler, whether or not to stretch, etc., and it is preferable to set at least one, or even two, or even all of these to be within the above-mentioned preferred ranges and forms.

[0119] Clark stiffness is calculated as the cube of the critical length (cm) divided by 100, and the critical length is proportional to the film's elastic modulus (E) and the cube of its thickness (h), and inversely proportional to its weight (W). Note that the weight (W) here is the weight corresponding to the critical length, and is the product of the film's specific gravity and volume.

[0120] Therefore, the Clark stiffness increases when the thickness (h) or modulus of elasticity (E) of the film is increased, and the Clark stiffness also increases when the specific gravity of the film is decreased. In this case, in order to increase the modulus of elasticity, a crystalline resin with a large modulus of elasticity may be used as the thermoplastic resin constituting the surface film, or the film may be stretched. In addition, in order to decrease the specific gravity of the film, a method may be used in which the content of inorganic filler and / or organic filler is decreased, or the porosity of the film is increased appropriately by controlling the stretching ratio.

[0121] On the other hand, the Clark stiffness decreases when the thickness (h) or modulus of elasticity (E) of the film is reduced, and the Clark stiffness also decreases when the specific gravity of the film is increased. In this case, in order to reduce the modulus of elasticity, a thermoplastic elastomer with a low modulus of elasticity may be used as the thermoplastic resin constituting the surface film, or the film may be made non-stretched. In addition, in order to increase the specific gravity of the film, a method may be used in which the content of inorganic filler and / or organic filler is increased, or the porosity of the film is appropriately reduced by controlling the stretching ratio.

[0122] [2-6] Other properties of the surface film [Maximum height of surface film] From the viewpoint of effectively reducing the maximum height of the laminate, the surface film (surface layer) according to the present invention preferably has a maximum surface height (maximum height before forming the laminate) smaller than the maximum surface height of the base layer. In one embodiment, the maximum surface height of the surface film is preferably less than 8 μm, preferably 6 μm or less, and more preferably 5 μm or less. On the other hand, the lower limit of the maximum surface height of the surface film is not particularly limited, but is, for example, 0.1 μm or more.

[0123] [Kurtosis of surface film] From the viewpoint of effectively reducing the kurtosis of the laminate, the surface film (surface layer) according to the present invention preferably has a surface kurtosis (kurtosis before forming the laminate) smaller than the kurtosis of the base layer. In one embodiment, the surface kurtosis of the surface film is preferably less than 8, preferably 6 or less, and more preferably 4 or less. In this specification, "kurtosis" refers to a value measured by the method described in the examples.

[0124] [3] Lamination process (lamination method) The method for laminating the substrate film and the surface film prepared as described above is not particularly limited, and a known method can be used as is or with appropriate modifications. In the lamination step, the surface film may be laminated to one side of the substrate film (the embodiment in FIG. 1) or to both sides of the substrate film (the embodiment in FIG. 2).

[0125] As a specific lamination method, the following method (1) or (2) is preferable.

[0126] (1) First, the above-mentioned thermoplastic resin composition for the base film is melt-kneaded in an extruder, and then the resin composition is extruded into a sheet shape by an extrusion die to form a base film (base layer). Next, while the above-mentioned resin composition (at least its surface) is still in a molten state (softened state), the above-mentioned surface film is pressure-welded (thermal lamination method); (2) First, the base film and the surface film are prepared according to the method described above, and then these films are bonded together using a hot melt adhesive or a solvent-based adhesive (adhesion method).

[0127] [3-1] Thermal lamination method As the above method (1), that is, the thermal lamination method, a known method can be used as is or with appropriate modifications.

[0128] In this method, the base film and the surface film are sandwiched between a pair of rolls, and these films are transported while at least one of the rolls is rotated. At least one of the rolls is a heating roll, and the films are bonded (thermocompression bonded) while being heated.

[0129] Specifically, it is preferable to form a base film (base layer) as a cast film using the thermoplastic resin composition for base film, and heat the base film using a heating roll while thermocompression bonding (pressure welding) to the surface film. In this case, the details of the method for forming the base film (base layer) are referred to the above item [1] Manufacturing process (manufacturing method) of the base film. In addition, the heating method of the heating roll is not particularly limited, and a known method can be adopted. In addition, the material of the heating roll is not particularly limited, and a metal roll, a rubber roll, etc. can be used.

[0130] The roll temperature during thermocompression bonding may be equal to or higher than the melting point of the thermoplastic resin constituting the base film and lower than the temperature at which the resin starts to deteriorate or decompose, and is preferably, for example, 30 to 95° C., and more preferably 50 to 85° C. If the roll temperature is equal to or higher than the lower limit, the adhesion between the films can be further improved, and if it is equal to or lower than the upper limit, deformation due to melting of the surface film can be suppressed.

[0131] The processing speed during thermocompression bonding is preferably 0.5 to 100 m / min, and more preferably 3 to 30 m / min. If the processing speed is equal to or higher than the lower limit, the productivity is improved, and if it is equal to or lower than the upper limit, the adhesion between the films can be further improved.

[0132] Furthermore, the pressure conditions during thermocompression bonding are preferably 3 to 15 MPa, and more preferably 5 to 10 MPa. If the pressure conditions are equal to or higher than the lower limit, the adhesion between the films can be further improved, and if the pressure conditions are equal to or lower than the upper limit, deformation of the surface film can be suppressed.

[0133] Among the above methods (1) and (2), the above method (1) (thermal lamination method) is preferred from the viewpoints of low environmental impact and fewer steps (i.e., excellent productivity). That is, a preferred embodiment of the production method according to the present invention includes laminating a surface film while the surface of the base film is in a molten state.

[0134] [3-2] Adhesion method As the above method (2), that is, the adhesion method, a known method can be used as is or with appropriate modifications.

[0135] The hot melt adhesive and solvent-based adhesive used in this case can be appropriately selected from known adhesives, and for example, the adhesives described in JP-A-8-332690 can be used. The form of adhesion using a hot melt adhesive is not particularly limited, and may be a form in which a hot melt adhesive layer is provided on the surface of a base film by co-extrusion and a surface film is bonded to the hot melt adhesive layer, or a form in which a surface film provided with a hot melt adhesive layer in advance is prepared and a surface film is bonded to the hot melt adhesive layer provided on the surface film.

[0136] Although the embodiments of the present invention have been described in detail, it is apparent that the same are illustrative and exemplary, not restrictive, and the scope of the present invention should be interpreted by the appended claims. EXAMPLES

[0137] The effects of the present invention will be described using the following examples and comparative examples. The following manufacturing examples, materials, amounts used, ratios, processing contents, processing procedures, etc. shown in the examples can be appropriately changed without departing from the spirit of the present invention. Therefore, the technical scope of the present invention is not limited only to the following examples. In the following examples, the indications "parts" or "%" may be used, but unless otherwise specified, they represent "parts by mass" or "% by mass". In addition, the ratios of the amounts of raw materials used as a solution or dispersion (units: "parts by mass", "% by mass") are all values ​​converted into solid content. Unless otherwise specified, each operation was performed at room temperature (25°C). The melt flow rate (MFR) of the resin and resin composition was measured at a temperature of 230°C and a load of 2.16 kg according to JIS K 7210-1:2014.

[0138] [Example 1] 1. Preparation of the substrate layer The following was used as recycled resin raw material after user use: synthetic paper manufactured by Yupo Corporation (containing homopolypropylene as the main component and further containing inorganic filler) with oil-based printing was crushed and used as recycled resin raw material. The recycled resin raw material was melt-kneaded in an extruder at 220°C to prepare resin composition 1 for forming the base layer. The MFR of resin composition 1 was 5.5g / 10min.

[0139] This was then extrusion molded and cooled to 50°C in a cooling device to obtain a substrate layer (substrate film) that was a single-layered unstretched sheet. The thickness of the substrate layer was 30 μm. The maximum particle diameter of the coarse particles contained in the substrate layer was measured by the method described above and found to be 300 μm. The obtained substrate layer (substrate film) was evaluated for maximum surface height, kurtosis, the presence or absence of white spots, and transition concentration by the method described in [Test Example] below. The results are shown in Table 1.

[0140] 2. Surface Layer Preparation As the surface layer, a polyolefin-based synthetic paper (containing homopolypropylene as the main component and further containing inorganic filler, manufactured by Yupo Corporation) was prepared. The synthetic paper was a synthetic paper in which a uniaxially oriented layer / biaxially oriented layer / uniaxially oriented layer were laminated in this order, and had a thickness of 60 μm, a porosity of 40%, and a Clark stiffness (maximum Clark stiffness) of 30.5 cm. 3 The Clark stiffness was measured in accordance with JIS P 8143:2009 (hereinafter the same).

[0141] 3. Preparation of Laminate The synthetic paper (surface film) prepared as the surface layer in 2 above was thermally laminated (heat roll temperature: 85°C, processing speed: 3.0 m / min, pressure condition: 5.0 MPa) on both sides of the base layer (i.e., the base layer before cooling) extruded and still in a softened (molten) state by the method described in 1 above to obtain a laminate with a thickness of 150 μm. The obtained laminate was evaluated for the maximum height of the surface, kurtosis, the presence or absence of white spots, and transition concentration by the method described in [Test Example] below. The results are shown in Table 1.

[0142] [Comparative Example 1] Resin composition A, which contains 17 parts by mass of titanium oxide-containing polypropylene masterbatch (trade name: White PPM-7Y788FX, manufactured by Sumika Color Co., Ltd., titanium oxide concentration is 60% by mass) having an MFR of 15 g / 10 min, and 83 parts by mass of homopropylene (trade name: MA3, manufactured by Japan Polypropylene Co., Ltd.) having an MFR of 11 g / 10 min, and resin composition 1 for forming the base layer prepared in 1. of Example 1, were melt-kneaded at a temperature of 220 ° C. in separate extruders, fed into one die and laminated in the die, and then co-extrusion molded to obtain a laminate having a thickness of 150 μm in which a layer (surface layer) made of resin composition A was formed on both sides of the base layer. The thickness of the base layer was 30 μm, the same as the base layer of Example 1, and the thickness of the surface layer obtained by co-extrusion molding was 60 μm in both cases.

[0143] In addition, when the Clark stiffness (maximum Clark stiffness) of a film (surface film) obtained by separately extruding resin composition A (surface layer forming composition) in a single layer (thickness 60 μm) was measured, 3 / 100 was less than.

[0144] The obtained laminate was evaluated for the maximum surface height, kurtosis, and the presence or absence of white spots by the method described in [Test Example] below. The results are shown in Table 1. Note that the base layer of Comparative Example 1 was prepared under the same conditions as the base layer prepared in 1. of Example 1 above, and therefore the results of the evaluation of the base layer of Comparative Example 1 (maximum particle size of the coarse particles contained, maximum surface height, kurtosis, the presence or absence of white spots, and transition concentration) refer to the results of the base layer (base film) obtained in 1. of Example 1 above.

[0145] [Example 2] A laminate was produced in the same manner as in Example 1, except that the thickness of the substrate layer was 80 μm in 1 of Example 1 above. The maximum surface height, kurtosis, the presence or absence of white spots, and transition concentration were evaluated for each of the substrate layer (substrate film) and the laminate in the same manner as in Example 1. The results are shown in Table 1.

[0146] [Comparative Example 2] A laminate was prepared in the same manner as in Comparative Example 1, except that the thickness of the substrate layer in Comparative Example 1 was 80 μm. As in Comparative Example 1, the laminate was evaluated for the maximum surface height, kurtosis, and the presence or absence of white spots. The results are shown in Table 1. The substrate layer in Comparative Example 2 was prepared under the same conditions as the substrate layer prepared in Example 2, and therefore the results of the evaluation of the substrate layer in Comparative Example 2 (maximum particle size of the coarse particles contained, maximum surface height, kurtosis, the presence or absence of white spots, and transition concentration) refer to the results of the substrate layer (substrate film) obtained in Example 2.

[0147] [Example 3] In the above Example 1, the thickness of the base layer was 60 μm, and the surface layer had a thickness of 45 μm, a porosity of 34%, and a Clark stiffness (maximum Clark stiffness) of 13.9 cm 3A laminate was produced in the same manner as in Example 1, except that a polyolefin-based synthetic paper (containing homopolypropylene as the main component and further containing inorganic filler, manufactured by Yupo Corporation) was used, in which the thickness of the laminate was 100 / 100 and a uniaxially oriented layer / biaxially oriented layer / uniaxially oriented layer were laminated in this order. As in Example 1, the maximum height, the presence or absence of kurtosis, and white spots were evaluated for each of the base layer (base film) and the laminate. The results are shown in Table 1.

[0148] [Example 4] 1. Preparation of the substrate layer The following was used as recycled resin raw material after user use: a printed paper with a coating layer containing a pigment on a sheet manufactured by Yupo Corporation (containing homopolypropylene as the main component and further containing inorganic filler) was crushed and used as recycled resin raw material. The recycled resin raw material was melt-kneaded in an extruder at 220°C to prepare resin composition 2 for forming the base layer. The MFR of resin composition 2 was 5.5g / 10min.

[0149] This was then extrusion molded and cooled to 50°C in a cooling device to obtain a substrate layer (substrate film) that was a single-layered unstretched sheet. The thickness of the substrate layer was 30 μm. The maximum particle diameter of the coarse particles contained in the substrate layer was measured by the method described above and found to be 800 μm. The obtained substrate layer (substrate film) was evaluated for maximum surface height, kurtosis, the presence or absence of white spots, and transition concentration by the method described in [Test Example] below. The results are shown in Table 1.

[0150] 2. Preparation of Laminate A laminate was produced in the same manner as in Example 1, except that the substrate layer in Example 1 was changed to a substrate layer (substrate film) produced using the above-mentioned resin composition 2. The maximum height of the surface, kurtosis, the presence or absence of white spots, and transition concentration of the laminate were evaluated in the same manner as in Example 1. The results are shown in Table 1.

[0151] [Test example] (Maximum height and kurtosis) The monolayer film (substrate film) and the laminate obtained in each Example and Comparative Example were cut into a size of 40 mm x 60 mm to prepare a test piece for measurement. The test piece was left to stand at 23°C and 50% RH for 24 hours or more, and then three points were selected within an area of ​​1 cm x 1 cm, and the maximum height and kurtosis were measured using a contact-type three-dimensional roughness measuring device (device name: SURFCOM (registered trademark) 1500 DX2, manufactured by Tokyo Seimitsu Co., Ltd.), and the average values ​​of the measured values ​​were calculated to be the maximum height and kurtosis values ​​of the test piece.

[0152] The maximum height (Rz) was measured in accordance with the method specified in JIS-B0601:2013.

[0153] Kurtosis is Sku (kurtosis) defined in ISO25178-2:2021, and was measured in accordance with the conditions defined in ISO25178-3:2021. Kurtosis is one of the three-dimensional surface property parameters, and means kurtosis, which is a measure of surface sharpness, and represents the sharpness (sharpness) of the height distribution. When Sku is 3, the surface shape is symmetrical (normal distribution) with respect to the average plane, and when Sku exceeds 3, the height distribution has a sharp shape, and when Sku is less than 3, the height distribution tends to have a crushed shape. The kurtosis of the laminate surface is preferably less than 10, and more preferably 8 or less.

[0154] <Printing evaluation (sample creation)> For the single-layer film (substrate film) consisting of only the substrate layer and the laminate obtained in each Example and Comparative Example, a black solid print was performed using an RI tester (manufactured by Ishikawajima Industrial Machinery Co., Ltd.) based on JIS K5701-1:2000 "Lithographic inks - Part 1: Test methods". For the black solid print, UV offset ink (product name: BC161, manufactured by T&K TOKA Co., Ltd.) was used, and a rubber roll with a hardness of 90 was used to transfer the ink to the substrate layer (substrate film) or laminate, the printing pressure was adjusted to 10 mm, and the ink build-up amount was 1.5 g / m. 2Next, a UV irradiation machine (Eye Inverter Grandage, model ECS-401GX, manufactured by Eye Graphics Co., Ltd.) was used to irradiate the sample with an irradiation intensity of 100 mJ / cm. 2 Thus, a sample for evaluating white spots and transition concentration was obtained.

[0155] (White space) The obtained evaluation samples were visually evaluated for the presence or absence of white spots.

[0156] (Transition concentration) The print density (transfer density) of the obtained evaluation samples was measured using a spectrophotometer (device name: SpectroEye (registered trademark), manufactured by X-Rite, Inc.). For a single-layer film (substrate film) consisting of only a substrate layer, the transfer density was measured at the protrusions and bulk (area other than the protrusions). For the laminates obtained in Examples 1, 2, and 4, no protrusions were observed on the surface and there was no unevenness in the transfer density, so the transfer density was measured at any point.

[0157] [Table 1]

[0158] The surface of the base layer had both high maximum height and high kurtosis, and printing on that surface resulted in white spots caused by the protrusions. In addition, the ink adhered thickly to the protrusions on the surface of the base layer, so the transfer concentration was high at the protrusions. On the other hand, the printing plate was pushed up by the protrusions and floated off the surface of the base layer, so the ink did not adhere sufficiently to the bulk parts (areas other than the protrusions), resulting in a low transfer concentration and uneven color concentration.

[0159] In contrast, the maximum height and kurtosis of the laminate obtained in the examples are significantly reduced compared to the values ​​of the substrate layer surface, and it is clear that the surface smoothing effect of the laminate is fully achieved. And, as a result of printing on the surface of the laminate obtained in the examples, no white spots were generated. Also, the transition concentration difference occurring at the protrusions and bulk parts on the substrate layer surface did not appear on the laminate surface.

[0160] On the other hand, in the laminates obtained in the comparative examples, although the kurtosis was reduced, the effect of reducing the maximum height was not sufficient, and the maximum height of the laminate surface exceeded 10 μm in all cases. In addition, when printing was performed on the laminates obtained in the comparative examples, white spots occurred due to the protrusions. [Industrial Applicability]

[0161] According to the present invention, it is possible to provide a laminate having excellent surface appearance and excellent printability, even when using a PCR resin or the like containing coarse foreign matter as a raw material. [Explanation of symbols]

[0162] 1 base material layer, 2 surface layer, 10 laminate.

Claims

1. A laminate having a base layer containing a thermoplastic resin and a surface layer laminated on at least one surface of the base layer, The maximum height of the surface of the base layer is 10 μm or more, The surface layer has a Clark stiffness of 10 cm 3 A laminate which is a film having a film thickness of 100 mm or more.

2. The surface layer has a Clark stiffness of 10 to 40 cm 3 2. The laminate of claim 1, which is a 100 / 100 film.

3. The laminate according to claim 1 or 2, wherein the surface layer has a thickness of 30 to 80 μm.

4. The laminate according to claim 1 or 2, wherein the thickness of the laminate is 80 to 400 μm.

5. The laminate according to claim 1 or 2, wherein the thermoplastic resin contained in the base material layer comprises a recycled resin.

6. A substrate film containing a thermoplastic resin and having a maximum height of 10 μm or more on at least one surface is provided with a Clark stiffness of 10 cm 3 A method for producing a laminate, comprising: laminating a surface film having a viscosity of 100 / 100 or more.

7. The thickness of the base film is 20 to 340 μm, The base film contains the thermoplastic resin and particles, The method according to claim 6, wherein the maximum particle size of the particles is 3 to 30 times the thickness of the base film.

8. The method according to claim 6 or 7, wherein the surface film is bonded to the substrate film in a molten state.

Citation Information

Patent Citations

  • Polyester biaxially stretched film

    JP2000141573A

  • Laminate and method for manufacturing laminate

    WO2022210896A1