Resin composition for polyethylene resin extrusion foaming and use thereof

A resin composition with controlled moisture content and specific additives produces extruded polyethylene resin foams with small cell diameters and high closed cell ratios, addressing the issue of poor product protection in conventional foams.

JP2024143796AInactive Publication Date: 2024-10-11KANEKA CORP
View PDF 1 Cites 0 Cited by

Patent Information

Application Number
JP2023056683
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Filing Date
2023-03-30
Publication Date
2024-10-11
Estimated Expiration
Not applicable · inactive patent

AI Technical Summary

Technical Problem

Conventional extruded polyethylene resin foams exhibit large average cell diameters, leading to poor product protection performance when used as cushioning materials.

Method used

A resin composition for polyethylene resin extrusion foaming with a moisture content of 300 ppm or less, containing a polyethylene resin, a cell nucleating agent, and optional anti-shrinkage and blowing agents, is used to produce foams with an average cell diameter of 650 μm or less and a closed cell ratio of 70% or more.

Benefits of technology

The solution results in extruded polyethylene resin foams with a small average cell diameter and high closed cell ratio, enhancing product protection and cushioning performance.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024143796000001
    Figure 2024143796000001
Patent Text Reader

Abstract

To provide a resin composition for polyethylene resin extrusion foaming that is capable of yielding a polyethylene resin extrusion foam with a small average cell diameter.SOLUTION: A resin composition for polyethylene resin extrusion foaming comprises a polyethylene resin composition and a cell nucleation agent, where the polyethylene resin composition has a moisture content of 300 ppm or less.SELECTED DRAWING: None
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a resin composition for extrusion foaming of a polyethylene resin, and use thereof. [Background technology]

[0002] Because of its excellent flexibility and abrasion resistance, polyethylene-based resin extruded foams are widely used as cushioning materials (e.g., packaging cushioning materials). For example, development of polyethylene-based resin extruded foams using polyethylene-based resins such as low-density polyethylene as packaging cushioning materials for transporting automobile parts and the like is progressing.

[0003] As an example of a polyethylene-based resin extrusion foam, Cited Document 1 describes a non-crosslinked polyethylene-based resin extrusion foam board obtained by extrusion foaming of a polyethylene-based resin composition containing, per 100 parts by weight of polyethylene-based resin, 0.03 to 1.3 parts by weight of a bubble nucleating agent consisting of a thermally decomposable foaming agent and a citrate salt, and 0.1 to 1.5 parts by weight of a shrinkage inhibitor, in which the ratio B / A of the amount of shrinkage inhibitor added to the amount A of the bubble nucleating agent is 10 or less, and the board satisfies the following requirements: (a) an expansion ratio of 5 to 30 times and (b) a thickness of 20 mm or more.

[0004] In recent years, with the growing momentum towards achieving the Sustainable Development Goals (SDGs), progress has been made in the development of technologies that use recycled polyethylene resins, etc., with the aim of not only reducing environmental pollution but also significantly reducing the amount of plastic waste generated and the amount of plastic used in manufacturing. [Prior art documents] [Patent documents]

[0005] [Patent Document 1] JP 2020-97687 A Summary of the Invention [Problem to be solved by the invention]

[0006] However, the above-mentioned conventional techniques have a problem in that the average cell diameter of the extruded polyethylene resin foam becomes large.

[0007] If the average cell diameter of the extruded polyethylene resin foam is large, problems such as poor product protection performance will arise when the extruded polyethylene resin foam is used as a cushioning material.

[0008] An object of one aspect of the present invention is to provide a resin composition for extrusion foaming of polyethylene-based resins, which can provide extruded polyethylene-based resin foams having a small average cell diameter. [Means for solving the problem]

[0009] Means for Solving the Problems The present inventors have conducted intensive studies to solve the above problems and have found that an extruded polyethylene resin foam having a small average cell diameter can be obtained by using a polyethylene resin composition having a water content of not more than a specific amount, thereby completing the present invention.

[0010] That is, one embodiment of the present invention includes the following configuration.

[0011] [1] A resin composition for extrusion foaming of a polyethylene-based resin, comprising a polyethylene-based resin composition and a bubble nucleating agent, The polyethylene resin composition for extrusion foaming, wherein the moisture content of the polyethylene resin composition is 300 ppm or less.

[0012] [2] The polyethylene resin composition for extrusion foaming according to [1], wherein the polyethylene resin composition contains 5 to 99% by weight of recycled polyethylene resin.

[0013] [3] The polyethylene resin composition for extrusion foaming according to [1] or [2], further comprising a shrinkage inhibitor.

[0014] [4] The resin composition for polyethylene resin extrusion foaming according to [3], wherein the shrinkage inhibitor contains a fatty acid ester.

[0015] [5] The resin composition for extrusion foaming of polyethylene-based resin according to any one of [1] to [4], which contains a foaming agent.

[0016] [6] The resin composition for polyethylene resin extrusion foaming according to [5], wherein the foaming agent includes a physical foaming agent.

[0017] [7] The resin composition for polyethylene resin extrusion foaming according to any one of [1] to [6], wherein the cell nucleating agent comprises a thermally decomposable foaming agent and citric acid (salt).

[0018] An extruded polyethylene resin foam obtained by extruding and foaming the resin composition for extrusion foaming of a polyethylene resin according to any one of [1] to [7], which satisfies the following: (a) Cell diameter is 650 μm or less; (b) Closed cell ratio is 70% or more.

[0019] A step A of melt-kneading the polyethylene resin extrusion foaming resin composition according to any one of [1] to [7] together with a foaming agent in an extruder; A process for producing an extruded polyethylene resin foam, comprising: a step B of extruding and foaming the molten resin obtained in the step A. Effect of the Invention

[0020] According to one aspect of the present invention, there is provided a resin composition for extrusion foaming of polyethylene-based resin, which can provide an extruded polyethylene-based resin foam having a small average cell diameter. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0021] An embodiment of the present invention will be described below, but the present invention is not limited thereto. The present invention is not limited to each configuration described below, and various modifications are possible within the scope of the claims. In addition, embodiments or examples obtained by appropriately combining the technical means disclosed in different embodiments or examples are also included in the technical scope of the present invention. Furthermore, new technical features can be formed by combining the technical means disclosed in each embodiment. All academic documents and patent documents described in this specification are incorporated herein by reference.

[0022] Unless otherwise specified in this specification, "A to B" representing a numerical range means "A or more (including A and greater than A) and B or less (including B and less than B)."

[0023] In this specification, a constitutional unit derived from an X monomer may be referred to as an "X unit."

[0024] 1. Technical Concept of One Embodiment of the Present Invention Extruded polyethylene-based resin foams with a large average cell diameter tend to have a harder feel and transfer cell patterns to materials in contact with them, compared with extruded polyethylene-based resin foams with a small average cell diameter, and therefore extruded polyethylene-based resin foams with a large average cell diameter tend to be avoided in some fields.

[0025] In the course of examining the prior art, the present inventors independently obtained the novel finding that the average cell diameter of an extruded polyethylene resin foam may vary depending on the moisture content in a polyethylene resin composition that is a raw material for the extruded polyethylene resin foam. In particular, the present inventors independently obtained the novel finding that the average cell diameter of an extruded polyethylene resin foam increases as the moisture content in the polyethylene resin composition increases.

[0026] The moisture content of the polyethylene resin composition may mainly depend on the components such as additives contained in the polyethylene resin composition and the management conditions of the raw material components. For example, various additives that are easy to absorb water, such as shrinkage inhibitors, and recycled polyethylene resins tend to have a high moisture content. Therefore, the present inventors have intensively studied the reason why the average cell diameter of the polyethylene resin extrusion foam increases due to moisture, and have concluded that, although it is not clear, some bubble nucleating agents added as nucleating agents are easily affected by moisture, and the nucleating action of such bubble nucleating agents is lost due to moisture.

[0027] Thus, the present inventors have found that a polyethylene-based resin extruded foam having a desired average cell diameter can be stably produced without being limited by the type of bubble nucleating agent by controlling the water content in the polyethylene-based resin composition to a specific amount or less, and have thus completed the present invention.

[0028] 2. Polyethylene resin composition for extrusion foaming A resin composition for extrusion foaming of polyethylene-based resin according to one embodiment of the present invention is a resin composition for extrusion foaming of polyethylene-based resin, which comprises a polyethylene-based resin composition and a bubble nucleating agent, and the polyethylene-based resin composition has a moisture content of 300 ppm or less. According to this constitution, a small average bubble diameter can be easily achieved.

[0029] The "resin composition for use in extrusion foaming of polyethylene-based resin according to one embodiment of the present invention" may also be referred to as the "present resin composition for use in extrusion foaming of polyethylene-based resin".

[0030] (Polyethylene resin composition) The resin composition for polyethylene-based resin extrusion foaming contains a polyethylene-based resin composition. In this specification, the term "polyethylene-based resin composition" refers to a composition containing a polyethylene-based resin. The polyethylene-based resin composition may contain a shrinkage inhibitor and / or a resin other than the polyethylene-based resin.

[0031] Examples of polyethylene-based resins include resins in which ethylene units account for 50 mol% or more (more specifically, 60 mol% or more, 70 mol% or more, 80 mol% or more, or 90 mol% or more) of 100 mol% of all constituent units.

[0032] Specific examples of polyethylene resins include crystalline polyethylene resins, more specifically high density polyethylene, medium density polyethylene, low density polyethylene (LDPE) having a branched structure, linear low density polyethylene (LLDPE), ethylene / vinyl acetate copolymer, ethylene / propylene copolymer, ethylene / propylene / 1-butene copolymer, ethylene / 1-butene copolymer, ethylene / 1-hexene copolymer, ethylene / 4-methyl-1-pentene copolymer, ethylene / 1-octene copolymer, styrene-modified polyethylene resin, etc. "Low density polyethylene having a branched structure" is sometimes called "branched low density polyethylene".

[0033] From the viewpoint of excellent foaming ability, the main component of the polyethylene resin is preferably a branched low-density polyethylene having a density of 935 kg / m 3 The following branched low density polyethylene is more preferable: "Main component of polyethylene resin" refers to a component that accounts for more than 50% by weight in 100% by weight of the polyethylene resin.

[0034] From the viewpoint of excellent foaming properties, the polyethylene resin preferably contains 60 wt % or more of branched low-density polyethylene, more preferably 70 wt % or more, even more preferably 80 wt % or more, and particularly preferably 90 wt % or more, based on 100 wt % of the polyethylene resin.

[0035] The lower limit of the density of the branched low density polyethylene resin is not particularly limited, but is, for example, 890 kg / m 3 From the viewpoint of excellent foaming properties, the density of the branched low-density polyethylene resin is 900 kg / m 3 ~930kg / m 3 is preferred, and 910 kg / m 3~925kg / m 3 More preferably, 913 kg / m 3 ~923kg / m 3 is particularly preferred.

[0036] The melt flow rate (MFR) of the polyethylene resin is preferably 0.05 to 15 g / 10 min, more preferably 0.5 to 10 g / 10 min, further preferably 0.8 to 5.0 g / 10 min, and particularly preferably 1.0 to 3.0 g / 10 min. The above-mentioned constitution has the advantage that it has melt tension and can prevent excessive shear heat generation in the extruder, making it easy to set conditions suitable for extrusion foaming.

[0037] The melting point of the polyethylene resin is preferably 100 to 130° C., more preferably 102 to 125° C., further preferably 103 to 120° C., particularly preferably 104 to 118° C., and most preferably 105 to 115° C. The above-mentioned configuration has the advantage that the temperature during extrusion foaming can be relatively easily adjusted, and the foaming ratio and the closed cell ratio can be easily adjusted.

[0038] The polyethylene resin may be an unused polyethylene resin, a recycled polyethylene resin, or a mixture thereof. In this specification, the term "recycled polyethylene resin" refers to a resin obtained by crushing and repelletizing scraps and defective products generated during the manufacturing process of a polyethylene resin foam, or a resin obtained by recovering and crushing and repelletizing buffer materials and the like produced from a polyethylene resin foam, or a resin obtained by crushing and repelletizing a non-foamed polyethylene resin molded body. When the recycled polyethylene resin is repelletized in the recycling process, cooling with water is used, such as passing through a water tank or spraying water, and the like, so that the recycled polyethylene resin may contain a lot of moisture. If the moisture is brought directly into the composition for extrusion foaming, the average bubble diameter of the extruded foam will be increased. In one embodiment of the present invention, the moisture can be appropriately removed by drying, so that even if a recycled polyethylene resin containing a lot of moisture is used, the average bubble diameter of the extruded foam can be reduced. As the recycled polyethylene resin, a resin obtained by crushing and repelletizing a foam and a resin obtained by crushing and repelletizing scraps and defective products generated during the manufacturing process are preferable.

[0039] The amount of unused polyethylene resin contained in the polyethylene resin composition is not limited. The polyethylene resin composition may contain, for example, 1 to 99% by weight, 10 to 99% by weight, 20 to 99% by weight, 30 to 99% by weight, 40 to 99% by weight, 50 to 99% by weight, 60 to 99% by weight, 70 to 99% by weight, 80 to 99% by weight, 90 to 99% by weight, or 100% by weight of unused polyethylene resin. From the viewpoint of realizing an extruded foam having a smaller average cell diameter, the amount of unused polyethylene resin contained in the polyethylene resin composition is preferably large.

[0040] The amount of recycled polyethylene resin contained in the polyethylene resin composition is not limited. The polyethylene resin composition may contain, for example, 1 to 99% by weight, 1 to 90% by weight, 1 to 80% by weight, 1 to 70% by weight, 1 to 60% by weight, 1 to 50% by weight, 1 to 40% by weight, 1 to 30% by weight, 1 to 20% by weight, 1 to 10% by weight, or 0% by weight of recycled polyethylene resin.

[0041] The moisture content of the recycled polyethylene resin is not limited, and may be, for example, 50 to 5000 ppm, 100 to 2000 ppm, 150 to 1500 ppm, or 150 to 800 ppm based on the weight of the recycled polyethylene resin. The lower the moisture content of the recycled polyethylene resin, the less the effect of coarsening the cell diameter, which is preferable. On the other hand, an extremely low moisture content tends to be difficult to adjust or control. When the moisture content and / or the amount of the recycled polyethylene resin is high, the moisture content of the polyethylene resin composition containing the recycled polyethylene resin can be adjusted by drying the polyethylene resin composition.

[0042] The type of polyethylene resin contained in the recycled polyethylene resin is not particularly limited. For example, when a recycled polyethylene resin containing a branched low-density polyethylene resin is used, the amount of the branched low-density polyethylene resin is also included in the amount of the branched low-density polyethylene resin contained in the polyethylene resin.

[0043] Examples of resins other than polyethylene-based resins include polyolefin-based resins such as polypropylene-based resins, and synthetic resins other than polyolefin-based resins.

[0044] Examples of polypropylene-based resins include polypropylene homopolymers, polypropylene / ethylene block copolymers, polypropylene / ethylene random copolymers, propylene / α-olefin copolymers, propylene / 1-butene copolymers, ethylene / 1-butene / propylene copolymers, propylene / chlorinated vinyl copolymers, propylene / maleic anhydride copolymers, long-chain branched polypropylenes having high melt tension, isoprene-modified polypropylenes, and polypropylenes containing ultra-high molecular weight components.

[0045] Examples of synthetic resins other than polyolefin-based resins include (a) thermoplastic resins such as vinyl acetate-based resins, polyester resins, acrylic resins, acrylic ester resins, styrene-based resins, polyamide resins, polycarbonate resins, and polyvinyl chloride resins; (b) polyamide-based elastomers such as polyamide / polyol copolymers; and (c) thermoplastic elastomers such as polyvinyl chloride-based elastomers, polybutadiene-based elastomers, ethylene / propylene rubber, and ethylene / propylene / butadiene rubber.

[0046] The polyethylene resin composition preferably contains 50% by weight or more of polyethylene resin, more preferably 60% by weight or more, more preferably 70% by weight or more, more preferably 75% by weight or more, more preferably 80% by weight or more, and even more preferably 85% by weight or more, based on 100% by weight of the resin component contained in the polyethylene resin composition. This configuration has the advantages of (a) the polyethylene resin composition having excellent foaming properties, and (b) being able to provide an extruded foam having a small average cell diameter and a high closed cell ratio.

[0047] The moisture content of the polyethylene resin composition is 300 ppm or less. The moisture content of the polyethylene resin composition may be 280 ppm or less, 260 ppm or less, 240 ppm or less, 220 ppm or less, 200 ppm or less, 180 ppm, 160 ppm or less, 140 ppm or less, 120 ppm or less, 100 ppm or less, 80 ppm or less, or 60 ppm or less. The lower limit of the moisture content of the polyethylene resin composition is not limited, and may be, for example, 0.1 ppm, 1 ppm, 5 ppm, or 10 ppm. With this configuration, the average bubble diameter can be reduced. Furthermore, with this configuration, the closed cell ratio can be increased.

[0048] The method for setting the moisture content of the polyethylene-based resin composition to the above-mentioned value is not limited, and examples thereof include (i) a method of adjusting the moisture content by drying the polyethylene-based resin composition, and (ii) a method of producing the polyethylene-based resin composition from a raw material having a low moisture content.

[0049] (bubble nucleating agent) The resin composition for extrusion foaming of polyethylene-based resin contains a bubble nucleating agent. In this specification, the term "bubble nucleating agent" refers to an agent that controls the formation of bubble nuclei in the resin composition for extrusion foaming of polyethylene-based resin. Examples of the bubble nucleating agent include a thermally decomposable foaming agent, an organic acid (salt), and an inorganic substance (e.g., talc, etc.). In this specification, the term "organic acid (salt)" refers to an organic acid and / or an organic acid salt. The bubble nucleating agent preferably contains a thermally decomposable foaming agent and / or an organic acid (salt). When the bubble nucleating agent contains a thermally decomposable foaming agent and / or an organic acid (salt), the average bubble diameter of the extruded foam can be made smaller more easily than when the bubble nucleating agent does not contain a thermally decomposable foaming agent and / or an organic acid (salt) and contains only an inorganic substance (e.g., talc, etc.). From the viewpoint of realizing an extruded foam with a smaller average bubble diameter, the bubble nucleating agent more preferably contains a thermally decomposable foaming agent and an organic acid (salt), and more preferably is made of a mixture of a thermally decomposable foaming agent and an organic acid (salt). More specifically, it is more preferable that the bubble nucleating agent contains a thermal decomposition type foaming agent and citric acid (salt).

[0050] Examples of the thermal decomposition type blowing agent include azodicarbonamide (ADCA), N,N'-dinitropentamethylenetetramine (DPT), 4,4'-oxybisbenzenesulfonylhydrazide (OBSH), hydrogen carbonate, and carbonate. Examples of the thermal decomposition type blowing agent include hydrogen carbonate, carbonate, and mixtures of hydrogen carbonate and carbonate. Examples of the hydrogen carbonate include sodium hydrogen carbonate.

[0051] Examples of organic acids (salts) include oxalic acid (salts), lactic acid (salts), succinic acid (salts), malic acid (salts), and citric acid (salts). Citric acid (salts) is preferred as an organic acid (salt) because it has a high effect of reducing the size of air bubbles. Examples of citric acid (salts) include citric acid, monosodium citrate, trisodium citrate, sodium hydrogen citrate, and potassium citrate.

[0052] As the bubble nucleation agent, a mixture of one or more selected from the group consisting of a mixture of bicarbonate and citric acid (salt), a mixture of carbonate and citric acid (salt), and a mixture of bicarbonate and a mixture of carbonate and citric acid (salt) is preferred, as these are easy to handle and have a high effect on generating bubble nuclei. A mixture of bicarbonate and citric acid (salt) is more preferred, and a mixture of sodium bicarbonate and monosodium citrate is particularly preferred.

[0053] The content ratio of the thermal decomposition type foaming agent and the organic acid (salt) in the bubble nucleating agent is preferably 10% by weight to 90% by weight of the thermal decomposition type foaming agent and 90% by weight to 10% by weight of the organic acid (salt), more preferably 20% by weight to 85% by weight of the thermal decomposition type foaming agent and 80% by weight to 15% by weight of the organic acid (salt), and even more preferably 30% by weight to 80% by weight of the thermal decomposition type foaming agent and 70% by weight to 20% by weight of the organic acid (salt). This configuration has the advantage that a small amount of the bubble nucleating agent can efficiently obtain the nucleation effect.

[0054] The amount of the bubble nucleating agent of the present invention is preferably 0.03 parts by weight to 1.50 parts by weight, more preferably 0.08 parts by weight to 1.20 parts by weight, and even more preferably 0.10 parts by weight to 1.00 parts by weight, relative to 100 parts by weight of the polyethylene resin composition. If the amount of the bubble nucleating agent is 0.03 parts by weight or more relative to 100 parts by weight of the polyethylene resin composition, the desired nucleation action is easily obtained. In addition, if the amount of the bubble nucleating agent is 1.50 parts by weight or less relative to 100 parts by weight of the polyethylene resin composition, the production cost is low and the risk of generation of foreign matter due to decomposition products of the bubble nucleating agent is low.

[0055] In the present invention, as the bubble nucleating agent, powdery bubble nucleating agent can be used directly, or the master batch of bubble nucleating agent can be used, which is considered to be mixed with raw resin and easy to handle.As the master batch of bubble nucleating agent, commercially available products can be used, such as Polyslen EE275F manufactured by Eiwa Chemical Industry Co., Ltd., Fine Cell Master SSC PO217K manufactured by Dainichiseika Chemical Industry Co., Ltd., etc.

[0056] (Shrinkage prevention agent) The polyethylene resin composition preferably contains a shrinkage inhibitor. Examples of shrinkage inhibitors that can be used include fatty acid esters, aliphatic amines, and fatty acid amides. The fatty acid esters are preferably esters of fatty acids having 8 to 30 carbon atoms and polyhydric alcohols having 3 to 7 hydroxyl groups. Examples of fatty acids having 8 to 30 carbon atoms include lauric acid, oleic acid, stearic acid, behenic acid, lignoceric acid, cerotic acid, heptacoic acid, montanic acid, melissic acid, and lacteric acid. Examples of polyhydric alcohols having 3 to 7 hydroxyl groups include glycerin, diglycerin, triglycerin, erythritol arabic acid, xylymaat, mannitol, sorbitol, and sorbitan. From the viewpoint of suitably replacing the physical foaming agent used with air, more specifically, preferred fatty acid esters include glycerin fatty acid esters (for example, stearate monoglyceride, behenate monoglyceride, or a mixture of stearate monoglyceride and behenate monoglyceride).

[0057] The shrinkage inhibitor preferably contains a fatty acid ester, and more preferably is a fatty acid ester (consisting only of a fatty acid ester). The shrinkage inhibitor preferably contains a glycerin fatty acid ester, and more preferably is a glycerin fatty acid ester (consisting only of a glycerin fatty acid ester). The shrinkage inhibitor may contain one or more selected from the group consisting of stearate monoglyceride, behenate monoglyceride, and a mixture of stearate monoglyceride and behenate monoglyceride, or may be one or more selected from the group (or may be composed only of one or more).

[0058] The moisture content of the shrinkage inhibitor is preferably 100 ppm or more and 10,000 ppm or less, more preferably 500 ppm or more and 8,000 ppm or less, even more preferably 1,000 ppm or more and 6,000 ppm or less, and particularly preferably 1,500 ppm or more and 3,000 ppm or less. The above-mentioned composition has the advantage that the moisture content can be adjusted relatively easily.

[0059] The amount of the shrinkage inhibitor of the present invention may be adjusted according to the formulation to be applied, the desired expansion ratio, etc., and is preferably 0.1 to 3.0% by weight, more preferably 0.3 to 2.0% by weight, and even more preferably 0.4 to 1.0% by weight, based on 100% by weight of the polyethylene resin composition. The above composition has the advantage that the shrinkage of the obtained foam can be easily prevented while minimizing the effect of the water content.

[0060] (foaming agent) The polyethylene resin composition for extrusion foaming preferably contains a foaming agent. Examples of the foaming agent include physical foaming agents such as (a) (a-1) aliphatic hydrocarbons such as propane, normal butane, isobutane, normal pentane, isopentane, and hexane; (a-2) alicyclic hydrocarbons such as cyclopentane and cyclobutane; (a-3) ethers such as dimethyl ether, diethyl ether, and methyl ethyl ether; (a-4) alcohols such as methanol and ethanol; (a-5) inorganic gases such as air, nitrogen, and carbon dioxide; and (a-6) water, as well as (b) chemical foaming agents including thermal decomposition type foaming agents such as sodium bicarbonate, azodicarbonamide, and dinitrosopentamethylenetetramine. Of these, the foaming agent is preferably a physical foaming agent because it is easy to obtain the desired expansion ratio, the desired closed cell ratio, and the desired average cell diameter, and more preferably an aliphatic hydrocarbon, and particularly preferably normal butane and / or isobutane.

[0061] The above-mentioned foaming agents may be used alone or in combination of two or more. For example, the above-mentioned foaming agents may contain only a physical foaming agent, or may contain a physical foaming agent and a foaming agent other than the physical foaming agent.

[0062] The amount of the foaming agent used is not particularly limited. The amount of the foaming agent used may be appropriately adjusted depending on the type of the foaming agent and the expansion ratio of the target extruded foam. The total amount of the foaming agent used is preferably 0.5 parts by weight to 20.0 parts by weight, more preferably 1.0 parts by weight to 15.0 parts by weight, even more preferably 1.0 parts by weight to 10.0 parts by weight, and most preferably 1.0 parts by weight to 5.0 parts by weight, based on 100 parts by weight of the polyethylene resin composition.

[0063] 3. Method for producing extruded polyethylene resin foam A method for producing an extruded polyethylene resin foam according to one embodiment of the present invention includes a step A of melt-kneading the resin composition for polyethylene resin extrusion foaming together with a foaming agent in an extruder, and a step B of extruding and foaming the molten resin obtained in the step A.

[0064] The "production method for an extruded polyethylene resin foam according to one embodiment of the present invention" may also be referred to as "the present production method." The "extruded polyethylene resin foam" may also be referred to as "extruded foam."

[0065] Since the present production method has the above-mentioned configuration, it is possible to produce an extruded polyethylene resin foam having a small average cell diameter. Specifically, in one embodiment of the present invention, it is believed that if the water content in the polyethylene resin composition is a specific amount or less, the loss of the nucleating action of the cell nucleating agent is prevented, and thus the average cell diameter of the extruded polyethylene resin foam can be reduced. However, the present invention is not limited to such a speculation.

[0066] [2-1. Process A] Step A is a step of melt-kneading a polyethylene resin extrusion foaming resin composition containing a polyethylene resin and a bubble nucleating agent together with a foaming agent in an extruder. The foaming agent may be the foaming agent contained in the polyethylene resin composition, or may be a foaming agent different from the foaming agent contained in the polyethylene resin composition, or may be both of them.

[0067] The polyethylene resin composition, the cell nucleating agent, and the foaming agent have already been described, and therefore their description will be omitted here.

[0068] (Melting and kneading with an extruder) In step A, a tandem extruder in which a twin screw extruder and a single screw extruder are connected, or a tandem extruder in which a single screw extruder and a single screw extruder are connected may be used as the extruder. A specific embodiment of step A may include, for example, a method in which the following operations (A1) to (A3) are carried out in order: (A1) a polyethylene resin composition and a bubble nucleating agent are supplied to a first extruder (first-stage extruder, twin screw); (A2) the supplied raw materials are melt-kneaded at a temperature suitable for kneading (for example, a temperature equal to or higher than the melting point of the polyethylene resin); (A3) a foaming agent is injected into the obtained mixture (melt-kneaded product) from the middle of the first extruder to prepare a molten resin.

[0069] [2-2. Process B] The step B is a step of extrusion foaming the molten resin obtained in the step A.

[0070] A specific embodiment of step B is, for example, a method in which the following operations (A4) to (A6) are performed in order: (A4) the obtained molten resin is fed from the first extruder to a second extruder (a second-stage extruder, single-screw) connected to the first extruder; (A5) the molten resin is cooled in the second extruder to a desired temperature; (A6) the molten resin is discharged from a die provided in the second extruder into a low-pressure (e.g., atmospheric pressure) environment to foam the molten resin and obtain an extruded foam. In step B, (i) in addition to the second extruder, a cooling device (e.g., a static mixer) connected to the second extruder may be further used, and (ii) instead of the second extruder, a cooling device connected to the first extruder may be further used. The cooling device can function to cool the molten resin to a desired temperature together with the second extruder, for example.

[0071] [4. Extruded polyethylene resin foam] The extruded polyethylene resin foam according to one embodiment of the present invention is preferably a polyethylene resin foam obtained by extrusion-foaming (for example, extrusion-foaming according to the method for producing an extruded polyethylene resin foam according to one embodiment of the present invention) of the resin composition for extrusion foaming according to one embodiment of the present invention, and satisfies the following (a) and (b): (a) the average cell diameter of the extruded polyethylene resin foam is 650 μm or less; (b) The extruded polyethylene resin foam has a closed cell ratio of 70% or more.

[0072] The "extruded polyethylene resin foam according to one embodiment of the present invention" may also be referred to as the "extruded foam".

[0073] The extruded foam is considered to contain (i) raw material substance A, which remains unreacted, and (ii) a new substance B that is generated by the reaction. Substances A and B are each considered to include many substances. There are circumstances that make it impossible or impractical to analyze and identify which substances are important in the extruded foam.

[0074] (Expansion Ratio) The expansion ratio of the extruded foam is not limited, and is preferably 5 to 30 times, more preferably 5 to 20 times, even more preferably 10 to 20 times, and particularly preferably 10 to 15 times. According to this configuration, the extruded foam has an advantage of being excellent in balance of light weight, gripping property and cushioning property of the product. In addition, according to this configuration, the processability of the extruded foam for making into a cushioning material, which is one of the main uses of the extruded foam, is improved. As a result, the extruded foam can be processed into a cushioning material and used as a cushioning material for a wide range of transported products from light parts to heavy parts. In this specification, the expansion ratio of the extruded foam is a value obtained by the measurement method described in the examples described later.

[0075] (average bubble diameter) The average cell diameter (cell size) of the extruded foam is 650 μm or less, more preferably 630 μm or less, more preferably 600 μm or less, more preferably 550 μm or less, more preferably 500 μm or less, more preferably 450 μm or less, more preferably 400 μm or less, and particularly preferably 350 μm or less. The lower limit of the average cell diameter of the extruded foam is not limited, but is preferably 100 μm or more, more preferably 150 μm or more, and particularly preferably 200 μm or more. This configuration has the advantages that (a) the extruded foam can be easily adjusted to a desired closed cell ratio and expansion ratio, and (b) the extruded foam has excellent product protection in the cushioning material application, which is the main application of the extruded foam. In this specification, the average cell diameter of the extruded foam is a value obtained by the measurement method described in the examples described later.

[0076] (Closed bubble rate) The extruded foam has a closed cell ratio of 70% or more, preferably 75% or more, more preferably 78% or more, more preferably 80% or more, more preferably 83% or more, more preferably 85% or more, more preferably 88% or more, and particularly preferably 90% or more. This configuration has the advantages of improving the cushioning performance, repeated use performance, and dimensional recovery during punching of the extruded foam as a cushioning material. EXAMPLES

[0077] Hereinafter, one embodiment of the present invention will be described in more detail with reference to examples and comparative examples, but the present invention is not limited to the following examples.

[0078] In the examples and comparative examples, the test methods and judgment criteria used for various evaluations are as follows.

[0079] <Melt flow rate (MFR)> The MFR of the polyethylene resin was measured in accordance with the provisions of Method A described in JIS K 7210 (1999). Specifically, the amount of resin (g) extruded from a die per unit time was measured at 190°C and a constant load (2.16 kg) using a Melt Indexer S-01 (manufactured by Toyo Seiki Seisakusho). The amount of resin (g) obtained was converted into the amount of resin (g) extruded in 10 minutes and calculated.

[0080] The unit time was 120 seconds when the melt flow rate was more than 0.5 g / 10 min and not more than 1.0 g / 10 min, 60 seconds when it was more than 1.0 g / 10 min and not more than 3.5 g / 10 min, 30 seconds when it was more than 3.5 g / 10 min and not more than 10 g / 10 min, 10 seconds when it was more than 10 g / 10 min and not more than 25 g / 10 min, 5 seconds when it was more than 25 g / 10 min and not more than 100 g / 10 min, and 3 seconds when it was more than 100 g / 10 min.

[0081] The amount of resin extruded from the die per unit time was defined as 1 unit of resin. In measuring the MFR, 3 units of resin were sampled, and the amount of resin (g) extruded per 10 minutes was calculated for each unit, and the average value was defined as the MFR of the polyethylene resin. If 3 units of resin could not be sampled in one measurement, the measurement was continued until 3 units could be sampled. If the melt flow rate measured at a certain unit time was not within the corresponding range, it was measured again at a unit time corresponding to that melt flow rate.

[0082] <Moisture percentage> The moisture content of each resin was measured using a trace moisture analyzer (CA-200 / VA-230, manufactured by Mitsubishi Chemical Analytech) at a set temperature of 180°C. The amount of sample used for the measurement was adjusted so that the measured moisture content was 100 to 500 μg. The measurement sample was taken from each resin immediately before use.

[0083] <Closed bubble rate> Three test pieces measuring 30 mm in length, 20 mm in width, and 20 mm in thickness were cut out from each of the extruded foams obtained in the Examples and Comparative Examples. The test pieces were used to measure the volume Vc (cm) of the test pieces using an air pycnometer (Tokyo Science Co., Ltd., air comparison specific gravity meter Model 1000) in accordance with the method described in ASTM D2856. 3 Next, the same test piece after the measurement was submerged in ethanol in a measuring cylinder. From the rise in the liquid level (ethanol level) of the measuring cylinder, the apparent volume Va (cm 3 This method of measuring the apparent volume is sometimes called the submersion method. The closed cell ratio (%) was calculated according to the following formula: Closed cell rate (%) = (Vc / Va) x 100.

[0084] The measurement was carried out on three test pieces per one extruded foam, and the arithmetic mean of the three measured values ​​was regarded as the closed cell ratio of the extruded foam.

[0085] <Extruded foam density> The weight W (kg) of the test piece used in the measurement of the closed cell ratio and the volume Va (m 3 ) and the density of the extruded foam was calculated according to the following formula: Extruded foam density (kg / m 3 )=W / Va.

[0086] The measurement was carried out on three test pieces per one extruded foam, and the arithmetic mean of the three measured values ​​was taken as the density of the extruded foam.

[0087] <Expansion ratio> The resin density of the raw material resin (e.g., (i) polyethylene-based resin, or (ii) a mixture of polyethylene-based resin and recycled polyethylene-based resin) used in the examples and comparative examples was measured in accordance with JIS K 7112. The extruded foam density (kg / m 3 ) and resin density (kg / m 3 ) and the expansion ratio was calculated by the following formula: Expansion ratio (times) = resin density / extruded foam density.

[0088] <Extruded foam size> For the extruded foams obtained in the examples and comparative examples, the surface perpendicular to the thickness direction was designated as surface a, the surface perpendicular to the extrusion direction was designated as surface b, and the surface perpendicular to the width direction was designated as surface c. Here, the thickness direction of the extruded foam can be said to be the short direction in the cross section perpendicular to the extrusion direction of the extruded foam, and the width direction of the extruded foam can be said to be the longitudinal direction in the cross section perpendicular to the extrusion direction of the extruded foam. The extruded foams obtained in the examples and comparative examples were cut along surface b to prepare three samples A each having a length of 20 mm in the extrusion direction. The length in the thickness direction and the length in the width direction were measured for sample A. The length in the thickness direction will be specifically described. For each sample A, the length in the thickness direction was measured at three locations in total, including the center in the width direction and 30 mm inward from both ends in the width direction. The average value of the measurements of a total of nine measurements, three locations each for three samples A, was taken as the length in the thickness direction (thickness dimension) of the extruded foam. The length in the width direction will be specifically described. For each sample A, the length in the width direction was measured. The average value of the values ​​of the three samples A was taken as the length in the width direction (width dimension) of the extruded foam. In addition, the product of the obtained thickness dimension and width dimension was calculated, and this product was defined as the cross-sectional area.

[0089] <Average bubble diameter> From each of the three samples A produced in the measurement of the size of the extruded foam, cubes (referred to as sample B) with sides of 5 to 10 mm were cut out for each of the measurement points (five locations) shown below. Sample B was cut along the planes parallel to each of the above-mentioned planes a, b, and c using a double-edged razor [Feather, high-stainless double-edged], with great care not to destroy the cell membrane (cell membrane). The obtained cut surfaces (three surfaces) were observed using a microscope [Keyence, VHX-900], and images of each cut surface were obtained. In each of the obtained images, a line segment with a length of 4000 μm was drawn, the number of cells n through which the line segment passed was measured, and the cell diameter was calculated using the following formula: Bubble diameter (μm) = 4000 / n.

[0090] The average bubble diameter (μm) was determined as the arithmetic mean of the bubble diameters obtained from the images of the three cut surfaces of sample B (15 pieces) obtained for each measurement point (5 points) of the three samples A. In other words, the average bubble diameter (μm) was determined as the arithmetic mean of the bubble diameters of 45 surfaces (3 surfaces × 5 points × 3 samples A).

[0091] The measurement points are explained for sample A. As shown below, five points were measured for one sample A: (a) The center of surface b of sample A in the width direction and thickness direction (one location, designated as "measurement point A"); (b) On surface b of sample A, the center portion in the thickness direction, between measurement point A and the end portion in the width direction (two points on both ends in the width direction); (c) On surface b of sample A, the center in the width direction, between measurement point A and the end in the thickness direction (two points on each end in the thickness direction).

[0092] <Polyethylene resin> The polyethylene resin used was a branched low-density polyethylene "C470" (manufactured by Ube Maruzen Polyethylene, MFR 2.0 g / 10 min, density 918 kg / m 3 , melting point Tm109℃), linear low-density polyethylene "0540F" (Ube Maruzen Polyethylene, MFR4.0g / 10min, density 904kg / m 3 The moisture content of the resin was essentially 0 ppm.

[0093] <Shrinkage prevention agent> As a shrinkage prevention agent, Riken Vitamin's "ELB348" (master batch containing glycerin fatty acid ester) was used.

[0094] <Bubble nucleating agent> The bubble nucleating agent used was "EE275F" manufactured by Eiwa Kasei, which is a mixture of a thermal decomposition type foaming agent and an organic acid (salt). EE275F is a master batch containing a mixture of sodium bicarbonate and citric acid (salt).

[0095] <Foaming agent> Isobutane was used as the blowing agent.

[0096] <Recycled polyethylene resin (recycled material)> <Recycled material A> The extruded foam obtained by the following manufacturing method was pulverized and fed to an extruder, extruded into strands, and the strands were cooled through a water tank and then cut and pelletized by a pelletizer. The pellets were adjusted to a target moisture content in a dryer and used as recycled polyethylene resin. (i) 100 parts by weight of a polyethylene resin composition consisting of 97.6% by weight of a polyethylene resin "C470" and 2.4% by weight of a shrinkage inhibitor "ELB348", and (ii) 2 parts by weight of a bubble nucleating agent were blended to prepare a raw material. The prepared raw material was fed to the first extruder of a tandem extruder. Here, as the tandem extruder, a tandem extruder was used in which a twin-screw extruder with a diameter of 40 mm was connected as the first extruder and a single-screw extruder with a diameter of 90 mm was connected as the second extruder. The first extruder was set to 220°C, that is, the raw material fed to the first extruder was melt-kneaded at 220°C. Here, 3.5 parts by weight of isobutane as a foaming agent was injected into the obtained molten kneaded product from the middle of the first extruder, to prepare a molten resin.

[0097] The obtained molten resin was then fed from the first extruder to the second extruder (diameter 90 mm). After that, in the second extruder, the molten resin was cooled to a temperature suitable for foaming by adjusting the barrel temperature and the screw rotation speed. Then, the molten resin was discharged from the die attached to the tip of the second extruder at an output rate of 50 kg / hour under atmospheric pressure to perform extrusion foaming. Here, the die had a rectangular shape, and the size of the opening of the die was 50 mm x 5 mm.

[0098] Next, the foam extruded from the die was shaped into a rectangular shape using a molding die, and the size of the foam was adjusted by adjusting the take-up speed using a molding machine to mold it into a plate shape with a width of 140 mm and a thickness of 55 mm, obtaining a plate-shaped extruded foam.

[0099] <Recycled material B> A recycled material was obtained in the same manner as for recycled material A, except that the following polyethylene resin composition was used: (i) 100 parts by weight of a polyethylene resin composition consisting of 82.6% by weight of polyethylene resin "C470", 15.0% by weight of polyethylene resin "0540F", and 2.4% by weight of shrinkage inhibitor "ELB348".

[0100] Example 1 A polyethylene resin composition consisting of a polyethylene resin "C470" and a shrinkage inhibitor "ELB348", and a bubble nucleating agent were prepared in the amounts shown in Table 1. The prepared raw materials were supplied to the first extruder of a tandem extruder. Here, as the tandem extruder, a tandem extruder was used in which a twin-screw extruder with a diameter of 40 mm was connected as the first extruder and a single-screw extruder with a diameter of 90 mm was connected as the second extruder. The first extruder was set to 220°C, that is, the raw materials supplied to the first extruder were melt-kneaded at 220°C. Here, 3.5 parts by weight of isobutane as a foaming agent was injected into the obtained melt-kneaded product from the middle of the first extruder. By such an operation, a molten resin was prepared.

[0101] The obtained molten resin was then fed from the first extruder to the second extruder (diameter 90 mm). After that, in the second extruder, the molten resin was cooled to a temperature suitable for foaming by adjusting the barrel temperature and the screw rotation speed. Then, the molten resin was discharged from the die attached to the tip of the second extruder at an output rate of 50 kg / hour under atmospheric pressure to perform extrusion foaming. Here, the die had a rectangular shape, and the size of the opening of the die was 50 mm x 5 mm.

[0102] The foam extruded from the die was then shaped into a rectangular shape by a molding die, and the size of the foam was adjusted by adjusting the take-up speed of the molding machine to form a plate with a width of 140 mm and a thickness of 55 mm, to obtain a plate-shaped extruded foam. The obtained plate-shaped extruded foam had a small average cell diameter and a high closed cell ratio. The measurement results of various physical properties of the obtained extruded foam are shown in Table 1.

[0103] (Examples 2 to 9) A plate-shaped extruded foam was obtained in the same manner as in Example 1, except that the formulation was changed as shown in Table 1. The plate-shaped extruded foam had a small average cell diameter and a high closed cell ratio. The measurement results of various physical properties of the extruded foam are shown in Table 1.

[0104] Comparative Example 1 Except for changing the moisture content of the polyethylene resin composition as shown in Table 1, a plate-shaped extruded foam was obtained in the same manner as in Example 1. The physical properties of the obtained extruded foam were measured and evaluated, and the results are shown in Table 1.

[0105] As shown in Table 1, the extruded foams of Examples 1 to 9 had small average cell diameters and high closed cell ratios. On the other hand, the extruded foam of Comparative Example 1 had a high closed cell ratio but a large average cell diameter. [Table 1] [Industrial Applicability]

[0106] According to one embodiment of the present invention, an extruded polyethylene resin foam having a small average cell diameter can be provided. Therefore, this embodiment of the present invention can be suitably used for various cushioning materials, packaging materials, heat insulating materials, and the like.

Claims

1. A resin composition for polyethylene-based resin extrusion foaming, comprising a polyethylene-based resin composition and a bubble nucleating agent, The polyethylene resin composition for extrusion foaming, wherein the moisture content of the polyethylene resin composition is 300 ppm or less.

2. The polyethylene resin composition for extrusion foaming according to claim 1, wherein the polyethylene resin composition contains 5 to 99% by weight of recycled polyethylene resin.

3. The polyethylene resin composition for extrusion foaming according to claim 1 , further comprising a shrinkage inhibitor.

4. The polyethylene resin composition for extrusion foaming according to claim 3 , wherein the shrinkage inhibitor comprises a fatty acid ester.

5. The resin composition for polyethylene resin extrusion foaming according to claim 1 , further comprising a foaming agent.

6. The polyethylene resin composition for extrusion foaming according to claim 5 , wherein the foaming agent comprises a physical foaming agent.

7. 2. The polyethylene resin composition for extrusion foaming according to claim 1, wherein the bubble nucleating agent comprises a thermally decomposable foaming agent and citric acid (salt).

8. An extruded polyethylene resin foam obtained by extrusion foaming the resin composition for extrusion foaming of a polyethylene resin according to any one of claims 1 to 7, and satisfying the following: (a) a cell diameter of 650 μm or less; (b) The closed cell ratio is 70% or more.

9. A step A of melt-kneading the polyethylene resin extrusion foaming resin composition according to any one of claims 1 to 7 together with a foaming agent in an extruder; A process for producing an extruded polyethylene resin foam, comprising: a process B for extruding and foaming the molten resin obtained in the process A.

Citation Information

Patent Citations

  • Foam board of extruded non-crosslinked polyethylene-based resin and method for producing the same

    JP2020097687A