Polymer film and laminate

A polymer film with voids and specific material properties addresses delamination issues in copper-clad laminates by enhancing adhesion and heat resistance, ensuring stability during reflow soldering.

JP2024143967APending Publication Date: 2024-10-11FUJIFILM CORP
View PDF 2 Cites 0 Cited by

Patent Information

Application Number
JP2023108855
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Priority Date
2023-03-28
Filing Date
2023-06-30
Publication Date
2024-10-11

AI Technical Summary

Technical Problem

Copper-clad laminates face issues with delamination during reflow soldering due to the need for both excellent adhesion to wiring base materials and the ability to conform to level differences, while maintaining heat resistance.

Method used

A polymer film with specific properties, including voids, materials that are liquid or solid at 260°C, and a dielectric loss tangent of 0.01 or less, is used to enhance step followability and heat resistance.

Benefits of technology

The polymer film exhibits excellent step followability and heat resistance, preventing peeling from metal layers during high-temperature processes by allowing water to enter voids and suppress bubble growth.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024143967000001
    Figure 2024143967000001
  • Figure 2024143967000002
    Figure 2024143967000002
  • Figure 2024143967000003
    Figure 2024143967000003
Patent Text Reader

Abstract

To provide a polymer film with superior adaptability to step changes and superior heat resistance, and also to provide a laminate or the like.SOLUTION: A polymer film includes material A, which is liquid at 260°C, and material B, which is solid at 260°C. The polymer film includes voids with a length of 0.01 μm or more in the major axis direction, and exhibits an elastic modulus of 0.60 MPa or less at 160°C and a dielectric loss tangent of 0.01 or less. Also provided are applications therefor.SELECTED DRAWING: None
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present disclosure relates to polymer films and laminates. [Background technology]

[0002] In recent years, the frequencies used in communication devices have tended to become very high. In order to suppress transmission loss in the high frequency band, it is required to lower the relative dielectric constant and dielectric loss tangent of insulating materials used in circuit boards. Copper-clad laminates are preferably used as components constituting circuit boards, and films are preferably used to manufacture copper-clad laminates.

[0003] For example, Patent Document 1 describes a polymer film that contains a polymer and a filler and has a phase-separated structure containing at least two phases, each of which has an elastic modulus of 0.01 GPa or more. Patent Document 2 describes a resin composition containing a styrene-based polymer, an inorganic filler, and a curing agent, in which the styrene-based polymer is an acid-modified styrene-based polymer having a carboxy group, the inorganic filler is silica and / or aluminum hydroxide, the particle size of the inorganic filler is 1 μm or less, and the content of the inorganic filler is 20 to 80 parts by mass relative to 100 parts by mass of the styrene-based polymer. [Prior art documents] [Patent documents]

[0004] [Patent Document 1] International Publication No. 2022 / 202789 [Patent Document 2] JP 2019-199612 A Summary of the Invention [Problem to be solved by the invention]

[0005] Usually, a copper-clad laminate is manufactured by laminating a copper foil on the surface of a polymer film. A wiring board is manufactured by stacking a copper-clad laminate and a wiring substrate so that the polymer film of the copper-clad laminate and the wiring substrate are in contact with each other. When manufacturing a wiring board, it is required that the polymer film deforms to conform to the steps formed on the surface of the wiring substrate from the viewpoint of adhesion. On the other hand, when a polymer film with excellent step conformability to a wiring substrate is used for a copper-clad laminate, delamination may occur during the reflow soldering process performed when mounting electronic components. For this reason, there has been a demand for a material that has both step conformability to a wiring substrate and excellent adhesion during reflow soldering (i.e., excellent heat resistance).

[0006] An object of one embodiment of the present disclosure is to provide a polymer film and a laminate that are excellent in step conformability and heat resistance. [Means for solving the problem]

[0007] Means for solving the above problems include the following aspects. <1> The material A is liquid at 260°C, and the material B is solid at 260°C. It contains voids with a length in the long axis direction of 0.01 μm or more, The elastic modulus at 160°C is 0.60 MPa or less, A polymer film with a dielectric tangent of 0.01 or less. <2> The ratio of voids to the total volume of the polymer film is 1% by volume to 15% by volume. <1> The polymer film according to claim 1. <3> The void has a length in the major axis direction of 0.5 μm to 10 μm. <1> or <2> The polymer film according to claim 1. <4> The distance between the gap and material B is 5 μm or less. <1> ~ <3> 13. The polymer film according to claim 12, <5> Material A is an elastomer containing structural units derived from styrene. <1> ~ <4> 13. The polymer film according to claim 12, <6> Material A is at least one selected from the group consisting of styrene-ethylene-butylene-styrene block copolymers, styrene-isobutylene-styrene block copolymers, styrene-ethylene-propylene-styrene copolymers, styrene-isoprene-styrene block copolymers, and hydrogenated products thereof; <1> ~ <5> 13. The polymer film according to claim 12, <7> Material B includes an aromatic polyester amide; <1> ~ <6> 13. The polymer film according to claim 12, <8> A layer A and a layer B disposed on at least one surface of the layer A, Layer B is a laminate comprising material A that is liquid at 260°C and material B that is solid at 260°C, containing voids with a length in the major axis direction of 0.01 μm or more, having an elastic modulus at 160°C of 0.60 MPa or less, and having a dielectric tangent of 0.01 or less. Effect of the Invention

[0008] According to one embodiment of the present disclosure, a polymer film and a laminate having excellent step conformability and heat resistance are provided. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0009] The contents of the present disclosure will be described in detail below. The following description of the components may be based on a representative embodiment of the present disclosure, but the present disclosure is not limited to such an embodiment. In this specification, the use of "to" indicating a numerical range means that the numerical values ​​before and after it are included as the lower limit and upper limit. In the numerical ranges described in the present disclosure in stages, the upper or lower limit value described in one numerical range may be replaced with the upper or lower limit value of another numerical range described in stages. In addition, in the numerical ranges described in the present disclosure, the upper or lower limit value of the numerical range may be replaced with a value shown in the examples. In addition, in the description of groups (atomic groups) in this specification, descriptions that do not indicate whether they are substituted or unsubstituted include those that have no substituents as well as those that have a substituent. For example, an "alkyl group" includes not only an alkyl group that has no substituents (unsubstituted alkyl groups) but also an alkyl group that has a substituent (substituted alkyl groups). In this specification, "(meth)acrylic" is a term used as a concept including both acrylic and methacrylic, and "(meth)acryloyl" is a term used as a concept including both acryloyl and methacryloyl. In addition, the term "process" in this specification includes not only an independent process but also a process that cannot be clearly distinguished from other processes, as long as the intended purpose of the process is achieved. Furthermore, in the present disclosure, a combination of two or more preferred embodiments is a more preferred embodiment. be. In addition, unless otherwise specified, the weight average molecular weight (Mw) and number average molecular weight (Mn) in the present disclosure are molecular weights detected by a gel permeation chromatography (GPC) analyzer using a column of TSKgel SuperHM-H (product name of Tosoh Corporation) in a solvent of PFP (pentafluorophenol) / chloroform = 1 / 2 (mass ratio) and a differential refractometer, and converted using polystyrene as a standard substance.

[0010] [Polymer film] The polymer film according to the present disclosure comprises material A which is liquid at 260°C and material B which is solid at 260°C, contains voids with a length in the major axis direction of 0.01 μm or more, has an elastic modulus at 160°C of 0.60 MPa or less, and has a dielectric tangent of 0.01 or less.

[0011] As a result of extensive investigations, the present inventors have found that the above-mentioned configuration makes it possible to provide a polymer film having excellent step conformability and heat resistance. Although the detailed mechanism by which the above effects are obtained is unclear, it is speculated as follows.

[0012] In the reflow soldering process carried out when mounting electronic components, the film is heated at high temperatures (e.g., 260°C), during which the water contained in the polymer film becomes supersaturated and diffuses, which is thought to cause bubble nuclei to form. The polymer film contains voids with a length of 0.01 μm or more in the long axis direction, which allows water to enter the voids and inhibits the growth of bubbles, which is thought to inhibit peeling between the polymer film and the metal layer. In other words, the film has excellent heat resistance. In addition, since the elastic modulus at 160° C. is 0.60 MPa or less, the polymer film has excellent conformability to unevenness.

[0013] In contrast, Patent Documents 1 and 2 do not include any description that focuses on voids.

[0014] <Material A> The polymer film according to the present disclosure includes material A that is liquid at 260° C. Material A may be a low molecular weight compound or a high molecular weight compound, so long as it is liquid at 260° C. The material A may be of only one type, or of two or more types. The fact that it is liquid at 260°C can be confirmed by the fact that its viscosity is 100,000 Pa·s or less when heated to 260°C.

[0015] Among these, from the viewpoint of conformability to unevenness, material A is preferably a thermoplastic resin or a thermoplastic elastomer, an uncured or semi-cured product of a thermosetting resin, or an uncured or semi-cured product of a thermosetting elastomer.

[0016] Examples of thermoplastic resins include polyurethane resins, polyester resins, (meth)acrylic resins, polystyrene resins, fluororesins, polyimide resins, fluorinated polyimide resins, polyamide resins, polyamideimide resins, polyetherimide resins, cellulose acylate resins, polyurethane resins, polyether ether ketone resins, polycarbonate resins, polyolefin resins (e.g., polyethylene resins, polypropylene resins, resins made of cyclic olefin copolymers, alicyclic polyolefin resins), polyarylate resins, polyethersulfone resins, polysulfone resins, fluorene ring-modified polycarbonate resins, alicyclic modified polycarbonate resins, and fluorene ring-modified polyester resins.

[0017] Examples of the thermoplastic elastomer include elastomers containing structural units derived from styrene (polystyrene-based elastomers), polyester-based elastomers, polyolefin-based elastomers, polyurethane-based elastomers, polyamide-based elastomers, polyacrylic-based elastomers, silicone-based elastomers, polyimide-based elastomers, etc. The thermoplastic elastomer may be a hydrogenated product.

[0018] Examples of polystyrene-based elastomers include styrene-butadiene-styrene block copolymers (SBS), styrene-isoprene-styrene block copolymers (SIS), polystyrene-poly(ethylene-propylene) diblock copolymers (SEP), polystyrene-poly(ethylene-propylene)-polystyrene triblock copolymers (SEPS), styrene-ethylene-butylene-styrene block copolymers (SEBS), and polystyrene-poly(ethylene / ethylene-propylene)-polystyrene triblock copolymers (SEEPS), styrene-isobutylene-styrene block copolymers (SIBS), and hydrogenated products thereof.

[0019] Among these, from the viewpoints of dielectric tangent and step-following ability, material A is preferably a thermoplastic elastomer, more preferably an elastomer containing a structural unit derived from styrene, and even more preferably at least one selected from the group consisting of a styrene-ethylene-butylene-styrene block copolymer, a styrene-isobutylene-styrene block copolymer, a styrene-ethylene-propylene-styrene copolymer, a styrene-isoprene-styrene block copolymer, and hydrogenated products thereof.

[0020] From the viewpoint of achieving both the ability to conform to unevenness and processability, the content of material A is preferably 40% by mass to 95% by mass, and more preferably 60% by mass to 90% by mass, based on the total mass of the polymer film.

[0021] The weight average molecular weight of the material A is preferably 1,000 or more, more preferably 10,000 or more, and even more preferably 30,000 or more. The upper limit of the weight average molecular weight is, for example, 1,000,000.

[0022] Material A is preferably used as a powder in the production of the polymer film. More preferably, the method of converting material A into a powder includes a swelling step of swelling material A with a liquid medium and a crushing step of crushing the swollen material A.

[0023] The liquid medium used in the swelling step is not particularly limited as long as it is a compound that is liquid at 25°C. When the swelling step is performed under heated conditions, a compound that becomes liquid at the heated temperature can be used. Examples of the liquid medium include water and organic solvents. The liquid medium may be one type or two or more types.

[0024] Examples of organic solvents include alcohols, ketones, alkyl halides, amides, sulfoxides, heterocyclic compounds, hydrocarbons, esters, and ethers.

[0025] In particular, from the viewpoint of swelling a specific polymer in a liquid medium, the absolute value of the difference between the solubility parameter of the liquid medium and the solubility parameter of a polymer having a weight average molecular weight of 1000 or more is 5 MPa. 1 / 2 ~10MPa 1 / 2 Preferably, the pressure is 6 MPa. 1 / 2 ~8MPa 1 / 2 It is more preferable that:

[0026] When two or more liquid media are used, the solubility parameter of the liquid media is a weighted average value.

[0027] In the present disclosure, the solubility parameter used is the Hansen solubility parameter. Hansen solubility parameters are calculated by Hildebrand. The solubility parameter introduced in the present invention is divided into three components, namely, the dispersion term δd, the polarity term δp, and the hydrogen bond term δh, and is expressed in a three-dimensional space. In this disclosure, the solubility parameter is expressed as δ (unit: MPa 1 / 2 ) and the value calculated using the following formula is used. δ(MPa) 1 / 2 =(δd 2 +δp 2 +δh 2 ) 1 / 2 The dispersion term δd, polar term δp, and hydrogen bond term δh have been extensively studied by Hansen and his successors, and are described in detail in Polymer Handbook (fourth edition), VII-698 to 711. Details of the Hansen solubility parameters are described in the book "Hansen Solubility Parameters; A Users Handbook (CRC Press, 2007)" by Charles M. Hansen. The solubility parameter of a polymer can be calculated from the molecular structure of the polymer by the Hoy method described in Polymer Handbook (fourth edition).

[0028] In the swelling step, from the viewpoint of making the particle size smaller by pulverization, the swelling degree of the swollen material A is preferably 1% to 1000%, more preferably 50% to 500%, and further preferably 100% to 250%.

[0029] In the present disclosure, the swelling degree is calculated by the following method. After swelling the polymer with a liquid medium, a measurement sample of about 1 g is taken from the swollen polymer and weighed. The weighed mass is designated as W1 (g). The measurement sample is dried for 3 hours and the dried measurement sample is weighed. The weighed mass is designated as W0 (g). The swelling degree is calculated from the following formula. The drying temperature when drying the measurement sample is the higher of the boiling point of the liquid medium used to swell the polymer and the glass transition temperature of the polymer. Swelling degree (%) = {(W1-W0) / W0} x 100

[0030] When material A is swelled with the liquid medium, the temperature of the liquid medium is not particularly limited as long as the liquid medium is in a liquid state, and is preferably, for example, 10°C to 60°C.

[0031] The means for pulverizing the swollen material A is not particularly limited, and examples thereof include a combination of a mortar and a pestle, and a pulverizer (for example, a ball mill, a bead mill, a roller mill, a jet mill, a hammer mill, an attritor, etc.).

[0032] After swelling, material A may be pulverized at room temperature. However, from the viewpoint of obtaining a powder with a smaller particle size, it is preferable to cool the swollen material A in an environment at a temperature of -50°C or lower and then pulverize it.

[0033] The temperature to which the swollen material A is cooled is preferably lower than the melting point of the liquid medium, and more preferably 10° C. or more lower than the melting point of the liquid medium. Specifically, the temperature to which the swollen material A is cooled is more preferably −80° C. or lower, and even more preferably −100° C. or lower.

[0034] <Material B> The polymer film according to the present disclosure contains a material B that is solid at 260° C. Material B may be a low molecular weight compound or a high molecular weight compound, so long as it is solid at 260° C. The material B may be one type only, or two or more types. The fact that it is a solid at 260°C can be confirmed by the fact that the elastic modulus when heated to 260°C is 0.1 MPa or more.

[0035] Examples of material B include thermosetting resins such as liquid crystal polymers, fluororesins, polymers of compounds having a cyclic aliphatic hydrocarbon group and a group having an ethylenically unsaturated bond, polyphenylene ether and modified products thereof, aromatic polyether ketone, phenolic resins, epoxy resins, polyimides, cyanate resins, bismaleimide resins, and triazine resins.

[0036] -Liquid crystal polymer- From the viewpoint of dielectric loss tangent, it is preferable that material B contains a liquid crystal polymer.

[0037] The type of liquid crystal polymer is not particularly limited, and any known liquid crystal polymer can be used. The liquid crystal polymer may be a thermotropic liquid crystal polymer that exhibits liquid crystallinity in a molten state, or a lyotropic liquid crystal polymer that exhibits liquid crystallinity in a solution state. In the case of a thermotropic liquid crystal, it is preferable that the liquid crystal polymer melts at a temperature of 450° C. or less.

[0038] Examples of liquid crystal polymers include liquid crystal polyester, liquid crystal polyester amide in which an amide bond is introduced into a liquid crystal polyester, liquid crystal polyester ether in which an ether bond is introduced into a liquid crystal polyester, and liquid crystal polyester carbonate in which a carbonate bond is introduced into a liquid crystal polyester.

[0039] From the viewpoint of liquid crystallinity, the liquid crystal polymer is preferably a polymer having an aromatic ring, and more preferably an aromatic polyester or an aromatic polyester amide.

[0040] Furthermore, the liquid crystal polymer may be a polymer in which an isocyanate-derived bond such as an imide bond, a carbodiimide bond, or an isocyanurate bond is further introduced into an aromatic polyester or an aromatic polyester amide.

[0041] The liquid crystal polymer is preferably a wholly aromatic liquid crystal polymer made using only aromatic compounds as raw material monomers.

[0042] Examples of the liquid crystal polymer include the following liquid crystal polymers. 1) (i) A compound obtained by polycondensation of an aromatic hydroxycarboxylic acid, (ii) an aromatic dicarboxylic acid, and (iii) at least one compound selected from the group consisting of an aromatic diol, an aromatic hydroxyamine, and an aromatic diamine. 2) Those obtained by polycondensation of multiple types of aromatic hydroxycarboxylic acids. 3) (i) a polycondensation product of an aromatic dicarboxylic acid and (ii) at least one compound selected from the group consisting of an aromatic diol, an aromatic hydroxyamine, and an aromatic diamine. 4) (i) Polyester such as polyethylene terephthalate and (ii) aromatic hydroxycarboxylic acid are polycondensed. Here, the aromatic hydroxycarboxylic acid, aromatic dicarboxylic acid, aromatic diol, aromatic hydroxyamine and aromatic diamine may each independently be replaced with a derivative capable of undergoing polycondensation.

[0043] The melting point of the liquid crystal polymer is preferably higher than 260°C, more preferably higher than 260°C and 350°C or lower, and further preferably higher than 260°C and 330°C or lower.

[0044] In the present disclosure, the melting point is measured using a differential scanning calorimeter. For example, it is measured using a product named "DSC-60A Plus" (manufactured by Shimadzu Corporation). The temperature rise rate in the measurement is 10°C / min.

[0045] The weight average molecular weight of the liquid crystal polymer is preferably 1,000,000 or less, more preferably 3,000 to 300,000, further preferably 5,000 to 100,000, and particularly preferably 5,000 to 30,000.

[0046] From the viewpoint of further reducing the dielectric tangent, the liquid crystal polymer preferably contains an aromatic polyesteramide. The aromatic polyesteramide is a resin having at least one aromatic ring and having an ester bond and an amide bond. Among them, from the viewpoint of heat resistance, the aromatic polyesteramide is preferably a wholly aromatic polyesteramide.

[0047] The aromatic polyester amide is preferably a crystalline polymer. The material B preferably contains a crystalline aromatic polyester amide. When the aromatic polyester amide is crystalline, the dielectric loss tangent is further reduced. The term "crystalline polymer" refers to a polymer that has a clear endothermic peak, not a stepwise change in endothermic amount, in differential scanning calorimetry (DSC). Specifically, for example, it means that the half-width of the endothermic peak is within 10°C when measured at a heating rate of 10°C / min. Polymers with a half-width exceeding 10°C and polymers without a clear endothermic peak are classified as amorphous polymers and are distinguished from crystalline polymers.

[0048] The aromatic polyester amide preferably contains a constitutional unit represented by the following formula 1, a constitutional unit represented by the following formula 2, and a constitutional unit represented by the following formula 3. -O-Ar 1 -CO- …Formula 1 -CO-Ar 2 -CO- …Formula 2 -NH-Ar 3 -O- …Formula 3 In formulas 1 to 3, Ar 1 , Ar 2 , and Ar 3 each independently represents a phenylene group, a naphthylene group, or a biphenylylene group. Hereinafter, the structural unit represented by formula 1 will also be referred to as "unit 1", etc.

[0049] The unit 1 can be introduced, for example, by using an aromatic hydroxycarboxylic acid as a raw material. The unit 2 can be introduced, for example, by using an aromatic dicarboxylic acid as a raw material. Unit 3 can be introduced, for example, by using an aromatic hydroxylamine as a starting material.

[0050] Here, the aromatic hydroxycarboxylic acid, aromatic dicarboxylic acid, aromatic diol, and aromatic hydroxylamine may each independently be replaced with a derivative capable of undergoing polycondensation.

[0051] For example, aromatic hydroxycarboxylic acids and aromatic dicarboxylic acids can be replaced with aromatic hydroxycarboxylic acid esters and aromatic dicarboxylic acid esters by converting the carboxy group to an alkoxycarbonyl group or an aryloxycarbonyl group. Aromatic hydroxycarboxylic acids and aromatic dicarboxylic acids can be replaced with aromatic hydroxycarboxylic acid halides and aromatic dicarboxylic acid halides by converting the carboxy groups to haloformyl groups. Aromatic hydroxycarboxylic acids and aromatic dicarboxylic acids can be replaced with aromatic hydroxycarboxylic acid anhydrides and aromatic dicarboxylic acid anhydrides by converting the carboxy groups to acyloxycarbonyl groups. Examples of polycondensable derivatives of compounds having a hydroxy group, such as aromatic hydroxycarboxylic acids and aromatic hydroxyamines, include those obtained by acylation of a hydroxy group into an acyloxy group (acylated products). For example, aromatic hydroxycarboxylic acids and aromatic hydroxylamines can be replaced with their acylated counterparts by acylation of the hydroxy group to convert it to an acyloxy group. Examples of the polycondensable derivatives of aromatic hydroxylamines include those obtained by acylation of the amino group to an acylamino group (acylated product). For example, aromatic hydroxyamines can be replaced with acylated products by acylation of the amino group to convert them to acylamino groups.

[0052] In formula 1, Ar 1 is preferably a p-phenylene group, a 2,6-naphthylene group, or a 4,4'-biphenylylene group, and more preferably a 2,6-naphthylene group.

[0053] Ar 1 When is a p-phenylene group, unit 1 is, for example, a constitutional unit derived from p-hydroxybenzoic acid. Ar 1 is a 2,6-naphthylene group, unit 1 is, for example, a constitutional unit derived from 6-hydroxy-2-naphthoic acid. Ar 1 When is a 4,4'-biphenylylene group, unit 1 is, for example, a constitutional unit derived from 4'-hydroxy-4-biphenylcarboxylic acid.

[0054] In formula 2, Ar 2 is preferably a p-phenylene group, an m-phenylene group, or a 2,6-naphthylene group, and more preferably an m-phenylene group.

[0055] Ar 2 When is a p-phenylene group, unit 2 is, for example, a constitutional unit derived from terephthalic acid. Ar 2 When is an m-phenylene group, unit 2 is, for example, a constitutional unit derived from isophthalic acid. Ar 2is a 2,6-naphthylene group, unit 2 is, for example, a constitutional unit derived from 2,6-naphthalenedicarboxylic acid.

[0056] In formula 3, Ar 3 is preferably a p-phenylene group or a 4,4'-biphenylylene group, and more preferably a p-phenylene group.

[0057] Ar 3 When is a p-phenylene group, unit 3 is, for example, a constitutional unit derived from p-aminophenol. Ar 3 is a 4,4'-biphenylylene group, unit 3 is, for example, a constitutional unit derived from 4-amino-4'-hydroxybiphenyl.

[0058] With respect to the total content of units 1, 2, and 3, the content of units 1 is preferably 30 mol% or more, the content of units 2 is preferably 35 mol% or less, and the content of units 3 is preferably 35 mol% or less. The content of unit 1 is more preferably 30 mol % to 80 mol %, further preferably 30 mol % to 60 mol %, and particularly preferably 30 mol % to 40 mol %, based on the total content of unit 1, unit 2, and unit 3. The content of unit 2 is preferably 10 mol % to 35 mol %, more preferably 20 mol % to 35 mol %, and particularly preferably 30 mol % to 35 mol %, based on the total content of unit 1, unit 2, and unit 3. The content of unit 3 is preferably 10 mol % to 35 mol %, more preferably 20 mol % to 35 mol %, and particularly preferably 30 mol % to 35 mol %, based on the total content of unit 1, unit 2, and unit 3. The total content of each structural unit is the sum of the amounts (moles) of each structural unit, which is calculated by dividing the mass of each structural unit constituting the aromatic polyesteramide by the formula weight of the structural unit.

[0059] The ratio of the content of units 2 to the content of units 3, expressed as [content of units 2] / [content of units 3] (mol / mol), is preferably 0.9 / 1 to 1 / 0.9, more preferably 0.95 / 1 to 1 / 0.95, and even more preferably 0.98 / 1 to 1 / 0.98.

[0060] The aromatic polyesteramide may have two or more independent types of the units 1 to 3. The aromatic polyesteramide may have other structural units than the units 1 to 3. The content of the other structural units is preferably 10 mol % or less, more preferably 5 mol % or less, based on the total content of all the structural units.

[0061] The aromatic polyesteramide is preferably produced by melt-polymerizing raw material monomers corresponding to the structural units constituting the aromatic polyesteramide.

[0062] The weight average molecular weight of the aromatic polyesteramide is preferably 1,000,000 or less, more preferably 3,000 to 300,000, further preferably 5,000 to 100,000, and particularly preferably 5,000 to 30,000.

[0063] -Fluoroplastics- Material B may be a fluororesin from the viewpoints of heat resistance and mechanical strength.

[0064] In the present disclosure, the type of fluororesin is not particularly limited, and any known fluororesin can be used.

[0065] Fluorine resins include homopolymers and copolymers that contain constitutional units derived from fluorinated α-olefin monomers, i.e., α-olefin monomers that contain at least one fluorine atom, and also include copolymers that contain constitutional units derived from fluorinated α-olefin monomers and constitutional units derived from non-fluorinated ethylenically unsaturated monomers that are reactive with the fluorinated α-olefin monomers.

[0066] Fluorinated α-olefin monomers include CF2=CF2, CHF=CF2, CH2=CF2, CHCl=CHF, CClF=CF2, CCl2=CF2, CClF=CClF, CHF=CCl2, CH2=CClF, CCl2=CClF, CF3CF=CF2, CF3CF=CHF, CF3CH=CF2, CF3CH=CH2, CHF2CH=CHF, CF3CF=CF2, and perfluoro(alkyl having 2 to 8 carbon atoms)vinyl ethers (e.g., perfluoromethyl vinyl ether, perfluoropropyl vinyl ether, and perfluorooctyl vinyl ether). Among them, the fluorinated α-olefin monomer is preferably at least one monomer selected from the group consisting of tetrafluoroethylene (CF2=CF2), chlorotrifluoroethylene (CClF=CF2), (perfluorobutyl)ethylene, vinylidene fluoride (CH2=CF2), and hexafluoropropylene (CF2=CFCF3). Non-fluorinated ethylenically unsaturated monomers include ethylene, propylene, butene, ethylenically unsaturated aromatic monomers (eg, styrene and α-methylstyrene), and the like. The fluorinated α-olefin monomers may be used alone or in combination of two or more kinds. The non-fluorinated ethylenically unsaturated monomers may be used alone or in combination of two or more kinds.

[0067] Examples of fluororesins include polychlorotrifluoroethylene (PCTFE), poly(chlorotrifluoroethylene-propylene), poly(ethylene-tetrafluoroethylene) (ETFE), poly(ethylene-chlorotrifluoroethylene) (ECTFE), poly(hexafluoropropylene), poly(tetrafluoroethylene) (PTFE), poly(tetrafluoroethylene-ethylene-propylene), poly(tetrafluoroethylene-hexafluoropropylene) (FEP), poly(tetrafluoroethylene-propylene) (FEPM), poly(tetrafluoroethylene-perfluoropropylene vinyl ether), poly(tetrafluoroethylene-perfluoroalkyl vinyl ether) (PFA) (e.g., poly(tetrafluoroethylene-perfluoropropyl vinyl ether)), polyvinyl fluoride (PVF), polyvinylidene fluoride (PVDF), poly(vinylidene fluoride-chlorotrifluoroethylene), perfluoropolyether, perfluorosulfonic acid, and perfluoropolyoxetane.

[0068] The fluororesin may have structural units derived from fluorinated ethylene or fluorinated propylene. The fluororesin may be used alone or in combination of two or more kinds.

[0069] The fluororesin is preferably FEP, PFA, ETFE or PTFE. FEP is available from DuPont under the trade name TEFLON FEP, or from Daikin Industries, Ltd. under the trade name NEOFLON FEP. PFA is available from Daikin Industries, Ltd. under the trade name NEOFLON PFA, from DuPont under the trade name TEFLON PFA, or from Solvay Solexis under the trade name HYFLON PFA.

[0070] More preferably, the fluororesin comprises PTFE. The PTFE may be a PTFE homopolymer, a partially modified PTFE homopolymer, or a combination comprising one or both of these. The partially modified PTFE homopolymer preferably comprises less than 1% by mass of units derived from comonomers other than tetrafluoroethylene, based on the total mass of the polymer.

[0071] The fluororesin may be a crosslinkable fluoropolymer having a crosslinkable group. The crosslinkable fluoropolymer can be crosslinked by a conventionally known crosslinking method. One representative crosslinkable fluoropolymer is a fluoropolymer having (meth)acryloyloxy. For example, the crosslinkable fluoropolymer is Formula:H2C=CR'COO-(CH2) n -R-(CH2) n -OOCR'=CH2 In the formula, R is an oligomer chain containing a constituent unit derived from a fluorinated α-olefin monomer, R' is H or -CH3, and n is 1 to 4. R may be a fluorine-based oligomer chain containing a constituent unit derived from tetrafluoroethylene.

[0072] A crosslinked fluoropolymer network can be formed by exposing a fluoropolymer having (meth)acryloyloxy groups to a free radical source to initiate a radical crosslinking reaction via the (meth)acryloyloxy groups on the fluororesin. The free radical source is not particularly limited, but preferably includes a photoradical polymerization initiator or an organic peroxide. Suitable photoradical polymerization initiators and organic peroxides are well known in the art. Crosslinkable fluoropolymers are commercially available, such as Viton B manufactured by DuPont.

[0073] -Polymer of a compound having a cyclic aliphatic hydrocarbon group and a group having an ethylenically unsaturated bond- Material B may be a polymer of a compound having a cyclic aliphatic hydrocarbon group and a group having an ethylenically unsaturated bond.

[0074] Examples of polymers of compounds having a cyclic aliphatic hydrocarbon group and a group having an ethylenically unsaturated bond include thermoplastic resins having structural units derived from cyclic olefin monomers such as norbornene or polycyclic norbornene monomers.

[0075] The polymer of the compound having a cyclic aliphatic hydrocarbon group and a group having an ethylenically unsaturated bond may be a ring-opening polymer of the above-mentioned cyclic olefin or a hydrogenated product of a ring-opening copolymer using two or more kinds of cyclic olefins, or may be an addition polymer of a cyclic olefin and an aromatic compound having an ethylenically unsaturated bond such as a chain olefin or a vinyl group. A polar group may be introduced into the polymer of the compound having a cyclic aliphatic hydrocarbon group and a group having an ethylenically unsaturated bond.

[0076] The polymer of a compound having a cyclic aliphatic hydrocarbon group and a group having an ethylenically unsaturated bond may be used alone or in combination of two or more kinds.

[0077] The ring structure of the cyclic aliphatic hydrocarbon group may be a monocyclic ring, a condensed ring in which two or more rings are condensed, or a bridged ring. Examples of the ring structure of the cyclic aliphatic hydrocarbon group include a cyclopentane ring, a cyclohexane ring, a cyclooctane ring, an isophorone ring, a norbornane ring, and a dicyclopentane ring. The compound having a cyclic aliphatic hydrocarbon group and a group having an ethylenically unsaturated bond is not particularly limited, and may be a (meth)acrylate compound having a cyclic aliphatic hydrocarbon group, a (meth)acrylamide compound having a cyclic aliphatic hydrocarbon group, or a vinyl compound having a cyclic aliphatic hydrocarbon group. Among them, a (meth)acrylate compound having a cyclic aliphatic hydrocarbon group is preferred. In addition, the compound having a cyclic aliphatic hydrocarbon group and a group having an ethylenically unsaturated bond may be a monofunctional ethylenically unsaturated compound or a polyfunctional ethylenically unsaturated compound. The number of cycloaliphatic hydrocarbon groups in a compound having a cycloaliphatic hydrocarbon group and a group having an ethylenically unsaturated bond may be one or more, and may be two or more. The polymer of a compound having a cyclic aliphatic hydrocarbon group and a group having an ethylenically unsaturated bond may be a polymer obtained by polymerizing at least one compound having a cyclic aliphatic hydrocarbon group and a group having an ethylenically unsaturated bond, and may be a polymer of a compound having two or more types of cyclic aliphatic hydrocarbon groups and a group having an ethylenically unsaturated bond, or may be a copolymer with another ethylenically unsaturated compound that does not have a cyclic aliphatic hydrocarbon group. The polymer of a compound having a cyclic aliphatic hydrocarbon group and a group having an ethylenically unsaturated bond is preferably a cycloolefin polymer.

[0078] -Polyphenylene ether- Material B may be a polyphenylene ether. The polyphenylene ether preferably has an average number of phenolic hydroxyl groups at the molecular terminals (number of terminal hydroxyl groups) per molecule of 1 to 5, and more preferably 1.5 to 3, from the viewpoints of dielectric tangent and heat resistance. The number of terminal hydroxyl groups of polyphenylene ether can be known from, for example, the specification value of the polyphenylene ether product. The number of terminal hydroxyl groups is expressed, for example, as the average number of phenolic hydroxyl groups per molecule of all polyphenylene ethers present in 1 mole of polyphenylene ether. The polyphenylene ether may be used alone or in combination of two or more kinds.

[0079] Examples of polyphenylene ethers include polyphenylene ethers composed of 2,6-dimethylphenol and at least one of a difunctional phenol and a trifunctional phenol, and poly(2,6-dimethyl-1,4-phenylene oxide). More specifically, the polyphenylene ether is preferably a compound having a structure represented by the formula (PPE).

[0080] [ka]

[0081] In formula (PPE), X represents an alkylene group having 1 to 3 carbon atoms or a single bond, m represents an integer of 0 to 20, n represents an integer of 0 to 20, and the sum of m and n represents an integer of 1 to 30. The alkylene group in X may, for example, be a dimethylmethylene group.

[0082] When the polyphenylene ether is thermally cured after film formation, from the viewpoints of heat resistance and film formability, the weight average molecular weight (Mw) is preferably 500 to 5,000, and more preferably 500 to 3,000. When the polyphenylene ether is not thermally cured, the weight average molecular weight (Mw) is not particularly limited, but is preferably 3,000 to 100,000, and more preferably 5,000 to 50,000.

[0083] -Aromatic polyether ketone- Material B may be an aromatic polyether ketone.

[0084] The aromatic polyether ketone is not particularly limited, and any known aromatic polyether ketone can be used.

[0085] The aromatic polyether ketone is preferably a polyether ether ketone.

[0086] Polyetheretherketone is a type of aromatic polyetherketone, and is a polymer in which bonds are arranged in the following order: ether bond, ether bond, and carbonyl bond. Each bond is preferably linked by a divalent aromatic group. The aromatic polyether ketones may be used alone or in combination of two or more kinds.

[0087] Examples of aromatic polyetherketones include polyetheretherketone (PEEK) having a chemical structure represented by the following formula (P1), polyetherketone (PEK) having a chemical structure represented by the following formula (P2), polyetherketoneketone (PEKK) having a chemical structure represented by the following formula (P3), polyetheretherketoneketone (PEEKK) having a chemical structure represented by the following formula (P4), and polyetherketoneetherketoneketone (PEKEKK) having a chemical structure represented by the following formula (P5).

[0088] [ka]

[0089] From the viewpoint of mechanical properties, n in each of the formulas (P1) to (P5) is preferably 10 or more, and more preferably 20 or more. On the other hand, from the viewpoint of easiness in producing the aromatic polyether ketone, n is preferably 5,000 or less, and more preferably 1,000 or less. That is, n is preferably 10 to 5,000, and more preferably 20 to 1,000.

[0090] Furthermore, material B may be in particulate form. When material B is in particulate form, material B may be organic particles or inorganic particles. When the polymer film contains particulate material B, it preferably also contains material B that is not particulate.

[0091] Examples of the resin constituting the organic particles include polyethylene, polystyrene, urea-formalin filler, polyester, cellulose, acrylic resin, fluororesin, cured epoxy resin, crosslinked benzoguanamine resin, crosslinked acrylic resin, and liquid crystal polymer. The resin constituting the organic particles may be one type or two or more types.

[0092] The organic particles may be fibrous, such as nanofibers, or hollow resin particles.

[0093] Among them, from the viewpoint of dielectric loss tangent and step followability, the organic particles are preferably fluororesin particles, polyester resin particles, polyethylene particles, liquid crystal polymer particles, or nanofibers of cellulose resin, more preferably polytetrafluoroethylene particles, polyethylene particles, or liquid crystal polymer particles, and particularly preferably liquid crystal polymer particles. Here, the liquid crystal polymer particles refer to, but are not limited to, a powdered liquid crystal obtained by polymerizing a liquid crystal polymer and pulverizing it with a pulverizer or the like. The preferred embodiments of the liquid crystal polymer constituting the liquid crystal polymer particles are the same as those of the liquid crystal polymer described above.

[0094] The average particle size of the organic particles is preferably from 5 nm to 20 μm, and more preferably from 100 nm to 10 μm, from the viewpoints of dielectric tangent and step conformability.

[0095] Examples of compounds constituting the inorganic particles include BN, Al2O3, AlN, TiO2, SiO2, barium titanate, strontium titanate, aluminum hydroxide, and calcium carbonate. The compounds constituting the inorganic particles may be one type or two or more types.

[0096] Among these, as the inorganic particles, from the viewpoints of dielectric tangent and step-following ability, metal oxide particles or fibers are preferred, silica particles, titania particles, or glass fibers are more preferred, and silica particles or glass fibers are particularly preferred.

[0097] From the viewpoint of dielectric tangent and step conformability, the average particle size of the inorganic particles is preferably 5 nm to 20 μm, more preferably 10 nm to 10 μm, further preferably 20 nm to 1 μm, and particularly preferably 25 nm to 500 nm.

[0098] In addition, material A and material B may contain a foaming agent that disappears or decomposes to release gas when heated. The foaming agent may be an organic foaming agent or an inorganic foaming agent.

[0099] Examples of organic foaming agents include particles containing an acrylic resin as a main component, particles containing an ethyl cellulose resin as a main component, particles containing a butyral resin as a main component, nitrosamine compounds such as dinitrosopentamethylenetetramine (DPT), azo compounds such as azodicarbonamide (ADCA), and hydrazine compounds such as 4,4'-oxybisbenzenesulfonylhydrazide (OBSH) and hydrazodicarbonamide (HDCA).

[0100] Examples of inorganic foaming agents include bicarbonates such as sodium bicarbonate; carbonates; and combinations of bicarbonates and organic acid salts such as sodium citrate.

[0101] From the viewpoint of heat resistance, the content of material B is preferably 5% by mass to 60% by mass, and more preferably 10% by mass to 40% by mass, based on the total mass of the polymer film.

[0102] The polymer film according to the present disclosure may contain, in addition to material A and material B, other additives. As the other additives, known additives can be used, such as a curing agent, a leveling agent, a defoaming agent, an antioxidant, an ultraviolet absorbing agent, a flame retardant, and a colorant.

[0103] <Void> The polymer film according to the present disclosure contains voids having a length in the major axis direction of 0.01 μm or more.

[0104] In the reflow soldering process carried out when mounting electronic components, the film is heated at high temperatures (e.g., 260°C), during which the water contained within the polymer film becomes supersaturated and diffuses, thought to cause the generation of bubble nuclei. It is thought that the polymer film contains voids with a length of 0.01 μm or more in the long axis direction, allowing water to enter the voids and suppressing the growth of bubbles, thereby suppressing peeling between the polymer film and the metal layer.

[0105] From the viewpoint of further improving heat resistance, the length of the voids in the major axis direction is preferably 0.5 μm to 10 μm.

[0106] The length in the long axis direction means the length of the longest part of the void, and the length in the short axis direction means the length of the shortest part in the direction perpendicular to the long axis direction.

[0107] The length of the voids in the minor axis direction is not particularly limited, and is, for example, 0.01 μm to 10 μm. The shape of the voids is not particularly limited, and may be, for example, elliptical, circular, or needle-like.

[0108] In the present disclosure, the length of a void in the major axis direction is measured by the following method. First, the surface of the polymer film is cut with a microtome to prepare a film cross-section sample. The cross-section is observed in 100 fields of view at 10,000 times magnification with a scanning electron microscope (SEM). 100 voids are arbitrarily selected. The length in the major axis direction of each selected void is measured, and the average value is used.

[0109] From the viewpoint of further improving heat resistance, the proportion of voids in the total volume of the polymer film (porosity) is preferably 1 to 15% by volume, and more preferably 4 to 9% by volume.

[0110] In the present disclosure, the porosity is measured by the following method. In the same manner as in the method of measuring the length of the long axis of the voids, 100 voids are selected at random. The cross-sectional area of ​​each selected void is measured. The void ratio is calculated based on the following formula. Porosity = {(total cross-sectional area of ​​voids) / (cross-sectional area of ​​polymer film)} x 100

[0111] Furthermore, from the viewpoint of further improving heat resistance, the distance between the gap and material B is preferably 5 μm or less, and more preferably 2 μm or less. The lower limit of the distance is not particularly limited, but is, for example, 0 μm.

[0112] Since material B is a solid at 260°C, it is believed that if the distance between the gap and material B is 5 μm or less, material B suppresses the growth of air bubbles, thereby suppressing peeling between the polymer film and the metal layer.

[0113] The distance between the gap and material B is measured by the following method. A cross-sectional sample is prepared by cutting the surface of the polymer film with a microtome. The cross-section is observed with an optical microscope at 50x magnification to confirm the distribution of material B. The same cross-sectional sample is observed with a scanning electron microscope (SEM) at 10,000x magnification to observe voids in the same position as the field of view observed with the optical microscope. For any 100 voids obtained, the distance to the nearest material B is measured, and the average value is taken as the distance between the void and material B.

[0114] The voids can be formed in the polymer film by, for example, mixing particles, coating and drying the mixture, or adding a foaming agent and subjecting the layer to foaming at a high temperature.

[0115] <Physical properties of polymer film> The polymer film according to the present disclosure has an elastic modulus of 0.60 MPa or less, preferably 500 MPa or less, and more preferably 0.49 MPa or less at 160° C. The lower limit of the elastic modulus at 160° C. is not particularly limited, but is, for example, 0.20 MPa.

[0116] Since the elastic modulus at 160° C. is 0.60 MPa or less, the polymer film has excellent conformability to unevenness.

[0117] In the present disclosure, the elastic modulus of a polymer film at 160° C. is measured by the following method. First, a film cross-section sample (length 2 mm × width 2 mm) is prepared by cutting the surface of a polymer film with a microtome. Next, the 160°C elastic modulus of the film cross-section sample is measured as the indentation elastic modulus using a nanoindentation method. The indentation elastic modulus is measured by applying a load at a loading rate of 0.28 mN / sec with a Vickers indenter using a microhardness tester (e.g., product name "DUH-W201", manufactured by Shimadzu Corporation), holding the maximum load of 10 mN for 10 seconds, and then unloading at a loading rate of 0.28 mN / sec.

[0118] The polymer film according to the present disclosure has a dielectric loss tangent of 0.01 or less, preferably 0.005 or less, and more preferably 0.003 or less. The lower limit of the dielectric loss tangent is not particularly limited, but is, for example, 0.0005.

[0119] In this disclosure, the dielectric loss tangent is measured by the following method. The dielectric loss tangent is measured by the resonance perturbation method at a frequency of 10 GHz. A 10 GHz cavity resonator ("CP531" manufactured by Kanto Electronics Application Development Co., Ltd.) was connected to a 10 GHz cavity resonator ("E8363B" manufactured by Nology Co., Ltd.), and a polymer film was inserted into the cavity resonator. The change in resonance frequency was measured before and after insertion for 96 hours in an environment with a temperature of 25°C and a humidity of 60%.

[0120] The average thickness of the polymer film according to the present disclosure is not particularly limited, but from the viewpoints of dielectric tangent and step conformability, it is preferably 5 μm to 90 μm, more preferably 10 μm to 70 μm, and particularly preferably 15 μm to 50 μm.

[0121] The average thickness of the polymer film is determined by measuring any five points using an adhesive film thickness meter, for example, an electronic micrometer (product name "KG3001A", manufactured by Anritsu Corporation), and averaging these values.

[0122] [Laminate] The laminate according to the present disclosure includes a layer A and a layer B disposed on at least one surface of layer A, where layer B includes material A that is liquid at 260°C and material B that is solid at 260°C, includes voids with a length in the major axis direction of 0.01 μm or more, has an elastic modulus at 160°C of 0.60 MPa or less, and has a dielectric loss tangent of 0.01 or less.

[0123] <Layer A> The laminate according to the present disclosure has a layer A on which a layer B described below is provided. From the viewpoint of making the dielectric loss tangent of the laminate 0.01 or less, it is preferable that the layer A contains a polymer having a dielectric loss tangent of 0.01 or less.

[0124] Layer A may contain only one type of polymer having a dielectric tangent of 0.01 or less, or may contain two or more types of polymers.

[0125] The dielectric tangent of the polymer having a dielectric tangent of 0.01 or less is preferably 0.005 or less, and more preferably greater than 0 and 0.003 or less, from the viewpoint of the dielectric tangent of the laminate.

[0126] Examples of polymers having a dielectric tangent of 0.01 or less include thermoplastic resins such as liquid crystal polymers, fluororesins, polymers of compounds having a cyclic aliphatic hydrocarbon group and a group having an ethylenically unsaturated bond, polyether ether ketone, polyolefin, polyamide, polyester, polyphenylene sulfide, polyether ketone, polycarbonate, polyether sulfone, polyphenylene ether and modified products thereof, and polyether imide; elastomers such as copolymers of glycidyl methacrylate and polyethylene; and thermosetting resins such as phenol resins, epoxy resins, polyimides, and cyanate resins.

[0127] From the viewpoint of the dielectric loss tangent of the laminate, the polymer having a dielectric loss tangent of 0.01 or less is preferably a liquid crystal polymer. That is, it is preferable that Layer A contains a liquid crystal polymer. The preferred embodiment of the liquid crystal polymer is the same as the preferred embodiment of the liquid crystal polymer that may be contained in the polymer film.

[0128] The layer A may contain a filler in addition to the polymer having a dielectric tangent of 0.01 or less.

[0129] The filler may be particulate or fibrous, and may be inorganic or organic particles. Specific examples of the inorganic and organic particles are as described above.

[0130] Among these, the filler contained in Layer A is preferably organic particles, more preferably liquid crystal polymer particles, from the viewpoints of the dielectric tangent, heat resistance, and step conformability of the laminate.

[0131] Layer A may contain only one type of filler, or may contain two or more types of fillers. When Layer A contains a filler, the content of the filler is preferably 30% by mass to 95% by mass, more preferably 50% by mass to 90% by mass, and particularly preferably 60% by mass to 80% by mass, relative to the total mass of Layer A, from the viewpoints of the dielectric tangent, heat resistance, and step-following ability of the laminate.

[0132] Layer A may contain additives other than the above-mentioned components. Preferred embodiments of other additives that may be contained in Layer A are the same as preferred embodiments of other additives that may be contained in the polymer film according to the present disclosure.

[0133] Furthermore, the layer A may contain, as other additives, resins other than the polymer having a dielectric loss tangent of 0.01 or less. Examples of resins other than polymers having a dielectric tangent of 0.01 or less include thermoplastic resins other than liquid crystal polyesters, such as polypropylene, polyamide, polyesters other than liquid crystal polyesters, polyphenylene sulfide, polyether ketone, polycarbonate, polyether sulfone, polyphenylene ether and modified products thereof, and polyether imide; elastomers such as copolymers of glycidyl methacrylate and polyethylene; and thermosetting resins such as phenol resins, epoxy resins, polyimide resins, and cyanate resins.

[0134] The total content of other additives in Layer A is preferably 25 parts by mass or less, more preferably 10 parts by mass or less, and even more preferably 5 parts by mass or less, per 100 parts by mass of the content of the polymer having a dielectric tangent of 0.01 or less.

[0135] The average thickness of layer A is not particularly limited, but from the viewpoints of the dielectric tangent, heat resistance, and suppression of wiring distortion of the laminate, it is preferably 5 μm to 90 μm, more preferably 10 μm to 70 μm, and particularly preferably 15 μm to 50 μm.

[0136] The method for measuring the average thickness of each layer in the laminate according to the present disclosure is as follows.

[0137] The laminate is cut in a plane perpendicular to the plane direction of the laminate, the thickness is measured at five or more points on the cross section, and the average value of the measurements is taken as the average thickness.

[0138] From the viewpoint of making the dielectric loss tangent of the laminate 0.01 or less, the dielectric loss tangent of Layer A is preferably 0.01 or less, more preferably 0.005 or less, and even more preferably greater than 0 and 0.003 or less.

[0139] <Layer B> The laminate according to the present disclosure has a layer B on at least one surface of the layer A. Layer B contains a material A that is liquid at 260°C and a material B that is solid at 260°C, contains voids with a length in the major axis direction of 0.01 µm or more, has an elastic modulus at 160°C of 0.60 MPa or less, and has a dielectric loss tangent of 0.01 or less.

[0140] Preferred embodiments of material A, material B, and voids contained in the laminate according to the present disclosure are the same as the preferred embodiments of material A, material B, and voids contained in the polymer film according to the present disclosure. Material A, which is liquid at 260°C, preferably has an elastic modulus of 0.10 MPa or less at 260°C, and material B, which is solid at 260°C, preferably has an elastic modulus of more than 0.10 MPa at 260°C.

[0141] In addition to material A and material B, layer B may contain other additives. Other additives include the same as other additives that may be included in the polymer films according to the present disclosure.

[0142] From the viewpoint of conformability to unevenness, the average thickness of Layer B is preferably from 5 μm to 50 μm, more preferably from 10 μm to 40 μm, and even more preferably from 15 μm to 30 μm.

[0143] From the viewpoint of adhesion to the metal layer, the laminate according to the present disclosure preferably further has a layer C in addition to the layer A and the layer B, and more preferably has the layer B, the layer A, and the layer C in this order.

[0144] <Layer C> Layer C is preferably an adhesive layer, that is, Layer C is preferably a surface layer (outermost layer).

[0145] From the viewpoint of the dielectric loss tangent of the laminate, the layer C preferably contains at least one polymer.

[0146] A preferred embodiment of the polymer used in the layer C is the same as a preferred embodiment of the polymer used in the layer A having a dielectric tangent of 0.01 or less.

[0147] The polymer contained in Layer C may be the same as or different from the polymer contained in Layer A or Layer B. From the viewpoint of adhesion between Layer A and Layer C, however, it is preferable that the polymer is the same as the polymer contained in Layer A.

[0148] Moreover, in order to bond the metal layer and the layer A, the layer C preferably contains an epoxy resin.

[0149] The epoxy resin is preferably a crosslinked product of a polyfunctional epoxy compound. The polyfunctional epoxy compound refers to a compound having two or more epoxy groups. The number of epoxy groups in the polyfunctional epoxy compound is preferably 2 to 4.

[0150] In particular, from the viewpoints of the dielectric tangent of the laminate and the adhesion to the metal layer, it is preferable that layer C contains an aromatic polyester amide and an epoxy resin.

[0151] The layer C may contain a filler. A preferred embodiment of the filler used in the layer C is the same as a preferred embodiment of the filler used in the layer A.

[0152] Layer C may contain additives other than those mentioned above. Preferred embodiments of the other additives used in Layer C are the same as the preferred embodiments of the other additives used in Layer A, except as described below.

[0153] The average thickness of Layer C is preferably smaller than the average thickness of Layer A from the viewpoints of the dielectric tangent of the laminate and the adhesion to metals.

[0154] Average thickness T of layer A A and the average thickness T of layer C C The ratio of T A / T C From the viewpoints of the dielectric tangent of the laminate and the adhesion to the metal layer, the value of is preferably greater than 1, more preferably 2 to 100, further preferably 2.5 to 20, and particularly preferably 3 to 10. Average thickness T of layer B B and the average thickness T of layer C C The ratio of T B / T C From the viewpoints of the dielectric tangent of the laminate and the adhesion to the metal layer, the value of is preferably greater than 1, more preferably 2 to 100, further preferably 2.5 to 20, and particularly preferably 3 to 10.

[0155] Furthermore, from the viewpoints of the dielectric tangent of the laminate and the adhesion to the metal layer, the average thickness of Layer C is preferably 0.1 μm to 20 μm, more preferably 0.5 μm to 15 μm, even more preferably 1 μm to 10 μm, and particularly preferably 2 μm to 8 μm.

[0156] The average thickness of the laminate according to the present disclosure is preferably 6 μm to 200 μm, more preferably 12 μm to 100 μm, and particularly preferably 20 μm to 80 μm, from the viewpoints of strength and electrical properties (characteristic impedance) when laminated with a metal layer.

[0157] The average thickness of the laminate is determined by measuring any five points using an adhesive film thickness meter, for example, an electronic micrometer (product name "KG3001A", manufactured by Anritsu Corporation), and averaging these values.

[0158] The laminate according to the present disclosure preferably has a dielectric loss tangent of 0.01 or less, more preferably 0.005 or less, and even more preferably greater than 0 and 0.003 or less.

[0159] <Method of manufacturing laminate> (Film forming) The method for producing the laminate according to the present disclosure is not particularly limited, and known methods can be referred to.

[0160] Suitable film-forming methods include, for example, co-casting, multi-layer coating, co-extrusion, etc. Among these, the co-casting method is preferred.

[0161] When the multilayer structure of the laminate is produced by a co-casting method or a multi-layer coating method, it is preferable to carry out the co-casting method or the multi-layer coating method using a composition for forming layer A, a composition for forming layer B, a composition for forming layer C, etc., in which the components of each layer, such as a liquid crystal polymer, are dissolved or dispersed in a solvent.

[0162] Examples of the solvent include halogenated hydrocarbons such as dichloromethane, chloroform, 1,1-dichloroethane, 1,2-dichloroethane, 1,1,2,2-tetrachloroethane, 1-chlorobutane, chlorobenzene, and o-dichlorobenzene; halogenated phenols such as p-chlorophenol, pentachlorophenol, and pentafluorophenol; ethers such as diethyl ether, tetrahydrofuran, and 1,4-dioxane; ketones such as acetone and cyclohexanone; esters such as ethyl acetate and γ-butyrolactone; and ethylene carbonate. Examples of the organic solvent include carbonates such as propylene carbonate and propylene carbonate; amines such as triethylamine; nitrogen-containing heterocyclic aromatic compounds such as pyridine; nitriles such as acetonitrile and succinonitrile; amides such as N,N-dimethylformamide, N,N-dimethylacetamide, N-methylpyrrolidone, and urea compounds such as tetramethylurea; nitro compounds such as nitromethane and nitrobenzene; sulfur compounds such as dimethyl sulfoxide and sulfolane; and phosphorus compounds such as hexamethylphosphoramide and tri-n-butylphosphoric acid, and two or more of these may be used.

[0163] As the solvent, since it is less corrosive and easy to handle, a solvent mainly composed of an aprotic compound, particularly an aprotic compound having no halogen atom, is preferred, and the ratio of the aprotic compound to the entire solvent is preferably 50% by mass to 100% by mass, more preferably 70% by mass to 100% by mass, and particularly preferably 90% by mass to 100% by mass. In addition, as the aprotic compound, since it is easy to dissolve the liquid crystal polymer, it is preferred to use amides such as N,N-dimethylformamide, N,N-dimethylacetamide, tetramethylurea, and N-methylpyrrolidone, or esters such as γ-butyrolactone, and N,N-dimethylformamide, N,N-dimethylacetamide, and N-methylpyrrolidone are more preferred.

[0164] In addition, the solvent is preferably a solvent mainly composed of a compound having a dipole moment of 3 to 5, since it is easy to dissolve the liquid crystal polymer. The proportion of the compounds 3 to 5 is preferably 50% by mass to 100% by mass, more preferably 70% by mass to 100% by mass, and particularly preferably 90% by mass to 100% by mass. As the aprotic compound, a compound having a dipole moment of 3 to 5 is preferably used.

[0165] Furthermore, as the solvent, a solvent mainly composed of a compound having a boiling point of 220° C. or lower at 1 atmospheric pressure is preferred because it is easy to remove, and the proportion of the compound having a boiling point of 220° C. or lower at 1 atmospheric pressure in the entire solvent is preferably 50% by mass to 100% by mass, more preferably 70% by mass to 100% by mass, and particularly preferably 90% by mass to 100% by mass. As the aprotic compound, it is preferable to use a compound having a boiling point of 220° C. or lower at 1 atmospheric pressure.

[0166] In the method for producing a laminate according to the present disclosure, a support may be used when the laminate is produced by the above-mentioned co-casting method, multi-layer coating method, co-extrusion method, or the like. Examples of the support include a metal drum, a metal band, a glass plate, a resin film, and a metal foil. Among these, the support is preferably a metal drum, a metal band, or a resin film. Examples of resin films include polyimide (PI) films, and examples of commercially available products include U-Pirex S and U-Pirex R manufactured by Ube Industries, Ltd., Kapton manufactured by DuPont-Toray Co., Ltd., and IF30, IF70, and LV300 manufactured by SKC Kolon PI. The support may have a surface treatment layer formed on its surface so that it can be easily peeled off. The surface treatment layer may be made of hard chrome plating, fluororesin, or the like. The average thickness of the support is not particularly limited, but is preferably from 25 μm to 75 μm, and more preferably from 50 μm to 75 μm.

[0167] The method for removing at least a part of the solvent from the cast or applied film-like composition (coating film) is not particularly limited, and any known drying method can be used.

[0168] (Stretching) The laminate according to the present disclosure can be appropriately combined with stretching in terms of controlling molecular orientation and adjusting the thermal expansion coefficient and mechanical properties. The stretching method is not particularly limited, and known methods can be referred to. It may be performed in a state containing a solvent or in a dry film state. Stretching in a state containing a solvent may be performed by gripping the laminate and stretching it, or it may be performed by utilizing autogenous shrinkage due to drying without stretching it. Stretching is particularly effective for the purpose of improving the breaking elongation and breaking strength when the film brittleness is reduced by adding an inorganic filler or the like.

[0169] <Application> The laminate according to the present disclosure can be used for various applications, and among others, can be suitably used as a film for electronic components such as printed wiring boards, and can be even more suitably used as a flexible printed circuit board. Moreover, the laminate according to the present disclosure can be suitably used as a liquid crystal polymer film for metal bonding. EXAMPLES

[0170] The present disclosure will be described in more detail below with reference to examples. The materials, amounts, ratios, processing contents, processing procedures, etc. shown in the following examples can be changed as appropriate without departing from the spirit of the present disclosure. Therefore, the scope of the present disclosure is not limited to the specific examples shown below.

[0171] Details of the materials used in preparing the polymer film and laminate are as follows:

[0172] <<Layer A>> <Polymer> P1: Aromatic polyesteramide prepared according to the following manufacturing method

[0173] -Synthesis of aromatic polyesteramide P1- Into a reactor equipped with a stirrer, a torque meter, a nitrogen gas inlet tube, a thermometer, and a reflux condenser, 940.9 g (5.0 mol) of 6-hydroxy-2-naphthoic acid, 415.3 g (2.5 mol) of isophthalic acid, 377.9 g (2.5 mol) of acetaminophen, and 867.8 g (8.4 mol) of acetic anhydride were placed, and the gas in the reactor was replaced with nitrogen gas. After that, the temperature was raised from room temperature (23°C, the same below) to 140°C over 60 minutes while stirring under a nitrogen gas stream, and the mixture was refluxed at 140°C for 3 hours. Next, while distilling off by-product acetic acid and unreacted acetic anhydride, the temperature was raised from 150°C to 300°C over 5 hours, and the temperature was maintained at 300°C for 30 minutes. The contents were then removed from the reactor and cooled to room temperature. The resulting solid was pulverized with a pulverizer to obtain a powdered aromatic polyesteramide P1a. The flow initiation temperature of the aromatic polyesteramide P1a was 193°C. The aromatic polyesteramide P1a was a wholly aromatic polyesteramide. The aromatic polyesteramide P1a was heated in a nitrogen atmosphere from room temperature to 160°C over 2 hours and 20 minutes, then heated from 160°C to 180°C over 3 hours and 20 minutes, and held at 180°C for 5 hours to carry out solid-state polymerization, and then cooled. The aromatic polyesteramide P1b was then pulverized in a pulverizer to obtain a powdered aromatic polyesteramide P1b. The flow-initiation temperature of the aromatic polyesteramide P1b was 220°C. The aromatic polyesteramide P1b was heated in a nitrogen atmosphere from room temperature to 180°C over 1 hour 25 minutes, then heated from 180°C to 255°C over 6 hours 40 minutes, and held at 255°C for 5 hours to carry out solid-state polymerization. The resulting mixture was then cooled to obtain a powdered aromatic polyesteramide P1. The flow initiation temperature of the aromatic polyesteramide P1 was 302° C. The melting point of the aromatic polyesteramide P1 was measured using a differential scanning calorimeter and found to be 311° C. The dielectric tangent of the aromatic polyesteramide P1 was 0.003.

[0174] <Filler> PP-1: Liquid crystal polymer particles prepared according to the following manufacturing method

[0175] -Synthesis of liquid crystal polymer particles PP-1- In a reactor equipped with a stirrer, a torque meter, a nitrogen gas inlet tube, a thermometer, and a reflux condenser, 1034.99g (5.5 mol) of 2-hydroxy-6-naphthoic acid, 89.18g (0.41 mol) of 2,6-naphthalenedicarboxylic acid, 236.06g (1.42 mol) of terephthalic acid, 341.39g (1.83 mol) of 4,4-dihydroxybiphenyl, and potassium acetate and magnesium acetate as catalysts were placed. After the gas in the reactor was replaced with nitrogen gas, acetic anhydride (1.08 molar equivalent to the hydroxyl group) was further added. Under a nitrogen gas stream, the temperature was raised from room temperature to 150°C over 15 minutes while stirring, and refluxed at 150°C for 2 hours. Next, while distilling off the by-produced acetic acid and unreacted acetic anhydride, the temperature was raised from 150°C to 310°C over 5 hours, and the polymer was taken out and cooled to room temperature. The obtained polymer was heated from room temperature to 295°C over 14 hours, and solid-phase polymerized at 295°C for 1 hour. After the solid-phase polymerization, the mixture was cooled to room temperature over 5 hours to obtain liquid crystal polymer particles PP-1. The liquid crystal polymer particles PP-1 had a median diameter (D50) of 7 μm, a dielectric dissipation factor of 0.0007, and a melting point of 334°C.

[0176] <<Layer B>> <Material A> A1: Hydrogenated styrene-ethylene-butylene-styrene block copolymer particles, frozen and crushed Tuftec M1913 manufactured by Asahi Kasei Chemicals Corporation (average particle size 5.0 μm (D50): coarse particles were removed using a 50 μm mesh). A2: Frozen and crushed product of hydrogenated styrene-isobutylene-styrene block copolymer (product name "SIBSTAR103T-UL", manufactured by Kaneka Corporation) swollen with N-methylpyrrolidone, average particle size 5.0 μm (D50)

[0177] <Material B> P1: the above aromatic polyester amide P1 B1: Silica particles, product name "AEROSIL (registered trademark) NX90S", manufactured by Nippon Aerosil Co., Ltd. B2: Foaming agent, product name "Techpolymer SSX-101", manufactured by Sekisui Plastics Co., Ltd. <Copper foil> M1: Product name "CF-T9DA-SV-18", manufactured by Fukuda Metal Foil and Powder Co., Ltd., average thickness 18 μm M2: Product name "MT18FL", manufactured by Mitsui Mining & Smelting Co., Ltd., average thickness 1.5 μm, with 18 μm of carrier copper M3: Product name "CF-T4X-SV-18", manufactured by Fukuda Metal Foil and Powder Co., Ltd., average thickness 18 μm

[0178] Next, in order to produce a polymer film and a laminate, a solution for forming a layer A, a solution for forming a layer B, and a solution for forming a layer C were prepared. Note that the polymer film was produced using the solution for forming a layer B.

[0179] - Preparation of solution for forming layer A - The polymers and fillers shown in Table 1 were mixed in the amounts (mass %) shown in Table 1, and N-methylpyrrolidone was added to adjust the solids concentration to 25 mass %, to obtain a layer A forming solution.

[0180] - Preparation of solution for forming layer B - Material A and material B shown in Table 1 were mixed in the amounts (mass %) shown in Table 1, and N-methylpyrrolidone was added to adjust the solids concentration to 20 mass % to obtain a solution for forming layer B.

[0181] - Preparation of solution for forming layer C - 8 parts by mass of aromatic polyesteramide P1 was added to 92 parts by mass of N-methylpyrrolidone and stirred at 140° C. for 4 hours in a nitrogen atmosphere to obtain an aromatic polyesteramide solution P1 (solid content concentration: 8% by mass). A layer C forming solution was prepared by mixing 0.04 parts by mass of an aminophenol type epoxy resin (product name "jER630", manufactured by Mitsubishi Chemical Corporation) with 10.0 parts by mass of the aromatic polyester amide solution P1.

[0182] [Preparation of polymer film with copper layer (single-sided copper-clad laminate)] -Films 1 to 11- The obtained solutions for forming Layer C, Layer A, and Layer B were fed to a slot die coater equipped with a slide coater, and applied to the treated surface of the copper foil shown in Table 1 in a three-layer configuration (Layer C / Layer A / Layer B) by adjusting the flow rate so as to obtain the film thickness shown in Table 1. The solvent was removed from the coating film by drying at 40°C for 4 hours. Furthermore, the temperature was raised from room temperature (25°C) to 300°C at a rate of 1°C / min under a nitrogen atmosphere. A heat treatment was performed by holding at 300°C for 2 hours to obtain a laminate (single-sided copper-clad laminate) in which the copper foil, Layer C, Layer A, and Layer B were laminated in this order. In addition, when the copper foil was M2 or M3, Layer C was not formed.

[0183] -Film 12- The solution for forming Layer B was applied onto a support (product name "Nitoflon #900UL", manufactured by Nitto Denko Corporation, average thickness 50 μm). The solution was dried at 40° C. for 4 hours to remove the solvent from the coating, and a polymer film having a support was obtained. For evaluation of the cross section, the 160° C. elastic modulus, and the dielectric tangent, the support was peeled off, and the sample was further heat-treated by increasing the temperature from room temperature (25° C.) to 300° C. at a rate of 1° C. / min in a nitrogen atmosphere and maintaining the temperature at 300° C. for 2 hours.

[0184] -Film A- The obtained solution for forming Layer C and solution for forming Layer A were fed to a slot die and applied to the copper foil shown in Table 1 by adjusting the flow rate so that the average thickness after drying was the thickness shown in Table 1. The coating was dried at 40°C for 4 hours to remove the solvent from the coating, and a polymer film (single-sided copper-clad laminate) having a copper layer was obtained. For evaluation of the dielectric loss tangent, a sample was used that had been further heat-treated by increasing the temperature from room temperature (25°C) to 300°C at a rate of 1°C / min in a nitrogen atmosphere and maintaining it at 300°C for 2 hours.

[0185] -Film B- The obtained solution for forming Layer A was fed to a slot die and applied to the copper foil shown in Table 1 by adjusting the flow rate so that the average thickness after drying would be the thickness shown in Table 1. The coating was dried at 40°C for 4 hours to remove the solvent from the coating, and a polymer film (single-sided copper-clad laminate) having a copper layer was obtained. For evaluation of the dielectric loss tangent, a sample was used that had been further heat-treated by increasing the temperature from room temperature (25°C) to 300°C at a rate of 1°C / min in a nitrogen atmosphere and maintaining it at 300°C for 2 hours.

[0186] -Film C- As film C, an LCP film (product name "Vextar CTQ", manufactured by Kuraray Co., Ltd., average thickness 50 μm) was used, and the treated side of the copper foil described in Table 1 was laminated at 300°C using a thermocompression bonding machine to obtain a polymer film having a copper layer (single-sided copper-clad laminate).

[0187] [Preparation of double-sided copper-clad laminate] The copper foil, the first film, and the second film shown in Table 2 were laminated in the order of copper foil / second film / first film. In Examples 1 to 8 and Comparative Examples 1 to 3, the copper foils were laminated so that the treated surface of the copper foil was in contact with layer B of the first film. In Examples 9 to 11, the second film was laminated on the opposite side of the support to the first film on the opposite side of the copper foil using a vacuum laminator, and the support of the second film was peeled off. After that, the film was heated from room temperature (25°C) to 300°C at a rate of 1°C / min in a nitrogen atmosphere, and then heat-treated by holding at 300°C for 2 hours to obtain a laminate (single-sided copper-clad laminate) in which the copper foil, the first film, and the second film were laminated in this order. Furthermore, the treated surface of the copper foil was in contact with layer B of the second film, and the first film was laminated so that the copper foil was the outermost layer. Using a laminator (product name "Vacuum Laminator V-130", manufactured by Nikko Materials Co., Ltd.), lamination was performed for 1 minute at 140°C and a lamination pressure of 0.4 MPa to obtain a precursor for a double-sided copper-clad laminate. Next, the obtained double-sided copper-clad laminate was subjected to thermocompression bonding at 230° C. and 4 MPa for 60 minutes using a thermocompression bonding machine (product name "MP-SNL", manufactured by Toyo Seiki Seisakusho Co., Ltd.) to produce a double-sided copper-clad laminate.

[0188] [Creating a wiring board] -Preparation of substrate A with wiring pattern- Copper foil (product name "CF-T9DA-SV-18", average thickness 18 μm, manufactured by Fukuda Metal Foil and Powder Co., Ltd.) and liquid crystal polymer film (product name "CTQ-50", average thickness 50 μm, manufactured by Kuraray Co., Ltd.) were prepared as a substrate. The copper foil, substrate, and copper foil were stacked in this order so that the treated surface of the copper foil was in contact with the substrate. A laminator (product name "Vacuum Laminator V-130", manufactured by Nikko Materials Co., Ltd.) was used to perform lamination processing for 1 minute under conditions of 140 °C and lamination pressure 0.4 MPa to obtain a precursor of a double-sided copper-clad laminate. Next, a thermocompression bonding machine (product name "MP-SNL", manufactured by Toyo Seiki Seisakusho Co., Ltd.) was used to thermocompress the obtained precursor of the double-sided copper-clad laminate for 10 minutes under conditions of 300 °C and 4.5 MPa to produce a double-sided copper-clad laminate. The surfaces of the copper foils on both sides of the double-sided copper-clad laminate were roughened, and a dry film resist was attached. The substrate was exposed to light so that the wiring pattern remained, developed, etched, and the dry film was removed to produce substrate A with a wiring pattern having a line / space of 100 μm / 100 μm including a ground line and three pairs of signal lines on both sides of the substrate. The length of the signal line was 50 mm, and the width was set so that the characteristic impedance was 50 Ω.

[0189] -Preparation of substrate B with wiring pattern- A copper foil (product name "MT18FL", average thickness 1.5 μm, with carrier copper foil (thickness 18 μm), manufactured by Mitsui Mining & Smelting Co., Ltd.) and a liquid crystal polymer film (product name "CTQ-50", average thickness 50 μm, manufactured by Kuraray Co., Ltd.) were prepared as a substrate. The copper foil and the substrate were stacked in this order so that the treated surface of the copper foil was in contact with the substrate. A laminator (product name "Vacuum Laminator V-130", manufactured by Nikko Materials Co., Ltd.) was used to perform lamination processing for 1 minute under conditions of 140 ° C and lamination pressure 0.4 MPa to obtain a precursor of a single-sided copper-clad laminate. Next, a thermocompression bonding machine (product name "MP-SNL", manufactured by Toyo Seiki Seisakusho Co., Ltd.) was used to thermocompress the obtained precursor of the single-sided copper-clad laminate for 10 minutes under conditions of 300 ° C and 4.5 MPa to produce a single-sided copper-clad laminate. The carrier copper foil on the opposite side of the substrate of the single-sided copper-clad laminate was peeled off, and the surface of the exposed 1.5 μm copper foil was roughened and laminated with a dry film resist. After pattern exposure and development, the areas where the resist pattern was not placed were plated. The dry film resist was then peeled off, and the copper exposed by the peeling process was removed by flash etching to produce substrate B with a wiring pattern with a line / space of 20 μm / 20 μm.

[0190] -Making a wiring board- The prepared substrate having a wiring pattern was superimposed on the layer B side of the prepared single-sided copper-clad laminate, and hot pressed at 160° C. and 4 MPa for 1 hour to obtain a wiring board. The obtained wiring board had a wiring pattern (ground line and signal line) embedded therein, and when substrate A with wiring pattern was used, the thickness of the wiring pattern was 18 μm, and when substrate B with wiring pattern was used, the thickness of the wiring pattern was 12 μm.

[0191] <<Evaluation>> The produced wiring board was subjected to the following measurements and evaluations, and the results are shown in Tables 1 and 2.

[0192] <<Measurement method>> [Elastic modulus at 160℃] The double-sided copper-clad laminate was etched to expose layer B. The elastic modulus in the exposed area was then measured as the indentation elastic modulus using a nanoindentation method. The indentation elastic modulus was measured using a microhardness tester (product name "DUH-W201", manufactured by Shimadzu Corporation) by applying a load with a Vickers indenter at a loading rate of 0.28 mN / sec, holding the maximum load of 10 mN for 10 seconds, and then unloading at a loading rate of 0.28 mN / sec.

[0193] [Dielectric tangent] The copper foil of the double-sided copper-clad laminate was removed with an aqueous solution of ferric chloride, washed with pure water, and dried to obtain a polymer film, which was then used for the measurement. The dielectric loss tangent was measured at a frequency of 10 GHz by the resonance perturbation method. A 10 GHz cavity resonator (Kanto Electronics Application Development Co., Ltd.'s "CP531") was connected to a network analyzer (Agilent Technology's "E8363B"), and the polymer film was inserted into the cavity resonator. The dielectric loss tangent of the polymer film was measured from the change in resonance frequency before and after insertion for 96 hours in an environment of 25°C temperature and 60% RH.

[0194] [Length of the gap in the long axis direction ("Length L" in Table 1)] The double-sided copper-clad laminate was cut with a microtome to prepare a film cross-section sample. Layer B of the cross section was observed with a scanning electron microscope (SEM) at 10,000x magnification in 100 fields of view. 100 voids were randomly selected from layer B. The length of each selected void in the major axis direction was measured, and the average value was used.

[0195] [Distance between the gap and material B ("Distance T" in Table 1)] The surface of the polymer film was cut with a microtome to prepare a film cross-section sample. The cross-section was observed with an optical microscope at 50x magnification to confirm the distribution of material B. The same film cross-section sample was observed with a scanning electron microscope (SEM) at 10,000x magnification to observe voids in the same position as the field of view observed with the optical microscope. For any 100 voids obtained, the distance to the nearest material B was measured, and the average value was taken as the distance T between the void and material B.

[0196] [Porosity] In the same manner as in the method for measuring the length in the long axis direction of the voids, 100 voids were randomly selected. The cross-sectional area of ​​each selected void was measured. The void ratio was calculated based on the following formula. Porosity = {(total cross-sectional area of ​​voids) / (cross-sectional area of ​​polymer film)} x 100

[0197] <<Evaluation method>> [Step-following ability] The wiring board was cut in the thickness direction with a microtome, and the cross section was observed with an optical microscope. The length L1 of the gap generated in the in-plane direction between layer B and the wiring pattern was measured. The average value for 10 points was calculated. The evaluation criteria are as follows: A: No gaps were found. B: The average value of L1 was less than 1 μm. C: The average value of L1 was 1 μm or more.

[0198] [Heat resistance] The prepared double-sided copper-clad laminate was cut into a size of 30 mm x 30 mm to prepare an evaluation sample. The evaluation sample was treated for 168 hours in a thermohygrostat at a temperature of 85°C and a relative humidity of 85%. The evaluation sample was then placed in an oven set at 260°C and heated for 15 minutes. After heating, the evaluation sample was cut with a razor, and the cross section was observed under an optical microscope to evaluate the state of peeling. A: No peeling was observed between layer B and the copper foil. B: Peeling was observed between layer B and the copper foil with a width of 1.0 mm or less. C: Peeling was observed between layer B and the copper foil with a width of more than 1.0 mm.

[0199] The measurement results and evaluation results are shown in Table 1. In Comparative Example 1, since there were no voids in Layer B, "-" is entered in the column relating to voids.

[0200] [Table 1]

[0201] [Table 2]

[0202] As shown in Table 1, Examples 1 to 11 contain material A which is liquid at 260°C and material B which is solid at 260°C, contain voids with a length in the major axis direction of 0.01 μm or more, have an elastic modulus of 0.60 MPa or less at 160°C, and have a dielectric tangent of 0.01 or less, and are therefore found to have excellent step-following ability and heat resistance. On the other hand, in Comparative Example 1, no voids were present in the polymer film, and it was found that the heat resistance was poor. In Comparative Example 2, the length of the voids in the major axis direction was less than 0.01 μm, and it was found that the heat resistance was poor. In Comparative Example 3, the elastic modulus at 160° C. was more than 0.60 MPa, and it was found that the step-following ability was poor.

Claims

1. The material A is liquid at 260° C., and the material B is solid at 260° C. The voids have a length in the major axis direction of 0.01 μm or more, The elastic modulus at 160°C is 0.60 MPa or less, A polymer film having a dielectric loss tangent of 0.01 or less.

2. 2. The polymer film according to claim 1, wherein the proportion of the voids in the total volume of the polymer film is 1 volume % to 15 volume %.

3. The polymer film according to claim 1 or 2, wherein the voids have a length in the major axis direction of 0.5 μm to 10 μm.

4. The polymer film according to claim 1 or 2, wherein the distance between the gap and material B is 5 μm or less.

5. The polymer film according to claim 1 or 2, wherein the material A is an elastomer containing a structural unit derived from styrene.

6. 3. The polymer film according to claim 1, wherein the material A is at least one selected from the group consisting of a styrene-ethylene-butylene-styrene block copolymer, a styrene-isobutylene-styrene block copolymer, a styrene-ethylene-propylene-styrene copolymer, a styrene-isoprene-styrene block copolymer, and hydrogenated products thereof.

7. The polymer film according to claim 1 or 2, wherein the material B comprises an aromatic polyesteramide.

8. A layer A and a layer B disposed on at least one surface of the layer A, The layer B comprises a material A that is liquid at 260°C and a material B that is solid at 260°C, comprises voids having a length in the major axis direction of 0.01 μm or more, has an elastic modulus at 160°C of 0.60 MPa or less, and has a dielectric loss tangent of 0.01 or less.

Citation Information

Patent Citations

  • Resin composition, adhesive film, coverlay film, laminate, copper foil with resin, and copper clad laminate with resin