Laminate film
A laminated film with balanced elastic modulus ratios and intermediate regions in polyimide resin layers addresses the challenge of maintaining puncture strength and dielectric properties in flexible printed circuit boards, enhancing their performance for 5G communication.
Patent Information
- Application Number
- JP2023163011
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Filing Date
- 2023-09-26
- Publication Date
- 2024-10-11
AI Technical Summary
Polyimide films used in flexible printed circuit boards face challenges in maintaining high puncture strength while controlling dielectric properties, particularly for high-speed communication applications like 5G, as they are prone to impact during processing.
A laminated film structure is developed with specific elastic modulus relationships between polyimide resin-containing layers, utilizing a scanning probe microscope to achieve a balanced mechanical properties, ensuring high puncture strength and suitable dielectric properties by adjusting the elastic modulus ratios and incorporating intermediate regions for force dispersion.
The laminated film exhibits enhanced puncture strength and improved dielectric properties, making it suitable for high-speed communication applications while minimizing burr formation during processing.
Smart Images

Figure 2024144018000038 
Figure 2024144018000039 
Figure 2024144018000040
Abstract
Description
[Technical field]
[0001] The present invention relates to a laminate film containing a polyimide-based resin-containing layer, particularly a laminate film that can be used as a substrate material compatible with printed circuit boards and antenna boards for high-frequency bands, and a laminate sheet and flexible printed circuit board each containing the laminate film. [Background technology]
[0002] Flexible printed circuit boards (hereinafter sometimes referred to as FPCs) are thin, lightweight, and flexible, allowing for three-dimensional, high-density mounting, and are used in many electronic devices such as mobile phones and hard disks, contributing to their miniaturization and weight reduction. Traditionally, polyimide resins, which have excellent heat resistance, mechanical properties, and electrical insulation properties, have been widely used in FPCs, and for example, metal-clad laminates such as copper-clad laminates (hereinafter sometimes abbreviated as CCL) used in FPCs are known to be laminates having copper foil layers on one or both sides of a polyimide film. In recent years, the fifth generation mobile communication system known as 5G has been coming into full swing (for example, Patent Document 1), and polyimide films suitable for high-speed communication applications beyond 5G have been studied. [Prior art documents] [Patent documents]
[0003] [Patent Document 1] Patent Publication No. 2021-161285 Summary of the Invention [Problem to be solved by the invention]
[0004] Polyimide films used in FPCs are subject to impacts in the thickness direction during processing, etc., and are required to have a puncture strength that can withstand these impacts. However, it is difficult to improve mechanical properties while controlling dielectric properties within an appropriate range. For this reason, there is a need to develop polyimide films with high puncture strength that can be used for high-speed communication applications beyond 5G.
[0005] An object of the present invention is to provide a laminate film having high puncture strength, and a laminate sheet and a flexible printed circuit board each including the laminate film. [Means for solving the problem]
[0006] As a result of intensive research to solve the above problems, the present inventors have found that the above problems can be solved by making the average elastic modulus of each polyimide-based resin-containing layer constituting the laminate film satisfy a specific relationship as measured by a scanning probe microscope (sometimes referred to as SPM), and have arrived at the present invention. That is, the present invention provides the following preferred embodiments.
[0007] [1] A laminated film comprising a polyimide-based resin-containing layer (PI-1) and a polyimide-based resin-containing layer (PI-2), The average elastic modulus of the layer (PI-1) and the layer (PI-2) measured by a scanning probe microscope in a cross section in the thickness direction of the laminated film is expressed by the formula (I): (E1r-E1a) / (E2r-E2a)≧1.00 (I) [In the formula, E1r represents the average elastic modulus of the layer (PI-1) during the retraction process of the cantilever probe, E1a represents the average elastic modulus of the layer (PI-1) during the indentation process of the cantilever probe, E2r represents the average elastic modulus of the layer (PI-2) during the retraction process, and E2a represents the average elastic modulus of the layer (PI-2) during the indentation process, where E1r-E1a>0 and E2r-E2a>0.] Laminated film that satisfies the above requirements. [2] In formula (I), 0.30 GPa ≦ E2r - E2a ≦ 1.50 GPa The laminate film according to [1], which satisfies the relationship: [3] Having an intermediate region between the layer (PI-1) and the layer (PI-2), the intermediate region is a region in which, when the elastic modulus of the laminate film is continuously measured along the thickness direction in a cross section of the laminate film in a process of pulling back a cantilever probe by a scanning probe microscope, the elastic modulus changes continuously from the E1r to the E2r, The laminate film according to [1] or [2], wherein the thickness of the intermediate region is 50 nm or more. [4] The laminate film according to any one of [1] to [3], further comprising a polyimide-based resin-containing layer (PI-3). [5] At least one of the polyimide-based resin-containing layer (PI-1) and the polyimide-based resin-containing layer (PI-2) contains a polyimide-based resin having a structural unit (A) derived from a tetracarboxylic acid anhydride, The structural unit (A) is represented by the formula (A1): [ka] [In formula (A1), R a1 each independently represents a halogen atom, or an alkyl group, an alkoxy group, an aryl group, or an aryloxy group which may have a halogen atom; k represents an integer from 0 to 2. and / or a structural unit (A1) derived from a tetracarboxylic acid anhydride represented by the formula (A2): [ka] [In formula (A2), R a2 each independently represents a halogen atom, or an alkyl group, an alkoxy group, an aryl group, or an aryloxy group which may have a halogen atom, and each 1 independently represents an integer of 0 to 3. The laminate film according to any one of [1] to [4], which contains a structural unit (A2) derived from a tetracarboxylic acid anhydride represented by the following formula: [6] At least one of the polyimide-based resin-containing layer (PI-1) and the polyimide-based resin-containing layer (PI-2) contains a polyimide-based resin having a diamine-derived structural unit (B), The structural unit (B) is represented by the formula (B1): [ka] [In formula (B1), R b1 each independently represents a halogen atom, or an alkyl group, an alkoxy group, an aryl group, or an aryloxy group which may have a halogen atom; W each independently represents -O-, -CH2-, -CH2-CH2-, -CH(CH3)-, -C(CH3)2-, -C(CF3)2-, -COO-, -OOC-, -SO-, -SO2-, -S-, -CO-, -N(R c a divalent linking group selected from the group consisting of -CONH- and -CONH-, or a single bond (wherein m is 2 or more and at least one W is the divalent linking group); R c represents a hydrogen atom or a monovalent hydrocarbon group having 1 to 12 carbon atoms which may be substituted with a halogen atom, m represents an integer of 1 to 4; and q each independently represents an integer of 0 to 4. The laminate film according to any one of [1] to [5], which contains a structural unit (B1) derived from a diamine represented by the following formula: [7] The polyimide-based resin-containing layer (PI-1) and the polyimide-based resin-containing layer (PI-2) each contain a polyimide-based resin having a tetracarboxylic acid anhydride-derived structural unit (A) and a diamine-derived structural unit (B), The structural unit (A) is represented by the formula (A1): [ka] [In formula (A1), R a1 each independently represents a halogen atom, or an alkyl group, an alkoxy group, an aryl group, or an aryloxy group which may have a halogen atom; k represents an integer from 0 to 2. and / or a structural unit (A1) derived from a tetracarboxylic acid anhydride represented by the formula (A2): [ka] [In formula (A2), R a2each independently represents a halogen atom, or an alkyl group, an alkoxy group, an aryl group, or an aryloxy group which may have a halogen atom, and each 1 independently represents an integer of 0 to 3. The structural unit (A2) is derived from a tetracarboxylic acid anhydride represented by the formula: The structural unit (B) is represented by the formula (B1): [ka] [In formula (B1), R b1 each independently represents a halogen atom, or an alkyl group, an alkoxy group, an aryl group, or an aryloxy group which may have a halogen atom; W each independently represents -O-, -CH2-, -CH2-CH2-, -CH(CH3)-, -C(CH3)2-, -C(CF3)2-, -COO-, -OOC-, -SO-, -SO2-, -S-, -CO-, -N(R c a divalent linking group selected from the group consisting of -CONH- and -CONH-, or a single bond (wherein m is 2 or more and at least one W is the divalent linking group); R c represents a hydrogen atom or a monovalent hydrocarbon group having 1 to 12 carbon atoms which may be substituted with a halogen atom, m represents an integer of 1 to 4; and q each independently represents an integer of 0 to 4. The laminate film according to any one of [1] to [6], which contains a structural unit (B1) derived from a diamine represented by the following formula: [8] At least the structural unit (A) of the polyimide resin contained in the polyimide resin-containing layer (PI-1) further contains 45 mol % or less of the formula (A3): [ka] [In formula (A3), Z represents a divalent organic group, R a3 each independently represents a halogen atom, or an alkyl group, an alkoxy group, an aryl group, or an aryloxy group which may have a halogen atom; Each s independently represents an integer from 0 to 3. The laminate film according to [7], comprising a structural unit (A3) derived from an ester bond-containing tetracarboxylic acid anhydride represented by the following formula: [9] A laminate sheet comprising a metal foil layer on one or both sides of the laminate film according to any one of [1] to [8].
[10] A flexible printed circuit board comprising the laminate sheet according to [9]. Effect of the Invention
[0008] According to the present invention, it is possible to provide a laminated film having high puncture strength. [Brief description of the drawings]
[0009] [Figure 1] 4 is a graph showing a force curve obtained at an arbitrary point on a sample cross section in a laminate film according to one embodiment of the present invention. [Diagram 2] FIG. 2 is a diagram showing a DMT elastic modulus image and coordinate axes of a sample cross section during the process of pulling back a cantilever probe in a laminate film according to one embodiment of the present invention. [Diagram 3] FIG. 3 is a diagram showing locations of X=40, 80, 120, 160, and 200 in the DMT elastic modulus image of FIG. 2. [Figure 4] 3 is a graph showing the elastic modulus profile at X=40 in the DMT elastic modulus image of FIG. 2. [Diagram 5] 3 is a graph showing a nine-point moving average line and intermediate region thickness of the average DMT elastic modulus profile obtained from the DMT elastic modulus image of FIG. 2. [Figure 6] FIG. 1 is a schematic cross-sectional view showing an example of a layer structure of a laminated film of the present invention. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0010] Hereinafter, the embodiments of the present invention will be described in detail. Note that the scope of the present invention is not limited to the embodiments described here, and various modifications can be made without departing from the spirit of the present invention. Note that the upper and lower limit values described in this specification can be arbitrarily combined to form a suitable numerical range.
[0011] [Laminated film] The laminate film of the present invention includes a polyimide-based resin-containing layer (PI-1) and a polyimide-based resin-containing layer (PI-2), and the average elastic modulus of the polyimide-based resin-containing layer (PI-1) and the polyimide-based resin-containing layer (PI-2) measured by a scanning probe microscope (SPM) in a cross section in the thickness direction of the laminate film is expressed by the formula (I): (E1r-E1a) / (E2r-E2a)≧1.00 (I) [In the formula, E1r represents the average elastic modulus of the layer (PI-1) during the pullback process of the cantilever probe (sometimes simply referred to as the "pullback process"); E1a represents the average elastic modulus of the layer (PI-1) during the pushback process of the cantilever probe (sometimes simply referred to as the "pullback process"); E2r represents the average elastic modulus of the layer (PI-2) during the pullback process; E2a represents the average elastic modulus of the layer (PI-2) during the pushback process; E1r-E1a>0, and E2r-E2a>0.] The relationship is satisfied. In this specification, the polyimide-based resin-containing layer means a layer that contains a polyimide-based resin (sometimes referred to as a PI-based resin). The polyimide-based resin-containing layer (PI-1) may be simply referred to as layer (PI-1), and the polyimide-based resin-containing layers other than layer (PI-1) may be similarly referred to as layer (PI-2) and layer (PI-3). Furthermore, in this specification, the "elastic modulus measured by a scanning probe microscope" may be referred to as the "elastic modulus by SPM" or the "DMT elastic modulus."
[0012] The present inventors have surprisingly found that, in a laminate film including a layer (PI-1) and a layer (PI-2), when the average DMT modulus of the layers (PI-1) and (PI-2) satisfies the relationship of formula (I), the puncture strength of the laminate film can be improved. In this specification, the puncture strength refers to the puncture strength from at least the layer (PI-2) side, and the laminate film of the present invention can exhibit a high puncture strength from at least the layer (PI-2) side. The reason is unclear, but it is thought that the balance of the mechanical properties of each layer in the laminate film falls within a certain range, making it easier for the laminate film to absorb and disperse forces applied in the thickness direction.
[0013] First, the smaller the values of (E1r-E1a) and (E2r-E2a), the closer each layer is to an elastic body. More specifically, in the SPM measurement, in the indentation process of the cantilever probe, the probe is pressed into the resin layer, so in addition to elastic deformation, plastic deformation, viscous deformation, etc. also occur, but the retraction process of the cantilever probe is a process after these deformations have occurred, so it can be considered that only elastic deformation occurs. Therefore, the closer the average elastic modulus (a value that takes into account not only elastic deformation but also plastic deformation, viscous deformation, etc.) derived from the force curve of the indentation process described later approaches the average elastic modulus (a value that is substantially composed of elastic deformation) derived from the force curve of the retraction process described later, that is, the smaller the values of (E1r-E1a) and (E2r-E2a), the greater the degree of elastic deformation in each layer, and the closer the physical properties are to an elastic body. Here, in (E1r-E1a) / (E2r-E2a) in formula (I), the balance between (E1r-E1a) and (E2r-E2a) is influential, but generally, as the value of (E2r-E2a), which is the denominator, becomes smaller, the layer (PI-2) becomes closer to an elastic body as described above, so it is considered that it is difficult to break when a needle is pierced from the layer (PI-2) side. On the other hand, as the value of (E1r-E1a), which is the numerator, becomes larger, the layer (PI-1) becomes less elastically deformed and more flexible, so that it becomes easier to disperse and absorb the force received in the thickness direction from the layer (PI-2) side. As a result, when (E1r-E1a) / (E2r-E2a) in the laminate film becomes larger than a certain value, it is considered that the laminate film becomes less likely to break.
[0014] In the laminated film of the present invention, (E1r-E1a) / (E2r-E2a) in formula (I) is preferably 1.02 or more, more preferably 1.04 or more, even more preferably 1.10 or more, even more preferably 1.15 or more, particularly preferably 1.20 or more, particularly more preferably 1.25 or more, particularly more preferably 1.35 or more, particularly more preferably 1.40 or more, and may be, for example, 1.50 or 2.00 or more. When (E1r-E1a) / (E2r-E2a) is equal to or more than the lower limit, the puncture strength of the laminated film can be further improved. In addition, (E1r-E1a) / (E2r-E2a) in formula (I) is preferably 10.0 or less, more preferably 8.00 or less, even more preferably 6.00 or less, even more preferably 4.00 or less, particularly preferably 3.00 or less, and may be, for example, 2.20 or less, 2.00 or less, or 1.80 or less. When the (E1r-E1a) / (E2r-E2a) is equal to or less than the upper limit, it is possible to suppress the generation of burrs or the enlargement of the burrs when forming through holes by processing with a drill, etc. When the laminate film has three or more PI resin-containing layers, it is sufficient that the relationship of formula (I) is satisfied between at least any two adjacent PI resin-containing layers.
[0015] In one embodiment of the present invention, in the laminated film of the present invention, (E1r-E1a) in formula (I) is preferably 0.20 GPa or more, more preferably 0.40 GPa or more, even more preferably 0.50 GPa or more, even more preferably 0.70 GPa or more, particularly preferably 0.80 GPa or more, and may be, for example, 0.90 GPa or more, 1.00 GPa or more, or 1.50 GPa or more. When (E1r-E1a) is equal to or more than the lower limit, the puncture strength of the laminated film is more easily increased. In addition, (E1r-E1a) in formula (I) is preferably 10.0 GPa or less, more preferably 8.00 GPa or less, even more preferably 6.00 GPa or less, even more preferably 4.00 GPa or less, particularly preferably 3.00 GPa or less, and may be, for example, 2.50 GPa or less, 2.00 GPa or less, 1.50 GPa or less, 1.10 GPa or less, or less than 1.0 GPa. When the (E1r-E1a) is equal to or less than the upper limit, the generation of burrs and the enlargement of the burrs can be suppressed when a through hole is formed by machining using a drill or the like.
[0016] In one embodiment of the present invention, in the laminated film of the present invention, (E2r-E2a) in formula (I) is preferably 5.00 GPa or less, more preferably 3.00 GPa or less, even more preferably 2.00 GPa or less, even more preferably 1.50 GPa or less, particularly preferably 1.10 GPa or less, and particularly preferably 1.00 GPa or less, and may be, for example, 0.95 GPa or less, 0.85 GPa or less, or 0.80 GPa or less. When (E2r-E2a) is less than the upper limit, it is easier to increase the puncture strength of the laminated film, and when a through hole is formed by processing with a drill or the like, it is possible to suppress the occurrence of burrs or the increase in the burrs. In addition, (E2r-E2a) in formula (I) is preferably 0.10 GPa or more, more preferably 0.20 GPa or more, even more preferably 0.30 GPa or more, even more preferably 0.40 GPa or more, particularly preferably 0.50 GPa or more, particularly more preferably 0.58 GPa or more, and particularly more preferably 0.60 GPa or more. When the (E2r-E2a) is equal to or more than the lower limit, the puncture strength of the laminated film is easily increased.
[0017] In one embodiment of the present invention, in the laminated film of the present invention, E1r in formula (I) is, for example, 2.0 GPa or more or 2.2 GPa or more, preferably 2.5 GPa or more, more preferably 2.6 GPa or more, even more preferably 2.7 GPa or more, even more preferably 2.8 GPa or more, and may be, for example, 3.0 GPa or more or 3.5 GPa or more. When the E1r is equal to or more than the lower limit, the puncture strength of the laminated film is more likely to be increased. In addition, E1r in formula (I) is usually 15.0 GPa or less, preferably 12.0 GPa or less, more preferably 10.0 GPa or less, even more preferably 8.0 GPa or less, even more preferably 5.0 GPa or less, and may be, for example, 4.0 GPa or less or 3.8 GPa or less. When the E1r is equal to or less than the upper limit, the generation of burrs or the enlargement of burrs can be suppressed when a through hole is provided by processing such as a drill.
[0018] In one embodiment of the present invention, in the laminated film of the present invention, E1a in formula (I) is, for example, 1.0 GPa or more or 1.2 GPa or more, preferably 1.5 GPa or more, more preferably 1.7 GPa or more, and even more preferably 1.8 GPa or more. When E1a is equal to or more than the lower limit, the puncture strength of the laminated film is more likely to be increased. In addition, E1a in formula (I) is usually 10.0 GPa or less, more preferably 8.0 GPa or less, even more preferably 5.0 GPa or less, and even more preferably 3.0 GPa or less, and may be, for example, 2.5 GPa or less or 2.1 GPa or less. When E1a is equal to or less than the upper limit, the generation of burrs or the enlargement of burrs can be suppressed when a through hole is formed by processing with a drill or the like.
[0019] In one embodiment of the present invention, in the laminated film of the present invention, E2r in formula (I) is preferably 1.0 GPa or more, more preferably 1.3 GPa or more, even more preferably 1.5 GPa or more, even more preferably 1.7 GPa or more, and particularly preferably 1.9 GPa or more. When E2r is equal to or more than the lower limit, the puncture strength of the laminated film is more likely to be increased. E2r in formula (I) is usually 12.0 GPa or less, preferably 10.0 GPa or less, even more preferably 9.0 GPa or less, even more preferably 8.0 GPa or less, particularly preferably 5.0 GPa or less, and particularly preferably 3.0 GPa or less, and may be, for example, 2.3 GPa or less, 2.2 GPa or less, or 2.1 GPa or less. When E2r is equal to or less than the upper limit, the generation of burrs or the enlargement of burrs can be suppressed when a through hole is formed by processing with a drill or the like.
[0020] In one embodiment of the present invention, in the laminated film of the present invention, E2a in formula (I) is preferably 0.8 GPa or more, more preferably 1.0 GPa or more, and even more preferably 1.2 GPa or more. When E2a is equal to or more than the lower limit, the puncture strength of the laminated film is more easily increased. E2a in formula (I) is usually 8.0 GPa or less, preferably 5.0 GPa or less, more preferably 3.0 GPa or less, and even more preferably 2.5 GPa or less, and may be, for example, 2.0 GPa or less, 1.8 GPa or less, or 1.5 GPa or less. When E2a is equal to or less than the upper limit, the generation of burrs or the enlargement of the burrs can be suppressed when a through hole is formed by processing with a drill or the like. In this specification, [(E1r-E1a) / (E2r-E2a)], (E1r-E1a), and / or (E2r-E2a) in formula (I) may be referred to as "parameter X".
[0021] The method for measuring the average DMT elastic modulus of each layer using SMP will be described below. (1) Preparation of test pieces (samples) The method for preparing the test specimen is not particularly limited as long as the cross section of the laminate film in the thickness direction can be observed, but when the laminate film is thin, it is preferable to embed a part of the cut laminate film in resin and prepare a test specimen with the cross section exposed. After embedding in resin so that the cross section in the thickness direction can be seen, the surface of the resin-embedded laminate film (the cross section in the thickness direction of the laminate film) can be cut with a knife attached to a microtome, for example, to expose the cross section.
[0022] (2) Acquisition of DMT elastic modulus images The DMT elastic modulus of the laminated film can be obtained by applying the DMT (Derjaguim-Muller-Toporov) theory to the relationship between the deformation amount of the sample and the load applied to the sample (force curve) obtained by SPM, and a DMT elastic modulus image can be obtained by performing mapping measurement on a two-dimensional plane on the sample. For example, a cantilever with a spring constant of 4 to 60 N / m is attached to a Bruker SPM, and a DMT elastic modulus image can be obtained by measuring using the Peak Force QNM (Quantitative Nanomechanical Mapping) mode. Note that the range in which the DMT elastic modulus image is obtained should include at least two adjacent layers and their interface, and it is preferable to set the interface of the two adjacent layers to be located near the center (near the center of the vertical axis (X-axis) of the DMT elastic modulus image).
[0023] Next, a method for measuring the DMT elastic modulus at each point will be described in detail with reference to Figures 1 and 2. Note that Figures 1, 2, and Figures 3 to 5 described later are used to clearly explain a method for determining (E1r-E1a) / (E2r-E2a) and the thickness of the intermediate region, and the present invention is not limited to these embodiments. Fig. 1 is a graph showing a force curve obtained at an arbitrary point on a sample cross section in a laminated film according to one embodiment of the present invention, and Fig. 2 is a diagram showing a DMT elastic modulus image and coordinate axes of a sample cross section during the process of pulling back a cantilever probe in a laminated film according to one embodiment of the present invention. In Fig. 1, the vertical axis (applied load / nN) of the force curve is represented by load F=kd, and the horizontal axis (indentation depth / nm) is represented by the deformation amount of the sample δ=Δz-d. k indicates the spring constant (N / m), d indicates the amount of bending of the spring (m), and z indicates the position of the needle (m). d can be detected by a laser, and z can be sensed by a piezo scanner.
[0024] First, when the cantilever is brought close to the sample, it comes into contact with the sample and is then pushed into the sample until the tip of the cantilever probe reaches the maximum load. Accordingly, a force curve (point A → point B → point C) for the pushing process can be obtained as shown in Figure 1. At point B, when it comes into contact with the sample, it is affected by the adhesive force and the load is applied in the negative direction. Next, when the cantilever that has been pushed into the sample up to the maximum load is pulled back, the load is removed at the sample surface, and after adhesion, the cantilever probe leaves the sample surface. Accordingly, a force curve (point C → point D → point E) for the pulling back process can be obtained as shown in Figure 1.
[0025] The DMT elastic modulus at each point can be calculated by performing an analysis of the force curve in the indentation process and the pullback process using the DMT theoretical formula. Specifically, when the numerical values from the minimum value to the maximum value of the F value in the pullback process of the force curve are replaced with numerical values from 0 to 1, fitting is performed for the range from 0.05 to 0.7 to calculate the DMT elastic modulus. By acquiring the DMT elastic modulus at all measurement points in the range in which the DMT elastic modulus image is to be acquired, the DMT elastic modulus image in the pullback process can be obtained. Similarly, in the indentation process of the force curve, fitting is performed to acquire the DMT elastic modulus at all measurement points, so that the DMT elastic modulus image in the indentation process can be obtained. The analysis using the DMT theoretical formula can be performed using analysis software (e.g., NanoScope Analysis ver.2.00) attached to the SPM or a known method, and in the latter case, for example, the following formula (a) can be used for calculation.
number
[0026] In SPM measurements, the measurement atmosphere can be room temperature, for example, 24°C, and atmospheric air, the cantilever movement speed can be set to 0.4 μm / s, and the maximum load can be set to 40 nN. The spring constant of the cantilever and the tip radius of the probe can be calculated using values built into the SPM device or by known methods. For example, the spring constant may be a value calculated by the Sader method, and the tip radius of the probe may be a value calculated by the reconstruction method.
[0027] (3) Calculation of (E1r-E1a) / (E2r-E2a) When the DMT elastic modulus images obtained above [layer (PI-2) on the top and layer (PI-1) on the bottom] are converted into coordinates, for example, when the Y coordinate of the DMT elastic modulus image is 0 to 1 from top to bottom and the X coordinate is 0 to 1 from left to right, the average value of the DMT elastic modulus from (X,Y)=(0,0) to (1,0.4) can be calculated to obtain the average DMT elastic modulus of layer (PI-2) in each process. In addition, the average value of the DMT elastic modulus from (X,Y)=(0,0.6) to (1,1) can be calculated to obtain the average DMT elastic modulus of layer (PI-1) in each process. Figure 2 shows a DMT elastic modulus image during the pull-back process, obtained by measuring 256 horizontal and 256 vertical points in an area of 5 μm horizontal (in-plane direction) × 5 μm vertical (thickness direction) on the sample cross section. The coordinates of the upper left end are (X,Y) = (0,0), the lower left end is (X,Y) = (0,255), the upper right end is (X,Y) = (255,0), and the lower right end is (X,Y) = (255,255). The average DMT elastic modulus (E2r) of the layer (PI-2) during the pullback process can be obtained by calculating the average value of the DMT elastic modulus at 256×100 points from (0,0) to (255,99), and the average DMT elastic modulus (E1r) of the layer (PI-1) during the pullback process can be obtained by calculating the average value of the DMT elastic modulus at 256×129 points from (X,Y)=(0,126) to (255,255). In the indentation process, the average DMT elastic modulus (E2a) of the layer (PI-2) during the indentation process and the average DMT elastic modulus (E1a) of the layer (PI-1) during the indentation process can be obtained by a similar method using the elastic modulus image during the indentation process. In this manner, E2r, E2a, E1r, and E1a in formula (I) can be determined, and (E1r-E1a) / (E2r-E2a) can be calculated.
[0028] The range in which the DMT elastic modulus image is obtained is preferably 0.05 to 0.6 times, more preferably 0.08 to 0.5 times, and even more preferably 0.1 to 0.4 times the thickness of the laminated film in terms of the horizontal (in-plane direction) and vertical (thickness direction) distances. For example, in a laminated film having a thickness of 20 to 65 μm, the range in which the DMT elastic modulus image is obtained may be 3 μm or more horizontal x 3 μm or more vertical, preferably 5 μm or more horizontal x 5 μm or more vertical, more preferably 10 μm or more horizontal x 10 μm or more vertical, and may be 10 μm or more horizontal x 10 μm or more vertical. In addition, the number of points (locations) for measuring the DMT elastic modulus may be 100 points or more x 100 points or more from the viewpoint of increasing the accuracy of determining the intermediate region, and may be preferably 128 points or more x 128 points or more, more preferably 200 points or more x 200 points or more, even more preferably 256 points or more x 256 points or more, and even more preferably 512 points x 512 points. The resolution is primarily determined by the range and number of measurement points for obtaining the DMT elastic modulus image, but when the thickness of the intermediate region is small, it is preferable to measure with a resolution of 40 nm / pixel or less, more preferably 20 nm / pixel or less. Note that (E1r-E1a) / (E2r-E2a) in formula (I) can be determined, for example, by the method described in the Examples.
[0029] In one embodiment of the present invention, the laminated film of the present invention preferably has an intermediate region between the layer (PI-1) and the layer (PI-2). The intermediate region is a region in which, when the elastic modulus of the laminated film in the process of pulling back the cantilever probe is continuously measured along the thickness direction in a cross section of the laminated film in the thickness direction by SPM, the elastic modulus changes from the average DMT elastic modulus (E1r) of the layer (PI-1) in the process of pulling back to the average DMT elastic modulus (E2r) of the layer (PI-2) in the process of pulling back. By having the intermediate region of the laminated film of the present invention, the puncture strength of the laminated film can be improved. This is presumably because the intermediate region in which the DMT elastic modulus in the process of pulling back corresponding to the elastic deformation changes continuously along the thickness direction makes it easier to disperse and absorb the force applied in the thickness direction.
[0030] The thickness of the intermediate region is usually 50 nm or more, preferably 100 nm or more, more preferably 250 nm or more or more than 250 nm, even more preferably 270 nm or more, even more preferably 300 nm or more, particularly preferably 350 nm or more, particularly more preferably 380 nm or more, particularly more preferably 450 nm or more, particularly more preferably 600 nm or more, extremely preferably 1000 nm or more, extremely more preferably 1500 nm or more, extremely more preferably 1700 nm or more, extremely particularly preferably 2000 nm or more, extremely particularly preferably 2300 nm or more, for example, 2600 nm or more or 2700 nm or more. When the thickness of the intermediate region is the lower limit or more, the force applied in the thickness direction is more easily dispersed and absorbed, so that the puncture strength of the laminated film can be further improved. The thickness of the intermediate region is usually 10,000 nm or less, preferably 8,000 nm or less, more preferably 5,000 nm or less, and even more preferably 3,500 nm or less, and may be, for example, 3,000 nm or less, less than 2,800 nm, or 2,700 nm or less. When the thickness of the intermediate region is equal to or less than the upper limit, the generation of burrs or the increase in the size of the burrs can be suppressed when a through hole is formed by processing such as a drill. When the laminated film has three or more PI resin-containing layers, it is preferable that the thickness of the intermediate region between at least any two adjacent PI resin-containing layers satisfies the above range.
[0031] An example of a method for calculating the thickness of the intermediate region will be described below. Fig. 3 is a diagram showing the locations of X=40, 80, 120, 160, and 200 in the DMT elastic modulus image of Fig. 2. Fig. 4 is a graph showing the DMT elastic modulus profile at X=40 in the DMT elastic modulus image of Fig. 2. Fig. 5 is a graph showing the 9-point moving average line of the average DMT elastic modulus profile obtained from the DMT elastic modulus image of Fig. 2 and the thickness of the intermediate region (the vicinity of the intermediate region of the 9-point moving average line of the average DMT elastic modulus profile was extracted, and the Y coordinate was reassigned so that the intermediate region was near the center).
[0032] First, according to the above-mentioned method, a DMT elastic modulus image, E1r and E2r are obtained during the pullback process of the cantilever probe.
[0033] Next, in the DMT elastic modulus image during the pullback process, where the Y coordinate is 0-1 from top to bottom and the X coordinate is 0-1 from left to right, for example, DMT elastic modulus profiles (horizontal axis: pixel, vertical axis: DMT elastic modulus (GPa)) corresponding to Y=0-1 are obtained at positions spaced apart at 0.2 intervals in the X coordinate. Specifically, by plotting the DMT elastic modulus at X=0.2, Y=0-1 [(X,Y)=(0.2,0)-(0.2,1)] in the DMT elastic modulus image during the pullback process as the vertical axis and the corresponding Y coordinate as the horizontal axis, a DMT elastic modulus profile at X=0.2 can be obtained. This DMT elastic modulus profile is also created for another X position. That is, in the DMT elastic modulus image during the pullback process, a profile of DMT elastic modulus measured continuously along the thickness direction of the laminate film is obtained for each of a plurality of lines spaced apart at equal intervals in the in-plane direction of the laminate film.
[0034] Next, for the obtained multiple DMT elastic modulus profiles, the average value of the DMT elastic modulus is calculated for each Y coordinate (0 to 1) of the DMT elastic modulus image in the pullback process, and an average DMT elastic modulus profile is created. Furthermore, a 9-point moving average line of the average DMT elastic modulus profile is created in the average DMT elastic modulus profile. At that time, the Y coordinate of the DMT elastic modulus image on the horizontal axis is converted from pixel units to nm units. Next, on the graph of the 9-point moving average line of the average DMT elastic modulus profile, a horizontal line (horizontal line 1) corresponding to the average DMT elastic modulus (E1r) of the layer (PI-1) obtained above and a horizontal line (horizontal line 2) corresponding to the average DMT elastic modulus (E2r) of the layer (PI-2) obtained above are drawn, and the region between these horizontal lines 1 and 2 can be regarded as an intermediate region, and the width of this region (distance of the Y coordinate) can be regarded as the thickness of the intermediate region. In other words, the intermediate region can be said to be a region in which the elastic modulus of the laminated film changes continuously from E1r to E2r when the elastic modulus of the laminated film is continuously measured along the thickness direction by SPM during the retraction process of the cantilever probe in the thickness direction cross section of the laminated film.
[0035] The number of profiles obtained to obtain an average DMT elastic modulus profile may be 3 or more, preferably 5 or more, more preferably 5. The number of moving average lines may be 5 or more, preferably 9 or more, more preferably 9.
[0036] From the viewpoint of accurately measuring the average DMT elastic modulus (1) of layer (PI-1), the average DMT elastic modulus (2) of layer (PI-2) and the thickness of the intermediate region, it is preferable to expand the field of view and measure again when the thickness of the intermediate region exceeds 60% of the range in which the elastic modulus image is obtained. The thickness of the intermediate region is preferably 60% or less of the range in which the elastic modulus image is obtained. The range for measuring the average DMT modulus of the layers (PI-1) and (PI-2) may be any range excluding the intermediate region between the layers (PI-1) and (PI-2), and may be appropriately changed depending on the range for obtaining the DMT modulus image and the size of the intermediate region. The range can be determined by predicting the approximate position of the intermediate region from the DMT modulus image, but it is preferable to determine the range after confirming the region in which the DMT modulus does not change continuously on the moving average line of the average DMT modulus profile. Although not limited thereto, in one embodiment of the present invention, for example, in the nine-point moving average line shown in FIG. 5, there is an intermediate region in which the DMT elastic modulus changes continuously between the approximately corrugated portion (1) corresponding to the layer (PI-1) and the approximately corrugated portion (2) corresponding to the layer (PI-2). The average DMT elastic modulus (1) of the layer (PI-1) and the average DMT elastic modulus (2) of the layer (PI-2) may be measured except for the range from the peak (maximum value) of the mountain closest to the intermediate region of the approximately corrugated portion (1) to the peak (minimum value) of the valley closest to the intermediate region of the approximately corrugated portion (2). In addition, it is preferable that the average DMT elastic modulus (1) and the average DMT elastic modulus of the layer (PI-2) are each determined from measurements of preferably 1500 points or more, more preferably 2000 points or more, even more preferably 3000 points or more, and particularly preferably 5000 points or more. The intermediate region and its thickness can be determined, for example, by the method described in the Examples.
[0037] An example of a method for calculating the intermediate region and its thickness will be described in more detail below with reference to Figures 3 to 5. Figure 3 is a diagram showing the locations of X=40, 80, 120, 160, and 200 in the DMT elastic modulus image during the pullback process in Figure 2. Figure 4 is a DMT elastic modulus profile at X=40 in the DMT elastic modulus image, which is plotted as the vertical axis of the DMT elastic modulus at X=40, Y=0-255 [(X,Y)=(40,0)-(40,255)] and the corresponding Y coordinate as the horizontal axis. Similarly, by creating DMT elastic modulus profiles corresponding to Y=0-255 at X=80, 120, 160, and 200 in the DMT elastic modulus image, a profile of DMT elastic modulus continuously measured along the thickness direction of the laminated film is obtained in each of the five lines. For the five DMT elastic modulus profiles obtained, the average value of the DMT elastic modulus is calculated for each Y coordinate (0 to 255) of the DMT elastic modulus image to create an average DMT elastic modulus profile, and further, a 9-point moving average line of the average DMT elastic modulus profile is created in the average DMT elastic modulus profile as shown in Figure 5. The thickness of the intermediate region can be obtained from the graph of the 9-point moving average line of the average DMT elastic modulus profile, horizontal line 1 indicating E1r, and horizontal line 2 indicating E2r.
[0038] The thickness of (E1r-E1a), (E2r-E2a), and (E1r-E1a) / (E2r-E2a) in formula (I) and the intermediate region can be controlled by appropriately adjusting the type and composition of the structural units constituting the PI resin contained in each PI resin-containing layer, the molecular weight of the PI resin, the composition and combination of each PI resin-containing layer in the laminate film, and / or the coating conditions in film formation, the state of the multilayer coating film at the time of imidization, the manufacturing method such as imidization conditions, etc. For example, the thickness of (E1r-E1a), (E2r-E2a), and (E1r-E1a) / (E2r-E2a) in formula (I) and the intermediate region can be appropriately adjusted based on preferred aspects advantageous for improving the pin puncture strength and reducing Df, which will be described later, such as the structural units of the preferred PI resin and their contents, the solvent contained in the preferred PI resin precursor solution, the state of the multilayer coating film at the time of imidization, which will be described later, and the preferred imidization conditions, which will be described later. As described later, by imidizing the multilayer coating film in a state where the solvent is sufficiently present (or well-dispersed) throughout the film during imidization, preferably by passing through a step of leaving the film to stand, as described later, (E1r-E1a) / (E2r-E2a) and the thickness of the intermediate region tend to increase, and (E1r-E1a) / (E2r-E2a) and the thickness of the intermediate region can be adjusted to the desired range. In addition, by creating a state where the solvent is sufficiently present throughout the multilayer coating film during imidization, by making adjacent PI resin-containing layers different layers (preferably an mPI layer and a TPI layer, respectively), and / or by making adjacent PI resin-containing layers have different thicknesses, (E1r-E1a) / (E2r-E2a) and the thickness of the intermediate region tend to increase, and (E1r-E1a) / (E2r-E2a) and the thickness of the intermediate region can be easily adjusted to the desired range.
[0039] <Layer configuration> A configuration suitable for obtaining a laminated film that satisfies formula (I) will be described below. A laminated film that satisfies formula (I) has high puncture strength, and particularly preferably has high puncture strength while having dielectric properties suitable for high-speed communication applications such as 5G. In this specification, the dielectric properties refer to dielectric properties such as Df and Dk, and increasing or improving the dielectric properties refers to decreasing Df and / or Dk. Furthermore, the mechanical properties refer to mechanical properties including puncture strength, bending resistance, and elastic modulus (including DMT elastic modulus), and increasing or improving the mechanical properties refers to, for example, increasing the puncture strength, bending resistance, and / or elastic modulus. Furthermore, the thermal properties may include CTE, glass transition temperature (hereinafter sometimes referred to as Tg), the degree of thermal denaturation or deterioration, and increasing or improving the thermal properties refers to, for example, decreasing the CTE, increasing the Tg, and / or reducing thermal denaturation or deterioration.
[0040] The laminated film of the present invention includes a PI-based resin-containing layer (PI-1) and a PI-based resin-containing layer (PI-2). The laminated film of the present invention may include other PI-based resin-containing layers than these PI-based resin-containing layers, or may include other layers than the PI-based resin-containing layer. Examples of other layers include a pressure-sensitive adhesive layer for bonding the PI-based resin-containing layer to the metal foil layer. In a preferred embodiment of the present invention, from the viewpoint of increasing the puncture strength of the laminated film, the laminated film of the present invention preferably includes a PI-based resin-containing layer (PI-3) in addition to the PI-based resin-containing layer (PI-1) and the PI-based resin-containing layer (PI-2). In such an embodiment, the laminated film of the present invention preferably includes the PI-based resin-containing layer (PI-2), the PI-based resin-containing layer (PI-1), and the PI-based resin-containing layer (PI-3) in this order, and more preferably includes them adjacent to each other in this order. The laminate film including the PI resin-containing layer (PI-1), the PI resin-containing layer (PI-2), and the PI resin-containing layer (PI-3) (sometimes referred to as PI resin-containing layers (PI-1) to (PI-3) or layers (PI-1) to (PI-3)) is sometimes referred to as the laminate film (L).
[0041] As shown in Fig. 6, the laminate film 1 in a preferred embodiment of the present invention is composed of three adjacent layers, a PI-based resin-containing layer 11, a PI-based resin-containing layer 12, and a PI-based resin-containing layer 13, which are laminated on a metal foil 21 to form a laminate sheet 2. From the viewpoint of easily controlling the parameter X and the thickness of the intermediate region within the above-mentioned specific range and realizing even higher pin puncture strength and dielectric properties, the PI-based resin-containing layer 11 preferably corresponds to layer (PI-2), the PI-based resin-containing layer 12 to layer (PI-1), and the PI-based resin-containing layer 13 to layer (PI-3). The laminate film 1 may also include other PI-based resin-containing layers other than the layers (PI-1), (PI-2), and (PI-3), or other layers other than the PI-based resin-containing layers. Examples of other layers include pressure-sensitive adhesive layers formed of polymeric materials such as acrylic resins other than PI resins.
[0042] In one embodiment of the present invention, the thickness of the laminated film is preferably 20 μm or more, more preferably 25 μm or more, even more preferably 30 μm or more, even more preferably 35 μm or more, particularly preferably 40 μm or more, and preferably 150 μm or less, more preferably 130 μm or less, even more preferably 100 μm or less, even more preferably 90 μm or less, particularly preferably 80 μm or less, particularly more preferably 70 μm or less, and particularly more preferably 60 μm or less. When the thickness of the laminated film is within the above range, the laminated film can have mechanical properties such as high puncture strength and flexibility suitable for flexible printed circuit boards and the like. In addition, since the Df of the laminated film can be reduced and the puncture strength can be improved, a laminated film having a good balance between mechanical properties suitable for flexible printed circuit boards and dielectric properties suitable for high-speed communication applications such as 5G can be obtained.
[0043] In one embodiment of the present invention, the thickness of the layer (PI-2) is preferably 0.05 to 0.3 times that of the layer (PI-1). When the thicknesses are in the above relationship, the laminated film can have mechanical properties such as high puncture strength and flexibility suitable for flexible printed circuit boards. In addition, since the Df of the laminated film can be reduced and the puncture strength can be improved, a laminated film having a good balance between mechanical properties suitable for flexible printed circuit boards and dielectric properties suitable for high-speed communication applications such as 5G can be obtained. In particular, when the thickness of the laminated film is 20 to 100 μm and the thickness of the layer (PI-2) is 0.05 to 0.3 times that of the layer (PI-1), the effects of the present invention are more easily obtained. The thickness of the layer (PI-2) is more preferably 0.08 times or more, even more preferably 0.10 times or more, particularly preferably 0.12 times or more, and more preferably 0.25 times or less, even more preferably 0.23 times or less, particularly preferably 0.20 times or less, relative to the thickness of the layer (PI-1). When the laminated film of the present invention has a layer (PI-3), the thickness of the layer (PI-3) may be selected from the range of the layer (PI-2) above.
[0044] In one embodiment of the present invention, the thickness of each PI resin-containing layer included in the laminate film is usually in the range of 0.5 to 100 μm, and may be appropriately determined depending on the function, use, etc. of each PI resin-containing layer. For example, in one embodiment of the present invention, the thickness of the layer (PI-1) is usually 5 μm or more, preferably 10 μm or more, more preferably 15 μm or more, even more preferably 20 μm or more, even more preferably 30 μm or more, and preferably 80 μm or less, more preferably 60 μm or less, even more preferably 55 μm or less, and even more preferably 50 μm or less. In addition, the thickness of the layer (PI-2) is usually 0.5 μm or more, preferably 1 μm or more, more preferably 2 μm or more, even more preferably 3 μm or more, even more preferably 4 μm or more, and preferably 20 μm or less, more preferably 15 μm or less, even more preferably 10 μm or less, and even more preferably 8 μm or less. The thickness of the layer (PI-2) and the thickness of the layer (PI-3) may be the same or different from each other, but from the viewpoint of suppressing warping of the laminated film, preferably one value is within ±25% of the other value, more preferably within ±20%. The thickness of each layer can be measured using, for example, a laser microscope or SPM. For example, when the laminated film has an intermediate region between the layer (PI-1) and the layer (PI-2), the intermediate region and its thickness can be obtained using SPM, and the distance from the surface of the layer (PI-1) to the interface between the intermediate region and the surface of the layer (PI-2) can be the thickness of the layer (PI-1), and the distance from the surface of the layer (PI-2) to the interface between the intermediate region and the surface of the layer (PI-2) can be the thickness of the layer (PI-2). For example, when the laminated film (L) has an intermediate region 1 between the layer (PI-1) and the layer (PI-2), and an intermediate region 2 between the layer (PI-1) and the layer (PI-3), the thickness of the layer (PI-1) can be the distance from the interface between the layer (PI-1) and the intermediate region 1 to the interface between the layer (PI-1) and the intermediate region 2, and can be obtained by determining the intermediate region 1, the intermediate region 2, the layer (PI-2), and the layer (PI-3) as described above, and subtracting the total thickness of these from the thickness (total thickness) of the laminated film. The thickness of each layer may be obtained, for example, by the method described in the Examples.
[0045] In the laminated film of the present invention, the polyimide-based resins constituting the layer (PI-1) and the layer (PI-2) are not particularly limited as long as they satisfy the formula (I). However, from the viewpoint of enhancing the puncture strength while maintaining excellent dielectric properties, the layer (PI-1) and the layer (PI-2) are each preferably a non-thermoplastic polyimide-based resin-containing layer (hereinafter sometimes referred to as an mPI layer) or a thermoplastic polyimide-based resin-containing layer (hereinafter sometimes referred to as a TPI layer), and it is more preferable that one of the layer (PI-1) and the layer (PI-2) is an mPI layer and the other is a TPI layer. The mPI layer generally becomes the main PI-based resin-containing layer in the laminated film for flexible printed circuit board applications. The TPI layer is a layer that can also function as an adhesive layer for bonding the laminated film to a metal foil (for example, a copper foil), and is preferably located in the outermost layer that can be in contact with the metal foil in the laminated film. In a laminated film containing three or more PI-based resin-containing layers, at least one PI-based resin-containing layer is preferably an mPI layer, and at least one layer (preferably at least two layers) of the PI-based resin-containing layers is preferably a TPI layer, and it is more preferable to have a TPI layer, an mPI layer, and a TPI layer in this order. Therefore, in the laminated film (L), the layer (PI-1) is preferably an mPI layer, and the layer (PI-2) and the layer (PI-3) are each preferably a TPI layer. When the laminated film (L) has such a layer structure, improved thermal physical properties can be ensured in the mPI layer, thermal deformation and deterioration can be suppressed, dimensional stability of the laminated film can be ensured, and the adhesiveness to a metal foil (for example, a copper foil) can be enhanced by the TPI layer. When the laminated film (L) contains a plurality of TPI layers or mPI layers, the configurations of the plurality of TPI layers or mPI layers contained may be the same or different from each other. Further, in the laminated film (L), usually, the configuration of the layer (PI-1) is different from that of the layer (PI-2) and the layer (PI-3), but the configuration of the layer (PI-2) and the layer (PI-3) may be the same or different.
[0046] <PI-based resin> The PI resin constituting each PI resin-containing layer in the laminate film of the present invention may be any resin that can constitute the PI resin-containing layer so as to satisfy formula (I). The PI resin is a resin that contains a repeating structural unit containing an imide group, and may contain a repeating structural unit containing both an imide group and an amide group. In the present invention, a "non-thermoplastic" polyimide resin is one having a storage modulus of 1.0×10 at 40° C. as measured using a dynamic viscoelasticity measuring device (DMA). 9 Pa or more, and the storage modulus at 300°C is 1.0 x 10 8 A "thermoplastic" polyimide resin has a storage modulus of 1.0×10 Pa or more at 40°C. 9 Pa or more, and the storage modulus at 300°C is 1.0 x 10 8 It means a polyimide resin having a storage modulus of less than Pa. The storage modulus can be measured, for example, by the method described in the Examples.
[0047] In the present invention, the PI resin constituting each PI resin-containing layer preferably contains a tetracarboxylic anhydride-derived structural unit (A) and a diamine-derived structural unit (B) from the viewpoint of increasing the pin puncture strength and dielectric properties of the laminated film. In the present invention, the term "structural unit derived from" means "structural unit derived from", for example, "structural unit (A) derived from tetracarboxylic anhydride" means "structural unit (A) derived from tetracarboxylic anhydride". In addition, "the PI resin-containing layer contains the structural unit (A)" means "the PI resin constituting the PI resin-containing layer contains the structural unit (A)", and the same applies to other structural units.
[0048] (Structural unit (A) derived from tetracarboxylic acid anhydride) The structural unit (A) derived from a tetracarboxylic acid anhydride (hereinafter, sometimes simply referred to as the structural unit (A)) is, for example, a structural unit represented by the formula (1): [ka] [In formula (1), Y represents a tetravalent organic group] It is preferable that the structural unit is a structural unit derived from a tetracarboxylic acid anhydride represented by the following formula:
[0049] In formula (1), Y's each independently represent a tetravalent organic group, preferably a tetravalent organic group having 4 to 40 carbon atoms, more preferably a tetravalent organic group having 4 to 40 carbon atoms and a cyclic structure. Examples of the cyclic structure include an alicyclic ring, an aromatic ring, and a heterocyclic structure. The organic group may have a hydrogen atom substituted with a halogen atom, a hydrocarbon group, an alkoxy group, or a halogenated hydrocarbon group, and in that case, the number of carbon atoms of these groups is preferably 1 to 8. In the present invention, the PI resin may contain multiple types of Y, and the multiple types of Y may be the same or different from each other. Examples of Y include groups or structures represented by formulae (31) to (40); groups in which hydrogen atoms in the groups represented by formulae (31) to (40) are substituted with methyl groups, ethyl groups, n-propyl groups, isopropyl groups, n-butyl groups, isobutyl groups, sec-butyl groups, tert-butyl groups, fluoro groups, chloro groups, or trifluoromethyl groups; and tetravalent chain hydrocarbon groups having 1 to 8 carbon atoms.
[0050] [ka] [In formulas (31) to (33), R 19 ~R 26 and R 23’ ~R 26’ each independently represents a hydrogen atom, an alkyl group having 1 to 6 carbon atoms, an alkoxy group having 1 to 6 carbon atoms, or an aryl group having 6 to 12 carbon atoms; R 19 ~R 26 and R 23’ ~R 26’ may be substituted with a halogen atom, V 1 and V 2 are each independently a single bond (except when e+d=1), -O-, -CH2-, -CH2-CH2-, -CH(CH3)-, -C(CH3)2-, -C(CF3)2-, -SO2-, -S-, -CO-, -N(R j )- or formula (a) [ka] (In formula (a), R 27 ~R 30 each independently represents a hydrogen atom or an alkyl group having 1 to 6 carbon atoms, D's each independently represent a single bond, -C(CH3)2- or -C(CF3)2; i represents an integer from 1 to 3; * represents a bond.) represents R j represents a hydrogen atom or a monovalent hydrocarbon group having 1 to 12 carbon atoms which may be substituted with a halogen atom, e and d each independently represent an integer of 0 to 2 (provided that e+d is not 0); f represents an integer from 0 to 3; g and h each independently represent an integer of 0 to 4; In formula (39), Z represents a divalent organic group. R a3 each independently represents a halogen atom, or an alkyl group, an alkoxy group, an aryl group, or an aryloxy group which may have a halogen atom; Each s is independently an integer of 0 to 3; In formula (40), R a2 each independently represents a halogen atom, or an alkyl group, an alkoxy group, an aryl group, or an aryloxy group which may have a halogen atom; 1 each independently represents an integer of 0 to 3; * represents a bond.
[0051] In the present invention, the PI resin constituting each PI resin-containing layer preferably contains, as Y in formula (1), at least one structure selected from the group consisting of structures represented by formulas (31), (32), (33), (39), and (40), more preferably at least one structure selected from the group consisting of structures containing a benzene skeleton, and further preferably at least one structure selected from the group consisting of structures represented by formulas (32), (39), and (40), from the viewpoint of improving the pin puncture strength, dielectric properties, and thermal properties of the laminate film.
[0052] In formulas (31) to (33), R 19 ~R 26 and R 23’ ~R 26’ are each independently preferably a hydrogen atom or an alkyl group having 1 to 6 carbon atoms, more preferably a hydrogen atom or an alkyl group having 1 to 3 carbon atoms, and further preferably a hydrogen atom.
[0053] In equation (31), V 1 and V 2 each independently preferably represents a single bond (except when e+d=1), -O-, -CH2-, -C(CH3)2-, -C(CF3)2- or -CO-, and more preferably represents a single bond (except when e+d=1), -O-, -C(CH3)2- or -C(CF3)2-.
[0054] In formula (31), e and d each independently preferably represent 0 or 1 (provided that e+d is not 0). Also, e+d preferably represents 1. In formula (31), when e is 0, the two benzene rings are V 1 When d is 0, the two benzene rings are V 2 indicates that there is no bond.
[0055] In the formulae (32) and (33), f preferably represents 0 or 1, and more preferably 0.
[0056] In formula (33), g and h each independently represent an integer of preferably 0 to 2, more preferably 0 or 1. Furthermore, g+h each independently represents an integer of preferably 0 to 2. When f is 1 or more, multiple g's and multiple h's may each independently be the same or different.
[0057] In formula (a), R 27 ~R 30 are each independently preferably a hydrogen atom or an alkyl group having 1 to 3 carbon atoms, more preferably a hydrogen atom. i is preferably 1 or 2, and when i is 2 or more, a plurality of D and R 27 ~R 30 may be the same or different, independently of each other.
[0058] In formula (39), Z preferably represents a divalent organic group having 4 to 40 carbon atoms, more preferably represents a divalent organic group having 4 to 40 carbon atoms and a cyclic structure, further preferably represents a divalent organic group having 4 to 40 carbon atoms and an aromatic ring, and particularly preferably represents a divalent organic group represented by formula (z1), formula (z2), or formula (z3): [ka] [In formulas (z1) to (z3), R z11 ~R z14 each independently represents a hydrogen atom or a monovalent hydrocarbon group which may have a halogen atom; R z2 each independently represents a monovalent hydrocarbon group which may have a halogen atom; n represents an integer of 1 to 4; each j independently represents an integer of 0 to 3; and * represents a bond. and particularly preferably represents a divalent organic group represented by formula (z1).
[0059] In formula (z1), R z11 ~R z14R in formula (z1) each independently represents preferably a hydrogen atom or an alkyl group which may have a halogen atom, more preferably a hydrogen atom or an alkyl group having 1 to 6 carbon atoms which may have a halogen atom, further preferably a hydrogen atom or an alkyl group having 1 to 3 carbon atoms which may have a halogen atom, and particularly preferably a hydrogen atom. z11 ~R z14 In a benzene ring having R z11 ~R z14 At least one of R may be a monovalent hydrocarbon group which may have a halogen atom. z11 ~R z14 It is particularly preferable that all of are hydrogen atoms.
[0060] In the formula (z1), n is preferably an integer of 1 to 3, more preferably 1 or 2, and further preferably 2.
[0061] In formula (z2), R z2 are each independently preferably an alkyl group which may have a halogen atom, more preferably an alkyl group having 1 to 6 carbon atoms which may have a halogen atom, and further preferably an alkyl group having 1 to 3 carbon atoms which may have a halogen atom.
[0062] In formula (z2), j's are preferably each independently 0 or 1, more preferably 0, and further preferably all j's are 0.
[0063] In formula (39), R a3 preferably each independently represents an alkyl group having 1 to 6 carbon atoms, an alkoxy group having 1 to 6 carbon atoms, or an aryl group having 6 to 12 carbon atoms. R a3 The hydrogen atoms contained in R may be substituted with halogen atoms, independently of each other. a3 each independently represents an alkyl group preferably having 1 to 6 carbon atoms, more preferably an alkyl group having 1 to 3 carbon atoms.
[0064] In the formula (39), each s preferably represents an integer of 0 to 2, and more preferably 0 or 1, independently.
[0065] In formula (40), R a2 preferably each independently represents an alkyl group having 1 to 6 carbon atoms, an alkoxy group having 1 to 6 carbon atoms, or an aryl group having 6 to 12 carbon atoms. R a2 The hydrogen atoms contained in R may be substituted with halogen atoms, independently of each other. a2 are each independently preferably an alkyl group having 1 to 6 carbon atoms, and more preferably an alkyl group having 1 to 3 carbon atoms.
[0066] In the formula (40), each 1 preferably represents an integer of 0 to 2, and more preferably 0 or 1, independently.
[0067] Specific examples of the structures represented by formulae (31) to (33), (39) and (40) include structures represented by formulae (41) to (56). In these formulae, * represents a bond.
[0068] [ka]
[0069] In one embodiment of the present invention, when the PI resin constituting the PI resin-containing layer contains at least one selected from the group consisting of the structures represented by the formulas (31) to (33), (39) and (40) as Y in formula (1), the proportion of the structural units derived from tetracarboxylic anhydrides represented by at least one selected from the group consisting of the structures represented by the formulas (31) to (33), (39) and (40) in which Y in formula (1) is at least one selected from the group consisting of the structures represented by the formulas (31) to (33), (39) and (40), in particular the proportion of the structural units derived from tetracarboxylic anhydrides represented by at least one selected from the group consisting of the structures represented by the formulas (32), (39) and (40) in which Y in formula (1) is at least one selected from the group consisting of the structures represented by the formulas (32), (39) and (40), is preferably 30 mol% or more, more preferably 50 mol% or more, even more preferably 70 mol% or more, particularly preferably 90 mol% or more, and preferably 100 mol% or less, based on the total amount of the structural units (A). The proportion within the above range is advantageous in improving the pin puncture strength and dielectric properties of the laminated film. The ratio of the structural units is, for example, 1 It can be measured using H-NMR, or can be calculated from the ratio of raw materials. The same applies to the calculation of the ratio of the structural units of the PI resin below. In addition, in this specification, the "total amount" of the structural unit means the amount of the unit when the structural unit is composed of one unit, and means the total amount of the units when the structural unit is composed of two or more units.
[0070] (Structural unit (A1) and structural unit (A2)) In one embodiment of the present invention, the PI resin contained in at least one of the layers (PI-1) and (PI-2) or at least one of the layers (PI-1) to (PI-3) constituting the laminate film of the present invention contains a structural unit (A), and the structural unit (A) is represented by the formula (A1): [ka] [In formula (A1), R a1 each independently represents a halogen atom, or an alkyl group, an alkoxy group, an aryl group, or an aryloxy group which may have a halogen atom; k represents an integer from 0 to 2. and / or a structural unit (A1) derived from a tetracarboxylic acid anhydride represented by the formula (A2): [ka] [In formula (A2), R a2 each independently represents a halogen atom, or an alkyl group, an alkoxy group, an aryl group, or an aryloxy group which may have a halogen atom, and each 1 independently represents an integer of 0 to 3. It is preferable that the tetracarboxylic acid anhydride-derived structural unit (A2) (hereinafter, may be simply abbreviated as structural unit (A2)) is represented by the following formula: In this specification, "at least one PI resin-containing layer" or "at least one PI resin-containing layer" can be read as "at least one of the PI resin-containing layers (PI-1) and (PI-2), or at least one of the PI resin-containing layers (PI-1) to (PI-3)."
[0071] When the PI resin contains the structural unit (A1) and / or the structural unit (A2) as the structural unit (A), it becomes easier to control the parameter X and the thickness of the intermediate region in the laminate film within the desired range, and the pin puncture strength and dielectric properties can be improved. In addition, the CTE of the laminate film tends to decrease, and the dimensional stability of the laminate film can be improved.
[0072] From the viewpoint of improving the puncture strength, dielectric properties, CTE, etc., in formula (A1) and formula (A2), R a1 and R a2 are preferably, independently, an alkyl group having 1 to 6 carbon atoms, an alkoxy group having 1 to 6 carbon atoms, or an aryl group having 6 to 12 carbon atoms. Examples of the alkyl group having 1 to 6 carbon atoms include a methyl group, an ethyl group, an n-propyl group, an isopropyl group, an n-butyl group, an isobutyl group, a sec-butyl group, a tert-butyl group, an n-pentyl group, a 2-methylbutyl group, a 3-methylbutyl group, a 2-ethylpropyl group, and an n-hexyl group. Examples of the alkoxy group having 1 to 6 carbon atoms include a methoxy group, an ethoxy group, a propyloxy group, an isopropyloxy group, an n-butoxy group, an isobutoxy group, a sec-butoxy group, a tert-butoxy group, a pentyloxy group, a hexyloxy group, and a cyclohexyloxy group. Examples of the aryl group having 6 to 12 carbon atoms include a phenyl group, a tolyl group, a xylyl group, a naphthyl group, and a biphenyl group. R a1 and R a2 The hydrogen atoms contained in R may be substituted with halogen atoms, independently of one another. Examples of the halogen atoms include fluorine atoms, chlorine atoms, bromine atoms, and iodine atoms. a1 and R a2 are each independently preferably an alkyl group having 1 to 6 carbon atoms, and more preferably an alkyl group having 1 to 3 carbon atoms.
[0073] The bonding positions of the two carboxylic acid anhydrides bonded to the benzene ring in formula (A1) are not particularly limited, but from the viewpoint of improving pin puncture strength, dielectric properties, CTE, etc., the bonding positions are preferably 1,2-positions and 4,5-positions, or 1,2-positions and 3,4-positions, and more preferably 1,2-positions and 4,5-positions. k is preferably 0 or 1, and more preferably 0.
[0074] The bonding positions of the two carboxylic acid anhydrides bonded to the benzene rings constituting the biphenyl skeleton in formula (A2) are not particularly limited and may be 3,4- or 2,3-, independently of each other, based on the single bond bonding the two benzene rings. From the viewpoint of improving the pin puncture strength, dielectric properties, CTE, and the like, 3,4- is preferred. In formula (A2), each 1 is independently preferably an integer of 0 to 2, more preferably 0 or 1, and further preferably 0.
[0075] In a preferred embodiment of the present invention, formula (A1) is represented by formula (A1-1): [ka] In another preferred embodiment of the present invention, the structural unit (A2) is a structural unit (A2-1) represented by the formula (A2-1): [ka] The structural unit (A2-1) is represented by the formula: When the PI resin contains the structural unit (A1-1) and / or the structural unit (A2-1) as the structural unit (A), it becomes easier to control the parameter X and the thickness of the intermediate region in the laminated film within the desired range, which is advantageous in improving the pin puncture strength and dielectric properties. Furthermore, the CTE of the laminated film tends to decrease, and the dimensional stability of the laminated film can be expected to improve.
[0076] In one embodiment of the present invention, the PI resin-containing layer preferably includes one or more of the following components. The PI resin in layers (PI-1) and (PI-2), or layers (PI-1) to (PI-3) in the laminate film each contains at least one of the structural unit (A1) and the structural unit (A2); The PI resin in the layer (PI-1) and the layer (PI-2), or in the layers (PI-1) to (PI-3) in the laminate film, each contains the structural unit (A1); In at least one PI resin-containing layer in the laminate film, preferably a TPI layer, the PI resin contains the structural unit (A1) and the structural unit (A2); In at least one PI resin-containing layer in the laminate film, preferably a TPI layer, the PI resin contains the structural unit (A1) and the structural unit (A2), and in at least another PI resin-containing layer, preferably an mPI layer, the PI resin contains the structural unit (A1) and / or the structural unit (A2). In at least one PI resin-containing layer in the laminate film, preferably the TPI layer, the PI resin contains the structural unit (A1) and the structural unit (A2), and in at least another PI resin-containing layer, preferably the mPI layer, the PI resin contains the structural unit (A1) but does not substantially contain the structural unit (A2). In this specification, "substantially does not contain structural units" means that the content of the structural unit is 1% by mass or less, preferably 0.1% by mass or less, more preferably 0.01% by mass or less, and particularly preferably 0.001% by mass or less. For example, "substantially does not contain structural unit (A2)" means that the content of structural unit (A2) is 1% by mass or less, preferably 0.1% by mass or less, more preferably 0.01% by mass or less, and particularly preferably 0.001% by mass or less, based on the total amount of structural units (A). Hereinafter, unless otherwise clearly stated, the same applies to other structural units.
[0077] In one embodiment of the present invention, when the PI resin contains the structural unit (A1) and / or the structural unit (A2), the content of each of them is preferably 10 mol% or more, more preferably 15 mol% or more, even more preferably 20 mol% or more, even more preferably 25% or more, and particularly preferably 30 mol% or more, based on the total amount of the structural unit (A), and is also preferably 90 mol% or less, more preferably 85 mol% or less, even more preferably 80 mol% or less, even more preferably 75 mol% or less, and particularly preferably 70 mol% or less. When the contents of the structural unit (A1) and the structural unit (A2) are each within the above range, it becomes easier to control the parameter X and the thickness of the intermediate region in the laminated film to the desired range, which is advantageous in improving the pin puncture strength and dielectric properties. Furthermore, the CTE of the laminated film tends to decrease, and improvement in the dimensional stability of the laminated film can be expected.
[0078] Furthermore, in one embodiment of the present invention, when the PI resin contains the structural unit (A1) and the structural unit (A2), the content ratio (molar ratio, (A1):(A2)) is preferably 10:90 to 90:10, more preferably 15:85 to 80:20, even more preferably 20:80 to 70:30, and even more preferably 25:75 to 65:35. When the content ratio of the structural unit (A1) to the structural unit (A2) is within the above range, the above-mentioned effects of the present invention that are expected from the PI resin having the structural unit (A1) and / or the structural unit (A2) are more easily achieved, and these effects can be further enhanced.
[0079] (Structural unit (A3)) In one embodiment of the present invention, the PI resin contained in at least one of the layers (PI-1) and (PI-2) or at least one of the layers (PI-1) to (PI-3) constituting the laminate film of the present invention has a structural unit (A) represented by the formula (A3): [ka] [In formula (A3), Z represents a divalent organic group, R a3 each independently represents a halogen atom, or an alkyl group, an alkoxy group, an aryl group, or an aryloxy group which may have a halogen atom; Each s independently represents an integer from 0 to 3. The copolymer may contain a structural unit (A3) derived from an ester bond-containing tetracarboxylic acid anhydride represented by the following formula (hereinafter, sometimes simply referred to as structural unit (A3)).
[0080] When the PI resin contains the structural unit (A3) as the structural unit (A), it is easy to control the parameter X and the thickness of the intermediate region in the laminate film to a desired range, which can be advantageous in improving the pin puncture strength and dielectric properties of the laminate film. In addition, the CTE of the laminate film tends to decrease, and the dimensional stability of the laminate film can be improved. Furthermore, since the pin puncture strength and dielectric properties can be increased even at a relatively low imidization temperature (e.g., 360°C or lower), even when a laminate sheet is produced by thermally imidizing a PI resin precursor coating film in a laminate configuration with a metal foil (e.g., copper foil), deterioration of the metal foil surface can be suppressed, and a laminate sheet having high pin puncture strength and excellent high-frequency properties can be obtained.
[0081] R in formula (A3) a3 As the above, R in the formula (39) a3 The same groups as those exemplified as above can be mentioned, and the preferred embodiments are also the same. In formula (A3), each s is preferably 0 or 1, more preferably 0, independently.
[0082] Z in the formula (A3) may be the same divalent organic group as exemplified as Z in the above-described formula (39), and preferred embodiments are also the same.
[0083] In a preferred embodiment of the present invention, formula (A3) is preferably a structural unit (A3-1) represented by formula (A3-1) or a structural unit (A3-2) represented by formula (A3-2). [ka]
[0084] When the PI resin contained in at least one layer of the PI resin-containing layer constituting the laminate film contains the structural unit (A3-1) and / or the structural unit (A3-2) as the structural unit (A), the parameter X in the laminate film and the thickness of the intermediate region can be easily controlled within a desired range, which can be advantageous in improving the pin puncture strength and dielectric properties of the laminate film. In addition, the CTE of the laminate film tends to decrease, and the dimensional stability of the laminate film can be improved. Furthermore, since the pin puncture strength and dielectric properties can be increased even at a relatively low imidization temperature (e.g., 360°C or lower), even when a laminate sheet is produced by thermally imidizing a PI resin precursor coating film in a laminated configuration with a metal foil (e.g., copper foil), deterioration of the metal foil surface can be suppressed, and a laminate sheet having high pin puncture strength and excellent high-frequency properties can be obtained.
[0085] In one embodiment of the present invention, when the PI resin constituting at least one PI resin-containing layer constituting the laminate film, preferably at least layer (PI-1), more preferably the mPI layer, contains the structural unit (A3) as the structural unit (A), particularly the structural unit (A3-1) and / or the structural unit (A3-2), the PI resin is not too rigid and can have a flexible structure with a certain degree of freedom, so that a branched structure is easily formed by heating during imidization, and the pin puncture strength of the laminate film can be further improved. In addition, the Df of the laminate film is further reduced, and the CTE is reduced, tending to improve the dimensional stability of the laminate film.
[0086] In one embodiment of the present invention, when the PI resin contains the structural unit (A3), the content thereof is preferably 3 mol% or more, more preferably 5 mol% or more, even more preferably 7 mol% or more, and even more preferably 10 mol% or more, based on the total amount of the structural unit (A), and may be, for example, 20 mol% or more, 30 mol% or more, or 40 mol% or more. The content of the structural unit (A3) is preferably 80 mol% or less, more preferably 70 mol% or less, even more preferably 65 mol% or less, and even more preferably 60 mol% or less. When the content of the structural unit (A3) is within the above range, the above-mentioned effects of the present invention that are expected from the PI resin having the structural unit (A3) are easily obtained, and the effects can be further enhanced.
[0087] In another embodiment of the present invention, the structural unit (A) of the PI resin contained in at least the PI resin-containing layer (PI-1) preferably contains 45 mol % or less (0 to 45 mol %) of the structural unit (A3) relative to the total amount of the structural unit (A). That is, in such an embodiment, the structural unit (A) of the PI resin may or may not contain the structural unit (A3), and when it contains the structural unit (A3), it contains it in an amount of 45 mol % or less. Furthermore, the content of the structural unit (A3) is more preferably 35 mol % or less, even more preferably 25 mol % or less, even more preferably 15 mol % or less, particularly preferably 5 mol % or less, and particularly preferably 1 mol % or less relative to the total amount of the structural unit (A), and the lower limit may be 0 mol %. When the content of the structural unit (A3), particularly the structural unit (A3-1) and / or the structural unit (A3-2) in the PI resin is less than the upper limit, the parameter X and the thickness of the intermediate region in the laminated film can be easily controlled to a desired range, and the pin puncture strength and dielectric properties of the laminated film can be further improved. In addition, the CTE of the laminated film tends to decrease, and improved dimensional stability of the laminated film can be expected.
[0088] In one embodiment of the present invention, it is more preferable that in at least one PI resin-containing layer constituting the laminate film, preferably the TPI layer, the PI resin contains the structural unit (A1) and the structural unit (A2), and that in at least another PI resin-containing layer, preferably the mPI layer, the PI resin contains at least two structural units selected from the structural unit (A1), the structural unit (A2), and the structural unit (A3), preferably the structural unit (A1) and the structural unit (A2) and / or the structural unit (A3).
[0089] (Structural unit (A4)) In one embodiment of the present invention, the PI resin may contain, as the structural unit (A), a structural unit (A4) (hereinafter sometimes simply referred to as structural unit (A4)) derived from a tetracarboxylic acid anhydride other than the structural units (A1), (A2), and (A3). In this specification, "structural unit (A4) derived from a tetracarboxylic acid anhydride other than structural unit (A1), structural unit (A2), and structural unit (A3)" means a structural unit derived from a tetracarboxylic acid anhydride that does not fall under any of structural units (A1), (A2), and (A3), and "the content of structural unit (A4)" means the total amount of structural unit (A4) when a plurality of structural units (A4) are present.
[0090] In one embodiment of the present invention, examples of the structural unit (A4) include structural units derived from tetracarboxylic anhydrides in which Y in formula (1) is represented by formula (31), or formula (33) to formula (38). From the viewpoint of improving the pin puncture strength and dielectric properties of the laminated film, preferably, Y in formula (1) is a structural unit derived from tetracarboxylic anhydrides represented by formula (42), or formula (44) to formula (49), or formula (53), and more preferably, Y in formula (1) is a structural unit derived from tetracarboxylic anhydrides represented by formula (42), or formula (46), or formula (49), or formula (53).
[0091] In one embodiment of the present invention, when the PI resin contains the structural unit (A4), the content thereof relative to the total amount of the structural units (A) may be, for example, 0.01 to 55 mol %, or 0.01 to 40 mol %, and is preferably 40 mol % or less, more preferably 35 mol % or less, even more preferably 30 mol % or less, and particularly preferably 25 mol % or less, and is usually 0.01 mol % or more, and preferably 10 mol % or more.
[0092] (Diamine-derived structural unit (B)) The PI resin constituting each PI resin-containing layer usually contains a diamine-derived structural unit (B) (hereinafter, sometimes simply abbreviated as structural unit (B)). The structural unit (B) is, for example, a structural unit represented by the formula (2): [ka] [In formula (2), X represents a divalent organic group] It is preferable that the diamine-derived structural unit is represented by the following formula:
[0093] In formula (2), X represents a divalent organic group, preferably a divalent organic group having 2 to 100 carbon atoms. Examples of the divalent organic group include a divalent aromatic group and a divalent aliphatic group, and examples of the divalent aliphatic group include a divalent acyclic aliphatic group or a divalent cyclic aliphatic group. Among these, from the viewpoint of increasing the pin puncture strength and dielectric properties of the laminated film, a divalent cyclic aliphatic group and a divalent aromatic group are preferred, and a divalent aromatic group is more preferred. The divalent organic group may have a hydrogen atom in the organic group substituted with a halogen atom, a hydrocarbon group, an alkoxy group, or a halogenated hydrocarbon group, and in that case, the number of carbon atoms in these groups is preferably 1 to 8. In this specification, the divalent aromatic group is a divalent organic group having an aromatic group, and may include an aliphatic group or other substituents in a part of its structure. Furthermore, a divalent aliphatic group is a divalent organic group having an aliphatic group, and may contain other substituents as part of its structure, but does not include an aromatic group.
[0094] In one embodiment of the present invention, the PI resin may contain multiple types of X, which may be the same or different from one another. Examples of X in formula (2) include groups (structures) represented by formulas (60) to (65); groups in which hydrogen atoms in the groups represented by formulas (60) to (65) are substituted with methyl, ethyl, n-propyl, isopropyl, n-butyl, isobutyl, sec-butyl, tert-butyl, fluoro, chloro, or trifluoromethyl groups.
[0095] [ka] [In formula (60) and formula (61), R a and R b each independently represents a halogen atom, or an alkyl group, an alkoxy group, an aryl group, or an aryloxy group which may have a halogen atom; R a and R b may be substituted with a halogen atom, W each independently represents a single bond, -O-, -CH2-, -CH2-CH2-, -CH(CH3)-, -C(CH3)2-, -C(CF3)2-, -COO-, -OOC-, -SO-, -SO2-, -S-, -CO-, -N(R c )- or -CONH-, R c represents a monovalent hydrocarbon group having 1 to 12 carbon atoms which may be substituted with a hydrogen atom or a halogen atom, t' represents an integer of 0 to 4, u represents an integer of 0 to 4, and n represents an integer of 0 to 4. In formula (62), ring A represents a cycloalkane ring having 3 to 8 carbon atoms. R d represents an alkyl group having 1 to 20 carbon atoms, r represents an integer of 0 or more and (the number of carbon atoms in ring A - 2) or less; S1 and S2 each independently represent an integer of 0 to 20; In formulas (60) to (65), * represents a bond.
[0096] Other examples of X in formula (2) include divalent acyclic aliphatic groups such as linear or branched alkylene groups such as ethylene, trimethylene, tetramethylene, pentamethylene, hexamethylene, propylene, 1,2-butanediyl, 1,3-butanediyl, 1,12-dodecanediyl, 2-methyl-1,2-propanediyl, and 2-methyl-1,3-propanediyl. The hydrogen atoms in the divalent acyclic aliphatic groups may be substituted with halogen atoms, and the carbon atoms may be substituted with heteroatoms such as oxygen and nitrogen atoms.
[0097] Among these, from the viewpoint of improving the pin puncture strength and dielectric properties of the laminated film, the PI resin in the present invention preferably contains, as X in formula (2), a structure represented by formula (60) or formula (61), and more preferably contains a structure represented by formula (60).
[0098] In formula (60) and formula (61), the bonds of each benzene ring or each cyclohexane ring may be bonded at any of the ortho-, meta-, or para-positions, or the α-, β-, or γ-positions, based on -W- or the single bond connecting each benzene ring or each cyclohexane ring, and from the viewpoint of improving the pin puncture strength and dielectric properties of the laminated film, they can be bonded preferably at the meta- or para-positions, or the β- or γ-positions, more preferably at the para- or γ-positions. When the amino group directly bonded to the benzene ring and the divalent linking group -W- are at the meta-positions, the flexibility of the polyimide molecular chain tends to be improved.
[0099] In formula (60) and formula (61), R a and R b are each independently preferably a halogen atom, or an alkyl group, alkoxy group or aryl group which may have a halogen atom, more preferably a halogen atom, an alkyl group having 1 to 6 carbon atoms, an alkoxy group having 1 to 6 carbon atoms, or an aryl group having 6 to 12 carbon atoms. Examples of the alkyl group having 1 to 6 carbon atoms, the alkoxy group having 1 to 6 carbon atoms, and the aryl group having 6 to 12 carbon atoms include those exemplified above. a and R bThe hydrogen atoms contained in R may be substituted, independently of one another, with a halogen atom, and examples of the halogen atom include a fluorine atom, a chlorine atom, a bromine atom, and an iodine atom. a and R b are preferably, independently of each other, an alkyl group having 1 to 6 carbon atoms or a fluorinated alkyl group having 1 to 6 carbon atoms, and from the viewpoint of adhesion to metal foil and the like, are more preferably a non-fluorine-containing alkyl group having 1 to 6 carbon atoms, further preferably a non-fluorine-containing alkyl group having 1 to 3 carbon atoms, and particularly preferably a methyl group.
[0100] In the formula (60) and the formula (61), t′ and u are each preferably an integer of 0 to 2, and more preferably 0 or 1, independently of each other.
[0101] In formula (60) and formula (61), each W is, independently of the other, preferably a single bond, -O-, -CH2-, -C(CH3)2-, -C(CF3)2-, -SO2-, -S-, -COO-, -OOC- or -CO-, more preferably a single bond, -O-, -CH2-, -C(CH3)2-, -C(CF3)2-, -COO-, -OOC- or -CO-, even more preferably a single bond, -O-, -CH2- or -C(CH3)2-, and particularly preferably -O- or -C(CH3)2-.
[0102] In the formula (60) and the formula (61), n is preferably an integer of 0 to 3, more preferably 1 to 3. When n is 2 or more, a plurality of W, R a and t' may be the same or different, and the positions of the bonds of each benzene ring relative to -W- may be the same or different.
[0103] When the PI resin of the present invention contains two or more structures represented by either of the formula (60) and the formula (61) as X in the formula (2), W, n, and R in one of the formulas (60) and (61) a , R b , t' and u are each independently W, n, R in the other formula (60) and formula (61).a , R b , t' and u may be the same or different.
[0104] In formula (62), examples of the cycloalkane ring having 3 to 8 carbon atoms represented by ring A include a cyclopropane ring, a cyclobutane ring, a cyclopentane ring, a cyclohexane ring, a cycloheptane ring, and a cyclooctane ring, and preferably a cycloalkane ring having 4 to 6 carbon atoms. In ring A, the bonds may be adjacent to each other or may not be adjacent to each other. For example, when ring A is a cyclohexane ring, the two bonds may be in an α-position, β-position, or γ-position relationship, and preferably in a β-position or γ-position relationship.
[0105] R in equation (62) d is preferably an alkyl group having 1 to 10 carbon atoms. In formula (62), r is preferably 0 or more and preferably 4 or less. S1 and S2 in formula (62) are each independently preferably 0 or more, more preferably 2 or more, and preferably 15 or less.
[0106] Specific examples of the structures represented by formulae (60) to (62) include structures represented by formulae (71) to (92). In these formulae, * represents a bond.
[0107] [ka]
[0108] In one embodiment of the present invention, when the PI resin constituting the PI resin-containing layer contains at least one diamine-derived structural unit represented by formula (60) and formula (61) as X in formula (2), the ratio of the diamine-derived structural unit represented by formula (60) and formula (61) in formula (2) is preferably 30 mol% or more, more preferably 50 mol% or more or more than 50 mol%, even more preferably 70 mol% or more, particularly preferably 90 mol% or more, and preferably 100 mol% or less, based on the total amount of structural unit (B). When the ratio of the diamine-derived structural unit represented by formula (60) and formula (61) in formula (2) is within the above range, it becomes easier to control the parameter X and the thickness of the intermediate region in the laminated film to a desired range, and the pin puncture strength and dielectric properties of the laminated film can be improved. In addition, the CTE of the laminated film tends to decrease, and improvement in the dimensional stability of the laminated film can be expected.
[0109] (Structural unit (B1)) In one embodiment of the present invention, at least one of the layers (PI-1) and (PI-2), or at least one of the layers (PI-1) to (PI-3) contains a diamine-derived structural unit (B), and the structural unit (B) is represented by the formula (B1): [ka] [In formula (B1), R b1 each independently represents a halogen atom, or an alkyl group, an alkoxy group, an aryl group, or an aryloxy group which may have a halogen atom; W each independently represents -O-, -CH2-, -CH2-CH2-, -CH(CH3)-, -C(CH3)2-, -C(CF3)2-, -COO-, -OOC-, -SO-, -SO2-, -S-, -CO-, -N(R c a divalent linking group selected from the group consisting of -CONH- and -CONH-, or a single bond (wherein m is 2 or more and at least one W is the divalent linking group); R c represents a monovalent hydrocarbon group having 1 to 12 carbon atoms which may be substituted with a hydrogen atom or a halogen atom, m represents an integer of 1 to 4; and q each independently represents an integer of 0 to 4. It is preferable that the copolymer contains a diamine-derived structural unit (B1) represented by the following formula (hereinafter, sometimes simply referred to as the structural unit (B1)).
[0110] When the PI resin contains the structural unit (B1) as the structural unit (B), it becomes easier to control the parameter X and the thickness of the intermediate region in the laminate film to a desired range, and the pin puncture strength and dielectric properties can be improved. In addition, the CTE can be reduced, which is expected to improve the dimensional stability of the laminate film and also contribute to improving the adhesion to the metal foil. Furthermore, since the pin puncture strength and dielectric properties of the laminate film obtained can be improved even at a relatively low imidization temperature (e.g., 360°C or lower), even if a laminate sheet is produced by thermally imidizing the PI resin precursor coating film in a laminate configuration with a metal foil (e.g., copper foil), deterioration of the metal foil surface can be suppressed, and a laminate sheet having high pin puncture strength and excellent high-frequency properties can be obtained.
[0111] R in formula (B1) b1 As the above, R in the formula (60) a and R b In formula (B1), q is preferably, independently of each other, an integer of 0 to 2, more preferably 0 or 1. In formula (B1), m is preferably, from the viewpoint of improving the pin puncture strength, dielectric properties, CTE, etc. of the laminated film, an integer of 1 to 3, more preferably 2 or 3. In formula (b2), a plurality of W, R b2 and q may be the same or different, and the position of -W- with respect to -NH2 of each benzene ring may be the same or different.
[0112] In formula (B1), -W- may be bonded independently to any of the ortho, meta, or para positions, or the α, β, or γ positions, and preferably to the meta or para positions, or the β or γ positions, and more preferably to the para or γ positions, based on -NH2 of each benzene ring. When m is 2 or more, in the benzene ring to which two Ws are bonded, the bonding positions of the two Ws may be in an ortho, meta, or para relationship, or in an α, β, or γ relationship, and preferably in a meta or para relationship, or in a β or γ relationship.
[0113] Specific examples of the structure represented by formula (B1) include structures represented by formulas (B1-1) to (B1-6). [ka] R in formula (B1-1) to formula (B1-6) b1 and q is R in formula (B1). b1 and q are defined the same as W 1 ~W 6 are each independently -O-, -CH2-, -CH2-CH2-, -CH(CH3)-, -C(CH3)2-, -C(CF3)2-, -COO-, -OOC-, -SO-, -SO2-, -S-, -CO-, -N(R c R represents a divalent linking group selected from the group consisting of -CONH- and -CONH-; c represents a monovalent hydrocarbon group having 1 to 12 carbon atoms which may be substituted with a hydrogen atom or a halogen atom. In addition, in formula (B1-4), a compound which overlaps with formula (B1-3) is treated as a compound of formula (B1-3).
[0114] R in formula (B1-1) to formula (B1-6) b1 and q is R in formula (B1). b1 The same embodiments as those exemplified as and q are exemplified, and the preferred embodiments are also the same.
[0115] W in formulas (B1-1) to (B1-6) 1 ~W6 are preferably, independently of each other, -O-, -CH2-, -CH2-CH2-, -CH(CH3)-, -C(CH3)2-, -C(CF3)2-, -COO-, -OOC-, -SO2-, -S-, -CO- or -CONH-. 1 is preferably -O-, -CH2-, -C(CH3)2-, -SO2-, -S- or -CO-. 2 , W 4 and W 6 Each of W in formula (B1-3) is preferably —O—. 3 is preferably -O-, -CH2-, -C(CH3)2-, -SO2-, -CO- or -CONH-, and W in formula (B1-5) 5 is preferably -C(CH3)2-, -O-, -SO2- or -CO-.
[0116] In one embodiment of the present invention, at least one of the layers (PI-1) and (PI-2) in the laminate film of the present invention, or at least one of the layers (PI-1) to (PI-3) preferably contains, as the structural unit (B), a structural unit derived from a diamine in which m in formula (B1) is 1 or 2, such as the structural unit (B1-1) and / or the structural unit (B1-2). As a structural unit derived from a diamine in which m is 2, for example, the structural unit (B1-2) is preferably contained. When such a structural unit is contained, it becomes easier to control the parameter X and the thickness of the intermediate region in the laminate film to a desired range, and the pin puncture strength and dielectric properties can be improved. In addition, the CTE of the laminate film tends to decrease, and the dimensional stability of the laminate film can be expected to be improved. Furthermore, the inclusion of these structural units can also contribute to improving the adhesion between the laminate film and the metal foil.
[0117] In another embodiment of the present invention, at least one of the layers (PI-1) and (PI-2) in the laminate film of the present invention, or at least one of the layers (PI-1) to (PI-3), preferably contains a diamine-derived structural unit in which m is 3 or 4, such as the structural unit (B1-3) to the structural unit (B1-6), as the structural unit (B), and more preferably contains a diamine-derived structural unit in which m is 3. As the diamine-derived structural unit in which m is 3, it is preferable to contain, for example, the structural unit (B1-5). When such a structural unit is contained, it becomes easier to control the parameter X and the thickness of the intermediate region in the laminate film to a desired range, and the pin puncture strength and dielectric properties can be improved. In addition, the CTE of the laminate film tends to decrease, and the dimensional stability of the laminate film can be expected to be improved. Furthermore, the inclusion of these structural units can also contribute to improving the adhesion between the laminate film and the metal foil.
[0118] In one embodiment of the present invention, the structural unit (B1) is preferably the structural unit (B1-2), and the structural unit (B1-2) is more preferably a structural unit represented by formula (B1-2') and / or formula (B1-2''). [ka] R in formula (B1-2') and formula (B1-2'') b1 , W 2 , and q is R in formula (B1-2). b1 , W 2 , and q are defined the same.
[0119] In one embodiment of the present invention, the constitutional unit represented by formula (B1-2') or formula (B1-2'') is preferably a constitutional unit represented by formula (B1-2'a) or formula (B1-2''a), respectively. [ka] When the structural unit (B) contains the above structural unit, it becomes easier to control the parameter X and the thickness of the intermediate region in the laminated film to a desired range, and the pin puncture strength and dielectric properties can be improved. In addition, the CTE of the laminated film tends to decrease, and the dimensional stability of the laminated film can be improved. Furthermore, the inclusion of these structural units can also contribute to improving the adhesion between the laminated film and the metal foil.
[0120] In another embodiment of the present invention, the structural unit (B1) is preferably the structural unit (B1-5), and the structural unit (B1-5) is more preferably a structural unit represented by formula (B1-5a). [ka] When the structural unit (B) contains the above structural unit, it becomes easier to control the parameter X and the thickness of the intermediate region in the laminate film within the desired range, which is advantageous in terms of improving the pin puncture strength and dielectric properties of the laminate film and reducing the CTE, etc.
[0121] In one embodiment of the present invention, when the PI resin constituting the PI resin-containing layer contains the structural unit (B1), the content thereof is preferably 3 mol% or more, more preferably 5 mol% or more, even more preferably 7 mol% or more, and even more preferably 10 mol% or more, for example, 20 mol% or more, 30 mol% or more, or 40 mol% or more, based on the total amount of the structural unit (B). When the content of the structural unit (B1) is equal to or more than the above lower limit, it becomes easier to control the parameter X and the thickness of the intermediate region in the laminated film within a desired range, which is advantageous in improving the puncture strength and dielectric properties of the laminated film, reducing the CTE, and the like. In addition, since the adhesion to the metal foil tends to increase as the total amount of the structural unit (B1) increases, from this viewpoint, the content of the structural unit (B1) may be, for example, 50 mol% or more, 60 mol% or more, or 70 mol% or more, based on the total amount of the structural unit (B). The content of the structural unit (B1) relative to the total amount of the structural units (B) is preferably no more than 99 mol %, more preferably no more than 95 mol %, and even more preferably no more than 90 mol %.
[0122] <Constituent unit (B2)> In one embodiment of the present invention, the PI resin constituting at least one of the layers (PI-1) and (PI-2) or at least one of the layers (PI-1) to (PI-3) in the laminate film of the present invention contains, as the structural unit (B), a structural unit represented by the formula (B2): [ka] [In formula (B2), R b2 each independently represents a halogen atom, or an alkyl group, an alkoxy group, an aryl group, or an aryloxy group which may have a halogen atom; p represents an integer from 0 to 4. It is preferable that the structural unit (B2) (hereinafter, sometimes simply referred to as structural unit (B2)) derived from a biphenyl skeleton-containing diamine represented by the following formula is contained. When the structural unit (B) contains the structural unit (B2), the PI resin is not too rigid and can have a flexible structure with a certain degree of freedom, so that a branched structure is easily formed by heating during imidization, and the crystallinity tends to increase, so that the parameter X and the thickness of the intermediate region in the laminated film can be easily controlled within a desired range, which is advantageous for improving the pin puncture strength and dielectric properties of the laminated film and reducing the CTE.
[0123] In formula (B2), R b2 R preferably independently represent a halogen atom, or an alkyl group, alkoxy group or aryl group which may have a halogen atom, and more preferably represent a halogen atom, an alkyl group having 1 to 6 carbon atoms, an alkoxy group having 1 to 6 carbon atoms, or an aryl group having 6 to 12 carbon atoms. Examples of the alkyl group having 1 to 6 carbon atoms, the alkoxy group having 1 to 6 carbon atoms, and the aryl group having 6 to 12 carbon atoms include those exemplified above. b2 The hydrogen atoms contained in R may be substituted, independently of one another, with a halogen atom, and examples of the halogen atom include the same as those mentioned above. b2are each independently preferably an alkyl group having 1 to 6 carbon atoms or a fluorinated alkyl group having 1 to 6 carbon atoms, and from the viewpoint of adhesion to metal foil and the like, are more preferably a non-fluorine-containing alkyl group having 1 to 6 carbon atoms, further preferably a non-fluorine-containing alkyl group having 1 to 3 carbon atoms, and particularly preferably a methyl group.
[0124] In formula (B2), p's are each independently preferably an integer of 0 to 2, and more preferably 0 or 1.
[0125] In formula (B2), the -NH2 group bonded to each benzene ring may be bonded at any of the ortho-, meta-, or para-position, or the α-, β-, or γ-position, based on the single bond connecting each benzene ring. From the viewpoint of improving the dielectric properties and pin puncture strength of the laminated film and reducing the CTE, it is preferably bonded to the meta- or para-position, or the β- or γ-position, and more preferably to the para- or γ-position.
[0126] In a preferred embodiment of the present invention, formula (B2) is represented by formula (B2'): [ka] It is preferable that the PI resin constituting at least one PI resin-containing layer contains, as the structural unit (B), a PI resin having a structural unit (B2), particularly a PI resin having a diamine-derived structural unit represented by formula (B2'), so that the PI resin is not too rigid and can have a flexible structure with a certain degree of freedom, and therefore the PI resin is likely to form a branched structure by heating during imidization, and also has a tendency to have high crystallinity, so that the parameter X in the laminated film and the thickness of the intermediate region can be easily controlled within a desired range, which is advantageous in improving the pin puncture strength and dielectric properties of the laminated film, reducing the CTE, and the like. Furthermore, since the above effect can be obtained even at a relatively low imidization temperature (for example, 360°C or lower), even if a laminated sheet is produced by thermally imidizing a PI resin precursor coating film in a laminated configuration with a metal foil (for example, copper foil), deterioration of the metal foil surface can be suppressed, and a laminated sheet having high pin puncture strength and excellent high-frequency characteristics can be obtained.
[0127] In one embodiment of the present invention, when the PI resin contains the structural unit (B2), the content thereof is preferably 1 mol% or more, more preferably 5 mol% or more, and even more preferably 10 mol% or more, based on the total amount of the structural unit (B), and may be, for example, 20 mol% or more, 30 mol% or more, more than 30 mol%, 40 mol% or more, or 50 mol% or more. When the content of the structural unit (B2) is equal to or more than the above lower limit, it becomes easier to control the parameter X and the thickness of the intermediate region in the laminated film within a desired range, which is advantageous in improving the puncture strength and dielectric properties of the laminated film, reducing the CTE, and the like. In addition, the structural unit (B1) is preferably 99 mol% or less, more preferably 95 mol% or less, and even more preferably 92 mol% or less, based on the total amount of the structural unit (B), and may be, for example, 90 mol% or less, 80 mol% or less, 70 mol% or less, or 60 mol% or less.
[0128] In one embodiment of the present invention, when the PI resin constituting the PI resin-containing layer contains the structural unit (B1) and the structural unit (B2), the total content thereof is preferably 30 mol% or more, more preferably 40 mol% or more, even more preferably 60 mol% or more, particularly preferably 70 mol% or more, particularly more preferably 80 mol% or more, particularly more preferably 90 mol% or more, particularly still more preferably 95 mol% or more, and preferably 100 mol% or less, based on the total amount of the structural unit (B). When the total content of the structural unit (B1) and the structural unit (B2) is equal to or more than the lower limit, the above-mentioned effects of the present invention that are expected from the PI resin having the structural unit (B1) and the structural unit (B2) are easily obtained, and the effects can be further enhanced.
[0129] Furthermore, in one embodiment of the present invention, when the PI resin contains the structural unit (B1) and the structural unit (B2), the content ratio (molar ratio, (B1):(B2)) is preferably 99:1 to 1:99, more preferably 95:5 to 5:95, and even more preferably 92:8 to 8:92, and may be, for example, 92:8 to 20:80, or 90:10 to 60:40. When the content ratio of the structural unit (B1) to the structural unit (B2) is within the above range, the above-mentioned effects of the present invention that are expected from the PI resin having the structural unit (B1) and the structural unit (B2) are more easily achieved, and these effects can be further enhanced.
[0130] In one embodiment of the present invention, the PI resin-containing layer constituting the laminate film preferably contains one or more of the following components. In the layer (PI-1) and the layer (PI-2), or in the layers (PI-1) to (PI-3) in the laminate film, the PI resin contains at least one of the structural unit (B1) and the structural unit (B2); The PI resin in layers (PI-1) and (PI-2), or layers (PI-1) to (PI-3) in the laminate film contains the structural unit (B1); In the layer (PI-1) and the layer (PI-2), or in the layers (PI-1) to (PI-3) in the laminate film, the PI resin contains a structural unit (B1) and a structural unit (B2). In at least one PI resin-containing layer in the laminate film, the PI resin contains a structural unit (B1) and a structural unit (B2);
[0131] (Structural unit (B3)) In one embodiment of the present invention, the structural unit (B) may contain a structural unit (B3) derived from a diamine other than the structural unit (B1) and the structural unit (B2) (hereinafter, may be abbreviated simply as the structural unit (B3)). Examples of the structural unit (B3) include a structural unit derived from a diamine in which m in the formula (B1) is 0, and a structural unit derived from a diamine in which X in the formula (2) is represented by the formulas (61) to (64), and among these, a structural unit derived from a diamine in which X in the formula (2) is represented by the formula (74) (structural unit derived from p-phenylenediamine) is preferred. In this specification, "structural unit (B3) derived from a diamine other than the structural unit (B1) and the structural unit (B2)" means a structural unit derived from a diamine different from both the structural unit (B1) and the structural unit (B2).
[0132] In one embodiment of the present invention, when the structural unit (B) contains the structural unit (B3), the content of the structural unit (B3) is preferably 25 mol % or less, more preferably 20 mol % or less, and even more preferably 10 mol % or less, relative to the total amount of the structural unit (B), and is usually 0.01 mol % or more.
[0133] In one embodiment of the present invention, the polyimide resin contained in the PI resin-containing layer (PI-1) may be the same as or different from the PI resin contained in the PI resin-containing layer (PI-2). From the viewpoints of improving the pin puncture strength and dielectric properties of the laminated film, reducing the CTE, etc., it is preferable that the PI resins contained in each layer are different. The different resins include not only those having different types of constituent units, but also those having the same type of constituent units but different contents (or ratios).
[0134] In one embodiment of the present invention, the PI resin-containing layer (PI-1) and the PI resin-containing layer (PI-2) each preferably contain a polyimide resin having at least two kinds of tetracarboxylic anhydride-derived structural units (A). In such an embodiment, the pin puncture strength and dielectric properties of the laminated film are easily improved, and the CTE is easily reduced.
[0135] In one embodiment of the present invention, the PI resin in the PI resin-containing layer (PI-1) and the PI resin-containing layer (PI-2) or the PI resin-containing layers (PI-1) to (PI-3), preferably the mPI layer and the TPI layer, contains the structural unit (A1) and / or the structural unit (A2) as the structural unit (A) and the structural unit (B1) as the structural unit (B), preferably the structural unit (B1) and the structural unit (B2).
[0136] In a preferred embodiment of the present invention, the PI resin contained in the PI resin-containing layer (PI-1) constituting the laminate film, preferably the mPI layer, contains, as the structural unit (A), at least two structural units selected from the structural unit (A1), the structural unit (A2), and the structural unit (A3) (preferably the structural unit (A1) and the structural unit (A2) and / or the structural unit (A3)). The PI resin contained in the PI resin-containing layer (PI-2), preferably the TPI layer, contains, as the structural unit (A), the structural unit (A1) and the structural unit (A2). Furthermore, the PI resins constituting the PI resin-containing layer (PI-1) and the PI resin-containing layer (PI-2), preferably the mPI layer and the TPI layer, each contain, as the structural unit (B), the structural unit (B1), preferably the structural unit (B1) and the structural unit (B2).
[0137] In a preferred embodiment of the present invention, when the laminate film (L) further comprises a PI resin-containing layer (PI-3), the PI resin contained in the PI resin-containing layer (PI-1), preferably the mPI layer, contains, as the structural unit (A), at least two structural units selected from the structural unit (A1), the structural unit (A2), and the structural unit (A3) (preferably the structural unit (A1) and the structural unit (A2) and / or the structural unit (A3)). The PI resin contained in the PI resin-containing layer (PI-2) and the PI resin-containing layer (PI-3), preferably the TPI layer, contains, as the structural unit (A), the structural unit (A1) and the structural unit (A2). Furthermore, the PI resin contained in the PI resin-containing layers (PI-1) to (PI-3), preferably the mPI layer and the TPI layer, each contains, as the structural unit (B1), preferably the structural unit (B1) and the structural unit (B2).
[0138] When the mPI layer, the TPI layer, the layer (PI-1), the layer (PI-2) and optionally the layer (PI-3) are each composed of a combination of the above-mentioned structural units, the PI resin of each layer is not too rigid and can have a flexible structure with a certain degree of freedom, so that the PI resin is likely to form a branched structure by heating during imidization and has a tendency to increase crystallinity. Furthermore, the interaction between two adjacent layers can be increased. Therefore, it becomes easier to control the parameter X and the thickness of the intermediate region in the laminate film composed of these layers to a desired range, and the above-mentioned effects of the present invention expected from the PI resin having each structural unit can be easily obtained, and the effects can be further enhanced.
[0139] <Layer (PI-1)> In one embodiment of the present invention, the PI resin constituting the layer (PI-1) contains, as the structural unit (A), the structural unit (A1) and / or the structural unit (A2), preferably at least two structural units selected from the structural unit (A1), the structural unit (A2) and the structural unit (A3), more preferably the structural unit (A1) and the structural unit (A2) and / or the structural unit (A3). When the layer (PI-1) contains these structural units, the content of the structural unit (A1) is preferably 20 mol% or more, more preferably 30 mol% or more, even more preferably 35 mol% or more, particularly preferably 40 mol% or more, and is preferably 80 mol% or less, more preferably 75 mol% or less, even more preferably 70 mol% or less, particularly preferably 65 mol% or less, based on the total amount of the structural units (A). The content of the structural unit (A2) is preferably 20 mol% or more, more preferably 30 mol% or more, even more preferably 35 mol% or more, particularly preferably 40 mol% or more, and is preferably 80 mol% or less, more preferably 75 mol% or less, even more preferably 70 mol% or less, and particularly preferably 65 mol% or less, based on the total amount of the structural unit (A). The content of the structural unit (A3) is preferably 3 mol% or more, more preferably 5 mol% or more, even more preferably 7 mol% or more, and even more preferably 10 mol% or more, based on the total amount of the structural unit (A). For example, it may be 20 mol% or more, 30 mol% or more, or 40 mol% or more, and is preferably 75 mol% or less, more preferably 70 mol% or less, even more preferably 65 mol% or less, and particularly preferably 60 mol% or less. In another embodiment, the content of the structural unit (A3) is preferably 45 mol% or less, more preferably 35 mol% or less, even more preferably 25 mol% or less, still more preferably 15 mol% or less, particularly preferably 5 mol% or less, and especially preferably 1 mol% or less, and the lower limit may be 0 mol%. When the contents of the structural units (A1), (A2) and / or (A3) are within the above ranges, the PI resin is not too rigid and can have a flexible structure with a certain degree of freedom, which tends to facilitate the formation of a branched structure by heating during imidization and to increase crystallinity, making it easier to control the parameter X and the thickness of the intermediate region in the laminated film within the desired range, and making it possible to obtain a laminated film with excellent pin puncture strength, dielectric properties and thermal properties.
[0140] On the other hand, in another embodiment of the present invention, the content of the structural unit (A2) in the PI resin constituting the layer (PI-1) is preferably less than 30 mol%, more preferably 25 mol% or less, even more preferably 20 mol% or less, and particularly preferably 10 mol% or less, based on the total amount of the structural unit (A). In one embodiment of the present invention, the layer (PI-1) may be substantially free of the structural unit (A2), and the lower limit of the content of the structural unit (A2) may be 0 mol%.
[0141] In one embodiment of the present invention, the PI resin constituting the layer (PI-1) preferably contains the structural unit (B1) as the structural unit (B). The structural unit (B1) preferably contains the structural unit (B1-2) and the structural unit (B1-5), more preferably contains the structural unit (B1-2), and even more preferably contains (B1-2''). The content of the structural unit (B1) in the PI resin constituting the layer (PI-1) is preferably 3 mol% or more, more preferably 5 mol% or more, even more preferably 7 mol% or more, and even more preferably 10 mol% or more, relative to the total amount of the structural units (B), and may be, for example, 20 mol% or more, 30 mol% or more, or 40 mol% or more, and is preferably 80 mol% or less, more preferably 75 mol% or less, even more preferably 70 mol% or less, and particularly preferably 65 mol% or less. The PI resin constituting the layer (PI-1) preferably further contains a structural unit (B2) as the structural unit (B). The content thereof, based on the total amount of the structural units (B), is preferably 10 mol % or more, more preferably 20 mol % or more, even more preferably 30 mol % or more or more than 30 mol %, even more preferably 35 mol % or more, and particularly preferably 40 mol % or more, and is preferably 99 mol % or less, more preferably 95 mol % or less, and even more preferably 92 mol % or less, and may be, for example, 90 mol % or less, 80 mol % or less, 70 mol % or less, or 60 mol % or less. When the content of the structural unit (B1) and / or the structural unit (B2) is within the above range, the PI resin is not too rigid and can have a flexible structure with a certain degree of freedom, so that a branched structure is easily formed by heating during imidization, and the crystallinity tends to be increased. This makes it possible to improve the pin puncture strength of the layer (PI-1) and reduce Df, and further effectively reduce the CTE, so that a laminate film with excellent pin puncture strength, dielectric properties, and thermal properties can be obtained.
[0142] <Layer (PI-2) and Layer (PI-3)> In one embodiment of the present invention, the laminated film includes a layer (PI-2) and may further include a layer (PI-3). The PI resin constituting the layer (PI-2) and the layer (PI-3) each includes the structural unit (A1) as the structural unit (A), and preferably includes the structural unit (A1) and the structural unit (A2). When these structural units are included, the content of the structural unit (A1) is preferably 10 mol% or more, more preferably 15 mol% or more, and even more preferably 20 mol% or more, and preferably 80 mol% or less, more preferably 70 mol% or less, and even more preferably 60 mol% or less, based on the total amount of the structural units (A). The content of the structural unit (A2) is preferably 20 mol% or more, more preferably 30 mol% or more, more preferably 40 mol% or more, even more preferably 50 mol% or more, particularly preferably 60 mol% or more, and preferably 90 mol% or less, more preferably 85 mol% or less, even more preferably 80 mol% or less, and even more preferably 75 mol% or less, based on the total amount of the structural units (A). When the content of the structural unit (A1) and / or the structural unit (A2) is within the above range, the PI resin is not too rigid and can have a flexible structure with a certain degree of freedom, so that the PI resin is likely to form a branched structure by heating during imidization and also tends to have high crystallinity. This makes it possible to improve the puncture strength of the layer (PI-2) and the layer (PI-3) and reduce Df, and further effectively reduce CTE, so that a laminate film having excellent puncture strength, dielectric properties, and thermal properties can be obtained. In addition, the effect of improving adhesion to metal foil can be expected.
[0143] In one embodiment of the present invention, the content of the structural unit (A3) in the PI resin constituting the layers (PI-2) and (PI-3) is preferably 10 mol% or less, more preferably 8 mol% or less, even more preferably 5 mol% or less, and particularly preferably 3 mol% or less, based on the total amount of the structural unit (A). In one embodiment of the present invention, the layers (PI-2) and (PI-3) may be substantially free of the structural unit (A3), and the lower limit of the content of the structural unit (A3) may be 0 mol%.
[0144] In one embodiment of the present invention, the PI resin constituting the layer (PI-2) and the layer (PI-3) preferably contains the structural unit (B1) as the structural unit (B). The structural unit (B1) preferably contains the structural unit (B1-2), and more preferably contains the structural unit (B1-2') that enhances the flexibility of the PI resin. The content of the structural unit (B1) in the PI resin constituting these layers is preferably 20 mol% or more, more preferably 30 mol% or more, even more preferably 35 mol% or more, particularly preferably 40 mol% or more, and is preferably 99 mol% or less, more preferably 95 mol% or less, and even more preferably 92 mol% or less, for example, 90 mol% or less, 80 mol% or less, 70 mol% or less, or 60 mol% or less, based on the total amount of the structural unit (B). In addition, it is preferable that the structural unit (B) further contains a structural unit (B2), and the content thereof is preferably 1 mol% or more, more preferably 5 mol% or more, and even more preferably 10 mol% or more. For example, it may be 20 mol% or more, 30 mol% or more, more than 30 mol%, or 40 mol% or more, and is preferably 80 mol% or less, more preferably 70 mol% or less, even more preferably 65 mol% or less, and particularly preferably 60 mol% or less. In the PI resin constituting the layers (PI-2) and (PI-3), when the content of the structural unit (B1) and / or the structural unit (B2) is within the above range, the PI resin is not too rigid and can have a flexible structure with a certain degree of freedom, so that the PI resin is likely to form a branched structure by heating during imidization and tends to increase crystallinity. This makes it possible to improve the puncture strength of the layers (PI-2) and (PI-3) and reduce Df, and also effectively reduce CTE, so that a laminate film with even better puncture strength, dielectric properties, and thermal properties can be obtained. In addition, an effect of improving adhesion to metal foil can be expected.
[0145] The various physical properties (e.g., molecular weight, glass transition temperature) of the PI resin containing the structural unit (A) and / or the structural unit (B) may be appropriately determined based on, for example, the following suitable ranges depending on the role and application of each PI resin-containing layer in the laminate film.
[0146] In one embodiment of the present invention, the PI resin constituting each PI resin-containing layer may contain a halogen atom, preferably a fluorine atom, which can be introduced, for example, by the above-mentioned halogen atom-containing substituent. When the PI resin contains a fluorine atom, the relative dielectric constant of the resulting PI resin-containing layer is easily reduced, leading to improved dielectric properties of the laminated film. Examples of fluorine-containing substituents that are preferable for introducing fluorine atoms into the PI resin include a fluoro group and a trifluoromethyl group. In another embodiment of the present invention, the PI resin preferably does not contain fluorine atoms from the viewpoint of increasing the adhesiveness of the resulting PI resin-containing layer to the metal foil. For this reason, for example, the PI resin constituting the PI resin-containing layer in contact with the metal foil, preferably the TPI layer, particularly the layer (PI-2) and layer (PI-3) in the laminate film, preferably does not contain fluorine atoms. In addition, when the PI resin contains fluorine, it tends to weaken the interaction between molecular chains, so when the PI resin does not contain fluorine atoms, the Df of the PI film tends to be reduced.
[0147] When the PI resin contains halogen atoms, the content of halogen atoms, particularly fluorine atoms, in the PI resin is preferably 0.1 to 35 mass%, more preferably 0.1 to 30 mass%, further preferably 0.1 to 20 mass%, and particularly preferably 0.1 to 10 mass%, based on the mass of the PI resin. If the content of halogen atoms is equal to or greater than the above lower limit, the heat resistance and dielectric properties of the resulting PI resin-containing layer are likely to be improved, leading to improved dielectric properties and thermal properties of the laminated film. If the content of halogen atoms is equal to or less than the above upper limit, it is advantageous in terms of cost, the CTE is likely to be reduced, and the synthesis of the PI resin is easy.
[0148] In one embodiment of the present invention, the imidization rate of the PI resin is preferably 90% or more, more preferably 93% or more, and even more preferably 95% or more, and is usually 100% or less. From the viewpoint of improving the pin puncture strength, dielectric properties, and thermal properties of the laminated film, it is preferable that the imidization rate is equal to or higher than the above lower limit. The imidization rate indicates the ratio of the molar amount of imide bonds in the PI resin to twice the molar amount of the constituent units derived from the tetracarboxylic acid compound in the PI resin. In addition, when the PI resin contains a tricarboxylic acid compound, it indicates the ratio of the molar amount of imide bonds in the PI resin to the sum of twice the molar amount of the constituent units derived from the tetracarboxylic acid compound in the PI resin and the molar amount of the constituent units derived from the tricarboxylic acid compound. The imidization rate can be determined by IR method, NMR method, etc.
[0149] In one embodiment of the present invention, the weight average molecular weight (Mw) of the PI resin in terms of polystyrene is preferably 5000 or more, more preferably 10000 or more, even more preferably 15000 or more, and particularly preferably 20000 or more, from the viewpoint of increasing the pin puncture strength. Also, from the viewpoint of ease of production of the varnish and film formability, it is preferably 1200000 or less, more preferably 1000000 or less, even more preferably 800000 or less, and particularly preferably 700000 or less. For example, the Mw of the mPI layer, particularly the layer (PI-1) in the laminate film, is preferably 5000 to 800000, more preferably 10000 to 700000. Also, the Mw of the TPI layer, particularly the layer (PI-2) and layer (PI-3) in the laminate film, is preferably 10000 to 1000000, more preferably 20000 to 900000, respectively.
[0150] In one embodiment of the present invention, the ratio (Mw / Mn) of the weight average molecular weight (Mw) to the number average molecular weight (Mn) of the PI resin of the present invention is preferably 1.1 or more, more preferably 1.3 or more, even more preferably 1.5 or more, particularly preferably 1.7 or more, and is preferably 15 or less, more preferably 12 or less, even more preferably 11 or less, particularly preferably 10 or less, from the viewpoint of pin puncture strength and adhesion to metal foil. For example, the Mw / Mn of the mPI layer, particularly the layer (PI-1) in the laminate film, is preferably 1.1 to 15, more preferably 1.5 to 10. The Mw / Mn of the TPI layer, particularly the layer (PI-2) and layer (PI-3) in the laminate film, is preferably 1.1 to 15, more preferably 1.5 to 10. The Mw and Mn can be determined by gel permeation chromatography (hereinafter sometimes referred to as GPC) measurement and standard polystyrene conversion.
[0151] In one embodiment of the present invention, the Tg of the PI resin is preferably 350° C. or less, more preferably 330° C. or less, even more preferably 310° C. or less, and particularly preferably 300° C. or less, from the viewpoint of improving the puncture strength of the laminated film and reducing Df and improving thermal properties. The Tg of the PI resin is preferably 200° C. or more, more preferably 205° C. or more, even more preferably 210° C. or more, and particularly preferably 220° C. or more, from the viewpoint of improving the puncture strength of the laminated film, reducing Df, and improving thermal properties. When the PI resin-containing layer includes an mPI layer and a TPI layer, the Tg of the PI resin constituting the mPI layer is preferably 350° C. or less, more preferably 330° C. or less, even more preferably 310° C. or less, and particularly preferably 295° C. or less, and preferably 220° C. or more, more preferably 230° C. or more, even more preferably 250° C. or more, even more preferably 260° C. or more, and particularly preferably 270° C. or more. When the Tg of the PI resin constituting the mPI layer is within the above range, the pin puncture strength of the laminated film can be increased, and the dielectric properties and thermal properties can be improved. The Tg of the PI resin constituting the TPI layer is preferably 310°C or less, more preferably 300°C or less, even more preferably 290°C or less, even more preferably 270°C or less, particularly preferably 250°C or less, and preferably 200°C or more, more preferably 210°C or more, even more preferably 220°C or more, particularly preferably 230°C or more. When the Tg of the PI resin constituting the TPI layer is within the above range, the pin puncture strength of the laminated film can be increased, and in addition to reducing Df and improving thermal properties, the adhesion to the metal foil can be improved. The Tg of the PI resin can be measured by dynamic viscoelasticity measurement. For example, it can be calculated based on the peak of a tan δ curve, which is the ratio of the storage modulus (E') to the loss modulus (E") obtained using a dynamic viscoelasticity measurement device.
[0152] In one embodiment including an mPI layer and a TPI layer as the PI resin-containing layer, when the Tg of the PI resin constituting the mPI layer is within the above range, preferably 250 to 330°C, and the Tg of the PI resin constituting the TPI layer is within the above range, preferably 220 to 300°C, each PI resin tends to form a preferred high-order structure with suppressed rotational motion. Therefore, in the case of this embodiment, each PI resin-containing layer can be formed by a PI resin having a high-order structure with maintained orientation, and it is considered that the strength against impact applied in the thickness direction of the PI resin-containing layer is increased, and the puncture strength of the laminated film is improved. In addition, it is estimated that the rotation of the polar group in each PI resin is suppressed, and the loss of electrical energy as thermal motion is reduced, so that a laminated film with a low Df can be obtained by using a PI resin with a Tg within the above range. Furthermore, by using such a PI resin, the pin puncture strength and dielectric properties of the resulting laminate film can be increased even at a low imidization temperature of, for example, 360°C or lower. Therefore, even when a laminate sheet is produced by thermally imidizing a PI resin precursor coating film in a laminate configuration with a metal foil (e.g., copper foil), deterioration of the metal foil surface can be suppressed, and a laminate sheet (CCL) can be obtained that has both high pin puncture strength and excellent high-frequency properties.
[0153] The Tg of the PI resin can be adjusted by appropriately adjusting the types and compositions of the structural units constituting the PI resin, the molecular weight and production method of the PI resin, particularly the imidization conditions, and the like. For example, the Tg can be adjusted to fall within the above-mentioned range by adjusting the Tg within the ranges described as preferred embodiments in this specification.
[0154] <Laminated film manufacturing method> The laminate film of the present invention can be produced, for example, by a method including a step of reacting a tetracarboxylic acid anhydride with a diamine, each of which is appropriately selected depending on the composition of the PI resin constituting each PI resin-containing layer in the laminate film, to obtain a PI resin precursor, and a step of imidizing the obtained PI resin precursor. For example, a method for producing the laminated film of the present invention includes a method in which a solution of the corresponding PI resin precursor is applied to a supporting substrate, pre-dried to obtain a multilayer coating film, and then imidization is performed. Imidization may be performed in a state in which the supporting substrate is peeled off. In one embodiment of the present invention, imidization is performed in a state in which sufficient solvent remains in the entire coating film, or in a state in which the resin layers are well blended with each other, making it easy to adjust the value of (E1r-E1a) / (E2r-E2a) to the range of formula (I) and easy to adjust the thickness of the intermediate region to a desired range. The reason is unclear, but the following reasons are thought to be the following. When the solvent remains in the entire coating film or the resin layers are well blended, the degree of freedom of the resin molecules is high until imidization, so the planar orientation of the resin is moderately reduced, and the degree of elastic deformation in the thickness direction cross section of each PI resin-containing layer obtained tends to increase (other than the elastic deformation component decreases). And, since the degree of disorder of the orientation differs between two or more PI resin-containing layers, preferably between the mPI layer and the TPI layer, the degree of increase in elastic deformation differs between each layer. Here, if the layer (PI-2) is one in which the molecular orientation is moderately disturbed and the degree of increase in elastic deformation is large, the decrease in the denominator (E2r-E2a) corresponding to the layer (PI-2) tends to be larger than the decrease in the numerator (E1r-E1a) corresponding to the layer (PI-1) (the denominator decreases more than the numerator), so the value of (E1r-E1a) / (E2r-E2a) tends to increase, and it is considered that formula (I) is easily satisfied. For example, in a preferred embodiment of the present invention, when a laminate film in which the layer (PI-1) is an mPI layer and the layer (PI-2) is a TPI layer is imidized under the above-mentioned conditions, the TPI layer tends to have a greater degree of elastic deformation than the mPI layer, which is prone to plastic deformation and viscous deformation, so the decrease in the denominator (E2r-E2a) corresponding to the TPI layer tends to be greater than the decrease in the numerator (E1r-E1a) corresponding to the mPI layer (the denominator decreases more), and it is considered that the value of (E1r-E1a) / (E2r-E2a) in formula (I) can increase. In addition, under the above-mentioned conditions, the PI resins constituting each layer tend to mix with each other near the interface of each layer, making it easier to form an intermediate region, which is considered to increase the thickness of the intermediate region. Furthermore, when the thickness relationship between layers (PI-1) and (PI-2) satisfies the above-mentioned relationship, plastic deformation or viscous deformation is more likely to occur in layer (PI-1), making it easier to adjust the value of (E1r-E1a) / (E2r-E2a) within the range of formula (I) and to adjust the thickness of the intermediate region within the desired range.
[0155] In a preferred embodiment of the present invention, the laminated film of the present invention can be produced by a method including, for example, a step of applying a solution of a corresponding PI resin precursor to a supporting substrate and pre-drying the solution to obtain a multilayer coating film (also referred to as a coating and pre-drying step); a step of leaving the obtained multilayer coating film (also referred to as a leaving step); and a step of heating the multilayer coating film to imidize the PI resin (also referred to as an imidization step). The supporting substrate may be peeled off or removed. Since such a production method includes a leaving step, preferably a leaving step at a low temperature described below, it is easy to adjust the parameter X and the thickness of the intermediate region in the obtained laminated film to a desired range.
[0156] (Preparation of PI resin precursor) Examples of the tetracarboxylic acid anhydride used in the synthesis of the PI resin precursor include aromatic tetracarboxylic acid compounds such as aromatic tetracarboxylic acid dianhydrides; and aliphatic tetracarboxylic acid compounds such as aliphatic tetracarboxylic acid dianhydrides. The tetracarboxylic acid compounds may be used alone or in combination of two or more. The tetracarboxylic acid compounds may be dianhydrides or tetracarboxylic acid compound analogues such as acid chloride compounds.
[0157] Examples of the tetracarboxylic acid compound include tetracarboxylic acid anhydrides represented by formula (A1), tetracarboxylic acid anhydrides represented by formula (A2), and tetracarboxylic acid anhydrides represented by formula (A3). Any tetracarboxylic acid compound known in the art can be appropriately selected and used. Examples of such tetracarboxylic acid compounds include pyromellitic anhydride (hereinafter, sometimes referred to as PMDA), 4,4'-(4,4'-isopropylidenediphenoxy)diphthalic anhydride (hereinafter, sometimes referred to as BPADA), 1,4,5,8-naphthalenetetracarboxylic dianhydride, 3,3',4,4'-biphenyltetracarboxylic dianhydride (hereinafter, sometimes referred to as BPDA), 4,4'-(hexafluoroisopropylidene)diphthalic dianhydride (hereinafter, sometimes referred to as 6FDA), 4,4'-oxydiphthalic an ... dianhydride (hereinafter sometimes referred to as ODPA), 2,2',3,3'-, 2,3,3',4'- or 3,3',4,4'-benzophenonetetracarboxylic dianhydride, 2,3',3,4'-biphenyltetracarboxylic dianhydride, 2,2',3,3'-biphenyltetracarboxylic dianhydride, p-phenylenebis(trimellitic acid monoester dianhydride) (hereinafter sometimes referred to as TAHQ), ester of trimellitic anhydride and 2,2',3,3',5,5'-hexamethyl-4,4'-biphenol (hereinafter sometimes referred to as TMPBP) (hereinafter, sometimes referred to as BP-TME), 4,4'-bis(1,3-dioxo-1,3-dihydroisobenzofuran-5-ylcarbonyloxy)biphenyl (hereinafter, sometimes referred to as BP-TME), 2,3',3,4'-diphenyl ether tetracarboxylic acid dianhydride, bis(2,3-dicarboxyphenyl)ether dianhydride, 3,3",4,4"-p-terphenyl tetracarboxylic acid dianhydride, 2,3,3",4"-p-terphenyl tetracarboxylic acid dianhydride, 2,2",3,3"-p-terphenyl tetracarboxylic acid dianhydride, 2,2-bis(2 ,3-dicarboxyphenyl)-propane dianhydride, 2,2-bis(3,4-dicarboxyphenyl)-propane dianhydride, bis(2,3-dicarboxyphenyl)methane dianhydride, bis(3,4-dicarboxyphenyl)methane dianhydride, 1,1-bis(2,3-dicarboxyphenyl)ethane dianhydride, 1,1-bis(3,4-dicarboxyphenyl)ethane dianhydride, 1,2,7,8-, 1,2,6,7-phenanthrene-tetracarboxylic dianhydride, 1,2,9,10-phenanthrene-tetracarboxylic dianhydride, 2,2-bis(3,4-dicarboxyphenyl)tetrafluoropropane dianhydride, 1,2,4,5-cyclohexanetetracarboxylic dianhydride (hereinafter sometimes referred to as HPMDA), 2,3,5,6-cyclohexanetetracarboxylic dianhydride, 2,3,6,7-naphthalenetetracarboxylic dianhydride, 1,2,5,6-naphthalenetetracarboxylic dianhydride, cyclopentane-1,2,3,4-tetracarboxylic dianhydride, 4,4'-bis(2,3-dicarboxyphenoxy)diphenylmethane dianhydride, 1,2, 3,4-Cyclobutanetetracarboxylic dianhydride (hereinafter sometimes referred to as CBDA), norbornane-2-spiro-α'-spiro-2"-norbornane-5,5',6,6'-tetracarboxylic anhydride, p-phenylenebis(trimellitate anhydride), 3,3',4,4'-diphenylsulfonetetracarboxylic dianhydride, 2,3,6,7-anthracenetetracarboxylic dianhydride, 4,8-dimethyl-1,2,3,5,6,7-hexahydronaphthalene-1,2,5,6-tetracarboxylic dianhydride , 2,6-dichloronaphthalene-1,4,5,8-tetracarboxylic dianhydride, 2,7-dichloronaphthalene-1,4,5,8-tetracarboxylic dianhydride, 2,3,6,7-tetrachloronaphthalene-1,4,5,8-tetracarboxylic dianhydride, 2,3,6,7-tetrachloronaphthalene-2,3,6,7-tetracarboxylic dianhydride, 1,4,5,8-tetrachloronaphthalene-1,4,5,8-tetracarboxylic dianhydride, 1,4,5,8-tetrachloronaphthalene-2,3,6,7-tetracarbo 2,3,8,9-perylene-tetracarboxylic dianhydride, 3,4,9,10-perylene-tetracarboxylic dianhydride, 4,5,10,11-perylene-tetracarboxylic dianhydride, 5,6,11,12-perylene-tetracarboxylic dianhydride, pyrazine-2,3,5,6-tetracarboxylic dianhydride, pyrrolidine-2,3,4,5-tetracarboxylic dianhydride, thiophene-2,3,4,5-tetracarboxylic dianhydride, bis(2,3-dicarboxyphenyl)sulfone dianhydride, bis(3,4-dicarboxyphenyl)sulfone dianhydride. Among them, it is preferable to use BPDA, PMDA, TAHQ and / or BP-TME in combination from the viewpoint of improving the puncture strength of the obtained laminated film and reducing Df and CTE. These tetracarboxylic acid compounds can be used alone or in combination of two or more.
[0158] Examples of diamine compounds used in the synthesis of the PI resin precursor include aliphatic diamines, aromatic diamines, and mixtures thereof. In this embodiment, the term "aromatic diamine" refers to a diamine having an aromatic ring, which may contain an aliphatic group or other substituents in a part of its structure. The aromatic ring may be a single ring or a condensed ring, and examples include a benzene ring, a naphthalene ring, an anthracene ring, and a fluorene ring, but are not limited to these. Among these, a benzene ring is preferable. The term "aliphatic diamine" refers to a diamine having an aliphatic group, which may contain other substituents in a part of its structure, but does not have an aromatic ring.
[0159] Examples of the diamine compound include diamines represented by formula (B1), diamines represented by formula (B2), and diamines represented by formula (2). Any diamine compound known in the art can be appropriately selected and used. Examples of such diamine compounds include 1,4-diaminocyclohexane, 4,4'-diamino-2,2'-dimethylbiphenyl (hereinafter sometimes referred to as m-Tb), 4,4'-diamino-3,3'-dimethylbiphenyl, 2,2'-bis(trifluoromethyl)-4,4'-diaminodiphenyl (hereinafter sometimes referred to as TFMB), 4,4'-diaminodiphenyl ether, 1,3-bis(3-aminophenoxy)benzene (hereinafter sometimes referred to as 1,3-APB), 1,4-bis(4-aminophenoxy)benzene (hereinafter sometimes referred to as TPE-Q), 1,3-bis(4-aminophenoxy)benzene (hereinafter sometimes referred to as TPE-R), 2,2-bis[4-(4-aminophenoxy)phenyl]propane (hereinafter sometimes referred to as BAPP), 2,2'-dimethyl-4,4'-diaminobiphenyl, 3,3'-dihydroxy-4,4'-diaminobiphenyl, 2,2-bis-[4-(3-aminophenoxy)phenyl]propane, bis[4-(4-aminophenoxy)]biphenyl, bis[4-(3-aminophenoxy)biphenyl, bis[1-(4- aminophenoxy)]biphenyl, bis[1-(3-aminophenoxy)]biphenyl, bis[4-(4-aminophenoxy)phenyl]methane, bis[4-(3-aminophenoxy)phenyl]methane, bis[4-(4-aminophenoxy)phenyl]ether, bis[4-(3-aminophenoxy)phenyl]ether, bis[4-(4-aminophenoxy)]benzophenone, bis[4-(3-aminophenoxy)]benzophenone, 2,2-bis-[4-(4-aminophenoxy)phenyl]hexafluoropropane, 2,2-bis-[4-(3 -aminophenoxy)phenyl]hexafluoropropane, 4,4'-methylenedi-o-toluidine, 4,4'-methylenedi-2,6-xylidine, 4,4'-methylene-2,6-diethylaniline, 4,4'-methylenedianiline, 3,3'-methylenedianiline, 4,4'-diaminodiphenylpropane, 3,3'-diaminodiphenylpropane, 4,4'-diaminodiphenylethane, 3,3'-diaminodiphenylethane, 4,4'-diaminodiphenylmethane, 3,3'-diaminodiphenylmethane, 3,3-diaminodiphenylether, 3,4'-Diaminodiphenyl ether, benzidine, 3,3'-diaminobiphenyl, 3,3'-dimethoxybenzidine, 4,4"-diamino-p-terphenyl, 3,3"-diamino-p-terphenyl, m-phenylenediamine, p-phenylenediamine (hereinafter sometimes referred to as p-PDA), resorcinol-bis(3-aminophenyl)ether, 4,4'-[1,4-phenylenebis(1-methylethylidene)]bisaniline, 4,4'-[1,3-phenylenebis(1-methylethylidene)]bisaniline, bis(p-aminocyclohexane p-xylyl)methane, bis(p-β-amino-tert-butylphenyl)ether, bis(p-β-methyl-δ-aminopentyl)benzene, p-bis(2-methyl-4-aminopentyl)benzene, p-bis(1,1-dimethyl-5-aminopentyl)benzene, 1,5-diaminonaphthalene, 2,6-diaminonaphthalene, 2,4-bis(β-amino-tert-butyl)toluene, 2,4-diaminotoluene, m-xylene-2,5-diamine, p-xylene-2,5-diamine, m-xylylenediamine, p-xylylenediamine, piperazine, 4 ,4'-Diamino-2,2'-bis(trifluoromethyl)bicyclohexane, 4,4'-Diaminodicyclohexylmethane, 4,4"-Diamino-p-terphenyl, Bis(4-aminophenyl)terephthalate, 1,4-Bis(4-aminophenoxy)-2,5-di-tert-butylbenzene, 4,4'-(1,3-phenylenediisopropylidene)bisaniline, 1,4-Bis[2-(4-aminophenyl)-2-propyl]benzene, 2,4-Diamino-3,5-diethyltoluene, 2,6-Diamino-3,5-diethyltoluene, 4,4'- Bis(3-aminophenoxy)biphenyl, 4,4'-(hexafluoropropylidene)dianiline, 1,2-diaminoethane, 1,3-diaminopropane, 1,4-diaminobutane, 1,5-diaminopentane, 1,6-diaminohexane, 1,2-diaminopropane, 1,2-diaminobutane, 1,3-diaminobutane, 2-methyl-1,2-diaminopropane, 2-methyl-1,3-diaminopropane, 1,3-bis(aminomethyl)cyclohexane, 1,4-bis(aminomethyl)cyclohexane, norbornanediamine, 2'-methoxy-4,4'-diaminobenzanilide, 4,4'-diaminobenzanilide, bis[4-(4-aminophenoxy)phenyl]sulfone, bis[4-(3-aminophenoxy)phenyl]sulfone, 9,9-bis[4-(4-aminophenoxy)phenyl]fluorene, 9,9-bis[4-(3-aminophenoxy)phenyl]fluorene, 4,4'-diaminodiphenyl sulfide, 3,3'-diaminodiphenyl sulfide, 4,4'-diaminodiphenyl sulfone, 3,3'-diaminodiphenyl sulfone, 2,5-diamino-1,3,4-oxadiazole, bis[4,4'-(4-aminophenoxy)]benzanilide, bis[4,4'-(3-aminophenoxy)]benzanilide, 2,6-diaminopyridine, 2,5-diaminopyridine, and the like. Among these, it is preferable to use m-Tb, BAPP, TPE-Q, 1,3-bis(4-aminophenoxy)benzene and / or TPE-R in combination from the viewpoint of improving the puncture strength of the resulting laminated film and reducing Df and CTE. The diamine compounds can be used alone or in combination of two or more kinds.
[0160] The PI resin precursor may be a product obtained by further reacting, in addition to the tetracarboxylic acid compound used in the synthesis of the PI resin precursor, other tetracarboxylic acids, dicarboxylic acids, tricarboxylic acids, and their anhydrides and derivatives, as long as the physical properties of the resulting PI film are not impaired.
[0161] Other tetracarboxylic acids include water adducts of the anhydrides of the above tetracarboxylic acid compounds.
[0162] Examples of the dicarboxylic acid compound include aromatic dicarboxylic acids, aliphatic dicarboxylic acids, and acid chloride compounds and acid anhydrides related thereto, and two or more of them may be used in combination.Specific examples include dicarboxylic acid compounds of terephthalic acid, isophthalic acid, naphthalenedicarboxylic acid, 4,4'-biphenyldicarboxylic acid, 3,3'-biphenyldicarboxylic acid, chain hydrocarbons having 8 or less carbon atoms, and compounds in which two benzoic acids are linked by a single bond, -O-, -CH2-, -C(CH3)2-, -C(CF3)2-, -SO2-, or a phenylene group, and acid chloride compounds thereof.
[0163] Examples of tricarboxylic acid compounds include aromatic tricarboxylic acids, aliphatic tricarboxylic acids, and their related acid chloride compounds, acid anhydrides, etc., and two or more of them may be used in combination.Specific examples include anhydride of 1,2,4-benzenetricarboxylic acid; 2,3,6-naphthalenetricarboxylic-2,3-anhydride; and a compound in which phthalic anhydride and benzoic acid are linked by a single bond, -O-, -CH2-, -C(CH3)2-, -C(CF3)2-, -SO2-, or a phenylene group.
[0164] In producing the PI resin precursor, the amounts of the diamine compound, tetracarboxylic acid compound, dicarboxylic acid compound, and tricarboxylic acid compound used can be appropriately selected depending on the ratio of each constituent unit of the desired PI resin precursor. In the present invention, the total number of moles of diamine compounds used per mole of the total amount of tetracarboxylic acid compounds is defined as the amine ratio. In a preferred embodiment of the present invention, the amine ratio is preferably 0.90 moles or more and preferably 0.999 moles or less per mole of the total amount of tetracarboxylic acid compounds. In another embodiment, the amine ratio is preferably 1.001 moles or more and preferably 1.10 moles or less per mole of the total amount of tetracarboxylic acid compounds. In one embodiment of the present invention, when the amine ratio is 1 or less, the amine ratio is preferably 0.90 mol to 0.999 mol, more preferably 0.95 mol to 0.997 mol, and even more preferably 0.97 mol to 0.995 mol. In one embodiment of the present invention, when the amine ratio is 1 or more, the amine ratio is preferably 1.001 mol or more and 1.10 mol or less, more preferably 1.002 mol or more and 1.06 mol or less, even more preferably 1.003 mol or more and 1.05 mol or less. If the amine ratio is close to 1.0 moles, the molecular weight tends to increase rapidly during synthesis, and if it is far from 1.0 moles, the molecular weight of the resulting PI resin tends to decrease. If the molecular weight increases rapidly, it grows unevenly in the synthesis mass, and the physical properties of the PI resin obtained from the PI resin precursor tend to be unstable. On the other hand, if the molecular weight is too low, the mechanical properties tend to decrease.
[0165] The reaction temperature between the diamine compound and the tetracarboxylic acid compound is preferably 50°C or less, more preferably 40°C or less, and even more preferably 30°C or less. The reaction temperature between the diamine compound and the tetracarboxylic acid compound is preferably 5°C or more, more preferably 10°C or more, and even more preferably 15°C or more. When the reaction temperature is within the above upper and lower limits, the effects of the present invention are easily obtained, and the reaction rate tends to be increased and the polymerization time can be shortened. The reaction time is not particularly limited, and may be, for example, about 0.5 to 36 hours, and preferably 1 to 24 hours.
[0166] The reaction between the diamine compound and the tetracarboxylic acid compound is preferably carried out in a solvent. The solvent is not particularly limited as long as it does not affect the reaction, and examples of the solvent include alcohol-based solvents such as water, methanol, ethanol, ethylene glycol, isopropyl alcohol, propylene glycol, ethylene glycol methyl ether, ethylene glycol butyl ether, 1-methoxy-2-propanol, 2-butoxyethanol, and propylene glycol monomethyl ether; phenol-based solvents such as phenol and cresol; ester-based solvents such as ethyl acetate, butyl acetate, ethylene glycol methyl ether acetate, propylene glycol methyl ether acetate, and ethyl lactate; lactone-based solvents such as γ-butyrolactone (hereinafter sometimes referred to as GBL) and γ-valerolactone; acetone, methyl ethyl ketone, cyclopentanone, cyclohexanone, 2-heptanone, methyl ethyl ketone, methyl ethyl ketone, methyl ethyl ketone, methyl ethyl ketone, methyl ethyl ketone, methyl ethyl ketone, methyl ethyl ketone, methyl ethyl ketone, methyl ethyl ether ... Examples of suitable solvents include ketone solvents such as triisobutyl ketone, aliphatic hydrocarbon solvents such as pentane, hexane, and heptane, alicyclic hydrocarbon solvents such as ethylcyclohexane, aromatic hydrocarbon solvents such as toluene and xylene, nitrile solvents such as acetonitrile, ether solvents such as tetrahydrofuran and dimethoxyethane, chlorine-containing solvents such as chloroform and chlorobenzene, amide solvents such as N,N-dimethylacetamide (hereinafter sometimes referred to as DMAc), N,N-dimethylformamide (hereinafter sometimes referred to as DMF), sulfur-containing solvents such as dimethylsulfone, dimethylsulfoxide, and sulfolane, carbonate solvents such as ethylene carbonate and propylene carbonate, pyrrolidone solvents such as N-methylpyrrolidone (hereinafter sometimes referred to as NMP), and combinations thereof. Among these, from the viewpoint of solubility, phenol solvents, lactone solvents, amide solvents, and pyrrolidone solvents, and more preferably amide solvents, can be used.
[0167] In one embodiment of the present invention, the boiling point of the solvent used in the reaction between the diamine compound and the tetracarboxylic acid compound is preferably suitable for the imidization conditions for controlling the parameter X and the thickness of the intermediate region in the laminate film within the desired range, and is preferably 230° C. or lower, more preferably 200° C. or lower, and even more preferably 180° C. or lower, and is preferably 100° C. or higher, and more preferably 120° C. or higher.
[0168] The reaction between the diamine compound and the tetracarboxylic acid compound may be carried out, as necessary, in an inert atmosphere such as a nitrogen atmosphere or an argon atmosphere or under reduced pressure conditions. It is preferable to carry out the reaction in an inert atmosphere, such as a nitrogen atmosphere or an argon atmosphere, in a strictly controlled dehydrated solvent with stirring.
[0169] The resulting PI resin precursor may be temporarily isolated by a conventional method, but may also be used as a PI resin precursor solution by diluting the reaction solution containing the PI resin precursor obtained by synthesis of the PI resin precursor with an appropriate solvent as necessary without isolating the PI resin precursor.
[0170] (Coating and pre-drying process) In the production of the laminated film of the present invention, the coating and pre-drying step is a step of applying a solution of a corresponding PI resin precursor to a supporting substrate and pre-drying the solution to obtain a multilayer coating film. Specifically, there is a method of obtaining a multilayer coating film by repeatedly applying a solution of a corresponding PI resin precursor to a supporting substrate and pre-drying the solution several times (sometimes called a sequential pattern), and a method of obtaining a multilayer coating film by simultaneously applying a solution of a corresponding PI resin precursor to each layer in a multilayer laminated state by multilayer extrusion and pre-drying the solution (sometimes called a simultaneous pattern). For example, in the case of a laminated film (L) having a PI-based resin-containing layer (PI-2), a PI-based resin-containing layer (PI-1), and a PI-based resin-containing layer (PI-3) in this order, the sequential pattern may be a process of coating a PI-based resin precursor solution corresponding to the PI-based resin-containing layer (PI-2) on a supporting substrate, pre-drying the solution to form a coating film, coating the PI-based resin precursor solution corresponding to the PI-based resin-containing layer (PI-1) on the coating film, pre-drying the solution to form a two-layer coating film, coating the PI-based resin precursor solution corresponding to the PI-based resin-containing layer (PI-3) on the two-layer coating film, pre-drying the solution to form a three-layer coating film. In addition, the simultaneous pattern may be a process of simultaneously coating a PI-based resin precursor solution corresponding to the PI-based resin-containing layer (PI-2), a PI-based resin precursor solution corresponding to the PI-based resin-containing layer (PI-1), and a PI-based resin precursor solution corresponding to the PI-based resin-containing layer (PI-3) on a supporting substrate by multilayer extrusion or the like, and pre-drying the solution to form a three-layer coating film.
[0171] The solvent contained in the PI resin precursor solution may be any of the solvents exemplified for use in the reaction of a diamine compound with a tetracarboxylic acid compound in the production of a PI resin precursor, and is preferably a lactone solvent, an amide solvent, or a pyrrolidone solvent, and more preferably an amide solvent. In one embodiment of the present invention, the boiling point of the solvent contained in the PI resin precursor solution is preferably suitable for the imidization conditions for controlling the parameter X in the laminate film and the thickness of the intermediate region within a desired range, and is preferably 230° C. or less, more preferably 200° C. or less, even more preferably 180° C. or less, particularly preferably 170° C. or less, and is preferably 100° C. or more, more preferably 120° C. or more.
[0172] The content of the PI resin precursor in the PI resin precursor solution is preferably 8% by mass or more, more preferably 10% by mass or more, even more preferably 12% by mass or more, and particularly preferably 13% by mass or more, based on the total amount of the PI resin precursor solution, and is preferably 30% by mass or less, more preferably 25% by mass or less, even more preferably 23% by mass or less, and particularly preferably 20% by mass or less. When the content of the PI resin precursor is within the above range, excellent processability during film formation is achieved.
[0173] The coating film of the PI resin precursor solution can be formed by coating the PI resin precursor solution on a supporting substrate by a known coating or application method. Known coating methods include, for example, roll coating methods such as wire bar coating, reverse coating, and gravure coating, die coating, comma coating, lip coating, spin coating, screen printing coating, fountain coating, dipping, spraying, curtain coating, slot coating, and drip molding. The PI resin precursor solution may be coated on the supporting substrate one layer at a time or in multiple batches to form a coating film of the PI resin precursor solution with multiple layers, or a laminated coating film of the PI resin precursor solution with multiple layers may be formed at the same time. For example, a co-extrusion method, a multi-layer curtain coating method, and the like can be used as a method for simultaneously forming a coating film with multiple layers.
[0174] Examples of the supporting substrate include metal plates (e.g., copper plates, etc.) such as metal foils (e.g., copper foils), SUS plates such as SUS foils and SUS belts, glass substrates, PET films, PEN films, PI resin films other than the PI resin-containing layer in the present invention, and polyamide resin films. Among them, from the viewpoint of excellent heat resistance, copper plates, SUS plates, glass substrates, PET films, PEN films, etc. are preferred, and from the viewpoint of adhesion and cost, copper plates, SUS plates, glass substrates, or PET films are more preferred. In one embodiment of the present invention, examples of the metal constituting the metal foil include aluminum, copper, iron, nickel, chromium, titanium, tantalum, stainless steel, and alloys thereof. Among these, the metal foil is preferably copper foil, copper alloy foil, SUS foil, aluminum foil, etc., and from the viewpoint of electrical conductivity and metal processability, copper foil or copper alloy foil is more preferred, and copper foil is particularly preferred.
[0175] In the coating and pre-drying steps, the temperature at which the multilayer coating film is pre-dried is preferably 60° C. or higher, more preferably 70° C. or higher, even more preferably 80° C. or higher, even more preferably 90° C. or higher, and preferably 200° C. or lower, more preferably 150° C. or lower, even more preferably 130° C. or lower. The pre-drying time is preferably 30 seconds or more, more preferably 1 minute or more, even more preferably 5 minutes or more, even more preferably 10 minutes or more, for example, 15 minutes or more, 20 minutes or more, or 25 minutes or more, and is preferably 24 hours or less, more preferably 12 hours or less, even more preferably 6 hours or less, and particularly preferably 1 hour or less. When the pre-drying temperature and pre-drying time are within the above ranges, the solvent tends to remain in the multilayer coating film during imidization.
[0176] (Standing process) The standing step is a step of standing the multilayer coating film obtained in the coating and preliminary drying steps. By subjecting the coating film to the standing step before the imidization step, the solvent is likely to remain in the entire coating film at the time of imidization, or the resin layers are likely to be well-adjusted, and the degree of freedom of the resin molecules can be increased until the time of imidization. This influence causes a moderate decrease in the planar orientation of the PI resin, that is, a moderate disturbance in the orientation in the planar direction, so that the degree of elastic deformation of the obtained PI resin-containing layer in the thickness direction cross section tends to increase. And, since the degree of disturbance in the orientation differs between the two or more PI resin-containing layers (preferably the mPI layer and the TPI layer), the degree of elastic deformation differs between the layers. Here, as described above, when the molecular orientation is moderately disturbed and the layer with a large degree of elastic deformation is the layer (PI-2) (preferably the TPI layer), the decrease in the denominator (E2r-E2a) corresponding to the layer (PI-2) is greater than the decrease in the numerator (E1r-E1a) corresponding to the layer (PI-1) (preferably the mPI layer), that is, the denominator tends to decrease more than the numerator due to the standing process, so the value of (E1r-E1a) / (E2r-E2a) in formula (I) tends to increase, and formula (I) is likely to be satisfied. In addition, when the solvent is well mixed into the entire coating film during imidization, that is, when the resin molecules have a high degree of freedom, the PI resins constituting each layer are likely to mix with each other near the interface of each layer, so the thickness of the intermediate region may be increased.
[0177] In the leaving step, the time for leaving the multilayer coating film (also called the leaving time) can be appropriately selected according to the temperature at which it is left (also called the leaving temperature), and is not particularly limited, but is preferably 3 hours or more, more preferably 6 hours or more, even more preferably 12 hours or more, even more preferably 18 hours or more, and particularly preferably 22 hours or more, for example, 24 hours or more, 30 hours or more, 36 hours or more, or 45 hours or more. The upper limit of the leaving time of the multilayer coating film is not particularly limited, and may usually be 450 hours or less, preferably 100 hours or less. When the leaving time of the multilayer coating film is within the above range, the solvent is likely to remain sufficiently (or be well blended) throughout the coating film during imidization, so that the parameter X in the laminated film and the thickness of the intermediate region are easily adjusted to the desired range.
[0178] In a preferred embodiment of the present invention, the standing step is preferably a step of standing (or storing) the multilayer coating film at a low temperature (preferably refrigerated). Standing (or storing) at a low temperature makes it easier to create a state in which the solvent remains more sufficiently throughout the coating film or the resin layers are more closely inter-layered, so that the degree of freedom of the resin molecules until imidization can be further increased, and it is easier to adjust the above-mentioned parameter X and the thickness of the intermediate region to a desired range. In the leaving step, the leaving temperature of the multilayer coating film is preferably 20°C or less, more preferably 15°C or less, even more preferably 10°C or less, even more preferably 8°C or less, and particularly preferably 5°C or less. When the leaving temperature of the multilayer coating film is below the upper limit, it is easier to create a state in which the solvent remains sufficiently throughout the coating film (or is well-dispersed) during imidization, so that the above-mentioned parameter X in the laminate film and the thickness of the intermediate region are more easily adjusted to the desired range. In addition, the lower limit of the leaving temperature of the multilayer coating film is usually -30°C or more, preferably -20°C or more, even more preferably -10°C or more, even more preferably -5°C or more, and particularly preferably 0°C or more. The leaving step may be carried out, for example, in air or an inert gas atmosphere, or in a closed space. In a preferred embodiment of the present invention, the laminate film obtained by the production method including the above-mentioned leaving step is likely to satisfy the above-mentioned parameter X and thickness of the intermediate region, and not only is it likely to obtain high puncture strength, but it is also likely to maintain a low Df.
[0179] (Imidization process) The imidization step is a step in which each PI resin in the multilayer coating film on the supporting substrate is imidized by, for example, heat treatment at 200° C. or higher and 500° C. or lower.
[0180] In one embodiment of the present invention, the imidization step preferably includes a step of increasing the temperature from a low temperature (referred to as a first temperature) to a high temperature (referred to as a second temperature) at a relatively high rate and maintaining the temperature at the high temperature. By increasing the temperature at a relatively high rate, preferably rapidly, to proceed with imidization, and then maintaining the temperature at a high temperature for a certain period of time to complete the imidization, this can be advantageous in terms of forming a higher-order structure or a branched structure of the PI resin, and the resulting laminated film can easily improve the pin puncture strength while maintaining a low Df. This can also be advantageous in terms of obtaining a smooth laminated film.
[0181] In one embodiment of the present invention, the first temperature is preferably 20°C or more and 50°C or less, more preferably 25°C or more and 35°C or less, and the second temperature is preferably 220°C or more and 450°C or less, more preferably 250°C or more and 400°C or less, even more preferably 300°C or more and 380°C or less, and particularly preferably 330°C or more and 360°C or less. According to the laminated film of the present invention, even if imidization is performed at a relatively low temperature of, for example, 360°C or less (preferably 350°C or less), it is possible to exhibit high pin puncture strength and reduce Df. Furthermore, if the imidization temperature is 360°C or less (preferably 350°C or less), even when copper foil is used as a supporting substrate, the thermal deterioration of the copper foil can be suppressed, so that a laminated sheet having excellent high frequency characteristics can be easily obtained. Moreover, the imidization temperature is preferably 200°C or more, more preferably 210°C or more, and even more preferably 220°C or more from the viewpoint of sufficiently improving the imidization rate, improving the pin puncture strength, and reducing Df.
[0182] In one embodiment of the present invention, the temperature rise from the first temperature to the second temperature may be performed at a single-stage temperature rise rate, or at a multi-stage temperature rise rate of two or more stages. In one embodiment of the present invention, when the temperature rise from the first temperature to the second temperature is performed in a single stage, the temperature rise rate is preferably 3.5°C / min or more, more preferably 5°C / min or more, even more preferably 7°C / min or more, even more preferably 9°C / min or more, and is preferably 50°C / min or less, more preferably 40°C / min or less, and even more preferably 35°C / min or less. When the temperature rise is performed at a multi-stage temperature rise rate of two or more stages, the temperature rise rate of the first stage and the temperature rise rate of the second stage may be the same or different, and it is preferable that the second stage or later is faster than the first stage. The temperature rise rate of the first stage may be preferably 1 to 15°C / min or less, more preferably 3 to 12°C / min or less, and the temperature rise rate of the second stage or later may be preferably 3 to 35°C / min, more preferably 8 to 25°C / min. The above-mentioned heating rate can be advantageous in terms of forming a higher-order structure or a branched structure of the PI resin, so that the obtained laminated film can easily have improved pin puncture strength while maintaining a low Df, and can also be advantageous in terms of obtaining a smooth laminated film.
[0183] In one embodiment of the present invention, the temperature rise time from the first temperature to the second temperature can be appropriately selected depending on these temperatures and the temperature rise rate, and is preferably 5 hours or less, more preferably 3 hours or less, even more preferably 2 hours or less, and particularly preferably 1 hour or less, and may be 50 minutes or less in some cases, and is preferably 3 minutes or more, more preferably 5 minutes or more, and even more preferably 7 minutes or more. When the temperature rise time from the first temperature to the second temperature is within the above range, the obtained laminate film is likely to have improved pin puncture strength while maintaining a low Df.
[0184] In one embodiment of the present invention, the holding time at the second temperature is preferably 1 minute or more, more preferably 3 minutes or more, and preferably 30 minutes or less, more preferably 20 minutes or less, and even more preferably 10 minutes or less. When the heating rate from the first temperature to the second temperature is within the above range, and further when the holding time at the second temperature is within the above range, this can be advantageous in terms of the formation of a higher-order structure or a branched structure of the PI resin, and the obtained laminate film tends to have improved pin puncture strength while maintaining a low Df.
[0185] After imidization, the multilayer coating film formed on the supporting substrate can be peeled off from the supporting substrate to obtain a laminate film. In one embodiment of the present invention, when the supporting substrate is a metal foil (e.g., copper foil), a laminate sheet in which the laminate film is laminated on the metal foil can be obtained without peeling off the coating film from the metal foil.
[0186] <Physical properties of laminated film> In one embodiment of the present invention, the content of the PI resin in each PI resin-containing layer constituting the laminate film is preferably 60% by mass or more, more preferably 70% by mass or more, even more preferably 80% by mass or more, and particularly preferably 90% by mass or more, based on the mass of the PI resin-containing layer. The upper limit of the PI resin content is not particularly limited, and may be, for example, 100% by mass or less, 99% by mass or less, or 95% by mass or less, based on the mass of the PI resin-containing layer. When the PI resin content is within the above range, a laminate film with improved pin puncture strength, dielectric properties, and thermal properties can be obtained.
[0187] In the laminated film of the present invention, each PI resin-containing layer may contain a filler as necessary. Examples of the filler include metal oxide particles such as silica and alumina, inorganic salts such as calcium carbonate, and polymer particles such as fluororesins and cycloolefin polymers. The filler may be used alone or in combination of two or more. When a filler is contained, the content thereof is preferably 50% by mass or less, more preferably 40% by mass or less, and even more preferably 30% by mass or less, and is preferably 0.01% by mass or more, based on the mass of the PI resin-containing layer.
[0188] In one embodiment of the present invention, each PI resin-containing layer constituting the laminated film of the present invention may contain additives as necessary. Examples of additives include antioxidants, flame retardants, crosslinking agents, surfactants, compatibilizers, imidization catalysts, weathering agents, lubricants, antiblocking agents, antistatic agents, antifogging agents, anti-dripping agents, and pigments. The additives may be used alone or in combination of two or more. The content of each additive may be appropriately selected within a range that does not impair the effects of the present invention. When various additives are included, the total content is preferably 7% by mass or less, more preferably 5% by mass or less, even more preferably 4% by mass or less, particularly preferably 1% by mass or less, and preferably 0.001% by mass or more, based on the mass of each PI resin-containing layer.
[0189] Printed circuits are required to have low transmission loss. Transmission loss is expressed as the sum of dielectric loss, which is loss caused by the electric field generated in the dielectric, and conductor loss, which is loss caused by the current flowing through the conductor. It is known that dielectric loss is approximately proportional to the index E, which is expressed by formula (i). E = Df × (Dk) 1 / 2 (i) [In formula (i), Df represents the dielectric tangent, and Dk represents the relative dielectric constant] In the high frequency range used in FPCs for high-speed communications such as 5G, dielectric loss tends to increase, so there is a particular demand for materials that have a small value of the index E and can suppress dielectric loss. On the other hand, high frequency signals concentrate current on the surface of the conductor. Therefore, conductor loss is related to the dielectric properties of the adjacent dielectric material and is approximately (Dk) 1 / 2 is known to be proportional to
[0190] The laminated film of the present invention has small Df and Dk, and also has small dielectric loss index E and conductor loss, so that the transmission loss can be reduced in a circuit including the laminated film. Therefore, the laminated film of the present invention can exhibit high pin puncture strength while maintaining excellent dielectric properties (especially while maintaining low Df).
[0191] In one embodiment of the present invention, the dielectric loss index E of the laminated film at 10 GHz is preferably 0.0080 or less, more preferably 0.0075 or less, even more preferably 0.0070 or less, even more preferably 0.0065 or less, particularly preferably 0.0060 or less, and particularly preferably 0.0059 or less. The smaller the index E, the lower the transmission loss of an electronic circuit including the laminated film, so there is no particular lower limit for the index E, and it may be, for example, 0 or more.
[0192] In one embodiment of the present invention, the Df of the laminate film at 10 GHz is preferably 0.0040 or less, more preferably 0.0035 or less, even more preferably 0.0034 or less, even more preferably 0.0033 or less, and particularly preferably 0.0032 or less, from the viewpoint of reducing the transmission loss of an electronic circuit when the laminate film is incorporated into the electronic circuit. The smaller the Df, the lower the transmission loss of an electronic circuit including the laminate film, so the lower limit of the Df is not particularly limited and may be, for example, 0 or more.
[0193] In one embodiment of the present invention, the Dk of the laminated film at 10 GHz is preferably 3.500 or less, more preferably 3.450 or less, and even more preferably 3.400 or less.
[0194] The Df and Dk of the laminated film can be measured using a vector network analyzer and a resonator, for example, by the method described in the Examples.
[0195] In one embodiment of the present invention, the coefficient of linear expansion (CTE) of the laminated film is preferably less than 45 ppm / K, more preferably 40 ppm / K or less, even more preferably 35 ppm / K or less, and even more preferably 32 ppm / K or less, and may be, for example, 31 ppm / K or less, 30 ppm / K or less, or 25 ppm / K or less. When the CTE of the laminated film is below the above upper limit, it is expected to have excellent thermal properties and high dimensional stability. In addition, the CTE of the laminated film is preferably 0 ppm / K or more, more preferably 5 ppm / K or more, even more preferably 8 ppm / K or more, and particularly preferably 10 ppm / K or more. When the CTE of the laminated film is within the above upper and lower limits, the CTE of the metal foil (particularly the copper foil) and the PI resin-containing layer of the laminated film become close to each other, so that the effect of suppressing peeling of the laminated film from the metal foil is obtained. The CTE can be measured, for example, by a thermomechanical analyzer (hereinafter sometimes referred to as "TMA") and is obtained by the method described in the examples.
[0196] The laminated film of the present invention may be subjected to a surface treatment such as corona discharge treatment, plasma treatment, ozone treatment, etc., by a method usually adopted industrially.
[0197] In one embodiment of the present invention, the laminated film of the present invention has a puncture strength (value) of preferably 12.0 or more, more preferably 14.0N or more, even more preferably 16.0N or more, even more preferably 20.0N or more, and particularly preferably 23.0N or more when the thickness of the laminated film is converted to 50 μm. In other words, the puncture strength per unit thickness of the laminated film of the present invention is preferably 0.24N / μm or more, more preferably 0.28N / μm or more, even more preferably 0.32N / μm or more, even more preferably 0.40N / μm or more, and particularly preferably 0.46N / μm or more. When the puncture strength of the laminated film is the lower limit or more, breakage when the film is subjected to an impact in the thickness direction can be effectively suppressed. The upper limit of the puncture strength of the laminated film is not limited and may be, for example, 50N or less. The puncture strength can be measured using a small tabletop tester in accordance with JIS Z 1707 under an environment of a temperature of 23° C. and a relative humidity of 50%. Specifically, it can be measured by the method described in the Examples below.
[0198] The laminated film of the present invention has a high puncture strength and can be suitably used as a substrate material compatible with printed circuit boards and antenna substrates. In addition, the laminated film of the present invention has a low Df and can achieve low transmission loss even in a high frequency band that transmits high frequency signals. Therefore, it is particularly suitable as a substrate material compatible with printed circuit boards and antenna substrates for high speed communication such as 5G.
[0199] [Laminated sheet] The laminate film of the present invention has a sufficiently high puncture strength and can reduce Df, so it can be suitably used for forming a metal-clad laminate used in an FPC. Therefore, the present invention includes a laminate sheet including the laminate film of the present invention and a metal foil layer. In one embodiment of the present invention, the laminate sheet of the present invention may include a metal foil layer on only one side of the laminate film of the present invention, or on both sides.
[0200] In one embodiment of the present invention, the metal constituting the metal foil layer may be any of the metals described above. Among these, the metal foil layer is preferably a copper foil layer, a copper alloy foil layer, a SUS foil layer, an aluminum foil layer, etc., and from the viewpoint of electrical conductivity and metal workability, a copper foil layer or a copper alloy foil layer is more preferable, and a copper foil layer is particularly preferable.
[0201] In one embodiment of the present invention, the thickness of the metal foil layer, particularly the copper foil layer, is preferably 1 μm or more, more preferably 5 μm or more, and from the viewpoint of facilitating fine circuitry and improving bending resistance, is preferably 100 μm or less, more preferably 50 μm or less, even more preferably 30 μm or less, and particularly preferably 20 μm or less. The thickness of the metal foil layer, particularly the copper foil layer, can be measured using a film thickness meter or the like. In addition, when the laminated film includes a metal foil layer, particularly a copper foil layer, on both sides, the thickness of each metal foil layer, particularly each copper foil layer, may be the same or different from each other.
[0202] The laminated sheet of the present invention may contain other layers such as functional layers in addition to the laminated film of the present invention and the metal foil layer, particularly the copper foil layer. Examples of the functional layer include an adhesive layer. The functional layers can be used alone or in combination of two or more kinds.
[0203] In one embodiment of the present invention, the laminate sheet of the present invention may be a metal-clad laminate composed of a laminate film consisting of a metal foil layer and two or more PI resin-containing layers, or may be a metal-clad laminate composed of a laminate film consisting of a metal foil layer, two or more PI resin-containing layers, and an adhesive layer. However, from the viewpoints of heat resistance, dimensional stability, and weight reduction, a metal-clad laminate not including an adhesive layer is preferred. In addition, the laminate film of the present invention can be formed at a relatively low imidization temperature, and even when a laminate sheet having a copper foil as the metal foil is produced by thermally imidizing a PI resin precursor coating film on a copper foil, it is possible to achieve sufficiently high pin puncture strength and low Df while suppressing deterioration of the copper foil surface. Therefore, the laminate sheet of the present invention has excellent high-frequency characteristics even without an adhesive layer.
[0204] In one embodiment of the present invention, the laminate film of the present invention and the metal foil layer, particularly the copper foil layer, may be in direct contact, or a functional layer may be inserted between the laminate film and the metal foil layer, particularly the copper foil layer, and they may be in contact via the functional layer; however, from the viewpoint of improving puncture strength and thermal properties, it is preferable that the laminate film and the metal foil layer, particularly the copper foil layer, are in direct contact.
[0205] <Method of manufacturing laminated sheet> The laminate sheet of the present invention can be produced, for example, by the following steps: A process of applying a solution of a corresponding PI-based resin precursor onto a metal foil and pre-drying the solution to obtain a multi-layer coating film; A step of leaving the obtained multi-layer coating film still; and A process of forming the laminated film of the present invention on the metal foil by heating the multi-layer coating film to imidize the PI resin. The composition can be produced by a method comprising the steps of:
[0206] In the above-mentioned production method, the description of each step in the production method of the laminated film of the present invention described above is similarly applied, and the preferred embodiments and the like are also similar.
[0207] The laminate sheet of the present invention may be produced by a method other than the above-mentioned method, for example, a method in which a multi-layer coating film of a PI-based resin precursor obtained by coating and drying a PI-based resin precursor solution on a support substrate other than the metal foil contained in the laminate sheet is peeled off from the substrate, and the peeled multi-layer coating film of the PI-based resin precursor is laminated to a metal foil. As a method for laminating a multi-layer coating film of a PI-based resin precursor and a metal foil, a method using a press or a lamination method using a heated roll may be adopted, and imidization of the PI-based resin precursor may be performed simultaneously in the lamination process. However, the laminate film of the present invention can be formed at a relatively low imidization temperature, and even if a laminate sheet in which the metal foil is a copper foil is produced by thermally imidizing the PI-based resin precursor coating film on a copper foil, high pin puncture strength and low Df can be achieved while suppressing deterioration of the copper foil surface. Therefore, the laminate sheet of the present invention has excellent high-frequency characteristics even when produced without undergoing the lamination process as described above.
[0208] [Flexible printed circuit board] The laminated film of the present invention has excellent puncture strength and can be suitably used as an FPC board material. In addition, the laminated film of the present invention can have a low Df, so that the transmission loss of an electric circuit incorporating the laminated film can be reduced. Furthermore, the laminated film of the present invention has a low CTE and excellent thermal properties, so that it can be suitably used as an FPC board material, particularly an FPC board material for high-speed communication such as 5G. Therefore, the present invention also includes a flexible printed circuit board including the laminated film or laminated sheet of the present invention. EXAMPLES
[0209] The present invention will be described in more detail below based on examples and comparative examples, but the present invention is not limited to the following examples.
[0210] The abbreviations used in the examples and comparative examples represent the following compounds. BPDA: 3,3',4,4'-biphenyltetracarboxylic dianhydride BP-TME: 4,4'-bis(1,3-dioxo-1,3-dihydroisobenzofuran-5-ylcarbonyloxy)biphenyl PMDA: Pyromellitic dianhydride m-Tb: 4,4'-diamino-2,2'-dimethylbiphenyl TPE-Q: 1,4-bis(4-aminophenoxy)benzene TPE-R: 1,3-bis(4-aminophenoxy)benzene
[0211] 1. Preparation of Polyimide Resin Precursor Solution (1) Polyimide resin precursor solution 1 48.61g (228.9mmol) of m-Tb and 66.92g (228.9mmol) of TPE-Q were dissolved in 1598g of DMAc, and then 118.22g (221.2mmol) of BP-TME was added and stirred for 1 hour at 20°C under a nitrogen atmosphere. Then, 48.25g (221.2mmol) of PMDA was added and stirred for 3 hours at 20°C under a nitrogen atmosphere to obtain PI resin precursor solution 1. The molar ratio of diamine monomer to acid dianhydride monomer used was 1.04.
[0212] (2) Polyimide resin precursor solution 2 After dissolving 44.34g (208.8mmol) of m-Tb and 61.06g (208.8mmol) of TPE-R in 1598g of DMAc, 85.39g (290.2mmol) of BPDA and 27.13g (124.4mmol) of PMDA were added in that order and stirred for 3 hours at 20°C under a nitrogen atmosphere to obtain PI resin precursor solution 2. The molar ratio of diamine monomer to acid dianhydride monomer used was 1.01.
[0213] (3) Polyimide resin precursor solution 3 9.87g (46.5mmol) of m-Tb and 122.35g (418.5mmol) of TPE-R were dissolved in 1890g of DMAc, and then 30.26g (138.7mmol) of PMDA and 95.25g (323.7mmol) of BPDA were added in that order and stirred for 3 hours at 20°C under a nitrogen atmosphere to obtain PI resin precursor solution 3. The molar ratio of diamine monomer to acid dianhydride monomer used was 1.01.
[0214] (4) Polyimide resin precursor solution 4 14.40g (67.8mmol) of m-Tb and 19.82g (67.8mmol) of TPE-Q were dissolved in 405g of DMAc, and then 7.11g (13.3mmol) of BP-TME was added and stirred for 1 hour at 20°C under a nitrogen atmosphere. Then, 14.50g (66.5mmol) of PMDA and 15.65g (53.2mmol) of BPDA were added and stirred for 3 hours at 20°C under a nitrogen atmosphere to obtain PI resin precursor solution 4. The molar ratio of diamine monomer to acid dianhydride monomer used was 1.02.
[0215] (5) Polyimide resin precursor solution 5 57.72 g (271.9 mmol) of m-Tb and 8.83 g (30.2 mmol) of TPE-Q were dissolved in 810 g of DMAc, and then 32.53 g (149.1 mmol) of PMDA and 43.87 g (149.1 mmol) of BPDA were added and stirred for 3 hours at 20°C under a nitrogen atmosphere to obtain PI resin precursor solution 5. The molar ratio of diamine monomer to acid dianhydride monomer used was 1.01.
[0216] 2. Preparation of Laminated Film (1) Example 1 The PI resin precursor solution 2 / PI resin precursor solution 1 / PI resin precursor solution 2 prepared above were simultaneously applied to the roughened surface (surface roughness; Rz=0.6 μm) of an electrolytic copper foil (thickness 12 μm) as an upper layer / middle layer / lower layer to a dry thickness of 5 μm / 40 μm / 5 μm, respectively, to form a three-layer laminated coating film of the PI resin precursor solution. Next, the three-layer laminated coating film was heated at 100 ° C for 12 minutes and dried, and then the laminate consisting of the copper foil and the three-layer laminated coating film was placed in a sealed container and left to stand for 24 hours in an environment at a temperature of 4 ° C. After that, it was confirmed that the laminate taken out of the sealed container had reached room temperature, and then it was fixed to a metal frame and heated from 30 ° C to 320 ° C over 10 minutes in an oxygen concentration 1% atmosphere, and then held at 320 ° C for 5 minutes. The obtained laminated film with copper foil, consisting of a PI resin-containing layer and a copper foil, was immersed in a large amount of ferric chloride aqueous solution with a concentration of 40% by mass at room temperature for 10 minutes, and then the ferric chloride aqueous solution was washed with pure water. After visually confirming that no copper remained, the film was dried at 80°C for 1 hour to obtain a laminated film 1 consisting of a layer (PI-2) (copper foil layer side), a layer (PI-1) and a layer (PI-3) (TPI layer, mPI layer and TPI layer) laminated in this order. The thickness of the laminated film 1 was 50 μm, the thickness of the intermediate region between the layer (PI-2) and the layer (PI-1) was 400 nm, the thicknesses of the layer (PI-2) and the layer (PI-3) were 4.8 μm, and the thickness of the layer (PI-1) was 39.6 μm.
[0217] (2) Example 2 A laminated film 2 was obtained by laminating a layer (PI-2) (copper foil layer side), a layer (PI-1) and a layer (PI-3) (TPI layer, mPI layer and TPI layer) in this order in the same manner as in Example 1, except that PI-based resin precursor solution 3 / PI-based resin precursor solution 1 / PI-based resin precursor solution 3 were simultaneously coated as the upper layer / middle layer / lower layer to a dry thickness of 5 μm / 40 μm / 5 μm, respectively. The thickness of the laminated film 2 was 50 μm, the thickness of the intermediate region between the layer (PI-2) and the layer (PI-1) was 1800 nm, the thicknesses of the layer (PI-2) and the layer (PI-3) were 4.1 μm, and the thickness of the layer (PI-1) was 38.2 μm.
[0218] (3) Example 3 The PI resin precursor solution 3 was applied to the roughened surface (surface roughness; Rz = 0.6 μm) of an electrolytic copper foil (thickness 12 μm) so as to have a dry thickness of 5 μm to obtain a coating film. The coating film was heated and dried at 120 ° C for 10 minutes, and the PI resin precursor solution 4 was applied to the dried coating film so as to have a dry thickness of 36 μm to obtain a two-layer laminate coating film. The two-layer laminate coating film was heated and dried at 120 ° C for 30 minutes, and the PI resin precursor solution 3 was applied to the dried two-layer laminate coating film so as to have a dry thickness of 5 μm to obtain a three-layer laminate coating film. The three-layer laminate coating film was heated and dried at 120 ° C for 30 minutes, and then the laminate consisting of the copper foil and the three-layer laminate coating film was placed in a sealed container and left to stand for 24 hours in an environment at a temperature of 4 ° C. After that, after confirming that the laminate taken out of the sealed container had reached room temperature, it was fixed to a metal frame, and heated from 30°C to 320°C over 10 minutes in an atmosphere with an oxygen concentration of 1%, and then held at 320°C for 5 minutes. The obtained laminated film with copper foil consisting of a PI-based resin-containing layer and a copper foil was immersed in a large amount of a 40% by mass concentration ferric chloride aqueous solution at room temperature for 10 minutes, and then the ferric chloride aqueous solution was washed with pure water. After visually confirming that no copper remained, it was dried at 80°C for 1 hour to obtain a laminated film 3 consisting of a layer (PI-2) (copper foil layer side), a layer (PI-1) and a layer (PI-3) (TPI layer, mPI layer and TPI layer) laminated in this order. The thickness of the laminated film 3 was 46 μm, the thickness of the intermediate region between the layer (PI-2) and the layer (PI-1) was 2500 nm, the thicknesses of the layers (PI-2) and (PI-3) were 3.8 μm, and the thickness of the layer (PI-1) was 33.5 μm.
[0219] (4) Example 4 The PI resin precursor solution 3 was applied to the roughened surface (surface roughness; Rz = 0.6 μm) of an electrolytic copper foil (thickness 12 μm) so as to have a dry thickness of 5 μm to obtain a coating film. The coating film was heated and dried at 120 ° C for 10 minutes, and the PI resin precursor solution 5 was applied to the dried coating film so as to have a dry thickness of 36 μm to obtain a two-layer laminate coating film. The two-layer laminate coating film was heated and dried at 120 ° C for 30 minutes, and the PI resin precursor solution 3 was applied to the dried two-layer laminate coating film so as to have a dry thickness of 5 μm to obtain a three-layer laminate coating film. The three-layer laminate coating film was heated and dried at 120 ° C for 30 minutes, and then the laminate consisting of the copper foil and the three-layer laminate coating film was placed in a sealed container and left to stand for 48 hours in an environment at a temperature of 4 ° C. After that, after confirming that the laminate taken out of the sealed container had reached room temperature, it was fixed to a metal frame, and heated from 30°C to 320°C over 10 minutes in an atmosphere with an oxygen concentration of 1%, and then held at 320°C for 5 minutes. The obtained laminated film with copper foil consisting of a PI-based resin-containing layer and a copper foil was immersed in a large amount of a 40% by mass concentration ferric chloride aqueous solution at room temperature for 10 minutes, and then the ferric chloride aqueous solution was washed with pure water. After visually confirming that no copper remained, it was dried at 80°C for 1 hour to obtain a laminated film 3 consisting of a layer (PI-2) (copper foil layer side), a layer (PI-1) and a layer (PI-3) (TPI layer, mPI layer and TPI layer) laminated in this order. The thickness of the laminated film 3 was 46 μm, the thickness of the intermediate region between the layer (PI-2) and the layer (PI-1) was 2800 nm, the thicknesses of the layers (PI-2) and (PI-3) were 3.6 μm, and the thickness of the layer (PI-1) was 33.2 μm.
[0220] (5) Comparative Example 1 The PI resin precursor solution 3 was applied to the roughened surface (surface roughness; Rz = 0.6 μm) of an electrolytic copper foil (thickness 12 μm) so that the dry thickness was 5 μm, to obtain a coating film. The coating film was heated and dried at 120 ° C for 10 minutes, and the PI resin precursor solution 1 was applied to the dried coating film so that the dry thickness was 36 μm, to obtain a two-layer laminate coating film. The two-layer laminate coating film was heated and dried at 120 ° C for 30 minutes, and the PI resin precursor solution 3 was applied to the dried two-layer laminate coating film so that the dry thickness was 5 μm, to obtain a three-layer laminate coating film. The three-layer laminate coating film was heated and dried at 120 ° C for 30 minutes. Thereafter, the laminate consisting of the copper foil and the three-layer laminate coating film was fixed to a metal frame, and the temperature was raised from 30 ° C to 320 ° C over 10 minutes in an oxygen concentration 1% atmosphere, and then held at 320 ° C for 5 minutes. The obtained laminated film with copper foil, consisting of a PI resin-containing layer and a copper foil, was immersed in a large amount of 40% by mass aqueous ferric chloride solution at room temperature for 10 minutes, and then the aqueous ferric chloride solution was washed with pure water. After visually confirming that no copper remained, the film was dried at 80°C for 1 hour to obtain a laminated film 5 consisting of a layer (PI-2) (copper foil layer side), a layer (PI-1) and a layer (PI-3) (TPI layer, mPI layer and TPI layer) laminated in this order. The thickness of the laminated film 5 was 46 μm, the thickness of the intermediate region between the layer (PI-2) and the layer (PI-1) was 250 nm, the thicknesses of the layer (PI-2) and the layer (PI-3) were 4.9 μm, and the thickness of the layer (PI-1) was 35.8 μm.
[0221] Measurements and evaluations were carried out on the laminated films 1 to 5 obtained in the examples and comparative examples. The measurement and evaluation methods are explained below.
[0222] <Film thickness measurement> From each of the laminate films 1 to 5 obtained in the examples and comparative examples, a 5 mm×5 mm portion was cut out and embedded in resin to prepare a film thickness measurement sample. The prepared film thickness measurement sample was cut with a microtome to prepare a measurement cross section, and the thickness of the laminate film was measured under the following conditions using a laser microscope. Equipment: Olympus Corporation LEXT OLS4100 Observation magnification: 100x
[0223] <Measurement of Df and Dk> From the laminated films 1 to 5 obtained in the examples and comparative examples, measurement samples of 50 mm × 50 mm were cut out respectively, and Df and Dk were measured under the following conditions. The measurement was carried out after conditioning the measurement samples at 23°C / 50%RH for 24 hours. Apparatus: Compact USB Vector Network Analyzer (product name: MS46122B) manufactured by Anritsu Corporation Cavity resonator (TE mode 10 GHz type) manufactured by A&T Co., Ltd. Measurement frequency: 10 GHz Measurement atmosphere: 23°C / 50%RH
[0224] <Measurement of Coefficient of Thermal Expansion (CTE)> The CTE of the laminated films 1 to 5 obtained in the examples and comparative examples was measured under the following conditions using a thermomechanical analyzer TMA, and the CTE from 50°C to 100°C was calculated. Apparatus: TMA / SS7100 manufactured by Hitachi High-Tech Science Corporation Load: 50.0 mN Temperature program: Heating from 20°C to 130°C at a rate of 5°C / min Test piece: Length 40 mm, width 5 mm
[0225] <Measurement of Storage Elastic Modulus> The storage elastic modulus of each PI-based resin formed from the above PI-based resin precursor solutions 1 to 5 was determined by measuring the PI-based resin films prepared by the following method under the following conditions. Each PI-based resin precursor solution was cast on a glass substrate so that the dry thickness became 30 μm to form a coating film of the PI-based resin precursor solution. The coating film was heated at 120°C for 30 minutes, and after the obtained film was peeled off from the glass substrate, the film was fixed to a gold frame. The film fixed to the gold frame was heated from 30°C to 320°C over 10 minutes in an atmosphere with an oxygen concentration of 1%, and then maintained at 320°C for 5 minutes to obtain a PI-based resin film. The storage modulus (E') was obtained by measuring the dynamic viscoelasticity using a dynamic viscoelasticity measuring device (IT Measurement and Control Co., Ltd., DVA-220) under the following samples and conditions. Test piece: 40 mm long, 5 mm wide, 30 μm thick rectangular prism Experimental mode: Single frequency, constant temperature rise Experimental method: Tensile Sample gripping length: 15mm Measurement start temperature: Room temperature ~ 342℃ Heating rate: 5℃ / min Frequency: 10Hz Static / dynamic stress ratio: 1.8 As a result of the measurement by the above method, the storage modulus of the PI resin film formed from the PI resin precursor solution 1 at 40 °C was 2.3 × 10 9 Pa, storage modulus at 300°C is 2.8×10 8 The PI resin film formed from the PI resin precursor solution 2 had a storage modulus of 2.3 × 10 Pa at 40 °C. 9 Pa, storage modulus at 300°C is 1.2×10 7 The PI resin film formed from the PI resin precursor solution 3 had a storage modulus of 2.4 × 10 Pa at 40 °C. 9 Pa, storage modulus at 300°C is 1.1×10 7 The PI resin film formed from the PI resin precursor solution 4 had a storage modulus of 4.3 × 10 Pa at 40 °C. 9 Pa, storage modulus at 300°C is 3.0×10 8 The PI resin film formed from the PI resin precursor solution 5 had a storage modulus of 7.5 × 10 Pa at 40 °C. 9 Pa, storage modulus at 300°C is 4.8×10 8 It was Pa. The laminate films consisting of three PI resin-containing layers obtained in Examples 1 to 5 and Comparative Example 1 were layer (PI-2), layer (PI-1), and layer (PI-3) on the copper foil side, in that order, and were confirmed to be a TPI layer / mPI layer / TPI layer.
[0226] <Measurement of puncture strength> The puncture strength of the laminated films 1 to 5 obtained in the examples and comparative examples was measured in accordance with JIS Z 1707 under an environment of 23°C temperature and 50% relative humidity using a small tabletop tester EZ-LX manufactured by Shimadzu Corporation. Specifically, using a test piece with a width of 50 mm and a length of 50 mm, a test was performed under the conditions of a load cell of 50 N and a test speed of 200 mm / min using a pressure probe of a needle with a diameter of 2.5 mm and a semicircular tip shape of 0.5 mm, and the fracture displacement was measured, and the maximum load at that time was taken as the puncture strength. The puncture strength was measured from the layer (PI-2) (TPI layer) side.
[0227] <Scanning Probe Microscope (SPM) Measurements> (Creating test pieces) A part of each of the laminated films 1 to 5 obtained in the examples and comparative examples was cut and embedded in resin so that the cross section in the thickness direction could be seen. Next, a glass knife was attached to an ultramicrotome (Leica, "Leica EM UC7"), and the blade was scanned in a direction perpendicular to the surface of the laminated film, and after reaching the surface of the resin-embedded film, 100 μm or more was cut in the depth direction of the test piece (plane direction relative to the laminated film). Then, a SYM knife (Syntec, "SYM2045 Ultra") was attached, and further cutting was performed by 1 μm or more. The cut cross section was used as the observation surface, and the obtained test piece (sample) was set in an SPM (Bruker, Dimension Icon). The cut cross section (observation surface) includes layer (PI-2) (TPI layer), layer (PI-1) (mPI layer), and layer (PI-3) (TPI layer).
[0228] (Acquisition of elastic modulus image by SPM) The mechanical properties of the sample cross section were evaluated under the following conditions, and the DMT elastic modulus (GPa) was calculated based on the DMT (Derjaguim-Muller-Toporov) theory, and a DMT elastic modulus image was obtained.
[0229] Specifically, first, the displacement of the piezo scanner and the warp of the cantilever were measured during the process of contact between the cantilever and the sample, and a curve (force curve) showing the relationship between the load F and the sample deformation δ was obtained. For each measurement point, the indentation process (the process in which the cantilever is pressed into the sample until it reaches the maximum load after the cantilever contacts the sample, the process from point A to point B to point C as shown in Figure 1) and the pullback process (the process from the point at which the cantilever is pressed into the sample until it is completely separated from the sample surface, the process from point C to point D to point E as shown in Figure 1) of the obtained force curve were analyzed using the DMT theoretical formula to obtain the DMT elastic modulus in each process.
[0230] In the analysis, analysis software (NanoScope Analysis ver.2.00) was used, and when the numerical values from the minimum to the maximum F value in the pullback process of the force curve were replaced with numerical values from 0 to 1, fitting was performed for the range from 0.05 to 0.7, and the DMT elastic modulus was calculated. The DMT elastic modulus in the pullback process was calculated at 512 points horizontally by 512 points vertically in a range of 10 μm × 10 μm on the sample cross section, and a DMT elastic modulus image in which this was stored was obtained. Similarly, fitting was performed in the indentation process of the force curve, and the DMT elastic modulus in the indentation process was calculated at 512 points horizontally by 512 points vertically in a range of 10 μm × 10 μm on the sample cross section, and a DMT elastic modulus image in which this was stored was obtained. The cantilever used was an RTESPA300 (manufactured by Bruker; nominal spring constant 40 N / m, nominal tip radius 8 nm). The cantilever spring constant was calculated using the Sader Method (reference A) built into the SPM device. The tip radius of the cantilever was calculated using the Reconstruction method (reference B) built into the SPM device at a position 2 nm above the tip. The force curve was acquired in Peak Force QNM (Quantitative Nanomechanical Mapping) mode, with the measurement location set so that the interface was located at the center, the layer (PI-2) was located above the center, and the layer (PI-1) was located below the center, as shown in Figure 2. The measurement conditions are shown below.
[0231] (Reference A) Sader JE, Sanelli JA, Adamson BD, Monty JP, Wei X ., Crawford SA, Rev. Sci. Instrum., 2012, Vol. 83, pp. 103705-1 to 103705-16 (Document B)ISO13095:2014
[0232] Equipment :Dimension Icon (Bruker) Cantilever: RTESPA-300 (Bruker) Measurement mode: Peak Force QNM Measurement atmosphere: 24℃ / atmosphere Measurement range: 10 μm x 10 μm (including the lower and middle layers on the copper foil side) Resolution: 512×512pixel(19.53nm / pixel) Cantilever movement speed: 0.4 μm / s Maximum load: 40nN Peak Force Frequency: 1kHz Peak Force Amplitude: 30 nm Feedback Gain:Auto
[0233] (Calculation of (E1r-E1a) / (E2r-E2a)) The upper left corner of the DMT elastic modulus image obtained in each process was set to (X,Y) = (0,0), the lower left corner was set to (X,Y) = (0,511), the upper right corner was set to (X,Y) = (511,0), and the lower right corner was set to (X,Y) = (511,511), and the average of the DMT elastic modulus values of 512 × 100 points from (0,0) to (511,99) was defined as the average DMT elastic modulus of the layer (PI-2) in each process (average elastic modulus measured by SPM). In addition, the average of the DMT elastic modulus values of 512 × 100 points from (X,Y) = (0,412) to (511,511) in the DMT elastic modulus image in each process was defined as the average DMT elastic modulus of the layer (PI-1) in each process (average elastic modulus measured by SPM). The average elastic modulus of layer (PI-1) during the pull-back process obtained as described above was defined as E1r, the average elastic modulus of layer (PI-1) during the push-in process was defined as E1a, the average elastic modulus of layer (PI-2) during the pull-back process was defined as E2r, and the average elastic modulus of layer (PI-2) during the push-in process was defined as E2a, and (E1r-E1a) / (E2r-E2a) was calculated.
[0234] (Calculation of the intermediate area and its thickness) In the DMT elastic modulus images obtained above during the pullback process, DMT elastic modulus profiles corresponding to Y = 0 to 511 were obtained when X = 50, 150, 250, 350, and 450, respectively. Specifically, the DMT elastic modulus at X = 50 and Y = 0 to 511 [(X,Y) = (50,0) to (50,511)] in the DMT elastic modulus images during the pullback process was plotted on the vertical axis and the corresponding Y (Y coordinate) on the horizontal axis to obtain a DMT elastic modulus profile at X = 50. This DMT elastic modulus profile was also created for X = 150, 250, 350, and 450. Next, for the five DMT elastic modulus profiles, the average value of the DMT elastic modulus was calculated for each Y value (0 to 511 of the Y coordinate) of the DMT elastic modulus image, and an average DMT elastic modulus profile was created. Further, in the average DMT elastic modulus profile, when n was an arbitrary value from 0 to 511 and Y = n, the average of the DMT elastic modulus at nine points from n - 4 to n + 4 was taken and used as the DMT elastic modulus value at Y = n (4 < n < 508) (a nine-point moving average line of the average DMT elastic modulus profile was created). In this line, the region that continuously changes from the average DMT elastic modulus of layer (PI-1) (average elastic modulus measured by SPM: E1r) to the average DMT elastic modulus of layer (PI-2) (average elastic modulus measured by SPM: E2r) was defined as the intermediate region, and the Y value width of this region was defined as the thickness of the intermediate region. At this time, by dividing the Y value width (pixel) by 19.53 pixel / nm, the conversion from pixel units to nm units was performed.
[0235] (Calculation of the thicknesses of layers (PI-1) to (PI-3)) From the surface of layer (PI-2) (TPI layer) to the interface between layer (PI-2) and the intermediate region, it was defined as layer (PI-2), and their distance was calculated as the thickness (nm) of layer (PI-2). Also, the thickness of the intermediate region between layer (PI-3) (the other TPI layer) and layer (PI-1) (mPI layer) and layer (PI-3) was calculated by the same analysis as above. The thickness of layer (PI-1) (mPI layer) was calculated by subtracting the thicknesses of layer (PI-2), layer (PI-3), and the two intermediate regions from the thickness (total thickness) of the laminated film obtained by the above laser microscope.
[0236] <Measurement of the burr height in the drilled part> Test pieces of 3 cm × 5 cm were cut out from the laminated films obtained in Examples 2 to 4, and were firmly fixed with tape to a polystyrene foam board with the layer (PI-2) (TPI layer) side facing up. A drill bit with a diameter of φ1 mm was attached to a drill (GBM 13 RE) manufactured by BOSCH, and a through-hole was drilled from directly above the laminated film under the condition of a rotation speed of 2,600 min-1. The through holes drilled on the layer (PI-2) (TPI layer) side of the laminated film were observed under the following conditions using a laser microscope (Olympus Corporation, LEXT OLS4100), and the height of the burrs around the through holes (height from the laminated film surface) was measured at five points on each sample, and the average value was calculated. The burr height was measured using the line roughness measurement function of the OLS4100. The burr heights in Examples 2 to 4 were 204 μm, 174 μm, and 197 μm, respectively. Observation magnification: 5x Cutoff: λc:80μm Filter: Gaussian filter
[0237] The results of the above measurements are shown in Table 1. In Table 1, the puncture strength is a value calculated based on the thickness of the laminated film being 50 μm.
[0238] [Table 1]
[0239] As shown in Table 1, it was confirmed that the laminated films obtained in Examples 1 to 4 had higher puncture strength than the laminated film of Comparative Example 1. [Explanation of symbols]
[0240] 1: Laminated film 2: Laminated sheet 11: Polyimide resin-containing layer (corresponding to layer (PI-2)) 12: Polyimide resin-containing layer (corresponding to layer (PI-1)) 13: Polyimide resin-containing layer (corresponding to layer (PI-3)) 21: Metal foil layer
Claims
1. A laminated film including a polyimide-based resin-containing layer (PI-1) and a polyimide-based resin-containing layer (PI-2), The average elastic modulus of the layer (PI-1) and the layer (PI-2) measured by a scanning probe microscope in a cross section in the thickness direction of the laminate film is represented by the formula (I): (E1r-E1a) / (E2r-E2a)≧1.00 (I) [wherein E1r represents the average elastic modulus of the layer (PI-1) during the pulling back process of the cantilever probe, E1a represents the average elastic modulus of the layer (PI-1) during the pressing process of the cantilever probe, E2r represents the average elastic modulus of the layer (PI-2) during the pulling back process, and E2a represents the average elastic modulus of the layer (PI-2) during the pressing process, E1r-E1a>0, and E2r-E2a>0] Laminated film that satisfies the above requirements.
2. In formula (I), 0.30 GPa≦E2r−E2a≦1.50 GPa The laminated film according to claim 1 , which satisfies the following relationship:
3. An intermediate region is provided between the layer (PI-1) and the layer (PI-2), the intermediate region is a region in which, when the elastic modulus of the laminate film is continuously measured along the thickness direction in a cross section of the laminate film in the process of pulling back a cantilever probe by a scanning probe microscope, the elastic modulus changes continuously from E1r to E2r, The laminated film according to claim 1 or 2, wherein the thickness of the intermediate region is 50 nm or more.
4. The laminate film according to claim 1 or 2, further comprising a polyimide-based resin-containing layer (PI-3).
5. At least one of the polyimide-based resin-containing layer (PI-1) and the polyimide-based resin-containing layer (PI-2) contains a polyimide-based resin having a structural unit (A) derived from a tetracarboxylic acid anhydride, The structural unit (A) is represented by the formula (A1): [Formula 1] [In formula (A1), R a1 each independently represents a halogen atom, or an alkyl group, an alkoxy group, an aryl group, or an aryloxy group which may have a halogen atom; k represents an integer of 0 to 2. A structural unit (A1) derived from a tetracarboxylic acid anhydride represented by the formula (A2): [Case 2] [In formula (A2), R a2 each independently represents a halogen atom, or an alkyl group, an alkoxy group, an aryl group, or an aryloxy group which may have a halogen atom, and each 1 independently represents an integer of 0 to 3. The laminate film according to claim 1 or 2, comprising a structural unit (A2) derived from a tetracarboxylic acid anhydride represented by the following formula:
6. At least one of the polyimide-based resin-containing layer (PI-1) and the polyimide-based resin-containing layer (PI-2) contains a polyimide-based resin having a structural unit (B) derived from a diamine, The structural unit (B) is represented by the formula (B1): [C3] [In formula (B1), R b1 each independently represents a halogen atom, or an alkyl group, an alkoxy group, an aryl group, or an aryloxy group which may have a halogen atom; Each W is independently -O-, -CH 2 --, --CH 2 -CH 2 -, -CH(CH 3 ) -, -C(CH 3 ) 2 -, -C(CF 3 ) 2 -, -COO-, -OOC-, -SO-, -SO 2 -, -S-, -CO-, -N(R ca divalent linking group selected from the group consisting of - and -CONH-, or a single bond (wherein m is 2 or more and at least one W is the divalent linking group); R c represents a hydrogen atom or a monovalent hydrocarbon group having 1 to 12 carbon atoms which may be substituted with a halogen atom, m represents an integer of 1 to 4; and q each independently represents an integer of 0 to 4. The laminate film according to claim 1 or 2, comprising a structural unit (B1) derived from a diamine represented by the following formula:
7. The polyimide-based resin-containing layer (PI-1) and the polyimide-based resin-containing layer (PI-2) each contain a polyimide-based resin having a tetracarboxylic acid anhydride-derived structural unit (A) and a diamine-derived structural unit (B), The structural unit (A) is represented by the formula (A1): [C4] [In formula (A1), R a1 each independently represents a halogen atom, or an alkyl group, an alkoxy group, an aryl group, or an aryloxy group which may have a halogen atom; k represents an integer of 0 to 2. A structural unit (A1) derived from a tetracarboxylic acid anhydride represented by the formula (A2): [C5] [In formula (A2), R a2 each independently represents a halogen atom, or an alkyl group, an alkoxy group, an aryl group, or an aryloxy group which may have a halogen atom, and each 1 independently represents an integer of 0 to 3. The structural unit (A2) is derived from a tetracarboxylic acid anhydride represented by the formula: The structural unit (B) is represented by the formula (B1): [C6] [In formula (B1), R b1 each independently represents a halogen atom, or an alkyl group, an alkoxy group, an aryl group, or an aryloxy group which may have a halogen atom; Each W is independently -O-, -CH 2 --, --CH 2 -CH 2 -, -CH(CH 3 ) -, -C(CH 3 ) 2 -, -C(CF 3 ) 2 -, -COO-, -OOC-, -SO-, -SO 2 -, -S-, -CO-, -N(R c a divalent linking group selected from the group consisting of - and -CONH-, or a single bond (wherein m is 2 or more and at least one W is the divalent linking group); R c represents a hydrogen atom or a monovalent hydrocarbon group having 1 to 12 carbon atoms which may be substituted with a halogen atom, m represents an integer of 1 to 4; and q each independently represents an integer of 0 to 4. The laminate film according to claim 1 or 2, comprising a structural unit (B1) derived from a diamine represented by the following formula:
8. At least the structural unit (A) contained in the polyimide-based resin contained in the polyimide-based resin-containing layer (PI-1) further contains 45 mol % or less of the structural unit (A) represented by the formula (A3): [C7] In formula (A3), Z represents a divalent organic group, R a3 each independently represents a halogen atom, or an alkyl group, an alkoxy group, an aryl group, or an aryloxy group which may have a halogen atom; Each s independently represents an integer of 0 to 3. The laminate film according to claim 7, further comprising a structural unit (A3) derived from an ester bond-containing tetracarboxylic acid anhydride represented by the following formula:
9. A laminate sheet comprising a metal foil layer on one or both sides of the laminate film according to claim 1 or 2.
10. A flexible printed circuit board comprising the laminate sheet according to claim 9.
Citation Information
Patent Citations
Flexible copper-clad laminate, flexible circuit board and use thereof
JP2015088631A
Polyimide system adhesive
JP2021161285A