Cellulose particles and method for producing cellulose particles
Cellulose particles with a comprehensive coating layer covering 60% to 100% of the base particles, excluding coupling agents, enhance impact resistance and maintain smoothness, addressing the inadequacies of conventional cellulose particles in molded products.
Patent Information
- Application Number
- JP2023163847
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2023-03-28
- Filing Date
- 2023-09-26
- Publication Date
- 2024-10-11
AI Technical Summary
Conventional cellulose particles with coating layers exhibit insufficient impact resistance, leading to potential cracking, chipping, or breaking of molded products due to exposure of hard base particles when impacted.
Cellulose particles with a coating layer covering 60% to 100% of the base particles, using a coating material that excludes coupling agents, and optionally including an intermediate layer, to enhance impact resistance.
The described cellulose particles provide superior impact resistance to molded products by minimizing exposure of hard base particles, improving cushioning and maintaining a smooth, moist skin feel.
Smart Images

Figure 2024144020000001 
Figure 2024144020000002 
Figure 2024144020000003
Abstract
Description
[Technical field]
[0001] The present invention relates to cellulose particles and a method for producing cellulose particles. [Background technology]
[0002] Patent Document 1 describes a hydrophobic cellulose powder, which is characterized in that a cellulose powder made of regenerated cellulose having a crystalline structure of cellulose II type is surface-coated with a compound represented by the following general formula (1) in an amount of 0.5 to 30% by weight. R1CH2CH2Si(OR2)3·········(1) (wherein R1 is a saturated hydrocarbon group having one or more carbon atoms or a saturated fluorocarbon group having one or more carbon atoms, and R2 is a saturated hydrocarbon group having one or more carbon atoms) has been proposed.
[0003] Patent Document 2 proposes "an average particle size D50 of 1 μm or more and 50 μm or less, a bulk density of 0.30 g / mL or less, and a specific volume of."
[0004] Patent Document 3 proposes "resin beads obtained by surface-treating core beads formed of a resin whose main component is cellulose with a surface treatment agent, the resin beads having a volume-based cumulative 50% particle size of 50 μm or less, a sphericity of 0.7 to 1.0, a surface smoothness of 70 to 100%, and a crystallinity of 60% or less." [Prior art documents] [Patent documents]
[0005] [Patent Document 1] Patent No. 4897289 [Patent Document 2] Patent Publication No. 2022-099605 Summary of the Invention [Problem to be solved by the invention]
[0006] The object of the present invention is to provide cellulose particles having base particles mainly composed of cellulose and a coating layer that coats the base particles and contains a coating material excluding a coupling agent, which results in a molded product with superior impact resistance compared to cellulose particles in which the coating layer has a coverage rate of less than 60% relative to the base particles. [Means for solving the problem]
[0007] Means for solving the above problems include the following aspects. <1> A base particle mainly composed of cellulose; a coating layer that coats the base particles and contains a coating material excluding a coupling agent; having The cellulose particles have a coverage rate of the coating layer relative to the base particles of 60% or more and 100% or less. <2> The coverage of the coating layer with respect to the base particles is 80% or more and 100% or less. <1> The cellulose particles according to claim 1. <3> The coverage of the coating layer with respect to the base particles is 90% or more and 100% or less. <2> The cellulose particles according to claim 1. <4> The amount of the coating layer relative to the base particles is 1% by mass or more and 40% by mass or less. <1> ~ <3> of 3. The cellulose particles according to claim 1 . <5> The amount of the coating layer relative to the base particles is 3% by mass or more and 30% by mass or less. <4> The cellulose particles according to claim 1. <6> The volume average particle size is 1 μm or more and 100 μm or less. <1> ~ <5> The cellulose particles according to any one of claims 1 to 5. <7> The coating layer contains at least one coating material selected from the group consisting of fatty acids, fatty acid metal salts, and amino acid compounds. <1> ~ <6> The cellulose particles according to any one of claims 1 to 5. <8> The fatty acid is at least one selected from the group consisting of straight-chain fatty acids and hydroxy fatty acids; The fatty acid metal salt is a straight chain fatty acid metal salt. <7> The cellulose particles according to claim 1. <9> An intermediate layer is provided between the base particles and the coating layer. <1> ~ <8> The cellulose particles according to any one of claims 1 to 5. <10> The intermediate layer contains at least one intermediate material selected from the group consisting of a polyamine compound, a polyquaternium, a polysaccharide compound, and a polyacrylic acid. <9> The cellulose particles according to claim 1. <11> obtaining base particles mainly composed of cellulose; coating the base particles with a coating material excluding a coupling agent; Including, the amount of the coating layer relative to the base particle is 1% by mass or more and 40% by mass or less, A method for producing cellulose particles, wherein a coverage rate of the coating layer with respect to the base particles is 60% or more and 100% or less. Effect of the Invention
[0008] <1> According to the invention, in cellulose particles having base particles mainly composed of cellulose and a coating layer that coats the base particles and contains a coating material excluding a coupling agent, the cellulose particles have excellent impact resistance of molded products compared to when the coating layer has a coverage rate of less than 60% with respect to the base particles. <2> According to the present invention, there are provided cellulose particles which give molded products with superior impact resistance, as compared with cases where the coverage rate of the coating layer with respect to the base particles is less than 80%. <3> According to the present invention, there are provided cellulose particles which have excellent impact resistance when molded, as compared with a case where the coverage rate of the coating layer with respect to the base particles is less than 90%. <4> According to the present invention, there are provided cellulose particles which give molded products with superior impact resistance, as compared with cases where the amount of the coating layer relative to the base particles is less than 1% by mass or more than 40% by mass. According to the invention related to 5), there are provided cellulose particles which give molded products having superior impact resistance, compared with cases in which the amount of the coating layer relative to the base particles is less than 3% by mass or more than 30% by mass. <6> According to the present invention, there is provided cellulose particles which give molded products with superior impact resistance compared to those having a volume average particle size of less than 1 μm or more than 100 μm. <7> According to the present invention, there are provided cellulose particles which provide molded products with superior impact resistance compared to those in which the coating layer contains a lipid compound. <8> According to the present invention, there are provided cellulose particles which give molded products with superior impact resistance compared to those in which the fatty acid is a branched fatty acid or the fatty acid metal salt is a branched fatty acid metal salt. <9> According to the present invention, there are provided cellulose particles which provide molded products with superior impact resistance compared to those having no intermediate layer between the base particles and the coating layer. <10> According to the present invention, there are provided cellulose particles which provide molded products with superior impact resistance compared to those in which the intermediate layer contains arginine or dextrin. <11> According to the invention, in a method for producing cellulose particles, which includes a step of obtaining base particles mainly composed of cellulose and a step of coating the base particles with a coating material excluding a coupling agent, a method for producing cellulose particles is provided in which the impact resistance of the molded product is superior to that when the amount of coating layer on the base particles is less than 1% by mass or exceeds 40% by mass, or when the coverage rate of the coating layer on the base particles is less than 60% or exceeds 100%. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0009] Hereinafter, an embodiment of the present invention will be described as an example. The description and examples are merely illustrative of the embodiment, and are not intended to limit the scope of the present invention. In the numerical ranges described in this specification, the upper or lower limit value described in one numerical range may be replaced with the upper or lower limit value of another numerical range described in another stepwise manner. In addition, in the numerical ranges described in this specification, the upper or lower limit value of the numerical range may be replaced with a value shown in the examples.
[0010] Each component may contain multiple types of the corresponding substance. When referring to the amount of each component in a composition, if the composition contains multiple substances corresponding to each component, the amount refers to the total amount of those multiple substances present in the composition, unless otherwise specified.
[0011] <Cellulose particles> The cellulose particles according to this embodiment have base particles containing cellulose as a main component, and a coating layer that coats the base particles and contains a coating material excluding a coupling agent. The coverage of the coating layer with respect to the base particles is 60% or more and 100% or less. Here, the coupling agent is a compound having an alkoxy group directly bonded to a metal element (metal element such as Si, Ti, or Al), and is a compound that undergoes a hydrolysis reaction and a condensation reaction.
[0012] The cellulose particles according to the present embodiment, due to the above-mentioned constitution, provide molded products with excellent impact resistance. The reason for this is presumed to be as follows.
[0013] Cellulose particles are expected to be a substitute for resin particles in various fields, including cosmetics, due to their high biodegradability and durability. In addition, various functions are required for cellulose particles as the products for each application become more highly functional.
[0014] The function is the impact resistance of the cellulose particles alone or of a molded product containing the cellulose particles. However, the impact resistance of conventional cellulose particles alone having a coating layer or of a molded product containing the cellulose particles is not sufficient, and when the molded product is dropped, the molded product may crack, chip, or break. This is thought to be because the coverage of the coating layer is low, exposing the hard base particles (i.e., hard cellulose), and when an impact is applied to the exposed part, the impact is transmitted to the cellulose particles, causing the molded product to crack, chip, or break.
[0015] Therefore, in the cellulose particles according to the present embodiment, the coverage of the coating layer on the base particles mainly composed of cellulose is set to 60% or more and 100% or less, so that the base particles (i.e., cellulose) are less likely to be exposed from the coating layer, and even if the molded product receives an impact, the coating layer of the cellulose particles can fully exhibit the function of cushioning the impact.
[0016] From the above, it is presumed that the cellulose particles according to this embodiment will result in molded articles with excellent impact resistance. Furthermore, in the cellulose particles of this embodiment, since the base particles (i.e., cellulose) are less likely to be exposed from the coating layer, the skin feel resulting from the hardness of the cellulose particles themselves is concealed, and the skin feel, such as moistness and smoothness, resulting from the coating layer is improved, making the particles suitable for use in cosmetics.
[0017] (Coverage rate of coating layer) In the cellulose particles according to this embodiment, the coverage of the coating layer with respect to the base particle is 60% or more and 100% or less, preferably 80% or more and 100% or less, and more preferably 90% or more and 100% or less. If the coverage rate of the coating layer is less than 60%, the hard base particles (that is, hard cellulose) are exposed in a large area, and the impact resistance of the molded product decreases.
[0018] The method for measuring the coverage of the coating layer is as follows. The target cellulose particles are stained with ruthenium. When observed under a scanning electron microscope (SEM), the coating layer appears black due to the ruthenium staining. The ruthenium-stained cellulose particles are observed under an SEM at a magnification of 3,500 times, and the ratio of the area of the observed black coating layer to the area of one observed cellulose particle is calculated. This operation is carried out for 50 cellulose particles, and the arithmetic mean value of the proportion of the area of the resulting coating layer is calculated, which is defined as the coverage rate of the coating layer.
[0019] (base particle) The base particles are particles on which a coating layer is to be formed, and contain cellulose as a main component. Here, "containing cellulose as a main component" means that the content of cellulose in the base particle is 90% by mass or more (preferably 95% by mass or more, 98% by mass or more, or 100% by mass).
[0020] The number average molecular weight of the cellulose is preferably 37,000 or more, and more preferably 45,000 or more. The upper limit of the number average molecular weight of the cellulose is not particularly limited, but may be, for example, 100,000 or less.
[0021] The moist feeling and smoothness are enhanced by setting the number average molecular weight of cellulose to 37,000 or more. The reason for this is presumed to be as follows. When the number average molecular weight is 37,000 or more, the increase in terminal hydroxyl groups is suppressed, the number of hydroxyl groups per unit volume is reduced, and the number and bond strength of intramolecular and extramolecular hydrogen bonds are reduced, which results in increased flexibility of the cellulose particles and facilitates improved moist feeling and smoothness.
[0022] The number average molecular weight of cellulose was measured by gel permeation chromatography (differential refractometer Optilab T-rEX / Wyatt Technology, multi-angle light scattering detector) The measurement is performed using a DAWN HELEOS II (Wyatt Technology) and columns (TSKgel α-M, α-3000, Tosoh) in dimethylacetamide (with 0.1M lithium chloride added) as the solvent.
[0023] -Other ingredients- The base particles may contain other components. Examples of other components include plasticizers, flame retardants, compatibilizers, release agents, light resistance agents, weather resistance agents, colorants, pigments, modifiers, anti-drip agents, antistatic agents, hydrolysis inhibitors, fillers, reinforcing agents (glass fibers, carbon fibers, talc, clay, mica, glass flakes, milled glass, glass beads, crystalline silica, alumina, silicon nitride, aluminum nitride, boron nitride, etc.), acid acceptors for preventing release of acetic acid (oxides such as magnesium oxide and aluminum oxide; metal hydroxides such as magnesium hydroxide, calcium hydroxide, aluminum hydroxide, and hydrotalcite; calcium carbonate; talc; etc.), and reactive trapping agents (for example, epoxy compounds, acid anhydride compounds, carbodiimides, etc.). The content of each of the other components is preferably 0% by mass or more and 5% by mass or less based on the total amount of the base particles, where "0% by mass" means that no other components are included.
[0024] (Cellulose particles having a coating layer) The coating layer preferably contains a coating material selected from hydrophobic compounds. Specifically, the coating layer preferably contains at least one coating material selected from the group consisting of fatty acids, fatty acid metal salts, and amino acid compounds. These coating materials increase the hydrophobicity of the coating layer, as well as flexibility and improve the impact resistance of the molded product. They also improve the moist feeling and smoothness.
[0025] ·fatty acid The fatty acids are linear or branched, saturated or unsaturated fatty acids. The fatty acids may also be mixtures of saturated and unsaturated fatty acids. The fatty acid is preferably a fatty acid having 14 to 22 carbon atoms (preferably 14 to 20 carbon atoms). Specific examples of linear fatty acids having 14 to 22 carbon atoms include behenic acid, arachidic acid, palmitic acid, stearic acid, isostearic acid, and myristic acid.
[0026] Fatty acid metal salts The fatty acid metal salt is a metal salt of a linear or branched, saturated or unsaturated fatty acid. The fatty acid metal salt may be a mixture of a saturated fatty acid metal salt and an unsaturated fatty acid metal salt. From the viewpoint of improving water repellency against high-temperature hot water and maintaining moist feeling, examples of the fatty acid metal salt include metal salts of fatty acids having 14 to 22 carbon atoms (preferably having 14 to 20 carbon atoms). Examples of the metal salts of fatty acids having 14 to 22 carbon atoms include metal salts of stearic acid, metal salts of behenic acid, palmitic acid, and myristic acid. The metal in the fatty acid metal salt may be a divalent metal. Examples of metals in fatty acid metal salts include magnesium, calcium, aluminum, barium, and zinc.
[0027] Among these, from the viewpoint of improving the impact resistance, moist feeling, and smoothness of the molded product, the fatty acid is preferably at least one selected from the group consisting of straight-chain fatty acids and hydroxy fatty acids, and the fatty acid metal salt is preferably a straight-chain fatty acid metal salt. It is presumed that these fatty acids and fatty acid salts are fixed by the affinity between the terminal carboxylic acid and the hydroxyl group, and form a sponge-like structure due to the repulsion between the outward-facing aliphatic groups. Therefore, the impact resistance, moist feeling, and smoothness of the molded product are easily improved.
[0028] Amino acid compounds The amino acid compound refers to amino acids and amino acid derivatives. Examples of the amino acid compound include lauroyl lysine, lauryl arginine, myristyl leucine, and stearoyl glutamic acid.
[0029] The coating material constituting the coating layer is not limited to the above-mentioned coating materials, and examples thereof include coating materials of lipid compounds (phospholipids, etc.), silicone compounds (dimethylsiloxane, hydrogen dimethicone, etc.), fluorinated compounds (perfluoropolyether, perfluorooctyltriethoxysilane, etc.), and ceramide compounds (hydroxypropylbispalmitamide MEA, etc.).
[0030] The amount of the coating layer on the base particles is preferably from 1% by mass to 40% by mass, more preferably from 3% by mass to 30% by mass, and even more preferably from 10% by mass to 30% by mass, from the viewpoint of improving the impact resistance, moist feel, and smoothness of the molded product. Here, the content of the coating material in the entire coating layer is preferably 90% by mass or more and 100% by mass or less, and more preferably 95% by mass or more and 100% by mass or less.
[0031] -Middle class- In the cellulose particles having a coating layer, it is preferable that an intermediate layer is provided between the base particle and the coating layer, and the intermediate layer preferably contains at least one intermediate material selected from the group consisting of a polyamine compound, a polyquaternium, a polysaccharide compound, and a polyacrylic acid.
[0032] In the cellulose particles according to the present embodiment, by providing an intermediate layer between the base particle and the coating layer, peeling of the coating layer is suppressed, and the impact resistance, moist feeling, and smoothness of the molded product are easily improved. In particular, the intermediate material enhances the adhesion between the cellulose base particle and the coating layer containing the coating material, and the impact resistance, moist feeling, and smoothness of the molded product are easily improved.
[0033] A polyamine compound is a general term for an aliphatic hydrocarbon having two or more primary amino groups. Examples of the polyamine compound include polyalkyleneimine, polyallylamine, polyvinylamine, and polylysine. From the viewpoint of improving biodegradability, the polyalkyleneimine is preferably a polyalkyleneimine having a structural unit with an alkylene group having 1 to 6 carbon atoms (preferably 1 to 4 carbon atoms, more preferably 1 to 2 carbon atoms), and more preferably polyethyleneimine. Examples of polyallylamine include homopolymers or copolymers of allylamine, allylamine amide sulfate, diallylamine, dimethylallylamine, and the like. An example of the polyvinylamine is one produced by hydrolyzing poly(N-vinylformamide) with an alkali, and a specific example thereof is "PVAM-0595B" manufactured by Mitsubishi Chemical Corporation. The polylysine may be one extracted from a natural product, one produced by a transformed microorganism, or one chemically synthesized.
[0034] Examples of polyquaterniums include polyquaternium-6, polyquaternium-7, polyquaternium-10, polyquaternium-11, polyquaternium-51, polyquaternium-61, and polyquaternium-64. The content of the polyquaternium is preferably 0.2% by mass or more and 2% by mass or less based on the total mass of the cellulose particles.
[0035] The coverage of the intermediate layer on the base particles is preferably from 0.1 to 20% by mass, more preferably from 0.2 to 2% by mass, from the viewpoint of improving the impact resistance, moist feel, and smoothness of the molded product. The content of the intermediate material in the entire intermediate layer is preferably 90% by mass or more and 100% by mass or less, and more preferably 95% by mass or more and 100% by mass or less.
[0036] The ratio of the coating amount of the coating layer to the coating amount of the intermediate layer (i.e., ratio = coating amount of coating layer / coating amount of intermediate layer) is preferably 0.05 or more and 400 or less, more preferably 1.5 or more and 150 or less, and even more preferably 5 or more and 150 or less, from the viewpoint of improving the impact resistance, moist feel, and smoothness of the molded product.
[0037] -External additives- The cellulose particles according to the present embodiment may contain inorganic particles. When inorganic particles are added externally, secondary aggregation between particles is suppressed, and the particles' inherent properties are easily exhibited. Therefore, the impact resistance, moist feeling, and smoothness of the molded product are easily improved. It is also assumed that the decrease in biodegradability is suppressed.
[0038] The external additive may be at least one selected from the group consisting of silicon-containing compound particles and metal oxide particles.
[0039] The silicon-containing compound particles refer to particles that contain silicon. The silicon-containing compound particles may be particles containing only silicon, or may be particles containing silicon and other elements.
[0040] The silicon-containing compound particles are preferably silica particles. The silica particles may be crystalline or amorphous as long as they are particles that are mainly composed of silica, i.e., SiO2. The silica particles may be particles manufactured from silicon compounds such as water glass and alkoxysilane as raw materials, or may be particles obtained by crushing quartz. As the metal oxide, oxides of metals other than silicon can be used. Examples of metal oxides include zinc oxide, magnesium oxide, iron oxide, and aluminum oxide.
[0041] The volume average particle size of the external additive is preferably from 1 nm to 100 nm, more preferably from 5 nm to 30 nm, from the viewpoint of texture (specifically, feel on the skin). The volume average particle diameter of the external additive is measured in the same manner as the volume average particle diameter of the cellulose.
[0042] The amount of the external additive added is preferably 0.1% by mass or more and 2% by mass or less with respect to the total mass of the cellulose particles (cellulose particles to which no external additive has been added).
[0043] (Volume average particle size) The volume average particle size of the cellulose particles according to this embodiment is preferably from 1 μm to 100 μm, more preferably from 2 μm to 20 μm, and further preferably from 4 μm to 10 μm. By setting the volume average particle diameter of the cellulose particles according to the present embodiment to 1 μm or more and 100 μm or less, the particle size becomes appropriate, flexibility is increased, and impact resistance of the molded product is improved. In addition, moist feeling and smoothness are also improved.
[0044] The volume average particle size of the cellulose particles is measured as follows. The particle size is measured using an LS particle size distribution analyzer "Beckman Coulter LS13 320 (manufactured by Beckman Coulter)" and the cumulative particle size distribution is plotted from the smallest diameter side on a volume basis. The particle size at 50% of the cumulative distribution is determined as the volume average particle size.
[0045] <Method of manufacturing cellulose particles> The method for producing cellulose particles according to this embodiment includes, for example, a step of obtaining base particles mainly composed of cellulose (hereinafter, "cellulose particle (base particle) producing step"), and a step of coating the base particles with a coating material other than a coupling agent and, if necessary, an intermediate material (hereinafter, "intermediate layer and coating layer forming step"). This makes it possible to obtain cellulose particles having a coating layer coverage of 60% to 100% of the base particles, preferably cellulose particles having a coating layer coverage of 1% to 40% by mass of the base particles and a coating layer coverage of 60% to 100% of the base particles. Specifically, the method for producing cellulose particles according to this embodiment is, for example, as follows. - Cellulose particle (mother particle) manufacturing process - (1) First, cellulose acylate is dissolved in a water-soluble organic solvent A to prepare a cellulose acylate solution A. (2) Next, the cellulose acylate solution A is added to a calcium carbonate dispersion obtained by dispersing calcium carbonate in water, and the mixture is stirred to prepare a cellulose acylate solution B. (3) Next, the cellulose acylate solution B is added to a mixed solution of carboxymethyl cellulose, the water-soluble organic solvent B, and water, and the mixture is stirred at high speed to prepare a cellulose acylate solution C. (4) Next, sodium hydroxide is added to the cellulose acylate solution C. The cellulose acylate dispersion C is heated to remove the water-soluble organic solvents A and B, and hydrochloric acid is added to form cellulose acylate particles. The cellulose acylate particles are then filtered, and the filtered cellulose acylate particles are dispersed in water to prepare a cellulose acylate particle dispersion. (5) Next, sodium hydroxide is added to the cellulose acylate particle dispersion, and the cellulose acylate particle dispersion is heated and stirred in a weak alkaline environment to saponify the cellulose acylate particles, thereby preparing a cellulose particle suspension. (6) Next, hydrochloric acid is added to the cellulose particle suspension to adjust the pH of the suspension to approximately neutral (for example, in the range of 6.5 to 7), and then the cellulose particles are filtered and washed with pure water repeatedly. After the conductivity of the filtrate reaches 10 μs / cm or less, the cellulose particles separated by filtration are dried.
[0046] Here, cellulose acylate is a cellulose derivative in which at least one hydroxyl group in cellulose is substituted (acylated) with an aliphatic acyl group. AC (R AC represents an aliphatic hydrocarbon group.) is a cellulose derivative substituted with. The water-soluble organic solvent A is a solvent in which 0.1% by mass to 10% by mass of water is dissolved at 25° C., and examples thereof include ethyl acetate and butyl acetate. The water-soluble organic solvent B is a solvent in which 0.1% by mass to 10% by mass of water is dissolved at 25° C., and examples thereof include methyl ethyl ketone and acetone.
[0047] In the above manufacturing process, the dynamic friction coefficient, bulk density, surface smoothness, solidity, etc. of the cellulose particles can be controlled by adjusting the mass ratio of water-soluble organic solvent A to water-soluble organic solvent B in the mixed solvent that dissolves the cellulose acylate. In addition, by adjusting the amount of carboxymethyl cellulose, the volume average particle size of the cellulose particles can be controlled. By controlling these factors, the cellulose particles according to the present embodiment can be obtained.
[0048] Here, cellulose acylate is a cellulose derivative in which at least one hydroxyl group in cellulose is substituted (acylated) with an aliphatic acyl group. AC (R AC represents an aliphatic hydrocarbon group. The water-soluble organic solvent A is a solvent in which 0.1% by mass to 10% by mass of water is dissolved at 25° C., and examples thereof include ethyl acetate and butyl acetate. The water-soluble organic solvent B is a solvent in which 0.1% by mass to 10% by mass of water is dissolved at 25° C., and examples thereof include methyl ethyl ketone and acetone.
[0049] - Intermediate layer and covering layer formation process - First, an aqueous dispersion of the base particles is prepared. Before preparing the aqueous dispersion, it is preferable to wash the base particles with an acid.
[0050] Next, the aqueous dispersion in which the base particles are dispersed is mixed with an aqueous solution containing the intermediate material that constitutes the intermediate layer. As a result, for example, the hydroxyl groups of the cellulose contained in the base particles react with the amine sites, carboxyl groups, amino groups, etc. of the compound that constitutes the intermediate layer, or the hydroxyl groups form hydrogen bonds, forming the intermediate layer. However, if no intermediate layer is to be formed, this operation is not performed.
[0051] After heating the aqueous dispersion in which the base particles on which the intermediate layer is formed are dispersed, the coating material that constitutes the coating layer is added and stirred, thereby forming the coating layer. Here, when forming the coating layer, the coverage rate of the coating layer is controlled by the heating temperature, the amount of coating material added, the addition time of the coating material, and the stirring time after the addition of the coating material.
[0052] The cellulose particles having the coating layer are then taken out from the mixture. The cellulose particles having the coating layer are taken out, for example, by filtering the mixture. The taken-out cellulose particles having the coating layer are preferably washed with water. This makes it possible to remove unreacted surface treatment polymer. The cellulose particles having the coating layer are then dried to obtain the cellulose particles according to this embodiment.
[0053] -External addition process- An external additive may be added to the obtained cellulose particles. The external addition step may be, for example, a process in which an external additive is added to cellulose particles using a mixing mill, a V-type blender, a Henschel mixer, a Loedige mixer, or the like.
[0054] <Application> Applications of the cellulose particles according to this embodiment include granular materials such as cosmetics, rolling agents, abrasives, scrubbing agents, display spacers, materials for forming beads, light diffusing particles, resin reinforcing agents, refractive index control agents, biodegradation promoters, fertilizers, water absorbing particles, toner particles, and anti-blocking particles.
[0055] The cellulose particles according to this embodiment are preferably used in cosmetics. Among these, the cellulose particles according to this embodiment are preferably used as a cosmetic additive. The cellulose particles according to this embodiment have excellent flexibility, and therefore when used as a cosmetic additive, the cosmetic spreads well and does not easily slide on the skin when applied to the skin.
[0056] The cellulose particles according to this embodiment can be used as a cosmetic additive in, for example, base makeup cosmetics (e.g., makeup base, concealer, foundation, face powder, etc.); makeup cosmetics (e.g., lipstick, gloss, lip liner, blush, eye shadow, eyeliner, mascara, eyebrows, nails, nail care cosmetics, etc.); skin care cosmetics (e.g., facial cleanser, cleansing, lotion, emulsion, serum, pack, face mask, eye and mouth care cosmetics, etc.); etc. In particular, since cosmetic additives for makeup cosmetics are required to be flexible and biodegradable, the resin particles according to this embodiment are preferably used as cosmetic additives for makeup cosmetics. EXAMPLES
[0057] Examples will be described below, but the present invention is not limited to these examples. In the following description, unless otherwise specified, all "parts" and "%" are based on mass.
[0058] <Preparing each ingredient> The following materials were prepared:
[0059] (covering material) ST-1: Calcium stearate (fatty acid metal salt), NOF Corp. "Calcium stearate plant extract" ST-2: Behenic acid (fatty acid), NOF Corporation "NAA-222S" ST-3: Lauroyl lysine (amino acid compound), Ajinomoto Co., Inc. "Amihope LL" ST-4: Hydrogenated lecithin (lipid compound), Nikko Chemicals Co., Ltd. "NIKKOL Lecithinol S-10" ST-5: Hydrogen dimethicone (silicone compound), Shin-Etsu Chemical Co., Ltd. "KF-9901" Chemical industry ST-6: Perfluorooctyltriethoxysilane (fluorinated compound), Fuluorochem,.Ltd. "Perfluorooctyltriethoxysilane" ST-7: Hydroxypropyl bispalmitamide MEA (ceramide compound), MACROCARE,.Ltd. "Pacificos CRM" ST-8: Isostearic acid, Fujifilm Wako Pure Chemical "Reagent" ST-9: Aluminum stearate, Fujifilm Wako Pure Chemical "Reagent" ST-10: Zinc stearate, Fujifilm Wako Pure Chemical "Reagent" ST-11: Magnesium myristate, Taihei Chemical Industry Co., Ltd. ST-12: Zinc myristate, Nitto Chemical Industry Co., Ltd. ST-13: Calcium behenate, Nitto Chemical Industries Co., Ltd. ST-14: Sodium stearoyl glutamate, Ajinomoto Co., Inc. "Amisoft" ST-15: Zinc stearate (fatty acid metal salt), Sakai Chemical Industry Co., Ltd. "SPZ-100F" ST-16: n-Octyltriethoxysilane (silane coupling agent), Fujifilm Wako Pure Chemical Industries, Ltd. "Reagents" ST-17: n-isopropyl triisostearoyl titanate (titanium coupling agent), Fujifilm Wako Pure Chemical "Reagent"
[0060] AA-1: Polyethyleneimine (polyamine compound), Nippon Shokubai Co., Ltd. "PEI-1500" AA-2: Polyacrylic acid (polyacrylic acid), Toa Gosei Co., Ltd. "Jurimer AC-10H" AA-3: Polyquaternium 11 (Polyquaternium), BASF Japan "Rubycut PQ11AT1" AA-4: Cationic guar gum (polysaccharide), Sumitomo Pharma Food & Chemical Co., Ltd. "Labor Gum CG-M"
[0061] <Examples 1 to 7, 10 to 22, Comparative Example 2> - Formation of mother particles - 130 parts of cellulose acylate (DAC "L-50" manufactured by Daicel Corporation, cellulose diacetate, weight average polymerization degree 570) was completely dissolved in 870 parts of ethyl acetate. This was added to a dispersion in which 60 parts by mass of calcium carbonate was dispersed in 500 parts by mass of pure water, and the mixture was stirred for 5 hours. This was added to a dispersion in which 5 parts by mass of carboxymethylcellulose and 400 parts by mass of methyl ethyl ketone were dispersed in 800 parts by mass of pure water, and the mixture was stirred for 10 minutes with a high-speed emulsifier. 10 parts by mass of sodium hydroxide was added to this, and the mixture was stirred at 80°C for 10 hours to remove ethyl acetate and methyl ethyl ketone. 20 parts by mass of dilute hydrochloric acid was added to this to dissolve calcium carbonate. The residue was filtered and dispersed again in pure water to obtain a slurry of cellulose acylate particles. 20 parts by mass of 20% sodium hydroxide aqueous solution was added to 500 parts by mass of cellulose acylate particle slurry (solid content 50 parts by mass), and the mixture was stirred at 40°C for 12 hours to saponify the cellulose acylate particles. Hydrochloric acid was added dropwise to the slurry until the pH of the slurry became 7. The slurry was then filtered, and the filtered product was washed with an excess amount of pure water, and the filtering and washing were repeated until the electrical conductivity of the filtrate became 10 μs / cm or less. Finally, the obtained cake-like filtered product was filtered, and the filtered product was freeze-dried to obtain saponified cellulose mother particles.
[0062] -Surface treatment- The cake-like cellulose base particles, which had been repeatedly filtered and washed until the electrical conductivity of the filtrate reached 10 μs / cm or less, were reslurried in pure water to obtain a base particle slurry. To 500 parts by mass of the base particle slurry (solid content 50 parts by mass), an intermediate material was added in an amount corresponding to the type and coating amount shown in Table 1, and the mixture was stirred for 1.5 hours while maintaining the temperature at 35° C. As a result, an intermediate layer with the coating amount shown in Table 1 was formed on the base particles. Next, the base particle slurry on which the intermediate layer has been formed is heated to a treatment temperature shown in Table 1, and then a coating material is added in an amount that results in the type and coating amount shown in Table 1, followed by stirring for the stirring time shown in Table 1. As a result, a coating layer with the coating amount shown in Table 1 was formed on the intermediate layer. Thereafter, the base particles on which the intermediate layer and the coating layer were formed were repeatedly filtered and washed until the filtrate had an electric conductivity of 10 μs / cm or less. After washing, the resulting cake was dried to obtain cellulose particles having an intermediate layer and a coating layer. The obtained particles were mixed in an FM mixer (FM40, manufactured by Nippon Coke and Engineering Co., Ltd.) for 4000 min while maintaining the mixer temperature at 25°C. -1 The mixture was stirred at a rotation speed of 1000 for 2 hours to tan the surface of the coating layer.
[0063] In addition, as indicated by "-" in Table 1, in some cases, cellulose particles were produced without forming an intermediate layer.
[0064] <Example 8> After dissolving cellulose acylate in ethyl acetate, saponified cellulose base particles were obtained in the same manner as in Example 1, except that the amount of carboxymethyl cellulose added was 12 parts by mass. Ta.
[0065] <Example 9> After dissolving cellulose acylate in ethyl acetate, the saponified cellulose base particles were prepared in the same manner as in Example 1, except that the amount of carboxymethyl cellulose added was 0.7 parts by mass. Got it.
[0066] <Example 23> A solution was prepared by adjusting the solid content to 5 parts by mass of aluminum chloride, which was half the amount of the surface treatment coating material. After adding the surface treatment coating material shown in Table 1, the obtained solution was added dropwise over 10 minutes. Apart from these operations, the same procedure as in Example 1 was repeated to obtain saponified cellulose base particles.
[0067] Comparative Example 1: Untreated Cellulose Particles The saponified cellulose base particle slurry was adjusted to a solids concentration of 10%, and 500 parts by mass was taken out. 17.5 parts by mass of 20% NaOH was added to this, and the mixture was stirred for 6 hours in an environment of 30°C. Hydrochloric acid was added to the saponified particle slurry to adjust the pH to 7, and the slurry was filtered and washed repeatedly until the filtrate had an electrical conductivity of 10 μs / cm or less, yielding cellulose particles. <Comparative Example 3: Cellulose particles surface-treated with fatty acid salt by dry treatment> In Example 1, 50 parts by mass of the saponified cellulose base particles and 15 parts by mass of zinc stearate ("SPZ-100F" by Sakai Chemical Industry Co., Ltd.) were placed in a small mixer. They were then dry mixed for 4 minutes to obtain cellulose particles on which a coating layer of zinc stearate was formed.
[0068] Comparative Example 4: Cellulose particles treated with propylethoxysilane In Example 1, 15 parts by mass of n-octyltriethoxysilane was dropped onto 50 parts by mass of saponified cellulose base particles. The dropping was carried out while stirring with a small heated mixer, thereby forming a coating layer of n-octyltriethoxysilane on the surface of the base particles. Thereafter, an aluminum chloride aqueous solution in which 0.1% by mass of aluminum chloride was dissolved in 20 times the amount of water was dropped onto the base particles on which the coating layer was formed, and the mixture was stirred for 30 minutes while maintaining the temperature at 35°C. The mixer temperature was then raised to 90°C, and the base particles were aged for 5 hours to obtain cellulose particles.
[0069] <Comparative Example 5: Cellulose particles treated with isopropyl triisomyristic titanate> Cellulose particles were obtained in the same manner as in Comparative Example 3, except that in Comparative Example 3, 15 parts by mass of n-isopropyl triisostearoyl titanate was dropped instead of n-octyltriethoxysilane, and a coating layer of n-isopropyl triisomyristyl titanate was formed on the surface of the base particles.
[0070] <Physical property evaluation> (particle properties) For the cellulose particles obtained in each example, the following particle properties were measured according to the methods described above. - Coverage rate of the coating layer Volume average particle size of cellulose particles (referred to as "particle size" in the table)
[0071] <Evaluation> The moist feeling and smoothness of the obtained cellulose particles and the impact resistance of the molded product were evaluated as follows.
[0072] -Moisturizing and smooth- Ten female panelists were asked to place 5 g of the cellulose granule sample on the back of their hand, spread it out, and then rate the moistness and smoothness of the sample, with 5 being the best and 0 being the worst. The scores of the 10 monitors were then averaged to evaluate the product.
[0073] -Impact resistance of molded products- Using the cellulose particles of each example, a powder foundation was obtained according to the formulation shown in Table 2 by a known method. The obtained powder foundation was molded in the same metal plate press, and the molded powder foundation was placed in a compact container. The compact container was then dropped from a height of 0.75 m. After the dropping operation was repeated three times, the condition of the powder foundation molded product was observed and evaluated according to the following criteria: A (◎): No change in the molded product B(〇): Slight cracks on the surface of the molded product C(△): Vibrations or chipping occurs inside the molded product. D(×): The molded product is broken into pieces
[0074] [Table 1]
[0075] [Table 2]
[0076] [Table 3]
[0077] From the above results, it is apparent that the cellulose particles of this Example provide molded products superior in impact resistance to the cellulose particles of the Comparative Example. In addition, the cellulose particles of this embodiment are excellent in moist feeling and smoothness. I understand.
[0078] The present embodiment includes the following aspects. (((1))) A base particle mainly composed of cellulose; a coating layer that coats the base particles and contains a coating material excluding a coupling agent; having The cellulose particles have a coverage rate of the coating layer relative to the base particles of 60% or more and 100% or less. (((2))) The cellulose particles according to (((1))), wherein the coverage of the coating layer with respect to the base particles is 80% or more and 100% or less. (((3))) The cellulose particles according to (((2))), wherein the coverage of the coating layer with respect to the base particles is 90% or more and 100% or less. (((4))) The cellulose particles according to any one of ((1))) to (((3))), wherein the coating layer has a coating amount of 1% by mass or more and 40% by mass or less based on the base particles. (((5))) The cellulose particles according to (((4))), wherein the amount of the coating layer applied to the base particles is 3% by mass or more and 30% by mass or less. (((6))) The cellulose particles according to any one of (((1))) to (((5))), having a volume average particle diameter of 1 μm or more and 100 μm or less. (((7))) The cellulose particles according to any one of (((1))) to (((6))), wherein the coating layer contains at least one coating material selected from the group consisting of fatty acids, fatty acid metal salts, and amino acid compounds. (((8))) The fatty acid is at least one selected from the group consisting of straight-chain fatty acids and hydroxy fatty acids; The cellulose particles according to (((7))), wherein the fatty acid metal salt is a straight-chain fatty acid metal salt. (((9))) The cellulose particles according to any one of ((1))) to (((8))), which have an intermediate layer between the base particle and the coating layer. (((10))) The cellulose particles according to (((9))), wherein the intermediate layer contains at least one intermediate material selected from the group consisting of polyamine compounds, polyquaterniums, polysaccharide compounds, and polyacrylic acids. (((11))) obtaining base particles mainly composed of cellulose; coating the base particles with a coating material excluding a coupling agent; Including, the amount of the coating layer relative to the base particle is 1% by mass or more and 40% by mass or less, A method for producing cellulose particles, wherein a coverage rate of the coating layer with respect to the base particles is 60% or more and 100% or less.
[0079] The advantages of the above aspect are as follows. According to the invention of (((1))), there is provided cellulose particles having base particles mainly composed of cellulose and a coating layer which coats the base particles and contains a coating material excluding a coupling agent, and the resulting molded product has superior impact resistance compared to cellulose particles in which the coating layer has a coverage rate of less than 60% with respect to the base particles. According to the invention related to (((2))), there are provided cellulose particles which give molded products with superior impact resistance, compared to cases where the coverage rate of the coating layer with respect to the base particles is less than 80%. According to the invention related to (((3))), there is provided cellulose particles which provide a molded product having superior impact resistance compared to a case where the coverage rate of the coating layer with respect to the base particles is less than 90%. According to the invention related to (((4))), cellulose particles are provided which give molded products with superior impact resistance, compared with cases in which the amount of the coating layer relative to the base particles is less than 1 mass % or exceeds 40 mass %. According to the invention related to 5)), there are provided cellulose particles which give molded products with superior impact resistance, compared with cases in which the amount of the coating layer relative to the base particles is less than 3 mass % or more than 30 mass %. According to the invention related to (((6))), there is provided cellulose particles which give molded products with superior impact resistance compared to those having a volume average particle diameter of less than 1 μm or more than 100 μm. According to the invention (((7))), there are provided cellulose particles which give molded products with superior impact resistance compared to those in which the coating layer contains a lipid compound. According to the invention related to (((8))), there is provided cellulose particles which give molded products with superior impact resistance compared to cases in which the fatty acid is a branched fatty acid or the fatty acid metal salt is a branched fatty acid metal salt. According to the invention related to (((9))), there are provided cellulose particles which give molded products with superior impact resistance compared to cases where no intermediate layer is provided between the base particles and the coating layer. According to the invention (((10))), there is provided a cellulose particle which provides a molded product having superior impact resistance compared to a case in which the intermediate layer contains arginine or dextrin. According to the invention related to (((11))), in a method for producing cellulose particles including a step of obtaining base particles mainly composed of cellulose and a step of coating the base particles with a coating material excluding a coupling agent, the method provides a molded product with superior impact resistance compared to cases where the amount of coating layer on the base particles is less than 1% by mass or exceeds 40% by mass, or where the coverage rate of the coating layer on the base particles is less than 60% or exceeds 100%.
Claims
1. A base particle mainly composed of cellulose; a coating layer that coats the base particles and contains a coating material excluding a coupling agent; having The cellulose particles have a coverage of 60% or more and 100% or less of the base particles with the coating layer.
2. 2. The cellulose granules according to claim 1, wherein the coverage of the coating layer with respect to the base particles is 80% or more and 100% or less.
3. The cellulose granules according to claim 2 , wherein the coverage of the coating layer with respect to the base particles is 90% or more and 100% or less.
4. 2. The cellulose granule according to claim 1, wherein the coating layer has a coating amount of 1% by mass or more and 40% by mass or less based on the base particle.
5. The cellulose granules according to claim 4 , wherein the amount of the coating layer relative to the base particle is 3% by mass or more and 30% by mass or less.
6. 2. The cellulose granules according to claim 1, having a volume average particle diameter of 1 μm or more and 100 μm or less.
7. 2. The cellulose particles according to claim 1, wherein the coating layer contains at least one coating material selected from the group consisting of fatty acids, fatty acid metal salts, and amino acid compounds.
8. The fatty acid is at least one selected from the group consisting of straight-chain fatty acids and hydroxy fatty acids; The cellulose particles according to claim 7 , wherein the fatty acid metal salt is a straight-chain fatty acid metal salt.
9. The cellulose particles according to claim 1 or 7, further comprising an intermediate layer between the base particle and the coating layer.
10. The cellulose particles according to claim 9 , wherein the intermediate layer comprises at least one intermediate material selected from the group consisting of a polyamine compound, a polyquaternium, a polysaccharide compound, and a polyacrylic acid.
11. obtaining base particles mainly composed of cellulose; coating the base particles with a coating material excluding a coupling agent; Including, the amount of the coating layer relative to the base particle is 1% by mass or more and 40% by mass or less, A method for producing cellulose particles, wherein a coverage rate of the coating layer with respect to the base particles is 60% or more and 100% or less.
Citation Information
Patent Citations
JP1973097289A
Resin beads, manufacturing method of resin beads, and products using resin beads
JP2022099605A
Cited By
Method for producing hydrophobic particles and hydrophobic particles
CN123127119A
Method for producing hydrophobic particles and hydrophobic particles
EP4843664A2