Laminated film, conductive film, current collector and battery

A laminated film with a multi-layer intermediate layer and enhanced surface wettability addresses issues of thickness variation and coating uniformity, providing improved mechanical properties and conductivity for conductive films used in electronic components.

JP2024144056APending Publication Date: 2024-10-11MITSUBISHI CHEM CORP
View PDF 3 Cites 0 Cited by

Patent Information

Application Number
JP2023195559
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Priority Date
2023-03-30
Filing Date
2023-11-17
Publication Date
2024-10-11

AI Technical Summary

Technical Problem

Existing conductive films used as current collectors in electronic components face issues with thickness variation, uneven coating of aqueous liquids, mechanical properties, and stability during peeling, especially when the intermediate layer is thin, leading to poor appearance and mechanical defects.

Method used

A laminated film structure with an intermediate layer composed of multiple layers, where at least one surface layer has a surface wettability index of 30 dyne/cm or more, using a resin composition containing a thermoplastic resin and a conductive filler, including a carboxylic acid-modified polyolefin resin, to enhance coating properties and mechanical strength, while maintaining high conductivity.

Benefits of technology

The laminated film achieves excellent coating properties for aqueous liquids, improved mechanical properties like tensile elongation at break, reduced thickness fluctuations, and stable peeling from outer layers, ensuring high conductivity and good appearance.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024144056000001
    Figure 2024144056000001
Patent Text Reader

Abstract

To provide a laminated film which is excellent in coating property of an aqueous liquid, is excellent in mechanical characteristics such as tensile breaking elongation, is small in thickness fluctuations, has good appearance, has an intermediate layer having high conductivity, and is also excellent in peelability between the intermediate layer and both outer layers.SOLUTION: A laminated film has an intermediate layer [I] composed of a resin composition (A) containing a thermoplastic resin (a1) and a conductive filler (a2), and both outer layers [II] composed of a resin composition (B) containing a thermoplastic resin (b1), where the intermediate layer [I] is a layer formed of a plurality of layers, and a surface wetting index of at least one surface layer (i-1) of the intermediate layer [I] is 30 dyne / cm or more.SELECTED DRAWING: None
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a laminated film, a conductive film, a current collector, and a battery. [Background technology]

[0002] In the electronics field, the main properties required of polymer materials vary depending on the product and application, but include moldability, heat resistance, durability, high strength, chemical resistance, and corrosion resistance. Resins that meet these requirements include thermoplastic resins such as polypropylene, polycarbonate, and polyimide, and thermosetting resins such as epoxy resins and phenolic resins.

[0003] A method of adding a conductive material to a polymeric material to give it electrical conductivity is known. However, 4 To obtain a highly conductive film with a conductivity of Ω·cm or less, a large amount of conductive material must be added to the polymer material, which can lead to poor extrusion moldability.

[0004] For example, Patent Document 1 discloses a method for producing a highly conductive film, which comprises co-extruding an intermediate layer made of a highly conductive thermoplastic resin composition containing 30 parts by weight or more of a carbon-based filler, and on both sides of the intermediate layer, as outer layers, peelable thermoplastic resin layers in which the force required to peel the outer layer in a 180° direction from the intermediate layer is 5 to 500 g / 15 mm width, and then cooling the thermoplastic resin layers on both sides.

[0005] Patent Document 2 discloses a method for producing a highly conductive film, in which a multilayer film is produced by co-extrusion, the multilayer film having an intermediate layer made of a conductive resin composition in which a conductive filler is blended with a thermoplastic resin (A), and both outer layers made of a thermoplastic resin (B) having good peelability from the thermoplastic resin (A), and the multilayer film is cooled and then both outer layers are peeled off, the method being characterized in that the ratio D / L of the draft ratio D to the lip gap L during co-extrusion is 11 or less.

[0006] Patent Document 3 also describes a thermal expansion coefficient flex circuit having an intermediate layer made of a resin composition (I) containing a conductive filler (A) and a thermoplastic resin (B) and two outer layers made of a resin composition (II) containing a thermoplastic resin (C), in which the ratio of the melt flow rate (MFR(I)) of the resin composition (I) to the melt flow rate (MFR(II)) of the resin composition (II) [MFR(I) / MFR(II)] is 0.1 or more and 3.5 or less, and the temperature of the resin composition (I) is 240° C., the shear rate is 10 to 100 sec -1 The laminated film has an average first normal stress difference of -0.015 MPa or more and an intermediate layer having a thickness of 50 μm or less. [Prior art documents] [Patent documents]

[0007] [Patent Document 1] Japanese Patent Application Publication No. 61-82611 [Patent Document 2] JP 2014-030899 A [Patent Document 3] JP 2020-157651 A Summary of the Invention [Problem to be solved by the invention]

[0008] A method for producing a laminated film includes, for example, using an extrusion molding machine, feeding a resin composition for an intermediate layer, which can become a conductive film, and a resin composition for an outer layer into the hopper of the extruder, melting and plasticizing them at a predetermined temperature, co-extruding them under predetermined film-forming conditions from the lip gap, which is the outlet of a T-die, introducing them into a cast roll at a predetermined temperature, and then cooling and solidifying them to obtain a laminated film.

[0009] In recent years, with the miniaturization and thinning of electronic components, the conductive film used as a part of the electronic components is required to be lighter and thinner. For this reason, if the desired thickness of the intermediate layer is, for example, 100 μm or less, the resin composition for the intermediate layer extruded from the outlet of the T-die during the production of the laminated film is easily affected by the peripheral members of the outlet that it comes into contact with, due to the thin thickness. As a result, there are problems such as a large variation in the thickness of the intermediate layer, a poor appearance such as uneven flow or holes in the intermediate layer, difficulty in obtaining mechanical properties such as tensile elongation at break, and a stick-slip (catching) problem when peeling the outer layer from the laminated film due to the unstable peeling of the outer layer.

[0010] In recent years, attempts have been made to use a conductive film as a negative electrode current collector, apply a negative electrode paint (e.g., a negative electrode water-based paint made by mixing a negative electrode active material, a binder, and an aqueous solvent) to the surface of the negative electrode current collector to form a negative electrode layer, and produce a battery. When forming the negative electrode layer, it is required that the negative electrode paint (particularly the negative electrode water-based paint) is applied uniformly to the surface of the negative electrode current collector, but there have been problems such as the negative electrode paint being repelled by the surface of the negative electrode current collector, causing unevenness, making it impossible to apply the negative electrode paint uniformly.

[0011] Studies have been made to obtain a film having higher conductivity in the manufacturing methods of a highly conductive film disclosed in Patent Documents 1 and 2, and in the laminated film having an intermediate layer that can become a conductive film disclosed in Patent Document 3. However, Patent Documents 1 to 3 do not make any particular study on the uniform application of a coating material for a negative electrode by modifying the surface characteristics of the negative electrode current collector when the conductive film is used as a negative electrode current collector, leaving room for further study.

[0012] Therefore, an object of the present invention is to provide a laminated film that has excellent coatability with aqueous liquids, excellent mechanical properties such as tensile elongation at break, small thickness variation, good appearance, an intermediate layer with high conductivity, and excellent peelability between the intermediate layer and both outer layers. Another object of the present invention is to provide a conductive film that has excellent coatability with aqueous liquids, excellent mechanical properties such as tensile elongation at break, small thickness variation, good appearance, and high conductivity. [Means for solving the problem]

[0013] The inventors have discovered that the above problem can be solved by forming the intermediate layer [I] as a layer composed of multiple layers and setting the surface wettability index of at least one of the surface layers (i-1) of the intermediate layer to a specific value or more (30 dyne / cm or more). That is, the present invention provides the following: <1> ~ <18> to provide. <1> A laminated film having an intermediate layer [I] made of a resin composition (A) containing a thermoplastic resin (a1) and a conductive filler (a2), and two outer layers [II] made of a resin composition (B) containing a thermoplastic resin (b1), wherein the intermediate layer [I] is a layer formed from a plurality of layers, and at least one surface layer (i-1) of the intermediate layer [I] has a surface wetting index of 30 dyne / cm or more. <2> At least one surface layer (i-1) of the intermediate layer [I] is a layer formed from a resin composition (A1) containing a thermoplastic resin (a1), a conductive filler (a2), and a carboxylic acid-modified polyolefin resin (a3). <1> The laminated film according to claim 1. <3> The content of the carboxylic acid-modified polyolefin resin (a3) ​​in the resin composition (A1) is 5% by mass or more and 50% by mass or less. <2> The laminated film according to claim 1. <4> The intermediate layer [I] is a two-layer structure of a surface layer (i-1) / a middle layer (i-2) or a three-layer structure of a surface layer (i-1) / a middle layer (i-2) / a surface layer (i-1). <1> ~ <3> 13. The laminate film according to claim 12 . <5> The intermediate layer (i-2) of the intermediate layer [I] is a layer formed from a resin composition (A2) containing a thermoplastic resin (a1) and a conductive filler (a2) and substantially not containing a carboxylic acid-modified polyolefin resin (a3). <4> The laminated film according to claim 1. <6> The thickness variation of the intermediate layer [I] is less than ±10 μm. <1> ~ <5> 13. The laminate film according to claim 12 . <7> The thickness (X) of the intermediate layer [I] is 1 μm or more and 100 μm or less, and the ratio (Y / X) of the thickness (Y) of each layer of the two outer layers [II] to the thickness (X) of the intermediate layer [I] is 1 or more and 5 or less, <1> ~ <6> 13. The laminate film according to claim 12 . <8> The peel strength between the intermediate layer [I] and both outer layers [II] is less than 0.1 N / cm. <1> ~ <7> 13. The laminate film according to claim 12 . <9> The thermoplastic resin (a1) is a polyolefin resin. <1> ~ <8> 13. The laminate film according to claim 12 . <10> The conductive filler (a2) is a carbon nanotube. <1> ~ <9> 13. The laminate film according to claim 12 . <11> The thermoplastic resin (b1) is a polyester resin. <1> ~ <10> 13. The laminate film according to claim 12 . <12> The thickness of the laminated film is 20 μm or more and 400 μm or less. <1> ~ <11> 13. The laminate film according to claim 12 . <13> The thickness of each of the outer layers [II] is 5 μm or more and 150 μm or less. <1> ~ <12> 13. The laminate film according to claim 12 . <14> The content of the conductive filler (a2) in the resin composition (A) is 0.1 mass % or more and 50 mass % or less. <1> ~ <13> 13. The laminate film according to claim 12 . <15> the above <1> ~ <14> 2. A conductive film, in which both outer layers [II] of the laminated film according to any one of the above items are peeled off. <16> A conductive film made of a resin composition (A) containing a thermoplastic resin (a1) and a conductive filler (a2), the conductive film being a layer formed from multiple layers, and at least one surface layer (i-1) of the conductive film having a surface wettability index of 30 dyne / cm or more. <17> the above <15> or <16> A collector using the conductive film according to claim 1. <18> the above <15> or <16> A battery using the conductive film according to claim 1. Effect of the Invention

[0014] According to the present invention, it is possible to provide a laminated film which has excellent coatability with aqueous liquids, excellent mechanical properties such as tensile elongation at break, small thickness variation, good appearance, an intermediate layer with high conductivity, and excellent peelability between the intermediate layer and both outer layers. Furthermore, according to the present invention, it is possible to provide a conductive film that has excellent coatability with aqueous liquids, excellent mechanical properties such as tensile elongation at break, small thickness variation, good appearance, and high conductivity. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0015] The present invention will be described in detail below. However, the content of the present invention is not limited to the embodiments described below.

[0016] <Terminology explanation> In the present invention, when expressed as "X to Y" (X and Y are any numbers), unless otherwise specified, it includes the meaning of "X or more and Y or less", as well as "preferably larger than X" and "preferably smaller than Y".

[0017] [Laminated film] The laminated film of the present invention is a laminated film having an intermediate layer [I] made of a resin composition (A) containing a thermoplastic resin (a1) and a conductive filler (a2), and two outer layers [II] made of a resin composition (B) containing a thermoplastic resin (b1), wherein the intermediate layer [I] is a layer formed from a plurality of layers, and at least one surface layer (i-1) of the intermediate layer [I] has a surface wetting index of 30 dyne / cm or more.

[0018] According to the present invention, it is possible to provide a laminated film having an intermediate layer with excellent aqueous liquid coatability, excellent mechanical properties such as tensile elongation at break, small thickness variation, good appearance, high conductivity, and excellent peelability between the intermediate layer and both outer layers. Also, according to the present invention, it is possible to provide a conductive film having excellent aqueous liquid coatability, excellent mechanical properties such as tensile elongation at break, small thickness variation, good appearance, and high conductivity. The reason for this is not entirely clear, but is thought to be as follows. By forming the intermediate layer as a layer consisting of multiple layers, even if a material with a low elongation rate is used for the middle layer (i-2) of the intermediate layer, by laminating a material with a high elongation rate for at least one surface layer (i-1) of the intermediate layer, the middle layer (i-2) will be elongated in a manner that follows the surface layer (i-1), and as a result, the elongation rate of the entire intermediate layer will be improved, and it is believed that mechanical properties such as tensile breaking elongation can be obtained. Furthermore, by setting the surface wetting index of at least one surface layer (i-1) of the intermediate layer, which can become a conductive film, to a specific value or more (30 dyne / cm or more), when an aqueous liquid is applied to at least one surface layer (i-1) of the intermediate layer, it is possible to make the interfacial surface tension of the surface layer (i-1) of the intermediate layer closer to the surface tension of the aqueous liquid, thereby reducing the contact angle when the aqueous liquid comes into contact with the surface of the intermediate layer, and making it easier to uniformly apply the aqueous liquid to the surface of at least one surface layer (i-1) of the intermediate layer. Here, when the intermediate layer that can be a conductive film is used as a negative electrode current collector, the negative electrode aqueous paint (for example, a negative electrode aqueous paint obtained by mixing a negative electrode active material, a binder, and an aqueous solvent) corresponds to the aqueous liquid.

[0019] In the present invention, the surface wettability index of at least one surface layer (i-1) of the intermediate layer [I] is 30 dyne / cm or more, preferably 31 dyne / cm or more, more preferably 32 dyne / cm or more. The upper limit is not particularly limited, but is usually 60 dyne / cm, preferably 50 dyne / cm. The surface wettability index of at least one of the surface layers (i-1) of the intermediate layer [I] can be set by appropriately adjusting the type and amount of resin contained in the resin composition (A1) constituting at least one of the surface layers (i-1) of the intermediate layer. When the wetting index is a specific value or higher (30 dyne / cm or higher), the aqueous liquid is less likely to be repelled by the surface of at least one of the outer layers (i-1) of the intermediate layer, and the aqueous liquid can be uniformly applied to at least one of the outer layers (i-1) of the intermediate layer. On the other hand, if the wetting index is less than a certain value (less than 30 dyne / cm), the aqueous liquid will be repelled by the surface of at least one of the outer layers (i-1) of the intermediate layer, making it easier for unevenness to occur, and there is a risk that the aqueous liquid will not be able to be applied uniformly to at least one of the outer layers (i-1) of the intermediate layer. The surface wettability index of at least one of the surface layers (i-1) of the intermediate layer [I] can be determined by the method described in the Examples.

[0020] <Middle layer [I]> (Layer composition of intermediate layer [I]) The intermediate layer [I] is a layer formed of a plurality of layers each made of a resin composition (A) containing a thermoplastic resin (a1) and a conductive filler (a2). The layer structure of the intermediate layer [I] is not particularly limited as long as it is a layer formed from multiple layers, but it is preferable to have a structure of two or more layers in which a surface layer (i-1) is laminated on at least one of the intermediate layers (i-2). Examples of the layer structure of the intermediate layer [I] include the following embodiments. The total number of layers forming the intermediate layer (i-2) can be appropriately adjusted depending on the application and purpose of use. ·Surface layer (i-1) / middle layer (i-2) ·Surface layer (i-1) / middle layer (i-2) / surface layer (i-1) The layer structure of the intermediate layer [I] in the present invention is preferably a layer structure formed from two layers, namely, surface layer (i-1) / middle layer (i-2), or a layer structure formed from three layers, namely, surface layer (i-1) / middle layer (i-2) / surface layer (i-1), and more preferably a layer structure formed from three layers, namely, surface layer (i-1) / middle layer (i-2) / surface layer (i-1). In addition, when the intermediate layer [I] has a layer structure formed of two layers, it is the same as a layer structure formed of three layers from which one of the surface layers (i-1) has been removed. Therefore, even if it has a two-layer structure, the intermediate layer (i-2) will be referred to as the intermediate layer for convenience.

[0021] (Surface layer (i-1)) At least one of the surface layers (i-1) of the intermediate layer [I] is preferably composed of a resin composition (A1) containing a thermoplastic resin (a1), a conductive filler (a2), and a carboxylic acid-modified polyolefin resin (a3), from the viewpoint of improving the applicability of an aqueous liquid to the intermediate layer [I].

[0022] (Middle layer (i-2)) On the other hand, from the viewpoint of obtaining mechanical properties such as tensile elongation at break, the middle layer (i-2) of the intermediate layer [I] is preferably composed of a resin composition (A2) containing a thermoplastic resin (a1) and a conductive filler (a2) and substantially not containing a carboxylic acid-modified polyolefin resin (a3). Here, "substantially not contained" means not contained at all, i.e., 0 mass%, but also means, for example, 0.05 mass% or less (in some cases, it may be 0.03 mass% or less, or 0.01 mass% or less), and also includes cases where the content is so low that it is hardly meaningful to include it.

[0023] (Thermoplastic resin (a1)) The resin composition (A) constituting the entire intermediate layer [I] formed from a plurality of layers contains a thermoplastic resin (a1). When the intermediate layer [I] is a layer formed of two or three layers, the resin composition (A1) constituting the surface layer (i-1) and the resin composition (A2) constituting the middle layer (i-2) contain a thermoplastic resin (a1).

[0024] The thermoplastic resin (a1) is not particularly limited, and various thermoplastic resins can be used. Among the thermoplastic resins, polyolefin resins are preferred from the viewpoint of ensuring the mechanical strength of the film.

[0025] Examples of polyolefin resins include homopolymers of α-olefins having about 2 to 8 carbon atoms, such as ethylene, propylene, 1-butene, 3-methyl-1-butene, 1-pentene, 4-methyl-1-pentene, and 1-hexene; copolymers of these α-olefins with other α-olefins having about 2 to 12 carbon atoms, such as ethylene, propylene, 1-butene, 3-methyl-1-butene, 1-pentene, 4-methyl-1-pentene, 1-hexene, 1-octene, and 1-decene, and vinyl compounds such as vinyl acetate, acrylic acid, methacrylic acid, acrylic acid esters, methacrylic acid esters, styrene, and vinyl chloride; and graft polymers obtained by grafting the vinyl compounds to the homopolymers or copolymers of the α-olefins. Among these, from the viewpoint of stabilizing the interfaces between the intermediate layer and both outer layers to be formed, polypropylene resins or polyethylene resins are preferred, and polypropylene resins are more preferred.

[0026] The polypropylene-based resin may be a propylene homopolymer (a homopolymer of propylene) or a copolymer of propylene and an olefin having 2 to 20 carbon atoms. One or more types of olefins may be used to be copolymerized with propylene. Specific examples of the propylene copolymer include a propylene-ethylene copolymer, a propylene-1-butene copolymer, and a propylene-ethylene-1-butene copolymer. Among these, from the viewpoint of film-forming properties of the intermediate layer, a propylene homopolymer is preferred.

[0027] The polyethylene resin may be an ethylene homopolymer (a homopolymer of ethylene) or may be copolymerized with ethylene and a comonomer component such as an α-olefin or a vinyl monomer. Specific examples of ethylene copolymers include ethylene-1-butene copolymer, ethylene-4-methyl-1-pentene copolymer, ethylene-1-hexene copolymer, ethylene-1-octene copolymer, ethylene-vinyl acetate copolymer, ethylene-acrylic acid copolymer, ethylene-methacrylic acid copolymer, ethylene-methyl methacrylate copolymer, ethylene-ethyl acrylate copolymer, and the like.

[0028] The isotactic pentad fraction, which indicates the stereoregularity of the polypropylene resin, is preferably from 80 to 99%, more preferably from 83 to 98%, and even more preferably from 85 to 97%. If the isotactic pentad fraction is too low, the mechanical strength of the film may decrease. On the other hand, the upper limit of the isotactic pentad fraction is set at the upper limit value that can be obtained industrially at present, but this will not apply in the future if a resin with higher regularity is developed at the industrial level. The isotactic pentad fraction means a three-dimensional structure in which all five methyl groups, which are side chains, are located in the same direction relative to the main chain formed by carbon-carbon bonds composed of any five consecutive propylene units, or the proportion thereof. 13It is determined from the pentad units in the polypropylene molecular chain measured by the signals in the methyl group region of the C-NMR spectrum. The assignment of the signals in the methyl group region is in accordance with A. Zambelli et al. (Macromol. 8, 687 (1975)).

[0029] In addition, Mw / Mn, a parameter indicating the molecular weight distribution of polypropylene-based resin, is preferably 1.5 or more, more preferably 2.0 or more. On the other hand, the upper limit is preferably 10.0 or less, more preferably 8.0 or less, and even more preferably 6.0 or less. The smaller Mw / Mn means the narrower the molecular weight distribution, but by making Mw / Mn 1.5 or more, sufficient extrusion moldability can be obtained and industrial mass production is possible. On the other hand, by making Mw / Mn 10.0 or less, the mechanical strength as a film can be ensured. Mw represents the weight average molecular weight, Mn represents the number average molecular weight, and Mw / Mn is obtained by GPC (gel permeation chromatography) method.

[0030] The melt flow rate (MFR) of the polypropylene resin is preferably 1.0 to 30 g / 10 minutes, and more preferably 5.0 to 20 g / 10 minutes. When the melt flow rate (MFR) is within the above range, even if the viscosity increases due to the incorporation of a conductive filler, the resin composition (A) has a sufficient melt viscosity during molding processing, and the mechanical strength of the film can be ensured. The melt flow rate (MFR) is a value measured in accordance with JIS K7210 under conditions of a temperature of 230° C. and a load of 2.16 kg.

[0031] Examples of polypropylene-based resins that can be used include commercially available products such as "Novatec PP" and "WINTEC" (manufactured by Japan Polypropylene Corporation), "NOTIO" and "TAFMER XR" (manufactured by Mitsui Chemicals, Inc.), "Zelas" and "Thermorun" (manufactured by Mitsubishi Chemical Corporation), "Sumitomo Noblen" and "Tafthren" (manufactured by Sumitomo Chemical Co., Ltd.), "Prime PP" and "Prime TPO" (manufactured by Prime Polymer Co., Ltd.), "Adflex", "Adsyl", and "HMS-PP (PF814)" (manufactured by SunAllomer Co., Ltd.), and "Versify" and "Inspire" (manufactured by The Dow Chemical Company).

[0032] (Thermoplastic resin (a1) content) The resin composition (A) constituting the entire intermediate layer [I] formed from a plurality of layers contains a thermoplastic resin (a1). In the resin composition (A), the content of the thermoplastic resin (a1) in the resin composition (A) is preferably 60 to 95 mass %, more preferably 65 to 90 mass %, and further preferably 70 to 88 mass %. When the content of the thermoplastic resin (a1) in the resin composition (A) is within the above range, the dispersibility of the conductive filler (a2) is good, the mechanical strength of the film is ensured, and when the outer layer is peeled off from the laminated film, the peeling of the outer layer is stabilized, making it easier to obtain a laminated film that has excellent peelability between the intermediate layer and both outer layers.

[0033] The resin composition (A1) constituting the surface layer (i-1) of the intermediate layer [I] contains a thermoplastic resin (a1). In the resin composition (A1), the content of the thermoplastic resin (a1) in the resin composition (A1) is preferably 60 to 98 mass %, more preferably 65 to 95 mass %, and further preferably 70 to 90 mass %. When the content of the thermoplastic resin (a1) in the resin composition (A1) is within the above range, the dispersibility of the conductive filler (a2) is good, the mechanical strength of the film is ensured, and when the outer layer is peeled off from the laminated film, the peeling of the outer layer is stabilized, making it easier to obtain a laminated film that has excellent peelability between the intermediate layer and both outer layers.

[0034] The resin composition (A2) constituting the intermediate layer (i-2) of the intermediate layer [I] contains a thermoplastic resin (a1). In the resin composition (A2), the content of the thermoplastic resin (a1) in the resin composition (A2) is preferably 60 to 99.5 mass %, more preferably 65 to 99 mass %, and further preferably 70 to 98 mass %. When the content of the thermoplastic resin (a1) in the resin composition (A2) is within the above range, the dispersibility of the conductive filler (a2) is good, the mechanical strength of the film is ensured, and it becomes easier to obtain an intermediate layer having excellent mechanical properties such as tensile elongation at break.

[0035] (Conductive filler (a2)) The resin composition (A) constituting the entire intermediate layer [I] formed from a plurality of layers contains a conductive filler (a2). When the intermediate layer [I] is a layer formed of two or three layers, the resin composition (A1) constituting the surface layer (i-1) and the resin composition (A2) constituting the middle layer (i-2) contain a conductive filler (a2).

[0036] The conductive filler (a2) is not particularly limited, and examples thereof include carbon fillers such as carbon black, carbon nanotubes, carbon nanofibers, graphite carbon, and carbon fibers; powdered or fibrous metals; metal oxides; metal nitrides; etc. Among these, carbon fillers are preferred, and at least one selected from carbon nanotubes and carbon black is more preferred. The conductive filler contained in the resin composition (A) constituting the entire intermediate layer [I], the resin composition (A1) constituting the surface layer (i-1), and the resin composition (A2) constituting the middle layer (i-2) is preferably carbon nanotubes, which can easily provide good conductivity even in small amounts and can easily keep the peel strength between the intermediate layer and both outer layers below a specific range (less than 0.1 N / cm). On the other hand, from the viewpoint of economy, carbon black is preferable. In particular, the conductive filler contained in the resin composition (A2) constituting the intermediate layer (i-2) is preferably carbon nanotubes, from the viewpoint of obtaining an intermediate layer having excellent mechanical properties such as tensile elongation at break.

[0037] The carbon nanotubes may be either single-walled or multi-walled carbon nanotubes. The method for producing the carbon nanotubes is not particularly limited, and any of pyrolysis methods such as thermal CVD and plasma CVD, arc discharge, and laser evaporation may be used. In the present invention, for example, carbon nanotubes described in JP 2018-127397 A can be used.

[0038] On the other hand, specific examples of carbon black include ketjen black, acetylene black, furnace black, channel black, carbon black produced as a by-product in the production of a synthetic gas containing hydrogen and carbon monoxide by partially oxidizing a hydrocarbon such as naphtha in the presence of hydrogen and oxygen, or carbon black obtained by oxidizing or reducing the carbon black, among which acetylene black and ketjen black are preferred. One or more of these carbon blacks may be used.

[0039] The carbon black is preferably in a particulate form with an aspect ratio of 1 to 5. When the carbon black is in a particulate form, the aspect ratio refers to the value obtained by dividing the length of the major axis of the spherical components constituting the carbon black structure by the length of the minor axis of the spherical components. When the carbon black is in a fibrous form, the aspect ratio refers to the value obtained by dividing the fiber length by the fiber diameter.

[0040] The average primary particle size of carbon black is preferably 10 nm or more, more preferably 20 nm or more. On the other hand, the upper limit is preferably 60 nm or less, more preferably 50 nm or less. By making the average primary particle size of carbon black 10 nm or more, the dispersibility in the resin composition (A) can be improved, and the occurrence of agglomerates due to non-dispersion of carbon black can be reduced. On the other hand, by making the average primary particle size of carbon black 60 nm or less, the volume resistivity, which is an index of conductivity when dispersed in the resin composition (A), can be reduced, and good conductivity can be obtained.

[0041] The DBP oil absorption of carbon black is preferably 50 ml / 100 g or more as a lower limit, more preferably 100 ml / 100 g or more. On the other hand, the upper limit is preferably 750 ml / 100 g or less, more preferably 400 ml / 100 g or less. When the DBP oil absorption is 50 ml / 100 g or more, the structure is large and good electrical conductivity can be obtained. On the other hand, when the DBP oil absorption is 750 ml / 100 g or less, the dispersibility in the resin composition (A) is improved, and it is possible to prevent the formation of agglomerates due to undispersed carbon black. DBP oil absorption indicates the degree of structure in which particles are aggregated through chemical or physical bonds due to the amount of dibutyl phthalate (DBP) used to fill the gaps between carbon black particles, and is the amount (ml) of DBP that can be contained per 100 g of carbon black.

[0042] Examples of carbon black that can be used include commercially available products under the trade names "BLACK PEARLS," "VULCAN," and "STERLING" (manufactured by Cabot Corporation), "Ketjen Black EC" (manufactured by Lion Specialty Chemicals), "Denka Black" (manufactured by Denki Kagaku Kogyo Co., Ltd.), "Toka Black" (manufactured by Tokai Carbon Co., Ltd.), "Asahi Carbon Black" (manufactured by Asahi Carbon Co., Ltd.), and "Mitsubishi Carbon Black" (manufactured by Mitsubishi Chemical Corporation).

[0043] (Conductive filler (a2) content) The resin composition (A) constituting the entire intermediate layer [I] formed from a plurality of layers contains a conductive filler (a2). In the resin composition (A), the content of the conductive filler (a2) in the resin composition (A) is preferably 0.1 mass % or more and 50 mass % or less, more preferably 1 to 40 mass %, even more preferably 2 to 30 mass %, even more preferably 2 to 20 mass %, and even more preferably 3 to 15 mass %. When the content of the conductive filler (a2) in the resin composition (A) is within the above range, the conductive filler can be well dispersed in the resin composition (A) and the conductive filler is less likely to form agglomerates due to undispersed conductive filler. This makes it easier to obtain a laminated film having a good appearance and an intermediate layer with high conductivity. In particular, when the conductive filler (a2) contained in the resin composition (A) is a carbon nanotube, the content of the carbon nanotube in the resin composition (A) is preferably 0.1 to 20 mass%, more preferably 0.5 to 15 mass%, even more preferably 1 to 10 mass%, and even more preferably 1.5 to 8 mass%. When the conductive filler (a2) contained in the resin composition (A) is carbon black, the content of the carbon black in the resin composition (A) is preferably 1 to 40 mass%, more preferably 3 to 35 mass%, even more preferably 5 to 30 mass%, and still more preferably 7 to 20 mass%.

[0044] When the intermediate layer [I] is a layer formed of two or three layers, the resin composition (A1) constituting the surface layer (i-1) contains a conductive filler (a2). In the resin composition (A1), the content of the conductive filler (a2) in the resin composition (A1) is preferably 0.1 to 20 mass %, more preferably 0.5 to 15 mass %, even more preferably 1 to 10 mass %, and even more preferably 1.5 to 8 mass %. When the content of the conductive filler (a2) in the resin composition (A1) is within the above range, the conductive filler has good dispersibility in the resin composition (A1) and is less likely to form agglomerates due to undispersed conductive filler. This makes it easier to obtain a laminate film having a good appearance and an intermediate layer with high conductivity. In particular, when the conductive filler (a2) contained in the resin composition (A1) is a carbon nanotube, the content of the carbon nanotube in the resin composition (A1) is preferably 0.1 to 20 mass%, more preferably 0.5 to 15 mass%, even more preferably 1 to 10 mass%, and even more preferably 1.5 to 8 mass%. When the conductive filler (a2) contained in the resin composition (A1) is carbon black, the content of the carbon black in the resin composition (A1) is preferably 1 to 40 mass%, more preferably 3 to 35 mass%, even more preferably 5 to 30 mass%, and still more preferably 7 to 20 mass%.

[0045] When the intermediate layer [I] is a layer formed of two or three layers, the resin composition (A2) constituting the intermediate layer (i-2) contains a conductive filler (a2). In the resin composition (A2), the content of the conductive filler (a2) in the resin composition (A2) is preferably 1 to 40 mass %, more preferably 1.5 to 35 mass %, even more preferably 2 to 30 mass %, and even more preferably 3 to 25 mass %. When the content of the conductive filler (a2) in the resin composition (A2) is within the above range, the conductive filler has good dispersibility in the resin composition (A2) and is less likely to form agglomerates due to undispersed conductive filler. This makes it easier to obtain a laminate film having an intermediate layer with good appearance and high conductivity, and makes it easier to obtain an intermediate layer with excellent mechanical properties such as tensile elongation at break. In particular, when the conductive filler (a2) contained in the resin composition (A2) is carbon nanotubes, the content of the carbon nanotubes in the resin composition (A2) is preferably 0.1 to 20 mass%, more preferably 0.5 to 15 mass%, even more preferably 1 to 10 mass%, and even more preferably 1.5 to 8 mass%. When the conductive filler (a2) contained in the resin composition (A2) is carbon black, the content of the carbon black in the resin composition (A2) is preferably 1 to 40 mass%, more preferably 1.5 to 35 mass%, even more preferably 2 to 30 mass%, and still more preferably 3 to 25 mass%.

[0046] (Carboxylic acid modified polyolefin resin (a3)) The resin composition (A1) constituting the surface layer (i-1) of the intermediate layer [I] preferably contains a carboxylic acid-modified polyolefin resin (a3) ​​from the viewpoint of improving the coatability of an aqueous liquid to the intermediate layer [I]. The carboxylic acid modified polyolefin resin (a3) ​​is a polyolefin resin modified with a carboxylic acid. The polyolefin resin to be modified with a carboxylic acid may be the same as the polyolefin resin described as the thermoplastic resin (a1). Examples of carboxylic acid compounds used for the carboxylic acid modification include acid anhydrides such as maleic anhydride, phthalic anhydride, acetic anhydride, and succinic anhydride, methacrylic acid, maleic acid, and acrylic acid. Among these, at least one selected from maleic anhydride, methacrylic acid, maleic acid, and acrylic acid is preferred, and maleic anhydride is more preferred. The carboxylic acid-modified polyolefin resin (a3) ​​may be formed by a copolymerization reaction between a raw material monomer of a polyolefin resin and a carboxylic acid compound, or may be formed by an addition reaction of a polyolefin resin with a carboxylic acid compound. The carboxylic acid-modified polyolefin resin (a3) ​​is preferably a maleic acid-modified polyolefin resin, more preferably a maleic acid-modified polypropylene resin or a maleic acid-modified polyethylene resin, and even more preferably a maleic acid-modified polypropylene resin. The polyolefin resin used in the carboxylic acid-modified polyolefin resin (a3) ​​and the polyolefin resin used in the thermoplastic resin (a1) may be the same or different.

[0047] The acid value of the carboxylic acid-modified polyolefin resin (a3) ​​is preferably 1 to 70 mgKOH / g, more preferably 10 to 65 mgKOH / g, and even more preferably 20 to 60 mgKOH / g, from the viewpoint of improving the coatability of an aqueous liquid to the intermediate layer [I]. When the acid value of the carboxylic acid-modified polyolefin resin (a3) ​​is within the above range, the surface wetting index of at least one of the surface layers (i-1) of the intermediate layer [I] can be made to be a specific value or more, making it easier to uniformly apply an aqueous liquid to the surface of the intermediate layer [I].

[0048] As the carboxylic acid modified polyolefin resin (a3), for example, commercially available products such as "UMEX 1001" and "UMEX 1010" (manufactured by Sanyo Chemical Industries, Ltd.) can be used.

[0049] (Content of carboxylic acid modified polyolefin resin (a3)) The resin composition (A1) constituting the surface layer (i-1) of the intermediate layer [I] preferably contains a carboxylic acid-modified polyolefin resin (a3). In the resin composition (A1), the content of the carboxylic acid-modified polyolefin resin (a3) ​​in the resin composition (A1) is preferably 5 mass% or more and 50 mass% or less, more preferably 5 to 40 mass%, even more preferably 5 to 30 mass%, and even more preferably 7 to 25 mass%. When the content of the carboxylic acid-modified polyolefin resin (a3) ​​is within the above range, the surface wetting index of at least one of the surface layers (i-1) of the intermediate layer [I] can be made to be a specific value or more, making it easier to uniformly apply an aqueous liquid to the surface of the intermediate layer [I].

[0050] (Additives) The resin composition (A) constituting the entire intermediate layer [I] formed from multiple layers, the resin composition (A1) constituting the surface layer (i-1) of the intermediate layer [I], and the resin composition (A2) constituting the middle layer (i-2) of the intermediate layer [I] may contain various additives as necessary to the extent that the properties of the intermediate layer [I] are not impaired. Examples of additives include inorganic particles such as silica, talc, kaolin, and calcium carbonate; pigments such as titanium oxide and carbon black; flame retardants, weather resistance stabilizers, heat resistance stabilizers, antistatic agents, melt viscosity improvers, crosslinking agents, lubricants, nucleating agents, plasticizers, antioxidants, antioxidants, light stabilizers, ultraviolet absorbers, neutralizing agents, anti-fogging agents, anti-blocking agents, slip agents, and colorants. When an additive is used, its content in the resin composition (A) is usually 30% by mass or less, preferably 0.0001 to 20% by mass, more preferably 0.001 to 15% by mass, and further preferably 0.01 to 10% by mass.

[0051] (Tensile elongation at break of intermediate layer [I]) In the laminated film, the tensile elongation at break in the longitudinal direction (MD) of the intermediate layer [I] is preferably 100% or more, more preferably 120% or more, even more preferably 150% or more, even more preferably 200% or more, even more preferably 250% or more, and even more preferably 300% or more. Here, the upper limit of the tensile elongation at break is not particularly limited, but is usually 500% or less, preferably 400% or less. The tensile elongation at break in the machine direction (MD) of the intermediate layer [I] can be determined by the method described in the Examples.

[0052] (Thickness variation of middle layer [I]) In the laminate film, the thickness variation of the intermediate layer [I] is preferably less than ±10 μm, more preferably ±8 μm or less, even more preferably ±5 μm or less, and even more preferably ±3 μm or less. By ensuring that the thickness variation of the intermediate layer [I] is within the above range, the interface between the intermediate layer and both outer layers to be formed is stabilized, the appearance of the intermediate layer is improved, and when the outer layers are peeled off from the laminated film, peeling of the outer layers is stabilized, making it easier to obtain a laminated film that has excellent peelability between the intermediate layer and both outer layers. The thickness variation is usually expressed in %, but in the present invention, it is expressed in μm. The thickness variation of the intermediate layer [I] can be determined by the method described in the Examples.

[0053] (Thickness (X) of middle layer [I]) In the laminate film, the thickness (X) of the intermediate layer [I] is preferably 1 μm or more and 200 μm or less, more preferably 3 to 180 μm, even more preferably 5 to 150 μm, even more preferably 5 to 100 μm, and even more preferably 5 to 80 μm. When the thickness (X) of the intermediate layer [I] is within the above range, the handling properties during film formation are improved, and the mechanical strength of the film is easily obtained. Therefore, the intermediate layer [I] can be particularly advantageously used in applications where lightweight and thin conductive films are required. The thickness (X) of the intermediate layer [I] can be determined by the method described in the Examples.

[0054] (Thickness of surface layer (i-1)) In the intermediate layer [I], the thickness of the surface layer (i-1) is preferably 1 to 80 μm, more preferably 1.5 to 50 μm, even more preferably 2 to 30 μm, and even more preferably 3 to 25 μm. When the thickness of the surface layer (i-1) is within the above range, the handling property during film formation is improved, and the mechanical strength required for the film is easily obtained. The surface layer (i-1) can be determined by the method described in the Examples.

[0055] (Thickness of middle layer (i-2)) In the intermediate layer [I], the thickness of the intermediate layer (i-2) is preferably 2 to 160 μm, more preferably 3 to 100 μm, even more preferably 4 to 60 μm, and even more preferably 6 to 50 μm. When the thickness of the intermediate layer (i-2) is within the above range, the handling properties during film formation are improved, and an intermediate layer having excellent mechanical properties such as tensile elongation at break is easily obtained. The intermediate layer (i-2) can be determined by the method described in the Examples.

[0056] (Thickness ratio of middle layer (i-2) to surface layer (i-1)) In the intermediate layer [I], the thickness ratio ((i-2) / (i-1)) of the middle layer (i-2) to the surface layer (i-1) is preferably 0.5 or more and 20 or less, more preferably 0.75 to 10, even more preferably 1.0 to 8, and even more preferably 1.2 to 5, from the viewpoint of film appearance and mechanical properties. Here, the thicknesses of the two surface layers (i-1) may be different, but are preferably the same. Such a thickness ratio can be adjusted by appropriately adjusting the extrusion amounts of the surface layers and the middle layer. In addition, within the above range, the film appearance and mechanical properties are favorable, which is preferable.

[0057] (Thickness ratio (Y / X) of the two outer layers [II] to the middle layer [I]) In the laminated film, the ratio (Y / X) of the thickness (Y) of each of the two outer layers [II] to the thickness (X) of the intermediate layer [I] is preferably from 1 to 5, more preferably from 1 to 4.5, even more preferably from 1 to 4, and even more preferably from 1 to 3.5. Here, the thicknesses of the layers of the two outer layers [II] may be different from each other, but are preferably the same. The thickness of the intermediate layer [I] and the thickness of each of the outer layers [II] can be set by appropriately adjusting the extrusion amount and extrusion speed of the resin compositions (A) and (B), the temperature and take-up speed of the casting roll, the lip gap of the T-die, the resin temperature during extrusion, and the like. When the thickness ratio (Y / X) is within the above range, it becomes easier to obtain a laminated film that has small thickness variation, a good appearance, an intermediate layer with high conductivity, and excellent peelability between the intermediate layer and both outer layers. On the other hand, if the thickness ratio (Y / X) is outside the above range, the thickness will fluctuate significantly, and the film will have poor appearance such as uneven flow or holes, and only an intermediate layer with poor conductivity will be obtained. In addition, when peeling the outer layer from the laminated film, the peeling of the outer layer will be unstable and stick-slip (catching) will occur, and so there is a risk that only a laminated film with poor peelability between the intermediate layer and both outer layers will be obtained.

[0058] (Peel strength between intermediate layer [I] and both outer layers [II]) In the laminated film of the present invention, the peel strength between the intermediate layer [I] and both outer layers [II] when T-type peeling is performed at a peeling speed of 100 mm / min in an environment at a temperature of 25° C. is preferably less than 0.1 N / cm, more preferably 0.08 N / cm or less, even more preferably 0.06 N / cm or less, even more preferably 0.04 N / cm or less, and even more preferably 0.035 N / cm or less. The lower limit is not particularly limited, but is preferably 0.001 N / cm, more preferably 0.005 N / cm, and even more preferably 0.01 N / cm. The peel strength between the intermediate layer [I] and both outer layers [II] can be set by, for example, setting the ratio (Y / X) of the thickness (Y) of both outer layers [II] to the thickness (X) of the intermediate layer [I] to be 1 or more and 5 or less, and by appropriately adjusting the type of conductive filler (a2), the type of resin constituting the intermediate layer [I], the type of resin constituting both outer layers [II], the melt viscosity of the resin constituting the intermediate layer [I], and the melt viscosity of the resin constituting both outer layers [II], etc. When the peel strength between the intermediate layer and both outer layers is within the above range, not only is it possible to suppress peeling defects such as adhesion of parts of both outer layers to the intermediate layer, but it is also possible to peel the outer layers smoothly and quickly from the intermediate layer, thereby improving the surface quality of the intermediate layer that can become a conductive film, and further improving the productivity of the conductive film, the current collector using the conductive film, and the battery using the conductive film. In addition, by ensuring that the peel strength between the intermediate layer and both outer layers is within the above range, it is possible to suppress the problem of the outer layers peeling off from the intermediate layer when the laminated film is wound up, while also preventing peeling defects such as parts of the outer layers adhering to the intermediate layer when peeling the outer layers from the laminated film. The peel strength between the intermediate layer and both outer layers can be determined by the method described in the Examples.

[0059] (Volume resistivity of intermediate layer [I]) In the laminate film, the volume resistivity of the intermediate layer [I] is preferably 500 Ω·cm or less, more preferably 300 Ω·cm or less, even more preferably 200 Ω·cm or less, even more preferably 100 Ω·cm or less, and even more preferably 80 Ω·cm or less. When the volume resistivity of the intermediate layer [I] is within the above range, a laminated film having an intermediate layer with high conductivity can be obtained, and the intermediate layer obtained by peeling and removing both outer layers from the laminated film can be used particularly advantageously in conductive film applications. The volume resistivity of the intermediate layer [I] can be determined by the method described in the Examples.

[0060] <Both Outer Layers [II]> Both outer layers [II] can function as protective films that protect the conductive film, which is the intermediate layer [I], without being peeled off until use.

[0061] (Thickness (Y) of both outer layers [II]) In the laminated film, the thickness (Y) of each of the two outer layers [II] is preferably 5 μm or more and 150 μm or less, more preferably 10 to 150 μm, even more preferably 20 to 130 μm, and even more preferably 25 to 100 μm. Here, the thicknesses of the two outer layers [II] may be different from each other, but are preferably the same. When the thickness (Y) of each of the two outer layers [II] is within the above range, the interface between the intermediate layer and both outer layers is formed stably, the appearance of the intermediate layer is good, and when the outer layer is peeled off from the laminated film, the peeling of the outer layer is stable, making it easier to obtain a laminated film that has excellent peelability between the intermediate layer and both outer layers. The thickness (Y) of each of the outer layers [II] can be determined by the method described in the Examples.

[0062] (Resin composition (B)) Both outer layers [II] are layers made of a resin composition (B) containing a thermoplastic resin (b1).

[0063] (Thermoplastic resin (b1)) The thermoplastic resin (b1) is not particularly limited, but from the viewpoints of stably peeling the outer layer when peeling it from the laminated film and of improving the peelability between the intermediate layer and both outer layers, it is preferable to use one or more types selected from polyester-based resins, polycarbonate-based resins, and polystyrene-based resins. In particular, when a polyolefin-based resin (preferably a polypropylene-based resin) is used as the thermoplastic resin (a1) constituting at least one of the surface layers (i-1) of the intermediate layer [I], the thermoplastic resin (b1) is preferably one or more selected from polyester-based resins, polycarbonate-based resins, and polystyrene-based resins, and more preferably a polyester-based resin.

[0064] (Additives) In addition to the thermoplastic resin (b1), the resin composition (B) may contain various additives as necessary, provided that the properties of both outer layers [II] are not impaired. Examples of additives include inorganic particles such as silica, talc, kaolin, and calcium carbonate, pigments such as titanium oxide and carbon black, flame retardants, weathering stabilizers, heat stabilizers, antistatic agents, melt viscosity modifiers, crosslinking agents, lubricants, nucleating agents, plasticizers, antioxidants, antioxidants, light stabilizers, ultraviolet absorbers, neutralizers, antifogging agents, antiblocking agents, slip agents, and colorants. When an additive is used, its content in the resin composition (B) is usually 30% by mass or less, preferably 0.0001 to 20% by mass, more preferably 0.001 to 15% by mass, and further preferably 0.01 to 10% by mass.

[0065] (Layer structure of laminated film) The laminated film in the present invention is not particularly limited as long as it is constructed by laminating outer layers [II] on both sides of an intermediate layer [I], but it can also be constructed as a four-layer or more structure in which another layer [III] is laminated on at least one of the two outer layers [II] within a range that does not impair the effects of the present invention. Specific examples of the other layer [III] include a strength retaining layer, a heat-resistant layer, an adhesive layer, and a barrier layer. Examples of the layer structure of the laminated film in the present invention include the following embodiments. ·Outer layer [II] / Intermediate layer [I] / Outer layer [II] Outer layer [II] / middle layer [I] / outer layer [II] / other layers [III] Other layers [III] / Outer layer [II] / Middle layer [I] / Outer layer [II] / Other layers [III] The laminated film of the present invention preferably has a three-layer structure in which an intermediate layer [I] and outer layers [II] are laminated on both sides of the intermediate layer [I], but the total number of layers can be appropriately adjusted depending on the application and purpose of use.

[0066] (Thickness of laminated film) The thickness of the laminated film is not limited, but is preferably 20 μm or more and 400 μm or less, more preferably 25 to 400 μm, even more preferably 30 to 350 μm, and even more preferably 50 to 300 μm.

[0067] [Laminated film manufacturing method] The method for producing the laminated film in the present invention is not particularly limited as long as it is a method that can form the intermediate layer into a layer formed from a plurality of layers. As a method for producing a laminated film, for example, when the intermediate layer [I] is a layer formed of two or three layers, an extrusion molding machine equipped with an extruder, a die, a cooling machine, a take-up machine (cast roll), and a cutter is used, and the resin composition (A1) constituting at least one surface layer (i-1) for the intermediate layer, the resin composition (A2) constituting the middle layer (i-2) for the intermediate layer, and the resin composition (B) for the outer layer are each put into separate hoppers of the extruder, melted and plasticized at a predetermined temperature, co-extruded under predetermined film-forming conditions from the lip gap, which is the discharge port of the T-die, and introduced at a predetermined speed to a cast roll at a predetermined temperature, and then cooled and solidified to obtain a laminated film. In addition, a multi-manifold die and a feed block can be used for laminating each layer.

[0068] In the method for producing a laminated film, the ratio (x1 / X) of the thickness (x1) of the intermediate layer [I] at the lip portion during co-extrusion to the thickness (X) of the intermediate layer [I] in the laminated film after film formation is 0.5 to 40, preferably 1 to 35, more preferably 2 to 30, even more preferably 3 to 25, and particularly preferably 9 to 20. When the thickness ratio (x1 / X) is within the above range, the interfaces between the intermediate layer and both outer layers to be formed are stabilized, making it easier to obtain a laminated film with small thickness fluctuation, good appearance, and excellent peelability between the intermediate layer and both outer layers. The thickness (x1) of the intermediate layer [I] in the lip portion and the thickness (X) of the intermediate layer [I] in the laminated film after film formation can be appropriately adjusted by film formation conditions such as the extrusion amount and extrusion speed of the resin composition, the temperature and take-up speed of the casting roll, the lip gap of the T-die, and the resin temperature during extrusion.

[0069] The thickness (x1) of the intermediate layer [I] at the lip portion during co-extrusion is preferably 100 μm or more and 500 μm or less, more preferably 120 to 400 μm, even more preferably 130 to 350 μm, and even more preferably 120 to 300 μm. When the thickness (x1) of the intermediate layer [I] in the lip portion is within the above range, the film can be easily handled during film formation, and the thickness of the intermediate layer [I] in the laminated film after film formation can be easily adjusted to a specific range (preferably 1 μm or more and 200 μm or less). The thickness (x1) of the intermediate layer [I] at the lip can be calculated by calculating the cross-sectional area ratio of the intermediate layer at the lip from the ratio of the extrusion amount of the intermediate layer to the extrusion amount of all layers, and then multiplying the cross-sectional area ratio by the lip gap. The thickness (x1) of the intermediate layer [I] at the lip can be calculated by the formula: Thickness (x1) of the intermediate layer at the lip = (Extrusion amount of intermediate layer / Extrusion amount of all layers) x Lip gap.

[0070] The thickness (X) of the intermediate layer [I] in the laminate film after film formation is preferably 1 μm or more and 200 μm or less, more preferably 3 to 180 μm, even more preferably 5 to 150 μm, even more preferably 5 to 100 μm, and even more preferably 5 to 80 μm. When the thickness (X) of the intermediate layer [I] is within the above range, the handling properties during film formation are improved, and the mechanical strength of the film is easily obtained. Therefore, the intermediate layer [I] can be particularly advantageously used in applications where lightweight and thin conductive films are required. The thickness (X) of the intermediate layer [I] can be determined by the method described in the Examples.

[0071] The temperature at which the resin composition (A1) constituting at least one surface layer (i-1) for the intermediate layer, the resin composition (A2) constituting the middle layer (i-2) for the intermediate layer, and the resin composition (B) for both outer layers are melt-plasticized, each of which is placed in a separate hopper of the extruder, is preferably 190 to 350°C, more preferably 195 to 300°C, and even more preferably 200 to 280°C. When the melt plasticizing temperature is within the above range, the handling property during film formation can be improved, and the flowability and moldability of the resin composition can be improved.

[0072] The temperature of the casting roll is preferably 70 to 150° C., more preferably 80 to 140° C., and even more preferably 90 to 130° C. The take-up speed of the casting roll is preferably 1.0 to 20 m / min, more preferably 2.0 to 15 m / min, and even more preferably 3.0 to 15 m / min. By setting the temperature of the casting roll and the take-up speed within the above ranges, the thickness of the intermediate layer [I] and the thicknesses of both outer layers [II] can be set within the desired ranges.

[0073] (Laminated film processing) The laminated film of the present invention may be subjected to a stretching process, or a surface treatment such as a corona treatment, a plasma treatment, a printing, a coating, or a vapor deposition, depending on the application and purpose of use, in order to improve physical properties such as mechanical strength, as long as the effects of the present invention are not impaired.

[0074] [Conductive film] The conductive film of the present invention is a conductive film made of a resin composition (A) containing a thermoplastic resin (a1) and a conductive filler (a2), the conductive film being a layer formed from multiple layers, and at least one surface layer (i-1) of the conductive film has a surface wetting index of 30 dyne / cm or more. The conductive film of the present invention is obtained by peeling and removing both outer layers of a laminated film. The conductive film may be obtained by peeling and removing both outer layers immediately after the production of the laminated film, or may be obtained by storing the laminated film and then peeling and removing both outer layers as necessary. It is preferable to store the conductive film in the form of a laminated film from the viewpoint of improving the handling property during transportation.

[0075] [Current collectors and batteries] The conductive film of the present invention has excellent coatability with aqueous liquids, excellent mechanical properties such as tensile elongation at break, small thickness variation, good appearance, and high conductivity, and can therefore be suitably used as a current collector and in batteries (e.g., lithium ion batteries). EXAMPLES

[0076] Next, the laminated film of the present invention will be described in detail with reference to examples and comparative examples, but the present invention is not limited to these.

[0077] Example 1 Surface layer (i-1) of intermediate layer [I] A resin composition (A1) was used, which contained 76 mass% of a polypropylene-based resin as the thermoplastic resin (a1), 4 mass% of carbon nanotubes as the conductive filler (a2), and 20 mass% of a maleic acid-modified polypropylene-based resin (manufactured by Sanyo Chemical Industries, Ltd., "UMEX 1001": acid value 26 mgKOH / g) as the carboxylic acid-modified polyolefin-based resin (a3). · Middle layer (i-2) of the middle layer [I] A resin composition (A2) containing 96 mass % of a polypropylene resin as the thermoplastic resin (a1) and 4 mass % of carbon nanotubes as the conductive filler (a2) was used. Both outer layers [II] As the thermoplastic resin (b1), a resin composition (B) made of polyethylene terephthalate (product name: ECOZEN T110, manufactured by SK Chemicals), which is a polyester-based resin, was used. The die used in the extrusion molding machine was a T-die with a lip gap adjustment mechanism of the actuation bolt type, and the lip gap at the discharge port of the T-die was set to 0.7 mm. A multi-manifold die and a feed block were used to stack each layer. An extrusion molding machine equipped with an extruder, a die, a cooler, a take-up (cast roll), and a cutter was used. Resin composition (A1) was put into the hopper of an extruder, resin composition (A2) was put into the hopper of another extruder, and resin composition (B) was put into the hopper of another extruder, the heater temperature was set to 240 ° C, and each resin composition was melted and plasticized in the extruder, and co-extruded from the lip of the T-die under the film-forming conditions shown in Table 1, guided to a cast roll at 100 ° C, and then cooled and solidified to obtain a laminated film ([II] / [I] / [II]). The thicknesses of the surface layers (i-1) arranged on both sides of the middle layer (i-2) of the intermediate layer were the same. The thicknesses of the outer layers arranged on both sides of the intermediate layer were also the same. Furthermore, the two outer layers [II] were peeled off from the obtained laminated film using a multi-axis winding slitter to obtain an intermediate layer [I] (conductive film). The obtained intermediate layer [I] (conductive film) and both outer layers [II] were evaluated by the methods described below. The evaluation results are shown in Table 1.

[0078] Example 2 Surface layer (i-1) of intermediate layer [I] A resin composition (A1) was used, which contained 86 mass% of a polypropylene-based resin as the thermoplastic resin (a1), 4 mass% of carbon nanotubes as the conductive filler (a2), and 10 mass% of a maleic acid-modified polypropylene-based resin (manufactured by Sanyo Chemical Industries, Ltd., "UMEX 1010": acid value 52 mgKOH / g) as the carboxylic acid-modified polyolefin-based resin (a3). · Middle layer [I] (i-2) A resin composition (A2) containing 76 mass % of a polypropylene resin as the thermoplastic resin (a1) and 24 mass % of carbon black as the conductive filler (a2) was used. Both outer layers [II] As the thermoplastic resin (b1), a resin composition (B) made of polyethylene terephthalate (product name: ECOZEN T110, manufactured by SK Chemicals), which is a polyester-based resin, was used. A laminated film ([II] / [I] / [II]) was obtained in the same manner as in Example 1 under the film-forming conditions shown in Table 1, using resin composition (A1) for the surface layer (i-1) of the intermediate layer [I], resin composition (A2) for the middle layer (i-2) of the intermediate layer [I], and resin composition (B) for both outer layers [II].

[0079] Comparative Example 1 ·Middle class [I] A resin composition (A1) containing 76 mass % of a polypropylene-based resin as the thermoplastic resin (a1) and 24 mass % of carbon black as the conductive filler (a2) was used. Both outer layers [II] As the thermoplastic resin (b1), a resin composition (B) made of polyethylene terephthalate (product name: ECOZEN T110, manufactured by SK Chemicals), which is a polyester-based resin, was used. A laminated film ([II] / [I] / [II]) was obtained in the same manner as in Example 1 under the film-forming conditions shown in Table 1, using resin composition (A1) for the intermediate layer [I] and resin composition (B) for both outer layers [II].

[0080] (Wetting Index) The intermediate layer (conductive film) obtained by peeling off both outer layers from a laminated film (width: 400 mm, length: 400 mm) was used as the measurement subject, and the wettability index of the conductive film surface was measured in accordance with JIS K6768:1999.

[0081] (Coatability evaluation) The intermediate layer (conductive film) obtained by peeling off and removing both outer layers from a laminated film (width: 400 mm, length: 400 mm) was used as the measurement subject. A negative electrode aqueous paint (a negative electrode aqueous paint formed by mixing a negative electrode active material, a binder, and an aqueous solvent) was applied to the conductive film, and the state of the application was visually observed and evaluated according to the following criteria. A: The amount of repelling that occurs on the surface of the conductive film is less than 10%. B: The amount of repelling that occurs on the surface of the conductive film is 10% or more and less than 50%. C: Repelling occurred on the surface of the conductive film in 50% or more areas.

[0082] (Tensile elongation at break) The intermediate layer (conductive film) obtained by peeling off both outer layers from the laminated film (width: 400 mm, length: 400 mm) was cut into a rectangular shape (width: 15 mm, length: 150 mm) so that the longitudinal direction (MD) of the film was the long axis to prepare a test piece, and the tensile elongation at break was measured using an autograph AGX-V manufactured by Shimadzu Corporation. A gauge was placed at 50 mm intervals in the center of the test piece, and a tensile test was performed using a tensile tester with a gripping distance of 50 mm and a tensile speed of 200 mm / min to measure the elongation at break and obtain the tensile elongation at break in the longitudinal direction (MD).

[0083] (Thickness of middle layer (X), thickness variation of middle layer) The intermediate layer (conductive film) obtained by peeling off and removing both outer layers from the laminated film (width: 400 mm, length: 400 mm) was used as the measurement subject. The thickness was measured using a 1 / 1000 mm dial gauge at three random locations at the center point in the width direction (TD) of the film and six random locations 100 mm to the left and right in the width direction from the center point, for a total of nine locations, and the average value was taken as the thickness (X) of the intermediate layer. The difference between each thickness value of the intermediate layer measured at a total of nine locations and the average thickness value of the intermediate layer measured at a total of nine locations was calculated, and the difference between the maximum and minimum values ​​obtained by the calculation was divided by 2 to obtain the thickness variation.

[0084] (Thickness of the surface layer (i-1) of the intermediate layer, thickness of the middle layer (i-2) of the intermediate layer) The intermediate layer was cut in the cross-sectional direction using a microtome, and the cut surface was observed under a microscope to measure the thickness of the surface layer (i-1) and the thickness of the intermediate layer (i-2).

[0085] (Thickness of both outer layers (Y)) Both outer layers peeled off from the laminated film were used as the measurement objects, and the thickness (Y) of both outer layers was determined in the same manner as the thickness (X) of the intermediate layer described above.

[0086] (Peel strength between middle layer and both outer layers) Only one of the two outer layers was peeled off from the laminated film, and the film was cut into a strip (width: 25 mm, length: 200 mm) with the longitudinal direction (MD) of the film as the long axis. A total of five such strips were prepared in the same manner and used as the measurement subjects. The outer layer of the strip-shaped film to be measured was T-peeled down to a length of 50 mm, and then the remaining outer layer (length 150 mm) was T-peeled at a peeling speed of 100 mm / min in an environment at 25°C to measure the tensile stress, and the maximum value was taken as the peel strength. The average peel strength of the five strip-shaped films was calculated and used as the peel strength between the intermediate layer and both outer layers.

[0087] (Volume resistivity of conductive film) The volume resistivity of the conductive film was measured by the four-terminal method using a Loresta AP (product name: Mitsubishi Chemical Corporation) in accordance with JIS K7194 for samples cut into a size of 100 mm length x 100 mm width. Note that if the volume resistivity of the conductive film is 100 Ω cm or less, there is no problem in practical use and it was rated as "A."

[0088] (Appearance evaluation of conductive film) The appearance of the conductive film was visually observed and evaluated according to the following criteria. Perforated A: No holes are observed per meter in the longitudinal direction (MD) of the film. B: Less than two holes are found per meter in the longitudinal direction (MD) of the film. C: Two or more holes are found per meter in the longitudinal direction (MD) of the film. Uneven flow A: There are no irregularities on the film surface. B: Irregularities are observed in either the machine direction (MD) or the width direction (TD) of the film (vertical streaks). C: Irregularities are observed in both the machine direction (MD) and the width direction (TD) of the film.

[0089] [Table 1]

[0090] From the results shown in Table 1, the following was confirmed: It was confirmed that the laminated films obtained in Examples 1 and 2 have an intermediate layer (conductive film) with a wettability index of 30 dyne / cm or more, excellent applicability of aqueous liquid to the conductive film, excellent mechanical properties such as tensile elongation at break, small thickness variation, good appearance, high conductivity, and excellent peelability between the intermediate layer and both outer layers. On the other hand, the laminated film obtained in Comparative Example 1 had an intermediate layer (conductive film) with a wettability index of less than 30 dyne / cm, and it was confirmed that the coatability of the aqueous liquid to the conductive film and mechanical properties such as tensile elongation at break were inferior to those of the Examples. [Industrial Applicability]

[0091] According to the present invention, it is possible to provide a laminated film which has excellent coatability with aqueous liquids, excellent mechanical properties such as tensile elongation at break, small thickness variation, good appearance, an intermediate layer with high conductivity, and excellent peelability between the intermediate layer and both outer layers. Furthermore, according to the present invention, it is possible to provide a conductive film that has excellent coatability with aqueous liquids, excellent mechanical properties such as tensile elongation at break, small thickness variation, good appearance, and high conductivity.

Claims

1. A laminated film having an intermediate layer [I] made of a resin composition (A) containing a thermoplastic resin (a1) and a conductive filler (a2), and two outer layers [II] made of a resin composition (B) containing a thermoplastic resin (b1), The intermediate layer [I] is a layer formed of a plurality of layers, A laminate film, in which at least one surface layer (i-1) of the intermediate layer [I] has a surface wettability index of 30 dyne / cm or more.

2. At least one surface layer (i-1) of the intermediate layer [I] is a layer formed from a resin composition (A1) containing a thermoplastic resin (a1), a conductive filler (a2), and a carboxylic acid-modified polyolefin resin (a3). The laminate film according to claim 1.

3. The laminate film according to claim 2, wherein the content of the carboxylic acid-modified polyolefin resin (a3) ​​in the resin composition (A1) is 5% by mass or more and 50% by mass or less.

4. The laminate film according to claim 1, wherein the intermediate layer [I] is a two-layer structure of surface layer (i-1) / middle layer (i-2) or a three-layer structure of surface layer (i-1) / middle layer (i-2) / surface layer (i-1).

5. The intermediate layer (i-2) of the intermediate layer [I] is a layer formed from a resin composition (A2) containing a thermoplastic resin (a1) and a conductive filler (a2) and substantially not containing a carboxylic acid-modified polyolefin resin (a3). The laminate film according to claim 4.

6. The laminated film according to claim 1, wherein the thickness variation of the intermediate layer [I] is less than ±10 μm.

7. The thickness (X) of the intermediate layer [I] is 1 μm or more and 100 μm or less, 2. The laminated film according to claim 1, wherein the ratio (Y / X) of the thickness (Y) of each of the outer layers [II] to the thickness (X) of the intermediate layer [I] is 1 or more and 5 or less.

8. 2. The laminated film according to claim 1, wherein the peel strength between the intermediate layer [I] and both outer layers [II] is less than 0.1 N / cm.

9. The laminate film according to claim 1 , wherein the thermoplastic resin (a1) is a polyolefin resin.

10. The laminated film according to claim 1 , wherein the conductive filler (a2) is a carbon nanotube.

11. The laminate film according to claim 1 , wherein the thermoplastic resin (b1) is a polyester-based resin.

12. 2. The laminate film according to claim 1, wherein the thickness of the laminate film is from 20 μm to 400 μm.

13. 2. The laminated film according to claim 1, wherein each of the outer layers [II] has a thickness of 5 μm or more and 150 μm or less.

14. The laminate film according to claim 1, wherein the content of the conductive filler (a2) in the resin composition (A) is 0.1 mass % or more and 50 mass % or less.

15. A conductive film, in which both outer layers [II] of the laminated film according to any one of claims 1 to 14 have been peeled off.

16. A conductive film made of a resin composition (A) containing a thermoplastic resin (a1) and a conductive filler (a2), The conductive film is a layer formed of multiple layers, A conductive film, wherein at least one surface layer (i-1) of the conductive film has a surface wettability index of 30 dyne / cm or more.

17. A current collector using the conductive film according to claim 15.

18. A battery using the conductive film according to claim 15.

Citation Information

Patent Citations

  • Manufacture of highly electroconductive film

    JP1986082611A

  • Production method of highly conductive film

    JP2014030899A

  • Laminate film

    JP2020157651A