Powder containing anion-modified cellulose nanofiber

Anion-modified cellulose nanofiber powders with controlled particle size and dispersion characteristics address the handling and workability issues of dried cellulose nanofibers, achieving reduced scattering and improved usability.

JP2024144090APending Publication Date: 2024-10-11NIPPON PAPER IND CO LTD
View PDF 1 Cites 0 Cited by

Patent Information

Application Number
JP2023216510
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Priority Date
2023-03-29
Filing Date
2023-12-22
Publication Date
2024-10-11

AI Technical Summary

Technical Problem

Dried cellulose nanofibers suffer from poor handling and workability due to scattering during processing and reduced properties post-drying, necessitating improved formulation to enhance their usability.

Method used

The development of anion-modified cellulose nanofiber powders with specific particle size, water content, and dispersion characteristics, including an average fiber diameter of 3-500 nm, water content of 20% or less, average particle diameter of 45 μm or more, and dispersion degree of less than 25%, along with defined angles of repose and collapse, to improve handling and workability.

Benefits of technology

The optimized powder formulation significantly reduces scattering and enhances handling and workability, ensuring easy redispersion and improved packaging performance.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024144090000001
    Figure 2024144090000001
Patent Text Reader

Abstract

To provide a powder containing anion-modified cellulose nanofiber having excellent handleability and workability.SOLUTION: There is provided a powder containing anion-modified cellulose nanofiber having an average fiber diameter of 3 to 500 nm, wherein the moisture content is 20 mass% or less, the average particle diameter is 45 μm or more and the degree of dispersion is less than 25%.SELECTED DRAWING: None
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a powder containing anionically modified cellulose nanofibers. [Background technology]

[0002] It is known that by introducing anionic groups such as carboxyl groups or carboxymethyl groups into cellulose molecular chains and mechanically processing (defibrating) them, they can be converted into cellulose nanofibers with nanoscale fiber diameters. Cellulose nanofibers are light, strong, and biodegradable, and their applications in a variety of fields are being considered.

[0003] Generally, cellulose nanofibers into which anionic groups have been introduced are produced in a state where they are stably dispersed in water, and are usually used in the form of a cellulose nanofiber dispersion of a given concentration for various purposes as an industrial material or an additive for food or cosmetics. In order to keep the state of the cellulose nanofiber stable, water is required that is several tens of times that of the cellulose nanofiber, but this high water content leads to increased costs for packaging, storage, transportation, etc. of the cellulose nanofiber, so the cellulose nanofiber is dried to produce a dried body, and when it is used, water is added to redisperse it, and it is used as a redispersion.

[0004] When an aqueous dispersion of cellulose nanofibers is dried to produce a dry solid, hydrogen bonds are formed between the fine cellulose fibers. As a result, even if water is added to this dry solid to redisperse it, the viscosity and other properties do not return to the same level as before drying, and drying methods are currently being investigated (Patent Document 1, etc.). [Prior art documents] [Patent documents]

[0005] [Patent Document 1] International Publication No. 2019 / 189318 Summary of the Invention [Problem to be solved by the invention]

[0006] Dried cellulose nanofibers are manufactured by subjecting cellulose nanofibers dispersed in water (wet state) to processes such as drying, crushing, classification, and recovery. The cellulose nanofiber powder manufactured in this way is then redispersed by adding water on the user's side, and used as a redispersion for various purposes. However, depending on the properties of the powder, dusting can occur during the process, making it difficult to handle and work with.

[0007] Therefore, an object of the present invention is to provide a powder containing anion-modified cellulose nanofibers that is easy to handle and work with. [Means for solving the problem]

[0008] As a result of extensive research into achieving this object, the present inventors have found that it is extremely effective to prepare a powder having a specific particle size and degree of dispersion, and have completed the present invention.

[0009] The present invention provides the following: (1) A powder containing anion-modified cellulose nanofibers having an average fiber diameter of 3 nm to 500 nm, a moisture content of 20 mass% or less, an average particle diameter of 45 μm or more, and a degree of dispersion of less than 25%. (2) The powder containing anion-modified cellulose nanofibers according to (1), having an angle of repose of 40 to 49°. (3) The powder containing anion-modified cellulose nanofibers according to (1), having a collapse angle of 15 to 24°. (4) The powder containing anion-modified cellulose nanofibers according to (1), wherein the difference angle is 20 to 25°. Effect of the Invention

[0010] According to the present invention, it is possible to provide a powder containing anion-modified cellulose nanofibers that is excellent in handleability and workability. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0011] The present invention will be described in detail below. In the present invention, "to" includes the end values. That is, "X to Y" includes the values ​​X and Y at both ends.

[0012] (Anion-modified cellulose nanofiber-containing powder) The present invention relates to a powder containing anion-modified cellulose nanofibers (anion-modified CNF) having an average fiber diameter of 3 nm to 500 nm, a moisture content of 20 mass% or less, an average particle diameter of 45 μm or more, and a degree of dispersion of less than 25%.

[0013] (moisture content) From the viewpoint of storage stability, the anion-modified CNF-containing powder of the present invention has a moisture content of 20% by mass or less, preferably 0 to 15% by mass, more preferably 0 to 10% by mass, and even more preferably 0 to 9.5% by mass. If the moisture content is higher than the upper limit, there is a problem that the possibility of spoilage increases. The powder may be dried to a moisture content of 0% (absolute dryness).

[0014] (Average particle size) From the viewpoint of ease of handling, the anion-modified CNF-containing powder of the present invention has a lower limit of the average particle diameter of 45 μm or more, preferably 50 μm or more, more preferably 60 μm or more, and an upper limit of 300 μm or less, preferably 250 μm or less, more preferably 150 μm or less. If the average particle diameter is too small, there is a problem that the powder is easily scattered and difficult to handle. Here, the average particle diameter (D50) is the particle diameter that includes 50% of the particle diameter distribution by volume, calculated from the minimum value. The particle diameter distribution can be measured using a laser diffraction / scattering type particle size distribution analyzer.

[0015] (Dispersion degree) From the viewpoint of handling and workability, the anion-modified CNF-containing powder of the present invention has a degree of dispersion of less than 25%, preferably less than 20%. The lower limit is preferably 8% or more. When the degree of dispersion is within the above range, the amount of scattering during the process is small, and the handling and workability are excellent. When the degree of dispersion is too large, the amount of scattering during the process increases, and the handling is poor. Furthermore, the workability is poor, such as poor sealing during packaging. On the other hand, when the degree of dispersion is too small, the flowability is low and the flowability is low, so clogging is likely to occur. The degree of dispersion can be measured using a powder property tester.

[0016] (Angle of repose) From the viewpoint of handling and workability, the anion-modified CNF-containing powder of the present invention has an angle of repose of preferably 40 to 49°, more preferably 42 to 48°. If the angle of repose is too large, deposition is likely to occur in the hopper, and if it is too small, the powder will not stop flowing from the feeder outlet, etc. The angle of repose can be measured using a powder property tester.

[0017] (Collapse angle) From the viewpoint of handling and workability, the anion-modified CNF-containing powder of the present invention has a collapse angle of preferably 15 to 24°, more preferably 17 to 22°. If the collapse angle is too large, a large impact is required to collapse the volume of the powder, and if it is too small, the powder will not stop flowing from the feeder outlet, etc. The collapse angle can be measured using a powder property tester.

[0018] (difference angle) From the viewpoint of handling and workability, the anion-modified CNF-containing powder of the present invention has a difference angle of preferably 20 to 25°, more preferably 21 to 25°. If the difference angle is too large, the powder becomes more likely to scatter due to high jetting properties, and if it is too small, a large force is required to discharge the powder, making it difficult to control the discharge amount. The difference angle can be calculated from the angle of repose and the angle of collapse measured using a powder property tester using the following formula. Difference angle = Angle of repose - Angle of collapse

[0019] (Anion-modified cellulose nanofiber) In the present invention, anion-modified cellulose nanofibers (anion-modified CNF) are fine fibers having an average fiber diameter (fiber width) of 3 to 500 nm and an aspect ratio of 100 or more, and can be obtained by defibrating anion-modified cellulose.

[0020] (Cellulose raw material) Examples of cellulose raw materials for producing anion-modified cellulose include those derived from plant materials (e.g., wood, bamboo, hemp, jute, kenaf, agricultural waste, cloth, pulp (softwood unbleached kraft pulp (NUKP), softwood bleached kraft pulp (NBKP), hardwood unbleached kraft pulp (LUKP), hardwood bleached kraft pulp (LBKP), softwood unbleached sulfite pulp (NUSP), softwood bleached sulfite pulp (NBSP), thermomechanical pulp (TMP), recycled pulp, waste paper, etc.), animal materials (e.g., ascidians), algae, microorganisms (e.g., acetic acid bacteria (Acetobacter)), microbial products, etc., and any of these can be used. Cellulose fibers derived from plants or microorganisms are preferred, and cellulose fibers derived from plants are more preferred.

[0021] (anion modified) In the present invention, anionic modification refers to the introduction of anionic groups into cellulose, specifically, the introduction of anionic groups into the pyranose ring of cellulose by carboxylation (oxidation) or substitution reaction. In the present invention, the carboxylation (oxidation) reaction refers to a reaction in which the hydroxyl group of the pyranose ring is directly oxidized to a carboxy group. In addition, in the present invention, the substitution reaction refers to a reaction in which anionic groups are introduced into the pyranose ring by a substitution reaction other than the carboxylation (oxidation).

[0022] Examples of the anion modification include carboxylation (oxidation), carboxymethylation, esterification, etc. Among them, carboxylation (oxidation), carboxymethylation, and phosphate esterification are more preferable, and carboxylation (oxidation) is particularly preferable.

[0023] (Carboxylation) In the present invention, when carboxylated (oxidized) cellulose is used as the anion-modified cellulose, the carboxylated cellulose (also called oxidized cellulose) can be obtained by carboxylating (oxidizing) the above-mentioned cellulose raw material by a known method. Although not particularly limited, during carboxylation, it is preferable to adjust the amount of carboxy groups to 0.6 to 2.0 mmol / g, and more preferably to adjust to 1.0 mmol / g to 2.0 mmol / g, based on the bone dry mass of the anion-modified cellulose nanofiber.

[0024] One example of a carboxylation (oxidation) method is a method in which a cellulose raw material is oxidized in water using an oxidizing agent in the presence of an N-oxyl compound and a compound selected from the group consisting of bromides, iodides, or a mixture thereof. This oxidation reaction selectively oxidizes the primary hydroxyl group at the C6 position of the glucopyranose ring on the cellulose surface, resulting in the formation of aldehyde groups and carboxy groups (-COOH) or carboxylate groups (-COO - The concentration of cellulose during the reaction is not particularly limited, but is preferably 5% by mass or less.

[0025] The term "N-oxyl compound" refers to a compound capable of generating a nitroxy radical. Any compound that can promote the desired oxidation reaction can be used as the N-oxyl compound. For example, 2,2,6,6-tetramethylpiperidine-1-oxy radical (TEMPO) and its derivatives (e.g., 4-hydroxyTEMPO) can be mentioned.

[0026] The amount of the N-oxyl compound used is not particularly limited as long as it is a catalytic amount capable of oxidizing the raw cellulose. For example, the amount is preferably 0.01 to 10 mmol, more preferably 0.01 to 1 mmol, and even more preferably 0.05 to 0.5 mmol per 1 g of bone dry cellulose. The amount is preferably about 0.1 to 4 mmol / L relative to the reaction system.

[0027] Bromides are compounds containing bromine, examples of which include alkali metal bromides that can dissociate and ionize in water. Also, iodides are compounds containing iodine, examples of which include alkali metal iodides. The amount of bromide or iodide used can be selected within a range that can promote the oxidation reaction. The total amount of bromide and iodide is, for example, preferably 0.1 to 100 mmol, more preferably 0.1 to 10 mmol, and even more preferably 0.5 to 5 mmol, per 1 g of bone-dry cellulose.

[0028] The oxidizing agent may be a known one, such as halogen, hypohalous acid, halous acid, perhalogen acid or their salts, halogen oxide, or peroxide. Among them, sodium hypochlorite is preferable because it is inexpensive and has a low environmental impact. The appropriate amount of the oxidizing agent to be used is, for example, preferably 0.5 to 500 mmol, more preferably 0.5 to 50 mmol, even more preferably 1 to 25 mmol, and most preferably 3 to 10 mmol, per 1 g of bone-dry cellulose. Also, for example, 1 to 40 mol is preferable per 1 mol of the N-oxyl compound.

[0029] The cellulose oxidation process can proceed efficiently even under relatively mild conditions. Therefore, the reaction temperature is preferably 4 to 40°C, or may be room temperature of about 15 to 30°C. As the reaction proceeds, carboxyl groups are generated in the cellulose, and a decrease in the pH of the reaction solution is observed. In order to efficiently proceed with the oxidation reaction, it is preferable to add an alkaline solution such as an aqueous sodium hydroxide solution to maintain the pH of the reaction solution at about 8 to 12, preferably 10 to 11. The reaction medium is preferably water, because it is easy to handle and does not easily cause side reactions.

[0030] The reaction time in the oxidation reaction can be appropriately set according to the degree of progress of the oxidation, and is usually from 0.5 to 6 hours, for example, about 0.5 to 4 hours.

[0031] The oxidation reaction may also be carried out in two stages. For example, the oxidized cellulose obtained by filtration after completion of the first-stage reaction can be oxidized again under the same or different reaction conditions, allowing efficient oxidation without reaction inhibition by table salt produced as a by-product in the first-stage reaction.

[0032] Another example of the carboxylation (oxidation) method is a method in which a cellulose raw material is oxidized by contacting it with an ozone-containing gas. This oxidation reaction oxidizes at least the hydroxyl groups at positions 2 and 6 of the glucopyranose ring, and decomposes the cellulose chain. The ozone concentration in the ozone-containing gas is 50 to 250 g / m 3 It is preferable that the thickness is 50 to 220 g / m 3 It is more preferable that the ozone is added to the cellulose raw material in an amount of 0.1 to 30 parts by mass, and more preferably 5 to 30 parts by mass, based on 100 parts by mass of the solid content of the cellulose raw material. The ozone treatment temperature is preferably 0 to 50°C, and more preferably 20 to 50°C. The ozone treatment time is not particularly limited, but is about 1 to 360 minutes, and is preferably about 30 to 360 minutes. When the ozone treatment conditions are within these ranges, it is possible to prevent cellulose from being excessively oxidized and decomposed, and the yield of oxidized cellulose is good. After the ozone treatment, an oxidizing agent may be used to perform a post-oxidation treatment. The oxidizing agent used in the post-oxidation treatment is not particularly limited, but examples thereof include chlorine-based compounds such as chlorine dioxide and sodium chlorite, oxygen, hydrogen peroxide, persulfuric acid, and peracetic acid. For example, these oxidizing agents are dissolved in a polar organic solvent such as water or alcohol to prepare an oxidizing agent solution, and the cellulose raw material is immersed in the solution to perform the post-oxidation treatment.

[0033] The amount of carboxy groups in the oxidized cellulose can be adjusted by controlling the reaction conditions, such as the amount of the oxidizing agent added and the reaction time.

[0034] (Carboxymethylation) In the present invention, when carboxymethylated cellulose is used as the anion-modified cellulose, the carboxymethylated cellulose may be obtained by carboxymethylating the above-mentioned cellulose raw material by a known method, or a commercially available product may be used. In either case, it is preferable that the degree of carboxymethyl group substitution per anhydrous glucose unit of cellulose is 0.01 to 0.50. An example of a method for producing such carboxymethylated cellulose can be mentioned as follows. Cellulose is used as a starting material, and 3 to 20 times by mass of water and / or lower alcohol, specifically water, methanol, ethanol, N-propyl alcohol, isopropyl alcohol, N-butanol, isobutanol, tertiary butanol, etc., are used as a solvent, or a mixture of two or more of them are used. In addition, when a lower alcohol is mixed, the mixing ratio of the lower alcohol is 60 to 95% by mass. As a mercerizing agent, 0.5 to 20 times by mole of an alkali metal hydroxide, specifically sodium hydroxide or potassium hydroxide, is used per anhydrous glucose residue of the starting material. The starting material, solvent, and mercerizing agent are mixed, and a mercerization treatment is carried out at a reaction temperature of 0 to 70° C., preferably 10 to 60° C., for a reaction time of 15 minutes to 8 hours, preferably 30 minutes to 7 hours. Then, a carboxymethylating agent is added at 0.05 to 10.0 times the moles per glucose residue, and an etherification reaction is carried out at a reaction temperature of 30 to 90° C., preferably 40 to 80° C., for a reaction time of 30 minutes to 10 hours, preferably 1 hour to 4 hours.

[0035] (Crystallization degree of cellulose type I) The crystallinity of cellulose type I in carboxymethylated cellulose is preferably 50% or more, more preferably 60% or more. The crystallinity of cellulose type I in carboxymethylated cellulose can be controlled by the concentration of the mercerizing agent during production, the temperature during treatment, and the degree of carboxymethylation. Since a high concentration of alkali is used in mercerization and carboxymethylation, the cellulose type I crystals are easily converted to type II, but the desired crystallinity can be maintained by, for example, adjusting the amount of alkali (mercerizing agent) used to adjust the degree of conversion. The upper limit of the crystallinity of cellulose type I is not particularly limited. In reality, it is thought that the upper limit is about 90%. The crystallinity of cellulose type I in carboxymethylated cellulose and the crystallinity of cellulose type I in carboxymethylated CNF obtained by defibrating it are usually the same.

[0036] In this specification, "carboxymethylated cellulose", which is a type of anion-modified cellulose used in the preparation of anion-modified CNF, refers to cellulose that maintains at least a part of its fibrous shape even when dispersed in water. Therefore, it is distinguished from carboxymethyl cellulose, which is a type of water-soluble polymer described later. When an aqueous dispersion of "carboxymethylated cellulose" is observed with an electron microscope, a fibrous substance can be observed. On the other hand, when an aqueous dispersion of carboxymethyl cellulose, which is a type of water-soluble polymer, is observed, no fibrous substance is observed. In addition, when "carboxymethylated cellulose" is measured by X-ray diffraction, a peak of cellulose type I crystals can be observed, but cellulose type I crystals are not observed in carboxymethyl cellulose, a water-soluble polymer.

[0037] (Esterification) In the present invention, when esterified cellulose is used as the anion-modified cellulose, the esterified cellulose can be obtained by a method of mixing a powder or an aqueous solution of phosphoric acid compound A with the above-mentioned cellulose raw material, or a method of adding an aqueous solution of phosphoric acid compound A to a slurry of the cellulose raw material.

[0038] Examples of the phosphoric acid compound A include phosphoric acid, polyphosphoric acid, phosphorous acid, hypophosphorous acid, phosphonic acid, polyphosphonic acid, and esters thereof. These may be in the form of a salt. Among these, compounds having a phosphoric acid group are preferred because they are low cost, easy to handle, and can be introduced into the cellulose of the pulp fiber to improve the defibration efficiency. Examples of compounds having a phosphoric acid group include phosphoric acid, sodium dihydrogen phosphate, disodium hydrogen phosphate, trisodium phosphate, sodium phosphite, potassium phosphite, sodium hypophosphite, potassium hypophosphite, sodium pyrophosphate, sodium metaphosphate, potassium dihydrogen phosphate, dipotassium hydrogen phosphate, tripotassium phosphate, potassium pyrophosphate, potassium metaphosphate, ammonium dihydrogen phosphate, diammonium hydrogen phosphate, triammonium phosphate, ammonium pyrophosphate, and ammonium metaphosphate. These can be used alone or in combination of two or more. Among these, phosphoric acid, sodium salts of phosphoric acid, potassium salts of phosphoric acid, and ammonium salts of phosphoric acid are more preferred from the viewpoints of high efficiency of phosphoric acid group introduction, ease of defibration in the defibration step described below, and ease of industrial application. Sodium dihydrogen phosphate and disodium hydrogen phosphate are particularly preferred. In addition, it is preferable to use the phosphoric acid compound A as an aqueous solution, since this increases the uniformity of the reaction and the efficiency of introducing the phosphoric acid group. The pH of the aqueous solution of the phosphoric acid compound A is preferably 7 or less, since this increases the efficiency of introducing the phosphoric acid group, but from the viewpoint of suppressing hydrolysis of the pulp fiber, a pH of 3 to 7 is preferable.

[0039] The following method can be given as an example of a method for producing cellulose phosphate. A phosphoric acid compound A is added to a dispersion of a cellulose raw material having a solid content concentration of 0.1 to 10% by mass while stirring to introduce a phosphoric acid group into the cellulose. When the cellulose raw material is taken as 100 parts by mass, the amount of phosphoric acid compound A added is preferably 0.2 to 500 parts by mass, more preferably 1 to 400 parts by mass, in terms of the amount of phosphorus element. If the proportion of phosphoric acid compound A is equal to or greater than the lower limit, the yield of fine cellulose fibers can be further improved. However, if the upper limit is exceeded, the effect of improving the yield reaches a plateau, which is not preferable from the viewpoint of cost.

[0040] In this case, in addition to the cellulose raw material and the phosphoric acid compound A, a powder or an aqueous solution of the other compound B may be mixed. The compound B is not particularly limited, but is preferably a nitrogen-containing compound exhibiting basicity. Here, "basicity" is defined as an aqueous solution exhibiting pink to red color in the presence of a phenolphthalein indicator, or an aqueous solution having a pH of more than 7. The nitrogen-containing compound exhibiting basicity used in the present invention is not particularly limited as long as it exhibits the effects of the present invention, but is preferably a compound having an amino group. Examples include, but are not limited to, urea, methylamine, ethylamine, trimethylamine, triethylamine, monoethanolamine, diethanolamine, triethanolamine, pyridine, ethylenediamine, and hexamethylenediamine. Among these, urea, which is low-cost and easy to handle, is preferred. The amount of compound B added is preferably 2 to 1000 parts by mass, more preferably 100 to 700 parts by mass, relative to 100 parts by mass of the solid content of the cellulose raw material. The reaction temperature is preferably 0 to 95°C, more preferably 30 to 90°C. The reaction time is not particularly limited, but is about 1 to 600 minutes, and more preferably 30 to 480 minutes. When the esterification reaction conditions are within these ranges, it is possible to prevent cellulose from being excessively esterified and becoming easily soluble, and the yield of phosphated cellulose is good. After the obtained phosphated cellulose suspension is dehydrated, it is preferable to heat treat it at 100 to 170°C from the viewpoint of suppressing hydrolysis of cellulose. Furthermore, it is preferable to heat it at 130°C or less, preferably 110°C or less while water is contained during the heat treatment, and after removing the water, heat treat it at 100 to 170°C.

[0041] The degree of substitution of phosphoric acid group per glucose unit of the phosphoric acid esterified cellulose is preferably 0.001 to 0.40. By introducing a phosphoric acid group substituent into cellulose, the cellulose particles are electrically repelled from each other. Therefore, the cellulose into which the phosphoric acid group has been introduced can be easily defibrated. If the degree of substitution of phosphoric acid group per glucose unit is less than 0.001, it cannot be defibrated sufficiently. On the other hand, if the degree of substitution of phosphoric acid group per glucose unit is more than 0.40, it may swell or dissolve, and may not be obtained as fine cellulose fibers. In order to perform defibration efficiently, it is preferable that the phosphoric acid esterified cellulose raw material obtained above is washed by boiling and then washing with cold water. The modification by these esterifications is a modification by substitution reaction. The degree of substitution in the esterified cellulose and the degree of substitution when the esterified cellulose is finely pulverized are usually the same.

[0042] Phosphated cellulose can be said to be cellulose into which an anionic group, a phosphorus oxoacid group, or a substituent derived from a phosphorus oxoacid group (sometimes simply referred to as a "phosphorus oxoacid group") has been introduced. Here, the phosphorus oxoacid group is, for example, a divalent functional group obtained by removing a hydroxyl group from phosphoric acid, specifically a group represented by -PO3H2. The substituent derived from the phosphorus oxoacid group includes a salt of the phosphorus oxoacid group, a phosphorus oxoacid ester group, and other substituents. The substituent derived from the phosphorus oxoacid group may be contained in the cellulose nanofiber as a group in which a phosphoric acid group is condensed (for example, a pyrophosphate group). The phosphorus oxoacid group may be, for example, a phosphorous acid group (phosphonic acid group), and the substituent derived from the phosphorus oxoacid group may be a salt of the phosphorous acid group, or the like.

[0043] The amount of phosphorus oxoacid groups, such as phosphate groups or phosphite groups, introduced into the phosphated cellulose is not particularly limited. During phosphate esterification, the amount of phosphorus oxoacid groups is preferably adjusted to 0.5 to 5 mmol / g, and more preferably 0.5 to 2.5 mmol / g, based on the bone dry mass of the anion-modified cellulose nanofiber.

[0044] (Defibrilization) The device used for defibrating anion-modified cellulose is not particularly limited, but devices such as high-speed rotation, colloid mill, high-pressure, roll mill, and ultrasonic devices can be used. When defibrating, it is preferable to apply a strong shear force to the aqueous dispersion of anion-modified cellulose. In particular, for efficient defibration, it is preferable to apply a pressure of 50 MPa or more to the aqueous dispersion and to use a wet high-pressure or ultra-high-pressure homogenizer capable of applying a strong shear force. The pressure is more preferably 100 MPa or more, and even more preferably 140 MPa or more. Furthermore, prior to defibration and dispersion treatment with the high-pressure homogenizer, the aqueous dispersion may be subjected to a pretreatment, if necessary, using a known mixing, stirring, emulsifying, and dispersing device such as a high-speed shear mixer.

[0045] (Dispersant) From the viewpoint of improving redispersibility, the anion-modified cellulose nanofiber-containing powder of the present invention preferably contains a dispersant. Examples of the dispersant include water-soluble polymers, surfactants, etc., and it is preferable to use a water-soluble polymer because the water-soluble polymer covers the low charge density areas on the surface of the anion-modified cellulose nanofibers, suppresses the formation of hydrogen bonds, and prevents aggregation of the cellulose nanofibers during drying.

[0046] (Water-soluble polymer) In the present invention, examples of water-soluble polymers include cellulose derivatives (carboxymethylcellulose, methylcellulose, hydroxypropylcellulose, ethylcellulose), xanthan gum, xyloglucan, dextrin, dextran, carrageenan, locust bean gum, alginic acid, alginates, pullulan, starch, potato starch, kudzu flour, modified starch (cationized starch, phosphorylated starch, phosphate cross-linked starch, phosphate monoesterified phosphate cross-linked starch, hydroxypropyl starch, hydroxypropylated phosphate cross-linked starch, acetylated adipic acid cross-linked starch, acetylated phosphate cross-linked starch, acetylated oxidized starch, sodium octenylsuccinate starch, starch acetate, oxidized starch), corn starch, gum arabic, and gellan. Gum, polydextrose, pectin, chitin, water-soluble chitin, chitosan, casein, albumin, soy protein lysate, peptone, polyvinyl alcohol, polyacrylamide, sodium polyacrylate, polyvinylpyrrolidone, polyvinyl acetate, polyamino acid, polylactic acid, polymalic acid, polyglycerin, latex, rosin-based sizing agent, petroleum resin-based sizing agent, urea resin, melamine resin, epoxy resin, polyamide resin, polyamide-polyamine resin, polyethyleneimine, polyamine, vegetable gum, polyethylene oxide, hydrophilic crosslinked polymer, polyacrylate, starch polyacrylic acid copolymer, tamarind gum, guar gum, and colloidal silica, and mixtures of one or more thereof. Among these, cellulose derivatives are preferred in terms of compatibility with anion-modified cellulose nanofibers, and carboxymethylcellulose and its salts are particularly preferred. It is believed that water-soluble polymers such as carboxymethylcellulose and its salts penetrate between anion-modified cellulose nanofibers and increase the distance between CNFs, thereby improving redispersibility.

[0047] When carboxymethylcellulose or a salt thereof is used as the water-soluble polymer, it is preferable to use a carboxymethylcellulose having a degree of substitution of carboxymethyl groups per anhydrous glucose unit of 0.55 to 1.6, more preferably 0.55 to 1.1, and even more preferably 0.65 to 1.1. In addition, a carboxymethylcellulose having a longer molecule (higher viscosity) is preferable because it has a higher effect of widening the distance between CNFs, and the B-type viscosity of a 1% by mass aqueous solution of carboxymethylcellulose at 25°C and 600 rpm is preferably 3 to 14000 mPa·s, more preferably 7 to 14000 mPa·s, and even more preferably 1000 to 8000 mPa·s. Note that the "carboxymethylcellulose or a salt thereof" as the water-soluble polymer referred to here is completely dissolved in water, and is therefore distinguished from the above-mentioned carboxymethylated cellulose whose fiber shape can be confirmed in water.

[0048] In the present invention, when the powder containing anion-modified cellulose nanofibers contains a dispersant, the compounding ratio of anion-modified CNF (bone dry solid content) to dispersant is preferably 2:8 to 8:2, more preferably 5:5 to 7:3, from the viewpoint of obtaining an effect of improving redispersibility. If the compounding ratio of the dispersant is too high above the upper limit, problems such as viscosity characteristics such as thixotropy, which is a characteristic of anion-modified CNF, and a decrease in dispersion stability may occur. If the compounding ratio of the dispersant is too low below the lower limit, sufficient redispersibility cannot be obtained.

[0049] (Powder manufacturing method) The method for producing the anion-modified CNF-containing powder of the present invention is not particularly limited. For example, an aqueous suspension containing anion-modified CNF and a dispersant blended as necessary is dehydrated and dried to obtain a dry solid, which is then pulverized by a pulverizer or the like, and the pulverized product is classified as necessary and recovered to obtain a powder, or the aqueous suspension is spray-dried to simultaneously dehydrate, dry, and pulverize the product, and the product is classified as necessary and recovered to obtain a powder.

[0050] The method for dehydrating and drying the aqueous suspension containing anion-modified CNF may be any method known in the art, such as spray drying, freeze drying, squeezing, air drying, hot air drying, and vacuum drying. Specific examples of drying apparatuses to be used include the following. That is, continuous tunnel drying apparatuses, band drying apparatuses, vertical drying apparatuses, vertical turbo drying apparatuses, multi-stage disk drying apparatuses, ventilation drying apparatuses, rotary drying apparatuses, air flow drying apparatuses, spray dryer drying apparatuses, spray drying apparatuses, cylindrical drying apparatuses, drum drying apparatuses, reduced pressure belt drying apparatuses, screw conveyor drying apparatuses, rotary drying apparatuses with heating tubes, vibration transport drying apparatuses, fluidized bed drying apparatuses, etc., batch type box drying apparatuses, ventilation drying apparatuses, vacuum box drying apparatuses, stirring drying apparatuses, shelf drying apparatuses, freeze drying apparatuses, etc., can be used alone or in combination of two or more. Among these, drum drying apparatuses and belt drying apparatuses are preferably used, and from the viewpoint of energy efficiency, drum drying apparatuses that directly supply heat energy to the material to be dried uniformly are more preferably used.

[0051] The method of pulverizing the anion-modified CNF-containing dry solid to obtain a pulverized product is not particularly limited. For example, the anion-modified CNF-containing dry solid can be pulverized with a pulverizer to obtain a pulverized product. Examples of pulverizers include cutting type mills: mesh mill (manufactured by HORAI Co., Ltd.), Atoms (manufactured by Yamamoto Hyakuma Seisakusho Co., Ltd.), knife mill (manufactured by Palman Co., Ltd.), cutter mill (manufactured by Tokyo Atomizer Manufacturing Co., Ltd.), CS cutter (manufactured by Mitsui Mining Co., Ltd.), rotary cutter mill (manufactured by Nara Machinery Manufacturing Co., Ltd.), turbo cutter (manufactured by Freund Corporation), pulp crusher (manufactured by Zuikou Co., Ltd.), shredder (manufactured by Kobe Steel Pantech Co., Ltd.), hammer type mills: jaw crusher (Makino Corporation), and the like. (manufactured by Makino Sangyo Co., Ltd.), Hammer Crusher (manufactured by Makino Sangyo Co., Ltd.), Impact Mill: Pulverizer (manufactured by Hosokawa Micron Co., Ltd.), Fine Impact Mill (manufactured by Hosokawa Micron Co., Ltd.), Super Micron Mill (manufactured by Hosokawa Micron Co., Ltd.), Innomizer (manufactured by Hosokawa Micron Co., Ltd.), Fine Mill (manufactured by Nippon Pneumatic Mfg. Co., Ltd.), CUM-type Centrifugal Mill (manufactured by Mitsui Mining Co., Ltd.), Exceed Mill (manufactured by Makino Sangyo Co., Ltd.), Ultraplex (manufactured by Makino Sangyo Co., Ltd.), Contraplex (manufactured by Makino Sangyo Co., Ltd.), Co., Ltd.), Coroplex (Makino Sangyo Co., Ltd.), Sample Mill (Seishin Co., Ltd.), Bantam Mill (Seishin Co., Ltd.), Atomizer (Seishin Co., Ltd.), Tornado Mill (Nikkiso Co., Ltd.), Nea Mill (Dalton Co., Ltd.), HT Type Fine Grinding Mill (Horai Co., Ltd.), Free Grinding Mill (Nara Machinery Works, Ltd.), New Cosmomizer (Nara Machinery Works, Ltd.), Turbo Mill (Freund Corporation), Gather Mill (Nishimura Machinery Works, Ltd.), Superpowder Darmill (manufactured by Nishimura Machinery Works, Ltd.), Blade mill (manufactured by Nisshin Engineering Inc.), Super rotor (manufactured by Nisshin Engineering Inc.), Npa crusher (manufactured by Sansho Industry Co., Ltd.), Wheeley crusher (manufactured by Sanki Manufacturing Co., Ltd.), Pulp crusher (manufactured by Zuikou Co., Ltd.), Jacobson fine grinder (manufactured by Kobe Steel Pantech Co., Ltd.), Universal mill (manufactured by Tokuju Co., Ltd.), Atomizer (manufactured by Tokyo Atomizer Manufacturing Co., Ltd.), Mill Star Dam (manufactured by Tokyo Atomizer Manufacturing Co., Ltd.),Airflow type mills: Stream Mill (manufactured by Nippon Coke Engineering Co., Ltd.), CGS type jet mill (manufactured by Mitsui Mining Co., Ltd.), Micron Jet (manufactured by Hosokawa Micron Corporation), Counter Jet Mill (manufactured by Hosokawa Micron Corporation), Cross Jet Mill (manufactured by Kurimoto Iron Works, Ltd.), Supersonic Jet Mill (manufactured by Japan Pneumatic Mfg. Co., Ltd.), Current Jet (manufactured by Nisshin Engineering Inc.), Jet Mill (manufactured by Sansho Industry Co., Ltd.), Ebara Jet Micronizer (manufactured by Ebara Corporation), Ebara Triad Jet (manufactured by Ebara Corporation), Selenium Mirror (manufactured by Masuko Sangyo Co., Ltd.), New Micro Sect Examples of such mills include matte (manufactured by Masuno Seisakusho Co., Ltd.), Cryptron (manufactured by Kawasaki Heavy Industries, Ltd.), disc mills: vibrating disc mills (manufactured by Retsch), centri-cutter (manufactured by Nippon Coke & Engineering Co., Ltd.), turbo disc mills (manufactured by Freund-Turbo Corporation), mortar-type high-speed grinders (manufactured by Makino Sangyo Co., Ltd.), vertical roller mills: vertical roller mills (manufactured by Chinon Co., Ltd.), vertical roller mills (manufactured by Schaeffler Japan Co., Ltd.), roller mills (manufactured by Kotobuki Giken Kogyo Co., Ltd.), VX mills (manufactured by Kurimoto Iron Works Co., Ltd.), KVM-type vertical mills (manufactured by EarthTechnica Co., Ltd.), and IS mills (manufactured by IHI Plant Engineering Co., Ltd.). The processing conditions for these pulverizers cannot be determined uniformly because the principles of pulverization are different. However, for example, a method can be used in which processing conditions that affect the pulverization process, such as the screen diameter at the pulverizer outlet and the rotation speed of the classification rotor, are adjusted, a calibration curve showing the relationship between the processing conditions and the particle size is created, and appropriate processing conditions are determined based on the calibration curve so as to obtain the desired average particle size.

[0052] The pulverized material containing anion-modified CNF may be classified as necessary. When classification is performed, it can be performed using a classification device that is attached to or attached to the pulverizer.

[0053] The type of device used to collect the pulverized material containing anion-modified CNF and the granulated material obtained by spray drying is not particularly limited. Examples of the collection device include a cyclone and a bag filter.

[0054] The anion-modified CNF-containing powder may be classified after collection.

[0055] The anion-modified CNF-containing powder of the present invention has an average particle size of 45 μm or more and a degree of dispersion of less than 25%, so that there is little dusting during processing, and it is easy to handle and easy to work with when performing redispersion work, etc. In addition, the anion-modified CNF-containing powder of the present invention has excellent initial water absorbency. EXAMPLES

[0056] The present invention will be described in more detail below by way of examples, but the present invention is not limited to these.

[0057] (Average fiber diameter and length of CNF) The powder was redispersed in water, the suspension was diluted, and 200 randomly selected fibers were analyzed using an atomic force microscope (AFM) and the average was taken. The aspect ratio was calculated according to the following formula. Aspect ratio = average fiber length / average fiber diameter

[0058] (Carboxylic group amount) The amount of carboxyl groups was calculated by preparing 60 mL of a 0.5% by mass slurry (aqueous dispersion) of carboxylated cellulose, adding 0.1 M aqueous hydrochloric acid to adjust the pH to 2.5, then adding 0.05 N aqueous sodium hydroxide dropwise and measuring the electrical conductivity until the pH reached 11, and using the following formula from the amount of sodium hydroxide (a) consumed in the neutralization stage of the weak acid where the change in electrical conductivity was gradual: amount of carboxyl groups [mmol / g carboxylated cellulose] = a [mL] × 0.05 / mass of carboxylated cellulose [g].

[0059] (Degree of carboxymethyl substitution) The degree of carboxymethyl substitution was measured by the following method. Approximately 2.0 g of the sample was weighed out and placed in a 300 mL Erlenmeyer flask with a stopper. 100 mL of a solution of 1000 mL of nitric acid methanol and 100 mL of special-grade concentrated nitric acid was added and shaken for 3 hours to convert the salt of carboxymethylated cellulose CNF (CMC) to H-CMC (hydrogen-type carboxymethylated CNF). 1.5 to 2.0 g of the bone-dry H-CMC was weighed out and placed in a 300 mL Erlenmeyer flask with a stopper. The H-CMC was moistened with 15 mL of 80% methanol, 100 mL of 0.1 N-NaOH was added, and the mixture was shaken at room temperature for 3 hours. Using phenolphthalein as an indicator, excess NaOH was back-titrated with 0.1 N-H2SO4, and the degree of carboxymethyl substitution (DS value) was calculated by the following formula. A = [(100 × F'-0.1N-H2SO4 (mL) × F) × 0.1] / (bone dry mass of H-CMC (g)) Degree of carboxymethyl substitution = 0.162 x A / (1-0.058 x A) F': Factor of 0.1N-NaOH F: Factor of 0.1N-H2SO4

[0060] The degree of carboxymethyl substitution in the CNF of carboxymethyl cellulose is usually the same as the degree of carboxymethyl substitution in the carboxymethyl cellulose before it is made into CNF.

[0061] (Crystallization degree of cellulose type I) The crystallinity of cellulose type I of carboxymethylated cellulose nanofibers was measured by the following method. The sample was placed in a glass cell and measured using an X-ray diffraction measuring device (LabX XRD-6000, Shimadzu Corporation). The degree of crystallinity was calculated using the method of Segal et al. The diffraction intensity at 2θ=10° to 50° in the X-ray diffraction pattern was used as the baseline, and the degree of crystallinity was calculated using the following formula from the diffraction intensity of the 002 plane at 2θ=22.6° and the diffraction intensity of the amorphous part at 2θ=18.5°.

[0062] Xc = (I002c - Ia) / I002c x 100 Xc = Crystallinity of cellulose type I (%) I002c: 2θ=22.6°, diffraction intensity of 002 plane Ia: 2θ=18.5°, diffraction intensity of amorphous part

[0063] The proportion of type I crystals in carboxymethylated cellulose nanofibers is usually the same as that in the carboxymethyl cellulose before it is made into CNF.

[0064] (Amount of phosphorus oxoacid groups) The amount of phosphorus oxoacid groups (amount of phosphate groups or phosphite groups) was measured by the following method. First, ion-exchanged water was added to the target CNF to prepare a slurry with a solid content of 0.2% by mass. The obtained slurry was treated with an ion-exchange resin, and then titrated with an alkali to measure the solid content.

[0065] Treatment with ion exchange resin was performed by adding 1 / 10 by volume of a strongly acidic ion exchange resin (Amberjet 1024; Organo Corporation, conditioned) to the above CNF-containing slurry, shaking for 1 hour, and then pouring onto a mesh with 90 μm openings to separate the resin and slurry.

[0066] In addition, the titration using alkali was performed by adding 10 μL of 0.1N sodium hydroxide solution to the CNF-containing slurry after the ion exchange resin treatment at 5 seconds, and measuring the change in the pH value of the slurry. The titration was performed while blowing nitrogen gas into the slurry 15 minutes before the start of the titration. In this neutralization titration, two points were observed where the increment (the differential value of pH with respect to the amount of alkali added) was maximum on the curve plotting the measured pH against the amount of alkali added. Of these, the first maximum point of the increment obtained after the start of the alkali addition is called the first end point, and the next maximum point of the increment is called the second end point. The amount of alkali required from the start of the titration to the first end point is equal to the amount of first dissociated acid in the slurry used for the titration. The amount of alkali required from the start of the titration to the second end point is equal to the total amount of dissociated acid in the slurry used for the titration. The amount of alkali (mmol) required from the start of titration to the first end point was divided by the solid content (g) in the slurry to be titrated, and this value was taken as the amount of phosphorus oxoacid groups (mmol / g).

[0067] (Measurement of moisture content) The moisture content of the powder was calculated as the difference between the mass of the obtained powder after drying at 105° C. for 3 hours or more (absolute dry mass) and the mass before drying.

[0068] (Average particle size) The average particle size (D50) of the powders used in the examples and comparative examples was determined from the particle size distribution based on the volume average particle size.

[0069] The particle size distribution was measured using a laser diffraction / scattering particle size distribution analyzer (Mastersizer 3000, manufactured by Spectris Co., Ltd.) under the condition of a particle refractive index of 1.5. The measurement was performed by directly putting the dry powder sample into the device.

[0070] (Dispersion degree) The degree of dispersion of the powders obtained in the examples and comparative examples was measured using a powder tester (Powder Tester PT-X type, manufactured by Hosokawa Micron Corp.) Specifically, 10 g of a sample was placed in the dispersion unit of the PT-X and dropped, and the degree of dispersion was calculated from the amount of powder that fell onto a watch glass using the following formula. Dispersion degree (%) = (10 (g) - amount of powder dropped onto the watch glass (g)) / 10 (g)

[0071] (Angle of repose) The repose angle of the powders obtained in the examples and comparative examples was determined by dropping and depositing the powder from the hole of a funnel onto a horizontal plate of a certain area until it took on a certain shape using a powder property tester (Powder Tester PT-X type, manufactured by Hosokawa Micron Corporation), and the value of the Angle Repose was determined as the value of the Angle Repose when a conical granule was formed.

[0072] (Collapse angle) The collapse angle of the powder obtained in the examples and comparative examples was measured by using a powder property tester (Powder Tester PT-X type, manufactured by Hosokawa Micron Corporation) to drop and deposit the powder from the hole of the funnel onto a horizontal plate of a certain area until it formed a certain shape, forming a cone-shaped granule. Next, a weight of a certain weight placed on the same base as the horizontal plate was dropped to give a certain impact to the powder, and after some of the powder flowed naturally and fell off the horizontal plate, the angle of elevation from a point on the outer periphery of the bottom surface to the apex of the cone for the remaining cone-shaped granule was taken as the collapse angle.

[0073] (difference angle) Using the angle of repose and the angle of collapse measured above, the difference angle was calculated according to the following formula. Difference angle = Angle of repose - Angle of collapse

[0074] (Ease of use when packaging) The workability during packaging was checked for the powders obtained in the Examples and Comparative Examples. The sample powder was placed in a polyethylene bag to fill 70% of the bag, which was then sealed. The adhesive part of the seal was visually inspected and evaluated according to the following criteria. A: There is little scattering of powder, no powder adheres to the adhesive part of the seal, and there is almost no deterioration of the sealability. B: A small amount of powder has scattered and adhered to the adhesive part of the seal, causing a slight decrease in the sealability. C: A lot of powder is scattered, and a lot of powder is attached to the adhesive part of the seal, causing a large decrease in sealing performance.

[0075] (Evaluation of initial water absorption) The powders obtained in the Examples and Comparative Examples were evaluated for their short-term water absorption (initial water absorption). 0.1 g of a specimen was placed flat on a rectangular glass plate. Then, 1 mL of pure water was evenly dropped onto the specimen using a dropper, and the water absorption immediately after was evaluated according to the following criteria. A: Immediately after dropping, the powder absorbed water and a gel layer was formed over the entire surface. B: Immediately after the dripping, the powder absorbed the water slowly, and a gel layer formed in some areas, but the remaining pure water separated into droplets on the powder. C: Immediately after dropping, the powder absorbed the water slowly, and most of the pure water separated into droplets on the powder.

[0076] (Production Example 1) (Production of carboxylated CNF1) 500g (bone dry) of bleached unbeaten kraft pulp (85% brightness) derived from coniferous trees was added to 20L of an aqueous solution of TEMPO (Sigma Aldrich) (0.025mmol / g relative to the cellulose raw material) and sodium bromide (1mmol / g relative to the cellulose raw material), and the mixture was stirred until the pulp was uniformly dispersed. An aqueous solution of sodium hypochlorite was added to the reaction system to a concentration of 5.2mmol / g to initiate the oxidation reaction. The pH of the system decreased during the reaction, but 3M aqueous sodium hydroxide was added successively to adjust the pH to 10. The reaction was terminated when the sodium hypochlorite was consumed and the pH of the system no longer changed. The mixture after the reaction was filtered through a glass filter to separate the pulp, and the pulp was thoroughly washed with water to obtain oxidized pulp (carboxylated cellulose). The pulp yield at this time was 90%, the time required for the oxidation reaction was 100 minutes, and the amount of carboxyl groups was 1.4mmol / g.

[0077] The oxidized pulp obtained in the above process was adjusted to 1.0% (w / v) with water and treated three times with an ultra-high pressure homogenizer (20°C, 150 MPa) to obtain a dispersion of carboxylated CNF1. The obtained fibers had an average fiber diameter of 4 nm and an aspect ratio of 220.

[0078] (Production Example 2) (Production of carboxylated CNF2) 500 g (bone-dry) of bleached softwood-derived dissolving kraft pulp (Buckeye DKP) was added to 50 L of an aqueous solution containing 7.8 g (0.05 mol) of TEMPO (Sigma Aldrich) and 75.5 g (0.74 mol) of sodium bromide, and the mixture was stirred until the pulp was uniformly dispersed. 1.6 L of 2 M aqueous sodium hypochlorite solution was added to the reaction system, and the oxidation reaction was started (oxidation treatment). The pH in the system decreased during the reaction, but 3 M aqueous sodium hydroxide solution was added successively to adjust the pH to 10. After reacting for 2 hours, the mixture was filtered through a glass filter and thoroughly washed with water to obtain carboxylated cellulose. A slurry of carboxylated cellulose was prepared by adjusting the concentration to 5.0% (w / v) with water, and hydrogen peroxide was added to the slurry at 2% (w / w) relative to the carboxylated cellulose, and the pH was adjusted to 11.3 with 3 M sodium hydroxide. The slurry was left at a temperature of 80°C for 2 hours to perform hydrolysis. This was adjusted to 5.0% (w / v) with water and treated five times with an ultra-high pressure homogenizer (20°C, 140 MPa) to obtain a dispersion of carboxylated CNF2. The amount of carboxy groups in the obtained carboxylated CNF2 was 1.7 mmol / g, the average fiber diameter was 3 nm, and the aspect ratio was 117.

[0079] (Production Example 3) (Production of carboxymethylated CNF) 500 parts of isopropanol (IPA) and 15 parts of sodium hydroxide dissolved in 200 parts of water were added to a 5L twin-shaft kneader with the rotation speed adjusted to 100 rpm, and 100 parts of hardwood pulp (LBKP, manufactured by Nippon Paper Industries Co., Ltd.) was added in terms of dry mass when dried at 100 ° C for 60 minutes. The mixture was stirred and mixed at 30 ° C for 90 minutes to prepare mercerized cellulose. 19 parts of sodium monochloroacetate dissolved in 20 parts of 90% IPA was further added while stirring, and after stirring at 30 ° C for 30 minutes, the mixture was heated to 70 ° C and carboxymethylation reaction was carried out at 70 ° C for 90 minutes. After the reaction was completed, the mixture was neutralized, washed with 65% aqueous methanol, deliquored, dried, and pulverized to obtain a sodium salt of carboxymethylated cellulose with a carboxymethyl substitution degree of 0.18 and a crystallinity degree of cellulose I type of 64%. The measurement method of the carboxymethyl substitution degree and the crystallinity degree of cellulose I type was as described above.

[0080] The sodium salt of carboxymethylated cellulose obtained in the above process was adjusted to 1.0% (w / v) with water and treated three times with an ultra-high pressure homogenizer (20°C, 150 MPa) to obtain a dispersion of carboxymethylated CNF. The obtained carboxymethylated CNF had an average fiber diameter of 8 nm and an aspect ratio of 60.

[0081] (Production Example 4) (Production of phosphorylated CNF) Bleached, unbeaten kraft pulp derived from softwood (brightness 85%, basis weight 245g / m 2The phosphorus oxo-oxidation treatment was carried out on the raw pulp (sheet-like) as follows. First, a mixed aqueous solution of ammonium dihydrogen phosphate and urea was added to 100 parts by mass (bone dry) of the raw pulp, and the mixture was adjusted to 45 parts by mass of ammonium dihydrogen phosphate, 120 parts by mass of urea, and 150 parts by mass of water, to obtain a chemical-impregnated pulp. Next, the obtained chemical-impregnated pulp was heated in a hot air dryer at 165°C for 250 seconds to introduce phosphoric acid groups into the cellulose in the pulp, thereby obtaining a phosphorylated pulp. 100 g of the obtained phosphorylated pulp (bone dry) was poured with 10 L of ion-exchanged water to obtain a pulp dispersion, which was stirred so that the pulp was uniformly dispersed, and then repeatedly filtered and dehydrated for washing. The washing end point was determined when the electrical conductivity of the filtrate became 100 μS / cm or less. Next, the phosphorylated pulp after washing was diluted with 10 L of ion-exchanged water, and then a 1N aqueous sodium hydroxide solution was added little by little while stirring, to obtain a phosphorylated pulp slurry having a pH of 12 to 13. The phosphorylated pulp slurry was dewatered and washed to obtain a neutralized phosphorylated pulp.

[0082] The infrared absorption spectrum of the phosphorylated pulp was measured using FT-IR. -1 Absorption due to the P=O of the phosphate group was observed near the nucleus, confirming that the phosphate group had been added to the pulp. In addition, when the obtained phosphorylated pulp was analyzed using an X-ray diffractometer, typical peaks were confirmed at two positions, near 2θ=14° to 17° and near 2θ=22° to 23°, confirming that it had cellulose type I crystals.

[0083] The phosphorylated pulp obtained in the above process was adjusted to 1.0% (w / v) with water and treated three times with an ultra-high pressure homogenizer (20°C, 150 MPa) to obtain a dispersion of phosphorylated CNF. The obtained fibers had an average fiber diameter of 4 nm and an aspect ratio of 200.

[0084] X-ray diffraction confirmed that the obtained CNF maintained cellulose type I crystals. The amount of phosphate groups (amount of first dissociated acid) was 1.45 mmol / g. The total amount of dissociated acid was 2.45 mmol / g.

[0085] Example 1 (Production of dried products) Carboxylated CNF1 (carboxyl group amount: 1.4 mmol / g, average fiber diameter: 4 nm, aspect ratio: 220) obtained in Production Example 1 was used as anion-modified CNF. Carboxymethylcellulose (trade name: F350HC-4, viscosity (1%, 25°C) about 3000 mPa·s, carboxymethyl substitution degree about 0.9) was added to a 0.7 mass% aqueous suspension of carboxylated CNF1 at 40 mass% relative to the anion-modified CNF (i.e., so that the solid content of carboxymethylcellulose was 40 mass parts when the solid content of anion-modified CNF was 100 mass parts), and the mixture was stirred for 60 minutes with a TK homomixer (12,000 rpm) to prepare an aqueous dispersion containing anion-modified CNF. The pH of this dispersion was about 7 to 8. A 5% aqueous sodium hydroxide solution was added to this aqueous dispersion to adjust the pH to 9, and then the solution was applied to the drum surface of a drum dryer D0405 (manufactured by Katsuragi Kogyo Co., Ltd.) to form a thin film with a thickness of approximately 100 to 200 μm. The solution was then dried at a drum surface temperature of 80°C, an internal dryer pressure of 2 kPa, and a drum rotation speed of 2 rpm to obtain a dried body containing anion-modified CNF with a moisture content of 5 mass%.

[0086] (Powder Production) The dried material containing CNF obtained as described above was pulverized using a hammer mill (Tokyo Atomizer Co., Ltd., Hammer Mill TAP-3) as a pulverizer to obtain a pulverized material. The particle size of the pulverized material obtained was adjusted by adjusting the screen diameter at the outlet of the pulverizer. The pulverized material after particle size adjustment was collected using a cyclone to obtain a powder containing anion-modified CNF. The moisture content of the obtained powder was 8% by mass.

[0087] Example 2 A pulverized product was obtained in the same manner as in Example 1, except that the dried body containing CNF obtained in Example 1 was pulverized using an impact mill (Pulverizer, manufactured by Hosokawa Micron Corporation) instead of a hammer mill as a pulverizer. The particle size of the pulverized product obtained was adjusted by adjusting the rotation speed of the classification rotor. The pulverized product after particle size adjustment was collected using a cyclone to obtain a powder containing anion-modified CNF. The moisture content of the obtained powder was 10% by mass.

[0088] Example 3 A pulverized product was obtained in the same manner as in Example 1, except that the dried body containing CNF obtained in Example 1 was pulverized using a disk mill (Nippon Coke Engineering Co., Ltd., Centri-cutter) instead of a hammer mill as a pulverizer. The pulverized product obtained was collected using a cyclone to obtain an anion-modified CNF-containing powder. The moisture content of the obtained powder was 9.7% by mass.

[0089] Example 4 A pulverized product was obtained in the same manner as in Example 1, except that the dried body containing CNF obtained in Example 1 was pulverized using an impact mill (Atomizer, manufactured by Tokyo Atomizer Mfg. Co., Ltd.) instead of a hammer mill as a pulverizer. The particle size of the pulverized product obtained was adjusted and collected in the same manner as in Example 1, to obtain a powder containing anion-modified CNF. The moisture content of the obtained powder was 9.3% by mass.

[0090] Example 5 A pulverized product was obtained in the same manner as in Example 1, except that the dried body containing CNF obtained in Example 1 was pulverized using a turbo mill (manufactured by Freund Corporation) as a pulverizer. The particle size of the pulverized product obtained was adjusted by adjusting the gap between the rotor and the liner. The pulverized product after particle size adjustment was collected using a cyclone to obtain a powder containing anion-modified CNF. The moisture content of the obtained powder was 7.8% by mass.

[0091] Example 6 (Production of dried products) Carboxymethylated CNF (carboxymethyl substitution degree: 0.18, average fiber diameter: 8 nm, aspect ratio: 60) obtained in Production Example 3 was used as the anion-modified CNF. Carboxymethylcellulose (manufactured by Nippon Paper Industries Co., Ltd., product name: F350HC-4, viscosity (1 mass%, 25 ° C, 60 rpm) about 3000 mPa s, carboxymethyl substitution degree about 0.90) was added to a 0.7 mass% aqueous suspension of carboxymethylated CNF at 40 mass% relative to the carboxymethylated CNF (i.e., so that the solid content of carboxymethylcellulose is 40 mass parts when the solid content of carboxymethylated CNF is 100 mass parts), and the mixture was stirred for 60 minutes with a TK homomixer (12,000 rpm) to prepare an aqueous dispersion containing carboxymethylated CNF as an anion-modified CNF. To this aqueous dispersion, 5% by mass of an aqueous sodium hydroxide solution was added to adjust the pH to 9, and then the mixture was applied to the drum surface of a drum dryer D0405 (manufactured by Katsuragi Kogyo Co., Ltd.) and dried for 1 minute at 140° C. The resulting dried product was scraped off to obtain a dried body containing anion-modified CNF.

[0092] (Powder Production) The dried body containing CNF obtained as described above was pulverized in the same manner as in Example 2 to obtain a pulverized product. The particle size of the obtained pulverized product was adjusted by adjusting the rotation speed of the classification rotor. The pulverized product after particle size adjustment was collected using a cyclone to obtain a powder containing anion-modified CNF. The moisture content of the obtained powder was 8.2% by mass.

[0093] Example 7 A dried body containing anion-modified CNF was produced in the same manner as in Example 2, except that the phosphorylated CNF obtained in Production Example 4 (phosphate group amount: 1.45 mmol / g, average fiber diameter: 4 nm, aspect ratio: 200) was used as the anion-modified CNF. This dried body was pulverized in the same manner as in Example 2 to obtain a pulverized product. The particle size of the obtained pulverized product was adjusted by adjusting the rotation speed of the classifying rotor. The pulverized product after particle size adjustment was collected using a cyclone to obtain a powder containing phosphorylated CNF. The moisture content of the obtained powder was 8.5% by mass.

[0094] Comparative Example 1 (Production of dried products) As an anion-modified CNF, a 5.0 mass% aqueous suspension (pH 7.5) of carboxylated CNF2 (carboxy group amount: 1.7 mmol / g, average fiber diameter: 3 nm, aspect ratio: 117) obtained in Production Example 2 was prepared, and dried using a two-fluid nozzle type spray dryer (OUDT-25, manufactured by Okawara Kakoki Co., Ltd.) at an inlet temperature of 160°C, an outlet temperature of 70°C, a drying air volume of 80 kg / h, and a liquid delivery volume of 54.2 kg / h to obtain a powdered dried CNF.

[0095] The resulting dried product was collected using a cyclone to obtain an anion-modified CNF powder, the moisture content of which was 4.4% by mass.

[0096] [Table 1]

[0097] As can be seen from Table 1, the powders containing anion-modified cellulose nanofibers having a fiber diameter of 3 to 500 nm in Examples 1 to 7, which have a moisture content of 20 mass% or less, an average particle diameter of 45 μm or more, and a degree of dispersion of less than 25%, have a suppressed amount of scattering during the process and are excellent in handleability. Furthermore, they have excellent workability during packaging. In addition, they have good initial water absorption. This indicates that, for example, when the powder is added to a tank filled with water and redispersed, the powder is unlikely to float on the water surface and is easily suspended in the water, and is considered to be excellent in dispersion and homogenization in water by stirring. On the other hand, the anion-modified cellulose nanofiber powder of Comparative Example 1, which has a small average particle diameter, has a degree of dispersion outside the above range, making it difficult to suppress the amount of scattering during the process and poor in handleability. Furthermore, they have poor workability during packaging, and there is a concern that poor sealing will occur during packaging. Furthermore, the initial water absorption is slow, and the water and powder separate and are difficult to mix. Usually, cellulose nanofiber powder is adjusted in various ways to ensure the redispersibility of the cellulose nanofiber when redispersed in a solvent. Therefore, the adhesive force between cellulose nanofiber powder particles is weaker than that of normal cellulose-based powders, and there is a concern that it may be more prone to scattering and less easy to work with than normal cellulose-based powders. The anion-modified cellulose nanofiber-containing powder of the present invention is the first to demonstrate that even if the cellulose nanofibers are adjusted to have good redispersibility, by adjusting the moisture content, average particle size, and dispersibility to an appropriate balance, a cellulose nanofiber powder with excellent workability and reduced scattering can be obtained.

Claims

1. A powder containing anion-modified cellulose nanofibers having an average fiber diameter of 3 nm to 500 nm, A powder containing anion-modified cellulose nanofibers, the powder having a moisture content of 20 mass% or less, an average particle size of 45 μm or more, and a degree of dispersion of less than 25%.

2. The anion-modified cellulose nanofiber-containing powder according to claim 1, having an angle of repose of 40 to 49°.

3. The anion-modified cellulose nanofiber-containing powder according to claim 1, having a collapse angle of 15 to 24°.

4. The anion-modified cellulose nanofiber-containing powder according to claim 1, wherein the difference angle is 20 to 25°.

Citation Information

Patent Citations

  • Method for producing cellulose nanofiber dry solid

    WO2019189318A1