Resin composition, film, laminated film, and molded article
A resin composition combining non-crosslinked linear polymers with reactive groups and crosslinked particles addresses the issue of achieving both low gloss and fine surface finish in matte films, enhancing the aesthetic appeal of molded products.
Patent Information
- Application Number
- JP2024004130
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2023-03-29
- Filing Date
- 2024-01-15
- Publication Date
- 2024-10-11
AI Technical Summary
Existing matte films using inorganic and organic crosslinked particles fail to achieve a fine surface finish while effectively reducing gloss, and non-crosslinked linear polymers with reactive groups lack sufficient shine suppression.
A resin composition combining non-crosslinked linear polymers with reactive groups and organic crosslinked particles in specific ratios, along with optional non-reactive polymers, to create films and laminated films that maintain surface fineness while significantly reducing gloss.
The composition achieves a low gloss level while maintaining surface fineness, providing a sense of depth and luxury, suitable for various applications.
Smart Images

Figure 2024144104000001 
Figure 2024144104000002 
Figure 2024144104000003
Abstract
Description
[Technical field]
[0001] The present invention relates to a resin composition, a film, a laminated film, and a molded article. [Background technology]
[0002] In order to improve the design of the surface of a molded article, a matte film has been proposed which is obtained by forming a resin composition in which a matte agent is kneaded into an acrylic matrix into a film. Known matting agents include non-crosslinked linear polymers having reactive groups, inorganic particles, organic crosslinked particles, and the like (Patent Document 1). [Prior art documents] [Patent documents]
[0003] [Patent Document 1] Japanese Patent Application Publication No. 10-237261 Summary of the Invention [Problem to be solved by the invention]
[0004] In order to impart a sense of depth and a sense of luxury to the surface of a molded article using a matte film, it is necessary not only to reduce gloss and suppress shine, but also to ensure a fine surface texture. However, inorganic particles and organic crosslinked particles that have been used as matting agents in the past have made the surface too rough, making it difficult to obtain a fine texture. Furthermore, when the amount of the particles is reduced to prevent the surface from becoming too rough, sufficient shine-reducing effect cannot be obtained.
[0005] On the other hand, when a non-crosslinked linear polymer having a reactive group is used, although a fine surface texture can be obtained, a sufficient shine suppressing effect cannot be obtained. In view of the above circumstances, an object of the present invention is to provide a resin composition that can sufficiently reduce gloss and suppress shine while maintaining surface fineness, as well as a film, a laminated film, and a molded article that use this resin composition. [Means for solving the problem]
[0006] As a result of intensive research, the present inventors have found that the above problems can be solved by using, as a matting agent, a non-crosslinked linear polymer having a reactive group and organic crosslinked particles in an appropriate ratio. That is, the present invention relates to the following [1] to
[13] .
[0007] [1] A rubber-containing polymer (A), a reactive non-crosslinked polymer (B), crosslinked particles (C), and optionally a non-reactive non-crosslinked polymer (D), A resin composition, wherein a mass ratio of the reactive non-crosslinked polymer (B) to a total mass of the reactive non-crosslinked polymer (B) and the crosslinked particles (C) [(B) / (B+C)] is 25 to 95 mass %. [2] The resin composition according to [1], wherein the crosslinked particles (C) have a volume-based average particle size, as measured by the Coulter method, of 0.5 to 20 μm. [3] The resin composition according to [1] or [2], wherein a mass ratio of the crosslinked particles (C) to a total mass of the rubber-containing polymer (A), the reactive non-crosslinked polymer (B), and the non-reactive non-crosslinked polymer (D) [(C) / (A+B+D)] is 0.5 to 20 mass%. [4] The resin composition according to any one of [1] to [3], wherein a mass ratio of the reactive non-crosslinked polymer (B) to a total mass of the rubber-containing polymer (A), the reactive non-crosslinked polymer (B), and the non-reactive non-crosslinked polymer (D) [(B) / (A+B+D)] is 0.9 to 40 mass%. [5] The resin composition according to any one of [1] to [4], wherein the reactive non-crosslinked polymer (B) has one or more reactive groups selected from the group consisting of a carboxy group, a hydroxy group, an acid anhydride group, an epoxy group, an isocyanate group, an amide group, an amino group, a cyano group, and an imine group. [6] The resin composition according to any one of [1] to [5], wherein the MFR retention (M2 / M1), which is the ratio of the melt flow rate (M2) measured in accordance with JIS K7210 under conditions of a temperature of 240°C and a load of 49 N after heating for 120 minutes at 240°C to the melt flow rate (M1) measured in accordance with JIS K7210 under conditions of a temperature of 240°C and a load of 49 N after heating for 4 minutes at 240°C, is 60 to 115%. [7] A film using the resin composition according to any one of [1] to [6]. [8] The film according to [7], wherein the 60° surface gloss of the film surface in accordance with JIS Z8741 is 15% or less, and the 85° surface gloss is 24% or less. [9] The film according to [7] or [8], wherein the product of the 60° surface gloss of the film surface in accordance with JIS Z8741 and the root mean square slope RΔq in accordance with JIS B0601-2001 (60° surface gloss × RΔq) is 2.60 or less.
[10] A film having a 60° surface gloss of 15% or less in accordance with JIS Z8741, an 85° surface gloss of 24% or less, and a product of the 60° surface gloss of JIS Z8741 and the root mean square slope RΔq of JIS B0601-2001 (60° surface gloss × RΔq) of 2.60 or less.
[11] A laminate film comprising a support layer and a matte layer formed using the resin composition according to any one of [1] to [6] laminated thereon.
[12] A molded article comprising a substrate and the film according to any one of [7] to
[10] that covers at least a portion of a surface of the substrate.
[13] A molded article comprising a substrate and the laminate film of
[11] covering at least a portion of the surface of the substrate. Effect of the Invention
[0008] According to the resin composition, film or laminated film of the present invention, the glossiness can be sufficiently reduced to suppress shine while maintaining the fineness of the surface. Furthermore, the molded article of the present invention has a sufficiently low gloss while maintaining the fineness of the surface, so that it can have a sense of depth and a luxurious feel. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0009] Hereinafter, an embodiment of the present invention will be described, however, the present invention is not limited to the following. In this specification and claims, a numerical range expressed using "~" means a range including the numerical values before and after "~" as the lower and upper limits, and "X~Y" means equal to or greater than X and equal to or less than Y. The term "(meth)acrylic acid alkyl ester" means one or both of an acrylic acid alkyl ester and a methacrylic acid alkyl ester, and does not have a reactive group unless otherwise specified. The (meth)acryloyl group means either or both of an acryloyl group and a methacryloyl group. The term "vinyl monomer" refers to a monomer having one vinyl group, no other unsaturated groups, and no reactive groups. The term "crosslinkable monomer" refers to a monomer having multiple unsaturated groups. The term "unsaturated group" refers to a carbon-carbon double bond at the end of a molecule. "Reactive groups" means functional groups that are capable of bonding with each other. The term "main component" means that the proportion of the component in the total mass of all components is 50% by mass or more.
[0010] <Resin composition> The resin composition of the present embodiment contains a rubber-containing polymer (A), a reactive non-crosslinked polymer (B), crosslinked particles (C), and optionally a non-reactive non-crosslinked polymer (D).
[0011] [Rubber-containing polymer (A)] The rubber-containing polymer (A) is a graft copolymer having a multilayer structure in which graft chains are bonded to an elastic polymer. The rubber-containing polymer (A) preferably contains an alkyl (meth)acrylate ester as a main component. The rubber-containing polymer (A) forms a matrix in the resulting film or matte layer, and has the effect of imparting excellent impact resistance and elongation to the film or matte layer.
[0012] The rubber-containing polymer (A) can be obtained by polymerizing a monomer component constituting an elastic polymer to obtain an elastic polymer, and then polymerizing a monomer component constituting a graft chain in the presence of the obtained elastic polymer. For example, an elastic polymer can be obtained by polymerizing a monomer component consisting of 50 to 99.9 mass% of an alkyl acrylate having an alkyl group with 1 to 8 carbon atoms, 0.1 to 10 mass% of a crosslinkable monomer, and 0 to 49.9 mass% of other vinyl monomers, and then polymerizing 10 to 400 parts by mass of a monomer component consisting of 50 to 100 mass% of an alkyl methacrylate having 1 to 8 carbon atoms in the alkyl group and 0 to 50 mass% of other vinyl monomers in at least one stage in the presence of 100 parts by mass of the obtained elastic polymer.
[0013] The monomer component constituting the elastic polymer preferably contains an acrylic acid alkyl ester having an alkyl group with 1 to 8 carbon atoms, a crosslinkable monomer, and optionally other vinyl monomers. By containing an acrylic acid alkyl ester having an alkyl group with 1 to 8 carbon atoms as the main component, better impact resistance and moldability can be obtained.
[0014] The alkyl acrylate ester having an alkyl group with a carbon number of 1 to 8 contained in this monomer component preferably has an alkyl group with a carbon number of 1 to 7, more preferably 1 to 6, and further preferably 1 to 4. By having the carbon number of 8 or less, heat resistance is further improved.
[0015] As the alkyl acrylate having an alkyl group of 1 to 8 carbon atoms, methyl acrylate, ethyl acrylate, propyl acrylate, butyl acrylate, 2-ethylhexyl acrylate, and octyl acrylate are preferred. In particular, alkyl acrylates having a low glass transition temperature (Tg) are preferred, and butyl acrylate is more preferred. If the Tg is low, the elastic polymer has good impact resistance and can be easily molded. The alkyl acrylate contained in the monomer component constituting the elastic polymer may be one type or two or more types.
[0016] The mass proportion of the alkyl acrylate having an alkyl group of 1 to 8 carbon atoms in the monomer components constituting the elastic polymer is preferably 50 to 99.9 mass%, more preferably 60 to 99.9 mass%, and still more preferably 70 to 99.9 mass%. When the mass ratio of the acrylic acid alkyl ester having an alkyl group carbon number of 1 to 8 is 50 mass% or more, the formability of the film becomes better. When the mass ratio is 99.9 mass% or less, a sufficient amount of crosslinkable monomer can be blended.
[0017] The crosslinkable monomer contained in the monomer component constituting the elastic polymer has a plurality of unsaturated groups. The number of unsaturated groups possessed by the crosslinkable monomer is preferably 2 to 8, more preferably 2 to 6, and further preferably 2 to 4. Examples of functional groups having an unsaturated group include (meth)acryloyl groups, allyl groups, ethylene glycol dimethacrylate, butanediol dimethacrylate, allyl acrylate, allyl methacrylate, diallyl phthalate, triallyl cyanurate, triallyl isocyanurate, divinylbenzene, diallyl maleate, trimethylolpropane triacrylate, and allyl cinnamate. Among these, (meth)acryloyl groups and allyl groups are preferred.
[0018] Preferred examples of the crosslinkable monomer contained in the monomer component constituting the elastic polymer include ethylene glycol dimethacrylate, butanediol dimethacrylate, allyl acrylate, allyl methacrylate, diallyl phthalate, triallyl cyanurate, triallyl isocyanurate, divinylbenzene, diallyl maleate, trimethylol triacrylate, and allyl cinnamate. The crosslinkable monomer contained in the monomer component constituting the elastic polymer may be one type or two or more types.
[0019] The mass proportion of the crosslinkable monomer in the monomer components constituting the elastic polymer is preferably 0.1 to 10 mass %, more preferably 0.1 to 5 mass %, and even more preferably 0.5 to 2 mass %. By setting the mass ratio of the crosslinkable monomer to 0.1% by mass or more, the resulting film or laminated film has better molding whitening resistance and can be molded without deteriorating optical properties such as transparency. By setting the mass ratio of the crosslinkable monomer to 10% by mass or less, the resulting film or laminated film can be imparted with more sufficient flexibility and toughness.
[0020] The other vinyl monomer contained in the monomer component constituting the elastic polymer is copolymerizable with the alkyl acrylate ester and the crosslinking monomer. Other vinyl monomers include alkyl methacrylates such as methyl methacrylate, butyl methacrylate, and cyclohexyl methacrylate, styrene, and acrylonitrile. The other vinyl monomer contained in the monomer component constituting the elastic polymer may be one type or two or more types.
[0021] The mass proportion of other vinyl monomers in the monomer components constituting the elastic polymer is preferably 0 to 49.9 mass %, more preferably 0 to 20 mass %, and even more preferably 0 to 15 mass %. By controlling the mass ratio of the other vinyl monomer to 49.9 mass% or less, the heat resistance of the obtained film or laminated film is further improved. The other vinyl monomer does not need to be contained in the monomer component constituting the elastic polymer.
[0022] From the viewpoint of resistance to molding whitening and impact resistance, the elastic polymer preferably has a glass transition temperature (hereinafter sometimes referred to as "Tg") of 0°C or lower, more preferably from -60 to -10°C. Two or more kinds of elastomeric polymers may be used in combination, and the monomer components constituting the graft chains may be polymerized in the presence of two or more kinds of elastomeric polymers.
[0023] The monomer component constituting the graft chain preferably contains an alkyl methacrylate ester having an alkyl group with 1 to 8 carbon atoms, and optionally contains other vinyl monomers. The methacrylic acid alkyl ester contained in this monomer component and having an alkyl group with 1 to 8 carbon atoms preferably has an alkyl group with 1 to 6 carbon atoms, and more preferably has an alkyl group with 1 to 4 carbon atoms. By having the carbon number of 8 or less, the weather resistance of the obtained film or laminated film is further improved.
[0024] Specific examples include methyl methacrylate, ethyl methacrylate, butyl methacrylate, 2-ethylhexyl methacrylate, and cyclohexyl methacrylate. The methacrylic acid alkyl ester contained in the monomer component constituting the graft chain may be one type or two or more types.
[0025] The mass ratio of the methacrylic acid alkyl ester having an alkyl group with 1 to 8 carbon atoms in the monomer components constituting the graft chain is preferably 50 mass% or more, more preferably 60 mass% or more, and even more preferably 70 mass% or more. There is no particular upper limit, and it is 100 mass% or less. When the mass proportion of the methacrylic acid alkyl ester having an alkyl group with 1 to 8 carbon atoms is 50 mass % or more, the heat resistance of the obtained film or laminated film is further improved.
[0026] The other vinyl monomer contained in the monomer component constituting the graft chain is copolymerizable with the alkyl methacrylate ester. Other vinyl monomers include alkyl acrylates, styrene, acrylonitrile, and the like.
[0027] The alkyl acrylate ester, which is optionally contained in the monomer component for forming the graft chain, may be either linear or branched. Specific examples thereof include methyl acrylate, ethyl acrylate, propyl acrylate, n-butyl acrylate, 2-ethylhexyl acrylate, and n-octyl acrylate. Among these, methyl acrylate and n-butyl acrylate are preferred. The other vinyl monomer contained in the monomer component constituting the graft chain may be one type or two or more types.
[0028] The mass proportion of the other vinyl monomer in the monomer components constituting the graft chain is preferably from 0 to 50 mass%, more preferably from 0 to 40 mass%, and further preferably from 5 to 20 mass%. By controlling the mass ratio of the other vinyl monomer to 50 mass % or less, the heat resistance of the obtained film or laminated film is further improved. The other vinyl monomer does not have to be included in the monomer component constituting the graft chain.
[0029] The monomer component constituting the graft chain is 10 to 400 parts by mass, preferably 20 to 200 parts by mass, per 100 parts by mass of the elastic polymer. By using 10 parts by mass or more of the monomer component constituting the graft chain per 100 parts by mass of the elastic polymer, deterioration of transparency due to aggregation of the elastic polymer can be further prevented. By using 400 parts by mass or less per 100 parts by mass of the elastic polymer, the impact resistance of the obtained film or laminated film can be further improved.
[0030] The monomer component constituting the graft chain preferably has a Tg of 15° C. or higher, more preferably 20° C. or higher, when polymerized alone. The higher the Tg, the better, and there is no particular upper limit, but it can be, for example, 200° C. or lower. When the Tg of the polymerized monomer components constituting the graft chains is equal to or higher than the lower limit, the heat resistance of the resulting film or laminated film is improved. When the Tg is equal to or lower than the upper limit, the impact resistance of the resulting film or laminated film is improved. When only the monomer components constituting the graft chains are polymerized, the Tg can be adjusted by the type of vinyl monomer used.
[0031] The monomer components constituting the graft chain may be used in combination of two or more kinds, and two or more monomer components constituting the graft chain may be polymerized sequentially in the presence of one or two or more kinds of elastic polymers.
[0032] The rubber-containing polymer (A) preferably has a mass average particle diameter of 0.03 to 0.4 μm as measured by dynamic light scattering. The mass average particle diameter of the rubber-containing polymer (A) is preferably 0.03 μm or more, more preferably 0.07 μm or more, and even more preferably 0.09 μm or more. From the viewpoint of film transparency, the mass average particle diameter is preferably 0.4 μm or less, more preferably 0.30 μm or less, more preferably 0.15 μm or less, and even more preferably 0.13 μm or less.
[0033] When the mass average particle diameter of the rubber-containing polymer (A) is 0.03 μm or more, the film using the resin composition of the present embodiment does not become brittle, and it becomes easier to obtain a laminated film that can be formed on a support layer without problems. When the mass average particle diameter of the rubber-containing polymer (A) exceeds 0.4 μm, the transparency of the film using the resin composition of the present embodiment is likely to decrease. The mass average particle size of the rubber-containing polymer (A) can be adjusted by the amount of emulsifier used in the polymerization.
[0034] The rubber-containing polymer (A) preferably has a gel content of 40% by mass or more and 99% by mass or less, more preferably 50% by mass or more and 95% by mass or less, and even more preferably 55% by mass or more and 90% by mass or less. When the gel content of the rubber-containing polymer (A) is at least the preferred lower limit, the mechanical strength of the resulting film or laminated film can be increased, making it easier to handle.
[0035] A film or laminated film using a resin composition in which the gel content of the rubber-containing polymer (A) is 40% by mass or more can be easily laminated onto a three-dimensional substrate, and therefore various resin molded products, wood products, metal molded products, etc., with excellent design can be obtained.
[0036] When the gel content of the rubber-containing polymer (A) is equal to or lower than the upper limit, the flowability and thermal stability during molding are not too low, and the melt viscosity can be kept low. In addition, the retention in the molding machine can be reduced, which is preferable because the thermal deterioration of the resin can be suppressed. The gel content of the rubber-containing polymer (A) can be adjusted by the content of the elastic polymer in the rubber-containing polymer (A).
[0037] The mass average molecular weight (Mw) of the acetone soluble portion of the rubber-containing polymer (A) is preferably 20,000 or more, more preferably 30,000 or more, and is preferably 100,000 or less, more preferably 80,000 or less. When the mass average molecular weight (Mw) of the rubber-containing polymer (A) is equal to or greater than the preferred lower limit, the mechanical strength of the resulting film or laminated film is improved, and cracks during molding can be suppressed. In addition, the resulting film or laminated film exhibits stress whitening resistance. When the mass average molecular weight (Mw) is equal to or less than the preferred upper limit, the resulting film or laminated film has increased flexibility and excellent processability. When the resulting film or laminated film is laminated to a substrate such as a steel plate and then bent, whitening does not occur at the bent portion, and the appearance of the resulting molded products is good.
[0038] The mass average molecular weight (Mw) of the rubber-containing polymer (A) can be adjusted by the amount of chain transfer agent used in the polymerization. The mass average molecular weight (Mw) of the rubber-containing polymer (A) can be measured by the method described in the Examples. The acetone-soluble portion refers to the polymer contained in the acetone solution obtained by dissolving 0.5 g of the rubber-containing polymer (A) in 50 mL of acetone and refluxing the solution at 65° C. for 4 hours.
[0039] The rubber-containing polymer (A) preferably has at least two Tgs, namely, the Tg derived from the elastic polymer and the Tg derived from the graft chain. The preferred values of the Tg derived from the elastic polymer and the Tg derived from the graft chain are as described above. The Tg is calculated from the FOX formula using the Tg values of the homopolymers of each monomer component (as described in Polymer Handbook [Polymer Handbook, J. Brandrup, Interscience, 1989]).
[0040] In addition, Tg can also be measured by the following method (however, when the value calculated from the above FOX formula differs from the value calculated from the above FOX formula, the value calculated from the above FOX formula is adopted). First, the acrylic resin composition is melted and formed into a sheet, and a test piece with dimensions of 1 mm thickness, 6 mm width, and 65 mm length is cut out. Using a dynamic viscoelasticity measuring device, the storage modulus (E') and loss modulus (E") of the test piece are measured in a tensile mode in accordance with ISO6721-4 under the conditions of an initial chuck distance of 2 cm, a measurement frequency of 0.1 Hz, a measurement temperature range of -90 to 150°C, a heating rate of 2°C / min, and a nitrogen gas flow of 200 mL / min, and tan δ (loss tangent) at each temperature is calculated from the formula tan δ = E" / E'. Next, when the value of tan δ is plotted against the temperature, two or more peaks appear. The temperature corresponding to the peak appearing on the lowest temperature side among these is taken as the Tg of the elastic polymer.
[0041] The Tg of the graft chain is defined as the temperature corresponding to the peak with the maximum tan δ value among the peaks appearing at temperatures higher than 20° C. The Tg of the graft chain obtained here is preferably that of the outermost layer of the rubber-containing polymer. The Tg of the rubber-containing polymer (A) can be adjusted by the type and amount of monomer used in the polymerization.
[0042] The mass proportion of the rubber-containing polymer (A) in the resin composition is preferably from 5.5 to 90 mass %, more preferably from 10 to 80 mass %, and further preferably from 20 to 75 mass %. The mass proportion of the elastic polymer in the rubber-containing polymer (A) in the resin composition is preferably from 5 to 50 mass %, more preferably from 10 to 40 mass %.
[0043] When the mass proportion of the elastic polymer in the resin composition is 5 mass% or more, a film or laminate film using the resin composition of this embodiment is less likely to become brittle, and the impact resistance and film-forming properties of the film or laminate film are further improved. When the mass proportion of the elastic polymer in the resin composition is 50 mass % or less, the thickness precision of the film or laminated film is excellent, and the productivity of the film or laminated film is further improved.
[0044] The method for producing the rubber-containing polymer (A) is not particularly limited, but it can be obtained by a polymerization method such as emulsion polymerization, suspension polymerization, etc. When emulsion polymerization is used, it is preferable to use an emulsifier, a radical polymerization initiator, and a chain transfer agent.
[0045] As the emulsifier, anionic, cationic or nonionic surfactants can be used. Anionic surfactants are particularly preferred. Specific examples of anionic surfactants include the following: rosin acid soap, potassium oleate, sodium stearate, sodium myristate, sodium N-lauroyl sarcosinate, dipotassium alkenyl succinate and other carboxylates, sodium lauryl sulfate and other sulfates, sodium dioctyl sulfosuccinate, sodium dodecylbenzene sulfonate, sodium alkyl diphenyl ether disulfonate and other sulfonates, sodium polyoxyethylene alkyl phenyl ether phosphate and other phosphates. Examples of methods for preparing an emulsion include (1) a method in which a monomer mixture is charged into water and then a surfactant is added, (2) a method in which a surfactant is charged into water and then a monomer mixture is added, and (3) a method in which a surfactant is charged into a monomer mixture and then water is added. Of these, methods (1) and (2) are preferred.
[0046] Specific examples of radical polymerization initiators include the following: persulfates such as potassium persulfate and sodium persulfate; organic peroxides such as t-butyl hydroperoxide, cumene hydroperoxide, and benzoyl peroxide; azo compounds such as azobisisobutyronitrile; and redox initiators in which these persulfates or organic peroxides are combined with a reducing agent. Among these, redox initiators are preferred, and sulfoxylate initiators in which ferrous sulfate, disodium ethylenediaminetetraacetic acid, sodium formaldehyde sulfoxylate, and hydroperoxide are combined are more preferred. The radical polymerization initiator can be added to either or both of the aqueous phase and the monomer phase.
[0047] Specific examples of the chain transfer agent include alkyl mercaptans having 2 to 20 carbon atoms, mercapto acids, thiophenol, and carbon tetrachloride. The chain transfer agent is preferably mixed during polymerization of the graft chains. The polymerization temperature varies depending on the type and amount of the polymerization initiator, but is preferably 40 to 120°C, more preferably 60 to 95°C.
[0048] When the emulsion polymerization method is used, it is preferable to recover the rubber-containing polymer (A) as a powder from the latex after the polymerization reaction. As a method for recovering it as a powder, for example, the latex is brought into contact with a coagulant to be coagulated or salted out, solid-liquid separated, washed with water in an amount of about 1 to 100 times the mass of the polymer, and made into a wet powder by a dehydration treatment such as filtration, and further, this wet powder is dried with a hot air dryer such as a squeeze dehydrator or a fluidized dryer. In addition, the latex may be directly dried by a spray drying method. The drying temperature and drying time of the polymer can be appropriately determined depending on the type of polymer.
[0049] Specific examples of the coagulant include organic salts such as sodium acetate and calcium acetate, and inorganic salts such as sodium chloride, potassium chloride, calcium chloride, magnesium chloride, and sodium sulfate. Among them, calcium salts such as calcium acetate and calcium chloride are preferred. In particular, calcium acetate is more preferred from the viewpoint of hot water whitening resistance of the molded body and from the viewpoint of reducing the moisture content of the recovered powder. The coagulant may be used alone or in combination of two or more. The coagulant is usually used as an aqueous solution. The concentration of the aqueous solution of the coagulant, preferably calcium acetate, is preferably 0.1% by mass or more, more preferably 1% by mass or more, from the viewpoint of stably coagulating and recovering the acrylic resin composition. In addition, the concentration of the aqueous solution of the coagulant, preferably calcium acetate, is preferably 20% by mass or less, more preferably 15% by mass or less, from the viewpoint of the amount of the coagulant remaining in the recovered powder being small, and in particular the performance of the molded body, such as hot water whitening resistance and colorability, is hardly deteriorated. In addition, when the concentration of calcium acetate exceeds 20% by mass, calcium acetate may precipitate due to saturation at 10° C. or less.
[0050] The method of contacting latex with the coagulant includes, for example, a method of continuously adding latex to an aqueous solution of the coagulant while stirring the solution and continuing to stir for a certain period of time, and a method of continuously injecting the aqueous solution of the coagulant and latex at a certain ratio into a container equipped with a stirrer while contacting them, and continuously extracting a mixture containing the coagulated powder and water from the container. The amount of the aqueous solution of the coagulant is preferably 10 parts by mass or more and 500 parts by mass or less per 100 parts by mass of latex. The temperature in the coagulation step is preferably 30°C or more and 100°C or less.
[0051] [Reactive non-crosslinked polymer (B)] The reactive non-crosslinked polymer (B) is a non-crosslinked linear polymer in the resin composition before film formation or matte layer formation, and is a component that crosslinks and becomes fine particles when heated during film formation, etc. The reactive non-crosslinked polymer (B) has the effect of enhancing the matting effect while maintaining the fineness of the surface.
[0052] The reactive non-crosslinked polymer (B) can be obtained, for example, by polymerizing monomer components consisting of 1 to 80 mass % of a (meth)acrylic acid alkyl ester having an alkyl group with 1 to 8 carbon atoms and a reactive group, 10 to 99 mass % of a methacrylic acid alkyl ester having an alkyl group with 1 to 13 carbon atoms, 0 to 79 mass % of an acrylic acid alkyl ester having an alkyl group with 1 to 8 carbon atoms, and 0 to 50 mass % of other vinyl monomers.
[0053] In the (meth)acrylic acid alkyl ester having a reactive group and an alkyl group having 1 to 8 carbon atoms contained in the monomer component constituting the reactive non-crosslinked polymer (B), the alkyl group preferably has a carbon number of 1 to 4. When the carbon number is 8 or less, a good matte appearance is achieved. The (meth)acrylic acid alkyl ester may be any of an acrylic acid alkyl ester, a methacrylic acid alkyl ester, or a mixture thereof, but from the viewpoint of heat resistance, a methacrylic acid alkyl ester is preferred.
[0054] Examples of the reactive group of the reactive non-crosslinked polymer (B) include a carboxy group, a hydroxy group, an acid anhydride group, an epoxy group, an isocyanate group, an amide group, an amino group, a cyano group, an imine group, an aldehyde group, and a sulfo group. Among them, it is preferable to use at least one selected from the group consisting of a carboxy group, a hydroxy group, an acid anhydride group, an epoxy group, an isocyanate group, an amide group, an amino group, a cyano group, and an imine group. In particular, a hydroxy group is preferable. These reactive groups can bond to each other and crosslink the reactive non-crosslinked polymer (B) when the resin composition is heated (usually at 150° C. or higher) during film formation, etc. For example, hydroxy groups can bond to each other by intermolecular dehydration condensation, etc.
[0055] Examples of monomers having a reactive group include hydroxyalkyl (meth)acrylates, acrylic acid, methacrylic acid, carboxyethyl (meth)acrylate, maleic acid, fumaric acid, crotonic acid, (meth)acrylamide, diethylacrylamide, aminoethyl (meth)acrylate, glycidyl alkyl (meth)acrylate, (meth)acryloyl isocyanate, and cyanoethyl acrylate. Among these, in terms of improving the matte appearance of the resulting film or molded article, it is preferable that the reactive non-crosslinked polymer (B) is a polymer containing a hydroxy group as a reactive group, and specifically, it is preferable that the reactive non-crosslinked polymer (B) is a polymer having a (meth)acrylic acid hydroxyalkyl ester as a monomer unit.
[0056] Examples of (meth)acrylic acid alkyl esters having a hydroxy group as a reactive group, i.e., (meth)acrylic acid hydroxyalkyl esters, include 2-hydroxyethyl methacrylate, 2-hydroxypropyl methacrylate, 2,3-dihydroxypropyl methacrylate, 2-hydroxyethyl acrylate, 4-hydroxybutyl acrylate, etc. Among these, 2-hydroxyethyl methacrylate is preferred from the viewpoint of excellent matte development.
[0057] The number of reactive groups possessed by the (meth)acrylic acid alkyl ester per monomer is preferably 1 to 3, and more preferably 1 to 2. If the number of reactive groups possessed by the (meth)acrylic acid alkyl ester is 1 or more, it can bond with reactive groups possessed by other (meth)acrylic acid alkyl esters, so that the reactive non-crosslinked polymer (B) can be crosslinked during film formation. If the number of reactive groups possessed by the (meth)acrylic acid alkyl ester is 2 or less, foreign matter in the film can be further reduced. The (meth)acrylic acid alkyl ester having a reactive group contained in the monomer component constituting the reactive non-crosslinked polymer (B) may be one type or two or more types.
[0058] The mass proportion of the (meth)acrylic acid alkyl ester having a reactive group in the monomer components constituting the reactive non-crosslinked polymer (B) is preferably 1 to 80 mass%, more preferably 5 to 50 mass%, and even more preferably 20 to 50 mass%. When the mass ratio of the (meth)acrylic acid alkyl ester having a reactive group is 1 mass % or more, the matte effect is further enhanced, and when it is 80 mass % or less, it is easy to avoid a decrease in elongation and a poor surface condition.
[0059] The alkyl methacrylate ester having an alkyl group with 1 to 13 carbon atoms contained in the monomer component constituting the reactive non-crosslinked polymer (B) preferably has an alkyl group with 1 to 8 carbon atoms, more preferably 1 to 4. By having the carbon number of 13 or less, the water resistance of the film or laminated film is further improved.
[0060] As the methacrylic acid alkyl ester having an alkyl group of 1 to 8 carbon atoms contained in the monomer component constituting the reactive non-crosslinked polymer (B), lower methacrylic acid alkyl esters such as methyl methacrylate, ethyl methacrylate, and butyl methacrylate are suitable, and among these, methyl methacrylate is preferred. The methacrylic acid alkyl esters having an alkyl group of 1 to 13 carbon atoms contained in the monomer component constituting the reactive non-crosslinked polymer (B) may be of one type or two or more types.
[0061] The mass proportion of the alkyl methacrylate ester in the monomer components constituting the reactive non-crosslinked polymer (B) is preferably 10 to 99 mass%, and from the viewpoint of water resistance, is more preferably 30 to 95 mass%, and further preferably 50 to 95 mass%.
[0062] The alkyl acrylate ester having an alkyl group with 1 to 8 carbon atoms contained in the monomer component constituting the reactive non-crosslinked polymer (B) preferably has an alkyl group with 1 to 8 carbon atoms, more preferably 1 to 4. By having the carbon number of 8 or less, the thermal decomposition resistance of the film or laminated film is further improved.
[0063] As the alkyl acrylate having 1 to 8 carbon atoms in the alkyl group contained in the monomer component constituting the reactive non-crosslinked polymer (B), lower alkyl acrylates such as methyl acrylate, ethyl acrylate, butyl acrylate, and 2-ethylhexyl acrylate are preferred, and among these, methyl acrylate, ethyl acrylate, and butyl acrylate are preferred. The alkyl acrylate ester having an alkyl group of 1 to 8 carbon atoms contained in the monomer component constituting the reactive non-crosslinked polymer (B) may be of one type or of two or more types.
[0064] The mass proportion of the alkyl acrylate in the monomer components constituting the reactive non-crosslinked polymer (B) is preferably 0 to 79 mass %, and more preferably 0 to 40 mass %, in order to improve the water whitening resistance of the film, and from the viewpoints of thermal decomposition and water whitening resistance, it is preferably 0.1 to 25 mass %, more preferably 0.1 to 20 mass %, and even more preferably 0.1 to 15 mass %. The alkyl acrylate ester may not be contained in the monomer component constituting the reactive non-crosslinked polymer (B).
[0065] Other vinyl monomers contained in the monomer components constituting the reactive non-crosslinked polymer (B) are copolymerizable with (meth)acrylic acid alkyl esters having an alkyl group with 1 to 8 carbon atoms and a reactive group, methacrylic acid alkyl esters having an alkyl group with 1 to 13 carbon atoms, and acrylic acid alkyl esters having an alkyl group with 1 to 8 carbon atoms.
[0066] Other vinyl monomers include vinyl aromatic monomers such as styrene, vinyl toluene, α-methylstyrene, and halogenated styrene; methacrylic acid, fumaric acid, maleic acid, and copolymerizable carboxylic acids and their esters, such as alkyl methacrylates having an alkyl group with 1 to 13 carbon atoms, alkyl acrylates having an alkyl group with 9 or more carbon atoms, vinyl halides such as vinyl chloride and vinyl bromide, vinyl esters such as vinyl acetate, and acrylonitrile. The other vinyl monomer contained in the monomer component constituting the reactive non-crosslinked polymer (B) may be one type or two or more types.
[0067] The mass proportion of other vinyl monomers in the monomer components constituting the reactive non-crosslinked polymer (B) is preferably 0 to 50 mass%, more preferably 0 to 30 mass%, and even more preferably 0 to 15 mass%. When the mass ratio of the other vinyl monomer is 50 mass % or less, the water resistance of the film is further improved. The other vinyl monomer does not need to be contained in the monomer component constituting the reactive non-crosslinked polymer (B).
[0068] The method for producing the reactive non-crosslinked polymer (B) is not particularly limited, but a method using suspension polymerization is preferred from the viewpoint of cost. As the initiator for suspension polymerization, those used in normal suspension polymerization are used, and examples thereof include organic peroxides and azo compounds. As the suspension stabilizer, those used in normal suspension polymerization are used, and examples thereof include organic colloidal polymeric substances, inorganic colloidal polymeric substances, inorganic fine particles, and combinations of these with surfactants. Suspension polymerization is usually carried out by suspending the monomer components together with a polymerization initiator in an aqueous solution in the presence of a suspension stabilizer. In addition, it is also possible to carry out the polymerization by dissolving a polymerizable material soluble in the monomer components in the monomer and using it.
[0069] The intrinsic viscosity of the reactive non-crosslinked polymer (B) before crosslinking is preferably 0.05 to 0.3 L / g, more preferably 0.06 to 0.15 L / g. Within this range, a constant good matte property is easily exhibited regardless of forming conditions such as conditions in the process of melt-kneading the components of the resin composition and conditions in the process of processing the obtained resin composition into a molded product such as a film.
[0070] To adjust the intrinsic viscosity, it is preferable to use a polymerization degree regulator such as mercaptan. As the mercaptan, n-octyl mercaptan, n-dodecyl mercaptan, t-dodecyl mercaptan, etc. are used, but the mercaptan is not limited to these and any known mercaptan can be used.
[0071] The mass average molecular weight Mw of the reactive non-crosslinked polymer (B) is preferably 30,000 or more, more preferably 50,000 or more, and is preferably 250,000 or less, more preferably 200,000 or less. If Mw is 30,000 or more, the dispersibility in the resin composition is improved, while if it is 250,000 or less, a fine matte appearance is easily expressed. The mass average molecular weight Mw of the reactive non-crosslinked polymer (B) can be measured by the method described in the Examples.
[0072] The reactive non-crosslinked polymer (B) is not particularly limited, but from the viewpoint of water whitening resistance, the glass transition temperature Tg before crosslinking is preferably 30° C. or higher, more preferably more than 50° C. Also, from the viewpoint of dispersibility during melt kneading in the compounding process, the glass transition temperature Tg is preferably 120° C. or lower, more preferably 110° C. or lower. The Tg of the polymer (B) is calculated from the FOX formula using the Tg values of the homopolymers of each monomer component (as described in Polymer Handbook [Polymer Handbook, J. Brandrup, Interscience, 1989]).
[0073] The mass proportion of the reactive non-crosslinked polymer (B) in the resin composition is preferably from 0.9 to 40 mass %, more preferably from 1.4 to 20 mass %, and further preferably from 1.9 to 15 mass %. If the amount of reactive non-crosslinked polymer (B) added is 0.9 parts by mass or more, a sufficient matte appearance is obtained. If the amount of reactive non-crosslinked polymer (B) added is 40 parts by mass or less, the flowability and thermal stability during molding are not too low, the melt viscosity can be kept lower, and the retention in the molding machine can be reduced, thereby suppressing thermal deterioration of the resin. In addition, fineness can be easily maintained.
[0074] [Crosslinked particles (C)] The crosslinked particles (C) are components that have already been crosslinked into fine particles in the resin composition before it is formed into a film or the like. The crosslinked particles (C) have the effect of enhancing the matting effect.
[0075] The crosslinked particles (C) can be obtained, for example, by polymerizing a monomer component consisting of 50.0 to 99.9 mass % of a (meth)acrylic acid alkyl ester having an alkyl group with 1 to 8 carbon atoms, 0.1 to 20 mass % of a crosslinkable monomer, and 0 to 49.9 mass % of other vinyl monomers.
[0076] The (meth)acrylic acid alkyl ester having an alkyl group with a carbon number of 1 to 8 contained in the monomer component constituting the crosslinked particles (C) preferably has an alkyl group with a carbon number of 1 to 6, more preferably 1 to 4. When the carbon number is 8 or less, weather resistance is further improved.
[0077] The (meth)acrylic acid alkyl ester may be any of an acrylic acid alkyl ester, a methacrylic acid alkyl ester, and a mixture thereof, but is preferably a methacrylic acid alkyl ester since it provides better water resistance. The (meth)acrylic acid alkyl ester contained in the monomer component constituting the crosslinked particles (C) may be one type or two or more types.
[0078] The mass proportion of the (meth)acrylic acid alkyl ester in the monomer components constituting the crosslinked particles (C) is preferably 50.0 to 99.9 mass%, more preferably 60 to 99.9 mass% from the viewpoint of heat resistance, and even more preferably 70 to 99.9 mass%.
[0079] The crosslinkable monomer contained in the monomer component constituting the crosslinked particles (C) has a plurality of unsaturated groups. The number of unsaturated groups possessed by the crosslinkable monomer is preferably 2 to 8, more preferably 2 to 6, and still more preferably 2 to 4. Examples of the functional group having an unsaturated group include a (meth)acryloyl group, an allyl group, and vinyl groups other than these. Among these, a (meth)acryloyl group and an allyl group are preferred.
[0080] Preferred examples of the crosslinkable monomer contained in the monomer component constituting the crosslinked particles (C) include trimethylolpropane trimethacrylate and trimethylolpropane triacrylate. Examples of the crosslinkable monomer contained in the monomer component constituting the crosslinked particles (C) include dialkylene glycol dimethacrylates such as ethylene glycol dimethacrylate, diethylene glycol dimethacrylate, dipropylene glycol dimethacrylate, dibutylene glycol dimethacrylate, etc., or acrylates of these methacrylates, vinyl group-containing polyfunctional monomers such as divinylbenzene, divinyl adipate, etc., and allyl group-containing polyfunctional monomers such as diallyl phthalate, diallyl maleate, allyl acrylate, allyl methacrylate, triallyl cyanurate, triallyl isocyanurate, etc. The crosslinkable monomer contained in the monomer component constituting the crosslinked particles (C) may be one type or two or more types.
[0081] The mass proportion of the crosslinkable monomer in the monomer components constituting the crosslinked particles (C) is preferably 0.1 to 20 mass%, more preferably 0.1 to 10 mass%, even more preferably 0.1 to 3 mass%, and particularly preferably 0.1 to 2 mass%. When the mass proportion of the crosslinkable monomer is 0.1 mass % or more, the matte property is further improved, and when it is 20 mass % or less, the impact resistance of the film is further improved.
[0082] The other vinyl monomer contained in the monomer component constituting the crosslinked particles (C) is copolymerizable with the (meth)acrylic acid alkyl ester having an alkyl group having 1 to 8 carbon atoms, and the crosslinkable vinyl monomer.
[0083] As the other vinyl monomer, the same monomers as the other vinyl monomers exemplified as the monomers constituting the elastic polymer of the rubber-containing polymer (A) can be used. The other vinyl monomer contained in the monomer component constituting the crosslinked particles (C) may be one type or two or more types.
[0084] The mass proportion of other vinyl monomers in the monomer components constituting the crosslinked particles (C) is preferably 0 to 49.9 mass%, more preferably 0 to 20 mass%, and even more preferably 15 mass% or less. By controlling the mass ratio of the other vinyl monomer to 49.9 mass % or less, the heat resistance is further improved. The other vinyl monomer does not necessarily have to be contained in the monomer component constituting the crosslinked particles (C).
[0085] The crosslinked particles (C) preferably have a volume-based average particle size measured by the Coulter method of 0.5 to 20 μm, more preferably 1 to 10 μm, further preferably 2 to 8 μm, and particularly preferably 2 to 6 μm. When the average particle size is equal to or larger than the preferred lower limit, the matte effect is easily enhanced, and when the average particle size is equal to or smaller than the preferred upper limit, fineness is easily maintained.
[0086] The method for producing the crosslinked particles (C) is not particularly limited, and examples thereof include suspension polymerization, emulsion polymerization, etc. It is preferable to produce the crosslinked particles (C) by suspension polymerization using an acrylic acid alkyl ester, a methacrylic acid alkyl ester, or a crosslinkable monomer having two or more non-conjugated double bonds per molecule that can be copolymerized with these monomers, so that the average particle size is 0.5 to 20 μm. The crosslinked particles (C) are separated and recovered from the polymer slurry obtained by such copolymerization by ordinary treatments such as washing, dehydration, drying, etc. The average particle size of the crosslinked particles (C) can be adjusted by the content of the crosslinkable monomer.
[0087] The mass proportion of the crosslinked particles (C) in the resin composition is preferably from 0.5 to 20 parts by mass, more preferably from 1 to 15 parts by mass, and even more preferably from 2 to 10 parts by mass. When the mass ratio of the crosslinked particles (C) in the resin composition is equal to or more than the preferred lower limit, the matte effect is easily enhanced, and when it is equal to or less than the preferred upper limit, fineness is easily maintained.
[0088] [Non-reactive non-crosslinked polymer (D)] The non-reactive non-crosslinked polymer (D) is a non-crosslinked polymer having no reactive groups, and is an optional component that forms a matrix together with the rubber-containing polymer (A) in the resulting film or matte layer.
[0089] The non-reactive non-crosslinked polymer (D) can be obtained, for example, by polymerizing a monomer component consisting of 50 to 100 mass % of an alkyl methacrylate ester having an alkyl group with 1 to 8 carbon atoms, 0 to 50 mass % of an alkyl acrylate ester having an alkyl group with 1 to 8 carbon atoms, and 0 to 49 mass % of other vinyl monomers.
[0090] The methacrylic acid alkyl ester having an alkyl group with a carbon number of 1 to 8 contained in the monomer component constituting the non-reactive non-crosslinked polymer (D) preferably has an alkyl group with a carbon number of 1 to 6, more preferably 1 to 4. When the carbon number is 8 or less, heat resistance is further improved.
[0091] As the methacrylic acid alkyl ester having an alkyl group of 1 to 8 carbon atoms contained in the monomer component constituting the non-reactive non-crosslinked polymer (D), lower methacrylic acid alkyl esters such as methyl methacrylate, ethyl methacrylate, and butyl methacrylate are suitable, and among these, methyl methacrylate is preferred. The methacrylic acid alkyl esters having an alkyl group of 1 to 8 carbon atoms contained in the monomer component constituting the non-reactive non-crosslinked polymer (D) may be of one type or two or more types.
[0092] The mass ratio of the methacrylic acid alkyl ester in the monomer components constituting the non-reactive non-crosslinked polymer (D) is preferably 50 to 100 mass%, more preferably 50 mass% or more in terms of weather resistance, further preferably 85 mass% or more, particularly preferably 92 mass% or more, while from the viewpoint of heat resistance, it is preferably 100 mass% or less, more preferably 99.9 mass% or less. The non-reactive non-crosslinked polymer (D) may be composed only of an alkyl methacrylate ester.
[0093] The alkyl acrylate ester having an alkyl group with 1 to 8 carbon atoms contained in the monomer component constituting the non-reactive non-crosslinked polymer (D) preferably has an alkyl group with 1 to 6 carbon atoms, more preferably 1 to 4. By having the carbon number of 8 or less, the impact resistance is further improved.
[0094] As the alkyl acrylate having 1 to 8 carbon atoms in the alkyl group contained in the monomer component constituting the non-reactive non-crosslinked polymer (D), lower alkyl acrylates such as methyl acrylate, ethyl acrylate, butyl acrylate, and 2-ethylhexyl acrylate are suitable, and among these, methyl acrylate is preferred. The alkyl acrylate ester having an alkyl group of 1 to 8 carbon atoms contained in the monomer component constituting the non-reactive non-crosslinked polymer (D) may be of one type or two or more types.
[0095] The mass proportion of the alkyl acrylate in the monomer components constituting the non-reactive non-crosslinked polymer (D) is preferably 0 to 50 mass%, more preferably 0 to 15 mass%, and even more preferably 0 to 8 mass%. By controlling the mass ratio of the alkyl acrylate to 50 mass% or less, the matte appearance of the film or laminated film is further improved. The alkyl acrylate does not need to be contained in the monomer component constituting the non-reactive non-crosslinked polymer (D).
[0096] Other vinyl monomers contained in the monomer components constituting the non-reactive non-crosslinked polymer (D) are copolymerizable with methacrylic acid alkyl esters having an alkyl group with 1 to 8 carbon atoms and acrylic acid alkyl esters having an alkyl group with 1 to 8 carbon atoms.
[0097] As the other vinyl monomer, there can be mentioned the same monomers as the other vinyl monomers exemplified as the monomers constituting the elastic polymer of the rubber-containing polymer (A). The other vinyl monomer contained in the monomer component constituting the reactive non-crosslinked polymer (B) may be one type or two or more types.
[0098] The mass proportion of other vinyl monomers in the monomer components constituting the non-reactive non-crosslinked polymer (D) is preferably 0 to 49 mass%, more preferably 0 to 15 mass%, and even more preferably 0 to 5 mass%, from the viewpoint of water whitening resistance of the film. The other vinyl monomer may not be included in the monomer component constituting the non-reactive non-crosslinked polymer (D).
[0099] The method for producing the non-reactive non-crosslinked polymer (D) is not particularly limited, but for example, a method based on emulsion polymerization or suspension polymerization is preferred.
[0100] The mass proportion of the non-reactive non-crosslinked polymer (D) in the resin composition is preferably from 0 to 49.9 mass %, and more preferably from 0 to 25 mass %. When the mass ratio of the non-reactive non-crosslinked polymer (D) in the resin composition is equal to or more than the preferred lower limit, the heat resistance is improved. The non-reactive non-crosslinked polymer (D) does not have to be contained in the resin composition.
[0101] [Blending ratio] In the resin composition in this embodiment, the mass ratio of the reactive non-crosslinked polymer (B) to the total mass (100 mass%) of the reactive non-crosslinked polymer (B) and the crosslinked particles (C) [(B) / (B+C)] is 25 to 95 mass%. [(B) / (B+C)] is preferably from 30 to 93 mass %, more preferably from 35 to 90 mass %, and most preferably from 50 to 90 mass parts. By making [(B) / (B+C)] 25% by mass or more, the fineness of the surface can be maintained. By making [(B) / (B+C)] 95% by mass or less, the glossiness can be sufficiently reduced.
[0102] In the resin composition in this embodiment, the mass ratio of the crosslinked particles (C) to the total mass (100 mass%) of the rubber-containing polymer (A), the reactive non-crosslinked polymer (B), and the non-reactive non-crosslinked polymer (D) [(C) / (A+B+D)] is preferably 0.5 to 20 mass%. [(C) / (A+B+D)] is more preferably 1 to 15 mass %, further preferably 2 to 10 mass %. By making [(C) / (A+B+D)] equal to or greater than the preferred lower limit, the effect of reducing glossiness is enhanced. By making [(C) / (A+B+D)] equal to or less than the preferred upper limit, it becomes easier to maintain the fineness of the surface.
[0103] In the resin composition in this embodiment, the mass ratio of the reactive non-crosslinked polymer (B) to the total mass (100 mass%) of the rubber-containing polymer (A), the reactive non-crosslinked polymer (B), and the non-reactive non-crosslinked polymer (D) [(B) / (A+B+D)] is preferably 0.9 to 40 mass%. [(B) / (A+B+D)] is more preferably from 1.4 to 20 mass %, and further preferably from 1.9 to 15 mass %. When [(B) / (A+B+D)] is equal to or greater than the preferred lower limit, the matte effect is easily enhanced. When [(B) / (A+B+D)] is equal to or less than the preferred upper limit, fineness is easily maintained. When the amount of reactive non-crosslinked polymer (B) added is 0.9 parts by mass or more, a sufficient matte appearance is obtained. When the amount of reactive non-crosslinked polymer (B) added is 40 parts by mass or less, the flowability and thermal stability during molding are not too low, the melt viscosity can be kept lower, and the retention in the molding machine can be reduced, which is preferable since thermal deterioration of the resin can be suppressed.
[0104] [Other ingredients] The resin composition of the present embodiment may contain general compounding agents, such as stabilizers, lubricants, processing aids, plasticizers, impact resistance aids, foaming agents, fillers, colorants, and ultraviolet absorbers, as necessary.
[0105] In particular, in terms of protecting the substrate, it is preferable that an ultraviolet absorber is added to impart weather resistance. The molecular weight of the ultraviolet absorber used is preferably 300 or more, and particularly preferably 400 or more. If an ultraviolet absorber with a molecular weight smaller than 300 is used, it may volatilize during vacuum molding or pressure molding in an injection mold, causing mold staining. The type of ultraviolet absorber is not particularly limited, but benzotriazole-based or triazine-based ultraviolet absorbers with a molecular weight of 400 or more are particularly preferably used. Specific examples of the former include Tinuvin (registered trademark) 234 from BASF Japan Co., Ltd. and Adeka STAB (registered trademark) LA-31 from ADEKA Corporation, and specific examples of the latter include Tinuvin 1577 from BASF Japan Co., Ltd. The ultraviolet absorber is preferably contained in a range of 0.1 to 5 mass% relative to the total mass of the resin composition (100 mass%).
[0106] In addition, from the viewpoint of weather resistance, it is preferable that a light stabilizer is added. As the light stabilizer, a known one can be used, but in particular, a radical scavenger such as a hindered amine light stabilizer is preferable. Commercially available products of such light stabilizers include Chimassorb (registered trademark) 944, Chimassorb 2020, and Tinuvin 770 from BASF Japan Ltd., and Adeka STAB LA-57G and Adeka STAB LA-72 from ADEKA Corporation (all of the above are product names).
[0107] [MFR retention rate] The resin composition of the present embodiment preferably has an MFR retention (M2 / M1) of 60 to 115%, which is the ratio of the melt flow rate (M2) measured in accordance with JIS K7210 under conditions of 240°C and a load of 49 N after heating for 120 minutes at 240°C to the melt flow rate (M1) (100%) measured in accordance with JIS K7210 under conditions of 240°C and a load of 49 N after heating for 4 minutes at 240°C. The MFR retention (M2 / M1) is more preferably from 80 to 110% by mass, and further preferably from 85 to 105% by mass.
[0108] When the MFR retention (M2 / M1) is within the preferred range, the thermal stability is excellent. An MFR retention rate (M2 / M1) of 60% or more is preferable because it can increase the thermal stability during molding, reduce the increase in melt viscosity due to thermal degradation of the resin, reduce retention in the molding machine, and suppress thermal degradation of the resin. If the MFR retention rate (M2 / M1) is 115% or less, the thermal stability during molding can be increased and the thermal decomposition of the resin can be suppressed to a low level, which is preferable since it can suppress thermal deterioration of the resin due to side reactions.
[0109] Films and laminated films made from resin compositions with an MFR retention rate (M2 / M1) of 60% or more and 115% or less are less susceptible to problems such as an increase in defects called fish eyes caused by thermal degradation over time. In addition, it is possible to obtain a film or a laminated film by continuing melt extrusion for a long period of time.
[0110] <Film> The film of the present embodiment is a film using a resin composition. As the resin composition, it is preferable to use the resin composition of the present embodiment described above. The film of the present embodiment may be produced by any method such as a T-die method or an inflation method, but the T-die method is preferred from the viewpoint of economy.
[0111] In particular, it is preferable to produce the resin composition in a molten state by cooling and solidifying it without sandwiching it between two metal rolls, thereby preventing thickness regulation and surface transfer, and by contacting only one metal roll at a time and cooling and solidifying it. The surface that does not contact the metal roll becomes the surface (matte surface). The back surface (the side in contact with the metal roll) of the obtained film may be printed.
[0112] The thickness of the film is preferably 1 μm or more, more preferably 5 μm or more, and even more preferably 20 μm or more, from the viewpoint of good handling and lamination properties of the film, and is preferably 500 μm or less, more preferably 300 μm or less, and even more preferably 200 μm or less, from the viewpoint of good film formability and processability when formed into a film. If the thickness of the film is equal to or greater than the lower limit, the appearance of the molded product is easily given sufficient depth. If the thickness of the film is equal to or less than the upper limit, the rigidity is not excessively large, and the film has good lamination properties and secondary processability. In addition, the mass per unit area can be reduced, which is economically advantageous. In addition, within the preferred range, film formation is easy and a stable film production is facilitated.
[0113] The film of the present embodiment has a total light transmittance of preferably 80% or more, more preferably 85% or more, and even more preferably 90% or more, as measured according to JIS K7361-1. If the total light transmittance is 80% or more, the decorative layer printed on the back surface of the film is beautiful when viewed from the front surface (matte surface) on which the decorative layer is not printed.
[0114] The film of the present embodiment is not particularly limited, but from the viewpoint of the beauty of the appearance as a matte film, the overall haze is preferably 95% or less, and more preferably 90% or less. The overall haze of the film is a value measured in accordance with JIS K7136.
[0115] The film of the present embodiment has a 60° surface gloss of the film surface (matte surface) according to JIS Z8741 of preferably 15% or less, more preferably 14% or less, and an 85° surface gloss of the film surface according to JIS Z8741 of preferably 24% or less, more preferably 23.5% or less. By keeping the 60° surface glossiness and the 85° surface glossiness at or below the preferred upper limit values, shine can be suppressed.
[0116] In the film of this embodiment, the product of the 60° surface gloss of the film surface in accordance with JIS Z8741 and the root mean square slope RΔq in accordance with JIS B0601-2001 (60° surface gloss × RΔq) is preferably 2.60 or less, and more preferably 2.42 or less. If the product of the 60° surface gloss and the root mean square slope RΔq is equal to or less than the preferred upper limit, the gloss is sufficiently low while maintaining the fineness of the surface, so that a sense of depth and luxury can be achieved.
[0117] <Laminated film> The laminated film of the present embodiment is a laminated film in which a matte layer using a resin composition is laminated on a support layer. As the resin composition, it is preferable to use the resin composition of the present embodiment described above.
[0118] The support layer is not particularly limited, but is preferably a composition that does not exhibit matte properties, is moldable, and contains a transparent resin as a main component. In particular, a composition containing a transparent acrylic resin is preferred because it does not exhibit matte properties, does not inhibit the matte properties of the matte layer, is easy to form into a film, and has good interlayer adhesion with the matte layer.
[0119] The support layer may be an acrylic resin composition that does not contain a matte component such as the reactive non-crosslinked polymer (B) in the resin composition of this embodiment and the crosslinked particles (C). An acrylic resin composition that contains the rubber-containing polymer (A) and the non-reactive non-crosslinked polymer (D) in the resin composition of this embodiment, an ultraviolet absorber, a light stabilizer, an antioxidant, and various additives can be suitably used.
[0120] The thickness of the laminated film is preferably 300 μm or less, more preferably 200 μm or less. Also, it is preferably 15 μm or more, more preferably 40 μm or more. If the thickness is 15 μm or more, sufficient depth can be obtained in the appearance of the molded product, which is preferable. In particular, when molding into a complex shape, sufficient thickness can be obtained by stretching. On the other hand, if the thickness is 300 μm or less, it has appropriate rigidity, which tends to improve lamination properties, secondary processability, etc., and is preferable. In addition, it is economically advantageous in terms of mass per unit area. Furthermore, the film-forming properties are stable, making it easy to manufacture the film.
[0121] The layer thickness ratio of the matte layer and the support layer in the laminated film is not particularly limited. However, from the viewpoint of the transparency, matte appearance and printability of the acrylic matte resin laminated film, it is preferably 1 / 99 to 99 / 1, and more preferably 50 / 50 to 10 / 90 (matte acrylic resin layer / transparent acrylic resin layer). In addition, if it is within the preferred range, film formation is easy and the laminated film is easy to manufacture stably.
[0122] The laminate film of the present embodiment preferably has a total light transmittance of 90% or more throughout the laminate film. If the total light transmittance is 90% or more, the laminate film has excellent design when laminated onto the surface of various three-dimensional resin molded products, woodwork products, or metal molded products.
[0123] The overall haze of the laminate film of the present embodiment is not particularly limited, but from the viewpoint of the beauty of the appearance as a matte film, it is preferably 95% or less, more preferably 90% or less, and even more preferably 85% or less. The overall haze of the film is a value measured in accordance with JIS K7136.
[0124] In the laminate film of this embodiment, the 60° surface gloss of the film surface (the surface of the matte layer opposite the support layer) according to JIS Z8741 is preferably 15% or less, more preferably 14% or less, and the 85° surface gloss of the film surface according to JIS Z8741 is preferably 24% or less, more preferably 23.5% or less. By keeping the 60° surface glossiness and the 85° surface glossiness at or below the preferred upper limit values, shine can be suppressed.
[0125] In the laminate film of this embodiment, the product of the 60° surface gloss in accordance with JIS Z8741 and the root-mean-square slope RΔq in accordance with JIS B0601-2001 of the film surface (the surface opposite the support layer of the matte layer) (60° surface gloss × RΔq) is preferably 2.60 or less, and more preferably 2.42 or less. If the product of the 60° surface gloss and the root mean square slope RΔq is equal to or less than the preferred upper limit, the gloss is sufficiently low while maintaining the fineness of the surface, so that a sense of depth and luxury can be achieved.
[0126] There is no particular limitation on the method for laminating the matte layer on the support layer, but it may be produced by laminating a single layer of acrylic matte resin film and a transparent acrylic resin film (transparent acrylic resin layer), or it may be produced by co-extrusion molding of an acrylic resin composition having matte properties and a composition for forming a transparent acrylic resin layer. Among these, the co-extrusion molding method is preferred.
[0127] <Molded product (P1)> The molded article (P1) of this embodiment is a molded article including a substrate and a film covering at least a part of the surface of the substrate. The film covering at least a part of the surface is the film according to the above embodiment.
[0128] The substrate is preferably made of a material that can be melt-bonded to the film of the above embodiment, such as ABS resin, AS resin, styrene resin, polycarbonate resin, vinyl chloride resin, acrylic resin, polyester resin, or a resin that contains these as a main component.
[0129] Among these, ABS resin, AS resin, polycarbonate resin, vinyl chloride resin, or resins containing these resins as main components are preferred because of their excellent adhesiveness, and it is more preferred to use ABS resin, polycarbonate resin, or resins containing these resins as main components. When the film is bonded to the substrate with an adhesive, polyolefins such as polypropylene and polyethylene, and celluloses such as wood and paper can also be used.
[0130] The molded product (P1) is preferably produced by subjecting a film to vacuum molding or pressure molding in an injection mold and then injection molding a resin substrate, or by hot pressing the film onto a substrate resin sheet. When a substrate to which the film cannot be melt-bonded is used, the film is bonded to the surface of the substrate using an adhesive. The film is adhered with the back surface (the surface in contact with the metal roll) facing the substrate.
[0131] <Molded product (P2)> The molded article (P2) of this embodiment is a molded article including a substrate and a laminate film covering at least a part of the surface of the substrate. The laminate film covering at least a part of the surface is the laminate film according to the above embodiment. The substrate may be the same as that of the molded article (P1). The molded article (P2) may be produced in the same manner as the molded article (P1), except that a laminated film is used instead of the film. The laminated film is adhered with the support side facing the substrate. EXAMPLES
[0132] The present invention will be further described below with reference to examples and comparative examples. In the following description, "parts" and "%" related to the ratios mean "parts by mass" and "% by mass", respectively, and the abbreviations / abbreviations mean the names of the compounds listed in Table 1. First, the evaluation method, the production examples of the rubber-containing polymer (A), and the reactive non-crosslinked polymer (B) will be described.
[0133] [Table 1]
[0134] <Evaluation method> [Mass average particle size of rubber-containing polymer (A)] The mass average particle diameter of the rubber-containing polymer (A) was measured by dynamic light scattering using a light scattering photometer DLS-700 (trade name) manufactured by Otsuka Electronics Co., Ltd.
[0135] [Gel content of acrylic rubber-containing polymer (A)] The acetone solution in which 0.5 g of the rubber-containing polymer (A) was dissolved in 50 mL of acetone as the pre-extraction mass M was refluxed at 65° C. for 4 hours. The obtained extract was centrifuged at 14,000 rpm for 30 minutes at 4° C. using a high-speed cooling centrifuge (manufactured by Hitachi Koki Co., Ltd., product name: CR21G). The solution was removed by decantation to obtain the remaining solid. The reflux, centrifugation, and decantation were repeated again for this solid, and the obtained solid was dried at 50° C. for 24 hours, and the mass of the acetone insoluble matter obtained was measured as the post-extraction mass m. The gel content G (%) of the rubber-containing polymer (A) was calculated from the pre-extraction mass M and the post-extraction mass m according to the following formula (1). Gel content G (%) = (mass after extraction m (g) / mass before extraction M (g)) x 100 ...Equation (1)
[0136] [Mass average molecular weight (Mw) of acrylic rubber-containing polymer (A) and reactive non-crosslinked polymer (B)] The mass average molecular weight (Mw) of the acrylic rubber-containing polymer (A) and the reactive non-crosslinked polymer (B) was measured in terms of polystyrene using a high-speed GPC device HLC-8420GPC (manufactured by Tosoh Corporation) equipped with a GPC column consisting of a TSKgel (registered trademark) SuperMultiporeHZ-N, a TSKgel guardcolumn SuperMP(HZ)-H, and a TSKgel Super H-RC connected together, in a solvent of THF.
[0137] [Tg of acrylic rubber-containing polymer (A) and reactive non-crosslinked polymer (B)] Tg was calculated from the Tg value of the homopolymer of each monomer component (given in Polymer Handbook, J. Brandrup, Interscience, 1989) according to the FOX formula.
[0138] [Intrinsic viscosity of reactive non-crosslinked polymer (B)] The intrinsic viscosity of the reactive non-crosslinked polymer (B) was measured in a chloroform solvent at 25° C. using an AVL-2C automatic viscometer manufactured by San Denshi Kogyo Co., Ltd.
[0139] [Melt flow rate (M1)] Using a melt indexer (Tateyama Scientific Co., Ltd., model: L227-42 (L220 type)), the melt flow rate (M1) was measured for a heating time of 4 minutes at a temperature of 240°C and a load of 49 N according to JIS K7210 (Method A) for a sample weight of 4 g. The sample cutting time interval was set to 30 to 120 seconds depending on the melt flow rate (M1) of the sample, and the discharge amount per unit time was measured, and the melt flow rate (M1) in units of g / 10 min was calculated.
[0140] [Melt flow rate (M2)] Using a melt indexer (Tateyama Scientific Co., Ltd., model: L227-42 (L220 type)), the melt flow rate (M2) was measured for a heating time of 120 minutes, measured with a sample amount of 4 g at a temperature of 240°C and a load of 49 N, according to JIS K7210 (Method A). The sample cutting time interval was set to 30 to 120 seconds depending on the melt flow rate (M2) of the sample, and the discharge amount per unit time was measured, and the melt flow rate (M2) in units of g / 10 min was calculated.
[0141] [MFR retention rate (M2 / M1)] The MFR retention rate (M2 / M1) was calculated as the ratio of the melt flow rate (M2) measured at 240°C for 20 minutes and then in accordance with JIS K7210 under conditions of 240°C and a load of 49 N to the melt flow rate (M1) measured at 240°C for 4 minutes and then in accordance with JIS K7210 under conditions of 240°C and a load of 49 N.
[0142] [Film transparency (total light transmittance, overall haze)] Using a haze meter (manufactured by Nippon Denshoku Industries Co., Ltd., trade name: Haze Meter NDH4000), the total light transmittance was measured according to JIS K7361-1 under conditions of a light source of D65 and a temperature of 25° C., and the overall haze was measured according to JIS K7136. The total light transmittance and overall haze of the laminate film are the total light transmittance and overall haze of the entire laminate film including the support layer.
[0143] [Film thickness] Using a film thickness gauge (manufactured by Mitutoyo Corporation, product name: ABS Digimatic Indicator), measurements were taken at five points in the film width direction (TD), and the film thickness was measured by calculating the average value. The thickness of each layer of the laminate film was determined by observing the cross section of the laminate film cut along the transverse direction (TD) using a microtome (manufactured by Leica Microsystems, product name: EM-UC7). Specifically, the cross section of the laminate film was observed using an optical microscope (manufactured by Hirox Japan, product name: KH-8700), and the obtained image was manually measured on the image analysis screen of the KH-8700.
[0144] [60° surface gloss] Using a glossmeter (Konica Minolta, Inc., product name: GM-268Plus), the film surface (the matte surface of a single-layer film, the matte layer surface of a laminated film; the same applies below) was measured at five points in each of the machine direction (MD) and the width direction (TD) in accordance with JIS Z8741, and the 60° surface gloss was measured by calculating the average value. The average value of the 60° surface gloss in the MD and TD was also calculated.
[0145] [85° surface gloss] Using a glossmeter (Konica Minolta, Inc., product name: GM-268Plus), the film surface was measured at five points in each of the longitudinal direction (MD) and transverse direction (TD) in accordance with JIS Z8741, and the 85° surface gloss was measured by calculating the average value. The average value of the 85° surface gloss in the MD and TD was also calculated.
[0267] [Root mean square slope of profile curve (RΔq)] The root mean square slope (RΔq) of the film surface was measured using a surface roughness measuring instrument (manufactured by Tokyo Seimitsu Co., Ltd., product name: SURFCOM (registered trademark) 1400D) in accordance with JIS B0601-2001 under the conditions of a measurement length of 4.0 mm, an evaluation length of 4.0 mm, a cutoff wavelength of 0.8 mm, and a measurement speed of 0.3 mm / s.
[0146] The root mean square slope (RΔq) of a profile represents the root mean square of the local slope dZ / dX in the sampling length, and is calculated by the following formula (2). The local slope here is the derivative of the height Z(x).
[0147]
number
[0148] [60° surface glossiness × RΔq] The 60° surface gloss of the film surface and the root mean square slope of the profile curve (RΔq) were measured using the method described above, and the average values in MD and TD were calculated. The product of the average value of the 60° surface gloss and the average value of the root mean square slope of the profile curve (RΔq) was defined as "60° surface gloss x RΔq".
[0149] [Detailed appearance] The film surface was visually observed and evaluated according to the following criteria. ◯: When visually observed from an angle of 60° from the perpendicular to the film surface, the surface irregularities are fine, uniform, and appear smooth. ×: When visually observed from an angle of 60° from the perpendicular to the film surface, the surface appears to have rough irregularities and a grainy feel.
[0150] [Film shine] The film surface was visually observed and evaluated according to the following criteria. ◯: When visually observed from angles of 60° and 85° from the perpendicular to the film surface, both showed a good low gloss feeling and no reflections of objects, fluorescent lights, etc. ×: When visually observed from angles of 60° and 85° from the perpendicular to the film surface, objects, fluorescent lights, etc. are reflected on at least one side, and their outlines are recognizable.
[0151] <Rubber-containing polymer (A)> [Production Example 1: Production of Rubber-Containing Polymer (A1)] After 10.8 parts of deionized water was charged into a vessel equipped with a stirrer, monomer components (a) consisting of 0.3 parts of MMA, 4.5 parts of n-BA, 0.2 parts of BDMA, 0.05 parts of AMA, and 0.025 parts of CHP were added and mixed by stirring at room temperature. Next, 1.3 parts of RS610 was added to the vessel while stirring, and the stirring was continued for 20 minutes to prepare "emulsion 1".
[0152] Next, 156.0 parts of deionized water was added to a polymerization vessel equipped with a reflux condenser, and the temperature was raised to 74°C. Furthermore, a mixture was prepared by adding 0.20 parts of sodium formaldehyde sulfoxylate, 0.0001 parts of ferrous sulfate, and 0.0003 parts of EDTA to 4.5 parts of deionized water, and this mixture was added to the polymerization vessel. Next, while stirring under a nitrogen atmosphere, the emulsion 1 was dropped into the polymerization vessel over 9 minutes, and the reaction was continued for 15 minutes to complete the polymerization of the first elastic polymer (Ia).
[0153] Then, the monomer component (b) consisting of 9.6 parts of MMA, 14.4 parts of n-BA, 1 part of BDMA, 0.25 parts of AMA and 0.016 parts of CHP was dropped into the polymerization vessel over 90 minutes, and the reaction was continued for 60 minutes to produce the second elastic polymer (Ib). In this way, the elastic polymer (I) containing the first elastic polymer (Ia) and the second elastic polymer (Ib) was obtained. In addition, when the monomer component (a) and the monomer component (b) were polymerized alone under the same conditions as above, the Tg of the first elastomeric polymer (Ia) was -48°C, and the Tg of the second elastomeric polymer (Ib) was -10°C.
[0154] Next, monomer component (c) consisting of 6 parts of MMA, 4 parts of MA, 0.075 parts of AMA, and 0.013 parts of CHP was dropped into the polymerization vessel over 45 minutes, and the reaction was continued for 60 minutes to form graft chains of intermediate polymer (II). When monomer component (c) was polymerized alone under the same conditions as above, the Tg of intermediate polymer (II) was 60°C.
[0155] Then, the monomer component (d) consisting of 57 parts of MMA, 3 parts of MA, 0.075 parts of t-BHP and 0.264 parts of n-OM was dropped into the polymerization vessel over 140 minutes, and the reaction was continued for 60 minutes to form a graft chain of the hard polymer (III), thereby obtaining a polymer latex of the rubber-containing polymer (A1). The average particle size of the obtained latex-like rubber-containing polymer (A1) was 0.11 μm. When the monomer component (d) was polymerized alone under the same conditions as above, the Tg of the hard polymer (III) was 99 ° C.
[0156] The obtained polymer latex of the rubber-containing polymer (A1) was filtered using a vibration filter equipped with a SUS mesh (average mesh size: 54 μm) as a filter medium, and then salted out in an aqueous solution containing 3.5 parts of calcium acetate, washed with water, recovered, and then dried to obtain a powdered rubber-containing polymer (A1). Table 2 shows a list of each monomer component. The gel content of the rubber-containing polymer (A1) was 70%, and Mw was 58,000.
[0157] [Production Example 2: Production of rubber-containing polymer (A2)] Each monomer component was changed as shown in Table 2, and a rubber-containing polymer (A2) was produced by the following method in which grafting was carried out in one step. Into a polymerization vessel equipped with a reflux condenser, 186.3 parts of deionized water was charged, and the temperature was raised to 79° C. Furthermore, a mixture was prepared by adding 0.25 parts of sodium formaldehyde sulfoxylate, 0.000025 parts of ferrous sulfate, and 0.000075 parts of EDTA to 3.4 parts of deionized water, and this mixture was charged into the polymerization vessel.
[0158] Next, while stirring under a nitrogen atmosphere, 1 / 10 of a mixture of monomer component (a) consisting of 11.25 parts of MMA, 12.5 parts of n-BA, 1.25 parts of St, 0.75 parts of BDMA, 0.09 parts of AMA and 0.044 parts of CHP and 0.75 parts of RS610 was dropped into the polymerization vessel over 4 minutes, and the reaction was continued for 15 minutes. Thereafter, the remaining 9 / 10 of the mixture was dropped into the polymerization vessel over 108 minutes, and then 0.125 parts of sodium formaldehyde sulfoxylate was added at the 40-minute reaction time point, and the reaction was continued for 55 minutes to complete the polymerization of the first elastic polymer (Ia).
[0159] Then, the monomer component (b) consisting of n-BA30.94 parts, St6.56 parts, BDMA0.09 parts, AMA0.66 parts and CHP0.106 parts was dropped into the polymerization vessel over 180 minutes, and then 0.125 parts of sodium formaldehyde sulfoxylate was added at the reaction time of 105 minutes, and the reaction was continued for 120 minutes to produce a second elastic polymer (Ib). In this way, an elastic polymer (I) containing a first elastic polymer (Ia) and a second elastic polymer (Ib) was obtained.
[0160] Then, monomer component (d) consisting of 35.63 parts of MMA, 1.88 parts of MA, 0.064 parts of t-BHP and 0.113 parts of n-OM was dropped into the polymerization vessel over 120 minutes to form graft chains of hard polymer (III), thereby obtaining polymer latex of rubber-containing polymer (A2). The average particle size of the obtained latex-like rubber-containing polymer (A2) was 0.26 μm.
[0161] The obtained polymer latex of the rubber-containing polymer (A2) was filtered using a vibration filter equipped with a SUS mesh (average mesh size: 54 μm) as a filter medium, and then salted out in an aqueous solution containing 5.0 parts of calcium acetate, washed with water, recovered, and then dried to obtain a powdered rubber-containing polymer (A2). Table 2 shows a list of each monomer component. The gel content of the rubber-containing polymer (A2) was 90%, and Mw was 45,000.
[0162] [Table 2]
[0163] <Reactive non-crosslinked polymer (B)> [Production Example 3: Production of Hydroxy Group-Containing Polymer] Into a polymerization vessel equipped with a reflux condenser, 262 parts of deionized water, 13.8 parts of 10% calcium phosphate slurry, 60.0 parts of MMA, 10.0 parts of MA, 30.0 parts of 2-hydroxyethyl methacrylate, 0.25 parts of n-dodecyl mercaptan, and 0.52 parts of lauroyl peroxide were charged as monomer components, and the atmosphere in the polymerization vessel was thoroughly replaced with nitrogen gas. Next, the monomer components were heated to 78°C while being stirred, and reacted for 2 hours under a nitrogen atmosphere. Next, the liquid temperature in the polymerization vessel was raised to 85°C, 0.022 parts of potassium persulfate was added, and the mixture was maintained for another 90 minutes to obtain polymer beads. The obtained polymer beads were sieved under a condition of 150 mesh (opening 100μm), and the beads that passed through the mesh were dehydrated and dried to obtain hydroxyl group-containing polymer beads. The obtained hydroxyl group-containing polymer had a Tg of 77°C, an intrinsic viscosity of 0.069L / g, an average particle size of 90μm, and a mass average molecular weight of 158,300.
[0164] <Crosslinked particles (C)> As the crosslinked particles (C), the following commercially available crosslinked particles (manufactured by Nippon Shokubai Co., Ltd., product names: Eposter (registered trademark) MV1002, Eposter MV1004, Eposter MV1006, Eposter MV1010) were used. Note that the following average particle sizes are all catalog values, and the average particle sizes are volume-based average particle sizes measured by the Coulter method.
[0165] Eposter MV1002: Volume-based average particle size 2.5 μm (99-100% polymethyl methacrylate crosslinked). Eposter MV1004: Volume-based average particle size 3.6 μm (99-100% polymethyl methacrylate crosslinked). Eposter MV1006: Volume-based average particle size 6.3 μm (99-100% polymethyl methacrylate crosslinked). Eposter MV1010: Volume-based average particle size 10.2 μm (99-100% polymethyl methacrylate crosslinked).
[0166] <Transparent acrylic resin> [Production Example 4: Production of transparent acrylic resin composition] 80 parts of the rubber-containing polymer (A1) obtained in Production Example 1, 10 parts of the rubber-containing polymer (A2) obtained in Production Example 2, 10 parts of an alkyl methacrylate-alkyl acrylate copolymer (manufactured by Mitsubishi Chemical Corporation; trade name: Dianale (registered trademark) BR-75) as a non-reactive non-crosslinked polymer (D), 1.1 parts of a benzotriazole-based ultraviolet absorber (manufactured by ADEKA Corporation; trade name: Adeka STAB (registered trademark) LA-31RG) as an additive, 0.2 parts of a hindered amine-based light stabilizer (manufactured by BASF Japan Ltd.; trade name: Chimassorb (registered trademark) 2020 FDL), 1 part of a hindered phenol-based antioxidant (manufactured by ADEKA Corporation; trade name: Adeka STAB AO-60), and 0.4 parts of a phosphorus-based antioxidant (manufactured by Johoku Chemical Industry Co., Ltd.; trade name: JP-333E) were added, and then mixed using a Henschel mixer. Thereafter, using a twin-screw extruder (manufactured by Toshiba Machine Co., Ltd., product name: TEM-35B, the same applies below) at a cylinder temperature of 180 to 240°C and a die head temperature of 240°C, the mixture was extruded into strands while removing impurities with a screen mesh (manufactured by Nippon Seisen Co., Ltd., product name: NF-12T, nominal filtration diameter 40 μm), and then cooled through a water tank and cut to obtain pellets of the transparent acrylic resin composition.
[0167] <Example 1> Pellets of a resin composition having matte properties were prepared with the formulation shown in Table 3. Specifically, 75 parts of the rubber-containing polymer (A1) obtained in Production Example 1 was used as the acrylic rubber-containing polymer (A), 11 parts of an alkyl methacrylate-alkyl acrylate copolymer (manufactured by Mitsubishi Chemical Corporation; product name: ACRYPET (registered trademark) VH (MMA / MA=97 / 3)) was used as the non-reactive non-crosslinked polymer (D), 14 parts of the hydroxyl group-containing polymer obtained in Production Example 3 was used as the reactive non-crosslinked polymer (B), 3 parts of acrylic fine particles (manufactured by Nippon Shokubai Co., Ltd.; product name: Eposter MV1002) were used as the crosslinked particles (C), and 10 parts of acrylic The composition contained 0.8 parts of a polymer external lubricant (manufactured by Mitsubishi Chemical Corporation; product name: Metablen (registered trademark) L-1000), 3 parts of a high molecular weight acrylic polymer (manufactured by Mitsubishi Chemical Corporation; product name: Metablen P-551A), and additives such as 1 part of a phosphorus-based antioxidant (manufactured by Johoku Chemical Industry Co., Ltd.; product name: JP-333E), 1.1 parts of a benzotriazole-based ultraviolet absorber (manufactured by ADEKA Corporation; product name: Adekastab LA-31RG), and 1.2 parts of a hindered amine-based light stabilizer (manufactured by BASF Japan Ltd.; product name: Chimassorb 0.3 parts of 2020 FDL), 0.7 parts of a hindered phenol-based antioxidant (manufactured by ADEKA CORPORATION; product name: Adeka STAB AO-60), and 2.5 parts of 9,9-bis[4-(2-hydroxyethoxy)-phenyl]fluorene (bisphenoxyethanol fluorene, BPEF (manufactured by Osaka Gas Chemicals Co., Ltd.; product name: OGSOL (registered trademark) MF-11) were mixed.
[0168] Thereafter, using a twin-screw extruder (Toshiba Machine Co., Ltd., product name: TEM-35B), the mixture was extruded into strands while removing impurities through a 200-mesh screen mesh under conditions of a cylinder temperature of 170 to 240 ° C and a die head temperature of 240 ° C, and then cut and pelletized after cooling through a water bath. The die outlet resin temperature was 294 ° C at a screw rotation speed of 300 rpm and a discharge rate of 20.0 kg / h. The melt flow rate (M1) of the obtained pellets was 1.44 g / 10 min, the melt flow rate (M2) was 1.22 g / 10 min, and the MFR retention rate (M2 / M1) was 86%. The evaluation results are shown in Table 3.
[0169] The pellets were used to prepare a monolayer film. Specifically, the pellets were dehumidified and dried at 85°C for one day and night, and a monolayer film having a thickness of 40 μm was formed using a 40 mmφ non-vent screw extruder (L / D=33) equipped with a 200 mesh screen mesh and a 500 mm wide T-die at a cylinder temperature of 200 to 240°C and a T-die temperature of 245°C.
[0170] The 60° surface gloss of the obtained monolayer film was 7.2% in MD and 7.7% in TD, the 85° surface gloss was 20.6% in MD and 20.1% in TD, and the root mean square slope of the profile curve (RΔq) was 0.152 in MD and 0.176 in TD. The evaluation results are shown in Table 3.
[0171] <Examples 2 to 12 and Comparative Examples 1 to 3> The same procedure as in Example 1 was carried out, except that the resin composition pellets were prepared in the formulations shown in Tables 3 to 5. The evaluation results of the obtained pellets and single layer film are shown in Tables 3 to 5. Incidentally, the pellets of the resin composition of Comparative Example 3 had a low MFR retention (M2 / M1) of 59% and was poor in thermal stability, so that a film was not produced.
[0172] <Example 13> The pellets obtained in Example 1 were used as the resin composition constituting the matte layer, and the pellets obtained in Production Example 4 were used as the resin composition constituting the support layer. These pellets were dehumidified and dried at 85 ° C. for one day. The resin composition constituting the matte layer was plasticized at a cylinder temperature of 200 to 240 ° C. using a 30 mm φ non-vent screw extruder equipped with a 200 mesh screen mesh, while the resin composition constituting the support layer was plasticized at a cylinder temperature of 220 to 240 ° C. using a 40 mm φ non-vent screw extruder equipped with a 200 mesh screen mesh, and then a 500 mm wide two-kind two-layer multi-manifold T die set at 245 ° C. was used to make a 75 μm thick laminated film so that the resin composition constituting the support layer was in contact with a mirror-cooled roll.
[0173] When the cross section of the laminated film was observed, the thickness of the matte layer was 7.5 μm, and the thickness of the support layer was 67.5 μm. In addition, the 60° surface gloss of the surface of the matte layer (the side on which the support layer was not laminated) was 12.6% in MD and 13.7% in TD, the 85° surface gloss was 20.5% in MD and 20.5% in TD, and the root mean square slope (RΔq) of the profile curve was 0.180 in MD and 0.177 in TD. The evaluation results of the obtained pellets and laminated film are shown in Table 5.
[0174] <Examples 14 to 19 and Comparative Examples 4 to 7> Pellets were prepared in the same manner as in Example 13, except that the pellets constituting the matte layer were made of the resin compositions shown in Tables 6 to 8, and laminate films were prepared in the same manner as in Example 9. Tables 6 to 8 show the evaluation results of the obtained pellets constituting the matte layer and the laminate film.
[0175] [Table 3]
[0176] [Table 4]
[0177] [Table 5]
[0178] [Table 6]
[0179] [Table 7]
[0180] [Table 8]
[0181] From the above examples and comparative examples, the following became clear. It was shown that the monolayer films and laminate films (Examples 1 to 19) using the resin composition of the present invention, by using the reactive non-crosslinked polymer (B) and the crosslinked particles (C) in combination, can effectively reduce the 60° surface gloss and 85° surface gloss, and suppress shine, compared to the monolayer films and laminate films (Comparative Examples 1 to 7) of the comparative examples. Furthermore, the 60° surface gloss×RΔq was 2.6 or less, and a film having a fine appearance was obtained. The acrylic matte resin films of Examples 1 to 19 had a fine appearance without shine, and had good design and decorative properties such as a luxurious feel and a deep feeling of the matte appearance.
[0182] When comparing the monolayer film of Comparative Example 1 with the monolayer film (Examples 1 to 12) having the same composition except for the presence or absence of the reactive non-crosslinked polymer (B), the monolayer film of Comparative Example 1 had a rough texture and an insufficient matting effect, so that the 60° surface gloss did not decrease and the appearance was shiny. Furthermore, in Comparative Example 1, in order to achieve a 60° surface gloss value equivalent to that of the Examples, it would have been necessary to add a larger amount of crosslinked particles (C), which was uneconomical.
[0183] When comparing the laminate films (Examples 13 to 19) having the same composition and layer structure except for the presence or absence of the reactive non-crosslinked polymer (B) with the laminate films of Comparative Examples 5 to 7, the texture of Comparative Examples 5 to 7 was rough and the matte effect was insufficient, so that the 60° surface gloss did not decrease and the appearance was shiny.
[0184] In addition, when comparing the single-layer films of Examples 1 to 12 and Comparative Example 2, which have the same composition except for the presence or absence of crosslinked particles (C), the matte effect in Comparative Example 2 was insufficient, so the 85° surface gloss did not decrease and the film had a shiny appearance. In addition, when comparing the laminate films of Examples 13 to 119 and Comparative Example 4, which have the same composition and layer structure except for the presence or absence of crosslinked particles (C), the matte effect in Comparative Example 4 was insufficient, so the 85° surface gloss did not decrease and the film had a shiny appearance. [Industrial Applicability]
[0185] The resin composition of the present invention can reduce both the 60° surface gloss and 85° surface gloss, which are the causes of shine, and can provide an acrylic matte resin film that has a fine-grained matte appearance and can be used for a variety of purposes.
[0186] The films, laminated films, and molded articles produced from the resin composition of the present invention are particularly suitable for vehicle applications and building material applications. Specific examples include automotive interior applications such as instrument panels, console boxes, meter covers, door lock bezels, steering wheels, power window switch bases, center clusters, and dashboards, automotive exterior applications such as weather strips, bumpers, bumper guards, side mudguards, body panels, spoilers, front grilles, strut mounts, wheel caps, center pillars, door mirrors, center ornaments, side moldings, door moldings, window moldings, windows, headlamp covers, taillamp covers, and windshield parts, and AV equipment and furniture product applications. the like; as surface decorative materials for furniture; as building interior materials for walls, ceilings, floors, etc.; as building exterior materials for exterior walls such as siding, fences, roofs, gates, gable boards, etc.; as surface decorative materials for furniture such as window frames, doors, handrails, thresholds, lintels, etc.; as optical components such as various displays, lenses, mirrors, goggles, window glass, etc.; as interior and exterior decoration materials for various types of vehicles other than automobiles, such as trains, airplanes, ships, etc.; as various packaging containers and materials such as bottles, cosmetic containers, accessory cases, etc.; and as miscellaneous goods for prizes, accessories, etc.
Claims
1. The composition comprises a rubber-containing polymer (A), a reactive non-crosslinked polymer (B), crosslinked particles (C), and optionally a non-reactive non-crosslinked polymer (D), A resin composition, wherein the mass ratio [(B) / (B+C)] of the reactive non-crosslinked polymer (B) to the total mass of the reactive non-crosslinked polymer (B) and the crosslinked particles (C) is 25 to 95 mass%.
2. The resin composition according to claim 1, wherein the crosslinked particles (C) have a volume-based average particle size measured by the Coulter method of 0.5 to 20 μm.
3. The resin composition according to claim 1, wherein the mass ratio [(C) / (A+B+D)] of the crosslinked particles (C) to the total mass of the rubber-containing polymer (A), the reactive non-crosslinked polymer (B), and the non-reactive non-crosslinked polymer (D) is 0.5 to 20 mass%.
4. The resin composition according to claim 1, wherein the mass ratio of the reactive non-crosslinked polymer (B) to the total mass of the rubber-containing polymer (A), the reactive non-crosslinked polymer (B), and the non-reactive non-crosslinked polymer (D) [(B) / (A+B+D)] is 0.9 to 40 mass%.
5. The reactive non-crosslinked polymer (B) contains a carboxy group, a hydroxy group, an acid anhydride group, an epoxy group, an isocyanate group, an amide group, an amino group, a cyano group, and an isocyanate group. The resin composition according to claim 1, further comprising one or more reactive groups selected from the group consisting of amine groups.
6. The resin composition according to claim 1, wherein the MFR retention (M2 / M1), which is the ratio of the melt flow rate (M2) measured in accordance with JIS K7210 after heating at 240°C for 120 minutes under conditions of a temperature of 240°C and a load of 49 N to the melt flow rate (M1) measured in accordance with JIS K7210 after heating at 240°C for 4 minutes under conditions of a temperature of 240°C and a load of 49 N, is 60 to 115%.
7. A film using the resin composition according to any one of claims 1 to 6.
8. 8. The film according to claim 7, wherein the 60° surface gloss of the film surface is 15% or less and the 85° surface gloss is 24% or less, according to JIS Z8741.
9. The film according to claim 7, wherein the product of the 60° surface gloss of the film surface according to JIS Z8741 and the root mean square slope RΔq according to JIS B0601-2001 (60° surface gloss × RΔq) is 2.60 or less.
10. A film, the 60° surface gloss of the film surface according to JIS Z8741 being 15% or less, the 85° surface gloss being 24% or less, and the product of the 60° surface gloss of the film surface according to JIS Z8741 and the root mean square slope RΔq of the film surface according to JIS B0601-2001 (60° surface gloss × RΔq) being 2.60 or less.
11. A laminated film comprising a matte layer formed by using the resin composition according to any one of claims 1 to 6 on a support layer.
12. A molded article comprising a substrate and the film according to claim 7 covering at least a portion of a surface of the substrate.
13. A molded article comprising a substrate and the laminate film of claim 11 covering at least a portion of the surface of the substrate.
Citation Information
Patent Citations
Matte acrylic film and matte molding laminated with acrylic film
JP1998237261A