Freeze-thaw hydrogel of polyvinyl alcohol and producing method thereof
By adjusting the onset temperature and water content in the freeze-thaw process, and using melt-kneaded PVOH, the hydrogel achieves low elution and high transparency, addressing drug delivery and visibility challenges in contact lenses.
Patent Information
- Application Number
- JP2024008807
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2023-03-28
- Filing Date
- 2024-01-24
- Publication Date
- 2024-10-11
AI Technical Summary
Conventional polyvinyl alcohol hydrogels used in contact lenses face issues with drug elution and reduced transparency due to the freeze-thaw process, making them unsuitable for sustained drug release applications.
The method involves setting the onset temperature of the absorption peak in differential scanning calorimetry to -5°C or lower and reducing the hydrogel's water content to 75% or less through multiple freeze-thaw treatments, along with melt-kneading PVOH in the presence of water to form a hydrogel with dense and uniform PVOH crystals, enhancing transparency and reducing elution.
The resulting hydrogel exhibits low drug elution and high transparency, suitable for contact lenses, ensuring effective drug delivery and clear visibility without issues.
Smart Images

Figure 2024144112000003 
Figure 2024144112000001 
Figure 2024144112000002
Abstract
Description
[Technical field]
[0001] The present invention relates to a freeze-thaw hydrogel of polyvinyl alcohol and a method for producing the same. [Background technology]
[0002] Contact lenses that have the ability to sustain the release of therapeutic drugs have been investigated so that the drugs can be delivered to the affected area of the eye over a long period of time by wearing the contact lenses containing the therapeutic drugs (Patent Document 1).
[0003] Chemically crosslinked hydrogels are used in contact lenses. When drugs are to be incorporated into such contact lenses, the hydrogels formed into the contact lenses after crosslinking must be impregnated with the drugs. However, there is a problem in that it is difficult to impregnate hydrogels having sustained release properties with drugs.
[0004] On the other hand, by repeatedly freezing and thawing an aqueous solution of polyvinyl alcohol, the polyvinyl alcohol can be physically crosslinked to form a hydrogel (Patent Document 2). [Prior art documents] [Patent documents]
[0005] [Patent Document 1] Special Publication No. 2008-539837 [Patent Document 2] Japanese Patent Application Publication No. 8-239538 Summary of the Invention [Problem to be solved by the invention]
[0006] Polyvinyl alcohol hydrogels made by the conventional freeze-thaw method have problems such as the polyvinyl alcohol dissolving in water heated to near body temperature, and the hydrogel becoming cloudy after freeze-thaw processing, making it difficult to make a highly transparent hydrogel, making them unsuitable for use as contact lenses.
[0007] An object of the present invention is to provide a hydrogel which is little eluted and highly transparent, and a production method which can obtain a hydrogel which is little eluted and highly transparent. [Means for solving the problem]
[0008] As a result of intensive research, the present inventors have found that a freeze-thaw hydrogel of polyvinyl alcohol with little elution and excellent transparency can be obtained by setting the onset temperature of the low-temperature side of the absorption peak of the melting point of water in the gel measured in differential scanning calorimetry at a temperature rise rate of 10° C. / min to −5° C. or less. In addition, the present inventors have found that a polyvinyl alcohol freeze-thaw hydrogel with little elution and excellent transparency can be obtained by subjecting an aqueous solution of polyvinyl alcohol to a first freeze-thaw treatment to make a hydrogel, setting the water content of the hydrogel to 75 mass% or less, and then performing a second freeze-thaw treatment, or by melt-kneading polyvinyl alcohol in the presence of water to make a polyvinyl alcohol composition containing water, and then performing a freeze-thaw treatment.
[0009] The present invention has the following aspects. [1] A freeze-thaw hydrogel of polyvinyl alcohol, A freeze-thawed hydrogel in which the onset temperature of the low-temperature side of the absorption peak observed in the range below 0°C is -5°C or lower when measured in differential scanning calorimetry under conditions of -50°C to 150°C and a heating rate of 10°C / min. [2] The freeze-thaw hydrogel described in [1], wherein the polyvinyl alcohol is a denatured polyvinyl alcohol. [3] The freeze-thaw hydrogel according to [2], wherein the polyvinyl alcohol is a modified polyvinyl alcohol having a cationic group or an anionic group. [4] The freeze-thaw hydrogel according to any one of [1] to [3], which is for use in contact lenses. [5] The freeze-thawed hydrogel according to any one of [1] to [4], which contains a drug. [6] A method for producing a freeze-thaw hydrogel of polyvinyl alcohol, comprising the steps of: A method for producing a freeze-thaw hydrogel, comprising the steps of: subjecting an aqueous polyvinyl alcohol solution to a first freeze-thaw process to prepare a hydrogel; adjusting the water content of the hydrogel to 75% by mass or less; and then subjecting the hydrogel to a second freeze-thaw process. [7] A method for producing a freeze-thaw hydrogel of polyvinyl alcohol, comprising the steps of: A method for producing a freeze-thaw hydrogel comprising melt-kneading polyvinyl alcohol in the presence of water to obtain a water-containing polyvinyl alcohol composition, and then subjecting the composition to a freeze-thaw treatment. [8] The method for producing a freeze-thaw hydrogel according to [7], wherein the water content of the polyvinyl alcohol composition is 70 mass% or less. Effect of the Invention
[0010] According to the present invention, there can be provided a hydrogel which is little eluted and has excellent transparency, and a production method by which a hydrogel which is little eluted and has excellent transparency can be obtained. [Brief description of the drawings]
[0011] [Figure 1] 1 is a graph showing the endothermic peak of water obtained by differential scanning calorimetry of the PVOH freeze-thaw hydrogel of Example 1. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0012] In this specification, the term "hydrogel" refers to a structure having a network structure formed by physically or chemically crosslinking polymer molecular chains, which swells by absorbing water into the network structure. "Polyvinyl alcohol freeze-thaw hydrogel" is a hydrogel formed by repeatedly freezing and thawing (defrosting) polyvinyl alcohol (hereinafter also referred to as "PVOH") in the presence of water. When PVOH is repeatedly frozen and thawed in the presence of water, physical crosslinks are formed between the molecular chains of PVOH through hydrogen bonds, resulting in a hydrogel. The symbol "~" indicating a range of values means that the values before and after it are included as the lower and upper limits.
[0013] [PVOH freeze-thaw hydrogel] The PVOH freeze-thaw hydrogel of the present invention (hereinafter also simply referred to as "freeze-thaw hydrogel") contains PVOH. PVOH is a polymer containing vinyl alcohol units, and is typically a saponification product of a polymer containing vinyl ester monomer units. PVOH may contain vinyl ester monomer units. The PVOH may be unmodified or modified. From the viewpoint of sustained release of the drug, modified PVOH is preferred.
[0014] <Unmodified PVOH> Unmodified PVOH is PVOH that does not contain any other monomer units than vinyl alcohol units and vinyl ester monomer units. Unmodified PVOH consists of only vinyl alcohol units, or consists of vinyl alcohol units and vinyl ester monomer units. Unmodified PVOH can usually be produced by polymerizing a vinyl ester monomer and then saponifying the polymer.
[0015] Examples of the vinyl ester monomer include aliphatic vinyl esters such as vinyl formate, vinyl acetate, vinyl propionate, vinyl valerate, vinyl butyrate, vinyl isobutyrate, vinyl pivalate, vinyl caprate, vinyl laurate, vinyl stearate, vinyl versatate, and vinyl trifluoroacetate, and aromatic vinyl esters such as vinyl benzoate. Among these, aliphatic vinyl esters having 3 to 20 carbon atoms, more preferably 4 to 10 carbon atoms, and particularly preferably 4 to 7 carbon atoms, and particularly preferably vinyl acetate, are preferred. These are usually used alone, but multiple types may be used simultaneously as necessary.
[0016] The polymerization of vinyl ester monomers can be carried out by any known polymerization method, such as solution polymerization, suspension polymerization, emulsion polymerization, etc. Among them, solution polymerization, which can efficiently remove reaction heat, is preferably carried out under reflux. As a solvent for solution polymerization, alcohol is usually used, and preferably a lower alcohol having 1 to 3 carbon atoms is used.
[0017] The saponification of the obtained polymer can be carried out by a conventionally known method, that is, by using an alkali catalyst or an acid catalyst in a state where the polymer is dissolved in an alcohol or water / alcohol solvent. As the alkali catalyst, for example, hydroxides or alcoholates of alkali metals such as potassium hydroxide, sodium hydroxide, sodium methylate, sodium ethylate, potassium methylate, and lithium methylate can be used.
[0018] Usually, transesterification using an alkali catalyst in an anhydrous alcohol solvent is preferably used in terms of reaction rate and ability to reduce impurities such as fatty acid salts. The reaction temperature of the saponification reaction is usually 20 to 60°C. If the reaction temperature is too low, the reaction rate tends to be slow and the reaction efficiency tends to decrease, and if the reaction temperature is too high, the reaction temperature may exceed the boiling point of the reaction solvent, and safety in terms of production tends to decrease. When saponification is performed under high pressure using a tower-type continuous saponification tower with high pressure resistance, saponification can be performed at a higher temperature, for example, 80 to 150°C, and it is possible to obtain a high degree of saponification in a short time even with a small amount of saponification catalyst.
[0019] After saponification, the unmodified PVOH is preferably washed with a washing liquid, such as alcohols such as methanol, ethanol, isopropyl alcohol, butanol, etc., and methanol is preferred from the viewpoints of washing efficiency and drying efficiency.
[0020] The washed unmodified PVOH is dried with hot air or the like in a continuous or batch manner. The drying temperature is usually 50 to 150°C. If the drying temperature is too high, the unmodified PVOH tends to deteriorate due to heat, and if the drying temperature is too low, the drying tends to take a long time. The drying time is usually 1 to 48 hours. If the drying time is too long, the unmodified PVOH tends to deteriorate due to heat, and if the drying time is too short, the drying tends to be insufficient or high-temperature drying tends to be required. The content of the solvent contained in the unmodified PVOH after drying is usually 0 to 10% by weight, particularly preferably 0.1 to 5% by weight, and further preferably 0.1 to 1% by weight.
[0021] The average saponification degree of the unmodified PVOH is preferably 95 mol% or more, more preferably 96 mol% or more, even more preferably 97 mol% or more, and may be 100 mol%. When the average saponification degree is equal to or more than the lower limit, gelation tends to be easily performed, and the dissolution rate of the gel tends to be reduced. The average degree of saponification is measured in accordance with JIS K 6726:1994, 3.5. The average saponification degree of PVOH does not change before and after the freeze-thaw hydrogel is formed. The average saponification degree of PVOH can be measured by re-dissolving the freeze-thawed hydrogel.
[0022] The average degree of polymerization of unmodified PVOH can generally be indicated by the viscosity of an aqueous solution. The viscosity of a 4% by mass aqueous solution of unmodified PVOH at 20° C. is preferably 5 to 100 mPa s, more preferably 13 to 70 mPa s, and even more preferably 17 to 40 mPa s. If the viscosity is equal to or greater than the lower limit, gelation tends to be facilitated and the dissolution rate of the gel tends to be reduced, while if the viscosity is equal to or less than the upper limit, the aqueous PVOH solution tends to be easier to handle and the drug release properties tend to be superior. The viscosity is measured in accordance with JIS K 6726:1994, 3.11.2. The average degree of polymerization of PVOH does not change before and after the freeze-thaw hydrogel is formed. The average degree of polymerization of PVOH can be measured by re-dissolving the freeze-thawed hydrogel.
[0023] <Modified PVOH> The modified PVOH typically contains a vinyl alcohol unit and a unit having a modifying group. The unit having a modifying group is a unit other than the vinyl alcohol unit and the vinyl ester monomer unit. The modified PVOH may contain a vinyl ester monomer unit. Modified PVOH can be produced by saponifying a polymer of a vinyl ester monomer and another unsaturated monomer, or by post-modifying PVOH.
[0024] The modified group is preferably at least one selected from the group consisting of cationic groups, anionic groups, and nonionic groups. Examples of the cationic group include diallyldimethylammonium base, (3-methacrylamidopropyl)trimethylammonium base, quaternary ammonium base such as [2-(methacryloyloxy)ethyl]trimethylammonium chloride, sulfonium group, oxonium group, and phosphonium group. Examples of the anionic group include a carboxy group and its salt, a sulfo group and its salt, and a phosphoric acid group and its salt. Examples of the nonionic group include an acetoacetate group, an acetal group, a urethane group, an ether group, a phosphoric acid ester group, an oxyalkylene group, an alkylene group, an amide group, a silanol group, an epoxy group, an olefin group, and a diol group. When an anionic drug is used as the drug, the modifying group is preferably a cationic group, since it has a high affinity with the anionic drug and provides good sustained release of the anionic drug.When a cationic drug is used as the drug, the modifying group is preferably an anionic group, since it has a high affinity with the cationic drug and provides good sustained release of the cationic drug. Modified PVOH having a cationic group is also referred to as cationic modified PVOH, and modified PVOH having an anionic group is also referred to as anionic modified PVOH.
[0025] An example of the modified PVOH is copolymer modified PVOH. The copolymer-modified PVOH can be produced by copolymerizing a vinyl ester monomer with another unsaturated monomer copolymerizable with the vinyl ester monomer, and saponifying the resulting copolymer.
[0026] As the other unsaturated monomer copolymerizable with the vinyl ester monomer, an unsaturated monomer having at least one modifying group selected from the group consisting of a cationic group, an anionic group, and a nonionic group is preferable, and an unsaturated monomer having a cationic group or an anionic group is particularly preferable. Examples of the unsaturated monomer having a cationic group include N-acrylamidomethyltrimethylammonium chloride, allyltrimethylammonium chloride, and diallyltrimethylammonium chloride. Examples of unsaturated monomers having an anionic group include unsaturated carboxylic acids or salts thereof, such as acrylic acid, methacrylic acid, crotonic acid, maleic acid, maleic anhydride, itaconic acid, and undecylenic acid; esters in which a portion of the carboxyl groups of polyvalent carboxylic acids, such as maleic acid, itaconic acid, and fumaric acid, has been esterified (e.g., monoalkyl esters of unsaturated dicarboxylic acids); and olefin sulfonic acids, such as ethylene sulfonic acid, allyl sulfonic acid, and methallyl sulfonic acid, or salts thereof. Examples of unsaturated monomers having a nonionic group include olefins such as ethylene, propylene, isobutylene, α-octene, α-dodecene, and α-octadecene; esters of unsaturated carboxylic acids in which all of the carboxy groups are esterified, such as acrylic acid, methacrylic acid, crotonic acid, maleic acid, maleic anhydride, itaconic acid, and undecylenic acid (dialkyl esters of unsaturated dicarboxylic acids); nitriles such as acrylonitrile and methacrylonitrile; amides such as diacetone acrylamide, acrylamide, and methacrylamide; alkyl vinyl ethers; dimethylallyl vinyl ketone; N-vinylpyrrolidone; vinyl chloride; vinylidene chloride; polyoxyalkylene (meth)allyl ethers such as polyoxyethylene (meth)allyl ether and polyoxypropylene (meth)allyl ether; polyoxyalkylene (meth)acrylates such as polyoxyethylene (meth)acrylate and polyoxypropylene (meth)acrylate; polyoxyethylene (meth)acrylamide, polyoxypropylene (meth)acrylamide, and the like. Examples of the vinyl compounds include polyoxyalkylene (meth)acrylamides such as acrylamide; polyoxyethylene (1-(meth)acrylamide-1,1-dimethylpropyl) esters; polyoxyalkylene vinyl ethers such as polyoxyethylene vinyl ether and polyoxypropylene vinyl ether; polyoxyalkylene allylamines such as polyoxyethylene allylamine and polyoxypropylene allylamine; polyoxyalkylene vinylamines such as polyoxyethylene vinylamine and polyoxypropylene vinylamine; hydroxyl-containing α-olefins such as 3-buten-1-ol, 4-penten-1-ol, and 5-hexen-1-ol, or acylated products thereof, vinyl ethylene carbonate; 2,2-dialkyl-4-vinyl-1,3-dioxolane; glycerin monoallyl ether; vinyl compounds such as 3,4-diacetoxy-1-butene; isopropenyl acetate; substituted vinyl acetates such as 1-methoxyvinyl acetate, 1,4-diacetoxy-2-butene, vinylene carbonate, and vinyl acetoacetate. These unsaturated monomers may be used alone or in combination of two or more. Of the above, diallyldimethylammonium chloride and monomethyl maleate are preferred.
[0027] The ratio of the other unsaturated monomer to the total of the vinyl ester monomer and the other unsaturated monomer (100 mol %) is preferably 0.5 to 20 mol %, more preferably 0.8 to 10 mol %. When the ratio of the other unsaturated monomer is within the above range, the degree of modification of the modified PVOH tends to be within the preferred range described later.
[0028] The production process after polymerization can be the same as that for the unmodified PVOH described above to obtain the modified PVOH.
[0029] Another example of modified PVOH is post-modified PVOH. Post-modified PVOH can be produced by post-modifying unmodified PVOH, typically by introducing a modifying group into the OH group of the vinyl alcohol unit of the unmodified PVOH. Examples of the post-modification method include a method of converting unmodified PVOH into acetoacetate, acetalization, urethanization, etherification, phosphoric acid esterification, oxyalkylenation, or dehydration condensation with an acid. Examples of the acetoacetate conversion method include a method of subjecting a hydroxyl group of unmodified PVOH to an acetoacetate transesterification reaction, a method of reacting unmodified PVOH with diketene, and the like. As the post-modified PVOH, from the viewpoint of solubility in water, a modified PVOH which has been converted into an acetoacetate ester is preferred.
[0030] The modified PVOH may be any one of the above-mentioned modified PVOHs, or a mixture of two or more of them. The modified PVOH may be a mixture of one or more of the above-mentioned modified PVOHs and unmodified PVOH.
[0031] The modification amount of the modified PVOH varies depending on the nature of the modifying group, but is preferably 0.1 to 30 mol%, more preferably 0.5 to 20 mol%, and even more preferably 1 to 10 mol%. If the modification amount is equal to or greater than the lower limit, the crosslink density of the freeze-thawed hydrogel is lowered, and not only the drug present near the surface of the freeze-thawed hydrogel but also the drug components present inside the freeze-thawed hydrogel tend to be easily eluted. If the modification amount is equal to or less than the upper limit, the rapid elution of the drug immediately after the freeze-thawed hydrogel is applied to the affected area tends to be suppressed. The modification amount is the ratio of the modifying group to 100 mol % of all units constituting the modified PVOH. The amount of modification is measured by NMR or titration. The amount of denaturation of the modified PVOH does not change before and after the freeze-thaw hydrogel is formed. The amount of denaturation of the modified PVOH can be measured by re-dissolving the freeze-thawed hydrogel. Methods for re-dissolving the freeze-thawed hydrogel include dissolution at high temperature and high pressure.
[0032] The average saponification degree of the modified PVOH is preferably 95 mol% or more, more preferably 96 mol% or more, further preferably 97 mol% or more, and may be 100 mol%. When the average saponification degree is equal to or more than the lower limit, gelation tends to be easily performed, and the dissolution rate of the gel tends to be reduced. The average degree of saponification is measured in accordance with JIS K 6726:1994, 3.5. The average saponification degree of the modified PVOH does not change before and after the freeze-thaw hydrogel is formed. The average saponification degree of the modified PVOH can be measured by re-dissolving the freeze-thawed hydrogel.
[0033] The average degree of polymerization of the modified PVOH can generally be indicated by the viscosity of an aqueous solution. The viscosity of a 4% by mass aqueous solution of modified PVOH at 20° C. is preferably 5 to 100 mPa s, more preferably 13 to 70 mPa s, and even more preferably 17 to 40 mPa s. If the viscosity is equal to or greater than the lower limit, gelation tends to be facilitated and the dissolution rate of the gel tends to be reduced, while if the viscosity is equal to or less than the upper limit, the aqueous PVOH solution tends to be easier to handle and the drug release properties tend to be superior. The viscosity is measured in accordance with JIS K 6726:1994, 3.11.2. The average degree of polymerization of the modified PVOH does not change before and after the freeze-thaw hydrogel is formed. The average degree of polymerization of the modified PVOH can be measured by re-dissolving the freeze-thawed hydrogel.
[0034] <Drugs> The freeze-thaw hydrogel preferably contains a drug. The drug is not particularly limited and can be appropriately selected from known drugs depending on the disease to be treated. The agent may be, for example, a nucleic acid, a protein, a carbohydrate (such as a polysaccharide), other organic compound, an inorganic compound, or a combination of two or more of these.
[0035] Examples of drugs applicable to ophthalmic diseases include, but are not limited to, anti-infective agents (antibacterial agents, antiviral agents, antifungal agents, antiprotozoal agents, etc.), angiogenesis inhibitors (anti-vascular endothelial growth factor (VEGF) agents, etc.), anti-inflammatory agents, intraocular pressure reducing agents, anti-cancer agents, anesthetics, autonomic nerve agents, steroids (corticosteroids, etc.), antihistamines, mast cell stabilizers, immunosuppressants, mitotic inhibitors, etc.
[0036] Non-limiting examples of antibacterial agents include bacitracin, chloramphenicol, ciprofloxacin, erythromycin, moxifloxacin, gatifloxacin, gentamicin, levofloxacin, sulfacetamide, polymyxin B, vancomycin, tobramycin, or combinations thereof. Non-limiting examples of antiviral agents include trifluridine, vidarabine, acyclovir, valacyclovir, famciclovir, foscarnet, ganciclovir, formivirsen, cidofovir, or combinations thereof. Non-limiting examples of anti-fungal agents include amphotericin B, natamycin, fluconazole, itraconazole, ketoconazole, miconazole, or combinations thereof. Non-limiting examples of antiprotozoal agents include polymyxin B, neomycin, clotrimazole, miconazole, ketoconazole, propamidine, polyhexamethylene biguanide, chlorhexidine, itraconazole, or combinations thereof.
[0037] Non-limiting examples of anti-inflammatory agents include any known steroidal anti-inflammatory agent (SAIDs), any known non-steroidal anti-inflammatory agent (NSAIDs), or a combination thereof. Non-limiting examples of SAIDs include glucocorticoids such as dexamethasone, prednisolone, fluorometholone, loteprednol, medrysone, rimexolone, etc. Non-limiting examples of NSAIDs include diclofenac, flurbiprofen, ketorolac, bromofenac, nepafenac, or a combination thereof.
[0038] Non-limiting examples of anti-neoplastic agents include chemotherapeutic agents well known in the art. Non-limiting examples of anesthetic agents include aminoamides, aminoesters, or combinations thereof. Non-limiting examples of aminoamides include lidocaine, prilocaine, mepivacaine, ropivacaine, or combinations thereof. Non-limiting examples of possible aminoesters include benzocaine, procaine, proparacaine, tetracaine, or combinations thereof.
[0039] Non-limiting examples of autonomic agents include acetylcholine, carbachol, pilocarpine, physostigmine, echothiophate, atropine, scopolamine, homotrapine, cyclopentolate, tropicamide, dipivefrin, epinephrine, phenylephrine, apraclonidine, brimonidine, cocaine, hydroxyamphetamine, naphazoline, tetrahydrozoline, dapiprazole, betaxolol, carteolol, levobunolol, metipranolol, timolol, bepotastine besylate, or combinations thereof.
[0040] Non-limiting examples of antihistamines include pheniramine, antazoline, naphazoline, emedastine, levocarbastine, cromolyn, or combinations thereof. Non-limiting examples of mast cell stabilizers include lodoxamide, pemirolast, nedocromil, olopatadine, ketotifen, azelastine, epinastine, or combinations thereof.
[0041] As the drug, an anionic drug, an amphoteric drug, or a cationic drug is preferred because it is easily adsorbed to the gel and its release is easily controlled. Anionic drugs are drugs that have anionic groups and exhibit a negative charge in water. Non-limiting examples of anionic agents include nucleic acids, tranilast, acitazanolast hydrate, sodium cromoglycate, glutathione, pranoprofen, bromfenac sodium, diclofenac sodium, or combinations thereof. As the nucleic acid of the drug, for example, antisense oligonucleotide can be mentioned.Antisense oligonucleotide is also called antisense nucleic acid, and refers to a single-stranded oligonucleotide that comprises a base sequence that can hybridize with at least a part of the transcription product of target gene or the target transcription product (i.e., complementary), and can suppress the expression of the transcription product of target gene or the level of the target transcription product mainly by antisense effect. The target gene or target transcript whose expression is suppressed, altered, or modified by the antisense effect is not particularly limited, but may be, for example, a gene derived from an organism into which the nucleic acid complex is introduced, such as a gene whose expression is increased in various diseases. The transcript of the target gene is an mRNA transcribed from genomic DNA encoding the target gene, and further includes an mRNA that has not been base-modified, an unprocessed mRNA precursor, and the like. The target transcript may include not only an mRNA but also a non-coding RNA (ncRNA) such as miRNA. More generally, the transcript may be any RNA synthesized by a DNA-dependent RNA polymerase. In one embodiment, the target transcript may be, for example, a metastasis associated lung adenocarcinoma transcript 1 (malat1) non-coding RNA, a scavenger receptor B1 (SR-B1) mRNA, or a dystrophia myotonica-protein kinase (DMPK) mRNA. The nucleotide sequences of genes and transcripts are available from publicly known databases, such as the NCBI (National Center for Biotechnology Information) database. The anionic drug may be used in combination with other drugs.
[0042] An amphoteric drug is one that has an anionic group and a cationic group and has a zero charge in water. The ophthalmic drug olopatadine has a single positively charged tertiary amine group and a single negatively charged carboxylic acid group and is therefore considered to have a net charge of zero. Non-limiting examples of amphoteric drugs include levocabastine hydrochloride, amlexanox, olopatadine, lomefloxacin hydrochloride, ofloxacin, norfloxacin, levofloxacin, tosufloxacin, pirenoxine, rapamycin, or combinations thereof. Amphoteric drugs may be used in combination with other drugs.
[0043] A cationic drug is one that has a cationic group and exhibits a positive charge in water. In one example, the cationic agent is a polymer. Exemplary cationic polymers include epsilon polylysine (εPLL), polyquat, and the like, which are antimicrobial peptides that contain multiple arginine and / or lysine groups. In another example, the cationic drug comprises a guanidinium group, which is a positively charged group that comprises a central carbon atom covalently bonded to three nitrogen atoms and has a double bond between one of the nitrogen atoms and the central carbon.Typical beneficial agents for ophthalmic applications that comprise at least one guanidinium group include antihistamines, such as epinastine and emedastine; glaucoma drugs, such as apraclonidine and brimonidine; guanine derivative antiviral drugs, such as ganciclovir and valganciclovir; arginine-containing antibacterial peptides, such as defensins and indolicidin; and biguanide antibacterial agents, such as chlorhexidine, alexidine, and polyhexamethylene biguanide (PHMB). Other cationic drugs for ophthalmic use include ketotifen, cationic steroids, neostigmine methylsulfate, oxybuprocaine hydrochloride, naphazoline nitrate, naphazoline hydrochloride, sodium chondroitin sulfate, pilocarpine hydrochloride, distigmine bromide, echothiopate iodide, epinepherine, epinepherine bitartrate, carteolol hydrochloride, befunolol hydrochloride, and ripasudil. The cationic drug may be used in combination with other drugs.
[0044] The freeze-thaw hydrogel may further contain other components other than PVOH and the drug, if necessary, within the scope of not significantly impairing the effects of the present invention. For example, when the freeze-thawed hydrogel is used for the treatment of ophthalmic diseases, known ingredients can be contained as ingredients other than the drug in preparations for ophthalmic diseases (eye drops, etc.). For example, when the freeze-thaw hydrogel is used for a contact lens, it may contain known ingredients (antioxidants, stabilizers, preservatives, osmotic pressure adjusting agents, etc.) other than the drug as blended ingredients for contact lenses. The other components may be used alone or in combination of two or more.
[0045] In the freeze-thaw hydrogel, the PVOH content is preferably 5 to 60 mass %, more preferably 10 to 50 mass %, based on the total mass of the freeze-thaw hydrogel. When the PVOH content is equal to or greater than the lower limit, the lens strength tends to be superior. When the PVOH content is equal to or less than the upper limit, the oxygen permeability tends to be superior.
[0046] In the freeze-thaw hydrogel, the drug content is set taking into consideration the dosage, release amount, etc. of the drug. The amount of the drug contained is not particularly limited, but can be set, for example, in the range of 0.1 to 20% by mass relative to the total mass of the freeze-thawed hydrogel, and in the range of 0.2 to 80% by mass relative to PVOH.
[0047] The saturated moisture content of the freeze-thaw hydrogel is preferably 50 to 90% by mass, more preferably 60 to 88% by mass. If the saturated moisture content is equal to or higher than the lower limit, the oxygen permeability tends to be better. If the saturated moisture content is equal to or lower than the upper limit, the strength of the gel tends to be better. The saturated moisture content of a freeze-thawed hydrogel is the moisture content of the freeze-thawed hydrogel immersed in purified water at 37°C for 24 hours. The saturated moisture content is measured by the dry weight method and calculated using the following formula. The freeze-thawed hydrogel is dried at 140°C for 1 hour. Saturated moisture content = {(mass after soaking) - (mass after drying)} / (mass after soaking) x 100
[0048] The compressive elastic modulus of the freeze-thawed hydrogel at 37°C is preferably 0.1 to 500 kPa, more preferably 1 to 400 kPa, and even more preferably 3 to 300 kPa. If the compressive elastic modulus is equal to or greater than the lower limit, the wearing comfort tends to be better. If the compressive elastic modulus is equal to or less than the upper limit, the wearing comfort tends to be better. The compressive modulus is measured by thermomechanical analysis (TMA method). The compressive elastic modulus of the freeze-thaw hydrogel can be adjusted by the number of repeated freeze-thaw cycles, the degree of saponification of PVOH, the degree of polymerization, etc. For example, the compressive elastic modulus tends to increase as the number of repeated freeze-thaw cycles increases.
[0049] In the freeze-thaw hydrogel, in the sustained release test described below, the cumulative dissolution rate of the drug component after 1 hour is preferably 90% by mass or less of the cumulative dissolution rate after 24 hours, more preferably 80% by mass or less, and even more preferably 70% by mass or less. If the cumulative dissolution rate after 1 hour is the upper limit value or less, the sustained release property is excellent.
[0050] Sustained release test: The frozen and thawed hydrogel is placed in a 24-well cell culture plate, 1000 μL of phosphate buffered saline (hereinafter also referred to as "PBS") is added, and after standing at 37 ° C for 15 minutes, the entire amount of the PBS is collected, and then, a new 1000 μL of PBS is added, and after standing at 37 ° C for 15 minutes (total 30 minutes), the entire amount of the PBS is collected, and then, a new 1000 μL of PBS is added, and after standing at 37 ° C for 30 minutes (total 1 hour), the entire amount of the PBS is collected. This is repeated, and the PBS collected 15 minutes, 30 minutes, 1 hour, 4 hours, 8 hours, and 24 hours after the first addition of PBS is used as a measurement sample, and the amount of the drug component dissolved is determined by high performance liquid chromatography (hereinafter also referred to as "HPLC"), and the cumulative dissolution rate at each time is calculated. Here, the "cumulative dissolution rate" is the mass percentage of the "total of drug components dissolved up to each time point" relative to the "drug content of the freeze-thawed hydrogel."
[0051] The shape of the freeze-thaw hydrogel is not particularly limited, and may be, for example, a sheet shape, a lens shape, etc. When the freeze-thaw hydrogel is in a sheet shape, the shape in top view is also not particularly limited, and may be, for example, a polygonal shape such as a square, a ring shape, a semicircular shape, a crescent shape, an arch shape, etc.
[0052] <Method of manufacturing freeze-thawed hydrogel> Methods for producing the freeze-thaw hydrogel of the present invention include, for example, the following methods (1) and (2). Method (1): A method in which a PVOH aqueous solution is converted into a hydrogel by a first freeze-thaw treatment, and the water content of the hydrogel is reduced to 75 mass % or less, and then a second freeze-thaw treatment is performed. Method (2): A method in which PVOH is melt-kneaded in the presence of water to obtain a PVOH composition containing water, and then the composition is subjected to a freeze-thaw treatment.
[0053] [Method (1)] The PVOH aqueous solution contains PVOH and water. The PVOH aqueous solution may contain a chemical. The PVOH aqueous solution may further contain other components in addition to PVOH, water, and the chemical. The aqueous PVOH solution can be prepared by mixing water and PVOH, and optionally a drug or other ingredients. The content of PVOH in the PVOH aqueous solution is preferably 5 to 30% by mass, more preferably 10 to 20% by mass, based on the total mass of the PVOH aqueous solution. If the content of PVOH is equal to or more than the lower limit, the gel strength of the resulting gel tends to be superior. If the content of PVOH is equal to or less than the upper limit, the oxygen permeability of the resulting gel tends to be superior. The content of water in the aqueous PVOH solution is preferably 60 to 95 mass %, and more preferably 70 to 90 mass %, based on the total mass of the aqueous PVOH solution.
[0054] In the first freeze-thaw treatment, the PVOH aqueous solution is frozen by lowering the temperature, and the frozen PVOH aqueous solution is thawed by raising the temperature (hereinafter also referred to as "freeze-thaw cycle") at least once. Although a hydrogel can be obtained by a single freeze-thaw cycle, it is preferable to repeat the freeze-thaw cycle at least twice, and more preferably at least three times, in order to obtain a hydrogel with sufficiently high strength. The upper limit of the number of times the freeze-thaw cycle is repeated is not particularly limited, and is, for example, 20 times, or further 10 times. The freezing temperature of the PVOH aqueous solution is preferably −5° C. or lower, more preferably −10° C. or lower, from the viewpoint of ease of physical crosslinking. After freezing the PVOH aqueous solution, it is preferable to hold the frozen PVOH aqueous solution at the freezing temperature before thawing the frozen aqueous solution. The holding time at the freezing temperature is preferably 30 minutes or more, more preferably 1 hour or more. The upper limit of the holding time at the freezing temperature is not particularly limited, but is, for example, 24 hours. The melting temperature of the PVOH aqueous solution is preferably 5° C. or higher, more preferably 10° C. or higher, from the viewpoint of ease of physical crosslinking. After thawing, the PVOH aqueous solution is preferably held at the melting temperature before freezing the PVOH aqueous solution in the next freeze-thaw cycle or before adjusting the water content of the hydrogel. The holding time at the melting temperature is preferably 30 minutes or more, more preferably 1 hour or more. The upper limit of the holding time at the melting temperature is not particularly limited, but is, for example, 24 hours.
[0055] After the first freeze-thaw treatment, the hydrogel is dried to adjust the water content of the hydrogel to 75% by mass or less. The water content may be adjusted by first drying the hydrogel to a large extent (for example, to a water content of 10% by mass or less) and then humidifying it. If the water content exceeds 75% by mass, the onset temperature on the low-temperature side of the absorption peak of the melting point of water in the hydrogel in differential scanning calorimetry does not reach -5°C or less, resulting in a hydrogel with a large amount of elution and reduced transparency. The water content of the hydrogel is more preferably 60% by mass or less, and even more preferably 50% by mass or less. The lower limit of the water content is preferably 10% by mass or more, particularly preferably 20% by mass or more, and particularly preferably 30% by mass or more. The water content is the ratio of the mass of water to the mass of the hydrogel, and is calculated from the mass of the hydrogel and the mass after drying the hydrogel at 140°C for 1 hour (mass after drying) using the following formula: Water content (mass%) = (mass of hydrogel - mass after drying) / mass of hydrogel × 100
[0056] After adjusting the water content, the freeze-thaw hydrogel of the present invention is obtained by carrying out a second freeze-thaw treatment. The conditions for the second freeze-thaw treatment may be the same as those for the first freeze-thaw treatment described above.
[0057] A film of a PVOH aqueous solution is formed on a substrate, and the first freeze-thaw treatment, adjustment of the water content, and second freeze-thaw treatment are carried out to obtain a film-like freeze-thaw hydrogel. The freeze-thaw hydrogel peeled off from the substrate may be further processed, such as by cutting. A PVOH aqueous solution is poured into a mold of any shape, and the first freeze-thaw treatment, adjustment of the water content, and second freeze-thaw treatment are carried out to obtain a freeze-thawed hydrogel of a shape corresponding to the mold. The freeze-thawed hydrogel removed from the mold may be further processed, such as by cutting.
[0058] [Method (2)] In the method (2), first, PVOH is melt-kneaded in the presence of water to obtain a PVOH composition containing water. The PVOH composition may contain a drug. The PVOH composition may contain other components in addition to PVOH, water, and the drug.
[0059] When PVOH is melt-kneaded in the presence of water, various extruders such as a single screw extruder or a twin screw extruder, a Banbury mixer, a Brabender, a plastograph, a heat roll, or a kneader can be used as a melt-kneading device. An extruder is preferred in that a PVOH composition containing water can be continuously produced, and a twin screw extruder is more preferred in that the chemicals and water can be mixed more uniformly. The L / D of the twin-screw extruder is preferably 25 or more, more preferably 40 or more, for kneading without unmelted matter, and is preferably 100 or less, more preferably 80 or less, for suppressing excessive evaporation of water during melt kneading.
[0060] The temperature (kneading temperature) when PVOH is melt-kneaded in the presence of water is preferably 80° C. or higher, and more preferably 90° C. or higher. The upper limit of the kneading temperature is sufficient as long as the PVOH composition containing water does not foam, and is preferably 120° C. or lower, and more preferably 110° C. or lower.
[0061] When an extruder is used for melt kneading, PVOH is charged from a hopper of the extruder, water is supplied from a hopper and / or a vent near the hopper, and PVOH and water are melt kneaded in the extruder to produce a PVOH composition containing water. The water content of the PVOH composition can be adjusted by adjusting the amount of PVOH charged and the amount of water supplied to the extruder. By simultaneously supplying the chemicals, a PVOH composition containing water and the chemicals can be obtained.
[0062] The water content of the PVOH composition after melt kneading is preferably 70% by mass or less, more preferably 60% by mass or less, in order to provide a hydrogel with high transparency and low elution amount after freeze-thaw treatment.The lower limit of the water content is preferably 10% by mass or more, particularly preferably 20% by mass or more, and particularly preferably 30% by mass or more. The water content of the PVOH composition can be measured in the same manner as the water content of the hydrogel described above, and can be calculated by the following formula. Water content (mass%)=(mass of PVOH composition−mass after drying) / mass of PVOH composition×100
[0063] A freeze-thaw hydrogel can be obtained by subjecting the PVOH composition after melt-kneading to a freeze-thaw treatment. The freeze-thaw treatment involves performing an operation of lowering the temperature of the PVOH composition to freeze it and then raising the temperature of the frozen PVOH composition to melt it (hereinafter, also referred to as the "freeze-thaw cycle") one or more times. Although a hydrogel can be obtained by one freeze-thaw cycle, it is preferable to repeat the freeze-thaw cycle two or more times, and more preferably three or more times, in terms of obtaining a hydrogel with sufficiently high strength. The upper limit of the number of times the freeze-thaw cycle is repeated is not particularly limited, but is, for example, 20 times, or even 10 times. The freezing temperature of the PVOH composition is preferably -5°C or lower, and more preferably -10°C or lower, from the viewpoint of ease of physical crosslinking. After freezing the PVOH composition, it is preferable to hold the frozen PVOH composition at the freezing temperature before melting the frozen PVOH composition. The holding time at the freezing temperature is preferably 30 minutes or more, and more preferably 1 hour or more. The upper limit of the holding time at the freezing temperature is not particularly limited, but is, for example, 24 hours. The melting temperature of the PVOH composition is preferably 5°C or higher, and more preferably 10°C or higher, from the viewpoint of ease of physical crosslinking.
[0064] <DSC onset temperature> The freeze-thaw hydrogel of the present invention has an onset temperature on the low-temperature side of the endothermic peak observed in the range of 0°C or lower when measured under the conditions of a temperature increase rate of 10°C / min from -50°C to 150°C in differential scanning calorimetry (hereinafter, also referred to as "DSC") (hereinafter, also referred to as the "DSC onset temperature") of -5°C or lower. The DSC onset temperature is the temperature at which the melting of ice occurs, and can also be said to be the melting point of water in the freeze-thaw hydrogel. When the DSC onset temperature is -5°C or lower, a freeze-thaw hydrogel with little elution and excellent transparency is obtained. The DSC onset temperature is more preferably -7°C or lower, and particularly preferably -8°C or lower. The lower limit of the DSC onset temperature is usually -20°C or higher.
[0065] The details of the method for measuring the DSC onset temperature are shown below. After soaking the hydrogel in water at 30°C for 1 hour, cut out about 5 mg of the hydrogel as a measurement sample and seal it in a high-pressure pan for measurement. Using a Mettler Toledo differential scanning calorimeter, hold the measurement sample in the holder at -50°C for 1 minute, then measure the endothermic peak when the temperature is raised from -50°C to 150°C at 10°C / min. There is an endothermic peak of water in the hydrogel below 0°C, and the temperature at the intersection of the tangent at the inflection point on the low-temperature side (the side where melting begins) of the endothermic peak and the extension of the baseline is the DSC onset temperature.
[0066] It is not clear why a DSC onset temperature of -5°C or lower results in a hydrogel with minimal dissolution and excellent transparency, but it is speculated that this is because more dense and uniform crystals are produced when the crystallization of PVOH progresses due to freezing and thawing. When the area occupied by the water clusters in the hydrogel becomes smaller, the surface free energy decreases and the melting temperature decreases, so that the onset temperature shifts to a lower temperature. In the case of method (1), in a state where PVOH crystals are partially formed by the freeze-thaw treatment, the water content is adjusted and the freeze-thaw treatment is performed again, so that the water in the hydrogel is well dispersed, and the PVOH crystals are generated uniformly and densely, so that the onset temperature decreases, and a hydrogel with excellent transparency and little elution is obtained. In the case of method (2), PVOH is melt-kneaded in the presence of water, and the freeze-thaw treatment is performed in a state where water is well dispersed in the PVOH composition, so that the PVOH crystals are generated uniformly and densely, so that the onset temperature decreases, and a hydrogel with excellent transparency and little elution is obtained.
[0067] <Action and effect> The freeze-thaw hydrogel of the present invention has little elution and is excellent in transparency. In the freeze-thaw hydrogel of the present invention, the crystallization of polyvinyl alcohol proceeds densely and uniformly by the freeze-thaw treatment, so that there is little elution and the hydrogel has excellent transparency. Therefore, when used as a medical contact lens, no problems occur when the lens is worn and visibility is ensured, making the hydrogel an excellent hydrogel for use in contact lenses.
[0068] When the freeze-thawed hydrogel of the present invention contains a drug, the freeze-thawed hydrogel of the present invention can be used, for example, to treat ophthalmic diseases. When the freeze-thawed hydrogel of the present invention is brought into contact with the cornea or conjunctiva, the drug is gradually dissolved from the freeze-thawed hydrogel into the tear fluid. Non-limiting examples of ophthalmic diseases include infections of the eye (including the skin, eyelid, conjunctiva, or lacrimal drainage system), orbital cellulitis, dacryoadenitis, styes, blepharitis, conjunctivitis, keratitis, corneal infiltrates, ulcers, endophthalmitis, panophthalmitis, viral keratitis, fungal keratitis, herpes zoster ophthalmicus, viral conjunctivitis, viral retinitis, uveitis, strabismus, retinal necrosis, scleritis, mucormycosis, dacryoductitis, acanthamoeba keratitis, toxoplasmosis, giardiasis, leishmaniasis, malaria, helminth infections, and glaucoma.
[0069] The freeze-thaw hydrogel of the present invention can be made into ophthalmic medical devices (contact lenses, punctal plugs, intraocular lenses, intraocular rings, etc.), medical gels (stents, patch sheets, simulated organs, etc.), gel scaffolds for cell culture, worms for fishing tackle, etc.
[0070] [Contact Lenses] The contact lenses of the present invention comprise the freeze-thaw hydrogels of the present invention. The contact lens of the present invention may consist solely of the freeze-thaw hydrogel of the present invention, or may consist of the freeze-thaw hydrogel of the present invention and other lens materials. When the freeze-thaw hydrogel of the present invention is opaque or translucent, it is preferable that the region of the contact lens through which the optical axis passes is made of another lens material.
[0071] Other lens materials may be used, for example, lens materials known in the art of contact lenses. The other lens material may be a hydrogel. Non-limiting examples of other lens materials include Polymacon, Ocufilcon D, Etafilcon, Omafilcon A, Nelfilcon, Hilafilcon B, Lotrafilcon B, Senofilcon A, Galyfilcon A, Netrafilcon A, Lidofilcon B, Bufilcon A, Deltafilcon A, Phemfilcon, Hioxifilcon A, Perfilcon A, Methafilcon A, and the like.
[0072] Examples of contact lenses consisting of the freeze-thaw hydrogel of the present invention and other lens materials include (1) a form in which the freeze-thaw hydrogel of the present invention is embedded in the other lens material in the shape of a lens, (2) a form in which the other lens material in the shape of a lens and the freeze-thaw hydrogel of the present invention are laminated, and (3) a form in which the freeze-thaw hydrogel of the present invention is interspersed in the other lens material in the shape of a lens.
[0073] In the above embodiment (1), the number of freeze-thawed hydrogels embedded in the other lens material may be one or more. A part of the freeze-thawed hydrogel may be exposed on the surface of the contact lens (for example, the surface in contact with the cornea or conjunctiva). The freeze-thaw hydrogel is preferably disposed in a region other than the region through which the optical axis of the contact lens passes. In this case, the shape of the freeze-thaw hydrogel may be annular, semicircular, crescent, arched, etc. Since the freeze-thaw hydrogel of the present invention has excellent transparency, it may be disposed in the region through which the optical axis of the contact lens passes.
[0074] A contact lens comprising the freeze-thawed hydrogel of the present invention and other lens materials can be produced with reference to known methods (e.g., the method described in JP-A-2012-511395). For example, the freeze-thawed hydrogel of the present invention is placed in a contact lens mold, a liquid lens material precursor is injected, and the injected lens material precursor is cured to produce a contact lens of the above form (1). EXAMPLES
[0075] The present invention will be described in more detail below with reference to examples, but the present invention is not limited to these examples. "Parts" refers to "parts by mass."
[0076] [Production of PVOH] <pvoh1> A reaction vessel equipped with a reflux condenser, a dropping device, and a stirrer was charged with 100 parts of vinyl acetate and 33 parts of methanol. While stirring, the temperature was raised under a nitrogen stream. After reaching the boiling point, 1.3 parts of acetyl peroxide was added to initiate polymerization. When the polymerization rate of vinyl acetate reached 81%, a predetermined amount of hydroquinone monomethyl ether was added to terminate the polymerization. Subsequently, unreacted vinyl acetate monomer was removed outside the system by distillation while blowing methanol vapor, and a methanol solution of vinyl acetate polymer was obtained. Next, the above solution was diluted with methanol to adjust the solid content concentration to 47%. This methanol solution was charged into a kneader, and while maintaining the solution temperature at 35°C, a 2% sodium methanol solution in sodium hydroxide was added at a ratio of 7 mmol per 1 mol of vinyl acetate structural unit to conduct saponification. As saponification progressed and the saponified product precipitated and became particulate, it was filtered off, washed well with methanol, and dried in a hot air dryer to obtain PVOH1. The average saponification degree of PVOH was 98.5 mol%, and the viscosity of a 4% aqueous solution was 27 mPa·s.
[0077] <PVOH2 (containing cationic groups)> Into a reaction vessel equipped with a reflux condenser, a dropping funnel, and a stirrer, 20 parts of methanol, 100 parts of vinyl acetate, and 0.7 part of a 65% aqueous solution of diallyldimethylammonium chloride were charged. Using acetyl peroxide as an initiator, heating under reflux was carried out under a nitrogen stream to initiate polymerization. 2.7 parts of a 65% aqueous solution of diallyldimethylammonium chloride were added dropwise over 5 hours immediately after the start of polymerization. When the polymerization rate reached 71%, m-dinitrobenzene was added as a polymerization inhibitor to terminate the polymerization. Subsequently, unreacted monomers were removed from the system by blowing methanol vapor to obtain a methanol solution of the copolymer. Next, the solution was diluted with methanol to adjust the concentration to 32%, charged into a kneader, and while maintaining the solution temperature at 35°C, a methanol solution of sodium hydroxide was added in an amount of 20 mmol based on the vinyl acetate monomer of the copolymer for saponification. The resulting solid was separated by filtration, washed well with methanol, and dried in a hot air dryer to obtain PVOH2 having a quaternary ammonium base, which is a cationic group and is the target product. The average saponification degree of the obtained cationic group-containing PVOH2 was 99.4 mol%, the viscosity of a 4% aqueous solution was 25.9 mPa·s, and the amount of quaternary ammonium modification was 1 mol%.
[0078] <PVOH3 (containing an anionic group)> In a reactor equipped with a reflux condenser, a dropping funnel, and a stirrer, 26 parts of methanol, 100 parts of vinyl acetate, and 0.1 parts of monomethyl maleate were charged, and the temperature was raised to 60°C under a nitrogen stream while stirring, and then 0.001 mol% (relative to the total amount of vinyl acetate) of t-butyl peroxy neodecanoate (the temperature at which the half-life is 1 hour is 65°C) was added as a polymerization catalyst to start polymerization. Immediately after the start of polymerization, 2.2 parts of monomethyl maleate (2 mol% relative to the total amount of vinyl acetate) and 0.008 mol% (relative to the total amount of vinyl acetate) of t-butyl peroxy neodecanoate were continuously added in accordance with the polymerization rate, and when the polymerization rate of vinyl acetate reached 73%, 0.01 parts of 4-methoxyphenol and 58 parts of methanol for dilution and cooling were added to terminate the polymerization. The amount of remaining active catalyst at the end of polymerization was 2 ppm relative to the total amount of the reaction solution. Next, the unreacted vinyl acetate monomer was removed from the system by blowing in methanol vapor to obtain a methanol solution of the copolymer. Next, the resulting methanol solution was diluted with methanol to adjust the solid concentration to 40% by mass, and a 4% by mass methanol solution of sodium hydroxide was mixed in such a ratio that 30 mmol of sodium hydroxide was used per mol of vinyl acetate units in the copolymer, and the saponification reaction was carried out at a temperature of 40-50°C for 25 minutes. The resin solidified by the saponification reaction was cut off to obtain the target product, PVOH3. The average saponification degree of the resulting PVOH3 was 99 mol%, the viscosity of a 4% by mass aqueous solution was 29 mPa s, and the amount of maleic acid modification was 2.1 mol%.
[0079] [Examples 1 and 2] PVOH shown in Table 1 was added to purified water while stirring, heated to 90°C, and stirred for 1 hour to completely dissolve. After slowly cooling to room temperature while stirring, purified water was added to adjust the PVOH concentration to 15% by mass, and sterilized in an autoclave at 120°C for 30 minutes. After cooling to room temperature, a nucleic acid was mixed as a model drug in an aqueous solution of PVOH at 0.8% by mass relative to PVOH to obtain a drug-containing PVOH solution. As the nucleic acid, an oligonucleotide represented by CdsTdsAdsGdsTdsTdsCdsAdsCdsTdsGdsAdsAdsTdsGdsCd (wherein each nucleic acid base is represented by A = adenine, T = thymine, G = guanine, C = cytosine, each sugar portion is represented by d = 2'-deoxyribose, and each internucleoside bond is represented by s = phosphorothioate) was used as Malat1 antisense. The obtained drug-containing PVOH solution was poured into a contact lens mold with a diameter of 11 mm and a base curve (BC) of 6.5, and the process of sandwiching the contact lens between a male and female mold, freezing at -20°C for 2 hours, and dissolving at 20°C for 1 hour was repeated five times to prepare a contact lens-shaped drug-containing hydrogel. The contact lens female mold was removed, and the hydrogel was dried on the male mold in an oven at 40°C for 1 hour, and then allowed to absorb moisture in a thermohygrostat at 60°C and 100% RH to adjust the water content of the hydrogel to the water content shown in Table 1. The hydrogel was again sandwiched between the contact lens molds, and freezing at -20°C for 2 hours and thawing at 20°C for 1 hour were repeated five times to obtain a contact lens-shaped drug-containing PVOH freeze-thawed hydrogel.
[0080] [Comparative Examples 1 and 2] The same drug-containing PVOH solution as in Examples 1 and 2 was injected into a contact lens mold with a diameter of 11 mm and a base curve (BC) of 6.5, which was then sandwiched between a male and female mold. The mold was then frozen at -20°C for 2 hours and thawed at 20°C for 1 hour. This process was repeated 10 times to obtain a contact lens-shaped drug-containing PVOH freeze-thawed hydrogel.
[0081] [Examples 3 to 6] As the PVOH, the above PVOH1 or a mixture of PVOH1 and PVOH3 mixed at the ratio described in Table 2 was supplied to the hopper of a twin-screw extruder with a diameter D = 15 mm and L / D = 60. From the vent port located at the second division from the hopper when the twin-screw extruder was divided into eight parts, 100 parts of water was supplied for every 100 parts of PVOH supplied to the hopper, and melt-kneaded at an extrusion temperature of 100 °C, a screw rotation speed of 200 rpm, and a discharge rate of 1 kg / h, and extruded into a sheet with a thickness of 200 μm to obtain a sheet of the PVOH composition containing water. The water content rate of the obtained sheet of the PVOH composition is shown in Table 2. A part of the obtained sheet of the PVOH composition was cut out, frozen at -20 °C for 2 hours, and the process of dissolving at 20 °C for 1 hour was repeated 10 times to obtain a sheet-like PVOH freeze-thaw hydrogel.
[0082] 〔Evaluation〕 The following properties of the obtained PVOH freeze-thaw hydrogel were evaluated.
[0083] <DSC onset temperature> After the PVOH freeze-thaw hydrogel was immersed in water at 30 °C for 1 hour, about 5 mg of the PVOH freeze-thaw hydrogel was cut out as a measurement sample and sealed in a high-pressure pan for measurement. Using a differential scanning calorimeter manufactured by Mettler Toledo, after holding the measurement sample in the holder at -50 °C for 1 minute, the endothermic peak was measured when the temperature was raised from -50 °C to 150 °C at 10 °C / min. Since there is an endothermic peak of water in the PVOH freeze-thaw hydrogel below 0 °C, the temperature at the intersection of the baseline on the low-temperature side (melting start side) of the endothermic peak and the tangent line at the inflection point was defined as the DSC onset temperature. The results are shown in Tables 1 and 2. Also, Fig. 1 shows a graph of the endothermic peak of water obtained by differential scanning calorimetry of the PVOH freeze-thaw hydrogel of Example 1.
[0084] <Elution rate> The PVOH freeze-thaw hydrogel was immersed in purified water at 37 °C for 24 hours, and the elution rate was calculated by the following formula from the mass change before and after immersion. The results are shown in Tables 1 and 2. Dissolution rate (%) = (mass of PVOH freeze-thawed hydrogel before immersion) - (mass of PVOH freeze-thawed hydrogel after immersion) / (mass of PVOH freeze-thawed hydrogel before immersion) x 100
[0085] <Light transmittance> For the contact lens-shaped PVOH freeze-thawed hydrogel, the PVOH freeze-thawed hydrogel was sandwiched between glass plates to a thickness of 1 mm, and for the sheet-shaped PVOH freeze-thawed hydrogel, the light transmittance at a wavelength of 600 nm was measured as is using an ultraviolet-visible near-infrared spectrophotometer (model: V-7200) manufactured by JASCO Corporation. Note that for the contact lens-shaped PVOH freeze-thawed hydrogel, the light transmittance was corrected using the light transmittance of the glass plate as a reference. The results are shown in Tables 1 and 2.
[0086] <Haze measurement> The contact lens-shaped PVOH freeze-thawed hydrogel was sandwiched between glass plates to a thickness of 1 mm, and the haze value was measured using a Haza Meter NDH4000 manufactured by Nippon Denshoku Industries Co., Ltd. The haze value was corrected using the haze value of the glass plate as a reference. The results are shown in Table 1.
[0087] [Table 1]
[0088] [Table 2]
[0089] The PVOH freeze-thaw hydrogels of Examples 1 and 2, in which the water content of the hydrogel was adjusted between the first freeze-thaw treatment and the second freeze-thaw treatment, had a low dissolution rate in warm water, a high light transmittance at 600 nm, and a low haze value, indicating that they had excellent stability and transparency in warm water. It can be seen that Comparative Examples 1 and 2, in which the moisture content was not adjusted, had a high elution rate and insufficient transparency. The PVOH freeze-thawed hydrogels of Examples 1 and 2 had lower DSC onset temperatures than the PVOH freeze-thawed hydrogels of Comparative Examples 1 and 2. This shows that the DSC onset temperature affects the dissolution rate and transparency. The freeze-thawed hydrogel produced by melt-kneading PVOH in the presence of water and then subjecting the resulting water-containing PVOH composition to a freeze-thaw treatment had a DSC onset temperature of -5°C or lower, a low dissolution rate in warm water, and a high light transmittance at 600 nm, and was found to have excellent stability and transparency in warm water, as in Examples 1 and 2.
Claims
1. A freeze-thaw hydrogel of polyvinyl alcohol, A freeze-thaw hydrogel, in which, when measured in differential scanning calorimetry under conditions of -50°C to 150°C and a heating rate of 10°C / min, the onset temperature on the low-temperature side of an absorption peak observed in the range of 0°C or lower is -5°C or lower.
2. The freeze-thaw hydrogel according to claim 1 , wherein the polyvinyl alcohol is a denatured polyvinyl alcohol.
3. The freeze-thaw hydrogel according to claim 2 , wherein the polyvinyl alcohol is a modified polyvinyl alcohol having a cationic group or an anionic group.
4. The freeze-thaw hydrogel according to any one of claims 1 to 3, which is for use in contact lenses.
5. The freeze-thaw hydrogel according to any one of claims 1 to 3, which contains a drug.
6. A method for producing a freeze-thaw hydrogel of polyvinyl alcohol, comprising the steps of: A method for producing a freeze-thaw hydrogel, comprising: subjecting an aqueous polyvinyl alcohol solution to a first freeze-thaw treatment to form a hydrogel; adjusting the water content of the hydrogel to 75% by mass or less; and then subjecting the hydrogel to a second freeze-thaw treatment.
7. A method for producing a freeze-thaw hydrogel of polyvinyl alcohol, comprising the steps of: A method for producing a freeze-thaw hydrogel comprising melt-kneading polyvinyl alcohol in the presence of water to obtain a water-containing polyvinyl alcohol composition, and then subjecting the composition to a freeze-thaw treatment.
8. The method for producing a freeze-thaw hydrogel according to claim 7, wherein the water content of the polyvinyl alcohol composition is 70 mass% or less.
Citation Information
Patent Citations
PVA hydrous gel and its production
JP1996239538A
Ophthalmic device for sustained delivery of active compounds
JP2008539837A
Cited By
Polyvinyl alcohol-keratin semi-interpenetrating network hydrogel as well as preparation method and application thereof
CN119708541A