Stretched porous film, roll, sanitary goods and method for producing stretched porous film
A stretched porous film using polybutylene adipate terephthalate and an inorganic filler addresses the issues of low moisture permeability and tear strength in conventional films, achieving high moisture permeability and tear strength while being biodegradable.
Patent Information
- Application Number
- JP2024034097
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2023-03-29
- Filing Date
- 2024-03-06
- Publication Date
- 2024-10-11
AI Technical Summary
Conventional stretched porous films containing polylactic acid resins lack sufficient moisture permeability and often experience breakage or decreased tear strength when the stretching ratio is increased.
A stretched porous film composed of polybutylene adipate terephthalate and an inorganic filler, with specific properties such as breaking elongation, tear strength, and molecular weight ranges, is developed to enhance moisture permeability and tear strength.
The film achieves excellent moisture permeability and tear strength, with moisture permeability ranging from 1000 to 15000 g/m²/24hrs and tear strength exceeding 0.5 N/mm, while maintaining biodegradability.
Smart Images

Figure 2024144192000001
Abstract
Description
[Technical field]
[0001] The present invention relates to a stretched porous film, a roll, a sanitary product, and a method for producing a stretched porous film. [Background technology]
[0002] Conventionally, a porous film is known in which a resin composition containing a polyolefin and an inorganic filler is stretched to cause interfacial peeling between the polyolefin and the inorganic filler, forming a large number of voids (micropores). In particular, a stretched porous film made of a resin composition containing a polyolefin and an inorganic filler has internal micropores that form interconnected pores, and is therefore used as a moisture-permeable, waterproof film that has high air permeability and moisture permeability while suppressing the permeation of liquids. Such stretched porous films are widely used in applications requiring breathability, moisture permeability, and waterproofness, such as sanitary products such as paper diapers and feminine hygiene products, clothing such as work clothes, jumpers, jackets, medical clothing, and chemical protective clothing, masks, covers, drapes, sheets, and wraps.
[0003] For example, Patent Document 1 discloses a porous film obtained by stretching a film containing 50 to 200 parts by mass of an inorganic filler per 100 parts by mass of a polyethylene resin at least in the machine direction of the film to make it porous, in which the polyethylene resin has a Z-average molecular weight (Mz) of 300,000 or more and contains linear low-density polyethylene made of a copolymer of ethylene and an α-olefin having 6 or more carbon atoms.
[0004] Meanwhile, in recent years, research has been actively conducted on replacing conventional plastic products with biodegradable resins or biomass resins (raw materials derived from plants) from the viewpoint of environmental conservation. For example, Patent Document 2 discloses a film that contains a thermoplastic resin (A), contains 1 to 70% by mass of a filler (B) in 100% by mass of all components of the film, has a porosity of 80% or less, has a tear strength in any direction of 200 mN or less, and has a tensile strength in any direction of less than 15 MPa. Patent Document 3 discloses a porous film that contains a biodegradable resin (A), contains 1 to 70% by mass of a filler (B) in 100% by mass of all components of the porous film, has a porosity of 5 to 80%, is stretched in only one direction, has a heat shrinkage of 0 to 10% in the stretching direction, a heat shrinkage of -5 to 5% in the orthogonal direction, and has an elongation at break of 15% or more in the orthogonal direction. In these documents, the use of polylactic acid resin as the thermoplastic resin is specifically considered. [Prior art documents] [Patent documents]
[0005] [Patent Document 1] JP 2007-161787 A [Patent Document 2] International Publication No. 2014 / 156952 [Patent Document 3] JP 2015-83661 A Summary of the Invention [Problem to be solved by the invention]
[0006] As described above, in the case of a stretched porous film, the constituent resin has been replaced from a polyolefin-based resin to a polylactic acid-based resin. However, the moisture permeability of the conventional stretched porous film containing a polylactic acid-based resin is not sufficient, and improvement is required.
[0007] In order to increase the moisture permeability of a stretched porous film, it is possible to increase the stretch ratio of the film. However, in the case of a conventional stretched porous film containing a polylactic acid resin, when the stretch ratio is increased, problems such as breakage of the film or a decrease in tear strength may occur.
[0008] In order to solve such problems of the conventional techniques, the present inventors have carried out studies with the aim of providing a stretched porous film having excellent moisture permeability and tear strength. [Means for solving the problem]
[0009] Examples of specific embodiments of the present invention are given below.
[0010] [1] A stretched porous film containing polybutylene adipate terephthalate and an inorganic filler, and having a breaking elongation in the TD direction of 50% or more. [2] The stretched porous film according to [1], having a breaking elongation in the TD direction of 100% or more and 800% or less. [3] The stretched porous film according to [1] or [2], wherein the breaking elongation in the TD direction is greater than the breaking elongation in the MD direction. [4] The stretched porous film according to any one of [1] to [3], wherein the breaking elongation in the TD direction is P and the breaking elongation in the MD direction is Q, the P / Q value is 1.2 or more. [5] The stretched porous film according to any one of [1] to [4], which has a tear strength in the MD direction of 0.5 N / mm or more. [6] The stretched porous film according to any one of [1] to [5], which has a tear strength in the TD direction of 5.0 N / mm or more. [7] The stretched porous film according to any one of [1] to [6], which has a tensile strength in the MD direction of 10.0 MPa or more. [8] The stretched porous film according to any one of [1] to [7], which has a tensile strength in the TD direction of 1.0 MPa or more. [9] The stretched porous film according to any one of [1] to [8], wherein the polybutylene adipate terephthalate has a weight average molecular weight (Mw) of 50,000 to 400,000.
[10] The stretched porous film according to any one of [1] to [9], wherein the molecular weight distribution (Mw / Mn) of the polybutylene adipate terephthalate is 1.5 to 5.0.
[11] The stretched porous film according to any one of [1] to
[10] , wherein the melting point of the polybutylene adipate terephthalate is 105 to 130°C.
[12] The stretched porous film according to any one of [1] to
[11] , wherein, in 100 mol % of constituent units derived from dicarboxylic acids constituting polybutylene adipate terephthalate, constituent units derived from terephthalic acid account for 40 to 60 mol % and constituent units derived from adipic acid account for 40 to 60 mol %.
[13] The stretched porous film according to any one of [1] to
[12] , wherein the inorganic filler has an average particle size of 0.1 to 10 μm.
[14] The stretched porous film according to any one of [1] to
[13] , wherein the inorganic filler is calcium carbonate.
[15] The stretched porous film according to any one of [1] to
[14] , which has a thickness of 10 to 150 μm.
[16] Moisture permeability of 1000 to 15000 g / m2 based on a film thickness of 20 μm 2 The stretched porous film according to any one of [1] to
[15] , wherein the stretched porous film has a shelf life of 24 hours.
[17] A roll obtained by rolling up the stretched porous film according to any one of [1] to
[16] .
[18] A sanitary product comprising a stretched porous film according to any one of [1] to
[16] .
[19] A step of mixing polybutylene adipate terephthalate and an inorganic filler to obtain a resin composition; A step of forming the resin composition into a sheet to obtain a sheet; A method for producing a stretched porous film, comprising the steps of: A method for producing a stretched porous film, wherein the stretched porous film has a breaking elongation in the TD direction of 50% or more. Effect of the Invention
[0011] According to the present invention, a stretched porous film having excellent moisture permeability and tear strength can be obtained. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0012] The present invention will be described in detail below. The following description of the constituent elements may be based on a representative embodiment or a specific example, but the present invention is not limited to such an embodiment. In this specification, when "X to Y" (X and Y are any numbers) is used, it means "X or more and Y or less" unless otherwise specified, and also means "preferably greater than X" or "preferably smaller than Y". In addition, when "X or more" (X is any number) or "Y or less" (Y is any number), it also means "preferably greater than X" or "preferably less than Y". In the following description, "film" and "sheet" are not clearly distinguished from each other, and when "film" is used, it includes "sheet", and when "sheet" is used, it includes "film".
[0013] In this specification, the MD direction of the film is the extrusion direction (or take-up direction or flow direction) during film formation and is also called the machine direction, while the TD direction is the direction perpendicular to the MD direction and is also called the transverse direction or width direction.
[0014] (Stretched porous film) The present embodiment relates to a stretched porous film (hereinafter also referred to as the present stretched porous film) that contains polybutylene adipate terephthalate and an inorganic filler and has a breaking elongation in the TD direction of 50% or more. The stretched porous film of the present embodiment has a large number of voids (micropores), and these voids are connected in the thickness direction, so that the film can exhibit high moisture permeability.
[0015] The pore size of the voids (micropores) is preferably 0.05 to 0.5 μm. If the pore size of the voids (micropores) is within the above range, the film can be made liquid-impermeable (waterproof) while allowing water vapor and air to pass through. The pore size can be evaluated as the maximum pore size measured by the bubble point method (JIS K3832:1990 or ASTM F316), and more specifically, the pore size can be measured using a perm porometer.
[0016] The stretched porous film is a uniaxially stretched film. Since the stretched porous film contains an inorganic filler, the resin composition is stretched in the manufacturing process to cause interfacial peeling between the polybutylene adipate terephthalate and the inorganic filler, thereby forming a film having a large number of voids (micropores) having the above-mentioned pore size.
[0017] Since the stretched porous film of the present embodiment has the above-mentioned configuration, it has both excellent moisture permeability and tear strength. Here, the moisture permeability can be measured by the following method. First, a measuring cup (inner diameter 60 mm, inner diameter area 28.27×10 -4 m 2 ) was used to seal calcium chloride, and the cup was then sealed with a stretched porous film. The measuring cup was then placed in a constant temperature and humidity environment at a temperature of 40°C and a relative humidity of 90%, and the moisture permeability (g / m2) was calculated from the increase in the mass of the measuring cup after 24 hours. 2 In this embodiment, the moisture permeability converted into a film thickness of 20 μm can be calculated using the following formula. Moisture permeability of 20 μm thickness = Moisture permeability (measured value) × film thickness (μm) / 20 (μm)
[0018] The moisture permeability converted into a film thickness of 20 μm is 1000 g / m 2 -24hrs or more is preferable, 2000g / m 2 More preferably, 24hrs or more, 3000g / m 2 More preferably, 24 hours or more, 4000g / m 2More preferably, 24 hours or more, 5000g / m 2 More preferably, 24 hours or more, 6000g / m 2 More preferably, 24 hours or more, and 7000g / m 2 It is particularly preferable that the moisture permeability is 15,000 g / m2 or more based on a film thickness of 20 μm. 2 It is preferable that the moisture permeability is 24 hours or less. Thus, the stretched porous film of the present embodiment has excellent moisture permeability.
[0019] The stretched porous film of this embodiment has the above-mentioned configuration, and therefore has high tear strength. The tear strength in the MD direction of the stretched porous film of this embodiment is preferably 0.5 N / mm or more, more preferably 0.6 N / mm or more. The upper limit of the tear strength in the MD direction of the stretched porous film is not particularly limited, but is preferably, for example, 5 N / mm or less. In this embodiment, the tear strength in the MD direction of the stretched porous film is particularly increased. Usually, when a uniaxially stretched film is produced, stretching is performed in the MD direction (longitudinal direction), so that the tear strength in the MD direction tends to decrease. However, in this embodiment, polybutylene adipate terephthalate is used as the resin constituting the stretched porous film, and further, the breaking elongation in the TD direction is set to a predetermined value or more, so that the tear strength in the MD direction, in which the tear strength is likely to decrease, can be effectively increased.
[0020] In addition, the tear strength in the TD direction of the stretched porous film of this embodiment is preferably 5.0 N / mm or more, more preferably 6.0 N / mm or more, and even more preferably 7.0 N / mm or more. The upper limit of the tear strength in the TD direction of the stretched porous film is not particularly limited, but is preferably, for example, 30 N / mm or less. In this embodiment, polybutylene adipate terephthalate is used as the resin constituting the stretched porous film, so that the tear strength in the TD direction (transverse direction) is also increased. By increasing the tear strength of the stretched porous film, breakage during film formation or printing of the film can be suppressed, and the strength of the stretched porous film when used in absorbent articles such as diapers is sufficient. The tear strength of this stretched porous film is measured in accordance with JIS K7128-1:1998 by cutting a sample to a length of 100 mm and a width of 25 mm in the measurement direction, making a 25 mm cut in the center of the width, and using a tensile tester at 23°C, 50% relative humidity, a tensile speed of 200 m / min, and a chuck distance of 25 mm.
[0021] The breaking elongation in the TD direction of the present stretched porous film is preferably 50% or more, more preferably 60% or more, even more preferably 70% or more, even more preferably 80% or more, even more preferably 90% or more, and particularly preferably 100% or more. The upper limit of the breaking elongation in the TD direction of the present stretched porous film is not particularly limited, but is preferably, for example, 800% or less. The breaking elongation in the TD direction can be controlled, for example, by appropriately selecting the type and amount of resin constituting the stretched porous film.
[0022] The MD breaking elongation of the stretched porous film is preferably 30% or more, more preferably 33% or more, and even more preferably 35% or more. The upper limit of the MD breaking elongation of the stretched porous film is not particularly limited, but is preferably 200% or less. The breaking elongation of the stretched porous film is measured in accordance with JIS K7127:1999, by cutting a sample into a length of 100 mm and a width of 10 mm in the measuring direction, and using a tensile tester under the conditions of 23°C, 50% relative humidity, a pulling speed of 200 m / min, and a chuck distance of 20 mm.
[0023] In this embodiment, the breaking elongation in the TD direction is preferably greater than that in the MD direction. In a typical stretched porous film using a polyolefin resin or a polylactic acid resin, the breaking elongation in the MD direction is usually greater than that in the TD direction, but in this embodiment, the breaking elongation in the TD direction is preferably increased and is greater than that in the MD direction.
[0024] Here, when the breaking elongation in the TD direction is P and the breaking elongation in the MD direction is Q, the value of P / Q is preferably 1.2 or more, more preferably 1.5 or more, even more preferably 1.8 or more, and particularly preferably 1.9 or more. The value of P / Q is preferably 20 or less, more preferably 18 or less, and even more preferably 15 or less. By setting the value of P / Q within the above range, the moisture permeability and tear strength of the stretched porous film can be more effectively increased.
[0025] In this embodiment, polybutylene adipate terephthalate, which has low crystallinity, is used as the base resin, and the breaking elongation in the TD direction of the stretched film is set to 50% or more. This prevents the molecular chains from being strongly oriented in the MD direction, and suppresses oriented crystallization, which is believed to make it easier to obtain a film with a good balance between moisture permeability and tear strength.
[0026] The tensile strength in the MD direction of the present stretched porous film is preferably 10.0 MPa or more, more preferably 12.0 MPa or more, and even more preferably 14.0 MPa or more. The tensile strength in the MD direction of the present stretched porous film is preferably 50 MPa or less, more preferably 48 MPa or less, and even more preferably 45 MPa or less.
[0027] The tensile strength of the stretched porous film in the TD direction is preferably 1.0 MPa or more, more preferably 1.2 MPa or more, and even more preferably 1.4 MPa or more. The tensile strength of the stretched porous film in the TD direction is preferably 10 MPa or less, more preferably 8 MPa or less, and even more preferably 7 MPa or less. The tensile strength of the stretched porous film is measured in accordance with JIS K7127:1999, by cutting a sample into a length of 100 mm and a width of 10 mm in the measurement direction, and using a tensile tester under the conditions of 23°C, relative humidity of 50%, a pulling speed of 200 m / min, and a chuck distance of 20 mm.
[0028] This stretched porous film has excellent biodegradability because it contains polybutylene adipate terephthalate as a constituent resin. In this specification, biodegradability refers to the property of a film being decomposed by the action of organisms such as microorganisms. Since this stretched porous film is a biodegradable film, it is a material that contributes to environmental problems.
[0029] The thickness of the present stretched porous film is preferably 5 μm or more, more preferably 10 μm or more, and even more preferably 15 μm or more. The thickness of the present stretched porous film is preferably 300 μm or less, more preferably 200 μm or less, and even more preferably 150 μm or less. By making the thickness of the present stretched porous film within the above range, it is possible to make the film thinner while maintaining a balance between moisture permeability and mechanical strength.
[0030] The present embodiment may relate to a rolled body obtained by rolling up a stretched porous film. Since the stretched porous film has appropriate strength and flexibility, it can be stored or distributed in the form of a roll.
[0031] (Polybutylene adipate terephthalate) The stretched porous film contains polybutylene adipate terephthalate (PBAT). Polybutylene adipate terephthalate is a biodegradable resin, and is preferably a thermoplastic resin. Polybutylene adipate terephthalate is a copolymer of adipic acid, terephthalic acid, and butanediol. Adipic acid, terephthalic acid, and butanediol may be copolymerized simultaneously or in multiple stages.
[0032] When synthesizing polybutylene adipate terephthalate, in addition to adipic acid, terephthalic acid, and butanediol, a small amount of other copolymerization components may be added. Examples of other copolymerization components include dicarboxylic acids other than terephthalic acid and adipic acid, and modifiers for the purpose of chain extension, terminal blocking, etc. These may be used alone or in combination of two or more. Examples of other dicarboxylic acids include oxalic acid, malonic acid, succinic acid, glutaric acid, pimelic acid, suberic acid, etc. These may be used alone or in combination of two or more. Examples of modifiers include polyisocyanate compounds, glycol compounds, etc. Examples of the polyisocyanate compound include diisocyanate compounds, and examples of the diisocyanate compound include hexamethylene diisocyanate, 4,4'-diphenylmethane diisocyanate, 2,4-tolylene diisocyanate, 2,6-tolylene diisocyanate, xylylene diisocyanate, 1,5-naphthylene diisocyanate, p-phenylene diisocyanate, isophorone diisocyanate, 4,4'-dicyclohexylmethane diisocyanate, tetramethylxylene diisocyanate, carbodiimide-modified MDI, and polymethylene phenyl polyisocyanate. Examples of the glycol compound include diols other than butanediol and polyalkylene glycols. Examples of the other diols include methanediol, ethanediol, propanediol, pentanediol, and hexanediol. Examples of polyalkylene glycols include polymethylene glycol, polyethylene glycol, polypropylene glycol, polybutylene glycol (polytetramethylene glycol), etc. These may be used alone or in combination of two or more kinds.
[0033] In 100 mol % of the dicarboxylic acid-derived constituent units constituting the polybutylene adipate terephthalate, the constituent units derived from terephthalic acid are preferably contained at 40 to 60 mol %, and the constituent units derived from adipic acid are preferably contained at 40 to 60 mol %. By setting the ratio of the constituent units derived from terephthalic acid and the constituent units derived from adipic acid among the dicarboxylic acid-derived constituent units constituting the polybutylene adipate terephthalate within the above range, a film having a good balance of mechanical strength, biodegradability, and flexibility can be easily obtained.
[0034] Examples of polybutylene adipate terephthalate include biodegradable synthetic polymer compounds listed in the positive list of the Japan Bioplastics Association's GreenPla (biodegradable plastic) classification number A-1. Commercially available products include, for example, F Blend C1200 manufactured by BASF and ECO-A05 manufactured by Taiwan Chang Chun Co., Ltd.
[0035] The weight average molecular weight (Mw) of polybutylene adipate terephthalate is preferably 50,000 or more, more preferably 70,000 or more, and even more preferably 100,000 or more. The weight average molecular weight (Mw) of polybutylene adipate terephthalate is preferably 400,000 or less, more preferably 350,000 or less, and even more preferably 300,000 or less. The weight average molecular weight can be determined by gel permeation chromatography (GPC) or the like. By setting the weight average molecular weight (Mw) of polybutylene adipate terephthalate within the above range, a film having a good balance between extrusion moldability and mechanical strength can be easily obtained.
[0036] The molecular weight distribution (Mw / Mn) of polybutylene adipate terephthalate is preferably 1.5 or more, more preferably 1.7 or more, and even more preferably 1.9 or more. The molecular weight distribution (Mw / Mn) of polybutylene adipate terephthalate is preferably 5.0 or less, more preferably 4.5 or less, and even more preferably 4.0 or less. By making the molecular weight distribution (Mw / Mn) of polybutylene adipate terephthalate fall within the above range, a film having a good balance of film formability, film rigidity, and impact resistance can be easily obtained.
[0037] The melting point of polybutylene adipate terephthalate is preferably 105°C or higher, more preferably 108°C or higher, and even more preferably 110°C or higher. The melting point of polybutylene adipate terephthalate is preferably 130°C or lower, more preferably 128°C or lower, and even more preferably 125°C or lower. The melting point of polybutylene adipate terephthalate is measured by DSC or the like in accordance with JIS K 7121 (2012). By setting the melting point of polybutylene adipate terephthalate within the above range, a film having a good balance between heat resistance and moldability can be easily obtained.
[0038] The content of polybutylene adipate terephthalate in the stretched porous film is preferably 20% by mass or more, more preferably 30% by mass or more, and even more preferably 40% by mass or more, based on the total mass of the stretched porous film. The content of polybutylene adipate terephthalate is preferably 80% by mass or less, more preferably 70% by mass or less, and even more preferably 60% by mass or less, based on the total mass of the stretched porous film. By setting the content of polybutylene adipate terephthalate in the stretched porous film within the above range, the moisture permeability and tear strength of the stretched porous film can be more effectively increased.
[0039] (Inorganic filler) The stretched porous film contains an inorganic filler. Examples of inorganic fillers include various carbonates such as calcium carbonate, magnesium carbonate, and barium carbonate, various sulfates such as magnesium sulfate, barium sulfate, and calcium sulfate, various oxides such as zinc oxide, silicon oxide (silica), zirconium oxide, magnesium oxide, calcium oxide, titanium oxide, magnesium oxide, iron oxide, and alumina, and other hydroxides such as aluminum hydroxide, silicate minerals, various composite oxides such as hydroxyapatite, mica, talc, kaolin, clay, montmorillonite, and zeolite, various phosphates such as lithium phosphate, calcium phosphate, and magnesium phosphate, and various salts such as lithium chloride and lithium fluoride. Among these, from the viewpoint of improving moisture permeability and strength, the inorganic filler is preferably at least one selected from the group consisting of calcium carbonate, barium carbonate, barium sulfate, silicon oxide (silica), and titanium oxide, more preferably at least one selected from the group consisting of calcium carbonate and barium sulfate, and particularly preferably calcium carbonate.
[0040] The average particle size of the inorganic filler is preferably 0.1 μm or more, more preferably 0.3 μm or more, and even more preferably 0.5 μm or more. The average particle size of the inorganic filler is preferably 10 μm or less, more preferably 8 μm or less, and even more preferably 5 μm or less. By setting the average particle size of the inorganic filler to the above lower limit or more, poor dispersion and secondary aggregation of the inorganic filler are suppressed, and it is preferable that the inorganic filler can be uniformly dispersed in the resin composition constituting the stretched porous film. If the average particle size is the above upper limit or less, it is possible to suppress the generation of large voids when the film is thinned, and the film can have sufficient strength and water resistance.
[0041] The average particle size of the inorganic filler is calculated from the specific surface area measured by the constant pressure transmission method using a Shimadzu powder specific surface area measuring instrument SS-100. The measurement conditions are as follows: sample weight 3.0 g, sample thickness 1.35 cm, cross-sectional area of the sample layer 2 cm 2, air pressure is 50cmH2O, and the viscosity coefficient of air is 181×10 -6 Calculate the average particle size as g / (cm sec).
[0042] The inorganic filler may be surface-treated. For example, in order to improve dispersibility and mixability with the resin, the inorganic filler may be coated in advance with a surface treatment agent such as a fatty acid, a fatty acid ester, or an alkylene glycol (methylene glycol, ethylene glycol, propylene glycol, diethylene glycol, etc.) to make it more compatible with the resin. Among these surface treatment agents, fatty acids are preferred from the viewpoint of moisture permeability.
[0043] The content of the inorganic filler in the stretched porous film is preferably 20% by mass or more, more preferably 30% by mass or more, and even more preferably 40% by mass or more, based on the total mass of the stretched porous film. The content of the inorganic filler is preferably 80% by mass or less, more preferably 70% by mass or less, and even more preferably 60% by mass or less, based on the total mass of the stretched porous film. By setting the content of the inorganic filler in the stretched porous film within the above range, the moisture permeability and tear strength of the stretched porous film can be more effectively increased.
[0044] The inorganic filler may be one of the above inorganic fillers, or may be a mixture of two or more inorganic fillers that differ in material, average particle size, surface treatment, etc. When the inorganic filler is composed of two or more types, the total amount is preferably within the above range.
[0045] (Other resins) The stretched porous film may contain other resins in addition to polybutylene adipate terephthalate. Examples of other resins include biodegradable resins other than polybutylene adipate terephthalate, such as biodegradable polyester resins such as polyhydroxyalkanoate (PHA), polycaprolactone, polybutylene succinate (PBS), polybutylene succinate adipate (PBSA), and polybutylene sebacate terephthalate (PBSeT), and biodegradable resins such as polylactic acid, polyvinyl alcohol, polyamide, and polyethylene glycol. These other resins may be used alone or in combination.
[0046] The stretched porous film may contain a resin other than the biodegradable resin described above, such as polyolefin resin, polystyrene resin, acrylic resin, polyvinyl chloride resin, polyvinylidene chloride resin, chlorinated polyethylene resin, polyester resin, polycarbonate resin, polyamide resin, ethylene-vinyl alcohol copolymer, ethylene-vinyl acetate copolymer, polymethylpentene resin, polyvinyl alcohol resin, cyclic olefin resin, polybutylene succinate resin, polyacrylonitrile resin, polyethylene oxide resin, cellulose resin, etc. Examples of the other resins include polyimide resins, polyurethane resins, polyphenylene sulfide resins, polyphenylene ether resins, polyvinyl acetal resins, polybutadiene resins, polybutene resins, polyamideimide resins, polyamide bismaleimide resins, polyarylate resins, polyetherimide resins, polyetheretherketone resins, polyetherketone resins, polyethersulfone resins, polyketone resins, polysulfone resins, aramid resins, fluorine resins, polyacetal resins, etc. One or more of these other resins may be used.
[0047] When the present stretched porous film contains other resins besides polybutylene adipate terephthalate, the content of the other resins is preferably 30% by mass or less, more preferably 20% by mass or less, even more preferably 15% by mass or less, and particularly preferably 10% by mass or less, based on the total mass of the stretched porous film. In a preferred embodiment, the present stretched porous film preferably contains only polybutylene adipate terephthalate as a constituent resin. This allows the film to exhibit excellent moisture permeability while enhancing biodegradability.
[0048] (optional ingredient) The stretched porous film may contain various additives as optional components. Examples of additives include plasticizers, lubricants, compatibilizers, processing aids, antioxidants, heat stabilizers, light stabilizers, UV absorbers, antiblocking agents, antifogging agents, matting agents, antibacterial agents, deodorants, antistatic agents, flame retardants, colorants, and pigments. Examples of plasticizers that can be used include low molecular weight polymers (oligomers) such as higher fatty acids, higher fatty acid esters, higher fatty acid amides, metal soaps, higher alcohols, petrolatum, paraffin wax, glycerin fatty acid esters, polyglycerin fatty acid esters, sorbitan fatty acid esters, propylene glycol fatty acid esters, castor oil, hydrogenated castor oil, hardened castor oil, dehydrated castor oil, aromatic esters, aromatic amides, polyesters, and the like. The content of additives is preferably 10% by mass or less, more preferably 5% by mass or less, based on the total mass of the stretched porous film. In this embodiment, the amount of plasticizer added may be 1% by mass or less, or 0.1% by mass or less, or the film may be substantially free of plasticizer. The stretched porous film can exhibit high flexibility even without the inclusion of a plasticizer.
[0049] (Method of manufacturing the stretched porous film) The method for producing the stretched porous film preferably includes, for example, a step of mixing polybutylene adipate terephthalate with an inorganic filler to obtain a resin composition, a step of forming the resin composition into a sheet to obtain a sheet, and a step of stretching the sheet. The step of stretching the sheet preferably includes a step of stretching the sheet in at least one axial direction. The stretched porous film obtained by the above production steps has a breaking elongation in the TD direction of 50% or more.
[0050] The stretched porous film may be either planar or tubular, but is preferably planar from the viewpoints of productivity (several pieces can be produced in the width direction of the raw sheet) and printing on the inner surface. The method for producing a planar film preferably includes, for example, a step of melting a resin composition using an extruder, extruding the resin composition into a film shape from a die, and cooling and solidifying the film with a cooling roll, air cooling, or water cooling to obtain an unstretched film, and a step of stretching the unstretched film in at least one axial direction to obtain a stretched porous film.
[0051] The step of obtaining the resin composition preferably includes a step of mixing the resin composition containing polybutylene adipate terephthalate and an inorganic filler, followed by melt-kneading. Specifically, it is preferable to mix the resin composition for an appropriate time using a mixer such as a tumbler mixer, a mixing roll, a Banbury mixer, a ribbon blender, or a super mixer, and then uniformly disperse the resin composition using an extruder such as a counter-rotating twin-screw extruder or a co-rotating twin-screw extruder.
[0052] In the process of obtaining a sheet (unstretched sheet), it is preferable to connect a die such as a T-die or a round die to the tip of an extruder and form the obtained resin composition into a film. Alternatively, a strand die may be connected to the tip of a kneader, and the resin composition may be pelletized once by a method such as strand cutting or die cutting. The pellets obtained (along with an additional composition in some cases) may then be introduced into a single-screw extruder or the like, and a die such as a T-die or a round die may be connected to the tip of the extruder to form the resin composition into a film. When forming the resin composition into a film, it is preferable to employ a film forming method such as inflation molding, tubular molding, or T-die molding. The extrusion temperature is preferably about 140 to 250°C.
[0053] In the process of stretching the sheet, the unstretched film is stretched at least uniaxially. For example, the resin is melted using an extruder, extruded from a T-die or a round die, cooled and solidified with a cooling roll, and stretched at least uniaxially by roll stretching in the MD direction (longitudinal direction) or tenter stretching in the transverse direction (perpendicular to the flow direction of the film, TD). Among them, the process of obtaining a stretched porous film preferably includes a process of uniaxially stretching in the MD direction (longitudinal direction), and this stretched porous film is preferably a uniaxially stretched porous film. The process of uniaxially stretching in the MD direction (longitudinal direction) may include a process of stretching two or more times in the same direction. The stretching temperature in this case is preferably 20 to 100°C, more preferably 30 to 90°C. The stretching ratio is preferably 2.5 to 6.0 times, more preferably 3.0 to 5.5 times. By setting the stretching ratio to the lower limit or more, a stretched porous film having excellent moisture permeability and excellent appearance due to uniform stretching can be obtained. On the other hand, by setting the stretching ratio to the upper limit or less, the breaking elongation of the film can be increased.
[0054] If necessary, the film may be subjected to a heat treatment or relaxation treatment at a temperature of 30°C or more and 110°C or less after stretching. When stretching is performed by roll stretching, the stretched film can be subjected to a heat treatment by contacting it with a heated roll (anneal roll) between the stretching step and the winding step. Alternatively, the film can be heated by the anneal roll while the speed of the next roll to be contacted is made slower than the anneal roll speed to perform a relaxation treatment. These heat treatments and relaxation treatments can also be performed in a separate step after stretching the unstretched film and winding up the stretched porous film.
[0055] The method for producing the present stretched porous film may, if necessary, include a step of performing a surface treatment or surface processing such as slitting, corona treatment, printing, application of an adhesive, coating, deposition, etc. The present stretched porous film may, for example, be printed, or may be a film having a printed layer.
[0056] (Application) The present stretched porous film can be suitably used in a wide range of applications, such as packaging materials for liquids, powders, and solids for various foods, medicines, and miscellaneous goods, agricultural materials, and construction materials, particularly in disposable applications. Specific applications include, for example, agricultural mulch films, tunnel films, greenhouse films, sunshades, weed control sheets, ridge sheets, germination sheets, forestry fumigation sheets, binding tapes containing flat yarns, backsheets for diapers and sanitary products, packaging sheets, hand warmer sheets, shopping bags, plastic bags, garbage bags, draining bags, compost bags, etc. Among these, the present stretched porous film is preferably used as a backsheet for diapers, sanitary products, etc., since it has excellent moisture permeability.
[0057] The present embodiment may relate to a sanitary product having the above-mentioned stretched porous film. Examples of the sanitary product include absorbent articles (diapers, sanitary products, etc.). EXAMPLES
[0058] The features of the present invention will be described in more detail below with reference to examples and comparative examples. The materials, amounts used, ratios, processing contents, processing procedures, etc. shown in the following examples can be appropriately changed without departing from the spirit of the present invention. Therefore, the scope of the present invention should not be interpreted as being limited by the specific examples shown below.
[0059] <Thickness> The thickness of the film was measured using a stand-type constant pressure thickness measuring instrument in accordance with JIS K7130:1999, and the average of 36 measured values was calculated.
[0060] <Breaking elongation / tensile strength> In accordance with JIS K7127:1999, samples were cut to a length of 100 mm and a width of 10 mm in the measurement direction, and the breaking elongation and tensile strength were measured using a tensile tester under conditions of 23°C, 50% relative humidity, a tensile speed of 200 m / min, and a chuck distance of 20 mm, and the average of the measured values for three samples was calculated.
[0061] <Tear strength> In accordance with JIS K7128-1:1998, a sample was cut to a length of 100 mm and a width of 25 mm in the measurement direction, a 25 mm notch was made in the center of the width, and the tear strength was measured using a tensile tester under conditions of 23°C, relative humidity 50%, a tensile speed of 200 m / min, and a chuck distance of 25 mm, and the average of the measured values for three samples was calculated.
[0062] <Moisture permeability (20μm equivalent)> In accordance with JIS Z0208:1976, a measuring cup (inner diameter 60 mm, inner surface area 28.27 × 10 -4 m 2 The measuring cup was placed in a constant temperature and humidity environment of 40°C and 90% relative humidity, and the moisture permeability (g / m2) was calculated from the increase in the mass of the measuring cup after 24 hours. 2 After calculating the average of the three measured values, the moisture permeability per 20 μm of film thickness (moisture permeability converted into a film thickness of 20 μm) was calculated using the following formula. Moisture permeability of 20 μm thickness = Moisture permeability (measured value) × sample thickness (μm) / 20 (μm)
[0063] <Biodegradability evaluation> In accordance with JIS K6954:2008, samples cut into 25mm x 25mm squares were placed in a composting container containing inoculum derived from chicken manure. The composting container was then placed in a thermostatic chamber at 58°C and a relative humidity of 90%, and the samples were taken out three days after the start of the test and their mass was measured. The value of sample mass (3 days after the start of the test) / sample mass (before the test) was calculated and evaluated according to the following criteria. A (pass): less than 0.95 B (fail): 0.95 or higher
[0064] <Polybutylene adipate terephthalate (A)> A-1: BASF "F Blend C1200" (density 1.270g / cm 3 , MFR 3.8g / 10min, melting point: 116°C, structural units derived from terephthalic acid in 100 mol% of structural units derived from dicarboxylic acid: 48.1 mol%, structural units derived from adipic acid: 51.9 mol%, weight average molecular weight: 150,000, Mw / Mn: 2.4)
[0065] <Inorganic filler (B)> B-1: Calcium carbonate "Lighton BS-0" manufactured by Bihoku Powder Industry Co., Ltd. (average particle size 1.0 μm, fatty acid surface treatment product) B-2: Calcium carbonate "CSK-5" manufactured by Kalfin Co., Ltd. (average particle size 1.5 μm, fatty acid surface treatment product) B-3: Calcium carbonate "Ryton 26A" (average particle size 0.85 μm, fatty acid surface treatment product) manufactured by Bihoku Funka Kogyo Co., Ltd. B-4: Bihoku Powder Industry Co., Ltd., calcium carbonate "Lighton BK" (average particle size 0.85 μm, polyethylene glycol surface treatment product)
[0066] <Polyethylene resin (C)> C-1: Linear low-density polyethylene "Novatec LL UF230" (density 0.921 g / cm3 , MFR 1.0g / 10min, melting point 121℃) C-2: Linear low-density polyethylene "Novatec LL UF961" (density 0.935 g / cm 3 , MFR 5.0g / 10min, melting point 127℃) C-3: Branched low-density polyethylene "Novatec LD LF441" (density 0.918 g / cm 3 , MFR2.3g / 10min, melting point 113℃)
[0067] <Polypropylene resin (D)> D-1: Polypropylene "Novatec PP SA03" (density 0.900g / cm 3 , MFR 30g / 10min, melting point 165℃)
[0068] <Plasticizer (E)> E-1: Hydrogenated castor oil "HCO-P3" manufactured by KF Trading Co., Ltd.
[0069] <Antioxidants (F)> F-1: Antioxidant "Irganox B225" manufactured by BASF Japan
[0070] <Example 1> After weighing the raw materials in the composition ratio shown in Table 1, they were put into a Henschel mixer and mixed and dispersed for 5 minutes. Next, the materials were melt-kneaded at a set temperature of 200°C using a co-rotating twin-screw extruder. The resin composition was extruded through a T-die connected to the tip of the co-rotating twin-screw extruder, taken up by a casting roll set at 35°C, and cooled and solidified to obtain an unstretched film with a thickness of 59 μm. The unstretched film obtained was then stretched 3.5 times in the machine direction at a temperature of 63°C using a roll-type stretching machine to obtain a stretched porous film.
[0071] <Examples 2 and 3> A stretched porous film roll was obtained in the same manner as in Example 1, except that the stretching ratio was changed.
[0072] <Example 4> An unstretched film having a thickness of 65 μm was obtained by the same method as in Example 1, except that the raw materials were changed to the composition ratio shown in Table 1. The obtained unstretched film was stretched 3.5 times in the machine direction at a temperature of 63° C. using a roll-type stretching machine to obtain a stretched porous film.
[0073] <Example 5> A stretched porous film roll was obtained in the same manner as in Example 4, except that the stretching ratio was changed.
[0074] <Example 6> An unstretched film having a thickness of 61 μm was obtained by the same method as in Example 1, except that the raw materials were changed to the composition ratio shown in Table 1. The obtained unstretched film was stretched 5 times in the machine direction at a temperature of 63° C. using a roll-type stretching machine to obtain a stretched porous film.
[0075] <Example 7> A stretched porous film roll was obtained in the same manner as in Example 6, except that the stretching ratio was changed.
[0076] <Example 8> An unstretched film having a thickness of 65 μm was obtained by the same method as in Example 1, except that the raw materials were changed to the composition ratio shown in Table 1. The obtained unstretched film was stretched 4.5 times in the machine direction at a temperature of 63° C. using a roll-type stretching machine to obtain a stretched porous film.
[0077] <Comparative Example 1> The raw materials were weighed in the composition ratio shown in Table 1, then charged into a Henschel mixer, mixed and dispersed for 5 minutes, and then melt-kneaded at a set temperature of 220°C using a co-rotating twin-screw extruder. The resin composition was extruded through a T-die connected to the tip of the co-rotating twin-screw extruder, taken up by a casting roll set at 35°C, and cooled and solidified to obtain an unstretched film with a thickness of 71 μm. The unstretched film obtained was then stretched 3 times in the machine direction at a temperature of 110°C using a roll-type stretching machine to obtain a stretched porous film.
[0078] <Comparative Example 2> A stretched porous film roll was obtained in the same manner as in Comparative Example 1, except that the stretching ratio was changed.
[0079] [Table 1]
[0080] The examples exhibited superior moisture permeability and tear strength compared to the comparative examples. The stretched porous films obtained in the examples also exhibited superior biodegradability.
Claims
1. A stretched porous film comprising polybutylene adipate terephthalate and an inorganic filler, and having a breaking elongation in the TD direction of 50% or more.
2. 2. The stretched porous film according to claim 1, wherein the breaking elongation in the TD direction is 100% or more and 800% or less.
3. 2. The stretched porous film according to claim 1, wherein the breaking elongation in the TD direction is greater than the breaking elongation in the MD direction.
4. 2. The stretched porous film according to claim 1, wherein the breaking elongation in the TD direction is P and the breaking elongation in the MD direction is Q, and the value of P / Q is 1.2 or more.
5. 2. The stretched porous film according to claim 1, having a tear strength in the MD direction of 0.5 N / mm or more.
6. 2. The stretched porous film according to claim 1, having a tear strength in the TD direction of 5.0 N / mm or more.
7. 2. The stretched porous film according to claim 1, having a tensile strength in the MD direction of 10.0 MPa or more.
8. 2. The stretched porous film according to claim 1, having a tensile strength in the TD direction of 1.0 MPa or more.
9. The stretched porous film according to claim 1, wherein the weight average molecular weight (Mw) of the polybutylene adipate terephthalate is 50,000 to 400,000.
10. The stretched porous film according to claim 1, wherein the molecular weight distribution (Mw / Mn) of the polybutylene adipate terephthalate is 1.5 to 5.
0.
11. The stretched porous film according to claim 1, wherein the melting point of the polybutylene adipate terephthalate is 105 to 130°C.
12. The stretched porous film according to claim 1, wherein the constituent units derived from terephthalic acid are 40 to 60 mol% and the constituent units derived from adipic acid are 40 to 60 mol% in 100 mol% of the constituent units derived from dicarboxylic acids constituting the polybutylene adipate terephthalate.
13. The stretched porous film according to claim 1, wherein the inorganic filler has an average particle size of 0.1 to 10 μm.
14. 2. The stretched porous film according to claim 1, wherein the inorganic filler is calcium carbonate.
15. 2. The stretched porous film according to claim 1, having a thickness of 10 to 150 μm.
16. Moisture permeability of 1000 to 15000 g / m2 based on a film thickness of 20 μm 2 The stretched porous film according to claim 1, wherein the stretching time is 24 hours.
17. A roll obtained by rolling up the stretched porous film according to any one of claims 1 to 16.
18. A sanitary product comprising the stretched porous film according to any one of claims 1 to 16.
19. A step of mixing polybutylene adipate terephthalate and an inorganic filler to obtain a resin composition; forming the resin composition into a sheet to obtain a sheet; A method for producing a stretched porous film, comprising the steps of: stretching the sheet; The method for producing a stretched porous film, wherein the stretched porous film has a breaking elongation in a TD direction of 50% or more.
Citation Information
Patent Citations
Polyethylene porous film
JP2007161787A
Porous film and manufacturing method therefor
JP2015083661A
film
WO2014156952A1