Polycarbonate resin and molded product
By adjusting the Hansen's solubility parameters and oxygen-to-carbon atom ratio of dihydroxy compounds in polycarbonate resin, the chemical resistance is enhanced, addressing the limitations of conventional polycarbonate resins in applications like automobile interiors and panels.
Patent Information
- Application Number
- JP2024037449
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2023-03-30
- Filing Date
- 2024-03-11
- Publication Date
- 2024-10-11
AI Technical Summary
Conventional polycarbonate resins lack sufficient chemical resistance, limiting their application in areas such as automobile interior materials and panels.
The polycarbonate resin is formulated with dihydroxy compounds whose Hansen's solubility parameters (δD, δP, δH) satisfy a specific relationship (21.4MPa ≤ √(δD²+δH²+δP²) ≤ 30MPa) and an oxygen-to-carbon atom ratio of 0.54 to 1.50, incorporating aliphatic or alicyclic dihydroxy compounds, enhancing chemical resistance.
The formulation significantly improves the chemical resistance of the polycarbonate resin, making it suitable for applications requiring durability against everyday chemicals.
Smart Images

Figure 2024144207000001 
Figure 2024144207000002 
Figure 2024144207000003
Abstract
Description
[Technical field]
[0001] The present invention relates to a polycarbonate resin and a molded article. [Background technology]
[0002] Polycarbonate resin has excellent heat resistance, transparency, mechanical strength, etc., and is widely used as an engineering plastic in electrical and electronic parts, automotive parts, optical recording media, lenses, panels, etc. However, its chemical resistance is not sufficient, and it will turn white when exposed to everyday items such as sunscreen, oils, etc.
[0003] Patent Document 1 discusses aromatic polycarbonate resins having excellent chemical resistance, and Patent Document 2 discusses aliphatic polycarbonate resins having excellent chemical resistance. [Prior art documents] [Patent documents]
[0004] [Patent Document 1] JP 6-145329 [Patent Document 2] Patent Publication No. 2022-150358 Summary of the Invention [Problem to be solved by the invention]
[0005] However, the above-mentioned conventional polycarbonate resins do not have sufficient chemical resistance, and further improvement is required for applications such as automobile interior materials, home appliances, panels, etc.
[0006] SUMMARY OF THE PRESENT EMBODIMENT An object of the present invention is to provide a polycarbonate resin having improved chemical resistance.
[0007] As a result of extensive research aimed at solving the above-mentioned problems, the present inventors have found that the above-mentioned problems can be solved when the three components of the Hansen solubility parameters of dihydroxy compounds, which are monomers constituting polycarbonate resins, satisfy a specific relationship, and have arrived at the present invention, which is described below.
[0008] That is, the gist of the present invention resides in the following [1] to [6]. [1] A polycarbonate resin in which the three components (δD, δP, δH) of the Hansen solubility parameters calculated by the COSMO-RS method for the dihydroxy compound, which is a monomer that constitutes the polycarbonate resin, satisfy the following formula (1). 21.4MPa 0.5 ≦Average molar composition ratio of the dihydroxy compound √(δD^2+δH^2+δP^2)≦30MPa 0.5 (1)
[0009] [2] The polycarbonate resin according to [1], wherein the average molar composition ratio obtained by dividing the number of oxygen atoms of the dihydroxy compound by the number of carbon atoms of the dihydroxy compound is 0.54 or more and 1.50 or less. [3] The polycarbonate resin according to [1] or [2], wherein the dihydroxy compound includes an aliphatic dihydroxy compound or an alicyclic dihydroxy compound.
[0010] [4] The polycarbonate resin according to any one of [1] to [3], wherein the polycarbonate resin has a glass transition temperature of 60° C. or higher. [5] A molded article obtained by molding the polycarbonate resin according to any one of [1] to [4]. [6] The molded article according to [5], wherein the molded article is a film. Effect of the Invention
[0011] According to the present invention, by making the three components of the Hansen solubility parameters of the dihydroxy compound, which is the monomer constituting the polycarbonate resin, have a predetermined relationship, it is possible to improve the chemical resistance of the polycarbonate resin. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0012] The present invention will be described in detail below, but the present invention is not limited to the following description, and can be modified in any manner without departing from the gist of the present invention. In this specification, when an expression is used with "XX to XX" followed by a numerical value or a physical property value, this means "greater than or equal to XX and less than or equal to XX."
[0013] The term "structural unit" refers to a partial structure constituting a resin, and a specific partial structure contained in a repeating structural unit. For example, it refers to a partial structure sandwiched between adjacent linking groups in a resin, or a partial structure sandwiched between a polymerizable reactive group present at the end of a polymer and a linking group adjacent to the polymerizable reactive group. More specifically, in the case of a copolymerized polycarbonate resin, a carbonyl group is a linking group, and a partial structure sandwiched between adjacent carbonyl groups, or a structural portion sandwiched between a terminal polymerizable functional group and adjacent carbonyl groups, is called a structural unit. In this specification, the mass ratio of each structural unit in the copolymeric polycarbonate resin is calculated assuming that the total mass of all structural units and linking groups is 100 mass %.
[0014] The following describes in detail an embodiment of the present invention. The description of the components described below is an example (representative example) of an embodiment of the present invention, and the present invention is not limited to the following content as long as it does not exceed the gist of the present invention.
[0015] <Polycarbonate resin> (Hansen solubility parameters of dihydroxy compounds) In the polycarbonate resin of the present invention, the three components (ΔD, ΔP, ΔH) of the Hansen solubility parameters of the dihydroxy compound, which is a monomer constituting the polycarbonate resin, calculated by the COSMO-RS method satisfy the following formula (1).
[0016] 21.4MPa 0.5≦Average molar composition ratio of the dihydroxy compound √(δD^2+δH^2+δP^2)≦30MPa 0.5 (1) In the present invention, the "average composition molar ratio of √(ΔD^2+ΔH^2+ΔP^2) of dihydroxy compounds" may be referred to as the chemical resistance index (R).
[0017] The Hansen solubility parameter (HSP) is a value used to predict the solubility of a substance and is composed of the following three parameters: δD: Energy due to intermolecular dispersion forces δP: Energy due to intermolecular dipole interactions δH: Energy due to hydrogen bonds between molecules
[0018] The inventors have discovered that for dihydroxy compounds, which are monomers that constitute polycarbonate resins, the square root of the sum of the squares of the three parameters mentioned above, i.e., √(δD^2+δH^2+δP^2), can be an indicator of the chemical resistance of polycarbonate resins.
[0019] Furthermore, it was found that in the case of copolymer polycarbonate resins composed of multiple types of dihydroxy compounds, the average composition molar ratio of the above value (√(δD^2+δH^2+δP^2)) can be an indicator of the chemical resistance of the copolymer polycarbonate resin.
[0020] The Hansen solubility parameters (HSP) and √(δD^2+δH^2+δP^2) values of preferred dihydroxy compounds are summarized in Table 1.
[0021] [Table 1]
[0022] For example, in Example 1 shown below, an isosorbide-based polycarbonate (A-3) is used as the polycarbonate resin, which is a copolymer polycarbonate containing ISB and CHDM in a molar composition ratio of 0.9 / 0.1 (ISB / CHDM). Therefore, for the isosorbide-based polycarbonate (A-3), the value of formula (1) is 22.64 x 0.9 + 18.66 x 0.1 = 22.24.
[0023] The Hansen solubility parameter (HSP) mentioned above is derived by the COSMO-RS method, which determines the electrostatic interactions of molecules. COSMO stands for Conductor-like Screening Model, and is a simulation method that uses a molecular model in a conductor to approximate the molecular state in a solution, and determines the three-dimensional structure and surface charge density of the molecules in the solution by quantum chemical calculations.
[0024] In addition, the √(δD^2+δH^2+δP^2) (chemical resistance index (R)) of the dihydroxy compound is set to 21.8 MPa from the viewpoint of improving the chemical resistance of the resulting polycarbonate resin. 0.5 More than 30MPa 0.5- The following is preferable: 22.0MPa 0.5 More than 30MPa 0.5- Less than 22.2MPa is more preferable. 0.5 More than 30MPa 0.5- The following is even more preferable. δD, δH, and δP used in the chemical resistance index (R) are indices that indicate the polarization of a compound, and the chemical resistance index (R) is a parameter that indicates the interaction between the resin and the compound. When the chemical resistance index (R) satisfies the above range, the interaction with chemicals is reduced, and as a result, excellent chemical resistance is exhibited. In order to satisfy this parameter, it is advisable to use a dihydroxy compound in which δD, δH, and δP are each large, that is, the polarization is large.
[0025] (Number of O atoms in dihydroxy compounds / number of C atoms) The present inventors further found that the value obtained by dividing the number of oxygen atoms of a dihydroxy compound constituting a polycarbonate resin by the number of carbon atoms of the dihydroxy compound can be an index of the chemical resistance of the polycarbonate resin.
[0026] Furthermore, it was found that in the case of a copolymer polycarbonate resin composed of multiple types of dihydroxy compounds, the average composition molar ratio of the above value (number of O atoms / number of C atoms) can be an indicator of the chemical resistance of the copolymer polycarbonate resin. In the present invention, the average composition molar ratio of (the number of O atoms / the number of C atoms) of a dihydroxy compound may be referred to as the oxygen atom ratio (O).
[0027] Here, the above values (number of O atoms / number of C atoms) of dihydroxy compounds that are considered to be preferable are summarized in Table 2.
[0028] [Table 2]
[0029] For example, in Example 1 shown below, an isosorbide-based polycarbonate (A-3) is used as the polycarbonate resin, which is a copolymer polycarbonate containing ISB and CHDM in a molar composition ratio of 0.9 / 0.1 (ISB / CHDM). Therefore, in the isosorbide-based polycarbonate (A-3), the average composition molar ratio of the number of O atoms / the number of C atoms is 0.67×0.9+0.25×0.1=0.628.
[0030] The average composition molar ratio (oxygen atom ratio (O)) of the dihydroxy compound (number of O atoms / number of C atoms) is preferably 0.54 or more and 1.50 or less, more preferably 0.54 or more and 1.00 or less, from the viewpoint of the chemical resistance of the resulting polycarbonate resin and the polymerizability of the resin. When the oxygen atom ratio (O) is large, the polarization of the polymer increases, which reduces the interaction with chemicals and improves the chemical resistance. Furthermore, when the oxygen atom ratio (O) is within the above range, the stability of the resin during polymerization is improved, and a moldable resin can be obtained.
[0031] (Aliphatic dihydroxy compounds, alicyclic dihydroxy compounds) The present inventors further discovered that by using an aliphatic dihydroxy compound or an alicyclic dihydroxy compound as the dihydroxy compound, which is a monomer constituting the polycarbonate resin, the polarizability of the polymer is improved and the chemical resistance of the polycarbonate resin is further improved.
[0032] With respect to the total dihydroxy compound-derived structural units constituting the polycarbonate resin (100% by mass), the structural units derived from aliphatic dihydroxy compounds and alicyclic dihydroxy compounds preferably account for 50% by mass or more, more preferably 70% by mass or more, and even more preferably 90% by mass or more. It is particularly preferable that all of the dihydroxy compound-derived structural units are structural units derived from aliphatic dihydroxy compounds or alicyclic dihydroxy compounds. Examples of the aliphatic dihydroxy compound include, but are not limited to, the following dihydroxy compounds: ethylene glycol, 1,3-propanediol, 1,2-propanediol, 1,4-butanediol, 1,5-heptanediol, 1,6-hexanediol, 1,9-nonanediol, 1,10-decanediol, 1,12-dodecanediol, 1,3-dihydroxyacetone, 1,3-butanediol, 1,2-butanediol, neopentyl glycol, hexylene glycol, diethylene glycol, triethylene glycol, tetraethylene glycol, polyethylene glycol, polypropylene glycol, polytetramethylene glycol, and the like. Examples of the alicyclic dihydroxy compound include, but are not limited to, the following dihydroxy compounds: 1,2-cyclohexanedimethanol, 1,3-cyclohexanedimethanol, 1,4-cyclohexanedimethanol, tricyclodecane dimethanol, pentacyclopentadecane dimethanol, 2,6-decalin dimethanol, 1,5-decalin dimethanol, 2,3-decalin dimethanol, 2,3-norbornane dimethanol, 2,5-norbornane dimethanol, 1,3-adamantanedimethanol, dihydroxy compounds derived from terpene compounds such as limonene, isosorbide, 1, 2-Cyclohexanediol, 1,4-cyclohexanediol, 3,4-dihydroxytetrahydrofuran, 1,4-dioxane-2,3-diol, 1,3-adamantanediol, hydrogenated bisphenol A, 2,2,4,4-tetramethyl-1,3-cyclobutanediol, 3,9-bis(1,1-dimethyl-2-hydroxyethyl-2,4,8,10-tetraoxaspiro[5,5]undecane, 2,5-dihydroxy-9-oxabicyclo[4,2,1]nonane, and the like can be used. Among these, from the viewpoint of chemical resistance, 1,4-butanediol, 1,4-cyclohexanedimethanol, 3,4-dihydroxytetrahydrofuran, 1,4-dioxane-2,3-diol, 1,3-dihydroxyacetone, isosorbide, 3,9-bis(1,1-dimethyl-2-hydroxyethyl-2,4,8,10-tetraoxaspiro[5,5]undecane, and 2,5-dihydroxy-9-oxabicyclo[4,2,1]nonane are preferred, and from the viewpoint of compatibility with heat resistance, 1,4-butanediol, 1,4-cyclohexanedimethanol, isosorbide, and 2,5-dihydroxy-9-oxabicyclo[4,2,1]nonane are particularly preferred.
[0033] (carbonic acid diester) As a monomer other than the dihydroxy compound constituting the polycarbonate resin of the present invention, a carbonate diester represented by the following formula (2) can be used.
[0034] [ka]
[0035] (In formula (2), R 1 and R 2 each represents an aliphatic hydrocarbon group having 1 to 18 carbon atoms which may have a substituent, or an aromatic hydrocarbon group which may have a substituent, and R 1 and R 2 may be the same or different.)
[0036] R 1 and R 2 is preferably a substituted or unsubstituted aromatic hydrocarbon group, more preferably an unsubstituted aromatic hydrocarbon group. Examples of the substituent of the aliphatic hydrocarbon group include an ester group, an ether group, an amide group, and a halogen atom, and examples of the substituent of the aromatic hydrocarbon group include an alkyl group such as a methyl group or an ethyl group.
[0037] Examples of the carbonic acid diester represented by the formula (2) include diphenyl carbonate (hereinafter sometimes abbreviated as DPC), substituted diphenyl carbonate such as ditolyl carbonate, and dialkyl carbonate such as dimethyl carbonate, diethyl carbonate, and di-tert-butyl carbonate, with diphenyl carbonate and substituted diphenyl carbonate being preferred, and diphenyl carbonate being particularly preferred.
[0038] The carbonate diester may contain impurities such as chloride ions, and these impurities may inhibit the polymerization reaction or deteriorate the hue of the resulting resin. Therefore, it is preferable to use a diester that has been purified, as necessary, by distillation or the like.
[0039] (Glass transition temperature of polycarbonate resin) The lower limit of the glass transition temperature of the polycarbonate resin of the present invention is preferably 60° C. or higher, more preferably 80° C. or higher, even more preferably 110° C. or higher, particularly preferably 120° C. or higher, and the upper limit is preferably 180° C. or lower, more preferably 160° C. or lower. When the glass transition temperature is within the above range, the flowability during molding is increased, and even when the molded product has a complex shape, the polycarbonate resin easily reaches the end of the mold during molding, and the desired molded product can be obtained. In addition, the decrease in strength at the weld part can be suppressed.
[0040] <Production method of polycarbonate resin> The polycarbonate resin of the present invention can be produced by a commonly used polymerization method. For example, it can be produced by a solution polymerization method or an interfacial polymerization method using phosgene or a carboxylic acid halide, or a melt polymerization method in which a reaction is carried out without using a solvent. Among these production methods, it is preferable to produce the polycarbonate resin by the melt polymerization method, which is excellent in productivity and can reduce the environmental load because it does not use a solvent or a highly toxic compound.
[0041] In addition, when a solvent is used in polymerization, the solvent may remain in the resin, and the plasticizing effect of the solvent may lower the glass transition temperature of the resin, which may cause quality fluctuations in the processing step described below. In addition, halogen-based organic solvents such as methylene chloride are often used as solvents, but if the halogen-based solvent remains in the resin, it may cause corrosion of the metal part when a molded product using this resin comes into contact with metal. Since the resin obtained by the melt polymerization method does not contain a solvent, it is also advantageous for stabilizing the processing step and product quality.
[0042] When producing a copolymerized polycarbonate resin by melt polymerization, the above-mentioned one or more specific dihydroxy compounds, diphenyl carbonate, and a polymerization catalyst are mixed, and an ester exchange reaction (also called a polycondensation reaction) is carried out in a molten state, and the reaction rate is increased while removing the elimination components from the system. At the end of the polymerization, the reaction is carried out under high temperature and high vacuum conditions until the desired molecular weight is reached. When the reaction is completed, the molten resin is extracted from the reactor, and the polycarbonate resin of the present invention is obtained.
[0043] In the polycondensation reaction, the reaction rate and the molecular weight of the resulting resin can be controlled by strictly adjusting the molar ratio of all dihydroxy compounds and all diester compounds used in the reaction. In the case of a polycarbonate resin, the molar ratio of diphenyl carbonate to all dihydroxy compounds is preferably adjusted to 0.85 to 1.15, more preferably adjusted to 0.90 to 1.10, and particularly preferably adjusted to 0.95 to 1.05.
[0044] If the molar ratio is too far above or below the range, it is not possible to produce a resin with the desired molecular weight. If the molar ratio is too small, the number of hydroxyl group terminals in the produced resin increases, which may deteriorate the thermal stability of the resin. Furthermore, a large amount of unreacted dihydroxy compound remains in the resin, which may cause dirt on the molding machine and poor appearance of the molded product in the subsequent molding process. On the other hand, if the molar ratio is too large, the rate of transesterification reaction may decrease under the same conditions, or the amount of remaining carbonic acid diester in the produced resin may increase, and these remaining low molecular weight components may also cause problems in the molding process.
[0045] The melt polymerization method is usually carried out in a multi-stage process of two or more stages. The polycondensation reaction may be carried out in two or more stages using one polymerization reactor by sequentially changing the conditions, or may be carried out in two or more stages using two or more reactors by changing the conditions for each stage, but from the viewpoint of production efficiency, it is carried out using two or more, preferably three or more reactors. The polycondensation reaction may be carried out in a batch system, a continuous system, or a combination of a batch system and a continuous system, but from the viewpoint of production efficiency and stability of quality, a continuous system is preferred.
[0046] In polycondensation reactions, it is important to properly control the balance between temperature and pressure in the reaction system. If either the temperature or pressure is changed too quickly, unreacted monomers may be distilled out of the reaction system. As a result, the molar ratio of dihydroxy compounds and diphenyl carbonate may change, and a resin with the desired molecular weight may not be obtained.
[0047] In addition, the polymerization rate of the polycondensation reaction is controlled by the balance between the hydroxyl group terminal and the carbonate group terminal. Therefore, particularly when polymerization is performed in a continuous manner, if the balance of the terminal groups fluctuates due to the distillation of unreacted monomers, it becomes difficult to control the polymerization rate at a constant rate, and the molecular weight of the resulting resin may fluctuate greatly. Since the molecular weight of the resin is correlated with the melt viscosity, when the resulting resin is molded, the melt viscosity may fluctuate, leading to problems such as failure to obtain molded products of uniform dimensions.
[0048] Hereinafter, the melt polycondensation reaction process will be described separately into a stage in which a monomer is consumed to produce an oligomer (first-stage reaction) and a stage in which polymerization is allowed to proceed to a desired molecular weight to produce a polymer (second-stage or subsequent reaction).
[0049] (First stage reaction) Specifically, the following conditions can be adopted as reaction conditions in the first stage reaction. That is, the internal temperature of the polymerization reactor is set in the range of usually 130° C. or more, preferably 150° C. or more, more preferably 170° C. or more, and usually 250° C. or less, preferably 240° C. or less, more preferably 230° C. or less. The pressure of the polymerization reactor (hereinafter, pressure refers to absolute pressure) is set in the range of usually 70 kPa or less, preferably 50 kPa or less, more preferably 30 kPa or less, and usually 1 kPa or more, preferably 3 kPa or more, more preferably 5 kPa or more. The reaction time is set in the range of usually 0.1 hours or more, preferably 0.5 hours or more, and usually 10 hours or less, preferably 5 hours or less, more preferably 3 hours or less.
[0050] The first-stage reaction is carried out while the monohydroxy compound derived from the diester compound generated is distilled out of the reaction system. For example, when diphenyl carbonate is used as the carbonic acid diester, the monohydroxy compound distilled out of the reaction system in the first-stage reaction is phenol.
[0051] In the first stage reaction, the lower the reaction pressure, the more the polymerization reaction can be accelerated, but on the other hand, the more unreacted monomers are distilled off. In order to simultaneously suppress the distillation of unreacted monomers and accelerate the reaction by reducing the pressure, it is effective to use a reactor equipped with a reflux condenser. It is especially good to use a reflux condenser in the early stages of the reaction when there is a lot of unreacted monomers.
[0052] (Second or subsequent reaction) In the second or subsequent reaction, the pressure of the reaction system is gradually lowered from the pressure of the first stage, and the monohydroxy compound generated is removed from the reaction system, and the pressure of the reaction system is finally set to 5 kPa or less, preferably 3 kPa or less, more preferably 1 kPa or less. The internal temperature is usually set to 210°C or more, preferably 220°C or more, and usually 260°C or less, preferably 255°C or less. The reaction time is usually set to 0.1 hours or more, preferably 0.5 hours or more, more preferably 1 hour or more, and usually 10 hours or less, preferably 5 hours or less, more preferably 3 hours or less. In order to suppress side reactions such as coloration, thermal deterioration, and crosslinking and to obtain a resin with good hue, weather resistance, and thermal stability, the maximum internal temperature in all reaction stages is set to 260°C or less, preferably 255°C or less, and more preferably 250°C or less.
[0053] (Transesterification catalyst) The transesterification catalyst (hereinafter, sometimes simply referred to as "catalyst" or "polymerization catalyst") that can be used during polymerization can have a very large effect on the reaction rate and the color tone and thermal stability of the resin obtained by polycondensation. The catalyst is not limited as long as it satisfies the transparency, hue, heat resistance, thermal stability, and mechanical strength of the produced resin, and includes basic compounds such as metal compounds of Group 1 or Group 2 (hereinafter, simply referred to as "Group 1" and "Group 2") in the long-form periodic table, basic boron compounds, basic phosphorus compounds, basic ammonium compounds, and amine-based compounds. At least one metal compound selected from the group consisting of metals of Group 2 of the long-form periodic table and lithium is preferably used.
[0054] As the Group 1 metal compound, for example, the following compounds can be used, but it is also possible to use Group 1 metal compounds other than these. Sodium hydroxide, potassium hydroxide, lithium hydroxide, cesium hydroxide, sodium hydrogen carbonate, potassium hydrogen carbonate, lithium hydrogen carbonate, cesium hydrogen carbonate, sodium carbonate, potassium carbonate, lithium carbonate, cesium carbonate, sodium acetate, potassium acetate, lithium acetate, cesium acetate, sodium stearate, potassium stearate, lithium stearate, cesium stearate, sodium borohydride, potassium borohydride, lithium borohydride, cesium borohydride, sodium tetraphenylborate, tetraphenylborate potassium tetraphenylborate, lithium tetraphenylborate, cesium tetraphenylborate, sodium benzoate, potassium benzoate, lithium benzoate, cesium benzoate, disodium hydrogen phosphate, dipotassium hydrogen phosphate, dilithium hydrogen phosphate, dicesium hydrogen phosphate, disodium phenylphosphate, dipotassium phenylphosphate, dilithium phenylphosphate, dicesium phenylphosphate, sodium, potassium, lithium, cesium alcoholates, phenolates, disodium salts, dipotassium salts, dilithium salts, and dicesium salts of bisphenol A. Of these, it is preferable to use lithium compounds from the viewpoints of polymerization activity and the hue of the obtained resin.
[0055] As the Group 2 metal compound, for example, the following compounds can be used, but it is also possible to use Group 2 metal compounds other than these. Calcium hydroxide, barium hydroxide, magnesium hydroxide, strontium hydroxide, calcium bicarbonate, barium bicarbonate, magnesium bicarbonate, strontium bicarbonate, calcium carbonate, barium carbonate, magnesium carbonate, strontium carbonate, calcium acetate, barium acetate, magnesium acetate, strontium acetate, calcium stearate, barium stearate, magnesium stearate, strontium stearate. Of these, it is preferable to use magnesium compounds, calcium compounds, and barium compounds, and from the viewpoints of polymerization activity and the hue of the resulting resin, it is more preferable to use magnesium compounds and / or calcium compounds, and it is most preferable to use calcium compounds.
[0056] It is also possible to use, in combination with the Group 1 metal compound and / or Group 2 metal compound, a basic compound such as a basic boron compound, a basic phosphorus compound, a basic ammonium compound, or an amine compound as an auxiliary, but it is particularly preferable to use at least one metal compound selected from the group consisting of metals in Group 2 of the long form periodic table and lithium.
[0057] The amount of the polymerization catalyst used is usually 0.1 μmol to 300 μmol, and preferably 0.5 μmol to 100 μmol, in terms of the amount of metal, per mol of the total dihydroxy compounds used in the polymerization.
[0058] If the amount of catalyst is too small, the polymerization rate will be slow, and the polymerization temperature will have to be increased accordingly to obtain a resin with a desired molecular weight. This will increase the thermal history during the polymerization reaction, and the color and weather resistance of the resulting resin will likely deteriorate. In addition, unreacted raw materials may volatilize during the polymerization, causing the molar ratio of the dihydroxy compound and the carbonic acid diester compound to be disrupted, and the desired molecular weight may not be achieved. On the other hand, if the amount of polymerization catalyst used is too large, undesirable side reactions may occur, causing the color of the resulting resin to deteriorate, and causing coloring or decomposition of the resin during molding.
[0059] Among the group 1 metals, sodium, potassium, and cesium may adversely affect the color if contained in a large amount in the resin. These metals may be mixed not only from the catalyst used, but also from the raw materials and reaction equipment. Regardless of the source, the total amount of compounds of these metals in the resin is preferably 2 μmol or less, preferably 1 μmol or less, and more preferably 0.5 μmol or less per 1 mol of the total dihydroxy compounds.
[0060] After the polycarbonate resin is polymerized as described above, it can usually be cooled and solidified, and pelletized with a rotary cutter, etc. The pelletization method is not limited, but examples thereof include a method in which the polycarbonate resin is withdrawn in a molten state from the final polymerization reactor, cooled and solidified in the form of strands, and pelletized, a method in which the polycarbonate resin is supplied in a molten state from the final polymerization reactor to a single-screw or twin-screw extruder, melt-extruded, cooled and solidified, and pelletized, or a method in which the polycarbonate resin is withdrawn in a molten state from the final polymerization reactor, cooled and solidified in the form of strands, pelletized once, and then supplied to a single-screw or twin-screw extruder again, melt-extruded, cooled and solidified, and pelletized.
[0061] <Molded products> The polycarbonate resin of the present invention described above can be molded into a molded article such as a film. The polycarbonate resin constituting the molded product may be a blend of two or more polycarbonate resins, and the blended polycarbonate resin mixture may exhibit the above-mentioned predetermined chemical resistance index (R) and the above-mentioned predetermined oxygen atomic ratio (O). It is necessary that the polycarbonate resin mixture obtained by blending two or more polycarbonate resins satisfies the above-mentioned preferable ranges of the chemical resistance index (R) and the oxygen atomic ratio (O), but it is not essential that each polycarbonate resin constituting the mixture satisfies the preferable ranges of the chemical resistance index (R) and the oxygen atomic ratio (O).
[0062] For example, in the case of isosorbide-based polycarbonate (A-4) shown in Production Example 4 below, 10 parts of A-1 (R is 21.45), 10 parts of A-2 (R is 20.65), and 80 parts of A-3 (R is 22.24) are mixed, and in this case, R of the mixture is calculated as 21.45 x 0.1 + 20.65 x 0.1 + 22.24 x 0.8 = 22.00. The R of the mixture satisfies formula (1), but the R of A-2 does not satisfy formula (1).
[0063] In addition, in the case of the same isosorbide-based polycarbonate (A-4), 10 parts of A-1 (O is 0.542), 10 parts of A-2 (O is 0.458), and 80 parts of A-3 (O is 0.628) are mixed, in which case the O of the mixture is calculated as 0.542 x 0.1 + 0.458 x 0.1 + 0.628 x 0.8 = 0.602. The O of the mixture satisfies the preferred range of the present application, but the O of A-2 does not satisfy the preferred range of the present application.
[0064] The polycarbonate resin and resin mixture of the present invention can be molded into a film or sheet by a commonly known method such as extrusion molding, either as is or after being pelletized with a melt extruder. The film or sheet can be suitably used for applications requiring chemical resistance, such as automobile interior materials, home appliances, outdoor building materials, panels, etc.
[0065] (Various additives) The polycarbonate resin or polycarbonate resin mixture constituting the molded article of the present invention may be blended with additives such as antioxidants, heat stabilizers, neutralizing agents (catalyst deactivators), light stabilizers, release agents, colorants, antistatic agents, slip agents, lubricants, plasticizers, compatibilizers, flame retardants, fillers, etc. The additives may also be mixed using a tumbler, super mixer, floater, V-type blender, Nauta mixer, Banbury mixer, extruder, etc.
[0066] Heat stabilizer By adding a heat stabilizer, it is possible to prevent a decrease in molecular weight and deterioration in color during melt processing, etc. Examples of such heat stabilizers include commonly known hindered phenol-based heat stabilizers and / or phosphorus-based heat stabilizers.
[0067] Examples of the hindered phenol-based heat stabilizer include 2,6-di-tert-butylphenol, 2,4-di-tert-butylphenol, 2-tert-butyl-4-methoxyphenol, 2-tert-butyl-4,6-dimethylphenol, 2,6-di-tert-butyl-4-methylphenol, 2,6-di-tert-butyl-4-ethylphenol, 2,5-di-tert-butylhydroquinone, n-octadecyl-3-(3',5'-di-tert-butyl-4'-hydroxyphenyl)propionate, 2-tert-butyl-6-(3'-tert-butyl-5'-methylphenyl)propionate, and the like. 2,2'-methylene-bis-(4-methyl-6-tert-butylphenol), 2,2'-methylene-bis-(6-cyclohexyl-4-methylphenol), 2,2'-ethylidene-bis-(2,4-di-tert-butylphenol), tetrakis-[methylene-3-(3',5'-di-tert-butyl-4'-hydroxyphenyl)propionate]-methane, 1,3,5-trimethyl-2,4,6-tris-(3,5-di-tert-butyl-4-hydroxybenzyl)benzene, and the like can be used. Among these, it is preferable to use tetrakis-[methylene-3-(3',5'-di-tert-butyl-4'-hydroxyphenyl)propionate]-methane, n-octadecyl-3-(3',5'-di-tert-butyl-4'-hydroxyphenyl)propionate, and 1,3,5-trimethyl-2,4,6-tris-(3,5-di-tert-butyl-4-hydroxybenzyl)benzene.
[0068] As the phosphorus-based heat stabilizer, for example, phosphorous acid, phosphoric acid, phosphonous acid, phosphonic acid, and esters thereof shown below can be used, but it is also possible to use phosphorus-based heat stabilizers other than these compounds. For example, triphenyl phosphite, tris(nonylphenyl)phosphite, tris(2,4-di-tert-butylphenyl)phosphite, tridecyl phosphite, trioctyl phosphite, trioctadecyl phosphite, didecyl monophenyl phosphite, dioctyl monophenyl phosphite, diisopropyl monophenyl phosphite, monobutyl diphenyl phosphite, monodecyl diphenyl phosphite, monooctyl diphenyl phosphite, bis(2,6-di-tert-butyl-4-methylphenyl)pentaerythritol diphosphite, 2,2-methylenebis(4,6-di-tert-butylphenyl)octyl phosphite , bis(nonylphenyl)pentaerythritol diphosphite, bis(2,4-di-tert-butylphenyl)pentaerythritol diphosphite, distearyl pentaerythritol diphosphite, tributyl phosphate, triethyl phosphate, trimethyl phosphate, triphenyl phosphate, diphenyl monoorthoxenyl phosphate, dibutyl phosphate, dioctyl phosphate, diisopropyl phosphate, 4,4'-biphenylenediphosphinic acid tetrakis(2,4-di-tert-butylphenyl), benzene phosphonic acid dimethyl, benzene phosphonic acid diethyl, benzene phosphonic acid dipropyl, etc. These heat stabilizers may be used alone or in combination of two or more.
[0069] Such a heat stabilizer may be added to a resin using an extruder and kneaded. When a film is formed by a melt extrusion method, the heat stabilizer may be added to an extruder to form a film, or the heat stabilizer may be added to a resin in advance using an extruder and formed into pellets or the like.
[0070] The amount of these heat stabilizers is preferably 0.0001 parts by mass or more, more preferably 0.0005 parts by mass or more, and even more preferably 0.001 parts by mass or more, and is preferably 1 part by mass or less, more preferably 0.5 parts by mass or less, and even more preferably 0.2 parts by mass or less, based on 100 parts by mass of the polycarbonate resin or resin mixture that forms the molded body.
[0071] Catalyst deactivator In order to neutralize and deactivate the catalyst used in the polymerization reaction, an acidic compound can be added as a catalyst deactivator. This can improve color tone and thermal stability. As the acidic compound used as the catalyst deactivator, a compound having a carboxylic acid group, a phosphoric acid group, or a sulfonic acid group, or an ester thereof can be used, but it is particularly preferable to use a phosphorus-based compound containing a partial structure represented by the following formula (3) or (4).
[0072] [ka]
[0073] [ka]
[0074] Examples of the phosphorus-based compound represented by the formula (3) or (4) include phosphoric acid, phosphorous acid, phosphonic acids, hypophosphorous acid, polyphosphoric acid, phosphonic acid esters, acidic phosphate esters, etc. Among the above, phosphorous acid, phosphonic acids, and phosphonic acid esters are more effective in deactivating the catalyst and inhibiting coloration, and phosphorous acid is particularly preferred.
[0075] Examples of the phosphonic acids include phosphonic acid (phosphorous acid), methylphosphonic acid, ethylphosphonic acid, vinylphosphonic acid, decylphosphonic acid, phenylphosphonic acid, benzylphosphonic acid, aminomethylphosphonic acid, methylene diphosphonic acid, 1-hydroxyethane-1,1-diphosphonic acid, 4-methoxyphenylphosphonic acid, nitrilotris(methylenephosphonic acid), and propylphosphonic anhydride.
[0076] Examples of the phosphonate ester include dimethyl phosphonate, diethyl phosphonate, bis(2-ethylhexyl) phosphonate, dilauryl phosphonate, dioleyl phosphonate, diphenyl phosphonate, dibenzyl phosphonate, dimethyl methylphosphonate, diphenyl methylphosphonate, diethyl ethylphosphonate, diethyl benzylphosphonate, dimethyl phenylphosphonate, diethyl phenylphosphonate, dipropyl phenylphosphonate, diethyl (methoxymethyl)phosphonate, diethyl vinylphosphonate, hydroxymethyl diethyl p-methylbenzylphosphonate, diethylphosphonoacetic acid, ethyl diethylphosphonoacetate, tert-butyl diethylphosphonoacetate, diethyl (4-chlorobenzyl)phosphonate, diethyl cyanophosphonate, diethyl cyanomethylphosphonate, diethyl 3,5-di-tert-butyl-4-hydroxybenzylphosphonate, diethylphosphonoacetaldehyde diethyl acetal, and diethyl (methylthiomethyl)phosphonate.
[0077] Examples of the acidic phosphate ester include phosphate diesters such as dimethyl phosphate, diethyl phosphate, divinyl phosphate, dipropyl phosphate, dibutyl phosphate, bis(butoxyethyl) phosphate, bis(2-ethylhexyl) phosphate, diisotridecyl phosphate, dioleyl phosphate, distearyl phosphate, diphenyl phosphate, and dibenzyl phosphate, or mixtures of diesters and monoesters, diethyl chlorophosphate, and zinc stearyl phosphate.
[0078] These may be used alone or in any combination and ratio of two or more.
[0079] If the amount of the phosphorus-based compound is too small, the effect of catalyst deactivation and coloring suppression is insufficient, and if the amount is too large, the resin may be colored, and the resin may be easily colored, especially in a durability test under high temperature and high humidity. The amount of the phosphorus-based compound is added in an amount corresponding to the amount of catalyst used in the polymerization reaction. The amount of the phosphorus-based compound is preferably 0.5 times or more and 5 times or less in terms of the amount of phosphorus atoms, more preferably 0.7 times or more and 4 times or less in terms of the amount of phosphorus atoms, relative to 1 mol of the metal catalyst used in the polymerization reaction, and particularly preferably 0.8 times or more and 3 times or less in terms of the amount of phosphorus atoms.
[0080] Light stabilizer Examples of light stabilizers include 2-(2'-hydroxy-5'-tert-octylphenyl)benzotriazole, 2-(3-tert-butyl-5-methyl-2-hydroxyphenyl)-5-chlorobenzotriazole, 2-(5-methyl-2-hydroxyphenyl)benzotriazole, 2-[2-hydroxy-3,5-bis(α,α-dimethylbenzyl)phenyl]-2H-benzotriazole, 2,2'-methylenebis(4-cumyl-6-benzotriazolephenyl), and 2,2'-p-phenylenebis(1,3-benzoxazin-4-one).
[0081] These light stabilizers may be used alone or in combination of two or more. The blending amount of such light stabilizers is preferably 0.01 to 2 parts by mass, assuming that the polycarbonate resin or resin mixture constituting the molded body is 100 parts by mass. In addition, the polycarbonate resin or resin mixture constituting the molded body of the present invention may be blended with a bluing agent to eliminate yellowness. As the bluing agent, any agent that is used for polycarbonate resins can be used without any particular problems. In general, anthraquinone dyes are easily available and are preferable.
[0082] Specific examples of bluing agents include Solvent Violet 13 (CA. No. (Color Index No.) 60725), Solvent Violet 31 (CA. No. 68210), Solvent Violet 33 (CA. No. 60725), Solvent Blue 94 (CA. No. 61500), Solvent Violet 36 (CA. No. 68210), Solvent Blue 97 (Bayer's "Macrolex Violet RR") and Solvent Blue 45 (CA. No. 61110).
[0083] These bluing agents may be used alone or in combination of two or more. These bluing agents are usually used in an amount of 0.1×10 -4 ~2×10 -4 It is mixed in a ratio of parts by mass.
[0084] (Polymer alloy) The polycarbonate resin or resin mixture constituting the molded article of the present invention may be mixed with other resins than the polycarbonate resin to form a polymer alloy. For example, it can be kneaded with one or more of synthetic resins such as aromatic polyesters, aliphatic polyesters, polyamides, polystyrenes, polyolefins, acrylics, amorphous polyolefins, ABS, AS, and polycycloolefins, biodegradable resins such as polylactic acid and polybutylene succinate, and rubbers. The blending amount of the other resin is preferably more than 0 mass % and 50 mass % or less, based on the resin mixture constituting the molded body (100 mass %).
[0085] <Method of manufacturing molded body> (film) As a method for producing the molded article of the present invention, a method for producing a film will be described below. The method for forming a film using the polycarbonate resin of the present invention can be a casting method in which the polycarbonate resin is dissolved in a solvent and cast, and then the solvent is removed, or a melt film-forming method in which the resin is melted without using a solvent to form a film.Specific examples of the melt film-forming method include a melt extrusion method using a T-die, a calendar molding method, a heat press method, a co-extrusion method, a co-melting method, a multi-layer extrusion method, and an inflation molding method. The method for producing the unstretched film is not particularly limited, but since the casting method may cause problems due to residual solvent, a melt film-forming method is preferred, and in particular, a melt extrusion method using a T-die is preferred because of the ease of subsequent stretching treatment.
[0086] When forming an unstretched film by a melt casting method, the forming temperature is preferably 280° C. or less, more preferably 270° C. or less, and particularly preferably 265° C. or less. If the forming temperature is too high, defects due to the generation of foreign matter or bubbles in the obtained film may increase, or the film may become discolored.
[0087] However, if the molding temperature is too low, the melt viscosity of the resin becomes too high, making it difficult to mold the raw film and possibly making it difficult to produce an unstretched film with a uniform thickness, so the lower limit of the molding temperature is usually at least 200° C., preferably at least 210° C., and more preferably at least 220° C. Here, the molding temperature of the unstretched film means the temperature during molding in the melt film-forming method, and is usually the value measured by measuring the resin temperature at the die outlet from which the molten resin is extruded.
[0088] In order to remove foreign matter from the resin, a polymer filter may be attached after the extruder, and the resin may be filtered and then extruded through a die to form a film. In this case, the extruder, polymer filter, and die must be connected by piping to transport the molten resin, and it is preferable to arrange each piece of equipment so that the residence time is minimized in order to minimize thermal deterioration in the piping.
[0089] The thickness of the unstretched film may vary depending on the application, but is preferably 5 μm or more, more preferably 15 μm or more, and even more preferably 30 μm or more, and is preferably 450 μm or less, more preferably 300 μm or less, even more preferably 200 μm or less, and particularly preferably 160 μm or less.
[0090] Depending on the application, the unstretched film is required to have no thickness unevenness. The unstretched film preferably has a set thickness of ±3 μm or less, more preferably ±2 μm or less, and particularly preferably ±1 μm or less.
[0091] The unstretched film is preferably a long film, and the length of the long film in the longitudinal direction is preferably 500 m or more, more preferably 1000 m or more, and particularly preferably 1500 m or more. From the viewpoints of productivity and quality, it is preferable to perform continuous stretching when producing the film of the present invention.
[0092] In this specification, the term "long" means that the longitudinal dimension of the film is sufficiently larger than the width direction, and essentially means that the film can be wound in the longitudinal direction into a coil shape. More specifically, the longitudinal dimension of the film is 10 times or more larger than the width direction.
[0093] The film of the present invention can be a laminated film having a layer made of the polycarbonate resin of the present invention on the surface of a substrate film. As the substrate film, an acrylic substrate or a polyester substrate can be used in terms of transparency, optical properties, and formability.
[0094] The laminated film can be produced by attaching, for example, a multi-manifold T-die to the tip of the above-mentioned extruder and co-extruding the polycarbonate resin of the present invention and the resin constituting the substrate.
[0095] (Other molded products) The polycarbonate resin of the present invention can be molded into a molded article by a commonly known method such as injection molding, extrusion molding, or compression molding. EXAMPLES
[0096] Examples of polycarbonate resin and molded products (films) obtained by molding the resin are shown below, but the present invention is not limited to the following examples as long as the gist of the invention is not exceeded. The methods for measuring the various properties are as follows.
[0097] <Method of measuring each characteristic> (1) Film thickness The thickness of the films obtained in each of the Examples and Comparative Examples was measured using a film thickness meter (547-301A) manufactured by Mitutoyo Corporation.
[0098] (2) Glass transition temperature The glass transition temperature of each polycarbonate resin was determined from the transition point of the thermogram measured using a differential scanning calorimeter ("DSC7020" manufactured by Hitachi High-Technologies Corporation) in accordance with JIS K7121, in which 10 mg of a sample was heated from 0°C to 200°C at a heating rate of 10°C / min, held at 200°C for 1 minute, cooled to 0°C at a cooling rate of 10°C / min, and then heated again to 200°C at a heating rate of 10°C / min.
[0099] (3) Chemical resistance evaluation of film A sunscreen made by Johnson & Johnson (product name: Neutrogena SPF45) was applied at 1.5 g / 100 cm to the surface of the polycarbonate resin layer of the laminated film obtained in each Example and Comparative Example and to the surface of the press film. 2 The film (test piece) on which the sunscreen was applied was placed in a thermostatic chamber maintained at 80°C and left there for 24 hours. The test piece was then washed with water and air-dried, and the surface of the test piece was visually observed and evaluated according to the following criteria to evaluate chemical resistance.
[0100] Evaluation criteria ○: No change on the sample surface. ×: Sunscreen is stuck to the surface of the sample, or the surface that has come into contact with the sunscreen is cloudy, or traces of the sunscreen remain.
[0101] (4) Calculation of Hansen solubility parameters The Hansen solubility parameters (δD, δP, δH) of dihydroxy compounds, which are monomers constituting each polycarbonate resin, were calculated using the software "COSMOquick" (Dassault Systèmes). More specifically, the molecular state in solution was approximated using a molecular model in a conductor for various molecular structures in advance, and then the three-dimensional structure and surface charge density of the molecule in solution were determined by molecular orbital calculation using the database "COSMO Fragment Data Base" (Dassault Systèmes). From the surface charge density obtained for the structure of the target compound, the intermolecular interaction energy between the target compound in solution and 29 reference solvents with known Hansen solubility parameters was calculated, and the chemical potential of the molecular surface segment was obtained. Furthermore, the activity coefficient was calculated from the chemical potential using the COSMO-RS method. The Hansen solubility parameter of the compound was determined so that the error between the activity coefficient calculated from the difference between the Hansen solubility parameters of the compound and the solvent and the activity coefficient calculated using the COSMO-RS method was minimized.
[0102] (5) Calculation of chemical resistance index (R) The chemical resistance index was calculated from the Hansen solubility parameters according to the following formula. R = √((δD×δD)+(δP×δP)+(δH×δH)) The above-mentioned average composition molar ratio means that when there are multiple dihydroxy compounds that are monomers constituting the polycarbonate resin, √((δD×δD)+(δP×δP)+(δH×δH)) is calculated for each dihydroxy compound, and the molar ratio average of each calculated value is calculated.
[0103] (6) Oxygen atom ratio of dihydroxy compounds (O) The number of oxygen atoms in the dihydroxy compound, which is a monomer constituting each polycarbonate resin, was divided by the number of carbon atoms in the dihydroxy compound, and the average molar composition ratio of the divided value was taken as the oxygen atom ratio (O). Here, the average molar composition ratio is, when a polycarbonate resin is composed of a plurality of dihydroxy compounds, the average of the above-mentioned divided values for each dihydroxy compound is calculated by the composition ratio (unit: mol) of the dihydroxy compounds.
[0104] <Film production> (Production Example 1: Isosorbide-based polycarbonate (A-1)) In a polymerization reactor equipped with a stirring blade and a reflux condenser controlled at 100°C, isosorbide (ISB), 1,4-cyclohexanedimethanol (CHDM), diphenyl carbonate (DPC) purified by distillation to a chloride ion concentration of 10 ppb or less, and calcium acetate monohydrate were added in a molar ratio of ISB / CHDM / DPC / calcium acetate monohydrate = 0.7 / 0.3 / 1.00 / 1.3 x 10 -6 The contents were then charged to a temperature of 0.0005% by volume to 0.001% by volume, and the contents were thoroughly substituted with nitrogen (oxygen concentration: 0.0005% by volume to 0.001% by volume). The contents were then heated using a heat medium. When the internal temperature reached 100°C, stirring was started, and the contents were melted and homogenized while controlling the internal temperature to 100°C. After that, the temperature was raised, and the internal temperature reached 210°C in 40 minutes.
[0105] When the internal temperature reached 210°C, the temperature was controlled to be maintained at that temperature, and simultaneously, pressure reduction was started, and the pressure was reduced to 13.3 kPa (absolute pressure, the same applies below) 90 minutes after reaching 210°C, and this pressure was maintained for another 60 minutes. Phenol vapor by-produced during the polymerization reaction was led to a reflux condenser. The components condensed in the reflux condenser were returned to the polymerization reactor, and the uncondensed phenol vapor was subsequently led to a condenser using 45°C hot water as a refrigerant and collected.
[0106] The contents oligomerized in the above polymerization reactor were once restored to atmospheric pressure, and then transferred to another polymerization reactor equipped with a stirring blade and a reflux condenser controlled in the same manner as above, and heating and decompression were started, so that the internal temperature reached 220°C and the pressure reached 200 Pa in 60 minutes. Thereafter, the internal temperature was reduced to 228°C and the pressure to 133 Pa or less over 20 minutes, and the pressure was restored when a predetermined stirring power was reached, and a molten polycarbonate copolymer was obtained from the outlet of the polymerization reactor.
[0107] The molten polycarbonate copolymer was continuously fed to a twin-screw extruder equipped with three vents and a water injection device, and an antioxidant and a mold release agent were continuously added, and low molecular weight substances such as phenol were volatilized under reduced pressure at each vent provided in the twin-screw extruder, and then pelletized with a pelletizer to obtain an isosorbide-based polycarbonate (A-1). The glass transition temperature of the isosorbide-based polycarbonate (A-1) was 124°C.
[0108] (Production Example 2: Isosorbide-based polycarbonate (A-2)) In Production Example 1, the molar ratio of ISB / CHDM / DPC / calcium acetate monohydrate was 0.5 / 0.5 / 1.00 / 1.3×10 -6 An isosorbide-based polycarbonate (A-2) was obtained by carrying out the reaction under the same conditions as in Production Example 1, except that the above-mentioned reaction mixture was changed to the above. The glass transition temperature of the isosorbide-based polycarbonate (A-2) was 99°C.
[0109] (Production Example 3: Isosorbide-based polycarbonate (A-3)) In Production Example 1, the molar ratio of ISB / CHDM / DPC / calcium acetate monohydrate was 0.9 / 0.1 / 1.00 / 1.3×10 -6 An isosorbide-based polycarbonate (A-3) was obtained by carrying out the reaction under the same conditions as in Production Example 1, except that the above-mentioned reaction mixture was changed to the above. The glass transition temperature of the isosorbide-based polycarbonate (A-3) was 148°C.
[0110] (Production Example 4: Isosorbide-based polycarbonate (A-4)) 10 parts of A-1 obtained in Production Example 1, 10 parts of A-2 obtained in Production Example 2, 80 parts of A-3 obtained in Production Example 3, and 0.8 parts of a hindered phenol-based antioxidant (ADEKA Corporation, product name: Adeka STAB AO-60) were added and mixed using a Henschel mixer. Using a twin-screw extruder (Toshiba Machine Co., Ltd., product name: TEM-35B), the mixture was extruded into a strand shape at a cylinder temperature of 170 to 230°C while removing impurities with a filter, and then cut after cooling through a water bath to obtain an isosorbide-based polycarbonate (A-4). The glass transition temperature of the isosorbide-based polycarbonate (A-4) was 137°C.
[0111] (Production Example 5: Isosorbide-based polycarbonate (A-5)) An isosorbide-based polycarbonate (A-5) was obtained in the same manner as in Production Example 4, except that 85 parts of A-1 obtained in Production Example 1, 15 parts of A-2 obtained in Production Example 2, and 0.8 parts of a hindered phenol-based antioxidant (manufactured by ADEKA CORPORATION, product name: Adeka STAB AO-60) were added. The glass transition temperature of the isosorbide-based polycarbonate (A-5) was 112°C.
[0112] (Production Example 6: Isosorbide-based polycarbonate (A-6)) An isosorbide-based polycarbonate (A-6) was obtained in the same manner as in Production Example 4, except that 75 parts of A-1 obtained in Production Example 1 and 25 parts of A-2 obtained in Production Example 2 were added. The glass transition temperature of the isosorbide-based polycarbonate (A-6) was 109°C.
[0113] (Production Example 7: Acrylic Rubber-Containing Polymer (G)) It was prepared in the same manner as Preparation Example 1 of International Publication No. WO2019 / 244791.
[0114] (Production Example 8: Acrylic resin composition (B)) 75 parts of the acrylic rubber-containing polymer (G) obtained in Production Example 7, 25 parts of alkyl methacrylate-alkyl acrylate copolymer (manufactured by Mitsubishi Chemical Corporation; trade name: ACRYPET VH), 1.1 parts of a benzotriazole-based ultraviolet absorber (manufactured by ADEKA Corporation; trade name: Adeka STAB LA-31G), 0.2 parts of a hindered amine-based light stabilizer (manufactured by BASF Japan Ltd.; trade name: Chimassorb2020FDL), and 0.1 parts of a hindered phenol-based antioxidant (manufactured by BASF Japan Ltd.; trade name: Irganox1076) were added, and then mixed using a Henschel mixer. Using a twin-screw extruder (manufactured by Toshiba Machine Co., Ltd., trade name: TEM-35B), the mixture was extruded into a strand shape at a cylinder temperature of 170 to 230 ° C. while removing impurities with a filter, and then cut after cooling through a water tank to obtain an acrylic resin composition (B).
[0115] (Production Example 9: Isosorbide-based polycarbonate (A-7)) In a polymerization reactor equipped with an agitator and a reflux condenser, isosorbide (ISB), 2,5-dihydroxy-9-oxabicyclo[4,2,1]nonane (CODA), diphenyl carbonate (DPC) purified by distillation to a chloride ion concentration of 10 ppb or less, and calcium acetate monohydrate were added in a molar ratio of ISB / CODA / DPC / calcium acetate monohydrate = 0.9 / 0.1 / 1.00 / 1.0 x 10. -5The contents were charged so that the temperature was 150°C, and the contents were fully replaced with nitrogen. The contents were then heated with a heat medium. When the internal temperature reached 150°C, stirring was started, and the contents were melted and homogenized while controlling the internal temperature to 150°C. After that, the temperature was raised, and the internal temperature was raised to 220°C in 30 minutes. When the internal temperature reached 220°C, the temperature was controlled to be maintained at this temperature, and at the same time, pressure reduction was started, and the pressure was reduced to 13.3 kPa (absolute pressure, the same applies below) in 90 minutes after reaching 220°C, and this pressure was maintained for another 45 minutes. Phenol vapor by-produced during the polymerization reaction was led to a reflux condenser. The components condensed in the reflux condenser were returned to the polymerization reactor, and the uncondensed phenol vapor was led to a condenser and collected. Next, the temperature was raised, and the internal temperature was raised to 240°C in 15 minutes. The pressure was reduced to 200 Pa in 45 minutes after reaching 240°C. Thereafter, the pressure was reduced to 133 Pa or less, and when a predetermined stirring power was reached, the pressure was restored, and a molten isosorbide-based polycarbonate (A-7) was obtained from the outlet of the polymerization reactor. The glass transition temperature of the isosorbide-based polycarbonate (A-7) was 169°C.
[0116] (Production Example 10: Isosorbide-based polycarbonate (A-8)) In Production Example 9, the molar ratio of ISB / CODA / DPC / calcium acetate monohydrate was 0.7 / 0.3 / 1.00 / 2.0×10 -5 An isosorbide-based polycarbonate (A-8) was obtained by carrying out the reaction under the same conditions as in Production Example 9, except that the above-mentioned reaction mixture was changed to the following: The glass transition temperature of the isosorbide-based polycarbonate (A-8) was 171°C.
[0117] (Production Example 11: Isosorbide-based polycarbonate (A-9)) In Production Example 9, 1,4-butanediol (14BG) was used instead of 2,5-dihydroxy-9-oxabicyclo[4,2,1]nonane (CODA), and the molar ratio of ISB / 1,4-butanediol (14BG) / DPC / calcium acetate monohydrate was 0.7 / 0.30 / 1.06 / 5.0×10 -6The reaction was carried out under the same conditions as in Production Example 9, except that the upper limit of the polymerization temperature was changed to 220°C, to obtain an isosorbide-based polycarbonate (A-9). The glass transition temperature of the isosorbide-based polycarbonate (A-9) was 121°C.
[0118] (Example 1: Preparation of laminated film) The isosorbide-based polycarbonate (A-3) obtained in Production Example 3 was used as the resin constituting the polycarbonate resin layer, and the acrylic resin composition (B) obtained in Production Example 8 was used as the resin constituting the acrylic resin layer. These were dehumidified and dried at 85° C. for one day. Using a 30 mmφ non-vented screw extruder, the isosorbide-based polycarbonate (A-3) was plasticized at a cylinder temperature of 200 to 240°C, while using a 40 mmφ non-vented screw extruder, the acrylic resin composition (B) was plasticized at a cylinder temperature of 220 to 240°C. Next, a 75 μm thick laminated film (polycarbonate resin layer / acrylic resin layer) was produced using a 500 mm wide two-kind, two-layer multi-manifold T-die set at 245°C, with the acrylic resin layer side in contact with a mirror-cooled roll.
[0119] (Examples 2 to 3, Comparative Examples 1 to 3) A laminated film was produced under the same conditions as in Example 1, except that the resin constituting the polycarbonate resin layer was changed to an isosorbide-based polycarbonate shown in Table 1.
[0120] (Examples 4 to 6: Preparation of Press Films) The isosorbide-based polycarbonate shown in Table 1 was molded into a sheet of 7 cm x 7 cm x 0.1 mm thickness using a small press made by Imoto Manufacturing Co., Ltd. The pressing temperature was 200°C. Cooling was performed at 20°C using the same type of press.
[0121] [Table 3]
[0122] [Table 4]
[0123] In Examples 1 to 6, in which the polycarbonate resin or the mixture of polycarbonate resins constituting the polycarbonate resin layer of the obtained laminate film or the pressed film of polycarbonate resin satisfied formula (1), the chemical resistance was good. In contrast, in Comparative Examples 1 to 3, in which the polycarbonate resin or polycarbonate resin mixture constituting the polycarbonate resin layer or polycarbonate resin film of the obtained laminate film did not satisfy formula (1), the surface of the polycarbonate resin layer side of the laminate after water washing and air drying, which had come into contact with the sunscreen, was cloudy and had poor chemical resistance.
Claims
1. A polycarbonate resin, in which the three components (δD, δP, δH) of the Hansen solubility parameters calculated by the COSMO-RS method of a dihydroxy compound, which is a monomer constituting the polycarbonate resin, satisfy the following formula (1). 21.4MPa 0.5 ≦Average molar composition ratio of the dihydroxy compound √(δD^2+δH^2+δP^2)≦30 MPa 0.5 ...(1)
2. 2. The polycarbonate resin according to claim 1, wherein the average molar composition ratio obtained by dividing the number of oxygen atoms of the dihydroxy compound by the number of carbon atoms of the dihydroxy compound is 0.54 or more and 1.50 or less.
3. 3. The polycarbonate resin according to claim 1, wherein the dihydroxy compound comprises an aliphatic dihydroxy compound or an alicyclic dihydroxy compound.
4. The polycarbonate resin according to claim 1 or 2, wherein the polycarbonate resin has a glass transition temperature of 60° C. or higher.
5. A molded article obtained by molding the polycarbonate resin according to claim 1 or 2.
6. The molded article according to claim 5 , wherein the molded article is a film.
Citation Information
Patent Citations
Polycarbonate and its production, and aromatic diol and its production
JP1994145329A
Polycarbonate resin composition and molding
JP2022150358A