Polycarbonate-based resin extrusion foam particle, and extrusion foam particle molding and method for manufacturing molding

By adjusting the glass transition temperature of polycarbonate resin with ester compounds and using low-pressure extrusion foaming, the method addresses productivity and moldability issues, resulting in high-fusion and lightweight molded articles.

JP2024144223APending Publication Date: 2024-10-11KANEKA CORP
View PDF 3 Cites 0 Cited by

Patent Information

Application Number
JP2024041552
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Priority Date
2023-03-30
Filing Date
2024-03-15
Publication Date
2024-10-11

AI Technical Summary

Technical Problem

Existing methods for producing polycarbonate resin foam particles face low productivity due to high-pressure and long-time processes, and issues with uneven plasticizer application leading to inconsistent product quality and moldability.

Method used

Incorporating a specific range of ester compounds as plasticizers with polycarbonate resin to adjust the glass transition temperature (Tg) for steam molding, using a low-pressure extrusion foaming method to produce polycarbonate resin foam particles with a low open cell ratio and improved fusion properties.

Benefits of technology

The method achieves extruded polycarbonate resin foam particles with high fusion properties and excellent moldability, enabling efficient production of lightweight and high-strength molded articles.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024144223000001
    Figure 2024144223000001
Patent Text Reader

Abstract

To provide polycarbonate-based resin extrusion foam particles which have a fusion property and are excellent in moldability, and a method for producing the same.SOLUTION: Polycarbonate-based resin extrusion foam particles contain a polycarbonate-based resin, and an ester compound having a number average molecular weight of 1,000 or less as a plasticizer, and have an expansion ratio of 3 to 15 times, wherein the content of the ester compound is 0.1 to 4 pts.wt. with respect to 100 pts.wt. of the polycarbonate-based resin.SELECTED DRAWING: None
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to extruded polycarbonate resin foam beads and molded articles of the extruded foam beads, and to methods for producing the same. [Background technology]

[0002] Expanded molded articles obtained by molding expanded resin beads are characterized by their flexibility in shape, excellent cushioning properties, light weight, and excellent heat insulating properties, and polystyrene-based expanded resin bead molded articles, polypropylene-based expanded resin bead molded articles, etc. are already widely used on the market. On the other hand, there continues to be a demand in the market for resin foamed bead moldings with higher functionality and performance, making the development of new technologies necessary.

[0003] Among them, polycarbonate-based resins have many unique characteristics compared to other types of resins, such as good dimensional stability up to a relatively high temperature range based on a high glass transition point Tg, excellent weather resistance, and relatively easy flame retardancy, and are expected to be used in various applications as foamed molded products. From this perspective, foamed beads using polycarbonate-based resins as a base material have been proposed. For example, Patent Document 1 describes pre-expanded beads obtained by injecting carbon dioxide into polycarbonate-based resin particles to obtain expandable particles and heating them with steam, and further describes a foamed molded product obtained by injecting carbon dioxide again into the pre-expanded particles and then heat-molding them in a mold with heated steam. However, in the method described therein, a high-pressure and long-term injection process is required in the stage of obtaining expandable particles from polycarbonate-based resin particles and further in the stage of obtaining pre-expanded particles for molding, and there is a problem that productivity is extremely poor.

[0004] For example, Patent Document 2 describes a manufacturing method for obtaining polycarbonate resin extruded foam particles by extruding and foaming a polycarbonate resin exhibiting specific viscoelastic properties. The method described therein employs an extrusion foaming method, and is therefore more productive. However, this document merely describes that extruded foam particles with a bulk ratio of up to about 4 times obtained by the extrusion foaming method exhibit a secondary foaming property of more than 2 times, and the moldability of the obtained extruded foam particles is unclear.

[0005] Furthermore, for example, Patent Document 3 describes a method in which a specific plasticizer is applied to the surface of pre-expanded particles prior to heat molding in order to improve fusion between the pre-expanded particles obtained by a method similar to that of Patent Document 1. However, even in the methods described therein, a high-pressure and long-term pressing step is required in the step of obtaining expandable particles from polycarbonate resin particles, and further in the step of obtaining pre-expanded particles for molding, resulting in a problem of extremely poor productivity.

[0006] Furthermore, the method of applying a plasticizer to the surface of the pre-expanded particles in order to obtain a satisfactory fusion state in the molded product requires an additional step, which reduces productivity. In addition, the amount of plasticizer applied to the surface of each pre-expanded particle is likely to be uneven, making it difficult to stabilize the quality of the product. [Prior art documents] [Patent documents]

[0007] [Patent Document 1] Japanese Unexamined Patent Publication No. 6-100724 [Patent Document 2] Patent Publication No. 2021-54959 [Patent Document 3] JP 2016-160400 A Summary of the Invention [Problem to be solved by the invention]

[0008] The present invention has been made in consideration of the above problems. That is, according to the manufacturing method of the present invention, extruded polycarbonate resin foam beads having a low open cell ratio can be obtained by the extrusion foaming method having excellent productivity. In addition, the extruded polycarbonate resin foam beads of the present invention can be easily made into a molded product having excellent fusibility by the widely used steam molding method. [Means for solving the problem]

[0009] To overcome the above-mentioned problems, the present inventors focused on the glass transition temperature Tg of polycarbonate-based resins.

[0010] Polycarbonate resins that are widely used generally have a Tg of about 143 to 150°C. When heated, the resin changes from a glassy to a rubbery state at this temperature and softens as the temperature increases.

[0011] On the other hand, the steam pressure that can be utilized in molding machines commonly used for steam molding polypropylene-based resin foam particles and polystyrene-based resin foam particles is approximately 0.45 MPa, and the maximum temperature is approximately 150°C, which is not necessarily sufficient to soften polycarbonate-based resin to the point where it can be fused.

[0012] Therefore, the present inventors attempted to lower the Tg of the polycarbonate-based resin extruded foam particles by incorporating a plasticizer as part of the base material when extruding and foaming a polycarbonate-based resin to obtain extruded foam particles, thereby adjusting the Tg to a range suitable for steam molding.

[0013] As a result, the inventors have found that by incorporating a plasticizer in a specific range of amount into a polycarbonate-based resin and carrying out extrusion foaming, it is possible to obtain extruded polycarbonate-based resin foam particles which have a low open cell ratio, can be molded by a steam molding method, and have excellent fusibility when molded, thereby completing the present invention.

[0014] That is, the present invention provides (1) Extruded polycarbonate resin foam particles containing a polycarbonate resin and an ester compound having a number average molecular weight of 1000 or less as a plasticizer, the extruded polycarbonate resin foam particles having an expansion ratio of 3 to 15 times, the ester compound being present in an amount of 0.1 to 4 parts by weight per 100 parts by weight of the polycarbonate resin. (2) The extruded polycarbonate resin foam particles according to (1), characterized in that the ester compound is a diester of a dicarboxylic acid. (3) The extruded polycarbonate resin foam particles according to (2), characterized in that the diester of the dicarboxylic acid is a diester of sebacic acid. (4) The extruded polycarbonate-based resin foam beads according to (1) or (2), characterized in that the open cell ratio of the extruded foam beads is 20% or less. (5). The extruded polycarbonate-based resin beads according to claim 1 or 2, wherein the polycarbonate-based resin contains a linear polycarbonate-based resin and a branched polycarbonate-based resin. (6) A polycarbonate-based resin extruded foamed bead molded product obtained by molding the polycarbonate-based resin extruded foamed bead according to (1) or (2). (7) The method for producing a polycarbonate-based resin extruded foamed particle molding according to (6), in which the polycarbonate-based resin extruded foamed particle is molded at a mold temperature of 130 to 170°C. (8) A method for producing extruded polycarbonate-based resin foam particles having an expansion ratio of 3 to 15 times, comprising melt-kneading a polycarbonate-based resin composition containing a polycarbonate-based resin, an ester compound having a number average molecular weight of 1000 or less as a plasticizer, and a foaming agent in an extruder, and extruding the mixture under a lower pressure atmosphere than that of the extruder, wherein the content of the ester compound is 0.1 to 4 parts by weight per 100 parts by weight of the polycarbonate-based resin. (9) The method for producing extruded polycarbonate resin foam particles according to claim 8, wherein the foaming agent is carbon dioxide. (10) The method for producing extruded polycarbonate resin foam beads according to claim 8 or 9, wherein the low-pressure atmosphere is air. Regarding. Effect of the Invention

[0015] According to one embodiment of the present invention, extruded polycarbonate resin foam particles having high fusibility and excellent moldability can be obtained. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0016] Specific embodiments of the present invention will be described in detail below. Note that the present invention is not limited to the following embodiments, and various modifications are possible without departing from the gist of the present invention.

[0017] The present invention relates to extruded polycarbonate-based resin foam particles having an expansion ratio of 3 to 15 times, which contain a polycarbonate-based resin and an ester compound having a number average molecular weight of 1000 or less as a plasticizer, and the content of the ester compound is 0.1 to 4 parts by weight per 100 parts by weight of the polycarbonate-based resin.

[0018] <Polycarbonate resin extruded particles> The extruded polycarbonate-based resin foam particles of the present embodiment contain a polycarbonate-based resin and an ester-based compound.

[0019] [Polycarbonate resin] The extruded foam particles according to this embodiment are mainly composed of polycarbonate resin. Polycarbonate resin is a polymer having a basic structure with a carbonate bond represented by -[-OXOC(=O)-]-. In the above formula, X represents a linking group, which is generally a hydrocarbon group, but X having a heteroatom or heterobond introduced therein may be used to impart various properties. The polycarbonate resin according to this embodiment preferably contains 80% by weight or more of polycarbonate repeating units, more preferably 90% by weight or more, when the total repeating units of the polycarbonate resin are taken as 100% by weight. The polycarbonate resin according to this embodiment may contain repeating units other than polycarbonate within the above range.

[0020] Generally, aliphatic polycarbonate resins and aromatic polycarbonate resins are known as polycarbonate resins. Although aliphatic polycarbonate resins have a low thermal decomposition temperature, they have good physical properties such as impact resistance, light weight, transparency, and heat resistance. Some aliphatic polycarbonate resins are biodegradable and have the advantage of low environmental impact. Aromatic polycarbonate resins have excellent physical properties such as heat resistance, transparency, hygiene, electrical properties, and mechanical properties, and are widely used in various applications. In this embodiment, it is also preferable to use aromatic polycarbonate resins.

[0021] Aromatic polycarbonate resins can be obtained, for example, by reacting a dihydric phenol with a carbonate precursor such as phosgene or a carbonate diester, etc. Examples of the reaction method include an interfacial polymerization method, a melt transesterification method, a solid-phase transesterification method of a carbonate prepolymer, and a ring-opening polymerization method of a cyclic carbonate compound.

[0022] Representative examples of dihydric phenols used in the production of polycarbonate resins include hydroquinone, resorcinol; 4,4'-biphenol, bis(4-hydroxyphenyl)methane, 1,1-bis(4-hydroxyphenyl)ethane, 1,1-bis(4-hydroxyphenyl)-1-phenylethane, 2,2-bis(4-hydroxyphenyl)propane, 2,2-bis(4-hydroxyphenyl)butane, bis(4-hydroxyphenyl)diphenylmethane, 2,2-bis(4-hydroxy-3-methylphenyl)propane, 2,2-bis(3-methyl-4-hydroxyphenyl)propane, 2,2-bis(4-hydroxy-3-isopropylphenyl)propane, 2,2-bis(4-hydroxy-3-t-butylphenyl)propane, 2,2-bis(4-hydroxy-3,5-dimethylphenyl)propane, and the like. Examples of bisphenols include, but are not limited to, 1,1-bis(3-t-butyl-4-hydroxyphenyl)propane, 2,2-bis(4-hydroxy-3,5-dibromophenyl)propane, 2,2-bis(3-bromo-4-hydroxyphenyl)propane, 2,2-bis(3,5-dichloro-4-hydroxyphenyl)propane, 2,2-bis(4-hydroxyphenyl)heptane, 1,1-bis(4-hydroxyphenyl)cyclopentane, 1,1-bis(4-hydroxyphenyl)cyclohexane, 1,1-bis(3,5-dichloro-4-hydroxyphenyl)cyclohexane, 1,1-bis(3,5-dibromo-4-hydroxyphenyl)cyclohexane, bis(4-hydroxyphenyl)sulfone, and bis(4-hydroxyphenyl)sulfide. These may be used alone or in combination of two or more. Of these, polycarbonate resins based on 2,2-bis(4-hydroxyphenyl)propane, i.e., bisphenol A, have a good balance of mechanical strength, heat insulation, flame retardancy, cushioning properties, etc., and can be particularly preferably used in this embodiment.

[0023] Examples of carbonate diesters used in the production of polycarbonate resins include diphenyl carbonate, dinaphthyl carbonate, bis(diphenyl) carbonate, dimethyl carbonate, diethyl carbonate, and dibutyl carbonate, with diphenyl carbonate being preferred.

[0024] The viscosity average molecular weight of the polycarbonate resin is not particularly limited, but is preferably in the range of 5000 to 50000, more preferably 7000 to 45000, and particularly preferably 10000 to 40000. When the average molecular weight is in the range of 5000 to 50000, it is possible to particularly easily obtain a foam having an excellent balance between physical properties such as heat resistance and mechanical properties and moldability, and having a good surface appearance.

[0025] The viscosity average molecular weight (Mv) of the polycarbonate-based resin of this embodiment is a value calculated from the intrinsic viscosity ([η]) obtained by measuring the viscosity of a methylene chloride solution of the polycarbonate-based resin using an Ubbelohde viscometer at a temperature of 20°C, and then using the following viscosity formula: [η]=1.23×10 - 4 Mv 0.83 The polycarbonate-based resin extrusion foam particles of the present embodiment at least contain a polycarbonate-based resin composition containing the above-mentioned polycarbonate-based resin. In addition, the polycarbonate-based resin composition preferably contains at least two kinds of polycarbonate-based resins, a linear polycarbonate-based resin and a branched polycarbonate-based resin, because it can obtain extrusion foam particles with a high expansion ratio. These polycarbonate-based resins will be described below.

[0026] (Linear polycarbonate resin) The linear polycarbonate resin in this embodiment is a polycarbonate resin having a linear structure. In the process of producing the linear polycarbonate resin, a branched structure may be mixed in, but in this embodiment, such a small amount of polycarbonate resin, for example, 0.1% or less, preferably 0.05% or less of the branched structure is also treated as a linear polycarbonate resin.

[0027] As described above, the linear polycarbonate resin can be produced from, for example, a dihydric phenol and phosgene or a carbonate precursor, and various types are commercially available. In this embodiment, any linear polycarbonate resin can be used. Examples include, but are not limited to, SD POLYCA (registered trademark) manufactured by Sumika Polycarbonate Co., Ltd., and Iupilon (registered trademark), Novarex (registered trademark), and Zanter (registered trademark) manufactured by Mitsubishi Engineering Plastics Corporation. It is also possible to use multiple linear polycarbonate resins in combination.

[0028] There are a wide variety of types of linear polycarbonate resins, and even when focusing on the melt flow rate (MFR) at 300°C and 1.2 kgf, various resins ranging from about 1 to 65 g / 10 min are commercially available. In this embodiment, it is preferable to use a resin with an MFR (300°C, 1.2 kgf) of 40 g / 10 min or more, further 52 to 70 g / 10 min, and particularly about 55 to 65 g / 10 min, as the linear polycarbonate resin. If such a resin has a relatively high melt flow rate among polycarbonate resins, it becomes easier to form extruded foam particles with a high expansion ratio when combined with a branched polycarbonate resin described below and foamed.

[0029] The viscosity average molecular weight of the linear polycarbonate resin is not particularly limited, but is preferably in the range of 5000 to 30000, more preferably 7000 to 25000, and particularly preferably 10000 to 20000. When the average molecular weight is in the range of 5000 to 30000, it is possible to particularly easily obtain a foam having an excellent balance between physical properties such as heat resistance and mechanical properties and moldability, and having a good surface appearance.

[0030] (Branched polycarbonate resin) The branched polycarbonate resin in this embodiment is a polycarbonate resin having a branched structure. The branched structure can be produced by copolymerizing the above-mentioned polycarbonate resin raw material with, for example, a polyfunctional aromatic compound having three or more functional groups. It is also possible to produce the branched structure by utilizing a side reaction during the melt transesterification reaction.

[0031] The polyfunctional compounds that can be used as raw materials for branched polycarbonate resins include 4,6-dimethyl-2,4,6-tris(4-hydroxyphenyl)heptene-2, 2,4,6-trimethyl-2,4,6-tris(4-hydroxyphenyl)heptane, 1,3,5-tris(4-hydroxyphenyl)benzene, 1,1,1-tris(4-hydroxyphenyl)ethane, 1,1,1-tris(3,5-dimethyl-4-hydroxyphenyl)ethane, 2,6-bis(2-hydroxy-5-methylbenzene), and Examples of the phenol include trisphenols such as 4-{4-[1,1-bis(4-hydroxyphenyl)ethyl]-α,α-dimethylbenzyl}phenol, phloroglucine, phloroglucide, tetra(4-hydroxyphenyl)methane, bis(2,4-dihydroxyphenyl)ketone, 1,4-bis(4,4-dihydroxytriphenylmethyl)benzene, trimellitic acid, pyromellitic acid, benzophenonetetracarboxylic acid, and acid chlorides thereof. Among them, 1,1,1-tris(4-hydroxyphenyl)ethane and 1,1,1-tris(3,5-dimethyl-4-hydroxyphenyl)ethane are preferred, and 1,1,1-tris(4-hydroxyphenyl)ethane is particularly preferred.

[0032] The branched structure in the branched polycarbonate resin, i.e., the constituent unit derived from a polyfunctional compound, is, for example, preferably about 0.03 to 1 mol %, more preferably about 0.07 to 0.7 mol %, and particularly preferably 0.1 to 0.4 mol %, of the total constituent units in the polycarbonate resin molecule (100 mol %). If the ratio of the branched structure is about 0.03 to 1 mol %, the branched polycarbonate resin has a good balance of high melt tension and fluidity, and is easily combined with the above-mentioned linear polycarbonate resin to form extruded polycarbonate resin foam particles with an appropriate foaming form. The ratio of the branched structure can be, for example, 1 It can be measured by H-NMR.

[0033] As the branched polycarbonate resin, various varieties are known, for example, with MFR (300°C, 1.2 kgf) ranging from 0.1 to 20 g / 10 min. In the present embodiment, any of these branched polycarbonate resins may be used, and a plurality of types may be used in combination. Preferably, a branched polycarbonate resin with MFR (300°C, 1.2 kgf) of 10 g / 10 min or less, particularly 1 to 10 g / 10 min, is used. When a branched polycarbonate resin with such an MFR is combined with the linear polycarbonate resin and foamed, it becomes easier to form extruded foam particles having an average cell diameter of more than 300 μm and 1000 μm or less and an open cell ratio of 0.1% to 30%. In particular, when it is combined with a linear polycarbonate resin having an MFR (300° C., 1.2 kgf) of 40 g / 10 min or more, it becomes possible to more easily produce extruded foam particles having an appropriate foaming form.

[0034] The viscosity average molecular weight of the branched polycarbonate resin is not particularly limited, but is preferably in the range of 10,000 to 50,000, more preferably 20,000 to 40,000, and further preferably 25,000 to 35,000. When the average molecular weight is in the range of 10,000 to 50,000, a foam having an excellent balance between physical properties such as heat resistance and mechanical properties and moldability, and having a good surface appearance can be particularly easily obtained.

[0035] The melt tension of the branched polycarbonate resin is not particularly limited, but can usually be higher than that of the linear polycarbonate resin. The melt tension of the branched polycarbonate resin at, for example, 280°C is preferably 2.0cN or more, more preferably 3.0cN or more. If the melt tension of the branched polycarbonate resin is, for example, 2.0cN or more at 280°C, the polycarbonate resin composition retains higher strength even in the molten state, and the foam cells are less likely to break. As a result, the expansion ratio of the obtained extruded polycarbonate resin foam particles can be further increased. In particular, when combined with a linear polycarbonate resin having an MFR (300°C, 1.2kgf) of 40g / 10min or more, the melt tension of the branched polycarbonate resin is preferably, for example, 4.0cN or more, and more preferably 5.0 or more. The upper limit of the melt tension is preferably 15 cN or less, particularly preferably 10 cN or less. If the melt tension is 15 cN or less, it becomes easier to suppress the formation of finer foam cells and the formation of more open cells.

[0036] The method for measuring the melt tension in this specification will be described below. In this specification, the melt tension can be measured, for example, by using a Capilograph (registered trademark) 1D (manufactured by Toyo Seiki Seisakusho, Ltd.). Specifically, the method includes the following steps (1) to (4): (1) a 9.55 mm diameter barrel heated to a test temperature (e.g., 280°C) is filled with a sample resin (branched polycarbonate resin) to be measured; (2) the sample resin is then heated for 10 minutes in the barrel heated to the test temperature (e.g., 280°C); (3) the sample resin is then discharged in a string-like form from a capillary die (diameter 1.0 mm, length 10 mm) at a constant piston descending speed (10 mm / min), while passing this string-like material through a tension detection pulley located 350 mm below the capillary die, and then winding is started using a winding roll at a winding speed of 10 m / min; (4) the load applied to the pulley with the load cell after the string-like material has been stably taken up is measured as the melt tension.

[0037] (Ester compounds) The ester compound of the present embodiment is not particularly limited as long as it is a compound having an ester bond and a number average molecular weight of 1000 or less, and examples of the ester compound include low molecular weight ester compounds.

[0038] The low molecular weight ester compound is preferably a compound having a number average molecular weight of 50 to 1000, particularly 50 to 500, and examples thereof include ester compounds of monocarboxylic acid or dicarboxylic acid with alcohol. Examples of monocarboxylic acid include aliphatic monocarboxylic acids such as formic acid, acetic acid, propionic acid, butyric acid, valeric acid, caproic acid, enanthic acid, caprylic acid, pelargonic acid, capric acid, lauric acid, myristic acid, palmitic acid, margaric acid, and stearic acid; aromatic carboxylic acids such as benzoic acid, salicylic acid, and naphthalene carboxylic acid. Examples of dicarboxylic acid include aliphatic dicarboxylic acids such as oxalic acid, malonic acid, succinic acid, glutaric acid, adipic acid, pimelic acid, suberic acid, azelaic acid, and sebacic acid; and aromatic dicarboxylic acids such as phthalic acid (o-phthalic acid), isophthalic acid, and terephthalic acid. Examples of alcohols that form ester compounds include methanol, ethanol, propanol, butanol, pentanol, hexanol, heptanol, and 2-ethylhexanol. Among low molecular weight ester compounds, diesters of dicarboxylic acids and alcohols are preferred, diesters of sebacic acid or azelaic acid and alcohols are more preferred, and diesters of sebacic acid and 2-ethylhexanol are preferred because of their high compatibility with polycarbonate resins.

[0039] The content of the ester compound is preferably 0.1 to 4 parts by weight, and more preferably 0.5 to 3.5 parts by weight, based on 100 parts by weight of the polycarbonate resin, since this improves the moldability of the extruded foamed beads.

[0040] (Foam nucleating agent) The polycarbonate resin composition may also contain a foaming nucleating agent (nucleating agent) such as talc, clay, silica, etc. The presence of the foaming nucleating agent can further increase the expansion ratio of the extruded polycarbonate resin beads. The content of the foaming nucleating agent is preferably 0.01 to 2 parts by weight, more preferably 0.05 to 1 part by weight, per 100 parts by weight of the polycarbonate resin.

[0041] (Other ingredients) In addition to the above components, the polycarbonate resin composition may further contain additives such as polymers other than polycarbonate resins, stabilizers, lubricants, flame retardants, antistatic agents, plasticizers other than ester compounds having a number average molecular weight of 1000 or less, water absorbents, antioxidants, deterioration inhibitors, colorants, and / or radiation suppressants, so long as the effects of the present invention are not impaired. The types and amounts of these components may be appropriately set depending on the effects to be obtained, and may be, for example, 0.01 to 5 parts by weight, particularly 0.1 to 1 part by weight, per 100 parts by weight of the polycarbonate resin.

[0042] Examples of polymers other than polycarbonate resins include polyolefin resins, polystyrene resins such as AS resins and ABS resins, polyamide resins, polyester resins, polyvinyl chloride resins, polyether resins, and elastomers such as SBR, NBR, SBS, SIS, SEBS, EPDM, and fluororubbers, but are not limited thereto. For example, by adding 1 to 5 parts by weight of such polymers to 100 parts by weight of the total of polycarbonate resins, the mechanical properties and moldability of the extruded polycarbonate resin foam particles can be improved. However, from the viewpoint of easily achieving the effects of the present invention, it is preferable that the polycarbonate resin composition does not contain such other polymers and is composed only of polycarbonate resin.

[0043] [Foaming agent (foaming gas)] As a foaming agent for producing the extruded polycarbonate resin foam beads of this embodiment, one or more foaming agents selected from the group consisting of physical type foaming agents and chemical type foaming agents can be used.

[0044] Specific examples of physical type blowing agents include, for example, hydrocarbons such as propane, n-butane, i-butane, n-pentane, i-pentane, neopentane, and cyclopentane; fluorinated hydrocarbons such as 1,1-difluoroethane, 1,2-difluoroethane, 1,1,1-trifluoroethane, 1,1,2-trifluoroethane, 1,1,1,2-tetrafluoroethane, 1,1,2,2-tetrafluoroethane, 1,1,1,2,2-pentafluoroethane, difluoromethane, and trifluoromethane; inorganic gases such as carbon dioxide, nitrogen, water, argon, and helium; and ethers such as dimethyl ether, diethyl ether, methyl ethyl ether, isopropyl ether, n-butyl ether, and diisoamyl ether. Among these, one or more of them can be used in combination.

[0045] Specific examples of chemical foaming agents include N,N'-dinitrosopentamethylenetetramine, p,p'-oxybis-benzenesulfonylhydrazide, hydrazodicarbonamide, sodium carbonate, calcium carbonate, potassium carbonate, sodium hydrogen carbonate, potassium hydrogen carbonate, azodicarbonamide, terephthalazide, 5-phenyltetrazole, p-toluenesulfonylsemicarbazide, etc. Among these, one or a mixture of two or more can be used.

[0046] Among the above-mentioned physical type blowing agents and chemical type blowing agents, it is particularly preferable to use carbon dioxide as the blowing agent. Carbon dioxide is a non-flammable substance that is harmless to living organisms, including humans. Therefore, by using carbon dioxide as the blowing agent, safety and environmental compatibility can be improved. Note that carbon dioxide used as the blowing agent may be in either a gaseous or liquid state.

[0047] The amount of the foaming agent used is preferably 0.1 to 10 parts by weight, and more preferably 0.5 to 7 parts by weight, per 100 parts by weight of the polycarbonate resin, since extruded foam beads having a low open cell ratio can be obtained.

[0048] <Polycarbonate resin extruded particles> The extruded polycarbonate resin foam particles of the present embodiment are foamed and formed into particles in the extrusion foaming step and the granulation step described below.

[0049] [Expansion ratio] In the extruded polycarbonate resin foam beads of the present embodiment, the expansion ratio is 3 to 15, particularly 4 to 8. By setting the expansion ratio within the above numerical range, a lightweight and high-strength foam molded article can be provided when the extruded polycarbonate resin foam beads are used to produce a foam molded article.

[0050] Here, the expansion ratio can be calculated from the density d2 (g / l) of the polycarbonate-based resin composition and the bulk density d1 (g / l) of the extruded polycarbonate-based resin particles. More specifically, it can be calculated by the following formula (3). Expansion ratio = d1 / d2 Formula (3) [Bulk density] The bulk density d1 can be calculated from the bulk V(l) and weight W(g) of the extruded polycarbonate resin particles measured, for example, by the following procedure, using the following formula (4): The extruded resin particles are placed in a container with a known volume V(l), such as a measuring cylinder, beaker, or bucket, until the container overflows; the powder surface (top) of the container is scraped off, and the weight W(g) of the extruded resin particles in the container is measured. Bulk density d1 (g / l) = W / V Equation (4) The bulk density of the polycarbonate-based resin extruded foam particles according to the present embodiment is preferably 80 to 240 g / l, particularly 110 to 180 g / l. By setting the bulk density within the above range, the particle size of the polycarbonate-based resin extruded foam particles can be made smaller, and the gaps between the polycarbonate-based resin extruded foam particles on the surface of the foam molded product produced using the polycarbonate-based resin extruded foam particles become smaller. As a result, the fusion property and appearance of the foam molded product as a whole can be further improved.

[0051] [Open cell ratio] The open cell ratio of the extruded polycarbonate resin foam beads of this embodiment is preferably 20% or less in order to obtain a molded article with good appearance, more preferably 10% or less, and even more preferably 7% or less.

[0052] <Production method of extruded polycarbonate resin foam particles> The extruded polycarbonate-based resin foam particles according to the present embodiment can be produced by the following method: a production method including at least a foaming agent kneading step of kneading a foaming agent into a polycarbonate-based resin composition containing a polycarbonate-based resin and an ester compound in an extruder, an extrusion-foaming step of extruding the polycarbonate-based resin composition kneaded with the foaming agent into an atmosphere having a lower pressure than that in the extruder to foam it, and a granulation step of cutting the extruded polycarbonate-based resin composition to granulate extruded polycarbonate-based resin foam particles.

[0053] The method for producing the extruded polycarbonate resin beads according to one embodiment of the present invention includes, for example, at least a blowing agent kneading step [step 1], an extrusion foaming step [step 2], and a granulation step [step 3]. In addition, it is preferable to include a resin kneading step [step 0] in the same extruder or a different kneader as a step preceding the blowing agent kneading step. Each step is described in detail below.

[0054] (i) Resin kneading step [step 0] In the resin kneading step [step 0], a polycarbonate resin and an ester compound having a number average molecular weight of 1000 or less are mixed, preferably melt-kneaded, to obtain a polycarbonate resin composition. In this step, additives such as nucleating agents, stabilizers, lubricants, flame retardants, antistatic agents, plasticizers other than the ester compound, water absorbents, antioxidants, deterioration inhibitors, colorants, and / or radiation inhibitors may be added as necessary.

[0055] Here, the weight ratio of linear polycarbonate resin to branched polycarbonate resin is 60:40 to 95:5, preferably 65:35 to 92:8, and more preferably 70:30 to 90:10. The linear polycarbonate resin is preferably a resin having an MFR (300°C, 1.2 kgf) of 40 g / 10 min or more, and the branched polycarbonate resin is preferably a resin having an MFR (300°C, 1.2 kgf) of 10 g / 10 min or less.

[0056] The resin kneading step [Step 0] is preferably carried out in the same device as the extruder used in [Step 1] and thereafter in terms of work efficiency, but it may also be carried out using a separate extruder for kneading or a batch-type internal mixer such as a Banbury mixer or a pressure kneader. In addition, the resin kneading can be carried out simultaneously with the kneading of the blowing agent in the blowing agent kneading step [Step 1] described below, so that [Step 0] can be virtually omitted.

[0057] (ii) Foaming agent kneading step [Step 1] In the foaming agent kneading step [Step 1], a foaming agent is kneaded into the polycarbonate-based resin composition in an extruder. The foaming agent can be dissolved and dispersed in the molten mixture of the polycarbonate-based resin composition by a mixing device or the like provided in the extruder.

[0058] In this [Step 1], the above-mentioned physical type foaming agents and chemical type foaming agents can be used as the foaming agent. In particular, it is preferable to use carbon dioxide as the foaming agent. Carbon dioxide is a non-flammable substance that is harmless to living organisms, including humans. Therefore, by using carbon dioxide as the foaming agent, safety and environmental compatibility can be improved.

[0059] In this [Step 1], it is preferable to use 0.1 to 10 parts by weight of carbon dioxide or other foaming agent per 100 parts by weight of polycarbonate-based resin. By setting the amount of foaming agent used within the above numerical range, the gas dispersion in the polycarbonate-based resin composition is good, and the foaming property of the resin composition can be improved.

[0060] The carbon dioxide used as the foaming agent may be in either a gaseous or liquid state. In consideration of the solubility, permeability, diffusibility, etc. in the polycarbonate resin composition, it is preferable to use carbon dioxide in a supercritical state at or above the critical temperature and the critical pressure.

[0061] (iii) Cooling step (optional step) The polycarbonate-based resin composition kneaded with the foaming agent is then subjected to the extrusion foaming step [step 2], during which a cooling step is preferably added as desired. In this optional cooling step, the polycarbonate-based resin composition kneaded with the foaming agent is transferred to an extruder (second-stage extruder) having a lower temperature than the extruder (first-stage extruder) used for kneading, and cooled. Although not limited here, for example, the temperature inside the first-stage extruder may be set to 240 to 320°C, particularly 260 to 300°C, and the cooling in the second-stage extruder may be performed at 180 to 220°C, particularly 185 to 210°C. In particular, by setting the cooling temperature in the second-stage extruder to the above numerical range, it becomes easy to increase the expansion ratio of the polycarbonate-based resin extruded foam particles and reduce the open cell ratio.

[0062] (iv) Extrusion foaming process [Process 2] In the extrusion foaming step [step 2], the polycarbonate-based resin composition kneaded with the foaming agent is extruded into an atmosphere with a lower pressure than that in the extruder to foam it. The pressure in the extruder is, for example, about 5 to 20 MPa, usually about 10 to 18 MPa, so that the polycarbonate-based resin composition is exposed to an atmosphere with a lower pressure than that in the extruder by extruding it from the extrusion port (die or die) outside the extruder, for example into the atmosphere or water, and foams.

[0063] Here, when the polycarbonate-based resin composition is extruded into the atmosphere, the polycarbonate-based resin composition is cooled relatively slowly in the subsequent granulation step [step 3], so that the polycarbonate-based resin composition can be sufficiently expanded. Therefore, in the extrusion foaming step [step 2], it is preferable to extrude the polycarbonate-based resin composition from the extruder into the atmosphere. The temperature of the polycarbonate-based resin composition in the extrusion foaming step [step 2] is preferably 200°C or lower. The die temperature at that time is preferably about 180 to 220°C, particularly about 185 to 210°C.

[0064] (v) Granulation process [Process 3] In the granulation step [step 3], the extruded polycarbonate-based resin composition is cut to granulate polycarbonate-based resin extrusion foam particles. The granulation step [step 3] can be carried out in the same environment (in air or water) as the above-mentioned extrusion foaming step [step 2], or in a different environment (in air or water), and is divided into the following three methods based on the difference in the extrusion environment: the underwater cut (hereinafter sometimes referred to as UWC) method, the watering cut (hereinafter sometimes referred to as WRC) method, and the hot cut (hereinafter sometimes referred to as HC) method.

[0065] The UWC method is a method in which cooling water adjusted to a predetermined pressure is filled in a chamber attached to the tip of the die so as to contact the resin discharge surface of the die, and the composition extruded from the die hole is cut in water. The WRC method is a method in which a cooling drum connected to the die is arranged downstream from the die, in which cooling water flows along the inner peripheral surface of the cooling drum, and the composition cut by the cutter in air is cooled in the cooling water while foaming or after foaming. The HC method is a method in which the composition is cut by a cutter in air, and the cut composition is cooled in air while foaming or after foaming. Among these, the HC method and the WRC method in which granulation is performed in air are preferred.

[0066] <Polycarbonate resin foam molding> The extruded polycarbonate resin beads of the present embodiment can be processed to produce a polycarbonate resin foamed molded article. The present invention also includes a polycarbonate resin foamed molded article produced by molding any of the extruded polycarbonate resin beads described above.

[0067] The method of processing the polycarbonate-based resin extrusion foam particles of this embodiment into a polycarbonate-based resin foamed molded product includes, but is not limited to, the so-called bead method in-mold molding, in which the polycarbonate-based resin extrusion foam particles are charged into a pressure-resistant container, heated, and the polycarbonate-based resin extrusion foam particles are molded in a mold. The polycarbonate-based resin extrusion foam particles of this embodiment can be molded at a low molding temperature, and the molding temperature is preferably 130 to 170°C, more preferably 140 to 160°C.

[0068] Polycarbonate-based resin foam molded products can be used as heat insulating materials for housing and automobiles, as well as industrial buffer materials and cooling agents. Since polycarbonate-based resin foam molded products have excellent heat resistance, they are suitable as heat insulating materials, soundproofing materials, buffer materials, etc. for the engine periphery of automobiles and for factory piping. Polycarbonate-based resin foam molded products also have excellent mechanical properties, so they are useful as heat insulating materials for pipelines, LNG refrigerated ships, etc. EXAMPLES

[0069] Next, in order to further clarify the effects of the present invention, examples and comparative examples will be described, but the present invention is not limited to these examples.

[0070] <Production of Examples and Comparative Examples> In the following examples and comparative examples, the following raw materials were used. [Polycarbonate resin] Linear polycarbonate resin: Mitsubishi Engineering's Iupilon (registered trademark) H-4000, MFR (300°C, 1.2kgf): 63g / 10min Branched polycarbonate resin: Novarex (registered trademark) M7027BF / NA manufactured by Mitsubishi Engineering, MFR (300°C, 1.2kgf): 2.4g / 10min [Ester compounds] Di(2-ethylhexyl) sebacate (Sanso Cizer DOS, manufactured by New Japan Chemical).

[0071] <Measurement> The glass transition temperatures of the above-mentioned polycarbonate-based resins and the properties of the extruded polycarbonate-based resin foam beads in each of the Examples and Comparative Examples were measured as follows.

[0072] Foaming ratio: The expansion ratio of the extruded polycarbonate resin beads was calculated by the following method: First, the bulk density of the extruded polycarbonate resin foam particles was measured according to the following procedures (1) to (3). (1) Put the extruded foam particles into a measuring cup whose internal volume vk(l) has been accurately measured in advance until it overflows; (2) Level the top of the cup, and measure the weight wb(g) of the extruded foam particles in the measuring cup. (3) Calculate the bulk density ρ1 of the extruded foam particles using the following formula. Bulk density ρ1(g / l)=wb(g) / vk(l) Next, the reconstituted resin prepared according to the procedure described below was used as a sample, and the density of the reconstituted resin was measured according to the procedures (4) to (6) described below. (4) The weight wr (g) of the returned resin is measured; (5) Next, the returned resin used for measuring the weight is submerged in ethanol in a measuring cylinder, and the volume vr (l) of the returned resin is measured based on the rise in the liquid level position in the measuring cylinder; (6) The density ρ2 of the returned resin (polycarbonate-based resin composition) is calculated using the following formula. Density of the returned resin ρ2(g / l)=wr(g) / vr(l) Using the obtained values ​​of ρ1 and ρ2, the expansion ratio was calculated according to the following formula. Expansion ratio (times) = ρ2 / ρ1 How to make the resin: The density of the resin mass obtained by resin-returning the polycarbonate-based resin extrusion foam particles was regarded as the density of the polycarbonate-based resin composition. The following (f1) to (f5) were carried out in order, and the obtained resin mass was used as the resin-returned mass of the extrusion foam particles: (f1) The extrusion foam particles were placed in a dryer adjusted to a temperature of 260°C; (f2) Then, the pressure in the dryer was reduced to -0.05MPa (gauge pressure) to -0.10MPa (gauge pressure) using a vacuum pump over 5 to 10 minutes; (f3) Then, the extrusion foam particles were left in the dryer for 30 minutes to prepare a resin mass (returned resin); (f4) Then, the temperature in the dryer was cooled to room temperature, and the pressure in the dryer was returned to normal pressure; (f5) Then, the resin mass was taken out of the dryer.

[0073] Open cell ratio: The open cell ratio of the extruded foam particles was measured using an air-comparison type specific gravity meter [Tokyo Science Co., Ltd., Model 1000] according to the method described in PROSEDURE C of ASTM D2856-87. Specifically, the open cell ratio of the extruded foam particles was calculated by carrying out the following (1) to (3) in order: (1) The volume Vc (cm) of the extruded foam particles was measured using an air-comparison type specific gravity meter. 3 (2) Next, the entire amount of the extruded foam particles after measuring Vc was submerged in ethanol in a measuring cylinder; (3) After that, the apparent volume Va (cm 3 ) of the extruded foam particles was calculated from the rise in the position of the ethanol in the measuring cylinder. 3 (4) The open cell ratio of the extruded foam particles was calculated using the following formula: Open cell rate (%) = ((Va-Vc) / Va) x 100.

[0074] Glass transition temperature: The glass transition temperature of the resin block of the polycarbonate-based resin composition obtained by the above-mentioned resin reversion was measured by differential scanning calorimetry (DSC) in accordance with JIS K7121:2012 (ISO 3146:2000).

[0075] ·Moldability: The obtained in-mold foam molded article was evaluated for the following (x1) to (x6), and if all of the following were satisfied, it was evaluated as ◯, and if any one of them was not satisfied, it was evaluated as ×. A polycarbonate-based resin in-mold foam molded article in which (x1) the polycarbonate-based resin extruded particles are sufficiently fused to each other, (x2) the gaps between the polycarbonate-based resin extruded particles are sufficiently filled, (x3) the surface is beautiful, (x4) the surface is not melted, (x5) the compressive strength is sufficient, and (x6) there is no shrinkage and the shape of the mold (metal mold) used for the in-mold foam molding is transferred.

[0076] Fusion rate: A cut of about 5 mm was made with a knife or the like from a point about 100 mm from one corner of the polycarbonate resin foam molded body to a point about 100 mm from the opposite side, and the cut was broken by hitting the part surrounded by the cut and the one corner with a hammer or the like. The fracture surface was visually inspected, and the total number of extruded foam particles present on the fracture surface and the number of extruded foam particles broken within the extruded foam particles on the fracture surface were counted. The ratio (%) of the number of extruded foam particles broken within the extruded foam particles on the fracture surface to the total number of extruded foam particles present on the fracture surface was calculated, and a ratio of 60% or more was evaluated as good (◯), a ratio of less than 60% and 40% or more was evaluated as fair (△), and a ratio of less than 40% was evaluated as unacceptable (×).

[0077] [Example 1] A mixture of the linear polycarbonate resin, the branched polycarbonate resin, and the ester compound in a weight ratio of 80:20:1.5 was fed from a hopper to a first-stage twin-screw extruder (manufactured by Technobel, screw diameter: 15 mm, L / D=30) at 0.6 kg / hour, and kneaded at 260° C. to prepare a polycarbonate resin composition. Carbon dioxide (carbon dioxide gas) as a foaming agent was injected into the molten polycarbonate resin composition from an injection section provided midway through the first-stage extruder in an amount of 1.7 parts by weight per 100 parts by weight of the linear polycarbonate resin and the branched polycarbonate resin combined.

[0078] Furthermore, the kneaded product was cooled by passing it through a melt cooler connected to the tip of the twin-screw extruder and set at 195°C, and then extruded under atmospheric pressure through a die with a diameter of 1.2 mm attached to the tip of the melt cooler to cause foaming, and cut at a cutter rotation speed of 600 rpm, followed by cooling in the atmosphere and granulation to produce the extruded polycarbonate resin foam particles of Example 1. The die temperature at this time was 192°C.

[0079] The resulting extruded polycarbonate resin beads were evaluated for expansion ratio, open cell ratio, and glass transition temperature. The results are shown in Table 1. Furthermore, the resulting extruded polycarbonate resin beads were heated with saturated steam at 150°C and foamed in a mold to obtain a molded product of the extruded polycarbonate resin beads, and the moldability and fusion rate were evaluated. The results are shown in Table 1.

[0080] [Table 1] [Examples 2-3, Comparative Examples 1-2] Except for changing the types and amounts of raw materials used as shown in Table 1 below, the same operations as in Example 1 were carried out to produce and evaluate extruded polycarbonate resin beads and in-mold foamed articles. The evaluation results are shown in Table 1.

[0081] [Comparative Example 3] The same procedure as in Comparative Example 2 was carried out, except that 100 parts by weight of the extruded polycarbonate resin beads obtained in Comparative Example 2 and 1 part by weight of an ester compound were hand-blended and spread, and then molded in a mold.

[0082] In Examples 1 to 3, extruded foam particles with a low open cell ratio could be obtained, and an in-mold foamed product with excellent moldability and fusion rate could be obtained. On the other hand, in Comparative Example 1, in which 5 parts by weight of an ester compound was used, polycarbonate-based resin extruded foam particles could be obtained, but the open cell ratio was high at 87%, and an in-mold foamed product could not be produced. In Comparative Example 2, in which an ester compound was not used, polycarbonate-based resin extruded foam particles could be obtained, but the fusion rate between the extruded foam particles in the in-mold foamed product was low, and the moldability was poor. In Comparative Example 3, an ester compound was spread on the polycarbonate-based resin extruded foam particles, but sufficient moldability could not be obtained.

Claims

1. The extruded polycarbonate-based resin foam particles contain a polycarbonate-based resin and an ester compound having a number average molecular weight of 1000 or less as a plasticizer, and have an expansion ratio of 3 to 15 times, and the content of the ester compound is 0.1 to 4 parts by weight per 100 parts by weight of the polycarbonate-based resin.

2. 2. The extruded polycarbonate resin foam particles according to claim 1, wherein the ester compound is a diester of a dicarboxylic acid.

3. 3. The extruded polycarbonate resin foam particles according to claim 2, wherein the diester of a dicarboxylic acid is a diester of sebacic acid.

4. 3. The extruded polycarbonate resin foam beads according to claim 1, wherein the extruded foam beads have an open cell ratio of 20% or less.

5. 3. The extruded polycarbonate-based resin foam particles according to claim 1, wherein the polycarbonate-based resin contains a linear polycarbonate-based resin and a branched polycarbonate-based resin.

6. 3. An extruded polycarbonate resin foamed bead molding produced by molding the extruded polycarbonate resin foamed bead according to claim 1 or 2.

7. 7. The method for producing an extruded polycarbonate-based resin foamed bead molding according to claim 6, wherein the extruded polycarbonate-based resin foamed bead is molded at a mold temperature of 130 to 170°C.

8. A method for producing extruded polycarbonate-based resin foam particles having an expansion ratio of 3 to 15 times, comprising melt-kneading a polycarbonate-based resin composition containing a polycarbonate-based resin, an ester compound having a number average molecular weight of 1000 or less as a plasticizer, and a foaming agent in an extruder, and extruding the mixture under a lower pressure atmosphere than that of the extruder, wherein the content of the ester compound is 0.1 to 4 parts by weight per 100 parts by weight of the polycarbonate-based resin.

9. The method for producing extruded polycarbonate resin foam particles according to claim 8, wherein the foaming agent is carbon dioxide.

10. 10. The method for producing extruded polycarbonate resin foam beads according to claim 8 or 9, wherein the low pressure atmosphere is air.

Citation Information

Patent Citations

  • Manufacture of laminate

    JP1998000724A

  • Polycarbonate resin foamed molding

    JP2016160400A

  • Method for producing polycarbonate resin foamed particle

    JP2021054959A