Abrasive pad manufacturing method and method for polishing surface of optical material or semiconductor material
By synergistically combining classification and expansion processes with a specific expansion ratio, the method creates a polishing pad with fine and uniform openings, improving polishing performance and reducing scratches, addressing the issue of non-uniform pores in existing pads.
Patent Information
- Application Number
- JP2024043092
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2023-03-29
- Filing Date
- 2024-03-19
- Publication Date
- 2024-10-11
AI Technical Summary
Existing polishing pads have large and non-uniform pores due to high expansion ratios of microspheres, leading to inadequate polishing performance and increased scratches on the polished surface.
A method combining classification and expansion processes with a specific expansion ratio to create a polishing pad with fine and uniform openings, involving the steps of preparing a composition with microspheres, classifying to remove coarse particles, mixing with an isocyanate-terminated urethane prepolymer and a curing agent, and curing to expand the microspheres by 1.5 to 3 times.
The method produces a polishing pad with fine and uniform openings, enhancing polishing performance and reducing scratches, while maintaining high precision and stability during the polishing process.
Smart Images

Figure 2024144235000001_ABST
Abstract
Description
[Technical field]
[0001] The present invention relates to a method for producing a polishing pad and a method for polishing the surface of an optical material or a semiconductor material. The polishing pad obtained by the production method of the present invention is used for polishing optical materials, semiconductor wafers, semiconductor devices, hard disk substrates, etc., and is particularly suitable for polishing devices in which an oxide layer, a metal layer, etc. are formed on a semiconductor wafer. [Background technology]
[0002] A polishing pad used for polishing semiconductor devices and the like has a polishing layer formed of a synthetic resin such as polyurethane, and voids are formed inside the polishing layer. The voids are open on the surface of the polishing layer, and during polishing, the abrasive grains contained in the polishing slurry are held in the open holes on the surface of the polishing layer, so that the polishing of the object to be polished progresses. As one method for forming voids inside the polishing layer, a method of mixing microspheres in resin is known, and in recent years, studies have been made to make the voids (openings) smaller and more uniform in order to achieve more precise polishing. Classification is a known method for obtaining particles of the same size from powders such as microspheres. To achieve more precise classification, it is also known to add liquids such as alcohol, glycol, and water as dispersion aids.
[0003] Patent Document 1 discloses a method for producing a polishing pad using microspheres from which fine powder and coarse particles have been removed by centrifugal separation and air classification. [Prior art documents] [Patent documents]
[0004] [Patent Document 1] Patent No. 7048395 Summary of the Invention [Problem to be solved by the invention]
[0005] In Patent Document 1, microspheres with a density of 800 to 1500 g / L after classification are expanded until the density becomes 10 to 100 g / L, and the expansion ratio is 8 to 150. The openings in the polishing layer manufactured through such a high expansion ratio have a large diameter and are not minute. As described above, there is a demand for polishing pads having fine and uniform openings.
[0006] The present invention has been made in consideration of the above-mentioned problems, and aims to provide a method for manufacturing a polishing pad having fine and uniform openings, and a method for polishing the surface of an optical material or semiconductor material using said polishing pad. [Means for solving the problem]
[0007] The present inventors have conducted extensive research to solve the above problems, and have found that the above problems can be solved by combining a classification process with an expansion process at a specific expansion ratio to act synergistically, thereby completing the present invention. Specific aspects of the present invention are as follows.
[0008] [1] A method for producing a polishing pad having a polishing layer, comprising: (1) providing a composition comprising a plurality of microspheres; (2) classifying the composition to remove coarse particles and obtain classified microspheres containing heat-expandable microspheres; (3) mixing the classified microspheres with an isocyanate-terminated urethane prepolymer and a curing agent to form a curable resin composition; and (4) A step of curing the curable resin composition to form the polishing layer, the step including expanding the heat-expandable microspheres by 1.5 to 3 times. The method for producing the polishing pad includes the steps of: [2] The method for producing a polishing pad according to [1], further comprising, between the steps (1) and (2), a step (A) of reducing the cohesive force between the plurality of microspheres contained in the composition. [3] The method for producing a polishing pad described in [2], wherein the step (A) includes a step (A') of drying the composition. [4] The method for producing a polishing pad described in [3], wherein the step (A') includes a step of (A'') placing the composition in an atmosphere of a gas having a dew point of -50°C or lower. [5] The method for producing a polishing pad described in [4], wherein the gas having a dew point of -50°C or lower includes an inert gas. [6] The method for producing a polishing pad according to any one of [1] to [5], wherein the classification in the step (2) is centrifugal classification. [7] A method for polishing a surface of an optical material or a semiconductor material, comprising a step of polishing the surface of the optical material or the semiconductor material using a polishing pad obtained by the method according to any one of [1] to [6].
[0009] (definition) In this specification, when a numerical range is expressed using "X to Y", the range includes the numerical values X and Y at both ends. In this specification, "classification" refers to dividing powder (a collection of fine particles) into a number of groups of particles based on their size. In this specification, "coarse particles" refers to particles or powder in which the proportion of particles or powder with a particle size of 10 μm or more in a composition containing microspheres before classification is 30 volume % or more. In this specification, "fine powder" refers to particles or powder in which the proportion of particles or powder with a particle size of 10 μm or more in a composition containing microspheres before classification is 10 volume % or less. Effect of the Invention
[0010] According to the method for producing a polishing pad of the present invention, a polishing pad having fine and uniform openings can be obtained. [Brief description of the drawings]
[0011] [Figure 1] FIG. 1 is a schematic diagram of a microsphere manufacturing apparatus applicable to the polishing pad manufacturing method of the present invention. [Diagram 2] FIG. 2 is a schematic diagram of a free vortex type centrifugal classifier. [Diagram 3] FIG. 3 is a cross-sectional photograph of the polishing pad of Example 1. [Figure 4] FIG. 4 is a cross-sectional photograph of the polishing pad of Example 2. [Diagram 5] FIG. 5 is a cross-sectional photograph of the polishing pad of Example 3. [Figure 6] FIG. 6 is a cross-sectional photograph of the polishing pad of Example 4. [Figure 7] FIG. 7 is a cross-sectional photograph of the polishing pad of Comparative Example 1. [Figure 8] FIG. 8 is a cross-sectional photograph of the polishing pad of Comparative Example 2. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0012] (action) As a result of intensive research, the inventors unexpectedly found that a polishing pad having fine and uniform pores can be manufactured by combining a classification process and an expansion process with a specific expansion ratio to act synergistically. Although the details of why such characteristics are obtained are not clear, it is assumed as follows.
[0013] By classifying a composition containing microspheres, coarse particles can be removed, and relatively small-sized microspheres can be obtained. However, if the expansion ratio of the microspheres obtained after classification is set to a large value, it is believed that the effect of the refinement by classification is not fully utilized. On the other hand, if the expansion ratio of the microspheres obtained after classification is set to a small value, the refinement by classification and the refinement by low expansion ratio act synergistically, and fine and uniform pores can be obtained.
[0014] The method for producing a polishing pad and the method for polishing the surface of an optical material or semiconductor material of the present invention will be described below.
[0015] 1. Manufacturing method of polishing pad The method for producing a polishing pad having a polishing layer of the present invention includes the steps of: (1) providing a composition comprising a plurality of microspheres; (2) classifying the composition to remove coarse particles and obtain classified microspheres containing heat-expandable microspheres; (3) mixing the classified microspheres with an isocyanate-terminated urethane prepolymer and a curing agent to form a curable resin composition; and (4) A step of curing the curable resin composition to form the polishing layer, the step including expanding the heat-expandable microspheres by 1.5 to 3 times. Includes. The method for producing a polishing pad of the present invention can provide a polishing pad having fine and uniform openings. In some cases, the polishing pad obtained by the production method of this embodiment can exhibit high polishing performance because the fine irregularities resulting from the fine and uniform openings act as polishing points.
[0016] <Process (1)> (composition) The plurality of microspheres contained in the composition may be, but is not limited to, in the form of a single microsphere, in the form of an aggregate formed from a plurality of microspheres, or may include or consist of a mixture thereof. The aggregate formed from the plurality of microspheres may be, but is not limited to, an aggregate that is relatively large in size and classified as a coarse particle as described below, an aggregate that is relatively small in size and not classified as a coarse particle, or may include or consist of a mixture thereof. The composition may further comprise, but is not limited to, fine powder, coarse particles, or a mixture thereof in addition to the plurality of microspheres. The fines may comprise or consist of debris resulting from the crushing of microspheres. The coarse particles may comprise or consist of relatively large sized agglomerates formed from a plurality of the microspheres described above, agglomerates formed from microspheres and microsphere fragments, or a mixture of two or more of these. The moisture content (water content) of the composition containing the microspheres in step (1) (before performing step (2) or before performing step (A) described below) is not particularly limited, but may be 1 to 7% by weight, 1 to 5% by weight, or 1 to 3% by weight. The moisture content of the composition can be measured based on the loss on drying method as described in the Examples below.
[0017] (microsphere) The microspheres are not particularly limited, but examples thereof include unexpanded heat-expandable microspheres that are composed of an outer shell (polymer shell) made of a thermoplastic resin and a low-boiling point hydrocarbon encapsulated in the outer shell.
[0018] The average particle size (D50, median diameter) of the composition containing the (unclassified) microspheres (such as the heat-expandable microspheres in an unexpanded state) in step (1) is not particularly limited, but is preferably 1 to 20 μm, more preferably 3 to 15 μm, and most preferably 6 to 12 μm. When the average particle size (D50) is within the above numerical range, the average pore size of the surface of the polishing layer is 20 μm or less even when the heat-expandable microspheres are expanded, and the object to be polished can be polished more precisely. The average particle size (D50, median diameter) can be measured using a laser diffraction particle size distribution analyzer (e.g., Mastersizer 2000, manufactured by Spectris Co., Ltd.).
[0019] The expansion initiation temperature of the unexpanded heat-expandable microspheres is not particularly limited, but is preferably 50 to 200°C, more preferably 80 to 170°C, and most preferably 90 to 140°C, from the viewpoint of reaction heat due to the polymerization reaction of the prepolymer, etc. The maximum expansion temperature of the unexpanded heat-expandable microspheres is not particularly limited, but is preferably 90 to 200°C, more preferably 110 to 170°C, and most preferably 120 to 170°C, from the viewpoint of reaction heat due to the polymerization reaction of the prepolymer, etc.
[0020] Examples of the polymer that forms the polymer shell include thermoplastic resins such as polyvinyl alcohol, polyvinylpyrrolidone, poly(meth)acrylic acid, polyacrylamide, polyethylene glycol, polyhydroxyether acrylate, maleic acid copolymers, polyethylene oxide, polyurethane, poly(meth)acrylonitrile, polyvinylidene chloride, polyvinyl chloride, and organic silicone resins, as well as copolymers of two or more of the monomers that constitute these resins (e.g., acrylonitrile-vinylidene chloride copolymers, acrylonitrile-methyl methacrylate copolymers, vinyl chloride-ethylene copolymers, etc.). The low-boiling point hydrocarbon encapsulated in the polymer shell may be, for example, isobutane, pentane, isopentane, petroleum ether, or a combination of two or more of these.
[0021] <Process (2)> The type of classification in step (2) is not particularly limited, but may include centrifugal classification, gravity classification, inertial classification, or a combination of two or more of these. Among these, centrifugal classification is preferred. By using centrifugal classification, the deterioration of microspheres caused by collision between microspheres or between microspheres and the inner wall of the classification device can be suppressed, and as a result, unexpected foaming failure of microspheres can be suppressed, so that the fineness and uniformity of the openings in the polishing layer can be improved. In addition, by using centrifugal classification, the aggregation force between microspheres can be further relaxed by the action of centrifugal force, and the classification can be performed in this state.
[0022] The average particle size (D50, median diameter) of the classified microspheres (such as the heat-expandable microspheres in an unexpanded state) obtained in step (2) is not particularly limited, but is preferably 0.5 to 15 μm, more preferably 1 to 10 μm, and most preferably 4 to 8 μm. When the average particle size is within the above-mentioned numerical range, even if the heat-expandable microspheres are expanded, the average pore size of the surface of the polishing layer becomes 20 μm or less, and the object to be polished can be polished more precisely. The average particle size (D50, median diameter) can be measured using a laser diffraction particle size distribution analyzer (for example, Mastersizer 2000, manufactured by Spectris Co., Ltd.).
[0023] <Process (3)> The curable resin composition formed by step (3) can be, for example, a two-liquid composition prepared by mixing liquid A containing an isocyanate-terminated urethane prepolymer with liquid B containing a curing agent component. The other components can be added to either liquid A or liquid B, but if problems arise, the composition can be divided into multiple liquids and mixed to form a composition consisting of three or more liquids. In step (3), the microspheres after the classification treatment can be mixed with an isocyanate-terminated urethane prepolymer to form Liquid A, and the Liquid A can be further mixed with Liquid B containing a curing agent to form a curable resin composition.
[0024] (Isocyanate-terminated urethane prepolymer) The isocyanate-terminated urethane prepolymer may be a product obtained by reacting a polyol component with a polyisocyanate component.
[0025] (Polyol component) As the polyol component, a low molecular weight polyol, a high molecular weight polyol, or a combination thereof can be used. In this specification, a low molecular weight polyol is a polyol having a number average molecular weight of 30 to 300, and a high molecular weight polyol is a polyol having a number average molecular weight of more than 300. The number average molecular weights of the high molecular weight polyol and the low molecular weight polyol can be measured as polyethylene glycol / polyethylene oxide (PEG / PEO) molecular weights based on gel permeation chromatography (GPC) under the following conditions. <Measurement conditions> Column: Ohpak SB-802.5HQ (exclusion limit 10000) + SB-803HQ (exclusion limit 100000) Mobile phase: 5mM LiBr / DMF Flow rate: 0.3ml / min (26kg / cm 2 ) Oven: 60℃ Detector: RI 40℃ Sample volume: 20 μl
[0026] Examples of the low molecular weight polyol include ethylene glycol, diethylene glycol, triethylene glycol, 1,2-propanediol, 1,3-propanediol, 1,3-butanediol, 1,4-butanediol, neopentyl glycol, pentanediol, 3-methyl-1,5-pentanediol, 1,6-hexanediol, and combinations of two or more of these.
[0027] Examples of the high molecular weight polyol include Polyether polyols such as polytetramethylene ether glycol (PTMG), polyethylene glycol, and polypropylene glycol; polyester polyols such as the reaction product of ethylene glycol with adipic acid and the reaction product of butylene glycol with adipic acid; Polycarbonate polyols; polycaprolactone polyols; or a combination of two or more thereof.
[0028] (Polyisocyanate component) Examples of the polyisocyanate component include: m-phenylene diisocyanate, p-phenylene diisocyanate, 2,6-tolylene diisocyanate (2,6-TDI), 2,4-tolylene diisocyanate (2,4-TDI), Naphthalene-1,4-diisocyanate, Diphenylmethane-4,4'-diisocyanate (MDI), 4,4'-methylene-bis(cyclohexyl isocyanate) (hydrogenated MDI), 3,3'-dimethoxy-4,4'-biphenyl diisocyanate, 3,3'-dimethyldiphenylmethane-4,4'-diisocyanate, Xylylene-1,4-diisocyanate, 4,4'-diphenylpropane diisocyanate, Trimethylene diisocyanate, Hexamethylene diisocyanate, Propylene-1,2-diisocyanate, butylene-1,2-diisocyanate, Cyclohexylene-1,2-diisocyanate, Cyclohexylene-1,4-diisocyanate, p-phenylene diisothiocyanate, Xylylene-1,4-diisothiocyanate, ethylidine diisothiocyanate, or a combination of two or more thereof. Among these, from the viewpoint of polishing properties, it is preferable to use tolylene diisocyanates such as 2,6-tolylene diisocyanate (2,6-TDI) and 2,4-tolylene diisocyanate (2,4-TDI).
[0029] The NCO equivalent (g / eq) of the isocyanate-terminated urethane prepolymer is preferably less than 600, more preferably 350 to 550, and most preferably 400 to 500. The NCO equivalent (g / eq) is within the above numerical range, so that the polishing layer can exhibit an appropriate hardness. The NCO equivalent (g / eq) is calculated by "(parts by mass of polyisocyanate compound + parts by mass of polyol compound) / [(number of functional groups per molecule of polyisocyanate compound x parts by mass of polyisocyanate compound / molecular weight of polyisocyanate compound)-(number of functional groups per molecule of polyol compound x parts by mass of polyol compound / molecular weight of polyol compound)]", and is a numerical value indicating the molecular weight of the prepolymer per NCO group.
[0030] (hardening agent) The curing agent contained in the curable resin composition may, for example, be an amine-based curing agent described below. Examples of polyamines constituting the amine-based curing agent include diamines, such as alkylenediamines such as ethylenediamine, propylenediamine, and hexamethylenediamine; diamines having an aliphatic ring such as isophoronediamine and dicyclohexylmethane-4,4'-diamine; diamines having an aromatic ring such as 3,3'-dichloro-4,4'-diaminodiphenylmethane (also known as methylenebis-o-chloroaniline) (hereinafter abbreviated as MOCA); diamines having a hydroxyl group such as 2-hydroxyethylethylenediamine, 2-hydroxyethylpropylenediamine, di-2-hydroxyethylethylenediamine, di-2-hydroxyethylpropylenediamine, 2-hydroxypropylethylenediamine, and di-2-hydroxypropylethylenediamine, particularly hydroxyalkylalkylenediamines; or combinations of two or more of these. Also usable are trifunctional triamine compounds and polyamine compounds having four or more functional groups.
[0031] A particularly preferred amine-based curing agent is the above-mentioned MOCA, the chemical structure of which is as follows:
[0032] [ka]
[0033] The total amount of the curing agent is such that the ratio of the number of moles of active hydrogen groups (such as NH2) in the curing agent to the number of moles of NCO in the isocyanate-terminated urethane prepolymer (number of moles of active hydrogen groups / number of moles of NCO) is preferably 0.70 to 1.10, more preferably 0.80 to 1.00, and most preferably 0.85 to 0.95.
[0034] (Other Ingredients) In addition, catalysts and the like that are generally used in the industry may be added to the curable resin composition. The polyisocyanate component can also be added later to the curable resin composition. The weight ratio of the additional polyisocyanate component to the total weight of the isocyanate-terminated urethane prepolymer and the additional polyisocyanate component is preferably 0.1 to 10.0% by weight, more preferably 0.5 to 8.0% by weight, and particularly preferably 1.0 to 5.0% by weight. As the polyisocyanate component additionally added to the polyurethane resin curable composition, the above-mentioned polyisocyanate components can be used without particular limitation, but 4,4'-methylene-bis(cyclohexyl isocyanate) (hydrogenated MDI) is preferred.
[0035] <Process (4)> The expansion ratio of the heat-expandable microspheres in step (4) is 1.5 to 3, preferably 1.5 to 2.5, and more preferably 1.5 to 2.0. A small expansion ratio of 1.5 to 3 acts synergistically with the refinement of the microspheres by classification in step (2), and a polishing layer having extremely fine and uniform pores can be formed. The expansion ratio of the above-mentioned heat-expandable microspheres can be measured according to the procedures and conditions described in (4) of (Evaluation Method) in [Examples] below.
[0036] Step (4) can be carried out inside a mold. In this case, the method for producing a polishing pad can further include a step (casting step) of pouring the curable resin composition obtained in step (3) into a mold between steps (3) and (4). In order to prevent the curable resin composition from curing before casting, the temperature of the mold during the casting step is preferably 140°C or less, 120°C or less, 100°C or less, or 90°C or less.
[0037] The temperature of the curable resin composition (or the mold temperature) at the start of step (4) (or at the end of casting) is not particularly limited, but is preferably 75 to 140°C to prevent excessive expansion of the heat-expandable microspheres, and may also be 75 to 130°C or 75 to 120°C.
[0038] The temperature increase in step (4) can be carried out over a period of 0 to 20 minutes, 0 to 15 minutes, or 0 to 10 minutes, assuming that the start of step (4) or the end of casting is 0 minutes. The temperature after heating of the curable resin composition in step (4) can be 100 to 160° C., 100 to 140° C., 110 to 135° C., or 120 to 130° C. The temperature after heating can be maintained for a period of 5 to 60 minutes, 5 to 40 minutes, 10 to 30 minutes, or 10 to 20 minutes, assuming that the start of step (4) or the end of casting is 0 minutes.
[0039] As shown in the Examples below, step (4) can be a primary curing step carried out inside the mold, and after the primary curing step, the formed resin foam can be extracted from the mold and the resin foam can be secondary cured. Even in this case, the pores of the resulting polishing pad are formed in step (4) (primary curing), and therefore the characteristics of the pores in the polishing pad are mainly determined by the conditions in step (4). The secondary curing temperature can be 100 to 140° C., 110 to 135° C., or 120 to 130° C. The secondary curing time can be 1 to 6 hours, 1 to 5 hours, or 1 to 4 hours.
[0040] The polishing pad has a polishing layer. The polishing layer is disposed in a position in direct contact with the object to be polished, and the other parts of the polishing pad may be made of a material for supporting the polishing pad, for example, a material having high elasticity such as rubber. Depending on the rigidity of the polishing pad, the polishing layer can be made into a polishing pad.
[0041] Apart from having fine and uniform openings, the polishing pad has no significant difference in shape from a general polishing pad and can be used in the same way as a general polishing pad; for example, the polishing pad can be rotated while the polishing layer is pressed against the object to be polished, or the object to be polished can be rotated while the object is pressed against the polishing layer to polish it.
[0042] The polishing pad can be produced by a commonly known manufacturing method such as molding, slab molding, etc. First, a block of polyurethane resin or the like is formed by such a manufacturing method, and the block is sliced or the like to form a sheet-like polishing layer, which is then laminated to a support or the like. Alternatively, the polishing layer can be formed directly on the support.
[0043] More specifically, a double-sided tape is attached to the surface of the polishing layer opposite to the polishing surface of the polishing layer, and the polishing pad is cut into a predetermined shape. There is no particular limitation on the double-sided tape, and any double-sided tape known in the art can be selected and used. In addition, the polishing pad may be a single-layer structure consisting of only the polishing layer, or may be a multi-layer structure in which other layers (lower layer, support layer) are attached to the surface of the polishing layer opposite to the polishing surface.
[0044] The polishing layer may further include a polyurethane resin. The polyurethane resin is not particularly limited, but may be a cured product of a curable resin composition containing an isocyanate-terminated urethane prepolymer, a curing agent, and heat-expandable microspheres. The polishing layer can be formed by preparing a curable resin composition containing an isocyanate-terminated urethane prepolymer, a curing agent, and heat-expandable microspheres, and foaming and curing the curable resin composition.
[0045] The content of the microspheres in the polishing layer (cured product of the curable resin composition) or in the polishing layer relative to the entirety is not particularly limited, but is preferably 0.1 to 10.0% by weight, more preferably 1.0 to 5.0% by weight, and most preferably 2.0 to 4.0% by weight. When the content of the microspheres is within the above numerical range, the desired polishing properties can be obtained.
[0046] The average pore size on the surface of the polishing layer is not particularly limited, but is preferably 5 to 20 μm, more preferably 8 to 18 μm, and most preferably 10 to 15 μm. When the average pore size is within the above numerical range, the object to be polished can be polished more precisely.
[0047] The number of openings per unit area on the surface of the polishing layer is not particularly limited, but is preferably 1200 to 3000 openings / mm 2 is preferable, and 1400 to 2800 pieces / mm 2 More preferably, 1600 to 2600 pieces / mm 2 is most preferred.
[0048] The porosity of the surface of the polishing layer is not particularly limited, but is preferably 10-50%, more preferably 10-45%, and most preferably 10-40%. When the porosity is within the above-mentioned range, the retention of the slurry is good, and the polished object can be polished stably. Here, the porosity of the surface of the polishing layer means the ratio (%) of the total area of the pores present on the surface of the polishing layer to the surface area of the polishing layer.
[0049] The average pore size, the number of pores per unit area, and the pore rate on the surface of the above-mentioned polishing layer can be measured based on the procedures and conditions described in item (2) of (Evaluation Method) in the [Examples] described later.
[0050] The density of the polishing layer is not particularly limited, but is preferably 0.60 to 1.20 g / cm 3 is preferable, and 0.65 to 1.15 g / cm 3 More preferably, 0.70 to 1.10 g / cm 3When the density is within the above range, the occurrence of scratches due to polishing by-products (polishing debris) can be suppressed. The Shore D hardness of the polishing layer is not particularly limited, but is preferably 35 to 75, more preferably 40 to 70, and most preferably 45 to 65. If the Shore D hardness is too low, it becomes difficult to flatten minor irregularities. If the Shore D hardness is too high, scratches may occur on the polished object. The density and Shore D hardness of the abrasive layer can be measured according to the procedures and conditions described in item (3) of (Evaluation Method) in [Examples] below.
[0051] <Process (A)> The method for producing a polishing pad may further include, between the steps (1) and (2), a step (A) of reducing the cohesive force between the plurality of microspheres contained in the composition. In the method for producing a polishing pad of the present invention, by combining step (A) and step (2), a plurality of loosened microspheres are classified. The combined effect of reducing the cohesive force and classification makes it difficult for the microspheres to form aggregates. As a result, it is believed that the fineness and uniformity of the openings in the polishing layer are improved.
[0052] Without being bound by theory, it can be inferred as follows. It can be inferred that the composition containing microspheres before classification contains components in which a plurality of microspheres are aggregated together to form aggregates of different sizes and shapes from individual microspheres. In this case, microspheres containing aggregates of various sizes and shapes are subjected to a classification process. It can be inferred that when classification is performed, very large aggregates can be removed as coarse particles, but relatively small aggregates cannot be removed as coarse particles and remain together with individual microspheres. If such aggregates exist together with the microspheres, it is considered that poor foaming is likely to occur when forming the openings in the polishing layer, and the uniformity of the openings is reduced. Therefore, it is considered that when the openings originating from the aggregates are formed, the fineness and uniformity of the openings are impaired. Considering the above, if the cohesive force between multiple microspheres is relaxed before classification, the classification is performed on the loosened multiple microspheres, and the synergistic effect of the cohesive force relaxation and classification makes it difficult for the microspheres to form agglomerates, and as a result, it is considered that the fineness and uniformity of the openings in the polishing layer are improved.When introducing microspheres into the polishing layer, it is considered that the classification process is the most effective process for releasing the cohesive state of the microspheres compared to other processes, so it is inferred that it is important to relax the cohesive force between multiple microspheres before classification.
[0053] The above (A) is not particularly limited, but may include or consist of (A') a step of drying the composition. It is presumed that liquid components such as moisture and semi-solid components are present on the surface of the microspheres, and that the liquid components and semi-solid components stick to each other between multiple microspheres, resulting in the development of cohesive force. It is believed that the liquid components and semi-solid components can be volatilized and removed by step (A'), and as a result, the cohesive force between multiple microspheres can be alleviated.
[0054] The type of drying in step (A') is not particularly limited, and examples thereof include a method of placing the material under an atmosphere of a gas having a low dew point, which will be described later, vacuum drying, reduced pressure drying, heat drying (provided that the heating is performed at a temperature at which the microspheres do not expand), or a combination of two or more of these. Among these, it is preferable to adopt a method of placing the material under an atmosphere of a gas having a low dew point, and by adopting this method, the material can be dried without affecting the resin component or encapsulated component that forms the microspheres.
[0055] Step (A') is not particularly limited, but may include or consist of (A'') a step of placing the composition under an atmosphere of a gas having a dew point of -50°C or lower. Since a gas having a dew point of -50°C or lower contains a small amount of moisture, by carrying out step (A''), the microspheres can be dried efficiently. Here, an atmosphere of a gas having a dew point of -50°C or lower does not necessarily mean an atmosphere in which the gas is present at 100% by volume, but may also include an atmosphere in which the gas is present at a content of 90% by volume or more but less than 100% by volume. The purity of the gas is not particularly limited, but may be 90% or more, 95% or more, or 99% or more. The purity of the gas is not particularly limited, but may be 100% or less, 99.99% or less, or 99.9% or less. The above numerical ranges for gas purity may be combined in any combination.
[0056] The gas having a dew point of -50°C or less is not particularly limited, and may contain or consist of an inert gas. By using an inert gas, the oxygen concentration around the microspheres or inside a container (such as a raw material tank) that stores the microspheres in step (A'') becomes equal to or lower than the dust explosion oxygen concentration, so that even if an ignition source such as static electricity occurs, the occurrence of a dust explosion can be prevented. When a gas with a low dew point is used, the inside of the apparatus becomes dry, which tends to make a dust explosion more likely to occur, but the occurrence of a dust explosion can be prevented by using an inert gas. The type of inert gas is not particularly limited, but may include nitrogen, carbon dioxide, helium, argon, or a combination of two or more of these. Among these, nitrogen is preferred. Carbon dioxide and argon have a larger molecular weight than nitrogen, so they tend to remain at the bottom of the container (raw material tank, etc.) that stores the microspheres, and the drying efficiency of the microspheres tends to be inferior to that of nitrogen. In addition, helium has a smaller molecular weight than nitrogen, so it tends to remain at the top of the container (raw material tank, etc.) that stores the microspheres, and the drying efficiency of the microspheres tends to be inferior to that of nitrogen.
[0057] The moisture content of the composition containing the microspheres after step (A) (before step (2)) is not particularly limited, but may be 0.01 to 3 wt%, 0.01 to 2 wt%, or 0.01 to 1 wt%. The moisture content of the composition can be measured based on the loss on drying method as described in the Examples below.
[0058] The time for step (A), the drying time for step (A'), or the time for placing under a gas atmosphere for step (A'') is not particularly limited, but is preferably 0.5 to 12 hours, more preferably 0.5 to 6 hours, and most preferably 0.5 to 3 hours. By setting these times within the above numerical ranges, the relaxation of the cohesive force between a plurality of microspheres is promoted.
[0059] <Microsphere manufacturing equipment> FIG. 1 is a schematic diagram of a microsphere manufacturing apparatus applicable to the polishing pad manufacturing method of the present invention. The manufacturing apparatus of FIG. 1 includes a raw material tank 10, a classifier 20, a coarse particle recovery tank 30, and a microsphere recovery tank 40. In Fig. 1, a raw material tank 10 and a classifier 20 are connected by piping, and a composition containing the above-mentioned multiple microspheres is supplied as a raw material from the raw material tank 10 to the classifier 20. The classifier 20 is also connected by piping to a coarse particle recovery tank 30 and a microsphere recovery tank 40. The coarse particles separated by the classifier 20 and the classified microspheres are supplied to the coarse particle recovery tank 30 and the microsphere recovery tank 40, respectively.
[0060] (Raw material tank) A composition containing the above-mentioned plurality of microspheres can be charged and stored in the raw material tank 10. In the example of the raw material tank 10 shown in Fig. 1, a composition containing microspheres A, coarse particles B, etc. is stored. The above-mentioned step (1) can be carried out in the raw material tank 10. The above-mentioned step (A) can be carried out on the above-mentioned composition in the raw material tank 10. For example, the raw material tank can be filled with nitrogen having a dew point of -50°C or less, and the above-mentioned composition can be placed under the nitrogen atmosphere. In the apparatus of Fig. 1, the raw material tank 10 is integrated with the classification device 20 through piping, but this is not necessarily limited to this form. For example, the raw material tank 10 can be separated from the classification device 20, and the above composition can be stored in such raw material tank 10 to carry out the above step (A). When producing a polishing pad, the raw material tank 10 can be connected to the classification device 20 and the above composition can be supplied.
[0061] (classifier) The above step (2) can be carried out in the classifying device 20. The classifier 20 is not particularly limited, but an Elbow Jet (manufactured by Matsubo Corporation) can be used as a device for inertial classification, and a semi-free vortex centrifugal classifier (e.g., Eddy Classifier, manufactured by Nisshin Engineering Inc.), a free vortex centrifugal classifier (e.g., Dispersion Separator, manufactured by Nippon Pneumatic Industry Co., Ltd.), or a forced vortex centrifugal classifier (e.g., Turboplex, manufactured by Hosokawa Micron Corporation) can be used as a device for centrifugal classification.
[0062] FIG. 2 is a schematic diagram of a free vortex type centrifugal classifier. The device in Fig. 2 generates a free vortex inside the device by taking in a secondary gas 202. This secondary gas 202 has the function of dispersing and reclassifying particles. A raw material composition C is supplied to the device together with a primary gas 201, and then, microspheres A separated by classification are sent from an outlet 22 at the bottom of the device to the outside (such as the microsphere recovery tank 40 in Fig. 1), and coarse particles B separated by classification are sent from the bottom of the device to the outside (such as the coarse particle recovery tank 30 in Fig. 1). The type of the primary gas and / or secondary gas is not particularly limited, but an inert gas, air, or a combination of two or more of them can be used. Among these, the use of an inert gas can promote the filling of the inside of the classifier 20 with the inert gas, and can further promote the relaxation of the cohesive force of the microspheres and the suppression of dust explosions. The type of inert gas is not particularly limited, but may include nitrogen, carbon dioxide, helium, argon, or a combination of two or more of these. Among these, it is preferable to use nitrogen. Carbon dioxide and argon have a larger molecular weight than nitrogen, and the balance of the specific gravity difference with the microspheres is poor, so the relaxation of the cohesive force of the microspheres tends to be insufficient compared to nitrogen. In addition, helium has a smaller molecular weight than nitrogen, and the balance of the specific gravity difference with the microspheres is poor, so the relaxation of the cohesive force of the microspheres tends to be insufficient compared to nitrogen.
[0063] (Coarse particle collection tank) The coarse particles B separated in the classifier 20 are collected in a coarse particle collection tank 30.
[0064] (Microsphere collection tank) The microspheres A classified in the classifier 20 are collected in a microsphere collection tank 40. The collected microspheres A can be used as a component of the curable resin composition in the above-mentioned step (3).
[0065] Regarding the microsphere manufacturing apparatus, the raw material tank 10, the classifier 20, the coarse particle recovery tank 30, the microsphere recovery tank 40, two or more of these components, or all of these components, can be filled with a gas having a dew point of -50°C or less. Among these, it is preferable to fill all of the above components with a gas having a dew point of -50°C or less. By filling all of the above components with the gas in this way, it is possible to consistently prevent the microspheres from agglomerating with each other, and as a result, it is possible to prevent the formation of coarse openings during the subsequent formation of the polishing layer. In addition, by using an inert gas as the gas to be filled in all of the above components, the oxygen concentration around the microspheres or inside all of the above components becomes equal to or lower than the dust explosion oxygen concentration, and the occurrence of a dust explosion can be more effectively prevented. The means for supplying the gas having a dew point of -50°C or less to each of the above-mentioned components in the production apparatus is not particularly limited, but the gas can be supplied by connecting a gas production apparatus, and the gas production apparatus can be attached to the classifier 20. The gas produced by the gas production apparatus can be distributed throughout all of the components through piping that connects the above-mentioned components.
[0066] The material of the raw material tank 10, the classifier 20, the coarse particle recovery tank 30, and / or the microsphere recovery tank 40 is not particularly limited, and may be ceramic, stainless steel, or a combination of two or more of these. Among these, it is preferable to use ceramic, which can prevent static electricity caused by friction and, as a result, suppress the occurrence of dust explosions.
[0067] As shown in Fig. 1, the raw material tank 10, the classifier 20, the coarse particle recovery tank 30, and the microsphere recovery tank 40 can all be connected to form an apparatus, which allows the production of classified microspheres to be carried out continuously, thereby improving productivity. Also, a polishing pad manufacturing apparatus can be formed by further connecting a mixer used in step (3) and a mold used in step (4) to the microsphere recovery tank 40, which allows the process from the introduction of raw materials to the production of polishing pads to be carried out continuously while preventing the microspheres from re-agglomerating, thereby further improving productivity.
[0068] 2. Method for polishing the surface of optical or semiconductor materials In the present invention, the method for polishing the surface of an optical material or a semiconductor material includes a step of polishing the surface of an optical material or a semiconductor material using the polishing pad obtained by the above "1. Method for producing a polishing pad". The method of polishing a surface of an optical or semiconductor material may further include applying a slurry to the surface of the polishing pad, the surface of the optical or semiconductor material, or both.
[0069] (slurry) The liquid component contained in the slurry is not particularly limited, but may be water (pure water), acid, alkali, organic solvent, or a combination thereof, and may be selected depending on the material of the workpiece to be polished, the desired polishing conditions, etc. The slurry is preferably mainly composed of water (pure water), and preferably contains 80% by weight or more of water based on the entire slurry. The abrasive component contained in the slurry is not particularly limited, but may be silica, zirconium silicate, cerium oxide, aluminum oxide, manganese oxide, or a combination thereof. The slurry may contain other components, such as organic matter soluble in the liquid component and a pH adjuster. EXAMPLES
[0070] The present invention will be experimentally described by the following examples, but the following description is not intended to limit the scope of the present invention to the following examples.
[0071] (material) The materials used in Examples 1 to 4 and Comparative Examples 1 and 2 described below are listed below.
[0072] Isocyanate-terminated urethane prepolymer: Prepolymer (1) A urethane prepolymer having an NCO equivalent of 455, which contains 2,4-tolylene diisocyanate as a polyisocyanate component, polytetramethylene ether glycol having a number average molecular weight of 650 and polytetramethylene ether glycol having a number average molecular weight of 1000 as high molecular weight polyol components, and diethylene glycol as a low molecular weight polyol component.
[0073] Hardener: MOCA ··· 3,3'-dichloro-4,4'-diaminodiphenylmethane (also known as methylenebis-o-chloroaniline) (MOCA) (NH2 equivalent = 133.5)
[0074] ·Microspheres: Microsphere (1)... Expancel (registered trademark) 461DU20 (Nippon Fillite Co., Ltd.) (unexpanded type, average particle size (D50) in unexpanded state: 6 to 9 μm, expansion start temperature: 100 to 106°C, maximum expansion temperature: 143 to 151°C, shell composition: acrylonitrile-vinylidene chloride copolymer)
[0075] <Treatment for reducing the cohesive force between multiple microspheres> Nitrogen (dew point -50°C, purity 99.9%) was blown into a raw material tank (material: ceramic, capacity: 5.0 L) and the raw material tank was sufficiently filled with the nitrogen to 90% by volume or more. 0.8 kg of microspheres (1) (composition containing microspheres) were added into the raw material tank filled with the nitrogen obtained in this way. The raw material tank containing the microspheres (1) was left to stand for 2 hours under conditions of an outside air temperature of 25°C and an outside air humidity of 40% RH to obtain microspheres (A) (composition containing microspheres). Meanwhile, another raw material tank (material: ceramic, capacity: 5.0 L) was prepared, and the inside was left filled with air (25°C, 40% RH) without filling it with gas such as nitrogen. 0.8 kg of microspheres (1) (composition containing microspheres) was put into the raw material tank filled with air. The raw material tank containing the microspheres (1) was left to stand for 2 hours under conditions of an outside air temperature of 25°C and an outside air humidity of 40% RH to obtain microspheres (B) (composition containing microspheres). Then, 10 g of each of the microspheres (1), (A), and (B) before being placed in the raw material tank was weighed out and left to stand in a desiccator (room temperature) containing dried silica gel for 2 days, and the moisture content (weight%) was calculated from the weight loss (loss on drying method). The measurement results are shown in Table 1.
[0076] [Table 1]
[0077] From the results in Table 1, the microspheres (A) obtained by standing in a raw material tank filled with nitrogen had a lower moisture content than the microspheres (1) before standing. On the other hand, the microspheres (B) obtained by leaving the material in the raw material tank filled with air had a moisture content equivalent to that of the microspheres (1) before leaving the material. It is believed that when the moisture content of the microspheres is low, there is less moisture present on the surfaces of the microspheres. Therefore, the surfaces of adjacent microspheres come into contact with each other in a state of low moisture (dry state), so that the cohesive force between adjacent microspheres is weak and they are likely to come apart. Therefore, it is believed that the cohesive force between adjacent microspheres (A) is weaker and they are likely to come apart more easily than microspheres (1) and (B).
[0078] <Process for classifying microspheres> 0.8 kg of the microspheres (A) were put into a free vortex type centrifugal classifier shown in Figure 2, and nitrogen (dew point -50°C, purity 99.9%) was used as the primary gas and secondary gas, and coarse particles were removed by centrifugal classification to obtain 0.28 kg of classified microspheres (A) (hereinafter referred to as "microspheres (A-1)"). The coarse particles and microspheres (A-1) were collected in separate collection tanks. Nitrogen (dew point -50°C, purity 99.9%) was continuously blown into the classifier and the collection tanks for the coarse particles and the classified microspheres, filling them with the nitrogen. Moreover, the microspheres (A) were classified in the same manner as in obtaining the microspheres (A-1) above, except that the pressure of the secondary gas in the classification treatment was changed so that the relative value (times) when the pressure of the secondary gas used to obtain the microspheres (A-1) above was taken as 1 was as shown in Table 2, and coarse particles were removed to obtain classified microspheres (A) (hereinafter referred to as "microspheres (A-2) and (A-3)", respectively). Further, the microspheres (B) were classified in the same manner as in obtaining the microspheres (A-1) except that 0.8 kg of the microspheres (B) was used instead of 0.8 kg of the microspheres (A), and coarse particles were removed to obtain classified microspheres (B) (hereinafter referred to as "microspheres (B-1)").
[0079] The yield (%) of the obtained microspheres (A-1) to (A-3) and microspheres (B-1) was calculated based on the following formula.
[0080]
number
[0081] Moreover, the particle sizes (D10, D50, D90 (μm)) of the obtained microspheres (A-1) to (A-3) and microspheres (B-1) and the raw material microsphere (1) were measured using a laser diffraction particle size distribution analyzer (Mastersizer 2000, manufactured by Spectris Co., Ltd.). The measured yield (%) and particle size are shown in Table 2.
[0082] [Table 2]
[0083] Example 1 100 g of prepolymer (1) was prepared as component A, 26.3 g of MOCA, a hardener, was prepared as component B, and 3.5 g of the microspheres (A-1) obtained as described above was prepared as component C. Note that the amounts are listed in grams to show the ratio of each component, but it is sufficient to prepare the required weight (parts) depending on the size of the block. The amounts below will also be listed in grams (parts). Components A and C were mixed, and the resulting mixture of components A and C was degassed under reduced pressure. Also, MOCA, which is component B, was degassed under reduced pressure. The degassed mixture of components A and C and the degassed component B were fed to a mixer to obtain a mixture of components A, B, and C. In the obtained mixture of components A, B, and C, the ratio of the number of moles of NH2 in MOCA of component B to the number of moles of NCO in prepolymer (1) of component A (number of moles of NH2 / number of moles of NCO) was 0.9. The content of microspheres (A) of component C in the entire mixture was 2.7% by weight. The obtained mixed liquid of components A, B, and C was poured into a mold (850 mm x 850 mm square shape) heated to 80°C. After the end of the pouring, the mold was heated and raised in temperature so that the temperature 10 minutes after the end of the pouring was 120°C. After that, the mold was maintained at 120°C for 10 to 20 minutes after the end of the pouring to perform primary curing and form a resin foam. The formed resin foam was removed from the mold and secondary cured in an oven at 120°C for 4 hours. The obtained resin foam after secondary curing was allowed to cool to 25°C and then heated again in an oven at 120°C for 5 hours. The obtained heated resin foam was sliced in the thickness direction to a thickness of 1.3 mm to prepare a urethane sheet, and a double-sided tape was attached to the back side of this urethane sheet to prepare a polishing pad.
[0084] (Examples 2 and 3) Except for using 3.5g of the microspheres (A-2) or (A-3) instead of 3.5g of the microspheres (A-1) of component C in Example 1, a urethane sheet was prepared in the same manner as in Example 1, and the polishing pads of Examples 2 and 3 were obtained (Example 2: microspheres (A-2), Example 3: microspheres (A-3)). In the obtained mixture of components A, B, and C, the ratio of the number of moles of NH2 in MOCA of component B to the number of moles of NCO in prepolymer (1) of component A (number of moles of NH2 / number of moles of NCO) was 0.9. The content of microspheres (A-2) or (A-3) of component C relative to the entire mixture was 2.7% by weight.
[0085] Example 4 A urethane sheet was prepared in the same manner as in Example 1, except that 3.5 g of the microspheres (B-1) were used instead of 3.5 g of the microspheres (A-1) of the component C in Example 1, to obtain a polishing pad of Example 4. In the obtained mixture of components A, B, and C, the ratio of the number of moles of NH2 in MOCA of component B to the number of moles of NCO in prepolymer (1) of component A (number of moles of NH2 / number of moles of NCO) was 0.9. The content of microspheres (B-1) of component C in the entire mixture was 2.7% by weight.
[0086] Comparative Example 1 In the same manner as in Example 1, a mixed liquid of components A, B and C was obtained. In the obtained mixed solution of components A, B, and C, the ratio of the number of moles of NH2 of MOCA of component B to the number of moles of NCO of prepolymer (1) of component A (number of moles of NH2 / number of moles of NCO) and the content of microspheres (A) of component C relative to the entire mixed solution were the same as in Example 1. The obtained mixed liquid of components A, B, and C was poured into a mold (850 mm x 850 mm square shape) heated to 90°C. After the end of the pouring, the mold was heated and raised in temperature so that the temperature 10 minutes after the end of the pouring was 140°C. After that, the mold was maintained at 140°C for 10 to 20 minutes after the end of the pouring to perform primary curing and form a resin foam. The formed resin foam was removed from the mold and secondary cured in an oven at 130°C for 4 hours. The obtained resin foam after secondary curing was allowed to cool to 25°C and then heated again in an oven at 130°C for 5 hours. The obtained heated resin foam was sliced in the thickness direction to a thickness of 1.3 mm to prepare a urethane sheet, and a double-sided tape was attached to the back side of this urethane sheet to prepare a polishing pad.
[0087] Comparative Example 2 A urethane sheet was prepared in the same manner as in Comparative Example 1, except that 3.5 g of the microspheres (B-1) were used instead of 3.5 g of the microspheres (A-1) of the component C in Comparative Example 1, to obtain a polishing pad of Comparative Example 2. In the obtained mixture of components A, B, and C, the ratio of the number of moles of NH2 in MOCA of component B to the number of moles of NCO in prepolymer (1) of component A (number of moles of NH2 / number of moles of NCO) was 0.9. The content of microspheres (B-1) of component C in the entire mixture was 2.7% by weight.
[0088] (Evaluation method) The polishing pads or urethane sheets of Examples 1 to 4 and Comparative Examples 1 and 2 were measured or evaluated for the following: (1) cross-section observation by SEM, (2) average pore size, pore ratio, and pore number, (3) density and Shore D hardness, (4) expansion ratio, (5) scratches, and (6) polishing rate. The measurement results are shown in Tables 3 and 4 below.
[0089] (1) Observation of cross section using SEM Each polishing pad was cut along the thickness direction, and the cross section was photographed with a scanning electron microscope (SEM) (JSM-5000LV, manufactured by JEOL Ltd.) The obtained SEM cross-sectional photographs are shown in Figures 3 to 8. FIG. 3 is a cross-sectional photograph of the polishing pad of Example 1 measured at a magnification of 200 times. FIG. 4 is a cross-sectional photograph of the polishing pad of Example 2 measured at a magnification of 200 times. FIG. 5 is a cross-sectional photograph of the polishing pad of Example 3 measured at a magnification of 200 times. FIG. 6 is a cross-sectional photograph of the polishing pad of Example 4 measured at a magnification of 200 times. FIG. 7 is a cross-sectional photograph of the polishing pad of Comparative Example 1 measured at a magnification of 200 times. FIG. 8 is a cross-sectional photograph of the polishing pad of Comparative Example 2 measured at a magnification of 200 times.
[0090] (2) Average pore diameter, porosity ratio, and number of pores Three areas (each rectangular with a length of 0.5 mm x width of 0.7 mm) were randomly selected from the surface of the polishing layer of the polishing pad without bias, and each area was observed at 400 times magnification using a laser microscope (VK-X1000, manufactured by KEYENCE). Each image obtained (rectangle with a length of 0.5 mm x width of 0.7 mm) was binarized using image processing software (WinROOF2018 Ver4.0.2, manufactured by Mitani Shoji) to confirm the openings, and the circle equivalent diameter (opening diameter) was calculated from the area of each opening. The cutoff value (lower limit) of the opening diameter was set to 5 μm, and noise components were excluded. ·Average pore diameter All the pore diameters contained in each of the above regions (images) were averaged to calculate the average pore diameter for each region. The average pore diameters of the three regions thus obtained were further averaged to calculate the final average pore diameter. ·Open area ratio The ratio (%) of the total area of the open parts per the area of each region (image) was calculated (total area of the open parts / area of the image (region) × 100). The opening ratios of the three regions thus obtained were further averaged to calculate the final opening ratio. ·Number of openings The number of apertures per area of each of the above regions (images) (number / mm 2 The numbers of pores in the three regions thus obtained were then averaged to calculate the final number of pores.
[0091] (3) Density and Shore D hardness (density) Density of urethane sheet (g / cm 3 ) was measured in accordance with the Japanese Industrial Standard (JIS K 6505). (Shore D hardness) The Shore D hardness of the urethane sheet was measured using a D-type hardness tester in accordance with the Japanese Industrial Standards (JIS-K-6253). Here, the measurement sample was obtained by stacking multiple urethane sheets as necessary so that the total thickness was at least 4.5 mm.
[0092] (4) Expansion ratio The expansion ratio of the microspheres was calculated based on the following formula. Expansion ratio = (average pore size calculated in (2) above) / (average particle size of microspheres before expansion (D50)) *The average particle size (D50) of the microspheres before expansion was 6 μm.
[0093] (5) Scratch The evaluation of scratches was carried out by polishing the substrate under the conditions described below (Polishing Test), and measuring the substrate after polishing using a wafer surface inspection device (KLA Tencor, Surfscan SP5) in high sensitivity measurement mode to detect defects (surface defects) with a size of 110 nm or more on the entire substrate. For each detected defect, an SEM image taken using a review SEM was analyzed, and the defects were classified into "particles," "pad debris," and "scratches," and the number of scratches among them was counted. The result is the average result of n4. Here, the classification "particles" refers to fine particles remaining on the surface of the object to be polished, the classification "pad debris" refers to debris from the polishing layer attached to the surface of the object to be polished, and the classification "scratches" refers to scratches on the surface of the object to be polished.
[0094] (Polishing test) Polishing machine used: F-REX300X (manufactured by Ebara Corporation) Disk: A188 (3M) Abrasive temperature: 20℃ Polishing platen rotation speed: 85 rpm Polishing head rotation speed: 86 rpm Grinding pressure: 3.5psi Polishing slurry: CSL-9044C (a mixture of CSL-9044C stock solution and pure water at a weight ratio of 1:1) (manufactured by Fujimi Corporation) Polishing slurry flow rate: 200ml / min Polishing time: 60 seconds Workpiece: Cu film substrate (disc-shaped, 300 mm in diameter) Pad break: 35N 10 minutes Conditioning: Ex-situ, 35N, 4 scans
[0095] (6) Polishing rate The polishing rate of the polishing pad was measured as follows for an object polished under the polishing conditions described in (5) (Polishing test) above. The Cu film substrate before and after the polishing test was measured in the diameter direction on the substrate, and the thickness at those points before and after the polishing test was measured. Based on the measured thickness, the average thickness before the polishing test and the average thickness after the polishing test were calculated, and the average polished thickness was calculated by taking the difference between these average values. The polishing rate was calculated by dividing the average polished thickness obtained by the polishing time. The thickness was measured using a four-probe sheet resistance measuring device (manufactured by KLA Tencor, product name "RS-200", measurement: DBS mode).
[0096] [Table 3]
[0097] [Table 4]
[0098] The polishing pads of Examples 1 to 3 were produced by expanding heat-expandable microspheres 1.5 to 3 times larger than the original size, which were classified after a process for reducing the cohesive force between the microspheres. The polishing pad of Example 4 was produced by expanding heat-expandable microspheres 1.5 to 3 times larger than the original size, which were classified without a process for reducing the cohesive force between the microspheres. On the other hand, the polishing pad of Comparative Example 1 was produced by using heat-expandable microspheres that had been classified after a process for reducing the cohesive force between the microspheres, and expanding the heat-expandable microspheres by more than three times their size.The polishing pad of Comparative Example 2 was produced by using heat-expandable microspheres that had been classified without a process for reducing the cohesive force between the microspheres, and expanding the heat-expandable microspheres by more than three times their size.
[0099] 3 to 8, it was found that fine and uniform openings were obtained in the polishing pads of Examples 1 to 4. On the other hand, it was found that the openings were large and non-uniform in the polishing pads of Comparative Examples 1 and 2. In this regard, the results of Table 3 show that the polishing pads of Examples 1 to 4 have an average pore size of 15 μm or less, a pore ratio of 30 to 35%, and a pore number of 1600 to 2600 pores / mm 2 On the other hand, the polishing pads of Comparative Examples 1 and 2 had an average pore size of 20 μm or more, a pore ratio of 35% or more, and a pore number of 1200 to 1300 pores / mm 2 Therefore, it was confirmed that the pores were large and non-uniform.
[0100] In addition, from the results of Table 4, the polishing pads of Examples 1 to 4 had a small number of scratches, and the occurrence of scratches was sufficiently suppressed, and the polishing rate exceeded 8000 Å, showing sufficient polishing performance. It is presumed that the polishing pads of Examples 1 to 4 have fine and uniform openings, and the fine irregularities resulting from the openings act as polishing points, thereby showing high polishing performance. On the other hand, the polishing pads of Comparative Examples 1 and 2 had a large number of scratches, and it was found that the occurrence of scratches could not be sufficiently suppressed compared to Examples 1 to 4. In addition, the polishing rate was also below 7000 Å, showing lower polishing performance compared to Examples 1 to 4.
[0101] 3 to 5 and the results in Tables 3 and 4, it was found that the polishing pads of Examples 1 to 3 were superior in terms of the fineness and uniformity of the pores obtained and the suppression of the occurrence of scratches compared to the polishing pad of Example 4. From these results, it was found that although the step of reducing the cohesive force between the multiple microspheres is not essential, it is effective in improving the fineness and uniformity of the pores and suppressing the occurrence of scratches.
[0102] From the above results, it was found that the polishing pad obtained by the production method of the present invention, which includes the steps of: (1) preparing a composition containing a plurality of microspheres; (2) classifying the composition to remove coarse particles and obtaining classified microspheres containing heat-expandable microspheres; (3) mixing the classified microspheres with an isocyanate-terminated urethane prepolymer and a curing agent to form a curable resin composition; and (4) curing the curable resin composition to form the polishing layer, in which the heat-expandable microspheres are expanded 1.5 to 3 times, has fine and uniform pores. [Explanation of symbols]
[0103] 10…Raw material tank 20...Classifying device 22...Exit 201... Primary gas 202...Secondary gas 30…Coarse particle collection tank 40...Microsphere collection tank A: Microspheres B...coarse particles C...Composition
Claims
1. A method for producing a polishing pad having a polishing layer, comprising the steps of: (1) providing a composition comprising a plurality of microspheres; (2) classifying the composition to remove coarse particles and obtain classified microspheres containing heat-expandable microspheres; (3) mixing the classified microspheres with an isocyanate-terminated urethane prepolymer and a curing agent to form a curable resin composition; and (4) A step of curing the curable resin composition to form the polishing layer, the step including expanding the heat-expandable microspheres by 1.5 to 3 times. A method for producing the polishing pad comprising the steps of:
2. 2. The method for producing a polishing pad according to claim 1, further comprising the step of: (A) reducing the cohesive force between the microspheres contained in the composition between the steps (1) and (2).
3. The method for producing a polishing pad according to claim 2 , wherein the step (A) comprises the step (A′) of drying the composition.
4. The method for producing a polishing pad according to claim 3, wherein the step (A') comprises the step of (A'') placing the composition in an atmosphere of a gas having a dew point of -50°C or lower.
5. The method for producing a polishing pad according to claim 4, wherein the gas having a dew point of −50° C. or less includes an inert gas.
6. The method for producing a polishing pad according to claim 1 or 2, wherein the classification in the step (2) is centrifugal classification.
7. 3. A method for polishing a surface of an optical or semiconductor material, comprising the step of polishing the surface of the optical or semiconductor material using a polishing pad obtainable by the method according to claim 1 or 2.
Citation Information
Patent Citations
Method for producing a chemical mechanical polishing layer with improved uniformity - Patents.com
JP7048395B2