Composition containing cellulose nanofiber
A composition of cellulose nanofibers and hydrophilic rubber enhances dispersibility and mechanical properties in rubber composites, addressing the dispersibility challenges and improving hardness and tensile strength.
Patent Information
- Application Number
- JP2024043525
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2023-03-30
- Filing Date
- 2024-03-19
- Publication Date
- 2024-10-11
AI Technical Summary
Existing technologies face challenges in achieving satisfactory dispersibility of cellulose nanofibers in rubber composites, particularly when the nanofiber content is high, which affects the mechanical properties of the resulting rubber molded articles.
A composition comprising cellulose nanofibers and a hydrophilic group-containing rubber derived from rubber latex, with a specific toluene insoluble content ratio, is used to enhance dispersibility and mechanical properties such as hardness, storage modulus, and tensile strength.
The composition effectively disperses cellulose nanofibers in rubber, resulting in rubber molded articles with improved mechanical properties, including hardness, storage modulus, and tensile strength.
Smart Images

Figure 2024144239000001 
Figure 2024144239000002 
Figure 2024144239000003
Abstract
Description
[Technical field]
[0001] One aspect of the present invention relates to a composition, a masterbatch, a rubber composite, and a cured rubber product, each of which includes cellulose nanofibers. [Background technology]
[0002] Conventionally, rubber molded articles are required to have a high level of balance among various properties such as mechanical strength, flexibility, abrasion resistance, and processability, and it is common to incorporate a filler into the rubber molded article for the purpose of improving, for example, hardness, elastic modulus, etc. In order for such a filler-containing rubber molded article to exhibit the desired properties, it is important that the filler is well dispersed in the rubber.
[0003] In recent years, due to the growing awareness of environmental issues, various attempts have been made to use cellulose, which is a low-density and renewable material, as a filler to be contained in rubber molded bodies. Among them, cellulose nanofibers are extremely promising as a filler for polymer molded bodies because they provide a good reinforcing effect per amount used to the polymer molded body when combined with various polymers to form the polymer molded body. If such cellulose nanofibers can be used in rubber molded bodies, it is possible to provide rubber molded bodies that have low specific gravity and excellent physical properties, can be used for a variety of purposes, and are also advantageous in terms of transportation costs and disposal costs. However, since cellulose nanofibers are essentially hydrophilic due to the contribution of hydroxyl groups in cellulose, it is difficult to mix them with rubber, which is generally a highly hydrophobic material, and various attempts have been made in the prior art to improve the dispersibility of cellulose nanofibers in rubber.
[0004] Patent Document 1 describes a cellulose nanofiber-containing aqueous resin composition comprising cellulose nanofibers and a polymer, characterized in that the composition is produced by polymerizing a polymerizable unsaturated monomer in an aqueous dispersion containing cellulose nanofibers in which a water-soluble cellulose compound is also present, the polymer being a copolymer obtained by polymerizing two or more types of ethylenically unsaturated monomers having vinyl groups, and the cellulose nanofiber-containing resin sheet produced from the aqueous resin composition has a relative tensile elongation within a specific range, and the formed resin sheet exhibits ultra-extensibility.
[0005] Patent Document 2 describes a composite resin composition containing an aqueous dispersion medium, resin particles emulsified in the aqueous dispersion medium, and cellulose nanofibers dispersed in the aqueous dispersion medium, wherein the resin particles include at least one type selected from the group consisting of (meth)acrylic resin particles, styrene-based resin particles, and (meth)acrylonitrile-based resin particles, and wherein when a liquid obtained by diluting the composite resin composition with water is dropped onto a measurement substrate and dried, and a sample is observed with an atomic force microscope, a structure in which the cellulose nanofibers are dispersed and the resin particles are clinging to the cellulose nanofibers is observed.
[0006] Patent Document 3 describes a composite resin composition containing an aqueous dispersion medium, resin particles emulsified in the aqueous dispersion medium, and cellulose nanofibers dispersed in the aqueous dispersion medium, wherein the resin particles include polymer particles formed by polymerization of a monomer component including an ethylenically unsaturated monomer surrounded by a cross-linking reactive polymer, and a protective layer formed of the cross-linking reactive polymer covering the polymer particles, wherein the cross-linking reactive polymer includes a structural unit derived from a reactive group-containing polymerizable monomer having a reactive group, and includes, as the structural unit, a specific amount of a structural unit derived from a carboxy group-containing polymerizable monomer having a carboxy group, and the composite resin composition has a haze value per specific content of cellulose nanofiber that is less than a specific value.
[0007] Patent Document 4 describes a rubber composition prepared using a master batch obtained by mixing rubber latex, microfibrillated plant fibers, and a cationic polymer, in which the amount of the cationic polymer added to the rubber component in the rubber latex is within a specific range. [Prior art documents] [Patent documents]
[0008] [Patent Document 1] JP 2020-094180 A [Patent Document 2] JP 2020-200436 A [Patent Document 3] JP 2022-077708 A [Patent Document 4] JP 2014-047328 A Summary of the Invention [Problem to be solved by the invention]
[0009] The techniques described in Patent Documents 1 to 4 can improve the dispersibility of cellulose nanofibers in rubber to a certain extent in a rubber composite containing cellulose nanofibers and rubber. However, when the cellulose nanofiber content in the rubber composite is relatively high, the dispersibility of the cellulose nanofibers in the rubber is not necessarily satisfactory.
[0010] The present invention aims to solve the above-mentioned problems and provide a cellulose nanofiber-containing composition, a cellulose nanofiber-containing masterbatch, a cellulose nanofiber-containing rubber composite, and a cellulose nanofiber-containing cured rubber product, in which cellulose nanofibers are well dispersed in rubber and which can form rubber molded products with excellent mechanical properties (particularly hardness, storage modulus, modulus, and tensile strength). [Means for solving the problem]
[0011] The present invention encompasses the following items. [1] A composition comprising cellulose nanofibers and a first rubber component which is a hydrophilic group-containing rubber derived from rubber latex, the first rubber component comprises a toluene-insoluble component, A composition, wherein when 0.5 g of the composition is stirred in 30 mL of toluene at 25°C, a toluene insoluble ratio, which is the ratio of dissolved residue to 100% by mass of solids in the composition, is 30% by mass or more and 99% by mass or less. [2] 2. The composition according to item 1, comprising 1 to 200 parts by mass of the first rubber component per 100 parts by mass of the cellulose nanofibers. [3] Item 3. The composition according to item 1 or 2, wherein the dissolved residue consists of the cellulose nanofibers and the first rubber component. [4] 4. The composition according to any one of items 1 to 3, wherein the first rubber component is a styrene-butadiene rubber. [5] 5. The composition according to any one of items 1 to 4, wherein a ratio of butadiene monomer units to all monomer units of the first rubber component is 20% by mass or more and 95% by mass or less. [6] 6. The composition according to any one of items 1 to 5, wherein the first rubber component has a glass transition temperature of 10° C. or lower. [7] 7. The composition according to any one of items 1 to 6, wherein the first rubber component has a residual monomer amount of 10% by mass or less. [8] 8. The composition according to any one of items 1 to 7, wherein the hydrophilic group of the first rubber component is at least one selected from the group consisting of a carboxy group, a hydroxy group, a sulfonyl group, and a phosphate group. [9] 9. The composition according to any one of items 1 to 8, wherein the first rubber component has a weight average molecular weight (Mw) of 5,000 or more and 400,000 or less.
[10] 10. The composition according to any one of items 1 to 9, further comprising a poorly soluble surfactant having a solubility of 20 g or less in 100 g of water at 25° C.
[11] 11. The composition of claim 10, wherein the surfactant further comprises two or more selected from the group consisting of alkylbenzenesulfonic acids, alkylsulfonic acids, alkylsulfosuccinic acids, polyoxyethylene alkylsulfuric acids, polyoxyethylene alkylarylsulfuric acids, polyoxyethylene distyryl phenyl ether sulfonic acids and their alkali metal or ammonium salts; fatty acid soaps; alkyltrimethylammonium bromides; alkylpyridinium bromides; imidazolinium laurates; polyoxyethylene alkylaryl ethers; polyoxyethylene alkyl ethers; polyoxyethylene sorbitan fatty acid esters; sorbitan fatty acid esters; polyoxyethylene oxypropylene block copolymers; and polyoxyethylene distyryl phenyl ethers.
[12] 12. The composition according to any one of items 1 to 11, which is in the form of a sheet, a pellet or a powder.
[13] An aqueous dispersion comprising cellulose nanofibers and a first rubber component which is a hydrophilic group-containing rubber derived from rubber latex, the first rubber component comprises a toluene-insoluble component, An aqueous dispersion, wherein when 0.5 g of a composition obtained by drying the aqueous dispersion is stirred in 30 mL of toluene at 25°C, the toluene-insoluble ratio, which is the ratio of dissolved residue to 100% by mass of solids in the composition, is 30% by mass or more and 99% by mass or less.
[14] A method for producing the composition according to any one of items 1 to 12, Obtaining an aqueous dispersion by mixing cellulose nanofibers with a rubber latex containing rubber particles having a hydrophilic group; and Optionally, drying the aqueous dispersion. A method comprising:
[15] Item 15. The method according to item 14, wherein the average particle size of the rubber particles is 1 μm or less.
[16] A masterbatch which is a kneaded product containing the composition according to any one of items 1 to 12 and a second rubber component.
[17] Item 17. The masterbatch according to item 16, wherein the second rubber component comprises one or more selected from the group consisting of natural rubber, styrene butadiene rubber, butadiene rubber, isoprene rubber, chloroprene rubber, ethylene propylene diene rubber, and butyl rubber and derivatives thereof.
[18] Item 18. The masterbatch according to item 16 or 17, comprising 10 parts by mass to 50 parts by mass of cellulose nanofibers per 100 parts by mass in total of the first rubber component and the second rubber component.
[19] A rubber composite, which is a kneaded product containing a component derived from the composition according to any one of items 1 to 12 or the masterbatch according to any one of items 16 to 18, and a third rubber component.
[20] Item 20. The rubber composite according to item 19, comprising 1 part by mass or more and 15 parts by mass or less of cellulose nanofiber per 100 parts by mass in total of the first rubber component, the second rubber component, and the third rubber component. [twenty one] 21. A rubber cured product, which is a cured product of the rubber composite according to item 19 or 20. [twenty two] 19. A method for producing a masterbatch according to any one of items 16 to 18, A method comprising a step of mixing a composition comprising cellulose nanofibers and a first rubber component with a second rubber component. [twenty three] 21. The method for producing a rubber composite according to item 19 or 20, A step of mixing a composition containing cellulose nanofibers and a first rubber component with a second rubber component to prepare a master batch; and mixing the master batch with a third rubber component to prepare a rubber composite; A method comprising: [twenty four] 21. The method for producing a rubber composite according to item 19 or 20, A method comprising the step of mixing a composition comprising cellulose nanofibers and a first rubber component with a third rubber component to prepare a rubber composite. [twenty five] 22. A method for producing a rubber cured product according to claim 21, A step of mixing a composition containing cellulose nanofibers and a first rubber component with a second rubber component to prepare a master batch; mixing the master batch with a third rubber component to prepare a rubber composite; and curing the rubber composite; A method comprising:
[26] 22. A method for producing a rubber cured product according to claim 21, A step of preparing a rubber composite by mixing a composition containing cellulose nanofibers and a first rubber component with a third rubber component; and curing the rubber composite; A method comprising: Effect of the Invention
[0012] According to one aspect of the present invention, there can be provided a cellulose nanofiber-containing composition, a cellulose nanofiber-containing masterbatch, a cellulose nanofiber-containing rubber composite, and a cellulose nanofiber-containing cured rubber product, in which the cellulose nanofibers are well dispersed in the rubber and which can form a rubber molded product with excellent mechanical properties (particularly hardness, storage modulus, modulus, and tensile strength). DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0013] Hereinafter, exemplary embodiments of the present invention (hereinafter, abbreviated as "present embodiments") will be described, but the present invention is not limited to these embodiments. Note that, unless otherwise specified, the characteristic values of the present disclosure are values measured by the method described in the [Examples] section of the present disclosure or a method that is understood to be equivalent to the above by a person skilled in the art.
[0014] ≪Composition≫ One aspect of the present invention provides a composition (also referred to simply as a composition or a rubber composition in this disclosure) comprising cellulose nanofibers and a first rubber component. The rubber composition may be combined with at least a second rubber component of the present disclosure to form a master batch, and may be combined with at least a third rubber component of the present disclosure to form a rubber composite.
[0015] Cellulose nanofibers are essentially hydrophilic due to their hydroxyl groups, while rubber is essentially hydrophobic, and it is usually difficult to uniformly disperse cellulose nanofibers in rubber. For example, the dispersibility of cellulose nanofibers in rubber can be improved to some extent by using modified rubber, but from the viewpoint of application to various uses, it is desired that cellulose nanofibers exhibit good dispersibility in combination with a wide range of rubber types. The present inventors have conducted various studies from this viewpoint and found that by using a composition containing cellulose nanofibers and the first rubber component of the present disclosure, cellulose nanofibers can be well dispersed in rubber in a master batch, rubber composite, or rubber composition relating to a combination of the composition and a wide range of rubber types. In one embodiment, the composition, master batch, rubber composite, or cured rubber of the present disclosure has excellent mechanical properties, such as hardness, storage modulus, modulus, and tensile strength.
[0016] In one embodiment, when 0.5 g of the composition is stirred in 30 mL of toluene at room temperature (25° C.), the toluene-insoluble content ratio (also referred to simply as the toluene-insoluble content ratio of the composition in this disclosure), which is the ratio of dissolved residue to 100% by mass of solid content in the composition, is 30% by mass or more and 99% by mass or less. In this disclosure, the amount of solid content in the composition and the toluene-insoluble content ratio of the composition or rubber component are values determined in more detail by the procedure described in the section [Examples] of this disclosure.
[0017] While substantially all of the cellulose nanofibers are insoluble in toluene, the first rubber component typically has a toluene-insoluble portion and a toluene-soluble portion. Thus, the toluene-insoluble portion in the composition is composed of substantially the entire amount of the cellulose nanofibers in the composition, the toluene-insoluble portion of the first rubber component, and other toluene-insoluble portions that may be optionally contained in the composition. In a typical embodiment, the composition can be substantially free of toluene-insoluble portions other than the insoluble portions of the cellulose nanofibers and the first rubber component. That is, in a typical embodiment, the dissolved residue is composed of the cellulose nanofibers and the toluene-insoluble portion of the first rubber component. In a more typical embodiment, the composition is composed of the cellulose nanofibers and the first rubber component. In a typical embodiment, the toluene-insoluble portion ratio of the composition is controlled within a predetermined range of the present disclosure by adjusting the cellulose nanofiber content of the composition and the toluene-insoluble portion ratio of the first rubber component.
[0018] Specifically, the toluene insoluble ratio of the composition increases when the cellulose nanofiber content in the composition is increased, but decreases when the toluene insoluble ratio of the first rubber component is increased, but decreases when the toluene insoluble ratio is decreased. In one embodiment, the toluene insoluble ratio of the composition is adjusted to a specific range by increasing the cellulose nanofiber content and decreasing the toluene insoluble ratio of the first rubber component. In such a composition, a first rubber component having a low toluene insoluble ratio, i.e., a first rubber component having a low gel fraction, is highly fluid and easily enters the gaps between cellulose nanofibers, so that the dispersibility of a large amount of cellulose nanofibers can be improved well even with a relatively small amount of use. A composition having a high cellulose nanofiber content and a low toluene insoluble ratio of the first rubber component can be advantageous for forming a rubber molded body containing a high amount of cellulose nanofibers and having excellent mechanical properties. On the other hand, the inclusion of a toluene insoluble component in the first rubber component can suppress re-aggregation of cellulose nanofibers due to excessive flow of the rubber component in the composition.
[0019] From the viewpoint of containing a high amount of cellulose nanofibers in the composition, in one embodiment, the toluene insoluble matter ratio of the composition is 30% by mass or more, or 40% by mass or more, or 50% by mass or more, or 60% by mass or more, or 70% by mass or more, and from the viewpoint of obtaining a good effect of improving the dispersibility of cellulose nanofibers due to the contribution of the first rubber component having a relatively low toluene insoluble matter ratio, in one embodiment, the toluene insoluble matter ratio is 99% by mass or less, or 90% by mass or less, or 85% by mass or less.
[0020] In one embodiment, the cellulose nanofiber content in the composition is 30% by mass or more, or 50% by mass or more, or 60% by mass or more, and in another embodiment, 85% by mass or less, or 75% by mass or less, or 70% by mass or less. In a preferred embodiment, from the viewpoint of using a large amount of cellulose nanofibers, the cellulose nanofiber content in the composition is 50% by mass or more, or 60% by mass or more, or 70% by mass or more.
[0021] In one embodiment, the content of the first rubber component in the composition is 20% by mass or more, or 40% by mass or more, or 50% by mass or more, and in one embodiment, 70% by mass or less, or 60% by mass or less, or 55% by mass or less. In a preferred embodiment, from the viewpoint of using a large amount of cellulose nanofibers, the content of the first rubber component in the composition is 50% by mass or less, or 40% by mass or less, or 30% by mass or less. Preferred examples of each component of the rubber composition of the present embodiment will now be described.
[0022] In the composition, the amount of the first rubber component per 100 parts by mass of cellulose nanofiber is preferably 1 part by mass or more, or 30 parts by mass or more, or 40 parts by mass or more, from the viewpoint of obtaining the above-mentioned advantages of the rubber latex, and is preferably 200 parts by mass or less, or 100 parts by mass or less, or 50 parts by mass or less, from the viewpoint of containing an appropriate amount of cellulose nanofiber to obtain the advantages of these components.
[0023] <Cellulose nanofiber> The rubber composition according to one embodiment includes cellulose nanofibers. As raw materials for the cellulose nanofibers, natural cellulose and regenerated cellulose can be used. As natural cellulose, wood pulp obtained from wood species (broadleaf or coniferous trees), non-wood pulp obtained from non-wood species (cotton, bamboo, hemp, bagasse, kenaf, cotton linters, sisal, straw, etc.), and cellulose aggregates produced by animals (e.g., ascidians), algae, and microorganisms (e.g., acetic bacteria) can be used. As regenerated cellulose, regenerated cellulose fibers (viscose, cupra, tencel, etc.), cellulose derivative fibers, and ultrafine threads of regenerated cellulose or cellulose derivatives obtained by electrospinning can be used.
[0024] The cellulose nanofiber refers to fine cellulose fibers that are mechanically defibrated by a grinding method such as a high-pressure homogenizer, a microfluidizer, a ball mill, a disk mill, or a mixer (e.g., a homomixer) after treating a cellulose raw material such as pulp with hot water at 100°C or higher to hydrolyze and weaken the hemicellulose. In one embodiment, the cellulose nanofiber has a number average fiber diameter of 1 nm or more and 1000 nm or less. The cellulose nanofiber may be chemically modified as described below, but in terms of the reinforcing effect as a filler, it is preferable to use a non-chemically modified cellulose nanofiber. For example, cellulose nanofibers that have been defibrated by chemical oxidation treatment using 2,2,6,6-tetramethylpiperidine-1-oxyl (TEMPO) phosphate ester or the like tend to have low heat resistance due to the ionic groups (e.g., carboxyl groups) introduced into the cellulose nanofibers, and also tend to have a small fiber diameter after defibration. In terms of the reinforcing effect as a filler, cellulose nanofibers that have been defibrated only mechanically (i.e., have not been subjected to chemical defibration treatment such as oxidation) are more advantageous. Therefore, in a preferred embodiment, the cellulose nanofibers have no ionic groups. In this disclosure, the cellulose nanofibers have no ionic groups means that the amount of ionic groups measured by conductometric titration is 0.1 mmol / g or less.
[0025] The slurry can be prepared by dispersing the cellulose fibers in a liquid medium. The dispersion of the cellulose fibers in the slurry can be carried out using a high-pressure homogenizer, a microfluidizer, a ball mill, a disk mill, a mixer (e.g., a homomixer), or the like, and the product of the defibration can be obtained as the product of the slurry preparation process of the present disclosure. The liquid medium in the slurry can further include water, and optionally, a liquid medium other than water (e.g., an organic solvent) in one or more combinations. Examples of the organic solvent include commonly used water-miscible organic solvents, such as alcohols having a boiling point of 50° C. to 170° C. (e.g., methanol, ethanol, n-propanol, i-propanol, n-butanol, i-butanol, s-butanol, t-butanol, etc.); ethers (e.g., propylene glycol monomethyl ether, 1,2-dimethoxyethane, diisopropyl ether, tetrahydrofuran, 1,4-dioxane, etc.); carboxylic acids (e.g., formic acid, acetic acid, lactic acid, etc.); esters (e.g., ethyl acetate, vinyl acetate, etc.); ketones (e.g., acetone, methyl ethyl ketone, methyl isobutyl ketone, cyclopentanone, cyclohexanone, etc.); and nitrogen-containing solvents (e.g., dimethylformamide, dimethylacetamide, acetonitrile, etc.). In a typical embodiment, the liquid medium in the slurry is substantially water alone.
[0026] Since the cellulose raw material contains alkali soluble matter and sulfuric acid insoluble matter (lignin, etc.), the alkali soluble matter and sulfuric acid insoluble matter may be reduced through a purification process such as delignification by cooking and a bleaching process. On the other hand, the purification process such as delignification by cooking and the bleaching process cut the molecular chains of cellulose, changing the weight average molecular weight and number average molecular weight, so it is desirable to control the purification process and bleaching process of the cellulose raw material so that the weight average molecular weight of the cellulose nanofiber and the ratio of the weight average molecular weight to the number average molecular weight are within an appropriate range.
[0027] In addition, since the refining process such as delignification by cooking and the bleaching process reduce the molecular weight of cellulose molecules, there is concern that these processes will result in a lower molecular weight of cellulose nanofibers and alter the cellulose raw material, increasing the proportion of alkali-soluble matter. Since alkali-soluble matter has poor heat resistance, it is desirable to control the refining process and bleaching process of the cellulose raw material so that the amount of alkali-soluble matter contained in the cellulose raw material is within a certain range or less.
[0028] [Specific surface area] The specific surface area of the cellulose nanofiber is preferably 2 m2 or less in order to obtain a good effect of improving the physical properties of the cellulose nanofiber. 2 / g or more, preferably 3m 2 / g or more, preferably 5m 2 / g or more, preferably 7m 2 / g or more, preferably 10m 2 / g or more, preferably 12m 2 / g or more, preferably 15m 2 / g or more, preferably 17m 2 / g or more, preferably 20m 2 / g or more, preferably 22m 2 / g or more, preferably 25m 2 / g or more, preferably 27m 2 From the viewpoint of favorable dispersion of the cellulose nanofibers in the rubber composite and the cured rubber, the cellulose nanofibers are preferably 400 m 2 / g or less, preferably 350m 2 / g or less, preferably 300m 2 / g or less, preferably 250m 2 / g or less, preferably 200m 2 / g or less, preferably 170m 2 / g or less, preferably 150m 2 / g or less, preferably 120m 2 / g or less, preferably 100m 2 / g or less.
[0029] The specific surface area of cellulose nanofibers is measured by measuring the BET specific surface area of a porous sheet of cellulose nanofibers with a specific surface area / pore distribution measuring device (e.g., Nova-4200e, manufactured by Quantachrome Instruments) using nitrogen gas. Specifically, after drying approximately 0.2 g of the porous sheet at 120°C under vacuum for 5 hours, the amount of nitrogen gas adsorbed at the boiling point of liquid nitrogen is measured at 5 points (multipoint method) in the range of relative vapor pressure (P / P0) between 0.05 and 0.2, and the BET specific surface area (m 2 / g) is calculated.
[0030] [Porous sheet] The method for producing a porous sheet is as follows: first, a concentrated cake of cellulose nanofibers with a solid content of 10% by mass or more in water as a liquid medium is added to tert-butanol, and a dispersion process is performed using a high-shear homogenizer (e.g., IKA, product name "Ultra Turrax T18", processing conditions: rotation speed 15,000 rpm x 3 minutes) until no aggregates are formed. The concentration is adjusted to 0.5% by mass for 0.5 g of cellulose nanofiber solids. 100 g of the resulting tert-butanol dispersion is filtered on filter paper. The filtrate is not peeled off from the filter paper, but is sandwiched between two sheets of larger filter paper, and dried in an oven at 150 °C for 5 minutes while pressing down the edges of the larger filter paper with a weight. The filter paper is then peeled off to obtain a porous sheet with little distortion. The air resistance R of this sheet is 10 g / m 2 A porous sheet with a permeability of 100 sec / 100 ml or less is used as the measurement sample.
[0031] In addition, various physical properties of cellulose nanofibers described later (crystallinity, crystal polymorphism, degree of polymerization, Mw, Mn, Mw / Mn, alkali-soluble content, average acid-insoluble content, T D , T 1% , T 250℃ The measurements of the above may vary greatly depending on the shape of the measurement sample. To ensure stable and reproducible measurements, a distortion-free porous sheet is used as the measurement sample.
[0032] The air permeability resistance R was measured by measuring the basis weight W (g / m2) of a porous sheet sample left to stand for one day in an environment of 23°C and 50% RH. 2 ), and then the air resistance R (sec / 100ml) is measured using an Oken air resistance tester (e.g., Asahi Seiko Co., Ltd., Model EG01). 2 Calculate the value per unit area. Weight 10g / m 2 Air resistance per unit (sec / 100ml) = R / W x 10
[0033] The specific surface area of cellulose nanofibers can be calculated by the equivalent fiber diameter of the cellulose nanofibers using the following formula, assuming that the cellulose nanofibers are cylindrical. The density of cellulose is 1.5 (g / cm 3 ), the volume per gram of cellulose is 6.7 × 10 -7 (m 3 / g). If the converted fiber diameter of the cellulose nanofiber is r (m), the average circumference of the cellulose nanofiber = πr, and the average cross-sectional area of the cellulose nanofiber = 0.25πr. 2 , so the total fiber length per 1 g of cellulose nanofiber is 6.7 × 10 -7 (m 3 / g) / average cross-sectional area (=0.25πr 2 ) Total surface area = specific surface area (m 2 / g) = 6.7 × 10 -7 (m 3 / g) / average cross-sectional area (=0.25πr 2 )×average outer circumference length (=πr)=6.7×10 -7 (m 3 / g) / 0.25r = 26.68×10 -7 (m 3 / g) / r Therefore, Converted fiber diameter r(m)=26.68×10 -7 (m 3 / g) / specific surface area (m 2 / g) For example, if the BET specific surface area of the porous sheet is 40 m2 The equivalent fiber diameter r of the cellulose nanofiber is calculated to be 66.7 nm.
[0034] In one aspect, the equivalent fiber diameter of the cellulose nanofiber is preferably 2 to 1000 nm from the viewpoint of obtaining a good effect of improving physical properties by the cellulose nanofiber. The equivalent fiber diameter of the cellulose nanofiber is more preferably 4 nm or more, or 5 nm or more, or 10 nm or more, or 15 nm or more, or 20 nm or more, and more preferably 900 nm or less, or 800 nm or less, or 700 nm or less, or 600 nm or less, or 500 nm or less, or 400 nm or less, or 300 nm or less, or 200 nm or less.
[0035] In one aspect, the number average fiber diameter of the cellulose nanofibers is preferably 2 to 1000 nm from the viewpoint of obtaining a good effect of improving physical properties by the cellulose nanofibers. The number average fiber diameter of the cellulose nanofibers is more preferably 4 nm or more, or 5 nm or more, or 10 nm or more, or 15 nm or more, or 20 nm or more, and more preferably 500 nm or less, or 450 nm or less, or 400 nm or less, or 350 nm or less, or 300 nm or less, or 250 nm or less.
[0036] From the viewpoint of satisfactorily improving the mechanical properties of a rubber composite containing cellulose nanofibers with a small amount of cellulose nanofibers, the average fiber length (L) / fiber diameter (D) ratio of the cellulose nanofibers is preferably 30 or more, or 50 or more, or 80 or more, or 100 or more, or 120 or more, or 150 or more. There is no particular upper limit, but from the viewpoint of handleability, it is preferably 5,000 or less.
[0037] In the present disclosure, the fiber length, fiber diameter, and L / D ratio of the cellulose nanofibers are determined by dispersing an aqueous dispersion of cellulose nanofibers using a high-shear homogenizer (e.g., Nippon Seiki Co., Ltd., product name "Excel Auto Homogenizer ED-7") under processing conditions: rotation speed 15,000 rpm × 5 minutes, diluting the aqueous dispersion with pure water to 0.1 to 0.5 mass%, casting it on mica, and air-drying it to obtain a measurement sample, and measuring it with a high-resolution scanning microscope (SEM) or atomic force microscope (AFM). Specifically, the length (L) and diameter (D) of 100 randomly selected cellulose nanofibers are measured in an observation field where the magnification is adjusted so that at least 100 cellulose nanofibers are observed, and the ratio (L / D) is calculated. The number average value of the fiber length (L), the number average value of the fiber diameter (D), and the number average value of the ratio (L / D) are calculated for the cellulose nanofibers.
[0038] Alternatively, the fiber length, fiber diameter, and L / D ratio of the cellulose nanofibers in a rubber composition, a master batch, a rubber composite, or a cured rubber product can be confirmed by measuring the solid rubber composition, master batch, rubber composite, or cured rubber product as a measurement sample using the above-mentioned measurement method.
[0039] Alternatively, the fiber length, fiber diameter, and L / D ratio of the cellulose nanofibers in a rubber composition, master batch, rubber composite, or cured rubber product can be confirmed by dissolving the rubber component of the rubber composition, master batch, rubber composite, or cured rubber product in an organic or inorganic solvent capable of dissolving the rubber component, isolating the cellulose nanofibers, thoroughly washing the cellulose nanofibers with the solvent, and then replacing the solvent with pure water to prepare an aqueous dispersion. The cellulose nanofiber concentration is diluted with pure water to 0.1 to 0.5% by mass, cast on mica, and air-dried to obtain a measurement sample, which is then measured using the above-mentioned measurement method. At this time, the measurement is performed on 100 or more randomly selected cellulose nanofibers.
[0040] The crystallinity of the cellulose nanofiber is preferably 55% or more. When the crystallinity is in this range, the mechanical properties (strength, dimensional stability) of the cellulose itself are high, so that when the cellulose nanofiber is dispersed in rubber, the strength and dimensional stability of the rubber composite tend to be high. A more preferable lower limit of the crystallinity is 60%, even more preferably 70%, and most preferably 80% or more. There is no particular upper limit for the crystallinity of the cellulose nanofiber, and the higher the better, but from the viewpoint of production, a preferable upper limit is 99%.
[0041] Alkali-soluble polysaccharides such as hemicellulose and acid-insoluble components such as lignin are present between the microfibrils and between the microfibril bundles of plant-derived cellulose nanofibers. Hemicellulose is a polysaccharide composed of sugars such as mannan and xylan, and plays a role in binding the microfibrils together by hydrogen bonding with cellulose. Lignin is also a compound having an aromatic ring, and is known to be covalently bonded to hemicellulose in the cell walls of plants. If there is a large amount of impurities such as lignin remaining in the cellulose nanofibers, discoloration may occur due to heat during processing. Therefore, from the viewpoint of suppressing discoloration of the rubber composite during extrusion processing and molding processing, it is desirable to set the crystallinity of the cellulose nanofibers within the above-mentioned range.
[0042] The degree of crystallinity here, when the cellulose is cellulose type I crystal (derived from natural cellulose), is calculated from the diffraction pattern (2θ / deg. is 10 to 30) obtained by measuring a sample by wide-angle X-ray diffraction using the Segal method, according to the following formula: Crystallinity (%) = ([diffraction intensity due to the (200) plane at 2θ / deg. = 22.5] - [diffraction intensity due to amorphous matter at 2θ / deg. = 18]) / [diffraction intensity due to the (200) plane at 2θ / deg. = 22.5] × 100
[0043] When the cellulose is cellulose II type crystal (derived from regenerated cellulose), the degree of crystallinity can be calculated from the absolute peak intensity h0 at 2θ=12.6° assigned to the (110) plane peak of cellulose II type crystal in wide-angle X-ray diffraction and the peak intensity h1 from the baseline at this interplanar spacing, according to the following formula: Crystallinity (%) =h1 / h0 ×100
[0044] Known cellulose crystal forms include type I, type II, type III, and type IV, of which types I and II are particularly widely used, and types III and IV have been obtained on a laboratory scale but are not widely used on an industrial scale. The cellulose nanofibers of the present disclosure are preferably cellulose nanofibers containing cellulose type I crystals or cellulose type II crystals, since they have relatively high structural mobility and, by dispersing the cellulose nanofibers in rubber, can provide rubber composites with a lower linear expansion coefficient and superior strength and elongation during tensile and bending deformation, and more preferably cellulose nanofibers containing cellulose type I crystals and having a crystallinity of 55% or more.
[0045] In addition, the degree of polymerization of the cellulose nanofiber is preferably 100 or more, more preferably 150 or more, more preferably 200 or more, more preferably 300 or more, more preferably 400 or more, more preferably 450 or more, and preferably 3500 or less, more preferably 3300 or less, more preferably 3200 or less, more preferably 3100 or less, and more preferably 3000 or less.
[0046] From the viewpoint of processability and mechanical property expression, it is desirable that the degree of polymerization of the cellulose nanofiber is within the above-mentioned range. From the viewpoint of processability, it is preferable that the degree of polymerization is not too high, and from the viewpoint of mechanical property expression, it is desirable that the degree of polymerization is not too low.
[0047] The degree of polymerization of cellulose nanofibers refers to the average degree of polymerization measured according to the reduced specific viscosity method using a copper ethylenediamine solution described in the Verification Test (3) of the "15th Revised Japanese Pharmacopoeia Commentary (published by Hirokawa Shoten)."
[0048] In one embodiment, the weight average molecular weight (Mw) of the cellulose nanofiber is 100,000 or more, more preferably 200,000 or more. The ratio (Mw / Mn) of the weight average molecular weight to the number average molecular weight (Mn) is 6 or less, preferably 5.4 or less. The larger the weight average molecular weight, the fewer the number of terminal groups of the cellulose molecule. In addition, since the ratio (Mw / Mn) of the weight average molecular weight to the number average molecular weight represents the width of the molecular weight distribution, the smaller the Mw / Mn, the fewer the number of terminals of the cellulose molecule. Since the terminals of the cellulose molecules are the starting points of thermal decomposition, when the cellulose molecules of the cellulose nanofibers not only have a large weight average molecular weight but also have a narrow molecular weight distribution, a cellulose nanofiber with particularly high heat resistance and a rubber composite containing the cellulose nanofiber and rubber can be obtained. The weight average molecular weight (Mw) of the cellulose nanofiber may be, for example, 600,000 or less, or 500,000 or less, from the viewpoint of the availability of the cellulose raw material. From the viewpoint of ease of production of cellulose nanofibers, the ratio (Mw / Mn) of weight average molecular weight to number average molecular weight (Mn) may be, for example, 1.5 or more, or 2 or more. Mw can be controlled to the above range by selecting a cellulose raw material having an Mw appropriate for the purpose, by appropriately performing physical and / or chemical treatment on the cellulose raw material within an appropriate range, etc. Mw / Mn can also be controlled to the above range by selecting a cellulose raw material having an Mw / Mn appropriate for the purpose, by appropriately performing physical and / or chemical treatment on the cellulose raw material within an appropriate range, etc. Each of the Mw and Mw / Mn of the cellulose fiber raw material may be within the above range in one embodiment. In both the control of Mw and the control of Mw / Mn, examples of the physical treatment include physical treatments that apply mechanical forces such as dry or wet grinding using a microfluidizer, ball mill, disk mill, etc., and impact, shear, friction, etc. using a crusher, homomixer, high-pressure homogenizer, ultrasonic device, etc., and examples of the chemical treatments include digestion, bleaching, acid treatment, regenerated cellulose, etc.
[0049] The weight average molecular weight and number average molecular weight of the cellulose nanofiber referred to here are values obtained by dissolving the cellulose nanofiber in N,N-dimethylacetamide containing added lithium chloride and then performing gel permeation chromatography using N,N-dimethylacetamide as a solvent.
[0050] Methods for controlling the degree of polymerization (i.e., average degree of polymerization) or molecular weight of cellulose nanofibers include hydrolysis. Hydrolysis promotes depolymerization of amorphous cellulose inside the cellulose nanofibers, decreasing the average degree of polymerization. At the same time, hydrolysis removes impurities such as hemicellulose and lignin in addition to the above-mentioned amorphous cellulose, making the inside of the fiber more porous.
[0051] The hydrolysis method is not particularly limited, and examples thereof include acid hydrolysis, alkali hydrolysis, hydrothermal decomposition, steam explosion, and microwave decomposition. These methods may be used alone or in combination of two or more. In the acid hydrolysis method, for example, α-cellulose obtained as pulp from a fibrous plant is used as a cellulose raw material, and this is dispersed in an aqueous medium, and an appropriate amount of a protonic acid, a carboxylic acid, a Lewis acid, a heteropoly acid, etc. is added, and the mixture is heated while stirring, so that the average degree of polymerization can be easily controlled. The reaction conditions such as temperature, pressure, and time at this time vary depending on the cellulose type, cellulose concentration, acid type, acid concentration, etc., but are appropriately adjusted so that the desired average degree of polymerization is achieved. For example, a condition in which a mineral acid aqueous solution of 2% by mass or less is used and cellulose nanofibers are treated at 100°C or higher under pressure for 10 minutes or more can be mentioned. Under these conditions, the catalyst component such as acid penetrates into the inside of the cellulose nanofibers, promoting hydrolysis, reducing the amount of catalyst component used, and making subsequent purification easier. The dispersion of the cellulose raw material during hydrolysis may contain, in addition to water, a small amount of an organic solvent within a range that does not impair the effects of the present invention.
[0052] Alkali-soluble polysaccharides that may be contained in cellulose nanofibers include hemicellulose, β-cellulose, and γ-cellulose. Alkali-soluble polysaccharides are understood by those skilled in the art as components obtained as the alkali-soluble portion of holocellulose obtained by solvent extraction and chlorine treatment of plants (e.g., wood) (i.e., components obtained by removing α-cellulose from holocellulose). Alkali-soluble polysaccharides are polysaccharides containing hydroxyl groups and have poor heat resistance, and may cause inconveniences such as decomposition when exposed to heat, yellowing during thermal aging, and a decrease in strength of cellulose nanofibers. Therefore, it is preferable that the content of alkali-soluble polysaccharides in cellulose nanofibers is low.
[0053] In one aspect, the average content of alkali-soluble polysaccharides in the cellulose nanofibers is preferably 20% by mass or less, 18% by mass or less, 15% by mass or less, or 12% by mass or less, relative to 100% by mass of the cellulose nanofibers, from the viewpoint of obtaining good dispersibility of the cellulose nanofibers. From the viewpoint of ease of production of the cellulose nanofibers, the above content may be 1% by mass or more, 2% by mass or more, or 3% by mass or more.
[0054] The average alkali-soluble polysaccharide content can be determined by the method described in the non-patent literature (Wood Science Experiment Manual, edited by the Japan Wood Research Society, pages 92-97, 2000), by subtracting the α-cellulose content from the holocellulose content (Wise method). This method is understood in the industry as a method for measuring the amount of hemicellulose. The alkali-soluble polysaccharide content is calculated three times for each sample, and the number average of the calculated alkali-soluble polysaccharide contents is taken as the average alkali-soluble polysaccharide content.
[0055] In one aspect, the average content of acid-insoluble components in the cellulose nanofibers is preferably 10% by mass or less, 5% by mass or less, or 3% by mass or less, relative to 100% by mass of the cellulose nanofibers, from the viewpoint of avoiding a decrease in heat resistance of the cellulose nanofibers and the associated discoloration. From the viewpoint of ease of production of the cellulose nanofibers, the above content may be 0.1% by mass or more, 0.2% by mass or more, or 0.3% by mass or more.
[0056] The average acid-insoluble content is determined as a quantitative determination of the acid-insoluble content using the Clason method described in the non-patent literature (Wood Science Experiment Manual, edited by the Japan Wood Research Society, pages 92-97, 2000). This method is understood in the industry as a method for measuring the amount of lignin. The sample is stirred in a sulfuric acid solution to dissolve cellulose, hemicellulose, etc., and then filtered through a glass fiber filter paper, and the resulting residue corresponds to the acid-insoluble content. The acid-insoluble content is calculated from the weight of the acid-insoluble content, and the number average of the acid-insoluble content calculated for the three samples is taken as the average acid-insoluble content.
[0057] The thermal decomposition temperature of cellulose nanofiber (T D ) is 270° C. or higher in one embodiment, from the viewpoint of being able to exhibit the heat resistance and mechanical strength desired for in-vehicle applications and the like, preferably 275° C. or higher, more preferably 280° C. or higher, and even more preferably 285° C. or higher. The higher the thermal decomposition onset temperature, the more preferable it is, but from the viewpoint of ease of production of cellulose nanofibers, it may be, for example, 320° C. or lower, or 300° C. or lower.
[0058] In this disclosure, T D is a value obtained from a graph in which the horizontal axis is temperature and the vertical axis is the weight residual rate % in thermogravimetry (TG) analysis. Starting from the weight of cellulose nanofiber at 150°C (a state in which most of the moisture has been removed) (weight loss of 0 wt%), the temperature is continued to be increased until the temperature at which the weight loss reaches 1 wt% (T 1% ) and the temperature at which the weight loss reaches 2 wt% (T 2%The temperature at the point where this line intersects with the horizontal line (baseline) that passes through the starting point of the weight loss of 0 wt% is called T D It is defined as: 1% weight loss temperature (T 1% ) is the above T D This is the temperature at which the weight loss reaches 1% by weight, starting from the weight at 150°C, when the temperature is continued to be increased using the method described above. Weight loss rate of cellulose nanofiber at 250°C (T 250℃ ) is the weight loss rate when cellulose nanofibers were kept at 250°C under nitrogen flow for 2 hours in TG analysis.
[0059] (chemical modification) The cellulose nanofibers may be chemically modified cellulose nanofibers. The cellulose nanofibers may be chemically modified in advance, for example, at the stage of raw pulp or linters, during or after the defibration treatment, or during or after the slurry preparation process, or during or after the drying (granulation) process.
[0060] As a modifying agent for cellulose nanofibers, a compound that reacts with the hydroxyl groups of cellulose can be used, and examples of such agents include esterifying agents, etherifying agents, and silylation agents. On the other hand, modifying agents having polar groups, such as carboxylic acids and phosphoric esters, tend to reduce the heat resistance of cellulose nanofibers by introducing ionic groups (e.g., carboxyl groups) into the cellulose nanofibers, and also tend to reduce the fiber diameter after defibration, so it is preferable not to use such agents from the viewpoint of the reinforcing effect as a filler. In a preferred embodiment, the chemical modification is acylation using an esterifying agent, and acetylation is particularly preferred. As the esterifying agent, acid halides, acid anhydrides, vinyl carboxylates, and carboxylic acids are preferred.
[0061] The acid halide may be at least one selected from the group consisting of compounds represented by the following formula: R 1 -C(=O)-X (In the formula, R 1is an alkyl group having 1 to 24 carbon atoms, an alkenyl group having 2 to 24 carbon atoms, or 1 to 24 cycloalkyl group or aryl group having 6 to 24 carbon atoms, and X is Cl, Br, or I. Specific examples of acid halides include, but are not limited to, acetyl chloride, acetyl bromide, acetyl iodide, propionyl chloride, propionyl bromide, propionyl iodide, butyryl chloride, butyryl bromide, butyryl iodide, benzoyl chloride, benzoyl bromide, and benzoyl iodide. Among them, acid chlorides can be preferably used in terms of reactivity and handling. In addition, in the reaction of acid halides, one or more alkaline compounds may be added to act as a catalyst and neutralize the by-product acidic substances. Specific examples of alkaline compounds include, but are not limited to, tertiary amine compounds such as triethylamine and trimethylamine; and nitrogen-containing aromatic compounds such as pyridine and dimethylaminopyridine.
[0062] Any suitable acid anhydride can be used as the acid anhydride. For example, anhydrides of saturated aliphatic monocarboxylic acids such as acetic acid, propionic acid, (iso)butyric acid, valeric acid, etc.; anhydrides of unsaturated aliphatic monocarboxylic acids such as (meth)acrylic acid, oleic acid, etc.; anhydrides of alicyclic monocarboxylic acids such as cyclohexanecarboxylic acid, etc.; anhydrides of aromatic monocarboxylic acids such as benzoic acid, 4-methylbenzoic acid, tetrahydrobenzoic acid, etc.; dibasic carboxylic acid anhydrides, for example, anhydrides of saturated aliphatic dicarboxylic acids such as succinic acid, adipic acid, etc.; unsaturated aliphatic dicarboxylic acid anhydrides such as maleic anhydride, itaconic anhydride, etc.; alicyclic dicarboxylic acid anhydrides such as 1-cyclohexene-1,2-dicarboxylic acid anhydride; and aromatic dicarboxylic acid anhydrides such as phthalic anhydride, naphthalic anhydride, hexahydrophthalic anhydride, methyltetrahydrophthalic anhydride, etc.; Examples of polybasic carboxylic acid anhydrides having three or more bases include polycarboxylic acids (anhydrides) such as trimellitic anhydride and pyromellitic anhydride. In addition, in the reaction of an acid anhydride, one or more types of acidic compounds such as sulfuric acid, hydrochloric acid, phosphoric acid, etc., or Lewis acids (for example, Lewis acid compounds represented by MYn, where M represents a semimetal element such as B, As, Ge, etc., or a base metal element such as Al, Bi, In, etc., or a transition metal element such as Ti, Zn, Cu, etc., or a lanthanoid element, n is an integer corresponding to the atomic valence of M and represents 2 or 3, and Y represents a halogen atom, OAc, OCOCF3, ClO4, SbF6, PF6, or OSO2CF3(OTf)), or alkaline compounds such as triethylamine, pyridine, etc. may be added as a catalyst.
[0063] The vinyl carboxylate may be represented by the following formula: R-COO-CH=CH2 {wherein R is any one of an alkyl group having 1 to 24 carbon atoms, an alkenyl group having 2 to 24 carbon atoms, a cycloalkyl group having 3 to 16 carbon atoms, and an aryl group having 6 to 24 carbon atoms.} is preferred. The vinyl carboxylate is more preferably at least one selected from the group consisting of vinyl acetate, vinyl propionate, vinyl butyrate, vinyl caproate, vinyl cyclohexanecarboxylate, vinyl caprylate, vinyl caprate, vinyl laurate, vinyl myristate, vinyl palmitate, vinyl stearate, vinyl pivalate, vinyl octylate, divinyl adipate, vinyl methacrylate, vinyl crotonate, vinyl octylate, vinyl benzoate, and vinyl cinnamate. In the esterification reaction with a vinyl carboxylate, one or more catalysts selected from the group consisting of alkali metal hydroxides, alkaline earth metal hydroxides, alkali metal carbonates, alkaline earth metal carbonates, alkali metal hydrogencarbonates, primary to tertiary amines, quaternary ammonium salts, imidazole and derivatives thereof, pyridine and derivatives thereof, and alkoxides may be added.
[0064] Examples of the alkali metal hydroxides and alkaline earth metal hydroxides include sodium hydroxide, potassium hydroxide, lithium hydroxide, calcium hydroxide, barium hydroxide, etc. Examples of the alkali metal carbonates, alkaline earth metal carbonates, and alkali metal hydrogen carbonates include lithium carbonate, sodium carbonate, potassium carbonate, cesium carbonate, magnesium carbonate, calcium carbonate, barium carbonate, lithium hydrogen carbonate, sodium hydrogen carbonate, potassium hydrogen carbonate, cesium hydrogen carbonate, etc.
[0065] The primary, secondary and tertiary amines refer to primary, secondary and tertiary amines, and specific examples thereof include ethylenediamine, diethylamine, proline, N,N,N',N'-tetramethylethylenediamine, N,N,N',N'-tetramethyl-1,3-propanediamine, N,N,N',N'-tetramethyl-1,6-hexanediamine, tris(3-dimethylaminopropyl)amine, N,N-dimethylcyclohexylamine and triethylamine.
[0066] Examples of imidazole and its derivatives include 1-methylimidazole, 3-aminopropylimidazole, and carbonyldiimidazole.
[0067] Examples of pyridine and its derivatives include N,N-dimethyl-4-aminopyridine and picoline.
[0068] Examples of the alkoxide include sodium methoxide, sodium ethoxide, and potassium t-butoxide.
[0069] The carboxylic acid may be at least one selected from the group consisting of compounds represented by the following formulas: R-COOH (In the formula, R represents an alkyl group having 1 to 16 carbon atoms, an alkenyl group having 2 to 16 carbon atoms, a cycloalkyl group having 3 to 16 carbon atoms, or an aryl group having 6 to 16 carbon atoms.)
[0070] Specific examples of carboxylic acids include at least one selected from the group consisting of acetic acid, propionic acid, butyric acid, caproic acid, cyclohexane carboxylic acid, caprylic acid, capric acid, lauric acid, myristic acid, palmitic acid, stearic acid, pivalic acid, methacrylic acid, crotonic acid, octylic acid, benzoic acid, and cinnamic acid.
[0071] Among these carboxylic acids, at least one selected from the group consisting of acetic acid, propionic acid, and butyric acid, and particularly acetic acid, is preferred from the viewpoint of reaction efficiency. In addition, in the reaction of carboxylic acid, one or more types of acidic compounds such as sulfuric acid, hydrochloric acid, phosphoric acid, etc., or Lewis acids (for example, Lewis acid compounds represented by MYn, where M represents a semimetal element such as B, As, Ge, etc., or a base metal element such as Al, Bi, In, etc., or a transition metal element such as Ti, Zn, Cu, etc., or a lanthanoid element, n is an integer corresponding to the atomic valence of M and represents 2 or 3, and Y represents a halogen atom, OAc, OCOCF3, ClO4, SbF6, PF6, or OSO2CF3(OTf)), or alkaline compounds such as triethylamine, pyridine, etc. may be added as a catalyst.
[0072] Among these esterification reactants, at least one selected from the group consisting of acetic anhydride, propionic anhydride, butyric anhydride, vinyl acetate, vinyl propionate, vinyl butyrate, and acetic acid, and among these, acetic anhydride and vinyl acetate are preferred from the viewpoint of reaction efficiency.
[0073] When cellulose nanofibers are chemically modified (for example, by hydrophobization such as acylation), the dispersibility of the cellulose nanofibers in rubber tends to be good, but the cellulose nanofibers of the present disclosure can exhibit good dispersibility in rubber even if they are unsubstituted or have a low degree of substitution. In one embodiment, the chemical modification is acylation from the viewpoint of obtaining chemically modified cellulose nanofibers with a high thermal decomposition onset temperature. The degree of acyl substitution (DS) may be 0 or more, and is preferably 0.1 or more, or 0.2 or more, or 0.25 or more, or 0.3 or more, or 0.5 or more in terms of obtaining esterified cellulose nanofibers with a high thermal decomposition onset temperature. In addition, since unmodified cellulose skeletons remain in the esterified cellulose nanofibers, it is preferably 1.7 or less, or 1.5 or less, or 1.2 or less, or 1.0 or less, or 0.8 or less, or 0.7 or less, or 0.6 or less, or 0.5 or less in terms of obtaining esterified cellulose nanofibers that combine high tensile strength and dimensional stability derived from cellulose with a high thermal decomposition onset temperature derived from chemical modification.
[0074] When the modification group of the chemically modified cellulose nanofiber is an acyl group, the degree of acyl substitution (DS) can be calculated from the reflection infrared absorption spectrum of the esterified cellulose nanofiber based on the peak intensity ratio between the peak derived from the acyl group and the peak derived from the cellulose skeleton. The peak of the absorption band of C=O based on the acyl group is at 1730 cm -1 The absorption band of CO based on the cellulose backbone appears at 1030 cm -1 The DS of esterified cellulose nanofibers can be calculated by creating a correlation graph between the DS obtained from solid-state NMR measurements of esterified cellulose nanofibers (described below) and the modification ratio (IR index 1030), which is defined as the ratio of the peak intensity of the absorption band of C=O based on acyl groups to the peak intensity of the absorption band of CO in the cellulose backbone chain, and using the calibration curve substitution degree DS = 4.13 × IR index (1030) calculated from the correlation graph.
[0075] The method for calculating the DS of esterified cellulose nanofibers using solid-state NMR is as follows: 13 C solid-state NMR measurement was performed, and the intensity can be calculated using the area intensity (Inf) of a signal assigned to one carbon atom derived from the modifying group relative to the total area intensity (Inp) of signals assigned to carbons C1-C6 derived from the pyranose ring of cellulose, which appear in the range from 50 ppm to 110 ppm, using the following formula. DS=(Inf)×6 / (Inp) For example, when the modifying group is an acetyl group, the signal at 23 ppm assigned to -CH3 can be used. Use 13 The conditions for the C solid-state NMR measurement are, for example, as follows: Equipment:Bruker Biospin Avance500WB Frequency: 125.77MHz Measurement method: DD / MAS method Waiting time: 75sec NMR sample tube: 4mmφ Accumulation times: 640 times (approx. 14 hours) MAS: 14,500Hz Chemical shift reference: glycine (external reference: 176.03 ppm)
[0076] The DS heterogeneity ratio (DSs / DSt), defined as the ratio of the degree of modification (DSs) of the fiber surface to the degree of modification (DSt) of the entire fiber of the chemically modified cellulose nanofiber (which is synonymous with the above-mentioned degree of acyl substitution (DS)), is preferably 1.05 or more. The larger the value of the DS heterogeneity ratio, the more pronounced the sheath-core-like heterogeneous structure (i.e., a structure in which the fiber surface is highly chemically modified while the fiber center retains a cellulose structure close to the original unmodified structure), and while maintaining high tensile strength and dimensional stability derived from cellulose, it is possible to improve the affinity with rubber when composited with rubber and improve the dimensional stability of the cured rubber. The DS heterogeneity ratio is more preferably 1.1 or more, or 1.2 or more, or 1.3 or more, or 1.5 or more, or 2.0 or more, and from the viewpoint of ease of production of the chemically modified cellulose nanofiber, it is preferably 30 or less, or 20 or less, or 10 or less, or 6 or less, or 4 or less, or 3 or less.
[0077] The value of DSs varies depending on the degree of modification of the esterified cellulose nanofiber, but as an example, it is preferably 0.1 or more, more preferably 0.2 or more, even more preferably 0.3 or more, even more preferably 0.5 or more, and preferably 3.0 or less, more preferably 2.5 or less, particularly preferably 2.0 or less, even more preferably 1.5 or less, particularly preferably 1.2 or less, and most preferably 1.0 or less. The preferred range of DSt is as described above for the acyl substituent (DS).
[0078] The smaller the coefficient of variation (CV) of the DS heterogeneity ratio of the chemically modified cellulose nanofiber, the smaller the variation in various physical properties of the rubber composite, and therefore the more preferable. The coefficient of variation is preferably 50% or less, or 40% or less, or 30% or less, or 20% or less. The coefficient of variation can be further reduced, for example, by a method in which the cellulose raw material is defibrated and then chemically modified to obtain chemically modified cellulose nanofibers (i.e., a sequential method), whereas it can be increased by a method in which the defibration and chemical modification of the cellulose raw material are simultaneously performed (i.e., a simultaneous method). Although the mechanism of this action is not clear, it is considered that in the simultaneous method, chemical modification is more likely to proceed in the thin fibers generated in the early stage of defibration, and when hydrogen bonds between cellulose microfibrils are reduced by chemical modification, defibration proceeds further, resulting in an increase in the coefficient of variation of the DS heterogeneity ratio.
[0079] The coefficient of variation (CV) of the DS heterogeneity ratio is calculated by taking 100 g of an aqueous dispersion of chemically modified cellulose nanofiber (solid content of 10 mass% or more) and freeze-pulverizing 10 g portions to use as measurement samples. The DS heterogeneity ratio is calculated from the DSt and DSs of the 10 samples, and then the standard deviation (σ) and arithmetic mean (μ) of the DS heterogeneity ratio among the obtained 10 samples are used to calculate the coefficient of variation (CV) of the DS heterogeneity ratio using the following formula. DS heterogeneity ratio = DSs / DSt Coefficient of variation (%) = standard deviation σ / arithmetic mean μ × 100
[0080] The DSs is calculated as follows. That is, the esterified cellulose nanofibers powdered by freeze-pulverization are placed on a dish-shaped sample stage with a diameter of 2.5 mm, the surface is pressed down to make it flat, and then measurement is performed by X-ray photoelectron spectroscopy (XPS). The XPS spectrum reflects the constituent elements and chemical bond state of only the surface layer of the sample (typically about a few nm). Peak separation is performed on the obtained C1s spectrum, and the DSs can be calculated by the following formula based on the area intensity (Ixf) of the peak assigned to one carbon atom derived from the modifying group relative to the area intensity (Ixp) of the peak (289 eV, CC bond) assigned to carbons C2-C6 derived from the pyranose ring of cellulose. DSs = (Ixf) × 5 / (Ixp) For example, if the modifying group is an acetyl group, after peak separation of the C1s spectrum at 285 eV, 286 eV, 288 eV, and 289 eV, the peak at 289 eV can be used for Ixp and the peak derived from the O-C=O bond of the acetyl group (286 eV) can be used for Ixf. The conditions for the XPS measurement are as follows, for example: Equipment used: ULVAC-Phi VersaProbe II Excitation source: mono.AlKα 15kV×3.33mA Analysis size: Approx. 200 μm φ Photoelectron extraction angle: 45° Capture Area Narrow scan: C 1s, O 1s Pass Energy: 23.5eV
[0081] <First rubber component> The rubber composition according to one embodiment includes a first rubber component. In one embodiment, the first rubber component is a rubber derived from a rubber latex (i.e., a colloidal water dispersion of rubber particles), and in one embodiment, is a hydrophilic group-containing rubber. The first rubber component may be a conjugated diene polymer or a hydrogenated product thereof, or a non-conjugated diene polymer, or may be an oligomer. The first rubber component may be an uncured (unvulcanized) rubber, or a crosslinked body. In one embodiment, the first rubber component includes a toluene-insoluble component. The toluene-insoluble component can suppress re-agglomeration of the cellulose nanofibers due to excessive flow of the rubber component in the composition.
[0082] In the first rubber component, the toluene insoluble ratio, more specifically the gel fraction, may be adjusted within a desired range. A first rubber component with a low toluene insoluble ratio has a high fluidity and tends to easily penetrate into the gaps between cellulose nanofibers, so even when used in a relatively small amount, it can contribute well to improving the dispersibility of cellulose nanofibers. The toluene insoluble ratio can be increased or decreased by adjusting the monomer composition of the first rubber component, and / or by controlling the properties of the first rubber component (e.g., degree of crosslinking, molecular weight, etc.). The above properties can be controlled by rubber polymerization conditions (e.g., the amount of crosslinkable monomer such as butadiene, the amount of chain transfer agent, polymerization temperature, etc.).
[0083] The toluene-insoluble content of the first rubber component is preferably 0.5% by mass or more, or 1% by mass or more, or 10% by mass or more, from the viewpoint of suppressing re-aggregation of cellulose nanofibers and obtaining a rubber molded body with excellent physical properties such as hardness and storage modulus, and is preferably 99% by mass or less, or 97% by mass or less, or 95% by mass or less, from the viewpoint of easily penetrating into the gaps between cellulose nanofibers and thus having an excellent effect of improving the dispersibility of the cellulose nanofibers, and of the first rubber component not becoming too hard and exhibiting good rubber elasticity.
[0084] The weight average molecular weight (Mw) of the first rubber component is preferably 4,000 or more, or 5,000 or more, or 6,000 or more, from the viewpoint of obtaining a rubber molded product having excellent physical properties such as hardness, storage modulus, modulus, and tensile strength, and is preferably 1,000,000 or less, or 800,000 or less, or 700,000 or less, or 400,000 or less, from the viewpoint of being able to reduce the toluene insoluble matter ratio and being excellent in the effect of improving the dispersibility of cellulose nanofibers, and of the first rubber component not becoming too hard and exhibiting good rubber elasticity.
[0085] Throughout this disclosure, the weight average molecular weight (Mw) or number average molecular weight (Mn) of the rubber components (more specifically, the first, second and third rubber components, and the liquid rubber) is a value obtained by measuring a chromatogram using gel permeation chromatography with a TSKgel GMH column (manufactured by Tosoh Corporation) using tetrahydrofuran as a solvent, and calculating from a calibration curve using standard polystyrene.
[0086] The glass transition temperature of the first rubber component is preferably 10° C. or lower, or 7° C. or lower, or 5° C. or lower, from the viewpoint of reducing the toluene insoluble content ratio and providing an excellent effect of improving the dispersibility of cellulose nanofibers, and the first rubber component not becoming too hard and showing good rubber elasticity, and is preferably −70° C. or higher, or −65° C. or higher, or −60° C. or higher, from the viewpoint of obtaining a rubber molded product having excellent physical properties such as hardness, storage modulus, modulus, and tensile strength. In the present disclosure, the glass transition temperature is a value measured using a differential scanning calorimeter (DSC) at a heating rate and a cooling rate of 10° C. / min.
[0087] [Monomer composition of the first rubber component] The first rubber component may be a conjugated diene polymer or a non-conjugated diene polymer such as an acrylic rubber, and in a preferred embodiment is a conjugated diene polymer. The copolymer may be either a random or block copolymer.
[0088] The conjugated diene polymer is preferably one or more selected from the group consisting of styrene-butadiene rubber, butadiene rubber, isoprene rubber, natural rubber, chloroprene rubber, acrylonitrile butadiene rubber, butyl rubber, chlorinated butyl rubber, brominated butyl rubber, and ethylene propylene diene rubber, and derivatives thereof, and in one embodiment, the rubber is modified with at least a hydrophilic group. The conjugated diene polymer is more preferably one or more selected from the group consisting of styrene-butadiene rubber, butadiene rubber, isoprene rubber, and derivatives thereof, and in one embodiment, the rubber is modified with at least a hydrophilic group. The conjugated diene polymer is particularly preferably one or more selected from the group consisting of styrene-butadiene rubber and derivatives thereof, and in one embodiment, the rubber is modified with at least a hydrophilic group. Here, the derivative means one that has been hydrogenated and / or modified with a modifying group. The modifying group is a hydrophilic group and / or a modifying group other than a hydrophilic group, and in one embodiment, the hydrophilic group is essentially included.
[0089] In one embodiment, the conjugated diene-based polymer is a copolymer containing a conjugated diene monomer and an aromatic vinyl monomer.
[0090] Examples of the conjugated diene monomer include 1,3-butadiene, isoprene, piperylene, 2,3-dimethyl-1,3-butadiene, 1,3-pentadiene, 3-methyl-1,3-pentadiene, 1,3-heptadiene, and 1,3-hexadiene, and these may be used alone or in combination of two or more. Among these, butadiene, isoprene, and combinations thereof are preferred, and butadiene is particularly preferred.
[0091] The aromatic vinyl monomer is not particularly limited as long as it is a monomer copolymerizable with the conjugated diene monomer, and examples thereof include styrene, p-methylstyrene, α-methylstyrene, ethylstyrene, p-tert-butylstyrene, vinylethylbenzene, vinylxylene, vinylnaphthalene, diphenylethylene, and divinylbenzene, which may be used alone or in combination of two or more. From the viewpoints of the moldability of the rubber composition and the impact resistance of the cured rubber, styrene is preferred.
[0092] Examples of monomers copolymerizable with conjugated diene monomers and aromatic vinyl monomers include ethylenically unsaturated carboxylic acid monomers, (meth)acrylic acid alkyl ester monomers having a hydrophilic group, (meth)acrylic acid alkyl ester monomers having no hydrophilic group, vinyl cyanide monomers, and monomers having hydrophilic groups such as sulfo, phosphate, and amide groups. These can be used alone or in combination of two or more. The carboxy group of the ethylenically unsaturated carboxylic acid monomer, the hydrophilic group of the (meth)acrylic acid alkyl ester monomer having a hydrophilic group, and the hydrophilic group of the cyano group, sulfo group, phosphate group, and amide group of the vinyl cyanide monomer are hydrophilic groups of the hydrophilic group-containing rubber.
[0093] Examples of the ethylenically unsaturated carboxylic acid monomer include monobasic ethylenically unsaturated carboxylic acid monomers such as acrylic acid and methacrylic acid, and dibasic ethylenically unsaturated carboxylic acid monomers such as itaconic acid, maleic acid, and fumaric acid. Of these, acrylic acid, methacrylic acid, itaconic acid, and fumaric acid are preferred.
[0094] Examples of the (meth)acrylic acid alkyl ester monomer having a hydrophilic group include 2-hydroxyethyl (meth)acrylate, 2-hydroxypropyl (meth)acrylate, and 2-hydroxybutyl (meth)acrylate.
[0095] Examples of (meth)acrylic acid alkyl ester monomers having no hydrophilic group include methyl (meth)acrylate, ethyl (meth)acrylate, butyl (meth)acrylate, 2-ethylhexyl (meth)acrylate, and cyclohexyl (meth)acrylate.
[0096] Examples of vinyl cyanide monomers include acrylonitrile, methacrylonitrile, α-chloroacrylonitrile, etc. Among these, acrylonitrile and methacrylonitrile are preferred.Examples of monomers having a hydrophilic group such as a sulfo group, a phosphoric acid group, or an amide group include sodium p-styrenesulfonate, alkylarylsulfosuccinate (e.g., ELEMINOL (trademark) JS-2 and JS-5 manufactured by Sanyo Chemical Industries, Ltd., and LATEMURU (trademark) S-120, S-180A, and S-180 manufactured by Kao Corporation), polyoxyethylene alkylpropenylphenyl ether sulfate (e.g., AQUALON (trademark) HS-10 and HS-1025 manufactured by Daiichi Kogyo Seiyaku Co., Ltd.), α-[1-[(allyloxy)methyl]-2-phenylpropenyl]-2-propenyloxymethyl]-2-phenyl ... -(nonylphenoxy)ethyl]-ω-polyoxyethylene sulfate salt (for example, ADEKA REASOAP (trademark) SE-1025N, etc., manufactured by ADEKA CORPORATION), ammonium = α-sulfonato-ω-1-(allyloxymethyl) alkyloxy polyoxyethylene (for example, Aqualon KH-10, etc., manufactured by Daiichi Kogyo Seiyaku Co., Ltd.), ether sulfate type ammonium salt (for example, ADEKA REASOAP (trademark) SR-10, SR-1025, etc., manufactured by ADEKA CORPORATION), dioctyl-2-methacryloyloxyethyl phosphate , diphenyl-2-methacryloyloxyethyl phosphate, monomethyl-2-methacryloyloxyethyl phosphate, dimethyl-2-methacryloyloxyethyl phosphate, monoethyl-2-methacryloyloxyethyl phosphate, diethyl-2-methacryloyloxyethyl phosphate, monoisopropyl-2-methacryloyloxyethyl phosphate, diisopropyl-2-methacryloyloxyethyl phosphate, mono-n-butyl-2-methacryloyloxyethyl phosphate, di-n-butyl-2-methacryloyloxyethyl phosphate Examples of such esters include diethyl phosphate, monobutoxyethyl-2-methacryloyloxyethyl phosphate, dibutoxyethyl-2-methacryloyloxyethyl phosphate, mono(2-ethylhexyl)-2-methacryloyloxyethyl phosphate, di(2-ethylhexyl)-2-methacryloyloxyethyl phosphate, acrylamide, methacrylamide, N-methylolacrylamide, N-methylacrylamide, N-methylmethacrylamide, glycidyl methacrylamide, and N,N-butoxymethylacrylamide.
[0097] The proportion of the conjugated diene monomer is preferably 20% by mass or more, more preferably 30% by mass or more, and even more preferably 35% by mass or more, and is preferably 95% by mass or less, more preferably 90% by mass or less, and even more preferably 85% by mass or less, relative to 100% by mass of the total amount of the above monomers. The use amount of the conjugated diene monomer within the above range is advantageous in terms of lowering the glass transition temperature while imparting good rubber elasticity to the first rubber component. In a preferred embodiment, the proportion of the butadiene monomer relative to 100% by mass of the total amount of the above monomers may be within the above range.
[0098] A chain transfer agent may be used in the polymerization of the conjugated diene polymer. The chain transfer agent is not particularly limited, but examples thereof include α-methylstyrene dimer, which is one of the dimers of nucleus-substituted α-methylstyrene; mercaptans such as n-butyl mercaptan, t-butyl mercaptan, t-dodecyl mercaptan, n-octyl mercaptan, and n-lauryl mercaptan; disulfides such as tetramethyl thiuradium disulfide and tetraethyl thiuradium disulfide; halogenated derivatives such as carbon tetrachloride and carbon tetrabromide, and 2-ethylhexyl thioglycolate. Among these, mercaptans can be preferably used. These can be used alone or in combination of two or more.
[0099] The amount of the chain transfer agent used is preferably 0.1 parts by mass or more, more preferably 0.15% by mass or more, and even more preferably 0.2% by mass or more, relative to 100% by mass of the total amount of the monomers, and is preferably 10% by mass or less, more preferably 9% by mass or less, and even more preferably 8% by mass or less. By setting the amount of the chain transfer agent used within the above range, the weight average molecular weight of the toluene-insoluble matter and tetrahydrofuran-soluble matter of the conjugated diene polymer can be easily set within the above range.
[0100] The chain transfer agent may be added by any known method, such as all at once, batchwise, continuous, or a combination thereof.
[0101] The random copolymer may be a random copolymer using the above-mentioned monomers.
[0102] The block copolymer may be a copolymer consisting of two or more blocks, and may be, for example, a block copolymer having the same monomer composition as that exemplified above for the random copolymer. For example, a block A of an aromatic vinyl monomer and a block B of a conjugated diene monomer and / or a copolymer of an aromatic vinyl monomer and a conjugated diene monomer may constitute a structure such as AB, ABA, or ABAB. The boundaries of each block do not necessarily need to be clearly distinguished. For example, when the block B is a copolymer of an aromatic vinyl monomer and a conjugated diene monomer, the aromatic vinyl monomer in the block B may be distributed uniformly or in a tapered shape. In addition, the block B may have a plurality of parts in which the aromatic vinyl monomer is distributed uniformly and / or a plurality of parts in which the aromatic vinyl monomer is distributed in a tapered shape. Furthermore, the block B may have a plurality of segments with different aromatic vinyl monomer contents. When the copolymer has a plurality of blocks A and B, their molecular weights and compositions may be the same or different.
[0103] The mass ratio of the aromatic vinyl compound unit to the conjugated diene compound unit in the block copolymer is desirably 10 / 90 to 70 / 30. More preferably, it is 15 / 85 to 55 / 45, and most preferably 20 / 80 to 45 / 55. Furthermore, these may be blended with two or more different mass ratios of the aromatic vinyl compound to the conjugated diene compound. Specific examples of the aromatic vinyl compound include styrene, α-methylstyrene, vinyltoluene, etc., and one or more compounds selected from these are used, among which styrene is particularly preferred.
[0104] The block copolymer may be a mixture of two or more types differing from each other in one or more of the bond type, molecular weight, aromatic vinyl compound type, conjugated diene compound type, 1,2-vinyl content or the total amount of 1,2-vinyl content and 3,4-vinyl content, aromatic vinyl compound component content, hydrogenation rate, etc.
[0105] (Modifying group) In one embodiment, the first rubber component has a hydrophilic group. In one embodiment, the hydrophilic group is introduced into the rubber polymer as a modified group. Therefore, the hydrophilic group derived from another component (e.g., an emulsifier) is not included in the hydrophilic group in the hydrophilic group-containing rubber. However, the hydrophilic group that is introduced into the rubber polymer by chemical bonding and forms a part of the rubber polymer, such as the hydrophilic group derived from a reactive emulsifier, is included in the hydrophilic group in the hydrophilic group-containing rubber. In the present disclosure, the hydrophilic group means a hydrogen bond-forming group. Examples of hydrophilic groups include carboxy groups, acid anhydride groups, aldehyde groups, hydroxy groups, sulfo groups, sulfonyl groups, phosphate groups, alkoxy groups, amino groups, amide groups, imide groups, nitro groups, cyano groups, isocyanate groups, and epoxy groups. From the viewpoint of good affinity with cellulose nanofibers, the hydrophilic group is preferably one or more types selected from the group consisting of carboxy groups, hydroxy groups, sulfo groups, sulfonyl groups, phosphate groups, amide groups, and cyano groups, and more preferably one or more types selected from the group consisting of carboxy groups, hydroxy groups, sulfonyl groups, and phosphate groups.
[0106] The first rubber component is preferably at least one selected from the group consisting of carboxy-modified natural rubber, acid anhydride-modified natural rubber, conjugated diene-based carboxy-modified butadiene rubber, carboxy-modified styrene-butadiene rubber, acid anhydride-modified butadiene rubber, acid anhydride-modified styrene-butadiene rubber, non-conjugated diene-based carboxy-modified acrylic rubber, etc. A conjugated diene-based hydrophilic group-modified rubber component is preferred.
[0107] The amount of monomer units having hydrophilic groups relative to 100% by mass of all monomer units of the first rubber component is preferably 0.1% by mass or more, or 0.2% by mass or more, or 0.3% by mass or more, from the viewpoint of increasing the affinity for cellulose nanofibers and obtaining a good effect of improving the dispersibility of cellulose nanofibers, and is preferably 50% by mass or less, or 40% by mass or less, or 35% by mass or less, from the viewpoint of improving the compatibility of the first rubber component with other rubber components (specifically, the second and third rubber components) in the rubber composite to thereby improve the physical properties of the rubber molded body.
[0108] In one embodiment, the first rubber component may have a modifying group other than the hydrophilic group, such as a (meth)acrylic acid alkyl ester group. .
[0109] In the present disclosure, the amount of modified groups such as hydrophilic groups in the rubber component can be confirmed by FT-IR (Fourier transform infrared spectroscopy), solid-state NMR (nuclear magnetic resonance), solution NMR, or a method of calculating the molar ratio of modified groups by combining a predetermined specified monomer composition with the quantitative analysis of elements not contained in unmodified rubber, and then calculating the weight ratio from the molar ratio. For the analysis, a rubber component sample from which emulsifiers and the like have been previously separated and removed by solvent washing (e.g., isopropanol washing) may be used.
[0110] In one embodiment, the amount of residual monomer in the first rubber component may be 10% by mass or less, or 5% by mass or less, or 1% by mass or less. The amount of residual monomer can be confirmed by subjecting a solvent extract of the first rubber component to gas chromatography analysis. For example, when the residual monomer is styrene, solvent extraction using methanol and isooctane may be performed, and the extracted monomer component may be subjected to gas chromatography analysis.
[0111] [Rubber latex] In one embodiment, the first rubber component is derived from rubber latex. The rubber latex may be obtained by emulsion polymerization. The composition may be, for example, a mixture containing cellulose nanofibers and rubber latex itself, or may be a mixture obtained by removing part or all of the water from the mixture to adjust the solid content concentration and optionally further molding into a desired shape. The first rubber component in the composition may or may not maintain the shape of rubber particles. In one embodiment, the water content in the composition may be 0.01% by mass or more, or 0.1% by mass or more, or 1% by mass or more, and in one embodiment, 20% by mass or less, or 15% by mass or less, or 10% by mass or less. In one embodiment, the composition is a dry body. In one embodiment, the water content in the dry body may be 0.1% by mass to 10% by mass.
[0112] For the rubber latex obtained by emulsion polymerization, for example, a non-reactive surfactant such as a conventionally known anionic surfactant, cationic surfactant, amphoteric surfactant or nonionic surfactant, or a so-called reactive surfactant in which an ethylenic double bond is introduced into the chemical structure of a surfactant having a hydrophilic group and a lipophilic group can be used.
[0113] Non-reactive surfactants include: non-reactive anionic surfactants, for example, alkyl sulfates, polyoxyethylene alkyl ether sulfates, alkyl benzene sulfonates, alkyl naphthalene sulfonates, alkyl sulfosuccinates, alkyl diphenyl ether disulfonates, naphthalene sulfonate-formaldehyde condensates, polyoxyethylene polycyclic phenyl ether sulfates, polyoxyethylene distyrenated phenyl ether sulfates, fatty acid salts, alkyl phosphates, polyoxyethylene alkyl phenyl ether sulfates, etc.; non-reactive nonionic surfactants, for example, polyoxyethylene alkyl ethers, polyoxyalkylene alkyl ethers, polyoxyethylene polycyclic phenyl ethers, polyoxyethylene distyrenated phenyl ethers, sorbitan fatty acid esters, polyoxyethylene sorbitan fatty acid esters, polyoxyethylene sorbitol fatty acid esters, glycerin fatty acid esters, polyoxyethylene fatty acid esters, polyoxyethylene alkyl amines, alkyl alkanolamides, polyoxyethylene alkyl phenyl ethers, and the like; Examples include:
[0114] Examples of reactive surfactants include alkylaryl sulfosuccinates (e.g., Eleminol (trademark) JS-2 and JS-5 manufactured by Sanyo Chemical Industries, Ltd., and Latemul (trademark) S-120, S-180A, and S-180 manufactured by Kao Corporation), polyoxyethylene alkylpropenylphenyl ether sulfates (e.g., Aqualon (trademark) HS-10 and HS-1025 manufactured by Daiichi Kogyo Seiyaku Co., Ltd.), and α-[1-[(allyloxy)methyl]-2-(nonylphenoxy) Examples of suitable alkyloxyalkylesters include ammonium α-sulfonato-ω-1-(allyloxymethyl)alkyloxypolyoxyethylene (e.g., Adeka Reasoap (trademark) SE-1025N manufactured by ADEKA CORPORATION), ammonium α-sulfonato-ω-1-(allyloxymethyl)alkyloxypolyoxyethylene (e.g., Aqualon KH-10 manufactured by Daiichi Kogyo Seiyaku Co., Ltd.), and ether sulfate ammonium salts (e.g., Adeka Reasoap (trademark) SR-10 and SR-1025 manufactured by ADEKA CORPORATION).
[0115] Examples of nonionic surfactants that are reactive surfactants include α-[1-[(allyloxy)methyl]-2-(nonylphenoxy)ethyl]-ω-hydroxypolyoxyethylene (e.g., Adeka Reasoap NE-20, NE-30, NE-40, etc., manufactured by Asahi Denka Kogyo Co., Ltd.), polyoxyethylene alkylpropenyl phenyl ether (e.g., Aqualon RN-10, RN-20, RN-30, RN-50, etc., manufactured by Dai-ichi Kogyo Seiyaku Co., Ltd.), and the like.
[0116] The polymerization temperature of the rubber latex obtained by emulsion polymerization is, for example, 45° C. to 100° C. From the viewpoints of production efficiency and quality such as flexibility of the obtained rubber latex, the polymerization temperature during the period from the start of polymerization to the end of addition of the monomer mixture is preferably 55° C. to 97° C., more preferably 65° C. to 95° C. By setting the polymerization temperature within the above range, the crosslinking reaction of the conjugated diene monomer is controlled, and the weight average molecular weight of the toluene-insoluble portion and tetrahydrofuran-soluble portion of the conjugated diene polymer can be easily set within the above range.
[0117] In one embodiment, the rubber particles in the rubber latex are a hydrophilic group-containing rubber. The specific embodiment of the rubber particles (monomer composition, molecular weight, glass transition temperature, modified group, etc.) may be the same as that described above for the first rubber component, and the description will not be repeated here. Cellulose nanofibers typically form loose aggregates, and rubber particles exist as dispersed particles in a mixture containing cellulose nanofibers and rubber latex. At this time, rubber particles, especially rubber particles having hydrophilic groups, can easily enter the voids of the cellulose nanofiber aggregates. The rubber particles enter the voids of the cellulose nanofiber aggregates, and the cellulose nanofibers are well dispersed in the rubber, thereby further improving the physical properties of the rubber composite. Rubber particles with a low toluene insoluble content ratio are advantageous in terms of ease of entry into the voids of the cellulose nanofiber aggregates.
[0118] The average particle size of the rubber particles in the rubber latex is preferably 1 μm or less, or 500 nm or less, or 300 nm or less, or 100 nm or less from the viewpoint of obtaining a good effect of improving dispersibility in cellulose nanofibers, and is preferably 5 nm or more, or 7 nm or more, or 10 nm or more from the viewpoint of handleability. The average particle size is a number average particle size measured by a particle size measuring device (MICROTRACMUP A150, manufactured by LEED & NORTHRUP) by a light scattering method.
[0119] The rubber latex contains rubber particles and water, and may optionally contain an emulsifier (an anionic emulsifier such as sodium dodecylbenzenesulfonate, or a nonionic emulsifier such as polyoxyethylene alkyl ether), etc. The content of rubber particles in the rubber latex is preferably 1% by mass or more, or 3% by mass or more, or 4% by mass or more, or 5% by mass or more, or 10% by mass or more from the viewpoint of obtaining the advantages of using the rubber latex well, and is preferably 60% by mass or less, or 55% by mass or less, or 52% by mass or less, or 50% by mass or less, or 48% by mass or less, or 45% by mass or less from the viewpoint of easily penetrating the gaps between the cellulose nanofibers.
[0120] <Additional Ingredients> In order to improve the performance of the composition, the composition may further contain additional components in addition to the cellulose nanofibers and the first rubber component. Examples of the additional components include surfactants, dispersants, heat stabilizers, antioxidants, antistatic agents, colorants, preservatives, and antifoaming agents. The content ratio of any additional component in the composition is appropriately selected within a range that does not impair the desired effects of the present invention, and may be, for example, 0.01% by mass to 50% by mass, or 0.1% by mass to 30% by mass. The composition may further contain components other than those exemplified in this disclosure, as long as the effects of the present invention are not impaired. In a typical embodiment, the additional components are substantially free of toluene-insoluble matter.
[0121] [Slightly soluble surfactants] When a poorly soluble surfactant is used, in a mixture containing cellulose nanofibers and rubber latex, the cellulose nanofibers are well dispersed in the rubber by penetrating into the voids in the cellulose nanofiber aggregates that have been made porous by the contribution of the surfactant, thereby further improving the dispersibility of the cellulose nanofibers in the rubber molded product. The surfactant may be a component of the rubber latex, or may be added separately from the rubber latex.
[0122] From the above viewpoint, the solubility of the poorly soluble surfactant in 100 g of water at 25° C. is 20 g or less in one embodiment. The solubility is preferably 15 g or less, or 12 g or less. From the viewpoint of affinity with cellulose nanofibers, the solubility is preferably 0.1 g or more, or 1 g or more, or 2 g or more.
[0123] The surfactant can be any of cationic surfactants, anionic surfactants, nonionic surfactants, and amphoteric surfactants.The surfactant is preferably a combination of two or more surfactants, such as alkylbenzenesulfonic acid, alkylsulfonic acid, alkylsulfosuccinic acid, polyoxyethylene alkylsulfuric acid, polyoxyethylene alkylarylsulfuric acid, polyoxyethylene distyrylphenyl ether sulfonic acid, and their alkali metal salts or ammonium salts; fatty acid soap; alkyltrimethylammonium bromide; alkylpyridinium bromide; imidazolinium laurate; polyoxyethylene alkylaryl ether; polyoxyethylene alkyl ether; polyoxyethylene sorbitan fatty acid ester; sorbitan fatty acid ester; polyoxyethylene oxypropylene block copolymer; and polyoxyethylene distyrylphenyl ether.
[0124] The amount of surfactant in the composition is preferably 1 to 100 parts by mass, or 5 to 80 parts by mass, or 10 to 70 parts by mass, or 20 to 55 parts by mass, or 30 to 50 parts by mass, per 100 parts by mass of cellulose nanofibers.
[0125] <Method for producing composition> One aspect of the present invention provides a method for making the composition of the present disclosure, the method comprising: Mixing cellulose nanofibers with the rubber latex of the present disclosure to obtain a mixture (in one embodiment, an aqueous dispersion); and Optionally, drying the mixture (in one embodiment, the aqueous dispersion); The preferred embodiments of each component of the composition and the rubber latex are as described above and will not be described again. For example, the average particle size of the rubber particles may be 1 μm or less.
[0126] The mixture may be obtained by mixing the cellulose nanofibers, rubber latex, and any additional components with a stirring means such as a rotation-revolution mixer, a planetary mixer, a homogenizer, a propeller-type stirrer, a rotary stirrer, an electromagnetic stirrer, an open roll, a Banbury mixer, a single-screw extruder, or a twin-screw extruder. In addition, the mixture may be stirred under heating in order to efficiently perform shearing. A mixing method using a homogenizer is preferred because it can promote dispersion by applying high shearing force and pressure. The order of addition of the components during mixing is not limited.
[0127] Drying of the mixture may be accomplished by vacuum drying, oven drying, twin-screw extrusion drying, spray drying, etc. In a preferred embodiment, the drying is vacuum drying.
[0128] <Shape of composition> The composition may have a shape such as a sheet, pellets, powder, etc. The composition may be formed into a sheet having a thickness of, for example, 10 mm to 30 mm using a rolling mill roll in order to improve the cohesiveness and handleability.
[0129] ≪Aqueous dispersion≫ One aspect of the present invention provides an aqueous dispersion containing cellulose nanofibers and a first rubber component that is a hydrophilic group-containing rubber derived from rubber latex. In the aqueous dispersion according to one aspect, the first rubber component contains a toluene-insoluble component, and when 0.5 g of a composition obtained by drying the aqueous dispersion is stirred in 30 mL of toluene at 25° C., the toluene-insoluble ratio, which is the ratio of dissolved residue to 100% by mass of solids in the composition, is 30% by mass or more and 99% by mass or less. In the aqueous dispersion, the preferred aspects of each component other than the dispersion medium may be the same as those described above for the composition. In one aspect, the composition of the present disclosure may be obtained by drying the aqueous dispersion of the present disclosure.
[0130] The aqueous dispersion contains a dispersion medium. The dispersion medium may be water alone. In one embodiment, the solid content ratio of the aqueous dispersion is 5% by mass or more, or 6% by mass or more, or 8% by mass or more, or 10% by mass or more, and in one embodiment, is 25% by mass or less, or 20% by mass or less, or 18% by mass or less, or 15% by mass or less.
[0131] <Master batch> One aspect of the present invention provides a masterbatch comprising the composition of the present disclosure and a second rubber component. In one aspect, the masterbatch is a kneaded product comprising the composition of the present disclosure and the second rubber component.
[0132] <Second rubber component> The second rubber component may be a conjugated diene polymer or a hydrogenated product thereof, or a non-conjugated diene polymer, or may be an oligomer. In one embodiment, the second rubber component may be an unvulcanized (uncured) rubber, and may be cured during vulcanization of the rubber composite.
[0133] In one embodiment, the weight average molecular weight (Mw) of the second rubber component is 1,000 or more and 2,000,000 or less, and may be selected depending on the application of the rubber molded article, the type of rubber, etc. In one embodiment, the weight average molecular weight (Mw) of the second rubber component is preferably 100,000 or more, or 150,000 or more, or 200,000 or more, from the viewpoint of obtaining a rubber molded article that is particularly excellent in hardness, storage modulus, etc., and is preferably 2,000,000 or less, or 1,500,000 or less, or 1,000,000 or less, or 800,000 or less, or 750,000 or less, or 700,000 or less, or 600,000 or less, from the viewpoint of easiness of dispersing cellulose nanofibers in the second rubber component and in the viewpoint that the second rubber component does not become too hard after curing and exhibits good rubber elasticity.
[0134] On the other hand, in another embodiment, when a copolymer of, for example, ethylene and one or more α-olefins having 3 to 20 carbon atoms is used as the second rubber component, the weight average molecular weight (Mw) of the second rubber component can be in a relatively low range, for example, 10,000 or more, preferably 10,000 to 100,000.
[0135] [Monomer composition of second rubber component] (Conjugated diene polymer) The conjugated diene polymer may be a homopolymer, a copolymer of two or more conjugated diene monomers, or a copolymer of a conjugated diene monomer and another monomer. The copolymer may be either random or block.
[0136] Examples of the conjugated diene monomer include 1,3-butadiene, isoprene, piperylene, 2,3-dimethyl-1,3-butadiene, 1,3-pentadiene, 3-methyl-1,3-pentadiene, 1,3-heptadiene, and 1,3-hexadiene, and these may be used alone or in combination of two or more. Among these, butadiene, isoprene, and combinations thereof are preferred, and butadiene is particularly preferred.
[0137] In one embodiment, the conjugated diene polymer is a copolymer of the above-mentioned conjugated diene monomer and aromatic vinyl monomer. Suitable examples of the copolymer of the conjugated diene monomer and aromatic vinyl monomer and the hydrogenated rubber may be the same as those described above for the first rubber component.
[0138] (Modified rubber) The second rubber component may be a modified rubber, and for example, in the conjugated diene polymer exemplified above, a modified group such as an epoxy group, an acid anhydride group, a carboxy group, an aldehyde group, a hydroxyl group, an alkoxy group, an amino group, an amide group, an imide group, a nitro group, an isocyanate group, or a mercapto group may be introduced. Examples of modified rubber include epoxy modified natural rubber, epoxy modified butadiene rubber, epoxy modified styrene butadiene rubber, carboxy modified natural rubber, carboxy modified butadiene rubber, carboxy modified styrene butadiene rubber, acid anhydride modified natural rubber, acid anhydride modified butadiene rubber, and acid anhydride modified styrene butadiene rubber.
[0139] The amount of the modifying group relative to 100 mol% of all monomer units is preferably 0.1 mol% or more, or 0.2 mol% or more, or 0.3 mol% or more from the viewpoint of affinity between the cellulose nanofiber and the second rubber component, and is preferably 5 mol% or less, or 3 mol% or less from the viewpoint of obtaining good physical properties of the cured rubber.
[0140] The second rubber component preferably contains at least one selected from the group consisting of styrene-butadiene rubber, butadiene rubber, isoprene rubber, natural rubber, chloroprene rubber, acrylonitrile butadiene rubber, butyl rubber, chlorinated butyl rubber, brominated butyl rubber, and ethylene propylene diene rubber, and derivatives thereof, more preferably at least one selected from the group consisting of natural rubber, styrene butadiene rubber, butadiene rubber, isoprene rubber, chloroprene rubber, ethylene propylene diene rubber, and butyl rubber, and derivatives thereof, and even more preferably at least one selected from the group consisting of styrene butadiene rubber, butadiene rubber, and isoprene rubber, and derivatives thereof. In one embodiment, the derivative is the hydrogenated rubber or modified rubber described above.
[0141] [Shape of the second rubber component] In one embodiment, the second rubber component may be rubber latex particles. In one embodiment, the second rubber component may be rubber latex particles obtained by emulsion polymerization or rubber obtained by solution polymerization, or a combination thereof.
[0142] (rubber latex) The second rubber component may be derived from rubber latex. In this case, the masterbatch may be a simple mixture of rubber latex (i.e., a colloidal water dispersion of rubber particles) and other components of the masterbatch, or may be a mixture in which the solid content is adjusted by removing part or all of the water from the mixture. The second rubber component in the masterbatch may or may not maintain the shape of the rubber particles. The polymer constituting the rubber particles as the second rubber component may have a monomer composition as exemplified above for the first rubber component. The rubber particles as the second rubber component may be an uncrosslinked rubber that is crosslinked during the formation of the rubber cured product, or may be a crosslinked body.
[0143] The toluene-insoluble ratio of the rubber particles as the second rubber component is preferably 0.1 mass% or more from the viewpoint of obtaining a rubber molded product excellent in hardness, storage modulus, etc., and is preferably 99 mass% or less, or 98 mass% or less from the viewpoint of the cured product not becoming too hard and exhibiting good rubber elasticity.
[0144] In one embodiment, the average particle size of the rubber particles as the second rubber component may be 5 nm to 10,000 nm. The average particle size is a number average particle size measured by a particle size measuring device (MICROTRACMUP A150, manufactured by LEED & NORTHRUP) by a light scattering method.
[0145] In the master batch, the content of the second rubber component derived from rubber particles is preferably 1 mass% or more, or 2 mass% or more, from the viewpoint of obtaining the above-mentioned advantages of the rubber particles, and from the viewpoint of containing an appropriate amount of other components (cellulose nanofibers, first rubber component, etc.) and obtaining the advantages of these components, the content is preferably 50 mass% or less, or 40 mass% or less, or 30 mass% or less.
[0146] The rubber particles are contained in the master batch by mixing the rubber latex with other components of the master batch to prepare the master batch. The rubber latex for constituting the second rubber component contains rubber particles and water, and may optionally contain an emulsifier (an anionic emulsifier such as sodium dodecylbenzenesulfonate, or a nonionic emulsifier such as polyoxyethylene alkyl ether). The content of the rubber particles in the rubber latex is preferably 1% by mass or more, or 5% by mass or more, or 10% by mass or more, and preferably 60% by mass or less, or 57% by mass or less, or 55% by mass or less.
[0147] When rubber particles are used as the second rubber component, the master batch contains at least water derived from the rubber latex. In one embodiment, the water content in the master batch is 0.01% by mass or more, or 0.1% by mass or more, or 1% by mass or more, and in one embodiment, 20% by mass or less, or 15% by mass or less, or 10% by mass or less.
[0148] (Thermoplastic elastomer) In one embodiment, the second rubber component may include or be a thermoplastic elastomer. In the present disclosure, an elastomer is, in one embodiment, a substance (specifically, a natural or synthetic polymer substance) that is elastic at room temperature (23°C). In addition, being elastic in one embodiment means that the storage modulus at 23°C and 10 Hz measured by dynamic viscoelasticity measurement is 1 MPa or more and 100 MPa or less. The thermoplastic elastomer may be a conjugated diene polymer, and in one embodiment, is a crosslinked product. The suitable monomer composition of the thermoplastic elastomer may be the same as that described above in the section (conjugated diene polymer) above.
[0149] The weight average molecular weight (Mw) of the thermoplastic elastomer is preferably 50,000 to 500,000 from the viewpoint of achieving both impact strength and fluidity.
[0150] The thermoplastic elastomer may have a core-shell structure. Examples of elastomers having a core-shell structure include core-shell type elastomers having a core that is a particulate rubber and a shell that is a glassy graft layer formed on the outside of the core. The core is preferably a butadiene rubber, an acrylic rubber, a silicone-acrylic composite rubber, or the like. The shell is preferably a glassy polymer such as a styrene resin, an acrylonitrile-styrene copolymer, or an acrylic resin.
[0151] The thermoplastic elastomer is preferably at least one selected from the group consisting of styrene-butadiene block copolymers, styrene-ethylene-butadiene block copolymers, styrene-ethylene-butylene block copolymers, styrene-butadiene-butylene block copolymers, styrene-isoprene block copolymers, styrene-ethylene-propylene block copolymers, styrene-isobutylene block copolymers, hydrogenated styrene-butadiene block copolymers, hydrogenated styrene-ethylene-butadiene block copolymers, hydrogenated styrene-butadiene-butylene block copolymers, hydrogenated styrene-isoprene block copolymers, and styrene homopolymers (polystyrene), and more preferably at least one selected from the group consisting of styrene-butadiene block copolymers, hydrogenated styrene-butadiene block copolymers, and polystyrene.
[0152] In one embodiment, at least a part of the thermoplastic elastomer may have an acidic functional group. In the present disclosure, when the thermoplastic elastomer has an acidic functional group, it means that the acidic functional group is added to the molecular skeleton of the elastomer via a chemical bond. In the present disclosure, the acidic functional group means a functional group capable of reacting with a basic functional group, etc., and specific examples thereof include a hydroxyl group, a carboxyl group, a carboxylate group, a sulfo group, and an acid anhydride group.
[0153] From the viewpoint of affinity between cellulose nanofibers and the elastomer component, the amount of acidic functional groups added in the elastomer is preferably 0.01% by mass or more, more preferably 0.1% by mass or more, even more preferably 0.2% by mass or more, and preferably 5% by mass or less, more preferably 3% by mass or less, and even more preferably 2% by mass or less, based on 100% by mass of the elastomer. The number of acidic functional groups is a value obtained by measuring a calibration curve sample in which an acidic substance has been mixed in advance using an infrared absorption spectrometer, and measuring the sample based on a calibration curve that has been prepared using the characteristic absorption band of the acid.
[0154] Examples of elastomers having an acidic functional group include elastomers having a core-shell structure having a shell layer formed using acrylic acid or the like as a copolymerization component, and elastomers which are modified products obtained by grafting an α,β-unsaturated dicarboxylic acid or a derivative thereof to an ethylene-α-olefin copolymer, polyolefin, aromatic compound-conjugated diene copolymer, or a hydrogenated aromatic compound-conjugated diene copolymer containing acrylic acid or the like as a monomer, in the presence or absence of a peroxide.
[0155] In a preferred embodiment, the elastomer is an anhydride modified elastomer.
[0156] Among these, modified products obtained by grafting an α,β-unsaturated dicarboxylic acid or a derivative thereof onto a polyolefin, an aromatic compound-conjugated diene copolymer, or a hydrogenated aromatic compound-conjugated diene copolymer in the presence or absence of a peroxide are more preferred, and among these, modified products obtained by grafting an α,β-unsaturated dicarboxylic acid or a derivative thereof onto an ethylene-α-olefin copolymer, or a hydrogenated aromatic compound-conjugated diene block copolymer in the presence or absence of a peroxide are particularly preferred.
[0157] Specific examples of the α,β-unsaturated dicarboxylic acid and its derivatives include maleic acid, fumaric acid, maleic anhydride, and fumaric anhydride, with maleic anhydride being particularly preferred.
[0158] In one embodiment, the elastomer may be a mixture of an elastomer having an acidic functional group and an elastomer not having an acidic functional group. When the total of the elastomer having an acidic functional group and the elastomer not having an acidic functional group is 100% by mass, the mixing ratio of the elastomer having an acidic functional group is preferably 10% by mass or more, more preferably 20% by mass or more, even more preferably 30% by mass or more, and most preferably 40% by mass or more, from the viewpoint of maintaining high toughness and physical property stability of the rubber composite. There is no particular upper limit, and substantially all of the elastomer may be an elastomer having an acidic functional group, but from the viewpoint of not causing problems in flowability, it is desirable to have 80% by mass or less.
[0159] [Additional Ingredients] The masterbatch may further contain additional components as necessary to improve its performance. Examples of the additional components include acid anhydride-modified rubber, rubber additives, dispersants, organic or inorganic fillers, antistatic agents, colorants, etc. The content ratio of any additional component in the masterbatch is appropriately selected within a range that does not impair the desired effects of the present invention, and may be, for example, 0.01% by mass to 50% by mass, or 0.1% by mass to 30% by mass. The master batch may further contain components other than those exemplified in this disclosure, as long as the effects of the present invention are not impaired.
[0160] The use of an acid anhydride-modified rubber is advantageous in improving the affinity between the cellulose nanofiber and the first, second and / or third rubber components. In one embodiment, the acid anhydride-modified rubber may be a liquid rubber or a solid rubber. In the present disclosure, the liquid rubber means a substance that has fluidity at 23°C and forms a rubber elastomer by crosslinking (more specifically, vulcanization) and / or chain extension. In one embodiment, the liquid rubber dissolved in cyclohexane is placed in a vial with a body diameter of 21 mm and a total length of 50 mm at 23°C, and then dried, so that the liquid rubber is filled in the vial to a height of 1 mm and sealed, and the vial is left standing for 24 hours in an upside-down state, and a movement of the substance of 0.1 mm or more in the vertical direction can be confirmed. In a typical embodiment, the liquid rubber has a relatively low molecular weight and thus has a liquid shape.
[0161] The number average molecular weight (Mn) of the liquid rubber is preferably 1,000 or more, or 1,500 or more, or 2,000 or more from the viewpoint of obtaining a rubber molded product having excellent hardness, storage modulus, etc., and is preferably 80,000 or less, or 50,000 or less, or 40,000 or less, or 30,000 or less, or 10,000 or less in terms of having high fluidity suitable for dispersing cellulose nanofibers well in the liquid rubber, and in terms of the liquid rubber not becoming too hard after curing and exhibiting good rubber elasticity.
[0162] The viscosity of the liquid rubber at 25°C is preferably 1,000,000 mPa·s or less, or 500,000 mPa·s or less, or 200,000 mPa·s or less, from the viewpoint of favorable dispersion of the cellulose nanofibers in the liquid rubber, and is preferably 100 mPa·s or more, or 300 mPa·s or more, or 500 mPa·s or more, from the viewpoint of obtaining a rubber molded product excellent in hardness, storage modulus, etc. The viscosity of the liquid rubber is a value measured using an E-type viscometer at a rotation speed of 10 rpm.
[0163] In a preferred embodiment, the acid anhydride-modified rubber is an acid anhydride-modified rubber containing at least one selected from the group consisting of styrene-butadiene rubber, butadiene rubber, isoprene rubber, and derivatives thereof.
[0164] In the masterbatch, the content of the acid anhydride modified rubber is preferably 0.1 mass% or more, or 1 mass% or more, or 2 mass% or more from the viewpoint of obtaining the advantages of the acid anhydride modified rubber, and from the viewpoint of containing suitable amounts of other components (cellulose nanofibers, first rubber component, etc.) and obtaining the advantages of these components, the content is preferably 80 mass% or less, or 60 mass% or less, or 40 mass% or less.
[0165] In addition, when an acid anhydride modified rubber is used, the rubber component of the present disclosure (more specifically, at least one of the first to third rubber components) and the acid anhydride modified rubber may be the same or different polymer species. The same polymer species means that the skeleton structure of the monomer constituting the polymer is the same. When the acid anhydride modified rubber and the rubber component are the same polymer species, the affinity between them is particularly good, so that the cellulose nanofibers are well dispersed and a uniform rubber composite can be easily produced. In one embodiment, the rubber component is solid at 25°C, unlike the liquid rubber, and the acid anhydride modified rubber is a liquid rubber. A rubber component that is the same polymer species as the liquid rubber typically has a higher molecular weight than the liquid rubber.
[0166] As the rubber additives, conventionally known stabilizers, softeners, anti-aging agents, etc. may be used. As the rubber stabilizer, one or more antioxidants such as 2,6-di-tert-butyl-4-hydroxytoluene (BHT), n-octadecyl-3-(4'-hydroxy-3',5'-di-tert-butylphenyl)propionate, 2-methyl-4,6-bis[(octylthio)methyl]phenol may be used. As the rubber softener, one or more process oils, extender oils, etc. may be used. However, the master batch of the present embodiment can form a soft rubber cured product in one embodiment, and therefore may not contain a rubber softener in one embodiment.
[0167] In a preferred embodiment, the masterbatch contains 10 to 50 parts by mass, or 15 to 30 parts by mass, of cellulose nanofibers and 1 to 25 parts by mass of surfactant, relative to 100 parts by mass of rubber components (specifically, the total of the first and second rubber components, and an optional additional rubber). In one embodiment, the component composition of the masterbatch may be the same as that described above for the composition. In the masterbatch, the ratio of [the total mass of the cellulose nanofibers and the first rubber component] / [the second rubber component] may be 1 / 99 to 99 / 1, or 5 / 95 to 95 / 5, or 10 / 90 to 90 / 10, or 20 / 80 to 80 / 20, or 30 / 70 to 70 / 30, or 40 / 60 to 60 / 40.
[0168] <Masterbatch manufacturing method> One aspect of the present invention provides a method for producing a masterbatch. The method includes a step of mixing a composition of the present disclosure, which contains cellulose nanofibers and a first rubber component, with a second rubber component. The mixing conditions are not particularly limited, and examples include a method of kneading at least once using a known internal kneader such as an internal mixer under conditions where the kneading discharge temperature is 135 to 180°C. The masterbatch may be molded into a sheet, for example, 10 mm to 30 mm thick, using a rolling mill roll to improve cohesiveness and handleability.
[0169] <Rubber composite> One aspect of the present invention provides a rubber composite that includes a component derived from the composition or masterbatch of the present disclosure, a third rubber component, and optionally additional components, and is typically a kneaded product containing these. By using the composition or masterbatch of the present disclosure, a rubber composite in which cellulose nanofibers are uniformly dispersed in the rubber can be obtained.
[0170] <Third rubber component> The specific preferred embodiment of the third rubber component may be the same as that described above for the second rubber component. The second rubber component and the third rubber component may be the same or different.
[0171] In one embodiment, the mass ratio of the composition of the present disclosure to the third rubber component (composition / third rubber component) may be 1 / 99 to 99 / 1, or 5 / 95 to 95 / 5, or 10 / 90 to 90 / 10, or 20 / 80 to 80 / 20, or 30 / 70 to 70 / 30, or 40 / 60 to 60 / 40.
[0172] In one embodiment, the mass ratio of the masterbatch of the present disclosure to the third rubber component (masterbatch / third rubber component) may be 1 / 99 to 99 / 1, or 5 / 95 to 95 / 5, or 10 / 90 to 90 / 10, or 20 / 80 to 80 / 20, or 30 / 70 to 70 / 30, or 40 / 60 to 60 / 40.
[0173] In the rubber composite, the total content of the first and second rubber components is preferably 5% by mass or more, more preferably 10% by mass or more, and even more preferably 15% by mass or more, in order to ensure that the content of cellulose nanofibers in the rubber composite is not too small and the effects of the present invention can be satisfactorily obtained, out of a total of 100% by mass of the first, second and third rubber components. In one embodiment, the content may be 50% by mass or less, 40% by mass or less, or 30% by mass or less, in terms of dispersibility of the cellulose nanofibers in the rubber composite.
[0174] The content of the rubber component in the rubber composite (specifically, the total of the first, second and third rubber components, and any additional rubber as an optional component) is, in one embodiment, 70% by mass or more, or 80% by mass or more, or 90% by mass or more, and in one embodiment, 99% by mass or less, or 95% by mass or less, or 90% by mass or less.
[0175] <Additional Ingredients> The rubber composite may, if necessary, use additional components similar to those exemplified for the masterbatch. The types and amounts of the additional components may be the same as those exemplified for the masterbatch.
[0176] In the rubber composite, the amount of cellulose nanofiber per 100 parts by mass of the first rubber component, the second rubber component, the third rubber component, and the additional rubber as an optional component is preferably 1 part by mass or more, and preferably 15 parts by mass or less.
[0177] The content of cellulose nanofibers in the rubber composite is, in one embodiment, 1% by mass or more, or 5% by mass or more, or 10% by mass or more, and in one embodiment, 30% by mass or less, or 20% by mass or less, or 10% by mass or less.
[0178] The content of the rubber component in the rubber composite (specifically, the total of the first, second and third rubber components, and any additional rubber as an optional component) is, in one embodiment, 70% by mass or more, or 80% by mass or more, or 90% by mass or more, and in one embodiment, 99% by mass or less, or 95% by mass or less, or 90% by mass or less.
[0179] <Method for manufacturing rubber composite> One aspect of the present invention provides a method for producing a rubber composite. The method according to one aspect includes a step of mixing a composition according to the present disclosure, which includes cellulose nanofibers and a first rubber component, with a second rubber component to prepare a masterbatch, and a step of mixing the masterbatch with a third rubber component to prepare a rubber composite. Another aspect of the method includes a step of mixing a composition, which includes cellulose nanofibers and the first rubber component, with the third rubber component to prepare a rubber composite.
[0180] The method of mixing the constituent materials of the rubber composite is not limited to the following, but examples thereof include a melt-kneading method using a general mixer such as an open roll, a Banbury mixer, a kneader, a single-screw extruder, a twin-screw extruder, or a multi-screw extruder, and a method of dissolving and mixing each component and then removing the solvent by heating. Among these, the melt-kneading method using a roll, a Banbury mixer, a kneader, or an extruder is preferred from the viewpoints of productivity and kneadability. In addition, both a method of kneading the constituent materials of the rubber composite of the present embodiment at once and a method of mixing them in multiple batches are applicable. The kneading conditions are not particularly limited, but examples thereof include a method of kneading at least once using a known closed kneader such as an internal mixer under conditions where the kneading discharge temperature is 135 to 180 ° C. From the viewpoint of obtaining good dispersibility of the cellulose nanofibers and good physical properties of the rubber molded body, it is preferable to produce the master batch of the present disclosure in advance.
[0181] <Cured rubber> The rubber composite of the present embodiment may be a vulcanized composition (cured rubber product) that has been subjected to a vulcanization treatment with a vulcanizing agent. The vulcanizing agent and vulcanization accelerator may be included in the composition, master batch, and / or rubber composite. Examples of the vulcanizing agent include, but are not limited to, radical generators such as organic peroxides and azo compounds, oxime compounds, nitroso compounds, polyamine compounds, sulfur, and sulfur compounds. Examples of sulfur compounds include sulfur monochloride, sulfur dichloride, disulfide compounds, and polymer polysulfur compounds. The content of the vulcanizing agent is preferably 0.01 parts by mass or more and 20 parts by mass or less, and more preferably 0.1 parts by mass or more and 15 parts by mass or less, relative to a total of 100 parts by mass of the uncured rubber in the rubber component. As the vulcanization method, a conventionally known method can be applied, and the vulcanization temperature is preferably 120°C or more and 200°C or less, and more preferably 140°C or more and 180°C or less.
[0182] In vulcanization, a vulcanization accelerator may be used as necessary. As the vulcanization accelerator, a conventionally known material may be used, and examples thereof include, but are not limited to, sulfenamide-based, guanidine-based, thiuram-based, aldehyde-amine-based, aldehyde-ammonia-based, thiazole-based, thiourea-based, and dithiocarbamate-based vulcanization accelerators. As the vulcanization aid, examples thereof include, but are not limited to, zinc oxide and stearic acid. The content of the vulcanization accelerator is preferably 0.01 parts by mass or more and 20 parts by mass or less, and more preferably 0.1 parts by mass or more and 15 parts by mass or less, relative to 100 parts by mass of the total of the uncured rubber in the rubber component.
[0183] <Method for producing cured rubber> One aspect of the present invention provides a method for producing a cured rubber product. In one aspect, the method comprises: A step of mixing a composition containing cellulose nanofibers and a first rubber component with a second rubber component to prepare a master batch; mixing the masterbatch with a third rubber component to prepare a rubber composite; and curing the rubber composite; Includes. In another aspect, the method comprises: A step of preparing a rubber composite by mixing a composition containing cellulose nanofibers and a first rubber component with a third rubber component; and curing the rubber composite; Includes.
[0184] Curing conditions include pressing for 20 minutes at 160° C. For example, the rubber composite may be molded by injection molding, extrusion molding, extrusion profile molding, blow molding, compression molding, or the like, and then cured.
[0185] The cured rubber may be formed into molded articles of various shapes. The molded articles can be used in a wide range of applications, such as industrial machine parts, general machine parts, automobile, railway, vehicle, ship, and aerospace-related parts, electronic and electrical parts, building and civil engineering materials, daily necessities, sports and leisure goods, wind power generation housing parts, containers and packaging parts, etc. Examples of applications include automobile parts (for example, exterior parts such as bumpers, fenders, door panels, various moldings, emblems, engine hoods, wheel caps, roofs, spoilers, and various aero parts, and interior parts such as instrument panels, console boxes, and trims), battery parts (automotive secondary battery parts, lithium ion secondary battery parts, fuel cases for solid methanol batteries, piping for fuel cells, etc.), electronic and electrical equipment parts (for example, various computers and their peripherals, junction boxes, various connectors, various office automation equipment, televisions, videos, disc players, chassis, refrigerators, air conditioners, and parts for liquid crystal projectors, etc.), etc.
[0186] One aspect of the present invention provides a shoe outsole, a tire, a vibration-proof rubber, or a power transmission belt comprising the rubber vulcanized product of the present disclosure. EXAMPLES
[0187] The following examples further illustrate exemplary embodiments of the present invention, but the present invention is not limited to these examples.
[0188] <Material evaluation method> <Solid content of composition containing water or rubber latex containing rubber particles> 1.5 g of the composition containing water or the rubber latex containing rubber particles was placed on a pre-weighed aluminum dish and dried for 1 hour at 130° C. The solid content was calculated from the ratio of the dried weight to the total weight.
[0189] <Amount of monomer units having hydrophilic groups relative to 100% by mass of all monomer units in rubber particles> The above amount was calculated from the charged amount.
[0190] <Residual monomer content of rubber particles> Solvent extraction was carried out using methanol and isooctane, and the extracted monomer components were subjected to gas chromatographic analysis (Shimadzu Corporation, GC-14B).
[0191] <Average particle size of rubber particles in rubber latex> The number average particle size was measured by a light scattering method using a particle size measuring device (MICROTRACMUP A150, manufactured by LEED & NORTHRUP).
[0192] <Glass transition temperature of rubber particles> 1.5 g of rubber latex containing rubber particles was collected and dried at 130° C. for 1 hour to obtain a film, from which a 20 mg sample was collected. The collected sample was heated from -120° C. to +160° C. at a heating rate of 20° C. / min using differential scanning calorimetry (DSC) in accordance with ASTM D3418-97 to obtain a differential scanning calorimetry curve and determine the glass transition temperature.
[0193] <Toluene insoluble content ratio of rubber particles> 0.5 g of the dried rubber composition or rubber latex containing rubber particles was mixed with 30 ml of toluene and shaken at room temperature (25°C) for 3 hours, then filtered through a metal net with 32 μm mesh, the residue was dried at 130°C for 1 hour, and the dry mass was weighed. The ratio of the dry mass of the residue to the total solid mass of 100 mass% of the composition or rubber particles in 0.5 g of the rubber composition or rubber particles was taken as the toluene insoluble ratio (mass%). The dried rubber latex containing rubber particles was obtained by collecting 6 g of rubber latex containing rubber particles and drying it at 130°C for 1 hour.
[0194] <Weight average molecular weight (Mw) of rubber particles> 10 g of rubber latex containing rubber particles was collected, and the pH was adjusted to 2 or less using ion exchange resin (Diaion SK1B manufactured by Mitsubishi Chemical). 2 g of 10% aluminum sulfate aqueous solution was added to this sample to coagulate the rubber particles. The coagulated rubber particles were thoroughly washed with isopropanol, then washed with water, and finally washed with methanol. The sample washed with methanol was vacuum dried at 40°C for 3 hours to obtain a dried product. 50 ml of tetrahydrofuran was added to 0.3 g of the dried product, and the mixture was left to stand for 24 hours, then shaken with a shaker for 3 hours, and then filtered through a 325 mesh. The tetrahydrofuran solution that passed through the 325 mesh was used as a molecular weight sample. A chromatogram was measured using gel permeation chromatography (GPC) using three columns packed with polystyrene gel connected together, and the weight average molecular weight (Mw) was calculated using a calibration curve using standard polystyrene. Tetrahydrofuran was used as a solvent.
[0195] <Solubility of surfactant at 25℃> The measurements were performed in the following manner. At 25°C, the light transmittance at a wavelength of 780 nm was measured when the surfactant concentration was 0 mass%, that is, 4 mL of pure water was placed in a quartz cell. Next, 4 mL of surfactant aqueous solutions prepared so that the surfactant concentrations were 0.1 mass%, 0.2 mass%, 0.5 mass%, 1 mass%, 5 mass%, 10 mass%, and 20 mass% were placed in a quartz cell, and the light transmittance at a wavelength of 780 nm was measured using a UV-visible spectrophotometer (JASCO Corporation, V-670). Each value was taken as Ts, and the light transmittance ratio Ts / Tw was calculated. In the region where the value of Ts / Tw changes linearly with respect to the surfactant concentration, a regression equation was created by the least squares method, and the surfactant concentration at which Ts / Tw=0.98 was calculated, and this was taken as the solubility at 25°C.
[0196] ≪Materials used≫ <Rubber component> [Modified liquid rubber] LR-1: Cray Valley Ricon184MA6 (maleic anhydride modified liquid styrene butadiene copolymer, Mn=9,100, 6 maleic anhydride molecules per molecular chain)
[0197] [Solution polymerized rubber] SBR-1: Asaprene Y031 (available from Asahi Kasei Corporation)
[0198] [Rubber latex] A rubber latex containing rubber particles was prepared by the following procedure. (Manufacturing example 1: SB-1) In a nitrogen-substituted pressure-resistant reactor, 1085 parts by mass of water, 20 parts by mass of sodium dodecylbenzenesulfonate (non-reactive emulsifier), and 2 parts by mass of itaconic acid (monomer having a carboxyl group as a hydrophilic group) were charged as polymerization initial raw materials all at once, and thoroughly stirred at 80 ° C. Next, as a monomer mixture and a chain transfer agent, 20 parts by mass of styrene, 75 parts by mass of butadiene, 0.5 parts by mass of methyl methacrylate (monomer having no hydrophilic group), 0.5 parts by mass of acrylonitrile (monomer having a cyano group as a hydrophilic group), 2 parts by mass of 2-hydroxyethyl acrylate (monomer having a hydroxyl group as a hydrophilic group), and 0.5 parts by mass of t-dodecyl mercaptan (t-DDM) were mixed (hereinafter abbreviated as "monomer mixture"), and 10% of the monomer mixture was added to the pressure-resistant vessel and thoroughly stirred. Next, 10 parts by mass of an aqueous sodium hydrogen sulfite solution with a solid content of 9% by mass was added to the pressure vessel, and 5 minutes later, 10 parts by mass of an aqueous sodium persulfate solution with a solid content of 30% by mass was added to the pressure vessel. 10 minutes after the addition of the aqueous sodium persulfate solution with a solid content of 30% by mass, the remaining 90% of the mixture of monomers, etc. was continuously added to the pressure vessel over 2 hours. Furthermore, 20 minutes after the addition of the aqueous sodium persulfate solution with a solid content of 30% by mass, an aqueous mixture in which 0.6 parts by mass of sodium hydroxide and 1.35 parts by mass of sodium persulfate were dissolved in 86 parts by mass of water was continuously added to the pressure vessel over 3 hours. 4 hours and 45 minutes after the addition of the aqueous sodium persulfate solution with a solid content of 30% by mass, the temperature in the pressure vessel was raised to 95°C, and the polymerization reaction was continued. After the reaction at 95°C for 30 minutes, the temperature in the pressure vessel was cooled to 30°C, and the polymerization reaction was terminated. Sodium hydroxide was added to this rubber component latex, and unreacted monomers and other mixtures were reduced by steam distillation, and the rubber component latex was filtered through a 200 mesh filter and adjusted to the pH shown in Table 1 with sodium hydroxide, thereby obtaining latex SB-1 containing a first rubber component.
[0199] (Manufacturing example 2: SB-2) In a nitrogen-substituted pressure-resistant reactor, 1085 parts by mass of water, 20 parts by mass of sodium dodecylbenzenesulfonate, and 2 parts by mass of itaconic acid were charged as polymerization initial raw materials all at once and thoroughly stirred at 80 ° C. Next, as a monomer mixture and a chain transfer agent, 20 parts by mass of styrene, 75 parts by mass of butadiene, 0.5 parts by mass of methyl methacrylate, 0.5 parts by mass of acrylonitrile, 2 parts by mass of 2-hydroxyethyl acrylate, and 1.9 parts by mass of t-dodecyl mercaptan were mixed, and 10% of the monomer mixture was added to the pressure-resistant vessel and thoroughly stirred. Next, 10 parts by mass of an aqueous sodium hydrogen sulfite solution with a solid content of 9% by mass was added to the pressure-resistant vessel, and 5 minutes later, 10 parts by mass of an aqueous sodium persulfate solution with a solid content of 30% by mass was added to the pressure-resistant vessel. Ten minutes after the addition of the aqueous sodium persulfate solution with a solid content of 30% by mass, the remaining 90% of the monomer mixture was continuously added to the pressure vessel over a period of two hours. Furthermore, 20 minutes after the addition of the aqueous sodium persulfate solution with a solid content of 30% by mass, an aqueous mixture in which 0.6 parts by mass of sodium hydroxide and 1.35 parts by mass of sodium persulfate were dissolved in 86 parts by mass of water was continuously added to the pressure vessel over a period of three hours. Four hours and 45 minutes after the addition of the aqueous sodium persulfate solution with a solid content of 30% by mass, the temperature in the pressure vessel was raised to 95°C, and the polymerization reaction was continued. After reacting for 30 minutes at 95°C, the temperature in the pressure vessel was cooled to 30°C, and the polymerization reaction was terminated. Sodium hydroxide was added to this rubber component latex to reduce the unreacted monomer mixture by steam distillation, and the rubber component latex was filtered through a 200-mesh filter and adjusted to the pH shown in Table 1 with sodium hydroxide to obtain latex SB-2 containing a first rubber component.
[0200] (Manufacturing example 3: SB-3) In a nitrogen-substituted pressure-resistant reactor, 1085 parts by mass of water, 20 parts by mass of sodium dodecylbenzenesulfonate, and 2 parts by mass of itaconic acid were charged as polymerization initial raw materials all at once, and thoroughly stirred at 80 ° C. Next, as the monomer mixture and the chain transfer agent, 20 parts by mass of styrene, 75 parts by mass of butadiene, 0.5 parts by mass of methyl methacrylate, 0.5 parts by mass of acrylonitrile, 2 parts by mass of 2-hydroxyethyl acrylate, and 3 parts by mass of t-dodecyl mercaptan were mixed, and 10% of the monomer mixture was added to the pressure-resistant vessel and thoroughly stirred. Next, 10 parts by mass of an aqueous solution of sodium hydrogen sulfite with a solid content of 9% by mass was added to the pressure-resistant vessel, and 5 minutes later, 10 parts by mass of an aqueous solution of sodium persulfate with a solid content of 30% by mass was added to the pressure-resistant vessel. 10 minutes after the addition of the aqueous solution of sodium persulfate with a solid content of 30% by mass, the remaining 90% of the monomer mixture was continuously added to the pressure-resistant vessel over 2 hours. Further, 20 minutes after the addition of the aqueous sodium persulfate solution having a solid content of 30% by mass, an aqueous mixture in which 0.6 parts by mass of sodium hydroxide and 1.35 parts by mass of sodium persulfate were dissolved in 86 parts by mass of water was continuously added to the pressure vessel over a period of 3 hours. Five hours and 45 minutes after the addition of the aqueous sodium persulfate solution having a solid content of 30% by mass, the temperature in the pressure vessel was raised to 95°C, and the polymerization reaction was continued. After reacting at 95°C for 30 minutes, the temperature in the pressure vessel was cooled to 30°C, and the polymerization reaction was terminated. Sodium hydroxide was added to this rubber component latex, and the mixture of unreacted monomers and the like was reduced by steam distillation, and the rubber component latex was filtered through a 200-mesh filter and adjusted to the pH shown in Table 1 with sodium hydroxide to obtain latex SB-3 containing a first rubber component.
[0201] (Manufacturing example 4: SB-4) In a nitrogen-substituted pressure-resistant reactor, 1160 parts by mass of water, 20 parts by mass of sodium dodecylbenzenesulfonate, and 2 parts by mass of itaconic acid were charged as the polymerization initial raw materials all at once and thoroughly stirred at 80 ° C. Next, as the monomer mixture and the chain transfer agent, 55 parts by mass of styrene, 40 parts by mass of butadiene, 0.5 parts by mass of methyl methacrylate, 0.5 parts by mass of acrylonitrile, 2 parts by mass of 2-hydroxyethyl acrylate, and 0.7 parts by mass of t-dodecyl mercaptan were mixed, and 10% of the monomer mixture was added to the pressure-resistant vessel and thoroughly stirred. Next, 3.3 parts by mass of an aqueous sodium hydrogen sulfite solution with a solid content of 9% by mass was added to the pressure-resistant vessel, and 5 minutes later, 3.3 parts by mass of an aqueous sodium persulfate solution with a solid content of 30% by mass was added to the pressure-resistant vessel. Ten minutes after the addition of the aqueous sodium persulfate solution with a solid content of 30% by mass, the remaining 90% of the monomer mixture was continuously added to the pressure vessel over a period of 2 hours. Furthermore, 2 hours and 50 minutes after the addition of the aqueous sodium persulfate solution with a solid content of 30% by mass, an aqueous mixture in which 1.35 parts by mass of sodium persulfate was dissolved in 50 parts by mass of water was continuously added to the pressure vessel over a period of 2 hours and 50 minutes. Five hours and 45 minutes after the addition of the aqueous sodium persulfate solution with a solid content of 30% by mass, the temperature in the pressure vessel was raised to 95°C, and the polymerization reaction was continued. After reacting at 95°C for 1 hour and 30 minutes, the temperature in the pressure vessel was cooled to 30°C, and the polymerization reaction was terminated. Sodium hydroxide was added to this rubber component latex to reduce the unreacted monomer mixture by steam distillation, and the rubber component latex was filtered through a 200-mesh filter and adjusted to the pH shown in Table 1 with sodium hydroxide to obtain latex SB-4 containing a first rubber component.
[0202] (Manufacturing example 5: SB-5) In a nitrogen-substituted pressure-resistant reactor, 1085 parts by mass of water, 20 parts by mass of sodium dodecylbenzenesulfonate, and 2 parts by mass of itaconic acid were charged as polymerization initial raw materials all at once and thoroughly stirred at 80 ° C. Next, as a monomer mixture and a chain transfer agent, 55 parts by mass of styrene, 40 parts by mass of butadiene, 0.5 parts by mass of methyl methacrylate, 0.5 parts by mass of acrylonitrile, 2 parts by mass of 2-hydroxyethyl acrylate, and 0.8 parts by mass of t-dodecyl mercaptan were mixed, and 10% of the monomer mixture was added to the pressure-resistant vessel and thoroughly stirred. Next, 10 parts by mass of an aqueous sodium hydrogen sulfite solution with a solid content of 9% by mass was added to the pressure-resistant vessel, and 5 minutes later, 10 parts by mass of an aqueous sodium persulfate solution with a solid content of 30% by mass was added to the pressure-resistant vessel. Ten minutes after the addition of the 30% by mass aqueous sodium persulfate solution, the remaining 90% of the monomer mixture was added continuously to the pressure vessel over a period of two hours. Furthermore, 2 hours and 20 minutes after the addition of the 30% by mass aqueous sodium persulfate solution, an aqueous mixture in which 0.6 parts by mass of sodium hydroxide and 1.35 parts by mass of sodium persulfate were dissolved in 86 parts by mass of water was added continuously to the pressure vessel over a period of three hours and 20 minutes. Five hours and 45 minutes after the addition of the 30% by mass aqueous sodium persulfate solution, the temperature in the pressure vessel was raised to 95°C, and the polymerization reaction was continued. After the reaction at 95°C for 1 hour and 30 minutes, the temperature in the pressure vessel was cooled to 30°C, and the polymerization reaction was terminated. Sodium hydroxide was added to this rubber component latex, and unreacted monomers and other mixtures were reduced by steam distillation, and the rubber component latex was filtered through a 200 mesh filter and adjusted to the pH shown in Table 1 with sodium hydroxide to obtain latex SB-5 containing a first rubber component.
[0203] (Manufacturing example 6: SB-6) In a nitrogen-substituted pressure-resistant reactor, 125 parts by mass of water and 12 parts by mass of an aqueous solution of Aqualon HS-1025 (polyoxyethylene nonylpropenyl phenyl ether ammonium sulfate) (a reactive emulsifier having a hydrophilic group) (solid content 25% by mass) were charged as the initial polymerization raw materials all at once, and thoroughly stirred at 90 ° C. Next, as the monomer mixture and the chain transfer agent, 17.5 parts by mass of styrene, 75 parts by mass of butadiene, 0.5 parts by mass of 2-ethylhexyl acrylate (a monomer having no hydrophilic group), 2 parts by mass of acrylic acid (a monomer having a carboxy group as a hydrophilic group), 5 parts by mass of methacrylic acid (a monomer having a carboxy group as a hydrophilic group), and 2.9 parts by mass of t-dodecyl mercaptan were mixed, and the mixture of monomers, etc. was continuously added to the pressure-resistant vessel over 7 hours. Next, 15 minutes after the mixture of monomers, etc. was added to the pressure-resistant vessel, 1.3 parts by mass of an aqueous solution of sodium persulfate having a solid content of 30% by mass was added. Further, 30 minutes after the monomer mixture was added to the pressure vessel, an aqueous mixture of 0.25 parts by mass of sodium hydroxide, 4 parts by mass of an aqueous solution of Aqualon HS-1025, and 0.8 parts by mass of sodium persulfate dissolved in 23 parts by mass of water was continuously added to the pressure vessel over a period of 7 hours and 30 minutes. 9 hours and 15 minutes after the addition of the aqueous solution of sodium persulfate with a solid content of 30% by mass, the temperature inside the pressure vessel was cooled to 30°C, and the polymerization reaction was terminated. Sodium hydroxide was added to this rubber component latex, and the unreacted monomer mixture was reduced by steam distillation, and the rubber component latex was filtered through a 200-mesh filter and adjusted to the pH shown in Table 1 with sodium hydroxide to obtain latex SB-6 containing a first rubber component.
[0204] (Manufacturing example 7: SB-7) In a nitrogen-substituted pressure-resistant reactor, 125 parts by mass of water and 12 parts by mass of an aqueous solution of Aqualon HS-1025 (solid content 25% by mass) were charged as the polymerization initial raw materials all at once, and thoroughly stirred at 90°C. Next, the monomer mixture and chain transfer agents, 17.5 parts by mass of styrene, 75 parts by mass of butadiene, 0.5 parts by mass of 2-ethylhexyl acrylate, 2 parts by mass of acrylic acid, 5 parts by mass of methacrylic acid, and 5 parts by mass of t-dodecyl mercaptan, were mixed, and the monomer mixture was continuously added to the pressure-resistant vessel over 7 hours. Next, 15 minutes after the monomer mixture was added to the pressure-resistant vessel, 1.3 parts by mass of an aqueous solution of sodium persulfate with a solid content of 30% by mass was added. Further, 30 minutes after the monomer mixture was added to the pressure vessel, an aqueous mixture of 0.25 parts by mass of sodium hydroxide, 4 parts by mass of an aqueous solution of Aqualon HS-1025, and 0.8 parts by mass of sodium persulfate dissolved in 23 parts by mass of water was continuously added to the pressure vessel over 7 hours and 30 minutes. 9 hours and 15 minutes after the addition of the aqueous solution of sodium persulfate with a solid content of 30% by mass, the temperature inside the pressure vessel was cooled to 30°C, and the polymerization reaction was terminated. Sodium hydroxide was added to this rubber component latex, and the unreacted monomer mixture was reduced by steam distillation, and the rubber component latex was filtered through a 200-mesh filter and adjusted to the pH shown in Table 1 with sodium hydroxide to obtain latex SB-7 containing a first rubber component.
[0205] (Manufacturing example 8:SB-8) In a nitrogen-substituted pressure-resistant reactor, 125 parts by mass of water and 12 parts by mass of an aqueous solution of Aqualon HS-1025 (solid content 25% by mass) were charged as the polymerization initial raw material all at once, and thoroughly stirred at 85°C. Next, the monomer mixture and chain transfer agent, 17.5 parts by mass of styrene, 75 parts by mass of butadiene, 0.5 parts by mass of 2-ethylhexyl acrylate, 2 parts by mass of acrylic acid, 5 parts by mass of methacrylic acid, and 7 parts by mass of t-dodecyl mercaptan, were mixed, and the monomer mixture was continuously added to the pressure-resistant vessel over 7 hours. Next, 15 minutes after the monomer mixture was added to the pressure-resistant vessel, 1.3 parts by mass of an aqueous solution of sodium persulfate with a solid content of 30% by mass was added. Further, 30 minutes after the monomer mixture was added to the pressure vessel, an aqueous mixture obtained by dissolving 0.25 parts by mass of sodium hydroxide, 4 parts by mass of an aqueous solution of Aqualon HS-1025, and 0.8 parts by mass of sodium persulfate in 23 parts by mass of water was continuously added to the pressure vessel over a period of 7 hours and 30 minutes. After the addition of the aqueous mixture was completed, the temperature in the pressure vessel was raised to 90°C to continue the polymerization reaction. After reacting at 90°C for 1 hour, the temperature in the pressure vessel was cooled to 30°C to terminate the polymerization reaction. Sodium hydroxide was added to this rubber component latex to reduce the unreacted monomer mixture by steam distillation, and the rubber component latex was filtered through a 200-mesh filter and adjusted to the pH shown in Table 1 with sodium hydroxide to obtain latex SB-8 containing a first rubber component.
[0206] (Comparative manufacturing example 9: SB-9) In a nitrogen-substituted pressure-resistant reactor, 1085 parts by mass of water and 20 parts by mass of sodium dodecylbenzenesulfonate were charged as polymerization initial raw materials all at once and thoroughly stirred at 80°C. Next, the monomer mixture and chain transfer agent were mixed with 24 parts by mass of styrene, 75 parts by mass of butadiene, 0.5 parts by mass of methyl methacrylate, 0.5 parts by mass of acrylonitrile, and 0.5 parts by mass of t-dodecyl mercaptan, and 10% of the monomer mixture was added to the pressure-resistant vessel and thoroughly stirred. Next, 10 parts by mass of an aqueous solution of sodium hydrogen sulfite with a solid content of 9% by mass was added to the pressure-resistant vessel, and 5 minutes later, 10 parts by mass of an aqueous solution of sodium persulfate with a solid content of 30% by mass was added to the pressure-resistant vessel. 10 minutes after the addition of the aqueous solution of sodium persulfate with a solid content of 30% by mass, the remaining 90% of the monomer mixture was continuously added to the pressure-resistant vessel over 2 hours. Further, 20 minutes after the addition of the aqueous sodium persulfate solution with a solid content of 30% by mass, an aqueous mixture in which 0.6 parts by mass of sodium hydroxide and 1.35 parts by mass of sodium persulfate were dissolved in 86 parts by mass of water was continuously added to the pressure vessel over a period of 3 hours. 4 hours and 45 minutes after the addition of the aqueous sodium persulfate solution with a solid content of 30% by mass, the temperature in the pressure vessel was raised to 95°C to continue the polymerization reaction. After reacting at 95°C for 30 minutes, the temperature in the pressure vessel was cooled to 30°C to terminate the polymerization reaction. Sodium hydroxide was added to this rubber component latex, and the unreacted monomer mixture was reduced by steam distillation, and the rubber component latex was filtered through a 200-mesh filter and adjusted to the pH shown in Table 1 with sodium hydroxide to obtain latex SB-9 containing the first rubber component. In SB-10, agglomerates were generated before and after the unreacted monomer mixture was reduced by steam distillation, and the particle size was enlarged.
[0207] (Manufacturing example 10:SB-10) In a nitrogen-substituted pressure-resistant reactor, 125 parts by mass of water and 12 parts by mass of an aqueous solution of Aqualon HS-1025 (solid content 25% by mass) were charged as polymerization initial raw materials all at once, and thoroughly stirred at 90°C. Next, as the monomer mixture and the chain transfer agent, 17.5 parts by mass of styrene, 75 parts by mass of butadiene, 0.5 parts by mass of 2-ethylhexyl acrylate, 2 parts by mass of acrylic acid, and 5 parts by mass of methacrylic acid were mixed, and the monomer mixture was continuously added to the pressure-resistant vessel over 7 hours. Next, 15 minutes after the monomer mixture was added to the pressure-resistant vessel, 1.3 parts by mass of an aqueous solution of sodium persulfate with a solid content of 30% by mass was added. Furthermore, 30 minutes after the monomer mixture was added to the pressure-resistant vessel, an aqueous mixture in which 0.25 parts by mass of sodium hydroxide, 4 parts by mass of an aqueous solution of Aqualon HS-1025, and 0.8 parts by mass of sodium persulfate were dissolved in 23 parts by mass of water was continuously added to the pressure-resistant vessel over 7 hours and 30 minutes. Nine hours and 15 minutes after the addition of the aqueous sodium persulfate solution with a solid content of 30% by mass, the temperature inside the pressure vessel was cooled to 30°C to terminate the polymerization reaction. Sodium hydroxide was added to this rubber component latex, and the unreacted monomer mixture was reduced by steam distillation, and the rubber component latex was filtered through a 200 mesh filter and adjusted to the pH shown in Table 1 with sodium hydroxide to obtain SB-10 containing a first rubber component latex. A large amount of residue was generated in SB-10 before the unreacted monomer mixture was reduced by steam distillation.
[0208] <Cellulose nanofiber> CNF-1: Microfibrillated cellulose 3 parts by mass of cotton linter pulp was immersed in 27 parts by mass of water and dispersed with a pulper. 30 parts by mass of the pulper-treated cotton linter pulp slurry (including 3 parts by mass of cotton linter pulp) was added to 170 parts by mass of water to disperse the mixture in water (solid content rate: 1.5% by mass), and the aqueous dispersion was beaten for 30 minutes using a SDR14 lab refiner (pressure type DISK type) manufactured by Aikawa Iron Works Co., Ltd. as a disc refiner device with a clearance between discs of 1 mm. Subsequently, thorough beating was performed under conditions in which the clearance was reduced to a level close to zero, to obtain a beaten aqueous dispersion (solid content concentration: 1.5% by mass). The obtained beaten aqueous dispersion was directly subjected to a high-pressure homogenizer (NSO15H manufactured by Niro Soavi Co., Ltd. (Italy)) for 10 times of refinement under an operating pressure of 100 MPa to obtain a fine cellulose fiber slurry (solid content concentration: 1.5% by mass). The mixture was then concentrated using a dehydrator to a solid content of 10% by mass to obtain a concentrated cake of fine fibrous cellulose CNF-1.
[0209] <Nonionic surfactant> Surfactant-1: Sannix GL-3000 (polyether polyol, solubility at 25°C: 1% by mass) manufactured by Sanyo Chemical Industries, Ltd.
[0210] <Vulcanization aid> Zinc oxide: available from Fujifilm Wako Pure Chemical Industries, Ltd. Stearic acid: available from Fujifilm Wako Pure Chemical Industries, Ltd.
[0211] <Anti-aging agent> Nocrac 6C: N-phenyl-N'-(1,3-dimethylbutyl)-p-phenylenediamine (available from Ouchi Shinko Chemical Co., Ltd.)
[0212] <Sulfur> Tsurumi Chemical Industry Co., Ltd. "Sulfax 200S" (powdered sulfur)
[0213] <Vulcanization accelerator> Vulcanization accelerator-1: N-cyclohexyl-2-benzothiazolylsulfenamide (Noccela CZ, available from Ouchi Shinko Chemical Co., Ltd.) Vulcanization accelerator-2: 1,3-diphenylguanidine (Noccelaer D, available from Ouchi Shinko Chemical Co., Ltd.)
[0214] <Production of rubber composition> <Examples A1 to A14> Rubber compositions (RC-1 to RC-14) Purified water was added to the concentrated cake of fine fibrous cellulose CNF-1 to prepare an aqueous dispersion with a final cellulose nanofiber content of 5% by mass, to which a surfactant and rubber latex particles were added according to the composition shown in Table 2, and mixed for 5 minutes using a centrifugal mixer ARE-310 manufactured by Thinky Corporation to obtain a dispersion of a cellulose nanofiber composition. Here, the weight of the cellulose nanofiber in Table 2 is the net solid content not including water in the dispersion. The obtained dispersion was dried at 80°C using SPH-201 manufactured by Espec Corporation. The obtained dried product was pulverized using a mini speed mill MS-05 manufactured by LabNect Co., Ltd. to obtain a powdered rubber composition.
[0215] <Evaluation of Rubber Composition> The rubber compositions were subjected to the following evaluations.
[0216] [Toluene insoluble ratio, weight average molecular weight of tetrahydrofuran soluble matter, and gas transition temperature of rubber composition] The weight average molecular weight of the soluble matter was measured by dissolving the rubber composition in tetrahydrofuran and measuring the weight average molecular weight of the extracted matter in the same manner as for the rubber component.
[0217] <Master batch> <Examples B1 to B15> Masterbatches for rubber modification (MB-1 to MB-15) In the first stage of mixing, a closed mixer (capacity: 0.35 L) equipped with a temperature control device was used to mix the solution polymerized rubber or modified liquid rubber and the rubber composition according to the composition shown in Table 3 under conditions of a filling rate of 65% and a rotor rotation speed of 30 to 100 rpm. At this time, the temperature of the closed mixer was controlled, and the discharge temperature was 155 to 160°C to obtain a rubber composition (compound). Next, in the second stage of mixing, the mixture obtained above was cooled to room temperature and then mixed again to improve the dispersion of CNF. In this case, the temperature of the internal mixer was also controlled, and the discharge temperature was adjusted to 155 to 160°C to obtain a master batch for rubber modification.
[0218] <Rubber composite and cured rubber> <Examples C1 to C12 and Comparative Examples C1 to C3> The master batch and the solution polymerized rubber or modified liquid rubber shown in Table 4 were kneaded according to the formulation shown in Table 4 by the following method to obtain a conjugated diene polymer composition. In the first stage of mixing, the master batch, solution polymerized rubber or modified liquid rubber, zinc oxide, and stearic acid were mixed at a filling rate of 65% and a rotor rotation speed of 30 to 100 rpm using an internal mixer (capacity 0.35 L) equipped with a temperature control device. At this time, the temperature of the internal mixer was controlled, and each rubber composite (compound) was obtained at a discharge temperature of 155 to 160°C. Next, in the second stage of mixing, the mixture obtained above was cooled to room temperature, and then an antioxidant was added and mixed again to improve the dispersion of the cellulose nanofibers. In this case, the temperature of the mixer was controlled to 155 to 160°C. After cooling, in the third stage of mixing, sulfur, vulcanization accelerator-1, and vulcanization accelerator-2 were added and mixed in an open roll set at 70°C. The mixture was then molded and vulcanized in a vulcanization press at 160°C for 25 minutes. The properties of the cured rubber after vulcanization were evaluated. The results are shown in Table 4.
[0219] <Examples C13 to C24 and Comparative Examples C4 to C7> The rubber composition shown in Table 5, and the solution polymerized rubber or modified liquid rubber were kneaded according to the formulation shown in Table 5 by the following method to obtain a conjugated diene polymer composition. In the first stage of mixing, the rubber composition, solution polymerized rubber or modified liquid rubber, zinc oxide, and stearic acid were mixed at a filling rate of 65% and a rotor rotation speed of 30 to 100 rpm using an internal mixer (capacity: 0.35 L) equipped with a temperature control device. At this time, the temperature of the internal mixer was controlled, and the discharge temperature was 155 to 160°C to obtain each rubber composite (compound). Next, in the second stage of mixing, the mixture obtained above was cooled to room temperature, and then an antioxidant was added and mixed again to improve the dispersion of the cellulose nanofibers. In this case, the temperature of the mixer was controlled to 155 to 160°C. After cooling, in the third stage of mixing, sulfur, vulcanization accelerator-1, and vulcanization accelerator-2 were added and mixed in an open roll set at 70°C. The mixture was then molded and vulcanized in a vulcanization press at 160°C for 25 minutes. The properties of the cured rubber after vulcanization were evaluated. The results are shown in Table 5.
[0220] <Evaluation of cured rubber> [Dispersibility of cellulose nanofibers] For the cured rubber composites and control samples of Examples C1 to C24, Comparative Examples C1 to C3, and Comparative Examples C5 to C7, while placed in a vulcanization press mold, the dispersion state of the cellulose nanofibers was visually evaluated in a 5 cm square area on the surface according to the following criteria. A: No visible aggregates B: A small number of aggregates (1 to 10) are observed. C: Many aggregates (11 or more) were observed.
[0221] [Hardness] For the cured rubber composites and control samples of Examples C1 to C24 and Comparative Examples C1 to C7, the hardness of the vulcanized products was measured using a Type A durometer in accordance with JIS K6253 "Testing method for hardness of vulcanized rubber and thermoplastic rubber." The measurements were performed at 25°C. [Storage modulus] For the cured rubber composites and control samples of Examples C1 to C24 and Comparative Examples C1 to C7, the storage modulus was evaluated at 25°C, a frequency of 10 Hz, and a strain of 1% using a TA Instruments ARES-G2 viscoelasticity tester by torsion.
[0222] [Tensile strength and tensile modulus] For the cured rubber composites and control samples of Examples C1 to C24 and Comparative Examples C1 to C7, the tensile strength and tensile modulus (50% and 100%) were measured in accordance with the tensile testing method of JIS K6251.
[0223] [Table 1]
[0224] [Table 2]
[0225] [Table 3]
[0226] [Table 4]
[0227] [Table 5] [Industrial Applicability]
[0228] The rubber composition according to the present disclosure can be formed into molded articles having good physical properties, and therefore can be suitably used in a wide range of applications, such as industrial machine parts, general machine parts, automobile, railway, vehicle, ship, and aerospace related parts, electronic and electrical parts, building and civil engineering materials, daily necessities, sports and leisure goods, housing parts for wind power generation, containers and packaging parts, etc.
Claims
1. A composition comprising cellulose nanofibers and a first rubber component which is a hydrophilic group-containing rubber derived from rubber latex, the first rubber component comprises a toluene-insoluble component, A composition, wherein when 0.5 g of the composition is stirred in 30 mL of toluene at 25° C., a toluene-insoluble ratio, which is a ratio of dissolved residue to 100% by mass of solids in the composition, is 30% by mass or more and 99% by mass or less.
2. The composition according to claim 1, comprising 1 to 200 parts by mass of the first rubber component per 100 parts by mass of the cellulose nanofibers.
3. The composition according to claim 1 or 2, wherein the dissolved residue comprises the cellulose nanofibers and the first rubber component.
4. The composition according to claim 1 or 2, wherein the first rubber component is a styrene-butadiene rubber.
5. The composition according to claim 1 or 2, wherein a ratio of butadiene monomer units to all monomer units of the first rubber component is 20% by mass or more and 95% by mass or less.
6. The composition according to claim 1 or 2, wherein the first rubber component has a glass transition temperature of 10° C. or lower.
7. The composition according to claim 1 or 2, wherein the first rubber component has a residual monomer amount of 10% by mass or less.
8. The composition according to claim 1 or 2, wherein the hydrophilic group contained in the first rubber component is at least one type selected from the group consisting of a carboxy group, a hydroxy group, a sulfonyl group, and a phosphate group.
9. The composition according to claim 1 or 2, wherein the first rubber component has a weight average molecular weight (Mw) of 5,000 or more and 400,000 or less.
10. 3. The composition according to claim 1, further comprising a sparingly soluble surfactant having a solubility of 20 g or less in 100 g of water at 25°C.
11. 11. The composition of claim 10, wherein the surfactant further comprises two or more selected from the group consisting of alkylbenzenesulfonic acids, alkylsulfonic acids, alkylsulfosuccinic acids, polyoxyethylene alkylsulfuric acids, polyoxyethylene alkylarylsulfuric acids, polyoxyethylene distyryl phenyl ether sulfonic acids and their alkali metal or ammonium salts; fatty acid soaps; alkyltrimethylammonium bromides; alkylpyridinium bromides; imidazolinium laurates; polyoxyethylene alkylaryl ethers; polyoxyethylene alkyl ethers; polyoxyethylene sorbitan fatty acid esters; sorbitan fatty acid esters; polyoxyethylene oxypropylene block copolymers; and polyoxyethylene distyryl phenyl ethers.
12. The composition according to claim 1 or 2, which is in the form of a sheet, pellet or powder.
13. An aqueous dispersion comprising cellulose nanofibers and a first rubber component which is a hydrophilic group-containing rubber derived from rubber latex, the first rubber component comprises a toluene-insoluble component, An aqueous dispersion, wherein when 0.5 g of a composition obtained by drying the aqueous dispersion is stirred in 30 mL of toluene at 25°C, a toluene-insoluble ratio, which is the ratio of dissolved residue to 100 mass% of solids in the composition, is 30 mass% or more and 99 mass% or less.
14. A method for producing the composition according to claim 1 or 2, comprising the steps of: Obtaining an aqueous dispersion by mixing cellulose nanofibers with a rubber latex containing rubber particles having a hydrophilic group; and Optionally, drying the aqueous dispersion. A method comprising:
15. 15. The method of claim 14, wherein the rubber particles have an average particle size of 1 μm or less.
16. A masterbatch which is a kneaded product containing the composition according to claim 1 and a second rubber component.
17. 17. The masterbatch of claim 16, wherein the second rubber component comprises at least one selected from the group consisting of natural rubber, styrene butadiene rubber, butadiene rubber, isoprene rubber, chloroprene rubber, ethylene propylene diene rubber, and butyl rubber and derivatives thereof.
18. The masterbatch according to claim 16, comprising 10 parts by mass to 50 parts by mass of cellulose nanofiber per 100 parts by mass of the total of the first rubber component and the second rubber component.
19. A rubber composite, which is a kneaded product containing a component derived from the composition according to claim 1 or 2 or the masterbatch according to any one of claims 16 to 18 and a third rubber component.
20. The rubber composite according to claim 19, comprising 1 part by mass or more and 15 parts by mass or less of cellulose nanofiber per 100 parts by mass of the first rubber component, the second rubber component, and the third rubber component combined.
21. A cured rubber product, which is a cured product of the rubber composite according to claim 19.
22. A method for producing the masterbatch according to any one of claims 16 to 18, comprising the steps of: A method comprising a step of mixing a composition comprising cellulose nanofibers and a first rubber component with a second rubber component.
23. 20. A method for producing a rubber composite according to claim 19, comprising: A step of mixing a composition containing cellulose nanofibers and a first rubber component with a second rubber component to prepare a master batch; and mixing the master batch with a third rubber component to prepare a rubber composite; A method comprising:
24. 20. A method for producing a rubber composite according to claim 19, comprising: A method comprising: mixing a composition comprising cellulose nanofibers and a first rubber component with a third rubber component to prepare a rubber composite.
25. A method for producing a cured rubber product according to claim 21, comprising the steps of: A step of mixing a composition containing cellulose nanofibers and a first rubber component with a second rubber component to prepare a master batch; mixing the master batch with a third rubber component to prepare a rubber composite; and curing the rubber composite; A method comprising:
26. A method for producing a cured rubber product according to claim 21, comprising the steps of: A step of mixing a composition containing cellulose nanofibers and a first rubber component with a third rubber component to prepare a rubber composite; and curing the rubber composite; A method comprising:
Citation Information
Patent Citations
Rubber composition and pneumatic tire
JP2014047328A
Aqueous resin composition containing cellulose nanofiber, manufacturing method therefor, ultra extended resin film and ultra extended resin product using the same
JP2020094180A
Composite resin composition
JP2020200436A
Composite resin composition, crosslinking resin composition, and method for producing composite resin composition
JP2022077708A