Tube container and manufacturing method thereof

A resin composition with EVOH and specific unsaturated aldehydes, combined with a polyolefin layer structure, addresses neck-in and die build-up issues in tube containers, ensuring uniformity and improved gas barrier properties.

JP2024144248APending Publication Date: 2024-10-11KURARAY CO LTD
View PDF 1 Cites 0 Cited by

Patent Information

Application Number
JP2024044529
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Priority Date
2023-03-29
Filing Date
2024-03-21
Publication Date
2024-10-11

AI Technical Summary

Technical Problem

Existing EVOH resin compositions used in tube containers are prone to neck-in during film formation with T-dies, leading to uneven thickness and poor appearance and strength in blow-molded containers, and also suffer from die build-up issues that degrade gas barrier properties and appearance during repeated use.

Method used

A resin composition containing EVOH with specific ratios of crotonaldehyde, 2,4-hexadienal, and 2,4,6-octatrienal, along with a polyolefin layer structure, is used to form a laminate that suppresses neck-in and die build-up, ensuring uniform gas barrier properties and good appearance.

Benefits of technology

The solution effectively prevents neck-in and die build-up, resulting in tube containers with uniform thickness, improved appearance, and enhanced gas barrier properties, suitable for viscous contents like toothpaste and wasabi paste.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024144248000001_ABST
    Figure 2024144248000001_ABST
Patent Text Reader

Abstract

To provide a tube container having a layer formed using a resin composition which contains EVOH and is suppressed from undergoing neck-in and die build-up during melt molding, and which has high uniformity in gas barrier property and a good appearance.SOLUTION: A tube container comprising a body part formed of a cylindrical laminate and having a storage part inside for storing a content, and a pouring part provided at one end of the body part, has an outermost layer (X) and an innermost layer (Y) of the laminate both made of a polyolefin resin, has a layer (α) made of a resin composition between the outermost layer (X) and the innermost layer (Y), the resin composition contains a specific amount of EVOH (A) and crotonaldehyde (B1), and further contains a specific amount of at least one member selected from the group consisting of 2,4-hexadienal (B2) and 2,4,6-octatrienal (B3).SELECTED DRAWING: Figure 1
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a tube container and a method for manufacturing the same. [Background technology]

[0002] Ethylene-vinyl alcohol copolymer (hereinafter sometimes abbreviated as "EVOH") is a polymeric material that is excellent in gas barrier properties such as oxygen, oil resistance, antistatic properties, mechanical strength, melt moldability, etc. For this reason, EVOH resin compositions are widely used as molding materials for containers, sheets, films, thermoformed containers, tube containers, etc. Melt molding is generally used for molding containers, etc. In particular, for tube containers, a multilayer structure consisting of a layer containing EVOH and a layer of another thermoplastic resin that is excellent in moisture resistance, impact resistance, etc. is widely used. Resin compositions to be subjected to melt molding are required to have excellent long-run performance, such as no defects such as fish eyes and streaks even when melt molding is performed for a long time.

[0003] Tube containers are widely used as containers for viscous contents (e.g., toothpaste and wasabi paste). These tube containers are generally composed of a top and a body, and melt molding is generally used to manufacture the laminate that constitutes the body. However, since EVOH has relatively active hydroxyl groups in its molecules, during melt molding, even inside an extrusion molding machine in an almost oxygen-free state, oxidation and crosslinking reactions may proceed in a high-temperature molten state, resulting in the generation of thermal degradation products. In particular, when the machine is operated continuously for a long period of time, the above-mentioned thermal degradation products accumulate inside the molding machine, generating gels and particles that cause fish eyes, and the EVOH resin composition may have insufficient long-run properties. In addition, these particles not only impair the appearance of the molded product, but also cause performance deterioration, so it is necessary to suppress their generation.

[0004] In contrast, Patent Document 1 describes that a resin composition containing EVOH and 0.01 to 100 ppm of an unsaturated aldehyde suppresses the occurrence of defects such as fish eyes, gels, and streaks, and has excellent long-run properties. [Prior art documents] [Patent documents]

[0005] [Patent Document 1] International Publication No. 2013 / 146961 Summary of the Invention [Problem to be solved by the invention]

[0006] It was found that, when the EVOH resin composition of Patent Document 1 is used, neck-in, in which the width of the extruded film is smaller than the effective width of the die, may be a problem in film molding using a T-die. It was also found that, when an EVOH resin composition that is prone to neck-in is used as a blow molding material, the appearance and strength of the resulting tube container tend to be insufficient, probably because the thickness of the layer formed is likely to be uneven. As a result of intensive research by the present inventors, it was surprisingly found that an EVOH resin composition containing specific types of unsaturated aldehydes in a specific ratio can suppress such neck-in. However, when the content of multiple types of unsaturated aldehydes is adjusted in an attempt to suppress neck-in, it was found that a new problem occurs in that die build-up (meaning deposits on the outer surface of the die lip) is likely to adhere to the outer surface of the discharge port (die lip) of the molten resin composition, depending on the ratio of the multiple types of unsaturated aldehydes. It has been found that when an EVOH resin composition that is prone to die build-up is used to make a tubular container, the gas barrier properties and appearance tend to deteriorate when the resulting tubular container is subjected to repeated operations such as squeezing or twisting.

[0007] The present invention has been made under these circumstances, and an object of the present invention is to provide a tubular container which contains EVOH, has a layer formed using a resin composition which is suppressed in terms of neck-in and die build-up during melt molding, and has highly uniform gas barrier properties and a good appearance, and a method for producing such a tubular container. [Means for solving the problem]

[0008] The above objectives are: [1] A tubular container comprising a body formed of a cylindrical laminate, the inside of which is a storage section for storing contents, and a pouring section provided at one end of the body, wherein both of an outermost layer (X) and an innermost layer (Y) of the laminate are made of a polyolefin resin, and a layer (α) made of a resin composition is provided between the outermost layer (X) and the innermost layer (Y), the resin composition comprises an ethylene-vinyl alcohol copolymer (A) having an ethylene unit content of 20 mol% or more and 60 mol% or less, and crotonaldehyde (B1), and further comprises at least one member selected from the group consisting of 2,4-hexadienal (B2) and 2,4,6-octatrienal (B3), and the resin composition satisfies the following formulas (1) and (2): 2.0≦b1 / (b2+b3)<150.0 (1) b2+2b3≦0.65 (2) In the above formulas (1) and (2), b1 is the content (ppm) of crotonaldehyde (B1) relative to the ethylene-vinyl alcohol copolymer (A), b2 is the content (ppm) of 2,4-hexadienal (B2) relative to the ethylene-vinyl alcohol copolymer (A), and b3 is the content (ppm) of 2,4,6-octatrienal (B3) relative to the ethylene-vinyl alcohol copolymer (A); [2] The tube container according to [1], wherein in the resin composition, the total content (b1+b2+b3) of crotonaldehyde (B1), 2,4-hexadienal (B2) and 2,4,6-octatrienal (B3) relative to the ethylene-vinyl alcohol copolymer (A) is 0.01 ppm or more and 7.0 ppm or less; [3] The tube container according to [1] or [2], wherein in the resin composition, the content b1 of crotonaldehyde (B1) is 0.01 ppm or more and 4.0 ppm or less; [4] The tube container of any one of [1] to [3], wherein in the resin composition, the content b2 of 2,4-hexadienal (B2) is 0.005 ppm or more and 0.65 ppm or less; [5] The tube container of any one of [1] to [4], wherein in the resin composition, the content b3 of 2,4,6-octatrienal (B3) is 0.325 ppm or less; [6] The tube container of any of [1] to [5], wherein the resin composition further contains a conjugated polyene compound (C), and the content c of the conjugated polyene compound (C) relative to the ethylene-vinyl alcohol copolymer (A) in the resin composition is 1 ppm or more and less than 300 ppm; [7] A tube container of [6], wherein the conjugated polyene compound (C) is sorbic acid; [8] The tube container of any of [1] to [7], wherein the laminate has a layer (γ) containing a carboxylic acid-modified polyolefin as a main component, and the layer (γ) is disposed between the layer (α) and the outermost layer (X) and between the layer (α) and the innermost layer (Y); [9] A tube container according to any one of [1] to [8], in which the mass ratio of polyolefin resin is 90 mass% or more;

[10] A tube container according to any of [1] to [9], wherein the container has a top opening at one opening of the body, the top opening has the extraction portion and a shoulder portion, and the laminate constituting the top opening is a laminate having a layer (α2) made of a resin composition, the resin composition comprising an ethylene-vinyl alcohol copolymer (A) having an ethylene unit content of 20 mol% or more and 60 mol% or less and crotonaldehyde (B1), and further comprising at least one member selected from the group consisting of 2,4-hexadienal (B2) and 2,4,6-octatrienal (B3), and the resin composition satisfies the following formulas (1) and (2): 2.0≦b1 / (b2+b3)<150.0 (1) b2+2b3≦0.65 (2) In the above formulas (1) and (2), b1 is the content (ppm) of crotonaldehyde (B1) relative to the ethylene-vinyl alcohol copolymer (A), b2 is the content (ppm) of 2,4-hexadienal (B2) relative to the ethylene-vinyl alcohol copolymer (A), and b3 is the content (ppm) of 2,4,6-octatrienal (B3) relative to the ethylene-vinyl alcohol copolymer (A);

[11] The tube container according to

[10] , wherein the cylindrical laminate is formed by overlapping the outermost layer (X) and the innermost layer (Y) at both ends of the laminate and heat-sealing the opposing surfaces;

[12] A tube container according to any one of [1] to

[11] , which is a container for filling food, cosmetics, or medical agents;

[13] A method for producing a tube container according to [1], comprising a step of molding, by blow molding, a cylindrical laminate having an outermost layer (X) and an innermost layer (Y) both made of a polyolefin resin, and having a layer (α) made of a resin composition between the outermost layer (X) and the innermost layer (Y);

[14] A method for producing a tube container according to

[10] , comprising the steps of: forming a body part of a tubular laminate, both of which are made of a polyolefin resin, and which has a layer (α) made of a resin composition between the outermost layer (X) and the innermost layer (Y) by tube molding; and joining a mouth part to one opening of the body part to produce a tube container;

[15] A method for producing a tube container according to

[10] , comprising the steps of: forming a laminate in which both an outermost layer (X) and an innermost layer (Y) are made of a polyolefin resin and a layer (α) made of a resin composition is between the outermost layer (X) and the innermost layer (Y); overlapping the outermost layer (X) and the innermost layer (Y) at both ends of the laminate and heat-sealing the opposing surfaces to form a tubular laminate (body), and joining a mouth part to one opening of the body to produce a tube container; This is achieved by providing Effect of the Invention

[0009] According to the present invention, there can be provided a tubular container having a layer formed using a resin composition that contains EVOH and is suppressed from undergoing neck-in and die build-up during melt molding, and which has highly uniform gas barrier properties and a good appearance, as well as a method for producing such a tubular container. [Brief description of the drawings]

[0010] [Figure 1] FIG. 1 is a cross-sectional view showing a specific example of a laminate for forming a body portion constituting a tube container of the present invention. [Diagram 2] 2(a) and (b) are cross-sectional views showing other examples of laminates for forming the body portion of the tube container of the present invention. [Diagram 3] FIG. 3 is a schematic diagram of a rotary blow molding machine used in the method for producing a tube container of the present invention. [Figure 4] FIG. 4 is a perspective view of an intermediate product in the process of manufacturing a tube container. [Diagram 5] FIG. 5 is a perspective view of a tube container. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0011] In this specification, the term "major component" means a component that is contained in an amount of more than 50 mass %. In this specification, the term "polyolefin resin" refers to a polyolefin resin that does not include the modified polyolefin described below. In this specification, the term "polyolefin resin" refers to polyolefin and modified polyolefin (such as acid-modified polyolefin). Modified polyolefin refers to a polymer obtained by modifying polyolefin. "Polyethylene resin" refers to polyethylene and modified polyethylene (acid-modified polyethylene, etc.). Modified polyethylene refers to a polymer obtained by modifying polyethylene. The term "polyethylene resin" refers to a homopolymer of ethylene, a copolymer of 80 mol % or more ethylene and 20 mol % or less of an α-olefin monomer, and a copolymer of 90 mol % or more ethylene and less than 10 mol % of a non-olefin monomer whose functional groups contain atoms other than carbon, oxygen, and hydrogen atoms. The term "acid-modified polyethylene resin" refers to a polymer obtained by modifying a polyethylene resin with an acid. The acid-modified polyethylene resin may be a polymer in which at least one of an acidic group and an acid anhydride group is introduced into a polyethylene resin. "Recycle", "recovery" or "reuse" means, for example, crushing and melt-kneading the tube container of the present invention, the laminate constituting the body of the tube container, or the laminate constituting the mouth of the tube container, and reusing it as a polyolefin resin. The composition (recovered material) obtained by recycling, recovery or reuse contains the materials constituting the layer (X), layer (α) and layer (Z), and the layer composed of such recovered material is called a recovered layer. The "overall average thickness" refers to the average thickness of the laminate used in the tube container of the present invention.

[0012] Tube containers are well known and are widely used as containers for storing mainly viscous contents (e.g., toothpaste and wasabi paste). These tube containers are generally composed of a top end having an extracting portion and a body portion, and examples of such methods include a method in which the pouring portion and the body portion are integrally molded by blow molding such as direct blow molding and rotary blow molding, a method in which a body portion that is a cylindrical laminate is molded by tube molding and a top end end having a pouring portion is joined to one end of the body portion, and a method in which a body portion that is a cylindrical laminate is molded by a co-extrusion molding machine equipped with a T-die and a top end end having a pouring portion is joined to one end of the body portion.

[0013] (Laminate) The laminate constituting the body of the tube container of the present invention has an outermost layer (X) made of a polyolefin resin and an innermost layer (Y) made of a polyolefin resin, and has a layer (α) made of a resin composition between the outermost layer (X) and the innermost layer (Y). When the tube container of the present invention has a top end, the top end may also have the same embodiment as the laminate constituting the body.

[0014] As the polyolefin resin constituting the outermost layer (X) and the innermost layer (Y), any polyolefin resin can be used, for example, linear low density polyethylene, low density polyethylene, medium density polyethylene, high density polyethylene, polypropylene, etc. Also, modified polyolefin resins obtained by modifying these polyolefin resins may be used. Among them, from the viewpoint of improving recyclability, the polyolefin resin preferably contains a polyethylene resin as a main component, and more preferably is a polyethylene resin. Since polyethylene resins are widely used in packaging materials regardless of whether they have gas barrier properties or not, recycling infrastructures for them are widely established in various countries. When the polyolefin resin contains a polyethylene resin as a main component, the polyethylene resin is preferably at least one selected from linear low density polyethylene, low density polyethylene, medium density polyethylene, and high density polyethylene, and more preferably at least one selected from linear low density polyethylene and low density polyethylene, or a mixture of at least one selected from linear low density polyethylene and low density polyethylene and high density polyethylene.

[0015] A printed layer may be provided on the outside of the outermost layer (X). The printed layer can be formed, for example, by applying a UV-curable ink to the outside of the outermost layer (X) and curing it by UV irradiation. Note that a printed layer provided further outside the "outermost layer" is not treated as the outermost layer in this specification, and the outermost layer (X) is considered to be the outermost layer.

[0016] The proportion of the polyolefin resin in the layer (X) is preferably 70% by mass or more, more preferably 80% by mass or more, and even more preferably 95% by mass or more, and the layer may be composed substantially of only the polyolefin resin. The polyolefin resin preferably contains a polyethylene resin as a main component, and the content of the polyethylene resin in the polyolefin resin is more preferably 70% by mass or more, more preferably 80% by mass or more, and particularly preferably 95% by mass or more, and the polyolefin resin may be composed substantially of only the polyethylene resin.

[0017] The proportion of polyolefin resin in layer (Y) is preferably 70% by mass or more, more preferably 80% by mass or more, and even more preferably 95% by mass or more, similarly to layer (X), and layer (Y) may be composed substantially of polyolefin resin only. Moreover, the polyolefin resin preferably contains polyethylene resin as a main component, and the content of polyethylene resin in the polyolefin resin is more preferably 70% by mass or more, more preferably 80% by mass or more, and particularly preferably 95% by mass or more, and layer (Y) may be composed substantially of polyethylene resin only.

[0018] From the viewpoint of improving recyclability, the proportion of the polyolefin resin in the laminate constituting the tube container of the present invention is preferably 70% by mass or more, more preferably 80% by mass or more, even more preferably 90% by mass or more, particularly preferably 93% by mass or more, and may be 95% by mass or more or 99% by mass or more. Moreover, the polyolefin resin preferably contains a polyethylene resin as a main component, and the content of the polyethylene resin in the polyolefin resin is more preferably 70% by mass or more, even more preferably 80% by mass or more, particularly preferably 95% by mass or more, and may be 99% by mass or more.

[0019] The average thickness of each of the layers (X) and (Y) is preferably 20 to 400 μm. From the viewpoint of imparting flexibility to the tube container, the average thickness is more preferably 300 μm or less, and even more preferably 250 μm or less. From the viewpoint of durability, the average thickness is more preferably 25 μm or more, and even more preferably 30 μm or more.

[0020] In addition, when a laminate is formed by a co-extrusion molding machine equipped with a T-die and then formed into a cylindrical body portion, it is preferable that the outermost layer (X) and the innermost layer (Y) are heat-sealable to each other.

[0021] Furthermore, a laminate can be formed using a co-extrusion molding device in the order of the outermost layer (X), the layer (γ) containing carboxylic acid-modified polyolefin as a main component, the layer (α) made of a resin composition, the layer (γ) containing carboxylic acid-modified polyolefin as a main component, and the innermost layer (Y). This laminate can be formed to have a predetermined layer structure by, for example, charging the resin composition forming the layer (α), the resin forming the outermost layer (X), the resin forming the layer (γ), and the resin composition forming the innermost layer (Y) into separate extruders and co-extruding them with these extruders. The layer (α) and the like will be described in detail below.

[0022] (layer(α)) The layer (α) is a layer made of a predetermined resin composition. The lower limit of the average thickness of the layer (α) is not particularly limited, but from the viewpoint of barrier properties and mechanical strength, it is preferably 0.5%, more preferably 1.0%, even more preferably 1.5%, and even more preferably 2.0% or 3.0% based on the total average thickness. On the other hand, the upper limit of the average thickness of the layer (α) is preferably 5.0%, more preferably 4.5%, and even more preferably 4.1% based on the total average thickness. If the thickness of the layer (α) exceeds 5.0%, it becomes difficult to recycle the laminate constituting the body part of the tube container, the laminate constituting the mouth part, and / or the tube container as a polyolefin resin.

[0023] <Resin composition> The resin composition used to form the layer (α) will be described below. The resin composition contains EVOH (A) and crotonaldehyde (B1), and further contains at least one selected from the group consisting of 2,4-hexadienal (B2) and 2,4,6-octatrienal (B3), and satisfies the following formulas (1) and (2). 2.0≦b1 / (b2+b3)<150.0 (1) b2+2b3≦0.65 (2) In the above formulas (1) and (2), b1 is the content (ppm) of crotonaldehyde (B1) relative to EVOH (A), b2 is the content (ppm) of 2,4-hexadienal (B2) relative to EVOH (A), and b3 is the content (ppm) of 2,4,6-octatrienal (B3) relative to EVOH (A). Note that in this specification, the content expressed in ppm is the content based on mass.

[0024] When the value of b1 / (b2+b3) is 2.0 or more and less than 150.0, the neck-in resistance is good, and the thickness unevenness of the layer (α) of the obtained tube container is reduced, so that the uniformity of the gas barrier property tends to be improved. On the other hand, 2,4-hexadienal (B2) and 2,4,6-octatrienal (B3) affect the die build-up, and 2,4,6-octatrienal (B3) in particular has a large effect on the die build-up. Therefore, when the value of b2+2b3 is 0.65 ppm or less, the resin composition has a suppressed die build-up, and the gas barrier property after squeezing the obtained tube container (hereinafter sometimes referred to as "squeezability") and the tube appearance tend to be good. A tube container formed by a blow molding method or a tube molding method using a resin composition in which neck-in and die build-up are suppressed tends to be less prone to lumps and has improved appearance and squeezability, so the resin composition can be suitably used as a melt molding material for a tube container, etc., by a blow molding method or a tube molding method. In this specification, crotonaldehyde (B1), 2,4-hexadienal (B2), and 2,4,6-octatrienal (B3) may be collectively referred to as an unsaturated aliphatic aldehyde (B).

[0025] (EVOH(A)) EVOH (A) is a copolymer having ethylene units and vinyl alcohol units, and the ethylene unit content is 20 mol% or more and 60 mol% or less. EVOH (A) is usually obtained by saponification of an ethylene-vinyl ester copolymer. The production and saponification of the ethylene-vinyl ester copolymer can be carried out by a known method. Examples of vinyl esters include vinyl acetate, vinyl formate, vinyl propionate, vinyl valerate, vinyl caprate, vinyl laurate, vinyl stearate, vinyl pivalate, vinyl versatate, and other aliphatic carboxylic acid vinyl esters, and vinyl acetate is preferred.

[0026] The ethylene unit content of EVOH (A) is 20 mol% or more, preferably 25 mol% or more, and more preferably 27 mol% or more. The ethylene unit content of EVOH (A) is 60 mol% or less, preferably 55 mol% or less, and more preferably 50 mol% or less. If the ethylene unit content is less than 20 mol%, the thermal stability during melt extrusion decreases, gelation becomes more likely, and streaks, fish eyes, bumps, etc. tend to occur. The occurrence of streaks, fish eyes, bumps, etc. becomes more noticeable when operating for a long time at a higher temperature or higher speed than usual conditions. If the ethylene unit content exceeds 60 mol%, the gas barrier property tends to decrease.

[0027] The saponification degree of EVOH (A) is preferably 90 mol% or more, more preferably 95 mol% or more, and even more preferably 99 mol% or more. When the saponification degree of EVOH (A) is 90 mol% or more, the resulting tube container tends to have good gas barrier properties, heat stability, moisture resistance, etc. Also, the saponification degree may be 100 mol% or less, 99.97 mol% or less, or 99.94 mol% or less.

[0028] In addition, EVOH (A) may have other structural units other than ethylene units, vinyl alcohol units and vinyl ester units, as long as the object of the present invention is not hindered. When EVOH (A) has the other structural units, the content of the other structural units relative to the total structural units of EVOH (A) is preferably 30 mol% or less, more preferably 20 mol% or less, even more preferably 10 mol% or less, even more preferably 5 mol% or less, and sometimes particularly preferably 1 mol% or less. In addition, when EVOH (A) has the other structural units, the content may be 0.05 mol% or more, or 0.10 mol% or more. Examples of the other structural units include structural units derived from unsaturated carboxylic acids such as acrylic acid, methacrylic acid, crotonic acid, itaconic acid, etc., or their anhydrides, salts, or mono- or dialkyl esters; nitriles such as acrylonitrile, methacrylonitrile, etc.; amides such as acrylamide, methacrylamide, etc.; olefin sulfonic acids such as vinyl sulfonic acid, allyl sulfonic acid, methallylsulfonic acid, etc., or their salts; vinyl silane compounds such as vinyltrimethoxysilane, vinyltriethoxysilane, vinyltri(β-methoxy-ethoxy)silane, γ-methacryloxypropylmethoxysilane, etc.; alkyl vinyl ethers, vinyl ketones, N-vinylpyrrolidone, vinyl chloride, vinylidene chloride, etc.

[0029] The other structural unit may be at least one of a structural unit (I) represented by the following formula (I), a structural unit (II) represented by the following formula (II), and a structural unit (III) represented by the following formula (III).

[0030] [ka]

[0031] In formula (I), formula (II) and formula (III), R 1 , R 2 , R 3 , R 4 , R 5 , R 6 , R 7 , R 8 , R9 , R 10 and R 11 each independently represents a hydrogen atom, an aliphatic hydrocarbon group having 1 to 10 carbon atoms, an alicyclic hydrocarbon group having 3 to 10 carbon atoms, an aromatic hydrocarbon group having 6 to 10 carbon atoms, or a hydroxyl group. 1 , R 2 and R 3 One pair of R 4 and R 5 , R 6 and R 7 may be bonded to form a part of a ring structure. Some or all of the hydrogen atoms in the aliphatic hydrocarbon group having 1 to 10 carbon atoms, the alicyclic hydrocarbon group having 3 to 10 carbon atoms, and the aromatic hydrocarbon group having 6 to 10 carbon atoms may be substituted with a hydroxyl group, an alkoxy group, a carboxyl group, or a halogen atom. In formula (III), R 12 and R 13 each independently represents a hydrogen atom, a formyl group, or an alkanoyl group having 2 to 10 carbon atoms.

[0032] When EVOH (A) has the above structural unit (I), (II) or (III), the flexibility and processability of the resin composition tend to be improved, and the stretchability, thermoformability and the like tend to be good.

[0033] In the structural unit (I), (II) or (III), examples of the aliphatic hydrocarbon group having 1 to 10 carbon atoms include an alkyl group, an alkenyl group, etc., examples of the alicyclic hydrocarbon group having 3 to 10 carbon atoms include a cycloalkyl group, a cycloalkenyl group, etc., and examples of the aromatic hydrocarbon group having 6 to 10 carbon atoms include a phenyl group, etc.

[0034] In the structural unit (I), the R 1 , R 2 and R 3 are preferably each independently a hydrogen atom, a methyl group, an ethyl group, a hydroxyl group, a hydroxymethyl group, or a hydroxyethyl group. Among these, from the viewpoint of further improving the moldability and the like of the resin composition, are more preferably each independently a hydrogen atom, a methyl group, a hydroxyl group, or a hydroxymethyl group.

[0035] The method for incorporating the structural unit (I) in EVOH (A) is not particularly limited, and examples thereof include a method of copolymerizing a monomer derived from the structural unit (I) in the polymerization of ethylene and a vinyl ester. Examples of monomers derived from the structural unit (I) include alkenes such as propylene, butylene, pentene, and hexene; 3-hydroxy-1-propene, 3-acyloxy-1-propene, 3-acyloxy-1-butene, 4-acyloxy-1-butene, 3,4-diacyloxy-1-butene, 3-acyloxy-4-hydroxy-1-butene, 4-acyloxy-3-hydroxy-1-butene, 3-acyloxy-4-methyl-1-butene, 4-acyloxy-2-methyl-1-butene, 4-acyloxy-3-methyl-1-butene, 3,4-diacyloxy-2-methyl-1-butene, 4-hydroxy-1-pentene, 5-hydroxy-1-pentene, 4 Examples of alkenes having a hydroxyl group or an ester group include alkenes having a hydroxyl group or an ester group, such as 5-dihydroxy-1-pentene, 4-acyloxy-1-pentene, 5-acyloxy-1-pentene, 4,5-diacyloxy-1-pentene, 4-hydroxy-3-methyl-1-pentene, 5-hydroxy-3-methyl-1-pentene, 4,5-dihydroxy-3-methyl-1-pentene, 5,6-dihydroxy-1-hexene, 4-hydroxy-1-hexene, 5-hydroxy-1-hexene, 6-hydroxy-1-hexene, 4-acyloxy-1-hexene, 5-acyloxy-1-hexene, 6-acyloxy-1-hexene, and 5,6-diacyloxy-1-hexene. Among them, from the viewpoints of copolymerization reactivity, processability in the resulting blow molding or tube molding, and gas barrier properties, propylene, 3-acyloxy-1-propene, 3-acyloxy-1-butene, 4-acyloxy-1-butene, and 3,4-diacyloxy-1-butene are preferred. Note that "acyloxy" is preferably acetoxy, and specifically, 3-acetoxy-1-propene, 3-acetoxy-1-butene, 4-acetoxy-1-butene, and 3,4-diacetoxy-1-butene are preferred. In the case of an alkene having an ester, it is derived into the above structural unit (I) during the saponification reaction.

[0036] In the above structural unit (II), R 4 and R 5 Preferably, both are hydrogen atoms. 4 and R 5 are both hydrogen atoms, and the above R 6 and R 7 It is more preferable that one of R is an aliphatic hydrocarbon group having 1 to 10 carbon atoms, and the other is a hydrogen atom. The aliphatic hydrocarbon group is preferably an alkyl group or an alkenyl group. From the viewpoint of placing special importance on the gas barrier property of the resulting tubular container, R 6 and R 7 It is more preferable that one of the R 6 and R 7 One of them is (CH2) h It is more preferable that the other of the substituents represented by OH (wherein h is an integer of 1 to 8) is a hydrogen atom. (CH2) h In the substituent represented by OH, h is preferably an integer of 1 to 4, more preferably 1 or 2, and even more preferably 1.

[0037] The method for incorporating the structural unit (II) in EVOH (A) is not particularly limited, and for example, a method of incorporating the structural unit (II) by reacting a monofunctional epoxy compound with EVOH (A) obtained by saponification reaction is used. As the monofunctional epoxy compound, the compounds represented by the following formulae (IV) to (X) are preferably used.

[0038] [ka]

[0039] In the above formulas (IV) to (X), R 14 , R 15 , R 16 , R 17 and R 18each independently represents a hydrogen atom, an aliphatic hydrocarbon group having 1 to 10 carbon atoms (such as an alkyl group or an alkenyl group), an alicyclic hydrocarbon group having 3 to 10 carbon atoms (such as a cycloalkyl group or a cycloalkenyl group), or an aliphatic hydrocarbon group having 6 to 10 carbon atoms (such as a phenyl group). Also, i, j, k, p, and q each independently represent an integer of 1 to 8. However, R 17 is a hydrogen atom, R 18 is a group other than a hydrogen atom.

[0040] Examples of the monofunctional epoxy compound represented by the above formula (IV) include epoxyethane (ethylene oxide), epoxypropane, 1,2-epoxybutane, 2,3-epoxybutane, 3-methyl-1,2-epoxybutane, 1,2-epoxypentane, 3-methyl-1,2-epoxypentane, 1,2-epoxyhexane, 2,3-epoxyhexane, 3,4-epoxyhexane, 3-methyl-1,2-epoxyhexane, 3-methyl-1,2-epoxyheptane, 4-methyl-1,2-epoxyheptane, 1,2-epoxyoctane, 2,3-epoxyoctane, 1,2-epoxynonane, 2,3-epoxynonane, 1,2-epoxydecane, 1,2-epoxydodecane, epoxyethylbenzene, 1-phenyl-1,2-epoxypropane, 3-phenyl-1,2-epoxypropane, etc. Examples of the monofunctional epoxy compound represented by the above formula (V) include various alkyl glycidyl ethers, etc. Examples of the monofunctional epoxy compound represented by the above formula (VI) include various alkylene glycol monoglycidyl ethers. Examples of the monofunctional epoxy compound represented by the above formula (VII) include various alkenyl glycidyl ethers. Examples of the monofunctional epoxy compound represented by the above formula (VIII) include various epoxy alkanols such as glycidol. Examples of the monofunctional epoxy compound represented by the above formula (IX) include various epoxy cycloalkanes. Examples of the monofunctional epoxy compound represented by the above formula (X) include various epoxy cycloalkenes.

[0041] Among the monofunctional epoxy compounds, an epoxy compound having 2 to 8 carbon atoms is preferred. In particular, from the viewpoint of ease of handling of the compound and reactivity, the number of carbon atoms in the monofunctional epoxy compound is more preferably 2 to 6, and even more preferably 2 to 4. In addition, it is particularly preferred that the monofunctional epoxy compound is a compound represented by the above formula (IV) or formula (V). Specifically, from the viewpoint of reactivity with EVOH (A), processability of the resin composition and the resulting tube container, gas barrier property, etc., 1,2-epoxybutane, 2,3-epoxybutane, epoxypropane, epoxyethane, or glycidol is preferred, and among them, epoxypropane or glycidol is more preferred.

[0042] In the structural unit (III), R 8 , R 9 , R 10 and R 11 is preferably a hydrogen atom or an aliphatic hydrocarbon group having 1 to 5 carbon atoms, and such an aliphatic hydrocarbon group is preferably a methyl group, an ethyl group, an n-propyl group, an isopropyl group, an n-butyl group, an isobutyl group, a tert-butyl group, or an n-pentyl group.

[0043] The method for incorporating the structural unit (III) in EVOH (A) is not particularly limited, and examples thereof include the method described in JP-A-2014-034647.

[0044] The lower limit of the melting point of EVOH (A) is preferably 140°C, more preferably 150°C, and even more preferably 160°C. On the other hand, the upper limit of the melting point is preferably 220°C, more preferably 210°C, and even more preferably 200°C. When the melting point of EVOH (A) is within the above range, the melt moldability is improved, and neck-in and die build-up during melt molding tend to be further suppressed. The melting point of EVOH (A) can be a value measured by the method described in the Examples.

[0045] The EVOH (A) may be used alone or in combination of two or more kinds.

[0046] The content of EVOH (A) in the resin composition is preferably 70% by mass or more, more preferably 80% by mass or more, particularly preferably 90% by mass or more, and may be 95% by mass or more, 99% by mass or more, or 99.9% by mass or more, from the viewpoint of gas barrier properties, etc. The resin constituting the resin composition may be substantially composed of only EVOH (A). On the other hand, the content of EVOH (A) in the resin composition may be, for example, 99.9% by mass or less, or 99% by mass or less.

[0047] (Unsaturated aliphatic aldehyde (B)) The resin composition contains crotonaldehyde (B1), and further contains at least one selected from the group consisting of 2,4-hexadienal (B2) and 2,4,6-octatrienal (B3).

[0048] The lower limit of the content b1 of crotonaldehyde (B1) relative to EVOH (A) in the resin composition is preferably 0.01 ppm, more preferably 0.20 ppm, even more preferably 0.40 ppm, and even more preferably 0.70 ppm or 1.20 ppm. On the other hand, the upper limit of the content b1 is preferably 4.0 ppm, more preferably 3.5 ppm, even more preferably 2.7 ppm, and even more preferably 2.0 ppm or 1.5 ppm. When the content b1 is within the above range, it is easy to adjust the values ​​of b1 / (b2+b3), b1+b2+b3, and b2+2b3 described below to suitable ranges. In addition, when the content b1 is within the above range, coloring tends to be suppressed.

[0049] In one embodiment, the resin composition contains 2,4-hexadienal (B2) at a specific ratio relative to crotonaldehyde (B1), and thus tends to suppress die build-up while exhibiting excellent neck-in resistance. The lower limit of the content b2 of 2,4-hexadienal (B2) relative to EVOH (A) in the resin composition is preferably 0.005 ppm, more preferably 0.01 ppm, and even more preferably 0.02 ppm. On the other hand, the upper limit of the content b2 is preferably 0.65 ppm, more preferably 0.20 ppm, more preferably 0.10 ppm, even more preferably 0.08 ppm, and particularly preferably 0.06 ppm. When the content b2 is within the above range, it is easy to adjust the values ​​of b1 / (b2+b3), b1+b2+b3, and b2+2b3 described below to suitable ranges. In addition, when the content b2 is within the above range, coloring tends to be suppressed.

[0050] In one embodiment, the resin composition contains 2,4,6-octatrienal (B3) at a specific ratio relative to crotonaldehyde (B1), and thus tends to suppress die build-up while exhibiting excellent neck-in resistance. Compared with 2,4-hexadienal (B2), 2,4,6-octatrienal (B3) has a greater effect on die build-up relative to the amount added. Therefore, from the viewpoint of suppressing die build-up while improving neck-in resistance, the resin composition preferably contains 2,4-hexadienal (B2) rather than 2,4,6-octatrienal (B3). The upper limit of the content b3 of 2,4,6-octatrienal (B3) relative to EVOH (A) in the resin composition is preferably 0.325 ppm, more preferably 0.23 ppm, even more preferably 0.07 ppm, and particularly preferably 0.04 ppm. The lower limit of the content B3 may be 0 ppm or 0.005 ppm. When the content b3 is in the above range, the values ​​of b1 / (b2+b3), b1+b2+b3, and b2+2b3 described below can be easily adjusted to a suitable range. In addition, when the content b3 is in the above range, coloring tends to be suppressed.

[0051] In the resin composition, the ratio (b1 / (b2+b3)) of the sum of the content b2 (ppm) of 2,4-hexadienal (B2) and the content b3 (ppm) of 2,4,6-octatrienal (B3) to the content b1 (ppm) of crotonaldehyde (B1) is 2.0 or more and less than 150.0, so that the resin composition has excellent neck-in resistance. Such neck-in resistance is an effect that is not seen when any of the unsaturated aliphatic aldehydes (B) is used alone, and is an effect that is only achieved when b1 / (b2+b3) is in a specific range. The lower limit of b1 / (b2+b3) is preferably 4.0, more preferably 8.0. On the other hand, the upper limit of b1 / (b2+b3) is preferably 60.0, more preferably 25.0, and even more preferably 13.0. By setting b1 / (b2+b3) within the above range, neck-in can be more sufficiently suppressed, and the appearance and squeezability of the tube container are improved.

[0052] In the resin composition, the upper limit of the sum (b2+2b3) of the content b2 (ppm) of 2,4-hexadienal (B2) and twice the content b3 (ppm) of 2,4,6-octatrienal (B3) is 0.65 ppm or less, preferably 0.50 ppm, more preferably 0.30 ppm, and even more preferably 0.10 ppm. If b2+2b3 exceeds the upper limit, the occurrence of die build-up cannot be suppressed, and the appearance and squeezability of the tube container become insufficient. b2+2b3 may be 0.005 ppm or more, or 0.01 ppm or more.

[0053] In the resin composition, the upper limit of the total content (b1+b2+b3) of crotonaldehyde (B1), 2,4-hexadienal (B2) and 2,4,6-octatrienal (B3) relative to EVOH (A) is preferably 7.0 ppm, more preferably 4.0 ppm, even more preferably 3.5 ppm, even more preferably 3.0 ppm, even more preferably 1.5 ppm, and in some cases, particularly preferably 1.0 ppm. By making b1+b2+b3 equal to or less than the upper limit, coloration of the resin composition can be sufficiently suppressed. On the other hand, the lower limit of b1+b2+b3 is preferably 0.01 ppm, more preferably 0.10 ppm, and even more preferably 0.30 ppm or 0.50 ppm.

[0054] (Conjugated polyene compound (C)) The resin composition preferably further contains a conjugated polyene compound (C). The conjugated polyene compound (C) can suppress the deterioration of color tone due to the oxidative deterioration of the EVOH (A) during melt molding. Here, the conjugated polyene compound (C) is a compound having a structure in which carbon-carbon double bonds and carbon-carbon single bonds are alternately connected and the number of carbon-carbon double bonds is two or more, that is, a compound having a so-called conjugated double bond. However, 2,4-hexadienal (B2) and 2,4,6-octatrienal (B3) are not considered to be conjugated polyene compounds (C). The conjugated polyene compound (C) may be a conjugated diene having two conjugated double bonds, a conjugated triene having three conjugated double bonds, or a conjugated polyene having more than two conjugated double bonds. In addition, the structure of the conjugated double bond may have multiple sets in one molecule. For example, a compound having three conjugated triene structures in the same molecule, such as tung oil, is also included in the conjugated polyene compound (C). The upper limit of the number of conjugated double bonds in the conjugated polyene compound (C) is preferably 7. If the resin composition contains a conjugated polyene compound (C) having 8 or more conjugated double bonds, the possibility of coloring of the pellets and thus the molded product increases.

[0055] The conjugated polyene compound (C) may have, in addition to the conjugated double bond, other functional groups such as a carboxy group and a salt thereof, a hydroxyl group, an ester group, an ether group, an amino group, an imino group, an amide group, a cyano group, a diazo group, a nitro group, a sulfone group and a salt thereof, a sulfonyl group, a sulfoxide group, a sulfide group, a thiol group, a phosphate group and a salt thereof, a phenyl group, a halogen atom, a double bond, or a triple bond.

[0056] The lower limit of the carbon number of the conjugated polyene compound (C) is preferably 4. The upper limit of the carbon number of the conjugated polyene compound (C) is preferably 30, and more preferably 10.

[0057] Examples of the conjugated polyene compound (C) include isoprene, 2,3-dimethyl-1,3-butadiene, 2,3-diethyl-1,3-butadiene, 2-t-butyl-1,3-butadiene, 1,3-pentadiene, 2,3-dimethyl-1,3-pentadiene, 2,4-dimethyl-1,3-pentadiene, 3,4-dimethyl-1,3-pentadiene, and 3-ethyl-1,3-pentadiene. , 2-methyl-1,3-pentadiene, 3-methyl-1,3-pentadiene, 4-methyl-1,3-pentadiene, 1,3-hexadiene, 2,4-hexadiene, 2,5-dimethyl-2,4-hexadiene, 1,3-octadiene, 1,3-cyclopentadiene, 1,3-cyclohexadiene, 1-phenyl-1,3-butadiene, 1,4-diphenyl-1,3-butadiene conjugated diene compounds such as ene, 1-methoxy-1,3-butadiene, 2-methoxy-1,3-butadiene, 1-ethoxy-1,3-butadiene, 2-ethoxy-1,3-butadiene, 2-nitro-1,3-butadiene, chloroprene, 1-chloro-1,3-butadiene, 1-bromo-1,3-butadiene, 2-bromo-1,3-butadiene, ocimene, phellandrene, myrcene, farnesene, sorbic acid, sorbic acid esters, and sorbic acid salts; conjugated triene compounds such as 1,3,5-hexatriene, 2,4,6-octatriene-1-carboxylic acid, eleostearic acid, tung oil, cholecalciferol, fulvene, and tropone; cyclooctatetraene, 2,4,6,8-decatetraene-1-carboxylic acid, retinol, and retinoic acid.

[0058] As the conjugated polyene compound (C), sorbic acid, sorbic acid esters, sorbic acid salts, myrcene or a mixture of two or more of these is preferred, and sorbic acid, sorbic acid salts (sodium sorbate, potassium sorbate, etc.) or a mixture of these is more preferred. Sorbic acid, sorbic acid salts or a mixture of these are highly effective in inhibiting oxidative deterioration at high temperatures and are also widely used industrially as food additives, and are therefore preferred from the standpoints of hygiene and availability.

[0059] The molecular weight of the conjugated polyene compound (C) is usually 1,000 or less, preferably 500 or less, more preferably 300 or less. When the molecular weight of the conjugated polyene compound (C) is the above upper limit or less, the dispersion state of the conjugated polyene compound (C) in the resin composition becomes good, and the appearance after melt molding tends to be improved. The lower limit of the molecular weight of the conjugated polyene compound (C) is, for example, 54, and may be 60 or 80.

[0060] The lower limit of the content c of the conjugated polyene compound (C) relative to the EVOH (A) in the resin composition is preferably 1 ppm, more preferably 3 ppm. The content c of the conjugated polyene compound (C) relative to the EVOH (A) in the resin composition is preferably less than 300 ppm, more preferably 100 ppm or less, even more preferably 70 ppm or less, even more preferably 30 ppm or less, and in some cases, particularly preferably 20 ppm or less, 10 ppm or less. When the content c of the conjugated polyene compound (C) is within the above range, the deterioration of the color during melt molding tends to be more suppressed.

[0061] (Other optional ingredients) The resin composition may contain, as optional components other than EVOH (A), unsaturated aliphatic aldehyde (B), and conjugated polyene compound (C), boron compounds, carboxylic acids, phosphorus compounds, metal ions, antioxidants, ultraviolet absorbers, plasticizers, antistatic agents, lubricants, colorants, fillers, heat stabilizers, other resins other than EVOH (A), metal salts of higher aliphatic carboxylic acids, etc. The resin composition may contain two or more of these components. When the resin composition contains other optional components, the upper limit of the total content is preferably 1 mass%, and in some cases 0.5 mass% is preferable.

[0062] The boron compound suppresses gelation during melt molding and also suppresses torque fluctuations (viscosity changes during heating) of an extrusion molding machine or the like. Examples of the boron compound include boric acids such as orthoboric acid, metaboric acid, and tetraboric acid; boric acid esters such as triethyl borate and trimethyl borate; alkali metal salts or alkaline earth metal salts of the boric acids, borate salts such as borax; and boron hydrides. Among these, boric acids are preferred, and orthoboric acid (hereinafter also referred to as "boric acid") is more preferred. The lower limit of the content of the boron compound relative to EVOH (A) is preferably 100 ppm, more preferably 500 ppm. The upper limit of the content of the boron compound relative to EVOH (A) is preferably 5,000 ppm, more preferably 3,000 ppm, and even more preferably 1,000 ppm. By setting the content of the boron compound to the above lower limit or more, torque fluctuations of an extrusion molding machine or the like can be sufficiently suppressed. On the other hand, by setting the content of the boron compound to the above upper limit or less, gelation is less likely to occur during melt molding, and the appearance of the tube container is improved. Note that the content of the boron compound is the content of the boron compound converted into orthoboric acid.

[0063] The carboxylic acid prevents the coloring of the tube container and suppresses gelation during melt molding. Examples of the carboxylic acid include formic acid, acetic acid, propionic acid, butyric acid, lactic acid, and salts thereof. The carboxylic acid is preferably a carboxylic acid having 4 or less carbon atoms or a saturated carboxylic acid, and more preferably an acetic acid. The acetic acid includes acetic acid and an acetate salt. As the acetic acid, it is preferable to use acetic acid and an acetate salt in combination, and it is more preferable to use acetic acid and sodium acetate in combination. The lower limit of the content of the carboxylic acid in EVOH (A) is preferably 50 ppm, more preferably 100 ppm, and even more preferably 150 ppm. The upper limit of the content of the carboxylic acid in EVOH (A) is preferably 1,000 ppm, more preferably 500 ppm, and even more preferably 400 ppm. By setting the content of the carboxylic acid to the above lower limit or more, a sufficient coloring suppression effect can be obtained and the occurrence of yellowing can be sufficiently suppressed. On the other hand, by setting the content of carboxylic acids to the above upper limit or less, gelation is less likely to occur during melt molding, particularly during long-term melt molding, and the appearance of the tubular container becomes good.

[0064] The phosphorus compound suppresses the occurrence of defects such as streaks and fish eyes, and coloring, and improves long-run properties. Examples of the phosphorus compound include phosphates such as phosphoric acid and phosphorous acid. The phosphate may be in the form of primary phosphate, secondary phosphate, or tertiary phosphate. The cationic species of the phosphate is not particularly limited, but is preferably an alkali metal salt or an alkaline earth metal salt, and among these, sodium dihydrogen phosphate, potassium dihydrogen phosphate, disodium hydrogen phosphate, and dipotassium hydrogen phosphate are more preferred, and sodium dihydrogen phosphate and dipotassium hydrogen phosphate are even more preferred. The lower limit of the content of the phosphorus compound relative to EVOH (A) is preferably 1 ppm, more preferably 10 ppm, even more preferably 20 ppm, and particularly preferably 30 ppm. The upper limit of the content of the phosphorus compound relative to EVOH (A) is preferably 200 ppm, more preferably 150 ppm, and even more preferably 100 ppm. By setting the content of the phosphorus compound to be equal to or more than the above lower limit or equal to or less than the above upper limit, the thermal stability is improved, and the generation of gel-like particles, coloration, etc. during long-term melt molding is less likely to occur.

[0065] Examples of the metal ion include monovalent metal ions, divalent metal ions, and other transition metal ions, and these may be composed of one or more kinds. Among them, monovalent metal ions and divalent metal ions are preferred. As the monovalent metal ion, an alkali metal ion is preferred, for example, an ion of lithium, sodium, potassium, rubidium, and cesium, and from the viewpoint of industrial availability, an ion of sodium or potassium is preferred. In addition, examples of the alkali metal salt that gives the alkali metal ion include an aliphatic carboxylate, an aromatic carboxylate, a carbonate, a hydrochloride, a nitrate, a sulfate, a phosphate, and a metal complex. Among them, an aliphatic carboxylate and a phosphate are preferred from the viewpoint of availability, and specifically, sodium acetate, potassium acetate, sodium phosphate, and potassium phosphate are preferred. In some cases, it may be preferred to include a divalent metal ion as the metal ion. When the metal ion includes a divalent metal ion, for example, thermal deterioration of EVOH when trim is recovered and reused (recycled) may be suppressed, and the occurrence of gels and bumps in the obtained molded body may be suppressed. Examples of divalent metal ions include beryllium, magnesium, calcium, strontium, barium, and zinc ions, and magnesium, calcium, or zinc ions are preferred from the viewpoint of industrial availability. Examples of divalent metal salts that provide divalent metal ions include carboxylates, carbonates, hydrochlorides, nitrates, sulfates, phosphates, and metal complexes, and carboxylates are preferred. Examples of carboxylic acids that constitute carboxylates are carboxylic acids having 1 to 30 carbon atoms, and specific examples include acetic acid, propionic acid, butyric acid, stearic acid, lauric acid, montanic acid, behenic acid, octanoic acid, sebacic acid, ricinoleic acid, myristic acid, palmitic acid, and the like, and among these, acetic acid and stearic acid are preferred. The lower limit of the content of metal ions in EVOH (A) is preferably 1 ppm, more preferably 100 ppm, and even more preferably 150 ppm. On the other hand, the upper limit of the content of metal ions is preferably 1,000 ppm, more preferably 400 ppm, and even more preferably 350 ppm. When the content of metal ions in EVOH (A) is 1 ppm or more, the interlayer adhesion of the resulting tubular container tends to be good.On the other hand, if the metal ion content is 1,000 ppm or less, coloration resistance tends to be good.

[0066] Examples of the antioxidant include 2,5-di-t-butylhydroquinone, 2,6-di-t-butyl-p-cresol, 4,4'-thiobis(6-t-butylphenol), 2,2'-methylene-bis(4-methyl-6-t-butylphenol), octadecyl-3-(3',5'-di-t-butyl-4'-hydroxyphenyl)propionate, etc. Examples of the ultraviolet absorber include ethylene-2-cyano-3,3'-diphenylacrylate, 2-(2'-hydroxy-5'-methylphenyl)benzotriazole, 2-(2'-hydroxy-3'-t-butyl-5'-methylphenyl)-5-chlorobenzotriazole, 2-hydroxy-4-methoxybenzophenone, 2,2'-dihydroxy-4-methoxybenzophenone, 2-hydroxy-4-oxybenzophenone, etc.

[0067] Examples of the plasticizer include dimethyl phthalate, diethyl phthalate, dioctyl phthalate, wax, liquid paraffin, phosphate ester, etc. Examples of the antistatic agent include pentaerythritol monostearate, sorbitan monopalmitate, sulfated polyolefins, polyethylene oxide, polyethylene glycol (trade name: Carbowax), etc.

[0068] Examples of the lubricant include ethylene bisstearamide and butyl stearate. Examples of the colorant include carbon black, phthalocyanine, quinacridone, indoline, azo pigments, and red iron oxide. Examples of the filler include glass fiber, wollastonite, calcium silicate, talc, and montmorillonite. Examples of the heat stabilizer include hindered phenol compounds and hindered amine compounds.

[0069] Examples of the resin other than EVOH (A) include polyamide, polyolefin, etc. Examples of the metal salt of higher aliphatic carboxylic acid include sodium stearate, potassium stearate, calcium stearate, magnesium stearate, etc.

[0070] In the resin composition, the total content of EVOH (A) and unsaturated aliphatic aldehyde (B) (crotonaldehyde (B1), 2,4-hexadienal (B2), and 2,4,6-octatrienal (B3)) is preferably 90% by mass or more, more preferably 95% by mass or more, even more preferably 98% by mass or more, and particularly preferably 99% by mass or more. The resin composition may be substantially composed of EVOH (A) and unsaturated aliphatic aldehyde (B), and the resin composition may be composed of EVOH (A) and unsaturated aliphatic aldehyde (B). In this specification, "consisting essentially of" means that optional components can be contained within a range that does not affect the effects of the present invention, and "consisting only of" means that optional components other than impurities that are inevitably contained are excluded.

[0071] The lower limit of the melt flow rate (MFR) of the resin composition at 210°C under a load of 2,160 g is preferably 0.5 g / 10 min, more preferably 1 g / 10 min. Meanwhile, the upper limit of this MFR is preferably 30 g / 10 min, more preferably 20 g / 10 min. When the MFR of the resin composition is in the above range, melt moldability and the like can be improved. In addition, when the MFR of the resin composition is in the above range, the neck-in resistance tends to be better.

[0072] <Method for preparing resin composition> The method for producing the resin composition is not particularly limited as long as it is a method capable of blending the unsaturated aliphatic aldehyde (B) into the EVOH (A). (1) copolymerizing ethylene with a vinyl ester; and (2) A step of saponifying the copolymer obtained in the step (1) and a method for producing a resin composition comprising the steps of:

[0073] The method of including the unsaturated aliphatic aldehyde (B) in the resin composition is not particularly limited, and examples thereof include a method of adding the unsaturated aliphatic aldehyde (B) in the above step (1), a method of adding the unsaturated aliphatic aldehyde (B) in the above step (2), and a method of adding the unsaturated aliphatic aldehyde (B) to the EVOH (A) obtained by the above step (2). When adopting the method of adding the unsaturated aliphatic aldehyde (B) in the above step (1) or the method of adding the unsaturated aliphatic aldehyde (B) in the above step (2), in order to include a desired amount of the unsaturated aliphatic aldehyde (B) in the obtained resin composition, it is necessary to increase the amount of the unsaturated aliphatic aldehyde (B) to be added in consideration of the amount consumed in the polymerization reaction in the above step (1) and the saponification reaction in the above step (2). Therefore, when the unsaturated aliphatic aldehyde (B) is added in the polymerization reaction or saponification reaction step, it is preferable to add the amount of the unsaturated aliphatic aldehyde (B) consumed. On the other hand, the method of adding the unsaturated aliphatic aldehyde (B) to the EVOH (A) obtained in the above step (2) is excellent in operability since it can be added without considering consumption in the process.

[0074] Examples of the method for adding the unsaturated aliphatic aldehyde (B) to EVOH (A) include a method of blending the unsaturated aliphatic aldehyde (B) with EVOH (A) in advance and granulating the mixture into pellets, a method of impregnating the strands precipitated in a process of precipitating a paste after saponification of an ethylene-vinyl ester copolymer with the unsaturated aliphatic aldehyde (B), a method of cutting the precipitated strands and then impregnating the unsaturated aliphatic aldehyde (B), a method of adding the unsaturated aliphatic aldehyde (B) to a remelted chip of a dried resin composition, a method of melt-kneading a blend of the components EVOH (A) and the unsaturated aliphatic aldehyde (B), a method of feeding the unsaturated aliphatic aldehyde (B) into a melt of EVOH (A) midway through an extruder to incorporate the unsaturated aliphatic aldehyde (B), and a method of blending the unsaturated aliphatic aldehyde (B) at a high concentration with a part of EVOH (A) to prepare a master batch, which is granulated, dry-blended with EVOH (A), and melt-kneading the master batch.

[0075] Among these, from the viewpoint of being able to disperse a trace amount of unsaturated aliphatic aldehyde (B) in EVOH (A) with high uniformity, a method of blending the unsaturated aliphatic aldehyde (B) with EVOH (A) in advance and pelletizing the mixture is preferred. Specifically, the unsaturated aliphatic aldehyde (B) is added to a solution obtained by dissolving EVOH (A) in a good solvent such as a water / methanol mixed solvent, and the resulting mixed solution is extruded from a nozzle or the like into a poor solvent to precipitate and / or solidify, which is then washed and / or dried to obtain resin composition pellets in which the unsaturated aliphatic aldehyde (B) is mixed with EVOH (A) with high uniformity.

[0076] Examples of methods for incorporating other components other than the unsaturated aliphatic aldehyde (B) in EVOH (A) include a method of mixing the above pellets with the other components and melt-kneading them, a method of mixing the other components together with the unsaturated aliphatic aldehyde (B) when preparing the above pellets, a method of immersing the above pellets in a solution containing the other components, a method of dry-blending the above pellets with the other components, etc. For mixing the other components, a ribbon blender, a high-speed mixer co-kneader, a mixing roll, an extruder, an intensive mixer, etc. can be used.

[0077] The resin composition used in the manufacture of the laminate constituting the body of the tube container of the present invention is preferably in the form of pellets from the viewpoint of ease of handling. The shape of the pellets of the resin composition is not particularly limited, but may be cylindrical, prismatic, spherical, or approximately spherical (lenticular), and among them, from the viewpoint of the conveying stability, handling, productivity, etc. of the pellets, cylindrical, spherical, or approximately spherical (lenticular) is preferred. In the case of a cylindrical shape, the diameter is preferably 1 mm or more and 10 mm or less, more preferably 2 mm or more and 8 mm or less, and the height is preferably 1 mm or more and 10 mm or less, more preferably 2 mm or more and 8 mm or less, and even more preferably 3 mm or more and 5 mm or less. In the case of a spherical or approximately spherical (lenticular) shape, the length in the short direction is preferably 1 mm or more and 10 mm or less, more preferably 2 mm or more and 8 mm or less, and the length in the long direction is preferably 1 mm or more and 10 mm or less, and more preferably 2 mm or more and 8 mm or less.

[0078] (Layer(β)) The laminate may have an outermost layer (X), an innermost layer (Y) and a layer (β) made of a thermoplastic resin different from the layer (α).

[0079] Examples of the thermoplastic resin constituting the layer (β) include polyethylene (linear low-density polyethylene, low-density polyethylene, medium-density polyethylene, high-density polyethylene, etc.), ethylene-vinyl acetate copolymer, ethylene-propylene copolymer, polypropylene, copolymer of propylene and α-olefin having 4 to 20 carbon atoms, homopolymer or copolymer of olefin such as polybutene or polypentene, polystyrene, polyvinyl chloride, polyvinylidene chloride, acrylic resin, vinyl ester resin, polyurethane elastomer, polycarbonate, chlorinated polyethylene, chlorinated polypropylene, etc. Among them, polyethylene, ethylene-propylene copolymer, ethylene-vinyl acetate copolymer, polypropylene, and polystyrene are preferred.

[0080] The thermoplastic resin can be appropriately selected from commercially available products. The layer (β) may contain other optional components as long as they do not impair the effects of the present invention.

[0081] When the laminate includes a layer (β), the lower limit of the average thickness of the layer (β) is not particularly limited, but may be preferably 5% and more preferably 10% of the total average thickness, while the upper limit of the average thickness of the layer (β) is not particularly limited, but may be preferably 20% and more preferably 15% of the total average thickness.

[0082] (layer(γ)) The laminate may have a layer (γ) containing a carboxylic acid-modified polyolefin as a main component. The layer (γ) may be disposed, for example, between the layer (α) and the outermost layer (X) and between the layer (α) and the innermost layer (Y). The layer (γ) can function as an adhesive layer between the layer (α) and other layers such as the outermost layer (X) and the innermost layer (Y). The carboxylic acid-modified polyolefin refers to an olefin polymer having a carboxy group or an anhydride group thereof obtained by chemically bonding an ethylenically unsaturated carboxylic acid or an anhydride thereof to an olefin polymer by addition reaction, graft reaction, or the like.

[0083] Examples of the ethylenically unsaturated carboxylic acid and its anhydride include monocarboxylic acid, monocarboxylic acid ester, dicarboxylic acid, dicarboxylic acid monoester, dicarboxylic acid diester, dicarboxylic acid anhydride, etc. Specific examples include maleic acid, fumaric acid, itaconic acid, maleic anhydride, itaconic anhydride, maleic acid monomethyl ester, maleic acid monoethyl ester, maleic acid diethyl ester, fumaric acid monomethyl ester, etc. Among these, dicarboxylic acid anhydrides such as maleic anhydride and itaconic anhydride are preferred, and maleic anhydride is more preferred.

[0084] The olefin polymer serving as the base polymer is, for example, Polyolefins such as low-, medium- or high-density polyethylene, linear low-density polyethylene, polypropylene, polybutene, etc.;

[0085] Examples of the comonomer include copolymers of olefins and comonomers such as ethylene-vinyl acetate copolymers and ethylene-ethyl acrylate copolymers. The comonomers are not particularly limited as long as they are monomers that can be copolymerized with olefins, and examples thereof include vinyl esters and unsaturated carboxylate esters. As the olefin-based polymers, linear low-density polyethylene, ethylene-vinyl acetate copolymers having a vinyl acetate content of 5% by mass or more and 55% by mass or less, and ethylene-ethyl acrylate copolymers having an ethyl acrylate content of 8% by mass or more and 35% by mass or less are preferred, and linear low-density polyethylene and ethylene-vinyl acetate copolymers having a vinyl acetate content of 5% by mass or more and 55% by mass or less are more preferred.

[0086] The carboxylic acid-modified polyolefin is obtained by introducing the ethylenically unsaturated carboxylic acid or its anhydride into the olefin polymer by addition reaction or graft reaction in the presence of a solvent such as xylene and a catalyst such as peroxide. The lower limit of the amount of the carboxylic acid or its anhydride added to the olefin polymer or the graft amount (modification degree) is preferably 0.01% by mass, more preferably 0.02% by mass, based on the olefin polymer. On the other hand, the upper limit of the amount of the carboxylic acid or its anhydride added to the olefin polymer or the graft amount (modification degree) is preferably 15% by mass, more preferably 10% by mass, based on the olefin polymer.

[0087] The layer (γ) may contain optional components within the range that does not impair the effects of the present invention.

[0088] The lower limit of the average thickness of the layer (γ) is not particularly limited, but is preferably 0.3%, more preferably 0.6%, even more preferably 1.2%, and even more preferably 2.0% relative to the overall average thickness. The upper limit of the average thickness of the layer (γ) is preferably 12%, more preferably 9%, and even more preferably 6% relative to the overall average thickness. By setting the average thickness of the layer (γ) as an adhesive resin layer to the above lower limit or more, the adhesiveness can be increased. In addition, by setting the average thickness of the layer (γ) to the above upper limit or less, the manufacturing cost can be suppressed.

[0089] (layer(δ)) The layer (δ) is a layer containing EVOH, a thermoplastic resin, and a carboxylic acid-modified polyolefin. The layer (δ) is preferably formed using recycled materials from the layer (α), the outermost layer (X), the innermost layer (Y), the layer (β), and the layer (γ) in the manufacturing process of the tube container. Examples of the recycled materials include burrs and products that fail inspections that occur in the manufacturing process of the tube container. When the tube container further has the layer (δ) as such a recycled layer, the burrs and products that fail inspections can be reused, and the loss of resin used in the manufacturing of the tube container can be reduced.

[0090] Although the layer (δ) can be used in place of the layer (β) described above, it is generally preferable to use the layers (β) and (δ) in a laminated manner, since the mechanical strength of the layer (δ) is generally lower than that of the layer (β). When the tube container is squeezed, stress is concentrated in the container, and the compressive stress against the impact acts on the inner layer side of the container at the stress concentration part, which may cause breakage. Therefore, it is preferable to arrange the layer (δ), which is weaker in strength, on the outer layer side than the layer (α). In addition, when it is necessary to recycle a large amount of resin, such as when there is a lot of burrs, recovery layers can be arranged on both sides of the layer (α) as layers (δ).

[0091] The upper limit of the EVOH content in the layer (δ) is preferably 9.0% by mass. When the EVOH content in the layer (δ) is equal to or less than the upper limit, cracks are unlikely to occur at the interface with other layers, and the destruction of the entire tube container caused by the cracks can be suppressed. The lower limit of the EVOH content in the layer (δ) is, for example, 3.0% by mass.

[0092] When the laminate includes a layer (δ), the lower limit of the average thickness of the layer (δ) is not particularly limited, but is preferably 10%, more preferably 20%, and even more preferably 30% of the total average thickness. The upper limit of the average thickness of the layer (δ) is preferably 60%, more preferably 55%, and even more preferably 50% of the total average thickness.

[0093] The layer structure of the tube container (inner surface) (Y) / (γ) / (α) / (γ) / (X) (outer surface) is preferable from the viewpoint of squeezability. In addition, the layer structure when the recovery layer (δ) is included is, for example, (Inner surface) (Y) / (γ) / (α) / (γ) / (δ) / (X) (Outer surface), (Inner surface) (Y) / (δ) / (γ) / (α) / (γ) / (δ) / (X)(Outer surface), The adhesive layer may also be omitted. (Inner surface)(Y) / (α) / (X)(Outer surface) When a plurality of layers (α) to (δ) are used, the resins constituting each layer may be the same or different.

[0094] <Manufacturing method of tube containers> The method for producing a tube container of the present invention includes a step of molding, by blow molding or tube molding, a cylindrical laminate having an outermost layer (X) and an innermost layer (Y) both made of a polyolefin resin, and a layer (α) made of a resin composition between the outermost layer (X) and the innermost layer (Y).

[0095] One embodiment of the manufacturing method of the tube container of the present invention will be described with reference to Figures 1 to 5. For example, the tube container 1 can be formed by blow molding, using resin composition pellets forming the layer (α) 12 and polyolefin resins such as low-density polyethylene forming the outermost layer (X) 11 and the innermost layer (Y) at a temperature of 100°C to 400°C in a blow molding machine, using, for example, a two-kind three-layer parison of outermost layer (X) / layer (α) / innermost layer (Y), and cooling at an internal mold temperature of 10°C to 30°C for 10 seconds to 30 minutes, to form a tube container with an overall average thickness of 200 μm to 1000 μm.

[0096] An example of a method for manufacturing a tube container by the rotary blow molding method will be described with reference to Fig. 3. The rotary blow molding machine 100 in Fig. 3 includes a rotor 112, metal molds 120 provided at approximately equal intervals on the outer periphery of the rotor 112, and a parison forming section 110. A cavity 121 having a shape corresponding to the tube container 1 is formed in the metal mold 120.

[0097] In the manufacture of the tube container 1 using the rotary blow molding machine 100, the rotor 112 is rotated around the rotation axis 113 in the direction of the arrow A. The parison 111 is discharged from the parison forming section 110, and a desired amount of the parison 111 is allowed to flow down into the open mold 120 (reference symbol 120a). The rotation speed of the rotor 112 is set to a speed at which the take-up speed of the parison 111 is equal to or greater than the discharge speed of the parison 111. If the take-up speed of the parison 111 is equal to or greater than the discharge speed of the parison 111, the parison 111 is filled in the cavity 121 with a uniform thickness. Then, the thickness of the body 10 of the obtained tube container 1 becomes uniform, and it is possible to prevent the deterioration of strength and water resistance caused by partial thinning of the body 10, and the occurrence of poor appearance of the body 10. After a given amount of parison 111 is filled in cavity 121, mold 120 is closed (reference symbol 120b), and gas 122 is blown into parison 111 to cool it. After cooling, mold 120 is opened (reference symbol 120c), and work-in-progress 101 in which tube container 1 is connected with flash 102 is taken out. By removing flash 102 from work-in-progress 101, tube container 1 is obtained.

[0098] The obtained tube container has an open body on the opposite side to the top end, like the tube container (intermediate) 1 in Figure 4(a). After filling the contents from the open end, the tube container can be sealed by crushing and heat sealing the open end.

[0099] The method for producing the laminate used in the tube container is not particularly limited, and examples thereof include extrusion lamination, dry lamination, extrusion blow molding, coextrusion lamination, coextrusion molding, coextrusion tube molding, coextrusion pipe molding, coextrusion blow molding, coinjection molding, and solution coating. From the viewpoint of versatility, coextrusion molding and coinjection molding are preferred, and it is more preferred to form the laminate using a coextrusion molding device. This laminate can be formed to have a predetermined layer structure by, for example, charging the resin composition forming the layer (α), the resin forming the outermost layer (X), the resin forming the layer (γ), and the resin composition forming the innermost layer (Y) into separate extruders and coextruding them with these extruders.

[0100] Each layer is extruded by operating an extruder equipped with a single screw at a predetermined temperature. The temperature of the extruder forming the layer (α) is, for example, 170°C to 240°C. The temperature of the extruder forming the outermost layer (X) and the innermost layer (Y) is, for example, 160°C to 220°C. The temperature of the extruder forming the layer (γ) is, for example, 160°C to 220°C. The temperature of the extruder forming the layer (δ) is, for example, 200°C to 240°C.

[0101] An example of a manufacturing method for molding and manufacturing a body portion that is a cylindrical laminate using a co-extrusion molding machine equipped with a T-die will be described with reference to Fig. 5. The body portion is made of a single sheet (laminate). It generally has a rectangular shape. Then, as shown in Fig. 5, this rectangular sheet (laminate) is rolled up, and the outermost layer (X) at one end is overlaid with the innermost layer (Y) at the other end, and the cylindrical body portion 10 is heat-sealed linearly over the entire axial length of the cylindrical body portion 10 to form the cylindrical body portion 10.

[0102] 5 is a perspective view of the cylindrical body thus formed. As can be seen from Fig. 5, at the seal portion 30, the sheet (laminate) is laminated in two layers.

[0103] Next, as shown in FIG. 4(a), the mouth head 22 of one of the two open ends of the cylindrical body 10 is joined. The mouth head 22 generally has an extraction section 21 and a shoulder section 20, and this shoulder section 20 is usually inserted into the cylindrical body 10 and joined by heat sealing or bonding all around.

[0104] After filling the other of the two open ends of the cylindrical body 10 with the contents, the open end is crushed and heat sealed to seal the tube container 1. Figure 4(b) shows the tube container 2 sealed in this way, and the sealed portion is designated by reference numeral 30.

[0105] This tube container 2 can be used by pouring out the contents from the pouring part 21 by pressing the cylindrical body part 10.

[0106] Hereinafter, specific examples of the present invention will be described with reference to the accompanying drawings, in which: Fig. 1 is a cross-sectional view showing a specific example of a laminate for forming a body portion constituting a tube container of the present invention.

[0107] In this laminate 10A, both the outermost layer (X) 11 and the innermost layer (Y) 13 are made of polyolefin resin. Of these, polyethylene resin is preferably used. Between the outermost layer (X) 11 and the innermost layer (Y) 13, a layer (α) 12 made of a resin composition is disposed.

[0108] The laminate 10B is a laminate formed by laminating five layers, which are, from the outside, an outermost layer (X) 11 made of a polyolefin resin, a layer (γ) 14 mainly composed of a carboxylic acid-modified polyolefin, a layer (α) 12 made of a resin composition, a layer (γ) 14 mainly composed of a carboxylic acid-modified polyolefin, and an innermost layer (Y) 13 made of a polyolefin resin.

[0109] The laminate 10C is a laminate constituted by laminating six layers, which are, from the outside, an outermost layer (X) 11 made of a polyolefin resin, a white polyolefin resin film (layer (β)) 15, a layer (γ) 14 mainly made of carboxylic acid-modified polyolefin, a layer (α) 12 made of a resin composition, a layer (γ) 14 mainly made of carboxylic acid-modified polyolefin, and an innermost layer (Y) 13 made of a polyolefin resin.

[0110] The contents contained in the tube container of the present invention are not particularly limited, but suitable contents include food, sanitary products, cosmetics, and pharmaceuticals. EXAMPLES

[0111] The present invention will be described in detail below with reference to examples, but the present invention is not limited to these examples.

[0112] [Evaluation method] (1) Measurement of ethylene unit content, degree of saponification, and modification amount of epoxypropane (modification amount relative to total vinyl alcohol units) The crude dried EVOH obtained in the synthesis example was dried in a vacuum dryer at 120°C for 12 hours. The vacuum-dried EVOH was dissolved in deuterated dimethyl sulfoxide (DMSO-d6) containing tetramethylsilane (TMS) as an internal standard and trifluoroacetic acid (TFA) as an additive, and the solution was analyzed by a 500 MHz spectrometer. 1 Measurement was performed at 80°C using H-NMR ("GX-500" manufactured by JEOL Ltd.), and the ethylene unit content and degree of saponification were determined from the peak intensity ratio of ethylene units, vinyl alcohol units, and vinyl ester units. When measuring the EVOH (A9) pellets obtained in Synthesis Example 9, the measurement was performed without vacuum drying, and the modification amount relative to all vinyl alcohol units was also calculated at the same time from the peak intensity of the epoxypropane-modified vinyl alcohol units. In the EVOH (A9) obtained in Synthesis Example 9, the modification amount of epoxypropane relative to all vinyl alcohol units is equal to the content of the structural unit (x) relative to all vinyl alcohol units.

[0113] (2) Sodium ion content, phosphate content, and boric acid content 0.5 g of the dried resin composition pellets obtained in the Reference Example, Reference Comparative Example, Examples, and Comparative Examples was placed in a Teflon (registered trademark) pressure vessel, and 5 mL of concentrated nitric acid was added thereto and decomposed at room temperature for 30 minutes. After 30 minutes, the vessel was closed, and the mixture was decomposed by heating at 150°C for 10 minutes and then at 180°C for 5 minutes using a wet decomposition apparatus (Actac Co., Ltd., "MWS-2"), and then cooled to room temperature. This treatment liquid was transferred to a 50 mL measuring flask (TPX (registered trademark)) and made up to 10 mL with pure water. The metal content of this solution was analyzed using an ICP emission spectrometer (PerkinElmer, Inc., "OPTIMA4300DV"), and the contents of sodium ions (sodium element), phosphoric acid, and boric acid were measured. The phosphoric acid content was calculated as a phosphate root equivalent value, and the boric acid content was calculated as an orthoboric acid equivalent value. In addition, a calibration curve prepared using a commercially available standard solution was used for the quantitative determination.

[0114] (3) Acetic acid content 20 g of the dried resin composition pellets obtained in the Reference Example, Reference Comparative Example, Examples, and Comparative Examples were added to 100 mL of ion-exchanged water and extracted by heating at 95° C. for 6 hours. The extract was neutralized and titrated with 1 / 50 N NaOH using phenolphthalein as an indicator to quantify the acetic acid content.

[0115] (4) Melt flow rate (MFR) The dried resin composition pellets obtained in the Reference Examples and Reference Comparative Examples were filled into a cylinder of Melt Indexer L244 (manufactured by Takara Kogyo Co., Ltd.) with an inner diameter of 9.55 mm and a length of 162 mm, and melted at 210°C. Then, a load was evenly applied to the molten resin composition using a plunger with a mass of 2,160 g and a diameter of 9.48 mm. The amount of resin composition extruded per unit time (g / 10 min) from an orifice with a diameter of 2.1 mm provided in the center of the cylinder was measured, and this was taken as the MFR.

[0116] (5) Determination of crotonaldehyde, 2,4-hexadienal and 2,4,6-octatrienal 0.50 g of the dried resin composition pellets obtained in the reference example, reference comparative example, examples and comparative examples were frozen and crushed to obtain a sample, which was weighed out to 50.0 mg in a glass tube for a thermal desorption gas chromatograph mass spectrometer to prepare a sample tube. Using the thermal desorption gas chromatograph mass spectrometer described below, the sample was heated under the following conditions to adsorb the entire amount of volatile gas from the sample once into the adsorption tube, and the gas re-emitted from the adsorption tube was separated in a column to detect the peaks of each component. A calibration curve was created from the peak areas of the standard samples of crotonaldehyde, 2,4-hexadienal and 2,4,6-octatrienal, and each was quantified by the absolute calibration curve method. When measuring the standard sample, the standard sample was impregnated into an adsorption tube (manufactured by Tenax (registered trademark) / Carboxen (registered trademark)), and the adsorption tube impregnated with the standard sample was used instead of the sample tube. The temperature at the time of release after sample adsorption was changed from the sample tube temperature of 170°C to the adsorption tube temperature of 260°C, but the measurement was performed in the same manner as in the measurement of the sample tube. (Heating desorption section) Device: TurboMatrix-ATD (PerkinElmer Japan) Temperature when adsorbing the sample to the adsorption tube: 170℃ (sample tube), -30℃ (adsorption tube), 250℃ (valve), 260℃ (transfer line) Adsorption time in the adsorption tube: 10 minutes Temperature at the time of release after sample adsorption: 170°C (sample tube), 260°C (adsorption tube), 250°C (valve), 260°C (transfer line) Adsorption tube discharge time: 35 minutes Carrier gas: Helium Carrier gas flow rate to column: 1.0 ml / min Pressure: 120kPa (Gas chromatograph mass spectrometry section) Equipment: 7890B GC System, 7977B MSD (Agilent Technologies) Column: DB-WAX UI (length: 30 m, inner diameter: 0.25 mm, film thickness: 0.50 μm) Column oven temperature: 40°C for 5 minutes, then heat up to 240°C at a rate of 10°C / min and hold for 10 minutes (total measurement temperature: 35 minutes) Transfer line (connection) temperature: 240℃ Ionization conditions: EI+ Detected ion mass range: m / z=29-600 Detection method: SCAN (Standard sample) Crotonaldehyde: Aldrich 2,4-Hexadienal: Aldrich 2,4,6-Octatrienal: Produced by NARD Laboratories

[0117] (6) Determination of sorbic acid and myrcene The dried resin composition pellets obtained in the Reference Example, Reference Comparative Example, Examples and Comparative Examples were freeze-pulverized, and 22 g of the pulverized material was loaded into a Soxhlet extractor and extracted with 100 mL of chloroform for 16 hours. The amounts of sorbic acid and myrcene in the obtained chloroform extract were quantitatively analyzed by high performance liquid chromatography to quantify the contents of sorbic acid and myrcene in the resin composition. For the quantification, a calibration curve prepared using sorbic acid and myrcene standards was used.

[0118] (7) Die build-up evaluation The dried resin composition pellets obtained in the Reference Example, Reference Comparative Example, Examples, and Comparative Examples were extruded from an extruder under the following conditions, and after 60 minutes, the die build-up (dye build-up) around the die was visually observed and evaluated according to the following criteria. In the cases of A to D, it was determined that the die build-up was suppressed. (Extruder conditions) Equipment: 20mmφ single screw extruder (D2020, manufactured by Toyo Seiki Seisakusho) L / D:20 Screw: Full flight Screen mesh: 50 mesh / 100 mesh / 50 mesh Die: φ1mm, 1 hole ·Setting temperature: C1 / C2 / C3 / D=180℃ / 220℃ / 220℃ / 220℃ ·Discharge amount: 1.44kg / h Rotational speed: 100 rpm (Evaluation: Criteria) A (Good): No eye gunk B (fairly good): There is a very small amount of eye mucus. C (Acceptable): A small amount of eye discharge is present D (slightly poor): There is obvious eye discharge E (bad): Large particles of resin are attached around the entire circumference of the die hole.

[0119] (8) Hue evaluation The yellow index (YI) value of the dried resin composition pellets obtained in the Reference Example, Reference Comparative Example, Examples, and Comparative Examples was measured and calculated using a LAB Scan XE manufactured by Hunter Co., Ltd. in accordance with JIS K7373: 2006. It was judged that the smaller the value, the more suppressed the yellowing and the better the hue.

[0120] (9) Evaluation of neck-in resistance during film formation Using the dried resin composition pellets obtained in the Reference Example, Reference Comparative Example, Examples, and Comparative Examples, a resin composition was extruded from a single screw extruder under the following conditions, and the width of the molten resin (melt curtain) discharged from the T-die 10 minutes after the dried resin composition pellets were charged was measured at a position 100 mm from the lip (the discharge port of the T-die). The width of the molten resin was evaluated according to the following criteria. In the cases of A to C, it was determined that neck-in was suppressed. (Extruder conditions) Extruder: L / D=26, 40mmφ single screw extruder Screw: Full flight Screw speed: 50 rpm Screen mesh: 50 mesh / 100 mesh / 50 mesh Die shape: T-type, lip width 550mm, lip spacing 0.7mm ·Setting temperature: C1 / C2 / C3 / D=170℃ / 240℃ / 260℃ / 260℃ (Evaluation: Criteria) A (Good): 85% or more of lip width B (Fair): More than 82.5% and less than 85% of the lip width C (Slightly poor): More than 80% and less than 82.5% of the lip width D (Poor): Less than 80% of the lip width

[0121] (10) Melting point measurement The crude dried product of EVOH obtained in the synthesis example was dried at 120 °C for 12 hours in a vacuum dryer. For the vacuum-dried EVOH, a differential scanning calorimeter "Q2000" manufactured by TA Instruments was used. The temperature was raised from 30 °C to 250 °C at a rate of 10 °C / min, cooled at 50 °C / min, and then the melting point was determined from the peak temperature measured by the second heating. When measuring the EVOH pellets obtained in Synthesis Example 9, the measurement was carried out without vacuum drying.

[0122] (11) Measurement of oxygen transmission rate (OTR) at the center of the film <Single-layer film preparation conditions> For the dried resin composition pellets obtained in the examples and comparative examples, films were formed under the following conditions to obtain single-layer films with a thickness of 20 μm. (Extruder conditions) · L / D: 26, single-screw extruder with a diameter of 40 mm · Screw: Full flight · Screw rotation speed: 30 rpm · Screen mesh: 50 mesh / 100 mesh / 50 mesh · Die shape: T-shaped, lip width 550 mm, lip gap 0.7 mm · Set temperature: C1 / C2 / C3 / D = 170 °C / 230 °C / 230 °C / 230 °C · Take-up roll temperature: 80 °C · Take-up roll speed: 10 - 11 m / min <OTR (Oxygen transmission rate) measurement>

[0123] From the obtained monolayer film having a thickness of 20 μm, a circular sample having a diameter of 90 mm was cut out centered in the center in the width direction, and after conditioning under conditions of 20°C and 65% RH, the oxygen permeability was measured at 20°C and 65% RH using an oxygen permeability measuring device (Modern Control's "OX-Tran2 / 20") in accordance with ISO14663-2 annex C.

[0124] (12) Preparation of the laminate A laminate was produced using the dried resin composition pellets obtained in the examples and comparative examples. The dried resin composition pellets were used as the material for the resin composition layers, and low-density polyethylene (LDPE) "Dowlex 209" (manufactured by The Dow Chemical Company, density 0.926 g / cm3) was used as the material for the outermost layer (X) and the innermost layer (Y). 3 ), and an acid-modified polypropylene "Admer (trademark) QF500" (Ad1) as an adhesive layer, a 3-kind 5-layer laminate ((inside) LDPE / Ad1 / resin composition layer / Ad1 / LDPE (outside) = 50 μm / 8 μm / 18 μm / 8 μm / 240 μm) was obtained under the following conditions. The film-forming equipment had a temperature-controllable take-up roll after the extruder with a film-forming die, and the obtained laminate was wound up by a winding machine. (Film forming conditions) EVOH extruder: Single screw extruder (lab machine ME type CO-EXT, manufactured by Toyo Seiki Seisakusho Co., Ltd.) Caliber 20mmφ, L / D=20, Screw full flight type Feeding section / compression section / metering section / die=175 / 210 / 220 / 230℃ LDPE extruder: Single screw extruder (GT-32-A, manufactured by Plastics Engineering Research Institute Co., Ltd.) Caliber 32mmφ, L / D=28, Screw full flight type Feeding section / compression section / metering section / die=170 / 200 / 210 / 230℃ Extruder for Ad1: Single screw extruder (SZW20GT-20MG-STD, manufactured by Technovel Co., Ltd.) Caliber 20mmφ, L / D=20, Screw full flight type Feeding section / compression section / metering section / die=150 / 200 / 230 / 230℃ Die: 300mm wide coat hanger die (manufactured by Plastics Engineering Research Institute Co., Ltd.) Take-up roll temperature: 80℃

[0125] (13) OTR Width Uniformity For the laminate produced in (12), the film was cut into a circle with a diameter of 90 mm, centered at a position 70 mm from the end of the film, and the OTR was measured under the same conditions as in (11). The difference from the OTR of the film at the center was taken, and the magnitude of the difference was evaluated on a three-level scale of A to C. Note that when the OTR of the laminate in this evaluation is highly uniform in the width direction, it can be determined that the OTR uniformity of the tube container obtained using the resin composition used in the evaluation is also high. Those rated C were determined to have low uniformity of the OTR in the width direction. (Evaluation: Criteria) A: The difference is less than 10% B: Difference is between 10% and 15% C: Difference is 15% or more

[0126] (14) Squeeze evaluation The obtained laminate was cut into a size of 10 cm x 10 cm to prepare a flat sheet, which was folded vertically and horizontally by hand toward the inside of the laminate, and then opened three times (squeezed), after which the OTR was measured. Note that if the degree of decrease in gas barrier properties after squeezing the laminate is small, it can be determined that the squeezability of the tube container obtained using such laminate is also good. (Evaluation: Criteria) A: Less than 5% difference from before squeeze B: Difference from before squeeze is 5% to 10% C: Difference from before squeeze is 10% to 15% D: The difference from before the squeeze is 15% or more (15) Appearance evaluation The appearance of the obtained laminate was evaluated by visual inspection. If the appearance of the laminate was good, it was naturally judged that the appearance of the tube container obtained using the laminate was also good. Those rated D were judged to have poor appearance characteristics. A: Uniform and no unevenness was observed B: Slight streaky unevenness was observed C: Some streaky unevenness was observed D: Severe unevenness was observed

[0127] <Synthesis Example 1> A 200L pressurized reactor equipped with a jacket, a stirrer, a nitrogen inlet, an ethylene inlet, and an initiator addition inlet was charged with 75.0 kg of vinyl acetate (hereinafter sometimes referred to as VAc) and 7.2 kg of methanol (hereinafter sometimes referred to as MeOH), and nitrogen bubbling was performed for 30 minutes to replace the atmosphere in the reactor with nitrogen. Next, the temperature in the reactor was adjusted to 65°C, and ethylene was introduced so that the reactor pressure (ethylene pressure) was 4.13 MPa, and 9.4 g of 2,2'-azobis(2,4-dimethylvaleronitrile) ("V-65" manufactured by Fujifilm Wako Pure Chemical Industries, Ltd.) was added as a polymerization initiator to start polymerization. During polymerization, the ethylene pressure was maintained at 4.13 MPa and the polymerization temperature at 65°C. After 4 hours, when the conversion rate of VAc (polymerization rate based on VAc) reached 49.7%, the reactor was cooled, and a solution in which 0.2 g of copper acetate was dissolved in 20 kg of methanol was added to the vessel to stop the polymerization. After the reaction vessel was opened to remove ethylene, nitrogen gas was bubbled through to remove ethylene completely. The polymerization liquid was then removed from the vessel and diluted with 20 L of MeOH. This liquid was fed from the top of a tower vessel, and MeOH vapor was fed from the bottom of the vessel to remove the unreacted monomers remaining in the polymerization liquid together with the MeOH vapor, to obtain a MeOH solution of ethylene-vinyl acetate copolymer (hereinafter sometimes referred to as EVAc).

[0128] Next, 150 kg of a 20% by mass MeOH solution of EVAc was charged into a 300 L reaction vessel equipped with a jacket, a stirrer, a nitrogen inlet, a reflux condenser, and a solution addition port. The solution was heated to 60° C. while blowing nitrogen gas into it, and a MeOH solution with a 2N concentration of sodium hydroxide was added at a rate of 450 mL / min for 2 hours. After the addition of the sodium hydroxide MeOH solution was completed, the temperature in the system was kept at 60° C., and the saponification reaction was allowed to proceed for 2 hours while stirring and discharging MeOH and methyl acetate produced by the saponification reaction out of the reaction vessel. Then, 8.7 kg of acetic acid was added to stop the saponification reaction.

[0129] After that, 120L of ion-exchanged water was added while heating and stirring at 80℃, MeOH was discharged from the reaction tank, and EVOH was precipitated. The precipitated EVOH was collected by decantation and crushed in a crusher. The obtained EVOH powder was put into a 1g / L acetic acid aqueous solution (bath ratio 20: 20L of aqueous solution per 1kg of powder) and washed with stirring for 2 hours. This was deliquified, and then put into a 1g / L acetic acid aqueous solution (bath ratio 20) and washed with stirring for 2 hours. The deliquified product was put into ion-exchanged water (bath ratio 20), washed with stirring for 2 hours, and then deliquified. This operation was repeated three times for purification. The electrical conductivity of the washing solution was 3μS / cm (measured with "CM-30ET" by Toa Denpa Kogyo Co., Ltd.). The resulting purified product was then immersed in 250 L of an aqueous solution containing 0.5 g / L of acetic acid and 0.1 g / L of sodium acetate with stirring for 4 hours, then the liquid was removed and the product was dried at 60°C for 16 hours to obtain 16.1 kg of crude dried EVOH.

[0130] The above-mentioned synthesis of EVOH was repeated to obtain 15.9 kg of crude EVOH, and a total of 32.0 kg of crude EVOH (A1) was obtained. The ethylene unit content, saponification degree, and melting point of the crude EVOH (A1) were measured according to the methods described in the above evaluation methods (1) and (10). The results are shown in Table 2.

[0131] <Synthesis Examples 2 to 8> The size of the pressurized reaction vessel, the amount of VAc and MeOH charged, the ethylene pressure, the amount of polymerization initiator added, the temperature inside the reaction vessel (temperature during polymerization), the reaction time, the conversion rate of VAc, the amount of EVAc MeOH solution charged in the saponification step, and the addition rate of sodium hydroxide MeOH solution were set as shown in Table 1, and the crude dried products of EVOH (A2) to EVOH (A8) were obtained in the same manner as in Synthesis Example 1, except that the synthesis was performed only once. The ethylene unit content, saponification degree, and melting point of the crude dried products of EVOH (A2) to EVOH (A8) were measured according to the methods described in the above evaluation methods (1) and (10). The results are shown in Table 2.

[0132] [Table 1]

[0133] [Table 2]

[0134] <Reference example 1> In a 60 L stirring tank equipped with a jacket, a stirrer and a reflux condenser, 2 kg of the crude dried EVOH (A1) obtained in Synthesis Example 1, 0.8 kg of water and 2.2 kg of MeOH were charged and stirred at 60°C for 5 hours to completely dissolve. To the obtained solution, sorbic acid, crotonaldehyde, 2,4-hexadienal and 2,4,6-octatrienal were added. This solution was extruded through a 4 mm diameter gold plate into a mixture of water / MeOH = 90 / 10 cooled to -5°C to precipitate in the form of strands, and the strands were cut into pellets with a strand cutter to obtain hydrous pellets of EVOH. The moisture content of the obtained hydrous pellets of EVOH was measured with a Mettler halogen moisture meter "HR73" and found to be 52% by mass.

[0135] The obtained EVOH hydrous pellets were placed in a 1g / L aqueous acetic acid solution (bath ratio 20) and washed with stirring for 2 hours. The pellets were deliquinated and then placed in a 1g / L aqueous acetic acid solution (bath ratio 20) and washed with stirring for 2 hours. After deliquification, the aqueous acetic acid solution was renewed and the same procedure was carried out. The pellets were washed with the aqueous acetic acid solution, deliquinated, placed in ion-exchanged water (bath ratio 20), washed with stirring for 2 hours, and then deliquinated three times. The procedure was repeated until the electrical conductivity of the washing solution was 3μS / cm or less (measured with Toa Denpa Kogyo Co., Ltd.'s "CM-30ET"), and EVOH hydrous pellets from which the catalyst residue from the saponification reaction had been removed were obtained.

[0136] The obtained hydrous pellets were put into an aqueous solution (bath ratio 20) with a sodium acetate concentration of 0.510 g / L, an acetic acid concentration of 0.8 g / L, and a phosphoric acid concentration of 0.04 g / L, and immersed for 4 hours while stirring periodically for chemical treatment. The pellets were dehydrated and dried at 80°C for 3 hours and at 105°C for 16 hours under a nitrogen stream with an oxygen concentration of 1% by volume or less to obtain cylindrical (average diameter 2.8 mm, average height 3.2 mm) dried resin composition pellets containing EVOH (A1), acetic acid, phosphoric acid, sodium ions (sodium salts), crotonaldehyde, 2,4-hexadienal, 2,4,6-octatrienal, and sorbic acid. The obtained dried resin composition pellets were evaluated according to the methods described in the above evaluation methods (2) to (9). The sodium ion content in the dried resin composition pellets was 100 ppm, the phosphoric acid content was 40 ppm in terms of phosphate radical, and the acetic acid content was 200 ppm. The contents of each component other than EVOH are based on the EVOH content. Other evaluation results are shown in Table 3. The amount of each component added was adjusted so that the contents of each component, crotonaldehyde, 2,4-hexadienal, 2,4,6-octatrienal, and sorbic acid, were as shown in Table 3.

[0137] <Reference Examples 2~61, Reference Comparative Examples 1~4, 6~24> Dry resin composition pellets were prepared and evaluated in the same manner as in Reference Example 1, except that the type of EVOH (A), the type and content of the unsaturated aliphatic aldehyde (B), the type and content of the conjugated polyene compound (C), and the content of boric acid were adjusted to be as shown in Tables 3 to 10. When the boric acid was contained at 800 ppm, an aqueous solution containing sodium acetate and the like (bath ratio 20) was used so that the boric acid concentration was 0.25 g / L, and when the boric acid was contained at 1800 ppm, an aqueous solution containing sodium acetate and the like (bath ratio 20) was used so that the boric acid concentration was 0.57 g / L. The sodium ion content of the EVOH in each dry resin composition pellet was 100 ppm, the phosphoric acid content was 40 ppm in terms of phosphate radical, and the acetic acid content was 200 ppm. Other evaluation results are shown in Tables 3 to 10. The contents of each component other than EVOH are all based on the content of EVOH.

[0138] <Reference Comparative Example 5> Crotonaldehyde, 2,4-hexadienal and 2,4,6-octatrienal were not added, and the hydrous pellets of EVOH from which the catalyst residues during the saponification reaction had been removed were placed in methanol (bath ratio 10), stirred and washed for 2 hours, and deliquored twice. The pellets obtained were placed in ion-exchanged water (bath ratio 20), stirred and washed for 2 hours, and deliquored three times. The dried resin composition pellets were prepared and evaluated in the same manner as in Reference Example 1. The sodium ion content in the dried resin composition pellets was 100 ppm, the phosphoric acid content was 40 ppm in terms of phosphoric acid radical, and the acetic acid content was 200 ppm. The contents of each component other than EVOH are all based on the content of EVOH. Other evaluation results are shown in Table 3. The contents of each component of crotonaldehyde, 2,4-hexadienal, 2,4,6-octatrienal and sorbic acid were below the detection limit.

[0139] [Table 3]

[0140] [Table 4]

[0141] [Table 5]

[0142] [Table 6]

[0143] [Table 7]

[0144] [Table 8]

[0145] [Table 9]

[0146] [Table 10]

[0147] From the Reference Examples and Reference Comparative Examples, it can be seen that when b1 / (b2+b3) is 2.0 or more and less than 150.0, the neck-in resistance is good, the smaller b1+b2+b3 is, the lower the YI is, the smaller the content c of the conjugated polyene compound (C) is, the lower the YI is, and the smaller the b2+b3 is, the lower the die build-up is.

[0148] A more detailed consideration based on Table 3 is as follows. In Reference Comparative Example 5, which does not contain an unsaturated aliphatic aldehyde (B), and Reference Comparative Examples 1 to 3 and 6 to 9, which contain each type of unsaturated aliphatic aldehyde (B) alone, neck-in is not suppressed. Furthermore, in Reference Comparative Example 10, in which the value of b1 / (b2+b3) is less than 2.0, neck-in is not suppressed. On the other hand, as can be seen from the reference examples, when the value of b1 / (b2+b3) is in the range of 2.0 or more and less than 150.0, neck-in is suppressed, and particularly when the value of b1 / (b2+b3) is around 10 (for example, 8.0 or more and 13.0 or less), as in Reference Examples 4, 5, 13, 14, 21 and 24, neck-in is most suppressed. In addition, in Comparative Example 4, where b2+2b3 exceeds 0.65 ppm, die build-up is not suppressed, whereas in the Reference Examples, when b2+2b3 is 0.65 ppm or less, die build-up is suppressed, and particularly when b2+2b3 is 0.10 ppm or less, die build-up is suppressed. In addition, as can be seen from Comparative Example 4, Reference Examples 1 to 7, 12 to 26, etc., it can be seen that the lower the total content of crotonaldehyde (B1), 2,4-hexadienal (B2), and 2,4,6-octatrienal (B3), the better the hue. Furthermore, it can be seen from Reference Examples 6 and 9 to 11 that the hue is better when the content of the conjugated polyene compound is smaller.

[0149] <Examples 1 to 7, Comparative Examples 1 and 2> The dried resin composition pellets obtained in Reference Examples 5, 28, 38, 43, 48, 2, and 7, and Reference Comparative Examples 4 and 3 were evaluated according to the methods described in the above evaluation methods (12) to (15). The evaluation results are shown in Table 11. Table 11 also lists the results of the evaluation of each of these dried resin composition pellets according to the above evaluation methods (5) to (10).

[0150] [Table 11] [Explanation of symbols]

[0151] 1 Tube container (intermediate) 2 Tube container (finished product) 10. Body (laminated body) 10A laminate 10B Laminate 10C Laminate 11 layers (X) 12 layers (α) 13 layers (Y) 14 layers (γ) 15 layers (β) 20 Shoulder 21 Pour section 22 Oral part 30 Heat seal section 100 Rotary Blow Molding Machine 101 Work in progress 102 Bali 110 Parison forming section 111 Parison 112 Rotating Body 113 Rotational Axis 120 Mold 121 Cavity 122 Gas

Claims

1. A tube container comprising a body portion formed of a cylindrical laminate, the inside of which serves as a storage portion for storing contents, and a pouring portion provided at one end of the body portion, the laminate has an outermost layer (X) and an innermost layer (Y) each made of a polyolefin resin, and has a layer (α) made of a resin composition between the outermost layer (X) and the innermost layer (Y); The resin composition includes an ethylene-vinyl alcohol copolymer (A) having an ethylene unit content of 20 mol% or more and 60 mol% or less and crotonaldehyde (B1), and further includes at least one selected from the group consisting of 2,4-hexadienal (B2) and 2,4,6-octatrienal (B3); The resin composition of the tube container satisfies the following formulas (1) and (2): 2.0≦b 1 / (b 2 +b 3 )<150.0 ・・・(1) b 2 +2b 3 ≦0.65 ・・・(2) In the above formulas (1) and (2), b 1 is the content (ppm) of crotonaldehyde (B1) relative to the ethylene-vinyl alcohol copolymer (A), and b 2 is the content (ppm) of 2,4-hexadienal (B2) relative to the ethylene-vinyl alcohol copolymer (A), and b 3 is the content (ppm) of 2,4,6-octatrienal (B3) relative to the ethylene-vinyl alcohol copolymer (A).

2. In the above resin composition, the total content of crotonaldehyde (B1), 2,4-hexadienal (B2) and 2,4,6-octatrienal (B3) relative to the ethylene-vinyl alcohol copolymer (A) (b 1 +b 2 +b 3 2. The tube container according to claim 1, wherein the content of fluorine-containing gas is 0.01 ppm or more and 7.0 ppm or less.

3. In the above resin composition, the content b of crotonaldehyde (B1) 1 The tube container according to claim 1 or 2, wherein the content of fluorine is 0.01 ppm or more and 4.0 ppm or less.

4. In the above resin composition, the content b of 2,4-hexadienal (B2) 2 The tube container according to claim 1 or 2, wherein the content of fluorine in the tube is 0.005 ppm or more and 0.65 ppm or less.

5. In the above resin composition, the content b of 2,4,6-octatrienal (B3) 3 The tube container according to claim 1 or 2, wherein the content of fluorine in the tube is 0.325 ppm or less.

6. 3. The tube container according to claim 1, wherein the resin composition further comprises a conjugated polyene compound (C), and the content c of the conjugated polyene compound (C) relative to the ethylene-vinyl alcohol copolymer (A) in the resin composition is 1 ppm or more and less than 300 ppm.

7. 7. The tube container according to claim 6, wherein the conjugated polyene compound (C) is sorbic acid.

8. 3. The tube container according to claim 1 or 2, wherein the laminate has a layer (γ) containing a carboxylic acid-modified polyolefin as a main component, and the layer (γ) is disposed between the layer (α) and the outermost layer (X) and between the layer (α) and the innermost layer (Y).

9. 3. The tube container according to claim 1, wherein the mass ratio of the polyolefin resin is 90 mass % or more.

10. A mouth part is provided at one opening of the body part, the mouth portion having the extraction portion and a shoulder portion, The laminate constituting the top portion is a laminate having a layer (α2) made of a resin composition, The resin composition includes an ethylene-vinyl alcohol copolymer (A) having an ethylene unit content of 20 mol% or more and 60 mol% or less and crotonaldehyde (B1), and further includes at least one selected from the group consisting of 2,4-hexadienal (B2) and 2,4,6-octatrienal (B3); The tube container according to claim 1 , wherein the resin composition satisfies the following formulas (1) and (2). 2.0≦b 1 / (b 2 +b 3 )<150.0 ・・・(1) b 2 +2b 3 ≦0.65 ・・・(2) In the above formulas (1) and (2), b 1 is the content (ppm) of crotonaldehyde (B1) relative to the ethylene-vinyl alcohol copolymer (A), and b 2 is the content (ppm) of 2,4-hexadienal (B2) relative to the ethylene-vinyl alcohol copolymer (A), and b 3 is the content (ppm) of 2,4,6-octatrienal (B3) relative to the ethylene-vinyl alcohol copolymer (A).

11. 11. The tube container according to claim 10, wherein the cylindrical laminate is formed by overlapping an outermost layer (X) and an innermost layer (Y) at both ends of the laminate and heat sealing the opposing surfaces of the laminate.

12. 3. The tube container according to claim 1 or 2, which is a container for filling food, daily hygiene products, cosmetics or medicines.

13. A method for producing the tube container according to claim 1, comprising the steps of: A method for producing a tube container, comprising a step of forming, by blow molding, a cylindrical laminate having an outermost layer (X) and an innermost layer (Y) both made of a polyolefin resin, and a layer (α) made of a resin composition between the outermost layer (X) and the innermost layer (Y).

14. A method for producing the tube container according to claim 1 or claim 10, comprising the steps of: a step of forming a body portion of a tubular laminate by tube molding, the body portion having an outermost layer (X) and an innermost layer (Y) both made of a polyolefin resin and a layer (α) made of a resin composition between the outermost layer (X) and the innermost layer (Y); and joining a mouth portion to one opening of the body portion to form a tube container.

15. A method for producing the tube container according to claim 1 or claim 10, comprising the steps of: a step of forming a laminate having an outermost layer (X) and an innermost layer (Y) both made of a polyolefin resin, and a layer (α) made of a resin composition between the outermost layer (X) and the innermost layer (Y); and overlapping the outermost layer (X) and the innermost layer (Y) at both ends of the laminate, and heat-sealing the opposing surfaces to form a cylindrical laminate (body portion), and joining a mouth portion to one opening of the body portion to form a tube container.

Citation Information

Patent Citations

  • Resin composition containing ethylene-vinyl alcohol copolymer

    WO2013146961A1