Manufacturing method for polishing pad
By embedding a fiber material within the resin, the convex portions of the polishing pad are reinforced, addressing the issue of peeling and enhancing the pad's durability and performance during polishing.
Patent Information
- Application Number
- JP2024046139
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2023-03-29
- Filing Date
- 2024-03-22
- Publication Date
- 2024-10-11
AI Technical Summary
Existing polishing pads face issues with convex portions of the resin peeling off during manufacturing and polishing due to insufficient strength, particularly when using an intaglio plate to transfer a concavo-convex pattern onto resin.
Embedding a fiber material inside the resin during the manufacturing process to increase the strength of the convex portions, ensuring they do not fall off during peeling from the intaglio plate and during polishing.
The embedded fiber material enhances the strength of the convex portions, preventing them from detaching during manufacturing and polishing, thereby improving the durability and effectiveness of the polishing pad.
Smart Images

Figure 2024144267000001_ABST
Abstract
Description
[Technical field]
[0001] The present invention relates to a method for producing a polishing pad. In particular, the polishing pad obtained by the production method of the present invention is used for lapping and polishing optical materials, semiconductor devices, glass substrates for hard disks, etc., and is particularly suitable for lapping and polishing sapphire, SiC, etc. [Background technology]
[0002] Polishing pads are used for lapping and polishing optical materials, semiconductor devices, glass substrates for hard disks, sapphire, and SiC. There are various types of polishing pads, including nonwoven fabric polishing pads, foamed or nonfoamed polyurethane polishing pads, fixed abrasive polishing pads, and polishing pads using a resin layer with a concave-convex pattern as the polishing surface.
[0003] Among these, polishing pads using a resin layer having a concave-convex pattern as a polishing surface have the advantage that the grooves forming the concave-convex pattern affect the fluidity of the slurry, resulting in uniform polishing of the workpiece. Methods for manufacturing such polishing pads include a method of forming grooves by cutting the surface of a flat base material, a method of forming a concave-convex pattern on a substrate by applying a screen printing method, and a method of manufacturing a mold having a concave-convex pattern and using the mold to perform molding.
[0004] For example, Patent Document 1 discloses a polishing pad (C50) on which a concave-convex pattern is formed by transferring from a plate (C72 in Figure 1) having a concave-convex pattern made of photosensitive resin, while Patent Document 2 discloses a polishing pad on which a concave-convex pattern is formed using a molding die made of silicone rubber or the like onto which a plate having a concave-convex pattern made of photosensitive resin is transferred. However, in the method of transferring a relief pattern to a resin using an intaglio plate as in Patent Documents 1 and 2, there were problems such as the fact that the hardened resin was difficult to peel off from the intaglio plate, and that the convex portions (C51) of the resin would develop cuts (C9), causing the convex portions (C51) to fall off (see Figures 1 and 2). [Prior art documents] [Patent documents]
[0005] [Patent Document 1] Patent Publication No. 2019-178248 [Patent Document 2] Patent Publication 2019-178258 Summary of the Invention [Problem to be solved by the invention]
[0006] The present invention has been made in consideration of the above problems, and provides a method for manufacturing a polishing pad having a polishing layer with excellent convex strength, in which the convex portions of the resin are less likely to fall off when a concave-convex pattern is transferred to the resin using an intaglio printing plate. [Means for solving the problem]
[0007] As a result of investigations, the inventors have discovered a method for manufacturing a polishing pad in which the strength of the protrusions is increased by embedding a fibrous material inside the resin, and this method can prevent the protrusions of the polishing pad from falling off during manufacture (when peeling off from the intaglio plate) and during polishing. The present invention encompasses the following. [1] A method for producing a polishing pad having a polishing layer having convex portions formed by curing a resin, comprising the steps of: A step of preparing an intaglio plate having a relief pattern formed thereon; pouring a resin material into the intaglio; embedding a sheet of fibrous material in the resin before the resin hardens; curing the resin; and peeling the cured resin from the intaglio to obtain the polishing layer. A method for manufacturing a polishing pad. [2] The method for manufacturing a polishing pad described in [1], wherein the polishing layer comprises the convex portion and a base portion provided below the convex portion, and the convex portion and the base portion are integrally molded from the same resin. [3] The method for manufacturing a polishing pad described in [1], wherein the fiber material is a woven fabric. [4] The method for producing a polishing pad described in [1], wherein the resin is a photocurable resin. [5] A method for producing a polishing pad having a polishing layer having convex portions formed by curing a resin, comprising the steps of: A step of preparing an intaglio plate having a relief pattern formed thereon; placing a sheet of fibrous material on said intaglio; pouring a resin material into the intaglio plate on which the fiber material is disposed; curing the resin; and peeling the cured resin from the intaglio to obtain the polishing layer. A method for manufacturing a polishing pad. Effect of the Invention
[0008] By embedding a fibrous material inside the resin, the strength of the convex parts of the polishing layer is increased, and it is possible to prevent the convex parts of the polishing pad from falling off during production (when peeling off from the intaglio) and during polishing. [Brief description of the drawings]
[0009] [Figure 1] FIG. 1 is a process diagram of a conventional method for producing a polishing layer. [Diagram 2] FIG. 2 is a schematic diagram illustrating damage and falling off C9 of the convex portions C51 when a conventional polishing layer is peeled off from an intaglio plate C72. [Diagram 3] FIG. 3 is a cross-sectional view of the polishing layer 11 of the polishing pad of the present invention. [Figure 4] FIG. 4 is a process diagram of a method for producing the polishing layer 11 of the polishing pad of the present invention. [Diagram 5] FIG. 5 is a cross-sectional view of another embodiment of the polishing layer 11 of the polishing pad of the present invention. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0010] Hereinafter, an embodiment of the present invention will be described in detail, however, the present invention is not limited to this embodiment and various modifications are possible without departing from the gist of the present invention.
[0011] The polishing layer 11 obtained by the manufacturing method of the present invention has a polishing layer 11 consisting of a convex portion 51 provided on the upper surface and a base portion 52 provided below the convex portion 51, as shown in Figure 3, and the polishing layer 11 is a polishing pad in which the convex portion 51 and the base portion 52 are integrally molded from the same resin 50, the polishing layer 11 has a concave-convex pattern, and a fiber material 6 is embedded inside the resin 50 of the base portion 52. In this specification, embedding a fiber material in a resin refers to putting all or a part of the fiber material into the resin. For convenience, the resin raw material before being poured into a mold (that is, the resin before being cured) and the cured resin will both be represented by the reference numeral 50.
[0012] <<Polishing pad manufacturing method>> A first embodiment of the method for producing a polishing pad of the present invention is as follows. Namely; A method for manufacturing a polishing pad having a polishing layer 11 having a protrusion 51 formed by curing a resin 50, comprising the steps of: A step (Step 1) of preparing an intaglio plate 72 having a concave-convex pattern; A step (Step 2) of pouring the resin material 50 into the intaglio 72; A step (Step 3) of embedding a sheet-shaped fiber material 6 in the resin 50 before the resin 50 hardens; A step (Step 4) of curing the resin 50; The method for producing a polishing pad further comprises a step (Step 5) of peeling off the cured resin 50 from the intaglio 72 to obtain the polishing layer 11.
[0013] In this specification, embedding a fiber material in a resin refers to putting all or a part of the fiber material into the resin. Fig. 1 shows a flow chart of a conventional method for manufacturing a polishing layer, and Fig. 4 shows a flow chart of a method for manufacturing a polishing layer 11 of a polishing pad according to the present invention (first embodiment). The following description will be mainly given with reference to Fig. 4.
[0014] (Step 1) An intaglio plate 72 having a concave-convex pattern formed thereon is prepared. The intaglio 72 on which the concave-convex pattern is formed may be a mold having a concave-convex pattern, an intaglio made of a photosensitive resin, an intaglio made of silicone rubber or the like, an intaglio made of a plastic material, or the like, and is not particularly limited as long as it can obtain a polishing layer 11 having convex portions 51 formed on its upper surface. Note that an intaglio is a plate that provides concave portions on the surface into which the resin is poured, thereby enabling convex portions to be formed in the resin material.
[0015] Note that a step of applying a release agent to the intaglio 72 may be included before pouring the resin raw material 50 into the intaglio 72. The release agent is not particularly limited as long as it can peel off the hardened resin from the intaglio 72, and examples of the release agent include silicone-based release agents and fluorine-based release agents, with fluorine-based release agents being preferred. The method of applying the release agent is not particularly limited as long as it can peel off the hardened resin from the intaglio 72, and examples of the method include a spray method and an electrostatic application method, with the spray method being preferred.
[0016] (Step 2) The resin material 50 is poured into the intaglio plate 72 . The method of pouring the resin raw material 50 into the intaglio 72 is not particularly limited as long as the resin raw material 50 is filled (pouring) into the recesses of the intaglio 72. Examples of the method include a gravity casting method in which the resin raw material is poured into the recesses by its own weight at room temperature and normal pressure, and a vacuum casting method in which the intaglio 72 and resin 50 are placed in a vacuum container, the pressure is reduced, and the resin raw material is poured into the recesses at atmospheric pressure. When pouring the resin 50, since the polishing layer 11 has a convex portion 51 and a base portion 52, it is necessary not only to pour the resin 50 into the concave portion of the intaglio 72, but also to pour the resin to a height that exceeds the height of the convex portion of the intaglio 72 to form the base 52.
[0017] The resin 50 is not particularly limited as long as a polishing pad using the resin layer 11 having a concave-convex pattern as a polishing surface can be obtained, but a curable resin composition is preferred. The curable resin composition is not particularly limited, and examples thereof include a thermosetting resin, a UV-curable resin, a photocurable resin composition containing a photopolymerization initiator and a polymerizable compound, a thermosetting resin composition containing a thermal polymerization initiator and a polymerizable compound, a curable resin composition containing a two-liquid mixed curable resin, etc. Furthermore, the curable resin composition may contain a crosslinking agent having two or more polymerizable functional groups, etc., as necessary.
[0018] The thermosetting resin is not particularly limited, but examples thereof include phenol resin, epoxy resin, acrylic resin, urethane resin, and formaldehyde resin.
[0019] The UV-curable resin is not particularly limited, but for example, a prepolymer having a number average molecular weight of about 1,000 to 10,000 is preferable. Examples of the material include isocyanurate-based resins, acrylic (methacrylic) ester resins and their urethane-modified resins, thiokol-based resins, etc., and a reactive diluent or organic solvent can be used appropriately depending on the application.
[0020] Examples of photopolymerization initiators include benzophenone compounds, acetophenone compounds, and thioxanthones. Examples of thermal polymerization initiators include azo compounds such as 2,2'-azobisbutyronitrile, and peroxides such as methyl ethyl ketone peroxide and benzoyl peroxide (BPO).
[0021] Specific examples of the resin include unsaturated carboxylic acids having a polymerizable unsaturated group, such as (meth)acrylic acid, itaconic acid, crotonic acid, isocrotonic acid, and maleic acid; unsaturated carboxylic acid esters having a polymerizable unsaturated group, such as (meth)acrylate, epoxy (meth)acrylate (vinyl ester resin), urethane (meth)acrylate, and polyester (meth)acrylate; polyesters having unsaturated groups; polyethers having a polymerizable unsaturated group; polyamides having a polymerizable unsaturated group; urethanes having a polymerizable unsaturated group; and aromatic compounds having a polymerizable unsaturated group, such as styrene.
[0022] The two-liquid mixed curable resin is not particularly limited, but examples thereof include prepolymers having different physical properties, such as epoxy resins, unsaturated polyester resins, and polyamide resins.
[0023] Among these, those that are easily cured into a desired shape and that cure at room temperature are preferred from the viewpoint of considering the heat resistance of the intaglio 72. Such curable resin compositions are not particularly limited, and examples thereof include curable resin compositions containing a polymerization initiator that acts at room temperature, UV-curable resin compositions and photocurable resin compositions that cure upon irradiation with light, and mixed-type curable resin compositions that cure by mixing two liquids. In terms of polishing (lapping) performance, vinyl ester resin or unsaturated polyester resin, which has high heat resistance (high deformation temperature), is preferred.
[0024] (Step 3) The process of embedding the sheet-shaped fiber material 6 in the resin 50 before the resin 50 hardens will be described. The method of embedding the sheet-like fiber material 6 in the resin 50 before the resin 50 hardens is not particularly limited as long as it is possible to embed the fiber material 6 in the resin 50. For example, one possible method is to pour the resin 50 into the intaglio 72, and then place the sheet-like fiber material 6 in the resin 50 in a low-viscosity state before it hardens, and apply pressure by its own weight or by hand, etc., to embed the fiber material 6 in the resin 50. The positional relationship between the fiber material 6 and the intaglio plate 72 may be such that the fiber material 6 does not come into contact with the uneven pattern of the intaglio plate 72, as shown in Figure 4, or such that the fiber material 6 comes into contact with the uneven pattern of the intaglio plate 72.
[0025] The timing for embedding the fiber material 6 in the resin 50 may include during or after the process of pouring the resin raw material 50 into the intaglio 72, but is not particularly limited as long as it is possible to embed it in the resin 50, and varies depending on the materials and strength adjustments of the resin raw material 50 and the fiber material 6.
[0026] The fiber material 6 embedded in the resin 50 of the base 52 of the polishing layer 11 of the polishing pad of the present invention may be in the form of a thread, a bundle, a cotton, a cloth, etc., with the cloth being preferred. Examples of the cloth-like fiber material include woven fabric, knitted fabric, nonwoven fabric, etc., with woven fabric and knitted fabric being preferred to increase the resin strength, and mesh fabric being particularly preferred.
[0027] Examples of the material of the fiber material 6 include organic fibers, inorganic fibers, synthetic fibers, semi-synthetic fibers, and regenerated fibers. Examples of the organic fibers include, but are not limited to, fibers derived from natural products such as cellulose, carbon fibers, pulp, chitin, and chitosan. Examples of the inorganic fibers include, but are not limited to, glass fibers, rock fibers, and metal fibers. Examples of the synthetic fibers include, but are not limited to, nylon, vinylon, vinylidene, polyester, polyolefin (e.g., polyethylene, polypropylene, etc.), polyurethane, acrylic, polyvinyl chloride, aramid, etc. Examples of the semi-synthetic fibers include, but are not limited to, acetate, triacetate, and promix. Examples of the regenerated fibers include, but are not limited to, rayon, cupra, polynosic rayon, lyocell, and tencel. The fiber material 6 embedded in the resin 50 of the base 52 of the polishing layer 11 of the polishing pad of the present invention is preferably polyethylene or polypropylene in terms of ease of availability and ease of processing.
[0028] The fiber diameter of the fiber material 6 is 100 μm or more and 300 μm or less, more preferably 150 μm or more and 250 μm or less. When the fiber diameter of the fiber material 6 is within the above range, it functions as a skeleton material for the resin 50 and can increase the strength of the polishing layer 11. If the fiber diameter is less than 100 μm, the strength may be insufficient, and if the fiber diameter is more than 300 μm, air may enter from the surroundings when the fiber material 6 is incorporated into the resin 50.
[0029] The mesh size of the fiber material 6 is 10 μm or more and 700 μm or less, more preferably 30 μm or more and 520 μm or less. When the mesh size of the fiber material 6 is within the above range, it can be appropriately incorporated into the resin and increase the strength of the resin 50. If the mesh size is less than 10 μm, the resin 50 will not blend well, and if the mesh size is more than 700 μm, it will not function as a skeleton material and the strength of the polishing layer 11 will be insufficient.
[0030] The thickness of the fiber material 6 is 100 μm or more and 500 μm or less, more preferably 150 μm or more and 300 μm or less. When the thickness of the fiber material 6 is within the above range, the strength of the polishing layer 11 can be increased without impairing the polishing performance as a polishing pad.
[0031] Furthermore, after embedding the fiber material 6 in the resin 50, and before curing the resin 50, a step of bonding a substrate to the surface of the resin 50 opposite to the surface that contacts the intaglio 72 may be further included. By using a substrate, the resin 50 is cured in a state in which the resin 50 is sandwiched between the substrate and the intaglio 72. This tends to improve the uniformity of the thickness of the obtained cured product, and to further improve the flatness of the back surface (the surface opposite to the surface that contacts the intaglio 72) of the obtained cured product.
[0032] (Step 4) The process of curing the resin raw material 50 will now be described. The method for curing the resin raw material 50 is not particularly limited as long as it is a method suitable for each resin raw material 50, and examples thereof include a photocuring method in which ultraviolet light or the like is irradiated, a thermal curing method in which heat is applied (including a method in which it is left at room temperature), and a method in which it is mixed and left as in the case of a two-liquid mixing type. Examples of the device to be used include a method using a device that irradiates light and a method using a thermostatic device, and the device that irradiates light is not particularly limited as long as it is a device that emits light in a wavelength range that includes the wavelength of light at which the photocurable resin is cured, and examples thereof include an ultraviolet irradiating device. The light to be irradiated is not particularly limited as long as it can cure the resin raw material 50, and examples thereof include ultraviolet light. Examples of light sources that emit such light include high-pressure mercury lamps, UV-LED lamps, and black light fluorescent lamps (BLBs). Among these, BLBs are preferred. The direction of light irradiation may be either the direction of irradiation from the lower surface 72A side of the plastic intaglio 72 or the direction of irradiation from the upper surface 50A side of the resin raw material 50. When irradiation is performed from the lower surface 72A side, the light can be sufficiently applied to the convex portions 51, so that the convex portions 51 are sufficiently cured. The wavelength of the ultraviolet irradiation is preferably 200 nm to 400 nm, and the irradiation time is preferably 3 minutes to 30 minutes. Examples of the thermosetting method that involves applying heat include a method in which the intaglio 72 with the resin raw material 50 poured therein is placed in an oven and heated, and a method in which the intaglio 72 is heated in advance and then the resin raw material 50 is poured into it. The timing for curing the resin raw material 50 is preferably such that the fiber material 6 is embedded in the resin 50 before curing and then the resin is cured.
[0033] (Step 5) The hardened resin 50 is peeled off from the intaglio 72 to obtain the polishing layer 11. The peeling can be performed by holding the edge of the polishing layer 11 and peeling it off from the intaglio 72. The polishing layer 11 thus obtained has a concave-convex pattern transferred from the intaglio 72, and the surfaces of the convex portions 51 of the concave-convex pattern become the polishing surface for polishing an object to be polished.
[0034] The bending strength of the obtained abrasive layer 11 is 30 MPa or more, preferably 30 to 1000 MPa, more preferably 40 to 900 MPa, and further preferably 50 to 800 MPa. The bending strength is obtained by measurement performed in accordance with JIS K7203. When the bending strength is within the above range, damage or deformation of the abrasive layer 11 can be suppressed when the abrasive layer 11 is peeled off from the intaglio 72.
[0035] In addition, it is preferable that the polishing layer 11 is composed of a protrusion 51 and a base 52 provided under the protrusion 52, and the base 52 and the protrusion 51 are integrally molded from the same resin and have a concave-convex pattern. By integrally molding the protrusion 51 and the base 52, the process of joining the protrusion 51 and the base 52 is eliminated, and costs can be reduced. In addition, the joining strength is higher than when the protrusion 51 and the base 52 are bonded, and the protrusion 51 is less likely to come off the base 52. The surface of the polishing layer 11 with the protrusion 51 becomes the polishing surface.
[0036] The average height of the protrusions 51 of the uneven pattern of the polishing layer 11 of the polishing pad of the present invention is preferably 0.3 mm or more and 1.5 mm or less, and more preferably 0.8 mm or more and 1.2 mm or less. If the average height of the protrusions 51 is less than 0.3 mm, the product life of the polishing pad will be shortened, and if it is more than 1.5 mm, there is a risk of it falling off or being damaged during production. In this specification, α in FIG. 3 (the distance from the surface of base 52 on the side of convex portion 51 to the highest point of convex portion 51) is referred to as the height of the convex portion. The shape of the protrusions 51 of the abrasive layer 11 is a truncated quadrangular pyramid in this example, but may also be a truncated cone shape such as a truncated circular cone, an approximately truncated circular cone, or an elliptical truncated cone, or a columnar shape such as a quadrangular prism, a circular cylinder, an approximately circular cylinder, or an elliptical cylinder.
[0037] Next, a second embodiment of the production method of the present invention will be described. The second embodiment is as follows. A method for manufacturing a polishing pad having a polishing layer 11 having a protrusion 51 formed by curing a resin 50, comprising the steps of: A step of preparing an intaglio plate 72 having a concave-convex pattern; placing a sheet-like fiber material 6 on the intaglio 72; pouring a resin raw material 50 into the intaglio 72 on which the fiber material 6 is disposed; curing the resin 50; and peeling off the cured resin 50 from the intaglio 72 to obtain the polishing layer 11. A method for manufacturing a polishing pad.
[0038] The second embodiment has many parts in common with the first embodiment, but in the second embodiment, the sheet-like fiber material 6 is placed before pouring the resin 50 into the intaglio 72, and then the resin 50 is poured in. By doing this, it is not necessary to embed the sheet-like fiber material 6, but it is necessary to prevent the sheet-like fiber material 6 from being washed away when the resin 50 is poured.
[0039] When the sheet-like fiber material 6 has openings like a mesh fabric, the second embodiment is preferably used.
[0040] FIG. 5 shows an abrasive layer 11 having a different shape from that shown in FIG. 3. The difference from the abrasive layer 11 in FIG. 5 is that it has a recess 53 on the opposite side to the protrusion 51. Providing the recess 53 can achieve further weight reduction and cost reduction. The recess 53 can be provided by intentionally reducing the amount of resin at the location where the protrusion 51 is to be formed in the above-mentioned Step 2, or by pressing a mold corresponding to the recess 53 from above after the step 3. The shape of the recess 53 is not particularly limited, and may be a shape having corners (for example, a truncated pyramid) as shown in FIG. 5, or a shape having a curved surface (for example, a dome shape). EXAMPLES
[0041] The present invention will be described in more detail below with reference to examples, but the present invention is not limited to these examples.
[0042] In each of the examples and comparative examples, unless otherwise specified, "parts" means "parts by mass".
[0043] (polishing pad manufacturing)
[0044] (Manufacture of polishing pad 1) A polypropylene resin sheet was vacuum molded to produce an intaglio plate 72 having a plurality of recesses in the shape of a truncated quadrangular pyramid with a height of 0.85 mm and a base of 1.5 mm on each side. Next, 90 parts of unsaturated polyester resin (product name: Rigolac, manufactured by Resonac Co., Ltd.) was poured into this intaglio 72. Before curing, a mesh fabric made of polypropylene with a fiber diameter of 150 μm, mesh size of 30 μm, and thickness of 300 μm was sunk from above the resin 50 into the interior as the fiber material 6, so that the fiber material 6 penetrated into the base 52. After the resin 50 was cured at room temperature (25° C.) for 30 minutes, the intaglio 72 was removed by peeling the resin 50 from the intaglio 72, and the polishing pad 1 was manufactured.
[0045] (Manufacture of polishing pad 2) Polishing pad 2 was manufactured in the same manner as polishing pad 1, except that the material of the polishing pad was vinyl ester resin (product name: Lipoxy, manufactured by Resonac Co., Ltd.) instead of unsaturated polyester resin, and the material of the mesh fabric was polyethylene fiber instead of polypropylene fiber.
[0046] It was confirmed that in manufacturing polishing pad 2, even if the material of the polishing pad and the material of the mesh fabric were changed, a polishing pad similar to polishing pad 1 could be manufactured using a plastic intaglio made of polypropylene resin.
[0047] (When peeled off from the intaglio plate) A peeling experiment was conducted on the resin 50 from the intaglio 72 using a peeling roller. As the peeling roller, for example, a combination of an adhesive tape and a rod-shaped peeling roller as described in JP-A-9-114384 can be used. When a peeling experiment was conducted under conditions that allowed the intaglio 72 to be peeled off from the resin 50 for the one including the mesh fabric in the base 52 according to the above embodiment and for the one not including the mesh fabric in the base 52, the convex portion 51 fell off or was damaged in the one not including the mesh fabric in the base 52, whereas the polishing pad 1 and the polishing pad 2 obtained using the plastic intaglio 72 made of polypropylene resin did not suffer from the falling off or damage in the convex portion 51 during peeling. [Industrial Applicability]
[0048] The method for producing a polishing pad of the present invention has industrial applicability as a method for producing a polishing pad used for lapping or polishing optical materials, semiconductor devices, glass substrates for hard disks, and the like.
[0049] 11 Polishing layer 72 Intaglio 72A Intaglio bottom surface 50 Resin raw materials 50A Top surface of resin raw material 51 Convex 52 Base 53 Recess 6. Textile materials C9 Falling off of convex part
Claims
1. A method for producing a polishing pad having a polishing layer having a convex portion formed by curing a resin, comprising the steps of: A step of preparing an intaglio plate having a relief pattern formed thereon; pouring a resin material into the intaglio; embedding a sheet of fibrous material in the resin before the resin hardens; curing the resin; and peeling the cured resin from the intaglio to obtain the polishing layer. A method for manufacturing a polishing pad.
2. 2. The method for producing a polishing pad according to claim 1, wherein the polishing layer comprises the convex portion and a base portion provided below the convex portion, and the convex portion and the base portion are integrally molded from the same resin.
3. The method for producing a polishing pad according to claim 1 , wherein the fibrous material is a woven fabric.
4. The method for producing a polishing pad according to claim 1 , wherein the resin is a photocurable resin.
5. A method for producing a polishing pad having a polishing layer having a convex portion formed by curing a resin, comprising the steps of: A step of preparing an intaglio plate having a relief pattern formed thereon; placing a sheet of fibrous material on said intaglio; pouring a resin material into the intaglio plate on which the fiber material is disposed; curing the resin; and peeling the cured resin from the intaglio to obtain the polishing layer. A method for manufacturing a polishing pad.
Citation Information
Patent Citations
Polishing pad and method for manufacturing the same
JP2019178248A
Polishing pad and method for manufacturing the same