Polar group-containing olefin copolymer and method for producing the same

JP2024144296APending Publication Date: 2024-10-11JAPAN POLYCHEM CORP
View PDF 3 Cites 0 Cited by

Patent Information

Application Number
JP2024048853
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Priority Date
2023-03-30
Filing Date
2024-03-26
Publication Date
2024-10-11

AI Technical Summary

Benefits of technology

【0021】 本発明によれば、オレフィン、炭酸ビニレン誘導体および特定の極性基含有モノマー由来の構造単位を含む新規な極性基含有エチレン共重合体、及びその製造方法を提供することができる。

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024144296000045
    Figure 2024144296000045
  • Figure 2024144296000046
    Figure 2024144296000046
  • Figure 2024144296000047
    Figure 2024144296000047
Patent Text Reader

Abstract

To provide a novel polar group-containing olefin copolymer and a method for producing the same.SOLUTION: The polar group-containing olefin copolymer contains a structural unit (A) derived from at least one C2-20 olefin, a structural unit (B) derived from at least one monomer represented by the following general formula (1), and a structural unit (C) derived from at least one monomer represented by the following general formula (2). (R1 and R2 each independently represent a hydrogen atom, a halogen atom, a hydroxyl group, a formyl group, a carboxy group, a C1-30 ester group, a C1-30 acyloxy group, or the like; R3 represents a hydrogen atom, a halogen atom, a C1-10 hydrocarbon group substituted with at least one halogen atom, or a C1-10 hydrocarbon group; and R4 represents a hydrogen atom, a silyl group which may be substituted with at least one C1-30 hydrocarbon group, or the like.)SELECTED DRAWING: None
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a novel polar group-containing olefin copolymer, and more particularly to a novel polar group-containing olefin copolymer having a main chain containing a structure derived from an olefin having 2 to 20 carbon atoms, a vinylene carbonate derivative, and a structure derived from a specific polar group-containing monomer, and a method for producing the same. [Background technology]

[0002] Among resin materials, olefin copolymers have excellent properties such as physical properties and moldability, and are also highly economical and environmentally friendly, making them important industrial materials in wide use. However, since olefin copolymers do not have polar groups, it has been difficult to apply them to applications requiring physical properties such as adhesion to other materials, printability, or compatibility with fillers. In recent years, research has been actively conducted into the introduction of polar groups into the polymer chains of olefin copolymers by copolymerization of olefins with polar vinyl monomers in the presence of late periodic metal complexes (Non-Patent Document 1). In addition, as copolymers of olefins and vinylene carbonate, polar group-containing olefin copolymers obtained by radical copolymerization of ethylene and vinylene carbonate have been reported (for example, Patent Documents 1 and 2). Furthermore, copolymerization of ethylene and vinylene carbonate using a metal catalyst and hydrolysis of the obtained polar group-containing olefin copolymer have been reported (Patent Document 3).

[0003] It has been reported that the cyclic carbonate structure introduced by copolymerization with vinylene carbonate easily reacts with amines and can be used for graft polymerization and crosslinking of polymer chains (e.g., Non-Patent Documents 2, 3). [Prior art documents] [Patent documents]

[0004] [Patent Document 1] U.S. Patent No. 2,847,398 [Patent Document 2] U.S. Pat. No. 3,114,728 [Patent Document 3] International Publication No. WO 00 / 56781 [Non-patent literature]

[0005] [Non-Patent Document 1] Chem. Rev., 2011, 111, 2363-2449. [Non-Patent Document 2] J.Polym.Sci.A:Polym.Chem.,2001,39,860-867. [Non-Patent Document 3] J.Network Polym.Japan,2015,36,160-166. [Non-Patent Document 4] Organometallics,2004,23,5121-5123. [Non-Patent Document 5] J.Am.Chem.Soc.,2009,131,12613-12622. Summary of the Invention [Problem to be solved by the invention]

[0006] Vinylene carbonate is a compound industrially produced by the chlorination of ethylene carbonate and subsequent dehydrochlorination, and is mainly used as an additive in lithium-ion batteries. On the other hand, since it contains a carbon-carbon double bond in its structure, it can also be used in copolymerization with α-olefins. Since the raw material ethylene carbonate can be produced from carbon dioxide, the copolymerization of vinylene carbonate with α-olefins can be regarded as a method of carbon dioxide fixation. In addition, the copolymerization of vinylene carbonate with α-olefins can introduce oxygen atoms into the vicinal positions of polyolefins. Non-Patent Documents 4 and 5 report that copolymerization of ethylene and acrylic esters does not proceed.

[0007] In this situation, an object of the present application is to provide a novel polar-group-containing ethylene copolymer containing structural units derived from an olefin, a vinylene carbonate derivative, and a specific polar-group-containing monomer, and a method for producing the same. [Means for solving the problem]

[0008] As a result of intensive research aimed at achieving the above-mentioned object, the present researchers have discovered a polar-group-containing olefin copolymer having a novel structure using an olefin, a vinylene carbonate derivative, and a specific polar-group-containing monomer, and a method for producing the same. That is, the present invention includes the following aspects.

[0009] <1> A structural unit (A) derived from at least one olefin having 2 to 20 carbon atoms; A polar group-containing olefin copolymer, comprising: a structural unit (B) derived from at least one monomer represented by the following general formula (1); and a structural unit (C) derived from at least one monomer represented by the following general formula (2):

[0010] [ka] (In formula (1), R 1 and R 2are each independently a hydrogen atom, a halogen atom, a hydroxyl group, a formyl group, a carboxy group, an ester group having 1 to 30 carbon atoms, an acyloxy group having 1 to 30 carbon atoms, an acyl group having 1 to 30 carbon atoms, an alkoxy group having 1 to 30 carbon atoms, an aryloxy group having 6 to 30 carbon atoms, an alkylthio group having 1 to 30 carbon atoms, an arylthio group having 6 to 30 carbon atoms, a nitro group, an amino group which may be substituted with at least one hydrocarbon group having 1 to 30 carbon atoms, a silyl group which may be substituted with at least one hydrocarbon group having 1 to 30 carbon atoms, an amido group which may be substituted with at least one hydrocarbon group having 1 to 30 carbon atoms, a hydrocarbon group having 1 to 30 carbon atoms substituted with at least one halogen atom, or a hydrocarbon group or heterocyclic group having 1 to 30 carbon atoms which may be substituted with at least one substituent containing at least one selected from the group consisting of an oxygen atom, a sulfur atom, and a nitrogen atom, or R 1 and R 2 may be bonded to each other to form a 4- to 10-membered ring.

[0011] [ka] (In formula (2), R 3 is a hydrogen atom, a halogen atom, a hydrocarbon group having 1 to 10 carbon atoms substituted with at least one halogen atom, or a hydrocarbon group having 1 to 10 carbon atoms. R 4 is a hydrogen atom, a silyl group which may be substituted with at least one hydrocarbon group having 1 to 30 carbon atoms, a hydrocarbon group having 1 to 30 carbon atoms which is substituted with at least one halogen atom, or a hydrocarbon group or heterocyclic group having 1 to 30 carbon atoms which may be substituted with at least one substituent containing at least one of an oxygen atom, a sulfur atom, or a nitrogen atom.

[0012] <2> The structural unit (B) is a structural unit represented by the following general formula (I), or a structural unit represented by the following general formula (I) and a structural unit represented by the following general formula (II), <1> 2. The polar group-containing olefin copolymer according to claim 1 .

[0013] [ka] (In formula (I) and formula (II), R 1 and R 2 is the same as above.)

[0014] <3> The structural unit (C) is represented by the following general formula (III): <1> or <2> 2. The polar group-containing olefin copolymer according to claim 1 .

[0015] [ka] (In formula (III), R 3 and R 4 is the same as above.)

[0016] <4> R of the structural unit (B) 1 and R 2 At least one of the above is a hydrogen atom. <1> ~ <3> 2. The polar group-containing olefin copolymer according to claim 1 . <5> R of the structural unit (C) 3 is a hydrogen atom. <1> ~ <4> 2. The polar group-containing olefin copolymer according to claim 1 . <6> R of the structural unit (B) 1 and R 2 are each a hydrogen atom. <1> ~ <5> 2. The polar group-containing olefin copolymer according to claim 1 . <7> The olefin is ethylene. <1> ~ <6> 2. The polar group-containing olefin copolymer according to claim 1 . <8> The content of the structural unit (B) is 0.01 mol % to 10 mol %. <1> ~ <7> 2. The polar group-containing olefin copolymer according to claim 1 . <9> The content of the structural unit (C) is 0.01 mol % to 30 mol %. <1> ~ <8> 2. The polar group-containing olefin copolymer according to claim 1 .

[0017] <10> A method for producing a polar group-containing olefin copolymer, comprising polymerizing at least one olefin having 2 to 20 carbon atoms, at least one monomer represented by the following general formula (1), and at least one monomer represented by the following general formula (2) in the presence of a catalyst containing at least one compound represented by the following general formula (101):

[0018] [ka] [In general formula (101), M represents a metal atom of Group 10 of the periodic table. Q represents an oxygen atom, a sulfur atom, -S(=O)2-O-, or -C(=O)-O-, and the left side of each of these groups is bonded to A and the right side is bonded to M. A represents a divalent hydrocarbon group having 1 to 30 carbon atoms which may have a substituent. R L represents a hydrogen atom, a hydrocarbon group having 1 to 20 carbon atoms which may contain a hetero atom, or a ligand coordinated to M. L represents a ligand coordinated to M. R x and R y each independently represents a hydrogen atom or a hydrocarbon group having 1 to 20 carbon atoms which may contain a heteroatom. R L and L and R x and R y may form a ring, R x and A or R y and A may form a ring.

[0019] [ka] (In formula (1), R 1 and R 2 is the same as above.)

[0020] [ka] (In formula (2), R 3 and R 4 is the same as above.) Effect of the Invention

[0021] According to the present invention, it is possible to provide a novel polar-group-containing ethylene copolymer containing structural units derived from an olefin, a vinylene carbonate derivative, and a specific polar-group-containing monomer, and a method for producing the same. [Brief description of the drawings]

[0022] [Figure 1] FIG. 1 shows the results of 13C-NMR measurement of the polar group-containing olefin copolymer 1 of Example 1. [Diagram 2] FIG. 2 shows a partially enlarged view of the 13C-NMR measurement result of the polar group-containing olefin copolymer 1 of Example 1. [Diagram 3] FIG. 3 shows the results of 1H-NMR measurement of the polar group-containing olefin copolymer 1 of Example 1. [Figure 4] FIG. 4 shows a partially enlarged view of the 1H-NMR measurement results of the polar group-containing olefin copolymer 1 of Example 1. [Diagram 5] FIG. 5 shows the results of HSQC measurement of the polar group-containing olefin copolymer 1 of Example 1. [Figure 6] FIG. 6 shows an enlarged view of a part of the HSQC measurement result of the polar group-containing olefin copolymer 1 of Example 1. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0023] The polar group-containing olefin copolymer of the present invention will be described in detail below for each item. In this specification, "(meth)acryloyl" refers to acryloyl and methacryloyl. In this specification, "to" indicating a numerical range is used to mean that the numerical values ​​before and after it are included as the lower limit and upper limit.

[0024] The polar group-containing olefin copolymer of the present invention comprises a structural unit (A) derived from at least one olefin having 2 to 20 carbon atoms, The polar group-containing olefin copolymer comprises a structural unit (B) derived from at least one monomer represented by the following general formula (1) and a structural unit (C) derived from at least one monomer represented by the following general formula (2):

[0025] [ka] (In formula (1), R 1 and R 2 are each independently a hydrogen atom, a halogen atom, a hydroxyl group, a formyl group, a carboxy group, an ester group having 1 to 30 carbon atoms, an acyloxy group having 1 to 30 carbon atoms, an acyl group having 1 to 30 carbon atoms, an alkoxy group having 1 to 30 carbon atoms, an aryloxy group having 6 to 30 carbon atoms, an alkylthio group having 1 to 30 carbon atoms, an arylthio group having 6 to 30 carbon atoms, a nitro group, an amino group which may be substituted with at least one hydrocarbon group having 1 to 30 carbon atoms, a silyl group which may be substituted with at least one hydrocarbon group having 1 to 30 carbon atoms, an amido group which may be substituted with at least one hydrocarbon group having 1 to 30 carbon atoms, a hydrocarbon group having 1 to 30 carbon atoms substituted with at least one halogen atom, or a hydrocarbon group or heterocyclic group having 1 to 30 carbon atoms which may be substituted with at least one substituent containing at least one selected from the group consisting of an oxygen atom, a sulfur atom, and a nitrogen atom, or R 1 and R 2 may be bonded to each other to form a 4- to 10-membered ring.

[0026] [ka] (In formula (2), R 3 is a hydrogen atom, a halogen atom, a hydrocarbon group having 1 to 10 carbon atoms substituted with at least one halogen atom, or a hydrocarbon group having 1 to 10 carbon atoms. R 4 is a hydrogen atom, a silyl group which may be substituted with at least one hydrocarbon group having 1 to 30 carbon atoms, a hydrocarbon group having 1 to 30 carbon atoms which is substituted with at least one halogen atom, or a hydrocarbon group or heterocyclic group having 1 to 30 carbon atoms which may be substituted with at least one substituent containing at least one of an oxygen atom, a sulfur atom, or a nitrogen atom.

[0027] As shown in FIG. 1 etc., the polar group-containing olefin copolymer of the present invention is a novel polar group-containing olefin copolymer, which contains, in the main chain of an olefin polymer having two or more carbon atoms such as ethylene (the wavy line in the chemical structural formula in the figure represents the main chain of the polymer), a structural unit (B) containing a polar group derived from a vinylene carbonate derivative represented by the general formula (1) above, and a structural unit (C) containing a polar group derived from an acrylic ester derivative represented by the general formula (2) above.

[0028] The polar group-containing olefin copolymer of the present invention may contain, as the structural unit (B), a structural unit represented by the following general formula (I) as an essential structural unit, i.e., may contain a structural unit represented by the following general formula (I), or a structural unit represented by the following general formula (I) and a structural unit represented by the following general formula (II). The polar group-containing olefin copolymer of the present invention may further contain, as the structural unit (C), a structure represented by the following general formula (III).

[0029] [ka] (In formula (I) and formula (II), R 1 and R 2 is the same as above.)

[0030] [ka] (In formula (III), R 3 and R 4 is the same as above.)

[0031] The polar group-containing olefin copolymer of the present invention has a structural unit derived from a vinylene carbonate derivative having an oxygen atom at a vicinal position and a structural unit derived from an acrylic acid ester derivative introduced into a polyolefin having two or more carbon atoms such as ethylene. This is expected to realize a function not found in conventional ethylene copolymers, such as an ethylene-vinylene carbonate-acrylic acid ester copolymer having a chelating ability to metals. Copolymers having such functions are expected to be used as supports for metal complex catalysts and adsorbents for recovering metal complexes.

[0032] In addition, it is believed that the polar group-containing olefin copolymer of the present invention can be further functionalized by carrying out graft polymerization using the different polar groups contained in the structural unit (B) or the structural unit (C). When the polar group-containing olefin copolymer of the present invention is made into a hydrolyzate, the acidity of the -OH protons derived from the vinylene carbonate derivative and the -COOH protons derived from the acrylate derivative differ, which makes it possible to perform different chemical modifications, and different material properties can be expected to be obtained from conventional olefin-acrylate copolymers. Furthermore, it is believed that carbon dioxide can be fixed by copolymerization of ethylene, vinylene carbonate derivatives, and acrylic acid ester derivatives. Polyethylene is the most widely produced plastic, and there is a clear demand for further functionalization and reduction of carbon dioxide emissions during its production.

[0033] (1) Structural unit (A) The structural unit (A) is a structural unit derived from at least one olefin having 2 to 20 carbon atoms. The monomer (monomer (A)) used in the present invention from which the structural unit (A) is derived is at least one type of olefin having 2 to 20 carbon atoms. The olefin having 2 to 20 carbon atoms may be a chain olefin or a cyclic olefin, and examples thereof include at least one type selected from the group consisting of α-olefins having 2 to 20 carbon atoms, including ethylene, and cyclic olefins having 4 to 20 carbon atoms.

[0034] The α-olefin having 2 to 20 carbon atoms used in the present invention is an α-olefin having 2 to 20 carbon atoms represented by the structural formula: CH2=CHR (wherein R is a hydrogen atom or a hydrocarbon group having 1 to 18 carbon atoms, which may have a linear structure or may be branched), and more preferably an α-olefin having 2 to 12 carbon atoms. Examples of the cyclic olefin having 4 to 20 carbon atoms include cyclobutene, cyclopentene, cyclohexene, and norbornene.

[0035] Specific examples of the monomer (A) include ethylene, propylene, 1-butene, 1-pentene, 1-hexene, 1-octene, 1-decene, 3-methyl-1-butene, 4-methyl-1-pentene, and norbornene, etc. From the viewpoint of the production efficiency of the polymer, the monomer (A) is preferably at least one selected from the group consisting of ethylene, propylene, 1-butene, and norbornene, and more preferably ethylene. The structural unit (A) may be one type alone or two or more types. Examples of combinations of two or more types include combinations of two or more types of the monomers (A) of the above specific examples. More specifically, examples of combinations of two types include structural units derived from ethylene-1-butene, ethylene-1-hexene, ethylene-1-octene, ethylene-norbornene, etc. Examples of combinations of three types include structural units derived from ethylene-1-butene-1-hexene, ethylene-1-butene-1-octene, etc.

[0036] In the present invention, the monomer (A) preferably contains ethylene as an essential component and may further contain one or more α-olefins having 3 to 20 carbon atoms, if necessary. The amount of ethylene in the monomer (A) may be 65 mol % to 100 mol % or 70 mol % to 100 mol % relative to 100 mol % of the entire monomer (A).

[0037] (2) Structural unit (B) The structural unit (B) is a structural unit derived from at least one type of monomer represented by the following general formula (1).

[0038] [ka] (In formula (1), R 1 and R 2 are each independently a hydrogen atom, a halogen atom, a hydroxyl group, a formyl group, a carboxy group, an ester group having 1 to 30 carbon atoms, an acyloxy group having 1 to 30 carbon atoms, an acyl group having 1 to 30 carbon atoms, an alkoxy group having 1 to 30 carbon atoms, an aryloxy group having 6 to 30 carbon atoms, an alkylthio group having 1 to 30 carbon atoms, an arylthio group having 6 to 30 carbon atoms, a nitro group, an amino group which may be substituted with at least one hydrocarbon group having 1 to 30 carbon atoms, a silyl group which may be substituted with at least one hydrocarbon group having 1 to 30 carbon atoms, an amido group which may be substituted with at least one hydrocarbon group having 1 to 30 carbon atoms, a hydrocarbon group having 1 to 30 carbon atoms substituted with at least one halogen atom, or a hydrocarbon group or heterocyclic group having 1 to 30 carbon atoms which may be substituted with at least one substituent containing at least one selected from the group consisting of an oxygen atom, a sulfur atom, and a nitrogen atom, or R 1 and R 2 may be bonded to each other to form a 4- to 10-membered ring.

[0039] In the general formula (1), examples of the halogen atom include a fluorine atom, a chlorine atom, a bromine atom, and an iodine atom. In the general formula (1), the ester group having 1 to 30 carbon atoms is -COORa where R a represents a hydrocarbon group having 1 to 30 carbon atoms. The number of carbon atoms in the ester group does not include the number of carbon atoms in the carbonyl group. a The lower limit of the carbon number is 1 or more, and may be 2 or more, and the upper limit of the carbon number is 30 or less, and may be 20 or less, or may be 10 or less.

[0040] R a Examples of the hydrocarbon group having 1 to 30 carbon atoms in the formula (I) include linear, branched, and cyclic saturated or unsaturated aliphatic hydrocarbon groups, aromatic hydrocarbon groups, and combinations thereof. Preferred examples of the hydrocarbon group having 1 to 30 carbon atoms include the following examples of alkyl groups having 1 to 30 carbon atoms, as well as alkenyl groups such as ethenyl, propenyl, butenyl, and pentenyl groups; aryl groups such as phenyl, methylphenyl, n-propylphenyl, i-propylphenyl, n-butylphenyl, i-butylphenyl, s-butylphenyl, t-butylphenyl, n-hexylphenyl, trimethylphenyl, pentamethylphenyl, biphenyl, naphthyl, anthracenyl, fluorenyl, and tolyl groups; and aralkyl groups such as benzyl, phenylethyl, phenylpropyl, naphthylmethyl, diphenylmethyl, and triphenylmethyl groups.

[0041] The alkyl group having 1 to 30 carbon atoms may be, for example, linear, branched, or cyclic, and examples thereof include a methyl group, an ethyl group, a 1-propyl group, a 1-butyl group, a 1-pentyl group, a 1-hexyl group, a 1-heptyl group, a 1-octyl group, a 1-nonyl group, a 1-decyl group, a t-butyl group, a tricyclohexylmethyl group, an isopropyl group, a 1-dimethylpropyl group, a 1,1,2-trimethylpropyl group, a 1,1-diethylpropyl group, an isobutyl group, a 1,1-dimethylbutyl group, a 2-pentyl group, Preferred examples of the aryl group include aryl, 3-pentyl, 2-hexyl, 3-hexyl, 2-ethylhexyl, 2-heptyl, 3-heptyl, 4-heptyl, 2-propylheptyl, 2-octyl, 3-nonyl, cyclopropyl, cyclobutyl, cyclopentyl, methylcyclopentyl, cyclohexyl, methylcyclohexyl, cycloheptyl, cyclooctyl, cyclododecyl, 1-adamantyl, 2-adamantyl, and norbornyl groups.

[0042] The hydrocarbon group may further have a substituent, and examples of the substituent include a halogen atom, an epoxy group, an amino group which may be substituted with a hydrocarbon group having 1 to 30 carbon atoms, an alkoxy group having 1 to 30 carbon atoms, an aryloxy group having 6 to 30 carbon atoms, a hydroxyl group, etc. The number of carbon atoms contained in the substituent is not included in the above carbon number. R a The hydrocarbon group in is preferably a hydrocarbon group having 1 to 8 carbon atoms, more preferably a hydrocarbon group having 1 to 6 carbon atoms, and even more preferably an unsubstituted hydrocarbon group having 1 to 6 carbon atoms.

[0043] Suitable specific examples of the ester group having 1 to 30 carbon atoms include a methoxycarbonyl group, an ethoxycarbonyl group, an n-propoxycarbonyl group, an isopropoxycarbonyl group, an n-butoxycarbonyl group, a t-butoxycarbonyl group, a cyclohexyloxycarbonyl group, a 2-ethylhexyloxycarbonyl group, a benzyloxycarbonyl group, and a phenoxycarbonyl group.

[0044] In the general formula (1), the acyloxy group having 1 to 30 carbon atoms is represented by -OCOR b where R b represents a hydrocarbon group having 1 to 30 carbon atoms. The number of carbon atoms in the acyloxy group does not include the number of carbon atoms in the carbonyl group. b The lower limit of the carbon number is 1 or more, and may be 2 or more, and the upper limit of the carbon number is 30 or less, and may be 20 or less, or may be 10 or less. The hydrocarbon group having 1 to 30 carbon atoms is the same as R a The same can be mentioned. Suitable specific examples of the acyloxy group having 1 to 30 carbon atoms include an acetyloxy group, a propionyloxy group, a (meth)acryloyloxy group, and a benzoyloxy group.

[0045] In the general formula (1), the acyl group having 1 to 30 carbon atoms is -COR c where R is a monovalent group represented by the formula: c represents a hydrocarbon group having 1 to 30 carbon atoms. The number of carbon atoms in the acyl group does not include the number of carbon atoms in the carbonyl group. c The lower limit of the carbon number is 1 or more, and may be 2 or more, and the upper limit of the carbon number is 30 or less, and may be 20 or less, or may be 10 or less. R c The hydrocarbon group having 1 to 30 carbon atoms in R a The same can be mentioned. Suitable specific examples of the acyl group having 1 to 30 carbon atoms include an acetyl group, a propionyl group, a (meth)acryloyl group, and a benzoyl group.

[0046] In the general formula (1), the alkoxy group having 1 to 30 carbon atoms is -OR d where R drepresents an alkyl group having 1 to 30 carbon atoms or an aralkyl group having 7 to 30 carbon atoms. The lower limit of the number of carbon atoms in the alkoxy group may be 1 or more, or may be 2 or more, and the upper limit may be 30 or less, or may be 20 or less, or may be 10 or less. R d The alkyl group having 1 to 30 carbon atoms and the aralkyl group having 7 to 30 carbon atoms in R a The same can be mentioned. Suitable specific examples of the alkoxy group having 1 to 30 carbon atoms include a methoxy group, an ethoxy group, an n-propoxy group, an i-propoxy group, an n-butoxy group, an i-butoxy group, an s-butoxy group, a t-butoxy group, an n-pentoxy group, an n-hexoxy group, a cyclopropoxy group, a cyclopentoxy group, a cyclohexyloxy group, an n-octoxy group, an n-deoxy group, and a benzyloxy group. In addition, an aryloxy group having 6 to 30 carbon atoms is represented by -OR d’ where R d’ represents an aryl group having 6 to 30 carbon atoms. The lower limit of the number of carbon atoms in the aryl group may be 6 or more, or may be 8 or more, and the upper limit may be 30 or less, or may be 20 or less, or may be 12 or less. R d’ The aryl group having 6 to 30 carbon atoms in R a Among these, those corresponding to aryl groups having 6 to 30 carbon atoms can be mentioned. Specific examples of the aryloxy group having 6 to 30 carbon atoms include a phenoxy group, a methylphenoxy group, an ethylphenoxy group, a butylphenoxy group, a naphthyloxy group, a fluorenyloxy group, and an anthracenyloxy group.

[0047] In the general formula (1), the alkylthio group having 1 to 30 carbon atoms is -SR e where R erepresents an alkyl group having 1 to 30 carbon atoms or an aralkyl group having 7 to 30 carbon atoms. The lower limit of the number of carbon atoms in the alkylthio group may be 1 or more, or may be 2 or more, and the upper limit may be 30 or less, or may be 20 or less, or may be 10 or less. R e The alkyl group having 1 to 30 carbon atoms and the aralkyl group having 7 to 30 carbon atoms in R a The same can be mentioned. Suitable specific examples of the alkylthio group having 1 to 30 carbon atoms include a methylthio group, an ethylthio group, and a benzylthio group.

[0048] An arylthio group having 6 to 30 carbon atoms is represented by -SR e’ where R e’ represents an aryl group having 6 to 30 carbon atoms. The lower limit of the number of carbon atoms in the aryl group may be 6 or more, or may be 8 or more, and the upper limit may be 30 or less, or may be 20 or less, or may be 12 or less. R e’ The aryl group having 6 to 30 carbon atoms in R a Among these, those corresponding to aryl groups having 6 to 30 carbon atoms can be mentioned. Specific examples of the arylthio group having 6 to 30 carbon atoms include a phenylthio group and a naphthylthio group.

[0049] In the general formula (1), the amino group which may be substituted with at least one hydrocarbon group having 1 to 30 carbon atoms is represented by -N(R f )R g where R f and R g each independently represents a hydrogen atom or a hydrocarbon group having 1 to 30 carbon atoms. The lower limit of the number of carbon atoms in the hydrocarbon group substituted by the substituted amino group may be 1 or more, or may be 2 or more, and the upper limit may be 30 or less, or may be 20 or less, or may be 10 or less. R f and R gThe hydrocarbon group having 1 to 30 carbon atoms in R a The same can be mentioned. Suitable specific examples of the amino group which may be substituted with a hydrocarbon group having 1 to 30 carbon atoms include an amino group (-NH2), a monomethylamino group, a dimethylamino group, a monoethylamino group, a diethylamino group, a monoisopropylamino group, a diisopropylamino group, a monophenylamino group, and a diphenylamino group.

[0050] In the general formula (1), the silyl group which may be substituted with at least one hydrocarbon group having 1 to 30 carbon atoms is represented by -SiR h R i R j where R h , R i and R j each independently represents a hydrogen atom or a hydrocarbon group having 1 to 30 carbon atoms. The lower limit of the number of carbon atoms in the hydrocarbon group substituted with the silyl group may be 1 or more, or may be 2 or more, and the upper limit may be 30 or less, or may be 20 or less, or may be 10 or less. R h , R i and R j The hydrocarbon group having 1 to 30 carbon atoms in R a The same can be mentioned. Suitable specific examples of the silyl group which may be substituted with a hydrocarbon group having 1 to 30 carbon atoms include a trimethylsilyl group, a triethylsilyl group, a tert-butyldimethylsilyl group, a triisopropylsilyl group, and a tert-butyldiphenylsilyl group.

[0051] In the general formula (1), the amide group which may be substituted with at least one hydrocarbon group having 1 to 30 carbon atoms is -CONR k R l or -NR k COR l where R k and R leach independently represents a hydrogen atom or a hydrocarbon group having 1 to 30 carbon atoms. The number of carbon atoms in the hydrocarbon group substituted by the substituted amide group does not include the number of carbon atoms in the carbonyl group, and k and R l The lower limit of the carbon number is 1 or more, and may be 2 or more, and the upper limit of the carbon number is 30 or less, and may be 20 or less, or may be 10 or less. R k and R l The hydrocarbon group having 1 to 30 carbon atoms in R a The same can be mentioned. Specific examples of the amide group which may be substituted with a hydrocarbon group having 1 to 30 carbon atoms include, for example, -CONH2, -CONH(CH3), -CON(CH3)2, -CONH(C2H5), -CON(C2H5)2, -CONH(i-C3H7), -CON(i-C3H7)2, -CONH(Ph), -CON(Ph)2, -NHCOCH3, -NHCOC2H5, etc. In this specification, Ph represents a phenyl group.

[0052] In the general formula (1), the hydrocarbon group having 1 to 30 carbon atoms and substituted with at least one halogen atom (halogen-substituted hydrocarbon group having 1 to 30 carbon atoms) is a group in which at least one hydrogen atom is substituted with a halogen atom. The hydrocarbon group having 1 to 30 carbon atoms is a group in which at least one hydrogen atom is substituted with a halogen atom. a Among them, an alkyl group and an aryl group are preferable from the viewpoint of availability. Examples of the halogen atom include a fluorine atom, a chlorine atom, a bromine atom, and an iodine atom. The lower limit of the number of carbon atoms in the halogen-substituted hydrocarbon group having 1 to 30 carbon atoms may be 1 or more, or may be 2 or more, and the upper limit may be 30 or less, or may be 20 or less, or may be 10 or less. Specific examples of the halogen-substituted hydrocarbon group having 1 to 30 carbon atoms include a halomethyl group in which 1 to 3 hydrogen atoms of a methyl group are substituted with halogen atoms, a chloroethyl group, a γ-chloropropyl group, a 3,3′,3″-trifluoropropyl group, a perfluoropropyl group, a perfluorophenyl group, a bromophenyl group, a chlorophenyl group, a fluorophenyl group, a dichlorophenyl group, etc., and examples of the halomethyl group include a chloromethyl group, a bromomethyl group, a fluoromethyl group, a dichloromethyl group, a trifluoromethyl group, etc.

[0053] In the general formula (1), the hydrocarbon group having 1 to 30 carbon atoms which may be substituted with at least one substituent selected from the group consisting of an oxygen atom, a sulfur atom, and a nitrogen atom is preferably a hydrocarbon group having 1 to 30 carbon atoms, and more preferably a hydrocarbon group having 1 to 30 carbon atoms, and more preferably a hydrocarbon group having 1 to 30 carbon atoms, and more preferably a hydrocarbon group having 1 to 30 carbon atoms, and further ... a As the hydrocarbon group having 1 to 30 carbon atoms which may be substituted with at least one substituent selected from the group consisting of an oxygen atom, a sulfur atom, and a nitrogen atom, among others, an alkyl group, an alkenyl group, an aryl group, or an aralkyl group is preferred in terms of production efficiency of the copolymer. Suitable specific examples of the unsubstituted hydrocarbon group having 1 to 30 carbon atoms include a methyl group, an ethyl group, a 1-propyl group, a 1-butyl group, a 1-pentyl group, a 1-hexyl group, an isopropyl group, an isobutyl group, a t-butyl group, a cyclopentyl group, a cyclohexyl group, an ethenyl group, a propenyl group, a butenyl group, and a phenyl group.

[0054] In general formula (1), the number of carbon atoms in the heterocyclic group which may be substituted with a substituent containing at least one selected from the group consisting of an oxygen atom, a sulfur atom, and a nitrogen atom is, for example, 2 or more, and the upper limit may be 8 or less, may be 6 or less, or may be 5 or less. Specific examples of the heterocyclic group include a pyridyl group, a furanyl group, a thienyl group, an oxazoyl group, an oxazolidinyl group, an isoxazolidinyl group, a thiazolyl group, a dihydrofuranyl group, and a tetrahydrofuranyl group.

[0055] Examples of the substituent containing at least one selected from the group consisting of an oxygen atom, a sulfur atom, and a nitrogen atom include a hydroxyl group, a formyl group, a carboxy group, an epoxy group, an ester group having 1 to 30 carbon atoms, an acyloxy group having 1 to 30 carbon atoms, an acyl group having 1 to 30 carbon atoms, an alkoxy group having 1 to 30 carbon atoms, an aryloxy group having 6 to 30 carbon atoms, a cyano group, a nitro group, an amino group which may be substituted with a hydrocarbon group having 1 to 30 carbon atoms, an amido group which may be substituted with a hydrocarbon group having 1 to 30 carbon atoms, an alkylthio group having 1 to 30 carbon atoms, an arylthio group having 6 to 30 carbon atoms, a sulfonyl group having 1 to 30 carbon atoms, a sulfoxide group having 1 to 30 carbon atoms, and a sulfonate ester group having 1 to 30 carbon atoms. The ester group having 1 to 30 carbon atoms, the acyloxy group having 1 to 30 carbon atoms, the acyl group having 1 to 30 carbon atoms, the alkoxy group having 1 to 30 carbon atoms, the aryloxy group having 6 to 30 carbon atoms, the amino group which may be substituted with a hydrocarbon group having 1 to 30 carbon atoms, the amide group which may be substituted with a hydrocarbon group having 1 to 30 carbon atoms, the alkylthio group having 1 to 30 carbon atoms, and the arylthio group having 6 to 30 carbon atoms may be the same as described above.

[0056] The sulfonyl group having 1 to 30 carbon atoms is -SOR m where R m represents a hydrocarbon group having 1 to 30 carbon atoms. The lower limit of the number of carbon atoms in the sulfonyl group may be 1 or more, or may be 2 or more, and the upper limit may be 30 or less, or may be 20 or less, or may be 10 or less. R m The hydrocarbon group having 1 to 30 carbon atoms in R a The same can be mentioned. Specific examples of the sulfonyl group having 1 to 30 carbon atoms include, for example, -SO2CH3 and -SO2Ph.

[0057] The sulfoxide group having 1 to 30 carbon atoms is -SOR n where R nrepresents a hydrocarbon group having 1 to 30 carbon atoms. With respect to the number of carbon atoms in the sulfoxide group, the lower limit may be 1 or more, or may be 2 or more, and the upper limit may be 30 or less, or may be 20 or less, or may be 10 or less. R n The hydrocarbon group having 1 to 30 carbon atoms in R a The same can be mentioned. Suitable specific examples of the sulfoxide group having 1 to 30 carbon atoms include -SOCH3 and -SOPh.

[0058] The sulfonic acid ester group having 1 to 30 carbon atoms is -OSO2R o where R o represents a hydrocarbon group having 1 to 30 carbon atoms. The lower limit of the number of carbon atoms in the sulfonate ester group may be 1 or more, or may be 2 or more, and the upper limit may be 30 or less, or may be 20 or less, or may be 10 or less. R o The hydrocarbon group having 1 to 30 carbon atoms in R a The same can be mentioned. Specific examples of the sulfonate group having 1 to 30 carbon atoms include, for example, -OSO2CH3 and -OSO2Ph.

[0059] From the viewpoint of production efficiency of the copolymer, the substituent containing at least one selected from the group consisting of an oxygen atom, a sulfur atom, and a nitrogen atom is preferably at least one selected from the group consisting of a hydroxyl group, an alkoxy group having 1 to 30 carbon atoms, an aryloxy group having 6 to 30 carbon atoms, an amino group which may be substituted with a hydrocarbon group having 1 to 30 carbon atoms, an alkylthio group having 1 to 30 carbon atoms, and an arylthio group having 6 to 30 carbon atoms, and more preferably at least one selected from the group consisting of an alkoxy group having 1 to 30 carbon atoms, an aryloxy group having 6 to 30 carbon atoms, and an amino group which may be substituted with a hydrocarbon group having 1 to 30 carbon atoms.

[0060] In general formula (1), R 1 and R2 are combined with each other to form R 1 and R 2 R may form a 4- to 10-membered ring together with the unsaturated bond to which it is bonded, or may form a 5- or 6-membered ring. 1 and R 2 The ring formed by bonding with each other may be a carbocyclic or heterocyclic ring, and the carbocyclic or heterocyclic ring may be a monocyclic or polycyclic ring. 1 and R 2 may be bonded to each other to form a saturated or unsaturated bond, or may form a -CO-O-CO- group, and may be a non-aromatic ring.

[0061] In the structural unit (B), the R 1 and R 2 at least one of which may be a substituent other than a hydrogen atom, is a halogen atom, a hydroxyl group, a formyl group, a carboxy group, an ester group having 1 to 30 carbon atoms, an acyloxy group having 1 to 30 carbon atoms, an acyl group having 1 to 30 carbon atoms, an alkoxy group having 1 to 30 carbon atoms, an aryloxy group having 6 to 30 carbon atoms, an alkylthio group having 1 to 30 carbon atoms, an arylthio group having 6 to 30 carbon atoms, a nitro group, an amino group which may be substituted with at least one hydrocarbon group having 1 to 30 carbon atoms, a silyl group which may be substituted with at least one hydrocarbon group having 1 to 30 carbon atoms, an amide group which may be substituted with at least one hydrocarbon group having 1 to 30 carbon atoms, a hydrocarbon group having 1 to 30 carbon atoms substituted with at least one halogen atom, or a hydrocarbon group or heterocyclic group having 1 to 30 carbon atoms which may be substituted with at least one substituent containing at least one type selected from the group consisting of an oxygen atom, a sulfur atom, and a nitrogen atom, or R 1 and R 2 may be bonded to each other to form a 4- to 10-membered ring. In addition, R in the general formula (1) 1 and R 2 may be the same or different.

[0062] On the other hand, in the structural unit (B), from the viewpoint of polymerization activity, the R 1 and R 2 may be a hydrogen atom, and 1 and R 2 However, each of them may be a hydrogen atom.

[0063] At least one monomer (monomer (B)) represented by the above general formula (1) from which the structural unit (B) is derived includes, for example, the following monomers, but is not limited thereto.

[0064] [ka]

[0065] The monomer (B) can be produced by appropriately combining conventionally known production methods. 1 and R 2 When at least one of the substituents is a substituent other than a hydrogen atom, for example, a silver-catalyzed cyclization reaction of propargyl alcohol with carbon dioxide, or a reaction using an acyloin and a carbonylating agent such as phosgene can be used to introduce the substituent. Substituents can also be introduced by referring to Synlett (2014), 25, P1178-1180., Tetrahedron Lett. (1972), 17, P1701-1704., and Adv. Synth. Catal. (2021), 363, P5129-5137. As the one monomer (B), a commercially available product may be used. The monomer (B) may be used in combination of two or more kinds.

[0066] The structural unit (B) derived from at least one monomer represented by general formula (1) preferably contains a structural unit represented by the following general formula (I), or a structural unit represented by the following general formula (I) and a structural unit represented by the following general formula (II).

[0067] [ka] (In formula (I) and formula (II), R 1 and R 2 are each independently as defined above.)

[0068] Furthermore, the structural unit (B) may contain an aldehyde structure contained at the polymer chain end. The aldehyde structure is presumed to be generated by the transfer and insertion of vinylene carbonate, followed by β-carbonate elimination, followed by decarboxylation and protonation. The presumed generation mechanism of the aldehyde structure is shown below. In the following scheme, M and Q are the same as those in formula (101) described later. In addition, the structural unit (B) is R 1 and R 2 When at least one of these is not a hydrogen atom, the polymer may contain a ketone structure at the end of the polymer chain.

[0069] [ka]

[0070] (3) Structural unit (C) The structural unit (C) is a structural unit derived from at least one type of monomer represented by the following general formula (2).

[0071] [ka] (In formula (2), R 3 is a hydrogen atom, a halogen atom, a hydrocarbon group having 1 to 10 carbon atoms substituted with at least one halogen atom, or a hydrocarbon group having 1 to 10 carbon atoms. R 4 is a hydrogen atom, a silyl group which may be substituted with at least one hydrocarbon group having 1 to 30 carbon atoms, a hydrocarbon group having 1 to 30 carbon atoms which is substituted with at least one halogen atom, or a hydrocarbon group or heterocyclic group having 1 to 30 carbon atoms which may be substituted with at least one substituent containing at least one of an oxygen atom, a sulfur atom, or a nitrogen atom.

[0072] R in Equation (2) 3 In the formula (1), examples of the halogen atom include the same as those described in the formula (1). Examples of the hydrocarbon group having 1 to 10 carbon atoms and substituted with at least one halogen atom include the same as those of the hydrocarbon group having 1 to 30 carbon atoms and substituted with at least one halogen atom described in the formula (1) having 1 to 10 carbon atoms. Examples of the hydrocarbon group having 1 to 10 carbon atoms include the same as those of the hydrocarbon group having 1 to 30 carbon atoms and substituted with at least one halogen atom described in the formula (1).

[0073] R in Equation (2) 3 may be a hydrogen atom, a halogen atom, or a hydrocarbon group having 1 to 3 carbon atoms substituted with at least one halogen atom, or a hydrocarbon group having 1 to 3 carbon atoms, or may be a hydrogen atom, a halogen atom, a trifluoromethyl group, or a methyl group, or may be a hydrogen atom or a methyl group, in terms of polymerization activity and comonomer content.

[0074] R in Equation (2) 4 In the above, examples of the silyl group which may be substituted with at least one hydrocarbon group having 1 to 30 carbon atoms, the hydrocarbon group having 1 to 30 carbon atoms which is substituted with at least one halogen atom, and the hydrocarbon group or heterocyclic group having 1 to 30 carbon atoms which may be substituted with at least one substituent containing at least one of an oxygen atom, a sulfur atom, or a nitrogen atom are the same as those explained in relation to the above formula (1).

[0075] R in Equation (2) 4may be a hydrogen atom, a silyl group which may be substituted with at least one hydrocarbon group having 1 to 6 carbon atoms, a hydrocarbon group having 1 to 6 carbon atoms substituted with at least one halogen atom, or a hydrocarbon group or heterocyclic group having 1 to 6 carbon atoms which may be substituted with at least one substituent containing at least one of an oxygen atom, a sulfur atom, or a nitrogen atom, or may be a hydrocarbon group having 1 to 6 carbon atoms.

[0076] At least one monomer (monomer (C)) represented by the above general formula (2) from which the structural unit (C) is derived includes, for example, the following monomers, but is not limited thereto.

[0077] [ka]

[0078] [ka]

[0079] The monomer (C) can be produced by appropriately combining conventionally known production methods. For example, it can be synthesized by the Reppe method in which acetylene is reacted with carbon monoxide and methanol is added. 4 Generally, it can be replaced by transesterification. Substituents can also be introduced by referring to Organometallics (2016), 35, P943-949., J. Org. Chem. (1989), 54, P1006-1012., and Tetrahedron Lett.(2018), 59, P3279-3282. As the monomer (C), a commercially available product may be used. The monomer (C) may be used in combination of two or more kinds.

[0080] The structural unit (C) derived from at least one monomer represented by general formula (2) preferably contains at least one structural unit represented by the following general formula (III).

[0081] [ka] (In formula (III), R 3 and R 4 is the same as above.)

[0082] (4) Other structural units The polar group-containing olefin copolymer of the present invention may further contain other structural units different from the structural unit (A), the structural unit (B) and the unit structure (C). Examples of the other structural units include structural units derived from other polar group-containing monomers such as vinyl acetate, allyl acetate, 3-butenyl acetate, acrylonitrile, 3-cyanopropene and vinyl ether.

[0083] (5) Polar group-containing olefin copolymer The polar group-containing olefin copolymer of the present invention contains a structural unit (A) derived from at least one olefin having 2 to 20 carbon atoms, a structural unit (B) derived from at least one monomer represented by the following general formula (1), and a structural unit (C) derived from at least one monomer represented by the following general formula (2). The polar-group-containing olefin copolymer of the present invention must contain at least one type of each of the structural unit (A), the structural unit (B) and the unit structure (C), and must contain structural units derived from a total of three or more types of monomers.

[0084] In the present invention, the ratio of the structural unit (A) in the polar group-containing olefin copolymer may be appropriately selected according to the desired physical properties, but the lower limit is usually 60.00 mol%, may be 70.00 mol%, may be 80.00 mol%, may be 90.00 mol%, may be 95.00 mol%, may be 96.00 mol%, may be 97.00 mol%, or may be 98.00 mol%, based on the total structural units of 100 mol%. On the other hand, the upper limit is usually 99.98 mol%, may be 99.95 mol%, may be 99.92 mol%, may be 99.90 mol%, may be 99.80 mol%, may be 99.60 mol%, may be 99.50 mol%, may be 99.20 mol%, may be 99.00 mol%, or may be 98.20 mol%.

[0085] The proportion of the structural unit (B) in the polar group-containing olefin copolymer may be appropriately selected according to the average molecular weight and the desired physical properties, but the lower limit is usually 0.01 mol%, may be 0.05 mol%, may be 0.10 mol%, may be 0.20 mol%, may be 0.25 mol%, may be 0.30 mol%, may be 0.50 mol%, or may be 1.00 mol%, based on 100 mol% of the total structural units. On the other hand, the upper limit is usually 10.00 mol%, may be 5.00 mol%, may be 4.80 mol%, may be 3.00 mol%, or may be 2.00 mol%.

[0086] The proportion of the structural unit (C) in the polar group-containing olefin copolymer may be appropriately selected according to the average molecular weight and the desired physical properties, and the lower limit is usually 0.01 mol%, may be 0.05 mol%, may be 0.10 mol%, may be 0.25 mol%, may be 0.50 mol%, or may be 0.80 mol%, based on 100 mol% of the total structural units. On the other hand, the upper limit is usually 30.00 mol%, may be 20.00 mol%, may be 15.00 mol%, may be 10.00 mol%, may be 5.00 mol%, may be 4.50 mol%, may be 2.50 mol%, or may be 2.00 mol% or less.

[0087] The combination of the structural units may be 80.00 to 99.20 mol% for the structural unit (A), 0.30 to 10.00 mol% for the structural unit (B), and 0.50 to 10.00 mol% for the structural unit (C), or may be 90.00 to 99.5 mol% for the structural unit (A), 0.25 to 5.00 mol% for the structural unit (B), and 0.25 to 5.00 mol% for the structural unit (C). Furthermore, the structural units (A) may be 90.00 to 99.20 mol%, the structural units (B) may be 0.30 to 5.00 mol%, and the structural units (C) may be 0.50 to 5.00 mol%.

[0088] The polar group-containing olefin copolymer of the present invention may further contain one or more other structural units. When the polar group-containing olefin copolymer of the present invention contains other structural units, the ratio of the other structural units in the polar group-containing olefin copolymer may be appropriately selected according to the desired physical properties, but the lower limit is usually 0.01 mol%, may be 0.05 mol%, may be 0.10 mol%, or may be 0.50 mol%, based on 100 mol% of the total structural units. On the other hand, the upper limit is usually 35.00 mol%, may be 30.00 mol%, may be 20.00 mol%, or may be 10.00 mol%.

[0089] A structure derived from one molecule of each monomer is defined as one structural unit in the polar group-containing olefin copolymer. The amount of structural units is the ratio of each structural unit expressed in mol % when the total structural units in the polar group-containing olefin copolymer is taken as 100 mol %.

[0090] The polar group-containing olefin copolymer of the present invention may be a random copolymer, block copolymer, graft copolymer, etc., of the structural unit (A), the structural unit (B), the structural unit (C), and other structural units contained as necessary. Among these, a random copolymer that can contain a large amount of the structural unit (B) and the structural unit (C) may be used.

[0091] The amount of structural units can be controlled by the selection of catalyst, the amount of monomer (A), monomer (B), monomer (C) and other monomers added during polymerization, and the pressure and temperature during polymerization. Specific means for increasing the amount of structural units derived from monomer (B) and monomer (C) in the copolymer include increasing the amount of monomer (B) and monomer (C) added during polymerization, selecting a catalyst, reducing the olefin pressure during polymerization, and increasing the polymerization temperature. For example, it is necessary to adjust these factors to control the copolymer to the desired region.

[0092] The amount of structural units in the polar group-containing olefin copolymer of the present invention is 1 H-NMR spectrum and 13 The C-NMR spectrum can be measured by the method described in the Examples. Furthermore, the presence of polar groups such as the structural units (B) and (C) in the polar-group-containing olefin copolymer of the present invention can also be confirmed by analyzing the IR spectrum.

[0093] The weight average molecular weight (Mw) of the polar group-containing olefin copolymer in the present invention is usually in the range of 1,000 to 2,000,000, preferably 10,000 to 1,500,000, more preferably 10,000 to 1,000,000, suitably 10,000 to 800,000, and even more suitably 5,000 to 600,000. When Mw is equal to or greater than the lower limit, physical properties such as mechanical strength and impact resistance tend to be sufficient, while when Mw is equal to or less than the upper limit, molding is easy in terms of melt viscosity.

[0094] The number average molecular weight (Mn) of the polar group-containing olefin copolymer of the present invention is usually in the range of 1,000 to 2,000,000, preferably 3,000 to 1,500,000, more preferably 3,000 to 1,000,000, more preferably 3,000 to 800,000, and even more preferably 3,000 to 600,000. When Mn is equal to or greater than the lower limit, physical properties such as mechanical strength and impact resistance tend to be sufficient, and when Mn is equal to or less than the upper limit, molding is easy in terms of melt viscosity.

[0095] The ratio of Mw to Mn (Mw / Mn) of the polar group-containing olefin copolymer of the present invention is usually in the range of 1.0 to 4.0, preferably 1.3 to 3.5, and more preferably 1.4 to 3.3. If Mw / Mn is 1.0 or more, various processabilities including molding tend to be sufficient, and if it is 4.0 or less, the mechanical properties tend to be good. In the present invention, Mw / Mn may be expressed as a molecular weight distribution parameter.

[0096] In the present invention, the weight average molecular weight (Mw) and the number average molecular weight (Mn) are determined by gel permeation chromatography (GPC). The GPC measurement in the present invention can be specifically performed by the method described in the Examples.

[0097] The polar group-containing olefin copolymer of the present invention is 13The number of methyl branches calculated by C-NMR is preferably 50 or less per 1,000 carbon atoms. Of these, the number of methyl branches is particularly preferably 5 or less per 1,000 carbon atoms. When the number of methyl branches satisfies this value, the elastic modulus is high and the mechanical strength of the molded article is also high. The number of methyl branches can be controlled by selecting the transition metal catalyst to be used or adjusting the polymerization temperature. As a specific means for reducing the number of methyl branches of the polar group-containing olefin copolymer of the present invention, lowering the polymerization temperature is effective. In order to reduce the number of methyl branches, for example, it is required to adjust these factors to control it to the desired copolymer region.

[0098] The number of methyl branches is as described in [Structure of Polar Group-Containing Olefin Copolymer] in the Examples section described later. 13 Using the C-NMR spectrum, the calculation is performed as follows: 13 The sum of the integrated intensities of the signals from methyl carbons in the range of 20.0 to 19.8 ppm, methine carbons in the range of 33.2 to 33.0 ppm, and methylene carbons in the range of 37.5 to 37.3 ppm in the C-NMR spectrum divided by 4 is I (B1) The number of methyl branches per total of 1,000 carbon atoms (total 1000C) is calculated using the following formula:

[0099] Number of methyl branches (number / total 1000C) = I (B1) ×1000 / I (トータル) Here, I (B1) , I (トータル) are the quantities shown in the following formulas, respectively. I (B1) =(I 20.0~19.8 +I 33.2~33.0 +I 37.5~37.3 ) / 4 I (トータル) =I 180.0~135.0 +I 120.0~2.0 Note that I is the integrated intensity, and the subscripts of I indicate the range of chemical shifts. For example, I 180.0~135.0 indicates the integrated intensity of the signal detected between 180.0 ppm and 135.0 ppm.

[0100] (6) Method for producing polar group-containing olefin copolymer (6-1) Catalyst The polar group-containing olefin copolymer of the present invention may be polymerized in the presence of a catalyst containing a transition metal, from the viewpoint of introducing at least one of the monomers (B) and (C) into the main chain of an olefin polymer having two or more carbon atoms in a one-step polymerization reaction, and from the viewpoint of making the molecular structure of the copolymer linear. The catalyst containing a transition metal is not particularly limited as long as it can be polymerized with at least one of the monomers (B), (C), and (A). For example, a transition metal compound of Groups 5 to 11 of the periodic table having a chelating ligand can be used.

[0101] Specific examples of preferred transition metals include vanadium, niobium, tantalum, chromium, molybdenum, tungsten, manganese, iron, platinum, ruthenium, cobalt, rhodium, nickel, palladium, and copper. Among these, preferred are transition metals of Groups 8 to 11, more preferred are transition metals of Group 10, and examples of the transition metals of Group 10 include nickel, palladium, and platinum, and particularly preferred are nickel (Ni) and palladium (Pd). These metals may be used alone or in combination.

[0102] Chelating ligands have at least two atoms selected from the group consisting of P, N, O, and S, and include ligands that are bidentate or multidentate, and are electronically neutral or anionic. Exemplary structures are given in the review by Brookhart et al. (Chem. Rev., 2000, 100, 1169). Preferred are bidentate anionic P,O ligands such as phosphorus sulfonates, phosphorus carboxylates, phosphorus phenoxides, phosphorus alkoxides, phosphorus enolates, and other bidentate anionic N,O ligands such as pyridine carboxylates, and other diimine, diphenoxide, and diamide ligands.

[0103] As the catalyst containing a transition metal, from the viewpoints of the production efficiency of the polymer, the molecular weight of the polymer, and the copolymerizability of the monomer (A) with the monomer (B) and the monomer (C), a catalyst containing a late transition metal selected from the group consisting of Group 8 to Group 10 transition metals is preferred, and among these, a catalyst containing a Group 10 transition metal is preferred, and further, a catalyst containing a Group 10 transition metal and having a chelating ligand containing one or more phosphorus atoms as a coordination point to the Group 10 transition metal is preferred.

[0104] As the catalyst containing a transition metal, in terms of the production efficiency of the polymer, the molecular weight of the polymer, and the copolymerizability of the monomer (A) with the monomer (B) and the monomer (C), it is particularly preferable that the catalyst containing a Group 10 transition metal is at least one kind of compound represented by the following general formula (101).

[0105] [ka] [In general formula (101), M represents a metal atom of Group 10 of the periodic table. Q represents an oxygen atom, a sulfur atom, -S(=O)2-O-, or -C(=O)-O-, and the left side of each of these groups is bonded to A and the right side is bonded to M. A represents a divalent hydrocarbon group having 1 to 30 carbon atoms which may have a substituent. R L represents a hydrogen atom, a hydrocarbon group having 1 to 20 carbon atoms which may contain a hetero atom, or a ligand coordinated to M. L represents a ligand coordinated to M. R x and R y each independently represents a hydrogen atom or a hydrocarbon group having 1 to 20 carbon atoms which may contain a heteroatom. R L and L and R x and R y may form a ring, R x and A or R y and A may form a ring.

[0106] In the general formula (101), M represents a metal atom of Group 10 of the periodic table, and among these, Ni or Pd is preferable. Q represents a divalent group represented by -S(=O)2-O-, -C(=O)-O-, -O-, or -S-, and is a site that coordinates one electron to M. The left side of each of the groups is bonded to A, and the right side is bonded to M. Among these, from the viewpoint of catalytic activity, Q is preferably -S(=O)2-O- or -O-, and particularly preferably -O-.

[0107] A is a divalent hydrocarbon group having 1 to 30 carbon atoms which links Q to the phosphorus atom and which may have a substituent. The divalent hydrocarbon group having 1 to 30 carbon atoms may be a divalent hydrocarbon group having 1 to 20 carbon atoms, and preferred examples thereof include an alkylene group, an arylene group, and a combination thereof. For example, the following formulas (a-1) to (a-7) are included. 101 )2] n n in - is an integer of 1 to 3, and -[C(R 101 )2]- indicates the number of repetitions. In the following formula, R 101 each independently represents a hydrogen atom, a hydrocarbon group having 1 to 20 carbon atoms which may have a substituent, or a substituent. 101 Adjacent substituents may be linked to each other to form an alicyclic ring, an aromatic ring, or a heterocyclic ring containing at least one heteroatom selected from the group consisting of an oxygen atom, a nitrogen atom, and a sulfur atom, in which case the ring has 5 to 8 members and may have a substituent on the ring.

[0108] R 101 The hydrocarbon group having 1 to 20 carbon atoms is R a Among these, the same hydrocarbon groups having 1 to 20 carbon atoms can be mentioned. Of the hydrocarbon groups having 1 to 20 carbon atoms, hydrocarbon groups having 1 to 15 carbon atoms are preferred, and hydrocarbon groups having 1 to 10 carbon atoms are more preferred. As the divalent hydrocarbon group having 1 to 30 carbon atoms for A, the following formula (a-2) or the following formula (a-7) is preferable in terms of catalytic activity.

[0109] [ka]

[0110] Examples of the substituent in A include a halogen atom, OR β , CO2R β , CO2M', CON(R α ) 2, COR β , O.C.(O)R β , S.R. β , SO2R β , SOR β , OSO2R β , PO(OR β ) 2-y (R α ) y , C.N., N.H.R. β , N(R β )2, Si(OR α ) 3-x (R α ) x , OSi(OR α ) 3-x (R α ) x , NO2, SO3M', PO3M'2, P(O)(OR β ) 2M′, or an epoxy-containing group, etc. (wherein R α represents a hydrogen atom or a hydrocarbon group having 1 to 20 carbon atoms, R β represents a hydrocarbon group having 1 to 20 carbon atoms, M' represents an alkali metal, an alkaline earth metal, ammonium, a quaternary ammonium or a phosphonium, x represents an integer of 0 to 3, and y represents an integer of 0 to 2). The hydrocarbon group having 1 to 20 carbon atoms is R a Among these, the same hydrocarbon groups having 1 to 20 carbon atoms can be mentioned.

[0111] L represents a ligand coordinated to M. L may be a zero-valent ligand that can be removed from the metal atom. L is preferably a compound having an electron-donating group and capable of stabilizing the metal complex by coordinating to the metal atom M. L may be a hydrocarbon compound having 1 to 20 carbon atoms and having at least one of oxygen, nitrogen, and sulfur atoms as an atom capable of coordinating, or a hydrocarbon compound having a carbon-carbon unsaturated bond capable of coordinating to the metal atom M and optionally containing a heteroatom. L preferably has 1 to 16 carbon atoms, more preferably 1 to 10 carbon atoms.

[0112] Preferred examples of L include cyclic unsaturated hydrocarbons, phosphines, pyridines, piperidines, alkyl ethers, aryl ethers, alkylaryl ethers, cyclic ethers, alkylnitrile derivatives, arylnitrile derivatives, alcohols, amides, aliphatic esters, aromatic esters, and amines. L having a sulfur atom includes dimethyl sulfoxide (DMSO). Examples of the nitrogen atom-containing trialkylamine include those having an alkyl group with 1 to 10 carbon atoms, those having an alkyl group with 1 to 10 carbon atoms, those having a dialkylamine, pyridine, 2-methylpyridine (also known as picoline), 2,6-dimethylpyridine (also known as 2,6-lutidine), aniline, 2,6-dimethylaniline, 2,6-diisopropylaniline, N,N,N',N'-tetramethylethylenediamine (TMEDA), 4-(N,N-dimethylamino)pyridine (DMAP), acetonitrile, benzonitrile, quinoline, and 2-methylquinoline. Examples of the oxygen atom-containing diethyl ether, tetrahydrofuran, and 1,2-dimethoxyethane. From the viewpoint of the stability and catalytic activity of the complex, DMSO, pyridine, picoline, 2,6-lutidine, and TMEDA are preferred, and DMSO, picoline, and 2,6-lutidine are more preferred. More preferred examples of L include cyclic olefins, phosphines, pyridines, cyclic ethers, aliphatic esters, and aromatic esters. More preferred examples of L include trialkylphosphines, pyridine, 2,6-lutidine, picolines, R β CO2Rβ (R β The definition of is as described above.

[0113] In the present invention, R L represents a hydrogen atom, a hydrocarbon group having 1 to 20 carbon atoms which may contain a heteroatom, or a ligand coordinated to M. R L When R is a ligand coordinated to M, the same as L can be mentioned, but it may be an anionic ligand rather than a neutral ligand. For example, when the ligand reacts with nickel(0)bis(1,5-cyclooctadiene) (Ni(cod)2) as a transition metal compound, the ligand derived from the transition metal compound is R L and L combine together to form a ring, forming a σ,π-cyclooct-4-enyl group.

[0114] The polymerization reaction in the present invention is carried out by reacting M and R L It is believed that the reaction is initiated by the insertion of an olefin such as ethylene or a copolymerizable monomer thereof into the bond of R L If the number of carbon atoms in R is too large, the initiation reaction tends to be inhibited. L The group preferably has 1 to 16 carbon atoms, excluding the carbon atoms contained in the substituent, and more preferably has 1 to 10 carbon atoms. R L Specific examples of the alkyl group include a hydride group, a methyl group, an ethyl group, an n-propyl group, an isopropyl group, an n-butyl group, an isobutyl group, an n-hexyl group, an n-octyl group, an n-decyl group, an n-dodecyl group, a cyclopentyl group, a cyclohexyl group, a benzyl group, a phenyl group, a p-methylphenyl group, a trimethylsilyl group, a triethylsilyl group, and a triphenylsilyl group. In addition, R L and L may be bonded to each other to form a ring. Examples of such a ring include a σ,π-cyclooct-4-enyl group and an acetylacetonato group, which are also preferred embodiments of the present invention.

[0115] R x and Ry each independently represents a hydrocarbon group having 1 to 30 carbon atoms which may have a substituent. R x and R y The hydrocarbon group having 1 to 30 carbon atoms in the above general formula (1) is a The same can be mentioned. R x and R y The substituent in may be the same as the substituent in A.

[0116] R x and R y is in the vicinity of the metal atom M and exerts steric and / or electronic interactions with the metal atom M. To exert such effects, R x and R y It is preferable that the bulk is large. R x and R y Each of these preferably has 3 to 30 carbon atoms, and more preferably 6 to 20 carbon atoms.

[0117] R x and R y are preferably each independently an alkyl group having 3 to 10 carbon atoms which may have a substituent, a cycloalkyl group having 6 to 20 carbon atoms which may have a substituent, or an aryl group having 6 to 20 carbon atoms which may have a substituent.

[0118] R x and R yThe alkyl group having 3 to 10 carbon atoms which may have a substituent in the formula (I) includes a linear or branched alkyl group having 3 to 10 carbon atoms which may have a substituent. Examples of the alkyl group having 3 to 10 carbon atoms which may have a substituent include a 1-propyl group, a 1-butyl group, a 1-pentyl group, a 1-hexyl group, a 1-heptyl group, a 1-octyl group, a 1-nonyl group, a 1-decyl group, an i-propyl group, a 1-dimethylpropyl group, a 1,1,2-trimethylpropyl group, a 1,1-diethylpropyl group, an i-butyl group, a sec-butyl group, a t-butyl group, a 1,1-dimethylbutyl group, a 2-pentyl group, a 3-pentyl group, a 2-hexyl group, a 3-hexyl group, a 2-ethylhexyl group, a 2-heptyl group, a 3-heptyl group, a 4-heptyl group, a 2-propylheptyl group, a 2-octyl group, a 3-nonyl group, a methoxymethyl group, an ethoxymethyl group, an i-propoxymethyl group, and a t-butoxymethyl group. The alkyl group having 3 to 10 carbon atoms which may have a substituent may be, among others, a branched alkyl group having 3 to 10 carbon atoms which may have a substituent, and may be an i-propyl group, an n-butyl group, an i-butyl group, a sec-butyl group, or a t-butyl group.

[0119] R x and R y Examples of the cycloalkyl group having 6 to 20 carbon atoms which may have a substituent include a cyclohexyl group, a cycloheptyl group, a cyclooctyl group, an adamantyl group, and the like which may be substituted with a linear or branched alkyl group having 3 to 10 carbon atoms which may contain a hetero atom. Also, it may be, for example, a cycloalkyl group described in paragraphs

[0104] to

[0113] of JP2018-141138A (X in paragraphs

[0104] to

[0113] of JP2018-141138A indicates the bonding position of P (phosphorus atom) in general formula (101) of the present invention). The cycloalkyl group having 6 to 20 carbon atoms which may have a substituent may be, among others, a cyclohexyl group or an adamantyl group substituted with a linear or branched alkyl group having 3 to 10 carbon atoms, and may be a 2-isopropyl-5-methylcyclohexyl group (menthyl group) or an adamantyl group.

[0120] R x and R y Among these, from the viewpoints of controlling the molecular weight of the polymer and controlling the copolymerizability with a polar monomer, it is more preferable that the alkyl group is an aryl group having 6 to 20 carbon atoms which may have a substituent.

[0121] R x and R y In the above, examples of the aryl group having 6 to 20 carbon atoms and which may have a substituent include a phenyl group, a naphthyl group, an anthracenyl group, etc., which may be substituted with a linear or branched alkyl group having 3 to 10 carbon atoms and which may contain a hetero atom. The aryl group having 6 to 20 carbon atoms preferably has a branched alkyl group having 3 to 6 carbon atoms, a silyl group substituted with a hydrocarbon group having 1 to 6 carbon atoms, or a substituent containing at least one of an oxygen atom and a nitrogen atom, and more preferably has a substituent containing at least one of an oxygen atom and a nitrogen atom. When the aryl group having 6 to 20 carbon atoms has a substituent containing at least one of an oxygen atom and a nitrogen atom, the substituent is preferably substituted at the ortho position relative to the carbon bonded to phosphorus in the aryl group. x and R y This is because at least one of the oxygen atom and the nitrogen atom in the aryl group can be spatially arranged so as to have an interaction with the metal atom M.

[0122] Preferred R x and R ySpecific examples of the aryl group include an i-propyl group, an n-butyl group, an i-butyl group, a sec-butyl group, a t-butyl group, a cyclohexyl group, a cycloheptyl group, a cyclooctyl group, a 2-isopropyl-5-methylcyclohexyl group, an adamantyl group, a phenyl group, a 2,6-dimethoxyphenyl group, a 2,4,6-trimethoxyphenyl group, a 2,6-di-t-butylphenyl group, a 2,4,6-tri-t-butylphenyl group, a 2,6-ditrimethylsilylphenyl group, a 4-methyl-2,6-dimethoxyphenyl group, a 4-t-butyl-2,6-dimethoxyphenyl group, 1,3-dimethoxy-2-naphthyl group, 2,6-diethoxyphenyl group, 2,4,6-triethoxyphenyl group, 4-methyl-2,6-diethoxyphenyl group, 4-t-butyl-2,6-diethoxyphenyl group, 1,3-diethoxy-2-naphthyl group, 2,6-diphenoxyphenyl group, 2,4,6-triphenoxyphenyl group, 4-methyl-2,6-diphenoxyphenyl group, 4-t-butyl-2,6-diphenoxyphenyl group, 1,3-diphenoxy-2-naphthyl group, 2,6-dimethoxymethylphenyl group, 2,4,6-trimethoxyphenyl group dimethylphenyl group, 4-methyl-2,6-dimethoxymethylphenyl group, 4-t-butyl-2,6-dimethoxymethylphenyl group, 1,3-dimethoxymethyl-2-naphthyl group, 2,6-diphenoxymethylphenyl group, 2,4,6-triphenoxymethylphenyl group, 4-methyl-2,6-diphenoxymethylphenyl group, 4-t-butyl-2,6-diphenoxymethylphenyl group, 1,3-diphenoxymethyl-2-naphthyl group, 2,6-di(2-methoxyethyl)phenyl group, 2,4,6-tri(2-methoxyethyl)phenyl group , 4-methyl-2,6-di(2-methoxyethyl)phenyl group, 4-t-butyl-2,6-di(2-methoxyethyl)phenyl group, 1,3-di(2-methoxyethyl)-2-naphthyl group, 2,6-di(2-phenoxyethyl)phenyl group, 2,4,6-tri(2-phenoxyethyl)phenyl group, 4-methyl-2,6-di(2-phenoxyethyl)phenyl group, 4-t-butyl-2,6-di(2-phenoxyethyl)phenyl group, 1,3-di(2-phenoxyethyl)-2-naphthyl group, and groups represented by the following chemical formulas. Among these, 2,6-dimethoxyphenyl group is preferred.

[0123] [ka] (In the chemical formula, * indicates the position of binding to the phosphorus atom.)

[0124] R x and R y may be bonded to A to form a ring structure. Specific examples of such structures include those described in paragraphs 0120 to 0121 of JP 2018-141138 A (the examples here are the R x or R y R corresponds to one of 16 and A are bonded to form a ring structure, and P and Q have the same meanings as in the general formula (101) of the present invention.

[0125] Among the compounds represented by general formula (101) of the present invention, a compound represented by the following general formula (102) or a compound represented by the following general formula (103) is preferred in terms of polymer production efficiency.

[0126] [ka] (In general formula (102), M, L, R L , R x and R y are the same as those in the general formula (101), and R 11 , R 12 , R 13 and R 14 R each independently represents a hydrogen atom, a hydrocarbon group having 1 to 20 carbon atoms which may have a substituent, or a substituent. 11 , R 12 , R 13 and R 14 Adjacent substituents may be linked to each other to form an alicyclic ring, an aromatic ring, or a heterocyclic ring containing at least one heteroatom selected from the group consisting of an oxygen atom, a nitrogen atom, and a sulfur atom. In this case, the ring has 5 to 8 members and may have a substituent on the ring.

[0127] In general formula (102), R 11 , R 12 , R 13 and R 14 The hydrocarbon group having 1 to 20 carbon atoms which may have a substituent and the substituent are the same as those described in A above. 101 It may be similar to the above.

[0128] Among them, R 11 The more bulky the group, the higher the molecular weight of the polymer tends to be. Therefore, the group is preferably a hydrocarbon group having 1 to 20 carbon atoms which may have a substituent, or a substituent, and is preferably a hydrocarbon group having 1 to 20 carbon atoms which may have a substituent. R 11 Specific examples of the hydrocarbon group having 1 to 30 carbon atoms and optionally substituted with a substituent used as the substituent include a methyl group, an ethyl group, a 1-propyl group, an i-propyl group, a 1-butyl group, an i-butyl group, a s-butyl group, a t-butyl group, a cyclopentyl group, a cyclohexyl group, a 1-adamantyl group, a 2-adamantyl group, a norbornyl group, a phenyl group, a biphenyl group, a naphthyl group, a phenanthryl group, an anthracenyl group, a fluorenyl group, a 2-methylphenyl group, a 3-methylphenyl group, a 4-methylphenyl group, a 2,4-dimethylphenyl group, a 2,5-dimethylphenyl group, a 3,5-dimethylphenyl group, Preferred examples of the phenyl group include a phenyl group, a 2-ethylphenyl group, a 3-ethylphenyl group, a 4-ethylphenyl group, a 2,3,4-trimethylphenyl group, a 2,4,5-trimethylphenyl group, a 3,4,5-trimethylphenyl group, a 2-i-propylphenyl group, a 3-i-propylphenyl group, a 4-i-propylphenyl group, a 2-t-butylphenyl group, a 3-t-butylphenyl group, a 4-t-butylphenyl group, a 2,4-di-t-butylphenyl group, a 2,5-di-t-butylphenyl group, a 3,5-di-t-butylphenyl group, a pentamethylphenyl group, and a pentafluorophenyl group.

[0129] Also, R 11Specific examples of the substituent used as the substituent include an n-propoxy group, an i-propoxy group, an n-butoxy group, a t-butoxy group, a phenoxy group, a p-methylphenoxy group, a p-methoxyphenoxy group, an ethoxycarbonyl group, a methylthio group, an ethylthio group, an n-propylthio group, an i-propylthio group, an n-butylthio group, a t-butylthio group, a phenylthio group, a cyclohexylamino group, a dimethylamino group, a diethylamino group, a di-n-propylamino group, a cyclohexylamino group, a carbazolyl group, a piperidyl group, a trimethylsilyl group, a triethylsilyl group, a dimethylphenylsilyl group, a trimethoxysilyl group, a triethoxysilyl group, a trimethylsilyloxy group, and a trimethoxysiloxy group. Among them, R 11 may be a hydrocarbon group having 4 to 20 carbon atoms which may have a substituent.

[0130] Suitable examples of the compound represented by the general formula (102) include the following compounds, but are not limited thereto. In the chemical formulas below, Ph represents a phenyl group, DMP represents a 2,6-dimethoxyphenyl group, iPr represents an isopropyl group, t-Bu represents a t-butyl group, Ad represents an adamantyl group, Cy represents a cyclohexyl group, Me represents a methyl group, TMS represents a trimethylsilyl group, and py represents pyridine.

[0131] [ka]

[0132] [ka] (In general formula (103), M, L, R L , R x and R y are the same as those in the general formula (101), and R 21 , R 22 , R 23 and R 24R each independently represents a hydrogen atom, a hydrocarbon group having 1 to 20 carbon atoms which may have a substituent, or a substituent. 21 , R 22 , R 23 and R 24 or a plurality of groups may be linked together to form an alicyclic ring, an aromatic ring, or a heterocyclic ring containing at least one heteroatom selected from the group consisting of an oxygen atom, a nitrogen atom, and a sulfur atom. In this case, the number of members in the ring is 5 to 8, and the ring may have a substituent. n is 0 or 1, and when n is 0, P is O, R 21 and R 22 is bonded directly to the carbon atom to which it is attached.)

[0133] R 21 and R 22 At least one of R is preferably a hydrocarbon group having 1 to 20 carbon atoms which may have a substituent, or a substituent, since this makes it possible to control the direction in which the olefin reacts by stereocontrol and to prevent chain transfer. 21 or R 22 It is preferable that one of the groups is an electron-withdrawing group, since this leads to further improved performance as an olefin polymerization catalyst. As the electron-withdrawing group, a trifluoromethyl group, a pentafluorophenyl group, a methoxycarbonyl group, etc. are preferably used.

[0134] Also, R 21 , R 22 , R 23 and R 24 or when a plurality of groups are linked to each other to form an alicyclic ring, an aromatic ring, or a heterocyclic ring containing at least one heteroatom selected from the group consisting of an oxygen atom, a nitrogen atom, and a sulfur atom, each ring has 5 to 8 members, but two or more rings may form a condensed ring.

[0135] Suitable examples of the compound represented by the general formula (103) include the following compounds, but are not limited thereto.

[0136] [ka]

[0137] [ka]

[0138] Further, preferred examples of the compound represented by the general formula (103) include transition metal complexes obtained by reacting the following compound with Ni(cod)2 or Ni(acac)2.

[0139] [ka]

[0140] The transition metal complex used in the present invention can be prepared by a conventionally known method. The transition metal-containing catalyst used in the present invention contains the above-mentioned transition metal complex as a main catalytic component, and may be used in combination with an activator, a carrier, etc., if necessary.

[0141] Al(R 31 ) s (OR 31 ) t X (3-(s+t)) In the general formula, R 31 each independently represents a hydrocarbon group having 1 to 20 carbon atoms; X represents a hydrogen atom, a halogen atom, or a siloxy group; s and t each independently represent a number of 0 or more and 3 or less, either s or t being greater than 0, and s+t being 3 or less. R 31 is a hydrocarbon group having 1 to 20 carbon atoms, preferably an alkyl group, alkenyl group, aryl group, aralkyl group, etc. having 1 to 12 carbon atoms. Among these, organoaluminum compounds in which s or t is 3 are preferred because they are good cocatalysts. Specific examples of the organoaluminum compound represented by the above general formula include trialkylaluminums such as trimethylaluminum, triethylaluminum, tripropylaluminum, triisobutylaluminum, and tri-n-octylaluminum; trialkoxyaluminums such as triethoxyaluminum, triisopropoxyaluminum, triisobutoxyaluminum, tri-sec-butoxyaluminum, and tri-tert-butoxyaluminum; and halogen- or alkoxy-containing alkylaluminums such as diethylaluminum monochloride and diethylaluminum monomethoxide. Among these, trialkylaluminums or trialkoxyaluminums are preferred, and trialkoxyaluminums are more preferred. The alkyl group of the trialkylaluminum may be the same as described above, and among these, a methyl group, an isobutyl group, and an n-octyl group are preferred, and among these, triisobutylaluminum or tri-n-octylaluminum is preferred. The alkoxy group of the trialkoxyaluminum may be the same as described above, and among them, a methoxy group, an ethoxy group, an isopropoxy group, an isobutoxy group, a sec-butoxy group, and a tert-butoxy group are preferable, and among these, triisopropoxyaluminum, triisobutoxyaluminum, trisec-butoxyaluminum, and tritert-butoxyaluminum are preferable.

[0142] As the carrier, any carrier can be used as long as it does not interfere with the gist of the present invention. In general, inorganic oxides and polymer carriers are preferably used. Specifically, SiO2, Al2O3, MgO, ZrO2, TiO2, B2O3, CaO, ZnO, BaO, ThO2, etc. or mixtures thereof can be mentioned, and mixed oxides such as SiO2-Al2O3, SiO2-V2O5, SiO2-TiO2, SiO2-MgO, SiO2-Cr2O3 can also be used, and inorganic silicates, polyethylene carriers, polypropylene carriers, polystyrene carriers, polyacrylic acid carriers, polymethacrylic acid carriers, polyacrylic acid ester carriers, polyester carriers, polyamide carriers, polyimide carriers, etc. can be used. There are no particular limitations on the particle size, particle size distribution, pore volume, specific surface area, etc. of these carriers, and any one can be used.

[0143] (6-2) Polymerization method for polar group-containing olefin copolymer: The method for polymerizing the polar group-containing olefin copolymer in the present invention is not limited. The polymerization method used may be solution polymerization in which all of the polymer produced is dissolved in a medium, slurry polymerization in which at least a portion of the polymer produced becomes a slurry in a medium, bulk polymerization in which the liquefied monomer itself is used as a medium, or high pressure ionic polymerization in which at least a portion of the polymer produced is dissolved in a monomer liquefied at high temperature and high pressure. The polymerization method may be any of batch polymerization, semi-batch polymerization, and continuous polymerization. Specific manufacturing processes and conditions are disclosed in, for example, JP-A-2010-260913 and JP-A-2010-202647.

[0144] The unreacted monomers and the medium may be separated from the produced polymer and recycled for use. When recycling, these monomers and the medium may be purified and reused, or may be reused without purification. A conventionally known method can be used to separate the produced polymer from the unreacted monomers and the medium. For example, methods such as filtration, centrifugation, solvent extraction, and reprecipitation using a poor solvent can be used.

[0145] The copolymerization temperature, copolymerization pressure and copolymerization time are not particularly limited, but usually, the optimum settings can be made within the following ranges, taking into consideration the productivity and process capacity. That is, the copolymerization temperature is usually -20°C to 290°C, preferably 0°C to 250°C, more preferably 0°C to 200°C, further preferably 10°C to 150°C, and particularly preferably 20°C to 100°C. The copolymerization pressure is 0.1 MPa to 100 MPa, preferably 0.3 MPa to 90 MPa, more preferably 0.5 MPa to 80 MPa, further preferably 1.0 MPa to 70 MPa, and particularly preferably 1.3 MPa to 60 MPa. The copolymerization time can be selected from the range of 0.1 minute to 50 hours, preferably 0.5 minutes to 40 hours, and further preferably 1 minute to 30 hours. In the present invention, the polymerization is generally carried out under an inert gas atmosphere, for example, a nitrogen or argon atmosphere, and preferably a nitrogen atmosphere.

[0146] There is no particular restriction on the supply of catalyst and monomer to the polymerization reactor, and various supply methods can be used depending on the purpose. For example, in the case of batch polymerization, a method can be used in which a predetermined amount of monomer is supplied to a copolymerization reactor in advance and a catalyst is supplied thereto. In this case, additional monomer or additional catalyst may be supplied to the copolymerization reactor. In addition, in the case of continuous polymerization, a method can be used in which a predetermined amount of monomer and catalyst are supplied to a copolymerization reactor continuously or intermittently to perform the copolymerization reaction continuously.

[0147] Regarding the control of the copolymer composition, a method of controlling by changing the monomer supply ratio can be generally used. Other methods include a method of controlling the copolymer composition by utilizing the difference in monomer reactivity ratio due to the difference in catalyst structure, and a method of controlling the copolymer composition by utilizing the polymerization temperature dependency of the monomer reactivity ratio. The molecular weight of the copolymer can be controlled by a conventionally known method, such as a method of controlling the molecular weight by controlling the polymerization temperature, a method of controlling the molecular weight by controlling the monomer concentration, or a method of controlling the molecular weight by controlling the ligand structure in a transition metal complex. EXAMPLES

[0148] The present invention will now be described in detail with reference to examples, but the present invention is not limited to these examples as long as they do not deviate from the gist of the invention. The physical properties of the polar group-containing olefin copolymer and the like were measured by the following methods.

[0149] [Structure of polar group-containing olefin copolymer] (1) 1 H-NMR and 13 C-NMR analysis Similar compounds of general formula (I) and general formula (II) 1 H-NMR and 13 The NMR spectrum was assigned with reference to the C-NMR spectrum (spectral database provided by the National Institute of Advanced Industrial Science and Technology), and the structure of the polar group-containing olefin copolymer was determined. Diethyl carbonate (δ) is a similar structure to that of general formula (I). 1 Around H=4.2ppm, δ 13 C = 64 ppm), and 2,3-butanediol (δ 1 H=3.8ppm, δ 13 It was verified by two-dimensional NMR that a signal was detected at a position equivalent to the chemical shift value of the cation (around C=71 ppm). The structure of the general formula (III) is 1 H=2.3ppm and δ 13 It was confirmed by two-dimensional NMR and DEPT135-NMR that a signal was detected at a chemical shift value of C=47 ppm. [Measurement conditions] 200 mg of the sample was placed in an NMR sample tube with an inner diameter of 10 mm together with 2.4 mL of a solvent (o-dichlorobenzene / deuterated bromide benzene (C6D5Br)) and hexamethyldisiloxane as a chemical shift standard substance, and dissolved uniformly in a block heater at 150°C.

[0150] ( 1 H-NMR) Equipment: Bruker Biospin AV400 NMR instrument Probe: 10mmφ cryoprobe Sample temperature: 120℃ Pulse angle: 4.5° Pulse interval: 2 seconds Accumulation count: 512 times Chemical shift: The chemical shift is set to 0.09 ppm for the proton signal of hexamethyldisiloxane, and the chemical shifts of the signals due to other protons are based on this. ( 13 C-NMR) Equipment: Bruker Biospin AV400 NMR instrument Probe: 10mmφ cryoprobe Sample temperature: 120℃ Pulse angle: 90° Pulse interval: 51.5 seconds Accumulation count: 512 times Decoupling conditions: Inverse gate decoupling method Chemical shift: The chemical shift was set to 1.98 ppm for the 13C signal of hexamethyldisiloxane, and the chemical shifts of other 13C signals were based on this. (DEPT135-NMR) Sample temperature: 120℃ Pulse angle: 90° Capture time: 2.9 seconds Wait time: 3 seconds Number of times accumulated: 128 times

[0151] (1H-DOSY) Equipment: Bruker Biospin AV400 NMR instrument Probe: 10mmφ cryoprobe Sample temperature: 120℃ Number of times: 32 F2 axis data points: 25208 F1 axis data points: 2 (2D-NMR:HSQC) Equipment: Bruker Biospin AV400 NMR instrument Probe: 10mmφ cryoprobe Sample temperature: 120℃ Number of times of accumulation: 128-256 times F2 axis data points: 1024 F1 axis data points: 50-64

[0152] <Calculation method for polar group-containing monomer content> (Ethylene (E), vinylene carbonate (VC), and t-butyl acrylate (tBA) copolymer) 13 Using the C-NMR spectrum, the content of each monomer was calculated from the following formula: VCc represents a structural unit represented by general formula (I), and VCo represents a structural unit represented by general formula (II). VC c Amount (mol%)=I(VC c )×100 / [I(VC c )+I(VC o )+I(tBA)+I(E) tBA amount (mol%)=I(tBA)×100 / [I(VC c )+I(VC o )+I(tBA)+I(E) Here, I(VC c ), I(VC o ), I(tBA), and I(E) are the quantities expressed by the following formulas. I(VC c )=(I 79.5~79.8 ) / 2 I(VC o )=(I 74.5~75.5 ) / 2 I(tBA)=I 79.1~79.5 I(E)=(I 2.0~120.0 +I 135.0~200.0 -I(VC c )×3-I(VC o )×2-I(tBA)×7) / 2 I is the integrated intensity, and the subscripts of I indicate the range of chemical shifts. For example, I 2.0~120.0 indicates the integrated intensity of the signal detected between 2.0 ppm and 120.0 ppm.

[0153] VC o Regarding 1 The formula was calculated using the H-NMR spectrum, where Al represents an aldehyde structure. VC o Amount (mol%)=IH (VC o )×100 / [I H (VC c )+I H (VC o )+I H (tBA)+I H (E) Here, I H (Al), I H (VC c ), I H (VC o ), I H (tBA), I H (E) is the quantity represented by the following formula, I H (Al)=I H、9.5~9.7 I H (VC c )=(I H、4.2~4.7 ) / 2 I H (VC o )=(I H、3.3~3.7 ) / 2 I H (tBA)=I H、2.1~2.5 I H (E)=(I H、0.1~6.0 -I H (VC c )×2-I H (VC o )×2-I H (tBA)×12) / 4 However, I H (VC o ) related to I H、3.3~3.7 If an impurity signal is present within the chemical shift range in I H、3.3~3.7 The integral value of the peak due to impurities was subtracted from the integral value of the peak due to impurities. o This was confirmed by the presence of a CH correlation peak having the same F1 value as the carbon atom-hydrogen atom correlation (CH correlation) peak derived from the compound, but a different F2 value. I H teeth 1 The integrated intensity of the H-NMR spectrum is shown. The numbers to the right of the H readings indicate the range of chemical shifts. For example, I H、0.1~6.0indicates the integrated intensity of the signal detected between 0.1 ppm and 6.0 ppm.

[0154] <Calculation method of aldehyde (Al) structure> 1 The aldehyde content (Al content) was calculated from the H-NMR spectrum according to the following formula: Al content (mol%) = I H (Al) × 100 / (I H (VC c )+I H (VC o )+I(tBA)+I H (E)+I H (Al)

[0155] (Ethylene (E), vinylene carbonate (VC), and methyl acrylate (MA) copolymer) 13 Using the C-NMR spectrum, the MA content was calculated according to the following formula: MA amount (mol%)=I(MA)×100 / (I(E')+I(MA)+I(VC c )+I(VC o )) VC c Amount (mol%)=I(VC c ) × 100 / (I(E') + I(MA) + I(VC c )+I(VC o )) VC o Amount (mol%)=I(VC o ) × 100 / (I(E') + I(MA) + I(VC c )+I(VC o )) Here, I(MA) and I(E') are quantities expressed by the following formulas. I(MA)=I 50.4~51.0 I(E')=((I 2.0~120.0 +I 135.0~200.0 -I(MA)×4-I(VC c )×3-I(VC o )×2) / 2

[0156] <Calculation method of aldehyde (Al) structure> 1 The aldehyde content (Al content) was calculated from the H-NMR spectrum according to the following formula: Al content (mol%) = I H (Al) × 100 / (I H (VC c )+I H (VC o )+I(MA)+I H (E')+I H (Al) Here, I H (M.A.), I. H (E') is the quantity represented by the following formula, I H (MA)=(I H、3.2~3.8 ) / 3 I H (E')=(I H、0.1~6.0 -I H (VC c )×2-I H (MA)×6) / 4

[0157] <Calculation method for ethylene content> The ethylene content was calculated by dividing the content of the polar group-containing comonomer by 100 mol % of the entire polymer. (Ethylene (E), vinylene carbonate (VC), and t-butyl acrylate (tBA) copolymer) Ethylene content (mol%) = 100 - (VC c Amount+VC o amount + tBA amount + Al amount) (Ethylene (E), vinylene carbonate (VC), and methyl acrylate (MA) copolymer) Ethylene content (mol%) = 100 - (VC c Amount+VC o amount + MA amount + Al amount)

[0158] (2) Number average molecular weight and weight average molecular weight The number average molecular weight and the weight average molecular weight were calculated by size exclusion chromatography using polystyrene as a molecular weight standard. The specific measurement method of GPC is as follows. Apparatus: Agilent Technologies PL-GPC 220 Detector: IR detector Column: Resonac AT-806MS (3 columns in series) Mobile phase solvent: orthodichlorobenzene (ODCB) Measurement temperature: 140℃ Flow rate: 1.0mL / min Injection volume: 0.3mL [Sample preparation] The polar group-containing olefin copolymer is dissolved at 1 mg / mL in ODCB containing 0.24 mg / mL TMP (2,4,6-trimethylphenol) at 140° C. for about 1 hour. The retention volume obtained by GPC measurement is converted to molecular weight using a calibration curve prepared in advance using standard polystyrene (PS). The standard polystyrenes used are the following brands manufactured by Tosoh Corporation: F380, F288, F128, F80, F40, F20, F10, F4, F1, A5000, A2500, and A1000. A calibration curve is prepared by injecting 0.3 mL of a solution containing 0.24 mg / mL TMP dissolved in ODCB for ethylene (co)polymer so that each is 0.5 mg / mL. A cubic equation obtained by approximating with the least squares method is used for the calibration curve. The viscosity equation used for conversion to molecular weight is [η] = K × M α The following numerical values ​​are used: PS:K = 1.38 x 10 -4 , α=0.700 PP:K = 1.03 x 10 -4 , α=0.780 PE:K = 3.92 x 10 -4 , α=0.733

[0159] (Synthesis Example 1: Synthesis of AL-16) 535 mg (1.67 mmol) of bis(2,6-dimethoxyphenyl)phosphine borane was weighed out in a Schlenk flask, and 21 mL of tetrahydrofuran was added. After cooling to -78°C, 1.2 mL (1.84 mmol) of n-butyllithium was slowly added dropwise. After the dropwise addition, the mixture was stirred at room temperature for 2 hours and 15 minutes. After cooling to 0°C, 0.18mL (1.67mmol) of 2,2-bis(trifluoromethyl)oxirane dissolved in 5.4mL of tetrahydrofuran was slowly added. After stirring at room temperature for 1 hour and 40 minutes, the solvent was completely removed and the residue was washed twice with 10mL of hexane. After washing, the solvent was completely removed and 16mL of tetrahydrofuran was added. After cooling to 0°C, 1.0mL (2.00mmol) of hydrochloric acid ether solution was slowly dropped. After stirring at room temperature for 30 minutes, 15mL of degassed water was added to extract the organic layer. The operation of adding 8mL of ether to the water layer and extracting the organic layer was repeated three times. The collected organic layer was dried over sodium sulfate, and then the sodium sulfate was removed using a glass filter. The collected solution was completely dried to obtain 722mg (1.44mmol) of residue. 14 mL of toluene was added to the above residue. 194 mg (1.73 mmol) of 1,4-diazabicyclo[2.2.2]octane dissolved in 7 mL of toluene was added thereto, and the mixture was heated to 60°C and stirred for 2 hours. After stirring, the solvent was completely removed and the mixture was purified by silica gel column chromatography using a solvent of hexane:acetone = 2:1. After purification, the product was recrystallized with 2 mL of tetrahydrofuran and 8 mL of hexane to obtain 471 mg of a solid. 31 P{ 1 The purity determined by {H}-NMR was 97%.

[0160] 1 H-NMR (400MHz, CDCl3)δ:7.22(t, J=8.4, 2H), 6.49(dd, J=8.4, 3.0Hz, 4H), 5.25(d, J=5.8Hz, 1H), 3.68(s, 12H), 3.19(s, 2H) 19 F-NMR (376MHz, CDCl3)δ:-77.3(d, J=17.5Hz) 31 P{ 1 H}-NMR(162MHz, CDCl3)δ:-62.0(septet, J=20.0Hz)

[0161] [ka]

[0162] [Synthesis example 2] (B27-DM) According to Synthesis Example 4 described in WO 2010 / 050256, the following 2-bis(2,6-dimethoxyphenyl)phosphano-6-pentafluorophenylphenol ligand (B-27DM) was used.

[0163] [ka]

[0164] [Synthesis example 3] (AL-40) (1) Synthesis of 2,2,6,6-tetramethylbenzo[1,2-d:5,4-d']bis([1,3]dioxole) The compound of the following chemical formula was synthesized according to the description in Bioorg. Med. Chem. Lett. 2014, 24, 2379-2382.

[0165] [ka]

[0166] (2) Synthesis of bis(2,2,6,6-tetramethylbenzo[1,2-d:5,4-d']bis([1,3]dioxol)-4-yl)chlorophosphine 2,2,6,6-Tetramethylbenzo[1,2-d:5,4-d']bis([1,3]dioxole) (5 g, 22.5 mmol, 1 eq) was dissolved in 50 mL of tetrahydrofuran. The resulting solution was cooled to 0°C, n-BuLi (24.8 mmol, 1.1 eq) was slowly added, and the mixture was stirred at 20°C for 2.5 h to obtain a yellow solution. The solution was cooled to -78°C, and PCl3 (1.39 g, 10.1 mmol, 0.45 eq) was added all at once. The mixture was warmed to 20°C and stirred for 1.5 h to obtain a yellow suspension. The suspension was dried to obtain 5.72 g of a yellow viscous mixture containing the target product. The resulting mixture was used in the next synthesis without purification. 31 P{ 1 H} NMR (162MHz, CDCl3)δ:46.3 (integration ratio 100%)

[0167] [ka]

[0168] (3) Synthesis of bis(2,2,6,6-tetramethylbenzo[1,2-d:5,4-d']bis([1,3]dioxol)-4-yl)phosphine Bis(2,2,6,6-tetramethylbenzo[1,2-d:5,4-d']bis([1,3]dioxol)-4-yl)chlorophosphine (5.72 g, 11.2 mmol, 1 eq) was dissolved in 50 mL of tetrahydrofuran. The resulting solution was cooled to 0°C, lithium aluminum hydride (0.64 g, 16.9 mmol, 1.5 eq) was added, and the mixture was stirred at 20°C for 12 hours to obtain a colorless suspension. The resulting suspension was cooled to 0°C, and 0.6 mL of water, 0.6 mL of 10% aqueous sodium hydroxide, and 1.8 mL of water were added in that order, and the resulting mixture was stirred at room temperature for 30 minutes to quench the reaction. The mixture was filtered, and the filtrate was evaporated to dryness to obtain a colorless solid. Subsequently, 30 mL of water was added to the resulting solid, and the product was extracted three times with 30 mL of dichloromethane. The combined organic layers were dried over sodium sulfate, the solid was filtered off, and the filtrate was concentrated to obtain a yellow crude product. The crude product was purified by silica gel chromatography (eluent: petroleum ether / ethyl acetate = 20 / 1) under atmospheric conditions, washed with 10 mL of hexane, and then evaporated to dryness to obtain 3.1 g (6.5 mmol, 58%) of the target compound as a colorless solid. 1 H NMR(400MHz, CDCl3)δ:6.26(s,2H),5.15(d,J=235Hz,1H),1.57(s,24H) 31 P{ 1 H} NMR(162MHz, CDCl3)δ:-126.8(s)

[0169] [ka] (4) Synthesis of AL-40 400 mg (0.84 mmol) of bis(2,2,6,6-tetramethylbenzo[1,2-d:5,4-d']bis([1,3]dioxol)-4-yl)phosphine was weighed out in a Schlenk tube, and 11 mL of tetrahydrofuran was added. The resulting solution was cooled to -78°C, and 0.58 mL (0.92 mmol) of n-BuLi was slowly added dropwise. After the dropwise addition was completed, the mixture was stirred at -78°C for 1 hour. The mixture was then warmed to 0°C, and 92 μL (0.84 mmol) of 2,2-bis(trifluoromethyl)oxirane dissolved in 2.8 mL of tetrahydrofuran was slowly added. The mixture was stirred at room temperature for 1 hour, and the solvent was distilled off. 14 mL of tetrahydrofuran was added to the residue, and the mixture was cooled to 0°C, and 1.0 mL (1.0 mmol) of a hydrochloric acid ether solution was slowly added dropwise. The mixture was stirred at 0°C for 1 hour, and then 8 mL of water was added under atmospheric pressure to wash the mixture, and the organic layer was separated. The operation of adding 4 mL of diethyl ether to the aqueous layer and extracting the organic layer was repeated three times. The collected organic layer was dried over sodium sulfate, and the sodium sulfate was removed by filtration. The filtrate was evaporated to dryness, and the obtained solid was purified by silica gel column chromatography (developing solvent: hexane / acetone = 10 / 1) under atmospheric pressure to obtain 242 mg of a solid. 31 The purity of AL-40 determined by P NMR was 99% or more. 1 H NMR (400MHz, CDCl3)δ:6.30(s, 2H), 4.76(d, J=3.4Hz, 1H), 3.25(brs, 2H), 1.58(s, 12H), 1.55(s, 12H) 19 F NMR(376MHz, CDCl3)δ:-77.0(d, J=22.0Hz) 31 P{ 1 H} NMR(162MHz, CDCl3)δ:-62.1(septet, J=22.9Hz)

[0170] [ka]

[0171] All the following operations were carried out under a nitrogen atmosphere. Example 1 (1) Preparation of catalyst solution In a 50 mL flask, 10.8 mg (39.3 μmol) of Ni(cod)2 (Tokyo Chemical Industry Co., Ltd., purity >97.0%) was weighed out and dissolved in 8 mL of toluene. In a separate flask, 12.1 mg (24.9 μmol) of AL-16 obtained in Synthesis Example 1 was weighed out. 5 mL of the toluene solution of Ni(cod)2 was weighed out and added to the flask containing AL-16. The resulting solution was warmed in a 40°C water bath and stirred for 15 minutes to obtain a catalyst solution. (2) Production of polar group-containing olefin copolymer In a 0.2 L autoclave equipped with a catalyst cylinder and a killer feeder, 74 mL of toluene, 1.72 g (20.0 mmol) of vinylene carbonate (VC, Aldrich, 99.5%, acid < 200 ppm, HO < 100 ppm), 0.6 mL (4.2 mmol) of t-butyl acrylate (tBA), and triisopropoxyaluminum (Al(O i Pr) 3) toluene solution (0.1M) 0.5mL was added and the temperature was raised to 90°C. High pressure nitrogen was added to this to make it 0.5MPa, and ethylene was added at 2.5MPa. 1mL of catalyst solution was added to the catalyst cylinder, and the catalyst was pressed into the autoclave with high pressure nitrogen, and this point was the reaction start time. Furthermore, 1mL of the above catalyst solution was pressed into the catalyst cylinder 5 minutes after the start of the reaction, and 2mL of the above catalyst solution was pressed into the catalyst cylinder 10 minutes after. After pressing the above catalyst solution three times, the catalyst cylinder was washed with 3mL of toluene each time, and the washing solution was pressed into the autoclave. 30 minutes after the start of the reaction, 1mL of a toluene solution of diacetic acid (2M) was pressed into the killer feeder to stop the reaction, the killer feeder was washed with 3mL of toluene, the washing solution was pressed in, and ethylene was depressurized. After cooling the inside temperature of the autoclave to room temperature, 100mL of acetone was added. The precipitated solid was collected by filtration, and the solid was washed twice with 100mL of acetone, and then dried under reduced pressure. The amount of the polar group-containing olefin copolymer 1 obtained was 0.23 g.

[0172] Example 2 (1) Preparation of catalyst solution In a 50 mL flask, 10.8 mg (39.3 μmol) of Ni(cod)2 was weighed out and dissolved in 8 mL of toluene. In a separate flask, 16.8 mg (29.8 μmol) of B-27DM obtained from Synthesis Example 2 was weighed out. 6 mL of the toluene solution of Ni(cod)2 was weighed out and added to the flask containing B-27DM. The resulting solution was warmed in a 40°C water bath and stirred for 15 minutes to obtain a catalyst solution.

[0173] (2) Production of polar group-containing olefin copolymer In a 0.2 L autoclave similar to that in Example 1, 74 mL of toluene, 1.76 g (20.5 mmol) of VC, 0.6 mL (4.2 mmol) of tBA, and Al(O i 0.5 mL of a toluene solution (0.1 M) of Pr)3 was added, and the temperature was raised to 90° C. High-pressure nitrogen was added to this to adjust the pressure to 0.5 MPa, and ethylene was added at 2.5 MPa. 2 mL of catalyst solution was added to the catalyst cylinder, and the catalyst was forced into the autoclave with high-pressure nitrogen, and this time was the reaction start time. After that, the catalyst cylinder was washed with 3 mL of toluene, and the washing liquid was forced into the autoclave. 30 minutes after the start of the reaction, 1 mL of a toluene solution of diacetic acid (2 M) was forced into the killer feeder to stop the reaction, the killer feeder was washed with 3 mL of toluene, the washing liquid was forced into the killer feeder, and the ethylene was depressurized. After the internal temperature of the autoclave was cooled to room temperature, 100 mL of acetone was added. The precipitated solid was collected by filtration, and the solid was washed twice with 100 mL of acetone, and then dried under reduced pressure. The polar group-containing olefin copolymer 2 obtained was 0.96 g.

[0174] Example 3 (1) Preparation of catalyst solution In a 50 mL flask, 27.7 mg (101 μmol) of Ni(cod)2 was weighed out and dissolved in 10 mL of toluene. In a separate flask, 45.2 mg (80.0 μmol) of B-27DM obtained from Synthesis Example 2 was weighed out. 8 mL of the toluene solution of Ni(cod)2 was weighed out and added to the flask containing B-27DM. The resulting solution was warmed in a 40°C water bath and stirred for 15 minutes to obtain a catalyst solution.

[0175] (2) Production of polar group-containing olefin copolymer In a 0.2 L autoclave similar to that in Example 1, 62 mL of toluene, 11.3 g (132.0 mmol) of VC, 2.20 mL (15.3 mmol) of tBA, and Al(O i 2 mL of a toluene solution (0.1 M) of Pr)3 was added, and the temperature was raised to 90° C. High-pressure nitrogen was added to this to adjust the pressure to 0.5 MPa, and ethylene was added at 2.5 MPa. 3mL of catalyst solution was added to the catalyst cylinder, and the catalyst was forced into the autoclave with high-pressure nitrogen, and this time was set as the reaction start time. Then, 3mL of toluene was used to wash the catalyst cylinder, and the washing liquid was forced into the autoclave. 11 minutes later, 1mL of catalyst solution was added to the catalyst cylinder, and the catalyst was forced into the autoclave with high-pressure nitrogen. Then, 3mL of toluene was used to wash the catalyst cylinder, and the washing liquid was forced into the autoclave. 30 minutes after the start of the reaction, 1mL of a toluene solution of diacetic acid (2M) was forced into the killer feeder to stop the reaction, the killer feeder was washed with 3mL of toluene, the washing liquid was forced into the autoclave, and ethylene was depressurized. After cooling the inside temperature of the autoclave to room temperature, 100mL of acetone was added. The precipitated solid was collected by filtration, and the solid was washed twice with 100mL of acetone, and then dried under reduced pressure. The polar group-containing olefin copolymer 3 obtained was 0.16g.

[0176] Example 4 (1) Preparation of catalyst solution In a 50 mL flask, 12.9 mg (50.2 μmol) of nickel (II) acetylacetonate (Ni(acac)2, Merck, purity >98%) was weighed out and dissolved in 10 mL of toluene. In a separate flask, 19.4 mg (29.6 μmol) of AL-40 obtained in Synthesis Example 3 was weighed out. 6 mL of the toluene solution of Ni(acac)2 was weighed out and added to the flask containing AL-40. The resulting solution was warmed in a 40°C water bath and stirred for 15 minutes to obtain a catalyst solution. (2) Production of polar group-containing olefin copolymer 87 mL of toluene, 3.2 mL (50.0 mmol) of VC, 0.4 mL (4.5 mmol) of MA, and 0.5 mL of a toluene solution of trioctyl aluminum (TNOA, 0.1 M) were added to a 0.2 L autoclave similar to that in Example 1, and the temperature was raised to 90°C. High pressure nitrogen was added to this to make it 0.5 MPa, and 2.5 MPa of ethylene was further added. 2 mL of catalyst solution was added to the catalyst cylinder, and the catalyst was forced into the autoclave with high pressure nitrogen, and this point was set as the reaction start time. Two minutes after the above catalyst solution was forced into the catalyst cylinder, the catalyst cylinder was washed with 3 mL of toluene, and the washing solution was forced into the autoclave. Thirty minutes after the start of the reaction, 3 mL of 1,2-butanediol was forced into the autoclave from the killer feeder to stop the reaction, and ethylene was depressurized. After the internal temperature of the autoclave was cooled to room temperature, 100 mL of acetone was added. The precipitated solid was collected by filtration, washed twice with 100 mL of acetone, and then dried under reduced pressure to obtain 2.99 g of polar group-containing olefin copolymer 4.

[0177] The conditions for each experiment are summarized in Table 1. Table 2 summarizes the analysis results of the copolymers obtained from each experiment. In addition, FIG. 1 shows the polar group-containing olefin copolymer 1. 13 The C-NMR spectrum is shown in FIG. 13 A partial enlarged view (around 73 to 83 ppm) of the C-NMR spectrum is shown. 1 The H-NMR spectrum is shown in FIG. 1 A partial enlarged view (around 3.5 to 3.7 ppm) of the H-NMR spectrum is shown.

[0178] [Table 1]

[0179] [Table 2]

[0180] FIG. 5 shows the HSQC spectrum of polar group-containing olefin copolymer 1. 1 In the H-NMR spectrum, peaks derived from impurities are indicated by "*". Ibr indicates the C-H correlation of a1 and a2, which are hydrogen atoms derived from the vinylene carbonate skeleton in the structure shown in Figures 1 and 2. The area surrounded by the dashed line in Figure 5 indicates the expanded area in Figure 6. FIG. 6 is an enlarged view of the dashed line portion of FIG. 5. 1 In the H-NMR spectrum, peaks due to impurities are indicated with "*". IIbr is a hydrogen atom derived from the ring opening of vinylene carbonate in the structure shown in Figure 4. H 1 and b H 6 shows the C-H correlations of 2. In Fig. 6, the C-H correlations due to impurities are indicated by circles.

[0181] As is clear from the NMR measurement results, a novel polar group-containing olefin copolymer was obtained in which an olefin, a structural unit (B) derived from a vinylene carbonate derivative represented by general formula (1), and a structural unit (C) derived from an acrylate derivative represented by general formula (2) were introduced into the main chain. In Table 2, the comonomer content (mol %) means the content ratio of the structural unit (B) derived from the vinylene carbonate derivative represented by general formula (1) or the structural unit (C) derived from the acrylic ester derivative represented by general formula (2) when the total structural units of the polymer are taken as 100 mol %. [Industrial Applicability]

[0182] The novel polar group-containing olefin copolymer of the present invention has vinylene carbonate having an oxygen atom at the vicinal position and a structural unit derived from an acrylic acid ester derivative introduced into a polyolefin having two or more carbon atoms such as ethylene, and therefore may realize functions not found in conventional olefin copolymers, such as chelating coordination. For example, the polar group-containing olefin copolymer of the present invention is expected to be used as a carrier for metal complex catalysts or an adsorbent for recovering metal complexes. Further, by carrying out graft polymerization on the polar group of the structural unit (B) of the polar group-containing olefin copolymer of the present invention, it becomes possible to carry out further functionality. Furthermore, by copolymerizing a polyolefin having two or more carbon atoms, such as ethylene, with a vinylene carbonate derivative and an acrylic acid ester derivative, carbon dioxide can be fixed.

Claims

1. A structural unit (A) derived from at least one olefin having 2 to 20 carbon atoms; A structural unit (B) derived from at least one monomer represented by the following general formula (1), A structural unit (C) derived from at least one monomer represented by the following general formula (2), A polar group-containing olefin copolymer comprising: 【Chemistry 1】 (In formula (1), R 1 and R 2 are each independently a hydrogen atom, a halogen atom, a hydroxyl group, a formyl group, a carboxy group, an ester group having 1 to 30 carbon atoms, an acyloxy group having 1 to 30 carbon atoms, an acyl group having 1 to 30 carbon atoms, an alkoxy group having 1 to 30 carbon atoms, an aryloxy group having 6 to 30 carbon atoms, an alkylthio group having 1 to 30 carbon atoms, an arylthio group having 6 to 30 carbon atoms, a nitro group, an amino group which may be substituted with at least one hydrocarbon group having 1 to 30 carbon atoms, a silyl group which may be substituted with at least one hydrocarbon group having 1 to 30 carbon atoms, an amide group which may be substituted with at least one hydrocarbon group having 1 to 30 carbon atoms, a hydrocarbon group having 1 to 30 carbon atoms substituted with at least one halogen atom, or a hydrocarbon group or heterocyclic group having 1 to 30 carbon atoms which may be substituted with at least one substituent containing at least one selected from the group consisting of an oxygen atom, a sulfur atom, and a nitrogen atom, or 1 and R 2 may be bonded to each other to form a 4- to 10-membered ring. 【Chemistry 2】 (In formula (2), R 3 is a hydrogen atom, a halogen atom, a hydrocarbon group having 1 to 10 carbon atoms substituted with at least one halogen atom, or a hydrocarbon group having 1 to 10 carbon atoms. R 4 is a hydrogen atom, a silyl group which may be substituted with at least one hydrocarbon group having 1 to 30 carbon atoms, a hydrocarbon group having 1 to 30 carbon atoms which is substituted with at least one halogen atom, or a hydrocarbon group or heterocyclic group having 1 to 30 carbon atoms which may be substituted with at least one substituent containing at least one of an oxygen atom, a sulfur atom, or a nitrogen atom.

2. The structural unit (B) comprises a structural unit represented by the following general formula (I), or a structural unit represented by the following general formula (I) and a structural unit represented by the following general formula (II): 【Chemistry 3】 (In formula (I) and formula (II), R 1 and R 2 is the same as above.)

3. 2. The polar group-containing olefin copolymer according to claim 1, wherein the structural unit (C) is represented by the following general formula (III): 【Chemistry 4】 (In formula (III), R 3 and R 4 is the same as above.)

4. R of the structural unit (B) 1 and R 2 3. The polar group-containing olefin copolymer according to claim 1, wherein at least one of the above is a hydrogen atom.

5. R of the structural unit (C) 3 The polar group-containing olefin copolymer according to claim 1 or 3, wherein is a hydrogen atom.

6. R of the structural unit (B) 1 and R 2 The polar group-containing olefin copolymer according to claim 1 or 2, wherein each of the is a hydrogen atom.

7. The polar group-containing olefin copolymer according to any one of claims 1 to 3, wherein the olefin is ethylene.

8. 3. The polar group-containing olefin copolymer according to claim 1, wherein the content of the structural unit (B) is 0.01 mol % to 10 mol %.

9. 4. The polar group-containing olefin copolymer according to claim 1, wherein the content of the structural unit (C) is 0.01 mol % to 30 mol %.

10. A method for producing a polar group-containing olefin copolymer, comprising polymerizing at least one olefin having 2 to 20 carbon atoms, at least one monomer represented by the following general formula (1), and at least one monomer represented by the following general formula (2) in the presence of a catalyst containing at least one compound represented by the following general formula (101): 【Chemistry 5】 [In general formula (101), M represents a metal atom of Group 10 of the periodic table. Q is an oxygen atom, a sulfur atom, or -S(=O) 2 It represents —O— or —C(═O)—O—, and the left side of each of the groups is bonded to A and the right side is bonded to M. A represents a divalent hydrocarbon group having 1 to 30 carbon atoms which may have a substituent. R L represents a hydrogen atom, a hydrocarbon group having 1 to 20 carbon atoms which may contain a hetero atom, or a ligand coordinated to M. L represents a ligand coordinated to M. R x and R y each independently represents a hydrogen atom or a hydrocarbon group having 1 to 20 carbon atoms which may contain a hetero atom. R L and L and R x and R y may form a ring, R x and A or R y and A may form a ring. 【Chemistry 6】 (In formula (1), R 1 and R 2 are each independently a hydrogen atom, a halogen atom, a hydroxyl group, a formyl group, a carboxy group, an ester group having 1 to 30 carbon atoms, an acyloxy group having 1 to 30 carbon atoms, an acyl group having 1 to 30 carbon atoms, an alkoxy group having 1 to 30 carbon atoms, an aryloxy group having 6 to 30 carbon atoms, an alkylthio group having 1 to 30 carbon atoms, an arylthio group having 6 to 30 carbon atoms, a nitro group, an amino group which may be substituted with at least one hydrocarbon group having 1 to 30 carbon atoms, a silyl group which may be substituted with at least one hydrocarbon group having 1 to 30 carbon atoms, an amide group which may be substituted with at least one hydrocarbon group having 1 to 30 carbon atoms, a hydrocarbon group having 1 to 30 carbon atoms substituted with at least one halogen atom, or a hydrocarbon group or heterocyclic group having 1 to 30 carbon atoms which may be substituted with at least one substituent containing at least one selected from the group consisting of an oxygen atom, a sulfur atom, and a nitrogen atom, or 1 and R 2 may be bonded to each other to form a 4- to 10-membered ring. 【Chemistry 7】 (In formula (2), R 3 is a hydrogen atom, a halogen atom, a hydrocarbon group having 1 to 10 carbon atoms substituted with at least one halogen atom, or a hydrocarbon group having 1 to 10 carbon atoms. R 4 is a hydrogen atom, a silyl group which may be substituted with at least one hydrocarbon group having 1 to 30 carbon atoms, a hydrocarbon group having 1 to 30 carbon atoms which is substituted with at least one halogen atom, or a hydrocarbon group or heterocyclic group having 1 to 30 carbon atoms which may be substituted with at least one substituent containing at least one of an oxygen atom, a sulfur atom, or a nitrogen atom.

Citation Information

Patent Citations

  • Vinylene carbonate-ethylene copolymer and method of producing same

    US2847398A

  • Binary blends of polyvinyl formal and ethylene vinylene carbonate copolymer and processes for making the same

    US3114728A

  • Linear functionalized copolymer and articles formed thereof

    WO2000056781A2