Dispersants for solid-containing phenolic foams

The incorporation of silicon-free quaternary ammonium compounds as surfactants in phenolic foam production stabilizes solid contents, addressing sedimentation and redispersion issues, ensuring uniform distribution and maintaining foam quality.

JP2024144342APending Publication Date: 2024-10-11EVONIK OPERATIONS GMBH
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
JP2024051475
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Priority Date
2023-03-28
Filing Date
2024-03-27
Publication Date
2024-10-11

AI Technical Summary

Technical Problem

The production of phenolic foams with solid contents faces challenges such as sedimentation, non-uniform distribution, and difficulty in redispersion, leading to non-uniform property profiles and increased viscosity.

Method used

A composition for phenolic foam production using silicon-free quaternary ammonium compounds as surfactants, particularly ester quats and alkyl quats, to stabilize and uniformly distribute solid contents, preventing sedimentation and enhancing redispersibility.

Benefits of technology

The use of silicon-free quaternary ammonium compounds ensures uniform distribution and easy handling of solids, reducing sedimentation and maintaining mechanical properties, thermal insulation, and surface quality of phenolic foams.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024144342000001
    Figure 2024144342000001
  • Figure 2024144342000002
    Figure 2024144342000002
  • Figure 2024144342000003
    Figure 2024144342000003
Patent Text Reader

Abstract

To provide a composition for producing phenolic foam which makes it possible to provide phenolic foam that comprises one or more solids and, in particular, avoids a significant increase in the viscosity of each component while not causing sedimentation, difficulty in redispersion after sedimentation, and / or inhomogeneous distribution in material.SOLUTION: A composition for producing phenolic foam comprises at least one phenolic resin, at least one blowing agent, at least one catalyst, and at least one solid. The composition comprises at least one surfactant selected from the group of silicon-free quaternary ammonium compounds.SELECTED DRAWING: None
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to the field of phenolic foams. The present invention relates in particular to a composition for producing phenolic foams, to a method for producing phenolic foams, to phenolic foams produced according to the invention and their use. In the context of the present invention, phenolic foams are understood to mean in particular foams obtained by reacting a phenolic resin with an acid as a catalyst with the addition of a blowing agent. Phenolic foams are known to the skilled artisan and are described, for example, in EP 3830174, EP 602004006376 (German translation), EP 2898005, EP 1922357, WO 2022043561, EP 4073155, AUS 2021238847 or WO 2006114777. Phenolic foams are also known alternatively as phenolic resin foams.

[0002] In the production of phenolic foams, cell stabilizing additives or foam stabilizing additives can generally be used, which are aimed at obtaining a homogeneous and less turbulent foam structure with fine cells, and thus have a significant positive effect on the use properties of the foam, in particular, for example, on the thermal insulation performance. For this purpose, foam stabilizers can usually be used, for example, foam stabilizers based on ethoxylated vegetable oils, for example, castor oil, as described, for example, in EP-A-3830174. The use of polyether-modified siloxanes (PES), as described, for example, in WO-A-2022043561, has proven to be particularly effective in further improving the use properties. In particular, the combination of ethoxylated vegetable oils and polyether-modified siloxanes results in excellent use properties. This combination is therefore a generally preferred type of foam stabilizer in the production of phenolic foams.

[0003] In connection with the provision of phenolic foams, it is of particular interest to produce them in a particularly cost-effective manner. A further interest is to produce them in a particularly sustainable manner, for example by using bio-based and / or recycled materials, and / or to improve the flame retardancy, for example by adding flame retardants. For this purpose, various solid contents can be used. The corresponding solid contents suitable for use in phenolic foams are known per se.

[0004] However, the use of solids entails significant problems with respect to dispersion and processing in the liquid starting material, including, inter alia, settling, difficulty in redispersing after settling, non-uniform distribution in the phenolic foam, and, inter alia, the resulting non-uniform property profile of the foams thus produced.

[0005] Against this background, a specific problem of the present invention was to make it possible to provide a phenolic foam containing one or more solids and to overcome the above-mentioned problems of settling, difficulties in redispersion after settling and / or non-uniform distribution in the material, in particular while avoiding a significant increase in the viscosity of each component.

[0006] In this context, it has been surprisingly found within the scope of the present invention that the use of one or more surfactants selected from the group of silicon-free quaternary ammonium compounds, such as ester quats and / or alkyl quats, allows the desired significant improvement of redispersion, sedimentation stability and a more uniform property profile of the material, whereby, advantageously, the viscosity of each component is not significantly affected.

[0007] The specific problem of the present invention is solved by the subject matter of the present invention, which is a composition for producing phenolic foam, comprising at least one phenolic resin, at least one blowing agent, at least one catalyst and at least one solid content, said composition comprising at least one surfactant selected from the group of silicon-free quaternary ammonium compounds.

[0008] Within the scope of the present invention, solids are understood to mean substances that are in a solid, aggregated state at 25° C. and 101.325 kPa.

[0009] The subject matter according to the invention has various advantages. The subject matter according to the invention makes it possible, for example, to provide a phenolic foam with a high solids content. Advantageously, this is possible without compromising other properties of the material, in particular its mechanical properties. In particular, the phenolic foam has very good thermal insulation properties and shows excellent long-term behavior and high surface quality. The invention allows a particularly uniform distribution of the solids in the phenolic foam. Overall, the invention allows easy processing of the solids in the scope of production. The solids can be easily introduced into the phenolic resin, for example, advantageously with at least one surfactant selected from the group of silicon-free quaternary ammonium compounds such as ester quats and / or alkyl quats. The invention makes it possible to significantly reduce or even avoid problems of settling during storage of dispersions of phenolic resin and solids. The invention also allows very good redispersibility of the solids, in particular in the case of settling after very long storage, so that, for example, constant stirring or mixing during storage is no longer necessary. The invention also allows a more uniform distribution of the solids in the phenolic foam, which results in a more uniform property profile.

[0010] Surfactants from the group of silicon-free quaternary ammonium compounds, such as ester quats, amidoamine quats, imidazolinium quats, cetylpyridinium chloride and / or alkyl quats themselves, are known to those skilled in the art.For example, ester quats and alkyl quats are silicon-free quaternary ammonium compounds with at least one long hydrocarbon group.Alkyl quats are generally tetraalkylammonium salts, while ester quats are generally based on quaternary triethanolmethylammonium compounds or quaternary diethanoldimethylammonium compounds that are esterified with at least one fatty acid.

[0011] Alkyl quats and ester quats have long been used in cosmetics or detergents and cleaning agents, such as fabric softeners, and their preparation has long been known to those skilled in the art. Alkyl quats can be prepared, for example, by reacting the corresponding amines with methylating agents, such as chloromethane or dimethyl sulfate. Ester quats can be prepared, for example, by esterifying methyldiethanolamine or triethanolamine with fatty acids, followed by quaternization, for example, with dimethyl sulfate or chloromethane.

[0012] The composition according to the invention comprises at least one surfactant selected from the group of silicon-free quaternary ammonium compounds. According to a particularly preferred embodiment of the invention, the at least one surfactant is selected from the group consisting of ester quats of formula (1), ester quats of formula (2), alkyl quats of formula (3), imidazolinium quats of formula (4), amidoamine quats of formula (5) and cetylpyridinium chloride; [ka] Where: R 1 is an acyl group of a saturated, monounsaturated or polyunsaturated, linear or branched fatty acid having a chain length of 8 to 22 carbon atoms, or an acyl group of ricinoleic acid, or hydrogen; Compounds of formula (1) or (2) may contain different groups R 1 provided that at least one group R 1 must be one of the acyl groups mentioned, R 2 are each independently an alkyl group having 1 to 6 carbon atoms or hydrogen, preferably hydrogen, methyl, ethyl, propyl or isopropyl, particularly preferably hydrogen or methyl, R 3 are each independently an alkyl group having 1 to 6 carbon atoms or hydrogen, preferably hydrogen, methyl, ethyl, propyl or isopropyl, particularly preferably methyl or hydrogen, R 4 is an alkyl group having 1 to 6 carbon atoms, or a hydroxyethyl group, or hydrogen, preferably methyl, ethyl, propyl or isopropyl, particularly preferably ethyl or methyl, very particularly preferably methyl, The compounds of formula (1) and / or (2) may have different groups R 4 may include n=0 to 20, preferably 0 to 10, particularly preferably 0; Where a=1-3 and b=1-3, where a+b=4, and / or [ka] Where: R 5 is a saturated, monounsaturated or polyunsaturated, linear or branched alkyl group having a chain length of 8 to 24 carbon atoms, The compound of formula (3) may be a compound having different groups R 5 may include R 6 is an alkyl group having 1 to 6 carbon atoms, or a hydroxyethyl group, or a benzyl group, or hydrogen, preferably methyl, ethyl, propyl, isopropyl or benzyl, particularly preferably ethyl or methyl, very particularly preferably methyl, The compound of formula (3) may be a compound having different groups R 6 may include Where c=1-3 and d=1-3, However, c+d=4, and / or [ka] Where: R 7 is an alkyl group having 1 to 6 carbon atoms, or a hydroxyethyl group, or hydrogen, preferably methyl, ethyl, propyl or isopropyl, particularly preferably ethyl or methyl, very particularly preferably methyl, R8 is a saturated, monounsaturated or polyunsaturated, linear or branched alkyl group having 8 to 22 carbon atoms or a group O(CO)R 10 where R 10 is an aliphatic, saturated, monounsaturated or polyunsaturated, linear or branched alkyl group having 7 to 21 carbon atoms, R 9 is an aliphatic, saturated, monounsaturated or polyunsaturated, linear or branched alkyl group having 7 to 21 carbon atoms, Z is an NH group or oxygen; e can take an integer value from 1 to 4, and / or [ka] Where: R 11 is a saturated, mono- or polyunsaturated, linear or branched alkyl group having a chain length of 7 to 21 carbon atoms, R 12 is an alkyl group having 1 to 6 carbon atoms, or a hydroxyethyl group, or hydrogen, preferably methyl, ethyl, propyl or isopropyl, particularly preferably ethyl or methyl, very particularly preferably methyl, The compound of formula (5) may be a compound having different groups R 12 Can contain f can take integer values ​​from 0 to 5. h=1 or 2 and g=2 or 3, where h+g=4, The compounds of formula (5) can have different values ​​for f when h=2 and different groups R 11 may include R 4 , R 6 , R 7 or R 12When contains a hydroxyethyl group, this group may be alkoxylated, and this optionally alkoxylated hydroxyethyl group may contain repeat units based on ethylene oxide, propylene oxide, butylene oxide and / or styrene oxide and may contain 1 to 15 repeat units, preferably 1 to 10 repeat units.

[0013] In particular, one or more surfactants according to the present invention selected from the group of silicon-free quaternary ammonium compounds mentioned above can be used, i.e. any mixture of such surfactants can also be used.In this case, it is particularly preferred to use the ester quat of formula (1) and / or the ester quat of formula (2).Therefore, it is particularly preferred to use at least one surfactant selected from the group consisting of the ester quat of formula (1) and the ester quat of formula (2).

[0014] Corresponding compositions comprising one or more corresponding silicon-free quaternary ammonium compounds show particularly favorable results with regard to the advantages according to the invention mentioned above.

[0015] In formula (1) and / or formula (2), R 1 are each independently selected from the acyl radicals of the acids of the group consisting of oleic acid, isostearic acid, lauric acid, palmitic acid, elaidic acid, vaccenic acid, gadoleic acid, icosenoic acid, cetoleic acid, erucic acid, nervonic acid, linoleic acid, α-linolenic acid, γ-linolenic acid, calendic acid, punicic acid, α-eleostearic acid, β-eleostearic acid, arachidonic acid, timnodonic acid, clupanodonic acid and cervonic acid.

[0016] Furthermore, it is preferred if in formula (1) a=b=2 and / or in formula (5) h=1 and g=3, which likewise corresponds to a further particularly preferred embodiment of the present invention.

[0017] The compositions according to the invention which additionally comprise at least one counter anion for the compounds of general formulae (1), (2), (3), (4) and / or (5) selected from the group consisting of chloride, bromide, iodide, alkylsulfate, ethylsulfate, alkylsulfonate, triflate, tosylate, phosphate, sulfate, hydrogensulfate, lactate, glycolate, acetate and citrate represent a further particularly preferred embodiment of the invention.

[0018] Particularly preferred compositions according to the invention are characterized in that at least one solid is selected from the group consisting of: (a) solid flame retardants, preferably ammonium polyphosphate, melamine, melamine-coated ammonium polyphosphate, melamine microencapsulated ammonium polyphosphate, melamine formaldehyde resin microencapsulated ammonium polyphosphate, melamine cyanurate, red phosphorus, zinc borate, melamine polyphosphate, expandable graphite and / or antimony trioxide, in particular red phosphorus and / or ammonium polyphosphate, (b) plastic powder, and (c) calcium carbonate, graphite, graphene, lignin, lignocellulose, a metal hydroxide, preferably aluminium hydroxide and / or magnesium hydroxide, a metal carbonate, preferably calcium carbonate, magnesium carbonate, barium carbonate and / or zinc carbonate, a metal oxide, preferably aluminium oxide and / or zinc oxide and / or a metal powder, preferably zinc.

[0019] This also represents a particularly preferred embodiment of the present invention.

[0020] It is possible to use one or more of the solids according to the invention, in particular the solids mentioned above, i.e. also any mixture of such solids can be used.

[0021] At least one solid component is in particular in powder form. This corresponds to a particularly preferred embodiment of the invention. Preferred particle sizes are described below.

[0022] The solid flame retardants suitable for use in phenolic foams are also known per se, and the present invention is not limited in the selection of the solid flame retardant.However, when a specific solid flame retardant, particularly as described above, is used in the composition according to the present invention, it corresponds to a preferred embodiment of the present invention.One or more solid flame retardants can be used, i.e. any mixture thereof can also be used.The use of red phosphorus and / or ammonium polyphosphate is very particularly preferred.

[0023] A particularly preferred embodiment of the invention exists when the composition according to the invention contains red phosphorus and / or ammonium polyphosphate as solid flame retardant.

[0024] There is a further particularly preferred embodiment of the present invention, where the composition according to the invention contains at least one plastic powder, which consists of at least one plastic selected from the group consisting of polyethylene, polypropylene, polyamide, such as in particular PA6, PA6.6, PA10, PA11 and / or PA12, polyester, such as in particular polyethylene terephthalate, polybutylene terephthalate and / or poly-ε-caprolactone, polystyrene, polyacrylate, polymethyl methacrylate, polycarbonate, styrene-acrylonitrile copolymer, polyether, polylactic acid, polyurethane, phenolic resin, phenolic foam, polysulfone, polyethersulfone, polyetherimide and polyimide or mixtures thereof, and the plastic powder can be particularly preferably formed from waste plastics, particularly preferably from phenolic resin waste plastics and / or phenolic foam waste plastics.

[0025] In particular, one or more of the abovementioned plastic powders may be used, ie any mixture of such plastic powders may also be used.

[0026] Waste plastics, in particular, (i) Plastics resulting from manufacturing waste obtained during the manufacture of plastics, such as cutting residues, sawdust, or materials that do not pass quality control; and / or (ii) Plastics resulting from end-of-life plastics, for example phenolic foam-based plastics resulting from used insulation materials and boards, or other used plastic parts and plastic semi-finished products. It is.

[0027] A further particularly preferred embodiment of the present invention also exists when the composition according to the invention comprises one or more plastic powders from waste plastics, preferably from phenolic resin waste plastics, particularly preferably from phenolic foam waste plastics.

[0028] There is a further particularly preferred embodiment of the present invention, where the composition according to the invention is characterized in that the solid content is a powder having an average particle size of preferably <500 μm, advantageously <250 μm, particularly preferably <150 μm, determined as a volume-based median value by laser diffraction spectroscopy, advantageously in accordance with ISO 13320:2020. In this case, the average particle size of the particles is determined by laser diffraction spectroscopy in accordance with ISO 13320:2020. The data on the average diameter (i.e. the average particle diameter) correspond to the volume-based median value, i.e. refer to the equivalent volume sphere diameter, 50% of the particles are smaller and 50% of the particles are larger.

[0029] A further particularly preferred embodiment of the present invention exists when the composition according to the invention is characterized in that at least one surfactant from the group of the silicon-free quaternary ammonium compounds is contained in a total amount of 0.1 to 20 parts by weight, advantageously 0.1 to 15 parts by weight, particularly preferably 0.1 to 10 parts by weight, based on 100 parts by weight of the total phenolic resin used.

[0030] According to a further preferred embodiment of the invention, the at least one solid component is present in the composition according to the invention in a total amount of 1 to 100 parts by weight, advantageously 1 to 60 parts by weight, particularly preferably 5 to 50 parts by weight, based on 100 parts by weight of the total phenolic resin used.

[0031] and / or further comprising an alkoxylated, preferably ethoxylated, castor oil in a total amount of 0.5 to 10 parts by weight, advantageously 1 to 8 parts by weight, based on 100 parts by weight of the total phenolic resin used; At least one polyether siloxane is further included in an amount of 0.5 to 10 parts by weight based on 100 parts by weight of the total phenolic resin used. When the composition according to the invention is characterized in that:

[0032] Polyether siloxanes, also known as polyether modified siloxanes (PES), are known per se and are described below.

[0033] At least one blowing agent is selected from the group consisting of: - Hydrocarbons having 3, 4 or 5 carbon atoms, preferably cyclo-, iso- and / or n-pentane And - halogenated hydrocarbons having 3, 4 or 5 carbon atoms, preferably hydrofluoroolefins and / or hydrohaloolefins, more preferably 1234ze, 1234yf, 1224yd, 1233zd(E) and / or 1336mzz There is a further preferred embodiment of the present invention when the composition according to the invention is characterized in that it is selected from the group consisting of:

[0034] In particular, one or more of the above blowing agents may be used, ie, any mixture of blowing agents may also be used.

[0035] A further object of the present invention is a process for the preparation of a phenolic foam using a reaction mixture comprising a composition comprising at least one phenolic resin, at least one blowing agent, at least one catalyst and at least one solid, which in a particularly preferred embodiment comprises at least one surfactant selected from the group of silicon-free quaternary ammonium compounds, such as, for example, ester quats or alkyl quats or amidoamine quats or imidazolinium quats, as described in detail above.

[0036] Particularly preferred phenolic foam formulations in the sense of the present invention have a melting point of 5 to 900 kg / m 3 and advantageously has the composition shown in Table 1, which corresponds to a preferred embodiment of the invention: [Table 1]

[0037] For further preferred embodiments and configurations of the method according to the invention, reference is also made to the explanations already given above in connection with the composition according to the invention.

[0038] A further subject of the present invention is a phenolic foam produced by the process according to the invention as described above, in particular using the composition according to the invention.

[0039] A further object of the present invention relates to the use of the aforementioned phenolic foam according to the invention as a thermal insulation material, preferably as an insulating board or sandwich element.

[0040] Particularly preferred compositions according to the invention comprise the following components: - at least one phenolic resin, at least one surfactant selected from the group of the silicon-free quaternary ammonium compounds and / or cetylpyridinium chloride, in particular as defined above by formula (1), (2), (3), (4) and / or (5), at least one blowing agent, - at least one catalyst, at least one foam stabilizer which is not a surfactant from the group of silicon-free quaternary ammonium compounds, - at least one solid component, - optionally further additives etc.

[0041] The production of phenolic foams (also referred to within the scope of the present invention as phenolic resin foams) is known per se. To produce phenolic foams, one or more phenolic resins, advantageously one or more so-called resole resins, can be used. The phenolic resins, advantageously resole resins, which can be used accordingly, are known per se. In particular, they can be produced in a known manner, for example by condensation of phenol or phenolic compounds, such as cresol, xylenol, p-alkylphenols, p-phenylphenol, resorcin, etc., and aldehydes, such as formaldehyde, furfural, acetaldehyde, etc., advantageously under basic conditions, for example by using catalytic amounts of alkali metal hydroxides, such as sodium hydroxide, potassium hydroxide or calcium hydroxide, or aliphatic amines, such as trimethylamine or triethylamine, preferably together with an excess of aldehyde. This is the usual route for the production of phenolic resins, advantageously resole resins, but the invention is not limited to the above-listed chemicals.

[0042] Here, the molar ratio of phenolic groups to aldehyde groups is not particularly limited. Preferably, the ratio is in the range of 1:1 to 1:3, particularly preferably in the range of 1:1.5 to 1:2.5. Advantageously, but not limited to, the phenolic resin has a free aldehyde content of 0.1% to 0.5% by weight. This can be determined by potentiometric titration according to ISO 11402:2004 with hydroxylamine hydrochloride.

[0043] The phenolic resins which can be preferably used in the production of foams are liquid at 25° C. and normal pressure, advantageously have a water concentration of about 1 to 25% by weight, preferably 5 to 20% by weight, and have methylol groups as reactive substituents, as described, for example, in EP 0 170 357. If desired, the viscosity of the phenolic resin can be adjusted, in particular by the water content. A high water content usually results in a low viscosity, which makes the resin easier to handle and mix during the production of foams.

[0044] The viscosity of the preferably usable phenolic resins at 25° C. and normal pressure is advantageously in the range of 1000 to 28000 mPa·s and can be measured by the usual methods known to the skilled artisan, for example with a Brookfield viscometer. Basic information on the production and composition of phenolic resins can be obtained from the prior art and is described in particular in, for example, EP 3830174, EP 2898005, WO 2022043561 or EP 4073155.

[0045] The surfactants according to the invention, in particular from the group of the silicon-free quaternary ammonium compounds and / or cetylpyridinium chloride defined above by the formulae (1), (2), (3), (4) and / or (5), have already been mentioned above.

[0046] Blowing agents and their use in the production of phenolic foams are known to those skilled in the art. The use of one or more blowing agents depends essentially on the type of system and the application of the resulting phenolic foam. Depending on the amount of blowing agent used, high or low density foams can be produced. For example, advantageously 5 kg / m according to ASTM D1622-20. 3 ~900kg / m 3 , preferably 5 to 500 kg / m 3 , particularly preferably 10 to 200 kg / m 3 , especially 12 to 100 kg / m 3 It is possible to produce foams having densities of

[0047] As blowing agents, one or more corresponding compounds having a suitable boiling point can be used, for example hydrocarbons having 3, 4 or 5 carbon atoms, preferably cyclo-, iso- or n-pentane, halogenated hydrocarbons, for example chlorinated hydrocarbons, for example dichloroethane, 1,2-dichloroethene, n-propyl chloride, isopropyl chloride, butyl chloride, isobutyl chloride, pentyl chloride, isopentyl chloride, 1,1-dichloroethene, trichloroethene or chloroethene, or hydrofluorocarbons (HFCs), for example HFC245fa, HFC134a or HFC365mfc, hydrofluoroolefins (HFOs) or hydrohaloolefins, preferably 1234ze, 1234yf, 1224yd, 1233zd(E) or 1336mzz and mixtures thereof.

[0048] Catalysts which can be used for the production of phenolic foams are known to the skilled person from the prior art and are described, for example, in EP 0170357 A1 or the German translation of EP 602004006376 A1. Advantageously, here, the usual organic and inorganic acids known from the prior art can be used. One or more acids can be used. Particularly preferably usable are sulfuric acid, phosphoric acid, benzenesulfonic acid, xylenesulfonic acid, p-toluenesulfonic acid, ethylbenzenesulfonic acid, naphtholsulfonic acid, cumenesulfonic acid and / or phenolsulfonic acid. In particular, mixtures of several of these compounds can be used as catalysts. The preferred amount of catalyst used for the complete reaction is in particular also influenced by the water content of the phenolic resin and / or the water content of the catalyst if it is present as an aqueous solution. For example, a higher water content may require a higher acid concentration.

[0049] Phenolic foams can be formed in a known manner, i.e., by reaction of a mixture containing, inter alia, a phenolic resin, a blowing agent, a foam stabilizer and a catalyst. When a catalyst is added to a mixture of a phenolic resin, a blowing agent and a foam stabilizer, an exothermic reaction occurs between the methylol groups and the phenol, forming methylene bridges and crosslinking. Water is eliminated by condensation. Here, the type and amount of acid used, the properties of the blowing agent and the structure of the foam stabilizer influence the exothermicity of the reaction and the foam formation.

[0050] The foam stabilizer and its use in the production of phenolic foam are generally known to those skilled in the art as mentioned above.For example, the use of ethoxylated castor oil is described in EP 3830174, and the use of ethoxylated castor oil and polyether modified siloxane is described in WO 2022043561.The use of ethoxylated castor oil and the use of ethoxylated castor oil and polyether modified siloxane correspond to the preferred embodiment of the present invention.

[0051] The solids content has already been discussed above.

[0052] As optional additives, one or more substances known from the prior art that are commonly used in the production of phenolic foams can be used, such as viscosity reducers, plasticizers, hardeners, liquid flame retardants, cell refining additives, colorants and / or fragrances. Suitable optional additives are described, for example, in EP-A-3830174, U.S. Pat. No. 4,444,912 and EP-A-1,922,357.

[0053] To reduce the viscosity of the phenolic resin, for example, monoethylene glycol or polyester polyols can be used. As hardeners, for example, compounds with amino groups, such as urea or dicyandiamide, can be used. Urea is preferably used. They can be used not only during foaming, but also already during the production of the phenolic resin.

[0054] The process for producing the phenolic foam according to the invention can be carried out using any known method, which is known to the person skilled in the art and is described, for example, in EP-A-3830174.

[0055] Unless otherwise apparent from the specification, all preferred or particularly preferred embodiments of the invention can be combined with one or more other preferred or particularly preferred embodiments of the invention.

[0056] The subject matter according to the present invention will be described below by way of example, but the scope of the present invention is clear from the entire specification and the claims, and the present invention is not limited to these exemplary embodiments. When ranges, general formulas or compound classes are given, these are intended to include not only the corresponding ranges or compound groups explicitly mentioned, but also all subranges and subcompound groups that can be obtained by extracting the individual values ​​(ranges) or compounds. When documents are cited within the present specification, their contents are fully incorporated into the disclosure of the present invention, in particular with regard to the subject matter in the context in which the documents are cited. Unless otherwise stated, percentages are data in weight percent. When average values ​​are given, these are numerical averages, unless otherwise stated. When parameters determined by measurement are given, the measurements were carried out at a temperature of 23° C. and at normal pressure, unless otherwise stated.

[0057] Working Example: Example 1: Preparation of phenolic foam For application technical comparison, the formulations in Table 2 and the dispersants in Table 3 were selected.

[0058] Comparative foaming was carried out by hand mixing. For this, the phenolic resin (batch amount 180±5 g), foam stabilizer, dispersant and solids were weighed into a beaker and mixed with a plate stirrer (diameter 6 cm) at 20° C. and 500 rpm for 15 minutes. The foaming agent was then added, mixed at 1500 rpm for 30 seconds and cooled to 18° C. The acid was then added and the mixture was stirred at 2000 rpm for 45 seconds and transferred to an aluminum mold with dimensions 25 cm×25 cm×7 cm, covered with a polyethylene film and thermostated at 50° C. After 1 hour, the foam was demolded and cured in an oven heated to 60° C. for 18 hours.

[0059] [Table 2]

[0060] [Table 3]

[0061] The surface and pore structure were subjectively rated on a scale of 1 to 10, with 10 representing a very fine foam with no (ideal) disturbances and 1 representing an extremely disturbed and coarse foam. Thermal conductivity (λ value, in mW / m K) was measured on 2.5 cm thick panels at an average temperature of 10 °C as specified in standard EN12667:2001 using a Hesto Lambda Control instrument, type HLC X206. Density was measured according to ASTM D1622-20.

[0062] The results are shown in Tables 4 to 8.

[0063] [Table 4]

[0064] [Table 5]

[0065] [Table 6]

[0066] [Table 7]

[0067] [Table 8]

[0068] The results show that the non-inventive dispersants lead to a much worse property profile when using solids, especially high thermal conductivity and poor surface. In contrast, the use of the inventive dispersants leads to a significantly improved property profile compared to the non-inventive dispersants.

[0069] Example 2: Dispersion Behavior For application technical comparison, the formulation shown in Table 9 was used. For this, the phenolic resin and dispersant were weighed (batch size 250 g) and mixed with a plate stirrer (diameter 6 cm) at 1000 rpm for 30 seconds. The solids were then added with the plate stirrer still running (2000 rpm) and mixed for a further 45 seconds. The formulation was then filled into a glass container, closed and the time to complete settling was measured.

[0070] After 21 days of upright storage at room temperature, all samples were redispersed and the redispersibility was rated on a scale of 1 to 3, where a score of 1 means that the sample could already be redispersed using a laboratory electric stirrer (300 rpm for 30 seconds). A score of 2 was given if redispersibility was possible at 800 rpm for 60 seconds. A score of 3 was given to samples where a very solid and dense sediment had formed and this sediment could not be redispersed by either of the two aforementioned methods.

[0071] [Table 9]

[0072] The results are shown in Tables 10 and 11.

[0073] [Table 10]

[0074] [Table 11]

[0075] In the cases tested, improvements in sedimentation stability and redispersibility could be achieved compared to formulations without dispersant or compared to formulations without a dispersant according to the invention.

[0076] In particular, the formation of solid, dense sediments could be avoided, so that, for example, constant stirring or mixing during long-term storage is no longer necessary, since the invention allows very good redispersibility of the solids in case of sedimentation after very long storage.

Claims

1. A composition for producing phenolic foam comprising at least one phenolic resin, at least one blowing agent, at least one catalyst, and at least one solids, characterized in that the composition comprises at least one surfactant selected from the group of silicon-free quaternary ammonium compounds.

2. the at least one surfactant is selected from the group consisting of an ester quat of formula (1), an ester quat of formula (2), an alkyl quat of formula (3), an imidazolinium quat of formula (4), an amidoamine quat of formula (5), and cetylpyridinium chloride; [Formula 1] Where: R 1 is the acyl group of a saturated, mono- or polyunsaturated, linear or branched fatty acid having a chain length of 8 to 22 carbon atoms, or the acyl group of ricinoleic acid, or hydrogen; The compounds of formula (1) or (2) may be formed by mixing different groups R 1 provided that at least one group R 1 must be one of the acyl groups mentioned, R 2 are each independently of one another an alkyl radical having 1 to 6 carbon atoms or hydrogen, preferably hydrogen, methyl, ethyl, propyl or isopropyl, particularly preferably hydrogen or methyl, R 3 are each independently of one another an alkyl radical having 1 to 6 carbon atoms or hydrogen, preferably hydrogen, methyl, ethyl, propyl or isopropyl, particularly preferably methyl or hydrogen, R 4 is an alkyl group having 1 to 6 carbon atoms, or a hydroxyethyl group, or hydrogen, preferably methyl, ethyl, propyl or isopropyl, particularly preferably ethyl or methyl, very particularly preferably methyl, The compounds of formula (1) and / or (2) may have different groups R 4may include n=0 to 20, preferably 0 to 10, particularly preferably 0; a=1 to 3 and b=1 to 3, where a+b=4, and / or [chemical 2] Where: R 5 is a saturated or mono- or polyunsaturated, linear or branched alkyl group having a chain length of 8 to 24 carbon atoms, The compound of formula (3) is a compound having different groups R 5 may include R 6 is an alkyl group having 1 to 6 carbon atoms, or a hydroxyethyl group, or a benzyl group, or hydrogen, preferably methyl, ethyl, propyl, isopropyl or benzyl, particularly preferably ethyl or methyl, very particularly preferably methyl, The compound of formula (3) is a compound having different groups R 6 may include Where c=1 to 3 and d=1 to 3, where c+d=4, and / or [C3] Where: R 7 is an alkyl group having 1 to 6 carbon atoms, or a hydroxyethyl group, or hydrogen, preferably methyl, ethyl, propyl or isopropyl, particularly preferably ethyl or methyl, very particularly preferably methyl, R 8 is a saturated, mono- or polyunsaturated, linear or branched alkyl group having 8 to 22 carbon atoms or a group O(CO)R 10 where R 10 is an aliphatic, saturated or mono- or polyunsaturated, linear or branched alkyl group having 7 to 21 carbon atoms, R 9is an aliphatic, saturated or mono- or polyunsaturated, linear or branched alkyl group having 7 to 21 carbon atoms, Z is an NH group or oxygen; e can take an integer value from 1 to 4; and / or [C4] Where: R 11 is a saturated or mono- or polyunsaturated, linear or branched alkyl group having a chain length of 7 to 21 carbon atoms; R 12 is an alkyl group having 1 to 6 carbon atoms, or a hydroxyethyl group, or hydrogen, preferably methyl, ethyl, propyl or isopropyl, particularly preferably ethyl or methyl, very particularly preferably methyl, The compound of formula (5) may be a compound having different groups R 12 Can contain f can take integer values ​​from 0 to 5; h=1 or 2 and g=2 or 3, where h+g=4, The compounds of formula (5) can have different values ​​for f when h=2 and different groups R 11 may include R 4 , R 6 , R 7 Or R 12 comprises a hydroxyethyl group, said group may be alkoxylated, said optionally alkoxylated hydroxyethyl group may comprise repeat units based on ethylene oxide, propylene oxide, butylene oxide and / or styrene oxide and may comprise from 1 to 15 repeat units, preferably from 1 to 10 repeat units.

3. In formula (1) and / or formula (2), R 13. The composition according to claim 2, characterized in that each of the is independently selected from the acyl radicals of the acids of the group consisting of oleic acid, isostearic acid, lauric acid, palmitic acid, elaidic acid, vaccenic acid, gadoleic acid, icosenoic acid, cetoleic acid, erucic acid, nervonic acid, linoleic acid, α-linolenic acid, γ-linolenic acid, calendic acid, punicic acid, α-eleostearic acid, β-eleostearic acid, arachidonic acid, timnodonic acid, clupanodonic acid and cervonic acid.

4. 4. The composition according to claim 2 or 3, characterized in that in formula (1) a=b=2 and / or in formula (5) h=1 and g=3.

5. 5. The composition according to claim 2, further comprising at least one counter anion selected from the group consisting of chloride ion, bromide ion, iodide ion, alkyl sulfate ion, ethyl sulfate ion, alkyl sulfonate ion, triflate ion, tosylate ion, phosphate ion, sulfate ion, hydrogen sulfate ion, lactate ion, glycolate ion, acetate ion and citrate ion for the compound of general formula (1), (2), (3), (4) and / or (5).

6. The at least one solid component is selected from the group consisting of: (a) solid flame retardants, preferably ammonium polyphosphate, melamine, melamine-coated ammonium polyphosphate, melamine microencapsulated ammonium polyphosphate, melamine formaldehyde resin microencapsulated ammonium polyphosphate, melamine cyanurate, red phosphorus, zinc borate, melamine polyphosphate, expandable graphite and / or antimony trioxide, in particular red phosphorus and / or ammonium polyphosphate, (b) plastic powder; and (c) calcium carbonate, graphite, graphene, lignin, lignocellulose, metal hydroxides, preferably aluminum hydroxide and / or magnesium hydroxide, metal carbonates, preferably calcium carbonate, magnesium carbonate, barium carbonate and / or zinc carbonate, metal oxides, preferably aluminum oxide and / or zinc oxide and / or metal powders, preferably zinc 6. The composition according to claim 1, wherein the compound is selected from the group consisting of:

7. The composition of claim 6, wherein the solid flame retardant comprises red phosphorus and / or ammonium polyphosphate.

8. 8. The composition according to claim 1 , characterized in that at least one plastic powder is contained, which is at least one plastic selected from the group consisting of polyethylene, polypropylene, polyamide, such as in particular PA6, PA6.6, PA10, PA11 and / or PA12, polyester, such as in particular polyethylene terephthalate, polybutylene terephthalate and / or poly-ε-caprolactone, polystyrene, polyacrylate, polymethyl methacrylate, polycarbonate, styrene-acrylonitrile copolymer, polyether, polylactic acid, polyurethane, phenolic resin, phenolic foam, polysulfone, polyethersulfone, polyetherimide and polyimide or mixtures thereof, and that the plastic powder can be particularly preferably formed from waste plastics, particularly preferably from phenolic resin waste plastics and / or phenolic foam waste plastics.

9. 9. The composition according to claim 1, wherein the at least one solid fraction is a powder having an average particle size of <500 μm, preferably <250 μm, particularly preferably <150 μm.

10. 10. The composition according to claim 1, wherein the at least one surfactant is present in a total amount of 0.1 to 20 parts by weight, preferably 0.1 to 15 parts by weight, particularly preferably 0.1 to 10 parts by weight, based on 100 parts by weight of the total phenolic resin used.

11. 11. The composition according to claim 1, wherein the at least one solid component is present in a total amount of 1 to 100 parts by weight, preferably 1 to 60 parts by weight, particularly preferably 5 to 50 parts by weight, based on 100 parts by weight of the total phenolic resin used.

12. and / or further comprising an alkoxylated, preferably ethoxylated, castor oil in a total amount of 0.5 to 10 parts by weight, preferably 1 to 8 parts by weight, based on 100 parts by weight of the total phenolic resin used; At least one polyether siloxane is further included in an amount of 0.5 to 10 parts by weight based on 100 parts by weight of the total phenolic resin used.

12. The composition according to any one of claims 1 to 11, characterized in that

13. The at least one blowing agent is selected from the group consisting of: - hydrocarbons having 3, 4 or 5 carbon atoms, preferably cyclo-, iso- and / or n-pentane; And halogenated hydrocarbons having 3, 4 or 5 carbon atoms, preferably hydrofluoroolefins and / or hydrohaloolefins, more preferably 1234ze, 1234yf, 1224yd, 1233zd(E) and / or 1336mzz 13. The composition according to claim 1, wherein the composition is selected from the group consisting of:

14. A process for producing a phenolic foam using a reaction mixture comprising the composition of any one of claims 1 to 13.

15. A phenolic foam produced by the method of claim 14.

16. 16. Use of the phenolic foam according to claim 15 for thermal insulation.