Resin composition and molding

A resin composition with a core-shell polymer and isosorbide polycarbonate enhances Charpy and surface impact strength, addressing the shortcomings of existing rubber-containing graft polymers in automotive parts by improving scratch hardness and impact resistance.

JP2024144373APending Publication Date: 2024-10-11MITSUBISHI CHEM CORP

Patent Information

Application Number
JP2024053777
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Priority Date
2023-03-30
Filing Date
2024-03-28
Publication Date
2024-10-11

AI Technical Summary

Technical Problem

Existing rubber-containing graft polymers mixed with thermoplastic resins result in insufficient Charpy impact strength, surface impact strength, and decreased scratch hardness, particularly in automotive parts applications where both properties are crucial for safety and appearance.

Method used

A resin composition comprising a core-shell polymer with specific monomer-derived structural units and a polycarbonate resin having an isosorbide skeleton, where the core-shell polymer has a polymer A portion as the shell and a polymer B portion as the core, with defined mass content and particle diameter, enhancing dispersibility and impact strength.

Benefits of technology

The resin composition improves scratch hardness and both Charpy and surface impact strength, ensuring safety and appearance in automotive parts while maintaining good impact resistance.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024144373000001
    Figure 2024144373000001
  • Figure 2024144373000002
    Figure 2024144373000002
  • Figure 2024144373000003
    Figure 2024144373000003
Patent Text Reader

Abstract

To provide a resin composition capable of producing a molding that has high tensile hardness and has both good Charpy impact strength and good surface impact strength, and a molding produced from the resin composition.SOLUTION: A resin composition contains a polymer (X) having a polymer A part including a structural unit derived from a vinyl monomer (a1) having a specific constitutional unit (-CO(CH2)5O-), and a polycarbonate resin (Y) having an isosorbide skeleton.SELECTED DRAWING: None
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a resin composition and a molded article. [Background technology]

[0002] The rubber-containing core-shell polymer is a rubber-like polymer graft-polymerized with a vinyl monomer. The rubber-containing core-shell polymer is produced by emulsion polymerization and can be dispersed in a wide variety of resins while maintaining a predetermined rubber particle size and rubber structure, and is therefore suitable for use in resins that require impact strength.

[0003] In order to improve the impact strength of a resin, it is generally believed that it is effective to uniformly disperse rubber in the resin, but rubber itself has low compatibility with general thermoplastic resins, and it is difficult to uniformly disperse rubber in a resin by itself.

[0004] It is known that rubber-like polymers are graft-polymerized with vinyl monomers to improve the dispersion of rubber in resins. Methyl methacrylate is preferably used as the vinyl monomer. This is because methyl methacrylate is highly compatible with a wide range of thermoplastic resins such as polycarbonate, styrene resins, and vinyl chloride resins.

[0005] Thermoplastic resins are also used in a variety of applications, including home appliances, office automation equipment, and automobile parts. In particular, in automobile parts applications, they are increasingly replacing metals in order to reduce the weight of car bodies, but resins are required to have sufficient impact strength (Charpy impact strength and dart impact strength).

[0006] For automotive parts applications, thermoplastic resins with added graft rubber are used from the viewpoint of impact strength. However, when graft rubber is added to a thermoplastic resin, while the Charpy impact strength improves, the dart impact strength may decrease. For automotive parts applications, it is required to achieve both Charpy impact strength and dart impact strength in order to ensure safety. [Prior art documents] [Patent documents]

[0007] [Patent Document 1] International Publication No. 2019 / 131374 Summary of the Invention [Problem to be solved by the invention]

[0008] However, when a rubber-containing graft polymer as described in Patent Document 1 is mixed with a thermoplastic resin to form a molded article, the Charpy impact strength and dart impact strength of the molded article are insufficient. In addition, resin products are often used in places where they are visible to people, particularly in the case of automotive parts, and therefore it is important that they are scratch-resistant and maintain a good appearance. However, when a rubber-containing graft polymer is added to a thermoplastic resin, the scratch hardness of the molded product surface may decrease.

[0009] The present invention has been made in consideration of the above circumstances, and an object of the present invention is to provide a resin composition which can give a molded article having high scratch hardness and good both Charpy impact strength and dart impact strength, and a molded article using the same. [Means for solving the problem]

[0010] Means for Solving the Problems In order to achieve the above object, the inventors of the present invention have conducted intensive research and have found that the above problems can be solved by forming a resin composition containing a polymer having structural units derived from a specific monomer and a polycarbonate resin having a specific skeleton, thereby completing the present invention.

[0011] That is, the present invention relates to the following. [1] A polymer (X) having a polymer A portion including a structural unit derived from a vinyl monomer (a1) having a structural unit represented by the following formula (1), A polycarbonate resin (Y) having an isosorbide skeleton, A resin composition comprising: -CO(CH 2 ) 5 O-···(1) [2] The resin composition according to [1], wherein the polymer (X) further has a polymer B portion containing a structural unit derived from a vinyl monomer (b1) different from the vinyl monomer (a1). [3] The resin composition according to [2], wherein the content of the polymer A portion is 10 to 50 mass % and the content of the polymer B portion is 50 to 90 mass % when the total of the polymer A portion and the polymer B portion is 100 mass %. [4] The polymer (X) is a core-shell polymer, The resin composition according to [2] or [3] above, wherein the polymer A portion constitutes a shell portion of the core-shell polymer, and the polymer B portion constitutes a core portion of the core-shell polymer. [5] The resin composition according to [4] above, wherein the average primary particle size of the core-shell polymer is 100 to 500 nm. [6] The polymer A portion further contains a structural unit derived from an alkyl (meth)acrylate (a2) having an alkyl group having 1 to 10 carbon atoms, The resin composition according to any one of the above [1] to [5], wherein the content of the structural units derived from the vinyl monomer (a1) is 1 to 30 mass % and the content of the structural units derived from the alkyl (meth)acrylate (a2) is 70 to 99 mass % relative to the total mass of all structural units constituting the polymer A portion. [7] The resin composition according to any one of the above [1] to [6], wherein the vinyl monomer (a1) is a monomer represented by the following formula (2): CH 2 =CR 1 COO(CH 2 ) q O[CO(CH 2 ) 5 O] n H (2) (In formula (2), R 1 represents a hydrogen atom or a methyl group, q represents an integer of 2 to 5, and n represents an integer of 1 or more. [8] R in the above formula (1)1 is a methyl group. [9] The resin composition according to the above [7] or [8], wherein n in the formula (1) is an integer of 1 to 5.

[10] The resin composition according to any one of the above [1] to [9], wherein the content of the polymer (X) is 1 to 30 mass%, and the content of the polycarbonate resin (Y) is 70 to 99 mass%, when the total of the polymer (X) and the polycarbonate resin (Y) is 100 mass%.

[11] A molded article comprising the resin composition according to any one of [1] to

[10] above. Effect of the Invention

[0012] According to the present invention, by preparing a resin composition containing a polymer having structural units derived from a specific monomer and a polycarbonate resin having a specific skeleton, it is possible to provide a resin composition which improves the scratch hardness of a molded article while also improving both the Charpy impact strength and dart impact strength, and a molded article using the same. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0013] Hereinafter, the embodiments of the present invention will be described in detail, but the present invention is not limited to the following embodiments as long as they do not deviate from the purpose of the present invention. As used herein, the following definitions apply: The term "structural unit" refers to a structural unit derived from a monomer, i.e., a structural unit formed by polymerization of a monomer, or a structural unit in which a portion of the structural unit is converted into a different structure by treating the polymer. The generic term for acrylate and methacrylate is "(meth)acrylate". The generic term for acrylic and methacrylic is "(meth)acrylic". The "molded article" is a molded product obtained by molding the resin composition of the present invention. A numerical range indicated by "to" means a numerical range including the numbers before and after "to" as the lower and upper limits. The numerical ranges of the contents, various physical property values, and property values ​​disclosed in this specification can be arbitrarily combined with the lower and upper limits to form new numerical ranges.

[0014] "Resin composition" A resin composition according to one embodiment of the present invention contains a polymer (X) and a polycarbonate resin (Y) shown below. In addition to the polymer (X) and the polycarbonate resin (Y), the resin composition may further contain components other than the polymer (X) and the polycarbonate resin (Y) (hereinafter also referred to as "optional components") as long as the effects of the present invention are not impaired.

[0015] [Polymer (X)] The polymer (X) has a polymer A portion shown below. The polymer (X) may be a polymer consisting of only the polymer A portion, but preferably has, in addition to the polymer A portion, a polymer B portion described below. When the polymer (X) has a polymer A portion and a polymer B portion, the polymer (X) may be a polymer in which the polymer A portion and the polymer B portion are covalently bonded to each other, or may be a polymer in which the polymer A portion and the polymer B portion are not covalently bonded to each other. When the polymer (X) is a polymer consisting only of a polymer A portion, the polymer (X) is the polymer A.

[0016] An example of the polymer in which a polymer A portion and a polymer B portion are covalently bonded is a block copolymer having a polymer A portion and a polymer B portion. An example of a polymer in which the polymer A portion and the polymer B portion are not covalently bonded is a polymer in which the polymer B portion is encapsulated or enveloped by the polymer A portion. Specifically, a polymer having a core-shell structure (hereinafter also referred to as a "core-shell polymer") in which one of the polymer A portion and the polymer B portion is contained in the core portion and the other is contained in the shell portion is included. The "core-shell structure" is a structure in which a portion called a core (core portion) is encapsulated in a portion called a shell (shell portion).

[0017] Among these, the polymer (X) is preferably a core-shell polymer, in which the polymer A portion constitutes the shell portion of the core-shell polymer and the polymer B portion constitutes the core portion of the core-shell polymer. If the polymer (X) is such a core-shell polymer, the polymer (X) is easily dispersed in the resin composition, and the impact resistance of the molded article is further improved. In addition, the polymer (X) can be easily handled as a powder. A preferred embodiment of the polymer (X) having a core-shell structure will be described in detail below as a typical example.

[0018] <Polymer A part> The polymer A portion contains a structural unit (hereinafter also referred to as "structural unit (a1)") derived from a vinyl monomer (a1) having a structural unit represented by the following formula (1). That is, the polymer A portion is composed of a polymer A containing the structural unit (a1). When the polymer A portion contains the structural unit (a1), the scratch hardness of the molded article is improved and the Charpy impact strength and dart impact strength are also improved. -CO(CH 2 ) 5 O-···(1)

[0019] As the vinyl monomer (a1), a monomer represented by the following formula (2) is preferred from the viewpoint of polymerizability. CH 2 =CR 1 COO(CH 2 ) q O[CO(CH 2 ) 5 O] n H (2) (In formula (2), R 1 represents a hydrogen atom or a methyl group, q represents an integer of 2 to 5, and n represents an integer of 1 or more. In formula (2), R 1 is preferably a methyl group, and n is preferably an integer of 1 to 5.

[0020] Examples of the monomer represented by the formula (2) include an adduct (hydroxy group-containing monomer) in which ε-caprolactone is added to an unsaturated fatty acid hydroxyalkyl ester such as 2-hydroxyethyl (meth)acrylate. Commercially available products can be used as such monomers, and examples thereof include those under the trade names "PLACCEL FA1", "PLACCEL FA2", "PLACCEL FA3", "PLACCEL FA4", "PLACCEL FA5", "PLACCEL FM1", "PLACCEL FM2", "PLACCEL FM3", "PLACCEL FM4", and "PLACCEL FM5" manufactured by Daicel Corporation. These vinyl monomers (a1) may be used alone or in combination of two or more.

[0021] It is preferable that the polymer A portion further contains a structural unit (hereinafter also referred to as "structural unit (a2)") derived from an alkyl (meth)acrylate (a2) (hereinafter also referred to as "monomer (a2)") having an alkyl group having 1 to 10 carbon atoms. In other words, it is preferable that the polymer A further contains the structural unit (a2). When the polymer A portion further contains the structural unit (a2), the scratch hardness of the molded article is further improved, and the Charpy impact strength and dart impact strength are also improved.

[0022] Examples of the monomer (a2) include alkyl acrylate monomers such as methyl acrylate, ethyl acrylate, n-propyl acrylate, n-butyl acrylate, 2-ethylhexyl acrylate, cyclohexyl acrylate, and n-octyl acrylate; and alkyl methacrylate monomers such as methyl methacrylate, ethyl methacrylate, n-propyl methacrylate, n-butyl methacrylate, hexyl methacrylate, cyclohexyl methacrylate, and 2-ethylhexyl methacrylate. These monomers (a2) may be used alone or in combination of two or more.

[0023] The content of the structural unit (a1) is preferably 1 to 30 mass% and the content of the structural unit (a2) is preferably 70 to 99 mass% relative to the total mass of all structural units constituting the polymer A portion (i.e., polymer A). When the contents of the structural units (a1) and (a2) are within the above ranges, entanglement at the molecular level between the polymer (X) and the polycarbonate resin (Y) described below is promoted, and the Charpy impact strength and dart impact strength of the molded article are improved. The content of the structural unit (a1) is more preferably 1 to 20 mass%, and even more preferably 5 to 15 mass%, while the content of the structural unit (a2) is more preferably 80 to 99 mass%, and even more preferably 85 to 95 mass%.

[0024] The polymer A portion may further contain a structural unit derived from a monomer (a3) ​​other than the vinyl monomer (a1) and the monomer (a2) (hereinafter, also referred to as "structural unit (a3)"). That is, the polymer A may further contain the structural unit (a3). The monomer (a3) ​​is not particularly limited as long as it is copolymerizable with at least one of the vinyl monomer (a1) and the monomer (a2), and examples thereof include aromatic vinyls such as styrene and α-methylstyrene; (meth)acrylate compounds such as (meth)acrylic acid and phenyl (meth)acrylate; unsaturated nitriles such as acrylonitrile and methacrylonitrile; vinyl ethers such as methyl vinyl ether and butyl vinyl ether; vinyl halides such as vinyl chloride and vinyl bromide; vinylidene halides such as vinylidene chloride and vinylidene bromide; and vinyl monomers having a glycidyl group such as glycidyl acrylate, glycidyl methacrylate, allyl glycidyl ether, and ethylene glycol glycidyl ether. Furthermore, crosslinkable monomers such as aromatic polyfunctional vinyl compounds such as divinylbenzene and divinyltoluene; polyhydric alcohols such as ethylene glycol dimethacrylate and 1,3-butanediol diacrylate; allyl carboxylate esters such as trimethacrylate, triacrylate, allyl acrylate and allyl methacrylate; and di- and triallyl compounds such as diallyl phthalate, diallyl sebacate and triallyl triazine can also be used in combination. These monomers (a3) ​​may be used alone or in combination of two or more.

[0025] <Polymer B part> The polymer B portion contains a structural unit (hereinafter also referred to as "structural unit (b1)") derived from a vinyl monomer (b1) different from the vinyl monomer (a1). That is, the polymer B portion is composed of a polymer B containing the structural unit (b1).

[0026] Examples of the vinyl monomer (b1) include conjugated diene compounds such as butadiene and isoprene; aromatic vinyls such as styrene and α-methylstyrene; alkyl (meth)acrylates such as butyl acrylate and 2-ethylhexyl acrylate; unsaturated nitriles such as acrylonitrile and methacrylonitrile; vinyl ethers such as methyl vinyl ether and butyl vinyl ether; vinyl halides such as vinyl chloride and vinyl bromide; vinylidene halides such as vinylidene chloride and vinylidene bromide; and vinyl monomers having a glycidyl group such as glycidyl acrylate, glycidyl methacrylate, allyl glycidyl ether, and ethylene glycol glycidyl ether. Furthermore, crosslinkable monomers such as aromatic polyfunctional vinyl compounds, such as divinylbenzene and divinyltoluene; polyhydric alcohols, such as ethylene glycol dimethacrylate and 1,3-butanediol diacrylate; allyl carboxylate esters, such as trimethacrylate, triacrylate, allyl acrylate and allyl methacrylate; and di- and triallyl compounds, such as diallyl phthalate, diallyl sebacate and triallyl triazine, can also be used in combination. Among these, from the viewpoint of the Charpy impact strength and dart impact strength of the molded article, it is preferable that the polymer B portion contains a constitutional unit derived from butadiene. These vinyl monomers (b1) may be used alone or in combination of two or more.

[0027] The content of the butadiene-derived structural units is preferably 40 to 100 mass% relative to the total mass of all structural units constituting the polymer B portion (i.e., polymer B), and the content of the structural units derived from vinyl monomers (b1) other than butadiene is preferably 0 to 60 mass%. If the content of the butadiene-derived structural units is equal to or greater than the above lower limit, sufficient impact resistance is likely to be obtained. The content of the structural units derived from butadiene is more preferably from 50 to 100% by mass, and further preferably from 60 to 100% by mass.

[0028] Polymer B is preferably composed of a polymer having a glass transition temperature of not more than 0° C. When the glass transition temperature of the polymer B portion is not more than the above upper limit, the impact strength and dart impact strength of the molded article tend to be better. The glass transition temperature of Polymer B is a value measured by differential scanning calorimetry (DSC) according to a method in accordance with JIS K 7121:2012.

[0029] Polymer B is preferably a rubber-like polymer, and specific examples thereof include butadiene rubber, styrene-butadiene copolymer rubber, silicone rubber, silicone-acrylic composite rubber (obtained by polymerizing one or more vinyl monomers including acrylate in the presence of a polymer obtained from a monomer mainly composed of dimethylsiloxane), acrylonitrile-butadiene copolymer rubber, acrylic rubber such as polybutyl acrylate, polyisoprene, polychloroprene, ethylene-propylene rubber, ethylene-propylene-diene terpolymer rubber, styrene-butadiene block copolymer, styrene-isoprene block copolymer rubber, and other block copolymers, as well as hydrogenated products thereof. Among these, butadiene rubber, styrene-butadiene copolymer rubber, acrylic-butadiene copolymer rubber, and silicone-acrylic composite rubber, each of which has a glass transition temperature of -20°C or lower, are preferred, with butadiene rubber being more preferred, since improvement in the impact strength of molded products at lower temperatures (below -20°C) is required, particularly in cold regions. These rubber-like polymers may be used alone or in combination of two or more.

[0030] <Content> When the total of the polymer A portion and the polymer B portion is taken as 100% by mass, the content of the polymer A portion is preferably 10 to 50% by mass, and the content of the polymer B portion is preferably 50 to 90% by mass. When the contents of the polymer A portion and the polymer B portion are within the above ranges, the dispersibility of the polymer (X) in the resin composition is improved, and the impact resistance of the molded article is improved. The content of the polymer A portion is more preferably 10 to 40 mass %, and further preferably 10 to 35 mass %, while the content of the polymer B portion is more preferably 60 to 90 mass %, and further preferably 65 to 90 mass %.

[0031] <Particle size> When the polymer (X) is a core-shell polymer, the average primary particle size of the core-shell polymer is preferably 100 to 500 nm. If the primary particle size is within the above range, scattering during blending or charging into a mixing device when preparing a resin composition can be suppressed, and dust explosions and the like are less likely to occur. In addition, the flow characteristics of the core-shell polymer are good, and clogging of pipes and the like during the production process can be suppressed. The average primary particle diameter of the core-shell polymer is more preferably more than 200 nm and not more than 500 nm, more preferably more than 200 nm and not more than 400 nm, further preferably 210 to 400 nm, and particularly preferably 210 to 350 nm. The average primary particle size of the core-shell polymer can be adjusted, for example, by adjusting the amount of emulsifier or adding an enlarger in the production of the core-shell polymer by emulsion polymerization.

[0032] The average primary particle size of the core-shell polymer can be measured by a particle size analyzer using the dynamic light scattering method or a capillary particle size distribution analyzer using the CHDF (Capillary HydroDynamic Fractionation) method. In this specification, the average primary particle size of the core-shell polymer is a value of the harmonic mean particle size based on the scattered light intensity calculated by cumulant analysis after measuring with a particle size distribution measuring device by dynamic light scattering. This measurement is performed, for example, using a concentrated particle size analyzer FPAR-1000 (manufactured by Otsuka Electronics Co., Ltd.) and calculating by analysis processing with the attached software.

[0033] <Method for producing polymer (X)> The method for producing the polymer (X) having a core-shell structure is not particularly limited, and the polymer can be produced by known methods such as suspension polymerization, solution polymerization, and emulsion polymerization. Among these, from the viewpoint of ease of production, production by emulsion polymerization is preferred. Specifically, it is preferred to produce the polymer (X) by graft polymerization, preferably emulsion polymerization, of the monomer component (m2) constituting the polymer A in the presence of the polymer B. That is, the polymer (X) is preferably a polymer obtained by emulsion polymerization of the monomer component (m2) in the presence of the polymer B.

[0034] (Production of Polymer B) Polymer B can be obtained, for example, by emulsion polymerization of the monomer component (m1) that constitutes polymer B. The monomer component (m1) contains a vinyl monomer (b1). The monomer component (m1) preferably contains butadiene, and may further contain, in addition to butadiene, one or more vinyl monomers (b1) other than butadiene that can be copolymerized with butadiene, as necessary. The content of butadiene relative to the total mass of the monomer component (m1) is preferably from 40 to 100 mass%, more preferably from 50 to 100 mass%, and further preferably from 60 to 100 mass%. The content of the vinyl monomer (b1) other than butadiene relative to the total mass of the monomer component (m1) is preferably from 0 to 60 mass%, more preferably from 0 to 50 mass%, and even more preferably from 0 to 40 mass%.

[0035] The emulsion polymerization of the monomer component (m1) is preferably carried out in the presence of a polymerization initiator. The polymerization initiator is not particularly limited as long as it is one used in general radical polymerization. Examples of the polymerization initiator include persulfates such as potassium persulfate (potassium peroxodisulfate), sodium persulfate, and ammonium persulfate; oil-soluble azo compounds such as azobisisobutyronitrile, 2,2'-azobis(2-methylbutyronitrile), 2,2'-azobis(2,4-dimethylvaleronitrile), 2,2'-azobis(4-methoxy-2,4-dimethylvaleronitrile), and 2-phenylazo-4-methoxy-2,4-dimethylvaleronitrile; 2,2'-azobis{2-methyl-N-[1,1-bis(hydroxymethyl)-2-hydroxyethyl]propionamide}, 2,2'-azobis{2-methyl-N-[2-(1-hydroxyethyl)]propionamide}, and 2,2'-azobis{2-methyl-N-[2-(1-hydroxyethyl)]propionamide}. water-soluble azo compounds such as 2,2'-azobis[2-(5-methyl-2-imidazolin-2-yl)propane] and its salts, 2,2'-azobis[2-(2-imidazolin-2-yl)propane] and its salts, 2,2'-azobis{2-[1-(2-hydroxyethyl)-2-imidazolin-2-yl]propane} and its salts, 2,2'-azobis(2-methylpropynamidine) and its salts, and 2,2'-azobis[N-(2-carboxyethyl)-2-methylpropionamidine]; and organic peroxides such as benzoyl peroxide, cumene hydroperoxide, t-butyl hydroperoxide, t-butyl peroxy-2-ethylhexanoate, and t-butyl peroxyisobutyrate. These polymerization initiators may be used alone or in combination of two or more. When an organic peroxide is used as a polymerization initiator, it can be used as a redox polymerization initiator in combination with a reducing agent such as ferrous sulfate or isoascorbic acid.

[0036] The emulsion polymerization of the monomer component (m1) is preferably carried out in the presence of an emulsifier. The emulsifier is not particularly limited, but examples thereof include anionic surfactants such as fatty acid salts, alkyl sulfate salts, alkylbenzene sulfonates, alkyl phosphate salts, and dialkyl sulfosuccinate salts; nonionic surfactants such as polyoxyethylene alkyl ethers, polyoxyethylene fatty acid esters, sorbitan fatty acid esters, and glycerin fatty acid esters; and cationic surfactants such as alkylamine salts. These emulsifiers may be used alone or in combination of two or more kinds.

[0037] In the emulsion polymerization of the monomer component (m1), a chain transfer agent may be further used in combination for the purpose of adjusting the molecular weight. Examples of the chain transfer agent include t-dodecyl mercaptan, n-octyl mercaptan, and α-methylstyrene. These chain transfer agents may be used alone or in combination of two or more.

[0038] The reaction temperature during emulsion polymerization is not particularly limited, but is preferably from 45 to 90°C, and more preferably from 50 to 85°C, for example. The reaction time during emulsion polymerization is not particularly limited, but is preferably, for example, 30 minutes to 8 hours, and more preferably 1 to 6 hours.

[0039] (Emulsion polymerization of monomer component (m2)) The monomer component (m2) contains a monomer (a1). The monomer component (m2) preferably further contains a monomer (a2) in addition to the monomer (a1). The monomer component (m2) may further contain a monomer (a3) ​​as necessary. The content of the monomer (a1) relative to the total mass of the monomer component (m2) is preferably from 1 to 30 mass%, more preferably from 1 to 20 mass%, and even more preferably from 5 to 15 mass%. The content of the monomer (a2) relative to the total mass of the monomer component (m2) is preferably from 70 to 99 mass%, more preferably from 80 to 99 mass%, and even more preferably from 85 to 95 mass%.

[0040] When the total of polymer B and monomer component (m2) is 100% by mass, the content of monomer component (m2) is preferably 10 to 50% by mass, more preferably 10 to 40% by mass, and further preferably 10 to 35% by mass. When the total of polymer B and the monomer component (m2) is taken as 100 mass %, the content of polymer B is preferably from 50 to 90 mass %, more preferably from 60 to 90 mass %, and further preferably from 65 to 90 mass %.

[0041] The emulsion polymerization of the monomer component (m2) is preferably carried out in the presence of an emulsifier. If necessary, the emulsion polymerization of the monomer component (m2) may be carried out in the presence of a polymerization initiator. As the emulsifier and the polymerization initiator, the emulsifier and the polymerization initiator exemplified above in the description of the production of the polymer (B) can be mentioned. In addition, in the emulsion polymerization of the monomer component (m2), a chain transfer agent may be further used in combination for the purpose of adjusting the molecular weight. Examples of the chain transfer agent include the chain transfer agents exemplified above in the explanation of the production of the polymer (B).

[0042] The reaction temperature during emulsion polymerization of the monomer component (m2) is not particularly limited, but is preferably from 45 to 90°C, and more preferably from 50 to 85°C, for example. The reaction time during emulsion polymerization of the monomer component (m2) is not particularly limited, but is preferably, for example, 30 minutes to 8 hours, and more preferably 1 to 6 hours.

[0043] The particle size may be adjusted by adding an enlargement agent when the monomer component (m2) is emulsion-polymerized. Various types of thickening agents can be used, including, for example, acid group-containing copolymers and oxyacid salts. Examples of acid group-containing copolymers include copolymers having acrylic acid, methacrylic acid, itaconic acid, or the like as components. Examples of oxyacid salts include alkali metal salts or alkaline earth metal salts of oxyacids, or one or more oxyacid salts selected from the group consisting of zinc, nickel, and aluminum. Specific examples of oxyacid salts include potassium salts, sodium salts, magnesium salts, calcium salts, nickel salts, and aluminum salts of oxyacids such as sulfuric acid, nitric acid, and phosphoric acid. These thickening agents may be used alone or in combination of two or more.

[0044] By emulsion polymerizing the monomer component (m2) in the presence of the polymer B, the polymer (X) is obtained in the form of a latex. The method for recovering the polymer (X) from the latex of the polymer (X) is not particularly limited, but for example, the latex of the polymer (X) can be dried by a spray drying method or a freeze drying method, or coagulated to obtain the polymer (X) as a powder. Among these, drying or coagulation by the spray drying method is preferred. In addition, when the polymer (X) is composed of only the polymer A portion, for example, the above-mentioned monomer component (m2) is emulsion polymerized in the presence of a polymerization initiator and an emulsifier to obtain the polymer (X) composed of the polymer A.

[0045] [Polycarbonate resin (Y)] The polycarbonate resin (Y) has an isosorbide skeleton. When the polycarbonate resin (Y) has an isosorbide skeleton, the scratch hardness of the molded article is improved. The polycarbonate resin (Y) having an isosorbide skeleton is preferably a polycarbonate resin containing a structural unit (hereinafter also referred to as "structural unit (c)") derived from a dihydroxy compound (hereinafter also referred to as "compound (c)") represented by the following formula (3). The polycarbonate resin (Y) may be composed only of the structural unit (c), i.e., a homopolycarbonate of the compound (c), or may be a polycarbonate resin containing, in addition to the structural unit (c), a structural unit other than the structural unit (c) (hereinafter, also referred to as a "copolymer polycarbonate resin"). From the viewpoint of further improving the impact resistance of the molded article, the polycarbonate resin (Y) is preferably a copolymer polycarbonate resin.

[0046] [ka]

[0047] Examples of compound (c) include stereoisomeric isosorbide, isomannide, isoidet, etc. Among these, isosorbide obtained by dehydration condensation of sorbitol produced from various starches, which are abundant and easily available as plant-derived resources, is most preferred in terms of availability and ease of production, weather resistance, optical properties, moldability, heat resistance, and carbon neutrality. These compounds (c) may be used alone or in combination of two or more.

[0048] When the polycarbonate resin (Y) is a copolymeric polycarbonate resin, the copolymeric polycarbonate resin is preferably a copolymeric polycarbonate resin containing the structural unit (c) and a structural unit (hereinafter also referred to as "structural unit (d)") derived from one or more dihydroxy compounds (hereinafter also referred to as "compound (d)") selected from the group consisting of aliphatic hydrocarbon dihydroxy compounds, alicyclic hydrocarbon dihydroxy compounds, and ether-containing dihydroxy compounds. Since the compound (d) has a flexible molecular structure, the toughness of the resulting polycarbonate resin (Y) can be improved by using the compound (d) as a raw material. Among the compounds (d), aliphatic hydrocarbon dihydroxy compounds and alicyclic hydrocarbon dihydroxy compounds, which have a large effect of improving toughness, are preferred, and alicyclic hydrocarbon dihydroxy compounds are more preferred.

[0049] Examples of aliphatic hydrocarbon dihydroxy compounds include straight-chain aliphatic dihydroxy compounds such as ethylene glycol, 1,3-propanediol, 1,2-propanediol, 1,4-butanediol, 1,5-heptanediol, 1,6-hexanediol, 1,9-nonanediol, 1,10-decanediol, and 1,12-dodecanediol; and branched-chain aliphatic dihydroxy compounds such as 1,3-butanediol, 1,2-butanediol, neopentyl glycol, and hexylene glycol. These aliphatic hydrocarbon dihydroxy compounds may be used alone or in combination of two or more.

[0050] Examples of dihydroxy compounds of alicyclic hydrocarbons include dihydroxy compounds which are primary alcohols of alicyclic hydrocarbons, such as dihydroxy compounds derived from terpene compounds, such as 1,2-cyclohexanedimethanol, 1,3-cyclohexanedimethanol, 1,4-cyclohexanedimethanol, tricyclodecane dimethanol, pentacyclopentadecane dimethanol, 2,6-decalin dimethanol, 1,5-decalin dimethanol, 2,3-decalin dimethanol, 2,3-norbornane dimethanol, 2,5-norbornane dimethanol, 1,3-adamantanedimethanol, and limonene; and dihydroxy compounds which are secondary or tertiary alcohols of alicyclic hydrocarbons, such as 1,2-cyclohexanediol, 1,4-cyclohexanediol, 1,3-adamantanediol, hydrogenated bisphenol A, and 2,2,4,4-tetramethyl-1,3-cyclobutanediol. These alicyclic hydrocarbon dihydroxy compounds may be used alone or in combination of two or more.

[0051] Examples of the ether-containing dihydroxy compound include oxyalkylene glycols and dihydroxy compounds containing an acetal ring. Examples of the oxyalkylene glycol include diethylene glycol, triethylene glycol, tetraethylene glycol, polyethylene glycol, and polypropylene glycol. These ether-containing dihydroxy compounds may be used alone or in combination of two or more.

[0052] In the polycarbonate resin (Y), the content of the structural unit (c) relative to 100 mol% of all structural units derived from dihydroxy compounds is preferably 30 mol% or more, more preferably 40 to 95 mol%, even more preferably 45 to 90 mol%, and particularly preferably 60 to 85 mol%. If the content of the structural unit (c) is within the above range, the content of biogenic substances can be further increased, and heat resistance can be further improved. The content of the structural unit (c) in the polycarbonate resin (Y) may be 100 mol %, but from the viewpoint of further increasing the molecular weight and further improving the impact resistance of the molded article, it is preferable that the polycarbonate resin (Y) further contains a structural unit other than the structural unit (c) (for example, the above-mentioned structural unit (d)).

[0053] The polycarbonate resin (Y) may further contain a structural unit (hereinafter also referred to as "structural unit (e)") derived from a dihydroxy compound (hereinafter also referred to as "compound (e)") other than the compounds (c) and (d). Examples of the compound (e) include dihydroxy compounds containing aromatic groups. However, when the polycarbonate resin (Y) contains a large amount of structural units derived from dihydroxy compounds containing aromatic groups, it becomes difficult to obtain a polycarbonate resin (Y) having a high molecular weight due to the above-mentioned reasons, and the effect of improving the impact resistance of the molded article may decrease. Therefore, from the viewpoint of further improving the impact resistance of the molded article, the content ratio of structural units derived from dihydroxy compounds containing aromatic groups is preferably 10 mol% or less, more preferably 5 mol% or less, relative to 100 mol% of all structural units derived from dihydroxy compounds.

[0054] The glass transition temperature of the polycarbonate resin (Y) is preferably 90°C or higher. If the glass transition temperature of the polycarbonate resin (Y) is equal to or higher than the above lower limit, the heat resistance and the content of biogenic substances of the resin composition can be improved in a well-balanced manner. From the same viewpoint, the glass transition temperature of the polycarbonate resin (Y) is more preferably 100°C or higher, further preferably 110°C or higher, and particularly preferably 120°C or higher. On the other hand, the glass transition temperature of the polycarbonate resin (Y) is preferably 170°C or lower. If the glass transition temperature of the polycarbonate resin (Y) is equal to or lower than the above upper limit, the melt viscosity can be reduced by the above-mentioned melt polymerization, and a polymer with a sufficient molecular weight can be obtained. In addition, when an attempt is made to increase the molecular weight by increasing the polymerization temperature to reduce the melt viscosity, the effect of improving the heat resistance by the structural unit (c) cannot be sufficiently obtained, and coloring may occur easily. From the viewpoint of achieving a better balance between improving the molecular weight and preventing coloration, the glass transition temperature of the polycarbonate resin (Y) is more preferably 165° C. or lower, further preferably 160° C. or lower, and particularly preferably 150° C. or lower. The glass transition temperature of the polycarbonate resin (Y) is a value calculated from the FOX formula using values ​​given in Polymer Handbook (J. Brandrup, Interscience, 1989).

[0055] The molecular weight of the polycarbonate resin (Y) can be expressed by reduced viscosity, and the higher the reduced viscosity, the higher the molecular weight. The reduced viscosity is usually 0.30 dL / g or more, and preferably 0.33 dL / g or more. If the reduced viscosity of the polycarbonate resin (Y) is equal to or higher than the above lower limit, the mechanical strength of the molded article can be further improved. On the other hand, the reduced viscosity is usually 1.20 dL / g or less, more preferably 1.00 dL / g or less, and even more preferably 0.80 dL / g or less. If the reduced viscosity of the polycarbonate resin (Y) is equal to or lower than the above upper limit, the flowability during molding of the resin composition can be improved, and the productivity and moldability can be further improved. The reduced viscosity of polycarbonate resin (Y) is a value measured using an Ubbelohde viscometer at a temperature of 20.0°C ± 0.1°C using a solution in which the concentration of polycarbonate resin (Y) is precisely adjusted to 0.6 g / dL using methylene chloride as a solvent.

[0056] The melt viscosity of the polycarbonate resin (Y) is preferably 400 to 3000 Pa·s. If the melt viscosity of the polycarbonate resin (Y) is within the above range, the molded body can be prevented from becoming brittle and the mechanical properties can be further improved. In addition, the flowability during molding of the resin composition can be improved, and the molded body can be prevented from being damaged in appearance or from having a deteriorated dimensional accuracy. Furthermore, coloring and foaming caused by an increase in resin temperature due to shear heating can be further prevented. From the same viewpoint, the melt viscosity of the polycarbonate resin (Y) is more preferably 600 to 2500 Pa·s, and even more preferably 800 to 2000 Pa·s. The melt viscosity of the polycarbonate resin (Y) is measured using a capillary rheometer at a temperature of 240°C and a shear rate of 91.2 sec -1 The melt viscosity is measured at 100° C. An example of a capillary rheometer is a product called “Capilograph” manufactured by Toyo Seiki Seisakusho Co., Ltd.

[0057] When the total of the polymer (X) and the polycarbonate resin (Y) is taken as 100% by mass, the content of the polymer (X) is preferably 1 to 30% by mass, and the content of the polycarbonate resin (Y) is preferably 70 to 99% by mass. If the contents of the polymer (X) and the polycarbonate resin (Y) are within the above ranges, the Charpy impact strength and dart impact strength of the molded article are further improved. The content of the polymer (X) is more preferably 1 to 20 mass%, further preferably 1 to 15 mass%, and particularly preferably 5 to 15 mass%, while the content of the polycarbonate resin (Y) is more preferably 80 to 99 mass%, further preferably 85 to 99 mass%, and particularly preferably 85 to 95 mass%.

[0058] The total content of the polymer (X) and the polycarbonate resin (Y) is preferably from 60 to 100 mass %, more preferably from 65 to 100 mass %, based on the total mass of the resin composition.

[0059] [Optional ingredients] Examples of the optional components include various well-known additives such as stabilizers, flame retardants, flame retardant assistants, hydrolysis inhibitors, antistatic agents, foaming agents, dyes, and pigments. These optional components may be used alone or in combination of two or more.

[0060] The content of the optional components in the resin composition is preferably from 0 to 40 mass %, more preferably from 0 to 35 mass %, based on the total mass of the resin composition.

[0061] [Method of producing resin composition] The resin composition can be produced, for example, by mixing or melt-kneading the polymer (X), the polycarbonate resin (Y), and, if necessary, any optional components. For the mixing or melt-kneading, for example, a tumbler, a V-type blender, a super mixer, a Nauta mixer, a Banbury mixer, a kneading roll, an extruder, or the like can be used.

[0062] [Effects] The resin composition of the present embodiment described above contains the above-mentioned polymer (X) and polycarbonate resin (Y). Therefore, by using the resin composition of the present embodiment, a molded article having high scratch hardness and good both of Charpy impact strength and dart impact strength can be obtained.

[0063] "Molded body" A molded article according to one embodiment of the present invention contains the above-mentioned resin composition according to the present invention. The molded article can be obtained by molding the resin composition into a desired shape. Examples of the molding method include injection molding, extrusion molding, blow molding, calendar molding, and other methods commonly used for molding thermoplastic resin compositions.

[0064] The molded article of the present embodiment contains the resin composition of the present invention, and therefore has high scratch hardness and is excellent in both Charpy impact strength and dart impact strength. The molded article of the present embodiment can be widely used industrially as various materials in the fields of automobiles, office automation equipment, home appliances, electrical and electronics, construction, lifestyle and cosmetics, medical supplies, etc. More specific uses of the molded article include automobile interior and exterior parts, office equipment, home appliances, building materials, etc. In particular, the molded article of the present invention is suitable for automobile interior and exterior parts because it has excellent Charpy impact strength and dart impact strength. Examples of automobile exterior parts include fenders, bumpers, fascias, door panels, side garnishes, pillars, radiator grilles, side protectors, side moldings, rear protectors, rear moldings, various spoilers, bonnets, roof panels, trunk lids, detachable tops, window reflectors, mirror housings, outer door handles, etc. Examples of automobile interior parts include instrument panels, center console panels, meter parts, various switches, car navigation parts, car audio-visual parts, auto mobile computer parts, etc. EXAMPLES

[0065] The present invention will be described in more detail below with reference to Production Examples and Examples. However, the present invention is not limited to the following Examples. In the following Examples, unless otherwise specified, "parts" means "parts by mass" and "%" means "% by mass".

[0066] [Measurement and Evaluation] <Measurement of average primary particle size> Measurement was performed at room temperature using a particle size distribution measuring device using a dynamic light scattering method (manufactured by Otsuka Electronics Co., Ltd., product name "Concentrated System Particle Size Analyzer FPAR-1000"), and the harmonic mean particle size based on the scattered light intensity calculated by cumulant analysis was taken as the average primary particle size of the core-shell polymer.

[0067] <Charpy impact test> The pelletized resin composition was fed into an injection molding machine (manufactured by Sumitomo Heavy Industries, Ltd., product name "Sumitomo Injection Molding Machine SE100DU") to obtain a molded body (test piece) of 80 mm length × 10 mm width × 4 mm thickness at a cylinder temperature of 240° C. and a mold temperature of 60° C. A Charpy impact test was performed using the obtained test piece as follows. The Charpy impact test was performed in accordance with ISO 179-1:2023, using a TYPE A notch in accordance with ISO 2818:2018, and the Charpy impact strength of the molded body was evaluated according to the following criteria. ◯: Charpy impact strength is 20kJ / m 2 That's all. ×: Charpy impact strength is 20 kJ / m 2 is less than.

[0068] <Surface impact test> The pelletized resin composition was fed into an injection molding machine (manufactured by Sumitomo Heavy Industries, Ltd., product name "Sumitomo Injection Molding Machine SE100DU") to obtain a molded body (test piece) of 100 mm length × 50 mm width × 2 mm thickness at a cylinder temperature of 240° C. and a mold temperature of 60° C. A surface impact test was performed using the obtained test piece as follows. The surface impact test was carried out using a DuPont impact tester (manufactured by Toyo Seiki Seisakusho Co., Ltd., product name "DuPont Impact Tester H-100") with a striker having a hemispherical tip with a diameter of 5 inches and a test specimen support table with an inner diameter of 10 inches. The tip of the striker was brought into horizontal contact with the test specimen cooled to the measurement temperature (23°C or 0°C), and then a 5 kg weight was allowed to fall vertically from a position of 1500 mm, and the form of destruction was visually confirmed. The fracture morphology was determined according to the classification described in ISO 6603-2:2000. Test pieces whose mechanical behavior was YD, YS, or YU were classified as having ductile fracture. The proportion of such fractures was measured, and the dart impact strength of the molded bodies was evaluated according to the following criteria. Good: The ductile fracture rate in a surface impact test at 0°C is 40% or more. ×: The ductile fracture rate in a surface impact test at 0° C. is less than 40%.

[0069] <Scratch hardness measurement test> The pellet-like resin composition was fed into an injection molding machine (manufactured by Sumitomo Heavy Industries, Ltd., product name "Sumitomo Injection Molding Machine SE100DU") to obtain a molded body (test piece) of 100 mm length × 50 mm width × 2 mm thickness at a cylinder temperature of 240° C. and a mold temperature of 60° C. The obtained test piece was used to perform a scratch hardness measurement test as follows. The scratch hardness measurement test was performed using an electric pencil scratch hardness tester (manufactured by Yasuda Seiki Seisakusho Co., Ltd.) in accordance with JIS K 5600-5-4:1999. After the test, the surface of the molded body was visually observed and the scratch hardness of the molded body was evaluated according to the following evaluation criteria. ◯: The surface of the molded product is not scratched when scratched with a 3B pencil. ×: When scratched with a 3B pencil, the surface of the molded product was scratched.

[0070] [Production of polybutadiene rubber latex (B-1)] Into a pressure resistant autoclave, 100 parts of 1,3-butadiene, 0.3 parts of t-dodecyl mercaptan, 0.28 parts of cumene hydroperoxide, 0.3 parts of tetrasodium pyrophosphate, 0.0036 parts of ferrous sulfate, 0.39 parts of sodium sulfate, 0.24 parts of glucose, 1.25 parts of potassium rosinate, 1.25 parts of potassium tallowate, and 200 parts of deionized water were charged and reacted with stirring at 53° C. for 12 hours to obtain a polybutadiene rubber latex (B-1).

[0071] [Production of Acid Group-Containing Copolymer Latex (K-1)] In a glass reactor equipped with a reflux condenser, 1.67 parts of potassium tallowate, 2.5 parts of sodium dioctyl sulfosuccinate, 0.3 parts of sodium formaldehyde sulfoxylate, 0.003 parts of ferrous sulfate, 0.009 parts of disodium ethylenediaminetetraacetate, and 196 parts of deionized water were charged, and the temperature inside the glass reactor was raised with stirring until the temperature reached 60° C. Next, a mixture consisting of 85 parts of n-butyl acrylate, 15 parts of methacrylic acid, and 0.5 parts of cumene hydroperoxide was continuously added to the mixture of the raw materials over a period of 2 hours, and the mixture was maintained for another 2 hours to carry out polymerization, thereby obtaining an acid group-containing copolymer latex (K-1).

[0072] [Production Example 1] <Production of Core-Shell Polymer (X-1)> 222 parts of polybutadiene rubber latex (B-1) (70 parts as charged monomer component) was charged into a glass reaction vessel (separable flask) equipped with a stirrer and a reflux condenser. The atmosphere in the separable flask was replaced with nitrogen by passing a nitrogen gas flow through the separable flask. 4.24 parts of acid group-containing copolymer latex (K-1) was added, the liquid temperature was raised to 40°C, and then maintained for 10 minutes. Next, an aqueous solution consisting of 0.94 parts of dipotassium alkenyl succinate and 27 parts of deionized water was added, and the liquid temperature was raised to 80°C. Furthermore, an aqueous solution consisting of 0.09 parts of sodium formaldehyde sulfoxylate dihydrate and 3.8 parts of deionized water was added. Then, a mixture of 27 parts of methyl methacrylate, 3 parts of unsaturated fatty acid hydroxyalkyl ester modified ε-caprolactone, and 0.11 parts of t-butyl hydroperoxide was added dropwise to the reaction vessel over 60 minutes, followed by heating and stirring for 120 minutes. In this manner, the monomer component (m2) containing the vinyl monomer (a1) and the monomer (a2) was graft polymerized onto the polybutadiene rubber, which is a rubber-like polymer, to obtain a core-shell polymer latex (X-1). The dipotassium alkenylsuccinate used was manufactured by Kao Corporation under the trade name "Latemul ASK," the t-butyl hydroperoxide used was manufactured by NOF Corporation under the trade name "Perbutyl H," and the unsaturated fatty acid hydroxyalkyl ester modified ε-caprolactone used was manufactured by Daicel Corporation under the trade name "Placcel FM1."

[0073] 2.2 parts of stabilizer emulsion were added to 288.18 parts of the obtained core-shell polymer latex (X-1) and mixed. Then, an aqueous solution of 5 parts of calcium acetate and 173 parts of deionized water was heated to 90°C, and the core-shell polymer latex (X-1) containing the stabilizer emulsion was added to the aqueous solution to form a slurry. The liquid temperature was raised to 95°C and held for 5 minutes to aggregate the slurry. The aggregate was collected, immersed in 1500 parts of deionized water, and the dehydration process was repeated twice, and the core-shell polymer (X-1) powder was obtained by drying at a temperature of 60°C for 12 hours. The average primary particle size of the core-shell polymer (X-1) was measured, and the results are shown in Table 1.

[0074] [Manufacturing Examples 2 to 6] <Core-shell polymers (X-2) to (X-5), (B-2)> Except for changing the graft composition to the components shown in Table 1, the same procedure as in Production Example 1 was repeated to obtain powders of the core-shell polymers (X-2) to (X-5) and (B-2). The average primary particle diameters of the obtained core-shell polymers (X-2) to (X-5) and (B-2) were measured. The results are shown in Table 1.

[0075] [Table 1]

[0076] The abbreviations in the table are as follows: The blending amount of Bd (polybutadiene rubber latex (B-1)) in the table is calculated as a pure content, that is, the amount (parts) as a charged monomer component. ·Bd: Polybutadiene rubber latex (B-1). ·MMA: Methyl methacrylate. FM1: unsaturated fatty acid hydroxyalkyl ester modified ε-caprolactone (manufactured by Daicel Corporation, trade name "Placcel FM1", 1 mol of 2-hydroxyethyl methacrylate adduct with caprolactone; in the formula (2), R 1 is a methyl group, q is 2, and n is 1, which corresponds to the vinyl monomer (a1). FM3: unsaturated fatty acid hydroxyalkyl ester modified ε-caprolactone (manufactured by Daicel Corporation, trade name "Placcel FM3", 3 mol of 2-hydroxyethyl methacrylate adduct with caprolactone; in the formula (2), R 1 is a methyl group, q is 2, and n is 3, which corresponds to the vinyl monomer (a1). FM5: unsaturated fatty acid hydroxyalkyl ester modified ε-caprolactone (manufactured by Daicel Corporation, trade name "Placcel FM5", 5 mol of 2-hydroxyethyl methacrylate adduct with caprolactone; in the formula (2), R 1is a methyl group, q is 2, and n is 5, which corresponds to the vinyl monomer (a1).

[0077] [Example 1] A mixture was obtained by blending the core-shell polymer (X-1) and a polycarbonate resin having an isosorbide skeleton (manufactured by Mitsubishi Chemical Corporation, product name "DURABIO D7340R", content of structural unit (c) 70 mol%) in the composition shown in Table 2. The resulting mixture was fed to a devolatilizing twin-screw extruder (manufactured by Ikegai Corporation, product name "PCM-30") heated to a barrel temperature of 240°C and kneaded to produce pellets of the resin composition of Example 1 blended with 10% by mass of the core-shell polymer. The pelletized resin composition was used to prepare a molded article, which was then subjected to a Charpy impact test, a dart impact test, and a scratch hardness measurement test. The results are shown in Table 2.

[0078] [Examples 2 to 6, Comparative Examples 1 and 2] Pellets of the resin composition were prepared in the same manner as in Example 1, except that the formulation was changed as shown in Tables 2 and 3, and the Charpy impact test, dart impact test, and scratch hardness measurement test were performed. The results are shown in Tables 2 and 3.

[0079] [Comparative Examples 3 and 4] A mixture was obtained by blending the core-shell polymer (X-1) or (X-4) and a polycarbonate resin not having an isosorbide skeleton (manufactured by Mitsubishi Engineering Plastics Corporation, product name "Iupilon S2000F") in the composition shown in Table 3. The resulting mixture was fed to a devolatilizing twin-screw extruder (manufactured by Ikegai Corporation, product name "PCM-30") heated to a barrel temperature of 280°C and kneaded to prepare pellets of the resin compositions of Comparative Examples 3 and 4 in which the core-shell polymer was blended at 10% by mass. The pelletized resin composition was used to prepare a molded article, which was then subjected to a Charpy impact test, a dart impact test, and a scratch hardness measurement test. The results are shown in Table 3.

[0080] [Table 2]

[0081] [Table 3]

[0082] The abbreviations in the table are as follows. DURABIO D7340R: Polycarbonate resin with an isosorbide skeleton (manufactured by Mitsubishi Chemical Corporation, product name "DURABIO D7340R", structural unit (c) / structural unit derived from 1,4-cyclohexanedimethanol = 70 / 30 mol%, glass transition temperature 120°C). The glass transition temperature was calculated from the FOX formula using the values ​​given in the Polymer Handbook (J. Brandrup, Interscience, 1989). Iupilon S2000F: Polycarbonate resin that does not have an isosorbide structure (manufactured by Mitsubishi Engineering Plastics Corporation, product name "Iupilon S2000F").

[0083] It was confirmed from the results of Examples 1 to 6 that the resin composition of the present invention can provide a molded article having high scratch hardness and excellent in both Charpy impact strength and dart impact strength. It was confirmed that the resin composition of Comparative Example 1, which did not contain the polymer (X), was inferior in Charpy impact strength. In Comparative Example 2, since the polymer (B-2) not containing the structural unit (a1) was used, it was confirmed that the dart impact strength was poor. In Comparative Examples 3 and 4, since a polycarbonate resin not having an isosorbide skeleton was used, it was confirmed that the scratch hardness was poor.

Claims

1. A polymer (X) having a polymer A portion including a structural unit derived from a vinyl monomer (a1) having a structural unit represented by the following formula (1), A polycarbonate resin (Y) having an isosorbide skeleton, A resin composition comprising: -CO(CH 2 ) 5 O- ・・・(1)

2. The resin composition according to claim 1, wherein the polymer (X) further has a polymer B portion containing a structural unit derived from a vinyl monomer (b1) different from the vinyl monomer (a1).

3. 3. The resin composition according to claim 2, wherein the content of the polymer A portion is 10 to 50 mass%, and the content of the polymer B portion is 50 to 90 mass%, when the total of the polymer A portion and the polymer B portion is 100 mass%.

4. The polymer (X) is a core-shell polymer, The resin composition according to claim 2 , wherein the polymer A portion constitutes a shell portion of the core-shell polymer, and the polymer B portion constitutes a core portion of the core-shell polymer.

5. The resin composition according to claim 4, wherein the average primary particle diameter of the core-shell polymer is 100 to 500 nm.

6. The polymer A portion further contains a structural unit derived from an alkyl (meth)acrylate (a2) having an alkyl group having 1 to 10 carbon atoms, The resin composition according to claim 1, wherein the content of the structural units derived from the vinyl monomer (a1) is 1 to 30 mass% and the content of the structural units derived from the alkyl (meth)acrylate (a2) is 70 to 99 mass% relative to the total mass of all structural units constituting the polymer A portion.

7. The resin composition according to claim 1, wherein the vinyl monomer (a1) is a monomer represented by the following formula (2): CH 2 =CR 1 P. 2 ) q P.S. 2 ) 5 O] n H ・・・(22) (In formula (2), R 1 represents a hydrogen atom or a methyl group, q represents an integer of 2 to 5, and n represents an integer of 1 or more.

8. R in the formula (1) 1 The resin composition according to claim 7, wherein is a methyl group.

9. The resin composition according to claim 7, wherein n in the formula (1) is an integer of 1 to 5.

10. The resin composition according to claim 1, wherein the content of the polymer (X) is 1 to 30 mass%, and the content of the polycarbonate resin (Y) is 70 to 99 mass%, when the total of the polymer (X) and the polycarbonate resin (Y) is 100 mass%.

11. A molded article comprising the resin composition according to any one of claims 1 to 10.

Citation Information

Patent Citations

  • Rubber-containing graft polymer, resin composition containing rubber-containing graft polymer, and molded article of same

    WO2019131374A1

Cited By

  • Method for manufacturing substrate with cured film, substrate with cured film, photosensitive resin composition, cured film formed by curing photosensitive resin composition, and display device having cured film or substrate with cured film

    JP2020166255A

  • Method for manufacturing a substrate with a cured film, a substrate with a cured film, a photosensitive resin composition, a cured film obtained by curing the photosensitive resin composition, and a display device having a cured film or a substrate with a cured film.

    JP7844098B2