Polyolefin-based resin molding material, method for producing polyolefin-based resin molding material, and molded body

By modifying PET bottle caps with an ethylene copolymer, the resin's flexibility and durability are enhanced, allowing for expanded applications and safe recycling into various products.

JP2024144387AInactive Publication Date: 2024-10-11JAPAN POLYETHYLENE CORP
View PDF 14 Cites 0 Cited by

Patent Information

Application Number
JP2024055194
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Priority Date
2023-03-29
Filing Date
2024-03-29
Publication Date
2024-10-11
Estimated Expiration
Not applicable · inactive patent

AI Technical Summary

Technical Problem

The challenge of recycling PET bottle caps made of polyolefin resin is hindered by variations in physical properties, particularly impact resistance and durability, which limits their application beyond their original use as caps, and the inclusion of contaminants complicates safe recycling.

Method used

A polyolefin resin molding material is produced by modifying recovered PET bottle caps with an ethylene copolymer, using a metallocene catalyst to enhance flexibility, impact resistance, and durability, achieving a composition with specific structural unit proportions and melt flow rates.

Benefits of technology

The modified resin exhibits improved flexibility, impact resistance, and durability, enabling broader applications beyond traditional PET bottle caps, while ensuring safety and hygiene for food packaging.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024144387000001
    Figure 2024144387000001
  • Figure 2024144387000002
    Figure 2024144387000002
  • Figure 2024144387000003
    Figure 2024144387000003
Patent Text Reader

Abstract

To provide a polyolefin-based resin molding material made by modifying a recovered polyolefin-based resin derived from recovered PET bottle caps to make it flexible and improve its impact resistance and durability (stress crack resistance).SOLUTION: A polyolefin-based resin molding material contains a recovered polyolefin-based resin derived from recovered polyolefin-based resin caps of PET bottles, and a modifier made of a specific ethylene copolymer. The content of the modifier is 1 to 99 mass% based on the total amount of the recovered polyolefin-based resin and the modifier.SELECTED DRAWING: None
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a polyolefin-based resin molding material and a manufacturing method thereof, and a molded article obtained by molding the polyolefin-based resin molding material. More specifically, the present invention relates to a recycled polyolefin-based resin molding material obtained by modifying a polyolefin-based recovered resin obtained by crushing or pelletizing recovered PET bottle caps, preferably by a material recycling method, a manufacturing method for the resin molding material, and a molded article obtained by molding the resin molding material. [Background technology]

[0002] Plastic containers, particularly PET (polyethylene terephthalate) bottles, have been in high demand as containers for soft drinks and the like since they were approved as containers for food and beverages due to their excellent mechanical strength, transparency, high gas barrier properties, non-pollution properties, etc. Small PET bottles in particular are highly used by consumers as small portable containers for beverages, and as the heat resistance and pressure resistance of PET bottles have been improved, they are also widely used as containers for portable hot beverages in winter and high-temperature sterilized beverages for long-term storage.

[0003] In the past, PET containers for soft drinks such as carbonated drinks were made of metals such as aluminum for the container lids, but polyolefin lids are now widely used for economic reasons. For containers for soft drinks, etc., essential performance requirements are hermetic sealing, ease of opening, food safety, and durability, and for lid members, technical improvements have been continuously studied for polyethylene resin lid members from the viewpoints of not only these performances but also various physical properties such as moldability, rigidity, and heat resistance, and a great number of improvements have been proposed.

[0004] Polyethylene-based resin molding materials suitable for PET bottle caps must be excellent in terms of high-speed moldability, high fluidity, rigidity, impact resistance, durability (stress crack resistance), slipperiness, low odor, food safety, and openability, and various resin molding materials have been investigated so far (for example, Patent Documents 1, 2, and 3).

[0005] Meanwhile, with the growing awareness of environmental issues in recent years, the recycling of resin products has also attracted attention, and various material recycling methods are being considered. For example, Patent Document 4 discloses a method for modifying used agricultural films mainly composed of polyethylene resins, in which an ethylene-vinyl acetate copolymer is added to pulverized used agricultural films. Patent Document 5 discloses a method for modifying plastic waste, which is a miscellaneous polyolefin resin containing polyethylene and / or polypropylene as a main material and polybutyl terephthalate and / or polyacetal resin as a secondary material, by adding polyethylene and / or an olefin thermoplastic elastomer as an additive resin to the plastic waste. [Prior art documents] [Patent documents]

[0006] [Patent Document 1] Patent No. 4926360 [Patent Document 2] Patent No. 4928858 [Patent Document 3] Patent No. 6167930 [Patent Document 4] JP 2022-173177 A [Patent Document 5] JP 2022-114370 A Summary of the Invention [Problem to be solved by the invention]

[0007] While PET bottle caps made from polyethylene resin have become widespread and widely used, in recent years, greater importance has been placed on environmental and recycling considerations for resin products, due to issues such as marine plastic waste and the need to reduce the use of virgin resin based on concepts such as the circular economy and carbon neutrality. There is also a growing demand for PET bottle caps to be recycled and used effectively as a plastic resource, rather than being discarded as single-use disposables.

[0008] PET bottle caps, along with PET bottle containers, are widely collected and recycled, and compared to other resin products, efforts are being made to use resources more effectively. However, collected PET bottle caps are a collection of products with various physical properties, from high to low, and therefore have problems in terms of performance, especially impact resistance and durability (stress crack resistance), and it is difficult to recycle them as PET bottle caps as they are, that is, to carry out so-called cap-to-cap recycling.

[0009] In addition, it is essential that safety and hygiene are guaranteed for packaging products for beverages or food, including PET bottle caps. If contaminated PET bottle caps or other foreign objects are mixed in during sorting and collection, cap-to-cap recycling is difficult from the perspective of safety and hygiene. Therefore, since strict quality control is required to implement cap-to-cap recycling, it is difficult to recycle all PET bottle caps, and in reality, recycling for uses other than beverage or food packaging products is also being promoted.

[0010] However, since collected PET bottle caps are resin molded articles with physical properties suitable for PET bottle caps, it is difficult to directly repurpose them for other uses. In particular, since PET bottle caps have excellent rigidity, it is difficult to apply them to applications that require flexibility, and the applicable applications are limited in their current state. Therefore, in order to apply them to a variety of applications, it is necessary to adjust the performance of collected PET bottle caps by adding some other resin material to them. Note that, when carrying out this modification, it is not sufficient to simply make them soft or adjust other properties. As mentioned above, collected PET bottle caps have variations in impact resistance and durability (stress crack resistance), so it is necessary to improve their performance by modification to a level where these properties do not become a problem. Therefore, it is not possible to use a modifier that reduces impact resistance and durability (stress crack resistance) when added.

[0011] In view of the state of the prior art, the present invention aims to provide a polyolefin-based resin molding material in which recovered polyolefin resin is regenerated as a base resin by homogenizing recovered PET bottle caps using material recycling techniques, for example, by crushing or pelletizing the recovered polyolefin resin, and the recovered polyolefin resin is modified to make it softer and improve its impact resistance and durability (stress crack resistance); and to provide a method for producing the polyolefin-based resin molding material, and a molded article obtained by molding the polyolefin-based resin molding material. [Means for solving the problem]

[0012] As a result of extensive research conducted by the present inventors to solve the above problems, it was discovered that polyolefin-based recovered resin, which is regenerated by crushing or pelletizing recovered PET bottle caps, can be modified by adding a modifier made of a specific ethylene-based copolymer to increase its flexibility, and that the polyolefin-based resin obtained by modification has superior impact resistance and significantly superior durability (stress crack resistance) compared to the raw material polyolefin-based recovered resin.

[0013] That is, the present invention provides the following polyolefin resin molding material. [1] A polyolefin-based resin molding material comprising a polyolefin-based recovered resin derived from recovered polyolefin-based resin caps of PET bottles, and a modifier made of an ethylene-based copolymer having the following characteristics (a), (b), and (c), wherein the content of the modifier is 1 to 99 mass% based on the total amount of the polyolefin-based recovered resin and the modifier. (a) The proportion of structural units derived from ethylene as a major component is 80 to 98 mol %, the proportion of structural units derived from an α-olefin having 4 to 12 carbon atoms as an essential minor component is 0.1 to 7 mol %, the proportion of structural units derived from propylene as an optional minor component is 19.9 to 0 mol %, and the total of the structural units derived from the ethylene, the structural units derived from the α-olefin, and the structural units derived from the propylene is 100 mol %. (b) The melt flow rate (MFR) (temperature: 190°C, load: 2.16 kg) is 0.1 to 100 g / 10 min. (c) Density is 0.880 to 0.940 g / cm 3 It is.

[0014] [2] A polyolefin-based resin molding material comprising a polyolefin-based recovered resin obtained by homogenizing post-market recovered polyolefin-based resin caps of PET bottles, and a modifier made of an ethylene-based copolymer having the following characteristics (a), (b), and (c), wherein the content of the modifier is 1 to 99 mass% based on the total amount of the polyolefin-based recovered resin and the modifier: (a) The proportion of structural units derived from ethylene as a major component is 80 to 98 mol %, the proportion of structural units derived from an α-olefin having 4 to 12 carbon atoms as an essential minor component is 0.1 to 7 mol %, the proportion of structural units derived from propylene as an optional minor component is 19.9 to 0 mol %, and the total of the structural units derived from the ethylene, the structural units derived from the α-olefin, and the structural units derived from the propylene is 100 mol %. (b) The melt flow rate (MFR) (temperature: 190°C, load: 2.16 kg) is 0.1 to 100 g / 10 min. (c) Density is 0.880 to 0.940 g / cm3 It is.

[0015] [3] The polyolefin resin molding material according to [1] or [2], wherein the modifier is an ethylene copolymer polymerized using a metallocene catalyst. [4] The polyolefin resin molding material according to any one of [1] to [3], which has an environmental stress crack resistance (ESCR) of 200 hours or more. [5] The polyolefin resin molding material according to any one of [1] to [4], which has the following characteristics (A) and (B): (A) The melt flow rate (MFR) (temperature 190°C, load 2.16 kg) is 0.1 to 100 g / 10 min. (B) Density is 0.880 to 0.970 g / cm 3 It is.

[0016] The present invention also provides the following method for producing a polyolefin resin molding material. [6] preparing a polyolefin-based recovered resin derived from recovered polyolefin-based resin caps of PET bottles; a step of preparing a modifier comprising an ethylene-based copolymer by polymerizing, using a metallocene catalyst, a monomer component having a ratio of 80 to 98 mol % of ethylene as a main component, a ratio of 0.1 to 7 mol % of an α-olefin having 4 to 12 carbon atoms as an essential subcomponent, and a ratio of 19.9 to 0 mol % of propylene as an optional subcomponent, the total of the ethylene, the α-olefin, and the propylene being 100 mol %; and mixing the polyolefin-based recovered resin with the modifier in a mass ratio such that the amount of the modifier is 1 to 99 mass% relative to the total amount of the polyolefin-based recovered resin and the modifier.

[0017] [7] A step of preparing a polyolefin-based recovered resin obtained by homogenizing a polyolefin-based resin cap of a PET bottle that has been collected from the market; a step of preparing a modifier comprising an ethylene-based copolymer by polymerizing, using a metallocene catalyst, a monomer component having a ratio of 80 to 98 mol % of ethylene as a main component, a ratio of 0.1 to 7 mol % of an α-olefin having 4 to 12 carbon atoms as an essential subcomponent, and a ratio of 19.9 to 0 mol % of propylene as an optional subcomponent, the total of the ethylene, the α-olefin, and the propylene being 100 mol %; and mixing the polyolefin-based recovered resin with the modifier in a mass ratio such that the amount of the modifier is 1 to 99 mass% relative to the total amount of the polyolefin-based recovered resin and the modifier.

[0018] The present invention also provides the following molded article. [8] A molded article obtained by molding the polyolefin resin molding material according to any one of [1] to [5]. Effect of the Invention

[0019] According to the present invention, it is possible to provide a polyolefin-based resin molding material in which polyolefin-based recovered resin derived from recovered polyolefin-based resin caps of PET bottles is modified to make it flexible and improve its impact resistance and durability (stress crack resistance). Furthermore, according to the present invention, it is possible to provide a method for producing the polyolefin-based resin molding material, and a molded article obtained by molding the polyolefin-based resin molding material. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0020] The characteristics of the polyolefin resin molding material of the present invention will be specifically described in detail below. In the present invention, the term "to" indicating a range of values ​​is used to mean that the values ​​before and after the range include the lower limit and upper limit.

[0021] The polyolefin-based resin molding material of the present invention is a resin composition comprising a polyolefin-based recycled resin derived from recycled polyolefin-based resin caps of PET bottles, and a modifier comprising the following ethylene-based copolymer, the content of the modifier being 1 to 99 mass% based on the total amount of the polyolefin-based recycled resin and the modifier. [Modifier made of ethylene copolymer] The modifier used in the present invention is an ethylene copolymer having the following characteristics (a), (b), and (c). (a) The proportion of structural units derived from ethylene as a major component is 80 to 98 mol %, the proportion of structural units derived from an α-olefin having 4 to 12 carbon atoms as an essential minor component is 0.1 to 7 mol %, the proportion of structural units derived from propylene as an optional minor component is 19.9 to 0 mol %, and the total of the structural units derived from ethylene, the structural units derived from the α-olefin having 4 to 12 carbon atoms, and the structural units derived from propylene is 100 mol %. (b) The melt flow rate (MFR) (temperature: 190°C, load: 2.16 kg) is 0.1 to 100 g / 10 min. (c) Density is 0.880 to 0.940 g / cm 3 It is.

[0022] The polyolefin-based resin molding material of the present invention is a resin composition modified by adding a modifier made of the specific ethylene-based copolymer described above to polyolefin-based recovered resin regenerated by crushing or pelletizing recovered PET bottle caps, and has higher flexibility and better impact resistance than the raw material polyolefin-based recovered resin, and is particularly significantly superior in durability (stress crack resistance). In the polyolefin resin molding material of the present invention, by adjusting the physical properties and the amount of the modifier, it is possible to obtain a resin molding material having physical properties similar to existing flexible polyethylenes such as existing linear low density polyethylene (LLDPE) or existing high density polyethylene (HDPE) whose rigidity is lower than that of a PET bottle cap. Moreover, the polyolefin resin molding material of the present invention modified to have physical properties similar to those of existing polyethylenes has the same or better impact resistance and excellent durability (stress crack resistance) compared to existing polyethylenes having the desired physical properties. Therefore, polyolefin-based resin molding materials obtained by modifying polyolefin-based recovered resin, which is regenerated by crushing or pelletizing collected PET bottle caps, using the method of the present invention can be used in applications where existing polyethylene is used, or in applications where existing polyethylene could not be used due to its insufficient impact resistance or durability (stress crack resistance). Therefore, according to the modification method of the present invention, it is possible to expand the applicable uses of the modified polyolefin-based resin to beyond the raw material PET bottle caps, making it possible to utilize recovered PET bottle caps in a wide range of fields.

[0023] 1. Polyolefin-based recycled resin In the present invention, polyolefin-based recovered resin derived from recovered polyolefin-based resin caps of PET bottles is modified. For example, in the present invention, polyolefin-based recovered resin obtained by homogenizing recovered polyolefin-based resin caps of PET bottles from the market is modified. In the present invention, recovered polyolefin-based resin caps for PET bottles may refer to market recovered polyolefin-based resin caps for PET bottles, specifically, polyolefin-based resin caps separated and recovered from used PET bottles, or recovered discarded or surplus caps generated during the production stage of polyolefin-based resin caps for PET bottles or the production stage of PET bottle beverages using such caps, or a mixture of these. Resin caps for PET bottles are molded products of polyolefin resins such as polyethylene and polypropylene worldwide, and polyethylene caps are particularly widely used. Polyolefin resin caps can be separated and collected by known methods, for example, only polyolefin resin caps can be separated depending on the specific gravity difference of the resins forming the caps, and if necessary, only polyethylene resin caps can be separated. Among the polyolefin resin caps for PET bottles, it is preferable to use collected products separated only to polyethylene caps from the viewpoint of improving the quality of the polyolefin resin molding material obtained in the present invention.

[0024] In the present invention, the polyolefin-based recovered resin derived from recovered polyolefin-based resin caps is a polyolefin-based recovered resin obtained by homogenizing recovered polyolefin-based resin caps, for example, a polyolefin-based resin composition in which the resin composition, properties, and other materials are homogenized by returning recovered polyolefin-based resin caps, which are composed of various polyolefin-based resin caps with different qualities, to a state of raw resin by a method belonging to material recycling such as crushing or pelletizing. Therefore, the polyolefin-based recovered resin used in the present invention is, for example, a polyolefin-based recovered resin obtained by crushing or pelletizing recovered polyolefin-based resin caps. Recycled resins obtained by crushing and homogeneously mixing the separated and collected PET bottle caps and processing them into pellets are generally commercially available. In the present invention, such commercially available products may be used as the polyolefin-based recovered resin derived from the collected polyolefin-based resin caps.

[0025] The physical properties of polyolefin-based recovered resin obtained from recovered PET bottle caps vary greatly depending on the ratio of the cap products of different qualities that are mixed in, so it is not possible to give a generalized physical property value. For example, if the recovered product is mostly composed of polyethylene PET bottle cap products, the physical properties of the polyolefin-based recovered resin obtained from the recovered product will be close to those of polyethylene PET bottle caps, and if the recovered product is mostly composed of polypropylene PET bottle cap products, the physical properties of the polyolefin-based recovered resin obtained from the recovered product will be close to those of polypropylene PET bottle caps. In addition, if the collected products contain PET bottle caps with poor performance such as impact resistance and durability (stress crack resistance), such as cheap imported products, the above-mentioned performance of the polyolefin-based recovered resin obtained from the collected products will be pulled in a more inferior direction and will decline. Since collected products generally contain a certain amount of PET bottle caps with poor performance, the performance of polyolefin-based recovered resin obtained from collected PET bottle caps is often low in impact resistance and durability (stress crack resistance) for use as PET bottle caps, and many of them have too low durability (stress crack resistance) in particular.

[0026] The polyolefin-based recycled resin to be modified in the present invention is not particularly limited, but as described above, it is preferable that the recycled resin is obtained by homogenizing the recycled products separated and limited to polyethylene caps, for example, by crushing or pelletizing the recycled products separated and limited to polyethylene caps. That is, it is preferable that the recycled resin contains a polyethylene-based resin as a main component. The ratio of polyethylene resin contained in the polyolefin-based recovered resin is preferably 60% by mass or more, more preferably 70% by mass or more, even more preferably 80% by mass or more, and most preferably 90% by mass or more. The polyolefin-based recovered resin may contain a polypropylene-based resin as a secondary component. The ratio of the polypropylene-based resin contained in the polyolefin-based recovered resin is preferably 40% by mass or less, more preferably 30% by mass or less, even more preferably 20% by mass or less, and most preferably 10% by mass or less. From the viewpoint of using a polyolefin-based recovered resin with stable performance, the polyolefin-based recovered resin modified in the present invention preferably has a flexural modulus indicating rigidity of 900 to 1200 MPa and an environmental stress crack resistance (ESCR) indicating durability (stress crack resistance) of 15 to 35 hours (h). However, since the present invention does not assume cap-to-cap recycling, even if the polyolefin-based recovered resin does not satisfy the above flexural modulus or ESCR, it can be used by adjusting the type and / or amount of the modifier.

[0027] 2. Characteristics of modifiers made from ethylene copolymers The modifier used in the present invention is an ethylene copolymer having the following characteristics (a), (b), and (c). (a) The proportion of structural units derived from ethylene as a major component is 80 to 98 mol %, the proportion of structural units derived from an α-olefin having 4 to 12 carbon atoms as an essential minor component is 0.1 to 7 mol %, the proportion of structural units derived from propylene as an optional minor component is 19.9 to 0 mol %, and the total of the structural units derived from the ethylene, the structural units derived from the α-olefin, and the structural units derived from the propylene is 100 mol %. (b) The melt flow rate (MFR) (temperature: 190°C, load: 2.16 kg) is 0.1 to 100 g / 10 min. (c) Density is 0.880 to 0.940 g / cm 3 It is. In the present invention, as the modifier, the ethylene copolymer having the above characteristics (a), (b) and (c) can be used alone or in combination of two or more kinds.

[0028] The ethylene-based copolymer is preferably a random copolymer polymerized by a catalytic polymerization method using a metallocene catalyst and substantially randomly polymerized in a linear manner, from the viewpoint of excellent impact resistance and durability (stress crack resistance) improving effects.

[0029] (a) Monomer composition of ethylene copolymer The monomer composition of the ethylene-based copolymer used as the modifier in the present invention is such that the proportion of constituent units derived from ethylene as the main component is 80 to 98 mol %, the proportion of constituent units derived from an α-olefin having 4 to 12 carbon atoms as an essential minor component is 0.1 to 7 mol %, the proportion of constituent units derived from propylene as an optional minor component is 19.9 to 0 mol %, and the total of the constituent units derived from the ethylene, the constituent units derived from the α-olefin, and the constituent units derived from the propylene is 100 mol %. In addition, one or more types of α-olefins can be used as the structural unit derived from an α-olefin having 4 to 12 carbon atoms. In addition, the amount of monomer-derived structural units such as ethylene-derived structural units is 13 The values ​​were measured and calculated by C-NMR.

[0030] The ethylene copolymer used in the present invention may contain structural units derived from propylene. The copolymer having ethylene and propylene as structural components is so-called ethylene propylene rubber (EPM), which contains more than 20 mol% of propylene and has a density of 0.870 g / cm. 3 Rubber-like polymers obtained by the following solution polymerization method are used in the field of elastomers, but the ethylene-based copolymer used in the present invention is a polymer that is completely different from these ethylene-propylene rubbers in terms of density range, amount of ethylene and propylene contained therein, and physical properties. In addition, among propylene polymers, propylene-ethylene copolymers that contain a small amount of ethylene component during the production process are also known, but these are also polymers that are significantly different from the ethylene copolymer used in the present invention in terms of propylene content, etc., and are also completely different in physical properties, etc.

[0031] When the ethylene copolymer used in the present invention does not contain a structural unit derived from propylene as a minor component, the proportion of structural units derived from ethylene is preferably 93 to 98 mol%, and the proportion of structural units derived from an α-olefin having 4 to 12 carbon atoms is preferably 2 to 7 mol%. When the ethylene copolymer does not contain a structural unit derived from propylene as a minor component, the total of the structural units derived from ethylene and the structural units derived from an α-olefin having 4 to 12 carbon atoms is 100 mol%. When the ethylene copolymer does not contain a structural unit derived from propylene as a minor component, the proportion of structural units derived from ethylene is more preferably 94 to 97 mol%, and the proportion of structural units derived from an α-olefin having 4 to 12 carbon atoms is more preferably 3 to 6 mol%. When the ethylene copolymer used in the present invention contains structural units derived from propylene as a minor component, the proportion of structural units derived from ethylene is preferably 80 to 98 mol%, the proportion of structural units derived from α-olefins having 4 to 12 carbon atoms is preferably 0.1 to 7 mol%, and the proportion of structural units derived from propylene is preferably 19.9 to 0.1 mol%. When the ethylene copolymer contains structural units derived from propylene as a minor component, the proportion of structural units derived from ethylene is more preferably 80 to 95 mol%, and even more preferably 80 to 90 mol%, the proportion of structural units derived from α-olefins having 4 to 12 carbon atoms is more preferably 0.5 to 7 mol%, and even more preferably 1 to 6 mol%, and the proportion of structural units derived from propylene is more preferably 15 to 1 mol%, and even more preferably 14 to 2 mol%.

[0032] The α-olefin having 4 to 12 carbon atoms is not particularly limited, but specific examples include 1-butene, 1-pentene, 1-hexene, 1-octene, 1-heptene, 4-methyl-pentene-1, 4-methyl-hexene-1, 4,4-dimethylpentene-1, etc. Among them, linear α-olefins such as 1-butene, 1-pentene, 1-hexene, 1-octene, and 1-heptene are preferred. As the α-olefin having 4 to 12 carbon atoms, an α-olefin having 4 to 10 carbon atoms is preferable, and an α-olefin having 4 to 8 carbon atoms is more preferable.

[0033] Specific examples of the ethylene copolymer that does not contain a structural unit derived from propylene include binary copolymers such as ethylene / 1-butene copolymer, ethylene / 1-hexene copolymer, ethylene / 1-octene copolymer, and ethylene / 4-methyl-pentene-1 copolymer; and ternary copolymers such as ethylene / butene / hexene terpolymer and ethylene / butene / octene terpolymer. Specific examples of the ethylene copolymer containing a structural unit derived from propylene include terpolymers such as ethylene / propylene / butene terpolymer, ethylene / propylene / hexene terpolymer, and ethylene / propylene / octene terpolymer.

[0034] (b) Melt flow rate (MFR) of ethylene copolymer The melt flow rate (MFR) (temperature 190°C, load 2.16 kg) of the ethylene copolymer used in the present invention is 0.1 to 100 g / 10 min, preferably 1 to 80 g / 10 min, more preferably 1 to 60 g / 10 min, and even more preferably 3 to 40 g / 10 min. If the MFR is less than 0.1 g / 10 min, when the ethylene copolymer is kneaded and modified with a polyolefin-based recycled resin obtained from recovered polyolefin-based resin caps of PET bottles, the mixture becomes poor, and the MFR of the modified product decreases, resulting in poor moldability of the modified product, which is undesirable. On the other hand, if the MFR exceeds 100 g / 10 min, mixing will be poor when the polyolefin-based recovered resin obtained from recovered polyolefin-based resin caps of PET bottles is kneaded with the ethylene-based copolymer to modify it. In addition, since the ethylene-based copolymer with a high MFR has a low molecular weight, a sufficient modification effect cannot be obtained from the viewpoints of impact resistance and durability (stress crack resistance), which is not preferable. In order to adjust the MFR of the ethylene copolymer used in the present invention, for example, a method of appropriately adjusting the polymerization temperature or the amount of hydrogen (amount of chain transfer agent) coexisting during the copolymerization reaction can be used. By increasing the polymerization temperature, the molecular weight of the ethylene copolymer can be decreased, resulting in a larger MFR. On the other hand, by decreasing the polymerization temperature, the molecular weight of the ethylene copolymer can be increased, resulting in a smaller MFR. In addition, in the copolymerization reaction of ethylene with propylene or an α-olefin having 4 to 12 carbon atoms, the molecular weight can be decreased by increasing the amount of hydrogen (amount of chain transfer agent) coexisting, resulting in a larger MFR, and the molecular weight can be increased by decreasing the amount of hydrogen (amount of chain transfer agent) coexisting, resulting in a smaller MFR.

[0035] (c) Density of ethylene copolymer The density of the ethylene copolymer used in the present invention is 0.880 to 0.940 g / cm 3 and preferably 0.880 to 0.930 g / cm 3 and more preferably 0.880 to 0.920 g / cm 3The density is 0.880g / cm 3 If the density is less than 0.940 g / cm3, it is difficult to produce it industrially, which is not preferable. 3 When the density exceeds 100%, the impact resistance of the ethylene copolymer becomes insufficient and the ESCR becomes low, so that sufficient modifying effect cannot be obtained from the viewpoints of impact resistance and durability (stress crack resistance), which is not preferable. In order to adjust the density of the ethylene copolymer used in the present invention, for example, a method of appropriately adjusting the comonomer content, polymerization temperature, catalyst amount, etc. is used.

[0036] (d) Other physical properties The flexural modulus of the ethylene copolymer used in the present invention is not particularly limited, but is preferably 300 MPa or less, more preferably 200 MPa or less, and even more preferably 100 MPa or less. In this case, the flexibility improving effect of the ethylene copolymer is particularly excellent. The lower limit of the flexural modulus of the ethylene copolymer is not particularly limited, but is usually 20 MPa or more.

[0037] The ESCR of the ethylene copolymer used in the present invention is not particularly limited, but is preferably 1000 hours or more, in which case the ethylene copolymer has a particularly excellent effect of improving durability (stress crack resistance). Moreover, the ethylene copolymer used in the present invention preferably does not break in a Charpy impact strength test, in which case the impact resistance improving effect of the ethylene copolymer is particularly excellent.

[0038] In order to make the ethylene-based copolymer used in the present invention have the above-mentioned preferred physical properties, it is effective to produce the ethylene-based copolymer using a monomer component that satisfies the above (a) and employing the below-mentioned preferred polymerization catalyst and polymerization method.

[0039] 3. Polymerization catalyst and polymerization method for ethylene copolymer The ethylene copolymer used in the present invention is produced by polymerizing the monomer components satisfying the above condition (a) by a catalytic polymerization method. The monomer component satisfying the above (a) is a monomer component in which the proportion of ethylene as a main component is 80 to 98 mol %, the proportion of an α-olefin having 4 to 12 carbon atoms as an essential subcomponent is 0.1 to 7 mol %, the proportion of propylene as an optional subcomponent is 19.9 to 0 mol %, and the sum of the ethylene, the α-olefin, and the propylene is 100 mol %. The catalyst used in the production of the ethylene copolymer is preferably a metallocene catalyst. The metallocene catalyst is not particularly limited, but preferably contains a metallocene compound and a cocatalyst as catalyst components. As the metallocene compound, it is preferable to use a metallocene compound such as a zirconium compound or a hafnium compound coordinated with a group having a cyclopentadienyl skeleton, etc. As the cocatalyst, a boron compound such as N,N-dimethylanilinium tetrakis(pentafluorophenyl)borate is preferably used. Ethylene copolymers polymerized using metallocene catalysts are linear random copolymers that have characteristics such as narrow molecular weight distribution and comonomer composition distribution, low low molecular weight content, etc. In terms of specific performance, they have excellent characteristics such as excellent impact resistance and durability (stress crack resistance), low sticky components, and low solvent extractable components.

[0040] The method for producing the ethylene copolymer is not particularly limited, but since it is desirable to carry out the polymerization at a high temperature of 150 to 330°C, it is preferable to use a high-pressure ionic polymerization method ("Polyethylene Technology Reader," Chapter 4, edited by Kazuo Matsuura and Naotaka Mikami, 2001).

[0041] 4. Amount of modifier consisting of ethylene copolymer In the present invention, the content of the modifier is appropriately adjusted within the range of 1 to 99% by mass relative to the total amount of the polyolefin-based recovered resin and the modifier (100% by mass). More specifically, the content of the modifier is appropriately adjusted according to the physical property value of the polyolefin-based recovered resin, the target physical property value of the polyolefin-based resin molding material after modification, and the physical property value of the modifier used. In general, the higher the content of the modifier, the more flexible the modified product is, i.e., the lower the flexural modulus, and the more the impact resistance and durability (stress crack resistance) are improved.

[0042] Although not particularly limited, in order to obtain a polyolefin-based resin molding material having the desired physical properties by obtaining a sufficient modifying effect from the modifier while taking advantage of the characteristics of the polyolefin-based recovered resin, the content of the modifier is preferably 10 to 80 mass%, more preferably 20 to 70 mass%, relative to 100 mass% of the total amount of the polyolefin-based recovered resin and the modifier.

[0043] 5. Manufacturing of polyolefin resin molding materials The method for producing the polyolefin resin molding material of the present invention is not particularly limited, but may be, for example, A step of preparing a polyolefin-based recovered resin derived from recovered polyolefin-based resin caps of PET bottles; a step of preparing a modifier comprising an ethylene-based copolymer by polymerizing, using a metallocene catalyst, a monomer component having a ratio of 80 to 98 mol % of ethylene as a main component, a ratio of 0.1 to 7 mol % of an α-olefin having 4 to 12 carbon atoms as an essential subcomponent, and a ratio of 19.9 to 0 mol % of propylene as an optional subcomponent, the total of the ethylene, the α-olefin, and the propylene being 100 mol %; and mixing the polyolefin-based recovered resin with the modifier in a mass ratio such that the amount of the modifier is 1 to 99 mass% with respect to the total amount of the polyolefin-based recovered resin and the modifier. The above-mentioned steps of preparing the polyolefin-based recovered resin, preparing the modifier, and mixing the polyolefin-based recovered resin and the modifier do not have to be performed at the same place. The polyolefin-based recovered resin derived from recovered polyolefin-based resin caps of PET bottles used in the manufacturing method may be a polyolefin-based recovered resin obtained by homogenizing recovered polyolefin-based resin caps of PET bottles from the market. The polyolefin-based recovered resin used in the manufacturing method is, for example, a polyolefin-based recovered resin obtained by crushing or pelletizing recovered polyolefin-based resin caps of PET bottles.

[0044] The method for preparing polyolefin-based recovered resin derived from recovered polyolefin-based resin caps of PET bottles is not particularly limited. For example, polyolefin-based recovered resin may be prepared by crushing or pelletizing recovered polyolefin-based resin caps of PET bottles using a material recycling method, or a commercially available product of such polyolefin-based recovered resin may be prepared. The method for preparing the modifier made of an ethylene-based copolymer is as described above in "3. Polymerization catalyst and polymerization method for ethylene-based copolymer."

[0045] In the step of mixing the polyolefin-based recovered resin with the modifier (hereinafter sometimes simply referred to as the "mixing step"), the mixing method is not particularly limited, and the mixture is mixed uniformly according to a conventional method for producing a resin composition. The polyolefin-based resin molding material of the present invention contains, as essential components, the above-mentioned recycled polyolefin resin and the above-mentioned ethylene copolymer modifier, and may further contain other components as necessary. The other components are usually added during the above-mentioned mixing step. The above-mentioned mixing step is carried out, for example, by dry-blending or melt-blending the pellets of polyolefin-based recovered resin and the pellets of the modifier, and adding other components in any order during blending. In the case of dry-blending, the pellets of polyolefin-based recovered resin and the pellets of the modifier are finally melt-blended in a molding machine. The blending method is appropriately selected according to the manufacturing process. In the case of melt-blending, the obtained polyolefin-based resin molding material may be pelletized by processing with a pelletizer.

[0046] As the other components, for example, in order to further enhance various physical properties of the polyolefin resin molding material of the present invention or to impart other physical properties, polymers other than the modifier made of the polyolefin recycled resin or the ethylene copolymer may be blended in a conventional manner, and additives such as antioxidants (phenolic, phosphorus-based, sulfur-based, etc.), ultraviolet absorbers, light stabilizers, lubricants, antistatic agents, antifogging agents, antiblocking agents, processing aids, coloring pigments, crosslinking agents, foaming agents, inorganic or organic fillers, flame retardants, and nucleating agents for accelerating the crystallization rate may also be blended. When the polyolefin-based resin molding material of the present invention contains components other than the polyolefin-based recovered resin or modifier, the content of the other components is appropriately adjusted within a range that does not impair the object of the present invention, and is not particularly limited. The content of the polymer other than the polyolefin-based recovered resin or the modifier made of the ethylene copolymer is usually 30 parts by mass or less, preferably 20 parts by mass or less, and more preferably 10 parts by mass or less, relative to 100 parts by mass of the total amount of the polyolefin-based recovered resin and modifier, and the content of various additives is usually 5 parts by mass or less, preferably 3 parts by mass or less, and more preferably 1 part by mass or less.

[0047] 6. Uses of polyolefin resin molding materials and molded bodies The polyolefin resin molding material of the present invention is excellent in flexibility, impact resistance, and durability (stress crack resistance), and further, is excellent in moldability, high fluidity, etc. Therefore, the polyolefin resin molding material of the present invention is suitable for use as various molded articles such as industrial parts and daily necessities that require such properties, and molded articles obtained by molding the polyolefin resin molding material of the present invention are suitably used in applications that require flexibility, impact resistance, and durability (stress crack resistance). The polyolefin-based resin molding material of the present invention is intended to be mainly used for applications other than beverage or food packaging products. However, when the safety and hygiene of the raw material, recovered PET bottle caps, and the polyolefin-based recovered resin regenerated as a material resin by homogenizing the recovered PET bottle caps using a material recycling method are guaranteed, the polyolefin-based resin molding material of the present invention can also be used for beverage or food packaging products. The polyolefin-based resin molding material of the present invention is difficult to use for PET bottle caps because of its insufficient rigidity, but has good flexibility and can be used for applications such as hinge caps and various container inner lids that require flexibility.

[0048] 7. Characteristics of polyolefin resin molding materials The polyolefin resin molding material of the present invention is not particularly limited, but preferably has the following characteristics (A) and (B). (A) The melt flow rate (MFR) (temperature 190°C, load 2.16 kg) is 0.1 to 100 g / 10 min. (B) Density is 0.880 to 0.970 g / cm 3 It is.

[0049] (A) Melt flow rate (MFR) of polyolefin resin molding material The melt flow rate (MFR) (temperature 190°C, load 2.16 kg) of the polyolefin resin molding material of the present invention is preferably 0.1 to 100 g / 10 min. When the polyolefin resin molding material of the present invention has an MFR of not less than the lower limit, the moldability is good, and when the MFR is not more than the upper limit, deterioration of impact resistance and durability (stress crack resistance) is suppressed. From this viewpoint, the MFR of the polyolefin resin molding material of the present invention is more preferably 1 to 80 g / 10 min, further preferably 2 to 50 g / 10 min, and may be 2 to 10 g / 10 min. The MFR of the polyolefin resin molding material of the present invention can be adjusted, for example, by changing the MFR of the modifier used or by changing the ratio of the modifier. By increasing the MFR of the modifier, the MFR of the polyolefin resin molding material can be increased. On the other hand, by decreasing the MFR of the modifier, the MFR of the polyolefin resin molding material can be decreased. In addition, for example, when using a modifier with a higher MFR than the MFR of the polyolefin recycled resin, the MFR of the polyolefin resin molding material can be increased by increasing the ratio of the modifier.

[0050] (B) Density of polyolefin resin molding material The density of the polyolefin resin molding material of the present invention is 0.880 to 0.970 g / cm 3 In the polyolefin resin molding material of the present invention, when the density is equal to or higher than the lower limit, the decrease in the heat resistance temperature of the molded product is suppressed, and when the density is equal to or lower than the upper limit, the deterioration of impact resistance and durability (stress crack resistance) is suppressed. From such a viewpoint, the density of the polyolefin resin molding material of the present invention is more preferably 0.900 to 0.950 g / cm. 3 and more preferably 0.910 to 0.940 g / cm 3 It is. The density of the polyolefin resin molding material of the present invention can be adjusted, for example, by changing the density of the modifier used or by changing the ratio of the modifier.

[0051] The physical properties of the polyolefin resin molding material of the present invention are adjusted depending on the application and are not particularly limited, but it is preferable that the material satisfies the following physical properties because it has high versatility. The flexural modulus of the polyolefin resin molding material of the present invention is preferably 800 MPa or less, more preferably 600 MPa or less. The lower limit of the flexural modulus is not particularly limited, but is usually 200 MPa or more. The environmental stress crack resistance (ESCR) of the polyolefin resin molding material of the present invention is preferably 200 hours or more, more preferably 300 hours or more, even more preferably 500 hours or more, still more preferably 800 hours or more, and most preferably 1000 hours or more. The Charpy impact strength of the polyolefin resin molding material of the present invention is preferably 10 KJ / m 2 More than 30KJ / m 2 It is particularly preferable that the steel sheet does not break in a Charpy impact strength test. The tensile impact strength of the polyolefin resin molding material of the present invention is preferably 150 KJ / m 2 More preferably, 200KJ / m 2 That's all.

[0052] In the case of molding the polyolefin resin molding material of the present invention into a molded article, the molding method is not particularly limited, but it is mainly injection molding. EXAMPLES

[0053] The present invention will be described in more detail in the following examples and comparative examples, but the present invention is not limited thereto.

[0054] [Measurement and evaluation methods] The measurement and evaluation methods used in the examples and comparative examples are as follows. (1) Melt flow rate (MFR) at a temperature of 190°C and a load of 2.16 kg: Measured in accordance with JIS-K6922-2:1997. (2) Density: Measured in accordance with JIS-K6922-1, 2:1997. (3) Flexural modulus: A 4 mm x 10 mm x 80 mm plate specimen injection molded at 210°C was used as a test piece, and the measurement was performed in accordance with JIS-K6922-2:1997.

[0055] (4) Charpy impact strength: Measured in accordance with JIS-K7111-1:2006. (5) Tensile impact strength: Measured in accordance with JIS-K6922-2:1997. (6) Tensile yield stress: Measured in accordance with JIS-K6922-2:1997. (7) Nominal tensile strain at break: Measured in accordance with JIS-K6922-2:1997. (8)ESCR: Measured in accordance with ASTM D 1693 at a temperature of 50°C using a 10 vol% aqueous solution of IGEPAL CO-630 manufactured by SIGMA-ALDRICH as the working solution.

[0056] (9) Evaluation of flexibility improvement effect Based on the flexural modulus of the modified polyolefin resin molding material, the flexibility modification effect was evaluated according to the following evaluation criteria. [Evaluation Criteria] ◯ (Good): The flexural modulus was lower than that of the raw material polyolefin-based recycled resin. × (bad): The flexural modulus was equal to or increased compared to that of the raw material polyolefin-based recovered resin.

[0057] (10) Impact resistance improvement effect evaluation Based on the Charpy impact strength and tensile impact strength of the modified polyolefin resin molding material, the impact resistance modification effect was evaluated according to the following evaluation criteria. [Evaluation Criteria] ○ (Good): The Charpy impact strength or tensile impact strength was increased compared to that of the raw material polyolefin-based recovered resin. Note that if the raw material polyolefin-based recovered resin was destroyed in the Charpy impact strength test, but the modified polyolefin-based resin molding material is no longer destroyed in the Charpy impact strength test, this means that the Charpy impact strength has increased. × (bad): The Charpy impact strength and the tensile impact strength were equal to or lower than those of the raw material polyolefin-based recovered resin.

[0058] (11) Evaluation of durability (resistance to stress cracks) Based on the ESCR of the modified polyolefin resin molding material, the durability (stress crack resistance) modification effect was evaluated according to the following evaluation criteria. [Evaluation Criteria] ○ (Good): Increased compared with the ESCR of the raw material, polyolefin-based recovered resin. × (bad): The ESCR was equal to or lower than that of the raw material polyolefin-based recovered resin.

[0059] (12) Overall evaluation of reform effects The overall evaluation of the modifying effect of the polyolefin resin molding material was performed according to the following evaluation criteria. [Evaluation Criteria] ◯ (Good): In the modified polyolefin resin molding material, the flexibility modification effect was judged to be ◯, the impact resistance modification effect was judged to be ◯, and the durability (stress crack resistance) modification effect was judged to be ◯. × (bad): The modified polyolefin resin molding material had an × rating in at least one of the above-mentioned flexibility modification effect judgment, impact resistance modification effect judgment, or durability (stress crack resistance) modification effect judgment.

[0060] [Preparation of polyolefin-based recycled resin] Recovered polyolefin-based resin caps of PET bottles were crushed and pelletized using a material recycling method to homogenize them and regenerate them as a material resin. As a polyolefin-based recovered resin, "PET bottle cap HDPE-white pellets" (polyethylene resin content: 99% by mass or more) manufactured by Shin-Ei Kasei Co., Ltd. was prepared. In all of the examples and comparative examples described below, the "PET bottle cap HDPE-white pellets" were used as the polyolefin-based recovered resin. The physical properties of the "PET bottle cap HDPE-white pellets" are shown in Table 1.

[0061] [Preparation of catalyst] A catalyst solution was prepared by adding an equimolar amount of “N,N-dimethylanilinium tetrakis(pentafluorophenyl)borate” to 0.05 mol of the complex “rac-dimethylsilylenebisindenylhafnium dimethyl” prepared by the method described in JP-A-10-218921, and diluting the mixture to 50 liters with toluene.

[0062] [Production of Modifier A] A stirred autoclave type continuous reactor with an internal volume of 5.0 liters was used, the pressure inside the reactor was kept at 80 MPa, ethylene and 1-hexene were continuously fed into the reactor as raw material gas (monomer components) at 40 kg / h while appropriately adjusting the feed rate, and the catalyst solution prepared above was continuously fed into the reactor, and the polymerization temperature was appropriately adjusted within the range of 150 to 250 ° C., thereby obtaining an ethylene-based copolymer, modifier A. Modifier A was an ethylene-based copolymer having the above characteristics (a), (b), and (c). The monomer composition and physical properties of modifier A are shown in Table 2. In Tables 2 and 3, the C2 content is the content of structural units derived from ethylene, the C3 content is the content of structural units derived from propylene, and the C4-12 content is the content of structural units derived from α-olefins having 4 to 12 carbon atoms.

[0063] [Production of Modifier B] A stirred autoclave type continuous reactor with an internal volume of 5.0 liters was used, the pressure inside the reactor was kept at 80 MPa, ethylene, propylene and 1-hexene were continuously fed into the reactor as raw material gas (monomer components) at 40 kg / h while appropriately adjusting the feed rate, and the catalyst solution prepared above was continuously fed into the reactor, and the polymerization temperature was appropriately adjusted within the range of 150 to 250 ° C. to obtain an ethylene-based copolymer, modifier B. Modifier B was an ethylene-based copolymer having the above characteristics (a), (b) and (c). The monomer composition and physical properties of modifier B are shown in Table 2.

[0064] [Production of Modifier C] Modifier C, an ethylene-based copolymer, was obtained by adjusting the polymerization temperature according to the manufacturing method of Modifier B described above. Modifier C was an ethylene-based copolymer having the above characteristics (a), (b) and (c). The monomer composition and physical properties of Modifier C are shown in Table 2.

[0065] Example 1 The polyolefin-based recycled resin (PET bottle cap HDPE-white pellets) and the pellets of the modifier A were dry-blended in a mass ratio of 50:50 (polyolefin-based recycled resin: modifier), and then 70 g of the resulting mixture was put into the chamber of a roller mixer (trade name: Labo Plastomill (registered trademark), model: R100) manufactured by Toyo Seiki Co., Ltd., equipped with a small mixer with a capacity of 100 ml. At the same time, 0.14 g of an antioxidant (manufactured by BASF Japan, trade name: IRGANOX B225) was also put in. After preheating the inside of the chamber at 190 ° C. for 3 minutes, the put-in materials were melt-blended by kneading at 190 ° C. and 40 rpm for 2 minutes to obtain a polyolefin-based resin molding material of Example 1. The physical properties of the obtained resin molding material are shown in Table 2. The resin molding material of Example 1 had improved flexibility, i.e., a lower flexural modulus, improved impact resistance, and significantly improved durability (stress crack resistance), compared to the raw polyolefin-based recovered resin shown in Table 1, and had completely different physical properties from the raw polyolefin-based recovered resin. The resin molding material of Example 1 exhibited physical properties similar to those of UJ960, a grade of linear low-density polyethylene (LLDPE) manufactured by Japan Polyethylene Co., Ltd., but its impact resistance exceeded that of UJ960, and its durability (stress crack resistance) was significantly higher than that of UJ960. The physical properties of UJ960 are shown in Table 2. Therefore, the resin molding material of Example 1 obtained by modification is believed to be applicable to applications in which UJ960 is used, as well as applications in which UJ960 could not be used due to insufficient impact resistance or durability (stress crack resistance).

[0066] Example 2 A polyolefin-based resin molding material of Example 2 was obtained in the same manner as in Example 1, except that the mass ratio of the polyolefin-based recycled resin to the modifier (polyolefin-based recycled resin:modifier) ​​was changed to 30:70. The physical properties of the obtained resin molding material are shown in Table 2. The resin molding material of Example 2 had improved flexibility, i.e., a lower flexural modulus, improved impact resistance, and significantly improved durability (stress crack resistance), compared to the raw polyolefin-based recovered resin shown in Table 1, and had completely different physical properties from the raw polyolefin-based recovered resin. The resin molding material of Example 2 exhibited physical properties similar to those of UJ460, a grade of linear low-density polyethylene (LLDPE) manufactured by Japan Polyethylene Co., Ltd., but its impact resistance exceeded that of UJ460, and its durability (stress crack resistance) was significantly higher than that of UJ460. The physical properties of UJ460 are shown in Table 2. Therefore, the resin molding material of Example 2 obtained by modification is believed to be applicable to applications in which UJ460 is used, as well as applications in which UJ460 could not be used due to insufficient impact resistance or durability (stress crack resistance).

[0067] Example 3 A polyolefin-based resin molding material of Example 3 was obtained in the same manner as in Example 1, except that Modifier B was used instead of Modifier A and the mass ratio of the polyolefin-based recycled resin to the modifier (polyolefin-based recycled resin:modifier) ​​was changed to 80:20. The physical properties of the obtained resin molding material are shown in Table 2. The resin molding material of Example 3 had improved flexibility, i.e., a lower flexural modulus, improved impact resistance, and significantly improved durability (stress crack resistance), compared to the raw polyolefin-based recovered resin shown in Table 1, and had completely different physical properties from the raw polyolefin-based recovered resin. The resin molding material of Example 3 exhibited similar physical properties to HJ260, a grade of high density polyethylene (HDPE) manufactured by Japan Polyethylene Co., Ltd., but its impact resistance exceeded that of HJ260, and its durability (stress crack resistance) was significantly higher than that of HJ260. The physical properties of HJ260 are shown in Table 2. Therefore, the resin molding material of Example 3 obtained by modification is believed to be applicable to applications in which HJ260 is used, as well as applications in which HJ260 could not be used due to insufficient impact resistance or durability (stress crack resistance).

[0068] Example 4 A polyolefin-based resin molding material of Example 4 was obtained in the same manner as in Example 1, except that Modifier B was used instead of Modifier A and the mass ratio of the polyolefin-based recycled resin to the modifier (polyolefin-based recycled resin:modifier) ​​was changed to 45:55. The physical properties of the obtained resin molding material are shown in Table 2. The resin molding material of Example 4 had improved flexibility, i.e., a lower flexural modulus, improved impact resistance, and significantly improved durability (stress crack resistance), compared to the raw polyolefin-based recovered resin shown in Table 1, and had completely different physical properties from the raw polyolefin-based recovered resin. The resin molding material of Example 4 exhibited physical properties similar to those of UJ460, a grade of linear low-density polyethylene (LLDPE) manufactured by Japan Polyethylene Co., Ltd., but its impact resistance exceeded that of UJ460, and its durability (stress crack resistance) was significantly greater than that of UJ460. Therefore, the resin molding material of Example 4 obtained by modification is believed to be applicable to applications in which UJ460 is used, as well as applications in which UJ460 could not be used due to insufficient impact resistance or durability (stress crack resistance).

[0069] Example 5 A polyolefin resin molding material of Example 5 was obtained in the same manner as in Example 1, except that Modifier C was used instead of Modifier A. The physical properties of the obtained resin molding material are shown in Table 2. The resin molding material of Example 5 had improved flexibility, i.e., a lower flexural modulus, improved impact resistance, and significantly improved durability (stress crack resistance), compared to the raw polyolefin-based recovered resin shown in Table 1, and had completely different physical properties from the raw polyolefin-based recovered resin. The resin molding material of Example 5 exhibited physical properties similar to those of UJ460, a grade of linear low-density polyethylene (LLDPE) manufactured by Japan Polyethylene Co., Ltd., but its durability (stress crack resistance) was significantly superior to that of UJ460. Therefore, the resin molding material of Example 5 obtained by modification is believed to be applicable to applications in which UJ460 is used, as well as applications in which UJ460 could not be used due to its insufficient durability (stress crack resistance). The resin molding material of Example 2 also exhibits physical properties similar to those of UJ460. However, the resin molding material of Example 5 has a higher ratio of polyolefin-based recycled resin than Example 2, and uses a smaller amount of modifying material than Example 2, resulting in a material with improved flexibility to the same level as Example 2. The resin molding material of Example 4 also exhibits physical properties similar to those of UJ460, but the resin molding material of Example 5 has a higher MFR than Example 4, a similar level of flexibility to Example 4, and better injection moldability than Example 4.

[0070] Comparative Example 1 A polyolefin resin molding material of Comparative Example 1 was obtained in the same manner as in Example 1, except that pellets of polyethylene resin HJ560, a grade of high density polyethylene (HDPE) for general injection molding manufactured by Japan Polyethylene Co., Ltd., were used as the modifier instead of Modifier A. The physical properties of the obtained resin molding material are shown in Table 3. The constituent unit ratio and physical properties of HJ560 are as shown in Table 3. In the resin molding material of Comparative Example 1, the modifier used does not contain a constitutional unit derived from an α-olefin having 4 to 12 carbon atoms, and the density of the modifier is 0.940 g / cm 3Since the difference in the elastic modulus was larger than that of the raw material polyolefin-based recovered resin shown in Table 1, the flexibility was deteriorated, that is, the flexural modulus was increased, and the impact resistance and durability (stress crack resistance) were also deteriorated.

[0071] Comparative Example 2 A polyolefin resin molding material of Comparative Example 2 was obtained in the same manner as in Example 1, except that pellets of polyethylene resin LJ802, a grade of low-density polyethylene (LDPE) for general injection molding manufactured by Japan Polyethylene Co., Ltd., were used as the modifier instead of Modifier A. The physical properties of the obtained resin molding material are shown in Table 3. The structural unit ratio and physical properties of LJ802 are as shown in Table 3, and it did not contain structural units derived from α-olefins having 4 to 12 carbon atoms. The resin molding material of Comparative Example 2 had improved flexibility, i.e., a decreased flexural modulus, and improved impact resistance, but deteriorated durability (stress crack resistance), compared to the raw material polyolefin-based recovered resin shown in Table 1.

[0072] Comparative Example 3 A polyolefin-based resin molding material of Comparative Example 3 was obtained in the same manner as in Comparative Example 2, except that the mass ratio of the polyolefin-based recycled resin to the modifier (polyolefin-based recycled resin:modifier) ​​was changed to 30:70. The physical properties of the obtained resin molding material are shown in Table 3. The resin molding material of Comparative Example 3 also had improved flexibility, i.e., a decreased flexural modulus, and improved impact resistance, compared to the raw polyolefin-based recovered resin shown in Table 1, but its durability (stress crack resistance) was deteriorated.

[0073] Comparative Example 4 A polyolefin-based resin molding material of Comparative Example 4 was obtained in the same manner as in Comparative Example 2, except that the mass ratio of the polyolefin-based recycled resin to the modifier (polyolefin-based recycled resin:modifier) ​​was changed to 80:20. The physical properties of the obtained resin molding material are shown in Table 3. The resin molding material of Comparative Example 4 also had improved flexibility, i.e., a decreased flexural modulus, and improved impact resistance, compared to the raw material polyolefin-based recovered resin shown in Table 1, but its durability (stress crack resistance) was deteriorated.

[0074] [Table 1]

[0075] [Table 2]

[0076] [Table 3]

[0077] In Examples 1 to 5, an ethylene copolymer having the above characteristics (a), (b) and (c) was used as the modifier, and therefore the modified polyolefin resin molding materials obtained in Examples 1 to 5 had improved flexibility, i.e., a lower flexural modulus, improved impact resistance and significantly improved durability (stress crack resistance), as compared with the raw polyolefin recovered resin, as described above, and had completely different physical properties from the raw polyolefin recovered resin. Therefore, the object of the present invention is to provide a recycled polyolefin resin molding material in which the polyolefin recovered resin, which is regenerated as a raw material resin by homogenizing the recovered PET bottle caps using a material recycling method, specifically by crushing or pelletizing them, is softened by modification and has improved impact resistance and durability (stress crack resistance), and further, the object of being able to provide a molded body molded using the polyolefin resin molding material was achieved in Examples 1 to 5. In addition, the resin molding materials obtained in Examples 1 to 5 exhibited physical property values ​​similar to existing linear low density polyethylene (LLDPE) or existing high density polyethylene (HDPE) in the range of rigidity lower than PET bottle caps, while having the same or improved impact resistance and significantly improved durability (stress crack resistance) compared to existing polyethylenes with similar physical properties. Therefore, the resin molding materials obtained in Examples 1 to 5 are applicable to applications in which these existing polyethylenes are used, and applications in which these existing polyethylenes could not be used due to insufficient impact resistance or durability (stress crack resistance). On the other hand, in Comparative Example 1, the HJ560 used as the modifier did not contain a structural unit derived from an α-olefin having 4 to 12 carbon atoms, and had too high a density, so the resin molding material obtained in Comparative Example 1 had poorer flexibility, impact resistance, and durability (stress crack resistance) than the raw polyolefin-based recovered resin. In Comparative Examples 2 to 4, the LJ802 used as the modifier did not contain a structural unit derived from an α-olefin having 4 to 12 carbon atoms, so the resin molding materials obtained in Comparative Examples 2 to 4 had improved flexibility and impact resistance, but poorer durability (stress crack resistance), than the raw polyolefin-based recovered resin.

Claims

1. A polyolefin-based resin molding material comprising a polyolefin-based recovered resin derived from recovered polyolefin-based resin caps of PET bottles, and a modifier made of an ethylene-based copolymer having the following characteristics (a), (b), and (c), wherein the content of the modifier is 1 to 99 mass% based on the total amount of the polyolefin-based recovered resin and the modifier. (a) The proportion of structural units derived from ethylene as a major component is 80 to 98 mol %, the proportion of structural units derived from an α-olefin having 4 to 12 carbon atoms as an essential minor component is 0.1 to 7 mol %, the proportion of structural units derived from propylene as an optional minor component is 19.9 to 0 mol %, and the total of the structural units derived from the ethylene, the structural units derived from the α-olefin, and the structural units derived from the propylene is 100 mol %. (b) The melt flow rate (MFR) (temperature: 190° C., load: 2.16 kg) is 0.1 to 100 g / 10 min. (c) density is 0.880 to 0.940 g / cm 3 It is.

2. A polyolefin-based resin molding material comprising a polyolefin-based recovered resin obtained by homogenizing commercially recovered polyolefin-based resin caps of PET bottles, and a modifier made of an ethylene-based copolymer having the following characteristics (a), (b), and (c), wherein the content of the modifier is 1 to 99 mass% based on the total amount of the polyolefin-based recovered resin and the modifier. (a) The proportion of structural units derived from ethylene as a major component is 80 to 98 mol %, the proportion of structural units derived from an α-olefin having 4 to 12 carbon atoms as an essential minor component is 0.1 to 7 mol %, the proportion of structural units derived from propylene as an optional minor component is 19.9 to 0 mol %, and the total of the structural units derived from the ethylene, the structural units derived from the α-olefin, and the structural units derived from the propylene is 100 mol %. (b) The melt flow rate (MFR) (temperature: 190° C., load: 2.16 kg) is 0.1 to 100 g / 10 min. (c) density is 0.880 to 0.940 g / cm 3 It is.

3. 3. The polyolefin resin molding material according to claim 1, wherein the modifier is an ethylene copolymer polymerized using a metallocene catalyst.

4. The polyolefin resin molding material according to claim 3, having an environmental stress crack resistance (ESCR) of 200 hours or more.

5. The polyolefin resin molding material according to claim 1 or 2, having the following characteristics (A) and (B): (A) The melt flow rate (MFR) (temperature: 190° C., load: 2.16 kg) is 0.1 to 100 g / 10 min. (B) Density is 0.880 to 0.970 g / cm 3 It is.

6. A step of preparing a polyolefin-based recovered resin derived from recovered polyolefin-based resin caps of PET bottles; a step of preparing a modifier consisting of an ethylene-based copolymer by polymerizing, using a metallocene catalyst, a monomer component having a ratio of 80 to 98 mol % of ethylene as a main component, a ratio of 0.1 to 7 mol % of an α-olefin having 4 to 12 carbon atoms as an essential subcomponent, and a ratio of 19.9 to 0 mol % of propylene as an optional subcomponent, the total of the ethylene, the α-olefin, and the propylene being 100 mol %; and mixing the polyolefin-based recovered resin and the modifier in a mass ratio such that the amount of the modifier is 1 to 99 mass% relative to the total amount of the polyolefin-based recovered resin and the modifier.

7. A step of preparing a polyolefin-based recovered resin obtained by homogenizing a polyolefin-based resin cap of a PET bottle that is collected from a market; a step of preparing a modifier consisting of an ethylene-based copolymer by polymerizing, using a metallocene catalyst, a monomer component having a ratio of 80 to 98 mol % of ethylene as a main component, a ratio of 0.1 to 7 mol % of an α-olefin having 4 to 12 carbon atoms as an essential subcomponent, and a ratio of 19.9 to 0 mol % of propylene as an optional subcomponent, the total of the ethylene, the α-olefin, and the propylene being 100 mol %; and mixing the polyolefin-based recovered resin and the modifier in a mass ratio such that the amount of the modifier is 1 to 99 mass% relative to the total amount of the polyolefin-based recovered resin and the modifier.

8. A molded article obtained by molding the polyolefin resin molding material according to claim 1 or 2.

Citation Information

Patent Citations

  • Flexible film with enhanced physical properties

    JP1996501812A

  • Composite paper

    JP2007185891A

  • Method for reusing waste of polypropylene resin molded body

    JP2017136816A

  • Polyethylene resin composition for thin container

    JP2018012801A