Curable resin composition, dry film, cured product and electronic component
The curable resin composition with an aminotriazine thermosetting catalyst addresses the issue of high melt viscosity in solder resists for FC-BGA packages, improving developability, resolution, and heat resistance while preventing lamination failures.
Patent Information
- Application Number
- JP2024056470
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2023-03-30
- Filing Date
- 2024-03-29
- Publication Date
- 2024-10-11
AI Technical Summary
Solder resists for FC-BGA packages face challenges in maintaining low melt viscosity to prevent lamination failures while achieving high developability, resolution, and heat resistance.
A curable resin composition containing an alkali-soluble resin, photopolymerization initiator, and a thermosetting catalyst with an aminotriazine skeleton, which has one or two amino groups attached to the triazine skeleton, is used to maintain low melt viscosity and improve developability, resolution, and heat resistance.
The composition effectively prevents lamination defects and enhances developability, resolution, and heat resistance, ensuring a stable solder resist application process.
Smart Images

Figure 2024144397000001 
Figure 2024144397000002 
Figure 2024144397000003
Abstract
Description
[Technical field]
[0001] The present invention relates to a curable resin composition, a dry film, a cured product, and an electronic component. [Background technology]
[0002] In recent years, with the rapid advancement of semiconductor components, electronic devices are becoming lighter, thinner, shorter, smaller, more powerful, and more multifunctional. Following this trend, miniaturization and increased pin counts of semiconductor packages are being put into practical use.
[0003] Specifically, IC packages called BGA (ball grid array), CSP (chip scale package), etc. are being used in place of IC packages called QFP (quad flat pack package), SOP (small outline package), etc. In recent years, FC-BGA (flip chip ball grid array) has also been put to practical use as an even higher density IC package. [Prior art documents] [Patent documents]
[0004] [Patent Document 1] Patent Publication No. 2022-009428 Summary of the Invention [Problem to be solved by the invention]
[0005] Solder resist, especially solder resist for the above-mentioned FC-BGA, is required to have high-level properties in terms of developability, resolution, heat resistance, etc. On the other hand, even if the above properties are satisfied, when applied to a dry film, there is a problem that the melt viscosity becomes high and lamination failure occurs when forming the solder resist, making it difficult to achieve both.
[0006] Therefore, an object of the present invention is to provide a curable resin composition which has improved developability, resolution, and heat resistance, while maintaining a low melt viscosity even when applied to a dry film, and which does not cause lamination defects when forming a solder resist; a dry film having a resin layer obtained from the composition; a cured product of the composition or the resin layer of the dry film; and an electronic component having the cured product. [Means for solving the problem]
[0007] To achieve the above object, the present inventors have focused on the fact that it is necessary to reduce the melt viscosity of a solder resist material in order to improve lamination defects, and have conducted extensive research. As a result, they have found that the problem can be solved by using a thermosetting catalyst containing an aminotriazine skeleton having a specific structure, and have completed the present invention.
[0008] That is, the curable resin composition of the present invention contains an alkali-soluble resin, a photopolymerization initiator, a thermosetting compound, and an aminotriazine skeleton-containing thermosetting catalyst, and is characterized in that the aminotriazine skeleton-containing thermosetting catalyst has a structure in which one or two amino groups are attached to a triazine skeleton. Here, the "structure in which one or two amino groups are attached to a triazine skeleton" refers to a structure in which an amino group is attached to one or two carbon atoms of the triazine skeleton, that is, a structure having a monoaminotriazinyl group or a diaminotriazinyl group, and is specifically represented by the following formula (1) or formula (2). TIFF2024144397000001.tif34161TIFF2024144397000002.tif31161 (in the formula, R 1 represents a group or atom other than an amino group, and R 2 represents a group or atom other than an amino group. Here, "amino group" refers to -NH2.)
[0009] In the curable resin composition of the present invention, the aminotriazine skeleton-containing heat curing catalyst preferably contains a silyl group or a hydroxyl group, and the aminotriazine skeleton-containing heat curing catalyst is preferably contained in an amount of 0.1 to 10.0 parts by mass per 100 parts by mass of the alkali-soluble resin, calculated as solid content. Furthermore, it is preferable that the melt viscosity at the lowest point in the range from 70°C to 130°C is less than 100 Pa s.
[0010] The dry film of the present invention is characterized by having a resin layer obtained by applying the curable resin composition of the present invention to a first film and drying it.
[0011] The cured product of the present invention is characterized in that it is obtained by curing the curable resin composition of the present invention or the resin layer of the dry film of the present invention.
[0012] The electronic component of the present invention is characterized by having the cured product of the present invention. Effect of the Invention
[0013] According to the present invention, it is possible to provide a curable resin composition which can maintain a low melt viscosity even when applied to a dry film while improving developability, resolution, and heat resistance, and which does not cause lamination defects when forming a solder resist; a dry film having a resin layer obtained from the composition; a cured product of the composition or the resin layer of the dry film; and an electronic component having the cured product. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0014] The curable resin composition of the present invention contains an alkali-soluble resin, a photopolymerization initiator, a thermosetting compound, and an aminotriazine skeleton-containing thermosetting catalyst, and is characterized in that the aminotriazine skeleton-containing thermosetting catalyst has a structure in which one or two amino groups are attached to a triazine skeleton.
[0015] The dry film made of the curable resin composition of the present invention can maintain a low melt viscosity compared to a dry film made of a curable resin composition that is commonly used and uses melamine, which has a structure similar to that of the aminotriazine skeleton-containing thermosetting catalyst of the present invention, as a thermosetting catalyst. Specifically, the melt viscosity at the lowest point in the range from 70°C to 130°C can be made less than 100 Pa s.
[0016] While melamine has a structure with three amino groups attached to a triazine skeleton, the aminotriazine skeleton-containing heat curing catalyst of the present invention has a structure with one or two amino groups attached to a triazine skeleton. That is, while melamine has a completely symmetrical structure, the aminotriazine skeleton-containing heat curing catalyst of the present invention has an asymmetric portion in its structure. Therefore, it is presumed that the aminotriazine skeleton-containing heat curing catalyst of the present invention can control the thermal reactivity in a curable resin composition, and thus can maintain a low melt viscosity of a dry film made of a curable resin composition containing the heat curing catalyst.
[0017] Each component of the curable resin composition of the present invention will be described below. In this specification, (meth)acrylate is a term that collectively refers to acrylate, methacrylate, and mixtures thereof, and the same applies to other similar expressions.
[0018] [Alkali-soluble resin] The alkali-soluble resin is a resin containing an alkali-soluble group in the molecule, and examples thereof include resins containing one or more alkali-soluble groups selected from the group consisting of phenolic hydroxyl groups, thiol groups, and carboxyl groups.Specific examples include phenolic hydroxyl group-containing resins (particularly, resins containing two or more phenolic hydroxyl groups), carboxyl group-containing resins, resins containing phenolic hydroxyl groups and carboxyl groups, and thiol group-containing resins (particularly, resins containing two or more thiol groups).As the alkali-soluble resin, carboxyl group-containing resins or phenolic hydroxyl group-containing resins are preferred, and carboxyl group-containing resins are more preferred.
[0019] As the alkali-soluble resin, from the viewpoint of developability, photocurability, development resistance, etc., a carboxyl group-containing resin is preferable, and a resin containing two or more carboxyl groups is more preferable. The alkali-soluble resin is more preferably a resin containing an ethylenically unsaturated group in addition to a carboxyl group. The ethylenically unsaturated group is preferably derived from acrylic acid or methacrylic acid or a derivative thereof. The carboxyl group-containing resin having an ethylenically unsaturated group may be referred to as a "carboxyl group-containing photosensitive resin" below. Note that, as the alkali-soluble resin, only a carboxyl group-containing resin having no ethylenically unsaturated group may be used. When the carboxyl group-containing resin does not have an ethylenically unsaturated group, in order to make the composition photocurable, it is necessary to use a compound having a plurality of ethylenically unsaturated groups in the molecule, i.e., a photopolymerizable monomer, which will be described later. Specific examples of the alkali-soluble resin include the following compounds. These compounds may be either oligomers or polymers.
[0020] (1) Carboxyl group-containing resins obtained by copolymerizing an unsaturated carboxylic acid such as (meth)acrylic acid with an unsaturated group-containing compound such as styrene, α-methylstyrene, lower alkyl (meth)acrylate, isobutylene, etc.
[0021] (2) Carboxyl group-containing urethane resins obtained by polyaddition reaction of diisocyanates such as aliphatic diisocyanates, branched aliphatic diisocyanates, alicyclic diisocyanates, and aromatic diisocyanates with carboxyl group-containing dialcohol compounds such as dimethylolpropionic acid and dimethylolbutanoic acid, and diol compounds such as polycarbonate polyols, polyether polyols, polyester polyols, polyolefin polyols, acrylic polyols, bisphenol A alkylene oxide adduct diols, and compounds having phenolic hydroxyl groups and alcoholic hydroxyl groups.
[0022] (3) Carboxylic acid-containing urethane resins obtained by polyaddition reaction of diisocyanates with partially acid anhydride-modified products of reaction products of bifunctional epoxy resins such as bisphenol A type epoxy resins, hydrogenated bisphenol A type epoxy resins, bisphenol F type epoxy resins, bisphenol S type epoxy resins, bixylenol type epoxy resins and biphenol type epoxy resins with monocarboxylic acid compounds having ethylenically unsaturated double bonds such as (meth)acrylic acid, carboxyl group-containing dialcohol compounds and diol compounds.
[0023] (4) A photosensitive urethane resin containing a carboxyl group, which is terminated with (meth)acrylation by adding a compound having one hydroxyl group and one or more (meth)acryloyl groups in the molecule, such as a hydroxyalkyl (meth)acrylate, during the synthesis of the resin (2) or (3).
[0024] (5) A carboxyl group-containing photosensitive urethane resin having a terminal (meth)acrylation formed by adding a compound having one isocyanate group and one or more (meth)acryloyl groups in the molecule, such as an equimolar reactant of isophorone diisocyanate and pentaerythritol triacrylate, during the synthesis of the resin (2) or (3).
[0025] (6) A carboxyl group-containing photosensitive resin obtained by reacting a difunctional or more polyfunctional epoxy resin with (meth)acrylic acid and adding a dibasic acid anhydride such as phthalic anhydride, tetrahydrophthalic anhydride, hexahydrophthalic anhydride, etc. to the hydroxyl groups present in the side chains. Here, the difunctional or more polyfunctional epoxy resin is preferably solid.
[0026] (7) A carboxyl group-containing photosensitive resin obtained by reacting a polyfunctional epoxy resin in which the hydroxyl groups of a difunctional epoxy resin are further epoxidized with epichlorohydrin with (meth)acrylic acid, and then adding a dibasic acid anhydride to the resulting hydroxyl groups. Here, the difunctional epoxy resin is preferably in a solid state.
[0027] (8) Carboxyl group-containing polyester resins obtained by reacting a dicarboxylic acid such as adipic acid, phthalic acid, or hexahydrophthalic acid with a bifunctional oxetane resin and then adding a dibasic acid anhydride such as phthalic anhydride, tetrahydrophthalic anhydride, or hexahydrophthalic anhydride to the resulting primary hydroxyl groups.
[0028] (9) A carboxyl group-containing photosensitive resin obtained by reacting an epoxy compound having two or more epoxy groups in one molecule with a compound having at least one alcoholic hydroxyl group and one phenolic hydroxyl group in one molecule, such as p-hydroxyphenethyl alcohol, and an unsaturated group-containing monocarboxylic acid, such as (meth)acrylic acid, and then reacting the alcoholic hydroxyl group of the resulting reaction product with a polybasic acid anhydride, such as maleic anhydride, tetrahydrophthalic anhydride, trimellitic anhydride, pyromellitic anhydride, adipic anhydride, or the like.
[0029] (10) A carboxyl group-containing photosensitive resin obtained by reacting a compound having two or more phenolic hydroxyl groups in one molecule, such as bisphenol A, bisphenol F, bisphenol S, a novolak type phenolic resin, poly-p-hydroxystyrene, a condensation product of naphthol and an aldehyde, or a condensation product of dihydroxynaphthalene and an aldehyde, with an alkylene oxide, such as ethylene oxide or propylene oxide, and reacting the reaction product with an unsaturated group-containing monocarboxylic acid, such as (meth)acrylic acid, and then reacting the resulting reaction product with a polybasic acid anhydride.
[0030] (11) A carboxyl group-containing photosensitive resin obtained by reacting a compound having two or more phenolic hydroxyl groups per molecule with a cyclic carbonate compound such as ethylene carbonate or propylene carbonate, reacting the reaction product obtained with an unsaturated group-containing monocarboxylic acid, and reacting the resulting reaction product with a polybasic acid anhydride.
[0031] (12) A carboxyl group-containing photosensitive resin obtained by further adding a compound having one epoxy group and one or more (meth)acryloyl groups in one molecule to any one of the resins (1) to (11).
[0032] The phenolic hydroxyl group-containing resin is not particularly limited as long as it has a phenolic hydroxyl group in the main chain or side chain, i.e., a hydroxyl group bonded to a benzene ring. A phenolic hydroxyl group-containing resin having two or more phenolic hydroxyl groups in one molecule is preferred. Examples of the phenolic hydroxyl group-containing resin having two or more phenolic hydroxyl groups in one molecule include, but are not limited to, catechol, resorcinol, hydroquinone, dihydroxytoluene, naphthalenediol, t-butylcatechol, t-butylhydroquinone, pyrogallol, phloroglucinol, bisphenol A, bisphenol F, bisphenol S, biphenol, bixylenol, novolac-type phenolic resin, novolac-type alkylphenolic resin, novolac resin of bisphenol A, dicyclopentadiene-type phenolic resin, Xylok-type phenolic resin, terpene-modified phenolic resin, polyvinylphenols, condensates of phenols and aromatic aldehydes having a phenolic hydroxyl group, and condensates of 1-naphthol or 2-naphthol and aromatic aldehydes.
[0033] The alkali-soluble resin is not limited to those listed above, and may be used alone or in combination. Among them, the carboxyl group-containing resin described in (10) or (11) above is preferably used because of its excellent insulation reliability.
[0034] The acid value of the alkali-soluble resin (particularly, the carboxyl group-containing resin) is preferably 40 to 150 mgKOH / g. By setting the acid value to 40 mgKOH / g or more, the alkali development becomes good. Also, by setting the acid value to 150 mgKOH / g or less, it becomes easy to draw a normal cured product pattern. More preferably, it is 50 to 130 mgKOH / g.
[0035] The weight average molecular weight of the alkali-soluble resin varies depending on the resin skeleton, but is generally preferably 2,000 to 150,000, more preferably 5,000 to 100,000. By making the weight average molecular weight 2,000 or more, it is possible to improve tack-free performance and resolution. In addition, by making the weight average molecular weight 150,000 or less, it is possible to improve developability and storage stability. The weight average molecular weight (Mw) can be determined from a standard polystyrene equivalent value by gel permeation chromatography (GPC).
[0036] The content of the alkali-soluble resin is preferably 15 to 60 mass %, more preferably 20 to 60 mass %, calculated as solid content based on the total amount of the curable resin composition. By making it 15 mass % or more, the coating strength can be improved. Also, by making it 60 mass % or less, the viscosity becomes appropriate and the processability is improved.
[0037] [Photopolymerization initiator] As the photopolymerization initiator, any photopolymerization initiator known as a photopolymerization initiator or a photoradical generator can be used.
[0038] Examples of the photopolymerization initiator include bis-(2,6-dichlorobenzoyl)phenylphosphine oxide, bis-(2,6-dichlorobenzoyl)-2,5-dimethylphenylphosphine oxide, bis-(2,6-dichlorobenzoyl)-4-propylphenylphosphine oxide, bis-(2,6-dichlorobenzoyl)-1-naphthylphosphine oxide, bis-(2,6-dimethoxybenzoyl)phenylphosphine oxide, and bis-(2,6-dimethoxybenzoyl)-2,4,4-trimethyl Bisacylphosphine oxides such as pentylphosphine oxide, bis-(2,6-dimethoxybenzoyl)-2,5-dimethylphenylphosphine oxide, and bis-(2,4,6-trimethylbenzoyl)-phenylphosphine oxide; 2,6-dimethoxybenzoyldiphenylphosphine oxide, 2,6-dichlorobenzoyldiphenylphosphine oxide, 2,4,6-trimethylbenzoylphenylphosphinic acid methyl ester, 2-methylbenzoyldiphenylphosphine oxide, piva monoacylphosphine oxides such as isopropyl phenylphosphinate and 2,4,6-trimethylbenzoyldiphenylphosphine oxide; 1-hydroxy-cyclohexyl phenyl ketone, 1-[4-(2-hydroxyethoxy)-phenyl]-2-hydroxy-2-methyl-1-propan-1-one, 2-hydroxy-1-{4-[4-(2-hydroxy-2-methyl-propionyl)-benzyl]phenyl}-2-methyl-propan-1-one, 2-hydroxy-2-methyl-1 -phenylpropan-1-one and other hydroxyacetophenones; benzoins such as benzoin, benzil, benzoin methyl ether, benzoin ethyl ether, benzoin n-propyl ether, benzoin isopropyl ether, and benzoin n-butyl ether; benzoin alkyl ethers; benzophenone, p-methylbenzophenone, Michler's ketone, methylbenzophenone, 4,4'-dichlorobenzophenone, and 4,4'-bisdiethylaminobenzophenone;Acetophenone, 2,2-dimethoxy-2-phenylacetophenone, 2,2-diethoxy-2-phenylacetophenone, 1,1-dichloroacetophenone, 1-hydroxycyclohexyl phenyl ketone, 2-methyl-1-[4-(methylthio)phenyl]-2-morpholino-1-propanone, 2-benzyl-2-dimethylamino-1-(4-morpholinophenyl)-butanone-1, 2-(dimethylamino)-2-[(4-methylphenyl)methyl)-1-[4-(4-morpholinyl)phenyl]-1-butanone acetophenones such as acetophenone, N,N-dimethylaminoacetophenone; thioxanthones such as thioxanthone, 2-ethylthioxanthone, 2-isopropylthioxanthone, 2,4-dimethylthioxanthone, 2,4-diethylthioxanthone, 2-chlorothioxanthone, 2,4-diisopropylthioxanthone; anthraquinone, chloroanthraquinone, 2-methylanthraquinone, 2-ethylanthraquinone, 2-tert-butylanthraquinone, 1-chloroanthraquinone, 2-amylanthraquinone anthraquinones such as acetophenone dimethyl ketal and benzil dimethyl ketal; benzoic acid esters such as ethyl 4-dimethylaminobenzoate, 2-(dimethylamino)ethyl benzoate, and p-dimethylbenzoic acid ethyl ester; 1,2-octanedione, 1-[4-(phenylthio)-, 2-(O-benzoyloxime)], ethanone, 1-[9-ethyl-6-(2-methylbenzoyl)-9H-carbazol-3-yl]-, 1-(O-acetyloxy)- ...acetyloxy)-1,2-octanedione, 1 oxime esters such as bis(η5-2,4-cyclopentadien-1-yl)-bis(2,6-difluoro-3-(1H-pyrrol-1-yl)phenyl)titanium, bis(cyclopentadienyl)-bis[2,6-difluoro-3-(2-(1-pyrrol-1-yl)ethyl)phenyl]titanium, and other titanocenes; phenyl disulfide 2-nitrofluorene, butyroin, anisoin ethyl ether, azobisisobutyronitrile, tetramethylthiuram disulfide, and the like. The photopolymerization initiator may be used alone or in combination of two or more kinds.;
[0039] The amount of the photopolymerization initiator is preferably 0.5 to 20 parts by mass relative to 100 parts by mass of the alkali-soluble resin, calculated as solid content. When the amount is 0.5 parts by mass or more, the surface curing property is good, and when the amount is 20 parts by mass or less, halation is unlikely to occur and good resolution is obtained.
[0040] [Thermosetting compound] The curable resin composition of the present invention contains a thermosetting compound. The thermosetting compound improves the heat resistance of the cured product and also improves adhesion to the base. As the thermosetting compound, known and commonly used thermosetting compounds such as isocyanate compounds, blocked isocyanate compounds, amino resins, benzoxazine resins, carbodiimide resins, cyclocarbonate compounds, epoxy compounds, polyfunctional oxetane compounds, and episulfide resins can be used. Among these, epoxy compounds, polyfunctional oxetane compounds, and episulfide resins are preferred, and epoxy compounds are more preferred. The thermosetting compounds can be used alone or in combination of two or more.
[0041] The epoxy compound is a compound having an epoxy group, and any of the conventionally known compounds can be used. Examples include polyfunctional epoxy resins having a plurality of epoxy groups in the molecule. Hydrogenated epoxy resins may also be used.
[0042] Polyfunctional epoxy resins include epoxidized vegetable oils; bisphenol A type epoxy resins; hydroquinone type epoxy resins; bisphenol type epoxy resins; thioether type epoxy resins; brominated epoxy resins; novolac type epoxy resins; biphenol novolac type epoxy resins; bisphenol F type epoxy resins; hydrogenated bisphenol A type epoxy resins; glycidylamine type epoxy resins; hydantoin type epoxy resins; alicyclic epoxy resins; trihydroxyphenylmethane type epoxy resins; bixylenol type or biphenol type epoxy resins, or mixtures thereof. ; bisphenol S type epoxy resin; bisphenol A novolac type epoxy resin; tetraphenylolethane type epoxy resin; heterocyclic epoxy resin; diglycidyl phthalate resin; tetraglycidyl xylenoylethane resin; naphthalene group-containing epoxy resin; epoxy resin having a dicyclopentadiene skeleton; glycidyl methacrylate copolymer epoxy resin; cyclohexylmaleimide and glycidyl methacrylate copolymer epoxy resin; epoxy-modified polybutadiene rubber derivative; CTBN-modified epoxy resin, etc., but are not limited thereto. These epoxy resins can be used alone or in combination of two or more. Among these, novolac type epoxy resin, bisphenol type epoxy resin, bixylenol type epoxy resin, biphenol type epoxy resin, biphenol novolac type epoxy resin, naphthalene type epoxy resin, or a mixture thereof is particularly preferred.
[0043] Examples of the polyfunctional oxetane compound include bis[(3-methyl-3-oxetanylmethoxy)methyl]ether, bis[(3-ethyl-3-oxetanylmethoxy)methyl]ether, 1,4-bis[(3-methyl-3-oxetanylmethoxy)methyl]benzene, 1,4-bis[(3-ethyl-3-oxetanylmethoxy)methyl]benzene, (3-methyl-3-oxetanyl)methyl acrylate, and (3-ethyl-3-oxetanyl)methyl acrylate. Examples of the oxetanes include polyfunctional oxetanes such as acrylate, (3-methyl-3-oxetanyl)methyl methacrylate, (3-ethyl-3-oxetanyl)methyl methacrylate, and their oligomers or copolymers, as well as ethers of oxetane alcohols and novolac resins, poly(p-hydroxystyrene), cardo-type bisphenols, calixarenes, calixresorcinarenes, or resins having hydroxyl groups such as silsesquioxane. Other examples include copolymers of unsaturated monomers having an oxetane ring and alkyl (meth)acrylates.
[0044] Examples of the episulfide resin include bisphenol A type episulfide resins, etc. Also, episulfide resins in which the oxygen atoms of the epoxy groups of novolac type epoxy resins are replaced with sulfur atoms using a similar synthesis method can be used.
[0045] Examples of amino resins such as melamine derivatives and benzoguanamine derivatives include methylolmelamine compounds, methylolbenzoguanamine compounds, methylolglycoluril compounds, and methylolurea compounds.
[0046] As the isocyanate compound, a polyisocyanate compound can be blended. Examples of the polyisocyanate compound include aromatic polyisocyanates such as 4,4'-diphenylmethane diisocyanate, 2,4-tolylene diisocyanate, 2,6-tolylene diisocyanate, naphthalene-1,5-diisocyanate, o-xylylene diisocyanate, m-xylylene diisocyanate and 2,4-tolylene isocyanate dimer; aliphatic polyisocyanates such as tetramethylene diisocyanate, hexamethylene diisocyanate, methylene diisocyanate, trimethylhexamethylene diisocyanate, 4,4-methylenebis(cyclohexyl isocyanate) and isophorone diisocyanate; alicyclic polyisocyanates such as bicycloheptane triisocyanate; and adducts, biuret and isocyanurates of the above-mentioned isocyanate compounds.
[0047] The blocked isocyanate compound may be an addition reaction product of an isocyanate compound and an isocyanate blocking agent. Examples of isocyanate compounds that can react with an isocyanate blocking agent include the above-mentioned polyisocyanate compounds. Examples of isocyanate blocking agents include phenol-based blocking agents, lactam-based blocking agents, active methylene-based blocking agents, alcohol-based blocking agents, oxime-based blocking agents, mercaptan-based blocking agents, acid amide-based blocking agents, imide-based blocking agents, amine-based blocking agents, imidazole-based blocking agents, and imine-based blocking agents.
[0048] The blending amount of the thermosetting compound is preferably 10 to 100 parts by mass, calculated as solid content, per 100 parts by mass of the alkali-soluble resin.
[0049] [Aminotriazine skeleton-containing heat curing catalyst] The curable resin composition of the present invention contains an aminotriazine skeleton-containing heat curing catalyst having a structure in which one or two amino groups are attached to a triazine skeleton. The "structure in which one or two amino groups are attached to a triazine skeleton" refers to a structure in which an amino group is attached to one or two carbon atoms of a triazine skeleton, i.e., a structure having a monoaminotriazinyl group or a diaminotriazinyl group, and is specifically represented by the following formula (1) or formula (2). By containing the aminotriazine skeleton-containing heat curing catalyst, the dry film made of the curable resin composition of the present invention can maintain a low melt viscosity. TIFF2024144397000003.tif34161TIFF2024144397000004.tif31161(in the formula, R 1 represents a group or atom other than an amino group, and R 2 represents a group or atom other than an amino group. Here, "amino group" refers to -NH2.)
[0050] Among them, the aminotriazine skeleton-containing heat curing catalyst preferably has a diaminotriazinyl group structure of formula (1).
[0051] Furthermore, the aminotriazine skeleton-containing heat curing catalyst preferably has a hydroxyl group, and more preferably has a hydrolyzable silyl group or silanol group represented by the following formula (3): The number of functional groups possessed by the aminotriazine skeleton-containing heat curing catalyst may be one or more than one. TIFF2024144397000005.tif14161 (in formula (3), R 3 is a hydrogen atom or an alkyl group having 1 to 4 carbon atoms, preferably a methyl group; R 4 each independently represents a hydrogen atom or an alkyl group having 1 to 4 carbon atoms, preferably an alkyl group having 1 to 2 carbon atoms, and p represents an integer of 0 to 3, preferably an integer of 0 to 1, particularly preferably 0.
[0052] Here, the hydrolyzable silyl group is an atomic group in which a hydrolyzable group is directly bonded to a silicon atom, and the hydrolyzable group is one that can form a hydroxyl group under the influence of water. In the formula (3), p is an integer of 0 to 2, and R4 is any alkyl group having 1 to 4 carbon atoms, the atomic group represented by formula (3) becomes a hydrolyzable silyl group, and -OR 4 The group represented by the following formula (1) is a hydrolyzable group.
[0053] When the aminotriazine skeleton-containing thermosetting catalyst has a hydrolyzable silyl group or silanol group of the formula (3), the silanol group generated by hydrolysis, if necessary, reacts with the epoxy group of the epoxy resin or the surface of the inorganic filler, and the silanol groups further undergo dehydration condensation with each other, whereby the aminotriazine skeleton-containing thermosetting catalyst is incorporated into the cured product.
[0054] In this way, it is believed that the hydrolyzable silyl group or silanol group contributes to the incorporation of the aminotriazine skeleton-containing thermosetting catalyst into the cured product, resulting in many amino groups being allocated to coordinate bonds with the conductor metal, and further improving the adhesion of the cured product of the curable resin composition of the present invention to a plated conductor.
[0055] From the viewpoint of enhancing the stability of the silanol group after hydrolysis, the aminotriazine skeleton-containing thermosetting catalyst preferably has a hydrolyzable silyl group or silanol group in which p in formula (3) is 1.
[0056] On the other hand, from the viewpoint of increasing the reactivity and improving the crosslinking density, the aminotriazine skeleton-containing thermosetting catalyst preferably has a hydrolyzable silyl group or silanol group in which p in formula (3) is 0.
[0057] Among the aminotriazine skeleton-containing heat curing catalysts, those having a hydroxyl group include, for example, (4,6-diamino-[1,3,5]triazin-2-ylamino)-methanol, 2-(4,6-diamino-[1,3,5]triazin-2-ylamino)-ethanol, 3-(4,6-diamino-[1,3,5]triazin-2-ylamino)-propanol, 4-(4,6-diamino-[1,3,5]triazin-2-ylamino)-butanol, 5-(4,6-diamino-[1,3,5]triazin-2-ylamino)-pentanol, 6-(4,6-diamino-[1,3,5]triazin-2-ylamino)-pentanol, 7-(4,6-diamino-[1,3,5]triazin-2-ylamino)-pentanol, 8-(4,6-diamino-[1,3,5]triazin-2-ylamino)-pentanol, 9-(4,6-diamino-[1,3,5]triazin-2-ylamino)-pentanol, 10-(4,6-diamino-[1,3,5]triazin-2-ylamino)-pentanol, 11-(4,6-diamino-[1,3,5]triazin-2-ylamino)-pentanol, 12-(4,6-diamino-[1,3,5]triazin-2-ylamino)-pentanol, 13-(4,6-diamino-[1,3,5]triazin-2-ylamino)-pentanol, 14-(4,6-diamino-[1,3,5]triazin-2-ylamino)-pentanol, 15-(4,6-diamino-[1,3,5]triazin-2-ylamino)-pentanol, 16-( No-[1,3,5]triazin-2-ylamino)-hexanol, 8-(4,6-diamino-[1,3,5]triazin-2-ylamino)-octanol, 10-(4,6-diamino-[1,3,5]triazin-2-ylamino)-decanol, 12-(4,6-diamino-[1,3,5]triazin-2-ylamino)-dodecanol, (4,6-bis-methylamino-[1,3,5]triazin-2-ylamino)-methanol, 2-(4,6-bis-methylamino-[1,3,5]triazin-2-ylamino)-ethanol, 3-(4,6- Bis-methylamino-[1,3,5]triazin-2-ylamino)-propanol, 4-(4,6-bis-methylamino-[1,3,5]triazin-2-ylamino)-butanol, 6-(4,6-bis-methylamino-[1,3,5]triazin-2-ylamino)-hexanol, 8-(4,6-bis-methylamino-[1,3,5]triazin-2-ylamino)-octanol, 10-(4,6-bis-methylamino-[1,3,5]triazin-2-ylamino)-decanol, 12-(4,6-bis ... azin-2-ylamino)-dodecanol, (4,6-bis-ethylamino-[1,3,5]triazin-2-ylamino)-methanol, 2-(4,6-bis-ethylamino-[1,3,5]triazin-2-ylamino)-ethanol, 3-(4,6-bis-ethylamino-[1,3,5]triazin-2-ylamino)-propanol, 4-(4,6-bis-ethylamino-[1,3,5]triazin-2-ylamino)-butanol, 6-(4,6-bis-ethylamino-[1,3,5]triazin-2-ylamino)-hexanol, 8-(4,6-Bis-ethylamino-[1,3,5]triazin-2-ylamino)-octanol, 10-(4,6-bis-ethylamino-[1,3,5]triazin-2-ylamino)-decanol, 12-(4,6-bis-ethylamino-[1,3,5]triazin-2-ylamino)-dodecanol, (4,6-bis-butylamino-[1,3,5]triazin-2-ylamino)-methanol, 2-(4,6-bis-butylamino-[1,3,5]triazin-2-ylamino)-ethanol, 3-(4,6-bis-butylamino-[1,3,5 ]triazin-2-ylamino)-propanol, 4-(4,6-bis-butylamino-[1,3,5]triazin-2-ylamino)-butanol, 6-(4,6-bis-butylamino-[1,3,5]triazin-2-ylamino)-hexanol, 8-(4,6-bis-butylamino-[1,3,5]triazin-2-ylamino)-octanol, 10-(4,6-bis-butylamino-[1,3,5]triazin-2-ylamino)-decanol, 12-(4,6-bis-butylamino-[1,3,5]triazin-2-ylamino)- Dodecanol, (4,6-bis-dimethylamino-[1,3,5]triazin-2-ylamino)-methanol, 2-(4,6-bis-dimethylamino-[1,3,5]triazin-2-ylamino)-ethanol, 3-(4,6-bis-dimethylamino-[1,3,5]triazin-2-ylamino)-propanol, 4-(4,6-bis-dimethylamino-[1,3,5]triazin-2-ylamino)-butanol, 6-(4,6-bis-dimethylamino-[1,3,5]triazin-2-ylamino)-hexanol, 8-(4,6-bis -Dimethylamino-[1,3,5]triazin-2-ylamino)-octanol, 10-(4,6-bis-dimethylamino-[1,3,5]triazin-2-ylamino)-decanol, 12-(4,6-bis-dimethylamino-[1,3,5]triazin-2-ylamino)-dodecanol, (4,6-bis-diethylamino-[1,3,5]triazin-2-ylamino)-methanol, 2-(4,6-bis-diethylamino-[1,3,5]triazin-2-ylamino)-ethanol, 3-(4,6-bis-diethylamino-[1,3,5]triazin-2-ylamino)-propanol, 4-(4,6-bis-diethylamino-[1,3,5]triazin-2-ylamino)-butanol, 6-(4,6-bis-diethylamino-[1,3,5]triazin-2-ylamino)-hexanol, 8-(4,6-bis-diethylamino-[1,3,5]triazin-2-ylamino)-octanol, 10-(4,6-bis-diethylamino-[1,3,5]triazin-2-ylamino)-decanol, 12-(4,6-bis-diethylamino-[1,3,5]triazin-2-ylamino)-dodecanol, (4,6-bis-dibutylamino-[1,3,5]triazin-2-ylamino)-methanol, 2-(4,6-bis-dibutylamino-[1,3,5]triazin-2-ylamino)-hexane, No-[1,3,5]triazin-2-ylamino)-ethanol, 3-(4,6-bis-dibutylamino-[1,3,5]triazin-2-ylamino)-propanol, 4-(4,6-bis-dibutylamino-[1,3,5]triazin-2-ylamino)-butanol, 6-(4,6-bis-dibutylamino-[1,3,5]triazin-2-ylamino)-hexanol, 8-(4,6-bis-dibutylamino-[1,3,5]triazin-2-ylamino)-octanol, 10-(4,6-bis-dibutylamino-[1,3,5]triazin-2-ylamino)-decanol, 12-(4,6-bis-dibutylamino-[1,3,5]triazin-2-ylamino)-dodecanol, etc.
[0058] Examples of the aminotriazine skeleton-containing heat curing catalyst having a hydrolyzable silyl group or silanol group of the formula (3) include N-trihydroxysilanylmethyl-[1,3,5]triazine-2,4,6-triamine, N-(2-trihydroxysilanyl-ethyl)-[1,3,5]triazine-2,4,6-triamine, N-(3-trihydroxysilanyl-propyl)-[1,3,5]triazine-2,4,6-triamine, N-(4-trihydroxysilanyl-butyl)-[1,3,5]triazine-2,4,6-triamine, N-(6-trihydroxysilanyl-propyl)-[1,3,5]triazine-2,4,6-triamine, N-(8-trihydroxysilanyl-propyl)-[1,3,5]triazine-2,4,6-triamine, N-(9-trihydroxysilanyl-propyl)-[1,3,5]triazine-2,4,6-triamine, N-(10-trihydroxysilanyl-propyl)-[1,3,5]triazine-2,4,6-triamine, N-(11-trihydroxysilanyl-propyl)-[1,3,5]triazine-2,4,6-triamine, N-(12-trihydroxysilanyl-propyl)-[1,3,5]triazine-2,4,6-triamine, N-(13-trihydroxysilanyl-propyl)-[1,3,5]triazine-2,4,6-triamine, N-(14-trihydroxysilanyl-propyl)-[1,3,5]triazine-2,4,6-triamine, N-(15-trihydroxysilanyl-propyl)-[1,3,5]triazine-2,4,6-triamine, N-(16-trihydroxysilanyl-propyl)-[1,3,5]triazine-2,4,6-triamine, N-(17-trihydroxysilanyl N-(8-trihydroxysilanyl-octyl)-[1,3,5]triazine-2,4,6-triamine, N-(10-trihydroxysilanyl-decyl)-[1,3,5]triazine-2,4,6-triamine, N-(12-trihydroxysilanyl-dodecyl)-[1,3,5]triazine-2,4,6-triamine, N-trimethoxysilanylmethyl-[1,3,5]triazine-2,4,6-triamine, N-(2-trimethoxysilanyl -ethyl)-[1,3,5]triazine-2,4,6-triamine, N-(3-trimethoxysilanyl-propyl)-[1,3,5]triazine-2,4,6-triamine, N-(4-trimethoxysilanyl-butyl)-[1,3,5]triazine-2,4,6-triamine, N-(6-trimethoxysilanyl-hexyl)-[1,3,5]triazine-2,4,6-triamine, N-(8-trimethoxysilanyl-octyl)-[1,3,5]triazine-2,4,6-triamine, N-(10-trimethoxysilanyl-decyl)-[1 ,3,5]triazine-2,4,6-triamine, N-(12-trimethoxysilanyl-dodecyl)-[1,3,5]triazine-2,4,6-triamine, N-triethoxysilanylmethyl-[1,3,5]triazine-2,4,6-triamine, N-(2-triethoxysilanyl-ethyl)-[1,3,5]triazine-2,4,6-triamine, N-(3-triethoxysilanyl-propyl)-[1,3,5]triazine-2,4,6-triamine, N-(4-triethoxysilanyl-butyl)-[1,3,5]triazine-2,4,6-Triamine, N-(6-triethoxysilanyl-hexyl)-[1,3,5]triazine-2,4,6-triamine, N-(8-triethoxysilanyl-octyl)-[1,3,5]triazine-2,4,6-triamine, N-(10-triethoxysilanyl-decyl)-[1,3,5]triazine-2,4,6-triamine, N-(12-triethoxysilanyl-dodecyl)-[1,3,5]triazine-2,4,6-triamine, N,N'-dimethyl-N"-trihydroxysilanylmethyl-[1,3,5]triazine-2,4,6-triamine N,N'-dimethyl-N"-(2-trihydroxysilanyl-ethyl)-[1,3,5]triazine-2,4,6-triamine, N,N'-dimethyl-N"-(3-trihydroxysilanyl-propyl)-[1,3,5]triazine-2,4,6-triamine, N,N'-dimethyl-N"-(4-trihydroxysilanyl-butyl)-[1,3,5]triazine-2,4,6-triamine, N,N'-dimethyl-N"-(6-trihydroxysilanyl-hexyl)-[1,3,5]triazine-2,4,6-triamine, N,N'-dimethyl-N"- (8-trihydroxysilanyl-octyl)-[1,3,5]triazine-2,4,6-triamine, N,N'-dimethyl-N"-(10-trihydroxysilanyl-decyl)-[1,3,5]triazine-2,4,6-triamine, N,N'-dimethyl-N"-(12-trihydroxysilanyl-dodecyl)-[1,3,5]triazine-2,4,6-triamine, N,N'-dimethyl-N"-trimethoxysilanylmethyl-[1,3,5]triazine-2,4,6-triamine, N,N'-dimethyl-N"-(2-trimethoxysilanyl-ethyl) -[1,3,5]triazine-2,4,6-triamine, N,N'-dimethyl-N"-(3-trimethoxysilanyl-propyl)-[1,3,5]triazine-2,4,6-triamine, N,N'-dimethyl-N"-(4-trimethoxysilanyl-butyl)-[1,3,5]triazine-2,4,6-triamine, N,N'-dimethyl-N"-(6-trimethoxysilanyl-hexyl)-[1,3,5]triazine-2,4,6-triamine, N,N'-dimethyl-N"-(8-trimethoxysilanyl-octyl)-[1,3,5]triazine-2,4,6-triamine, N,N'-dimethyl-N"-(10-trimethoxysilanyl-decyl)-[1,3,5]triazine-2,4,6-triamine, N,N'-dimethyl-N"-(12-trimethoxysilanyl-dodecyl)-[1,3,5]triazine-2,4,6-triamine, N,N'-dimethyl-N"-triethoxysilanylmethyl-[1,3,5]triazine-2,4,6-triamine, N,N'-dimethyl-N"-(2-triethoxysilanyl-ethyl)-[1,3,5]triazine-2,4,6-triamine, N,N'-dimethyl-N"-(3-triethoxysilanyl-propyl)-[1,3,5]triazine-2,4,6-triamine, N, N'-dimethyl-N"-(4-triethoxysilanyl-butyl)-[1,3,5]triazine-2,4,6-triamine, N,N'-dimethyl-N"-(6-triethoxysilanyl-hexyl)-[1,3,5]triazine-2,4,6-triamine, N,N'-dimethyl-N"-(8-triethoxysilanyl-octyl)-[1,3,5]triazine-2,4,6-triamine, N,N'-dimethyl-N"-(10-triethoxysilanyl-decyl)-[1,3,5]triazine-2,4,6-triamine, N,N'-dimethyl-N"-(12-triethoxysilanyl-dodecyl)-[1,3,5]triazine-2,4,6-triamine, etc.
[0059] These aminotriazine skeleton-containing heat curing catalysts can be synthesized by known methods. For the aminotriazine skeleton-containing heat curing catalysts having a diaminotriazinyl group and a hydroxyl group, the method described in International Publication No. 2013 / 005021 can be referred to. For the aminotriazine skeleton-containing heat curing catalysts having a hydrolyzable silyl group or silanol group of formula (3), the method described in U.S. Patent No. 2949434 or Chemistry-A European Journal, Vol. 15, pp. 6279-6288 can be referred to.
[0060] In addition, the aminotriazine skeleton-containing thermosetting catalyst having a hydroxyl group may also include a triazine compound represented by chemical formula (4). The triazine compound represented by chemical formula (4) can be synthesized by reacting 2,4-diamino-6-vinyl-1,3,5-triazine represented by chemical formula (5) with an alcohol compound represented by chemical formula (6) using an appropriate amount of an acidic compound in an appropriate amount of reaction solvent at an appropriate reaction temperature and reaction time. TIFF2024144397000006.tif34159 (wherein multiple R 1 may be the same or different, and independently represent a hydrogen atom, an alkyl group having 1 to 4 carbon atoms, a hydroxyl group, or a methoxy group. n represents an integer of 0 to 10. TIFF2024144397000007.tif30159TIFF2024144397000008.tif34157(In the formula, multiple R 1 may be the same or different, and independently represent a hydrogen atom, an alkyl group having 1 to 4 carbon atoms, a hydroxyl group, or a methoxy group. n represents an integer of 0 to 10.
[0061] Examples of the alcohol compound represented by chemical formula (6) include ethylene glycol, 1,4-butanediol, 1,6-hexanediol, 1,8-octanediol, 1,10-decanediol, 2,2-dihydroxyethanol, glycerin, 1,2,4-butanetriol, 1,3,4-butanetriol, 1,2,6-hexanetriol, 1,2,8-octanetriol, and 1,2,10-decanetriol.
[0062] Examples of the acidic compound include hydrochloric acid, sulfuric acid, acetic acid, phosphoric acid, nitric acid, and hydrobromic acid.
[0063] Examples of the reaction solvent include water, alcohol solvents such as methanol and ethanol, halogenated solvents such as chloroform and dichloromethane, hydrocarbon solvents such as toluene and hexane, ether solvents such as tetrahydrofuran and 1,4-dioxane, and dimethyl sulfoxide (DMSO).
[0064] The reaction temperature can be appropriately set within the range of 10 to 100° C. The reaction time is determined according to the reaction temperature, but is preferably set to 0.5 to 24 hours, and more preferably set to 1 to 6 hours.
[0065] After the reaction of 2,4-diamino-6-vinyl-1,3,5-triazine represented by the above-mentioned chemical formula (5), the alcohol compound represented by the chemical formula (6) and the acidic compound, the target triazine compound represented by the chemical formula (4) can be obtained from the obtained reaction mixture by, for example, a crystallization operation or an extraction operation. If necessary, the target triazine compound represented by the chemical formula (4) can be further purified by washing with a solvent such as water or by treatment with activated carbon.
[0066] Examples of the aminotriazine skeleton-containing thermosetting catalyst include 2,4-diamino-6-vinyl-s-triazine (VT), compounds having a diaminotriazinyl group and a hydroxyl group (VD-3, VD-4), and a compound having a diaminotriazinyl group and a hydrolyzable silyl group of formula (3) (VD-5) (all manufactured by Shikoku Chemical Industry Co., Ltd.).
[0067] These aminotriazine skeleton-containing heat curing catalysts may be used alone or in combination of two or more.
[0068] The aminotriazine skeleton-containing thermosetting catalyst is preferably contained in an amount of 0.03 to 20.0 parts by mass, more preferably 0.1 to 10.0 parts by mass, even more preferably 0.1 to 8.0 parts by mass, and most preferably 2.0 to 8.0 parts by mass, relative to 100 parts by mass of the alkali-soluble resin, calculated as solid content. By containing 0.03 parts by mass or more, better resolution can be obtained. Also, by containing 20.0 parts by mass or less, better resolution can be obtained.
[0069] (Photopolymerizable monomer) The photopolymerizable monomer is contained in order to promote photocuring of the photosensitive resin composition. Examples of the photopolymerizable monomer include (meth)acrylate monomers having a (meth)acryloyl group in the molecule.
[0070] Examples of the (meth)acrylate monomer include polyfunctional allyl compounds such as triallyl isocyanurate, diallyl phthalate, and diallyl isophthalate; alkylene polyol poly(meth)acrylates such as ethylene glycol di(meth)acrylate, butanediol di(meth)acrylates, neopentyl glycol di(meth)acrylate, 1,6-hexanediol di(meth)acrylate, trimethylolpropane tri(meth)acrylate, pentaerythritol tetra(meth)acrylate, and dipentaerythritol hexa(meth)acrylate; acrylates; polyoxyalkylene glycol poly(meth)acrylates such as diethylene glycol di(meth)acrylate, triethylene glycol di(meth)acrylate, ethoxylated trimethylolpropane triacrylate, and propoxylated trimethylolpropane tri(meth)acrylate; poly(meth)acrylates such as hydroxypivalic acid neopentyl glycol ester di(meth)acrylate; and isocyanurate-type poly(meth)acrylates such as tris[(meth)acryloxyethyl]isocyanurate. These may be used alone or in combination of two or more.
[0071] The content of the photopolymerizable monomer is preferably 5 parts by mass to 100 parts by mass, more preferably 5 parts by mass to 70 parts by mass, relative to 100 parts by mass of the alkali-soluble resin, calculated as solid content. By adjusting the content to 5 parts by mass to 100 parts by mass, the photocurability and the resolution are improved.
[0072] (Inorganic filler) The curable resin composition of the present invention may contain an inorganic filler. The inorganic filler is not particularly limited, and may be any known and commonly used inorganic filler, such as silica, such as amorphous silica, crystalline silica, fused silica, and spherical silica, Neuburg silica, aluminum hydroxide, glass powder, talc, clay, magnesium carbonate, calcium carbonate, natural mica, synthetic mica, aluminum hydroxide, barium sulfate, barium titanate, iron oxide, non-fibrous glass, hydrotalcite, mineral wool, aluminum silicate, calcium silicate, and zinc oxide. The inorganic filler preferably contains 5% by mass or more of silica. By blending 5% by mass or more of silica, better thermal shock resistance can be obtained. Examples of silica include fused silica, spherical silica, amorphous silica, and crystalline silica, and spherical silica is preferable.
[0073] The inorganic filler is preferably a surface-treated inorganic filler, and more preferably, the surface of the inorganic filler is subjected to a surface treatment capable of introducing a curable reactive group. Here, the curable reactive group is not particularly limited as long as it is a group that undergoes a curing reaction with a curable compound such as an alkali-soluble resin or a thermosetting compound, and may be a photocurable reactive group or a thermosetting reactive group. Examples of the photocurable reactive group include a methacryl group, an acrylic group, a vinyl group, and a styryl group, and examples of the thermosetting reactive group include an epoxy group, an amino group, a hydroxyl group, a carboxyl group, an isocyanate group, an imino group, an oxetanyl group, a mercapto group, a methoxymethyl group, a methoxyethyl group, an ethoxymethyl group, an ethoxyethyl group, and an oxazoline group. The method of introducing a curable reactive group into the surface of the inorganic filler is not particularly limited, and it may be introduced using a known and commonly used method, and the surface of the inorganic filler may be treated with a surface treatment agent having a curable reactive group, for example, a coupling agent having a curable reactive group as an organic group. As the coupling agent, a silane coupling agent, a titanium coupling agent, a zirconium coupling agent, an aluminum coupling agent, etc. can be used. In addition, examples of surface-treated inorganic fillers that do not have a curable reactive group include inorganic fillers that have been subjected to silica-alumina surface treatment, titanate-based coupling agent treatment, aluminate-based coupling agent treatment, fluorene-based coupling agent treatment, and organic treatment. In addition, as a surface treatment, the inorganic filler may be coated with a hydrated oxide of silicon, a hydrated oxide of aluminum, a hydrated oxide of zirconium, a hydrated oxide of zinc, a hydrated oxide of titanium, etc.
[0074] The average particle size of the inorganic filler is preferably 0.01 to 0.8 μm. Here, in this specification, the average particle size of the inorganic filler is the average particle size (D50) including not only the particle size of the primary particles but also the particle size of the secondary particles (aggregates), and is the value of D50 measured by a laser diffraction method. An example of a measuring device using the laser diffraction method is Microtrac MT3300EXII manufactured by Microtrac-Bell.
[0075] The inorganic filler may have an average particle size adjusted, and is preferably pre-dispersed, for example, by a bead mill or a jet mill. The inorganic filler is preferably blended in a slurry state, which facilitates high dispersion, prevents aggregation, and makes handling easier.
[0076] The inorganic filler may be used alone or in combination of two or more. The amount of the inorganic filler in the curable resin composition is preferably 5 to 80 mass %, which provides toughness greater than that of the resin alone.
[0077] (Thermosetting catalyst) The curable resin composition of the present invention may contain other heat curing catalysts within the range that does not impair the characteristics of the present invention. Examples of such heat curing catalysts include imidazole derivatives such as imidazole, 2-methylimidazole, 2-ethylimidazole, 2-ethyl-4-methylimidazole, 2-phenylimidazole, 4-phenylimidazole, 1-cyanoethyl-2-phenylimidazole, and 1-(2-cyanoethyl)-2-ethyl-4-methylimidazole; amine compounds such as dicyandiamide, benzyldimethylamine, 4-(dimethylamino)-N,N-dimethylbenzylamine, 4-methoxy-N,N-dimethylbenzylamine, and 4-methyl-N,N-dimethylbenzylamine; hydrazine compounds such as adipic acid dihydrazide and sebacic acid dihydrazide; and phosphorus compounds such as triphenylphosphine. Also usable are guanamine, acetoguanamine and benzoguanamine, and it is preferable to use these compounds which also function as adhesion promoters in combination with the heat curing catalyst.
[0078] The amount of the thermosetting catalyst is preferably 0.05 to 20 parts by mass, more preferably 0.1 to 15 parts by mass, based on 100 parts by mass of the thermosetting compound, calculated as solid content.
[0079] (hardening agent) The curable resin composition of the present invention may contain a curing agent. Examples of the curing agent include phenolic resins, polycarboxylic acids and their acid anhydrides, cyanate ester resins, active ester resins, maleimide compounds, alicyclic olefin polymers, etc. The curing agents may be used alone or in combination of two or more.
[0080] (Coloring agent) The curable resin composition of the present invention may contain a colorant. As the colorant, a known colorant such as red, blue, green, yellow, black, or white may be used, and any of a pigment, dye, and coloring matter may be used. However, from the viewpoint of reducing the environmental load and the effect on the human body, it is preferable that the colorant does not contain a halogen.
[0081] The amount of colorant added is not particularly limited, but is preferably 10 parts by mass or less, and more preferably 0.1 to 7 parts by mass, per 100 parts by mass of the alkali-soluble resin.
[0082] (Organic solvent) The curable resin composition of the present invention may contain an organic solvent for the purpose of adjusting the viscosity when preparing the composition or applying it to a substrate or a carrier film (hereinafter referred to as the "first film"). Examples of the organic solvent include ketones such as methyl ethyl ketone and cyclohexanone; aromatic hydrocarbons such as toluene, xylene, and tetramethylbenzene; glycol ethers such as cellosolve, methyl cellosolve, butyl cellosolve, carbitol, methyl carbitol, butyl carbitol, propylene glycol monomethyl ether, dipropylene glycol monomethyl ether, dipropylene glycol diethyl ether, diethylene glycol monomethyl ether acetate, and tripropylene glycol monomethyl ether; esters such as ethyl acetate, butyl acetate, butyl lactate, cellosolve acetate, butyl cellosolve acetate, carbitol acetate, butyl carbitol acetate, propylene glycol monomethyl ether acetate, dipropylene glycol monomethyl ether acetate, and propylene carbonate; aliphatic hydrocarbons such as octane and decane; and petroleum-based solvents such as petroleum ether, petroleum naphtha, and solvent naphtha. Known and commonly used organic solvents can be used. These organic solvents may be used alone or in combination of two or more kinds.
[0083] (Other optional ingredients) Furthermore, the curable resin composition of the present invention may contain other additives that are well known and commonly used in the field of electronic materials, such as thermal polymerization inhibitors, ultraviolet absorbers, silane coupling agents, plasticizers, flame retardants, antistatic agents, antiaging agents, antibacterial and antifungal agents, defoamers, leveling agents, thickeners, adhesion-imparting agents, thixotropy-imparting agents, photoinitiator assistants, sensitizers, thermoplastic resins, organic fillers, release agents, surface treatment agents, dispersants, dispersion assistants, surface modifiers, stabilizers, phosphors, and AB or ABA block copolymers.
[0084] The curable resin composition of the present invention may be used in the form of a dry film or in the form of a liquid. When used in the form of a liquid, it may be a one-component type or a two-component or more type.
[0085] Next, the dry film of the present invention has a resin layer obtained by applying and drying the curable resin composition of the present invention on the first film. When forming a dry film, first, the curable resin composition of the present invention is diluted with the organic solvent to adjust the viscosity to an appropriate level, and then coated on the first film to a uniform thickness using a comma coater, blade coater, lip coater, rod coater, squeeze coater, reverse coater, transfer roll coater, gravure coater, spray coater, or the like. Thereafter, the applied composition is usually dried at a temperature of 40 to 130°C for 1 to 30 minutes to form a resin layer. There is no particular restriction on the coating thickness, but it is generally appropriately selected within the range of 3 to 150 μm, preferably 5 to 60 μm, in terms of the film thickness after drying.
[0086] As the first film, a plastic film is used, and for example, a polyester film such as polyethylene terephthalate (PET), a polyimide film, a polyamideimide film, a polypropylene film, a polystyrene film, etc. can be used. There is no particular limitation on the thickness of the first film, but it is generally appropriately selected in the range of 10 to 150 μm. It is more preferably in the range of 15 to 130 μm.
[0087] After forming a resin layer made of the curable resin composition of the present invention on the first film, it is preferable to further laminate a peelable cover film (hereinafter, referred to as "second film") on the surface of the resin layer for the purpose of preventing dust from adhering to the surface of the resin layer. As the peelable second film, for example, a polyethylene film, a polytetrafluoroethylene film, a polypropylene film, surface-treated paper, etc. can be used. As the second film, it is sufficient that the adhesive force between the resin layer and the first film is smaller than that between the second film and the first film when the second film is peeled off.
[0088] In the present invention, the curable resin composition of the present invention may be applied to the second film and dried to form a resin layer, and the first film may be laminated on the surface of the resin layer. That is, in the present invention, either the first film or the second film may be used as the film to which the curable resin composition of the present invention is applied when producing a dry film.
[0089] The electronic part of the present invention has a cured product obtained from the curable resin composition of the present invention or the resin layer of the dry film. In the present invention, the electronic part means a part used in an electronic circuit, and includes active parts such as printed wiring boards, transistors, light-emitting diodes, and laser diodes, as well as passive parts such as resistors, capacitors, inductors, and connectors, and the cured product obtained from the curable resin composition of the present invention exerts the effects of the present invention as an insulating cured coating film for these parts.
[0090] As a method for producing the cured product of the present invention, for example, the curable resin composition of the present invention is adjusted to a viscosity suitable for the coating method using the organic solvent, and coated on a substrate by a method such as dip coating, flow coating, roll coating, bar coating, screen printing, or curtain coating, and then the organic solvent contained in the composition is evaporated and dried (temporarily dried) at a temperature of 60 to 100° C. To form a tack-free resin layer, a dry film is attached to the substrate by a laminator or the like so that the resin layer is in contact with the substrate, and then the first film is peeled off to form a resin layer on the substrate.
[0091] The above-mentioned substrates include printed wiring boards and flexible printed wiring boards on which circuits have been formed in advance using copper or the like, as well as materials such as paper phenol, paper epoxy, glass cloth epoxy, glass polyimide, glass cloth / non-woven epoxy, glass cloth / paper epoxy, synthetic fiber epoxy, copper-clad laminates for high-frequency circuits made from fluororesin, polyethylene, polyphenylene ether, polyphenylene oxide, cyanate, etc., including copper-clad laminates of all grades (FR-4, etc.), as well as metal substrates, polyimide films, PET films, polyethylene naphthalate (PEN) films, glass substrates, ceramic substrates, wafer plates, etc.
[0092] The volatilization drying or heat curing described later, which is carried out after application of the curable resin composition of the present invention, can be carried out using a hot air circulation drying oven, an IR oven, a hot plate, a convection oven, or the like (a method in which hot air in a dryer equipped with a heat source of an air heating method using steam is brought into countercurrent contact with the substrate, or a method in which hot air is blown onto the substrate from a nozzle).
[0093] After forming a resin layer on a printed wiring board, the resin layer is selectively exposed to active energy rays through a photomask with a predetermined pattern formed thereon, and the unexposed areas are developed with a dilute alkaline aqueous solution (e.g., 0.3 to 3 mass% aqueous sodium carbonate solution) to form a pattern of a cured product. The cured product is then irradiated with active energy rays and then heat-cured (e.g., 100 to 220°C), or is irradiated with active energy rays after heat-curing, or is heat-cured only to form a final finish curing (main curing) (main curing), thereby forming a cured product with excellent properties such as adhesion and hardness, or a cured coating film in the case of a coating film.
[0094] The exposure machine used for the above-mentioned active energy ray irradiation may be a machine equipped with a high pressure mercury lamp, an ultra-high pressure mercury lamp, a metal halide lamp, a mercury short arc lamp, or the like, and capable of irradiating ultraviolet rays in the range of 350 to 450 nm, and further, a direct imaging machine (for example, a laser direct imaging machine that directly draws an image with a laser based on CAD data from a computer) may also be used. The lamp light source or laser light source of the direct imaging machine may have a maximum wavelength in the range of 350 to 450 nm. The exposure dose for forming an image varies depending on the film thickness, etc., but is generally 10 to 1,000 mJ / cm. 2 , preferably 20 to 800 mJ / cm 2 The range may be:
[0095] The developing method can be a dipping method, a shower method, a spray method, a brush method, or the like, and the developing solution can be an aqueous alkali solution of potassium hydroxide, sodium hydroxide, sodium carbonate, potassium carbonate, sodium phosphate, sodium silicate, ammonia, amines, or the like.
[0096] The curable resin composition of the present invention is preferably used for forming a cured film on a printed wiring board for semiconductor packaging, more preferably for forming a permanent coating, and even more preferably for forming a solder resist, an interlayer insulating layer, a coverlay, etc. Furthermore, since the curable resin composition of the present invention can obtain a cured product with excellent crack resistance, it can be preferably used for forming a permanent coating such as a solder resist used in a printed wiring board having a fine-pitch wiring pattern that is greatly affected by defects due to crack generation, for example, a package substrate. EXAMPLES
[0097] The present invention will be described in more detail below using examples, but the present invention is not limited to the following examples. In the following, "parts" and "%" are all based on mass unless otherwise specified.
[0098] (Synthesis of alkali-soluble resin A-1) Into an autoclave equipped with a thermometer, a nitrogen introduction device / alkylene oxide introduction device, and a stirrer, 119.4 parts by mass of novolac cresol resin (product name "Shounol CRG951", manufactured by Aica Kogyo Co., Ltd., OH equivalent: 119.4), 1.19 parts by mass of potassium hydroxide, and 119.4 parts by mass of toluene were introduced, and the system was replaced with nitrogen while stirring, and heated to increase the temperature. Next, 63.8 parts by mass of propylene oxide was gradually added dropwise, and the mixture was heated to 125-132°C and 0-4.8 kg / cm. 2 The mixture was reacted at room temperature for 16 hours. After that, it was cooled to room temperature, and 1.56 parts by mass of 89% phosphoric acid was added to the reaction solution to neutralize the potassium hydroxide, to obtain a propylene oxide reaction solution of a novolac cresol resin with a solid content of 62.1% and a hydroxyl value of 182.2 mgKOH / g (307.9 g / eq.). This was an average of 1.08 moles of propylene oxide added per equivalent of phenolic hydroxyl group. 293.0 parts by mass of the resulting propylene oxide reaction solution of the novolac cresol resin, 43.2 parts by mass of acrylic acid, 11.53 parts by mass of methanesulfonic acid, 0.18 parts by mass of methyl hydroquinone, and 252.9 parts by mass of toluene were introduced into a reactor equipped with a stirrer, a thermometer, and an air inlet tube, and the mixture was reacted at 110°C for 12 hours while blowing air at a rate of 10 ml / min and stirring. The water produced by the reaction was distilled as an azeotropic mixture with toluene, and 12.6 parts by mass of water was distilled. The mixture was then cooled to room temperature, and the resulting reaction solution was neutralized with 35.35 parts by mass of a 15% aqueous sodium hydroxide solution, and then washed with water. The toluene was then replaced with 118.1 parts by mass of diethylene glycol monoethyl ether acetate in an evaporator and distilled off to obtain a novolac acrylate resin solution. Next, 332.5 parts by mass of the obtained novolac type acrylate resin solution and 1.22 parts by mass of triphenylphosphine were introduced into a reactor equipped with a stirrer, a thermometer, and an air inlet tube, and 60.8 parts by mass of tetrahydrophthalic anhydride were gradually added while blowing air at a rate of 10 ml / min and stirring, and the mixture was reacted at 95 to 101 ° C for 6 hours, cooled, and then removed. In this way, a solution of alkali-soluble resin A-1 (photosensitive carboxyl group-containing resin) with a solid content of 70.6% and an acid value of the solid content of 87.7 mg KOH / g was obtained.
[0099] (Preparation of Curable Resin Composition) Using the obtained alkali-soluble resin A-1, various components shown in Table 1 were blended in the indicated ratios (parts by mass), premixed with a stirrer, and then kneaded with a three-roll mill to prepare the curable resin compositions of Examples 1 to 7 and Comparative Examples 1 to 3.
[0100] [Table 1]
[0101] (*1) Alkali-soluble resin A-1 synthesized above (The values in Table 1 are calculated as solid content.) (*2) IGM Resins photoinitiator Omnirad 819 Bis-(2,4,6-trimethylbenzoyl)-phenylphosphine oxide (*3) Dicyclopentadiene type epoxy resin HP-7200L manufactured by DIC Corporation (*4) Aminotriazine skeleton-containing heat curing catalyst (having a structure with two amino groups attached to a triazine skeleton) VD-5 manufactured by Shikoku Chemicals Corporation, has a structure represented by the following formula (7). TIFF2024144397000010.tif31159(*5) Aminotriazine skeleton-containing heat curing catalyst (having a structure with two amino groups attached to a triazine skeleton) VD-3 manufactured by Shikoku Chemical Industry Co., Ltd., has a structure represented by the following formula (8). TIFF2024144397000011.tif33157(*6) Melamine (*7) DIC Corporation thermosetting catalyst LA3018-50P (*8) Dicyandiamide (*9) Acrylate monomer: Dipentaerythritol hexaacrylate (*10) Silica YA050C-HHL manufactured by Admatechs Co., Ltd. (average particle size 50 nm, solid content 60% by mass)
[0102] The following evaluations were carried out on the thus obtained curable resin compositions of Examples 1 to 7 and Comparative Examples 1 to 3. The results are shown in Table 1.
[0103] (Preparation of dry film) The curable resin compositions of Examples 1 to 7 and Comparative Examples 1 to 3 obtained as described above were diluted with 300 g of methyl ethyl ketone, and the mixture was stirred with a stirrer for 15 minutes to obtain a coating liquid. The coating liquid was applied onto a polyethylene terephthalate film (Embret PTH-25, manufactured by Unitika Co., Ltd.) having a thickness of 38 μm, and typically dried at a temperature of 80° C. for 15 minutes to form a photosensitive resin layer having a thickness of 20 μm. Next, a polypropylene film (OPP-FOA, manufactured by Futamura Chemical Co., Ltd.) having a thickness of 18 μm was laminated onto the photosensitive resin layer to produce a photosensitive dry film.
[0104] (Evaluation of developability) A substrate with electrolytic copper plating of 17 μm on a copper-clad laminate of 1.6 mm thick FR-4 and 18 μm thick copper foil was etched to a depth of 1.0 μm using CZ-8101B processing by MEC Co., Ltd. The dry film prepared by the above method, specifically the photosensitive resin layer exposed by peeling the polypropylene film from the dry film, was laminated thereon using a vacuum laminator (CVP-300: manufactured by Nikko Materials Co., Ltd.) under conditions of a vacuum pressure of 3 hPa and a vacuum time of 30 seconds in a first chamber at 90°C, and then pressed under conditions of a press pressure of 0.5 MPa and a press time of 30 seconds. Then, the polyethylene terephthalate film was peeled off from the resin layer of the photosensitive dry film. The obtained substrate was developed for 60 seconds using a 1% Na2CO3 aqueous solution at 30°C under a spray pressure of 0.2 MPa, and the presence or absence of development residue was confirmed. The evaluation criteria for developability were as follows. ⊚: No residue was observed after 60 seconds of development. ◯: After 60 seconds of development, there was residue, but after 90 seconds of development, there was no residue. Δ: After 90 seconds of development, there was residue, but after 120 seconds of development, there was no residue. ×: Residue was found after 120 seconds of development.
[0105] (Evaluation of resolution) A substrate made of 17 μm electrolytic copper plating on a 1.6 mm thick copper-clad laminate of FR-4 and 18 μm thick copper foil was etched to a depth of 1.0 μm using CZ-8101B treatment by MEC Co., Ltd. The dry film prepared by the above method, specifically the photosensitive resin layer exposed by peeling the polypropylene film from the dry film, was laminated thereon using a vacuum laminator (CVP-300: Nikko Materials Co., Ltd.) under conditions of a vacuum pressure of 3 hPa and a vacuum time of 30 seconds in a first chamber at 90°C, and then pressed under conditions of a pressure of 0.5 MPa and a press time of 30 seconds. Next, exposure was performed with each opening pattern of 40 to 60 μm using an exposure device equipped with a high-pressure mercury lamp. The exposure amount was adjusted using a step tablet (Photec 41 step) so that the gloss sensitivity was 10 steps, and 10 minutes after exposure, the polyethylene terephthalate film was peeled off from the resin layer of the photosensitive dry film to expose the photosensitive resin layer. Then, a 1% by mass Na2CO3 aqueous solution at 30°C was sprayed at a pressure of 2 kg / cm 2 The substrate with this cured film was placed in a UV conveyor furnace with an integrated exposure of 1,000 mJ / cm. 2 After irradiating with ultraviolet light under the above conditions, the resin was heated and cured at 150°C for 60 minutes. The opening diameter of the cured product was observed with a SEM at a magnification of 1,300 times to check for the occurrence of halation or undercut. The evaluation criteria for resolution were as follows: ◎: A good aperture diameter was obtained with an aperture diameter of 50 μm. ◯: A good aperture diameter was obtained with an aperture diameter of 55 μm. ×: A satisfactory opening diameter was not obtained with an opening diameter of 55 μm.
[0106] (Evaluation of Melt Viscosity) The dry films prepared by the above method were laminated at a lamination temperature of 40° C. using a vacuum laminator (CVP-300: manufactured by Nikko Materials Co., Ltd.) to prepare a resin layer (laminate of resin layers) having a thickness of about 400 μm and a width of 25 mm, and the melt viscosity was measured using a MARS40 manufactured by Thermo Scientific under the measurement conditions of a heating rate of 5° C. / min, a measurement frequency of 1 Hz, and a measurement pressure of 3 Pa. The evaluation criteria for melt viscosity were as follows. Good: The lowest melt viscosity in the range from 70°C to 130°C was less than 100 Pa s. ×: The melt viscosity at the lowest point in the range from 70°C to 130°C was 100 Pa·s or more.
[0107] (Evaluation of circuit embedding) This evaluation was carried out to evaluate whether or not lamination failure occurred. A substrate on which a copper circuit with a copper thickness of 18 μm and L / S=20 μm / 20 μm was formed was subjected to etching treatment equivalent to 1.0 μm using CZ-8101B treatment manufactured by MEC Co., Ltd. The dry film prepared by the above method, specifically the photosensitive resin layer exposed by peeling off the polypropylene film from the dry film, was laminated thereon using a vacuum laminator (CVP-300: manufactured by Nikko Materials Co., Ltd.) under conditions of a vacuum pressure of 3 hPa and a vacuum time of 30 seconds in a first chamber at 90°C, and then pressing was performed under conditions of a press pressure of 0.5 MPa and a press time of 30 seconds. Next, exposure was performed by solid exposure using an exposure device equipped with a high-pressure mercury lamp. The exposure dose was adjusted using a step tablet (Photec 41 step) so that the gloss sensitivity was 10 steps, and 10 minutes after exposure, the polyethylene terephthalate film was peeled off from the resin layer of the photosensitive dry film to expose the photosensitive resin layer. Then, a 1% by mass Na2CO3 aqueous solution at 30°C was sprayed at a pressure of 2 kg / cm 2 The substrate with this cured film was placed in a UV conveyor furnace with an integrated exposure of 1,000 mJ / cm. 2 After irradiating with ultraviolet light under the above conditions, the material was heat-cured at 150°C for 60 minutes. The cured material was examined under an optical microscope to evaluate the presence or absence of voids between L / S. The evaluation criteria for circuit embedding were as follows: A: No voids were observed. ×: Voids were observed.
[0108] (Evaluation of heat resistance) A substrate with a cured film was prepared in the same manner as for the evaluation of resolution, except that the entire surface was exposed to light. A rosin-based flux was applied to the cured film on the prepared substrate, which was then passed through a reflow oven previously set to a maximum of 260°C, and the cured coating film was evaluated for blistering and peeling. The evaluation criteria for heat resistance were as follows: ◎: No swelling or peeling even after 10 passes or more. ◯: No swelling or peeling occurred even after 5 or more but less than 10 passes. △: No swelling or peeling occurred even after passing once or more but less than five times. ×: Blistering and peeling occurred after one application.
[0109] From the results shown in the above table, it is understood that the present invention can provide a curable resin composition and the like that can maintain a low melt viscosity even when applied to a dry film while improving developability, resolution, and heat resistance, and does not cause lamination defects when forming a solder resist. Furthermore, it is understood that the developability and heat resistance are improved when the blending amount of the aminotriazine skeleton-containing thermosetting catalyst having a structure in which one or two amino groups are attached to a triazine skeleton is in the range of 0.1 to 10.0 parts by mass, calculated as solid content, relative to 100 parts by mass of the alkali-soluble resin.
Claims
1. Alkali-soluble resin, Photopolymerization initiator, A thermosetting compound, and Aminotriazine skeleton-containing heat curing catalyst wherein the aminotriazine skeleton-containing heat curing catalyst has a structure in which one or two amino groups are attached to a triazine skeleton.
2. The curable resin composition according to claim 1 , wherein the aminotriazine skeleton-containing heat curing catalyst contains a silyl group or a hydroxyl group.
3. 2. The curable resin composition according to claim 1, comprising, in terms of solid content, 0.1 to 10.0 parts by mass of the aminotriazine skeleton-containing thermosetting catalyst per 100 parts by mass of the alkali-soluble resin.
4. The curable resin composition according to claim 1, having a melt viscosity at the lowest point in the range of from 70°C to 130°C of less than 100 Pa·s.
5. A dry film comprising a resin layer obtained by applying the curable resin composition according to claim 1 to a first film and drying the applied resin layer.
6. A cured product obtained by curing the curable resin composition according to claim 1 or the resin layer of the dry film according to claim 5.
7. An electronic part comprising the cured product according to claim 6.
Citation Information
Patent Citations
Curable resin composition, dry film, cured product, and printed wiring board
JP2022009428A