Phenoxy resin and use thereof
A novel phenoxy resin with a specific structure addresses the thermal conductivity limitations of bisphenol A epoxy resins, enhancing thermal conductivity and fluidity for improved heat dissipation insulating materials.
Patent Information
- Application Number
- JP2024116966
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2019-12-25
- Filing Date
- 2024-07-22
- Publication Date
- 2024-10-11
- Estimated Expiration
- 2040-06-09
AI Technical Summary
Existing bisphenol A epoxy resins have limitations in thermal conductivity, and there is a need for improved thermal conductivity in heat dissipation insulating materials used in electrical and electronic equipment.
A novel phenoxy resin with a specific structure, represented by general formula (1), is synthesized by reacting a bifunctional phenol compound, enhancing thermal conductivity through a mesogenic structure with an ester bond between benzene rings.
The phenoxy resin exhibits excellent thermal conductivity and fluidity, improving the thermal conductivity and moldability of resin materials, making them suitable for heat dissipation insulating materials.
Smart Images

Figure 2024144471000025 
Figure 2024144471000001 
Figure 2024144471000002
Abstract
Description
[Technical field]
[0001] The present invention relates to a novel phenoxy resin and its use. [Background technology]
[0002] Various developments have been made in the field of heat dissipation and insulation materials. For example, the technology described in Patent Document 1 is known as this type of technology. Patent Document 1 describes a thermosetting resin composition using bisphenol A type epoxy resin, a phenolic curing agent, and boron nitride particles as a thermally conductive filler as a heat dissipation and insulation material constituting electric / electronic devices and the like (Table 1 of Patent Document 1).
[0003] Moreover, Patent Document 2 describes an encapsulating resin composition containing a biphenyl-type epoxy resin represented by a specific general formula. [Prior art documents] [Patent documents]
[0004] [Patent Document 1] JP 2015-193504 A [Patent Document 2] JP 2019-151691 A Summary of the Invention [Problem to be solved by the invention]
[0005] However, there is room for improvement in terms of thermal conductivity in the bisphenol A type epoxy resin described in Patent Document 1. Note that Patent Document 2 does not mention thermal conductivity. [Means for solving the problem]
[0006] As a result of investigations, the present inventors have found that high thermal conductivity can be achieved by using a novel phenoxy resin having a specific structure, and have completed the present invention. According to the present invention, There is provided a phenoxy resin comprising a repeating unit represented by the following general formula (1). [ka] (In general formula (1), R 1 ~R 4 each independently represents a hydrogen atom, a halogen atom, a hydroxyl group, an amino group, an alkyl group having 1 to 6 carbon atoms, an alkoxy group having 1 to 6 carbon atoms, or an allyl group. Q 1 ~Q 4 each independently represents a hydrogen atom, an alkyl group having 1 to 6 carbon atoms, or an alkoxy group having 1 to 6 carbon atoms. * represents a bond.)
[0007] According to the present invention, there is provided a thermosetting resin composition containing the above-mentioned phenoxy resin. According to the present invention, there is provided a thermally conductive resin composition comprising the above-mentioned thermosetting resin composition. According to the present invention, there is provided a thermally conductive resin sheet comprising the thermally conductive resin composition.
[0008] Further, according to the present invention, The following general formula (a): [ka] (In general formula (a), R 1 ~R 4 each independently represents a hydrogen atom, a halogen atom, a hydroxyl group, an amino group, an alkyl group having 1 to 6 carbon atoms, an alkoxy group having 1 to 6 carbon atoms, or an allyl group, 1 ~R 4 may be the same or different.) and a difunctional epoxy compound (a) represented by the general formula (b): [ka] (In general formula (b), Q 1 ~Q 4 each independently represents a hydrogen atom, an alkyl group having 1 to 6 carbon atoms, or an alkoxy group having 1 to 6 carbon atoms; 1 ~Q4 may be the same or different.) The present invention provides a method for producing a phenoxy resin containing a repeating unit represented by the following general formula (1), by reacting a difunctional phenol compound (b) represented by the following general formula (1): [ka] (In general formula (1), R 1 ~R 4 is the same as in formula (a), and Q 1 ~Q 4 is the same as in formula (b). * indicates a bond.) Effect of the Invention
[0009] According to the present invention, there are provided a phenoxy resin having excellent thermal conductivity and a resin material using the same. [Brief description of the drawings]
[0010] [Figure 1] 1 is a cross-sectional view showing a configuration of a metal base substrate according to an embodiment of the present invention. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0011] Hereinafter, an embodiment of the present invention will be described with reference to the drawings. In all drawings, similar components are given similar reference symbols and their explanations will be omitted as appropriate. In addition, "~" indicates "above" to "below" unless otherwise specified.
[0012] [Phenoxy resin (A)] The phenoxy resin (A) of the present embodiment contains a repeating unit represented by the following general formula (1): The phenoxy resin (A) has a novel structure (mesogen structure) having an ester bond between two benzene rings, and has excellent thermal conductivity.
[0013] [ka]
[0014] In general formula (1), R 1 ~R 4 each independently represents a hydrogen atom, a halogen atom, a hydroxyl group, an amino group, an alkyl group having 1 to 6 carbon atoms, an alkoxy group having 1 to 6 carbon atoms, or an allyl group.
[0015] R 1 ~R 4 From the viewpoint of the effects of the present invention, is preferably an alkyl group having 1 to 6 carbon atoms, an alkoxy group having 1 to 6 carbon atoms, or an allyl group, more preferably an alkyl group having 1 to 6 carbon atoms, and particularly preferably an alkyl group having 1 to 3 carbon atoms.
[0016] Q 1 ~Q 4 each independently represents a hydrogen atom, an alkyl group having 1 to 6 carbon atoms, or an alkoxy group having 1 to 6 carbon atoms.
[0017] Q 1 ~Q 4 From the viewpoint of the effects of the present invention, is preferably a hydrogen atom or an alkyl group having 1 to 6 carbon atoms, more preferably a hydrogen atom or an alkyl group having 1 to 3 carbon atoms, and particularly preferably a hydrogen atom. * indicates a bond.
[0018] The phenoxy resin (A) of the present embodiment preferably has a structure represented by the following general formula (2) at its terminal, and more preferably has said structure at at least one of both terminals. [ka]
[0019] In general formula (2), R 1 ~R 4 has the same meaning as in formula (1). * indicates a bond. The biphenyl skeleton in the structure represented by formula (2) may be the biphenyl skeleton in formula (1).
[0020] The phenoxy resin (A) of the present embodiment is not particularly limited as long as it contains a repeating unit represented by general formula (1) and preferably further has a structure represented by the following general formula (2) at at least one of both ends. Specific examples of the phenoxy resin (A) include phenoxy resins represented by the following general formula (3).
[0021] [ka]
[0022] In general formula (3), R 1 ~R 4 and Q 1 ~Q 4 has the same meaning as in general formula (1). 1 ~R 4 Q may be the same or different, and there may be multiple 1 ~Q 4 may be the same or different. n is a number of 1 or more and 50 or less, and preferably a number of 2 or more and 30 or less, on average.
[0023] The weight average molecular weight (Mw) of the phenoxy resin (A) is from 2,000 to 30,000, preferably from 2,000 to 20,000, and more preferably from 2,000 to 10,000. Mw is measured by gel permeation chromatography and is expressed as a value converted using a standard polystyrene calibration curve. By setting the Mw within the above range, the thermal conductivity and flowability of the phenoxy resin can be further improved.
[0024] In this embodiment, a molecular weight distribution curve for the phenoxy resin is obtained using GPC (Gel Permeation Chromatography). The weight average molecular weight (Mw), number average molecular weight (Mn), and polydispersity index (PDI: Mw / Mn) of the phenoxy resin (A) are calculated using polystyrene-equivalent values obtained from a calibration curve of standard polystyrene (PS) obtained by GPC measurement.
[0025] The measurement conditions for GPC are, for example, as follows. Tosoh Corporation gel permeation chromatography device HLC-8320GPC Column: TSK-GEL GMH, G2000H, SuperHM-M manufactured by Tosoh Corporation Detector: RI detector for liquid chromatography Measurement temperature: 40℃ Solvent: THF Sample concentration: 2.0 mg / ml
[0026] The weight average molecular weight (Mw), number average molecular weight (Mn), and polydispersity index (PDI: Mw / Mn) of the phenoxy resin (A) are calculated using polystyrene-equivalent values obtained from a calibration curve of standard polystyrene (PS) obtained by GPC measurement.
[0027] The polydispersity (Mw / Mn) of the phenoxy resin (A) is, for example, 1.00 to 5.00, preferably 1.20 to 4.00, and more preferably 1.30 to 3.50. By setting the polydispersity within the above range, the thermal conductivity and fluidity of the phenoxy resin (A) can be further improved.
[0028] From the viewpoint of the effects of the present invention, the epoxy equivalent of the phenoxy resin (A) is 300 g / eq or more and 6,000 g / eq or less, preferably 350 g / eq or more and 5,000 g / eq or less, and more preferably 400 g / eq or more and 4,500 g / eq or less.
[0029] The melt viscosity of the phenoxy resin (A) at 180° C. is 50 mPa·s or less, and preferably 30 mPa·s or less, which provides excellent moldability and excellent production stability of resin sheets and resin films.
[0030] [Production method of phenoxy resin (A)] The phenoxy resin (A) containing a repeating unit represented by general formula (1) of the present embodiment can be synthesized by reacting a bifunctional epoxy compound (a) represented by general formula (a) with a bifunctional phenol compound (b) represented by general formula (b), as shown in the following reaction formula.
[0031] [ka]
[0032] In general formula (a), R 1 ~R 4 is the same as in formula (1), and in formula (b), Q 1 ~Q 4 has the same meaning as general formula (1). The above reaction can be carried out in the absence of a solvent or in the presence of a reaction solvent using a reaction catalyst.
[0033] As the reaction solvent, aprotic organic solvents such as methyl ethyl ketone, dioxane, tetrahydrofuran, acetophenone, N-methylpyrrolidone, dimethyl sulfoxide, N,N-dimethylacetamide, sulfolane, propylene glycol monomethyl ether, and cyclohexanone can be suitably used. By using a reaction solvent, the initial viscosity can be reduced and the reactivity of the monomers is improved.
[0034] As the reaction catalyst, a conventionally known polymerization catalyst can be used, and alkali metal hydroxides, tertiary amine compounds, quaternary ammonium compounds, tertiary phosphine compounds, quaternary phosphonium compounds, and imidazole compounds are preferably used.
[0035] Specifically, a bifunctional epoxy compound (a), a bifunctional phenol compound (b), a reaction catalyst, and optionally a reaction solvent are added and melt-mixed under stirring. The heating temperature during melt-mixing is about 90 to 120°C, the mixing time is about 30 minutes to 2 hours, and the reaction pressure is normal pressure.
[0036] After melt mixing, the mixed solution is heated and the polymerization reaction is carried out at a predetermined reaction temperature under reduced pressure or normal pressure at a reaction temperature of about 140 to 180° C., a reaction time of about 2 to 10 hours, and a reaction pressure of about 1 to 760 Torr.
[0037] After the reaction is completed, the phenoxy resin (A) can be obtained as a resin dissolved in a suitable solvent by performing solvent replacement, etc. The phenoxy resin (A) obtained by the solvent reaction can also be obtained as a solvent-free solid resin by performing a solvent removal treatment using an evaporator, etc. The phenoxy resin (A) of the general formula (1) of this embodiment can be obtained by the above synthesis method.
[0038] The phenoxy resin (A) of the present embodiment can be obtained as a mixture containing impurities such as ionic impurities and low molecular weight components. When the phenoxy resin contains these components, it can also be called a phenoxy resin composition.
[0039] The phenoxy resin (A) can be obtained by purifying the crude phenoxy resin (phenoxy resin composition) containing impurities obtained after synthesis. By setting the allowable values of impurities as described below, it is possible to obtain a desired phenoxy resin composition and reduce the purification load. Furthermore, by containing a specified amount of impurities, a specified effect can be obtained. In this specification, the phenoxy resin (A) can be defined as containing impurities such as ionic impurities and low molecular weight components, but not containing a solvent.
[0040] From the viewpoint of insulating properties, the phenoxy resin (A) of the present embodiment may contain ionic impurities in an amount of 1,500 ppm or less, preferably 1,300 ppm or less, and more preferably 1,200 ppm or less.
[0041] The ionic impurities include F-, Cl - , NO2 - , Br ― , NO3 ― , PO4 3- , SO42- , (COO)2 2- , CH3COO - , H.C.O.O. - etc. can be mentioned. The ionic impurity concentration can be measured, for example, as follows. First, the phenoxy resin (A) is weighed into a container, ultrapure water is added, and the container is sealed. Next, hot water extraction is performed by heat treatment at a temperature of 125°C for 20 hours using a thermostatic bath. Next, the phenoxy resin (A) and the like are removed from the solution obtained by hot water extraction by centrifugation, filtration, or the like to prepare a test liquid. Next, the ionic impurity content in the test liquid is measured using an ion chromatography analyzer by a calibration curve method using a standard solution. The ionic impurity content in the phenoxy resin (A) used to prepare the test liquid was taken as the ionic impurity concentration.
[0042] The ionic impurities may include hydrolyzable chlorine. From the viewpoint of insulating properties, the phenoxy resin (A) of the present embodiment may contain ionic impurities including hydrolyzable chlorine in the above-mentioned amounts. The hydrolyzable chlorine concentration can be measured, for example, as follows. First, phenoxy resin (A), an acetone-methanol mixed solution, and a methanol solution of CH3ONa are mixed, and BTB solution is added as an indicator. Next, nitric acid is added until the solution turns yellow, and then the above indicator is added. This solution is subjected to potentiometric titration with an aqueous silver nitrate solution using an automatic titrator (using a silver electrode) to determine the amount of hydrolyzable chlorine. The amount of hydrolyzable chlorine relative to phenoxy resin (A) is taken as the hydrolyzable chlorine concentration.
[0043] The low molecular weight component contained in the phenoxy resin (A) of this embodiment is a component having a weight average molecular weight Mw of 1,000 or less. The low molecular weight component may contain at least one of the monomer components (C) (difunctional epoxy compound (a), difunctional phenol compound (b)) contained in the phenoxy resin (A) and a low molecular weight component (B) having Mw of 1k or less and not including the monomer component (C). The low molecular weight component (B) may be composed of one or more polymers of the monomer components (C).
[0044] By reducing the amount of low molecular weight components contained in the phenoxy resin (A), the thermal conductivity can be further increased, and further, the flowability of the phenoxy resin (A) can be improved.
[0045] The peak area corresponding to the low molecular weight components (B+C) in the phenoxy resin (A) having Mw of 1k or less is calculated from the ratio of the total area of components having a weight average molecular weight Mw of 1,000 or less to the total area (100%) of the entire molecular weight distribution based on data on molecular weight obtained, for example, by GPC measurement.
[0046] The low molecular weight component (B+C) having an Mw of 1k or less includes a monomer component (C) and a low molecular weight component (B) having an Mw of 1,000 or less that does not contain the monomer component (C).
[0047] The total peak area of 100% is defined as the sum of the peak areas of the phenoxy resin (A), the monomer component (C), and the low molecular weight component (B) having an Mw of 1,000 or less and not including the monomer component (C).
[0048] The peak area of the low molecular weight components (B+C) can be 10% or less, preferably 7% or less, thereby making it possible to further improve the thermal conductivity of the phenoxy resin (A).
[0049] In the molecular weight distribution of the phenoxy resin (A) measured by GPC, the peak area of the low molecular weight component (B) having Mw of 1,000 or less can be 7% or less, preferably 5% or less, relative to the total peak area (100%), which can further improve the thermal conductivity of the phenoxy resin (A).
[0050] The low molecular weight component (B) having an Mw of 1,000 or less does not contain the monomer component (C). The peak area ratio of the low molecular weight component (B) having an Mw of 1,000 or less represents the content ratio of low-molecular weight components (low molecular weight polymer components) contained in the low molecular weight component.
[0051] In the molecular weight distribution of the phenoxy resin (A) obtained by GPC measurement, the peak area of the monomer component (C) relative to the total peak area (100%) can be 3% or less, preferably 2% or less, thereby further improving the thermal conductivity of the phenoxy resin (A). Furthermore, the melting point and melt viscosity of the phenoxy resin (A) can be adjusted by the molecular weight of the phenoxy resin (A) and the amount of the low molecular weight component.
[0052] In this embodiment, for example, by appropriately selecting the type and amount of each component contained in the phenoxy resin (A), the preparation method of the phenoxy resin (A), etc., it is possible to control the peak area of the low molecular weight components (B+C) in the phenoxy resin (A), the peak area of the low molecular weight component (B), and the Mw and Mw / Mn of the phenoxy resin (A). Among these, for example, appropriately selecting the synthesis conditions of the phenoxy resin (A), such as the reaction temperature, reaction time, and removal of monomers, can be cited as an element for setting the peak area of the low molecular weight components (B+C) in the phenoxy resin (A), the peak area of the low molecular weight component (B), and the Mw and Mw / Mn of the phenoxy resin (A) in the desired numerical range.
[0053] Hereinafter, a resin material using the phenoxy resin (A) of this embodiment will be described. The resin material of the present embodiment includes a phenoxy resin (A) or a phenoxy resin composition. The content can be appropriately adjusted based on various applications and other blending components. For example, the content of the phenoxy resin (A) in the thermosetting resin composition used for the heat dissipation insulating material is, for example, 1 mass % to 70 mass %, preferably 2 mass % to 50 mass %, and more preferably 3 mass % to 45 mass %, based on the non-volatile components (100 mass %) of the thermosetting resin composition not including a filler.
[0054] Here, the term "filler" includes ordinary fillers such as a thermally conductive filler, an inorganic filler, or an organic filler, which will be described later. That is, a thermosetting resin composition that does not contain a filler is composed of resin components other than a filler, and includes, as the resin components, for example, a thermosetting resin and a phenoxy resin. It also refers to the non-volatile content (100 mass%) in the thermosetting resin composition, and refers to the remainder excluding water, solvents, and other solvents. The thermosetting resin composition may contain a thermosetting resin other than the phenoxy resin (A).
[0055] Examples of the thermosetting resin include epoxy resin, polyimide resin, benzoxazine resin, unsaturated polyester resin, phenol resin, melamine resin, silicone resin, cyanate resin, bismaleimide resin, acrylic resin, phenol derivatives, and derivatives thereof. As the thermosetting resin, a monomer, oligomer, or polymer having two or more reactive functional groups in one molecule can be used, and the molecular weight or molecular structure is not particularly limited. These may be used alone or in combination of two or more.
[0056] The thermosetting resin composition may contain a curing agent, if necessary. The curing agent is selected depending on the type of thermosetting resin, and is not particularly limited as long as it reacts with the thermosetting resin.
[0057] Examples of the curing agent include phenolic resin curing agents, amine curing agents, acid anhydride curing agents, mercaptan curing agents, etc. These may be used alone or in combination of two or more.
[0058] (Cure accelerator) The thermosetting resin composition may contain a curing accelerator as necessary. The type and amount of the curing accelerator are not particularly limited, but an appropriate one can be selected from the viewpoints of reaction rate, reaction temperature, storage property, and the like.
[0059] Examples of the curing accelerator include imidazoles, organic phosphorus compounds, tertiary amines, phenolic compounds, organic acids, etc. These may be used alone or in combination of two or more. Among these, from the viewpoint of improving heat resistance, it is preferable to use nitrogen atom-containing compounds such as imidazoles.
[0060] The thermosetting resin composition may contain a thermally conductive filler. The thermally conductive filler may contain, for example, highly thermally conductive inorganic particles having a thermal conductivity of 20 W / m·K or more. The highly thermally conductive inorganic particles may contain, for example, at least one selected from alumina, aluminum nitride, boron nitride, silicon nitride, silicon carbide, and magnesium oxide. These may be used alone or in combination of two or more.
[0061] The thermally conductive filler may contain boron nitride in the form of monodisperse particles, agglomerated particles, or a mixture thereof, of scaly boron nitride. The scaly boron nitride may be granulated. By using agglomerated particles of scaly boron nitride, the thermal conductivity can be further increased. The agglomerated particles may be sintered particles or non-sintered particles.
[0062] The thermosetting resin composition may contain a silane coupling agent. This can improve the compatibility of the thermally conductive filler in the thermosetting resin composition. The coupling agent may be added to the thermosetting resin composition, or may be used by treating the surface of the thermally conductive filler.
[0063] The thermosetting resin composition of the present embodiment may contain other components in addition to the above-mentioned components. Examples of the other components include an antioxidant and a leveling agent. The thermosetting resin composition of the present embodiment can be produced, for example, by the following method.
[0064] The above components can be dissolved in a solvent, mixed, and stirred to prepare a resin varnish (a thermosetting resin composition in the form of a varnish). This mixing can be performed using various mixers such as those for ultrasonic dispersion, high-pressure collision dispersion, high-speed rotation dispersion, bead mill, high-speed shear dispersion, and rotation-revolution dispersion.
[0065] The solvent is not particularly limited, but examples thereof include acetone, methyl isobutyl ketone, toluene, ethyl acetate, cyclohexane, heptane, cyclohexanone, tetrahydrofuran, dimethylformamide, dimethylacetamide, dimethylsulfoxide, ethylene glycol, cellosolve-based solvents, carbitol-based solvents, anisole, and N-methylpyrrolidone.
[0066] (Thermal conductive resin sheet) The thermally conductive resin sheet of the present embodiment includes a carrier substrate and a resin layer formed on the carrier substrate and made of the thermosetting resin composition of the present embodiment.
[0067] The resin sheet can be obtained, for example, by applying a varnish-like thermosetting resin composition onto a carrier substrate to obtain a coating film (resin layer) and then subjecting the coating film to a solvent removal treatment. The solvent content in the resin sheet can be 10% by weight or less based on the entire thermosetting resin composition. For example, the solvent removal treatment can be performed under conditions of 80°C to 200°C and 1 minute to 30 minutes.
[0068] In this embodiment, the carrier substrate may be, for example, a polymer film or a metal foil. Examples of the polymer film include, but are not limited to, polyolefins such as polyethylene and polypropylene, polyesters such as polyethylene terephthalate and polybutylene terephthalate, polycarbonates, release papers such as silicone sheets, and thermoplastic resin sheets having heat resistance such as fluorine-based resins and polyimide resins. Examples of the metal foil include, but are not limited to, copper and / or copper-based alloys, aluminum and / or aluminum-based alloys, iron and / or iron-based alloys, silver and / or silver-based alloys, gold and gold-based alloys, zinc and zinc-based alloys, nickel and nickel-based alloys, and tin and tin-based alloys.
[0069] (Resin substrate) The resin substrate of the present embodiment includes an insulating layer made of the cured product of the thermosetting resin composition. This resin substrate can be used as a material for a printed circuit board on which electronic components such as LEDs and power modules are mounted.
[0070] (Metal base board) As an example of this embodiment, a metal base substrate 100 will be described with reference to FIG. FIG. 1 is a cross-sectional view showing an example of the configuration of a metal base substrate 100. As shown in FIG.
[0071] As shown in Fig. 1, the metal base substrate 100 may include a metal substrate 101, an insulating layer 102 provided on the metal substrate 101, and a metal layer 103 provided on the insulating layer 102. The insulating layer 102 may be made of one material selected from the group consisting of a resin layer made of the above-mentioned thermosetting resin composition, a cured product of the thermosetting resin composition, and a laminate. Each of the resin layer and the laminate may be made of a thermosetting resin composition in a B-stage state before the circuit processing of the metal layer 103, and may be a cured product obtained by curing the resin composition after the circuit processing.
[0072] The metal layer 103 is provided on the insulating layer 102 and is subjected to circuit processing. Examples of metals constituting the metal layer 103 include one or more selected from copper, copper alloys, aluminum, aluminum alloys, nickel, iron, tin, and the like. Among these, the metal layer 103 is preferably a copper layer or an aluminum layer, and is particularly preferably a copper layer. By using copper or aluminum, the circuit processing property of the metal layer 103 can be improved. The metal layer 103 may be a metal foil available in a plate shape, or a metal foil available in a roll shape.
[0073] The lower limit of the thickness of the metal layer 103 is, for example, 0.01 mm or more, and preferably 0.035 mm or more, so long as it is applicable to applications requiring a high current. The upper limit of the thickness of the metal layer 103 is, for example, 10.0 mm or less, and preferably 5 mm or less. If the thickness is less than this value, the circuit processability can be improved, and the substrate as a whole can be made thinner.
[0074] The metal substrate 101 has a role of dissipating heat accumulated in the metal base substrate 100. The metal substrate 101 is not particularly limited as long as it is a heat dissipating metal substrate, but may be, for example, a copper substrate, a copper alloy substrate, an aluminum substrate, or an aluminum alloy substrate, with a copper substrate or an aluminum substrate being preferred, and a copper substrate being more preferred. By using a copper substrate or an aluminum substrate, the heat dissipation properties of the metal substrate 101 can be improved.
[0075] The thickness of the metal substrate 101 can be appropriately set as long as it does not impair the object of the present invention. The upper limit of the thickness of the metal substrate 101 is, for example, 20.0 mm or less, and preferably 5.0 mm or less. By using a metal substrate 101 having a thickness of this value or less, the workability of the metal base substrate 100 in the outer shaping, cutting, and other processes can be improved.
[0076] The lower limit of the thickness of the metal substrate 101 is, for example, 0.01 mm or more, and preferably 0.6 mm or more. By using a metal substrate 101 having a thickness of this value or more, the heat dissipation properties of the metal base substrate 100 as a whole can be improved.
[0077] In this embodiment, the metal base substrate 100 can be used for various substrate applications, but because of its excellent thermal conductivity and heat resistance, it can be used as a printed circuit board that uses an LED or a power module.
[0078] The metal base substrate 100 may have a metal layer 103 that is circuitized by etching or the like into a pattern. In this metal base substrate 100, a solder resist (not shown) may be formed on the outermost layer, and connection electrodes may be exposed so that electronic components can be mounted thereon by exposure and development.
[0079] Although the embodiments of the present invention have been described above, these are merely examples of the present invention, and various configurations other than those described above can be adopted as long as they do not impair the effects of the present invention. EXAMPLES
[0080] The present invention will be described in more detail below with reference to examples, but the present invention is not limited to these. The raw materials used in the examples are as follows: (Epoxy compounds) Epoxy compound a: Tetramethylbiphenyl type epoxy resin represented by the following chemical formula (bifunctional epoxy compound, with mesogen structure, manufactured by Mitsubishi Chemical Corporation, YX4000)
[0081] [ka]
[0082] Epoxy compound b: a 50 / 50 mixture of a biphenyl type epoxy represented by the following chemical formula (i) and a tetramethylbiphenyl type epoxy represented by the following chemical formula (ii) (bifunctional epoxy compound, with mesogen structure, manufactured by Mitsubishi Chemical Corporation, YL6121)
[0083] [ka]
[0084] (Phenol compounds) Phenol compound a: ester group-containing bisphenol represented by the following chemical formula (bifunctional phenol compound, with mesogen structure, Ueno Pharmaceutical Co., Ltd., HQHBA)
[0085] [ka]
[0086] <Synthesis of phenoxy resin> Example 1 Epoxy compound a (59 parts by weight), phenol compound a (35 parts by weight), triphenylphosphine (TPP) (0.05 parts by weight), and solvent (cyclohexanone) (6 parts by weight) were added to a reactor and melt-mixed at 100°C to 110°C for 1 hour. The mixture was then heated to 150°C, and reacted while removing the solvent under reduced pressure at that temperature. It was confirmed by GPC that the desired molecular weight was reached, and the reaction was stopped to obtain phenoxy resin 1 represented by the following chemical formula. The reaction was carried out for 16 hours. After the reaction, cyclohexanone (100 parts by weight relative to the resin) was added to dissolve the resin and cooled to room temperature. After cooling, the mixture was purified by reprecipitation using methanol to obtain 113 parts by weight of phenoxy resin 1 (the average value of the number of repeating units n in the chemical formula is 15).
[0087] [ka]
[0088] Example 2 A synthetic method similar to that of Example 1 was used to obtain 112 parts by weight of phenoxy resin 2 (the average number of repeating units n in the chemical formula is 19) represented by the following general formula, except that epoxy resin a was changed to epoxy resin b.
[0089] [ka]
[0090] In the above general formula, R is a hydrogen atom or a methyl group, and the R bonded to each biphenyl skeleton is the same.
[0091] Comparative Example 1 As the phenoxy resin, a bisphenol A type phenoxy resin (without mesogen structure, manufactured by Mitsubishi Chemical Corporation, YP-55) represented by the following chemical formula was used.
[0092] [ka]
[0093] The physical properties of the phenoxy resins in the examples and comparative examples were measured by the following methods. (Molecular weight, dispersity, and peak area) The GPC measurement conditions are as follows. Tosoh Corporation gel permeation chromatography device HLC-8320GPC Column: Tosoh Corporation TSK-GEL GMH, G2000H, SuperHM-M Detector: RI detector for liquid chromatography ·Measurement temperature: 40℃ Solvent: THF Sample concentration: 2.0 mg / ml
[0094] The weight average molecular weight (Mw), number average molecular weight (Mn), and polydispersity index (PDI: Mw / Mn) were calculated using polystyrene-equivalent values obtained from a calibration curve of standard polystyrene (PS) obtained by GPC measurement.
[0095] Based on the data on molecular weight obtained by the GPC measurement, the peaks in the molecular weight distribution were classified into (A) phenoxy resin with Mw over 1k, (B) low molecular weight components with Mw of 1k or less that do not contain monomers, and (C) monomers. The sum of (B) and (C) is the low molecular weight component with Mw of 1k or less.
[0096] When the total area of the molecular weight distribution obtained by the above GPC measurement was taken as 100%, the area ratio (%) of the peak area corresponding to the low molecular weight component (above (B) + (C)) having Mw of 1k or less contained in the phenoxy resin to be measured was calculated.
[0097] The phenoxy resins of the examples and comparative examples were evaluated by measuring their melt viscosity and thermal conductivity by the following methods. (Melt Viscosity) Approximately 0.1 g of ground phenoxy resin was weighed out using a cone plate viscometer CV-1S manufactured by Toa Kogyo Co., Ltd., and placed on a stage preheated to a specified temperature (150°C, 165°C, 180°C), and the torque value was measured when the cone rotation speed was 94 rpm to 750 rpm. The measured torque value was used to calculate the melt viscosity (mPa s) of the phenoxy resin.
[0098] (Thermal Conductivity) -Making resin molded products A mixture of 100 parts by weight of phenoxy resin and 2 parts by weight of catalyst (2-methylimidazole) was set in a mold coated with a release agent and compression molded at 180°C for 30 minutes to obtain a resin molded product with a diameter of 10 mm and a thickness of 1 mm. It was then cured in an oven at 180°C for 180 minutes to obtain a resin molded product (a sample for measuring thermal conductivity). Density of resin molding The density measurement was performed in accordance with JIS K 6911 (general test method for thermosetting plastics). The test pieces were cut from the above resin molded bodies to a size of 2 cm length x 2 cm width x 2 mm thickness. The unit of density (SP) is g / cm3.
[0099] -Specific heat of resin molded body The specific heat (Cp) of the resin molded article obtained above was measured by a DSC method.
[0100] -Measurement of thermal conductivity of resin molded products From the obtained resin molded body, a test piece was cut to a diameter of 10 mm and a thickness of 1 mm for thickness direction measurement. Next, the thermal diffusion coefficient (α) of the plate-shaped test piece in the thickness direction was measured by the laser flash method using a Xe flash analyzer TD-1RTV manufactured by ULVAC. The measurement was performed under the condition of air atmosphere and 25°C. For the resin molded article, the thermal conductivity was calculated based on the measured values of the thermal diffusion coefficient (α), specific heat (Cp), and density (SP) obtained, according to the following formula. Thermal conductivity [W / m K]=α[m 2 / s]×Cp[J / kg K]×Sp[g / cm 3 ]
[0101] [Table 1]
[0102] The phenoxy resins of the examples showed superior thermal conductivity compared to the comparative examples. Such novel phenoxy resins can be used as resin materials, and can be suitably used as heat dissipating insulating materials such as heat dissipating insulating substrates and sheets.
Claims
1. A phenoxy resin comprising a repeating unit represented by the following general formula (1): 【Chemistry 1】 (In general formula (1), R 1 ~R 4 each independently represents a hydrogen atom, a halogen atom, a hydroxyl group, an amino group, an alkyl group having 1 to 6 carbon atoms, an alkoxy group having 1 to 6 carbon atoms, or an allyl group. Q 1 ~Q 4 each independently represents a hydrogen atom, an alkyl group having 1 to 6 carbon atoms, or an alkoxy group having 1 to 6 carbon atoms. * represents a bond.)
2. The phenoxy resin according to claim 1, having a structure represented by the following general formula (2) at its terminal. 【Chemistry 2】 (In general formula (2), R 1 ~R 4 is the same as in formula (1). * indicates a bond.
3. The phenoxy resin according to claim 1 or 2, represented by the following general formula (3): 【Chemistry 3】 (In general formula (3), R 1 ~R 4 and Q. 1 ~Q 4 has the same meaning as in general formula (1). 1 ~R 4 may be the same or different, and multiple Q 1 ~Q 4 may be the same or different. n is the average value and is a number between 1 and 50.)
4. The phenoxy resin according to any one of claims 1 to 3, having a weight average molecular weight of 2,000 or more and 30,000 or less.
5. The phenoxy resin according to any one of claims 1 to 4, having an epoxy equivalent of 300 g / eq or more and 6,000 g / eq or less.
6. Further, the weight average molecular weight Mw of the low molecular weight component is 1,000 or less, The phenoxy resin according to any one of claims 1 to 5, wherein in the molecular weight distribution of the phenoxy resin obtained by gel permeation chromatography, the peak area of the low molecular weight component is 10% or less relative to the total peak area of 100%.
7. The phenoxy resin according to any one of claims 1 to 6, having an ionic impurity concentration of 1,500 ppm or less.
8. 8. The phenoxy resin of claim 7, wherein said ionic impurities include hydrolyzable chlorides.
9. A thermosetting resin composition comprising the phenoxy resin according to any one of claims 1 to 8.
10. A thermally conductive resin composition comprising the thermosetting resin composition according to claim 9.
11. A thermally conductive resin sheet comprising the thermally conductive resin composition according to claim 10.
12. The following general formula (a): 【Chemistry 4】 (In general formula (a), R 1 ~R 4 each independently represents a hydrogen atom, a halogen atom, a hydroxyl group, an amino group, an alkyl group having 1 to 6 carbon atoms, an alkoxy group having 1 to 6 carbon atoms, or an allyl group. and a bifunctional epoxy compound (a) represented by the general formula (b): 【Chemistry 5】 (In general formula (b), Q 1 ~Q 4 each independently represents a hydrogen atom, an alkyl group having 1 to 6 carbon atoms, or an alkoxy group having 1 to 6 carbon atoms. A method for producing a phenoxy resin containing a repeating unit represented by the following general formula (1), comprising reacting a bifunctional phenol compound (b) represented by the following general formula (1): 【Chemistry 6】 (In general formula (1), R 1 ~R 4 is the same as in formula (a), and Q 1 ~Q 4 has the same meaning as in formula (b). * indicates a bond.)
13. The method for producing a phenoxy resin according to claim 12, wherein the phenoxy resin has a structure represented by the following general formula (2) at an end thereof: 【Chemistry 7】 (In general formula (2), R 1 ~R 4 is the same as in formula (1). * indicates a bond.
14. The method for producing a phenoxy resin according to claim 12 or 13, wherein the phenoxy resin is represented by the following general formula (3): 【Chemistry 8】 (In general formula (3), R 1 ~R 4 and Q. 1 ~Q 4 has the same meaning as in general formula (1). 1 ~R 4 may be the same or different, and multiple Q 1 ~Q 4 may be the same or different. n is the average value and is a number between 1 and 50.)
Citation Information
Patent Citations
Novel epoxy resin and resin composition containing the same
JP1997227654A
Boron nitride particle, resin composition and heat-conductive sheet
JP2015193504A
Resin composition for encapsulation and power module
JP2019151691A