Polarizing plate and display device

The circularly polarizing plate with specific polarizer and retardation film compositions and structures prevents iodine elution, ensuring stable retardation values and image quality in high humidity environments.

JP2024144518AInactive Publication Date: 2024-10-11SUMITOMO CHEM CO LTD
View PDF 30 Cites 0 Cited by

Patent Information

Application Number
JP2024117679
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Priority Date
2019-02-04
Filing Date
2024-07-23
Publication Date
2024-10-11
Estimated Expiration
Not applicable · inactive patent

AI Technical Summary

Technical Problem

The in-plane retardation value of retardation films using polymerizable liquid crystal compounds increases in high temperature and high humidity environments, affecting the visibility of organic EL display devices.

Method used

A circularly polarizing plate is designed with a polarizer having a boron content of 1.00% by weight or more, moisture permeability of 50g/m²·24hr or more in protective films, and a retardation film made of hardened polymerizable liquid crystal compounds, with specific alignment films and adhesive layers to prevent iodine elution.

Benefits of technology

The in-plane retardation value of the retardation film remains stable in high temperature and high humidity conditions, maintaining image quality and visibility in organic EL display devices.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024144518000005
    Figure 2024144518000005
  • Figure 2024144518000006
    Figure 2024144518000006
  • Figure 2024144518000001
    Figure 2024144518000001
Patent Text Reader

Abstract

To provide a circular polarizing plate having a retardation film using a polymerizable liquid crystal compound which is difficult to increase an in-plane retardation value of the retardation film before and after being left under a high temperature and high humidity environment.SOLUTION: A circular polarizing plate has a polarizing plate and a retardation film, in which the polarizing plate includes a polarizer and a protective film bonded to at least one surface of the polarizer. The polarizer is a film in which iodine is adsorbed and oriented to a polyvinyl alcohol-based resin film, a boron content of the polarizer is 2.76 wt.% or more and 10.00 wt.% or less, moisture permeability of the protective film is 50 g / m2 24 hr or more, the retardation film includes a retardation layer composed of a layer formed by curing a polymerizable liquid crystal compound, and an orientation film, the orientation film is arranged on the polarizer layer of the retardation film, and the orientation film is composed of a polymer having a cinnamoyl group.SELECTED DRAWING: None
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a polarizing plate and a display device. [Background technology]

[0002] In recent years, image display devices, such as organic electroluminescence (hereinafter, also referred to as organic EL) display devices, have rapidly become widespread. Organic EL display devices are equipped with a circular polarizing plate that includes a polarizer and a retardation film (lambda / 4 plate). The placement of the circular polarizing plate can prevent reflection of external light and improve the visibility of the screen.

[0003] With the rise of organic EL display devices, there is a strong demand for thinner image display devices, and thus a demand for thinner circular polarizing plates as well. A change from conventional retardation films made of molded resin films to retardation films made of liquid crystal compounds that can be made thinner is being considered (see, for example, Patent Document 1). Retardation films using polymerizable liquid crystal compounds are produced by coating and aligning the polymerizable liquid crystal compounds on a substrate, and fixing the oriented state by irradiating the compound with light as necessary. [Prior art documents] [Patent documents]

[0004] [Patent Document 1] JP 2017-54093 A Summary of the Invention [Problem to be solved by the invention]

[0005] It has been found that when a circularly polarizing plate having a retardation film using a polymerizable liquid crystal compound is placed in a high-temperature, high-humidity environment, the in-plane retardation value of the retardation film increases. The increase in the in-plane retardation value can change the reflection hue and deteriorate the visibility of the image display device. The object of the present invention is to provide a circularly polarizing plate having a retardation film using a polymerizable liquid crystal compound, in which the in-plane retardation value of the retardation film is unlikely to increase before and after being placed in a high-temperature, high-humidity environment. [Means for solving the problem]

[0006] [1] A circular polarizing plate having a polarizing plate and a retardation film, The polarizing plate includes a polarizer and a protective film attached to at least one surface of the polarizer, the polarizer is a polyvinyl alcohol-based resin film having iodine adsorbed thereon and oriented therein; The boron content of the polarizer is 1.00% by weight or more, The moisture permeability of the protective film is 50 g / m 2 - 24 hours or more, The retardation film is a circular polarizing plate including a retardation layer formed of a cured layer of a polymerizable liquid crystal compound. [2] The circularly polarizing plate according to [1], wherein the polarizer has a thickness of 20 μm or less. [3] The circularly polarizing plate according to [1] or [2], wherein the polarizer has a luminosity-corrected single transmittance of 40% or more. [4] When the polarizer is maintained at 80°C for 4 hours, the shrinkage stress in the absorption axis direction per 2 mm width is 60 N / mm 2 The circularly polarizing plate according to any one of the above [1] to [3]. [5] The circularly polarizing plate according to any one of [1] to [4], wherein the polarizer has a single hue with an a* value of −0.90 or more and −0.60 or less and a b* value of 2.70 or more and 3.70 or less. [6] The retardation film includes an alignment film, The circularly polarizing plate according to any one of [1] to [5], wherein the alignment film is located between the polarizer and the retardation layer. [7] The circularly polarizing plate according to any one of [1] to [6], wherein the polarizing plate and the retardation film are attached to each other with an active energy ray-curable adhesive. [8] The polarizing plate has a protective film on both sides of a polarizer, The moisture permeability of one protective film is 500g / m 2 - 24 hours or more, The moisture permeability of the other protective film is 100g / m 2 The circularly polarizing plate according to any one of [1] to [7], wherein the lifetime is 24 hours or less. [9] The circularly polarizing plate according to any one of [1] to [8], further comprising a front panel, a light-shielding pattern, and a touch sensor.

[10] A display device comprising the circular polarizing plate according to any one of [1] to [9] and a display element. Effect of the Invention

[0007] According to the present invention, it is possible to provide a circular polarizing plate having a retardation film using a polymerizable liquid crystal compound, in which the in-plane retardation value of the retardation film is unlikely to increase before and after being placed in a high-temperature, high-humidity environment. [Brief description of the drawings]

[0008] [Figure 1] FIG. 2 is a schematic cross-sectional view showing a layer structure of a circular polarizing plate. [Diagram 2] FIG. 1 is a schematic cross-sectional view illustrating an example of a layer structure of an organic EL display device. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0009] <Circular polarizing plate> The circular polarizing plate of the present invention has a polarizing plate and a retardation film. The polarizing plate and the retardation film can be laminated, for example, via an adhesive layer. Examples of the adhesive layer include a pressure-sensitive adhesive layer and an adhesive layer described below. In the present invention, the polarizing plate refers to a laminate including a polarizer and a protective film attached to at least one surface of the polarizer.

[0010] Hereinafter, an example of the layer structure of the circular polarizer of the present invention will be described with reference to FIG. 1. In FIG. 1, the adhesive layers for bonding the polarizer 10 and the protective films 11 and 12 are not shown. The circular polarizer 100 shown in FIG. 1(a) has a layer structure in which a polarizer 1 in which a first protective film 11 is laminated on one surface of the polarizer 10 and a second protective film 12 is laminated on the other surface of the polarizer 10, and a retardation film 2 including a layer 20 in which a polymerizable liquid crystal compound is cured are laminated via an adhesive layer 13. Furthermore, the circular polarizer 100 has an adhesive layer 14 on the surface of the retardation film 2 opposite to the polarizer 1. The adhesive layer 14 can be an adhesive layer for bonding to an organic EL display element, a touch sensor, or the like.

[0011] The circular polarizing plate 101 shown in FIG. 1(b) has a layer structure in which a polarizing plate 1 in which a first protective film 11 is laminated on one surface of a polarizer 10 and a second protective film 12 is laminated on the other surface of the polarizer 10, and a retardation film 2 are laminated via an adhesive layer 13. In the circular polarizing plate 101, the retardation film 2 has a layer structure in which a layer 20 of a cured polymerizable liquid crystal compound and a layer 21 of a cured polymerizable liquid crystal compound are laminated via an adhesive layer 15. Furthermore, the circular polarizing plate 101 has an adhesive layer 14 on the surface of the retardation film 2 opposite to the polarizing plate 1. The adhesive layer 14 can be an adhesive layer for attaching to an organic EL display element, a touch sensor, or the like.

[0012] The circular polarizing plate 103 shown in FIG. 1(c) has a layer structure in which a polarizing plate 1 having a first protective film 11 laminated on one surface of a polarizer 10 and a retardation film 2 are laminated via an adhesive layer 13. In the circular polarizing plate 103, the polarizing plate 1 is a polarizing plate having a protective film only on one surface of the polarizer 10. In the circular polarizing plate 103, the retardation film 2 has a layer structure in which a layer 20 of a cured polymerizable liquid crystal compound and a layer 21 of a cured polymerizable liquid crystal compound are laminated via an adhesive layer 15. Furthermore, the circular polarizing plate 103 has an adhesive layer 14 on the surface of the retardation film 2 opposite to the polarizing plate 1. The adhesive layer 14 can be an adhesive layer for bonding to an organic EL display element, a touch sensor, or the like.

[0013] As shown in Fig. 1, the retardation film may have one retardation layer or two retardation layers. In addition to the retardation layer, the retardation film preferably has an alignment film for aligning a polymerizable liquid crystal compound during its production. As shown in Fig. 1, the polarizing plate may have a protective film laminated on only one surface of the polarizer, or on both surfaces.

[0014] The circular polarizing plate may have layers other than the layers shown in Fig. 1. Examples of layers that the circular polarizing plate may further have include a front plate, a light-shielding pattern, a touch sensor, etc. The front plate may be disposed on the side of the polarizing plate opposite to the side on which the retardation film is laminated.

[0015] The light-shielding pattern can be formed on the surface of the front plate on the polarizing plate side. The light-shielding pattern is formed in the frame (non-display area) of the image display device, and can prevent the wiring of the image display device from being visually recognized by the user.

[0016] The touch sensor is disposed on a surface of the retardation film opposite to the polarizing plate side. The touch sensor may be disposed between the front plate and the polarizing plate. The touch sensor is used as an input unit. As the touch sensor, various types such as a resistive film type, a surface acoustic wave type, an infrared type, an electromagnetic induction type, and a capacitance type have been proposed, and any of these types may be used. Among them, the capacitance type is preferable. The capacitance type touch sensor is divided into an active area and a non-active area located on the outer periphery of the active area. The active area is an area corresponding to an area (display area) where a screen is displayed on a display panel, and is an area where a user's touch is sensed, and the non-active area is an area corresponding to an area (non-display area) where a screen is not displayed on a display device. The touch sensor may include a substrate having a flexible characteristic; a sensing pattern formed in the active area of ​​the substrate; and each sensing line formed in the non-active area of ​​the substrate for connecting to an external driving circuit via the sensing pattern and a pad part. The substrate of the touch sensor is preferably one having a toughness of 2,000 MPa% or more from the viewpoint of suppressing cracks that may occur in the touch sensor. More preferably, the toughness is 2,000 MPa% to 30,000 MPa%. Here, toughness is defined as the area under the curve up to the breaking point in a stress (MPa)-strain (%) curve obtained through a tensile test of a polymer material.

[0017] The shape of the main surface of the circular polarizing plate can be substantially rectangular. The main surface means the surface having the widest area corresponding to the display surface. Being substantially rectangular means that at least one of the four corners (corners) may be cut or rounded to be obtuse, a part of the end face perpendicular to the main surface may have a recessed part (notch) recessed in the in-plane direction, or a part of the main surface may have a hole cut out in the shape of a circle, an ellipse, a polygon, or a combination thereof.

[0018] The size of the circular polarizing plate is not particularly limited. When the circular polarizing plate is substantially rectangular, the length of the long side is preferably 6 cm or more and 35 cm or less, more preferably 10 cm or more and 30 cm or less, and the length of the short side is preferably 5 cm or more and 30 cm or less, more preferably 6 cm or more and 25 cm or less.

[0019] <Polarizing plate> In the present invention, the polarizing plate includes a polarizer and a protective film attached to at least one surface of the polarizer. That is, the polarizing plate refers to a laminate consisting of a polarizer and a protective film attached to one or both surfaces of the polarizer. The protective film included in the polarizing plate may have a surface treatment layer such as a hard coat layer, an antireflection layer, or an antistatic layer, which will be described later. The polarizer and the protective film can be laminated via, for example, an adhesive layer or a pressure-sensitive adhesive layer. The members included in the polarizing plate will be described below.

[0020] (1) Polarizer The polarizer of the polarizing plate may be an absorption-type polarizer that absorbs linearly polarized light having a vibration plane parallel to its absorption axis and transmits linearly polarized light having a vibration plane perpendicular to the absorption axis (parallel to the transmission axis). In the present invention, the polarizer used is a polyvinyl alcohol-based resin film in which iodine is adsorbed and oriented.

[0021] The phenomenon that the in-plane retardation value of the retardation film increases in a high-temperature and high-humidity environment is due to the fact that moisture reacts with iodine (especially I3 - The present inventors have found through their studies that this occurs when iodine is dissolved from the polyvinyl alcohol-based resin film and the iodine migrates to the retardation film. Therefore, when the polarizer is a polyvinyl alcohol-based resin film in which iodine is adsorbed and aligned as in the present invention, it is easy to obtain the effect that the retardation value is unlikely to increase in a high-temperature and high-humidity environment.

[0022] In order to prevent iodine from eluting in a high-temperature and high-humidity environment, it is preferable to increase the crosslink density of the polarizer. As described later, the polarizer is manufactured through a process of immersing a polyvinyl alcohol-based resin film in an aqueous boric acid solution, and the boric acid crosslinks polyvinyl alcohol-based resin chains. If the crosslink density of the polarizer is large, iodine is easily retained in the polarizer even in a humid and hot environment. Since the crosslink density of the polarizer is considered to be related to the boron content in the polarizer, in the present invention, the boron content of the polarizer is 1.00% by weight or more, preferably 1.80% by weight or more, more preferably 2.00% by weight or more, and even more preferably 2.50% by weight or more. Although the upper limit is not particularly limited, the boron content of the polarizer may be 10.00% by weight or less, 8.00% by weight or less, or 6.00% by weight or less. The boron content of the polarizer is measured by a method described in the examples described later.

[0023] In other words, in order to prevent iodine from dissolving in a high-temperature, high-humidity environment, it is preferable to increase the shrinkage stress of the polarizer. This is because the shrinkage stress of the polarizer reflects the degree of crosslinking by boric acid. When the polarizer is held at 80°C for 4 hours, the shrinkage stress in the absorption axis direction per 2 mm width is 60 N / mm 2 It is preferable that the resistance is 80N / mm or more. 2 More preferably, it is 85N / mm 2 Although there is no particular upper limit, the contraction force of the polarizer is preferably 120 N / mm 2 It may be less than or equal to 110N / mm 2 The shrinkage force of the polarizer is measured in detail by the method described in the Examples below. The boron content and shrinkage stress can be controlled by, for example, a stretching treatment or a crosslinking treatment.

[0024] The polarizer can be produced, for example, by a method including the steps of uniaxially stretching a polyvinyl alcohol-based resin film; dyeing the polyvinyl alcohol-based resin film with iodine to adsorb iodine; treating the polyvinyl alcohol-based resin film with the iodine adsorbed thereon with a crosslinking liquid such as an aqueous boric acid solution; treating the polyvinyl alcohol-based resin film with metal ions; and washing the polyvinyl alcohol-based resin film with water.

[0025] As the polyvinyl alcohol resin, a saponified polyvinyl acetate resin can be used. As the polyvinyl acetate resin, in addition to polyvinyl acetate, which is a homopolymer of vinyl acetate, copolymers of vinyl acetate with other monomers copolymerizable therewith can be mentioned. Examples of other monomers copolymerizable with vinyl acetate include unsaturated carboxylic acids, olefins, vinyl ethers, unsaturated sulfonic acids, and (meth)acrylamides having an ammonium group.

[0026] In this specification, "(meth)acrylic" means at least one selected from acrylic and methacrylic. The same applies to "(meth)acryloyl", "(meth)acrylate", etc.

[0027] The saponification degree of the polyvinyl alcohol resin is usually 85 to 100 mol%, preferably 98 mol% or more. The polyvinyl alcohol resin may be modified, and for example, polyvinyl formal or polyvinyl acetal modified with aldehydes can be used. The average polymerization degree of the polyvinyl alcohol resin is usually 1000 to 10000, preferably 1500 to 5000. The average polymerization degree of the polyvinyl alcohol resin can be determined in accordance with JIS K 6726.

[0028] Such a polyvinyl alcohol-based resin is used as a raw film for a polarizer. The method for forming the polyvinyl alcohol-based resin is not particularly limited, and a known method is used. The thickness of the polyvinyl alcohol-based raw film is not particularly limited, but it is preferable to use one having a thickness of 5 to 35 μm in order to make the thickness of the polarizer 15 μm or less. More preferably, it is 20 μm or less.

[0029] The uniaxial stretching of the polyvinyl alcohol-based resin film can be performed before, simultaneously with, or after dyeing with iodine. When the uniaxial stretching is performed after dyeing, the uniaxial stretching may be performed before or during the crosslinking treatment. The uniaxial stretching may also be performed in a plurality of these stages.

[0030] In the uniaxial stretching, the film may be stretched uniaxially between rolls having different peripheral speeds, or may be stretched uniaxially using a heated roll. The uniaxial stretching may be dry stretching in which stretching is performed in the atmosphere, or wet stretching in which stretching is performed in a state where the polyvinyl alcohol-based resin film is swollen using a solvent or water. The stretching ratio is usually 3 to 8 times.

[0031] As a method for dyeing a polyvinyl alcohol-based resin film with iodine, for example, a method of immersing the film in an aqueous solution containing iodine is adopted. Note that it is preferable that the polyvinyl alcohol-based resin film is subjected to an immersion treatment in water before the dyeing treatment.

[0032] As a crosslinking treatment after dyeing with iodine, a method of immersing the dyed polyvinyl alcohol resin film in an aqueous solution containing boric acid is usually adopted. The aqueous solution containing boric acid preferably contains potassium iodide.

[0033] The boric acid concentration of the boric acid-containing aqueous solution is preferably 1.0 to 8.0 parts by weight, more preferably 1.5 to 6.0 parts by weight, and more preferably 2.0 to 5.5 parts by weight or less, relative to 100 parts by weight of water. The potassium iodide concentration of the boric acid-containing aqueous solution is preferably 0.1 to 20 parts by weight, more preferably 1.0 to 15 parts by weight, relative to 100 parts by weight of water. Increasing the boric acid concentration makes it easier to increase the boron content.

[0034] The temperature of the boric acid-containing aqueous solution is preferably 40 to 80° C., and more preferably 60 to 70° C. Increasing the temperature facilitates the crosslinking reaction. The crosslinking treatment time is preferably 1 second to 10 minutes, and more preferably 10 seconds to 5 minutes.

[0035] The crosslinking treatment may be performed once or in multiple steps. When the crosslinking treatment is performed in multiple steps, the boric acid concentration, the potassium iodide concentration, the temperature of the boric acid-containing aqueous solution, and the crosslinking treatment time may be the same or different in each crosslinking treatment.

[0036] The metal ion treatment can be carried out by immersing the polyvinyl alcohol resin film in an aqueous solution containing a metal salt. By the metal ion treatment, various metal ions can be contained in the polyvinyl alcohol resin film. As the metal ion, in particular, from the viewpoint of color tone adjustment and durability, metal ions of transition metals such as cobalt, nickel, zinc, chromium, aluminum, copper, manganese, and iron are preferable. Among these metal ions, zinc ions are preferable from the viewpoint of color tone adjustment and heat resistance. Examples of zinc salts include zinc halides such as zinc chloride and zinc iodide, zinc sulfate, and zinc acetate.

[0037] The zinc ion concentration in the zinc salt aqueous solution is, for example, 0.1 to 10% by weight, preferably 0.5 to 7% by weight. The zinc salt solution preferably contains potassium ions such as potassium iodide and iodine ions. The potassium iodide concentration in the zinc salt solution is, for example, 0.1 to 10% by weight, preferably 0.2 to 5% by weight.

[0038] The zinc content in the polarizer is preferably 2.00% by weight or less, more preferably 1.00% by weight or less, preferably 0.03% by weight or more, and more preferably 0.05% by weight or more. When the zinc content of the polarizer is within the above range, it is easy to prevent iodine from eluting in a high-temperature and high-humidity environment. The zinc content is measured using a commercially available X-ray fluorescence analyzer. The zinc content can be controlled by metal ion treatment or the like.

[0039] The iodine content in the polarizer is preferably 3.3% by weight or less, more preferably 3.0% by weight or less, preferably 1.9% by weight or more, and more preferably 2.2% by weight or more. When the iodine content of the polarizer is within the above range, the amount of iodine that can be dissolved can be reduced while maintaining good polarization performance. The iodine content is measured using a commercially available X-ray fluorescence analyzer. The iodine content can be controlled by dyeing, crosslinking, washing, etc.

[0040] The thickness of the polarizer is preferably 20 μm or less, more preferably 15 μm or less, further preferably 10 μm or less, and particularly preferably 8 μm or less. The thickness of the polarizer is usually 2 μm or more, and preferably 3 μm or more. Reducing the thickness of the polarizer contributes to reducing the amount of iodine contained in the polarizer, so that the amount of iodine that can be dissolved can be reduced. On the other hand, by ensuring a certain degree of thickness, the transportability of the film can be improved and the polarization performance of the obtained polarizer can be ensured.

[0041] The polarizer thus obtained preferably has a luminosity-corrected single transmittance of 50% or less, more preferably 45% or less, and preferably 40% or more, and more preferably 42% or more. When the luminosity-corrected single transmittance of the polarizer is in the above range, the amount of iodine that can be dissolved can be reduced while maintaining good polarizing performance.

[0042] The polarizer thus obtained preferably has a luminosity-corrected polarization degree of 99.999% or less, more preferably 99.995% or less, preferably 99.985% or more, and more preferably 99.990% or more. When the luminosity-corrected polarization degree of the polarizer is in the above range, the amount of iodine that can be dissolved can be reduced while maintaining good polarizing performance.

[0043] The single hue of the polarizer thus obtained is preferably -0.90 or more and -0.60 or less, more preferably -0.88 or more and -0.65 or less. The b* value is 2.70 or more and 3.70 or less, more preferably 2.80 or more and 3.60 or less. When the single hue of the polarizer is blue, that is, when the b* value is small, the retardation value of the retardation film is likely to increase in a humid and hot environment, so the effect of the present invention is remarkable. The hue of the polarizer can be measured by a commercially available spectrophotometer.

[0044] (2) Protective film The circularly polarizing plate of the present invention has a protective film on at least one surface of the polarizer, and preferably has a protective film on the surface of the polarizer opposite to the retardation film side. 2 The moisture permeability of the protective film is measured by the method described below.

[0045] The protective film laminated on the polarizer can be a thermoplastic resin having light-transmitting properties (preferably optically transparent). Examples of the protective film include films made of polyolefin resins such as linear polyolefin resins (polypropylene resins, etc.) and cyclic polyolefin resins (norbornene resins, etc.); cellulose resins such as triacetyl cellulose and diacetyl cellulose; polyester resins such as polyethylene terephthalate and polybutylene terephthalate; polycarbonate resins; (meth)acrylic resins such as methyl methacrylate resins; polystyrene resins; polyvinyl chloride resins; acrylonitrile-butadiene-styrene resins; acrylonitrile-styrene resins; polyvinyl acetate resins; polyvinylidene chloride resins; polyamide resins; polyacetal resins; modified polyphenylene ether resins; polysulfone resins; polyethersulfone resins; polyarylate resins; polyamideimide resins; polyimide resins, etc.

[0046] Examples of linear polyolefin resins include linear olefin homopolymers such as polyethylene resins (polyethylene resins which are homopolymers of ethylene, and copolymers mainly composed of ethylene) and polypropylene resins (polypropylene resins which are homopolymers of propylene, and copolymers mainly composed of propylene), as well as copolymers composed of two or more types of linear olefins.

[0047] Cyclic polyolefin resin is a general term for resins polymerized with cyclic olefin as a polymerization unit, and examples thereof include resins described in JP-A-1-240517, JP-A-3-14882, JP-A-3-122137, etc. Specific examples of cyclic polyolefin resins include ring-opening (co)polymers of cyclic olefins, addition polymers of cyclic olefins, copolymers (typically random copolymers) of cyclic olefins and chain olefins such as ethylene and propylene, and graft polymers modified with unsaturated carboxylic acids or derivatives thereof, as well as hydrogenated products thereof. Among these, norbornene resins using norbornene monomers such as norbornene or polycyclic norbornene monomers as cyclic olefins are preferably used.

[0048] The polyester resin is a resin having an ester bond, excluding the cellulose ester resin described below, and is generally made of a polycondensate of a polyvalent carboxylic acid or its derivative and a polyhydric alcohol. As the polyvalent carboxylic acid or its derivative, a divalent dicarboxylic acid or its derivative can be used, for example, terephthalic acid, isophthalic acid, dimethyl terephthalate, and dimethyl naphthalenedicarboxylate. As the polyhydric alcohol, a divalent diol can be used, for example, ethylene glycol, propanediol, butanediol, neopentyl glycol, and cyclohexanedimethanol. A representative example of the polyester resin is polyethylene terephthalate, which is a polycondensate of terephthalic acid and ethylene glycol.

[0049] The (meth)acrylic resin is a resin whose main constituent monomer is a compound having a (meth)acryloyl group. Specific examples of the (meth)acrylic resin include poly(meth)acrylic acid ester such as polymethyl methacrylate; methyl methacrylate-(meth)acrylic acid copolymer; methyl methacrylate-(meth)acrylic acid ester copolymer; methyl methacrylate-acrylic acid ester-(meth)acrylic acid copolymer; methyl (meth)acrylate-styrene copolymer (MS resin, etc.); copolymers of methyl methacrylate and a compound having an alicyclic hydrocarbon group (e.g., methyl methacrylate-cyclohexyl methacrylate copolymer, methyl methacrylate-norbornyl (meth)acrylate copolymer, etc.). Preferably, poly(meth)acrylic acid C such as polymethyl (meth)acrylate is used. 1-6 A polymer containing an alkyl ester as a main component is used, and more preferably, a methyl methacrylate-based resin containing methyl methacrylate as a main component (50 to 100% by weight, preferably 70 to 100% by weight) is used.

[0050] The cellulose ester resin is an ester of cellulose and a fatty acid. Specific examples of the cellulose ester resin include cellulose triacetate, cellulose diacetate, cellulose tripropionate, and cellulose dipropionate. In addition, copolymers thereof and those in which a part of the hydroxyl group is modified with another substituent are also included. Among these, cellulose triacetate (triacetyl cellulose) is particularly preferred.

[0051] Polycarbonate resins are engineering plastics made of polymers in which monomer units are bonded via carbonate groups.

[0052] The thickness of the protective film is usually 1 to 100 μm, but from the viewpoints of strength, handleability, etc., it is preferably 5 to 60 μm, more preferably 10 to 55 μm, and even more preferably 15 to 40 μm.

[0053] The protective films attached to one or both sides of the polarizer may be made of the same or different thermoplastic resins, may have the same or different thicknesses, and may have the same or different retardation properties.

[0054] The phenomenon that the in-plane retardation value of the retardation film increases under a high-temperature and high-humidity environment as described above is believed to occur because moisture dissolves iodine contained in the polarizer, and the iodine migrates to the retardation film. Therefore, the effect of the present invention is remarkable when moisture is easily introduced into the polarizer or when iodine is easily dissolved from the polarizer under a high-temperature and high-humidity environment. Examples of such an embodiment include an embodiment in which a protective film with high moisture permeability is laminated on the opposite side of the polarizer from the retardation film side, and an embodiment in which a protective film is not laminated on the retardation film side of the polarizer.

[0055] From this perspective, the moisture permeability of the protective film provided on the opposite side of the polarizing plate from the retardation film side is 50 g / m 2 24hr or more, 100g / m 2 24hr or more, 500g / m 2 The moisture permeability of the protective film may be, for example, 1000 g / m 2 The moisture permeability is based on JIS Z 0208 and is the value measured at a temperature of 40°C and a relative humidity of 90%.

[0056] When the polarizing plate has protective films on both sides of the polarizer, the moisture permeability of one of the protective films is 50 g / m 2 24hr or more (or 100g / m 2 24hr or more, even 500g / m 2 24hr or more), the moisture permeability of the other protective film is 1000g / m 2 -24hr or less is preferable, 500g / m 2 24hr or less is more preferable, and 100g / m 2More preferably, 24 hr or less, and 50 g / m 2 It is particularly preferable that the time is 24 hours or less.

[0057] When the polarizing plate has protective films on both sides of the polarizer, the moisture permeability of the protective film placed on the opposite side of the polarizer to the retardation film side is set to 50 g / m 2 24hr or more (or 100g / m 2 24hr or more, even 500g / m 2 24 hr or more), the moisture permeability of the protective film placed on the retardation film side of the polarizer is 1000 g / m 2 -24hr or less is preferable, 500g / m 2 24hr or less is more preferable, and 100g / m 2 More preferably, 24 hr or less, and 50 g / m 2 It is particularly preferable that the time is 24 hours or less.

[0058] As described above, at least one of the protective films may have a surface treatment layer (coating layer) such as a hard coat layer, an antiglare layer, a light diffusion layer, an antireflection layer, a low refractive index layer, an antistatic layer, or an antifouling layer on its outer surface (the surface opposite to the polarizer). The thickness of the protective film includes the thickness of the surface treatment layer. These surface treatment layers can contribute to preventing moisture from penetrating into the polarizer.

[0059] The protective film can be attached to the polarizer via an adhesive layer or a pressure-sensitive adhesive layer described below. The adhesive for forming the adhesive layer is preferably a water-based adhesive or an active energy ray-curable adhesive.

[0060] When laminating the polarizer and the protective film, at least one of the laminating surfaces may be subjected to a surface activation treatment in order to enhance adhesion. Examples of the surface activation treatment include dry treatments such as corona treatment, plasma treatment, discharge treatment (glow discharge treatment, etc.), flame treatment, ozone treatment, UV ozone treatment, and ionizing active ray treatment (ultraviolet ray treatment, electron beam treatment, etc.); and wet treatments such as ultrasonic treatment using a solvent such as water or acetone, saponification treatment, and anchor coat treatment. These surface activation treatments may be performed alone or in combination of two or more.

[0061] When protective films are attached to both sides of the polarizer, the adhesives used to attach these protective films may be the same or different.

[0062] Instead of the protective film, a protective layer may be formed on at least one surface of the polarizer. The protective layer may be formed on the polarizer without an adhesive layer or a pressure-sensitive adhesive layer, that is, the protective layer may be formed in contact with the polarizer. The protective layer may be a layer containing a (meth)acrylic resin. The protective layer can prevent iodine from migrating from the polarizer. The protective layer may be a single layer or may be formed of multiple layers.

[0063] The layer containing a (meth)acrylic resin can be formed by coating a composition containing a (meth)acrylic resin on a polarizer, and then heating or irradiating with active energy rays, or by coating a composition containing a (meth)acrylic resin on a substrate film, and then heating or irradiating with active energy rays. In the latter case, a polarizer may be formed on the layer containing a (meth)acrylic resin.

[0064] The (meth)acrylic resin refers to a polymer in which a monomer having a (meth)acryloyl group is the main component among the monomers constituting the (meth)acrylic resin. Here, the main component refers to the monomer with the largest content (mass%) among the monomer components constituting the (meth)acrylic resin. By using a (meth)acrylic resin as a material for forming the protective layer, it is possible to suppress the deterioration of the optical properties of the circularly polarizing plate even in a humid and hot environment.

[0065] The (meth)acrylic resin is preferably a polymer of a photopolymerizable monomer, and may be, for example, a polymer of a monofunctional monomer or a polyfunctional monomer having a (meth)acryloyl group, either alone or in combination of two or more kinds. The (meth)acrylic resin may be a polymer of a monomer other than the monomer having a (meth)acryloyl group, for example, a monomer having a vinyl group.

[0066] The monomer having a (meth)acryloyl group is not particularly limited, but may be a compound having one or more (meth)acryloyl groups in the molecule, which may be used alone or in a mixture of two or more.Specific examples include dipentaerythritol hexa(meth)acrylate, dipentaerythritol penta(meth)acrylate, pentaerythritol tetra(meth)acrylate, ditrimethylolpropane tetra(meth)acrylate, ethylene oxide or propylene oxide added compounds of the above (meth)acrylates; oligoester(meth)acrylates having four or more (meth)acryloyl groups in the molecule, oligoether(meth)acrylates, oligourethane(meth)acrylates, oligoepoxy(meth)acrylates, oligomelamine(meth)acrylates, and polyfunctional acrylates having a dendrimer structure.

[0067] The thickness of the layer containing the (meth)acrylic resin is usually 0.1 μm or more, preferably 0.3 μm or more, more preferably 0.5 μm or more, and usually 20.0 μm or less, preferably 15 μm or less, more preferably 10 μm or less.

[0068] <Retardation film> The circular polarizing plate of the present invention has a retardation film. The retardation film has a retardation layer. The retardation layer preferably has a layer composed of a composition containing a polymerizable liquid crystal compound. The layer composed of the composition containing the polymerizable liquid crystal compound specifically means a layer in which the polymerizable liquid crystal compound is cured. In this specification, a layer that gives a retardation of λ / 2, a layer that gives a retardation of λ / 4 (positive A layer), a positive C layer, etc. may be collectively referred to as a retardation layer. Furthermore, the retardation film preferably includes an alignment film described later.

[0069] The layer that gives a retardation of λ / 2 preferably means a layer having an in-plane retardation value of 200 to 280 nm at a wavelength of 550 nm, and more preferably means a layer having an in-plane retardation value of 215 to 265 nm. The layer that gives a retardation of λ / 4 preferably means a layer having an in-plane retardation value of 100 to 160 nm at a wavelength of 550 nm, and more preferably means a layer having an in-plane retardation value of 110 to 150 nm. The positive C layer can be a layer showing a refractive index relationship of nx≒ny<nz. The retardation value in the thickness direction of the positive C layer can be -50 nm to -150 nm at a wavelength of 550 nm, and can be -70 nm to -120 nm. Here, nx is the refractive index in the direction where the in-plane refractive index is maximum (i.e., the slow axis direction), ny is the refractive index in the direction orthogonal to the slow axis in the plane (i.e., the fast axis direction), and nz is the refractive index in the thickness direction.

[0070] The retardation layer may exhibit normal wavelength dispersion or may exhibit reverse wavelength dispersion. When the retardation film has a plurality of retardation layers, each retardation layer may exhibit normal wavelength dispersion or may exhibit reverse wavelength dispersion. When the retardation film has a retardation layer exhibiting reverse wavelength dispersion, the reflection hue is likely to change when the retardation value increases in a humid and hot environment, and the visibility of the display device is likely to deteriorate. Therefore, when the retardation film has a retardation layer exhibiting reverse wavelength dispersion, the effect of the present invention is remarkable.

[0071] In the present invention, it is preferable that the layer that imparts a retardation of λ / 4 has reverse wavelength dispersion. Specifically, it is preferable that the layer that gives a retardation of λ / 4 satisfies the following formula. 0.80 <Re(450) / Re(550)<1.00 …(1) 1.00 <Re(650) / Re(550)<1.30 …(2) In the formula, Re(λ) represents an in-plane retardation value at a wavelength of λ nm.

[0072] The layer in which the polymerizable liquid crystal compound is cured is formed, for example, on an alignment film provided on a substrate. The substrate has a function of supporting the alignment film and may be a long substrate. This substrate functions as a releasable support and can support a retardation layer for transfer. Furthermore, it is preferable that the surface of the substrate has an adhesive strength sufficient to enable peeling. Examples of the substrate include the resin films exemplified as the material for the protective film.

[0073] The thickness of the substrate is not particularly limited, but is preferably in the range of 20 μm to 200 μm. When the thickness of the substrate is 20 μm or more, strength is imparted. On the other hand, when the thickness is 200 μm or less, an increase in processing waste and wear of the cutting blade can be suppressed when the substrate is cut into sheets of substrate.

[0074] The substrate may be subjected to various anti-blocking treatments. Examples of the anti-blocking treatment include an easy-adhesion treatment, a treatment for kneading a filler or the like, and an embossing (knurling) treatment. By subjecting the substrate to such an anti-blocking treatment, it is possible to effectively prevent the substrates from sticking to each other when the substrates are wound up, that is, so-called blocking, and it is possible to produce an optical film with high productivity.

[0075] The layer of the cured polymerizable liquid crystal compound is formed on the substrate via the alignment film. That is, the substrate and the alignment film are laminated in this order, and the layer of the cured polymerizable liquid crystal compound is laminated on the alignment film.

[0076] The alignment film may be a vertical alignment film, an alignment film that aligns the molecular axis of the polymerizable liquid crystal compound horizontally, or an alignment film that aligns the molecular axis of the polymerizable liquid crystal compound at an angle. The type of alignment film can be selected according to the polymerizable liquid crystal compound and the desired retardation characteristics. The alignment film is preferably one that has solvent resistance that does not dissolve the composition containing the polymerizable liquid crystal compound described later by coating, etc., and has heat resistance in the heat treatment for removing the solvent and orienting the liquid crystal compound. Examples of the alignment film include an alignment film containing an orienting polymer, a photoalignment film, and a groove alignment film that forms a concave-convex pattern or a plurality of grooves on the surface to align the liquid crystal compound.

[0077] The thickness of the alignment film is usually in the range of 10 nm to 10,000 nm, preferably in the range of 10 nm to 1,000 nm, more preferably 500 nm or less, and further preferably in the range of 10 nm to 200 nm. When the retardation film includes an alignment film and the alignment film is disposed between the polarizer and the retardation layer, the alignment film can exhibit a function of blocking migration of iodine. The thickness of the alignment film for fully exhibiting the function of blocking iodine migration is, for example, 0.3 μm or more, preferably 0.5 μm or more, more preferably 0.7 μm or more, and further preferably 1.0 μm or more.

[0078] An alignment film containing an alignment polymer is usually obtained by applying a composition in which an alignment polymer is dissolved in a solvent to a substrate, and then removing the solvent, or by applying an alignment polymer composition to a substrate, removing the solvent, and then rubbing (rubbing method). Examples of alignment polymers include polyamides and gelatins having an amide bond in the molecule, polyimides having an imide bond in the molecule, and polyamic acids, which are hydrolyzates thereof, polyvinyl alcohol, alkyl-modified polyvinyl alcohol, polyacrylamide, polyoxazole, polyethyleneimine, polystyrene, polyvinylpyrrolidone, polyacrylic acid, and polyacrylic acid esters. Among them, polyvinyl alcohol is preferred. The alignment polymers can be used alone or in combination of two or more kinds.

[0079] A photo-alignment film is usually obtained by applying a composition containing a polymer or monomer having a photoreactive group and a solvent to a substrate, removing the solvent, and then irradiating the substrate with polarized light (preferably polarized UV). Photo-alignment films are also advantageous in that the direction of the alignment control force can be arbitrarily controlled by selecting the polarization direction of the polarized light to be irradiated.

[0080] The photoreactive group refers to a group that generates liquid crystal alignment ability by irradiation with light. Specifically, it includes groups involved in photoreactions that induce molecular alignment or are the origin of liquid crystal alignment ability, such as isomerization reaction, dimerization reaction, photocrosslinking reaction, or photodecomposition reaction, caused by irradiation with light. Among them, groups involved in dimerization reaction or photocrosslinking reaction are preferred in terms of excellent alignment ability. As the photoreactive group, a group having an unsaturated bond, particularly a double bond, is preferred, and a group having at least one selected from the group consisting of a carbon-carbon double bond (C=C bond), a carbon-nitrogen double bond (C=N bond), a nitrogen-nitrogen double bond (N=N bond), and a carbon-oxygen double bond (C=O bond) is particularly preferred.

[0081] Examples of photoreactive groups having a C=C bond include vinyl groups, polyene groups, stilbene groups, stilbazolyl groups, stilbazolium groups, chalcone groups, and cinnamoyl groups. Examples of photoreactive groups having a C=N bond include groups having structures such as aromatic Schiff bases and aromatic hydrazones. Examples of photoreactive groups having an N=N bond include azobenzene groups, azonaphthalene groups, aromatic heterocyclic azo groups, bisazo groups, formazan groups, and groups having an azoxybenzene structure. Examples of photoreactive groups having a C=O bond include benzophenone groups, coumarin groups, anthraquinone groups, and maleimide groups. These groups may have substituents such as alkyl groups, alkoxy groups, aryl groups, allyloxy groups, cyano groups, alkoxycarbonyl groups, hydroxyl groups, sulfonic acid groups, and halogenated alkyl groups.

[0082] Among them, photoreactive groups involved in photodimerization are preferred, and cinnamoyl and chalcone groups are preferred because the amount of polarized light irradiation required for photoalignment is relatively small and a photoalignment film having excellent thermal stability and stability over time is easily obtained. As the polymer having a photoreactive group, one having a cinnamoyl group such that the terminal of the polymer side chain has a cinnamic acid structure is particularly preferred.

[0083] Polymerizable liquid crystal compounds can be classified into rod-shaped type (rod-shaped liquid crystal compounds) and discotic type (discotic liquid crystal compounds) based on their shape. They are further classified into low molecular type and high molecular type. Note that a polymer generally refers to a compound having a degree of polymerization of 100 or more (Polymer Physics, Phase Transition Dynamics, by Masao Doi, page 2, Iwanami Shoten, 1992). In the present invention, any type of polymerizable liquid crystal compound can be used. Two or more rod-shaped liquid crystal compounds, two or more discotic liquid crystal compounds, or a mixture of a rod-shaped liquid crystal compound and a discotic liquid crystal compound may be used.

[0084] As the rod-shaped liquid crystal compound, for example, those described in claim 1 of JP-T-11-513019 or those described in paragraphs

[0026] to

[0098] of JP-A-2005-289980 can be preferably used. As the discotic liquid crystal compound, for example, those described in paragraphs

[0020] to

[0067] of JP-A-2007-108732 or those described in paragraphs

[0013] to

[0108] of JP-A-2010-244038 can be preferably used.

[0085] Two or more kinds of polymerizable liquid crystal compounds may be used in combination. In that case, it is preferable that at least one kind has two or more polymerizable groups in the molecule. That is, it is preferable that the layer in which the polymerizable liquid crystal compound is hardened is a layer formed by fixing a liquid crystal compound having a polymerizable group by polymerization. In this case, it is no longer necessary to show liquid crystallinity after it becomes a layer.

[0086] The polymerizable liquid crystal compound has a polymerizable group capable of undergoing a polymerization reaction. The polymerizable group is preferably a functional group capable of undergoing an addition polymerization reaction, such as a polymerizable ethylenically unsaturated group or a ring-polymerizable group. More specifically, examples of the polymerizable group include a (meth)acryloyl group, a vinyl group, a styryl group, an allyl group, etc. Among these, a (meth)acryloyl group is preferable.

[0087] The layer in which the polymerizable liquid crystal compound is cured can be formed by, for example, applying a composition containing the polymerizable liquid crystal compound onto an alignment film and irradiating it with active energy rays. The composition may contain components other than the above-mentioned polymerizable liquid crystal compound. The composition preferably contains a polymerization initiator. The polymerization initiator used is selected from, for example, a thermal polymerization initiator or a photopolymerization initiator depending on the type of polymerization reaction. For example, photopolymerization initiators include α-carbonyl compounds, acyloin ethers, α-hydrocarbon-substituted aromatic acyloin compounds, polynuclear quinone compounds, and combinations of triaryl imidazole dimers and p-aminophenyl ketones. The amount of the polymerization initiator used is preferably 0.01 to 20% by mass, more preferably 0.5 to 5% by mass, based on the total solid content in the composition.

[0088] The composition may contain a polymerizable monomer from the viewpoint of uniformity and strength of the coating film. Examples of the polymerizable monomer include radically polymerizable or cationic polymerizable compounds. Among them, polyfunctional radically polymerizable monomers are preferred.

[0089] The polymerizable monomer is preferably one that can be copolymerized with the above-mentioned polymerizable liquid crystal compound. The amount of the polymerizable monomer used is preferably 1 to 50% by mass, more preferably 2 to 30% by mass, based on the total mass of the polymerizable liquid crystal compound.

[0090] The composition may contain a surfactant from the viewpoint of uniformity and strength of the coating film. Examples of the surfactant include conventionally known compounds, and among these, fluorine-based compounds are particularly preferred.

[0091] The composition may contain a solvent, and preferably contains an organic solvent. Examples of the organic solvent include amides (e.g., N,N-dimethylformamide), sulfoxides (e.g., dimethyl sulfoxide), heterocyclic compounds (e.g., pyridine), hydrocarbons (e.g., benzene, hexane), alkyl halides (e.g., chloroform, dichloromethane), esters (e.g., methyl acetate, ethyl acetate, butyl acetate), ketones (e.g., acetone, methyl ethyl ketone), and ethers (e.g., tetrahydrofuran, 1,2-dimethoxyethane). Among these, alkyl halides and ketones are preferred. The composition may contain two or more types of organic solvents.

[0092] The composition may contain various alignment agents, such as a vertical alignment promoter such as a polarizer interface side vertical alignment agent and an air interface side vertical alignment agent, and a horizontal alignment promoter such as a polarizer interface side horizontal alignment agent and an air interface side horizontal alignment agent. Furthermore, the composition may contain an adhesion improver, a plasticizer, and a polymer in addition to the above components.

[0093] The active energy rays include ultraviolet rays, visible light, electron beams, and X-rays, and are preferably ultraviolet rays. Examples of the light source of the active energy rays include a low pressure mercury lamp, a medium pressure mercury lamp, a high pressure mercury lamp, an ultra-high pressure mercury lamp, a xenon lamp, a halogen lamp, a carbon arc lamp, a tungsten lamp, a gallium lamp, an excimer laser, an LED light source emitting light in the wavelength range of 380 to 440 nm, a chemical lamp, a black light lamp, a microwave excited mercury lamp, and a metal halide lamp.

[0094] The irradiation intensity of the ultraviolet light is, for example, 100 mW / cm 2 ~3,000mW / cm 2 The ultraviolet irradiation intensity is preferably an intensity in a wavelength region effective for activating a cationic polymerization initiator or a radical polymerization initiator. The ultraviolet irradiation time is usually 0.1 seconds to 10 minutes, preferably 0.1 seconds to 5 minutes, more preferably 0.1 seconds to 3 minutes, and further preferably 0.1 seconds to 1 minute. The ultraviolet light can be irradiated once or in multiple divided times.

[0095] In this embodiment, the thickness of the retardation layer is preferably 0.5 μm or more. The thickness of the retardation layer is preferably 10 μm or less, more preferably 5 μm or less. The above upper limit and lower limit can be arbitrarily combined. When the thickness of the retardation layer is equal to or greater than the lower limit, sufficient durability can be obtained. When the thickness of the retardation layer is equal to or less than the upper limit, it can contribute to thinning of the circular polarizer. The thickness of the retardation layer can be adjusted so that the desired in-plane retardation value and thickness direction retardation value of the layer that gives a retardation of λ / 4, the layer that gives a retardation of λ / 2, or the positive C layer can be obtained.

[0096] The retardation film may include one layer of a cured polymerizable liquid crystal compound, or may include two or more layers of a cured polymerizable liquid crystal compound. When the retardation film includes two layers of a cured polymerizable liquid crystal compound, the two layers are preferably a layer that gives a retardation of λ / 4 and a positive C layer, or a layer that gives a retardation of λ / 4 and a layer that gives a retardation of λ / 2. When the retardation film includes two layers of a cured polymerizable liquid crystal compound, the retardation film may be manufactured by forming a layer of a cured polymerizable liquid crystal compound on each of the alignment films and laminating the two layers via an adhesive layer, or a layer of a cured polymerizable liquid crystal compound may be further formed on the layer of a cured polymerizable liquid crystal compound. After laminating the two layers, the substrate can be peeled off leaving the alignment film, or both the alignment film and the substrate can be peeled off.

[0097] From the viewpoint of preventing the migration of iodine, it is preferable to have an alignment film between the layer in which the polymerizable liquid crystal compound is cured and the polarizer. The alignment film can also function to prevent iodine from penetrating into the layer in which the polymerizable liquid crystal compound is cured. Therefore, when the retardation film includes one layer in which the polymerizable liquid crystal compound is cured, the retardation film is preferably configured to have an alignment film and a layer in which the polymerizable liquid crystal compound is cured, stacked in this order from the side closer to the polarizer. When the retardation film includes two layers in which the polymerizable liquid crystal compound is cured, the retardation film is preferably configured to have an alignment film, a layer in which the polymerizable liquid crystal compound is cured, an adhesive layer, a layer in which the polymerizable liquid crystal compound is cured, and an alignment film, stacked in this order from the side closer to the polarizer, and an alignment film, a layer in which the polymerizable liquid crystal compound is cured, an alignment film, and a layer in which the polymerizable liquid crystal compound is cured, stacked in this order from the side closer to the polarizer.

[0098] The thickness of the retardation film is preferably from 3 to 30 μm, and more preferably from 5 to 25 μm.

[0099] <Adhesive layer> Examples of the adhesive layer include a pressure-sensitive adhesive layer and an adhesive layer described later. The adhesive layer can be a layer for laminating a polarizer and a protective film, a polarizing plate and a retardation film, two retardation layers, or a circular polarizing plate to an image display element or a touch sensor.

[0100] From the viewpoint of preventing migration of iodine, the adhesive layer for laminating the polarizing plate and the retardation film is preferably an adhesive layer, more preferably an active energy ray curable adhesive layer. The thickness of the adhesive layer for laminating the polarizing plate and the retardation film is preferably 1.0 μm or more, more preferably 1.5 μm or more, and even more preferably 2.0 μm or more.

[0101] <Adhesive layer> The adhesive layer can be composed of an adhesive composition containing as a main component a resin such as a (meth)acrylic, rubber, urethane, ester, silicone, or polyvinyl ether resin. Among them, a pressure-sensitive adhesive composition having a (meth)acrylic resin as a base polymer, which is excellent in transparency, weather resistance, heat resistance, etc., is preferable. The pressure-sensitive adhesive composition may be of an active energy ray curing type or a heat curing type. The thickness of the pressure-sensitive adhesive layer is usually 3 to 30 μm, and preferably 3 to 25 μm.

[0102] As the (meth)acrylic resin (base polymer) used in the pressure-sensitive adhesive composition, for example, a polymer or copolymer containing one or more (meth)acrylic acid esters as monomers, such as butyl (meth)acrylate, ethyl (meth)acrylate, isooctyl (meth)acrylate, and 2-ethylhexyl (meth)acrylate, is preferably used. It is preferable to copolymerize a polar monomer into the base polymer. Examples of the polar monomer include monomers having a carboxyl group, a hydroxyl group, an amide group, an amino group, an epoxy group, and the like, such as (meth)acrylic acid, 2-hydroxypropyl (meth)acrylate, hydroxyethyl (meth)acrylate, (meth)acrylamide, N,N-dimethylaminoethyl (meth)acrylate, and glycidyl (meth)acrylate.

[0103] The adhesive composition may contain only the base polymer, but usually further contains a crosslinking agent. Examples of the crosslinking agent include divalent or higher metal ions that form a carboxylate metal salt with a carboxyl group; polyamine compounds that form an amide bond with a carboxyl group; polyepoxy compounds or polyols that form an ester bond with a carboxyl group; and polyisocyanate compounds that form an amide bond with a carboxyl group. Among them, polyisocyanate compounds are preferred.

[0104] <Adhesive layer> Examples of the aqueous adhesive include an adhesive made of an aqueous polyvinyl alcohol resin solution, an aqueous two-liquid urethane emulsion adhesive, and the like. Among them, an aqueous adhesive made of an aqueous polyvinyl alcohol resin solution is preferably used. Examples of the polyvinyl alcohol resin include a vinyl alcohol homopolymer obtained by saponifying polyvinyl acetate, which is a homopolymer of vinyl acetate, a polyvinyl alcohol copolymer obtained by saponifying a copolymer of vinyl acetate and another monomer copolymerizable therewith, and a modified polyvinyl alcohol polymer in which the hydroxyl groups of these are partially modified. The aqueous adhesive may contain a crosslinking agent such as an aldehyde compound (such as glyoxal), an epoxy compound, a melamine compound, a methylol compound, an isocyanate compound, an amine compound, or a polyvalent metal salt.

[0105] When using a water-based adhesive, it is preferable to carry out a drying step to remove water contained in the water-based adhesive after laminating the members together. After the drying step, a curing step may be carried out, for example, at a temperature of 20 to 45°C.

[0106] The active energy ray-curable adhesive is an adhesive containing a curable compound that is cured by irradiation with active energy rays such as ultraviolet rays, visible light, electron beams, and X-rays, and is preferably an ultraviolet ray-curable adhesive.

[0107] The curable compound may be a cationic polymerizable curable compound or a radical polymerizable curable compound. Examples of the cationic polymerizable curable compound include an epoxy compound (a compound having one or more epoxy groups in the molecule), an oxetane compound (a compound having one or more oxetane rings in the molecule), or a combination thereof. Examples of the radical polymerizable curable compound include a (meth)acrylic compound (a compound having one or more (meth)acryloyloxy groups in the molecule), other vinyl compounds having a radical polymerizable double bond, or a combination thereof. A cationic polymerizable curable compound and a radical polymerizable curable compound may be used in combination. The active energy ray curable adhesive usually further contains a cationic polymerization initiator and / or a radical polymerization initiator for initiating the curing reaction of the curable compound.

[0108] <Front plate> The present invention includes a circularly polarizing plate with a front plate, in which a circularly polarizing plate and a front plate are laminated via an adhesive layer. The front plate is disposed on the viewing side of the polarizing plate. The front plate can be laminated to the polarizing plate via an adhesive layer. Examples of the adhesive layer include the above-mentioned pressure-sensitive adhesive layer and adhesive layer. As shown in Figs. 2(a), (b), and (c), the front plate 4 can be laminated on the protective film 11 of the polarizing plate 1 via a pressure-sensitive adhesive layer 16.

[0109] Examples of the front plate include glass and resin film having a hard coat layer on at least one side. As the glass, for example, highly transparent glass or reinforced glass can be used. In particular, when a thin transparent surface material is used, chemically reinforced glass is preferable. The thickness of the glass can be, for example, 100 μm to 5 mm.

[0110] A front panel comprising a hard coat layer on at least one side of a resin film can have flexible properties, unlike the rigidity of existing glass. The thickness of the hard coat layer is not particularly limited, and may be, for example, 5 to 100 μm.

[0111] The resin film may be a film formed of a polymer such as a cycloolefin derivative having a unit of a monomer containing a cycloolefin such as norbornene or a polycyclic norbornene monomer, cellulose (diacetyl cellulose, triacetyl cellulose, acetyl cellulose butyrate, isobutyl ester cellulose, propionyl cellulose, butyryl cellulose, acetyl propionyl cellulose), ethylene-vinyl acetate copolymer, polycycloolefin, polyester, polystyrene, polyamide, polyetherimide, polyacrylic, polyimide, polyamideimide, polyethersulfone, polysulfone, polyethylene, polypropylene, polymethylpentene, polyvinyl chloride, polyvinylidene chloride, polyvinyl alcohol, polyvinyl acetal, polyether ketone, polyether ether ketone, polyethersulfone, polymethyl methacrylate, polyethylene terephthalate, polybutylene terephthalate, polyethylene naphthalate, polycarbonate, polyurethane, or epoxy. The resin film may be an unstretched, uniaxially or biaxially stretched film. Each of these polymers may be used alone or in a mixture of two or more. As the resin film, preferred are polyamideimide film or polyimide film having excellent transparency and heat resistance, uniaxially or biaxially stretched polyester film, cycloolefin derivative film having excellent transparency and heat resistance and capable of handling large-sized films, polymethyl methacrylate film, and triacetyl cellulose and isobutyl ester cellulose films having no transparency and no optical anisotropy. The thickness of the resin film may be 5 to 200 μm, preferably 20 to 100 μm.

[0112] The hard coat layer can be formed by curing a hard coat composition containing a reactive material that forms a crosslinked structure by irradiation with light or heat energy. The hard coat layer can be formed by curing a hard coat composition containing a photocurable (meth)acrylate monomer or oligomer and a photocurable epoxy monomer or oligomer at the same time. The photocurable (meth)acrylate monomer can include one or more selected from the group consisting of epoxy (meth)acrylate, urethane (meth)acrylate, and polyester (meth)acrylate. The epoxy (meth)acrylate can be obtained by reacting an epoxy compound with a carboxylic acid having a (meth)acryloyl group.

[0113] The hard coat composition may further include at least one selected from the group consisting of a solvent, a photoinitiator, and an additive. The additive may include at least one selected from the group consisting of inorganic nanoparticles, a leveling agent, and a stabilizer, and may further include components commonly used in the art, such as an antioxidant, a UV absorber, a surfactant, a lubricant, and an antifouling agent.

[0114] <Light blocking pattern> The light-shielding pattern may be provided as at least a part of a front panel or a bezel or a housing of a display device to which the front panel is applied. The light-shielding pattern may be formed on the display element side of the front panel. The light-shielding pattern may hide each wiring of the display device so that it is not visible to a user. The color and / or material of the light-shielding pattern is not particularly limited, and the light-shielding pattern may be formed of a resin material having various colors such as black, white, gold, etc. In one embodiment, the thickness of the light-shielding pattern may be in the range of 2 μm to 50 μm, preferably 4 μm to 30 μm, and more preferably 6 μm to 15 μm. In addition, in order to suppress the inclusion of air bubbles and the visibility of the boundary due to the step between the light-shielding pattern and the display part, a shape may be imparted to the light-shielding pattern.

[0115] <Method of manufacturing circularly polarizing plate> A method for producing a circular polarizing plate will be described using the circular polarizing plate 100 shown in Fig. 1(a) as an example. The circular polarizing plate 100 can be produced by laminating a polarizing plate 1 and a retardation film 2 with a pressure-sensitive adhesive layer 13 interposed therebetween.

[0116] The polarizing plate 1 can be manufactured by laminating the polarizer 10 and the protective films 11 and 12 with an adhesive layer interposed therebetween. The polarizing plate may be manufactured by preparing a long member, laminating the respective members by roll-to-roll and then cutting them into a predetermined shape, or by cutting the respective members into a predetermined shape and then laminating them together. After laminating the protective films 11 and 12 to the polarizer 10, a heating step or a humidity adjustment step may be performed.

[0117] The retardation film 2 can be manufactured, for example, as follows. An alignment film is formed on a substrate, and a coating liquid containing a polymerizable liquid crystal compound is applied onto the alignment film. In a state where the polymerizable liquid crystal compound is aligned, active energy rays are irradiated to harden the polymerizable liquid crystal compound. An adhesive layer 14 formed on a release film is laminated on the layer of hardened polymerizable liquid crystal compound. Next, the substrate and / or the alignment film is peeled off. Next, an adhesive layer 13 formed on a release film is laminated on a protective film 12. The retardation film 2 may be manufactured by preparing long members, laminating the respective members by roll-to-roll and then cutting them into a predetermined shape, or by laminating the respective members after cutting them into a predetermined shape.

[0118] Then, the release film laminated on the adhesive layer 13 is peeled off, and the retardation film 2 and the polarizing plate 1 are attached to each other via the adhesive layer 13, whereby the circularly polarizing plate 100 can be produced.

[0119] <Application> Circularly polarizing plates can be used in various display devices. A display device is a device having a display element, and includes a light-emitting element or a light-emitting device as a light source. Examples of display devices include liquid crystal display devices, organic EL display devices, inorganic electroluminescence (hereinafter also referred to as inorganic EL) display devices, electron emission display devices (e.g., field emission display devices (FEDs) and surface field emission display devices (SEDs)), electronic paper (display devices using electronic ink or electrophoretic elements, plasma display devices, projection display devices (e.g., grating light valve (GLV) display devices, display devices having digital micromirror devices (DMDs)), and piezoelectric ceramic displays. Liquid crystal display devices include both transmissive liquid crystal display devices and semi-transmissive liquid crystal display devices. These display devices may be display devices that display two-dimensional images, or stereoscopic display devices that display three-dimensional images. Circularly polarizing plates can be used particularly effectively in organic EL display devices or inorganic EL display devices.

[0120] The display device of the present invention includes the circular polarizing plate of the present invention and a display element. An example of the display device of the present invention is shown in Fig. 2. In Fig. 2(a), (b), and (c), organic EL display devices 104, 105, and 106 have a layer structure in which a circular polarizing plate is laminated on an organic EL display element 3 via an adhesive layer 14 laminated on a retardation film 20. EXAMPLES

[0121] [Boron content] 0.2 g of the polarizer was dissolved in 200 g of a 1.9 wt % mannitol aqueous solution. The resulting aqueous solution was titrated with a 1 mol / L sodium hydroxide aqueous solution, and the boron content of the polarizer was calculated by comparing the amount of sodium hydroxide solution required for neutralization with a calibration curve.

[0122] [Phase difference value] The retardation values ​​of the circularly polarizing plate and the retardation film were measured using a retardation measuring device (KOBRA-WPR manufactured by Oji Scientific Instruments Co., Ltd.).

[0123] [Hue evaluation] When measuring the reflected hue, a MIRO (5011GP) manufactured by ALANOD was used as the reflector. This reflector is a specular reflector having a reflecting surface formed by vapor deposition.

[0124] The evaluation sample was placed on the reflector. The reflection hue (a*, b*) was measured using a spectrophotometer (CM-2600d manufactured by Konica Minolta, Inc.). The reflection hue was a value when the light source was D65, and was measured by the SCI method (including regular reflection light).

[0125] [Luminous sensitivity corrected single transmittance, luminous sensitivity corrected polarization, single hue] The luminosity-corrected single transmittance, luminosity-corrected polarization degree, and single hue were calculated by performing luminosity correction using a 2-degree visual field (C light source) according to JIS Z 8701 on the transmittance and polarization degree obtained using an absorptiometer with an integrating sphere (V7100 manufactured by JASCO Corporation).

[0126] [Measurement of moisture permeability] The moisture permeability (water vapor transmission rate) of the protective film is measured under conditions of 40°C and 90% RH based on the method described in JIS Z 0208, and is measured at 1m 2 Moisture permeability per day (24 hours) (g / m 2 24hr).

[0127] [Shrinkage stress] A measurement sample with a width of 2 mm and a length of 10 mm, with the absorption axis direction as the long side, was cut out from the protective film of the polarizing plate. This sample was set in a thermomechanical analyzer (EXSTAR-6000 manufactured by SII Nano Technology Inc.) and the shrinkage stress in the absorption axis direction (long side direction) that occurred when the sample was kept at 80°C for 4 hours while keeping the dimensions constant was measured.

[0128] [Example 1] [Production Example 1: Preparation of a laminate including a retardation layer 1] Five parts of a photoalignment material (weight average molecular weight: 30,000) having the following structure was mixed with 95 parts of cyclopentanone, and the resulting mixture was stirred at 80° C. for 1 hour to obtain a composition for forming a horizontal alignment film. TIFF2024144518000001.tif2676

[0129] To 100 parts of a mixture of polymerizable liquid crystal compound A and polymerizable liquid crystal compound B shown below in a mass ratio of 90:10, 1.0 part of a leveling agent (F-556; manufactured by DIC Corporation) and 6 parts of a polymerization initiator, 2-dimethylamino-2-benzyl-1-(4-morpholinophenyl)butan-1-one ("Irgacure 369 (Irg369)", manufactured by BASF Japan Ltd.) were added.

[0130] Furthermore, N-methyl-2-pyrrolidone (NMP) was added so that the solid content concentration became 13%, and the mixture was stirred at 80° C. for 1 hour to obtain a retardation layer forming composition (1).

[0131] Polymerizable liquid crystal compound A was produced by the method described in JP-A-2010-31223. The polymerizable liquid crystal compound B was produced according to the method described in JP-A-2009-173893. The molecular structures of each compound are shown below.

[0132] (Polymerizable liquid crystal compound A) TIFF2024144518000002.tif47168

[0133] (Polymerizable liquid crystal compound B) TIFF2024144518000003.tif17138

[0134] A substrate film made of a cycloolefin polymer (COP) film (ZF-14, 23 μm thick, manufactured by Zeon Corporation) was subjected to a corona treatment once at an output of 0.3 kW and a treatment speed of 3 m / min using a corona treatment device (AGF-B10, manufactured by Kasuga Electric Co., Ltd.) The composition for forming a horizontal alignment film was applied to the surface of the substrate that had been subjected to the corona treatment using a bar coater. The coating film was dried at 80°C for 1 minute and then irradiated with a polarized UV irradiator (SPOT CURE SP-7; manufactured by Ushio Inc.) at 100 mJ / cm 2 The thickness of the obtained horizontal alignment film was measured with a laser microscope (LEXT, manufactured by Olympus Corporation) and found to be 100 nm.

[0135] Next, in an environment of room temperature 25°C and humidity 30% RH, the retardation layer forming composition (1) was passed through a PTFE membrane filter (manufactured by Advantec Toyo Co., Ltd., product number: T300A025A) with a pore size of 0.2 μm, and applied using a bar coater onto a substrate film with an alignment film kept at 25°C. The coating film was dried at 120°C for 1 minute, and then irradiated with ultraviolet light (under a nitrogen atmosphere, wavelength: 365 nm, accumulated light amount at wavelength 365 nm: 1000 mJ / cm2) using a high-pressure mercury lamp (Uniquer VB-15201BY-A, manufactured by Ushio Inc.). 2 The thickness of the resulting coating film was measured with a laser microscope (LEXT, manufactured by Olympus Corporation) and found to be 2 μm.

[0136] In this way, a laminate was obtained in which a layer of the cured polymerizable liquid crystal compound (retardation layer 1), a horizontal alignment film, and a substrate film were laminated in this order. The retardation layer 1 was a retardation layer exhibiting a retardation value of λ / 4. The retardation layer 1 exhibited reverse wavelength dispersion.

[0137] [Production Example 2: Preparation of a laminate including a retardation layer 2] As a composition for forming a vertical alignment film, a mixture of 2-phenoxyethyl acrylate, tetrahydrofurfuryl acrylate, dipentaerythritol triacrylate, and bis(2-vinyloxyethyl) ether in a ratio of 1:1:4:5, to which LUCIRIN TPO was added as a polymerization initiator in a ratio of 4% was used.

[0138] The retardation layer forming composition (2) was prepared by mixing a photopolymerizable nematic liquid crystal compound (RMM28B, manufactured by Merck) and a solvent so that the solid content was 1 to 1.5 g. The solvent used was a mixed solvent obtained by mixing methyl ethyl ketone (MEK), methyl isobutyl ketone (MIBK), and cyclohexanone (CHN) in a mass ratio (MEK:MIBK:CHN) of 35:30:35.

[0139] A polyethylene terephthalate (PET) film having a thickness of 38 μm was prepared as a substrate film. A composition for forming a vertical alignment film was applied to one side of the substrate film to a thickness of 3 μm at a dose of 200 mJ / cm 2 A vertical alignment film was formed by irradiating the liquid crystal layer with ultraviolet light of 1000 nm.

[0140] On the vertical alignment layer, the retardation layer forming composition (2) was applied by die coating. The coating amount was 4 to 5 g (wet). The coating was dried at a drying temperature of 75° C. for 120 seconds. The coating was then irradiated with ultraviolet (UV) rays to polymerize the polymerizable liquid crystal compound.

[0141] In this way, a laminate was obtained in which a layer of the cured polymerizable liquid crystal compound (retardation layer 2), a vertical alignment film, and a base film were laminated in this order. The retardation layer 2 was a positive C plate. The total thickness of the retardation layer 2 and the alignment film was 4 μm.

[0142] [Production Example 3: Preparation of a laminate of retardation layers] The laminate including the retardation layer 1 and the laminate including the retardation layer 2 were bonded together with an ultraviolet-curing adhesive so that the retardation layer surfaces (surfaces opposite to the surface on the substrate film side) of the two layers were bonded together. Then, the ultraviolet-curing adhesive was cured by irradiating ultraviolet light. In this way, a retardation layer laminate including two retardation layers, the retardation layer 1 and the retardation layer 2, was produced.

[0143] [Production Example 4: Preparation of polarizer] A polyvinyl alcohol film having a thickness of 20 μm, a degree of polymerization of 2,400, and a degree of saponification of 99.9% or more was uniaxially stretched to a stretching ratio of 4.5 times in a dry state, and while maintaining the tension, it was immersed for 60 seconds at 28°C in a dye bath containing 0.05 parts by weight of iodine and 5 parts by weight of potassium iodide per 100 parts by weight of water.

[0144] Next, the film was immersed in a boric acid aqueous solution 1 containing 5.5 parts by weight of boric acid and 15 parts by weight of potassium iodide per 100 parts by weight of water at 64° C. for 110 seconds. Next, the film was immersed in a boric acid aqueous solution 2 containing 5.5 parts by weight of boric acid and 15 parts by weight of potassium iodide per 100 parts by weight of water at 67° C. for 30 seconds. Thereafter, the film was washed with pure water at 3° C. and dried to obtain a polarizer.

[0145] The luminosity-corrected single transmittance of the obtained polarizer was 42.15%, and the luminosity-corrected polarization degree was 99.995%. The single hue a* of the polarizer was -0.88, and the single hue b* was 3.69. The contraction stress of the polarizer was 99.9 N / mm 2 It was.

[0146] [Production Example 5: Preparation of polarizing plate] A saponified triacetyl cellulose (TAC) film 1 (KC2UATAC, manufactured by Konica Minolta, Inc., thickness 25 μm) was bonded to one surface of the obtained polarizer by nip rolls via a water-based adhesive. A saponified triacetyl cellulose (TAC) film 2 (ZRG20SL, manufactured by Fujifilm Corporation, thickness 20 μm) was bonded to the other surface of the polarizer in the same manner as the TAC film 1. The obtained laminate was dried at 60° C. for 2 minutes while maintaining the tension of 430 N / m to obtain a polarizing plate having a TAC film on both sides of the polarizer. The water-based adhesive was prepared by adding 3 parts of carboxyl-modified polyvinyl alcohol (Kuraray Poval KL318, manufactured by Kuraray Co., Ltd.) and 1.5 parts of water-soluble polyamide epoxy resin (Sumirez Resin 650, manufactured by Taoka Chemical Co., Ltd., aqueous solution with a solid content concentration of 30%) to 100 parts of water. The moisture permeability of the TAC film 1 was 1200 g / m 2 The moisture permeability of TAC film 2 was 1500 g / m2 -It was 24 hours.

[0147] An acrylic adhesive layer was laminated on the two surfaces of the TAC film of the polarizing plate. The base film used to form the retardation layer 1 was peeled off from the retardation layer laminate produced in Production Example 3. The exposed horizontal alignment film and the acrylic adhesive layer were attached to each other. The angle between the absorption axis of the polarizer and the slow axis of the retardation layer 1 was 45°. Next, the base film used to form the retardation layer 2 was peeled off, and an acrylic adhesive layer was laminated on the exposed vertical alignment film.

[0148] In this way, a circularly polarizing plate having a polarizing plate and a retardation film laminated thereon was obtained. The circularly polarizing plate had a layer structure in which a TAC film 1, a polarizer, a TAC film 2, an adhesive layer, a horizontal alignment film, a retardation layer 1, an adhesive layer, a retardation layer 2, a vertical alignment film, and an adhesive layer were laminated in this order.

[0149] [Example 2] A circularly polarizing plate was produced in the same manner as in Example 1, except that the TAC film 1 was attached to only one side of the polarizer. The circularly polarizing plate had a layer structure in which the TAC film 1, a polarizer, a pressure-sensitive adhesive layer, a horizontal alignment film, a retardation layer 1, an adhesive layer, a retardation layer 2, a vertical alignment film, and a pressure-sensitive adhesive layer were laminated in this order.

[0150] [Example 3] A circularly polarizing plate was produced in the same manner as in Example 2, except that the content of boric acid in the boric acid aqueous solution 2 was changed to 2.3 parts by weight when producing the polarizer. The shrinkage stress of the polarizer was 88.2 N / mm 2 The luminosity-corrected single transmittance of the obtained polarizer was 42.85%, and the luminosity-corrected polarization degree was 99.985%. The single hue a* of the polarizer was -0.69, and the single hue b* was 2.81.

[0151] [Example 4] A circularly polarizing plate was produced in the same manner as in Example 2, except that the content of boric acid in the boric acid aqueous solution 2 was changed to 1.8 parts by weight when producing the polarizer. The shrinkage stress of the polarizer was 80.2 N / mm 2The luminosity-corrected single transmittance of the obtained polarizer was 42.56%, and the luminosity-corrected polarization degree was 99.993%. The single hue a* of the polarizer was -0.81, and the single hue b* was 3.17.

[0152] [Example 5] A circularly polarizing plate was produced in the same manner as in Example 2, except that the content of boric acid in the boric acid aqueous solution 2 was changed to 1.1 parts by weight when producing the polarizer. The shrinkage stress of the polarizer was 63.2 N / mm 2 The luminosity-corrected single transmittance of the obtained polarizer was 42.30%, and the luminosity-corrected polarization degree was 99.994%. The single hue a* of the polarizer was -0.90, and the single hue b* was 3.25.

[0153] [Example 6] A polarizing plate was produced in the same manner as in Example 4. An acrylic pressure-sensitive adhesive layer was laminated on the surface of the polarizer of the polarizing plate. The retardation layer 1 and the acrylic pressure-sensitive adhesive layer were attached to each other in the laminate including the retardation layer 1 produced in Production Example 1. The angle between the absorption axis of the polarizer and the slow axis of the retardation layer 1 was 45°. After lamination, the base film used to form the retardation layer 1 was peeled off. The exposed horizontal alignment film and the retardation layer 2 produced in Production Example 2 were laminated with an ultraviolet-curable adhesive. Next, the ultraviolet-curable adhesive was cured by irradiating ultraviolet rays. Next, the base film used to form the retardation layer 2 was peeled off, and an acrylic adhesive layer was laminated on the exposed vertical alignment film. In this way, a circularly polarizing plate having a polarizing plate and a retardation film laminated thereon was obtained. The circularly polarizing plate had a layer structure in which a TAC film 1, a polarizer, a pressure-sensitive adhesive layer, a retardation layer 1, a horizontal alignment film, an adhesive layer, a retardation layer 2, a vertical alignment film, and a pressure-sensitive adhesive layer were laminated in this order.

[0154] [Example 7] The cumulative amount of ultraviolet light irradiated when hardening the polymerizable liquid crystal compound is 1500 mJ / cm 2 A laminate including a retardation layer was produced in the same manner as in Production Example 1, except that the above-mentioned conditions were met. A circularly polarizing plate was produced in the same manner as in Example 3, except that the retardation layer 1 was changed to the above retardation layer.

[0155] [Example 8] The cumulative amount of ultraviolet light irradiated when hardening the polymerizable liquid crystal compound is 700 mJ / cm 2 A laminate including a retardation layer was produced in the same manner as in Production Example 1, except that the above-mentioned conditions were met. A circularly polarizing plate was produced in the same manner as in Example 3, except that the retardation layer 1 was changed to the above retardation layer.

[0156] [Comparative Example 1] A circularly polarizing plate was produced in the same manner as in Example 2, except that the content of boric acid in the boric acid aqueous solution 2 was changed to 0.7 parts by weight when the polarizer was produced. The shrinkage stress of the polarizer is 26.2N / mm 2 The luminosity-corrected single transmittance of the obtained polarizer was 42.35%, and the luminosity-corrected polarization degree was 99.994%. The single hue a* of the polarizer was -1.00, and the single hue b* was 3.35.

[0157] The circularly polarizing plates prepared in the examples and comparative examples were cut into pieces of 150 mm x 50 mm using a super cutter, and were attached to a glass plate via an acrylic adhesive layer. The circularly polarizing plate attached to the glass was placed in an oven at a temperature of 85°C and a relative humidity of 85% RH for 24 hours. The change in retardation value and the change in reflection hue before and after placing in the oven are shown in Table 1.

[0158] [Table 1] [Industrial Applicability]

[0159] The present invention is useful because it can provide a circularly polarizing plate in which the retardation value of the retardation film is unlikely to increase even when placed in a high-temperature and high-humidity environment. [Explanation of symbols]

[0160] 1 Polarizing plate 2 Phase contrast film 3. Organic EL display element 4 Front plate 10 Polarizer 11,12 Protective film 13, 14, 16 Adhesive layer 15 Adhesive layer 20,21 Layer of hardened polymerizable liquid crystal compound 100,101,103 Circular polarizing plate 104,105,106 Organic EL display device

Claims

1. A circular polarizing plate having a polarizing plate and a retardation film, The polarizing plate includes a polarizer and a protective film attached to at least one surface of the polarizer, the polarizer is a polyvinyl alcohol-based resin film having iodine adsorbed thereon and oriented therein; The boron content of the polarizer is 2.76% by weight or more and 10.00% by weight or less, The moisture permeability of the protective film is 50 g / m 2 - 24 hours or more, The retardation film includes a retardation layer formed of a layer of a cured polymerizable liquid crystal compound, and an alignment film, the alignment film is disposed on the polarizer side of the retardation film, The alignment film is a circular polarizing plate made of a polymer having a cinnamoyl group.

2. 2. The circularly polarizing plate according to claim 1, wherein the polarizer has a thickness of 20 μm or less.

3. 3. The circularly polarizing plate according to claim 1, wherein the polarizer has a luminosity-corrected single transmittance of 40% or more.

4. When the polarizer was held at 80° C. for 4 hours, the shrinkage stress in the absorption axis direction per 2 mm width was 60 N / mm 2 The circularly polarizing plate according to any one of claims 1 to 3, wherein the circularly polarizing plate is a circularly polarizing plate having the above structure.

5. 5. The circularly polarizing plate according to claim 1, wherein the polarizer has a single hue having an a* value of -0.90 or more and -0.60 or less and a b* value of 2.70 or more and 3.70 or less.

6. 6. The circularly polarizing plate according to claim 1, wherein the polarizing plate and the retardation film are attached to each other with an active energy ray-curable adhesive.

7. The polarizing plate includes a protective film on both sides of a polarizer, The moisture permeability of one protective film is 500 g / m 2 - 24 hours or more, The moisture permeability of the other protective film is 100 g / m 2 The circularly polarizing plate according to any one of claims 1 to 6, which has a shelf life of 24 hours or less.

8. The polarizing plate has a moisture permeability of 50 g / m on the side opposite to the retardation layer of the polarizer. 2 The circularly polarizing plate according to any one of claims 1 to 6, which has a protective film having a durability of 24 hours or more, and has no protective film on the retardation layer side of the polarizer.

9. The circularly polarizing plate according to any one of claims 1 to 8, further comprising a front panel, a light-shielding pattern, and a touch sensor.

10. A display device comprising the circular polarizer according to any one of claims 1 to 9 and a display element.

Citation Information

Patent Citations

  • Manufacturing method for polarizing film, polarizing plate and display device

    JP2001141926A

  • Polarizing plate, circularly polarizing plate, and elliptically polarizing plate

    JP2004272202A

  • Polarizing plate

    JP2005049698A

  • Manufacturing method for polarizing plate, polarizing plate and picture display device using the polarizing plate

    JP2005309394A

  • Polarizer plate, optical compensation film incorporating polarizer plate, liquid crystal display and light emitting display device

    JP2005338736A