In-vehicle reflection control film

The in-vehicle reflection control film optimizes specular and diffuse light control to enhance visibility and identifiability of external light images, addressing the inadequacies of existing technologies in managing reflected light in in-vehicle display devices.

JP2024144532AActive Publication Date: 2024-10-11TOPPAN TOMOEGAWA OPTICAL FILM CO LTD
View PDF 4 Cites 0 Cited by

Patent Information

Application Number
JP2024117917
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Priority Date
2021-05-14
Filing Date
2024-07-23
Publication Date
2024-10-11
Estimated Expiration
2042-05-13

AI Technical Summary

Technical Problem

Existing in-vehicle display devices suffer from inadequate control of reflected light, which affects visibility and the ability to utilize external light images as information about the vehicle's surroundings.

Method used

An in-vehicle reflection control film comprising a base material with a reflection control layer that includes an anti-glare layer and a low-refractive index layer, optimized to control specularly reflected light and diffuse light appropriately, with specific optical properties to enhance visibility and identifiability of external light images.

Benefits of technology

The film effectively suppresses glare and ensures clear, distinguishable visibility of both displayed and reflected images, allowing the external light images to be recognized as useful information for the driver.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024144532000001_ABST
    Figure 2024144532000001_ABST
Patent Text Reader

Abstract

To provide an in-vehicle reflection control film having an optical characteristic suited for in-vehicle use.SOLUTION: An in-vehicle reflection control film 10 includes a base material 1 and a reflection control layer 5 stacked on the base material 1. When a light amount of specularly reflected light of light incident from an oblique direction of 30° with respect to a normal line of the base material 1 on the base material 1 on which the reflection control layer 5 is not stacked, is defined as 100%, a light amount of specularly reflected light of light incident from an oblique direction of 30° with respect to the normal line of the reflection control film 10 on the reflection control layer 5 of the in-vehicle reflection control film 10 is 0 to 20.61%, a light amount of reflected light in a direction of a reflection angle ±5° of the specularly reflected light is 0.3 to 2.0%, and haze is 3 to 11%.SELECTED DRAWING: Figure 1
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to an in-vehicle reflection control film for use in an in-vehicle display device or the like. [Background technology]

[0002] Conventionally, center information displays and center console displays have been used as in-vehicle display devices installed in vehicles for car navigation systems, etc. In recent years, the number of in-vehicle display devices has been increasing, and new uses of in-vehicle display devices such as digital outer monitors, digital inner monitors, and digital meter clusters are expected. Since light enters the interior of a vehicle from various directions through the windows, the visibility of the in-vehicle display device can be ensured by providing the in-vehicle display device with an optical film having an anti-reflection function.

[0003] For example, Patent Document 1 describes an antireflection film that is configured by laminating a plurality of layers on an optical substrate and has a reflectance of 0.1% or less for light incident at an angle of 45 degrees in a wavelength range of 300 to 660 nm. Patent Document 2 describes an optical sheet in which translucent inorganic particles and / or translucent organic particles are dispersed on at least one surface of a transparent substrate. [Prior art documents] [Patent documents]

[0004] [Patent Document 1] JP 2001-74903 A [Patent Document 2] Patent No. 5725216 Summary of the Invention [Problem to be solved by the invention]

[0005] In addition to the display image, the display surface of an in-vehicle display device may also reflect images of lights from nearby vehicles, street lamps, etc. Until now, it has been common to suppress reflections on the display surface in order to ensure the visibility of the display image, but adequate consideration has not been given to suitable control of reflected light in in-vehicle display devices, and there is also room for improvement in the optical properties required for optical films used in in-vehicle display devices.

[0006] Therefore, an object of the present invention is to provide an in-vehicle reflection control film having optical properties suitable for in-vehicle use. [Means for solving the problem]

[0007] The reflection control film for vehicle mounting according to the present invention is a reflection control film for vehicle mounting comprising a substrate and a reflection control layer laminated on the substrate, the reflection control layer comprising an antiglare layer laminated on the substrate and a low refractive index layer laminated on the antiglare layer without any other layer therebetween, characterized in that when the amount of specularly reflected light of light incident on a substrate not laminated with a reflection control layer from a direction at an oblique angle of 30° to the normal to the substrate is taken as 100%, the amount of specularly reflected light of light incident on the reflection control layer of the reflection control film for vehicle mounting from a direction at an oblique angle of 30° to the normal to the reflection control film is 0 to 20.61%, the amount of reflected light in a direction at a reflection angle of ±5° of the specularly reflected light is 0.3 to 2.0%, and the haze is 3 to 11%. Effect of the Invention

[0008] According to the present invention, it is possible to provide an in-vehicle reflection control film having optical properties suitable for in-vehicle use. [Brief description of the drawings]

[0009] [Figure 1] FIG. 1 is a cross-sectional view showing the configuration of an in-vehicle reflection control film according to an embodiment. [Diagram 2] FIG. 2 is a diagram for explaining the direction of light reflection. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0010] FIG. 1 is a cross-sectional view showing the configuration of an in-vehicle reflection control film according to an embodiment.

[0011] The reflection control film 10 for mounting in a vehicle according to this embodiment (hereinafter simply referred to as “reflection control film”) includes a substrate 1 and a reflection control layer 5 laminated on one surface of the substrate 1.

[0012] The substrate 1 is a film that serves as the base of the reflection control film 10, and is made of a material that is excellent in the transparency of visible light. Materials that can be used to form the substrate 1 include polyolefins such as polyethylene and polypropylene, polyesters such as polyethylene terephthalate, polybutylene terephthalate, and polyethylene naphthalate, polyacrylates such as polymethyl methacrylate, polyamides such as nylon 6 and nylon 66, polyimides, polyarylates, polycarbonates, triacetyl cellulose, polyacrylates, polyvinyl alcohol, polyvinyl chloride, cycloolefin copolymers, norbornene-containing resins, transparent resins such as polyethersulfone and polysulfone, and inorganic glass. Among these, a film made of polyethylene terephthalate can be preferably used. The thickness of the substrate 1 is not particularly limited, but is preferably 10 to 200 μm.

[0013] The surface of the substrate 1 may be subjected to a surface modification treatment in order to improve adhesion to the reflection control layer 5. Examples of the surface modification treatment include an alkali treatment, a corona treatment, a plasma treatment, a sputtering treatment, application of a surfactant or a silane coupling agent, and Si vapor deposition.

[0014] In this embodiment, the reflection control layer 5 includes an antiglare layer 2 and a low reflection layer 3 in this order from the substrate 1 side.

[0015] The antiglare layer 2 is an optically functional layer having fine irregularities on its surface, which scatters external light with the irregularities to reduce glare from the external light. The antiglare layer 2 is formed by applying a coating liquid containing a binder resin and organic and / or inorganic fine particles to the substrate 1 and curing the coating film.

[0016] As the binder resin, an active energy ray curable resin that is cured by irradiation with ionizing radiation or ultraviolet light can be used, for example, a monofunctional, difunctional, trifunctional or higher functional (meth)acrylate monomer can be used. In this specification, "(meth)acrylate" is a general term for both acrylate and methacrylate, and "(meth)acryloyl" is a general term for both acryloyl and methacryloyl.

[0017] Examples of monofunctional (meth)acrylate compounds include 2-hydroxyethyl (meth)acrylate, 2-hydroxypropyl (meth)acrylate, 2-hydroxybutyl (meth)acrylate, n-butyl (meth)acrylate, isobutyl (meth)acrylate, t-butyl (meth)acrylate, glycidyl (meth)acrylate, acryloylmorpholine, N-vinylpyrrolidone, tetrahydrofurfuryl acrylate, cyclohexyl (meth)acrylate, 2-ethylhexyl (meth)acrylate, and isobornyl (meth)acrylate. acrylate, isodecyl (meth)acrylate, lauryl (meth)acrylate, tridecyl (meth)acrylate, cetyl (meth)acrylate, stearyl (meth)acrylate, benzyl (meth)acrylate, 2-ethoxyethyl (meth)acrylate, 3-methoxybutyl (meth)acrylate, ethyl carbitol (meth)acrylate, phosphate (meth)acrylate, ethylene oxide modified phosphate (meth)acrylate, phenoxy (meth)acrylate, ethylene oxide modified phenoxy (meth)acrylate, propylene oxide ethylene oxide modified phenoxy (meth)acrylate, nonylphenol (meth)acrylate, ethylene oxide modified nonylphenol (meth)acrylate, propylene oxide modified nonylphenol (meth)acrylate, methoxydiethylene glycol (meth)acrylate, methoxypolyethylene glycol (meth)acrylate, methoxypropylene glycol (meth)acrylate, 2-(meth)acryloyloxyethyl-2-hydroxypropyl phthalate, 2-hydroxy-3-phenoxypropyl (meth)acrylate, 2-(meth)acryloyloxyethyl-2-hydroxypropyl phthalate, ) acryloyloxyethyl hydrogen phthalate, 2-(meth)acryloyloxypropyl hydrogen phthalate, 2-(meth)acryloyloxypropyl hexahydrohydrogen phthalate, 2-(meth)acryloyloxypropyl tetrahydrohydrogen phthalate, dimethylaminoethyl (meth)acrylate, trifluoroethyl (meth)acrylate, tetrafluoropropyl (meth)acrylate, hexafluoropropyl (meth)acrylate, octafluoropropyl (meth)acrylate, 2-adamantane,Examples of the mono(meth)acrylate include adamantane derivative mono(meth)acrylates such as adamantyl acrylate having a monovalent mono(meth)acrylate derived from an adamantanediol.

[0018] Examples of bifunctional (meth)acrylate compounds include di(meth)acrylates such as ethylene glycol di(meth)acrylate, diethylene glycol di(meth)acrylate, butanediol di(meth)acrylate, hexanediol di(meth)acrylate, nonanediol di(meth)acrylate, ethoxylated hexanediol di(meth)acrylate, propoxylated hexanediol di(meth)acrylate, diethylene glycol di(meth)acrylate, polyethylene glycol di(meth)acrylate, tripropylene glycol di(meth)acrylate, polypropylene glycol di(meth)acrylate, neopentyl glycol di(meth)acrylate, ethoxylated neopentyl glycol di(meth)acrylate, tripropylene glycol di(meth)acrylate, and hydroxypivalic acid neopentyl glycol di(meth)acrylate.

[0019] Examples of trifunctional or higher (meth)acrylate compounds include tri(meth)acrylates such as trimethylolpropane tri(meth)acrylate, ethoxylated trimethylolpropane tri(meth)acrylate, propoxylated trimethylolpropane tri(meth)acrylate, tris(2-hydroxyethyl)isocyanurate tri(meth)acrylate, and glycerin tri(meth)acrylate, as well as trifunctional (meth)acrylate compounds such as pentaerythritol tri(meth)acrylate, dipentaerythritol tri(meth)acrylate, and ditrimethylolpropane tri(meth)acrylate. and polyfunctional (meth)acrylate compounds having three or more functional groups such as pentaerythritol tetra(meth)acrylate, ditrimethylolpropane tetra(meth)acrylate, dipentaerythritol tetra(meth)acrylate, dipentaerythritol penta(meth)acrylate, ditrimethylolpropane penta(meth)acrylate, dipentaerythritol hexa(meth)acrylate, and ditrimethylolpropane hexa(meth)acrylate, as well as polyfunctional (meth)acrylate compounds in which a portion of these (meth)acrylates is substituted with an alkyl group or ε-caprolactone.

[0020] In addition, urethane (meth)acrylate can also be used as the active energy ray curable resin. Examples of the urethane (meth)acrylate include those obtained by reacting a polyester polyol with an isocyanate monomer or a prepolymer, and then reacting the resulting product with a (meth)acrylate monomer having a hydroxyl group.

[0021] Examples of urethane (meth)acrylates include pentaerythritol triacrylate hexamethylene diisocyanate urethane prepolymer, dipentaerythritol pentaacrylate hexamethylene diisocyanate urethane prepolymer, pentaerythritol triacrylate toluene diisocyanate urethane prepolymer, dipentaerythritol pentaacrylate toluene diisocyanate urethane prepolymer, pentaerythritol triacrylate isophorone diisocyanate urethane prepolymer, dipentaerythritol pentaacrylate isophorone diisocyanate urethane prepolymer, and the like.

[0022] The above-mentioned active energy ray curable resin may be used alone or in combination of two or more. In addition, the above-mentioned active energy ray curable resin may be a monomer in the coating liquid or a partially polymerized oligomer.

[0023] In addition, as the active energy ray curable resin, in addition to the above-mentioned compounds having radical polymerizable functional groups, monomers, oligomers, and prepolymers having cationic polymerizable functional groups such as epoxy groups, vinyl ether groups, and oxetane groups can be used alone or in combination. Examples of the monomer include unsaturated polyesters, epoxy acrylates, epoxy compounds such as tetramethylene glycol diglycidyl ether, propylene glycol diglycidyl ether, neopentyl glycol diglycidyl ether, bisphenol A diglycidyl ether, and various alicyclic epoxies, and oxetane compounds such as 3-ethyl-3-hydroxymethyloxetane, 1,4-bis{[(3-ethyl-3-oxetanyl)methoxy]methyl}benzene, and di[1-ethyl(3-oxetanyl)]methyl ether.

[0024] The above-mentioned resin material can be cured by irradiation with ultraviolet light, provided that a photopolymerization initiator is added. As the photopolymerization initiator, radical polymerization initiators such as acetophenone, benzophenone, thioxanthone, benzoin, and benzoin methyl ether, and cationic polymerization initiators such as aromatic diazonium salts, aromatic sulfonium salts, aromatic iodonium salts, and metallocene compounds can be used alone or in combination.

[0025] The organic fine particles are a material that mainly forms fine irregularities on the surface of the antiglare layer 2 and imparts a function of diffusing external light. As the organic fine particles, resin particles made of a light-transmitting resin material such as an acrylic resin, a polystyrene resin, a styrene-(meth)acrylic acid ester copolymer, a polyethylene resin, an epoxy resin, a silicone resin, polyvinylidene fluoride, or a polyethylene fluoride resin can be used. The refractive index of the resin particle material is preferably 1.40 to 1.75. In order to adjust the refractive index or dispersion of the resin particles, two or more types of resin particles having different materials (refractive indexes) may be mixed and used.

[0026] The inorganic fine particles added to the base resin of the optical functional layer are preferably nanoparticles having an average particle size of 10 to 200 nm, and the amount of inorganic fine particles added is preferably 0.1 to 5.0%.

[0027] The inorganic fine particles are a material for adjusting the precipitation and aggregation of the organic fine particles in the antiglare layer 2. As the inorganic fine particles, silica fine particles, metal oxide fine particles, various mineral fine particles, etc. can be used. As the silica fine particles, for example, colloidal silica or silica fine particles surface-modified with a reactive functional group such as a (meth)acryloyl group can be used. As the metal oxide fine particles, for example, alumina, zinc oxide, tin oxide, antimony oxide, indium oxide, titania, zirconia, etc. can be used. As the mineral fine particles, for example, mica, synthetic mica, vermiculite, montmorillonite, iron montmorillonite, bentonite, beidellite, saponite, hectorite, stevensite, nontronite, magadiite, ilealite, kanemite, layered titanic acid, smectite, synthetic smectite, etc. can be used. The mineral fine particles may be either natural products or synthetic products (including substitution products and derivatives), or a mixture of both may be used. Among the mineral fine particles, layered organic clay is more preferable. The layered organic clay refers to a swelling clay having an organic onium ion introduced between its layers. The organic onium ion is not limited as long as it can be made organic by utilizing the cation exchange property of the swelling clay. When a layered organic clay mineral is used as the mineral fine particles, the above-mentioned synthetic smectite can be suitably used. The synthetic smectite has a function of increasing the viscosity of the coating liquid for forming the antiglare layer, suppressing the settling of the resin particles and inorganic fine particles, and adjusting the uneven shape of the surface of the optical functional layer.

[0028] A leveling agent may be added to the coating solution for forming the antiglare layer. The leveling agent has the function of orienting on the surface of the coating film during drying, making the surface tension of the coating film uniform, and reducing surface defects of the coating film.

[0029] Furthermore, an organic solvent may be added to the resin composition for forming the optical functional layer as appropriate. As the organic solvent, one or more of the following may be used in combination: alcohols such as methanol, ethanol, 1-propanol, 2-propanol, butanol, isopropyl alcohol, isobutanol, ketones such as acetone, methyl ethyl ketone, cyclohexanone, methyl isobutyl ketone, ketone alcohols such as diacetone alcohol, aromatic hydrocarbons such as benzene, toluene, xylene, glycols such as ethylene glycol, propylene glycol, hexylene glycol, glycol ethers such as ethyl cellosolve, butyl cellosolve, ethyl carbitol, butyl carbitol, diethyl cellosolve, diethyl carbitol, propylene glycol monomethyl ether, esters such as methyl lactate, ethyl lactate, methyl acetate, ethyl acetate, amyl acetate, ethers such as dimethyl ether, diethyl ether, N-methylpyrrolidone, dimethylformamide, water, etc.

[0030] The low-reflection layer 3 is an optically functional layer that reduces the surface reflection of the reflection control film 10 by canceling out light reflected on the surface of the low-reflection layer 3 through interference with light reflected on the interface between the low-reflection layer 3 and the anti-glare layer 2. The low-reflection layer 3 can be formed by applying a coating liquid containing a binder resin and low-refractive index fine particles onto the surface of the anti-glare layer 2 and curing the coating.

[0031] The binder resin used in forming the low reflective layer 3 is not particularly limited, and the compounds exemplified as the material for the antiglare layer 2 can be used.

[0032] The low refractive index particles are, for example, LiF, MgF, 3NaF·AlF or AlF (each of which has a refractive index of 1.4), or Na 3 AlF 6Fine particles such as cryolite (refractive index 1.33) and silica fine particles having internal voids can be preferably used. Silica fine particles having internal voids can have the refractive index of the voids (approximately 1) of air, and are therefore useful for lowering the refractive index of the low reflection layer 3. Specifically, porous silica particles and silica particles having a shell structure can be used.

[0033] The average particle diameter of the low refractive index fine particles is preferably 1 nm or more and 100 nm or less. If the average particle diameter of the low refractive index fine particles exceeds 100 nm, light is significantly reflected due to Rayleigh scattering, and the low reflection layer 3 may be whitened, resulting in a decrease in the transparency of the reflection control film 10. On the other hand, if the average particle diameter of the low refractive index fine particles is less than 1 nm, problems such as non-uniformity of particles in the low reflection layer 3 may occur due to particle aggregation.

[0034] If necessary, a solvent or various additives may be added to the coating liquid for forming the low reflection layer 3. As the solvent, for example, those exemplified as the materials for the antiglare layer 2 may be used. As the additives, for example, a defoaming agent, a leveling agent, an antioxidant, an ultraviolet absorbing agent, a light stabilizer, a polymerization inhibitor, a photosensitizer, etc. may be used.

[0035] In addition, when the coating film of the coating liquid for forming the low reflection layer is cured by ultraviolet irradiation, a photopolymerization initiator is added to the coating liquid. As the photopolymerization initiator, the materials exemplified as the material of the antiglare layer 2 can be used.

[0036] The refractive index of the low-reflection layer 3 is preferably lower than that of the anti-glare layer 2 and in the range of 1.25 to 1.50. The lower the refractive index of the refractive index layer, the closer it is to the refractive index of air (refractive index = 1), and the easier it is to achieve low reflectance; however, since a large amount of low-refractive index material needs to be added, the mechanical strength may be reduced and the layer may be easily scratched. On the other hand, if the refractive index of the low-reflection layer exceeds 1.50, the difference in refractive index with air becomes large, and this may result in an increase in reflectance.

[0037] The film thickness of the low-reflective layer 3 is preferably within a range of 5 nm to 1 μm in terms of the properties as an optical interference layer, but it is more preferable in terms of thinning and suppressing reflectance to design the optical film thickness obtained by multiplying the film thickness of the low-reflective layer 3 by the refractive index of the low-reflective layer 3 to be approximately equal to ¼ of the wavelength of visible light (the wavelength to be suppressed).

[0038] Fig. 2 is a diagram for explaining the direction of reflection of light, when the in-vehicle display device is viewed from above.

[0039] External light such as the light of nearby vehicles and street lights may enter the display surface of the in-vehicle display device. In order to reduce the glare caused by reflected light and ensure the visibility of the display surface of the in-vehicle display device, it is preferable to suppress the reflection of external light on the display surface of the in-vehicle display device. Conventionally, optical films used in image display devices have been designed to improve the visibility of the displayed image and to reduce the reflection of the image of incident light on the display surface as much as possible. On the other hand, the image of external light reflected on the display surface of the in-vehicle display device can be regarded as information representing the situation around the vehicle. In particular, digital outer monitors and digital inner monitors, which are expected to be used more widely in the future, are installed at or near the positions where optical mirrors were previously installed, and light from nearby vehicles and street lights is likely to enter them, so it would be meaningful if the reflected image could be used as information for grasping the surrounding situation. However, there has been no technical idea of ​​ensuring the visibility and identifiability of the reflected image so that the reflected image on the display surface can be used as a kind of information, and no consideration has been given to what attributes are necessary for optical films to ensure the visibility and identifiability of the reflected image.

[0040] In order to utilize the image reflected on the display surface of the in-vehicle display device as information about the surroundings of the vehicle, the image discernibility is important. Here, the image discernibility means that the occupant can distinguish the displayed image displayed on the image display device from the reflected image, and can recognize what the reflected image is. The inventor of the present application has studied and found that if the image of external light reflected on the display surface of the in-vehicle display device is too clear, it is difficult to distinguish the displayed image from the image of external light, but if the reflection of the external light incident on the display surface is suppressed too much, the visibility of the displayed image is improved, but the image of external light cannot be used to grasp the situation around the vehicle. In addition, there is a method of suppressing the reflectance by diffusion, such as an anti-glare film, but it was found that if the diffusion of light on the display surface of the in-vehicle display device is too strong, the image of external light becomes blurred, making it difficult to distinguish what the reflected image is.

[0041] In order to ensure the discernibility of the image reflected on the display surface, the attributes (optical properties) required for the optical film for in-vehicle use were examined in detail, and it was found that it is effective to control the amount of specular reflected light Lr of light Li incident from a 30° oblique direction with respect to the normal line of the display surface of the in-vehicle display device, and the amount of reflected light Lr' and Lr'' reflected in the direction of the reflection angle of this specular reflected light in the direction of ±5° (see Figure 2). More specifically, assuming a digital outer monitor or digital inner mirror that is installed in a position where external light is relatively likely to enter as the in-vehicle display device, and taking into consideration the mounting position of the in-vehicle display device, the direction of the display surface facing the driver, and the angle of the display surface with respect to the front-rear direction of the vehicle, it was found that light is likely to enter the display surface of the in-vehicle display device from a 30° oblique direction with respect to the normal line. In addition, it was found that when light Li is incident from a 30° oblique direction with respect to the normal line of the display surface of the in-vehicle display device, the light that enters the eyes of the driver who views the in-vehicle display device is light having a reflection angle of about ±5° with the specular reflected light Lr as the center. Although FIG. 2 assumes a vehicle in which the driver's seat is on the left side, the same applies when the driver's seat is on the right side.

[0042] Therefore, various studies were conducted focusing on the light amounts of specularly reflected light Lr (reflection angle: 30°), reflected light Lr' (reflection angle: 25°), and reflected light Lr'' (reflection angle: 35°), and it was found that the optical characteristics shown in the following items (1) to (3) are necessary to ensure the discrimination of reflected images. In the following, the amount of specularly reflected light of light incident on a substrate without a reflection control layer from a direction obliquely 30° to the normal to the substrate is defined as the reference light amount (=100%). (1) The amount of specular reflected light Lr, which is light that is specularly reflected from light Li incident on a reflection control layer laminated on a substrate from a direction at an angle of 30° with respect to the normal line of the substrate, is 0 to 25% of the reference light amount, (2) For a reflection control layer laminated on a substrate, the amount of light reflected in a direction at a reflection angle of ±5° of specularly reflected light Lr of light Li incident from a direction at an angle of 30° to the normal line of the substrate, i.e., the amount of reflected light Lr' reflected in a direction at an angle of 25° to the normal line of the substrate and the amount of reflected light Lr'' reflected in a direction at an angle of 35° to the normal line, are both 0.3 to 2.0% of the reference light amount, (3) The haze of the reflection control film 10 is 3 to 11%. The haze is a value measured in accordance with JIS K7105.

[0043] The reflection control film 10 according to the present invention has these optical properties, and thus suppresses the reflection of the incident light Li from a direction oblique at 30° to the normal line of the display surface of the in-vehicle display device, and moderately diffuses the incident light Li. As a result, the image of the incident light Li can be visually recognized by the driver as an image that is neither too clear nor too blurred. Therefore, the image of the incident light Li can be easily distinguished from the display image, making it easy to grasp what the image is, and improving the identifiability of the reflected image.

[0044] The light amounts of the reflected lights Lr' and Lr'' are parameters that mainly affect the blurring of the reflected image. When the light amount of the reflected lights Lr' and Lr'' exceeds 2.0% of the reference light amount, the reflected image becomes too blurred, making it difficult to recognize what the reflected image is. On the other hand, when the light amount of the reflected lights Lr' and Lr'' is less than 0.3% of the reference light amount, the reflected image becomes too clear, which may make it difficult to distinguish between the displayed image and the reflected image. In particular, when the light amount of the reflected lights Lr' and Lr'' is less than 0.3% of the reference light amount and the light amount of the specular reflected light Lr exceeds 25% of the reference light amount, the reflected image becomes too clear, making it difficult to distinguish between the displayed image and the reflected image. Moreover, regardless of the light amount of the reflected lights Lr' and Lr'', when the light amount of the specular reflected light Lr exceeds 25% of the reference light amount, the visibility of the displayed image may decrease due to the specular reflected light being too bright. Furthermore, haze is a parameter related to all of the light amounts of specularly reflected light Lr and reflected light Lr' and Lr". When the haze of reflection control film 10 is less than 3%, the light diffusion decreases and the light amounts of reflected light Lr' and Lr" become smaller than the above-mentioned lower limit, so that the reflected image tends not to be blurred appropriately. On the other hand, when the haze of reflection control film 10 exceeds 11%, the light diffusion becomes strong and the light amounts of reflected light Lr' and Lr" become larger than the above-mentioned upper limit, so that the reflected image tends to be blurred more and to be difficult to recognize.

[0045] As explained above, reflection control film 10 according to the present invention is intended to utilize the image of external light reflected on the display surface of an image display device as a kind of information showing the situation around the vehicle, and by providing the optical characteristics of items (1) to (3) above, it is possible to achieve both visibility of the displayed image and distinguishability of the image of external light reflected on the display surface. Conventionally, there has been no idea of ​​utilizing the image of external light reflected on the display surface of an image display device as information, and therefore no consideration has been given to the requirements necessary for an optical film to utilize the image of external light as information, but reflection control film 10 according to the present invention has excellent distinguishability of the reflected image as described above, and is therefore extremely effective as an optical film that realizes an unprecedented idea.

[0046] The reflection control film 10 according to the present invention is typically used as an optical film provided on the outermost surface of an image display device, but the lamination position in the laminate constituting the image display device is not particularly limited as long as the desired optical properties can be exhibited. In addition, one or more optical functional layers such as an antistatic layer, an antifouling layer, an infrared absorbing layer, an ultraviolet absorbing layer, and a color correction layer may be provided on the reflection control layer 5 of the reflection control film 10. EXAMPLES

[0047] Hereinafter, examples in which the reflection control film according to the embodiment is specifically implemented will be described.

[0048] (Examples 1 to 5, Comparative Examples 9 to 11) A reflection control film was produced by laminating an antiglare layer and a low reflection layer in this order on a substrate as an antireflection layer. A 40 μm-thick triacetyl cellulose film was used as the substrate. An antiglare layer was formed by applying a coating liquid for forming an antiglare layer on the substrate, drying the coating film, and polymerizing and curing the coating film. Thereafter, a low reflection layer was formed by applying a coating liquid for forming a low reflection layer on the antiglare layer, drying the coating film, and polymerizing and curing the coating film.

[0049] A reflection control film was produced by laminating an antiglare layer on a substrate as an antireflection layer. A 40 μm-thick triacetyl cellulose film was used as the substrate. A coating solution for forming an antiglare layer was applied onto the substrate, dried, and then the coating film was polymerized and cured to form an antiglare layer. (Comparative Examples 1 to 8) A reflection control film was produced by laminating an antiglare layer on a substrate as an antireflection layer. A 40 μm-thick triacetyl cellulose film was used as the substrate. A coating solution for forming an antiglare layer was applied onto the substrate, dried, and then the coating film was polymerized and cured to form an antiglare layer.

[0050] Comparative Example 12 A reflection control film was produced by laminating a hard coat layer and a low reflection layer as an anti-reflection layer on a substrate. A 40 μm-thick triacetyl cellulose film was used as the substrate. A hard coat layer was formed by applying a coating liquid for forming a hard coat layer on the substrate, drying the coating film, and polymerizing and curing the coating film. Then, a low reflection layer was formed by applying a coating liquid for forming a low reflection layer on the hard coat layer, drying the coating film, and polymerizing and curing the coating film.

[0051] The compositions of the coating liquid for forming the antiglare layer, the coating liquid for forming the low reflection layer, and the coating liquid for forming the hard coat layer used in the examples and comparative examples are shown in Tables 1 to 3. Each coating liquid was diluted to a concentration suitable for coating using the solvents shown in Tables 1 to 3.

[0052] [Table 1]

[0053] [Table 2]

[0054] [Table 3]

[0055] [Haze value] The haze was measured using a haze meter (NDH2000, manufactured by Nippon Denshoku Industries Co., Ltd.) in accordance with JIS K7105.

[0056] [Reflected light amount] Using a goniophotometer (GP-5, Murakami Color Research Laboratory Co., Ltd.), light approximating a D65 light source was irradiated from the antireflection layer side at an incident angle of 30°, and the intensity of the specular reflected light at a reflection angle of 30° and the reflected light at reflection angles of 23° to 37° was measured.

[0057] [evaluation] With the reflection control films of Examples 1 to 5 and Comparative Examples 1 to 12 attached to the surface of a liquid crystal display device iPad (registered trademark) Air (4th generation), an image was displayed on the display screen under darkroom conditions (no incident light from the surroundings), with the center of the liquid crystal display device at a height of 100 cm from the floor and the evaluator's visual position at a horizontal linear distance of 50 cm from the center of the display screen. In this state, fluorescent light was incident at an incident angle of 30°, and evaluation was performed under three conditions: regular reflection direction and regular reflection direction ±5°.

[0058] The evaluation criteria in Table 4 are as follows: the average score of the three conditions by the 15 evaluators is 4 to 5 points (◯), 3 to less than 4 points (△), and 1 to less than 3 points (×). " was rated as a pass. <Evaluation criteria> 5 points: The displayed image and the reflected fluorescent light image can be clearly recognized and distinguished. 4 points: The displayed image and the reflected fluorescent light image can be recognized and distinguished. 3 points: The displayed image and the reflected fluorescent light image can be recognized and distinguished, but the displayed image or the reflected fluorescent light image is partially blurred. 2 points: Either the displayed image or the reflected fluorescent light image cannot be recognized, or the displayed image and the reflected fluorescent light image cannot be distinguished. Score 1: Neither the displayed image nor the reflected fluorescent light image can be recognized or distinguished.

[0059] Table 4 shows the evaluation of the layer structure, haze, reflected light amount (amount of reflected light at reflection angles of 30°, 25°, and 35°), and image discrimination of the reflection control films according to Examples 1 to 5 and Comparative Examples 1 to 12. In addition, "AGLR" in the layer structure of Table 3 indicates that the antireflection layer is composed of an antiglare layer and a low reflection layer, "AG" indicates that the antireflection layer is composed of an antiglare layer, and "HCLR" indicates that the antireflection layer is composed of a low reflection layer on a hard coat layer. The unit of the reflected light amount is "%", and the value of the reflected light amount is a value expressed as 100% of the intensity of the regular reflection light when D65 light source approximation light is incident at an incident angle of 30° on a substrate not laminated with an antireflection layer.

[0060] [Table 4]

[0061] The reflection control films according to Examples 1 to 5 had a haze of 3 to 11%, which moderately diffused incident light, and the low-reflection layer suppressed surface reflection, with the amount of regular reflection being 25% or less and the intensity of reflected light at reflection angles of 25° and 35° being within the range of 0.3 to 2.0%. It was confirmed that the reflection control films satisfying these conditions made it possible to distinguish between the displayed image and the reflected image of the fluorescent lamp, and to recognize what the reflected image was.

[0062] The reflection control films according to Comparative Examples 1 to 5 had a haze in the range of 3 to 11%, but because they did not have a low reflection layer, the amount of specular reflected light exceeded 25%, and the amount of reflected light at a reflection angle of 25° and at a reflection angle of 35° also exceeded 2.0%. Because the amount of specular reflected light was high, it was possible to recognize what the reflected image of the fluorescent light was, but the high amount of specular reflected light made it difficult to distinguish between the displayed image and the reflected image, resulting in lower evaluations than Examples 1 to 5.

[0063] The reflection control films according to Comparative Examples 6 and 7 do not have a low reflection layer, but the high haze increases the diffusion of incident light, and the amount of specularly reflected light is suppressed to be smaller than that of Comparative Examples 1 to 5. This allows the display image and the reflected image to be distinguished. However, while the amount of specularly reflected light is suppressed to a certain extent, the amount of reflected light at a reflection angle of 25° and at a reflection angle of 35° is close to 5.0%, so the reflected image of the fluorescent lamp is viewed in a relatively dark and blurred state, and it is not possible to recognize what the reflected image is.

[0064] The reflection control film of Comparative Example 8 did not have a low-reflection layer and the amount of reflected light was not suppressed, so the amount of specularly reflected light was too high, making it impossible to distinguish between the displayed image and the image of the fluorescent lamp reflected in it.

[0065] In the reflection control films according to Comparative Examples 9 and 10, the reflection control layer was composed of an antiglare layer and a low reflection layer as in Examples 1 to 5, but the high haze caused high diffusion of incident light, and the amount of reflected light at a reflection angle of 25° and at a reflection angle of 35° exceeded 2.0%. While the amount of specularly reflected light was suppressed to 25% or less, the amount of reflected light at a reflection angle of 25° and at a reflection angle of 35° increased, so that the reflected image was viewed in a relatively dark and blurred state, and it was impossible to recognize what the reflected image was.

[0066] In the reflection control films according to Comparative Examples 11 and 12, the amount of reflected light at a reflection angle of 25° and at a reflection angle of 35° was less than 0.3% due to the small haze. As a result, the reflected image became clear, and it was impossible to distinguish between the displayed image and the reflected image of the fluorescent lamp.

[0067] From the above, it was confirmed that the reflection control film of the present invention can distinguish between the displayed image and the reflected image of the image display device when light is incident at an angle of 30° to the normal to the display surface of the image display device, and can also recognize what the reflected image is.

[0068] Tables 5 to 8 show the haze, reflected light amount (amount of reflected light at reflection angles of 23°, 24°, 25°, 26°, 27°, 30°, 33°, 34°, 35°, 36°, and 37°), the sum of the reflected light amounts at reflection angles of 23° and 24°, the sum of the reflected light amounts at reflection angles of 26° and 27°, the sum of the reflected light amounts at reflection angles of 23° and 24°, and the sum of the reflected light amounts at reflection angles of 25°, for the reflection control films of Examples 1 to 5 and Comparative Examples 1 to 12. The evaluation of image discrimination is summarized as follows: the sum of the reflected light amounts at reflection angles of 26° and 27° divided by the reflected light amount at a reflection angle of 25°, the sum of the reflected light amounts at reflection angles of 33° and 34°, the sum of the reflected light amounts at reflection angles of 36° and 37° divided by the reflected light amount at a reflection angle of 35°, and the sum of the reflected light amounts at reflection angles of 36° and 37° divided by the reflected light amount at a reflection angle of 35°. The unit of the reflected light amount is "%", and the value of the reflected light amount is a value expressed as 100% when the intensity of the regular reflected light when the D65 light source approximation light is incident on a substrate without an anti-reflection layer at an incident angle of 30°. The units for the value obtained by dividing the sum of the reflected light amounts at reflection angles of 23° and 24° by the amount of reflected light at a reflection angle of 25°, the value obtained by dividing the sum of the reflected light amounts at reflection angles of 26° and 27° by the amount of reflected light at a reflection angle of 25°, the value obtained by dividing the sum of the reflected light amounts at reflection angles of 33° and 34° by the amount of reflected light at a reflection angle of 35°, and the value obtained by dividing the sum of the reflected light amounts at reflection angles of 36° and 37° by the amount of reflected light at a reflection angle of 35° are dimensionless. Haze and evaluation are the same as those described for Table 4.

[0069] [Table 5]

[0070] [Table 6]

[0071] [Table 7]

[0072] [Table 8]

[0073] The reflection control films according to Examples 1 to 5 have a haze of 3 to 11%, which allows the incident light to be diffused appropriately, and the surface reflection is suppressed by the low reflection layer, so that the amount of regular reflection is 25% or less, and the intensity of the reflected light at reflection angles of 25° and 35° is within the range of 0.3 to 2.0%. Furthermore, the value obtained by dividing the sum of the reflected light amounts at reflection angles of 26° and 27° by the reflected light amount at a reflection angle of 25° is within the range of 8.30 to 9.50. The value obtained by dividing the sum of the reflected light amounts at reflection angles of 33° and 34° by the reflected light amount at a reflection angle of 35° is within the range of 6.89 to 7.87. It was confirmed that the reflection control films satisfying these conditions enable the display image to be distinguished from the image of the fluorescent lamp reflected therein, and also enable the user to recognize what the reflected image is.

[0074] The reflection control films according to Comparative Examples 1 to 5 had a haze in the range of 3 to 11%, but because they did not have a low refractive index layer, the amount of regular reflection exceeded 25%, and the amount of reflection at a reflection angle of 25° and the amount of reflection at a reflection angle of 35° also exceeded 2.0%. Furthermore, the value obtained by dividing the sum of the amount of reflection at reflection angles of 26° and 27° by the amount of reflection at a reflection angle of 25° was in the range of 5.77 to 6.20. The value obtained by dividing the sum of the amount of reflection at reflection angles of 33° and 34° by the amount of reflection at a reflection angle of 35° was in the range of 5.36 to 5.62. Because the amount of regular reflection was high, it was possible to recognize what the reflected image was, but because the amount of regular reflection was high, it became difficult to distinguish between the displayed image and the reflected image, and the evaluation was lower than that of Examples 1 to 5.

[0075] The reflection control films according to Comparative Examples 6 and 7 do not have a low refractive index layer, but the high haze increases the diffusion of incident light, and the amount of regular reflection light is suppressed to be smaller than that of Comparative Examples 1 to 5. Therefore, it was possible to distinguish between the display image and the reflected image. However, while the amount of regular reflection light was suppressed to a certain extent, the amount of reflected light at a reflection angle of 25° and the amount of reflected light at a reflection angle of 35° were close to 5.0%, so the reflected image was relatively dark and was viewed in a blurred state, and it was not possible to recognize what the reflected image was. Furthermore, the value obtained by dividing the sum of the reflected light amounts at reflection angles of 26° and 27° by the reflected light amount at a reflection angle of 25° was 4.74 in Comparative Example 6 and 3.73 in Comparative Example 7. The value obtained by dividing the sum of the reflected light amounts at reflection angles of 33° and 34° by the reflected light amount at a reflection angle of 35° was 4.78 in Comparative Example 6 and 3.63 in Comparative Example 7.

[0076] The reflection control film according to Comparative Example 8 did not have a low refractive index layer and did not suppress the amount of reflected light, so the amount of regular reflected light was too high, making it impossible to distinguish between the displayed image and the reflected image. Furthermore, the sum of the reflected light amounts at reflection angles of 26° and 27° divided by the reflected light amount at a reflection angle of 25° was 17.12. The sum of the reflected light amounts at reflection angles of 33° and 34° divided by the reflected light amount at a reflection angle of 35° was 11.91.

[0077] In the reflection control films according to Comparative Examples 9 and 10, the reflection control layer is composed of an antiglare layer and a low refractive index layer as in Examples 1 to 5, but the high haze increases the diffusivity of incident light, and the amount of reflected light at a reflection angle of 25° and at a reflection angle of 35° exceeds 2.0%. While the amount of regular reflection light is suppressed to 25% or less, the amount of reflected light at a reflection angle of 25° and at a reflection angle of 35° increases, so that the reflected image is relatively dark and is visually recognized in a blurred state, and it is not possible to recognize what the reflected image is. Furthermore, the value obtained by dividing the sum of the reflected light amounts at reflection angles of 26° and 27° by the reflected light amount at a reflection angle of 25° was 5.11 in Comparative Example 9 and 4.41 in Comparative Example 10. The value obtained by dividing the sum of the reflected light amounts at reflection angles of 33° and 34° by the reflected light amount at a reflection angle of 35° was 5.08 in Comparative Example 9 and 4.30 in Comparative Example 10.

[0078] In the reflection control films according to Comparative Examples 11 and 12, the amount of reflected light at a reflection angle of 25° and the amount of reflected light at a reflection angle of 35° were smaller than 0.3% due to the small haze. Therefore, the reflected image was clear, and it was impossible to distinguish between the displayed image and the reflected image. Furthermore, the value obtained by dividing the sum of the reflected light amounts at reflection angles of 26° and 27° by the reflected light amount at a reflection angle of 25° was 18.19 in Comparative Example 11 and 97.00 in Comparative Example 12. The value obtained by dividing the sum of the reflected light amounts at reflection angles of 33° and 34° by the reflected light amount at a reflection angle of 35° was 13.65 in Comparative Example 11 and 5.00 in Comparative Example 12.

[0079] The value obtained by dividing the sum of the reflected light amounts at reflection angles of 26° and 27° by the reflected light amount at a reflection angle of 25° is larger than the value obtained by dividing the sum of the reflected light amounts at reflection angles of 33° and 34° by the reflected light amount at a reflection angle of 35°. This is because the closer the reflection angle is to 0°, the more susceptible it is to the influence of incident light. In addition, in Examples 1 to 5, the smaller the haze, the smaller the value obtained by dividing the sum of the reflected light amounts at reflection angles of 23° and 24° by the reflected light amount at a reflection angle of 25°, the value obtained by dividing the sum of the reflected light amounts at reflection angles of 26° and 27° by the reflected light amount at a reflection angle of 25°, the value obtained by dividing the sum of the reflected light amounts at reflection angles of 33° and 34° by the reflected light amount at a reflection angle of 35°, and the value obtained by dividing the sum of the reflected light amounts at reflection angles of 36° and 37° by the reflected light amount at a reflection angle of 35°. In addition, when comparing Examples 1 to 5 with Comparative Examples 1 to 5 in which a low refractive index layer is not formed, the lower the reflectance, the smaller the value obtained by dividing the sum of the reflected light amounts at reflection angles of 23° and 24° by the reflected light amount at a reflection angle of 25°, the value obtained by dividing the sum of the reflected light amounts at reflection angles of 26° and 27° by the reflected light amount at a reflection angle of 25°, the value obtained by dividing the sum of the reflected light amounts at reflection angles of 33° and 34° by the reflected light amount at a reflection angle of 35°, and the value obtained by dividing the sum of the reflected light amounts at reflection angles of 36° and 37° by the reflected light amount at a reflection angle of 35°. Therefore, reducing the haze and reducing the reflectance contribute to reducing the value obtained by dividing the sum of the reflected light amounts at reflection angles of 26° and 27° by the reflected light amount at a reflection angle of 25°, etc.

[0080] The sum of the reflected light amounts at reflection angles of 23° and 24° divided by the reflected light amount at a reflection angle of 25° and the sum of the reflected light amounts at reflection angles of 36° and 37° divided by the reflected light amount at a reflection angle of 35° do not show a large difference between the examples and the comparative examples. On the other hand, the sum of the reflected light amounts at reflection angles of 26° and 27° divided by the reflected light amount at a reflection angle of 25° and the sum of the reflected light amounts at reflection angles of 33° and 34° divided by the reflected light amount at a reflection angle of 35° show a significant difference between the examples and the comparative examples. In particular, in the examples 1 to 5, the sum of the reflected light amounts at reflection angles of 26° and 27° divided by the reflected light amount at a reflection angle of 25° and the sum of the reflected light amounts at reflection angles of 33° and 34° divided by the reflected light amount at a reflection angle of 35° were 6.89 to 9.50, and therefore the evaluation results were superior to those of the comparative examples 1 to 12. This is believed to be advantageous in that, when the relationship between the amount of reflected light at reflection angles of 25° to 7° and the relationship between the amount of reflected light at reflection angles of 33° to 35° satisfy the above condition, when the human eye sees light incident at an angle, it will be able to distinguish between the displayed image and the reflected image of the fluorescent lamp, and will also be able to recognize what the reflected image is.

[0081] Since the value obtained by dividing the sum of the reflected light amounts at reflection angles of 26° and 27° by the amount of reflected light at a reflection angle of 25° and the value obtained by dividing the sum of the reflected light amounts at reflection angles of 33° and 34° by the amount of reflected light at a reflection angle of 35° are within the above ranges, it has been confirmed that the reflection control film of the present invention is capable of distinguishing between the displayed image and the reflected image of the image display device when light is incident at an angle of 30° to the normal to the display surface of the image display device, and of recognizing what the reflected image is. [Industrial Applicability]

[0082] The reflection control film according to the present invention can be used as an optical film for use in image display devices, and is particularly suitable for use in vehicle-mounted display devices. [Explanation of symbols]

[0083] 1 Base material 2 Anti-glare layer 3 Low reflective layer 5 Reflection Control Layer 10. Reflection control film for automobiles

Claims

1. A reflection control film for vehicle mounting comprising a substrate and a reflection control layer laminated on the substrate, the reflection control layer comprises an antiglare layer laminated on the substrate, and a low refractive index layer laminated on the antiglare layer without any other layer therebetween; when the amount of specularly reflected light of light incident on a substrate on which a reflection control layer is not laminated, from a direction at an oblique angle of 30° with respect to the normal line of the substrate, is taken as 100%, the amount of specularly reflected light of light incident on the reflection control layer of the in-vehicle reflection control film from a direction at an oblique angle of 30° with respect to the normal line of the reflection control film is 0 to 20.61%, and the amount of reflected light in a direction of a reflection angle of ±5° of the specularly reflected light is 0.3 to 2.0%, An in-vehicle reflection control film having a haze of 3 to 11%.

2. The reflection control film for vehicle installation according to claim 1, characterized in that the value obtained by dividing the sum of the reflected light amounts at reflection angles of 26° and 27° by the reflected light amount at a reflection angle of 25° and the value obtained by dividing the sum of the reflected light amounts at reflection angles of 33° and 34° by the reflected light amount at a reflection angle of 35° are 6.89 to 9.50.

Citation Information

Patent Citations

  • Antiglare laminate and display equipped with the same

    JP2009204728A

  • Optical film and production method of the same

    JP2014102356A

  • Device for pulling out linear body

    JP1982025216A

  • Antireflection film and optical device

    JP2001074903A