Rubber composition for tires

A modified hydrogenated petroleum resin enhances silica dispersibility in tire rubber compositions, improving rolling resistance, abrasion resistance, and processability by blending it with diene rubber polymer and silica.

JP2024144634APending Publication Date: 2024-10-11IDEMITSU KOSAN CO LTD
View PDF 1 Cites 0 Cited by

Patent Information

Application Number
JP2024121349
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Filing Date
2024-07-26
Publication Date
2024-10-11

AI Technical Summary

Technical Problem

The dispersibility of silica in rubber compositions for tires is insufficient with certain types of petroleum resins, leading to inadequate performance in rolling resistance, abrasion resistance, and processability.

Method used

A rubber composition for tires is formulated with a specific modified hydrogenated petroleum resin that enhances silica dispersibility, containing 0.1 to 10% silicon element, a weight average molecular weight of 500 to 5,000, a molecular weight distribution of 1.1 to 3.5, and a softening point of 60 to 150°C, blended with diene rubber polymer and silica.

Benefits of technology

The composition improves silica dispersibility, resulting in tires with enhanced rolling resistance, abrasion resistance, and processability.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024144634000002
    Figure 2024144634000002
  • Figure 2024144634000001
    Figure 2024144634000001
Patent Text Reader

Abstract

To provide a rubber composition that allows for improved dispersibility of silica, and a tire including the rubber composition that exhibits superior rolling resistance, wear resistance, and processability.SOLUTION: A rubber composition for tires includes at least a diene rubber polymer, silica, and a modified hydrogenated petroleum resin that fulfills the following (A1)-(A3): (A1) a silicon element content of 0.1-10 mass% in terms of silicon atom; (A2) a weight average molecular weight of 500-5,000; and (A3) a molecular weight distribution (Mw / Mn) of 1.1-3.5.SELECTED DRAWING: None
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a rubber composition for tires, and more particularly to a rubber composition for tires that can improve the dispersibility of silica in the rubber composition to obtain tires that are excellent in rolling resistance, abrasion resistance, processability, and the like. [Background technology]

[0002] 2. Description of the Related Art In recent years, increasing demands for improved fuel efficiency in automobiles have led to demands for higher performance tires, specifically, improved abrasion resistance, processability, and also improved rolling resistance of tires.

[0003] In this regard, petroleum resins are easily compatible with rubber components and have a high softening point, and therefore have conventionally been compounded in rubber compositions for tires to reinforce the rubber components and increase the elastic modulus of vulcanized rubber. Furthermore, for the purpose of improving rolling resistance, a method of compounding silica in rubber compositions for tires has generally been adopted.

[0004] However, depending on the type of petroleum resin, the dispersibility of silica may be insufficient, in which case there is a problem that the expected effects cannot be fully obtained (see, for example, Patent Document 1). [Prior art documents] [Patent documents]

[0005] [Patent Document 1] JP 2017-88671 A Summary of the Invention [Problem to be solved by the invention]

[0006] The present invention has been made in consideration of the above problems, and has an object to provide a rubber composition for tires which, by blending a specific modified hydrogenated petroleum resin therein, improves the dispersibility of silica in the rubber composition, thereby enabling to obtain tires having excellent rolling resistance, abrasion resistance and processability. [Means for solving the problem]

[0007] The present inventors have discovered a rubber composition for tires that can improve the dispersibility of silica in the rubber composition by compounding a specific modified hydrogenated petroleum resin, thereby making it possible to obtain a tire that is excellent in rolling resistance, abrasion resistance, and processability.

[0008] That is, according to the present invention, the following [1] to [6] are provided. [1] A rubber composition for tires, comprising at least a diene-based rubber polymer, silica, and a modified hydrogenated petroleum resin satisfying the following (A1) to (A3): (A1) Silicon element is contained in an amount of 0.1 to 10 mass% in terms of silicon atoms. (A2) Weight average molecular weight is 500~5,000 (A3) Molecular weight distribution (Mw / Mn) is 1.1 to 3.5 [2] The modified hydrogenated petroleum resin is 1 The rubber composition for tires according to [1], wherein the integral ratio of aromatic hydrogen in H-NMR measurement [integral value of peak in 6.5 to 7.5 ppm region / (sum of integral value of peak in 0 to 3.0 ppm region and integral value of peak in 6.5 to 7.5 ppm region)] is 0 to 15%. [3] The rubber composition for tires according to [1] or [2], wherein the modified hydrogenated petroleum resin has a softening point of 60 to 150°C. [4] The rubber composition for tires according to any one of [1] to [3], comprising 1 to 20 parts by mass of the modified hydrogenated petroleum resin per 100 parts by mass of the diene rubber polymer. [5] The rubber composition for tires according to any one of [1] to [4], comprising 10 to 150 parts by mass of the silica per 100 parts by mass of the diene rubber polymer. [6] A tire using the rubber composition for tires according to any one of [1] to [5]. Effect of the Invention

[0009] According to the present invention, it is possible to provide a rubber composition capable of improving the dispersibility of silica in the rubber composition, and a tire using the same, which has excellent rolling resistance, abrasion resistance and processability. [Brief description of the drawings]

[0010] [Figure 1] 2 is an optical microscope photograph of the rubber composition obtained in Example 1. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0011] The upper and lower limit values ​​of the numerical ranges described in this specification can be combined in any way. For example, when "A to B" and "C to D" are described as numerical ranges, the numerical ranges "A to D" and "C to B" are also included in the scope of the present invention. In addition, unless otherwise specified, a numerical range of "lower limit value to upper limit value" described in this specification means not less than the lower limit value and not more than the upper limit value. In this specification, the numerical values ​​in the examples are numerical values ​​that can be used as upper or lower limits.

[0012] [Rubber composition for tires] The rubber composition for tires of the present invention contains at least a diene rubber polymer, silica, and a modified hydrogenated petroleum resin that satisfies the following (A1) to (A3). (A1) Silicon element is contained in an amount of 0.1 to 10 mass% in terms of silicon atoms. (A2) Weight average molecular weight is 500~5,000 (A3) Molecular weight distribution (Mw / Mn) is 1.1 to 3.5

[0013] [Diene rubber polymer] Examples of the diene rubber polymer in the present invention include various rubber polymers having an isoprene unit and / or a butadiene unit in the molecule. Specific examples include natural rubber (NR), synthetic isoprene rubber (IR), butadiene rubber (BR), styrene-butadiene rubber (SBR), nitrile rubber (NBR), chloroprene rubber (CR), butyl rubber (IIR), styrene-isoprene copolymer rubber, butadiene-isoprene copolymer rubber, and styrene-isoprene-butadiene copolymer rubber.

[0014] These diene rubber polymers may be used alone or in combination of two or more. Among these, it is preferable to use natural rubber, synthetic isoprene rubber, styrene butadiene rubber, or butadiene rubber.

[0015] (Modified hydrogenated petroleum resin) In this specification, the term "petroleum resin" refers to a resin obtained by polymerizing or copolymerizing one or more unsaturated compounds selected from aliphatic olefins and aliphatic diolefins having 4 to 10 carbon atoms, which are obtained as by-products during the production of olefins such as ethylene by thermal decomposition of petroleum such as naphtha, or aromatic compounds having 8 or more carbon atoms and having an olefinically unsaturated bond. Petroleum resins can be roughly classified into, for example, "aliphatic petroleum resins" obtained by polymerizing aliphatic olefins or aliphatic diolefins, "aromatic petroleum resins" obtained by polymerizing aromatic compounds having olefinic unsaturated bonds, and "aliphatic-aromatic copolymer petroleum resins" obtained by copolymerizing aliphatic olefins or aliphatic diolefins with aromatic compounds having olefinic unsaturated bonds.

[0016] Examples of the aliphatic olefins having 4 to 10 carbon atoms include butene, pentene, hexene, and heptene. Examples of the aliphatic diolefins having 4 to 10 carbon atoms include butadiene, pentadiene, isoprene, piperylene, cyclopentadiene, dicyclopentadiene, and methylpentadiene. Examples of aromatic compounds having 8 or more carbon atoms and an olefinically unsaturated bond include styrene, α-methylstyrene, β-methylstyrene, vinyltoluene, vinylxylene, indene, methylindene, and ethylindene. Furthermore, the raw material compounds for the petroleum resin do not all need to be by-products in the production of olefins by thermal decomposition of petroleum such as naphtha, and chemically synthesized unsaturated compounds may also be used.

[0017] Preferable examples of petroleum resins include dicyclopentadiene-based petroleum resins obtained by polymerization of cyclopentadiene or dicyclopentadiene, dicyclopentadiene-styrene-based petroleum resins obtained by copolymerizing these cyclopentadiene or dicyclopentadiene with styrene, C5-based petroleum resins obtained by polymerization of isoprene or piperylene, and C9-based petroleum resins obtained by polymerization of C9 monomers such as indene or vinyltoluene.

[0018] In this specification, the term "hydrogenated petroleum resin" refers to a petroleum resin obtained by adding hydrogen atoms to the above-mentioned petroleum resin. Hydrogenated petroleum resins include fully hydrogenated petroleum resins in which substantially no unsaturated bonds remain and partially hydrogenated petroleum resins in which unsaturated bonds remain, and fully hydrogenated petroleum resins are preferred. The hydrogenated petroleum resin is preferably a hydrogenated aliphatic-aromatic copolymer petroleum resin.

[0019] The modified hydrogenated petroleum resin contains 0.1 to 10 mass % of silicon element calculated as silicon atom. The silicon element is preferably derived from an organosilane structure. The silicon element content can be measured by ICP emission spectrometry, specifically, by the method described in the examples. The modified hydrogenated petroleum resin contains silicon element in an amount calculated as silicon atoms of 0.1 to 10 mass %, preferably 0.3 to 8 mass %, more preferably 0.5 to 5 mass %, and even more preferably 0.5 to 4 mass %.

[0020] The modified hydrogenated petroleum resin is preferably a silane-modified hydrogenated petroleum resin having an organosilane structure, and more preferably a modified hydrogenated petroleum resin in which an alkoxysilyl group is bonded to the main chain of the hydrogenated petroleum resin via a bond. Here, "the alkoxysilyl group is bonded to the main chain of the hydrogenated petroleum resin via a bonding portion" means that, for example, a bonding portion is bonded directly to a carbon atom contained in a hydrogenated polymer (hydrogenated petroleum resin) obtained by polymerizing aliphatic olefins, aliphatic diolefins, and an aromatic compound having an olefinically unsaturated bond as described above and adding hydrogen atoms, and further an alkoxysilyl group is bonded to the carbon atom.

[0021] The alkoxysilyl group is preferably a trialkoxysilyl group having an alkoxy group having 1 to 20 carbon atoms, which may be linear or branched, and more preferably a trialkoxysilyl group having an alkoxy group having 1 to 10 carbon atoms, which may be linear or branched. Specific examples include a trimethoxysilyl group, a triethoxysilyl group, and a tripropoxysilyl group, and the like, with the trimethoxysilyl group and the triethoxysilyl group being preferred.

[0022] The bonding portion may be any divalent or higher organic group that can bond to a carbon atom in the main chain of the hydrogenated petroleum resin and to which an alkoxysilyl group can be bonded, and is preferably an alkylene group, more preferably an alkylene group having 2 to 3 carbon atoms.

[0023] The modified hydrogenated petroleum resin is 1 The integral ratio of aromatic hydrogen in H-NMR measurement [integral value of the peak in the 6.5 to 7.5 ppm region / (sum of the integral value of the peak in the 0 to 3.0 ppm region and the integral value of the peak in the 6.5 to 7.5 ppm region)] is preferably 0 to 15%, more preferably 0 to 10%, and further preferably 0 to 5%. 1 The integral ratio of aromatic hydrogen in H-NMR measurement can be specifically measured by the method described in the Examples. 1 The integral ratio of aromatic hydrogen in H-NMR measurement is a value indicating the ratio of aromatic sites in the modified hydrogenated petroleum resin, 1 When the integral ratio of aromatic hydrogen in H-NMR measurement is within the above range, the composition has low odor and excellent colorlessness.

[0024] The weight average molecular weight (Mw) of the modified hydrogenated petroleum resin is from 500 to 5,000, preferably from 600 to 3,000, more preferably from 700 to 2,000, and even more preferably from 800 to 1,500. The weight average molecular weight is an index of fluidity when melted, and the smaller the weight average molecular weight, the greater the fluidity when melted, and the better the processability when applied to a rubber composition for tires. By having the weight average molecular weight within the above range, the rubber composition can be excellent in processability when applied to a rubber composition for tires while maintaining heat resistance. The weight average molecular weight can be specifically measured by the method described in the Examples.

[0025] The molecular weight distribution (weight average molecular weight / number average molecular weight, Mw / Mn) of the modified hydrogenated petroleum resin is from 1.1 to 3.5, preferably from 1.3 to 3.0, more preferably from 1.5 to 3.0, and even more preferably from 2.0 to 2.5. The molecular weight distribution indicates the degree of dispersion of molecular weights, and becomes broad when the amount of low molecular weight components or high molecular weight components is extremely large. The molecular weight distribution can be specifically measured by the method described in the Examples. When the molecular weight distribution is within the above range, the composition has low odor and excellent coatability.

[0026] The number average molecular weight (Mn) of the modified hydrogenated petroleum resin is preferably from 100 to 4,500, more preferably from 250 to 2,500, and even more preferably from 300 to 1,500.

[0027] The softening point of the modified hydrogenated petroleum resin is preferably from 60 to 150°C, more preferably from 80 to 140°C, and even more preferably from 90 to 130°C. The softening point can be measured by a ring and ball method, specifically, by the method described in the examples. When the softening point is within the above range, the rubber composition for tires has an excellent balance between heat resistance and processability.

[0028] [Method of manufacturing modified hydrogenated petroleum resin] The method for producing the modified hydrogenated petroleum resin is not particularly limited, but the following method is preferred from the viewpoints of efficiently introducing silane into the resin and improving heat resistance. The method for producing the modified hydrogenated petroleum resin is preferably a method in which a hydrogenated petroleum resin is reacted with a compound having a carbon-carbon double bond and an alkoxysilyl group in the presence of a compound that generates radicals.

[0029] The hydrogenated petroleum resin used in the above-mentioned production method is synonymous with the "hydrogenated petroleum resin" described in the above section [Modified hydrogenated petroleum resin], and specifically, is a petroleum resin obtained by adding hydrogen atoms to a petroleum resin. Hydrogenated petroleum resins include fully hydrogenated petroleum resins in which substantially no unsaturated bonds remain, and partially hydrogenated petroleum resins in which unsaturated bonds remain, and the hydrogenated petroleum resin used in the above-mentioned production method is preferably a fully hydrogenated petroleum resin. The hydrogenated petroleum resin is preferably a hydrogenated aliphatic-aromatic copolymer petroleum resin.

[0030] The petroleum resin used as the raw material for the hydrogenated petroleum resin has the same meaning as the "petroleum resin" explained in the section [Modified hydrogenated petroleum resin] above, and is specifically as follows. Petroleum resins are resins obtained by polymerizing or copolymerizing one or more unsaturated compounds selected from aliphatic olefins and aliphatic diolefins having 4 to 10 carbon atoms, which are obtained as by-products during the production of olefins such as ethylene by thermal decomposition of petroleum such as naphtha, or aromatic compounds having 8 or more carbon atoms and having an olefinically unsaturated bond. Petroleum resins can be roughly classified into, for example, "aliphatic petroleum resins" obtained by polymerizing aliphatic olefins or aliphatic diolefins, "aromatic petroleum resins" obtained by polymerizing aromatic compounds having olefinic unsaturated bonds, and "aliphatic-aromatic copolymer petroleum resins" obtained by copolymerizing aliphatic olefins or aliphatic diolefins with aromatic compounds having olefinic unsaturated bonds.

[0031] Examples of the aliphatic olefins having 4 to 10 carbon atoms include butene, pentene, hexene, and heptene. Examples of the aliphatic diolefins having 4 to 10 carbon atoms include butadiene, pentadiene, piperylene, isoprene, cyclopentadiene, dicyclopentadiene, and methylpentadiene. Examples of aromatic compounds having 8 or more carbon atoms and an olefinically unsaturated bond include styrene, α-methylstyrene, β-methylstyrene, vinyltoluene, vinylxylene, indene, methylindene, and ethylindene. Furthermore, the raw material compounds for the petroleum resin do not all need to be by-products in the production of olefins by thermal decomposition of petroleum such as naphtha, and chemically synthesized unsaturated compounds may also be used.

[0032] Preferable examples of petroleum resins include dicyclopentadiene-based petroleum resins obtained by polymerization of cyclopentadiene or dicyclopentadiene, dicyclopentadiene-styrene-based petroleum resins obtained by copolymerizing these cyclopentadiene or dicyclopentadiene with styrene, C5-based petroleum resins obtained by polymerization of isoprene or piperylene, and C9-based petroleum resins obtained by polymerization of C9 monomers such as indene or vinyltoluene.

[0033] The compound having a carbon-carbon double bond and an alkoxysilyl group used in the above production method is a compound in which one or more organic groups having a carbon-carbon double bond and one or more alkoxy groups are bonded to a silicon atom. Examples of the organic group having a carbon-carbon double bond include vinyl, allyl, butenyl, cyclohexenyl, cyclopentadienyl, and (meth)acryloxypropyl, with vinyl, methacryloxy, and acryloxy groups being preferred. Examples of the alkoxy group include a methoxy group, an ethoxy group, an isopropoxy group, and a butoxy group. The number of alkoxy groups bonded to the silicon atom is preferably one or more, more preferably two or more, and even more preferably three. Specific examples of the compound having a carbon-carbon double bond and an alkoxysilyl group include vinyltriethoxysilane, vinyltrimethoxysilane, methacryloxypropyltrimethoxysilane, and methacryloxypropyltriethoxysilane, with vinyltriethoxysilane and vinyltrimethoxysilane being preferred. The amount of the compound having a carbon-carbon double bond and an alkoxysilyl group used in the production method is, in terms of silicon atoms of the compound having a carbon-carbon double bond and an alkoxysilyl group, preferably 0.1 to 10 mass%, more preferably 0.3 to 8 mass%, even more preferably 0.5 to 5 mass%, and even more preferably 1 to 4 mass%, based on the hydrogenated petroleum resin.

[0034] The radical-generating compound used in the above-mentioned production method can be a compound generally known as a radical polymerization initiator. The compound that generates radicals can be appropriately selected from, for example, various organic peroxides and azo compounds such as azobisisobutyronitrile and azobisisovaleronitrile, and among these, organic peroxides are preferred. Examples of organic peroxides include diacyl peroxides such as dibenzoyl peroxide, di(3,5,5-trimethylhexanoyl)peroxide, dilauroyl peroxide, didecanoyl peroxide, and di(2,4-dichlorobenzoyl)peroxide; hydroperoxides such as t-butyl hydroperoxide, cumene hydroperoxide, diisopropylbenzene hydroperoxide, and 2,5-dimethylhexane-2,5-dihydroperoxide; di-t-butyl peroxide, dicumyl peroxide, 2,5-dimethyl-2,5-di(t-butylperoxy)hexane, 1,1-di(t-butylperoxy)cyclohexane, 1,1-di(t-hexylperoxy)cyclohexane, 2,5-dimethyl-2,5-di(t-butylperoxy)hexyne-3, and α,α'-bis(t-butylperoxide). Examples of the peroxycarbonates include dialkyl peroxides such as diisopropyl peroxybenzene; peroxyketals such as 1,1-bis(t-butylperoxy)-3,3,5-trimethylcyclohexane and 2,2-bis(t-butylperoxy)butane; alkyl peresters such as 2,5-dimethyl-2,5-di(2-ethylhexanoylperoxy)hexane, n-butyl 4,4-di(t-butylperoxy)valerate, t-butyl peroxyoctoate, t-butyl peroxypivalate, t-butyl peroxyneodecanoate, and t-butyl peroxybenzoate; and peroxycarbonates such as di-2-ethylhexyl peroxydicarbonate, diisopropyl peroxydicarbonate, di-sec-butyl peroxydicarbonate, and t-butyl peroxyisopropyl carbonate. Among these, dialkyl peroxides are preferred. These may be used alone or in combination of two or more. The amount of the radical-generating compound used is not particularly limited, but is preferably 0.01 to 10% by mass, and more preferably 0.01 to 5% by mass, based on the hydrogenated petroleum resin.

[0035] As described above, a suitable method for producing the modified hydrogenated petroleum resin is a method of reacting a hydrogenated petroleum resin with a compound having a carbon-carbon double bond and an alkoxysilyl group in the presence of a compound that generates radicals. As long as the reaction proceeds sufficiently, there are no limitations on the reaction method. However, (1) a method of mixing a molten hydrogenated petroleum resin, a compound having a carbon-carbon double bond and an alkoxysilyl group, and a compound that generates radicals, and reacting the resulting mixture by generating radicals by heating or the like, is preferred, and (2) a method of dissolving a hydrogenated petroleum resin, a compound having a carbon-carbon double bond and an alkoxysilyl group, and a compound that generates radicals in an organic solvent, and reacting the resulting mixture by generating radicals by heating or the like is more preferred. (1) A method of mixing a molten hydrogenated petroleum resin, a compound having a carbon-carbon double bond and an alkoxysilyl group, and a compound that generates radicals, and reacting the resulting mixture by heating or the like is more preferred.

[0036] In the case of the above-mentioned method (1), it is preferable to melt the hydrogenated petroleum resin, mix it with a compound having a carbon-carbon double bond and an alkoxysilyl group, add a compound that generates radicals, and heat the mixture to react the hydrogenated petroleum resin with the carbon-carbon double bond portion of the compound having a carbon-carbon double bond and an alkoxysilyl group, thereby obtaining a modified hydrogenated petroleum resin. In the present method, when the hydrogenated petroleum resin has a low melt viscosity, it is preferable to carry out the reaction while stirring in a normal reaction apparatus, whereas when the hydrogenated petroleum resin has a high melt viscosity, it is preferable to carry out the reaction while melt-kneading using a roll mill, a Banbury mixer, an extruder, or the like. The reaction temperature is preferably from 100 to 300°C, more preferably from 100 to 200°C.

[0037] In the case of the above method (2), it is preferable to dissolve the hydrogenated petroleum resin in an organic solvent, mix it with a compound having a carbon-carbon double bond and an alkoxysilyl group, add a compound that generates radicals, and heat the mixture to react the hydrogenated petroleum resin with the carbon-carbon double bond portion of the compound having a carbon-carbon double bond and an alkoxysilyl group, thereby obtaining a modified hydrogenated petroleum resin. In the present method, examples of organic solvents that can be used include hydrocarbon solvents such as pentane, hexane, heptane, cyclohexane, toluene, xylene, and decahydronaphthalene; halogenated hydrocarbon solvents such as chlorobenzene, dichlorobenzene, and trichlorobenzene; and liquefied α-olefins. The reaction temperature is preferably from -50 to 300°C, more preferably from 0 to 300°C, further preferably from 100 to 300°C, and even further preferably from 100 to 200°C.

[0038] The blending amounts of the diene rubber polymer and the modified hydrogenated petroleum resin in the rubber composition for tires of this embodiment are preferably such that the rubber composition contains 1 to 20 parts by mass, and more preferably 5 to 15 parts by mass, of the modified hydrogenated petroleum resin per 100 parts by mass of the diene rubber polymer.

[0039] By making the content of the modified hydrogenated petroleum resin equal to or more than the lower limit, the dispersibility of silica in the rubber composition is improved, so that the deterioration of abrasion resistance caused by the aggregation of silica can be suppressed, and the content of oil and silane coupling agent can be reduced or eliminated, so that the processability is also improved. Furthermore, the rolling resistance is improved compared to the content of silica, so that the rubber composition for tires has excellent rolling resistance, abrasion resistance and processability in general.

[0040] (silica) The silica in the present invention is not particularly limited, and examples thereof include wet silica (hydrated silicic acid) and dry silica (anhydrous silicic acid), among which dry silica is preferred. The colloidal properties of the silica are not particularly limited, but the nitrogen adsorption specific surface area (BET) by the BET method is 150 to 250 m 2 / g is preferably used, and more preferably 180 to 230 m 2 The BET of silica is measured according to the BET method described in ISO 5794. The amount of silica blended in the rubber composition for tires of this embodiment is preferably 10 to 150 parts by mass, and more preferably 30 to 100 parts by mass, based on 100 parts by mass of the diene rubber polymer.

[0041] The rubber composition for tires may contain fillers other than silica. As the other fillers, for example, various inorganic fillers such as carbon black, titanium oxide, aluminum silicate, clay, or talc can be used, and these can be used alone or in combination of two or more. Among these, carbon black is preferably used.

[0042] The carbon black is not particularly limited, and various grades of furnace carbon black, such as SAF, ISAF, HAF, and FEF, which are used as reinforcing agents for rubber, can be used.

[0043] In addition to the above-mentioned components, the rubber composition for tires may contain various additives that are generally used in rubber compositions, such as oil, zinc oxide, stearic acid, antioxidants, wax, vulcanizing agents, vulcanization accelerators, flame retardants, curing accelerator catalysts, and silane coupling agents, within the range that does not impair the effects of the present invention.

[0044] The vulcanizing agent includes sulfur or a sulfur-containing compound (e.g., sulfur chloride, sulfur dichloride, polymeric polysulfide, morpholine disulfide, alkylphenol disulfide, etc.), which may be used alone or in combination of two or more. The amount of the vulcanizing agent is not particularly limited, but is preferably 0.1 to 10 parts by mass, more preferably 0.5 to 5 parts by mass, per 100 parts by mass of the diene rubber polymer.

[0045] As the vulcanization accelerator, for example, various vulcanization accelerators such as sulfenamide-based, thiuram-based, thiazole-based, or guanidine-based vulcanization accelerators can be used, and any one of them can be used alone or in combination of two or more. The amount of the vulcanization accelerator is not particularly limited, but is preferably 0.1 to 7 parts by mass, more preferably 0.5 to 5 parts by mass, based on 100 parts by mass of the diene rubber polymer.

[0046] The curing catalyst accelerates the curing by sulfur and accelerates the reaction between the macrosilane coupling agent (modified olefin polymer) and the diene rubber by sulfur. Examples of the curing catalyst include organometallic catalysts and tertiary amines. Examples of the organometallic catalysts include organometallic compounds such as dibutyltin dilaurate, dibutyltin diacetate, dibutyltin dioctoate, and tin octenate, as well as lead octenate and lead naphthenate. Examples of tertiary amines include N-triethylamine, N-methylmorpholine bis(2-dimethylaminoethyl) ether, N,N,N',N",N"-pentamethyldiethylenetriamine, N,N,N'-trimethylaminoethyl-ethanolamine, bis(2-dimethylaminoethyl) ether, N-methyl-N'-dimethylaminoethylpiperazine, and imidazole compounds in which the secondary amine functional group of the imidazole ring is substituted with a cyanoethyl group. These may be used alone or in combination of two or more. Among the above catalysts, dibutyltin dilaurate, dibutyltin diacetate, and dibutyltin dioctate are particularly preferred. The content of the curing-accelerating catalyst in the rubber composition for tires of the present invention is preferably 0.005 to 2.0 mass %, and more preferably 0.01 to 0.5 mass %, in the rubber composition for tires of the present invention.

[0047] For the purpose of further improving the dispersibility of silica in tire rubber, conventional silane coupling agent can be added to the extent that does not affect the effect of the present invention.As the silane coupling agent, sulfide-based silane coupling agent, mercapto-based silane coupling agent, vinyl-based silane coupling agent, amino-based silane coupling agent, glycidoxy-based silane coupling agent, nitro-based silane coupling agent, chloro-based silane coupling agent, etc. can be mentioned, and bis(3-triethoxysilylpropyl)tetrasulfide, bis(2-triethoxysilylethyl)tetrasulfide, 3-trimethoxysilylpropylbenzothiazoletetrasulfide, 3-mercaptopropyltrimethoxysilane are preferred. The content of the silane coupling agent in the rubber composition for tires of the present invention is 15 mass % or less based on the total amount of silica contained in the rubber composition for tires of the present invention.

[0048] The rubber composition for tires can be prepared by kneading in a conventional manner using a commonly used mixer such as a Banbury mixer, a kneader, a roll, etc. That is, in the first mixing stage, other additives except for the vulcanizing agent and the vulcanization accelerator are added and mixed with the diene rubber polymer together with the modified olefin polymer and silica, and then, in the final mixing stage, the vulcanizing agent and the vulcanization accelerator are added and mixed to the obtained mixture to prepare the rubber composition for tires. EXAMPLES

[0049] The present invention will be specifically described with reference to the following examples and comparative examples, although the present invention is not limited to the following examples.

[0050] [Analysis and evaluation of modified hydrogenated petroleum resins] [1. Silicon element concentration] 0.1 g of the modified hydrogenated petroleum resin, modified petroleum resin, or hydrogenated petroleum resin obtained in the Examples and Comparative Examples was heated in an electric furnace at 550°C for 12 hours, and a measurement solution was prepared by alkali fusion of the ash. ICP emission spectrometry was then performed (ICP emission spectrometry apparatus: 720-ES, manufactured by Agilent Technologies, Inc.) to determine the silicon concentration.

[0051] 2. Molecular weight and molecular weight distribution The average molecular weight was measured by gel permeation chromatography (GPC) using a GPC measuring device (HLC8220, detector: RI, columns: TSK-GEL GHXL-L, G4000HXL, G2000HXL, tetrahydrofuran as eluent, all manufactured by Tosoh Corporation), and the number average molecular weight (Mn) and weight average molecular weight (Mw) in terms of polystyrene were obtained, and the molecular weight distribution (Mw / Mn) was calculated.

[0052] [3. Integral ratio of aromatic hydrogen] Using a nuclear magnetic resonance (NMR) device (JNM-EX400, manufactured by JEOL Ltd.), the solvent was deuterated chloroform, and the number of accumulations was 256. 1 H-NMR measurement was performed, and the ratio of the integral value of the peak in the 6.5-7.5 ppm region (peak of aromatic hydrogen) to the sum of the integral values ​​of the peaks in the 0-3.0 ppm region and the 6.5-7.5 ppm region [integral value of the peak in the 6.5-7.5 ppm region / (integral value of the peak in the 0-3.0 ppm region and the sum of the integral values ​​of the peaks in the 6.5-7.5 ppm region)] was obtained. In this case, if there are peaks in the 0-3.0 ppm region and the 6.5-7.5 ppm region due to additives (antioxidants, etc.) or solvents (chloroform, etc.) in the raw materials, the standard substances were measured in the same manner, and the integral values ​​were subtracted from the integral value to obtain the above-mentioned integral value. However, the resin in the comparative example was a silane-modified untreated hydrogenated petroleum resin, and the integral ratio was obtained in the same manner.

[0053] [4. Softening point] Measurements were performed in accordance with JIS K 6863:1994.

[0054] [Production of petroleum resins and hydrogenated petroleum resins] Production Example 1 (Production of petroleum resin) 180 g of xylene was added to a 1-liter autoclave and the temperature was raised to 260° C. Then, a mixture of 100 g of dicyclopentadiene and 100 g of styrene was added over 3 hours. The temperature was maintained for an additional 75 minutes to carry out a polymerization reaction, and a polymer mixture was obtained. Thereafter, xylene was recovered from the resulting polymer mixture, and the mixture was then maintained at 20 mmHg for 2 hours to distill off low boiling points to obtain a petroleum resin having a softening point of 63.0°C.

[0055] Production Example 2 (Production of hydrogenated petroleum resin) 180 g of the petroleum resin obtained in Production Example 1, 180 g of ethylcyclohexane, and 4 g of a nickel-based catalyst (N110 series) manufactured by JGC Catalysts and Chemicals were charged into a 1-liter autoclave. Hydrogen was charged to 5 MPa, and the temperature was raised from room temperature to 230°C. Thereafter, while maintaining the hydrogen pressure at 5 MPa, a hydrogenation reaction was carried out for 8 hours to obtain a hydrogenated petroleum resin. The softening point of the obtained hydrogenated petroleum resin was 100°C. This is referred to as hydrogenated petroleum resin E.

[0056] [Production of modified petroleum resins and modified hydrogenated petroleum resins] Production Example 3 Into a 500 mL separable flask equipped with a nitrogen inlet tube and a stirring blade was placed 110 g of the hydrogenated petroleum resin E obtained in Production Example 2, and the mixture was heated to 140° C. in an oil bath under a nitrogen stream. Once the hydrogenated petroleum resin had dissolved, 12 g of vinyltrimethoxysilane (manufactured by Tokyo Chemical Industry Co., Ltd.) was added with stirring, and the mixture was stirred until it became uniform. Next, 0.5 g of an organic peroxide (2,5-dimethyl-2,5-di(t-butylperoxy)hexane, trade name "Perhexa (registered trademark) 25B", manufactured by NOF Corporation) was added dropwise. After the addition, the mixture was stirred at an internal temperature (reaction mixture temperature) of 145° C. for 1 hour to react. After the reaction was completed, the contents of the flask were removed onto a stainless steel tray and dried under vacuum at 150° C. for 1 hour to obtain 102 g of modified hydrogenated petroleum resin A. The analysis and evaluation results of the obtained modified hydrogenated petroleum resin A are shown in Table 1.

[0057] [Table 1]

[0058] Example 1 (Production of rubber composition for tires) In a Labo Plastomill (volume 50 g), 100 parts by mass of styrene-butadiene copolymer rubber (SBR) (manufactured by JSR Corporation, product name JSR0120) was masticated for 2 minutes, and then 2 parts by mass of stearic acid (manufactured by New Japan Chemical Co., Ltd.), 60 parts by mass of silica (manufactured by Admatec Corporation, product name Admafine S0-C4), and 15 parts by mass of the modified hydrogenated petroleum resin A obtained in Production Example 3 were added, and the mixture was taken out after a total kneading time of 8 minutes. The rotation speed was adjusted so that the compound temperature at the time of removal was 140 to 150°C. The resulting compound was cooled to room temperature, and then sheeted using a heat press. The cross sections of the center and edge of the sheet were observed under an optical microscope. The photographs are shown in Figure 1.

[0059] As is clear from Fig. 1, the rubber composition for tires of the present embodiment has excellent dispersibility of silica. Therefore, by using this rubber composition, a tire having excellent rolling resistance, abrasion resistance, and processability can be obtained. [Industrial Applicability]

[0060] The rubber composition for tires of the present embodiment is formulated with a specific modified hydrogenated petroleum resin, which further improves the dispersibility of silica, thereby making it possible to obtain a tire that is excellent in rolling resistance, abrasion resistance, and processability.

Claims

1. The rubber composition for tires comprises at least a diene-based rubber polymer, silica, and a modified hydrogenated petroleum resin that satisfies the following (A1) to (A3): (A1) Contains 0.1 to 10 mass% silicon element calculated as silicon atom (A2) Weight average molecular weight is 500 to 5,000 (A3) Molecular weight distribution (Mw / Mn) is 1.1 to 3.5

2. The modified hydrogenated petroleum resin is 1 2. The rubber composition for tires according to claim 1, wherein an integral ratio of aromatic hydrogen in H-NMR measurement [integral value of peak in 6.5 to 7.5 ppm region / (sum of integral value of peak in 0 to 3.0 ppm region and integral value of peak in 6.5 to 7.5 ppm region)] is 0 to 15%.

3. The rubber composition for tires according to claim 1 or 2, wherein the softening point of the modified hydrogenated petroleum resin is 60 to 150°C.

4. The rubber composition for tires according to any one of claims 1 to 3, comprising 1 to 20 parts by mass of the modified hydrogenated petroleum resin per 100 parts by mass of the diene rubber polymer.

5. The rubber composition for tires according to any one of claims 1 to 4, comprising 10 to 150 parts by mass of said silica per 100 parts by mass of said diene rubber polymer.

6. A tire using the rubber composition for tires according to any one of claims 1 to 5.

Citation Information

Patent Citations

  • Tire rubber composition

    JP2017088671A